Method for producing polyolefin block copolymer and polyolefin block copolymer resin composition

A method combining modified polyolefin with nitrile oxide groups and acyclic diene-derived polymers addresses scratch resistance and compatibility issues in polyolefins, resulting in a copolymer with improved mechanical properties and reduced surface bleed.

JP2024135861APending Publication Date: 2024-10-04JAPAN POLYPROPYLENE CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023046749
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Polyolefins suffer from insufficient scratch resistance, surface hardness, and poor adhesion and compatibility with other resins, with existing modification methods leading to issues like molecular weight decrease and odor due to peroxide use, and surface bleed of additives causing stickiness.

Method used

A method involving the reaction of a modified polyolefin with nitrile oxide groups and a polymer derived from an acyclic diene, such as an acrylonitrile-butadiene-styrene copolymer, to form a block copolymer with improved compatibility and scratch resistance, avoiding peroxide-induced molecular chain scission.

Benefits of technology

The method produces a polyolefin block copolymer with enhanced scratch resistance, compatibility, and mechanical properties, maintaining high molecular weight and reducing surface bleed and odor issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135861000017
    Figure 2024135861000017
  • Figure 2024135861000018
    Figure 2024135861000018
  • Figure 2024135861000019
    Figure 2024135861000019
Patent Text Reader

Abstract

To provide a method for producing a block copolymer of polyolefin and a polymer having a non-cyclic diene-derived structural unit, which gives a copolymer excellent in compatibility of a polyolefin part with a polymer part having a non-cyclic diene-derived structural unit and scratch resistance.SOLUTION: A method for producing a polyolefin block copolymer includes a step of mixing a polyolefin modified body (A) having at least one nitrile oxide group, with a polymer (B) having a non-cyclic diene-derived structural unit.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a polyolefin block copolymer and a polyolefin block copolymer resin composition. [Background technology]

[0002] Polyolefins such as polyethylene and polypropylene are excellent in moldability, mechanical properties, transparency, hygiene, etc., and are therefore used in a wide range of fields, such as industrial applications and daily necessities applications, as films, sheets, fibers, nonwoven fabrics, molded products (containers, etc.), modifiers, etc. On the other hand, polyolefins have a lower surface hardness than resins such as polystyrene (PS) and polymethyl methacrylate (PMMA), and therefore may have insufficient scratch resistance. As a method for improving scratch resistance, it is known to add a lubricant, a silicone copolymer, silicone oil, etc. to the polyolefin layer that constitutes the surface to improve the slipperiness of the surface (Patent Documents 1 to 3).

[0003] Polyolefins are known to have poor reactivity and are difficult to modify because they have a saturated hydrocarbon skeleton and are non-polar. They are also known to have poor adhesion and compatibility with other resins. As a method for solving these problems, a method of modifying polyolefins using peroxides and unsaturated dicarboxylic anhydrides such as maleic anhydride is known (Patent Documents 4 and 5).

[0004] Meanwhile, in recent years, attempts have been made to introduce polar functional groups such as nitrile oxide groups into polyolefins having a carbon-carbon double bond at one of the two ends of the main chain (Patent Document 6). Examples 33B and 34B of Patent Document 6 show that a polyolefin modified with a nitrile oxide group was reacted with ethylene-propylene-dicyclopentadiene rubber to produce a block copolymer, and that the tensile modulus, breaking stress, and breaking strain of the block polymer were dramatically improved. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2021-154730 A [Patent Document 2] JP 2017-206587 A [Patent Document 3] JP 2017-125086 A [Patent Document 4] JP 2008-106256 A [Patent Document 5] Japanese Patent Application Publication No. 7-173229 [Patent Document 6] International Publication No. 2019 / 107450 Summary of the Invention [Problem to be solved by the invention]

[0006] The films or molded articles obtained from the resin compositions of Patent Documents 1 to 3 have problems such as stickiness of the surface and odor due to bleeding of the lubricant, silicone-based compound, etc. onto the surface. In the polyolefin modification methods of Patent Documents 4 and 5, the use of peroxides causes side reactions such as molecular chain scission and molecular weight reduction of polyolefin, which in turn causes problems such as deterioration of mechanical properties and odor. The block copolymer obtained in Patent Document 6 shows a certain improvement in mechanical properties such as tensile elongation at break, but does not take into consideration scratch resistance. In addition, it is expected that the surface hardness will decrease, and the scratch resistance is considered to be at an insufficient level.

[0007] An object of the present invention is to provide a method for producing a block copolymer of a polyolefin and a polymer having structural units derived from acyclic dienes, which method gives a copolymer having excellent compatibility and scratch resistance between the polyolefin portion and the polymer portion having structural units derived from acyclic dienes. [Means for solving the problem]

[0008] As a result of intensive research aimed at solving the above problems, the present inventors have found that a polyolefin block copolymer having excellent compatibility and scratch resistance can be obtained by reacting a polyolefin modified product having at least one nitrile oxide group with a polymer having a structural unit derived from a non-cyclic diene, and have thus completed the present invention. The present invention relates to the following [1] to [9].

[0009] [1] A method for producing a polyolefin block copolymer, comprising the step of mixing a polyolefin modified product (A) having at least one nitrile oxide group and a polymer (B) having a structural unit derived from a non-cyclic diene. [2] The method for producing a polyolefin block copolymer according to [1], wherein the polymer (B) is a copolymer further having at least one selected from the group consisting of a structural unit derived from acrylonitrile or a derivative thereof and a structural unit derived from styrene or a derivative thereof. [3] The method for producing a polyolefin block copolymer according to [1] or [2], wherein the polymer (B) is an acrylonitrile-butadiene-styrene copolymer. [4] The method for producing a polyolefin block copolymer according to any one of [1] to [3], wherein the modified product (A) is obtained by addition reaction of a polyolefin (C) having a carbon-carbon double bond at at least one end of a main chain and having a carbon-carbon double bond terminal ratio of 20% or more with a compound (D) represented by the following general formula [I]: [ka] In the general formula [I], s is an integer of 2 to 4; R 1 and R 2 are each independently a hydrocarbon group having 4 to 10 carbon atoms or a halogenated hydrocarbon group having 4 to 10 carbon atoms; X are each independently a divalent hydrocarbon group, -O-, -S- or -N(R 3 )-and;R 3is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms; A is a hydrocarbon group having 1 to 20 carbon atoms which may contain at least one heteroatom having a valence of s. [5] The method for producing the polyolefin block copolymer according to any one of [1] to [4], wherein the modified product (A) is represented by the following general formula [II]: [ka] In the general formula [II], s is an integer of 2 to 4; n is an integer of 1 to 3; s>n; R 1 and R 2 are each independently a hydrocarbon group having 4 to 10 carbon atoms or a halogenated hydrocarbon group having 4 to 10 carbon atoms; X are each independently a divalent hydrocarbon group, -O-, -S- or -N(R 3 )-and;R 3 is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms; A is a hydrocarbon group having 1 to 20 carbon atoms which may contain at least one s-valent heteroatom; R 4 , R 5 and R 6 are each independently a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms; R 7 is a group derived from a polyolefin. [6] The method for producing a polyolefin block copolymer according to any one of [1] to [5], wherein the step of mixing the modified product (A) and the polymer (B) is carried out at 80 to 300°C. [7] The method for producing a polyolefin block copolymer according to any one of [1] to [6], wherein the step of mixing the modified product (A) and the polymer (B) is carried out by melt-kneading. [8] A polyolefin block copolymer resin composition comprising a melt-kneaded product of a polyolefin modified product (A) having at least one nitrile oxide group and an acrylonitrile-butadiene-styrene copolymer. [9] The polyolefin block copolymer resin composition according to [8], comprising a polyolefin block copolymer having a structure derived from an acrylonitrile-butadiene-styrene copolymer and a structure represented by the following general formula [III]: [ka] In the general formula [III], s is an integer of 2 to 4; n is an integer of 1 to 3; s>n; R 1 and R 2 are each independently a hydrocarbon group having 4 to 10 carbon atoms or a halogenated hydrocarbon group having 4 to 10 carbon atoms; X are each independently a divalent hydrocarbon group, -O-, -S- or -N(R 3 )-and;R 3 is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms; A is a hydrocarbon group having 1 to 20 carbon atoms which may contain at least one s-valent heteroatom; R 4 , R 5 and R 6 are each independently a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms; R 7 is a group derived from a polyolefin; * represents a pair of sn pairs, and each pair of * independently represents a reaction site with a double bond derived from butadiene in the structure derived from the acrylonitrile-butadiene-styrene copolymer. Effect of the Invention

[0010] According to the present invention, it is possible to provide a method for producing a polyolefin block copolymer which gives a copolymer having excellent compatibility between a polyolefin portion and a polymer portion having a structural unit derived from a non-cyclic diene and excellent scratch resistance. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a 1H-NMR spectrum of the modified polyolefin (A1) used in the examples. [Diagram 2]FIG. 2 is an SEM photograph of the MD cross section of the polyolefin block copolymer of Example 2, which was prepared using a flat test piece for evaluating physical properties, observed at a magnification of 2000 times. [Diagram 3] FIG. 3 is a SEM photograph of the MD cross section of the mixture of polypropylene and acrylonitrile-butadiene-styrene copolymer of Comparative Example 4, which was prepared using a flat test piece for evaluating physical properties, observed at a magnification of 2000 times. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The following definitions of terms apply throughout the specification and claims. The term "polymer" collectively refers to a homopolymer made of one type of monomer and a copolymer made of multiple types of monomers. When there is no particular need to distinguish between the two, they are collectively referred to simply as "polymer." "Polyethylene" refers to an ethylene homopolymer or an ethylene-(α-olefin having 3 or more carbon atoms) copolymer having a ratio of ethylene units of more than 50 mol %. Polyethylene may have 1 mol % or less of diene compound units. "Polypropylene" refers to a propylene homopolymer or a propylene-(ethylene or an α-olefin having 4 or more carbon atoms) copolymer containing 50 mol % or more of propylene units. Polypropylene may contain 1 mol % or less of diene compound units. The term "1,3-dipole functional group" refers to a functional group capable of undergoing a 1,3-dipole cycloaddition reaction with an unsaturated bond (such as a carbon-carbon double bond, a carbon-carbon triple bond, or a carbon-nitrogen triple bond). "Main chain" refers to a linear molecular chain such that all molecular chains other than the main chain are considered pendant. The phrase "substantially free of solvent" means that no solvent is present other than that which is unavoidably mixed in during production. The symbol "~" indicating a range of numerical values ​​means that the numerical values ​​before and after it are included as the lower limit and upper limit.

