Method for producing resin composition, method for manufacturing synthetic resin pellet, and molding

Incorporating polyamines into resin compositions with plant fibers reacts with corrosive gases to prevent mold corrosion and improve releasability and heat resistance, addressing mold issues and thermal stability in resin compositions.

JP2024135722APending Publication Date: 2024-10-04STANLEY ELECTRIC CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023046552
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Resin compositions containing synthetic resins and plant fibers face issues of mold corrosion and insufficient releasability due to the thermal decomposition of lignin and hemicellulose, generating corrosive gases, and lack of heat resistance.

Method used

Incorporating a polyamine with at least one primary or secondary amine into the resin composition to react with corrosive gases generated from plant fibers, enhancing mold releasability and heat resistance by forming carboxylic acid amides and imines, which suppress mold corrosion and improve the resin's thermal stability.

Benefits of technology

The method effectively prevents mold corrosion and enhances mold releasability while improving the heat resistance of the resin composition, ensuring better mold separation and thermal stability during injection molding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135722000001_ABST
    Figure 2024135722000001_ABST
Patent Text Reader

Abstract

To provide a method for producing a resin composition and a method for manufacturing a synthetic resin pellet which suppress corrosion of a mold used for molding a resin composition containing a synthetic resin and a vegetable fiber, and can improve releasability from a mold and heat resistance, and a molding.SOLUTION: A method for producing a resin composition includes a step of melting and kneading a vegetable fiber 11, a polyolefin-based resin, and polyamine 20 having at least one of primary amine and secondary amine, and obtaining a resin composition.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing plant fibers and a synthetic resin, a method for producing synthetic resin pellets, and a molded article. [Background technology]

[0002] Conventionally, in order to ensure the strength of a resin composition, a method has been adopted in which vegetable fibers or inorganic materials such as calcium carbonate, talc, or glass fibers are mixed as a filler into the base synthetic resin. In particular, vegetable fibers have a lower specific gravity than inorganic materials, and are therefore used as a filler as a method for improving the strength of a resin composition while reducing its weight.

[0003] However, since plant fibers are composed of components such as lignin and hemicellulose, when the temperature of the plant fibers rises to a high temperature (about 200° C.), the lignin and hemicellulose undergo thermal decomposition to generate corrosive gases such as carboxylic acids. Therefore, when a resin composition composed of plant fibers and a synthetic resin is injection molded at high temperatures, there is a risk that the mold used for injection molding may be corroded.

[0004] For example, Patent Document 1 discloses a method for producing a molded body made of plant fibers and synthetic resin, in which calcium oxide is added as an acid scavenger when producing the molded body. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2014 / 017274 Summary of the Invention [Problem to be solved by the invention]

[0006] However, there is a concern that a resin composition containing a synthetic resin and plant fibers corrodes a mold used for molding and has insufficient releasability from the mold, resulting in a molded body not being able to be released from the mold. In addition, there is a problem that the resin composition made of a synthetic resin and plant fibers has insufficient heat resistance.

[0007] The present invention has been made in consideration of the above-mentioned points, and aims to provide a method for producing a resin composition and synthetic resin pellets, as well as a molded product, which suppresses corrosion of a mold used in molding a resin composition containing a synthetic resin and a plant fiber and has improved releasability from the mold and heat resistance. [Means for solving the problem]

[0008] The method for producing the resin composition of the present invention comprises the steps of: The method includes a step of melt-kneading plant fibers, a polyolefin resin, and a polyamine having at least one of a primary amine and a secondary amine to obtain a resin composition. [Brief description of the drawings]

[0009] [Figure 1] 1A to 1C are diagrams illustrating a process for producing a resin composition and a molded article according to the present invention. [Diagram 2] FIG. 1 is a diagram showing a reaction process between a corrosive gas and a primary amine and / or a secondary amine. [Diagram 3] 1A to 1C are diagrams illustrating a process for producing a resin composition and a molded article according to the present invention. [Figure 4] FIG. 2 is a diagram showing a manufacturing process of the synthetic resin pellet of the present invention. [Diagram 5] 1 is a table summarizing the results of comparison between examples and comparative examples of the resin composition of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] An embodiment of the present invention will be described. As shown in Fig. 1, in the method for producing a resin composition of this embodiment, synthetic resin pellets 10 containing plant fibers and polyamine 20 having at least one of a primary amine and a secondary amine are melt-kneaded in a twin-screw mixer 40 at a screw rotation speed of 250 rpm and a cylinder temperature of 200°C to obtain a resin composition 30. The resin composition 30 is injected into a molding machine 41 and injection molded at high temperature to obtain a molded body 31.

