Fiber-reinforced resin and method for producing the same

By optimizing the crystal long period, crystallinity, and annealing conditions of fiber-reinforced resins, the bending properties are enhanced, addressing the limitations of existing resins and expanding their applicability.

JP2024135738AActive Publication Date: 2024-10-04MITSUI CHEMICALS INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023046578
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

Existing fiber-reinforced resins, particularly those described in Patent Document 1, often fail to meet the required bending properties for various applications.

Method used

A fiber-reinforced resin composition with a matrix resin having a crystal long period of 200 Å or more at 23°C, crystallinity of 45% or more, and a melting point of 163°C or less, combined with carbon fibers and specific annealing conditions to enhance lamella thickness and delay crystallization, improving bending properties.

Benefits of technology

The resulting resin exhibits significantly improved bending properties, making it suitable for diverse applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135738000001
    Figure 2024135738000001
  • Figure 2024135738000002
    Figure 2024135738000002
  • Figure 2024135738000003
    Figure 2024135738000003
Patent Text Reader

Abstract

To provide a fiber-reinforced resin that is a UD sheet from which a molding having enhanced flexural property can be obtained or its molding, and a method for producing the same.SOLUTION: A fiber-reinforced resin contains a plurality of reinforcement fibers oriented in one direction, and a matrix resin containing a thermoplastic resin, wherein the matrix resin has a long period of crystal at 23°C determined by an X-ray small angle scattering method of 200 Å or more. The fiber-reinforced resin can be produced by the steps of: preparing a composite material containing a plurality of reinforcement fibers oriented in one direction, and a matrix resin containing a thermoplastic resin; and annealing the fiber-reinforced resin at the following annealing temperature range when a melting point of the matrix resin is represented by Tm. Tm-20°C<annealing temperature<Tm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fiber-reinforced resin and a method for producing the same. [Background technology]

[0002] A thin-film fiber-reinforced resin (hereinafter, simply referred to as "Uni-Direction (UD) sheet") is known, which contains a plurality of reinforcing fibers aligned in one direction and a resin composition (matrix resin) impregnated into the reinforcing fibers. This UD sheet is used as various reinforcing materials due to its high strength.

[0003] Patent Document 1 describes a UD sheet in which polypropylene resin and phenol- and phosphorus-based antioxidants are essential components of the resin part, and the crystallinity of the resin part exceeds 50% by adding a crystal nucleating agent or by heating to a temperature higher than the glass transition temperature of the polypropylene resin and then cooling. Patent Document 1 also describes that the UD sheet had good thermal stability and bending properties in the fused material obtained by laminating, heating, and pressing the sheet. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-43672 A Summary of the Invention [Problem to be solved by the invention]

[0005] As described in Patent Document 1, various methods for improving the bending properties of molded articles of UD sheets have been investigated. However, according to the findings of the present inventors, molded articles obtained from the UD sheet described in Patent Document 1 sometimes do not satisfy the bending properties required for various applications.

[0006] The present invention has been made in consideration of the problems with the conventional technology described above, and has an object to provide a UD sheet that can produce a molded article with improved bending properties, or a fiber-reinforced resin that is that molded article, and a method for producing the same. [Means for solving the problem]

[0007] One embodiment of the present invention for solving the above problems relates to the following fiber reinforced resins [1] to [7]. [1] A composite material comprising a plurality of reinforcing fibers oriented in one direction and a matrix resin containing a thermoplastic resin; The matrix resin has a long crystal period of 200 Å or more at 23° C. as determined by small angle X-ray scattering. Fiber reinforced resin. [2] The matrix resin has a crystallinity of 45% or more at 80°C. [1] The fiber-reinforced resin according to the present invention. [3] The matrix resin comprises polypropylene; The fiber-reinforced resin according to [1] or [2]. [4] The polypropylene has a melting point of 163°C or less. [3] The fiber-reinforced resin according to the present invention. [5] The polypropylene has a melt flow rate (MFR) of 100 mm / 10 min or more, measured at 230°C under a load of 2.16 kg in accordance with ASTM D1238. The fiber-reinforced resin according to [3] or [4]. [6] The reinforcing fibers include carbon fibers. The fiber-reinforced resin according to any one of [1] to [5]. [7] The fiber volume fraction (Vf) is 20% or more and 60% or less; The fiber-reinforced resin according to any one of [1] to [6].

[0008] Another embodiment of the present invention for solving the above problems relates to a method for producing a fiber-reinforced resin as described below in [8]. [8] A step of preparing a composite material including a plurality of reinforcing fibers oriented in one direction and a matrix resin including a thermoplastic resin; annealing the composite at an annealing temperature in the following range, where Tm is the melting point of the matrix resin; Tm-20℃ < Annealing temperature < Tm A method for producing a fiber reinforced resin comprising the steps of: Effect of the Invention

[0009] According to the present invention, there are provided a UD sheet which can give a molded article having improved bending properties, or a fiber reinforced resin which is the molded article thereof, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [Fiber reinforced resin] One embodiment of the present invention relates to a fiber-reinforced resin including a plurality of reinforcing fibers arranged in one direction and a matrix resin including a thermoplastic resin.

[0011] This fiber-reinforced resin may be a single layer UD sheet, a laminate made by laminating and fusing a plurality of UD sheets, or a molded product made by processing the UD sheet or the laminate into a predetermined shape or fusing it to another member.

[0012] This fiber-reinforced resin has a long crystal period of 200 Å or more at 23°C as determined by small-angle X-ray scattering. In other words, the lamellar thickness of the crystals in the matrix resin is thicker than in the past. This allows the crystals in the matrix resin to efficiently improve bending properties.