[0013] <Method of producing polyolefin block copolymer> The method for producing a polyolefin block copolymer includes a step of mixing a polyolefin modified product (A) having at least one nitrile oxide group and a polymer (B) having a structural unit derived from a non-cyclic diene. The modified product (A) and the polymer (B) are mixed, and the carbon-carbon double bond remaining in the polymer (B) is reacted with the nitrile oxide group of the modified product (A), thereby obtaining a polyolefin block copolymer. In the production method of the present invention, since no peroxide is used, the molecular chain of the modified product (A) is hardly cut, and the modified product (A) and the polymer (B) are bonded by the reaction of the nitrile oxide group with the carbon-carbon double bond, so that the molecular weight of the block copolymer is not easily reduced. In addition, since the polyolefin portion and the polymer portion having a structural unit derived from a non-cyclic diene are reacted in one molecule of the block copolymer, the affinity and compatibility between the polyolefin portion and the polymer portion having a structural unit derived from a non-cyclic diene are improved compared to the case of simply mixing a polyolefin and a polymer having a structural unit derived from a non-cyclic diene. As a result, it becomes possible to finely disperse domains derived from polymers having structural units derived from acyclic dienes in the polyolefin, and to obtain polyolefin block copolymers having excellent mechanical properties such as scratch resistance and tensile elongation at break.

[0014] [Polyolefin modified product (A)] (hereinafter also referred to as "modified product (A)") The polyolefin modified product (A) has at least one nitrile oxide group. The nitrile oxide group of the modified product (A) reacts with the carbon-carbon double bond remaining in the polymer (B) to produce a polyolefin block copolymer. At least one nitrile oxide group is contained in one molecule, and preferably 1 to 3 nitrile oxide groups are contained in one molecule. The nitrile oxide group may be bonded to the end of the modified product (A), or may be bonded in the middle of the molecular chain, or may be bonded to both. The modified product (A) may be used alone or in combination of two or more kinds.

[0015] The polyolefin in the modified polyolefin (A) may be a polymer of an alkene having a carbon number of 2 to 20, such as polyethylene or polypropylene. One type of polyolefin may be used alone, or two or more types may be used in combination. The polyethylene may contain more than 0 mol% and less than 50 mol% of an α-olefin other than ethylene as a comonomer. Also, the polyethylene may contain more than 0 mol% and 1 mol% or less of a diene compound as a comonomer. The content of the diene as a comonomer is preferably 0 mol%. The polypropylene may contain more than 0 mol% and not more than 50 mol% of an α-olefin other than propylene as a comonomer. Also, the polypropylene may contain more than 0 mol% and not more than 1 mol% of a diene compound as a comonomer. The content of the diene as a comonomer is preferably 0 mol%. Examples of the α-olefin include ethylene, propylene, butene, hexene, octene, and 4-methyl-1-pentene. Examples of the diene compound include vinylnorbornene, dicyclopentadiene, ethylidenenorbornene, and 1,4-hexadiene.

[0016] [Polymer (B) having a structural unit derived from acyclic diene] (hereinafter also referred to as "polymer (B)") The polymer (B) has a structural unit derived from a non-cyclic diene. The polymer (B) has at least one carbon-carbon double bond in the molecule. The carbon-carbon double bond may be present at the end of the polymer (B), in the middle of the molecular chain, or in both. The polymer (B) may be used alone or in combination of two or more kinds.

[0017] Examples of the acyclic dienes include linear non-conjugated dienes such as 1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, 5-methyl-1,5-heptadiene, 6-methyl-1,5-heptadiene, 6-methyl-1,7-octadiene, and 7-methyl-1,6-octadiene; linear conjugated dienes such as 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, 1,3-hexadiene, 1,3-heptadiene, and 1,3-octadiene; and compounds in which some of the hydrogen atoms of these non-conjugated dienes or conjugated dienes have been substituted with alkyl groups, halogen atoms, or the like. Among them, from the viewpoint of facilitating the incorporation of at least one carbon-carbon double bond in the polymer (B) and enhancing the reactivity with the modified product (A), the acyclic diene is preferably a chain conjugated diene compound having 4 to 8 carbon atoms, and 1,3-butadiene is particularly preferable. One type of acyclic diene may be used alone, or two or more types may be used in combination.

[0018] The polymer (B) may be a homopolymer containing only structural units derived from acyclic dienes, or a copolymer containing structural units derived from acyclic dienes and other structural units. Compounds forming other structural units include compounds having at least one cyclic or acyclic unsaturated bond, excluding acyclic dienes, and specifically include acyclic monoenes or trienes or higher polyenes such as α-olefins; cyclic monoenes, dienes or trienes or higher polyenes such as styrene; and monomers having functional groups such as acrylonitrile, meth(acrylic) acid, meth(acrylic) acid esters, and meth(acryl)amides. Among them, the polymer (B) is preferably a copolymer further having at least one selected from the group consisting of structural units derived from acrylonitrile or its derivatives from the viewpoint of heat resistance, scratch resistance and oil resistance of the polyolefin block copolymer, and structural units derived from styrene or its derivatives from the viewpoint of moldability and dimensional stability of the polyolefin block copolymer. Examples of the acrylonitrile derivatives include acrylonitrile, methacrylonitrile, and ethacrylonitrile. Examples of the styrene derivatives include styrene, α-methylstyrene, o-, m-, or p-methylstyrene, vinylxylene, pt-butylstyrene, o-ethylstyrene, o-chlorostyrene, and o,p-dichlorostyrene. The other structural units may be used alone or in combination of two or more kinds.

[0019] From the viewpoints of the heat resistance, scratch resistance, oil resistance, moldability and dimensional stability of the polyolefin block copolymer, the polymer (B) is particularly preferably an acrylonitrile-butadiene-styrene copolymer.

[0020] From the viewpoint of availability, the lower limit of the acrylonitrile-derived units in the acrylonitrile-butadiene-styrene copolymer is preferably 2% by mass, more preferably 5% by mass, and even more preferably 10% by mass. The upper limit of the acrylonitrile-derived units is preferably 30% by mass, more preferably 20% by mass, and even more preferably 15% by mass. Similarly, the lower limit of the butadiene-derived units in the acrylonitrile-butadiene-styrene copolymer is preferably 30% by mass, more preferably 40% by mass, and even more preferably 50% by mass.The upper limit of the butadiene-derived units is preferably 90% by mass, more preferably 85% by mass, and even more preferably 80% by mass. Similarly, the lower limit of the styrene-derived units in the acrylonitrile-butadiene-styrene copolymer is preferably 5% by mass, more preferably 8% by mass, and even more preferably 10% by mass, and the upper limit of the styrene-derived units is preferably 50% by mass, more preferably 45% by mass, and even more preferably 40% by mass. The total of the units derived from acrylonitrile, the units derived from butadiene and the units derived from styrene is 100% by mass.

[0021] Acrylonitrile-butadiene-styrene copolymers are commercially available, and examples thereof include UMG ABS (registered trademark) EX18A, EX10U, and TJ3G manufactured by Techno UMG Co., Ltd., and Toyolac (registered trademark) 500 322, 700 314, and 100 322 manufactured by Toray Industries, Inc.

[0022] [Method of producing polyolefin block copolymer] The method for producing a polyolefin block copolymer includes mixing the modified product (A) and the polymer (B). The blending ratio of the modified product (A) to the polymer (B) is preferably 99:1 to 10:90, more preferably 95:5 to 30:70, further preferably 90:10 to 50:50, and particularly preferably 90:10 to 75:25, based on mass.

[0023] The step of mixing the modified body (A) and the polymer (B) is preferably carried out at a temperature of 80 to 300°C, more preferably 150 to 280°C, and further preferably 180 to 220°C.

[0024] From the viewpoint of promoting the reaction between the modified product (A) and the polymer (B), the mixing step is preferably carried out by melt kneading. Examples of the melt kneading method include a method using a known device such as a twin screw extruder or a Banbury mixer. Details of the melt kneading method are described in, for example, "Thermoplastic Elastomers 2nd.ed.", Hanser Gardner Publications, 1996, p.153-190. When melt-kneading is performed, all the components may be melt-kneaded at once, or a portion of the components may be melt-kneaded, and then the remaining components may be added and melt-kneaded. Melt-kneading may be performed two or more times. After melt-kneading, additional heat treatment may be performed.

[0025] <Preferred embodiment of the polyolefin modified material (A)> The modified polyolefin (A) is preferably one obtained by addition reaction of a polyolefin (C) (hereinafter also referred to as "polyolefin (C)") having a carbon-carbon double bond at at least one end of the main chain and a carbon-carbon double bond terminal rate of 20% or more, with a compound (D) represented by the following general formula [I]: [ka] In the general formula [I], s is an integer of 2 to 4; R 1 and R 2 are each independently a hydrocarbon group having 4 to 10 carbon atoms or a halogenated hydrocarbon group having 4 to 10 carbon atoms; X are each independently a divalent hydrocarbon group, -O-, -S- or -N(R 3 )-and;R 3 is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms; A is a hydrocarbon group having 1 to 20 carbon atoms which may contain at least one heteroatom having a valence of s.