[0011] The plant fibers 11 refer to natural fibers obtained from plants, and their main components are cellulose, hemicellulose, and lignin, which are structural components of plant cell walls. As shown in Fig. 2, hemicellulose and lignin are thermally decomposed at high temperatures (about 200°C) to generate reactive substances such as organic acids such as carboxylic acids, which are corrosive gases 11A, and aldehydes.

[0012] Carboxylic acid reacts with primary amines and / or secondary amines to form carboxylic acid amides. This prevents the carboxylic acid from reacting with the mold (e.g., iron) used in injection molding, causing the mold to corrode. As an example, the reaction mechanism of carboxylic acid and primary amine is shown below. [ka]

[0013] In addition, aldehydes react with primary amines and / or secondary amines to form imines. This prevents the aldehyde from reacting with the mold (e.g., iron) used in injection molding, causing the mold to corrode. As an example, the reaction mechanism between the aldehyde and primary amine is shown below. [ka]

[0014] Corrosive gas 11A generated from hemicellulose or lignin contains a large proportion of long-chain fatty acids. The long-chain fatty acids reacted with primary amines and / or secondary amines are oriented in the flow direction due to the flow during injection molding. Since most of the long-chain fatty acids are hydrophobic hydrocarbon groups, the resin composition exerts a wax effect on its surface layer, resulting in high releasability from a hydrophobic mold.

[0015] Since the resin composition 30 contains the polyamine 20 having at least one of a primary amine and a secondary amine, the melting point is increased, and therefore the heat resistance of the resin composition can be improved.

[0016] Examples of the plant fiber 11 used in the resin composition of the present invention include wood flour, wood fibers such as paper, cellulose fibers, cellulose nanofibers, biomass materials derived from plants, cellulose extracted from plants or separately synthesized, hemicellulose, lignin, etc. Examples of the wood flour that can be used include wood flour derived from conifers, broad-leaved trees, rice straw, rice husks, wheat straw, bamboo, pine, cedar, cypress, kenaf, pulp, sisal hemp, Manila hemp, jute hemp, coconut, corn, reed, palm, and papyrus.

[0017] The blending amount of the plant fiber 11 is preferably 10% by weight (wt%) to 85% by weight, more preferably 30% by weight to 70% by weight, based on the total amount of the resin composition 30. When the blending amount of the plant fiber is low, it is difficult to ensure sufficient strength, so the blending amount of the plant fiber is preferably 10% by weight or more, more preferably 30% by weight or more. In addition, the strength increases as the blending amount of the plant fiber increases, but on the other hand, the fluidity of the resin composition decreases and it becomes difficult to knead sufficiently, so the blending amount of the plant fiber is preferably 85% by weight or less, more preferably 70% by weight or less. When it is difficult to knead the resin composition sufficiently, the reaction between the primary amine and / or the secondary amine and the corrosive gas 11A becomes insufficient, and most of the corrosive gas 11A remains in an unreacted state. Therefore, the corrosion of the mold used during injection molding is not sufficiently suppressed. In addition, it is difficult to ensure sufficient moldability due to the decrease in the fluidity of the resin composition.

[0018] The synthetic resin used in the resin composition 30 of the present invention may be a polyolefin resin such as polypropylene (PP), polybutylene terephthalate (PBT), or polyethylene (PE).

[0019] The amount of the synthetic resin is preferably 15% by weight to 90% by weight, and more preferably 30% by weight to 70% by weight, based on the total amount of the resin composition 30. When the amount of the synthetic resin is low, the fluidity of the resin composition decreases and it becomes difficult to knead it sufficiently, so the amount of the synthetic resin is preferably 15% by weight or more, and more preferably 30% by weight or more. When it is difficult to knead the resin composition sufficiently, the reaction between the primary amine and / or the secondary amine and the corrosive gas 11A becomes insufficient, and most of the corrosive gas 11A remains in an unreacted state. Therefore, the corrosion of the mold used during injection molding is not sufficiently suppressed. In addition, when the amount of the synthetic resin is high, it is difficult to ensure sufficient strength, so the amount of the synthetic resin is preferably 90% by weight or less, and more preferably 70% by weight or less. In addition, since the synthetic resin is made from fossil fuels such as petroleum, reducing the amount of the synthetic resin is also useful from the viewpoint of environmental resource conservation.

