Water dispersion for shielding material
The aqueous dispersion with a black pigment and specific copolymer forms uniform irregularities on the coating film, addressing particle sedimentation issues and achieving a low-gloss, high-quality light-shielding film.
Patent Information
- Application Number
- JP2023046560
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing shielding materials face issues with particle sedimentation and uneven distribution, leading to unstable quality and glossiness in coating films due to the incorporation of large particles.
An aqueous dispersion comprising a black pigment, a neutralized isobutylene/maleic anhydride copolymer, a water-soluble resin with an acid value of 240 or less, and water, which forms uniform irregularities on the coating film during drying, achieving diffuse reflection and low gloss without large particles.
The solution results in an environmentally friendly dispersion that forms a black, low-gloss, and highly compatible light-shielding film with excellent redispersibility and shielding properties.
Smart Images

Figure 2024135726000001 
Figure 2024135726000002 
Figure 2024135726000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous dispersion for a shielding material capable of forming a shielding material such as a black, low-gloss light-shielding film or a shielding film. [Background technology]
[0002] Conventionally, black anti-reflective paints and anti-reflective films have been used not only in optical devices such as cameras, but also in luminous display devices such as meters to prevent peripheral reflection and block visible light, thereby improving visibility. They are also used as internal anti-reflective black paints for optical elements to form coating films on the edges, ridges, and edges of optical elements such as lenses and prisms, and to absorb stray light that causes flare and ghosts. In addition, black anti-reflective paints have attracted attention as paints that improve design due to their jet black color.
[0003] Examples of such coating materials and resin compositions for shielding materials include: 1) An internal reflection-preventive black paint for optical elements, comprising at least a metal oxide, carbon black, a binder resin, a dispersant, and a solvent, the metal oxide being at least one selected from ferric oxide, triiron tetraoxide, ferric oxyhydroxide, and zirconia, having a pH of 3.0 to 8.0, and being contained in an amount of 25 to 75% by mass in the solid content of the black paint, the carbon black having a volatile content of 0.6 to 6.0% by mass and a pH of 3.0 to 8.0, and being contained in an amount of 2 to 20% by mass in the solid content of the black paint, the dispersant being composed of a phthalocyanine compound and a polymeric dispersant, the phthalocyanine compound being contained in an amount of 1 to 20% by mass relative to the carbon black, and the polymeric dispersant having an amine value of 5 mgKOH / g to 100 mgKOH / g, and being contained in an amount of 5 to 40% by mass relative to the total of the metal oxide and the carbon black (see, for example, Patent Document 1). 2) A light-shielding film including at least a black layer, the content of the black pigment included in the black layer being 20 to 60% by mass with respect to the total mass of the black layer, the reflectance of light having at least one wavelength selected from the wavelength range of 800 to 1000 nm being 3.0% or less, and the transmittance of light having a wavelength of 400 to 750 nm being 50% or less (see, for example, Patent Document 2). 3) A surface anti-reflective coating is known which contains a binder resin, carbon black, hydrophobically treated dry silica, roughening particles, and a solvent, the roughening particles being polyamide resin particles having an average particle size of 10 μm or more and 20 μm or less, the amount of the polyamide resin particles being added being 24 parts by mass or more and 44 parts by mass or less relative to 100 parts by mass of the binder resin, and the amount of the hydrophobically treated dry silica being 14 parts by mass or more relative to 100 parts by mass of the binder resin (see, for example, Patent Document 3).
