Polyimide resin
The polyimide resin with ethylenically unsaturated bonds addresses the issues of dielectric loss tangent and film retention in semiconductor substrates, enhancing electrical performance and stability.
Patent Information
- Application Number
- JP2023046843
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing photosensitive resin compositions used in semiconductor package substrates face challenges in achieving low dielectric loss tangent and maintaining excellent film retention properties, which are crucial for high-speed communication devices.
A polyimide resin is developed with a specific structure containing an ethylenically unsaturated bond, which forms crosslinked structures upon exposure to light, reducing solubility in developers and minimizing polar group introduction, thereby improving dielectric properties and film retention.
The polyimide resin composition achieves enhanced film retention and reduced dielectric loss tangent, resulting in improved electrical performance and stability for semiconductor devices.
Smart Images

Figure 2024135928000001 
Figure 2024135928000002 
Figure 2024135928000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyimide resin and a method for producing the same. The present invention also relates to a photosensitive resin composition, a photosensitive film, a semiconductor package substrate and a method for producing the same, and a semiconductor device, each using the polyimide resin. [Background technology]
[0002] Polyimide resins, which have excellent heat resistance and insulating properties, have conventionally been used for insulating layers of semiconductor devices (see, for example, Patent Document 1). Such polyimide resins can be used, for example, as materials for photosensitive resin compositions for forming insulating layers. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2003-084435 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, with the increase in communication speed and capacity in communication devices, photosensitive resin compositions used in semiconductor package substrates for communication devices are required to have a low dielectric tangent. In addition, photosensitive resin compositions are also required to have excellent film retention. The film retention of a photosensitive resin composition refers to the property of the photosensitive resin composition being less likely to lose thickness when exposed to light and comes into contact with a developer.
[0005] The present invention has been made in view of the above problems, and has an object to provide a polyimide resin capable of giving a photosensitive resin composition excellent in film retention and dielectric tangent of the cured product and a method for producing the same; a photosensitive resin composition containing the polyimide resin; a photosensitive film containing the photosensitive resin composition; a semiconductor package substrate containing a cured product of the photosensitive resin composition and a method for producing the same, and a semiconductor device. [Means for solving the problem]
[0006] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by a novel polyimide resin having a structure in which a specific group containing an ethylenically unsaturated bond is bonded to the methylene group of a polyimide resin containing a methylene group connecting two benzene rings via a carbon-carbon double bond, thereby completing the present invention. That is, the present invention includes the following.
[0007] [1] A polyimide resin comprising a repeating unit represented by the following formula (1): [ka] (In formula (1), X 1 represents a tetravalent organic group, Y 1 represents a divalent organic group, X 1 and Y 1 At least one of the above contains at least two benzene rings and a divalent group represented by formula (1-1) linking the two benzene rings. [ka] (In formula (1-1), R 1 and R 2 represents a hydrogen atom, -CN, -NO2, -COH, -R, -OR, -COR, -COOR, -CONHR, -CONR2, -SR, -SOR, or -SOR; R 1 and R 2 At least one of the above contains an ethylenically unsaturated bond, R 1 and R 2 may be joined together to form a non-aromatic ring which may have a substituent; Each R independently represents an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent. * represents a bond.) [2] In formula (1), X 1 contains one or more structures selected from the group consisting of a structure represented by the following formula (X1-1) and a structure represented by the following formula (X1-2): [ka] (In the formula (X1-1) and the formula (X1-2), R 11 and R 12 represents a hydrogen atom, -CN, -NO2, -COH, -R, -OR, -COR, -COOR, -CONHR, -CONR2, -SR, -SOR, or -SOR; R 11 and R 12 At least one of the above contains an ethylenically unsaturated bond, R 11 and R 12 may be joined together to form a non-aromatic ring which may have a substituent; R each independently represents an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent; R 13 and R 14 each independently represents a substituent; L 1 represents a divalent organic group; n 11 and n 12 each independently represents an integer of 0 to 3; n 13 and n 14 each independently represents an integer of 0 or more and 2 or less. * represents a bond.) [3] L 1 is a methylene group, -C(=O)-, or -C(=CR 11 R 12 )-. The polyimide resin according to [2]. [4] In equation (1), Y 1contains one or more structures selected from the group consisting of a structure represented by the following formula (Y1-1), a structure represented by the following formula (Y1-2), a structure represented by the following formula (Y1-3), and a structure represented by the following formula (Y1-4). [ka] (In the formulae (Y1-1), (Y1-2), (Y1-3) and (Y1-4), R 21 and R 22 represents a hydrogen atom, -CN, -NO2, -COH, -R, -OR, -COR, -COOR, -CONHR, -CONR2, -SR, -SOR, or -SOR; R 21 and R 22 At least one of the above contains an ethylenically unsaturated bond, R 21 and R 22 may be joined together to form a non-aromatic ring which may have a substituent; R each independently represents an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent; R 23 and R 24 each independently represents a substituent; L 2 represents a divalent organic group; n 21 and n 22 each independently represents an integer of 0 to 4; n 23 and n 24 each independently represents an integer of 0 to 3; n 25 represents an integer between 0 and 3; n 26 represents an integer between 0 and 5; n 27 denotes an integer between 0 and 2; n 28 indicates an integer between 0 and 4 inclusive. * represents a bond.) [5] L 2 is a methylene group, -C(=O)-, or -C(=CR 21 R 22 )-. The polyimide resin according to [4]. [6] R 1 and R 2 At least one of the above is represented by the following formula (1-2): [ka] (In formula (1-2), R 15 , R 16 and R 17 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms; p1 represents an integer from 0 to 10; * represents a bond.) [7] The polyimide resin according to any one of [1] to [6], which has a weight average molecular weight of 5,000 or more. [8] A photosensitive resin composition comprising the polyimide resin according to any one of [1] to [7], a crosslinking agent, and a photoradical generator. [9] The photosensitive resin composition according to [8], further comprising a sensitizer.
[10] The photosensitive resin composition according to [8] or [9], wherein the amount of the polyimide resin is 40% by mass or more and 95% by mass or less, based on 100% by mass of the non-volatile components of the photosensitive resin composition.
[11] A photosensitive resin composition layer comprising: a support; and a photosensitive resin composition layer formed on the support; A photosensitive film, wherein a photosensitive resin layer contains the photosensitive resin composition according to any one of [8] to
[10] .
[12] A semiconductor package substrate comprising a cured product of the photosensitive resin composition according to any one of [8] to
[10] .
[13] A semiconductor device comprising the semiconductor package substrate according to
[12] .
[14] A step of forming a photosensitive resin composition layer containing the photosensitive resin composition according to any one of [8] to
[10] on a circuit board; A step of irradiating the photosensitive resin composition layer with actinic rays; developing the photosensitive resin composition layer; A method for manufacturing a semiconductor package substrate, comprising:
[15] A method for producing the polyimide resin according to any one of [1] to [7], comprising reacting a precursor resin containing a repeating unit represented by the following formula (1') with a Wittig reagent or a phosphonic acid diester compound: [ka] (In formula (1'), X 2 represents a tetravalent organic group, Y 2 represents a divalent organic group, X 2 and Y 2 At least one of the above contains at least two benzene rings and a carbonyl group connecting the two benzene rings.
[16] A method for producing the polyimide resin according to any one of [1] to [7], comprising reacting a precursor resin containing a repeating unit represented by the following formula (1') with a β-dicarbonyl compound: [ka] (In formula (1'), X 2 represents a tetravalent organic group, Y 2 represents a divalent organic group, X 2 and Y 2 At least one of the above contains at least two benzene rings and a carbonyl group connecting the two benzene rings.
[17] A method for producing the polyimide resin according to any one of [1] to [7], comprising reacting a precursor resin containing a repeating unit represented by the following formula (1') with Meldrum's acid, and then reacting with an alcohol compound. [ka] (In formula (1'), X 2 represents a tetravalent organic group, Y 2 represents a divalent organic group, X 2 and Y 2 At least one of the above contains at least two benzene rings and a carbonyl group connecting the two benzene rings.
[18] A method for producing the polyimide resin according to any one of [1] to [7], comprising reacting a tetracarboxylic dianhydride represented by the following formula (1'-a) with a diamine compound represented by the following formula (1'-b): [ka] (In formula (1'-a), X 1 represents a tetravalent organic group. 1 represents a divalent organic group. 1 and Y 1 At least one of the above contains at least two benzene rings and a divalent group represented by formula (1-1) linking the two benzene rings. Effect of the Invention
[0008] According to the present invention, it is possible to provide a polyimide resin capable of giving a photosensitive resin composition having excellent film retention and dielectric tangent of the cured product and a method for producing the same; a photosensitive resin composition containing the polyimide resin; a photosensitive film containing the photosensitive resin composition; a semiconductor package substrate containing a cured product of the photosensitive resin composition and a method for producing the same, and a semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described in detail below with reference to the following embodiments and examples. However, the present invention is not limited to the following embodiments and examples, and may be modified and implemented as desired without departing from the scope of the claims and their equivalents.
[0010] <Terminology explanation> As used herein, the term "optionally substituted" in reference to a compound or group means both the case where none of the hydrogen atoms of the compound or group are substituted with a substituent, and the case where some or all of the hydrogen atoms of the compound or group are substituted with a substituent.
[0011] In this specification, the term "organic group" refers to a group containing at least carbon atoms as skeletal atoms, and may be linear, branched, or cyclic. In this specification, unless otherwise specified, the number of skeletal atoms of an organic group is preferably 1 to 3000, more preferably 1 to 1000, even more preferably 1 to 100, still more preferably 1 to 50, and particularly preferably 1 to 30 or 1 to 20. Examples of the organic group include groups consisting of one or more skeletal atoms (including at least a carbon atom) selected from carbon atoms, oxygen atoms, nitrogen atoms, and sulfur atoms.
[0012] In this specification, the term "dielectric constant" refers to the "relative dielectric constant" unless otherwise specified.
[0013] <Polyimide resin> A polyimide resin according to one embodiment of the present invention contains a repeating unit represented by formula (1).
[0014] [ka]
[0015] (In formula (1), X 1 represents a tetravalent organic group; Y 1 represents a divalent organic group; X 1 and Y 1 At least one of these contains at least two benzene rings and a divalent group represented by formula (1-1) linking the two benzene rings.
[0016] [ka]
[0017] (In formula (1-1), R 1 and R 2 represents a hydrogen atom, -CN, -NO2, -COH, -R, -OR, -COR, -COOR, -CONHR, -CONR2, -SR, -SOR, or -SOR; R 1 and R 2 At least one of the above contains an ethylenically unsaturated bond, R 1 and R 2 may be joined together to form a non-aromatic ring which may have a substituent; Each R independently represents an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent.
[0018] According to the polyimide resin of this embodiment, a photosensitive resin composition having excellent film retention and dielectric loss tangent of the cured product can be obtained. Without being bound by a specific theory, the present inventors speculate that the mechanism by which the above-mentioned effects are obtained is as follows. However, the technical scope of the present invention is not limited by the mechanism described below.
[0019] The polyimide resin according to the present embodiment contains an ethylenically unsaturated bond. The term "ethylenically unsaturated bond" refers to a non-aromatic carbon-carbon unsaturated bond. Examples of the ethylenically unsaturated bond include non-aromatic carbon-carbon double bonds and carbon-carbon triple bonds, and preferably non-aromatic carbon-carbon double bonds. The ethylenically unsaturated bond reacts with light exposure to form a crosslinked structure, which effectively reduces the solubility in the developer, thereby improving the film remaining property of the photosensitive resin composition containing this polyimide resin. In addition, in the past, when an ethylenically unsaturated bond was introduced into a polyimide resin, many polar groups tended to be introduced together with the ethylenically unsaturated bond, but the polyimide resin according to the present embodiment does not introduce or can introduce only a small number of polar groups. Therefore, the polarity of the photosensitive resin composition and its cured product can be reduced, and the electrical properties such as the dielectric tangent can be improved.
[0020] - Explanation of the divalent group represented by formula (1-1) - [ka]
[0021] In formula (1-1), R 1 and R 2 represents a hydrogen atom, -CN, -NO2, -COH, -R, -OR, -COR, -COOR, -CONHR, -CONR2, -SR, -SOR, or -SO2R. 1 and R 2 and may be the same or different. Among them, a hydrogen atom, -CN, -NO2, -COH, -R, -COR, or -COOR is preferable; a hydrogen atom, -R, -COR, or -COOR is more preferable; and a hydrogen atom, -COR, or -COOR is even more preferable.
[0022] Each R independently represents an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent.
[0023] The alkyl group in R means a linear, branched and / or cyclic monovalent aliphatic saturated hydrocarbon group. The number of carbon atoms in the alkyl group is preferably 1 to 18, more preferably 1 to 10, and further preferably 1 to 6. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a sec-pentyl group, a neopentyl group, a tert-pentyl group, a hexyl group, an isohexyl group, a heptyl group, an isoheptyl group, an octyl group, an isooctyl group, a tert-octyl group, a cyclopentyl group, a cyclohexyl group, and a cyclohexylmethyl group.
[0024] The alkenyl group in R means a linear, branched and / or cyclic monovalent aliphatic unsaturated hydrocarbon group having at least one carbon-carbon double bond. The number of carbon atoms in the alkenyl group is preferably 2 to 18, more preferably 2 to 10, and even more preferably 2 to 6. Examples of the alkenyl group include a vinyl group, a propenyl group (allyl group, 1-propenyl group, isopropenyl group), a butenyl group (1-butenyl group, crotyl group, methallyl group, isocrotyl group, etc.), a pentenyl group (1-pentenyl group, etc.), a hexenyl group (1-hexenyl group, etc.), a heptenyl group (1-heptenyl group, etc.), an octenyl group (1-octenyl group, etc.), a cyclopentenyl group (2-cyclopentenyl group, etc.), a cyclohexenyl group (3-cyclohexenyl group, etc.), and the like.
[0025] The aryl group in R means a monovalent aromatic hydrocarbon group obtained by removing one hydrogen atom from an aromatic carbon ring. The number of carbon atoms in the aryl group is preferably 6 to 18, and more preferably 6 to 10. Examples of the aryl group include a phenyl group, a 1-naphthyl group, and a 2-naphthyl group.
[0026] The "substituent" in the "optionally substituted alkyl group" represented by R and the "substituent" in the "optionally substituted alkenyl group" represented by R are not particularly limited, and examples thereof include halogen atoms, -NO2, -CN, -COH, -OH, -SH, -NH2, -COOH, -R y , -COR x , -OR x , -SR x , -SOR x , -SO2R x , -NHR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, -NHCOR x Examples of monovalent substituents include the following.
[0027] The "substituent" in the "aryl group which may have a substituent" represented by R is not particularly limited, and examples thereof include a halogen atom, -NO2, -CN, -COH, -OH, -SH, -NH2, -COOH, -R x , -COR x , -OR x , -SR x , -SOR x , -SO2R x , -NHR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, -NHCOR x Examples of monovalent substituents include the following.
[0028] The above R x are each independently (1) an alkyl group which may be substituted with a group selected from the group consisting of a halogen atom, a nitro group, a cyano group, a hydroxy group, an amino group, an aryl group, an alkyl-substituted aryl group, an alkenyl-substituted aryl group, an alkoxy group, an alkenyloxy group, an aryloxy group, an aralkyloxy group, an alkylcarbonyl group, an alkenylcarbonyl group, an arylcarbonyl group, an aralkylcarbonyl group, an alkylcarbonyloxy group, an alkenylcarbonyloxy group, an arylcarbonyloxy group, an aralkylcarbonyloxy group, an alkyloxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an aralkyloxycarbonyl group, an alkylamino group, a di(alkyl)amino group, an alkenylamino group, an alkylalkenylamino group, an alkylcarbonylamino group, an alkenylcarbonylamino group, an alkylcarbamoyl group, and an alkenylcarbamoyl group; (2) an alkenyl group which may be substituted with a group selected from the group consisting of a halogen atom, a nitro group, a cyano group, a hydroxy group, an amino group, an aryl group, an alkyl-substituted aryl group, an alkenyl-substituted aryl group, an alkoxy group, an alkenyloxy group, an aryloxy group, an aralkyloxy group, an alkylcarbonyl group, an alkenylcarbonyl group, an arylcarbonyl group, an aralkylcarbonyl group, an alkylcarbonyloxy group, an alkenylcarbonyloxy group, an arylcarbonyloxy group, an aralkylcarbonyloxy group, an alkyloxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an aralkyloxycarbonyl group, an alkylamino group, a di(alkyl)amino group, an alkenylamino group, an alkylalkenylamino group, an alkylcarbonylamino group, an alkenylcarbonylamino group, an alkylcarbamoyl group, and an alkenylcarbamoyl group; or (3) An aryl group which may be substituted with a group selected from the group consisting of a halogen atom, a nitro group, a cyano group, a hydroxy group, an amino group, an alkyl group, an alkenyl group, an aryl group, an aralkyl group, an alkyl-substituted aryl group, an alkenyl-substituted aryl group, an alkoxy group, an alkenyloxy group, an aryloxy group, an aralkyloxy group, an alkylcarbonyl group, an alkenylcarbonyl group, an arylcarbonyl group, an aralkylcarbonyl group, an alkylcarbonyloxy group, an alkenylcarbonyloxy group, an arylcarbonyloxy group, an aralkylcarbonyloxy group, an alkyloxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an aralkyloxycarbonyl group, an alkylamino group, a di(alkyl)amino group, an alkenylamino group, an alkylalkenylamino group, an alkylcarbonylamino group, an alkenylcarbonylamino group, an alkylcarbamoyl group, and an alkenylcarbamoyl group. Represents.