[0020] As the polyamine 20 having at least one of a primary amine and a secondary amine used in the resin composition 30 of the present invention, an aromatic amine can be used in addition to an aliphatic amine such as polyethyleneimine, polyallylamine, polyvinylamine, polypropyleneimine, polybutyleneimine, or polyisopropyleneimine. If the boiling point of the polyamine having at least one of a primary amine and a secondary amine is low, there is a concern that it will evaporate when melted and kneaded with the plant fiber 11 and the synthetic resin. Therefore, it is more preferable to use an aliphatic amine or aromatic amine having a boiling point or decomposition temperature of 250° C. or higher.

[0021] The amount of polyamine 20 having at least one of primary amine and secondary amine is preferably 0.05% by weight to 5.00% by weight, more preferably 0.1% by weight to 3.0% by weight, relative to the plant fiber 11. When the amount of polyamine is less than 0.05% by weight, the amount of primary amine and / or secondary amine is insufficient relative to the corrosive gas 11A, so that a large amount of the corrosive gas 11A remains unreacted. Therefore, the corrosion of the mold used during molding is not sufficiently suppressed. When the amount of polyamine is more than 5.00% by weight, the amount of polyamine is excessive relative to the corrosive gas 11A generated from the plant fiber 11. The excess polyamine reacts with the hydrophobic component of the resin composition that exhibits releasability from a hydrophobic mold, thereby reducing the releasability of the resin composition from the mold.

[0022] The weight average molecular weight (Mw) of the polyamine 20 having at least one of the primary amine and the secondary amine is preferably 300 to 100,000, more preferably 10,000 to 100,000, and further preferably 10,000 to 70,000. If the weight average molecular weight of the polyamine is smaller than 300, the polyamine will volatilize due to heat during melt-kneading with the plant fiber 11 and the synthetic resin. Therefore, the wax effect on the surface of the resin composition will not be expressed, and the mold releasability will decrease. In addition, if the weight average molecular weight is small, the toxicity of the polyamine is high, so care must be taken when handling it. Therefore, the workability during production will decrease. If the weight average molecular weight of the polyamine is larger than 100,000, the viscosity of the resin composition will increase, making it difficult to knead it sufficiently. Therefore, the reaction between the primary amine and / or the secondary amine and the corrosive gas will be insufficient, and a large amount of the corrosive gas will remain in an unreacted state. Therefore, the corrosion of the mold used during injection molding will be insufficiently suppressed. Furthermore, when the weight-average molecular weight of the polyamine is greater than 100,000, the proportion of tertiary amines per unit mass becomes large, and the proportion of primary amines and / or secondary amines that react with the corrosive gas 11A becomes small, resulting in insufficient inhibition of corrosion of the mold used during injection molding.

[0023] The present invention will be described in more detail below with reference to modified examples, although the present invention is not limited to these modified examples. [Variation 1] A first modified example of the method for producing a resin composition of this embodiment will be described. As shown in Fig. 3, in the first modified example of the method for producing a resin composition of this embodiment, a plant fiber 11, a synthetic resin 12, and a polyamine 20 having at least one of a primary amine and a secondary amine are melt-kneaded in a twin-screw mixer 40 at a screw rotation speed of 250 rpm and a cylinder temperature of 200°C to obtain a resin composition 30. The resin composition 30 is injected into a molding machine 41 and injection molded at high temperature to obtain a molded body 31.

[0024] [Variation 2] A second modified example of the method for producing a resin composition according to the present embodiment will be described below. As shown in Fig. 4, in the second modified example of the method for producing a resin composition according to the present embodiment, synthetic resin pellets 10 containing plant fibers and polyamine 20 containing at least one of a primary amine and a secondary amine are melt-kneaded in a twin-screw mixer 40 at a screw rotation speed of 250 rpm and a cylinder temperature of 200°C to obtain synthetic resin pellets 32 containing plant fibers and polyamine as a resin composition.