[0004] However, in the coating materials, resin compositions, and the like for shielding materials described in the above Patent Documents 1 to 3, particles of 1 μm or more may be blended in order to obtain a low-gloss coating film. In such cases, problems may arise such as uneven distribution of the particles due to settling or floating of the particles, and unstable quality unless the particles are sufficiently stirred before use. Thus, there is currently a strong demand for an aqueous dispersion for shielding materials that can form a black, low-gloss coating film, and the like. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP-A-9-143410 (claims, examples, etc.) [Patent Document 2] JP 2014-105282 A (Claims, Examples, etc.) [Patent Document 3] JP 2019-119855 A (Claims, Examples, etc.) Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above-mentioned problems and current situations of the conventional technology and aims to solve these problems, and has an object to provide an aqueous dispersion for a shielding material and a shielding material which can form a black, low-gloss shielding material such as a light-shielding film or a shielding film by forming irregularities on the surface during the drying process of a coating film or the like containing a black pigment and causing diffuse reflection, without blending large particles. [Means for solving the problem]
[0007] In view of the above-mentioned problems in the conventional art, the present inventors have conducted intensive research and have found that the above-mentioned intended aqueous dispersion for a shielding material and shielding material can be obtained by containing at least a black pigment, a neutralized product of a copolymer having specific physical properties, a water-soluble resin and / or a resin emulsion, and water, thereby completing the present invention.
[0008] That is, the aqueous dispersion for shielding material of the present invention is characterized by containing at least a black pigment, a neutralized product of an isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion having an acid value of 240 or less, and water. The glass transition temperature (Tg) of the water-soluble resin and the resin in the resin emulsion is preferably 140° C. or lower. Furthermore, it is preferable that the composition contains a polyol having two or more OH groups. The shielding material of the present invention is characterized by using the aqueous dispersion for shielding material having the above-mentioned constitution. The surface roughness Ra of the shielding material is preferably 0.2 to 2.0 μm. Effect of the Invention
[0009] According to the present invention, there is provided an aqueous dispersion for a shielding material and a shielding material, which are environmentally friendly aqueous dispersions without incorporating large particles, and which can form shielding materials such as light-shielding films and shielding films that are black and have a high degree of redispersibility and low gloss by forming unevenness on the surface during the drying process of a coating film or the like containing a black pigment, causing diffuse reflection. The objects and advantages of the invention will be realized and obtained by means of the elements and combinations particularly pointed out in the claims. Both the foregoing general description and the following detailed description are exemplary and explanatory but are not restrictive of the invention as claimed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following describes in detail the embodiments of the present invention. However, please note that the technical scope of the present invention is not limited to the embodiments described in detail below, but extends to the inventions described in the claims and their equivalents. The present invention can be implemented based on the contents disclosed in this specification and common technical knowledge in the relevant field (including design matters and obvious matters).
[0011] <Water dispersion for shielding materials> The aqueous dispersion for shielding material of the present invention is characterized by containing at least a black pigment, a neutralized product of an isobutylene-maleic anhydride copolymer, a water-soluble resin and / or a resin emulsion having an acid value of 240 or less, and water.
[0012] <Black pigment> The black pigment used in the present invention may be, for example, at least one selected from carbon-based black pigments and oxide-based black pigments. Examples of carbon-based black pigments include carbon blacks such as furnace black, acetylene black, thermal black, and channel black, black mica, graphite powder, graphite powder, and carbon nanotubes that are commercially available. Examples of oxide-based black pigments include at least one selected from the group consisting of cobalt oxide, iron tetroxide, ferrous oxide, manganese oxide, titanium black, chromium oxide, bismuth oxide, stannous oxide, cupric oxide or copper-iron-manganese oxide, aniline black, perylene black, iron manganese bismuth black, cobalt iron chrome black, copper chrome manganese black, iron chrome black, manganese bismuth black, manganese yttrium black, iron manganese oxide spinel black, copper chromite spinel black, hematite, magnetite, micaceous iron oxide, titanium black, and iron-containing metal oxides and composite metal oxides.