[0029] The above R yrepresents an aryl group which may be substituted with a group selected from the group consisting of a halogen atom, a nitro group, a cyano group, a hydroxy group, an amino group, an aryl group, an alkyl-substituted aryl group, an alkenyl-substituted aryl group, an alkoxy group, an alkenyloxy group, an aryloxy group, an aralkyloxy group, an alkylcarbonyl group, an alkenylcarbonyl group, an arylcarbonyl group, an aralkylcarbonyl group, an alkylcarbonyloxy group, an alkenylcarbonyloxy group, an arylcarbonyloxy group, an aralkylcarbonyloxy group, an alkyloxycarbonyl group, an alkenyloxycarbonyl group, an aryloxycarbonyl group, an aralkyloxycarbonyl group, an alkylamino group, a di(alkyl)amino group, an alkenylamino group, an alkylalkenylamino group, an alkylcarbonylamino group, an alkenylcarbonylamino group, an alkylcarbamoyl group, and an alkenylcarbamoyl group.
[0030] The above R x and R y In the above, the halogen atom is preferably a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom.
[0031] The above R x and R y In the above, the alkyl group may be the same as the alkyl group in R.
[0032] The above R x and R y In the above, the alkenyl group may be the same as the alkenyl group in R.
[0033] The above R x and R y In the above, the aryl group may be the same as the aryl group in R.
[0034] The above R x and R yIn the above formula, the aralkyl group refers to an alkyl group substituted with one or more (preferably one) aryl groups. The number of carbon atoms in the aralkyl group is preferably 7 to 19, and particularly preferably 7 to 11. Examples of the aralkyl group include a benzyl group, a phenethyl group, a hydrocinnamyl group, an α-methylbenzyl group, an α-cumyl group, a 1-naphthylmethyl group, and a 2-naphthylmethyl group.
[0035] The above R x and R y In the above, the alkyl-substituted aryl group refers to an aryl group substituted with one or more alkyl groups. The number of carbon atoms in the alkyl-substituted aryl group is preferably 7 to 19, and particularly preferably 7 to 11. Examples of the alkyl-substituted aryl group include a 4-methylphenyl group, a 3-methylphenyl group, a 2-methylphenyl group, a 2,4-dimethylphenyl group, a 3,5-dimethylphenyl group, a 2,4,6-trimethylphenyl group, a 4-ethylphenyl group, a 3-ethylphenyl group, and a 2-ethylphenyl group.
[0036] The above R x and R y In the above, the alkenyl-substituted aryl group refers to an aryl group substituted with one or more alkenyl groups. The number of carbon atoms in the alkenyl-substituted aryl group is preferably 8 to 20, and particularly preferably 8 to 12. Examples of the alkenyl-substituted aryl group include a 4-vinylphenyl group, a 3-vinylphenyl group, a 2-vinylphenyl group, a 2,4-divinylphenyl group, a 3,5-divinylphenyl group, a 4-isopropenylphenyl group, a 3-isopropenylphenyl group, a 2-isopropenylphenyl group, and a 4-allylphenyl group.
[0037] The above R x and R y In the above, an alkoxy group is a monovalent group formed by bonding an alkyl group to an oxygen atom (i.e., R s1 -O-(R s1means a group represented by an alkyl group). The number of carbon atoms in the alkoxy group is preferably 1 to 18, more preferably 1 to 10, and further preferably 1 to 6. Examples of the alkoxy group include a methoxy group, an ethoxy group, a propyloxy group, an isopropyloxy group, a butyloxy group, an isobutyloxy group, a sec-butyloxy group, and a tert-butyloxy group.
[0038] The above R x and R y In the above, the alkenyloxy group is a monovalent group in which an alkenyl group is bonded to an oxygen atom (i.e., R s2 -O-(R s2 means an alkenyl group). The number of carbon atoms in the alkenyloxy group is preferably 2 to 18, more preferably 2 to 10, and further preferably 2 to 6. Examples of the alkenyloxy group include a vinyloxy group, a propenyloxy group (an allyloxy group, a 1-propenyloxy group, an isopropenyloxy group), and the like.
[0039] The above R x and R y In the above, an aryloxy group is a monovalent group formed by bonding an aryl group to an oxygen atom (i.e., R s3 -O-(R s3 means a group represented by an aryl group). The number of carbon atoms in the aryloxy group is preferably 6 to 18, and particularly preferably 6 to 10. Examples of the aryloxy group include a phenoxy group, a 1-naphthoxy group, and a 2-naphthoxy group.
[0040] The above R x and R y In the above, the aralkyloxy group is a monovalent group formed by bonding an aralkyl group to an oxygen atom (i.e., R s4 -O-(R s4 means an aralkyl group). The number of carbon atoms in the aralkyloxy group is preferably 7 to 19, and particularly preferably 7 to 11. Examples of the aralkyloxy group include a benzyloxy group and an α-methylbenzyloxy group.
[0041] The above R x and R y In the above, an alkylcarbonyl group is a monovalent group in which an alkyl group is bonded to one side of a carbonyl group (i.e., R s1 -C(=O)-(R s1 means a group represented by an alkyl group). The number of carbon atoms in the alkylcarbonyl group is preferably 2 to 19, more preferably 2 to 11, and further preferably 2 to 7. Examples of the alkylcarbonyl group include an acetyl group, a propanoyl group, and a butanoyl group.
[0042] The above R x and R y In the above, the alkenylcarbonyl group is a monovalent group in which an alkenyl group is bonded to one side of a carbonyl group (i.e., R s2 -C(=O)-(R s2 means an alkenyl group). The number of carbon atoms in the alkenylcarbonyl group is preferably 3 to 19, more preferably 3 to 11, and further preferably 3 to 7. Examples of the alkenylcarbonyl group include a vinylcarbonyl group, a propenylcarbonyl group (allylcarbonyl group, 1-propenylcarbonyl group, isopropenylcarbonyl group), and the like.
[0043] The above R x and R y In the above, an arylcarbonyl group is a monovalent group in which an aryl group is bonded to one side of a carbonyl group (i.e., R s3 -C(=O)-(R s3 means a group represented by an aryl group). The number of carbon atoms in the arylcarbonyl group is preferably 7 to 19, and particularly preferably 7 to 11. Examples of the arylcarbonyl group include a benzoyl group, a 1-naphthoyl group, and a 2-naphthoyl group.
[0044] The above R x and R y In the above, the aralkylcarbonyl group is a monovalent group in which an aralkyl group is bonded to one side of a carbonyl group (i.e., R s4 -C(=O)-(R s4means an aralkyl group). The number of carbon atoms in the aralkylcarbonyl group is preferably 7 to 19, and particularly preferably 7 to 11. Examples of the aralkylcarbonyl group include a benzylcarbonyl group and an α-methylbenzylcarbonyl group.
[0045] The above R x and R y In the above, an alkylcarbonyloxy group is a monovalent group formed by bonding an alkylcarbonyl group to an oxygen atom (i.e., R s1 -C(=O)-O-(R s1 means a group represented by an alkyl group). The number of carbon atoms in the alkylcarbonyloxy group is preferably 2 to 19, more preferably 2 to 11, and still more preferably 2 to 7. Examples of the alkylcarbonyloxy group include an acetyloxy group, a propanoyloxy group, and a butanoyloxy group.
[0046] The above R x and R y In the above, the alkenylcarbonyloxy group is a monovalent group formed by bonding an alkenylcarbonyl group to an oxygen atom (i.e., R s2 -C(=O)-O-(R s2 means an alkenyl group). The number of carbon atoms in the alkenylcarbonyloxy group is preferably 3 to 19, more preferably 3 to 11, and still more preferably 3 to 7. Examples of the alkenylcarbonyloxy group include a vinylcarbonyloxy group, a propenylcarbonyloxy group (an allylcarbonyloxy group, a 1-propenylcarbonyloxy group, an isopropenylcarbonyloxy group), and the like.
[0047] The above R x and R y In the above, an arylcarbonyloxy group is a monovalent group formed by bonding an arylcarbonyl group to an oxygen atom (i.e., R s3 -C(=O)-O-(R s3means a group represented by an aryl group). The number of carbon atoms in the arylcarbonyloxy group is preferably 7 to 19, and particularly preferably 7 to 11. Examples of the arylcarbonyloxy group include a benzoyloxy group, a 1-naphthoyloxy group, and a 2-naphthoyloxy group.
[0048] The above R x and R y In the above, the aralkylcarbonyloxy group is a monovalent group formed by bonding an aralkylcarbonyl group to an oxygen atom (i.e., R s4 -C(=O)-O-(R s4 means an aralkyl group). The number of carbon atoms in the aralkylcarbonyl group is preferably 7 to 19, and particularly preferably 7 to 11. Examples of the aralkylcarbonyloxy group include a benzylcarbonyloxy group and an α-methylbenzylcarbonyloxy group.
[0049] The above R x and R y In the above, the alkyloxycarbonyl group is a monovalent group in which an alkoxy group is bonded to one side of a carbonyl group (i.e., R s1 -OC(=O)-(R s1 means a group represented by an alkyl group). The number of carbon atoms in the alkyloxycarbonyl group is preferably 2 to 19, more preferably 2 to 11, and still more preferably 2 to 7. Examples of the alkyloxycarbonyl group include a methoxycarbonyl group, an ethoxycarbonyl group, a propoxycarbonyl group, and an isopropoxycarbonyl group.
[0050] The above R x and R y In the above, the alkenyloxycarbonyl group is a monovalent group in which an alkenyloxy group is bonded to one side of a carbonyl group (i.e., R s2 -OC(=O)-(R s2means an alkenyl group). The number of carbon atoms in the alkenyloxycarbonyl group is preferably 3 to 19, more preferably 3 to 11, and further preferably 3 to 7. Examples of the alkenyloxycarbonyl group include a vinyloxycarbonyl group, a propenyloxycarbonyl group (an allyloxycarbonyl group, a 1-propenyloxycarbonyl group, an isopropenyloxycarbonyl group), and the like.
[0051] The above R x and R y In the above, the aryloxycarbonyl group is a monovalent group in which an aryloxy group is bonded to one side of a carbonyl group (i.e., R s3 -OC(=O)-(R s3 means a group represented by an aryl group). The number of carbon atoms in the aryloxycarbonyl group is preferably 7 to 19, and particularly preferably 7 to 11. Examples of the aryloxycarbonyl group include a phenoxycarbonyl group, a 1-naphthoxycarbonyl group, and a 2-naphthoxycarbonyl group.
[0052] The above R x and R y In the above, the aralkyloxycarbonyl group is a monovalent group in which an aralkyloxy group is bonded to one side of a carbonyl group (i.e., R s4 -OC(=O)-(R s4 means an aralkyl group). The number of carbon atoms in the aralkylcarbonyl group is preferably 7 to 19, and particularly preferably 7 to 11. Examples of the aralkyloxycarbonyl group include a benzyloxycarbonyl group and an α-methylbenzyloxycarbonyl group.
[0053] The above R x and R y In the above, an alkylamino group is an amino group mono-substituted with an alkyl group (i.e., R s1 -NH-(R s1means a group represented by an alkyl group). The number of carbon atoms in the alkylamino group is preferably 1 to 18, more preferably 1 to 10, and further preferably 1 to 6. Examples of the alkylamino group include an N-methylamino group, an N-ethylamino group, and an N-propylamino group.
[0054] The above R x and R y In the formula, a di(alkyl)amino group is an amino group di-substituted with an alkyl group (i.e., (R s1 -)2N-(R s1 are independently an alkyl group). The number of carbon atoms in the di(alkyl)amino group is preferably 2 to 18, more preferably 2 to 10, and further preferably 2 to 6. Examples of the di(alkyl)amino group include an N,N-dimethylamino group, an N,N-diethylamino group, an N-ethyl-N-methylamino group, and an N,N-dipropylamino group.
[0055] The above R x and R y In the formula (I), an alkenylamino group is an amino group mono-substituted with an alkenyl group (i.e., R s2 -NH-(R s2 means an alkenyl group). The number of carbon atoms in the alkenylamino group is preferably 2 to 19, more preferably 2 to 11, and further preferably 2 to 7. Examples of the alkenylamino group include an N-vinylamino group and an N-allylamino group.
[0056] The above R x and R y In the formula (I), an alkylalkenylamino group is an amino group substituted with both an alkyl group and an alkenyl group (i.e., (R s1 -)(R s2 -)N-(R s1 is an alkyl group, R s2means a group represented by an alkenyl group). The number of carbon atoms in the alkylalkenylamino group is preferably 3 to 19, more preferably 3 to 11, and further preferably 3 to 7. Examples of the alkylalkenylamino group include an N-methyl-N-vinylamino group and an N-allyl-N-methylamino group.
[0057] The above R x and R y In the formula (I), an alkylcarbonylamino group is an amino group mono-substituted with an alkylcarbonyl group (i.e., R s1 -C(=O)-NH-(R s1 means a group represented by an alkyl group). The number of carbon atoms in the alkylcarbonylamino group is preferably 2 to 19, more preferably 2 to 11, and further preferably 2 to 7. Examples of the alkylcarbonylamino group include an N-acetylamino group, an N-propanoylamino group, and an N-butanoylamino group.
[0058] The above R x and R y In the formula (I), an alkenylcarbonylamino group is an amino group mono-substituted with an alkenylcarbonyl group (i.e., R s2 -C(=O)-NH-(R s2 means a group represented by an alkenyl group). The number of carbon atoms in the alkenylcarbonylamino group is preferably 3 to 20, more preferably 2 to 11, and further preferably 2 to 7. Examples of the alkenylcarbonylamino group include an N-vinylcarbonylamino group, an N-allylcarbonylamino group, an N-(1-propenylcarbonyl)amino group, and an N-isopropenylcarbonylamino group.
[0059] The above R x and R y In the formula (I), an alkylcarbamoyl group is a carbamoyl group mono-substituted with an alkyl group (i.e., R s1 -NH-C(=O)-(R s1means a group represented by an alkyl group). The number of carbon atoms in the alkylcarbamoyl group is preferably 2 to 19, more preferably 2 to 11, and still more preferably 2 to 7. Examples of the alkylcarbamoyl group include an N-methylcarbamoyl group, an N-ethylcarbamoyl group, and an N-propylcarbamoyl group.
[0060] The above R x and R y In the formula (I), an alkenylcarbamoyl group is a carbamoyl group mono-substituted with an alkenyl group (i.e., R s2 -NH-C(=O)-(R s2 means a group represented by an alkenyl group). The number of carbon atoms in the alkenylcarbamoyl group is preferably 3 to 20, more preferably 3 to 12, and still more preferably 3 to 8. Examples of the alkenylcarbamoyl group include an N-vinylcarbamoyl group and an N-allylcarbamoyl group.
[0061] In one embodiment, each R is preferably, (1) Halogen atoms, -NO2, -CN, -COH, -OH, -NH2, -COOH, -R y , -COR x , -OR x , -NHR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, and -NHCOR x an alkyl group optionally substituted with a group selected from (2) Halogen atoms, -NO2, -CN, -COH, -OH, -NH2, -COOH, -R y , -COR x , -OR x , -NHR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, and -NHCORx an alkenyl group optionally substituted with a group selected from (3) Halogen atoms, -NO2, -CN, -COH, -OH, -NH2, -COOH, -R x , -COR x , -OR x , -NHR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, and -NHCOR x (R x and R y as above).
[0062] In one embodiment, each R is preferably independently (1)-R y , -COR x , -OR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, and -NHCOR x an alkyl group optionally substituted with a group selected from (2)-R y , -COR x , -OR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, and -NHCOR x an alkenyl group optionally substituted with a group selected from (3)-R x , -COR x , -OR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHRx , -CON(R x )2, and -NHCOR x (R x and R y as above).