[0026] [Polyolefin (C)] The "polyolefin" in the polyolefin (C) includes polyethylene, polypropylene, and the like. The polyolefin (C) may be used alone or in combination of two or more. The definitions of polyethylene and polypropylene are as described above.

[0027] The polyolefin (C) has a carbon-carbon double bond at at least one end of the main chain. From the viewpoint of reactivity, the carbon-carbon double bond terminal ratio in the polyolefin (C) is preferably 20% or more, more preferably 40% or more, and even more preferably 60 to 200%. The polyolefin (C) may have a carbon-carbon double bond in the middle of the main chain, or may have a carbon-carbon double bond at the end or middle of the side chain. Here, the carbon-carbon double bond terminal ratio means the ratio of terminal carbon-carbon double bond groups present per molecular chain of polyolefin (C). When all polyolefin (C) has a carbon-carbon double bond group at only one end, the carbon-carbon double bond terminal ratio is 100%. The carbon-carbon double bond terminal ratio can take a value of 0 to 200%. Note that the calculation of the carbon-carbon double bond terminal ratio in polyolefin (C) does not include carbon-carbon double bonds at the ends of side chains.

[0028] As the carbon-carbon double bond, vinyl group and vinylidene group are preferred. As the carbon-carbon double bond, vinyl group is preferred from the viewpoint of excellent reactivity with nitrile oxide group of the compound represented by general formula [I]. The nitrile oxide group, which is a 1,3-dipole functional group, is more reactive with sterically small olefin bonds than with sterically large olefin bonds.

[0029] When the polyolefin (C) is a polypropylene having a carbon-carbon double bond at at least one end of the main chain (hereinafter referred to as "double bond-containing polypropylene"), the polypropylene generally has the following end groups. Examples of structures having a vinyl group at the end include structural formulas (1-a) and (1-f). Examples of structures having a vinylidene group at the end include structural formula (1-b). [ka]

[0030] Furthermore, when the polyolefin (C) is a double bond-containing polypropylene, in addition to regular monomer units inside the polymer chain, the polypropylene may generate the following internal olefins due to the reaction mechanism, and these may become monomer units constituting the polymer. [ka]

[0031] Polyolefin (C) can generally be produced by coordination polymerization of α-olefins using a transition metal catalyst without using a chain transfer agent. Usually, when producing polyolefins, the molecular weight is adjusted by a chain transfer agent, so the terminal structure of the polyolefin is a saturated terminal. On the other hand, in coordination polymerization using a transition metal catalyst, if a chain transfer agent such as hydrogen or organoaluminum is not used, the terminal end of the polyolefin becomes a carbon-carbon double bond. In particular, terminal double bonds are likely to be produced in a polymerization system in which the molecular weight is adjusted by the polymerization temperature. In addition, hydrogen generation is accompanied by carbon-carbon double bonds that may be produced in the middle of the main chain and in the side chain. These are described in Macromolecules, Vol. 38, 2005, pp. 6988-6996 and Topics in Catalysis, Vol. 7, 1999, pp. 145-163, etc.

[0032] Examples of transition metal catalysts include complex catalysts (Phillips catalysts, metallocene catalysts, post-metallocene catalysts, etc.) and Ziegler-Natta catalysts, among which Phillips catalysts, metallocene catalysts, and post-metallocene catalysts are preferred, and metallocene catalysts and post-metallocene catalysts are particularly preferred in terms of the wide range of production possibilities. In addition, if the carbon-carbon double bond terminal ratio satisfies the above range, a chain transfer agent may be used as necessary.

[0033] (Calculation method for carbon-carbon double bond terminal ratio) The carbon-carbon double bond terminal ratio means the ratio of molecular chains having a carbon-carbon double bond group at the end to the total polymer chains of the polyolefin (C). The carbon-carbon double bond terminal ratio can be calculated according to the method described in JP 2021-4376 A.

[0034] Specifically, the carbon-carbon double bond terminal ratio is calculated by the following formula. (Carbon-carbon double bond terminal rate) = (total number of carbon-carbon double bond terminals) / {((total number of terminals) - (number of LCBs)) ÷ 2} × 100 Here, the total number of carbon-carbon double bond terminals is 1 The total number of carbon-carbon double bond ends per 1,000 monomer units calculated by H-NMR. 1 H-NMR and 13 The LCB number is the total number of terminals per 1000 monomer units calculated by C-NMR. 13 This is the number of methine carbons in the main chain to which branched chains having 7 or more carbon atoms per 1,000 monomer units are bonded, as calculated by C-NMR.

[0035] The following is a description of polypropylene containing double bonds: 1 H-NMR and 13 A method for identifying the percentage of carbon-carbon double bond terminals using C-NMR is described below.

[0036] 1. Sample preparation and measurement conditions 200 mg of sample was placed in an NMR sample tube with an inner diameter of 10 mm together with 2.4 ml of a mixed solution of o-dichlorobenzene / deuterated bromide benzene (C6D5Br) and hexamethyldisiloxane, a chemical shift standard substance, and dissolved uniformly in a block heater at 150°C. NMR measurements are performed at 120°C using a Bruker Biospin AV400 NMR apparatus equipped with a 10 mmφ cryoprobe. To quantify the number of carbon-carbon double bond ends, 1 H-NMR is used. 1 The H-NMR measurement conditions are a sample temperature of 120°C, a pulse angle of 4.5°, a pulse interval of 2 seconds, and an accumulation count of 512. The chemical shift is set to 0.09 ppm for the proton signal of hexamethyldisiloxane, and the chemical shifts of the signals due to other protons are based on this. To quantify the saturated ends, 13Using C-NMR. 13 The C-NMR measurement conditions are a sample temperature of 120°C, a pulse angle of 45°, a pulse interval of 18 seconds, and an accumulation of 3072 times, and the measurement is performed using the broadband decoupling method. 13 The C signal was set to 1.98 ppm, and the other 13 The chemical shifts of the C signals are based on this.

[0037] 2. Calculation method for the number of carbon-carbon double bond ends Examples of the structure having a vinyl group at the end include the structural formulae (1-a) and (1-f). 1 In H-NMR, the proton signals of the unsaturated bonds of the structural formula (1-a) 1-propenyl and the structural formula (1-f) 1-butenyl are as follows: 1 It is detected overlapping with the signals at 5.08-4.85 ppm and 5.86-5.69 ppm in the H-NMR spectrum. i ] is the total number of 1-propenyl and 1-butenyl units, and the amount of unsaturated bonds per 1,000 monomer units is 1 It is calculated from the signal intensity of the H-NMR spectrum according to the following formula. Structural formula (1-a) + Structural formula (1-f): [V i ]=I vi ×1000 / I total

[0038] The structure having a vinylidene group at the end is represented by the structural formula (1-b). d ] is the number of propyl-vinylidene units, the amount of unsaturated bonds per 1000 monomer units, 1 It is calculated from the signal intensity of the H-NMR spectrum according to the following formula. Structural formula (1-b):[V d ]=I vd ×1000 / I total Similarly, the number of i-butenyl groups [i-butenyl], the number of vinylene terminals [terminal vinylene], and the number of internal vinylidenes [internal vinylidene] can be calculated from the following formula. Structural formula (1-d): [i-butenyl] = I ibu ×1000 / I total Structural formula (1-g): [Terminal vinylene] = I vnl ×1000 / I total Structural formula (1-m): [internal vinylidene] = I ivd ×1000 / I total

[0039] Here, I vi , I vd , I ibu , I vnl and I ivd represent characteristic values ​​of signals based on structural formula (1-a)+structural formula (1-f), structural formula (1-b), structural formula (1-d), structural formula (1-g) and structural formula (1-m), respectively, and are quantities represented by the following formulas. I vi =(I 5.08~4.85 +I 5.86~5.69 ) / 3, I vd =(I 4.79~4.65 ) / 2, I ibu =I 5.30~5.08 , I vnl =(I 5.58~5.30 ) / 2, I ivd =(I 4.85~4.79 ) / 2

[0040] I is the integrated intensity, and the subscripts of I indicate the range of chemical shifts. For example, I 5.08~4.85 indicates the integrated intensity of the signal detected between 5.08 ppm and 4.85 ppm. Also, I total is the quantity shown in the following formula: I total =I C3 +I vi +I vd +I ibu +I vnl +I ivd I C3 represents a characteristic value of a signal based on propylene, and is a quantity represented by the following formula: I C3 = 1 / 6 × I main I main What is 1 It is the sum of the proton signals of the polymer main chain and saturated terminals detected in the H-NMR spectrum from 4.00 to 0.00 pm.

[0041] 3. Calculation method for the number of saturated ends The number of saturated ends is given below per 1000 monomer units: 13 It is calculated from the signal intensity of the C-NMR spectrum using the following formula. Structural formula (1-c): [i-butyl] = I i-butyl ×1000 / I total-C Structural formula (1-e): [n-butyl] = I nbu ×1000 / I total-C Structural formula (1-h): [n-propyl] = I npr ×1000 / I total-C Structural formula (1-i): [2,3-dimethylbutyl] = I 2,3-dime ×1000 / I total-C Structural formula (1-j): [3,4-dimethylpentyl] = I 3,4-dime ×1000 / I total-C

[0042] Furthermore, double bond-containing polypropylene may have the following 2,1 bond and 1,3 bond based on irregular insertion of propylene in addition to the structure based on regular 1,2 insertion of propylene inside the polymer. [ka]

[0043] Here, I i-butyl , I nbu , I npr , I 2,3-dime , I 3,4-dime represent characteristic values ​​of signals based on structural formula (1-c), structural formula (1-e), structural formula (1-h), structural formula (1-i) and structural formula (1-j), respectively, and are quantities represented by the following formulas. I i-butyl =(I 23.80~23.70 +I 25.80~25.70 ) / 2 I nbu =I 14.06~14.02 I npr =(I 14.44~14.42 +I 30.46~30.45 ) / 2 I 2,3-dime =(I 16.21~16.17 +I 31.86~31.81 ) / 2 I 3,4-dime =I 12.0~11.60

[0044] Also, I total-C is the quantity shown in the following formula: I total-C =I i-butyl +I nbu +I npr +I 2,3-dime +I 3,4-dime +I 1,2-P +I 2,1-P +I 1,3-P I 1,2-P is the characteristic value of the signal based on the 1,2-inserted propylene bond, I 2,1-P is the characteristic value of the signal based on the 2,1 inserted propylene bond, I 1,3-P represents a characteristic value of a signal based on 1,3-inserted propylene bond, and is the quantity shown by the following formula: I 1,2-P =I 48.80~44.50 I 2,1-P =(I 35.72~35.63 +I 35.83~35.77 ) / 2 I 1,3-P =I 37.41-37.21 / 2

[0045] 4. Calculation method for total number of ends The total number of ends is 13 C-NMR and 1 It is the total number of terminals per 1000 monomer units calculated by each H-NMR, specifically, the sum of the numbers of terminals of the structural formulas (1-a) to (1-j) per 1000 monomer units.