[0013] Among these black pigments, it is preferable to use carbon black, which has excellent light-shielding properties, and commercially available products such as Mitsubishi Chemical's #5, #10, #20, #25, #30, #32, #33, #40, #44, #45, #47, #52, #85, #95, CF9, MA7, MA8, MA11, MA100, MA220, and MA230, and Printex series such as Printex25, 35, 40, 45, 55, 150T, U, V, P, and L6, manufactured by Evonik Industries, and perylene black pigments, which have improved electrical reliability, and commercially available products such as BASF's Lumogen Black Series and Paliogen Black Series, are preferably used. Aluminum flake pigments (black interference aluminum pigments) with excellent heat-shielding properties can also be used.
[0014] These black pigments can be used either alone or in combination of two or more (hereinafter simply referred to as "at least one"). In addition, it is preferable that these black pigments have an average particle size of 1 μm or less in order to effectively exhibit other functions such as hiding power, optical properties, light-shielding properties, light reflectivity, and design properties without impairing performance such as processability. In addition, in the present invention, black resin particles used as coloring materials in inks for writing instruments, such as black resin particles containing a black pigment and resin particles in which a resin emulsion is colored with a black dye, are not included in the present invention from the standpoints of light resistance, light transmittance, etc.
[0015] In addition to black pigments such as the carbon-based black pigments and oxide-based black pigments, inorganic pigments, organic pigments, and dyes other than the above-mentioned black pigments can be used from the viewpoint of complementary colors of the above-mentioned black pigments, etc., within a range that does not impair the effects of the present invention. Examples of inorganic pigments and organic pigments include azo pigments, disazo pigments, isoindolinone pigments, quinophthalone pigments, isoindoline pigments, anthraquinone pigments, anthrone pigments, xanthene pigments, diketopyrrolopyrrole pigments, anthraquinone (anthrone) pigments, perinone pigments, quinacridone pigments, indigotine pigments, dioxazine pigments, phthalocyanine pigments, and azomethine pigments. Examples of inorganic pigments include red pigments such as manganese oxide-alumina, chromium oxide-tin oxide, iron oxide, cadmium sulfide-selenium sulfide, blue pigments such as cobalt oxide, zirconia-vanadium oxide, chromium oxide-divanadium pentoxide, yellow pigments such as zirconium-silicon-praseodymium, vanadium-tin, chromium-titanium-antimony, green pigments such as chromium oxide, cobalt-chromium, alumina-chromium, and pink pigments such as aluminum-manganese, iron-silicon-zirconium, and the like. Examples of dyes that can be used include dyes in any form, such as oil-soluble dyes, acid dyes, direct dyes, basic dyes, mordant dyes, acid mordant dyes, etc. The dyes may be used in the form of lakes or salts of dyes and nitrogen-containing compounds.
[0016] In the present invention (including examples), the "average particle size" is a value measured by laser diffraction or dynamic light scattering. In the laser diffraction method, it is a value of D50 calculated on a volume basis. This measurement can be performed using, for example, a particle size distribution analyzer HRA9320-X100 manufactured by Nikkiso Co., Ltd., and the average particle size measured using dynamic light scattering is, for example, the average particle size value calculated using a concentrated particle size analyzer FPAR-1000 (manufactured by Otsuka Electronics Co., Ltd.) by cumulant method analysis in scattering intensity distribution.
[0017] The (total) content of these black pigments is preferably 0.5 to 50 mass%, more preferably 2 to 40 mass%, and particularly preferably 5 to 30 mass%, based on the total amount of the aqueous dispersion for the shielding material (hereinafter simply referred to as "total amount of dispersion"). By making the content of this black pigment 0.5% by mass or more, it is possible to realize the formation of a coating film with low gloss and uniformity of unevenness and excellent shielding properties, while by making the content 50% by mass or less, it is preferable because an increase in viscosity is suppressed and the fluidity of the aqueous dispersion for shielding material is improved.