[0063] In one embodiment, each R is preferably, independently (1) (a) an aryl group optionally substituted with a group selected from an alkyl group, an alkenyl group, an alkoxy group, an alkenyloxy group, an alkylcarbonyl group, an alkenylcarbonyl group, and a di(alkyl)amino group, (b) an alkoxy group, (c) an alkenyloxy group, (d) an alkylcarbonyl group, (e) an alkenylcarbonyl group, (f) an alkylcarbonyloxy group, (g) an alkenylcarbonyloxy group, (h) an alkyloxycarbonyl group, (i) an alkenyloxycarbonyl group, (j) a di(alkyl)amino group, (k) an alkylcarbonylamino group, (l) an alkenylcarbonylamino group, (m) an alkylcarbamoyl group, and (n) an alkenylcarbamoyl group; (2) (a) an aryl group optionally substituted with a group selected from an alkyl group, an alkenyl group, an alkoxy group, an alkenyloxy group, an alkylcarbonyl group, an alkenylcarbonyl group, and a di(alkyl)amino group, (b) an alkoxy group, (c) an alkenyloxy group, (d) an alkylcarbonyl group, (e) an alkenylcarbonyl group, (f) an alkylcarbonyloxy group, (g) an alkenylcarbonyloxy group, (h) an alkyloxycarbonyl group, (i) an alkenyloxycarbonyl group, (j) a di(alkyl)amino group, (k) an alkylcarbonylamino group, (l) an alkenylcarbonylamino group, (m) an alkylcarbamoyl group, and (n) an alkenylcarbamoyl group; or (3) (a) an aryl group which may be substituted with a group selected from an alkyl group and an alkenyl group, (b) an alkyl group, (c) an alkenyl group, (d) an alkoxy group, (e) an alkenyloxy group, (f) an alkylcarbonyl group, (g) an alkenylcarbonyl group, (h) an alkylcarbonyloxy group, (i) an alkenylcarbonyloxy group, (j) an alkyloxycarbonyl group, (k) an alkenyloxycarbonyl group, (l) a di(alkyl)amino group, (m) an alkylcarbonylamino group, (n) an alkenylcarbonylamino group, (o) an alkylcarbamoyl group, and (p) an aryl group which may be substituted with a group selected from an alkenylcarbamoyl group.
[0064] In one embodiment, R is particularly preferably, (1) an alkyl group optionally substituted with a group selected from (a) an aryl group, (b) an alkoxy group, (c) an alkenyloxy group, (d) an alkylcarbonyl group, (e) an alkenylcarbonyl group, (f) an alkylcarbonyloxy group, (g) an alkenylcarbonyloxy group, (h) an alkyloxycarbonyl group, and (i) an alkenyloxycarbonyl group; (2) an alkenyl group optionally substituted with a group selected from (a) an aryl group, (b) an alkoxy group, (c) an alkenyloxy group, (d) an alkylcarbonyl group, (e) an alkenylcarbonyl group, (f) an alkylcarbonyloxy group, (g) an alkenylcarbonyloxy group, (h) an alkyloxycarbonyl group, and (i) an alkenyloxycarbonyl group; or (3) An aryl group optionally substituted with a group selected from (a) an aryl group, (b) an alkyl group, (c) an alkenyl group, (d) an alkoxy group, (e) an alkenyloxy group, (f) an alkylcarbonyl group, (g) an alkenylcarbonyl group, (h) an alkylcarbonyloxy group, (i) an alkenylcarbonyloxy group, (j) an alkyloxycarbonyl group, and (k) an alkenyloxycarbonyl group.
[0065] In formula (1-1), R 1 and R 2At least one of the above contains an ethylenically unsaturated bond. 1 and R 2 Among these, the one containing an ethylenically unsaturated bond is preferably -R z , -OR z , -COR z , -COOR z , -CONHR z , -CONR z 2, -SR z , -SOR z , and -SO2R z Here, R z represents an alkyl group having a substituent containing an ethylenically unsaturated bond, an alkenyl group which may have a substituent, or an aryl group having a substituent containing an ethylenically unsaturated bond.
[0066] R z The alkyl group, alkenyl group, and aryl group in R may be the same as the alkyl group, alkenyl group, and aryl group in R. z Examples of the "substituent containing an ethylenically unsaturated bond" in the "alkyl group having a substituent containing an ethylenically unsaturated bond" in the above formula include those containing an ethylenically unsaturated bond among the "substituents" in the "alkyl group which may have a substituent" represented by R. z Examples of the "substituent" in the "optionally substituted alkenyl group" in the formula (I) include the same as the "substituent" in the "optionally substituted alkenyl group" represented by R. z Examples of the "substituent containing an ethylenically unsaturated bond" in the "aryl group having a substituent containing an ethylenically unsaturated bond" in the above formula include those containing an ethylenically unsaturated bond among the "substituents" in the "aryl group which may have a substituent" represented by R.
[0067] R containing an ethylenically unsaturated bond 1 and R 2 As for -R z , -COR z , or -COORz is preferred;-COR z , or -COOR z is more preferred;-COOR z is more preferred.
[0068] Among them, R containing an ethylenically unsaturated bond 1 and R 2 As the group, the group represented by the following formula (1-2) is particularly preferable. 1 and R 2 At least one of R is preferably represented by the following formula (1-2). 1 and R 2 Only one of R may be a group represented by the following formula (1-2): 1 and R 2 may both be groups represented by the following formula (1-2).
[0069] [ka]
[0070] (In formula (1-2), R 15 , R 16 and R 17 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms; p1 represents an integer of 0 to 10; * represents a bond.)
[0071] In formula (1-2), R 15 , R 16 and R 17 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms. The aliphatic hydrocarbon group may be an aliphatic unsaturated hydrocarbon group, but is preferably an aliphatic saturated hydrocarbon group. Examples of the aliphatic hydrocarbon group having 1 to 3 carbon atoms include an alkyl group having 1 to 3 carbon atoms. Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and a 2-propyl group, and a methyl group is preferred. Among these, R 15 is preferably a hydrogen atom or a methyl group, and R 16 and R 17is more preferably a hydrogen atom.
[0072] In formula (1-2), p1 represents an integer of 0 to 10, preferably an integer of 1 to 7, more preferably an integer of 2 to 5, and further preferably 2.
[0073] R 1 and R 2 may be bonded together to form a non-aromatic ring which may have a substituent. The non-aromatic ring means a ring other than an aromatic ring having aromaticity throughout the ring. Thus, the non-aromatic ring includes both a non-aromatic carbocycle having only carbon atoms as ring constituent atoms, and a non-aromatic heterocycle having heteroatoms such as oxygen atoms, nitrogen atoms, and sulfur atoms as ring constituent atoms in addition to carbon atoms. The non-aromatic ring may be a monocyclic non-aromatic ring, a polycyclic non-aromatic ring, or a fused ring having aromaticity partially condensed to a part of the ring. The non-aromatic ring may be a saturated ring consisting of only a single bond, or an unsaturated ring having a double bond in addition to a single bond. The non-aromatic ring is preferably a 3-21 membered non-aromatic ring, more preferably a 4-18 membered non-aromatic ring, and even more preferably a 5-14 membered non-aromatic ring.
[0074] R 1 and R 2 Specific preferred examples of the "non-aromatic ring" in the "non-aromatic ring which may have a substituent" formed by the above formula include monocyclic non-aromatic carbon rings such as a cyclobutane ring, a cyclopentane ring, a cyclohexane ring, a cycloheptane ring, a cyclooctane ring, a cyclononane ring, a cyclodecane ring, a cycloundecane ring, a cyclododecane ring, a cyclopentene ring, a cyclopentadiene ring, a cyclohexene ring, a 1,3-cyclohexadiene ring, and a 1,4-cyclohexadiene ring; and monocyclic non-aromatic heterocycles such as a 1,3-dioxane ring, a 1,3-dioxolane ring, a tetrahydropyran ring, a tetrahydrofuran ring, a 2,3-dihydro-2H-pyran ring, a 4,5-dihydro-2H-pyran ring, a 2H-pyran ring, a 4H-pyran ring, a 2,3-dihydrofuran ring, and a 2,5-dihydrofuran ring.
[0075] R 1 and R2 The "substituent" in the "non-aromatic ring which may have a substituent" formed by is not particularly limited, and examples thereof include a halogen atom, -NO2, -CN, -COH, -OH, -SH, -NH2, -COOH, -R x , -COR x , -OR x , -SR x , -SOR x , -SO2R x , -NHR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, -NHCOR x , ═O, or other monovalent or divalent substituents (R x as above).
[0076] In formula (1-1), R 1 and R 2 are bonded to form a non-aromatic ring which may have a substituent, the formula (a1): [ka]
[0077] The structure represented by the above formula is preferably represented by the following formulas (aa-1) to (aa-10).
[0078] [ka]
[0079] (In formulas (aa-1) to (aa-10), A 1 and A 2 are each independently -CO- or -CR a R b - indicates; B 1 and B. 2 Each independently represents -O-, -NR c -or-CRa R b - indicates; C 1 is -O- or -NR c - indicates; R a and R b each independently represents a hydrogen atom or a substituent, Two R's bonded to adjacent carbon atoms a may be bonded together to form a non-aromatic ring which may have a substituent, or an aromatic ring which may have a substituent, R attached to the same carbon atom a and R b may be joined together to form a non-aromatic ring which may have a substituent; R c each independently represents a hydrogen atom, an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent. However, in formula (aa-1), A 1 , A 2 , B 1 , B 2 , R a and R b At least one of A contains an ethylenically unsaturated bond. 1 , A 2 , C 1 , R a and R b At least one of A contains an ethylenically unsaturated bond. 1 , A 2 , B 1 , R a and R b At least one of the above contains an ethylenically unsaturated bond.
[0080] In formulas (aa-1) to (aa-10), A 1 and A 2 are each independently -CO- or -CR a R b -; preferably -CR a Rb -It is.
[0081] In formulas (aa-1) to (aa-10), B 1 and B. 2 Each independently represents -O-, -NR c -or-CR a R b -; preferably -O- or -CR a R b -It is.
[0082] In formulae (aa-1) to (aa-10), C 1 is -O- or -NR c -; preferably -O-.
[0083] In formulas (aa-1) to (aa-10), R a and R b Each of R 1 and R 2 each independently represents a hydrogen atom or a substituent. a may be bonded together to form a non-aromatic ring which may have a substituent, or an aromatic ring which may have a substituent. a and R b may be bonded together to form a non-aromatic ring which may have a substituent.
[0084] R a and R b or 2 R aPreferred specific examples of the "non-aromatic ring" in the "non-aromatic ring which may have a substituent" formed by the formula (I) include monocyclic non-aromatic saturated carbon rings such as a cyclobutane ring, a cyclopentane ring, a cyclohexane ring, a cycloheptane ring, a cyclooctane ring, a cyclononane ring, a cyclodecane ring, a cycloundecane ring, and a cyclododecane ring; a bicyclo[2.2.1]heptane ring (norbornane ring), a bicyclo[4.4.0]decane ring (decalin ring), a bicyclo[5.3.0]decane ring, a bicyclo[4.3.0]nonane ring (hydrindane ring), a bicyclo[3.2.1]octane ring, a bicyclo[5.4.0]undecane ring, a bicyclo[3.3.0]octane ring, a bicyclo[3.3.1]nonane ring, a tricyclo[5.2.1.0 2,6 ] Decane ring (tetrahydrodicyclopentadiene ring), tricyclo[3.3.1.1 3,7 ]Decane ring (adamantane ring), tricyclo[6.2.1.0 2,7 ]Undecane ring and other bicyclic or higher non-aromatic saturated carbocyclic rings; and non-aromatic carbocyclic rings in which an aromatic ring (such as a benzene ring or a naphthalene ring) is condensed to a part of the ring, such as an indane ring, an indene ring, a tetralin ring, a 1,2-dihydronaphthalene ring, a 1,4-dihydronaphthalene ring, a fluorene ring, a 9,10-dihydroanthracene ring, or a 9,10-dihydrophenanthrene ring.
[0085] R a and R b The "substituent" represented by and two R a The "substituent" in the "optionally substituted aromatic ring" formed by is not particularly limited, and examples thereof include a halogen atom, -NO2, -CN, -COH, -OH, -SH, -NH2, -COOH, -R x , -COR x , -OR x , -SR x , -SOR x , -SO2R x , -NHR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x)2, -NHCOR x (R x as above).
[0086] The aromatic ring means a ring that follows the Huckel rule, in which the number of electrons contained in the π electron system on the ring is 4p+2 (p is a natural number). The aromatic ring includes both an aromatic carbocycle having only carbon atoms as ring constituent atoms, and an aromatic heterocycle having heteroatoms such as oxygen atoms, nitrogen atoms, and sulfur atoms as ring constituent atoms in addition to carbon atoms. The aromatic ring may be a monocyclic aromatic ring or a polycyclic aromatic ring. In one embodiment, the aromatic ring is preferably a 5- to 14-membered aromatic ring, more preferably a 6- to 14-membered aromatic ring, and even more preferably a 6- to 10-membered aromatic ring. Two R a Examples of the "aromatic ring" in the "optionally substituted aromatic ring" formed by include a benzene ring, a naphthalene ring, an anthracene ring, and a phenanthrene ring.
[0087] R a and R b or 2 R a The "substituent" in the "non-aromatic ring which may have a substituent" formed by is not particularly limited, and examples thereof include a halogen atom, -NO2, -CN, -COH, -OH, -SH, -NH2, -COOH, -R x , -COR x , -OR x , -SR x , -SOR x , -SO2R x , -NHR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, -NHCOR x , ═O, or other monovalent or divalent substituents (R x as above).
[0088] R a and R bIn one embodiment, each of these independently represents preferably a hydrogen atom, a halogen atom, a nitro group, a cyano group, an alkyl group, an alkenyl group, an aryl group, an aralkyl group, an alkyl-substituted aryl group, an alkenyl-substituted aryl group, an alkoxy group, an alkenyloxy group, an aryloxy group, an aralkyloxy group, an alkylcarbonyl group, an alkenylcarbonyl group, an arylcarbonyl group, an aralkylcarbonyl group, an alkylcarbonyloxy group, an alkenylcarbonyloxy group, an arylcarbonyloxy group, an aralkylcarbonyloxy group, an alkyloxycarbonyl group, is preferably a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, an aralkyl group, an alkyl-substituted aryl group, an alkenyl-substituted aryl group, an alkoxy group, an alkenyloxy group, an aryloxy group, or an aralkyloxy group; more preferably a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, an aralkyl group, an alkyl-substituted aryl group, or an alkenyl-substituted aryl group; and particularly preferably a hydrogen atom or an alkyl group.
[0089] In formulas (aa-1) to (aa-10), R c each independently represents a hydrogen atom, an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent.
[0090] R c The "substituents" in the "optionally substituted alkyl group" shown in c The "substituent" in the "alkenyl group which may have a substituent" is not particularly limited, and examples thereof include a halogen atom, -NO2, -CN, -COH, -OH, -SH, -NH2, -COOH, -R y , -COR x , -OR x , -SR x , -SOR x , -SO2R x , -NHR x , -N(R x )2, -COORx , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, -NHCOR x (R x and R y as above).
[0091] R c The "substituent" in the "aryl group which may have a substituent" represented by is not particularly limited, and examples thereof include a halogen atom, -NO2, -CN, -COH, -OH, -SH, -NH2, -COOH, -R x , -COR x , -OR x , -SR x , -SOR x , -SO2R x , -NHR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, -NHCOR x (R x as above).
[0092] R c In one embodiment, each independently is preferably a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, an aralkyl group, an alkyl-substituted aryl group, or an alkenyl-substituted aryl group; particularly preferably a hydrogen atom or an alkyl group.
[0093] In formula (1-1), R 1 and R 2 Since at least one of them contains an ethylenically unsaturated bond, R 1 and R 2 The "non-aromatic ring which may have a substituent" formed by A also contains an ethylenically unsaturated bond. 1 , A 2 , B 1 , B2 , R a and R b At least one of A contains an ethylenically unsaturated bond. 1 , A 2 , C 1 , R a and R b At least one of A contains an ethylenically unsaturated bond. 1 , A 2 , B 1 , R a and R b At least one of them contains an ethylenically unsaturated bond.
[0094] In formula (1-1), formula (a1): [ka]
[0095] Specific examples of the structure represented by the formula include structures represented by the following formulas (a-1) to (a-131).
[0096] [ka]
[0097] [ka]
[0098] [ka]
[0099] [ka]
[0100] [ka]
[0101] [ka]
[0102] [ka]
[0103] [ka]
[0104] -tetravalent organic group X 1 Description of - In formula (1), X 1 represents a tetravalent organic group. This tetravalent organic group X 1 It is preferable that the divalent organic group Y in formula (1) contains at least two benzene rings and a divalent group represented by formula (1-1) that connects the two benzene rings. Hereinafter, the "structure containing at least two benzene rings and a divalent group represented by formula (1-1) that connects the two benzene rings" may be referred to as the "specific structure". 1 When the specific structure is included, the tetravalent organic group X 1 On the other hand, the divalent organic group Y 1 does not contain a specific structure, a tetravalent organic group X 1 includes specific structures.