[0013] When increasing the crystallinity of the matrix resin, the crystallization rate can be delayed to allow each crystal (lamella) to grow sufficiently and to make the lamellar thickness sufficiently thick. For example, when attempting to increase the crystallinity of a thermoplastic resin by annealing (heat treatment), annealing is usually performed at a temperature near the middle between the glass transition temperature (Tg) and the melting point (Tm), at which the crystallization acceleration is the fastest. In contrast, annealing is performed at a temperature closer (higher) than the above-mentioned middle temperature to deliberately delay crystallization, thereby making the lamellar thickness sufficiently thick and improving the bending properties of the fiber-reinforced resin. In addition, by increasing the annealing temperature, the bending properties of the fiber-reinforced resin at high temperatures can also be improved. Alternatively, crystallization may be delayed more than usual by using a crystal nucleating agent with a slow crystallization rate or by not using a crystal nucleating agent.

[0014] From the above viewpoints, the long period of the crystal of the matrix resin at 23° C. is preferably 200 Å to 500 Å, more preferably 200 Å to 450 Å, and even more preferably 250 Å to 400 Å. Furthermore, from the viewpoint of improving the bending properties of the fiber-reinforced resin at high temperatures, the long period of the crystal of the matrix resin at 80° C. is preferably 200 Å to 500 Å, more preferably 200 Å to 450 Å, and even more preferably 250 Å to 400 Å.

[0015] The crystallinity of the matrix resin at 23° C. is preferably 48% or more, more preferably 48% to 70%, and more preferably 50% to 60%. From the viewpoint of improving the bending properties of the fiber reinforced resin at high temperatures, the crystallinity of the matrix resin at 80° C. is preferably 45% or more, more preferably 45% to 70%, and more preferably 48% to 60%.

[0016] The long period of the crystal is the period of the structure of the combined crystalline portion (lamella portion) and amorphous portion in the matrix resin, and the degree of crystallinity is the normal degree of crystallinity of the matrix resin (for example, the ratio of α crystals in the case of polypropylene).

[0017] The long period of the crystal is measured by small angle X-ray scattering (SAXS) using CuKα radiation, and the degree of crystallinity is measured by wide angle X-ray diffraction (WAXD) using CuKα radiation.

[0018] The material of the matrix resin is not particularly limited as long as it is a crystalline thermoplastic resin.

[0019] Examples of the thermoplastic resin include polyolefin resins including polyethylene, polypropylene, polybutene, and poly4-methyl-1-pentene, polyamide resins, polyester resins, polystyrene resins, thermoplastic polyimide resins, polyamideimide resins, polycarbonate resins, polyphenylene ether resins, polyphenylene sulfide resins, polyacetal resins, acrylic resins, polyetherimide resins, polysulfone resins, polyether ketone resins, polyether ether ketone resins, polyarylate resins, polyether nitrile resins, vinyl chloride resins, ABS resins, and fluororesins. The polyolefin may be a copolymer including an ethylene / propylene copolymer, an ethylene / 1-butene copolymer, an ethylene / propylene / diene copolymer, an ethylene / carbon monoxide / diene copolymer, an ethylene / ethyl (meth)acrylate copolymer, an ethylene / glycidyl (meth)acrylate copolymer, and an ethylene / vinyl acetate / glycidyl (meth)acrylate copolymer. These thermoplastic resins may be derived from fossil fuels, may be derived from biomass raw materials, or may be a mixture thereof.

[0020] Of these, polyamide resins and polyolefin resins are preferred from the viewpoint of further improving the moldability of the fiber-reinforced resin, polyolefin resins are more preferred because they can easily increase the lamellar thickness and thus the bending strength of the molded body, and polypropylene is even more preferred because it has good heat resistance, chemical resistance, and water resistance.

[0021] The matrix resin may be a resin composition containing an additive. Examples of the additive include known fillers (inorganic fillers, organic fillers), pigments, dyes, crystal nucleating agents, weathering stabilizers, heat stabilizers, antistatic agents, antislip agents, antioxidants, antifungal agents, antibacterial agents, flame retardants, and softeners. For example, when the UD sheet is fused by laser irradiation in producing a molded product, the matrix resin is preferably a resin composition containing a dye that absorbs the laser of the irradiated wavelength. The dye may be any dye that absorbs light of any wavelength between 300 nm and 3000 nm, and is preferably carbon black.

[0022] The matrix resin may also contain other components, such as resins other than those mentioned above and short fibers having a length shorter than the reinforcing fibers oriented in one direction.

[0023] When the matrix resin is polypropylene, the polypropylene preferably has a melting point of more than 150°C and not more than 165°C. The higher the melting point of polypropylene, the more likely it is that it will form a sufficiently large amount of crystalline components, and thus improve the bending properties of the molded article. The melting point of polypropylene is usually 165°C or less. According to the findings of the present inventors, the use of polypropylene with a melting point lower than 165°C makes it easier to increase the lamellar thickness (increase the long period), and to improve the bending properties of the molded article. From the above viewpoint, the polypropylene preferably has a melting point of 163°C or less, more preferably more than 150°C and not more than 163°C, even more preferably 155°C or more and not more than 163°C, and particularly preferably 160°C or more and not more than 163°C. The melting point of polypropylene is a value measured by the DSC method. When the matrix resin contains a plurality of polypropylene resins, the melting point of the matrix resin is the temperature at which the largest peak of the mixture of these plurality of polypropylenes is indicated.

[0024] The type of polypropylene is not particularly limited, and may be a propylene homopolymer, a propylene copolymer, or a mixture thereof. The stereoregularity of the polypropylene is also not particularly limited, and may be isotactic, syndiotactic, or atactic. The stereoregularity is preferably isotactic or syndiotactic.