[0046] 5.How to calculate the number of LCBs The double bond-containing polypropylene may have a long chain branched (LCB) structure. The number of long chain branches (LCB number) is 13 The number per 1000 propylene monomer units is calculated using the following formula using the integrated signal intensities of the branch point carbons (methine carbons) at 31.72 to 31.66 ppm and three methylene carbons bonded to the branch point carbons (methine carbons) at 44.09 to 44.03 ppm, 44.78 to 44.72 ppm, and 44.90 to 44.84 ppm when the intensity of the methylene carbons in the propylene main chain at 49.00 to 44.33 ppm is normalized to 1000 by C-NMR. Number of LCBs = [(I 44.09~44.03 +I 44.78~44.72 +I 44.90~44.84 +I 31.72~31.66 ) / 4] / I 49.00~44.33

[0047] [Compound (D) represented by general formula [I]] The compound (D) represented by the general formula [I] has a nitrile oxide group, which is a 1,3-dipole functional group. The nitrile oxide group can undergo a 1,3-dipole cycloaddition reaction with the unsaturated bond of the polyolefin (C) in the absence of a catalyst, forming an isoxazoline skeleton. In addition, the compound (D) represented by the general formula [I] is advantageous in that the nitrile oxide group is unlikely to dimerize, and therefore the 1,3-dipole cycloaddition reaction can proceed. The compound (D) represented by the general formula [I] may be used alone or in combination of two or more kinds. [ka]

[0048] In the general formula [I], s is an integer of 2 to 4. From the viewpoint of suppressing reactions between polymers, s is preferably an integer of 2 to 3, and more preferably 2.

[0049] R 1 and R 2are each independently a hydrocarbon group having 4 to 10 carbon atoms or a halogenated hydrocarbon group having 4 to 10 carbon atoms. Examples of the hydrocarbon group having 4 to 10 carbon atoms or the halogenated hydrocarbon group having 4 to 10 carbon atoms include a tert-butyl group, an isobutyl group, a phenyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 4-chlorophenyl group, a 2,4-dimethylphenyl group, and a 3,4-dimethylphenyl group. R 1 and R 2 As the aryl group, an aryl group having 6 to 8 carbon atoms is preferable because the nitrile oxide group is unlikely to dimerize. Examples of the aryl group having 6 to 8 carbon atoms include a phenyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 2,4-dimethylphenyl group, and a 4-chlorophenyl group, among which a phenyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, and a 2,4-dimethylphenyl group are preferable, and a phenyl group is more preferable. R 1 and R 2 may be the same or different. 1 and R 2 are preferably the same, since this increases the molecular symmetry, makes the compound more likely to be solidified, and provides excellent storage stability at room temperature.

[0050] X is independently a divalent hydrocarbon group, -O-, -S- or -N(R 3 )-. X is -O-, -S- or -N(R 3 )- is preferred, -O- or -S- is preferred, and -O- is more preferred. R 3 R is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. Examples of the hydrocarbon group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, and a hexyl group. 3 As the substituent, a hydrogen atom or a methyl group is preferable because the compound can be easily synthesized. The divalent hydrocarbon group for X includes an alkylene group having 1 to 3 carbon atoms, an arylene group having 6 to 8 carbon atoms, and a combination thereof.

[0051] A is a hydrocarbon group having 1 to 20 carbon atoms which may contain at least one heteroatom having a valence of s. A carbon atom in the hydrocarbon group may be replaced with a heteroatom or a group containing a heteroatom. Examples of the heteroatom include an oxygen atom, a nitrogen atom, and a sulfur atom. Examples of the hydrocarbon group include hydrocarbon groups such as an alkylene group, a cycloalkylene group, and an arylene group; combinations of a hydrocarbon group and various bonds (-O-, -C(=O)-, -NH-, -S-, -S(=O)2-, etc.); combinations of a hydrocarbon group and a polar functional group (a hydroxy group, a mercapto group, a carboxy group, an amino group, an amide group, an alkoxy group, etc.); combinations of a hydrocarbon group, various bonds, and a polar functional group, etc. The hydrocarbon group may have a substituent. Examples of the substituent include an alkyl group, a cycloalkyl group, a silyl group, an aryl group, a heterocyclyl group, a heteroaryl group, and an acyl group; halogen atoms such as fluorine, chlorine, bromine, and iodine; and alkyl groups and aryl groups which partially contain the halogen atoms.

[0052] The compound (D) represented by the general formula [I] may be the following nitrile oxide compounds (i) to (ii) because they tend to have a high melting point and are excellent in storage stability at room temperature. (i) A nitrile oxide compound, in which, in the general formula [I], s is 2 and A is an alkylene group having 2 to 10 carbon atoms. (ii) A nitrile oxide compound in which, in the general formula [I], s is 2 and A is a group represented by the general formula [IV] described below.

[0053] It is believed that the melting point of the nitrile oxide compound can be increased by introducing an alkylene group having a high symmetry and a short carbon chain, as in (i). It is believed that the melting point of the nitrile oxide compound can be increased by introducing a group represented by the general formula [IV] having a highly symmetrical and rigid arylene group as in (ii).

[0054] A in (i) is an alkylene group having 2 to 10 carbon atoms. In order to solidify the nitrile oxide compound and to develop a melting point close to that of polyolefin, A in (i) is preferably an alkylene group having 3 to 8 carbon atoms, and more preferably an alkylene group having 4 to 6 carbon atoms. Examples of A in (i) include a 1,2-ethylene group, a 1,3-propylene group, a 2-methyl-1,3-propylene group, a 2,2-dimethyl-1,3-propylene group, a 1,4-butylene group, a 1,5-pentylene group, a 1,6-hexylene group, a 1,7-heptylene group, a 1,8-octylene group, a 3-methyl-1,5-pentylene group, a 1,4-cyclohexylene group, a 1,4-cyclohexadimethylene group, a 1-methyl-1,2-ethylene group, and a 1-methyl-1,3-propylene group. In (i), A is preferably a 1,3-propylene group, a 1,4-butylene group, a 1,6-hexylene group, a 1,4-cyclohexadimethylene group, a 1,4-cyclohexylene group, or a 3-methyl-1,5-pentylene group, and more preferably a 1,4-butylene group, a 1,6-hexylene group, or a 3-methyl-1,5-pentylene group.

[0055] In (ii), A is a group represented by the general formula [IV]. -(R 4 ′-O) t -R 5 ′-(OR 4 ') t - [IV]

[0056] t is 0 or 1. In terms of ease of production of the nitrile oxide compound, t is preferably 1, and in terms of the melting point of the nitrile oxide compound, t is preferably 0. R 4′ is an alkylene group having 2 to 4 carbon atoms. 4′ Examples of R include a 1,2-ethylene group and a 1,3-propylene group. 4′ As the alkyl group, a 1,2-ethylene group is preferable since the melting point of the nitrile oxide compound can be increased as the number of carbon atoms decreases.

[0057] R 5′R is a group represented by general formula [V] or a group represented by general formula [VI]. 5′ As the functional group, a group represented by the general formula [VI] is preferred from the viewpoint of increasing the distance between the polyolefin terminal and the introduced functional group after modification of the polyolefin (C) and increasing the reactivity of the modified polyolefin (A).

[0058] [ka]

[0059] R 6′ ~R 9′ are each independently a hydrogen atom, a hydrocarbon group having 1 to 6 carbon atoms, or a halogen atom; R 6′ and R 7′ may be linked to form an aromatic ring or an aliphatic ring, R 8′ and R 9′ may be linked to form an aromatic ring or an aliphatic ring. Examples of the hydrocarbon group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a hexyl group, a cyclohexyl group, and a phenyl group. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. R 6′ ~R 9′ As the alkyl group, a hydrogen atom, a methyl group, an ethyl group, an isopropyl group, a tert-butyl group, a phenyl group, and a chlorine atom are preferable, a hydrogen atom, a methyl group, an isopropyl group, and a tert-butyl group are more preferable, and a hydrogen atom and a methyl group are even more preferable.

[0060] R 10′ ~R 17′ are each independently a hydrogen atom, a hydrocarbon group having 1 to 6 carbon atoms, or a halogen atom; R 10′ and R 11′ may be linked to form an aromatic ring or an aliphatic ring, R 12′ and R 13′ may be linked to form an aromatic ring or an aliphatic ring, R 14′ and R 15′ may be linked to form an aromatic ring or an aliphatic ring, R 16′ and R 17′may be linked to form an aromatic ring or an aliphatic ring. Examples of the hydrocarbon group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a hexyl group, a cyclohexyl group, and a phenyl group. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. R 10′ ~R 17′ As the alkyl group, a hydrogen atom, a methyl group, an ethyl group, an isopropyl group, a tert-butyl group, a phenyl group, and a chlorine atom are preferable, a hydrogen atom, a methyl group, an isopropyl group, and a tert-butyl group are more preferable, and a hydrogen atom and a methyl group are even more preferable.