[0025] The uses of the molded article made from the resin composition of the present invention are not particularly limited, and it can be used for automobile exterior and interior parts, fixtures, daily necessities such as stationery, etc. In addition, since the molded article made from the resin composition of the present invention has excellent heat resistance, it is particularly useful for use in the vicinity of a heat source such as a light source, such as a housing or bracket of a vehicle lamp. EXAMPLES

[0026] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0027] Example 1 Polypropylene (PP) was used as the synthetic resin, wood flour derived from broadleaf trees as the plant fiber, and polyethyleneimine (PEI) with a weight-average molecular weight of 300 as the polyamine. Polypropylene, wood flour, and polyethyleneimine were melt-kneaded in a weight ratio of 44.99:54.98:0.027 to produce pellets of polypropylene blended with wood flour. In other words, the amount of polyethyleneimine added to the wood flour was 0.05% by weight.

[0028] Example 2 Polypropylene (PP) was used as the synthetic resin, wood flour derived from broadleaf trees as the plant fiber, and polyethyleneimine (PEI) with a weight average molecular weight of 10,000 as the polyamine. Polypropylene, wood flour, and polyethyleneimine were melt-kneaded in a weight ratio of 44.99:54.98:0.027 to produce pellets of polypropylene mixed with wood flour. In other words, the amount of polyethyleneimine added to the wood flour was 0.05% by weight.

[0029] Example 3 Polypropylene (PP) was used as the synthetic resin, wood flour derived from broadleaf trees as the plant fiber, and polyethyleneimine (PEI) with a weight average molecular weight of 70,000 as the polyamine. Polypropylene, wood flour, and polyethyleneimine were melt-kneaded in a weight ratio of 44.99:54.98:0.027 to produce pellets of polypropylene mixed with wood flour. In other words, the amount of polyethyleneimine added to the wood flour was 0.05% by weight.

[0030] Example 4 Polypropylene (PP) was used as the synthetic resin, wood flour derived from broadleaf trees as the plant fiber, and polyethyleneimine (PEI) with a weight-average molecular weight of 100,000 as the polyamine. Polypropylene, wood flour, and polyethyleneimine were melt-kneaded in a weight ratio of 44.99:54.98:0.027 to produce pellets of polypropylene mixed with wood flour. In other words, the amount of polyethyleneimine added to the wood flour was 0.05% by weight.

[0031] Example 5 Polypropylene (PP) was used as the synthetic resin, wood flour derived from broadleaf trees as the plant fiber, and polyethyleneimine (PEI) with a weight-average molecular weight of 10,000 as the polyamine. Polypropylene, wood flour, and polyethyleneimine were melt-kneaded in a weight ratio of 44.98:54.97:0.055 to produce pellets of polypropylene mixed with wood flour. In other words, the amount of polyethyleneimine added to the wood flour was 0.10% by weight.

[0032] Example 6 Polypropylene (PP) was used as the synthetic resin, wood flour derived from broadleaf trees as the plant fiber, and polyethyleneimine (PEI) with a weight-average molecular weight of 10,000 as the polyamine. Polypropylene, wood flour, and polyethyleneimine were melt-kneaded in a weight ratio of 44.27:54.11:1.623 to produce pellets of polypropylene mixed with wood flour. In other words, the amount of polyethyleneimine added to the wood flour was 3.00% by weight.

[0033] Example 7 Polypropylene (PP) was used as the synthetic resin, wood flour derived from broadleaf trees as the plant fiber, and polyethyleneimine (PEI) with a weight-average molecular weight of 10,000 as the polyamine. Polypropylene, wood flour, and polyethyleneimine were melt-kneaded in a weight ratio of 43.80:53.53:2.676 to produce pellets of polypropylene mixed with wood flour. In other words, the amount of polyethyleneimine added to the wood flour was 5.00% by weight.

[0034] Example 8 Polypropylene (PP) was used as the synthetic resin, wood flour derived from coniferous trees as the plant fiber, and polyethyleneimine (PEI) with a weight-average molecular weight of 10,000 as the polyamine. Polypropylene, wood flour, and polyethyleneimine were melt-kneaded in a weight ratio of 44.98:54.97:0.055 to produce pellets of polypropylene mixed with wood flour. In other words, the amount of polyethyleneimine added to the wood flour was 0.10% by weight.

[0035] Example 9 Polypropylene (PP) was used as the synthetic resin, wood flour derived from coniferous trees as the plant fiber, and polyethyleneimine (PEI) with a weight-average molecular weight of 10,000 as the polyamine. Polypropylene, wood flour, and polyethyleneimine were melt-kneaded in a weight ratio of 44.27:54.11:1.623 to produce pellets of polypropylene mixed with wood flour. In other words, the amount of polyethyleneimine added to the wood flour was 3.00% by weight.