[0025] The polypropylene may be unmodified polypropylene (P1), modified polypropylene (P2) containing a carboxylate or the like bonded to the polymer chain, or a mixture of these, but is preferably a mixture of these. In the above mixture, the mass ratio of unmodified polypropylene (P1) to the total mass of unmodified polypropylene (P1) and modified polypropylene (P2) [(P1) / (P1+P2)] is preferably 80% by mass or more and 99% by mass or less, more preferably 85% by mass or more and 98% by mass or less, and even more preferably 90% by mass or more and 97% by mass or less.

[0026] The unmodified polypropylene (P1) preferably has a melt flow rate (MFR) of 50 g / 10 min or more, more preferably 100 g / 10 min or more and 500 g / 10 min or less, and even more preferably 130 g / 10 min or more and 500 g / 10 min or less, measured at 230° C. and under a load of 2.16 kg according to ASTM D1238. When the MFR is within this range, the resin 144 can be easily impregnated into the reinforcing fiber 200 sufficiently.

[0027] The unmodified polypropylene (P1) preferably has a weight average molecular weight (Mw) of 50,000 or more and 300,000 or less, and more preferably 50,000 or more and 200,000 or less.

[0028] The unmodified polypropylene (P1) is a resin component mainly composed of structural units derived from propylene, and the content of structural units derived from propylene is 50 mol % or more. The unmodified polypropylene (P1) may contain structural units derived from α-olefins other than propylene, conjugated or non-conjugated dienes, or polyenes in addition to the structural units derived from propylene.

[0029] When the unmodified polypropylene (P1) is a copolymer, examples of the α-olefin as a copolymerization component include α-olefins (including propylene) having 2 to 20 carbon atoms, including ethylene, 1-butene, 3-methyl-1-butene, 4-methyl-1-pentene, 3-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 1-nonene, 1-octene, 1-heptene, 1-hexene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. Among these, 1-butene, ethylene, 4-methyl-1-pentene, and 1-hexene are preferred, and 1-butene and 4-methyl-1-pentene are more preferred. Examples of the conjugated dienes and non-conjugated dienes as copolymerization components include butadiene, ethylidene norbornene, dicyclopentadiene, and 1,5-hexadiene. These α-olefins, conjugated dienes, and non-conjugated dienes may be used in combination of two or more kinds.

[0030] The modified polypropylene (P2) is a polypropylene containing a carboxylate bonded to a polymer chain. In particular, when the modified polypropylene (P2) contains a carboxylate, the interfacial adhesive strength between the reinforcing fiber 200 and the resin 144 tends to increase.

[0031] The weight average molecular weight (Mw) of the modified polypropylene (P2) is preferably 1,000 or more and 100,000 or less, and more preferably 2,000 or more and 80,000 or less.

[0032] The modified polypropylene (P2) can be synthesized by a known method such as a method of radical graft polymerization of an unmodified propylene-based polymer with a monomer having a carboxylic acid structure.

[0033] The unmodified propylene polymer may be a propylene polymer similar to the unmodified polypropylene (P1) described above, but is preferably a propylene homopolymer or a copolymer of propylene and an α-olefin, such as an ethylene-propylene copolymer, a propylene-1-butene copolymer, or an ethylene-propylene-1-butene copolymer.

[0034] The monomer having a carboxylic acid structure may be a monomer having a carboxylic acid group or a monomer having a carboxylic acid ester. The carboxylic acid group may be neutralized, and the carboxylic acid ester may be saponified. Specific examples of these include ethylenically unsaturated carboxylic acids, their anhydrides, or their esters, and compounds having unsaturated vinyl groups other than olefins.

[0035] Examples of the ethylenically unsaturated carboxylic acids include (meth)acrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, and isocrotonic acid, etc. Examples of the anhydrides include nadic acid (endo-cis-bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic acid), maleic anhydride, and citraconic anhydride, etc.

[0036] Examples of the compound having an unsaturated vinyl group other than the above olefins include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, and the like. (meth)acrylic acids including acrylate, octadecyl (meth)acrylate, stearyl (meth)acrylate, tridecyl (meth)acrylate, lauroyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and diethylaminoethyl (meth)acrylate. esters, hydroxyl group-containing vinyls including hydroxyethyl acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl acrylate, lactone-modified hydroxyethyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl acrylate; epoxy group-containing vinyls including glycidyl (meth)acrylate and methyl glycidyl (meth)acrylate; isocyanate group-containing vinyls including vinyl isocyanate and isopropenyl isocyanate; aromatic vinyls including styrene, α-methylstyrene, vinyl toluene, and t-butylstyrene; amides including acrylamide, methacrylamide, N-methylol methacrylamide, N-methylol acrylamide, diacetone acrylamide, and maleic acid amide; vinyl esters including vinyl acetate and vinyl propionate; N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,These include aminoalkyl (meth)acrylates such as N-dimethylaminopropyl (meth)acrylate, N,N-dipropylaminoethyl (meth)acrylate, N,N-dibutylaminoethyl (meth)acrylate, and N,N-dihydroxyethylaminoethyl (meth)acrylate; unsaturated sulfonic acids such as styrene sulfonic acid, sodium styrene sulfonate, and 2-acrylamido-2-methylpropanesulfonic acid; and unsaturated phosphoric acids such as mono(2-methacryloyloxyethyl) acid phosphate and mono(2-acryloyloxyethyl) acid phosphate. Two or more of these may be used.

[0037] Of these, ethylenically unsaturated carboxylic anhydrides are preferred, with maleic anhydride being more preferred.