[0061] u is 0 or 1. u is preferably 1 from the viewpoints of increasing the distance between the terminal end of the polyolefin and the introduced functional group after modification of the polyolefin (C) and increasing the reactivity of the modified polyolefin (A). Q is -C(R 18′ )(R 19′ Q is -C(R )-, -C(=O)-, -S- or -S(=O)2-, because it has high solubility in polyolefins during melt blending. 18′ )(R 19′ )- is more preferred. R 18′ and R 19′ are each independently a hydrogen atom, a hydrocarbon group having 1 to 6 carbon atoms, or a halogen atom; R 18′ and R 19′ may be linked to form an aromatic ring or an aliphatic ring. Examples of the hydrocarbon group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a hexyl group, a cyclohexyl group, and a phenyl group. R 18′ and R 19′ An example of a bonded group of R is a 1,1-cyclohexylene group. Examples of halogen atoms include fluorine, chlorine, bromine and iodine atoms. 18′ and R 19′ As the alkyl group, a hydrogen atom, a methyl group, an ethyl group and a phenyl group are preferable.

[0062] The melting point of the compound (D) represented by the general formula [I] is preferably 25 to 300°C, more preferably 40 to 280°C, further preferably 60 to 260°C, and particularly preferably 80 to 240°C. If the melting point of the compound is equal to or higher than the lower limit of the range, the mobility at room temperature is decreased, and therefore the storage stability at room temperature is improved. If the melting point of the compound is equal to or lower than the upper limit of the range, the compound is easily melted during the melting reaction, and the reactivity is increased. In order to increase the melting point of the compound represented by general formula [I] to 25° C. or higher, for example, a highly symmetric structure may be added to A to increase the symmetry of the molecular structure, or a highly rigid group or a short-chain group may be introduced into A.

[0063] [Method for producing modified polyolefin (A)] The method for producing the polyolefin modified product (A) is not particularly limited, but a method including an addition reaction between a double bond of the polyolefin (C) and at least one of the nitrile oxide groups of the compound (D) represented by the general formula [I] is preferred.

[0064] The amount of the compound (D) represented by the general formula [I] is preferably 0.001 to 10 parts by mass, more preferably 0.01 to 8 parts by mass, and even more preferably 0.05 to 6 parts by mass, relative to 100 parts by mass of the polyolefin (C). The amount of the compound (D) represented by the general formula [I] is preferably 0.1 to 8.0 equivalents, more preferably 0.5 to 5.0 equivalents, and even more preferably 1.0 to 3.0 equivalents, relative to 1 equivalent of the carbon-carbon double bond of the polyolefin (C).

[0065] The nitrile oxide group in the compound (D) represented by the general formula [I] is easily irreversibly isomerized to an isocyanate group by heating in the presence of an isomerization accelerator. For this reason, it is preferable not to add an isomerization accelerator for isocyanate groups when producing the polyolefin modified product (A). Examples of the isomerization accelerator include fatty acid compounds such as stearic acid and lauric acid, fatty acid amide compounds such as stearic acid amide and oleic acid amide, and fatty acid metal salt compounds such as calcium stearate, calcium laurate, and zinc octylate.

[0066] The modified polyolefin (A) can be obtained, for example, by mixing the polyolefin (C) with the compound (D) represented by the general formula [I] and subjecting the mixture to a heat treatment. The heat treatment may be carried out in a solvent or in the absence of a solvent while melt-kneading the mixture.

[0067] The solvent may be a hydrocarbon solvent, and examples thereof include toluene, xylene, hexane, cyclohexane, benzene, etc. When a solvent is used, the mixing temperature is preferably 50 to 200° C., more preferably 60 to 180° C., and even more preferably 80 to 150° C. When a solvent is used, the mixing time is preferably 30 minutes to 24 hours, more preferably 1 hour to 15 hours, and even more preferably 2 hours to 10 hours.

[0068] From the viewpoint of productivity, the heat treatment is preferably carried out by melt kneading in the substantial absence of a solvent to add-react the polyolefin (C) with the compound (D) represented by the general formula [I].

[0069] Examples of the melt-kneading method include a method using a known device such as a twin-screw extruder, a Banbury mixer, etc. Details of the melt-kneading method are described in, for example, "Thermoplastic Elastomers 2nd.ed.", Hanser Gardner Publications, 1996, pp. 153-190. When melt-kneading is performed, all the components may be melt-kneaded at once, or a portion of the components may be melt-kneaded, and then the remaining components may be added and melt-kneaded. Melt-kneading may be performed two or more times. After melt-kneading, additional heat treatment may be performed.

[0070] In the case where there is substantially no solvent, that is, when melt-kneading is performed, the melt-kneading temperature is preferably 80 to 300°C. By melt-kneading a mixture of polyolefin (C) and compound (D) represented by general formula [I] at 80 to 300°C, the double bond of the polyolefin (C) and at least one of the nitrile oxide groups of the compound (D) are subjected to an addition reaction, and the remaining nitrile oxide groups of the compound (D) can be left unreacted. The melt-kneading temperature is more preferably 100 to 280°C, and further preferably 120 to 260°C. The kneading time means the residence time in melt-kneading by an extruder. The melt-kneading time is preferably 1 second to 30 minutes, and more preferably 10 seconds to 5 minutes.

[0071] In the method for producing the polyolefin modified product (A) described above, a polyolefin having a carbon-carbon double bond is used, and therefore the polyolefin can be modified with the compound represented by general formula [I] under industrially advantageous high-temperature conditions.

[0072] <Structure of modified polyolefin (A)> The modified polyolefin (A) is preferably one obtained by the above-mentioned method for producing the modified polyolefin (A). In this case, the modified polyolefin (A) has at least one isoxazoline skeleton and at least one nitrile oxide group.

[0073] In another embodiment of the present invention, the polyolefin modified product (A) is represented by the following general formula [II]. [ka] In the general formula [II], s is an integer of 2 to 4; n is an integer of 1 to 3; s>n; R 1 and R 2 are each independently a hydrocarbon group having 4 to 10 carbon atoms or a halogenated hydrocarbon group having 4 to 10 carbon atoms; X are each independently a divalent hydrocarbon group, -O-, -S- or -N(R 3 )-and;R 3is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms; A is a hydrocarbon group having 1 to 20 carbon atoms which may contain at least one s-valent heteroatom; R 4 , R 5 and R 6 are each independently a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms; R 7 is a group derived from a polyolefin.

[0074] In the general formula [II], s is an integer of 2 to 4. From the viewpoint of suppressing an increase in viscosity of the polyolefin modified product (A), s is preferably an integer of 2 to 3, and more preferably 2.

[0075] n is an integer of 1 to 3. From the viewpoints of use of the polyolefin modified product (A) as a filler dispersant and of producing a block copolymer by reaction with other resins, n is preferably an integer of 1 to 2, and particularly preferably 1, with the proviso that s>n.

[0076] R 1 and R 2 R are each independently a hydrocarbon group having 4 to 10 carbon atoms or a halogenated hydrocarbon group having 4 to 10 carbon atoms. 1 and R 2 Examples of the formula include R 1 and R 2 The same can be mentioned, and preferred embodiments are also the same.

[0077] X is independently a divalent hydrocarbon group, -O-, -S- or -N(R 3 )- and R 3 X and R are each a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. A is a hydrocarbon group having 1 to 20 carbon atoms which may contain at least one heteroatom having a valence of s. 3 Examples of A include X and R in the general formula [I]. 3 and A are the same as those in A, and preferred embodiments are also the same.

[0078] R 4 , R5 and R 6 are each independently a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms. Examples of the hydrocarbon group having 1 to 8 carbon atoms include a methyl group, an ethyl group, an isopropyl group, a n-propyl group, a n-butyl group, a tert-butyl group, an isobutyl group, a n-hexyl group, a cyclohexyl group, a phenyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 2,4-dimethylphenyl group, and a 3,4-dimethylphenyl group. Among these, an alkyl group having 1 to 8 carbon atoms is preferred. Examples of the alkyl group having 1 to 8 carbon atoms include a methyl group, an ethyl group, an isopropyl group, a n-propyl group, a n-butyl group, and a n-hexyl group. R 4 R is preferably a hydrogen atom, a methyl group, an ethyl group, an n-butyl group, or an n-hexyl group. 5 and R 6 As the alkyl group, a hydrogen atom and a methyl group are preferred, and a hydrogen atom is more preferred, from the viewpoints of reducing steric hindrance around the double bond and increasing reactivity.

[0079] R 7 is a group derived from a polyolefin. The polyolefin is preferably polyolefin (C). Polyolefin (C) is as described above.

[0080] (Structure Characterization of Modified Polyolefin (A)) The isoxazoline skeleton of the polyolefin modified material (A) is specified as follows: 1 This can be done by H-NMR. Specifically, the polyolefin modified material (A) is placed in an NMR sample tube with an inner diameter of 10 mm together with a mixed solution of o-dichlorobenzene / deuterated bromide benzene (C6D5Br) and hexamethyldisiloxane, a chemical shift standard substance, and dissolved uniformly in a block heater at 150°C. NMR measurements are performed at 120°C using a Bruker Biospin AV400 NMR device equipped with a 10mmφ cryoprobe.

[0081] FIG. 1 shows the structure of the modified polyolefin (A1) used in the examples. 1The polyolefin modified material (A1) is a polyolefin modified material having a general formula [II] R 4 , R 5 and R 6 are all hydrogen atoms, but as shown in Figure 1, R 4 The hydrogen atom signals of R 5 and R 6 The hydrogen atom signals of R are observed in the range of 2.3 to 3.0 ppm, and based on this, the isoxazoline skeleton can be identified. 4 , R 5 and R 6 Similarly, when the alkyl group has 1 to 8 carbon atoms, 1 The isoxazoline skeleton can be identified by H-NMR.