[0036] Example 10 Polypropylene (PP) was used as the synthetic resin, wood flour derived from coniferous trees as the plant fiber, and polyallylamine (PAA) with a weight average molecular weight of 10,000 as the polyamine. Polypropylene, wood flour, and polyallylamine were melt-kneaded in a weight ratio of 44.98:54.97:0.055 to produce pellets of polypropylene mixed with wood flour. In other words, the amount of polyethyleneimine added to the wood flour was 0.10% by weight.

[0037] Example 11 Polypropylene (PP) was used as the synthetic resin, wood flour derived from coniferous trees as the plant fiber, and polyallylamine (PAA) with a weight average molecular weight of 10,000 as the polyamine. Polypropylene, wood flour, and polyallylamine were melt-kneaded in a weight ratio of 44.27:54.11:1.623 to produce pellets of polypropylene blended with wood flour. In other words, the amount of polyethyleneimine added to the wood flour was 3.00% by weight.

[0038] Comparative Example 1 Polypropylene (PP) was used as the synthetic resin, and wood flour derived from broadleaf trees was used as the plant fiber. Polypropylene and wood flour were melt-kneaded in a ratio of 45:55 to produce wood-flour-blended polypropylene pellets.

[0039] (Evaluation of releasability) Test pieces were prepared by injection molding the wood flour-blended polypropylene pellets of Examples 1 to 11 and Comparative Example 1. The contact area between the test piece and the mold after the ejection step in injection molding was visually checked to evaluate the mold releasability on a five-level scale of A to E. The evaluation was as follows: A when 100% of the surface of the test piece was separated from the mold; B when 70% or more and less than 100% of the surface of the test piece was separated from the mold; C when 50% or more and less than 70% of the surface of the test piece was separated from the mold; D when 20% or more and less than 50% of the surface of the test piece was separated from the mold; and E when less than 20% of the surface of the test piece was separated from the mold. FIG. 5 shows the evaluation results of the mold releasability of Examples 1 to 11 and Comparative Example.

[0040] (Corrosivity evaluation) 100 test pieces were prepared by injection molding the wood powder-blended polypropylene pellets of Examples 1 to 11 and Comparative Example 1. The state of the surface of the mold was confirmed every time a test piece was prepared, and the corrosiveness was evaluated on a scale of 5 from A to E based on the number of test pieces prepared until the surface of the mold was contaminated. Here, the surface of the mold is contaminated when rust is confirmed on the surface of the mold. The evaluation was as follows: A when no contamination of the mold surface was confirmed when 100 test pieces were prepared; B when contamination of the mold surface was confirmed when 31 to 99 test pieces were prepared; C when contamination of the mold surface was confirmed when 11 to 30 test pieces were prepared; D when contamination of the mold surface was confirmed when 2 to 10 test pieces were prepared; and E when contamination of the mold surface was confirmed when one test piece was prepared. FIG. 5 shows the evaluation results of the corrosiveness of Examples 1 to 11 and Comparative Example.

[0041] (Evaluation of heat resistance) The deflection temperature under load of the wood flour-blended polypropylene pellets of Examples 1 to 11 and Comparative Example 1 was measured in accordance with ISO-75 at a load of 0.45 MPa and a heating rate of 2°C / min. The measurements were performed three times each, and the heat resistance was evaluated on a five-level scale of A to E based on the average. When the deflection temperature under load was 140°C or higher, it was rated as A; when the deflection temperature under load was 130°C or higher and lower than 140°C, it was rated as B; when the deflection temperature under load was 125°C or higher and lower than 130°C, it was rated as C; when the deflection temperature under load was 120°C or higher and lower than 125°C, it was rated as D; and when the deflection temperature under load was lower than 120°C, it was rated as E. The evaluation results of the heat resistance of Examples 1 to 11 and Comparative Example are shown together in FIG. 5.

[0042] As is clear from FIG. 5, according to Examples 1 to 11, which are wood flour-blended polypropylene pellets to which polyethyleneimine or polyacrylamine has been added, it is clear that the mold releasability during injection molding is ensured, corrosion of the mold during injection molding is inhibited, and excellent heat resistance is imparted.