[0038] The modified polypropylene (P2) can be synthesized by a known method. For example, the unmodified propylene-based polymer and the monomer having a carboxylic acid structure may be reacted in an organic solvent in the presence of a polymerization initiator, and then the solvent may be removed, or the unmodified propylene-based polymer may be heated and melted to obtain a melt, and the carboxylic acid having an unsaturated vinyl group may be stirred and reacted in the presence of a polymerization initiator, or a mixture of the unmodified propylene-based polymer, the carboxylic acid having an unsaturated vinyl group, and a polymerization initiator may be fed to an extruder, reacted while being heated and kneaded, and then converted into a carboxylate by a method such as neutralization or saponification.

[0039] Examples of the polymerization initiator include various peroxide compounds including benzoyl peroxide, dichlorobenzoyl peroxide, dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(peroxybenzoate)hexyne-3, and 1,4-bis(tert-butylperoxyisopropyl)benzene, as well as azo compounds including azobisisobutyronitrile, etc. Two or more of these polymerization initiators may be used in combination.

[0040] Examples of the organic solvent include aromatic hydrocarbons including xylene, toluene, and ethylbenzene, aliphatic hydrocarbons including hexane, heptane, octane, decane, isooctane, and isodecane, alicyclic hydrocarbons including cyclohexane, cyclohexene, methylcyclohexane, and ethylcyclohexane, ester solvents including ethyl acetate, n-butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and 3-methoxybutyl acetate, and ketone solvents including methyl ethyl ketone and methyl isobutyl ketone. Of these, the organic solvent is preferably an aromatic hydrocarbon, an aliphatic hydrocarbon, or an alicyclic hydrocarbon, and more preferably an aliphatic hydrocarbon or an alicyclic hydrocarbon. Two or more of these organic solvents may be mixed together.

[0041] In this case, from the viewpoint of treating the raw material of the modified polypropylene (P2) in the form of an aqueous dispersion, the monomer having a carboxylic acid structure is preferably neutralized or saponified.

[0042] The neutralization or saponification may be carried out by a known method using a basic substance such as an alkali metal or alkaline earth metal including sodium, potassium, lithium, calcium, magnesium, zinc, and the like, other metals, inorganic amines including hydroxylamine and ammonium hydroxide, and the like, organic amines including ammonia, (tri)methylamine, (tri)ethanolamine, (tri)ethylamine, dimethylethanolamine, morpholine, and the like, oxides, hydroxides, or hydrides of alkali metals or alkaline earth metals such as zinc including sodium oxide and sodium peroxide, oxides, hydroxides, or hydrides of other metals, weak acid salts of alkali metals or alkaline earth metals including sodium carbonate, and weak acid salts of other metals.

[0043] The degree of neutralization or saponification by these neutralizations or saponifications is preferably 50% or more and 100% or less, more preferably 70% or more and 100% or less, and even more preferably 85% or more and 100% or less, from the viewpoint of increasing both the stability of the aqueous dispersion and the adhesion to the reinforcing fiber 200. It is preferable that all of the carboxylic acid groups in the modified polypropylene (P2) are neutralized or saponified, but some of the carboxylic acid groups may remain without being neutralized or saponified.

[0044] The salt components of the carboxylic acid group can be detected and the amount thereof measured by a method of detecting the metal species forming the salt by ICP emission spectrometry, or by a method of identifying the structure of the salt of the acid group by IR, NMR, mass spectrometry or elemental analysis.

[0045] The matrix resin preferably has a melt flow rate (MFR) of 50 g / 10 min or more, more preferably 100 g / 10 min to 500 g / 10 min, and even more preferably 130 g / 10 min to 500 g / 10 min, as measured at 230° C. under a load of 2.16 kg according to ASTM D1238. When the MFR is within this range, it is easy to slow down the cooling rate and retard the crystallization rate, and it is easy to increase the lamellar thickness and increase the crystallization degree.

[0046] The type of reinforcing fiber is not particularly limited, and the reinforcing fiber may be carbon fiber, glass fiber, aramid fiber, alumina fiber, silicon carbide fiber, boron fiber, metal fiber, etc. Among these, carbon fiber and glass fiber are preferred, and carbon fiber is more preferred.

[0047] The carbon fiber has a surface oxygen concentration ratio [O / C], which is the ratio of the number of oxygen (O) and carbon (C) atoms on the surface of the carbon fiber measured by X-ray photoelectron spectroscopy, of preferably 0.05 to 0.5, more preferably 0.08 to 0.4, and even more preferably 0.1 to 0.3. When the surface oxygen concentration ratio is 0.05 or more, a sufficient amount of functional groups can be secured on the carbon fiber surface, and the adhesion to the matrix resin can be further improved. When the surface oxygen concentration ratio is 0.5 or less, the carbon fiber has excellent handleability and productivity. The surface oxygen concentration ratio [O / C] can be measured by the method described in International Publication No. 2017 / 183672. The surface oxygen concentration ratio [O / C] can be controlled by known methods including electrolytic oxidation treatment, chemical oxidation treatment, and gas phase oxidation treatment, but control by electrolytic oxidation treatment is preferred.

[0048] The fiber length (average fiber length) of the reinforcing fibers can be 15 mm or more, preferably 20 mm or more, more preferably 100 mm or more, and even more preferably 500 mm or more. The longer the fiber length of the reinforcing fibers, the higher the bending strength of the fiber reinforced resin. The upper limit of the fiber length of the reinforcing fibers can be appropriately determined depending on the shape and size of the fiber reinforced resin, and can be, for example, 50 m or less.

[0049] The average diameter of the reinforcing fibers is preferably 1 μm or more and 20 μm or less, more preferably 4 μm or more and 10 μm or less. The larger the average diameter of the reinforcing fibers, the higher the bending strength of the fiber-reinforced resin. The smaller the average diameter of the reinforcing fibers, the easier it is to mold the body.