[0018] The neutralized isobutylene-maleic anhydride copolymer used in the present invention is a neutralized copolymer of isobutylene and maleic anhydride, and in the present invention, when used in combination with a water-soluble resin (including a resin emulsion) described later, it serves as a component that exerts the function of providing a coating film containing a black pigment with low gloss and uniform formation of unevenness, as well as good abrasion resistance and water-resistant adhesion. In the neutralized product of isobutylene-maleic anhydride copolymer used, the basic structure of the isobutylene-maleic anhydride copolymer is represented by the following formula (I), and the following formula (II) is an ammonia-neutralized product (modified product) of isobutylene-maleic anhydride copolymer that can be preferably used in the present invention.
[0019] [ka]
[0020] [ka]
[0021] In the present invention, in addition to the ammonia-neutralized product of the above formula (II), sodium hydroxide-neutralized product and amine-neutralized product may be used. The values of n in the above formula (I), l and m in (II), and j and k in the following formula (III) vary depending on the weight-average molecular weight described below, and the preferred ranges are determined. In the present invention, the copolymer may be a neutralized product obtained by imidizing (imide-modifying) an isobutylene-maleic anhydride copolymer represented by the following formula (III) and neutralizing the copolymer with ammonia, sodium hydroxide, an amine, or the like. [ka]
[0022] The weight-average molecular weight of each neutralized product of the isobutylene-maleic anhydride copolymer of the above formulas (II), (III) and the like is preferably 3,000 to 400,000, more preferably 5,000 to 200,000, particularly preferably 30,000 to 100,000, and most preferably 50,000 to 70,000. This weight-average molecular weight is a value calculated in terms of polystyrene by aqueous gel permeation chromatography (GPC) analysis. The above isobutylene-maleic anhydride copolymer and its neutralized product can be a commercially available product, for example, "ISOBAM" manufactured by Kuraray Co., Ltd., and examples thereof include neutralized products of ISOBAM-04, 06, 10, and 18, and ISOBAM-104 and 110, which are commercially available products of ammonia neutralization (modification) of the isobutylene-maleic anhydride copolymer in the above formula (II), and further examples include neutralized products of ISOBAM-304, 306, and 310. When preparing a neutralized product of the isobutylene-maleic anhydride copolymer [from the above formula (I) etc.] to be used, for example, when all the carboxyl groups of the isobutylene-maleic anhydride copolymer are neutralized, the degree of neutralization is set to 1, and each neutralized product can be obtained by calculating and preparing the necessary amounts of ammonia, sodium hydroxide, amine, etc. to be used for neutralization.
[0023] The content of the neutralized product of the isobutylene-maleic anhydride copolymer is preferably 0.01 to 4 mass %, more preferably 0.05 to 3 mass %, and particularly preferably 0.1 to 2 mass %, in terms of solid content, based on the total amount of the dispersion. If the content of the neutralized isobutylene-maleic anhydride copolymer is less than 0.01% by mass, the gloss of the coating film cannot be suppressed sufficiently, resulting in a glossy appearance and making it impossible to obtain a low gloss. On the other hand, if the content exceeds 4% by mass, the viscosity increases, making it difficult to apply evenly, which can have an adverse effect on film formation.
[0024] The water-soluble resin and resin emulsion used in the present invention function as a fixing agent, dispersant, and stabilizer, and are not particularly limited as long as the acid value of the resin is 240 or less. For example, at least one selected from water-soluble resins having a hydrophobic portion in the molecule, such as polyacrylic acid, acrylic resins, water-soluble styrene-acrylic resins, water-soluble styrene-maleic acid resins, polyvinyl alcohol, polyvinylpyrrolidone, water-soluble maleic acid resins, water-soluble styrene resins, water-soluble ester-acrylic resins, ethylene-maleic acid copolymers, polyethylene oxide, and water-soluble urethane resins, and resin emulsions such as acrylic emulsions, vinyl acetate emulsions, urethane emulsions, styrene-butadiene emulsions, styrene-acrylonitrile emulsions, silicone resin emulsions, and silicone acrylic copolymer emulsions, can be mentioned. From the viewpoint of storage stability of the ink, the lower limit of the acid value is desirably 10 or more. By adjusting the acid value of the resin to 240 or less, a coating film having uniform unevenness can be formed.