[0043] In particular, from the results of Examples 2 to 11, it is clear that when the weight-average molecular weight of polyethyleneimine is 10,000 or more, 100% of the surface of the test piece is separated from the mold after ejection in injection molding, so that better releasability can be ensured. In addition, it is clear that better corrosion resistance can be ensured because contamination was not observed on the mold surface until 30 or more test pieces were produced, and it is clear that better heat resistance can be ensured because the deflection temperature under load is 130°C or more.

[0044] From the results of Examples 5 to 11, it is clear that when the amount of polyethyleneimine added to the wood flour is 0.10% or more, no contamination of the mold surface was observed when 100 test pieces were produced by injection molding, thereby ensuring better corrosion resistance.

[0045] From the results of Examples 5 to 6 and Examples 8 to 10, it is clear that when the weight average molecular weight of the polyethyleneimine or polyacrylamine is 10,000 or more and 70,000 or less, and the amount of polyethyleneimine or polyacrylamine added to the wood flour is 0.05% or more and 3.00% or less, the deflection temperature under load of the test specimen is 140°C or more, and therefore even better heat resistance can be ensured.

[0046] From the results of Examples 8 to 11, it is clear that even when wood flour derived from coniferous trees is used, when the amount of polyethyleneimine added to the wood flour is 0.10% or more and 3.00% or less, the same effect is achieved as when wood flour derived from broad-leaved trees is used.

[0047] From the results of Examples 10 to 11, it is clear that even when a polyallylamine with a weight average molecular weight of 10,000 is used as the polyamine, when the amount of polyallylamine added to the wood flour is 0.10% or more and 3.00% or less, the same effect is achieved as when polyethyleneimine is used as the polyamine.

[0048] In contrast, in Comparative Example 1, which is a pellet of polypropylene blended with wood flour made of polypropylene and wood flour derived from broadleaf trees, 80% or more of the surface of the test piece after the ejection step in injection molding is in contact with the mold, and sufficient releasability from the mold during injection molding is not ensured. In addition, contamination was confirmed on the surface of the mold in the production of one test piece, so corrosion of the mold during injection molding was not suppressed, and furthermore, the deflection temperature under load of the test piece is less than 120°C, which clearly indicates that sufficient heat resistance cannot be imparted.

[0049] As described above, the resin composition and the method for producing synthetic resin pellets, and the molded body of the present invention can suppress corrosion of a mold used for molding a resin composition containing a synthetic resin and a plant fiber, and can improve releasability from the mold and heat resistance. [Explanation of symbols]

[0050] 10. Synthetic resin pellets containing plant fibers 11 Plant Fiber 11A Corrosive gas 12 Synthetic resin 20 Polyamines 30 Resin composition 31 Molded body 32 Synthetic resin pellets containing plant fibers and polyamines 40 Twin screw mixer 41 Molding machine

Claims

1. A method for producing a resin composition, comprising the step of melt-kneading plant fibers, a polyolefin resin, and a polyamine having at least one of a primary amine and a secondary amine to obtain a resin composition.

2. A method for producing the resin composition according to claim 1, The blending amount of the plant fiber is 10 wt % or more and 85 wt % or less with respect to the resin composition, A method for producing a resin composition, wherein the blending amount of the polyolefin resin is 15 wt % or more and 90 wt % or less with respect to the resin composition.

3. A method for producing the resin composition according to claim 1, The polyamine has a weight average molecular weight of 10,000 or more and 100,000 or less.

4. A method for producing the resin composition according to claim 1, A method for producing a resin composition, wherein the amount of the polyamine added is 0.1 wt % or more and 5.0 wt % or less with respect to the plant fibers.

5. A method for producing the resin composition according to claim 1, The weight average molecular weight of the polyamine is 10,000 or more and 70,000 or less, A method for producing a resin composition, wherein the amount of the polyamine added is 0.1 wt % or more and 3.0 wt % or less with respect to the plant fibers.

6. A method for producing the resin composition according to claim 1, A method for producing a resin composition, wherein the plant fiber is wood flour derived from a coniferous tree.

7. A method for producing the resin composition according to claim 1, A method for producing a resin composition used for a housing or bracket of a vehicle lamp.

8. A molded article made of a resin composition obtained by the method according to any one of claims 1 to 7.

9. A method for producing resin pellets, comprising the step of melt-kneading plant fibers, a polyolefin resin, and a polyamine having at least one of a primary amine and a secondary amine to obtain resin pellets.

Citation Information

Patent Citations

  • Vehicle lamp

    WO2014017274A1