[0050] The reinforcing fibers may be sized with a sizing agent. The sizing agent is not particularly limited, but preferably contains unmodified polyolefin and modified polyolefin, and more preferably contains modified polyolefin containing a metal carboxylate. The modified polyolefin is, for example, a carboxylic acid group, a carboxylic anhydride group, or a carboxylic acid ester group grafted onto the polymer chain of an unmodified polyolefin, and a salt is formed between the functional group and a metal cation.

[0051] The unmodified polyolefin is preferably an ethylene-based polymer having 50 mol% or more of structural units derived from ethylene, or a propylene-based polymer having 50 mol% or more of structural units derived from propylene. Examples of the ethylene-based polymer include ethylene homopolymers and copolymers of ethylene and α-olefins having 3 to 10 carbon atoms. Examples of the propylene-based polymer include propylene homopolymers and copolymers of propylene and ethylene or α-olefins having 4 to 10 carbon atoms. The unmodified polyolefin is preferably homopolypropylene, homopolyethylene, ethylene-propylene copolymer, propylene-1-butene copolymer, or ethylene-propylene-1-butene copolymer. The monomers constituting these unmodified polyolefins and modified polyolefins may be derived from component fossil fuels, may be derived from biomass raw materials, or may be mixtures thereof.

[0052] The content of reinforcing fibers relative to the total volume of the fiber reinforced resin (fiber volume fraction (Vf)) is preferably 10 volume % or more and 70 volume % or less, more preferably 15 volume % or more and 60 volume % or less, and even more preferably 20 volume % or more and 60 volume % or less. The larger the fiber volume fraction (Vf), the higher the bending strength of the fiber reinforced resin can be. The smaller the fiber volume fraction (Vf), the easier it is to mold.

[0053] The fiber reinforced resin may be a single layer UD sheet, or a laminate formed by laminating and fusing a plurality of UD sheets. It may also be a molded product formed by processing the UD sheet or its laminate into a predetermined shape or fusing it to another member. When the fiber reinforced resin is a laminate of a plurality of UD sheets, each layer (each layer derived from the UD sheet) contained in the fiber reinforced resin may be laminated so that the angles at which the reinforcing fibers are oriented are the same, or may be laminated so that the angles at which the reinforcing fibers are oriented are different for each layer. From the viewpoint of increasing the strength against loads applied from a plurality of directions, it is preferable that the fiber reinforced resin has a plurality of layers in which the angles at which the reinforcing fibers are oriented are different for each layer. In this case, the multiple layers may include only one or more layers in which the reinforcing fiber is oriented at a different angle in only one direction (for example, one or more layers in which the orientation angle is 90° relative to the reference layer (0°)), or one or more layers in which the reinforcing fiber is oriented at different angles in different directions (for example, one or more layers in which the orientation angles are 45°, 90°, and 135° relative to the reference layer (0°)). When the fiber-reinforced resin has multiple layers in which the reinforcing fiber is oriented at different angles, it is preferable to set the orientation angle of the reinforcing fiber included in each layer so that the angle of the reinforcing fiber included in the multiple layers is quasi-isotropic (i.e., when the fiber-reinforced resin is viewed as a whole, layers in which the reinforcing fiber is oriented equally in each direction are arranged) (for example, 0° / 90° / 0°, 0° / 45° / 90° / 135° / 135° / 90° / 45° / 0°, etc.).

[0054] When a laminate of multiple UD sheets is used, the number of layers of fiber-reinforced resin is preferably 2 to 24 layers, more preferably 2 to 18 layers. The fewer the number of layers, the higher the formability of the fiber-reinforced resin, making it easier to form molded bodies with more diverse shapes. The more layers there are, the more possible it is to stack the reinforcing fiber layers so as to control the strength in a specific direction.

[0055] When a laminate of multiple UD sheets is used, the thickness of the fiber reinforced resin is preferably 40 μm to 3000 μm, more preferably 100 μm to 2000 μm, even more preferably 300 μm to 1500 μm, and particularly preferably 300 μm to 1200 μm. The thicker the fiber reinforced resin, the higher the bending strength of the fiber reinforced resin. The thinner the fiber reinforced resin, the easier it is to mold.

[0056] The fiber-reinforced resin, which is a single layer UD sheet or a laminate of multiple UD sheets, may be fused or fastened to the surface of another article. Also, the fiber-reinforced resin, which is a laminate of multiple UD sheets, may be a pipe-shaped molded body obtained by sequentially fusing the UD sheets around a mandrel and then pulling out the mandrel. The shape of such a molded body is not particularly limited.

[0057] The fiber reinforced resin may be a random sheet obtained by randomly scattering UD sheets cut into chips in a mold and applying heat and pressure. The random sheet is a molded product having a plurality of blocks including a plurality of reinforcing fibers oriented in one direction and a matrix resin including a thermoplastic resin.

[0058] [Method of manufacturing fiber-reinforced resin] The above-mentioned fiber-reinforced resin can be produced by the steps of preparing a composite material containing a plurality of reinforcing fibers oriented in one direction and a matrix resin containing a thermoplastic resin, and annealing the composite material.

[0059] In the process of preparing the composite material, a single layer UD sheet, its laminate, and its molded body are prepared. These may be produced in this process or may be purchased as already produced materials.

[0060] For example, a composite material that is a single-layer UD sheet can be produced by impregnating reinforcing fibers aligned in one direction with a molten thermoplastic resin composition. The method of impregnation is not particularly limited, and can be a known method such as a roller impregnation method in which the reinforcing fibers are brought into contact (rubbed) with the surface of a rotating roller to which a molten thermoplastic resin composition is attached. The thermoplastic resin composition to be impregnated is a resin composition having the same composition as the matrix resin.

[0061] Moreover, the single-layer UD sheets thus produced can be stacked and heated and pressurized to fuse the matrix resins together to produce a composite material, which is a laminate of multiple UD sheets. At this time, the reinforcing fibers for each layer can be changed as described above.