[0025] The mass average molecular weight of the resin having an acid value of 240 or less is preferably 2,000 or more, more preferably 3,000 to 300,000, and particularly preferably 5,000 to 200,000. By using a resin having a mass average molecular weight of 2,000 or more, it is possible to further improve abrasion resistance and water-resistant adhesion. In the present invention, the "acid value of a resin" refers to the number of milligrams of KOH required to neutralize 1 g of resin, and is a value measured, for example, in accordance with JIS-K3054.
[0026] The water-soluble resins and resin emulsions having an acid value of 240 or less can be commercially available. For example, water-soluble resins such as BASF's PDX6157 (acid value: 205), JDX6500 (acid value: 85), and PDX-6137A (acid value: 240), and Seiko PMC's M-30 (acid value: 155) can be used. Resin emulsions such as BASF's PDX-7741 (acid value: 52), PDX-7787 (acid value: 100), and PDX-7158 (acid value: 54), Taisei Fine Chemical's WBR-016 (acid value: 7), and Mitsui Chemicals MC's Takelac W-5661 (acid value: 48) can be used.
[0027] More preferably, from the viewpoints of dispersibility of coloring materials, viscosity adjustment, and fixing power, the water-soluble resin and resin emulsion used are those having an acid value of 240 or less and a glass transition temperature (Tg) of 140° C. or less, and more preferably, acrylic resins, water-soluble styrene-acrylic resins, styrene maleic acid, water-soluble urethane resins, acrylic resin emulsions, and other resin emulsions having a glass transition temperature (Tg) of 120° C. or less, particularly preferably 100° C. or less. The lower limit of the glass transition temperature (Tg) is preferably −50° C. or more from the viewpoints of line drawing quality such as low gloss and abrasion resistance.
[0028] By setting the acid value of the resin to be a water-soluble resin or resin emulsion of 240 or less and the glass transition temperature (Tg) to 140°C or less, cracking on the coating film surface can be further suppressed and the shielding properties, abrasion resistance, and water-resistant adhesion can be further improved. In the present invention, the "glass transition temperature" is Tg measured in accordance with JIS K7121, and can be measured using, for example, Rigaku thermo plus evo DSC8230 (manufactured by Rigaku Corporation).
[0029] The water-soluble resin and resin emulsion may be commercially available products. For example, water-soluble resins include Joncryl JDX6500 (Tg; 65° C.), JDX6180 (acid value: 230, Tg: 134° C.), 52J (acid value: 238, Tg; 56° C.), 70J (acid value: 240, Tg; 102° C.), and PDX-6137A (acid value: 240, Tg; 102° C.), all of which are manufactured by BASF. ) can be used, and for resin emulsions, BASF's Joncryl PDX352D (acid value: 51, Tg; 52°C), PDX7199 (acid value: 31, Tg; 88°C), and PDX7537 (acid value: 59, Tg; -4°C), or Seiko PMC's KE-1062 (acid value: 149, Tg: 96°C) and PE-1304 (acid value: 142, Tg; 9°C) can be used.
[0030] The content of these water-soluble resins and resin emulsions (total: solid content) is preferably 0.1 to 20 mass % based on the total amount of the dispersion, more preferably 0.5 to 15 mass %, and particularly preferably 1 to 10 mass %. If the content of this water-soluble resin or resin emulsion is less than 0.1% by mass, the abrasion resistance will decrease and the shielding properties will deteriorate. On the other hand, if it exceeds 20% by mass, the viscosity will increase, resulting in deterioration of workability and coatability.