[0105] X 1 If X contains a specific structure, 1 It is preferable that the tetravalent organic group X contains one or more structures selected from the group consisting of a structure represented by the following formula (X1-1) and a structure represented by the following formula (X1-2). 1 may contain only one or more structures selected from the group consisting of a structure represented by the following formula (X1-1) and a structure represented by the following formula (X1-2).
[0106] [ka]
[0107] (In the formula (X1-1) and the formula (X1-2), R 11 and R 12 represents a hydrogen atom, -CN, -NO2, -COH, -R, -OR, -COR, -COOR, -CONHR, -CONR2, -SR, -SOR, or -SOR, and R 11 and R 12 At least one of R contains an ethylenically unsaturated bond, 11 and R 12 may be bonded together to form a non-aromatic ring which may have a substituent; each R independently represents an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent; R 13 and R 14 each independently represents a substituent; L 1 represents a divalent organic group; n 11 and n 12 each independently represents an integer of 0 to 3; n 13 and n 14 Each independently represents an integer of 0 or more and 2 or less. * represents a bond.)
[0108] In formula (X1-1) and formula (X1-2), R 11 and R 12 represents a hydrogen atom, -CN, -NO2, -COH, -R, -OR, -COR, -COOR, -CONHR, -CONR2, -SR, -SOR, or -SOR. R is as described above. 11 and R 12 At least one of R contains an ethylenically unsaturated bond. 11 and R 12 R may be bonded together to form a non-aromatic ring which may have a substituent. 11 and R 12 These R may be the same or different. 11 and R 12 R in formula (1-1), including preferred ranges and examples thereof 1and R 2 is the same as:
[0109] In formula (X1-1) and formula (X1-2), R 13 and R 14 R each independently represents a substituent. 13 and R 14 The "substituent" represented by is not particularly limited, but examples thereof include halogen atoms, -NO2, -CN, -COH, -OH, -SH, -NH2, -COOH, -R x , -COR x , -OR x , -SR x , -SOR x , -SO2R x , -NHR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, -NHCOR x (R x as above).
[0110] R 13 and R 14 are each independently, preferably, an alkyl group, an alkenyl group, an aryl group, an aralkyl group, an alkyl-substituted aryl group, an alkenyl-substituted aryl group, an alkoxy group, an alkenyloxy group, an aryloxy group, or an aralkyloxy group; more preferably, an alkyl group, an alkenyl group, an aryl group, an aralkyl group, an alkyl-substituted aryl group, or an alkenyl-substituted aryl group; further preferably, an alkyl group; still more preferably, an alkyl group having 4 or more carbon atoms; still more preferably, an alkyl group having 4 to 14 carbon atoms; and particularly preferably, a tert-butyl group.
[0111] In formula (X1-2), L 1 represents a divalent organic group. 1is preferably a divalent aliphatic hydrocarbon group which may have a substituent, more preferably a divalent aliphatic saturated hydrocarbon group which may have a substituent, further preferably an alkylene group which may have a substituent, and particularly preferably a methylene group which may have a substituent.
[0112] L 1 The "substituent" in the "divalent aliphatic hydrocarbon group which may be substituted", the "substituent" in the "divalent aliphatic saturated hydrocarbon group which may be substituted", the "substituent" in the "alkylene group which may be substituted", and the "substituent" in the "methylene group which may be substituted" are not particularly limited, and examples thereof include halogen atoms, -NO2, -CN, -COH, -OH, -SH, -NH2, -COOH, -R y , -COR x , -OR x , -SR x , -SOR x , -SO2R x , -NHR x , -N(R x )2, -COOR x , -OCOR x , -CONH2, -CONHR x , -CON(R x )2, -NHCOR x monovalent substituents such as oxo, ═CR 11 R 12 (R 11 , R 12 , R x and R y is as described above). Among these, a divalent substituent is preferred.
[0113] Furthermore, L 1 is preferably a methylene group which may be substituted by a divalent substituent, and more preferably an oxo group or =CR 11 R 12 A methylene group optionally substituted with is more preferred.
[0114] In formula (X1-1), n 11 and n 12each independently represents an integer of 0 or more and 3 or less, preferably 0 or 1, and more preferably 0.
[0115] In formula (X1-2), n 13 and n 14 each independently represents an integer of 0 or more and 2 or less, is preferably 0 or 1, and is more preferably 0.
[0116] In formula (X1-2), L 1 represents a methylene group having no substituent, a methylene group substituted with an oxo group (i.e., -C(=O)-), and =CR 11 R 12 methylene group substituted with (i.e., -C(=CR 11 R 12 )-) is preferred. Therefore, the structure represented by formula (X1-2) is preferably represented by formula (X1-2-1), formula (X1-2-2) or formula (X1-2-3). In formula (X1-2-3), two R 11 may be the same or different. Also, two R 12 may be the same or different.
[0117] [ka]
[0118] (In formulas (X1-2-1) to (X1-2-3), each symbol is as defined above.)
[0119] In formula (1), the tetravalent organic group X 1 When X contains one or more structures selected from the group consisting of a structure represented by formula (X1-1) and a structure represented by formula (X1-2), 1 may contain any structure in combination with one or more structures selected from the group consisting of the structure represented by formula (X1-1) and the structure represented by formula (X1-2). 1contains only one or more structures selected from the group consisting of the structure represented by formula (X1-1) and the structure represented by formula (X1-2). That is, preferably, 1 is represented by formula (X1-1) or formula (X1-2).
[0120] In formula (1), Y 1 When X contains a specific structure (i.e., a structure containing at least two benzene rings and a divalent group represented by formula (1-1) connecting the two benzene rings), 1 may be a tetravalent organic group not containing a specific structure.
[0121] The number of carbon atoms of the tetravalent organic group not containing a specific structure is preferably 6 to 40. Examples of such tetravalent organic groups include organic groups containing an aromatic ring or a non-aromatic carbon ring having two pairs of two bonds at the ortho position to each other. Among them, it is preferable that the tetravalent organic group contains an aromatic ring. Examples of such tetravalent organic groups include the following groups (x-1) to (x-9). In addition, a group obtained by combining two or more of the following groups (x-1) to (x-9) may be used as the tetravalent organic group. Among them, the group (x-8) and the group (x-9) are more preferable. In the formula, * represents a bond.
[0122] [ka]
[0123] The above-mentioned groups (x-1) to (x-9) may have a substituent. Examples of the substituent include linear, branched, or cyclic alkyl groups having 1 to 10 carbon atoms, such as methyl, ethyl, propyl, and n-butyl groups; halogen atoms, such as fluorine, chlorine, and bromine; alkoxy groups having 1 to 10 carbon atoms, such as methoxy, ethoxy, and propoxy groups; hydroxy groups; and halogen-substituted alkyl groups, such as trifluoromethyl groups. The above-mentioned substituents may further have a substituent (hereinafter sometimes referred to as "secondary substituents"). The number of the substituents may be one or more.
[0124] -Divalent organic group Y 1 Description of - In formula (1), Y 1 represents a divalent organic group. This divalent organic group Y 1 It is preferable that the tetravalent organic group X in formula (1) contains a specific structure (i.e., a structure containing at least two benzene rings and a divalent group represented by formula (1-1) connecting the two benzene rings). 1 When the specific structure is included, the divalent organic group Y 1 On the other hand, the tetravalent organic group X in formula (1) may or may not contain a specific structure. 1 does not contain a specific structure, a divalent organic group Y 1 includes specific structures.
[0125] Y 1 When Y contains a specific structure, 1 It is preferable that the divalent organic group Y contains one or more structures selected from the group consisting of a structure represented by the following formula (Y1-1), a structure represented by the following formula (Y1-2), a structure represented by the following formula (Y1-3), and a structure represented by the following formula (Y1-4). 1 may contain only one or more structures selected from the group consisting of a structure represented by the following formula (Y1-1), a structure represented by the following formula (Y1-2), a structure represented by the following formula (Y1-3), and a structure represented by the following formula (Y1-4).
[0126] [ka]
[0127] (In the formulas (Y1-1), (Y1-2), (Y1-3) and (Y1-4), R 21 and R 22 represents a hydrogen atom, -CN, -NO2, -COH, -R, -OR, -COR, -COOR, -CONHR, -CONR2, -SR, -SOR, or -SOR, and R 21 and R 22 At least one of R contains an ethylenically unsaturated bond,21 and R 22 may be bonded together to form a non-aromatic ring which may have a substituent; each R independently represents an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent; R 23 and R 24 each independently represents a substituent; L 2 represents a divalent organic group; n 21 and n 22 each independently represents an integer of 0 to 4; n 23 and n 24 each independently represents an integer of 0 to 3; n 25は , an integer between 0 and 3; n 26 represents an integer between 0 and 5; n 27 represents an integer between 0 and 2; n 28 represents an integer of 0 to 4. * represents a bond.
[0128] In formulae (Y1-1) to (Y1-4), R 21 and R 22 represents a hydrogen atom, -CN, -NO2, -COH, -R, -OR, -COR, -COOR, -CONHR, -CONR2, -SR, -SOR, or -SOR. R is as described above. 21 and R 22 At least one of R contains an ethylenically unsaturated bond. 21 and R 22 R may be bonded together to form a non-aromatic ring which may have a substituent. 21 and R 22 These R may be the same or different. 21 and R 22 R in formula (1-1), including preferred ranges and examples thereof 1 and R 2 is the same as:
[0129] In formulae (Y1-1) to (Y1-4), R 23 and R 24Each of R independently represents a substituent. 23 and R 24 R in formulas (X1-1) to (X1-2), including preferred ranges and examples thereof 13 and R 14 is the same as:
[0130] In formula (Y1-2) and formula (Y1-4), L 2 represents a divalent organic group. 2 In the formula (X1-2), L, including preferred ranges and examples thereof, 1 is the same as:
[0131] In formula (Y1-1), n 21 and n 22 each independently represents an integer of 0 or more and 4 or less, preferably 0, 1, 2, or 3, more preferably 0 or 1, and even more preferably 0.
[0132] In formula (Y1-2), n 23 and n 24 each independently represents an integer of 0 or more and 3 or less, preferably 0, 1 or 2, more preferably 0 or 1, and even more preferably 0.
[0133] In formula (Y1-3), n 25 represents an integer of 0 or more and 3 or less, preferably 0 or 1, and more preferably 0.
[0134] In formula (Y1-3), n 26 represents an integer of 0 or more and 5 or less, preferably 0, 1, 2, or 3, more preferably 0, 1, or 2, and even more preferably 0.
[0135] In formula (Y1-4), n 27 represents an integer of 0 or more and 2 or less, preferably 0 or 1, and more preferably 0.
[0136] In formula (Y1-4), n 28represents an integer of 0 or more and 4 or less, preferably 0, 1, 2, or 3, more preferably 0, 1, or 2, and even more preferably 0.
[0137] In formula (Y1-2) and formula (Y1-4), L 2 represents a methylene group having no substituent, a methylene group substituted with an oxo group (i.e., -C(=O)-), and =CR 21 R 22 methylene group substituted with (i.e., -C(=CR 21 R 22 Therefore, the structure represented by formula (Y1-2) is preferably represented by the following formula (Y1-2-1), formula (Y1-2-2) or formula (Y1-2-3). In formula (Y1-2-3), two R 21 may be the same or different. Also, two R 22 may be the same or different. The structure represented by formula (Y1-4) is preferably represented by the following formula (Y1-4-1), formula (Y1-4-2) or formula (Y1-4-3). In formula (Y1-4-3), two R 21 may be the same or different. Also, two R 22 may be the same or different.
[0138] [ka]
[0139] (In formulas (Y1-2-1) to (Y1-2-3) and formulas (Y1-4-1) to (Y1-4-3), each symbol is as defined above.)
[0140] In formula (1), the divalent organic group Y 1 contains one or more structures selected from the group consisting of a structure represented by formula (Y1-1), a structure represented by formula (Y1-2), a structure represented by formula (Y1-3), and a structure represented by formula (Y1-4), 1may contain any structure in combination with one or more structures selected from the group consisting of the structure represented by formula (Y1-1), the structure represented by formula (Y1-2), the structure represented by formula (Y1-3), and the structure represented by formula (Y1-4). 1 contains only one or more structures selected from the group consisting of a structure represented by formula (Y1-1), a structure represented by formula (Y1-2), a structure represented by formula (Y1-3), and a structure represented by formula (Y1-4). That is, preferably, 1 is represented by formula (Y1-1), formula (Y1-2), formula (Y1-3) or formula (Y1-4).
[0141] In formula (1), X 1 When Y contains a specific structure (i.e., a structure containing at least two benzene rings and a divalent group represented by formula (1-1) connecting the two benzene rings), 1 may be a divalent organic group that does not contain a specific structure.
[0142] The number of carbon atoms of the divalent organic group not containing a specific structure is preferably 6 to 40. Such a divalent organic group preferably contains an aromatic ring. Examples of such a divalent organic group include the following groups (y-1) to (y-20). Furthermore, a group obtained by combining two or more of the following groups (y-1) to (y-20) may be used as the divalent organic group. Among them, the group (y-2) is more preferable. In the formula, * represents a bond.
[0143] [ka]
[0144] [ka]
[0145] [ka]
[0146] The above-mentioned groups (y-1) to (y-20) may have a substituent. Examples of the substituent include the same examples as the substituents that the groups (x-1) to (x-9) may have. The number of types of the substituent may be one or more.
[0147] -Examples of preferred repeating units- Preferably, the polyimide resin according to this embodiment contains a repeating unit represented by any one of the following formulas (2) to (7).
[0148] [ka]
[0149] (In formulas (2) to (7), each symbol is as defined above.)
[0150] More preferably, the polyimide resin according to the present embodiment contains a repeating unit represented by any one of the following formulas (2), (3-1) to (3-3), (4), (5-1) to (5-3), (6), and (7-1) to (7-3). 11 may be the same or different, and the two R 12 may be the same or different. In addition, in formula (5-3) and formula (7-3), two R 21 may be the same or different, and the two R 22 may be the same or different.
[0151] [ka]
[0152] [ka]
[0153] [ka]
[0154] More preferably, the polyimide resin according to the present embodiment contains a repeating unit represented by any one of the following formulas (2-1-1) to (2-1-4), (3-1-1) to (3-3-4), (4-1-1) to (4-1-4), (5-1-1) to (5-3-4), (6-1-1) to (6-1-4), and (7-1-1) to (7-3-4). In the formulas (3-3-2) to (3-3-4), (5-3-2) to (5-3-4), and (7-3-2) to (7-3-4), the two R may be the same or different. In the formulas (3-3-1) to (3-3-4), (5-3-1) to (5-3-4), and (7-3-1) to (7-3-4), the two R 15 may be the same or different, and the two R 16 may be the same or different, and the two R 17 may be the same or different, and two p1's may be the same or different.
[0155] [ka]
[0156] [ka]
[0157] [ka]
[0158] [ka]
[0159] [ka]
[0160] [ka]
[0161] [ka]
[0162] [ka]
[0163] [ka]
[0164] [ka]
[0165] [ka]
[0166] [ka]
[0167] (In the above formula, each symbol is as defined above.)
[0168] -Any structural unit- The polyimide resin according to the present embodiment may contain an arbitrary structural unit other than the repeating unit represented by formula (1) in combination with the repeating unit represented by formula (1). The polyimide resin according to the present embodiment may be a copolymer containing the repeating unit represented by formula (1) and an arbitrary structural unit. There is no limitation on the structure of this copolymer, and it may be, for example, a random copolymer, an alternating polymer, or a block copolymer. The arbitrary structural unit may be, for example, a polyimide unit other than the repeating unit represented by formula (1). Here, the "polyimide unit" refers to a repeating unit containing an imide structure.
[0169] -Content of repeating unit represented by formula (1)- The polyimide resin according to the present embodiment preferably contains many repeating units represented by formula (1), and therefore preferably contains few optional structural units. For example, the mass of the repeating units represented by formula (1) is preferably 40% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, even more preferably 70% by mass or more, and even more preferably 80% by mass or more, based on the total mass of the polyimide resin according to the present embodiment (100%). The polyimide resin according to the present embodiment may contain only the repeating units represented by the above-mentioned formula (1) as repeating units, and therefore may not contain any optional structural units. The repeating units represented by formula (1) contained in the polyimide resin according to the present embodiment may be one type, or two or more types.
[0170] - Weight average molecular weight of polyimide resin - The weight average molecular weight (Mw) of the polyimide resin according to the present embodiment is not particularly limited, but is preferably 3,000 or more, more preferably 5,000 or more, even more preferably 10,000 or more, and particularly preferably 15,000 or more, and is preferably 1 million or less, more preferably 500,000 or less, and even more preferably 200,000 or less. The weight average molecular weight of the resin can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).