[0062] Furthermore, the single layer UD sheet or laminated UD sheet thus produced can be processed into a predetermined shape, or even welded or fastened to the surface of another article to produce a composite material, which is a molded body of the UD sheet. The shape of such a molded body is not particularly limited. It is preferable that it does not melt or deform at the heating temperature during annealing. However, this does not apply when the other article is deformed by heating during annealing to be molded into a desired shape at the same time.

[0063] The annealing is performed at an annealing temperature in the following range, where Tm is the melting point of the matrix resin. Tm-20℃ < Annealing temperature < Tm

[0064] As described above, when attempting to increase the crystallization degree of a thermoplastic resin, annealing is usually performed at a temperature near the middle between the glass transition temperature (Tg) and the melting point (Tm) at which the crystallization acceleration is the fastest. In contrast, in this embodiment, annealing is performed at a temperature closer (higher) to Tm than the above-mentioned middle temperature, deliberately delaying crystallization. This makes it possible to sufficiently increase the lamellar thickness (increase the long period) and improve the bending properties of the fiber-reinforced resin. From the viewpoint of sufficiently increasing the lamellar thickness, it is preferable to perform annealing at an annealing temperature in the following range. Tm-15℃ < Annealing temperature < Tm-10℃

[0065] When the matrix resin contains multiple types of resin, the melting point of the matrix resin is the melting point of the mixture of these multiple types of resin. The melting point of the matrix resin can be measured by a differential scanning calorimeter (DSC). When the matrix resin is a mixture of multiple types of resin, the maximum peak measured by the DSC method is the melting point.

[0066] Annealing may be performed on a single layer UD sheet or a laminated UD sheet. The UD sheet with improved bending properties can be used as a reinforcing material by joining it to other articles by fastening, attaching it with an adhesive, or fusing the surface of the UD sheet to other articles. Annealing may also be performed on a molded product obtained by processing the UD sheet or joining it to other articles.

[0067] The manufacturing method of the above-mentioned fiber reinforced resin is not limited to this. For example, when manufacturing a UD sheet, a matrix resin may be formed using a thermoplastic resin composition containing a crystal nucleating agent with a slow crystallization acceleration.

[0068] [Other embodiments] The above-described embodiments are exemplary embodiments of the present invention, and it goes without saying that the present invention may include embodiments other than the above-described embodiments within the scope of its core technical concept.

[0069] For example, the method for producing the above-mentioned molded article is not limited to one including only these steps, and may include other steps as long as the desired molded article is produced.

[0070] [Application] The uses of the fiber-reinforced resin molded article are not limited, and include primary structural materials including main wings, vertical and horizontal stabilizers, secondary structural materials including ailerons, rudders and elevators, interior materials including seats and tables, parts and members of general flying objects such as aircraft and helicopters including power units, hydraulic cylinders, and composite brakes, rocket parts and members including nozzle cones and motor cases, satellite parts and members including antennas, structures, solar panels, battery cases and telescopes, machine parts and members including frames, shafts, rollers, leaf springs, machine tool heads, robot arms, transport hands and synthetic fiber pots, high-speed rotating body parts and members including centrifuge rotors and uranium enrichment cylinders, parabolic antennas, battery parts, radars, audio speaker cones, computer parts, printer parts, electronic and electrical parts and members including personal computer housings and tablet housings, frame parts, semi-structural parts, exterior panel parts, interior and exterior parts, power units, other equipment - hydraulic cylinders, brakes, battery cases, drive shafts, engine parts, spoilers, racing car bodies, crash cones, chairs, tabs, etc. Automobile and motorcycle parts and components including covers, telephone covers, under covers, side covers, transmission covers, battery trays, rear steps, spare tire containers, bus body walls and truck body walls, interior materials, floor panels, ceiling panels, linear motor car bodies, Shinkansen and railway car bodies, vehicle parts and components including window wipers, trolleys and seats, ship hulls including yachts, cruisers and boats, ship parts and components and bodies including masts, rudders, propellers, rigid sails, screws, military ship hulls, submarine hulls and deep sea exploration vessels, actuators, Pressure vessel parts and components including cylinders, cylinders, hydrogen tanks, CNG tanks and oxygen tanks, scientific equipment parts and components including agitator blades, pipes, tanks, pit floors and plant piping, wind power generation parts and components including blades, skins, skeletal structures and de-icing systems, X-ray diagnostic equipment parts, medical and nursing equipment parts and supplies including wheelchairs, artificial bones, artificial legs and arms, crutches, nursing aids and robots (power assist suits), walkers and nursing beds, CF composite cables, concrete reinforcing members, guardrails, bridges, tunnel walls, hoods,It can be used in civil engineering and infrastructure parts and components, including cables, tension rods, strand rods and flexible pipes; offshore oil field mining parts and components, including marine risers, flexible jumpers, flexible risers and drilling risers; sports and leisure products, including fishing rods, reels, golf clubs, tennis rackets, badminton rackets, skis, poles, snowboards, ice hockey sticks, snowmobiles, archery equipment, kendo bamboo swords, baseball bats, swimming diving boards, sports equipment for the disabled and sports helmets; bicycle parts, including frames, disc wheels, rims, handlebars and saddles; daily necessities, including glasses, bags, umbrellas and ballpoint pens; and other industrial parts and components, including plastic pallets, containers, logistics materials, resin molds, furniture, umbrellas, helmets, pipes, scaffolding boards, safety shoes, protectors, fuel cell covers, drone blades, frames, jigs and jig frames. EXAMPLES

[0071] The present invention will be described in detail based on examples, but the present invention is not limited to these examples.