[0031] In the present invention, it is preferred to further contain a polyol having two or more OH groups from the viewpoints of improving the flexibility of the coating film and suppressing unevenness in the appearance of the coating film. Examples of polyols having two or more OH groups include ethylene glycol, diethylene glycol, 1,2-propylene glycol, dipropylene glycol, neopentyl glycol, 2-butyl-2-ethyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,4-cyclohexanediol, 1,6-hexanediol, cyclohexanedimethanol, glycerin, and sugar alcohols. Examples of sugar alcohols include at least one of disaccharide alcohols such as isomaltitol, maltitol, and lactitol; trisaccharide alcohols such as maltotriitol, isomaltotriitol, and panitol; tetrasaccharide or higher sugar alcohols such as oligosaccharide alcohols; reduced starch saccharification products and reduced starch hydrolysates made of disaccharide or higher sugar alcohols.
[0032] The content of these polyols having two or more OH groups is preferably from 0.05 to 40% by mass, more preferably from 0.1 to 30% by mass, and particularly preferably from 0.5 to 20% by mass, based on the total amount of the dispersion. If the content of the polyol having two or more OH groups is less than 0.05% by mass, the further effects of the present invention cannot be achieved. On the other hand, if the content exceeds 40% by mass, the drying properties deteriorate and the solubility and dispersibility of the colorant and resin become unstable.
[0033] The aqueous dispersion for shielding material of the present invention contains at least the above-mentioned black pigment, the neutralized product of isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion having an acid value of 240 or less, and a polyol having two or more OH groups which is preferably contained, as well as water (tap water, purified water, distilled water, ion-exchanged water, pure water, etc.) as a solvent as the remainder, and may also contain, as appropriate, dispersants, lubricants, pH adjusters, rust inhibitors, preservatives or antibacterial agents, thickeners, and the like within ranges that do not impair the effects of the present invention.
[0034] Usable dispersants include nonionic and anionic surfactants and water-soluble resins, and preferably water-soluble polymers. Examples of the lubricant include nonionic lubricants such as fatty acid esters of polyhydric alcohols, higher fatty acid esters of sugars, polyoxyalkylene higher fatty acid esters, and alkyl phosphates, which are also used as surface treatment agents for pigments; anionic lubricants such as alkyl sulfonates and alkyl aryl sulfonates of higher fatty acid amides; derivatives of polyalkylene glycols, fluorine-based surfactants, and polyether-modified silicones.
[0035] Examples of pH adjusters include ammonia, urea, monoethanolamine, diethanolamine, triethanolamine, alkali metal salts of carbonates and phosphoric acids such as sodium tripolyphosphate and sodium carbonate, and hydrates of alkali metals such as sodium hydroxide. Examples of rust inhibitors include benzotriazole, tolyltriazole, dicyclohexylammonium nitrite, and saponins, while examples of preservatives or antibacterial agents include phenol, sodium omadine, sodium benzoate, and benzimidazole-based compounds. Examples of the thickener that can be used include cellulose derivatives, such as hydroxyalkyl cellulose, carboxymethyl cellulose (CMC) or a salt thereof, fermented cellulose, crystalline cellulose, polysaccharides, etc. Examples of polysaccharides that can be used include xanthan gum, guar gum, hydroxypropylated guar gum, casein, gum arabic, gelatin, amylose, agarose, agaropectin, arabinan, curdlan, callose, carboxymethyl starch, chitin, chitosan, quince seed, glucomannan, gellan gum, tamarind seed gum, dextran, nigeran, hyaluronic acid, pustulan, funoran, HM pectin, porphyran, laminaran, lichenan, carrageenan, alginic acid, tragacanth gum, alkaloid gum, succinoglycan, locust bean gum, tara gum, etc. Examples of synthetic polymers include polyacrylic acids, polyvinyl alcohol, polyethylene oxide, polyvinylpyrrolidone, polyvinyl methyl ether, bisacrylamide methyl ether, polyacrylamide, polyethyleneimine, polyethylene glycol, polydioxolane, polystyrene sulfonic acid, and polypropylene oxide. These may be used alone or in combination of two or more. If commercially available products of these are available, they may be used.