[0171] -Method of manufacturing polyimide resin- The polyimide resin according to the present embodiment is a polyimide resin containing a carbonyl group connecting two benzene rings, such as a carbonyl group of a benzophenone skeleton, an anthrone skeleton, or an anthraquinone skeleton, by modifying the carbonyl group to add -C(=CR 1 R 2 )-(i.e., a group represented by formula (1-1)), -C(=CR 11 R 12 )-or-C(=CR 21 R 22The polyimide resin containing a carbonyl group serves as a precursor of the polyimide resin according to the present embodiment, and may be referred to as a "precursor resin" hereinafter.
[0172] The precursor resin may be a polyimide resin having a group -C(=CR 1 R 2 )-, group-C(=CR 11 R 12 )- or the group -C(=CR 21 R 22 A polyimide resin having a structure in which the repeating unit represented by the following formula (1') is substituted for the repeating unit represented by the following formula (1') can be used.
[0173] [ka] (In formula (1'), X 2 represents a tetravalent organic group; Y 2 represents a divalent organic group; X 2 and Y 2 At least one of the above contains at least two benzene rings and a carbonyl group connecting the two benzene rings.
[0174] Preferably, X 2 contains one or more structures selected from the group consisting of a structure represented by the following formula (X2'-1) and a structure represented by the following formula (X2'-2); or Y 2 includes one or more structures selected from the group consisting of a structure represented by the following formula (Y2'-1), a structure represented by the following formula (Y2'-2), a structure represented by the following formula (Y2'-3), and a structure represented by the following formula (Y2'-4):
[0175] [ka] (In formula (X2'-1) and formula (X2'-2), each symbol is as defined above.)
[0176] [ka] (In formulas (Y2'-1), (Y2'-2), (Y2'-3) and (Y2'-4), each symbol is as defined above.)
[0177] Specific examples of the precursor resin for producing the polyimide resin of the present embodiment containing the repeating unit represented by formula (2) include polyimide resins containing the repeating unit represented by formula (2'). Also, examples of the precursor resin for producing the polyimide resin of the present embodiment containing the repeating unit represented by formula (3) include polyimide resins containing the repeating unit represented by formula (3'). Furthermore, examples of the precursor resin for producing the polyimide resin of the present embodiment containing the repeating unit represented by formula (4) include polyimide resins containing the repeating unit represented by formula (4'). Also, examples of the precursor resin for producing the polyimide resin of the present embodiment containing the repeating unit represented by formula (5) include polyimide resins containing the repeating unit represented by formula (5'). Furthermore, examples of the precursor resin for producing the polyimide resin of the present embodiment containing the repeating unit represented by formula (6) include polyimide resins containing the repeating unit represented by formula (6'). Also, examples of the precursor resin for producing the polyimide resin of the present embodiment containing the repeating unit represented by formula (7) include polyimide resins containing the repeating unit represented by formula (7').
[0178] [ka]
[0179] [ka]
[0180] (In the above formula, each symbol is as defined above.)
[0181] The modification of the carbonyl group of the precursor resin can be carried out, for example, by reacting the precursor resin with a Wittig reagent (a phosphorus ylide compound) or a phosphonic acid diester compound under basic conditions (Wittig reaction or Horner-Wadsworth-Emmons reaction). An example of the Wittig reagent is Ph3P=CR 1 R 2 , Ph3P=CR 11 R 12 , Ph3P=CR 21 R 22 Examples of the phosphonic acid diester compound include (R h O)2(O=)P-CHR 1 R 2 , (R h O)2(O=)P-CHR 11 R 12 , (R h O)2(O=)P-CHR 21 R 22 Here, Ph represents a phenyl group, and R h represents an alkyl group, and the other symbols are as defined above.
[0182] The carbonyl group of the precursor resin may be modified, for example, by reacting the precursor resin with a β-dicarbonyl compound under basic conditions (Knoevenagel condensation reaction). 1 and R 2 When both are -COR or -COOR or are combined to form a ring, R in formulae (X1-1) and (X1-2) 11 and R 12 are both -COR or -COOR or are combined together to form a ring, and R 21 and R 22 are both -COR or -COOR or are combined to form a ring. 1 R 2 , CH2R 11 R 12 , CH2R 21 R22 , where each symbol is as defined above.
[0183] The carbonyl group of the precursor resin may be modified, for example, by reacting the precursor resin with Meldrum's acid under basic conditions and then reacting it with an alcohol compound represented by R-OH (Knoevenagel condensation reaction). 1 and R 2 When one of R is a hydrogen atom and the other is -COOR, R in formulas (X1-1) and (X1-2) 11 and R 12 is a hydrogen atom and the other is -COOR, and R in formulae (Y1-1) to (Y1-4) 21 and R 22 is a hydrogen atom and the other is -COOR.
[0184] The reaction conditions may be the same as or similar to the general reaction conditions for the Wittig reaction, Horner-Wadsworth-Emmons reaction, or Knoevenagel condensation reaction. Examples of the base that may be used include piperazine and potassium carbonate. A solvent may also be used in the reaction. Examples of the solvent that may be used include N-methylpyrrolidone, tetrahydrofuran, and dimethyl ether. The reaction temperature may be set appropriately within the range of -80°C to 250°C. The reaction time may be within the range of 0.1 hours to 50 hours. After the reaction, the product may be purified by a known method.
[0185] The above-mentioned reaction rate of the carbonyl group of the precursor resin may be less than 100 mol%, and thus the above-mentioned carbonyl group linking two benzene rings may remain in the polyimide resin according to this embodiment. In addition, the above-mentioned reaction rate of the carbonyl group may be preferably 10 mol% or more, more preferably 20 mol% or more, even more preferably 30 mol% or more, and particularly preferably 40 mol% or more in one example. Therefore, in one embodiment, the remaining rate of the carbonyl group linking two benzene rings in the polyimide resin according to this embodiment may be preferably less than 90 mol%, more preferably less than 80 mol%, even more preferably less than 70 mol%, and particularly preferably less than 60 mol%.
[0186] The precursor resin can be produced, for example, by reacting a tetracarboxylic dianhydride with a diamine compound. Thus, by reacting a tetracarboxylic dianhydride represented by the following formula (1"-a) with a diamine compound represented by the following formula (1"-b), a precursor resin containing a repeating unit represented by formula (1') can be produced, via which a polyimide resin containing a repeating unit represented by formula (1) can be produced.
[0187] [ka]
[0188] Therefore, when a tetracarboxylic dianhydride containing a carbonyl group linking two benzene rings is used, a polyimide resin containing one or more structures selected from the group consisting of a structure represented by formula (2) and a structure represented by formula (3) can be produced. For example, by reacting a tetracarboxylic dianhydride represented by the following formula (2"-a) with a diamine compound represented by the following formula (2"-b), a polyimide resin containing a repeating unit represented by formula (2) can be produced via a precursor resin containing a repeating unit represented by formula (2'). In addition, by reacting a tetracarboxylic dianhydride represented by the following formula (3"-a) with a diamine compound represented by the following formula (3"-b), a polyimide resin containing a repeating unit represented by formula (3) can be produced via a precursor resin containing a repeating unit represented by formula (3').
[0189] [ka]
[0190] In addition, when a diamine compound containing a carbonyl group linking two benzene rings is used, a polyimide resin containing one or more structures selected from the group consisting of a structure represented by formula (4), a structure represented by formula (5), a structure represented by formula (6), and a structure represented by formula (7) can be produced. For example, a tetracarboxylic dianhydride represented by the following formula (4"-a) is reacted with a diamine compound represented by the following formula (4"-b) to produce a precursor resin containing a repeating unit represented by formula (4'), and then a polyimide resin containing a repeating unit represented by formula (4). In addition, a tetracarboxylic dianhydride represented by the following formula (5"-a) is reacted with a diamine compound represented by the following formula (5"-b) to produce a precursor resin containing a repeating unit represented by formula (5'), and then a polyimide resin containing a repeating unit represented by formula (5). Furthermore, for example, by reacting a tetracarboxylic dianhydride represented by the following formula (6"-a) with a diamine compound represented by the following formula (6"-b), a precursor resin containing a repeating unit represented by formula (6') can be produced, via which a polyimide resin containing a repeating unit represented by formula (6) can be produced. Furthermore, for example, by reacting a tetracarboxylic dianhydride represented by the following formula (7"-a) with a diamine compound represented by the following formula (7"-b), a precursor resin containing a repeating unit represented by formula (7') can be produced, via which a polyimide resin containing a repeating unit represented by formula (7) can be produced.
[0191] [ka]
[0192] (In the above formula, each symbol is as defined above.)
[0193] The reaction between the tetracarboxylic dianhydride and the diamine compound can be carried out by a known method or a method similar thereto. A solvent may be used in the reaction. Examples of the solvent that can be used include N-methylpyrrolidone, γ-butyrolactone, and dimethylsulfoxide, and non-ketone solvents are preferred. The reaction temperature can be appropriately set within a range of 20°C to 200°C. The reaction time can be within a range of 0.1 hours to 50 hours. In addition, a precursor resin may be obtained by reacting the tetracarboxylic dianhydride with the diamine compound to obtain a polyamic acid, and then dehydrating and ring-closing the polyamic acid.
[0194] The polyimide resin according to the present embodiment can be produced, for example, by a production method including a step of reacting a tetracarboxylic dianhydride with a diamine compound, in which at least one of the tetracarboxylic dianhydride and the diamine compound has a specific structure. Thus, the polyimide resin according to the present embodiment can be produced by a production method including reacting a tetracarboxylic dianhydride represented by the following formula (1'-a) with a diamine compound represented by the following formula (1'-b).
[0195] [ka]
[0196] (In formula (1'-a) and formula (1'-b), each symbol is as defined above.)
[0197] Among the tetracarboxylic dianhydrides represented by formula (1'-a), X having a specific structure 1 The diamine compound having the formula (1'-b) can be produced, for example, by a method including modifying a carbonyl group of a tetracarboxylic dianhydride containing a carbonyl group linking two benzene rings. 1 can be prepared, for example, by a method comprising modifying a carbonyl group of a diamine compound containing the carbonyl group linking two benzene rings.
[0198] Therefore, in the polyimide resin according to the present embodiment, for example, a carbonyl group of a tetracarboxylic dianhydride containing a carbonyl group connecting two benzene rings is modified to add -C(=CR 1 R 2 )-(i.e., a divalent group represented by formula (1-1)) or -C(=CR 11 R 12 )- and reacting the tetracarboxylic dianhydride with a diamine compound. As a specific example, a polyimide resin containing a repeating unit represented by formula (2) may be produced by a method comprising the steps of modifying a carbonyl group of a tetracarboxylic dianhydride represented by formula (2″-a) to obtain a tetracarboxylic dianhydride represented by formula (2′-a) below, and reacting the tetracarboxylic dianhydride with a diamine compound represented by formula (2′-b). Also, a polyimide resin containing a repeating unit represented by formula (3) may be produced by a method comprising the steps of modifying a carbonyl group of a tetracarboxylic dianhydride represented by formula (3″-a) to obtain a tetracarboxylic dianhydride represented by formula (3′-a) below, and reacting the tetracarboxylic dianhydride with a diamine compound represented by formula (3′-b).
[0199] [ka]
[0200] (In the above formula, each symbol is as defined above.)
[0201] In addition, the polyimide resin according to the present embodiment can be obtained by modifying the carbonyl group of a diamine compound containing a carbonyl group connecting two benzene rings, to thereby add -C(=CR 1 R 2 )-(i.e., a divalent group represented by formula (1-1)) or -C(=CR 21 R 22) and reacting the diamine compound with a tetracarboxylic dianhydride. As a specific example, a polyimide resin containing a repeating unit represented by formula (4) may be produced by a method including a step of modifying a carbonyl group of a diamine compound represented by formula (4″-b) to obtain a diamine compound represented by formula (4′-b) and reacting the diamine compound with a tetracarboxylic dianhydride represented by formula (4′-a). Also, a polyimide resin containing a repeating unit represented by formula (5) may be produced by a method including a step of modifying a carbonyl group of a diamine compound represented by formula (5″-b) to obtain a diamine compound represented by formula (5′-b) and reacting the diamine compound with a tetracarboxylic dianhydride represented by formula (5′-a). Furthermore, a polyimide resin containing a repeating unit represented by formula (6) may be produced by a method comprising the steps of modifying a carbonyl group of a diamine compound represented by formula (6″-b) to obtain a diamine compound represented by formula (6′-b) and reacting the diamine compound with a tetracarboxylic dianhydride represented by formula (6′-a). Also, a polyimide resin containing a repeating unit represented by formula (7) may be produced by a method comprising the steps of modifying a carbonyl group of a diamine compound represented by formula (7″-b) to obtain a diamine compound represented by formula (7′-b) and reacting the diamine compound with a tetracarboxylic dianhydride represented by formula (7′-a).
[0202] [ka]
[0203] (In the above formula, each symbol is as defined above.)
[0204] The modification of the carbonyl groups of the tetracarboxylic dianhydride and the diamine compound can be carried out by the above-mentioned Wittig reaction, Horner-Wadsworth-Emmons reaction, or Knoevenagel condensation reaction. The reaction conditions for these reactions can be the same as or similar to the general reaction conditions, and for example, the above-mentioned conditions can be adopted. In addition, the above-mentioned reaction rate of the tetracarboxylic dianhydride and the diamine compound with respect to the carbonyl groups can be the same as the reaction rate with respect to the precursor resin. Furthermore, the reaction between the tetracarboxylic dianhydride and the diamine compound can be carried out by a known method or a method similar thereto, and for example, the above-mentioned conditions can be adopted. The carbonyl group linking the two benzene rings may remain in the obtained polyimide resin. In one example, the range of the remaining rate of the carbonyl group linking the two benzene rings in the obtained polyimide resin can be the same as the range of the remaining rate in the above-mentioned manufacturing method using the precursor resin.
[0205] The above-described production method may further include a combination of known reactions such as a decarboxylation reaction, a deprotection reaction, an oxidation reaction, a reduction reaction, a radical cyclization reaction, a nucleophilic substitution reaction, an alkylation reaction, a halogenation reaction, a condensation reaction, etc. Furthermore, if necessary, copolymerization with an arbitrary monomer may be performed to introduce an arbitrary structural unit into the polyimide resin.
[0206] <Photosensitive resin composition> The photosensitive resin composition according to one embodiment of the present invention includes the above-mentioned polyimide resin (A), crosslinking agent (B), and photoradical generator (C). This photosensitive resin composition can generally be used as a negative-type photosensitive resin composition.
[0207] The photosensitive resin composition according to the present embodiment has excellent film retention. As described above, "film retention" refers to the property that the thickness of the exposed photosensitive resin composition is not easily reduced when it comes into contact with a developer. This film retention can be expressed by the ratio of the thickness of the photosensitive resin composition layer after exposure and development to the thickness of the photosensitive resin composition layer before exposure and development. The ratio is sometimes called "film retention rate", and generally, the higher the film retention rate, the better the film retention.
[0208] When the photosensitive resin composition is cured, a cured product can be obtained. According to the photosensitive resin composition of the present embodiment, a cured product having excellent dielectric properties can be obtained, and in particular, a cured product having excellent dielectric loss tangent can be obtained.
[0209] Without being bound by any particular theory, the inventors speculate that the mechanism by which the above-mentioned excellent effects are obtained is as follows, however, the technical scope of the present invention is not limited by the mechanism described below.
[0210] When the photosensitive resin composition according to this embodiment is exposed to light, the (C) photoradical generator generates radicals, which react with the (B) crosslinking agent to form a crosslinked structure. Since the crosslinked structure is formed by the reaction of the (B) crosslinking agent, the exposed photosensitive resin composition can have a lower solubility in a developer than the non-exposed photosensitive resin composition. In addition, in the photosensitive resin composition according to this embodiment, the (A) polyimide resin contains an ethylenic double bond having radical reactivity, so that when exposed to light, not only the (B) crosslinking agent but also the (A) polyimide resin reacts to form a crosslinked structure. Therefore, the crosslinked structure can be made dense and the solubility in the developer can be effectively reduced, so that the amount of the photosensitive resin composition reduced when it comes into contact with the developer can be reduced, and as a result, high film retention can be obtained.
[0211] In addition, conventionally, polyimide resins containing ethylenically unsaturated bonds tend to contain many polar groups such as hydroxyl groups, and therefore the polarity of the cured product tends to be high, leading to high dielectric properties. In contrast, the polyimide resin (A) according to the above-mentioned embodiment can reduce the content of polar groups. For example, the generation of polar groups can be avoided in the reaction of introducing ethylenically unsaturated bonds into the polyimide resin, so that the content of polar groups can be reduced. Therefore, the cured product of the photosensitive resin composition containing the polyimide resin (A) can have low polarity, so that the dielectric loss tangent can be reduced to achieve excellent dielectric properties.