[0072] 1. Preparation of UD sheet 1-1. Preparation of UD sheet 1 (Example 1) 1-1-1. Reinforced fiber A carbon fiber bundle (manufactured by Mitsubishi Rayon Co., Ltd., Pyrofil TR50S12L, filament count 24000, strand strength 5000 MPa, strand modulus 242 GPa) was prepared. This carbon fiber bundle was immersed in acetone and subjected to ultrasonic waves for 10 minutes, and then the carbon fiber bundle was pulled out and washed with acetone three times, and dried at room temperature for 8 hours to remove the adhering sizing agent.

[0073] A mixture obtained by mixing 100 parts by mass of a propylene-based resin (S1), 10 parts by mass of a propylene-based resin (S2), and 3 parts by mass of a surfactant was fed from the hopper of a twin-screw extruder (manufactured by Ikegai Iron Works Co., Ltd., PCM-30, L / D=40) at a rate of 3000 g / hour. Furthermore, a 20% aqueous potassium hydroxide solution was continuously fed from a feed port provided at the vent of the extruder at a rate of 90 g / hour, and the mixture was continuously extruded at a heating temperature of 210°C. The extruded resin mixture was cooled to 110°C with a jacketed static mixer installed at the extrusion port, and further poured into warm water at 80°C to obtain an emulsion with a solid content concentration of 45%.

[0074] The propylene-based resin (S1) is a propylene-butene copolymer. The propylene-based resin (S1) has a Shore D hardness of 52 and a weight average molecular weight of 350,000 as measured by GPC.

[0075] Propylene-based resin (S2) was a modified resin obtained by mixing 96 parts by mass of propylene-butene copolymer, 4 parts by mass of maleic anhydride, and 0.4 parts by mass of a polymerization initiator (Perhexy 25B, manufactured by NOF Corporation) and modifying the mixture at a heating temperature of 160°C for 2 hours. Propylene-based resin (S2) had a weight average molecular weight of 20,000, an acid value of 45 mgKOH / g, a maleic anhydride content of 4% by mass, and a melting point of 140°C, as measured by GPC.

[0076] The surfactant is also potassium oleate.

[0077] The emulsion was applied to the carbon fiber by roller impregnation. After that, the carbon fiber was dried online at 130°C for 2 minutes to remove low boiling point components, and a reinforcing fiber bundle with a sizing agent applied thereto was obtained. The amount of the sizing agent applied to the reinforcing fiber bundle was 0.87% by mass.

[0078] 1-1-2. Matrix resin A matrix resin mixture was obtained by melting and kneading 98 parts by mass of the propylene-based resin (P1) and 2.0 parts by mass of the propylene-based resin (P2) at 180° C. The melting point of this matrix resin mixture was 163° C. as measured by the DSC method, and the MFR measured at 230° C. and a load of 2.16 kg in accordance with ASTM D1238 was 230 g / 10 min.

[0079] The propylene resin (P1) was an unmodified propylene resin (Moplen (registered trademark) HP560W, manufactured by Lyondell Basell, having an MFR of 450 g / 10 min and a flexural modulus of 1600 MPa measured at 230° C. under a load of 2.16 kg in accordance with ASTM D1238).

[0080] The propylene resin (P2) was a modified polypropylene grafted with 0.5% by mass of maleic anhydride (MFR measured at 230°C under a load of 2.16 kg in accordance with ASTM D1238 was 9.1 g / 10 min, and flexural modulus was over 700 MPa).

[0081] The melting point was measured by DSC using a 5 mg sample taken with a Diamond DSC manufactured by PerkinElmer Co., Ltd. and a standard pan manufactured by PerkinElmer Co., Ltd. Specifically, the evaluation was performed under a nitrogen atmosphere with a first heating rate of 10°C / min, a 10 minute hold at 230°C, a 10°C drop rate of 10°C / min, a 1 minute hold at 30°C, and a heating rate of 10°C / min, and the peak at the second heating was taken as the melting point.

[0082] 1-1-3. Creation of UD sheet The spread carbon fiber bundles were aligned and brought into contact with an impregnation roll coated with the molten matrix resin mixture, so that the carbon fiber bundles were impregnated with the matrix resin mixture. The temperature of the molten matrix resin mixture was 260°C, and the temperature of the impregnation roll was also 260°C.

[0083] The sheet-like composite material thus obtained contained 66.6% by mass of carbon fiber and a total of 33.4% by mass of the propylene-based resin (P1) and the propylene-based resin (P2). The volume-based content of the carbon fiber in the sheet-like composite material (fiber volume fraction: Vf) was 50% by volume. The thickness of the sheet-like composite material was 150 μm. The MFR of the matrix resin was 230 g / 10 min (measured at 230° C. and with a load of 2.16 kg in accordance with ASTM D1238).

[0084] The obtained sheet-like composite material was placed in an air oven (WFO-410 manufactured by espec) and annealed at 160°C for 1 hour. It was then stored in a constant temperature room (23°C, 50RH%) for 72 hours to obtain UD sheet 1, which is a fiber-reinforced resin.

[0085] 1-2. Preparation of UD sheet 2 (Example 2) UD sheet 2 was obtained in the same manner as UD sheet 1, except that the annealing was performed at 150° C. for 1 hour.

[0086] 1-3. Preparation of UD sheet 3 (Comparative Example 1) The sheet-like composite material obtained in the production of the UD sheet 1 and before annealing was designated as the UD sheet 3.

[0087] 1-4. Preparation of UD sheet 4 (Comparative Example 2) UD sheet 4 was obtained in the same manner as UD sheet 1, except that the annealing was performed at 140° C. for 1 hour.

[0088] 1-5. Preparation of UD sheet 5 (Comparative Example 3) UD sheet 5 was obtained in the same manner as UD sheet 1, except that the annealing was performed at 140° C. for 2 hours.