[0082] The nitrile oxide group in the polyolefin modified material (A) can be identified by IR measurement. Specifically, a pressed piece of 40 mm × 30 mm × 0.5 mmt was prepared at 175°C using pellets of the polyolefin modified material (A), and IR measurement was performed. -1 The absorbance of the nitrile oxide group is calculated from the peak height of the nitrile oxide group observed around 2210 cm. -1 and 2310cm -1 2258cm when the line connecting -1 is the peak height.

[0083] <Polyolefin block copolymer resin composition> Another aspect of the present invention is a polyolefin block copolymer resin composition comprising a melt-kneaded product of a polyolefin modified material (A) having at least one nitrile oxide group and an acrylonitrile-butadiene-styrene copolymer. The polyolefin modified material (A) is preferably obtained by the above-mentioned method for producing the polyolefin modified material (A). The polyolefin block copolymer resin composition has excellent compatibility between the polyolefin portion and the acrylonitrile-butadiene-styrene copolymer portion, and the block copolymer can maintain a high molecular weight, so that the molded article obtained has excellent mechanical properties. Furthermore, the present inventors have found that the molded article obtained from the block copolymer resin composition exhibits unexpectedly excellent scratch resistance.

[0084] The polyolefin block copolymer preferably has a structure derived from an acrylonitrile-butadiene-styrene copolymer and a structure represented by the following general formula [III]. [ka] In the general formula [III], s, n, R 1 , R 2 , X, A, R 4 , R 5 , R 6 and R 7 is as described above; * is a pair of sn pairs, and * in each pair is independently a reaction site with the butadiene-derived double bond in the structure derived from the acrylonitrile-butadiene-styrene copolymer. In the polyolefin block copolymer, it is considered that the nitrile oxide group of the modified polyolefin (A) reacts with the carbon-carbon double bond remaining in the acrylonitrile-butadiene-styrene copolymer to form an isoxazoline skeleton.

[0085] In the structure derived from the acrylonitrile-butadiene-styrene copolymer, the lower limit of the units derived from acrylonitrile is preferably 2% by mass, more preferably 5% by mass, and even more preferably 10% by mass, and the upper limit of the units derived from acrylonitrile is preferably 30% by mass, more preferably 20% by mass, and even more preferably 15% by mass. In the structure derived from the acrylonitrile-butadiene-styrene copolymer, the lower limit of the butadiene-derived units is preferably 30% by mass, more preferably 40% by mass, and even more preferably 50% by mass, and the upper limit of the butadiene-derived units is preferably 90% by mass, more preferably 85% by mass, and even more preferably 80% by mass. In the structure derived from the acrylonitrile-butadiene-styrene copolymer, the lower limit of the units derived from styrene is preferably 5% by mass, more preferably 8% by mass, and even more preferably 10% by mass, and the upper limit of the units derived from styrene is preferably 50% by mass, more preferably 45% by mass, and even more preferably 40% by mass. The total of the units derived from acrylonitrile, the units derived from butadiene and the units derived from styrene is 100% by mass.

[0086] From the viewpoint of improving scratch resistance, in the polyolefin block copolymer, the blending ratio of the modified product (A) and the acrylonitrile-butadiene-styrene copolymer is preferably 99:1 to 10:90, more preferably 95:5 to 30:70, even more preferably 90:10 to 50:50, and particularly preferably 90:10 to 75:25, on a mass basis.

[0087] The polyolefin block copolymer resin composition may contain other components (resins, fillers, additives, etc.) within the scope of not impairing the object of the present invention. The other components can be blended before mixing the polyolefin modified material (A) and the polymer (B), while they are being mixed and reacted, or into the polyolefin block copolymer after the reaction is completed. The other components may also be blended during the production of the polyolefin modified material (A) and the polymer (B). The amount of the other components is usually 0.001 to 250 parts by mass relative to 100 parts by mass of the polyolefin block copolymer. From the viewpoint of improving scratch resistance, the amount is preferably 0.001 to 240 parts by mass relative to 100 parts by mass of the polyolefin block copolymer. If the amount of the other components is less than 0.001 parts by mass, the effect of the added other components may not be sufficiently obtained, and if it is more than 250 parts by mass, the scratch resistance may not be sufficiently obtained.

[0088] Examples of the filler include inorganic fillers (talc, calcium carbonate, calcined kaolin, etc.) and organic fillers (fibers, wood powder, cellulose powder, etc.). Examples of additives include antioxidants (phenol-based, sulfur-based, phosphorus-based, lactone-based, vitamin-based, etc.), weathering stabilizers, ultraviolet absorbers (benzotriazole-based, tridiamine-based, anilide-based, benzophenone-based, etc.), heat stabilizers, light stabilizers (hindered amine-based, benzoate-based, etc.), antistatic agents, nucleating agents, pigments, adsorbents (metal oxides such as zinc oxide and magnesium oxide), metal chlorides (iron chloride, calcium chloride, etc.), hydrotalcite, aluminates, lubricants, mineral oils, silicone compounds, and the like.

[0089] <Applications of polyolefin block copolymers> Polyolefin block copolymers have excellent mechanical properties such as compatibility between the polyolefin portion and the polymer portion having a structural unit derived from acyclic dienes, scratch resistance, and tensile elongation at break, and can be suitably used in fields such as metals, woodworking, automotive repair paints, and adhesion modifiers for different resins. EXAMPLES

[0090] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.

[0091] <Measurement of physical properties, analysis, etc.> (Melting point measurement 1) Using a melting point measurement apparatus (SMP3, manufactured by Stuart Scientific), the compound represented by general formula [I] was heated at a rate of 1°C / min, and the temperature (°C) at which all the solid melted was determined as the melting point of the compound represented by general formula [I]. (Melting point measurement 2) The melting point (Tm) of polyolefin (C) was measured in accordance with JIS K 7121:2012 using a differential scanning calorimeter (DSC, TA Instruments, Q2000). The polymer powder of polyolefin (C) was heated in a press at 200°C for 3 minutes, and then cooled at 23°C for 5 minutes to form a sheet. This sheet-shaped molded product was used as a sample. The temperature of the sample was once raised to 200°C and left to stand for 5 minutes, then the temperature was lowered to 40°C at a rate of 10°C / min, and the temperature was measured again at a rate of 10°C / min. The temperature at the endothermic peak top was taken as the melting point. The unit is °C.

[0092] (Calculation method for carbon-carbon double bond terminal ratio) The carbon-carbon double bond terminal ratio of the polyolefin (C) was calculated in accordance with JP 2021-4376 A. 200 mg of sample was placed in a 10 mm diameter NMR sample tube together with 2.4 ml of o-dichlorobenzene / deuterated bromide benzene (C6D5Br) mixed solution and hexamethyldisiloxane, a chemical shift standard substance, and dissolved uniformly in a block heater at 150°C. NMR measurements were performed at 120°C using a Bruker Biospin AV400 NMR instrument equipped with a 10 mm diameter cryoprobe.

[0093] To quantify the number of carbon-carbon double bond ends, 1 H-NMR was used. 1 The H-NMR measurement conditions were a sample temperature of 120°C, a pulse angle of 4.5°, a pulse interval of 2 seconds, and an accumulation count of 512. The chemical shift of the proton signal of hexamethyldisiloxane was set to 0.09 ppm, and the chemical shifts of the signals due to other protons were based on this. To quantify the number of saturated ends and LCBs, 13 C-NMR was used. 13The C-NMR measurement conditions were a sample temperature of 120°C, a pulse angle of 45°, a pulse interval of 18 seconds, and an accumulation of 3072 times. The measurement was performed using the broadband decoupling method. 13 The C signal was set at 1.98 ppm, and the other 13 The chemical shifts of the C signals were based on this.

[0094] The above 1 H-NMR and 13 Based on the C-NMR measurement results and in accordance with the method described in the specification, the total number of carbon-carbon double bond ends, the total number of ends, and the number of LCBs were calculated, and the carbon-carbon double bond end ratio was calculated from the following formula. (Carbon-carbon double bond terminal rate) = (total number of carbon-carbon double bond terminals) / {((total number of terminals) - (number of LCBs)) ÷ 2} × 100 Here, the total number of carbon-carbon double bond terminals is 1 The total number of carbon-carbon double bond ends per 1,000 monomer units calculated by H-NMR. 1 H-NMR and 13 The LCB number is the total number of terminals per 1000 monomer units calculated by C-NMR. 13 This is the number of methine carbons in the main chain to which branched chains having 7 or more carbon atoms per 1,000 monomer units are bonded, as calculated by C-NMR.

[0095] (Identification of isoxazoline structure) The isoxazoline skeleton of the polyolefin modified product is specified as follows: 1 The measurements were performed by H-NMR. Specifically, the modified polyolefin was placed in an NMR sample tube with an inner diameter of 10 mm together with a mixed solution of o-dichlorobenzene / deuterated bromide benzene (C6D5Br) and hexamethyldisiloxane, a chemical shift standard substance, and dissolved uniformly in a block heater at 150°C. The NMR measurements were performed at 120°C using a Bruker Biospin AV400 NMR device equipped with a 10mmφ cryoprobe.

[0096] (Identification of nitrile oxide group) The nitrile oxide group in the modified polyolefin was identified by IR measurement. Specifically, a pressed piece of 40 mm × 30 mm × 0.5 mmt was prepared at 175 ° C. using a pellet of the modified polyolefin, and IR measurement was performed. -1 The presence or absence of a peak of a nitrile oxide group observed in the vicinity was confirmed.

[0097] (MFR measurement) For the pellets of the examples and comparative examples, MFR (temperature: 230° C. and load: 2.16 kg) was measured in accordance with JIS K 7210-1:2014.

[0098] (Preparation of flat test pieces) Using a molding machine (Toshiba Machine Co., Ltd. EC20 type injection molding machine) and the following mold, flat test pieces for evaluating physical properties were produced under the following conditions. Mold: For one flat test piece (40 x 80 x 2t (mm)) for evaluating physical properties. Molding conditions: Molding temperature 200℃, mold temperature 40℃, injection pressure 40MPa, injection time 8 seconds, cooling time 12 seconds.