[0212] -(A) Polyimide resin- The photosensitive resin composition according to the present embodiment contains a polyimide resin (A) as component (A). The polyimide resin (A) is a polyimide resin containing a repeating unit represented by formula (1), and the details thereof are as described above. The polyimide resin (A) may be used alone or in combination of two or more kinds.
[0213] The amount of the (A) polyimide resin in the photosensitive resin composition is preferably 40% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, and preferably 95% by mass or less, more preferably 92% by mass or less, even more preferably 89% by mass or less, particularly preferably 85% by mass or less, based on 100% by mass of the non-volatile components of the photosensitive resin composition. When the amount of the (A) polyimide resin is equal to or more than the lower limit of the above range, the dielectric loss tangent of the cured product of the photosensitive resin composition can be effectively reduced. When the amount of the polyimide resin is equal to or less than the upper limit of the above range, the film residual property can be effectively increased.
[0214] -(B) Crosslinking agent- The photosensitive resin composition according to this embodiment includes a crosslinking agent (B) as the component (B). The crosslinking agent (B) does not include those corresponding to the component (A). When the photosensitive resin composition is irradiated with active light rays and radicals are generated from the photoradical generator (C), a crosslinking reaction of the crosslinking agent (B) occurs, and the solubility in the developer can be reduced. Therefore, during development, it becomes possible to selectively remove the photosensitive resin composition from areas other than those where the crosslinking reaction has progressed, and a negative pattern can be advantageously formed. The crosslinking agent (B) may be used alone or in combination of two or more.
[0215] As the (B) crosslinking agent, a compound capable of proceeding with a crosslinking reaction by exposure to light can be used. As such a (B) crosslinking agent, a compound having an ethylenically unsaturated bond is preferable. Furthermore, as the (B) crosslinking agent, a compound having an ethylenically unsaturated bond, in which at least one carbon atom at the α-position of the ethylenically unsaturated bond is bonded to a carbonyl group or an aromatic group, is more preferable. The carbon atom at the α-position of the ethylenically unsaturated bond refers to the first carbon atom adjacent to the carbon atom bonded by the ethylenically unsaturated bond.
[0216] (B) crosslinking agent generally contains a group having an ethylenically unsaturated bond. Hereinafter, the "group having an ethylenically unsaturated bond" may be referred to as "ethylenically unsaturated group". The ethylenically unsaturated group is usually a monovalent group, and examples thereof include a vinyl group, an allyl group, a propargyl group, a butenyl group, an ethynyl group, a phenylethynyl group, a maleimide group, a nadimide group, and a (meth)acryloyl group. From the viewpoint of the reactivity of photoradical polymerization, a (meth)acryloyl group and a phenylethynyl group are preferred, and a (meth)acryloyl group is more preferred. The "(meth)acryloyl group" includes a methacryloyl group, an acryloyl group, and a combination thereof. (B) crosslinking agent contains an ethylenically unsaturated bond, and therefore is capable of photoradical polymerization. However, in order to perform photoradical polymerization under general conditions, a compound having a carbonyl group or an aromatic group at at least one of the α-positions of the ethylenically unsaturated bond is preferred.
[0217] The number of ethylenically unsaturated bonds per molecule of the (B) crosslinking agent is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more. When the (B) crosslinking agent contains two or more ethylenically unsaturated groups per molecule, the ethylenically unsaturated groups may be the same or different.
[0218] The (B) crosslinking agent is preferably a compound represented by the following formula (B-1).
[0219] [ka]
[0220] (In formula (B-1), R 1b each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms; Z 1b each independently represents a linear or branched alkylene group having 1 to 20 carbon atoms which may contain an oxygen atom, an arylene group which may contain an oxygen atom, or a linear or branched alkenylene group having 2 to 20 carbon atoms which may contain an oxygen atom; A 1b is a linear, cyclic or branched n b represents an organic group having 1-valent valence; n b represents an integer from 2 to 6.)
[0221] In formula (B-1), R 1b each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms. Examples of the linear or branched alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a 1-butyl group, a s-butyl group, and a t-butyl group. Among them, R 1b is preferably a hydrogen atom or a methyl group.
[0222] In formula (B-1), Z 1b each independently represents a linear or branched alkylene group having 1 to 20 carbon atoms which may contain an oxygen atom, an arylene group which may contain an oxygen atom, or a linear or branched alkenylene group having 2 to 20 carbon atoms which may contain an oxygen atom.
[0223] The "straight-chain or branched alkylene group having 1 to 20 carbon atoms" in the "straight-chain or branched alkylene group having 1 to 20 carbon atoms which may contain an oxygen atom" is preferably a straight-chain or branched alkylene group having 1 to 10 carbon atoms, more preferably a straight-chain or branched alkylene group having 1 to 6 carbon atoms. Examples of such alkylene groups include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, and the like, with a methylene group being preferred. The alkylene group which may contain an oxygen atom may be an oxyalkylene group. Specific examples of such groups include those shown in the following (b1-1) to (b1-6). In the formula, "*" represents a bond, n b1 and n b2 represents an integer from 1 to 20, and n b3 and n b4 represents an integer from 1 to 10, and n b5 represents an integer from 1 to 19, and n b6 represents an integer from 1 to 9.
[0224] [ka]
[0225] The "arylene group" in the "arylene group which may contain an oxygen atom" is preferably an arylene group having 6 to 20 carbon atoms, more preferably an arylene group having 6 to 15 carbon atoms, and even more preferably an arylene group having 6 to 10 carbon atoms. Examples of such arylene groups include a phenylene group and a naphthylene group. The arylene group which may contain an oxygen atom may be an aryleneoxy group. Specific examples of such groups include those shown in the following (b2-1) and (b2-2). In the formula, "*" represents a bond, n b7 and n b8 represents an integer from 1 to 3.
[0226] [ka]
[0227] In the "linear or branched alkenylene group having 2 to 20 carbon atoms which may contain an oxygen atom", the "linear or branched alkenylene group having 2 to 20 carbon atoms which may contain an oxygen atom" is preferably a linear or branched alkenylene group having 2 to 10 carbon atoms, more preferably a linear or branched alkenylene group having 2 to 6 carbon atoms. Examples of such alkenylene groups include ethenylene, propenylene, butenylene, pentenylene, and hexenylene groups. The alkenylene group which may contain an oxygen atom may be an oxyalkenylene group. Specific examples of such groups include those shown in the following (b3-1) and (b3-2). In the formula, "*" represents a bond, and n b9 ~n b10 represents an integer of 1 to 10. The alkenylene group is preferably a propenylene group.
[0228] [ka]
[0229] Among them, Z 1b As the alkyl group, a linear or branched alkylene group having 1 to 20 carbon atoms which may contain an oxygen atom is preferable, an oxyalkylene group is more preferable, and an oxymethylene group is further preferable.
[0230] In formula (B-1), A 1b is a linear, cyclic or branched n b represents an n-valent organic group. b The valence organic group is, for example, a n-type organic group which may contain an oxygen atom. b n-valent hydrocarbon radical derived from bisphenol b n-valent group derived from fluorene b n-valent group derived from tricyclodecane b n-valent group or isocyanuric group b Examples of the n-valent group include an n-valent group which may contain an oxygen atom. b The n-valent hydrocarbon group may contain an oxygen atom. baliphatic hydrocarbon group having n valence, which may contain an oxygen atom b and n-valent aromatic hydrocarbon groups which may contain an oxygen atom. b A 4-valent aliphatic hydrocarbon group is preferred. 1b Specific examples of the group represented by include the following (b4-1) to (b4-7), in which "*" represents a bond.
[0231] [ka]
[0232] In formula (B-1), n b represents a positive integer of 2 to 6, preferably represents a positive integer of 2 to 5, more preferably represents an integer of 2 to 4, and further preferably represents 2 or 3.
[0233] The (B) crosslinking agent is preferably a compound represented by the following formula (B-2).
[0234] [ka]
[0235] In formula (B-2), R 2b each independently represents a hydrogen atom or a methyl group, and a methyl group is preferable.
[0236] Specific examples of the (B) crosslinking agent include the following compounds (b5-1) to (b5-11), however, the (B) crosslinking agent is not limited thereto.
[0237] [ka]
[0238] [ka]
[0239] As the (B) crosslinking agent, commercially available products can be used, such as NK Ester-D-TMP, 4G, 9G, 14G, 23G, and DCP manufactured by Shin-Nakamura Chemical Co., Ltd.
[0240] The amount of the (B) crosslinking agent in the photosensitive resin composition is, relative to 100% by mass of the non-volatile components of the photosensitive resin composition, preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 2% by mass or more, particularly preferably 5% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, particularly preferably 10% by mass or less.
[0241] The mass ratio of the crosslinking agent (B) to the polyimide resin (A) ((B) / (A)) is preferably 0.01 or more, more preferably 0.02 or more, even more preferably 0.04 or more, and particularly preferably 0.08 or more, and is preferably 1.0 or less, more preferably 0.8 or less, even more preferably 0.6 or less, even more preferably 0.4 or less, and particularly preferably 0.2 or less.
[0242] -(C) Photoradical generator- The photosensitive resin composition according to the present embodiment includes a photoradical generator (C) as the component (C). The photoradical generator (C) does not include those corresponding to the above-mentioned components (A) to (B). As the photoradical generator (C), a compound capable of generating radicals upon receiving actinic rays can be used. Usually, a crosslinking reaction can proceed by radicals generated from the photoradical generator (C). In the photosensitive resin composition, the portion where the crosslinking reaction by radicals has occurred has improved resistance to a developer. Therefore, during development, it becomes possible to selectively remove the photosensitive resin composition from the portion where the crosslinking reaction has proceeded, and a negative pattern can be advantageously formed. The photoradical generator (C) may be used alone or in combination of two or more.
[0243] (C) Examples of the photoradical generator include benzophenone derivatives such as benzophenone, o-benzoylmethylbenzoate, 4-benzoyl-4'-methyldiphenyl ketone, dibenzyl ketone, and fluorenone; acetophenone derivatives such as 2,2'-diethoxyacetophenone, 2-hydroxy-2-methylpropiophenone, and 1-hydroxycyclohexylphenyl ketone; thioxanthone derivatives such as thioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, and diethylthioxanthone; benzyl derivatives such as benzil, benzil dimethyl ketal, and benzyl-β-methoxyethyl acetal; benzoin derivatives such as benzoin and benzoin methyl ether; and 1-phenyl-1,2-butanedione-2 -(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-benzoyl)oxime, 1,3-diphenylpropanetrione-2-(o-ethoxycarbonyl)oxime, 1-phenyl-3-ethoxypropanetrione-2-(o-benzoyl)oxime and other oximes; N-arylglycines such as N-phenylglycine; peroxides such as benzoyl perchloride; aromatic biimidazoles; titanocenes; α-(n-octanesulfonyloxyimino)-4-methoxybenzyl cyanide; and the like. Among these, oximes are preferred from the viewpoint of photosensitivity.
[0244] (C) The photoradical generator may be a commercially available product, such as "Irgacure-OXE02" and "Irgacure-OXE04" manufactured by BASF.
[0245] The amount of the (C) photoradical generator in the photosensitive resin composition is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 1 mass% or more, relative to 100 mass% of the nonvolatile components of the photosensitive resin composition, and is preferably 10 mass% or less, more preferably 8 mass% or less, and even more preferably 6 mass% or less.
[0246] The mass ratio ((C) / (A)) of the photoradical generator (C) to the polyimide resin (A) is preferably 0.001 or more, more preferably 0.01 or more, even more preferably 0.02 or more, and is preferably 0.1 or less, more preferably 0.08 or less, even more preferably 0.06 or less.
[0247] -(D) Sensitizer- The photosensitive resin composition according to the present embodiment may contain any component in combination with the above-mentioned components (A) to (C). For example, the photosensitive resin composition may contain a sensitizer (D). The sensitizer (D) as the component (D) does not include those corresponding to the above-mentioned components (A) to (C). The sensitizer (D) can generally be excited by receiving light, but the sensitizer (D) itself does not generate radicals. In addition, when the sensitizer (D) is excited, it can usually transfer its energy to the photoradical generator (C). Then, the photoradical generator (C) that has received the energy can generate radicals. Therefore, by using the sensitizer (D), it is possible to improve the photosensitivity of the photosensitive resin composition. The sensitizer (D) may be used alone or in combination of two or more types.
[0248] (D) Examples of sensitizers include benzophenones such as Michler's ketone, 4,4'-bis(diethylamino)benzophenone, and 4-morpholinobenzophenone; cyclic alkanes such as 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, and 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone; chalcones such as 4,4'-bis(dimethylamino)chalcone and 4,4'-bis(diethylamino)chalcone; p-di Indanones such as methylaminocinnamylidene indanone and p-dimethylaminobenzylidene indanone; thiazoles such as 2-(p-dimethylaminophenylbiphenylene)-benzothiazole, 2-(p-dimethylaminophenylvinylene)benzothiazole, and 2-(p-dimethylaminophenylvinylene)isonaphthothiazole; acetones such as 1,3-bis(4'-dimethylaminobenzal)acetone and 1,3-bis(4'-diethylaminobenzal)acetone; coumarins such as 3-acetyl-7-dimethylaminocoumarin, 3-ethoxycarbonyl-7-dimethylaminocoumarin, 3-benzyloxycarbonyl-7-dimethylaminocoumarin, 3-methoxycarbonyl-7-diethylaminocoumarin, and 3-ethoxycarbonyl-7-diethylaminocoumarin; N-phenyl-N'-ethylethanolamine, N-phenyldiethanolamine, Np-tolyldiethanolamine, N-phenylethanolamine, isoamyl dimethylaminobenzoate, diethyl amines such as isoamyl diaminobenzoate; heterocyclic compounds such as 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 2-(p-dimethylaminostyryl)benzoxazole, 2-(p-dimethylaminostyryl)benzthiazole, 2-(p-dimethylaminostyryl)naphtho(1,2-d)thiazole, 1-phenyl-5-mercaptotetrazole, and 1-p-hydroxyphenyl-5-mercaptotetrazole; and styrenes such as 2-(p-dimethylaminobenzoyl)styrene.
[0249] Among these, the sensitizer (D) is preferably a heterocyclic compound, and more preferably a compound represented by the following formula (D-1).
[0250] [ka]
[0251] In formula (D-1), R 1d represents a hydrogen atom, a linear or branched alkyl group having 1 to 7 carbon atoms, a halogen atom, a hydroxyl group, a methoxy group, or a t-butoxy group. Examples of the linear or branched alkyl group having 1 to 7 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, and a t-butyl group. Among these, R 1d R is preferably a hydroxy group, a methoxy group, or a t-butoxy group having an oxygen atom, more preferably a hydrogen atom or a hydroxy group, and more preferably a hydrogen atom. 1d The bonding position of may be any of the ortho, meta, or para positions based on the position of the phenylene group bonding to the nitrogen atom of mercaptotetrazole, and the para position is preferred.
[0252] The compound represented by formula (D-1) is preferably either a compound represented by the following (D-2) or a compound represented by the following (D-3).
[0253] [ka]
[0254] The amount of the sensitizer (D) in the photosensitive resin composition is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 1 mass% or more, relative to 100 mass% of the non-volatile components of the photosensitive resin composition, and is preferably 20 mass% or less, more preferably 15 mass% or less, and even more preferably 10 mass% or less.
[0255] The mass ratio of the sensitizer (D) to the polyimide resin (A) ((D) / (A)) is preferably 0.001 or more, more preferably 0.01 or more, even more preferably 0.05 or more, and is preferably 0.5 or less, more preferably 0.3 or less, even more preferably 0.1 or less.
[0256] -(E) Optional Additives- The photosensitive resin composition according to the present embodiment may further contain (E) an optional additive, within a range that does not significantly impair the desired effects of the present invention. (E) The optional additives include, for example, adhesion aids; surfactants such as fluorine-based surfactants, nonionic surfactants, cationic surfactants, anionic surfactants, and silicone-based surfactants; thermoplastic resins; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, carbon black, and naphthalene black; polymerization inhibitors such as hydroquinone, phenothiazine, methylhydroquinone, hydroquinone monomethyl ether, catechol, and pyrogallol; thickeners such as bentone and montmorillonite; silicone-based, fluorine-based, and vinyl resin-based defoamers; flame retardants such as epoxy resins, antimony compounds, phosphorus-based compounds, aromatic condensed phosphate esters, and halogen-containing condensed phosphate esters; thermosetting resins such as phenolic resins and cyanate ester-based resins; and the like. (E) The optional additives may be used alone or in combination of two or more.
[0257] -(F) Solvent- The photosensitive resin composition may contain a solvent (F) as an optional component in combination with the non-volatile components (A) to (E) described above. The solvent (F) is preferably a volatile component capable of uniformly dissolving at least one of the components (A) to (E).