[0089] 1-6. Preparation of UD sheet 6 (Example 3) UD sheet 6 was obtained in the same manner as UD sheet 1, except that the amount of matrix resin mixture supplied to the impregnation roll was changed. The volume-based carbon fiber content (fiber volume fraction: Vf) in the sheet-like composite material obtained by impregnation and in UD sheet 6 obtained by subsequent annealing was 38 volume %. The thickness of the sheet-like composite material was 150 μm.

[0090] 1-7. Preparation of UD sheet 7 (Comparative Example 4) The sheet-like composite material obtained in the production of the UD sheet 6 and before annealing was used as the UD sheet 7.

[0091] 2. Evaluation The crystallinity and long period of the lamellae of each UD sheet were measured by the following method.

[0092] (Crystallization degree) To determine the degree of crystallinity, WAXD measurement was carried out by the transmission method using a NANO-Viewer manufactured by Rigaku Corporation. The measurement conditions were as follows: ·Incoming X-ray: CuKα ray Detector: X-ray photon counting two-dimensional detector PILATUS Distance between sample and detector: 70mm (for measurement at 23°C), 100mm (for measurement at 80°C) Sample thickness: 3mm ·Measurement temperature: room temperature, 80℃

[0093] The scattering intensity I obtained by WAXD measurement is plotted against the magnitude q of the scattering vector defined by equation (1) (2θ is the scattering angle, λ is the incident X-ray wavelength), as shown in the scattering intensity curve I(q) (the vertical axis is I(q) and the horizontal axis is q; q is 5 nm -1 From 25 nm -1 The range of the scattering intensity S originating from the crystalline phase is separated using a known analysis program. c and the scattering intensity S due to the amorphous phase a Calculate the crystallinity φ C was calculated using equation (2).

[0094] In this case, the broad peak observed near 2θ:11° was designated as Sa, and the peaks observed near 2θ:9.8°, 11.2°, 11.8°, 12.9°, 14.8°, and 15.3° were designated as Sc.

[0095]

number

[0096] (Long period of lamella) To determine the long period of the lamellae, SAXS measurements were performed using the transmission method with a NANO-Viewer manufactured by Rigaku Corporation. The measurement conditions were as follows: ·Incoming X-ray: CuKα ray Detector: PILATUS X-ray photon counting two-dimensional detector Distance between sample and detector: 1350mm Sample thickness: 3mm ·Measurement temperature: 23℃, 80℃

[0097] The long period L is expressed as q on the scattering intensity curve I(q) (vertical axis is I(q) and horizontal axis is q) obtained by plotting the scattering intensity I obtained by SAXS measurement against the magnitude q of the scattering vector defined by equation (1). 2 The Lorentz correction scattering curve obtained by multiplying 2 × I(q), the horizontal axis is q, and the peak position qm was calculated according to equation (3).

[0098]

number

[0099] 2-2. Bending test For UD Sheets 1 to 7, the flexural modulus and flexural strength were measured in accordance with the method specified in JIS K7171 (2016) at a test speed of 1 mm / min, a support distance of 48 mm, and test temperatures of room temperature (23°C) and 80°C.

[0100] The melting points and MFR of the matrix resins, fiber volume fraction (Vf), annealing temperatures and differences between the melting points of the matrix resins and the annealing temperatures, annealing times, long crystal periods, crystallinity, and bending test results for UD Sheets 1 to 7 are shown in Tables 1 and 2. The bending test results (flexural modulus and bending strength) are also shown as rates of change (rate of increase) based on samples that were not annealed (UD Sheets 3 and 7).

[0101] [Table 1]

[0102] [Table 2]

[0103] As is clear from Tables 1 and 2, fiber-reinforced resins with a crystal long period of 200 Å or more at 23°C, as determined by small-angle X-ray scattering, had significantly improved bending properties compared to fiber-reinforced resins with a long period of less than 200 Å. [Industrial Applicability]

[0104] The fiber reinforced resin according to the present invention has high bending strength. Therefore, the present invention is expected to open up possibilities for using fiber reinforced resins in a wider variety of applications, including as reinforcing materials, and to contribute to the development of various fields related to fiber reinforced resins.

Claims

1. The composite material includes a plurality of reinforcing fibers arranged in one direction and a matrix resin including a thermoplastic resin, The matrix resin has a long crystal period of 200 Å or more at 23° C. as determined by small angle X-ray scattering. Fiber reinforced resin.

2. The matrix resin has a crystallinity of 45% or more at 80°C. The fiber reinforced resin according to claim 1.

3. The matrix resin comprises polypropylene. The fiber reinforced resin according to claim 1.

4. The polypropylene has a melting point of 163° C. or less. The fiber reinforced resin according to claim 3.

5. The polypropylene has a melt flow rate (MFR) of 100 mm / 10 min or more measured at 230° C. under a load of 2.16 kg in accordance with ASTM D1238. The fiber reinforced resin according to claim 3.

6. The reinforcing fibers include carbon fibers. The fiber reinforced resin according to claim 1.

7. The fiber volume fraction (Vf) is 20% or more and 60% or less. The fiber reinforced resin according to claim 1.

8. A step of preparing a composite material including a plurality of reinforcing fibers oriented in one direction and a matrix resin including a thermoplastic resin; annealing the composite at an annealing temperature in the following range, where Tm is the melting point of the matrix resin; Tm-20°C < annealing temperature < Tm A method for producing a fiber reinforced resin comprising the steps of:

Citation Information

Patent Citations

  • Polypropylene composition

    JP1995018151A

  • Long-fiber reinforced polyamide resin molded product

    JP2013253215A

  • Composite material for thermoforming

    JP2017043672A