[0036] The aqueous dispersion for a shielding material of the present invention is prepared by appropriately combining at least the above-mentioned black pigment, a neutralized product of an isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion having an acid value of 240 or less, water, a polyol preferably having two or more OH groups, and other components depending on the application of the shielding material, stirring and mixing the components with a stirrer such as a homomixer, a homogenizer, or a disper, and further removing coarse particles in the dispersion by filtration or centrifugation, as necessary, to obtain an aqueous dispersion for a shielding material that can form a black, low-gloss light-shielding film, shielding film, etc. Moreover, the pH (25°C) of the aqueous dispersion for a shielding material of the present invention is preferably adjusted to 5 to 10 with a pH adjuster or the like from the viewpoints of usability, safety, and stability of the dispersion itself, and more preferably 6 to 9.5.
[0037] The aqueous dispersion for a shielding material of the present invention thus constituted contains at least the above-mentioned black pigment, a neutralized product of an isobutylene-maleic anhydride copolymer, a water-soluble resin and / or a resin emulsion having an acid value of 240 or less, and water. During the drying process, uniform irregularities are formed on the surface of a coating film containing the black pigment, causing diffuse reflection, thereby obtaining an aqueous dispersion for a shielding material that can form a black, low-gloss light-shielding film, a shielding film, etc. By further adding a polyol having two or more OH groups to the aqueous dispersion for a shielding material having the above composition, it is possible to obtain an aqueous dispersion for a shielding material that can form a shielding material such as a light-shielding film or a shielding film that is black, has low gloss, and has excellent shielding properties.
[0038] Shielding material of the present invention The shielding material of the present invention is composed of the above-mentioned aqueous dispersion for a shielding material of the present invention, and can form a black, low-gloss shielding material such as a light-shielding film or a shielding film by forming uniform irregularities on the surface during the drying process of the coating film and causing diffuse reflection without blending large particles. A shielding material such as a light-shielding film or a shielding film can be applied to a substrate and dried to form a surface anti-reflective coating film. The substrate can be a known one such as glass, a resin plate, a resin film, or a metal. The method for forming the coating film is not particularly limited, and a known coating method can be used. For example, the coating method can be spray, brush, roller, roll coat, applicator, dip coating, or the like. The drying method can be selected according to the application, such as hot air, far infrared rays, or natural drying. The thickness of the coating film is appropriately adjusted according to the application, and is preferably 0.5 μm or more and 3.0 μm or less. The obtained black anti-reflective film can be used to improve visibility, etc., by preventing reflection in the peripheral area and blocking visible light in optical instruments such as cameras and display devices accompanied by light emission such as meters. In addition, the above dispersion can be used to form a coating film on the peripheral area such as the edge, ridge, or edge of an optical element such as a lens or a prism, and can also be used as an internal anti-reflective black coating film for optical elements to absorb stray light that causes flare and ghosts. In addition, it can be used as a black anti-reflective coating film.
[0039] In the present invention, a shielding material such as a shielding film obtained by using the aqueous dispersion for a shielding material having the above-mentioned characteristics preferably has a surface roughness Ra of 0.2 to 2.0 μm, more preferably 0.2 to 1.60 μm, and particularly preferably 0.4 to 0.8 μm. In this case, if the surface roughness Ra of the shielding material exceeds 2.0 μm, the abrasion resistance of the coating film will decrease. In the present invention (including the examples described later), the surface roughness (arithmetic mean roughness Ra) was measured using a laser microscope (VK-8500 manufactured by Keyence Corporation) under smoothing conditions (filter size 3×3, filter type simple average, number of runs 1), lens magnification 10x, color ultra-depth mode, and other settings conforming to standard specifications. Methods for realizing such surface roughness on a coating surface of a cycloolefin polymer (COP) or the like include, for example, gravure printing, flexographic printing, screen printing, inkjet printing, slot die, and / or vapor deposition, in particular physical vapor deposition, chemical vapor deposition, and / or sputtering, spray coating, and the like. EXAMPLES
[0040] Next, the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0041] [Water dispersion for shielding material of the present invention: Examples 1 to 13 and Comparative Examples 1 to 4] Each aqueous dispersion for shielding materials was prepared according to the blending composition shown in the following Table 1. The pH of each aqueous dispersion for shielding materials at room temperature (25°C) was measured with a pH meter (manufactured by HORIBA Corporation) and was within the range of 7.9 to 8.2. Each of the aqueous dispersions for shielding materials obtained above was evaluated for the glossiness and uniformity of the coating film, the scratch resistance, and the water-resistant adhesion by the following evaluation methods. The results are shown in Table 1 below.