[0258] Examples of the (F) solvent include ether compounds having 2 to 9 carbon atoms, such as dimethyl ether, diethyl ether, methyl ethyl ether, tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, and triethylene glycol dimethyl ether; ketone compounds having 2 to 6 carbon atoms, such as acetone and methyl ethyl ketone; saturated hydrocarbon compounds having 5 to 10 carbon atoms, such as normal pentane, cyclopentane, normal hexane, cyclohexane, methylcyclohexane, and decalin; benzene, tetrahydrofuran, dioxane, triethylene glycol dimethyl ether, and other ether compounds having 2 to 6 carbon atoms. aromatic hydrocarbon compounds having 6 to 10 carbon atoms, such as benzene, xylene, mesitylene, and tetralin; ester compounds having 3 to 9 carbon atoms, such as methyl acetate, ethyl acetate, γ-butyrolactone, and methyl benzoate; halogen-containing compounds having 1 to 10 carbon atoms, such as chloroform, methylene chloride, and 1,2-dichloroethane; nitrogen-containing compounds having 2 to 10 carbon atoms, such as acetonitrile, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; and sulfur-containing compounds, such as dimethyl sulfoxide.
[0259] Examples of the (F) solvent include N-ethyl-2-pyrrolidone, tetrahydrofuran, N,N-dimethylacetamide, dimethyl sulfoxide, hexamethylphosphoramide, pyridine, cyclopentanone, α-acetyl-γ-butyrolactone, tetramethylurea, 1,3-dimethyl-2-imidazolinone, N-cyclohexyl-2-pyrrolidone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone, anisole, ethyl acetate, ethyl lactate, and butyl lactate.
[0260] The component (F) may be used alone or in combination of two or more types.
[0261] The amount of the (F) solvent is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on 100% by mass of the entire photosensitive resin composition including the (F) solvent, and is preferably 99% by mass or less, more preferably 97% by mass or less, and even more preferably 95% by mass or less. The amount of the (F) solvent in the photosensitive resin composition layer of the photosensitive film is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, based on 100% by mass of the entire photosensitive resin composition including the (F) solvent, and is preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less.
[0262] -Method for producing photosensitive resin composition- The photosensitive resin composition according to this embodiment can be produced by a method including appropriately mixing the above-mentioned components and, if necessary, kneading or stirring the mixture with a kneading device such as a triple roll mill, a ball mill, a bead mill, or a sand mill, or a stirring device such as a super mixer or a planetary mixer.
[0263] -Characteristics of photosensitive resin composition- The photosensitive resin composition according to this embodiment can have excellent film remaining properties. Therefore, when the photosensitive resin composition according to this embodiment is used, a reduction in thickness due to exposure and development can be suppressed, and a high film remaining ratio can be obtained. For example, a photosensitive resin composition layer is formed by the photosensitive resin composition. The photosensitive resin composition layer is exposed and developed. In this case, the ratio of the thickness of the photosensitive resin composition layer after development based on the thickness of the photosensitive resin composition layer before exposure (i.e., the film remaining ratio) can be increased. In one example, the specific range of the film remaining ratio is preferably 30% or more, more preferably 40% or more, even more preferably 50% or more, and even more preferably 60% or more. A specific method for measuring the film remaining ratio can be adopted as described in <Test 2. Evaluation of film remaining ratio> in the examples described later.
[0264] According to the photosensitive resin composition of this embodiment, preferably, a cured product having excellent dielectric properties can be obtained. Usually, the photosensitive resin composition is cured through exposure and development to obtain a cured product. This cured product can have excellent dielectric properties. For example, when the photosensitive resin composition is cured to obtain a cured product by the method described in <Test 1. Measurement of dielectric constant and dielectric loss tangent> in the examples described later, the dielectric loss tangent Df of the cured product is preferably 0.015 or less, more preferably 0.012 or less, even more preferably 0.010 or less, and particularly preferably 0.009 or less. There is no particular restriction on the lower limit, and it can be, for example, 0.001 or more. In addition, the relative dielectric constant Dk of the cured product is preferably 5 or less, more preferably 4 or less, and even more preferably 3 or less. The relative dielectric constant Dk and dielectric loss tangent Df of the cured product can be measured by a cavity resonance perturbation method using a measuring device ("HP8362B" manufactured by Agilent Technologies) at a measurement frequency of 5.8 GHz and a measurement temperature of 23°C. As a specific measuring method, the method described in <Test 1. Measurement of dielectric constant and dielectric loss tangent> in the Examples can be adopted.
[0265] -Uses of photosensitive resin compositions- The photosensitive resin composition according to the present embodiment is not particularly limited in its application. The photosensitive resin composition according to the present embodiment can be used in a wide range of applications in which photosensitive resin compositions are used, such as photosensitive films, insulating resin sheets such as prepregs, silicon wafers, circuit boards (laminated boards, multilayer printed wiring boards, semiconductor package boards, etc.), solder resists, buffer coat films, underfill materials, die bonding materials, semiconductor encapsulants, hole filling resins, and component embedding resins.
[0266] Among them, the photosensitive resin composition according to the present embodiment is a photosensitive resin composition for an insulating layer of a semiconductor package substrate (a semiconductor package substrate having an insulating layer formed from a cured product of the photosensitive resin composition), a photosensitive resin composition for an interlayer insulating layer (a semiconductor package substrate having an interlayer insulating layer formed from a cured product of the photosensitive resin composition), a photosensitive resin composition for plating (a semiconductor package substrate having a plating formed on a cured product of the photosensitive resin composition), a photosensitive resin composition for solder resist (a semiconductor package substrate having a solder resist formed from a cured product of the photosensitive resin composition), a photosensitive resin composition for a rewiring formation layer of a wafer level package (a semiconductor package substrate having a rewiring formation layer formed from a cured product of the photosensitive resin composition), The photosensitive resin composition can be suitably used as a wafer-level package having a cured product of the photosensitive resin composition as a rewiring formation layer, a fan-out wafer-level package having a cured product of the photosensitive resin composition as a rewiring formation layer, a fan-out panel-level package having a rewiring formation layer, a photosensitive resin composition for a buffer coat (a semiconductor device having a buffer coat made of a cured product of the photosensitive resin composition), or a photosensitive resin composition for an insulating layer for a display (a display having an insulating layer made of a cured product of the photosensitive resin composition).
[0267] <Photosensitive film> The above-mentioned photosensitive resin composition can be applied to a photosensitive film. The photosensitive film includes a support and a photosensitive resin composition layer formed on the support. The photosensitive resin composition layer includes the above-mentioned photosensitive resin composition, and preferably includes only the photosensitive resin composition. The photosensitive film may also include a support, a photosensitive resin composition layer, and a protective film in this order.
[0268] Examples of the support include a polyethylene terephthalate film, a polyethylene naphthalate film, a polypropylene film, a polyethylene film, a polyvinyl alcohol film, a triacetyl acetate film, and the like, with a polyethylene terephthalate film being particularly preferred.
[0269] Examples of commercially available supports include, but are not limited to, "Alphan MA-410" and "E-200C" manufactured by Oji Paper Co., Ltd., "GF-1" and "GF-8" manufactured by Tamapoly Co., Ltd., polypropylene films manufactured by Shin-Etsu Film Co., Ltd., and polyethylene terephthalate films such as PS series such as "PS-25" manufactured by Teijin Co., Ltd. In order to facilitate removal, it is preferable that the surface of these supports is coated with a release agent such as a silicone coating agent or a non-silicone coating agent. Examples of supports whose surfaces have been treated with such release agents include "AL-5" manufactured by Lintec Corporation. The thickness of the support is preferably in the range of 5 μm to 100 μm, and more preferably in the range of 10 μm to 50 μm.
[0270] The thickness of the photosensitive resin composition layer is not particularly limited and may be, for example, 1 μm or more and 100 μm or less. In particular, it is preferably 2 μm or more, more preferably 4 μm or more, and is preferably 50 μm or less, more preferably 30 μm or less.
[0271] The photosensitive resin composition layer may be protected by a protective film. When the photosensitive resin composition layer is protected by a protective film, the adhesion of dust and scratches on the surface of the photosensitive resin composition layer can be suppressed. As the protective film, for example, a film made of the same material as the above-mentioned support can be used. The thickness of the protective film is not particularly limited, but is preferably in the range of 1 μm to 40 μm, more preferably in the range of 5 μm to 30 μm, and further preferably in the range of 10 μm to 30 μm. It is preferable that the adhesive strength between the photosensitive resin composition layer and the protective film is smaller than the adhesive strength between the photosensitive resin composition layer and the support.
[0272] The photosensitive film can be produced, for example, by a method including coating the photosensitive resin composition on a support and, if necessary, drying the (F) solvent.
[0273] <Semiconductor package substrate> A semiconductor package substrate according to an embodiment of the present invention includes a cured product of the above-mentioned photosensitive resin composition. Usually, the cured product forms an insulating layer of the semiconductor package substrate. Therefore, the insulating layer includes a cured product of the photosensitive resin composition, and preferably includes only a cured product of the photosensitive resin composition. The insulating layer is preferably used as a rewiring formation layer, an interlayer insulating layer, a buffer coat film, or a solder resist.
[0274] In the first example, the semiconductor package substrate can be manufactured using the above-mentioned photosensitive resin composition, and the cured product of the photosensitive resin composition is used as an insulating layer. Specifically, the manufacturing method of the semiconductor package substrate according to the first example includes the following steps: (I) forming a photosensitive resin composition layer containing a photosensitive resin composition on a circuit board; (II) a step of irradiating the photosensitive resin composition layer with actinic rays; (III) developing the photosensitive resin composition layer; Includes, in this order.
[0275] -Process (I)- The method for producing a semiconductor package substrate according to the first example includes a step (I) of forming a photosensitive resin composition layer on a circuit board. Examples of the method for forming the photosensitive resin composition layer include a method of directly applying a resin varnish containing a photosensitive resin composition onto a circuit board, and a method of using the photosensitive film.
[0276] When the resin varnish containing the photosensitive resin composition is directly applied onto the circuit board, the (F) solvent is dried or volatilized to form a photosensitive resin composition layer on the circuit board.
[0277] Examples of methods for applying resin varnish include gravure coating, microgravure coating, reverse coating, kiss reverse coating, die coating, slot die, lip coating, comma coating, blade coating, roll coating, knife coating, curtain coating, chamber gravure coating, slot orifice, spin coating, slit coating, spray coating, dip coating, hot melt coating, bar coating, applicator, air knife coating, curtain flow coating, offset printing, brush coating, and full-surface printing using screen printing.
[0278] The resin varnish may be applied in several steps, may be applied in one step, or may be applied by combining a plurality of different methods. Among them, the die coating method, which has excellent uniformity of application, is preferable. In addition, in order to prevent contamination by foreign matter, it is preferable to carry out the application process in an environment where foreign matter generation is low, such as a clean room.
[0279] After the resin varnish is applied, it is dried in a drying oven such as a hot air oven or a far infrared oven as necessary. The drying conditions are preferably 80° C. to 120° C. for 3 minutes to 13 minutes. In this manner, a photosensitive resin composition layer is formed on the circuit board.
[0280] Examples of the circuit board include a substrate having a support substrate such as a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The circuit board may be a substrate having a patterned conductor layer (circuit) formed on one or both sides of the support substrate. The circuit board may also include a substrate having a multi-layer structure in which conductor layers and insulating layers are alternately laminated, in which one or both sides of the outermost layer of the circuit board are patterned conductor layers (circuits). The surface of the conductor layer may be previously roughened by blackening, copper etching, or the like.
[0281] On the other hand, when a photosensitive film is used, the photosensitive film is laminated on one or both sides of the circuit board using a vacuum laminator. Such lamination is usually performed so that the photosensitive resin composition layer is bonded to the circuit board. When the photosensitive film has a protective film, the protective film is removed before lamination. Lamination can be performed by preheating the photosensitive film and the circuit board as necessary, and pressing the photosensitive resin composition layer onto the circuit board while applying pressure and heat. For the photosensitive film, a method of laminating the film onto the circuit board under reduced pressure by a vacuum lamination method is preferably used.
[0282] The lamination conditions are not particularly limited, but for example, the pressure bonding temperature (lamination temperature) is preferably 70° C. to 140° C., and the pressure bonding pressure is preferably 1 kgf / cm. 2 ~11kgf / cm 2 (9.8×10 4 N / m 2 ~107.9×10 4 N / m 2 ), the pressure bonding time is preferably 5 seconds to 300 seconds, and lamination is preferably performed under reduced pressure with an air pressure of 20 mmHg (26.7 hPa) or less. The lamination process may be a batch process or a continuous process using rolls. The vacuum lamination method can be performed using a commercially available vacuum laminator. Examples of commercially available vacuum laminators include a vacuum applicator manufactured by Nikko Materials Co., Ltd., a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a roll-type dry coater manufactured by Hitachi Industries Co., Ltd., and a vacuum laminator manufactured by Hitachi AIC Co., Ltd.
[0283] -Process (II)- The manufacturing method of a semiconductor package substrate according to the first example includes a step (II) of irradiating the photosensitive resin composition layer with active light after forming a photosensitive resin composition layer on a circuit board. In this step (II), an exposure treatment is usually performed in which active light is irradiated to a predetermined portion of the photosensitive resin composition layer through a mask. Examples of active light include ultraviolet light, visible light, electron beams, and X-rays, and ultraviolet light is particularly preferred. The irradiation dose of ultraviolet light is usually 10 mJ / cm. 2 ~1000mJ / cm 2 There are two types of exposure methods: contact exposure, in which a mask is brought into close contact with the circuit board, and non-contact exposure, in which a parallel beam is used for exposure without contact, and either method may be used.
[0284] In step (II), for example, a mask having a via pattern such as a round hole pattern may be used to perform exposure processing to form a latent image corresponding to the via hole. The via diameter (opening diameter) of the via hole is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less. The lower limit is not particularly limited, but may be 0.1 μm or more, 0.5 μm or more, etc.
[0285] After the exposure, a heat treatment may be carried out as necessary. The heat treatment can quickly reduce the solubility of the exposed portion of the photosensitive resin composition layer in a developer.
[0286] -Process (III)- The method for producing a semiconductor package substrate according to the first example includes a step (III) of developing the photosensitive resin composition layer after the exposure in the step (II). In this step (III), the unexposed portion of the photosensitive resin composition layer is usually removed with a developer. By the development, holes such as via holes are formed in the photosensitive resin composition layer, and a desired pattern can be obtained. The development is usually performed by wet development.
[0287] In the case of the wet development, a developer that is safe, stable, and easy to operate is used, such as an alkaline solution, an aqueous developer, an organic solvent, etc. As a developing method, a known method such as spraying, rocking immersion, brushing, scraping, etc. is appropriately adopted.
[0288] Examples of alkaline aqueous solutions used as the developer include aqueous solutions of alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide, carbonates or bicarbonates such as sodium carbonate and sodium bicarbonate, alkali metal phosphates such as sodium phosphate and potassium phosphate, alkali metal pyrophosphates such as sodium pyrophosphate and potassium pyrophosphate, and aqueous solutions of organic bases that do not contain metal ions, such as tetraalkylammonium hydroxide. An aqueous solution of tetramethylammonium hydroxide (TMAH) is preferred because it does not contain metal ions and does not affect the semiconductor chip.
[0289] These alkaline aqueous solutions may contain additives such as surfactants and antifoaming agents to improve the development effect. The pH of the alkaline aqueous solution is, for example, preferably in the range of 8 to 12, more preferably in the range of 9 to 11. The base concentration of the alkaline aqueous solution is preferably 0.1% by mass to 10% by mass. The temperature of the alkaline aqueous solution can be appropriately selected according to the developability of the photosensitive resin composition layer, and is preferably 20°C to 50°C.
[0290] Examples of organic solvents used as developers include acetone, ethyl acetate, alkoxyethanols having an alkoxy group having 1 to 4 carbon atoms, ethyl alcohol, isopropyl alcohol, butyl alcohol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, cyclopentanone, and cyclohexanone.
[0291] The concentration of such an organic solvent is preferably 2% by mass to 90% by mass based on the total amount of the developer. The temperature of such an organic solvent can be adjusted according to the developability. Furthermore, such an organic solvent can be used alone or in combination of two or more kinds. Examples of organic solvent-based developers used alone include 1,1,1-trichloroethane, N-methylpyrrolidone, N,N-dimethylformamide, cyclopentanone, cyclohexanone, methyl isobutyl ketone, and γ-butyrolactone.
[0292] In forming a pattern, two or more kinds of developing methods may be used in combination as necessary. The developing methods include a dip method, a bath method, a spray method, a high-pressure spray method, brushing, slapping, etc., and the high-pressure spray method is suitable for improving resolution. When adopting a spray method, the spray pressure is preferably 0.05 MPa to 0.3 MPa.
[0293] -Optional process- The method for producing a semiconductor package substrate according to the first example may further include any step in combination with the above-mentioned steps (I) to (III). For example, the method for producing a semiconductor package substrate may include a heat curing (post-baking) step as necessary after the completion of step (III). The curing of the photosensitive resin composition layer can proceed in the above-mentioned steps (I) to (III), but the heat curing step can further proceed the curing of the photosensitive resin composition to obtain an insulating layer with excellent mechanical strength.