[0099] (Scratch resistance) The obtained flat test piece was scratched at a scratching speed of 100 mm / min using a "SCRATCH & MAR TESTER" manufactured by ROCKWOOD SYSTEMS AND EQUIPMENT Co., Ltd., while applying a load of 3, 5, 7, 10 or 13 N to the scratch tip that had been processed into a shape (curvature radius 0.5 mm, ball-shaped), and the shape of the scratch was visually judged at an angle of 90 degrees to the test piece, and the maximum load at which whitening of the scratch was not noticeable was taken as the measurement value. When the load applied to the scratch tip was 3 N and whitening of the scratch was observed, the measurement value was taken as 0 N. The number of n was 5, and the average value of the measurement values ​​was taken as the evaluation value of scratch resistance. The test environment was 23°C and 50% RH. The higher the evaluation value, the better the scratch resistance. If the evaluation value was 3N or more, it was determined that the scratch resistance was good, if it was 5N or more, it was determined that the scratch resistance was even better, and if it was 7N or more, it was determined that the scratch resistance was particularly excellent.

[0100] (mirror gloss) The specular gloss of the obtained flat test piece was measured at 23° C., 50% RH and an incidence angle of 60° using a VG-2000 model manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS Z8741.

[0101] <Polyolefin (C)> (PP1: Propylene homopolymer) [PP1 Production] <Catalyst synthesis example 1> (1) Synthesis of metallocene complexes (1-a) Synthesis of rac-dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-i-propylphenyl)indenyl}]hafnium (complex (1-a)): rac-Dichloro[1,1′-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-i-propylphenyl)indenyl}]hafnium was synthesized according to the method of Synthesis Example 1 in JP2012-149160A.

[0102] (1-b) Synthesis of rac-dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium (complex (1-b)): rac-Dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium was synthesized according to the method of Example 7 of JP-A-11-240909.

[0103] (2) Preparation of metallocene catalyst (2-a) Chemical treatment of ion-exchangeable layered silicate In a 1L three-neck flask equipped with a stirring blade and a reflux device, 645.1g of distilled water and 82.6g of 98% sulfuric acid were added and heated to 95°C. 100g of ion-exchange layered silicate (montmorillonite, Benclay KK manufactured by Mizusawa Chemical Industry Co., Ltd., Al = 9.78 mass%, Si = 31.79 mass%, Mg = 3.18 mass%, Al / Si (molar ratio) = 0.320, average particle size 14 μm) was added to this aqueous solution, and the reaction was carried out at 95°C for 320 minutes. After 320 minutes, 0.5L of distilled water was added to stop the reaction, and the resulting reaction product was filtered to obtain 255g of a cake-like solid. 1 g of this cake-like solid contained 0.31 g of the chemically treated montmorillonite (intermediate). The chemical composition of the chemically treated montmorillonite (intermediate) was Al = 7.68 mass%, Si = 36.05 mass%, Mg = 2.13 mass%, and Al / Si (molar ratio) = 0.222. 1545g of distilled water was added to the cake-like solid to form a slurry, and the temperature was raised to 40°C. 5.734g of lithium hydroxide hydrate was added as a solid to the obtained slurry, and the reaction was carried out at 40°C for 1 hour. After 1 hour, the reaction slurry was filtered and washed three times with 1L of distilled water to obtain a cake-like solid again. The collected cake-like solid was dried in a normal pressure dryer at 110°C to obtain 80 g of chemically treated montmorillonite. The chemical composition of this chemically treated montmorillonite was Al = 7.68 mass%, Si = 36.05 mass%, Mg = 2.13 mass%, Al / Si (molar ratio) = 0.222, and Li = 0.53 mass%. The obtained chemically treated montmorillonite was dried under reduced pressure in an oil bath at 200°C for at least 2 hours and used in the subsequent procedures.

[0104] (2-b) Prepolymerization Unless otherwise specified, the experiments were carried out under a nitrogen atmosphere using equipment that had been thoroughly dried to remove moisture. 10 g of the chemically treated montmorillonite after the reduced pressure drying in (2-a) above was placed in a 1 L three-neck flask, and 66 mL of heptane was added. Triisobutylaluminum (25 mmol: 34.0 mL of a heptane solution with a concentration of 143 mg / mL) was added to this slurry with stirring, and then the mixture was stirred for 1 hour. After 1 hour, the obtained slurry was washed with heptane until the residual liquid ratio was 1 / 100, and the total volume was reduced to 50 mL to prepare a chemically treated montmorillonite slurry. In another 200 mL flask, 105 μmol of the above complex (1-a) was dissolved in 21 mL of toluene to prepare complex solution 1. Furthermore, in another 200 mL flask, 45 μmol of the above complex (1-b) was dissolved in 9 mL of toluene to prepare complex solution 2. Triisobutylaluminum (0.42 mmol: 0.6 mL of a heptane solution with a concentration of 143 mg / mL) was added to the above chemically treated montmorillonite slurry, and then the entire amount of the above complex solution 1 was added and stirred at room temperature for 20 minutes. Thereafter, triisobutylaluminum (0.18 mmol: 0.25 mL of a heptane solution with a concentration of 143 mg / mL) was further added to this solution, and then the entire amount of the above complex solution 2 was added and stirred at room temperature for 1 hour. After 1 hour, 170 mL of heptane was added to this slurry, and then this slurry was introduced into a 1 L autoclave. After the internal temperature of the autoclave was set to 40°C, propylene was fed at 5g / hour, and prepolymerization was carried out while maintaining 40°C for 4 hours with stirring. Then, the propylene feed was stopped, and residual polymerization was carried out for 1 hour. After 1 hour, the slurry in the autoclave was extracted into a 1L three-neck flask. The supernatant of the obtained slurry was removed by decantation, and triisobutylaluminum (6 mmol: 8.5 mL of a heptane solution with a concentration of 143 mg / mL) was added to the remaining slurry portion and stirred for 5 minutes. Then, the mixture was dried under reduced pressure at 40°C for 1 hour with stirring to obtain 30.9 g of a prepolymerization catalyst. The prepolymerization ratio (the value obtained by dividing the amount of prepolymerized polymer by the amount of solid catalyst) was 2.09. This prepolymerization catalyst was designated as catalyst 1.

[0105] <Polymerization> A 20L autoclave was dried thoroughly in advance by passing nitrogen through it under heating, and then the inside of the vessel was replaced with propylene and cooled to room temperature, and 18.7mL of a heptane solution of triisobutylaluminum (140mg / mL) and 0.85N (normal)L of hydrogen were introduced. Next, 5000g of liquid propylene was introduced and the temperature was raised to 63°C. Then, 230mg of the above catalyst 1 (excluding the prepolymerized polymer) was pumped into the autoclave with high-pressure argon to start polymerization, and the temperature was quickly raised to 70°C. The temperature was kept at 70°C, and after 1 hour from the start of polymerization, the unreacted propylene was quickly purged to stop the polymerization. As a result, about 1730g of polymer powder (PP1) was obtained. The carbon-carbon double bond terminal ratio of PP1 was 65.2%, and the melting point (Tm) was 156°C.

[0106] 100 parts by mass of the above PP1 was mixed with 0.1 part by mass of a phenolic antioxidant, IRGANOX (registered trademark) 1010, manufactured by BASF Japan Ltd., 0.2 part by mass of a phosphorus-based antioxidant, IRGAFOS (registered trademark) 168, manufactured by BASF Japan Ltd., and 0.05 part by mass of a neutralizing agent, BKS (registered trademark), manufactured by Nitto Kasei Kogyo Co., Ltd., and the mixture was measured in accordance with JIS K 7210-1:2014 to find that the MFR (temperature 230°C, load 2.16 kg) was 20 g / 10 min.

[0107] <Other polyolefins> [PP2] The product name "Novatec (registered trademark) PP" manufactured by Japan Polypropylene Corporation was used as a grade having the following composition (PP2). PP2 is a polymer powder of propylene homopolymer polymerized with a Ziegler-Natta catalyst, with a carbon-carbon double bond terminal ratio of 0.0% and a melting point (Tm) of 160°C. As with PP1, each additive was mixed into PP2, and the MFR was measured, resulting in a MFR of 20 g / 10 min.

[0108] <Compound represented by general formula [I]> The compound represented by the following formula [VII] having a melting point of 95°C was synthesized according to Example 2A of WO 2019 / 107450. [ka]

[0109] <Production of modified polyolefin (A1)> For the production of the polyolefin modified material (A1), a twin-screw kneader "KZW15" manufactured by Technobel Co., Ltd. was used. 300 g of PP1 and 2 equivalents of the compound represented by formula [VII] relative to the carbon-carbon double bond of PP1 were mixed in a plastic bag to obtain a mixture. The entire mixture was charged into the feeder of KZW15, which had been preheated to 180° C., and the reaction was started at a screw rotation speed of 400 rpm. After melt kneading for 10 seconds, the strand obtained from the die outlet was cut, and pellets of the polyolefin modified product (A1) were collected.

[0110] The pellets thus obtained were used to prepare pressed pieces of 40 mm × 30 mm × 0.5 mmt at 175 °C, and IR measurements were performed to obtain a value of 2258 cm -1 A peak corresponding to a nitrile oxide group was observed in the vicinity. Polyolefin modified material (A1) 1 The H NMR spectrum is shown in FIG. 1. As shown in FIG. 1, R 4 The hydrogen atom signals of R 5 and R 6 The hydrogen atom signals were observed in the range of 2.3 to 3.0 ppm, and based on this, the presence of the isoxazoline skeleton was confirmed.