[0042] (Method for evaluating the low gloss and uniformity of shielding materials (coatings)) A coating film was formed on a COP film measuring 21 cm x 30 cm using a 9 µm bar coater, and the coating film was subjected to a visual sensory evaluation according to the following criteria. <Evaluation criteria> A: The coating is uniform and has a sufficiently low gloss. B: The coating film has a slightly low gloss. C: For coating
[0043] It has a glossy finish without low gloss. (Method of Evaluating Redispersibility of Dispersion) 10 ml of each of the obtained aqueous dispersions for shielding materials was filled into a 15 ml glass bottle with a lid together with a stirring ball (φ6.4 mm, stainless steel), and the bottle was sealed. After storing the bottle with the cap facing up at 40° C. for one month, each dispersion was shaken. The number of shakes until the stirring ball started to move in the glass bottle with a lid was evaluated according to the following criteria. <Evaluation criteria> A: 1 to 5 times B: 6~15 times C: 16 times or more
[0044] (Method of evaluating the adhesion of shielding materials (coatings)) A coating was formed on a COP film measuring 21 cm x 30 cm using a 9 μm bar coater, and this coating was cut into a grid pattern at 2 mm intervals using a cutter. Cellophane tape was then applied on top of the cutout, and the resulting coating was peeled off and subjected to a visual sensory evaluation according to the following evaluation criteria. <Evaluation criteria> A: The coating has no peeling and has sufficient adhesion. B: The coating film peels off and adhesion is somewhat weak. C: Most of the coating has peeled off and adhesion is insufficient.
[0045] [Table 1]
[0046] As is clear from the results in Table 1 above, it was found that the aqueous dispersions for shielding materials of Examples 1 to 13 according to the present invention have excellent sedimentation resistance, can form uniform coating films with low gloss, and have excellent shielding properties, as compared with the aqueous dispersions for shielding materials of Comparative Examples 1 to 4 which are outside the scope of the present invention. [Industrial Applicability]
[0047] The aqueous dispersion can be suitably used for a shielding material and a shielding material suitable for anti-reflection black coating films on the inner surface of optical elements for preventing reflection in light-emitting display devices such as optical instruments and meters, and for blocking visible light.
Claims
1. An aqueous dispersion for a shielding material, comprising at least a black pigment, a neutralized product of an isobutylene-maleic anhydride copolymer, a water-soluble resin and / or a resin emulsion having an acid value of 240 or less, and water.
2. 2. The aqueous dispersion for a shielding material according to claim 1, wherein the glass transition temperature (Tg) of the water-soluble resin and the resin emulsion is 140° C. or lower.
3. 3. The aqueous dispersion for a shielding material according to claim 1, further comprising a polyol having two or more OH groups.
4. A shielding material, comprising the aqueous dispersion for shielding material according to claim 1 or 2.
5. 5. The shielding material according to claim 4, wherein the surface roughness Ra of the shielding material is 0.2 to 2.0 μm.
Citation Information
Patent Citations
Aqueous solution of hydrophobic coloring agent, its production and water-color ink using the same
JP1997143410A
Ink composition
JP2014105282A
Water-based ink composition for writing instrument, and writing instrument using the same
JP2019119855A
Cited By
Allergen reduction agent and allergen reduction coating
WO2026094983A1