[0111] <Acrylonitrile-butadiene-styrene copolymer (hereinafter referred to as "ABS")> ABS (B1): Techno UMG Co., Ltd., UMG ABS (registered trademark) EX18A ABS (B2): Techno UMG Co., Ltd., UMG ABS (registered trademark) EX10U ABS (B3): Techno UMG Co., Ltd., UMG ABS (registered trademark) TJ3G

[0112] Example 1 270 g of pellets of polyolefin modified material (A1) and 30 g of pellets of ABS (B1) were mixed, and the entire mixture was charged into the feeder of KZW15 preheated to 200° C., and the reaction was started at a screw rotation speed of 400 rpm. After melt kneading for 10 seconds, the strand obtained from the die outlet was cut, and polymer 1 was recovered as pellets.

[0113] Example 2 Polymer 2 was recovered as pellets in the same manner as in Example 1, except that the amount of pellets of the polyolefin modified material (A1) was changed to 240 g and the amount of pellets of ABS (B1) was changed to 60 g.

[0114] Example 3 Polymer 3 was recovered as pellets in the same manner as in Example 2, except that ABS (B1) was changed to ABS (B2).

[0115] Example 4 Polymer 4 was recovered as pellets in the same manner as in Example 2, except that ABS (B1) was changed to ABS (B3).

[0116] Example 5 Polymer 5 was recovered as pellets in the same manner as in Example 1, except that the amount of pellets of the polyolefin modified material (A1) was changed to 195 g and the amount of pellets of ABS (B1) was changed to 105 g.

[0117] Example 6 Polymer 6 was recovered as pellets in the same manner as in Example 1, except that the amounts of pellets of polyolefin modified product (A1) were changed to 180 g, PP2 to 60 g, and ABS (B1) to 60 g.

[0118] Example 7 Polymer 7 was recovered as pellets in the same manner as in Example 1, except that the amounts of pellets of polyolefin modified product (A1) were changed to 120 g, PP2 to 120 g, and ABS (B1) to 60 g.

[0119] Example 8 Polymer 8 was recovered as pellets in the same manner as in Example 1, except that the amounts of pellets of polyolefin modified product (A1) were changed to 60 g, PP2 to 180 g, and ABS (B1) to 60 g.

[0120] Example 9 Polymer 9 was recovered as pellets in the same manner as in Example 1, except that the amounts of pellets of polyolefin modified product (A1) were changed to 30 g, PP2 to 210 g, and ABS (B1) to 60 g.

[0121] Comparative Example 1 300 g of pellets of the polyolefin modified material (A1) were placed in the feeder of KZW15, which had been preheated to 200°C, and melt-kneaded for 10 seconds at a screw rotation speed of 400 rpm. The strand obtained at the die outlet was then cut, and polymer C1 was recovered as pellets.

[0122] Comparative Example 2 Polymer C2 was recovered as pellets in the same manner as in Comparative Example 1, except that PP1 was used instead of the pellets of the polyolefin modified product (A1).

[0123] Comparative Example 3 Polymer C3 was recovered as pellets in the same manner as in Example 1, except that PP1 was used instead of the pellets of the polyolefin modified product (A1).

[0124] Comparative Example 4 Polymer C4 was recovered as pellets in the same manner as in Example 2, except that PP1 was used instead of the pellets of the polyolefin modified product (A1).

[0125] Comparative Example 5 Polymer C5 was recovered as pellets in the same manner as in Example 3, except that PP1 was used instead of the pellets of the polyolefin modified product (A1).

[0126] Comparative Example 6 Polymer C6 was recovered as pellets in the same manner as in Example 4, except that PP1 was used instead of the pellets of the polyolefin modified product (A1).

[0127] Comparative Example 7 Polymer C7 was recovered as pellets in the same manner as in Example 5, except that PP1 was used instead of the pellets of the polyolefin modified product (A1).

[0128] Table 1 shows the formulations of Examples 1 to 9 and Comparative Examples 1 to 7, as well as the evaluation results of the resulting pellets.

[0129] [Table 1]

[0130] <Consideration> As shown in Table 1, the polyolefin block copolymers of Examples 1 to 9 obtained by melt-kneading the polyolefin modified product (A1) and ABS (B1) to (B3), respectively, have lower MFR, higher molecular weight, and significantly improved scratch resistance, compared to Comparative Examples 3 to 7 obtained by simply melt-kneading a mixture of the propylene homopolymer PP1 and ABS (B1) to (B3). This phenomenon is believed to be due to the fact that in the examples, the block copolymer is produced, improving the compatibility between the polyolefin portion and the ABS portion, resulting in improved interfacial strength between the two portions. Comparing Examples 1 to 5, Examples 1 to 4, in which the blending ratio of the polyolefin modified material (A1) to the ABS (B1) to (B3) is 90:10 to 80:20 by mass, have even better scratch resistance. Comparative Example 1, which used only the polyolefin modified product (A1), and Comparative Example 2, which used only PP1, were inferior in scratch resistance. In addition, although the mechanism of action is unclear, the molded articles obtained from the pellets of Examples 1 to 9 had lower gloss than those of Comparative Examples 1 to 7. Therefore, the polyolefin block copolymer according to the present invention can be suitably used in applications requiring the elimination of gloss and the enhancement of design, such as automotive interior materials and matte films.

[0131] Figures 2 and 3 show cross-sectional SEM photographs of molded articles obtained from the pellets of Example 2 and Comparative Example 4, respectively. Comparing the areas surrounded by ellipses in each figure, it can be seen that in Figure 3, the ABS domains (black areas in the photograph) are stretched and elongated in the lateral direction, forming large clumps, whereas in Figure 2, many fine ABS domains are present. That is, it can be seen that in the polyolefin block copolymer of Example 2, the dispersibility of the ABS domains in the polyolefin is dramatically improved, and the compatibility between the two is greatly improved. [Industrial Applicability]

[0132] The production method of the present invention can produce a polyolefin block copolymer having excellent compatibility between the polyolefin portion and the polymer portion having a structural unit derived from acyclic diene, excellent scratch resistance, and excellent mechanical properties such as tensile elongation at break. The polyolefin block copolymer can be suitably used in fields such as metal, woodwork, automotive repair paints, and adhesion modifiers for different resins.

Claims

1. A method for producing a polyolefin block copolymer, comprising the step of mixing a polyolefin modified product (A) having at least one nitrile oxide group and a polymer (B) having a structural unit derived from a non-cyclic diene.

2. The method for producing a polyolefin block copolymer according to claim 1, wherein the polymer (B) is a copolymer further having at least one selected from the group consisting of a structural unit derived from acrylonitrile or a derivative thereof and a structural unit derived from styrene or a derivative thereof.

3. The method for producing a polyolefin block copolymer according to claim 1, wherein the polymer (B) is an acrylonitrile-butadiene-styrene copolymer.

4. The method for producing a polyolefin block copolymer according to claim 1, wherein the modified product (A) is obtained by addition reaction of a polyolefin (C) having a carbon-carbon double bond at at least one end of a main chain and having a carbon-carbon double bond terminal ratio of 20% or more with a compound (D) represented by the following general formula [I]: [Formula 1] In the general formula [I], s is an integer from 2 to 4; R 1 and R 2 each independently represents a hydrocarbon group having 4 to 10 carbon atoms or a halogenated hydrocarbon group having 4 to 10 carbon atoms, Each X is independently a divalent hydrocarbon group, -O-, -S- or -N(R 3 ) - and R 3 is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, A is a hydrocarbon group having 1 to 20 carbon atoms which may contain at least one heteroatom having a valence of s.

5. The method for producing a polyolefin block copolymer according to claim 1 , wherein the modified product (A) is represented by the following general formula [II]: [chemical 2] In the general formula [II], s is an integer from 2 to 4; n is an integer from 1 to 3, s>n, R 1 and R 2 each independently represents a hydrocarbon group having 4 to 10 carbon atoms or a halogenated hydrocarbon group having 4 to 10 carbon atoms, Each X is independently a divalent hydrocarbon group, -O-, -S- or -N(R 3 ) - and R 3 is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, A is a hydrocarbon group having 1 to 20 carbon atoms which may contain at least one s-valent heteroatom; R 4 , R 5 and R 6 are each independently a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms, R 7 is a group derived from a polyolefin.

6. The method for producing a polyolefin block copolymer according to claim 1, wherein the step of mixing the modified product (A) and the polymer (B) is carried out at 80 to 300°C.

7. The method for producing a polyolefin block copolymer according to claim 1 or 6, wherein the step of mixing the modified product (A) and the polymer (B) is carried out by melt kneading.

8. A polyolefin block copolymer resin composition comprising a melt-kneaded product of a polyolefin modified product (A) having at least one nitrile oxide group and an acrylonitrile-butadiene-styrene copolymer.

9. The polyolefin block copolymer resin composition according to claim 8, comprising a polyolefin block copolymer having a structure derived from an acrylonitrile-butadiene-styrene copolymer and a structure represented by the following general formula [III]: [C3] In the general formula [III], s is an integer from 2 to 4; n is an integer from 1 to 3, s>n, R 1 and R 2 each independently represents a hydrocarbon group having 4 to 10 carbon atoms or a halogenated hydrocarbon group having 4 to 10 carbon atoms, Each X is independently a divalent hydrocarbon group, -O-, -S- or -N(R 3 ) - and R 3 is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, A is a hydrocarbon group having 1 to 20 carbon atoms which may contain at least one s-valent heteroatom; R 4 , R 5 and R 6 are each independently a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms, R 7 is a group derived from a polyolefin, The symbol * denotes a pair of sn pairs, and each pair of * independently represents a reaction site with a double bond derived from butadiene in the structure derived from the acrylonitrile-butadiene-styrene copolymer.

Citation Information

Patent Citations

  • JP125086A

  • Production of modified polyolefin

    JP1995173229A

  • Compatibilizer for thermoplastic resin

    JP2008106256A

  • Multilayer film, adhesive film, decorative film, decorative adhesive film, and automobile protective film

    JP2021154730A

  • JP206587A