[0294] The thermal curing step may be, for example, a heating step using a clean oven. The thermal curing may be carried out in air or in an inert gas atmosphere such as nitrogen. The heating conditions may be appropriately selected depending on factors such as the type and content of the resin component in the photosensitive resin composition. Specific heating conditions are preferably selected from the range of 150°C to 250°C for 20 minutes to 180 minutes, more preferably 160°C to 230°C for 30 minutes to 120 minutes.
[0295] The method for producing a semiconductor package substrate according to the first example may further include a drilling step and a desmearing step after forming an insulating layer as a cured photosensitive resin composition layer. These steps may be performed according to various methods known to those skilled in the art for use in the production of semiconductor package substrates.
[0296] After forming the insulating layer, if desired, a hole-making process may be performed on the insulating layer formed on the circuit board to form holes such as via holes and through holes. The hole-making process may be performed by a known method such as a drill, a laser, or plasma, or by a combination of these methods as necessary. Among these, a hole-making process using a laser such as a carbon dioxide laser or a YAG laser is preferred.
[0297] The desmear process is a process of performing a desmear treatment on an insulating layer. Generally, resin residue (smear) adheres to the inside of holes such as via holes and through holes formed in the drilling process. Since such smears can cause poor electrical connection, it is preferable to perform a process to remove the smears (desmear treatment) in this process.
[0298] The desmear treatment may be performed by a dry desmear treatment, a wet desmear treatment, or a combination thereof.
[0299] An example of the dry desmear treatment is a desmear treatment using plasma. The desmear treatment using plasma can be performed using a commercially available plasma desmear treatment device. Among the commercially available plasma desmear treatment devices, examples suitable for manufacturing semiconductor package substrates include a microwave plasma device manufactured by Nissin Co., Ltd. and an atmospheric pressure plasma etching device manufactured by Sekisui Chemical Co., Ltd.
[0300] The wet desmear treatment may be, for example, a desmear treatment using an oxidizing agent solution. When the desmear treatment is performed using an oxidizing agent solution, it is preferable to perform a swelling treatment using a swelling liquid, an oxidation treatment using an oxidizing agent solution, and a neutralization treatment using a neutralizing liquid in this order. Examples of the swelling liquid include "Swelling Dip Securigance P" and "Swelling Dip Securigance SBU" manufactured by Atotech Japan. The swelling treatment is preferably performed by immersing a substrate having a hole such as a via hole in a swelling liquid heated to 60°C to 80°C for 5 to 10 minutes. The oxidizing agent solution is preferably an alkaline permanganate solution, and examples of the solution include a solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The oxidation treatment using an oxidizing agent solution is preferably performed by immersing a substrate after the swelling treatment in an oxidizing agent solution heated to 60°C to 80°C for 10 to 30 minutes. Commercially available alkaline permanganate aqueous solutions include, for example, "Concentrate Compact CP" and "Dosing Solution Securiganth P" manufactured by Atotech Japan. The neutralization treatment using a neutralizing solution is preferably carried out by immersing the substrate after the oxidation treatment in the neutralizing solution at 30°C to 50°C for 3 to 10 minutes. The neutralizing solution is preferably an acidic aqueous solution, and a commercially available product thereof is, for example, "Reduction Solution Securiganth P" manufactured by Atotech Japan.
[0301] When the dry desmear treatment and the wet desmear treatment are performed in combination, the dry desmear treatment may be performed first, or the wet desmear treatment may be performed first.
[0302] In the case where the insulating layer is formed as any of a redistribution layer, an interlayer insulating layer, and a solder resist, a hole drilling step and a desmearing step may be performed after the thermal curing step. In addition, in the manufacturing method of the semiconductor package substrate, a conductor layer forming step may be further performed.
[0303] The conductor layer forming step is a step of forming a conductor layer on an insulating layer. The conductor layer may be formed by sputtering after the insulating layer is formed. The conductor layer may also be formed by a combination of electroless plating and electrolytic plating. Furthermore, a plating resist having a reverse pattern to the conductor layer may be formed, and the conductor layer may be formed only by electroless plating. As a method for subsequent pattern formation, for example, a subtractive method, a semi-additive method, or the like known to those skilled in the art may be used.
[0304] In the second example, the semiconductor package substrate can be manufactured using the above-mentioned photosensitive resin composition, and the cured product of the photosensitive resin composition is used as a rewiring formation layer. Specifically, the manufacturing method of the semiconductor package substrate according to the second example includes the following steps: (A) a step of laminating a temporary fixing film on a substrate; (B) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (C) forming an encapsulation layer on the semiconductor chip; (D) peeling the substrate and the temporary fixing film from the semiconductor chip; (E) a step of forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off; (F) forming a rewiring layer as a conductor layer on the rewiring formation layer; and (G) forming a solder resist layer on the rewiring layer; The method for manufacturing a semiconductor package substrate includes: (H) dicing the plurality of semiconductor package substrates into individual semiconductor package substrates; may also include
[0305] -Process (A)- Step (A) is a step of laminating a temporary fixing film on a substrate. The lamination conditions for the substrate and the temporary fixing film are not particularly limited, but for example, the pressure bonding temperature (lamination temperature) is preferably 70° C. to 140° C., and the pressure bonding pressure is preferably 1 kgf / cm. 2 ~11kgf / cm 2The pressure bonding time is preferably 5 to 300 seconds, and lamination is preferably performed under reduced pressure with an air pressure of 20 mmHg or less. The lamination process may be a batch process or a continuous process using rolls. The vacuum lamination method can be performed using a commercially available vacuum laminator. Examples of commercially available vacuum laminators include a vacuum applicator manufactured by Nikko Materials Co., Ltd., a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a roll-type dry coater manufactured by Hitachi Industries Co., Ltd., and a vacuum laminator manufactured by Hitachi AIC Co., Ltd.
[0306] Examples of the substrate include silicon wafers; glass wafers; glass substrates; metal substrates such as copper, titanium, stainless steel, and cold-rolled steel (SPCC); substrates such as FR-4 substrates in which glass fibers are impregnated with epoxy resin or the like and then heat-cured; and substrates made of bismaleimide triazine resins such as BT resin.
[0307] The temporary fixing film may be made of any material that can be peeled off from the semiconductor chip and can temporarily fix the semiconductor chip. Commercially available products include "Riva Alpha" manufactured by Nitto Denko Corporation.
[0308] -Process (B)- Step (B) is a step of temporarily fixing the semiconductor chip on the temporary fixing film. The temporary fixing of the semiconductor chip can be performed using, for example, a device such as a flip chip bonder or a die bonder. The layout and number of the semiconductor chips can be appropriately set depending on the shape and size of the temporary fixing film, the number of semiconductor packages to be produced, etc. For example, the semiconductor chips may be temporarily fixed by arranging them in a matrix shape of multiple rows and multiple columns.
[0309] -Process (C)- Step (C) is a step of forming an encapsulating layer on the semiconductor chip. The encapsulating layer can be made of any material having insulating properties, and the above-mentioned photosensitive resin composition can be used. The encapsulating layer is usually formed by a method including a step of forming an encapsulating resin composition layer on the semiconductor chip and a step of curing the resin composition layer to form the encapsulating layer.
[0310] The formation of the encapsulating resin composition layer is preferably carried out by a compression molding method, in which a semiconductor chip and an encapsulating resin composition are usually placed in a mold, and pressure and, if necessary, heat are applied to the encapsulating resin composition in the mold to form an encapsulating resin composition layer that covers the semiconductor chip.
[0311] A specific operation of the compression molding method may be, for example, as follows. An upper mold and a lower mold are prepared as molds for compression molding. An encapsulating resin composition is applied to the semiconductor chip temporarily fixed on the temporary fixing film as described above. The semiconductor chip to which the encapsulating resin composition is applied is attached to the lower mold together with the substrate and the temporary fixing film. Then, the upper mold and the lower mold are clamped, and heat and pressure are applied to the encapsulating resin composition to perform compression molding.
[0312] A specific operation of the compression molding method may be, for example, as follows. An upper mold and a lower mold are prepared as molds for compression molding. An encapsulating resin composition is placed on the lower mold. A semiconductor chip is attached to the upper mold together with a substrate and a temporary fixing film. Then, the upper mold and the lower mold are clamped together so that the encapsulating resin composition placed on the lower mold contacts the semiconductor chip attached to the upper mold, and heat and pressure are applied to perform compression molding.
[0313] The molding conditions vary depending on the composition of the encapsulating resin composition, and appropriate conditions can be adopted so that good encapsulation is achieved. For example, the temperature of the mold during molding is preferably a temperature at which the encapsulating resin composition can exhibit excellent compression moldability, and is preferably 80°C or higher, more preferably 100°C or higher, particularly preferably 120°C or higher, and preferably 200°C or lower, more preferably 170°C or lower, and particularly preferably 150°C or lower. The pressure applied during molding is preferably 1 MPa or higher, more preferably 3 MPa or higher, particularly preferably 5 MPa or higher, and preferably 50 MPa or lower, more preferably 30 MPa or lower, and particularly preferably 20 MPa or lower. The cure time is preferably 1 minute or more, more preferably 2 minutes or more, particularly preferably 5 minutes or more, and preferably 60 minutes or lower, more preferably 30 minutes or lower, and particularly preferably 20 minutes or lower. Usually, the mold is removed after the encapsulating resin composition layer is formed. The mold may be removed before or after the encapsulating resin composition layer is cured.
[0314] The compression molding method may be performed by discharging the encapsulating resin composition filled in a cartridge into a lower mold.
[0315] -Process (D)- Step (D) is a step of peeling off the substrate and the temporary fixing film from the semiconductor chip. It is desirable to adopt an appropriate peeling method according to the material of the temporary fixing film. For example, the peeling method may be a method of heating, foaming or expanding the temporary fixing film to peel it off. In addition, for example, the peeling method may be a method of irradiating the temporary fixing film with ultraviolet light through the substrate to reduce the adhesive strength of the temporary fixing film to peel it off.
[0316] In the method of peeling off the temporary fixing film by heating, foaming or expanding it, the heating conditions are usually 100° C. to 250° C. for 1 second to 90 seconds or 5 minutes to 15 minutes. In the method of peeling off the temporary fixing film by reducing the adhesive strength of the temporary fixing film by irradiating it with ultraviolet light, the irradiation amount of ultraviolet light is usually 10 mJ / cm 2 ~1000mJ / cm 2 It is.
[0317] -Process (E)- Step (E) is a step of forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film are peeled off. The rewiring formation layer can be formed using the above-mentioned photosensitive resin composition. The method for forming the rewiring formation layer can include forming a photosensitive resin composition layer in the same manner as in step (I) in the first example.
[0318] When forming the rewiring formation layer, via holes may be formed in the rewiring formation layer to provide interlayer connection between the semiconductor chip and the rewiring layer.
[0319] The via hole can be formed by carrying out an exposure step of irradiating the surface of the photosensitive resin composition layer for forming the rewiring formation layer with active light through a mask, and a development step of developing and removing the non-exposed portion not irradiated with active light. The amount and time of irradiation of the active light can be appropriately set according to the photosensitive resin composition layer. Examples of the exposure method include a contact exposure method in which a mask is closely attached to the photosensitive resin composition layer and exposed, and a non-contact exposure method in which a mask is not closely attached to the photosensitive resin composition layer and exposed using parallel light. The exposure and development methods can be carried out as described in the first example.
[0320] The shape of the via hole is not particularly limited, but is generally circular (approximately circular). The top diameter of the via hole is preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 20 μm or less, and is preferably 0.1 μm or more, preferably 0.5 μm or more, and more preferably 1.0 μm or more. Here, the top diameter of the via hole refers to the diameter of the opening of the via hole on the surface of the rewiring formation layer.
[0321] After forming the photosensitive resin composition layer and forming via holes as necessary, a thermal curing step may be carried out. The thermal curing method may be the same as that described in the first example.
[0322] -Process (F)- Step (F) is a step of forming a redistribution layer as a conductor layer on the redistribution formation layer. The method of forming the redistribution layer on the redistribution formation layer can be the same as the method of forming a conductor layer on an insulating layer in the first example. Steps (E) and (F) may be repeated to alternately stack (build up) the redistribution formation layer and the redistribution layer.
[0323] -Process (G)- Step (G) is a step of forming a solder resist layer on the rewiring layer. Any material having insulating properties can be used as the material of the solder resist layer. Among them, photosensitive resins and thermosetting resins are preferred from the viewpoint of ease of manufacturing the semiconductor package substrate. The above-mentioned photosensitive resin composition may be used as the material of the solder resist layer.
[0324] In step (G), bumping processing may be performed to form bumps, if necessary. The bumping processing can be performed by a method such as solder balls or solder plating. In addition, the formation of via holes in the bumping processing can be performed in the same manner as in step (E).
[0325] The method for manufacturing a semiconductor package substrate may include a step (H) in addition to the steps (A) to (G). The step (H) is a step of dicing a plurality of semiconductor package substrates into individual semiconductor package substrates to separate them. The method for dicing the semiconductor package substrates into individual semiconductor package substrates is not particularly limited.
[0326] <Semiconductor device> A semiconductor device according to an embodiment of the present invention includes the above-mentioned semiconductor package substrate. Examples of the semiconductor device on which the semiconductor package substrate is mounted include various semiconductor devices used in electrical products (e.g., computers, mobile phones, smartphones, tablet devices, wearable devices, digital cameras, medical devices, televisions, etc.) and vehicles (e.g., motorcycles, automobiles, trains, ships, aircraft, etc.). EXAMPLES
[0327] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. In the following description, the terms "parts" and "%" used to express amounts refer to "parts by mass" and "% by mass", respectively, unless otherwise specified. Furthermore, the operations described below were carried out in the atmosphere at room temperature and normal pressure (25°C and 1 atm) unless otherwise specified.
[0328] <Synthesis Example 1: Synthesis of Polyimide Resin A1> 25.8 g of 3,3',4,4'-benzophenonetetracarboxylic dianhydride was placed in a 1 L separable flask, and 500 mL of N-methyl-2-pyrrolidone was added to the separable flask and stirred at room temperature. 26.9 g of 4,4'-diaminophenyloxide (ODA) was then added to the separable flask, and the flask was heated in an oil bath until the internal temperature reached 40°C, and polymerization was carried out for 5 hours.
[0329] Next, 1 mL of triethylamine, 0.43 g of piperazine, and 17.1 g of ethylene glycol monoacetoacetate monomethacrylate were added to the reaction liquid, which was then heated to 100° C. and stirred for 5 hours.
[0330] Next, 10.4 g of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA) was added to the reaction solution, and the reaction solution was heated to 80° C. and stirred for 3 hours. 120 mL of n-heptane was added, and azeotropic dehydration was carried out for 5 hours.
[0331] Next, the obtained reaction solution was dropped into 6 L of ultrapure water to precipitate polyimide resin A1, thereby purifying it. The purified polyimide resin A1 was filtered and then dried under heating at 80°C in a vacuum dryer to obtain 60 g of polyimide resin A1 containing a structure represented by the following formula (A1). The weight average molecular weight of polyimide resin A1 was measured by gel permeation chromatography (standard polystyrene equivalent) to be 40,000. The infrared absorption spectrum (IR spectrum) of the obtained polyimide resin A1 was as follows. IR(cm -1): 1750, 1650, 1593, 1497, 1462, 1415, 1385, 1365, 1307, 1279, 1241, 1160, 1113, 1058, 1014, 966, 929, 874, 842, 768, 698, 607, 587, 563, 530
[0332] [ka]
[0333] <Synthesis Example 2: Synthesis of Polyimide Resin A2> 25.8 g of 3,3',4,4'-benzophenonetetracarboxylic dianhydride was placed in a 1 L separable flask, and 500 mL of N-methyl-2-pyrrolidone was added to the separable flask and stirred at room temperature. 26.9 g of 4,4'-diaminophenyloxide (ODA) was then added to the separable flask, and the flask was heated in an oil bath until the internal temperature reached 40°C, and polymerization was carried out for 5 hours.
[0334] Next, 1 mL of triethylamine, 0.43 g of piperazine, 11.5 g of Meldrum's acid in N-methylpyrrolidone were added to the reaction solution, and the mixture was stirred for 5 hours at 40° C. 9.3 g of hydroxyethyl acrylate was added, and the mixture was stirred for 2 hours at 100° C.
[0335] Next, 10.4 g of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA) was added to the reaction solution, and the reaction solution was heated to 80° C. and stirred for 3 hours. 120 mL of n-heptane was added, and azeotropic dehydration was carried out for 5 hours.
[0336] Next, the obtained reaction solution was dropped into 6 L of ultrapure water to precipitate polyimide resin A2, which was then purified. The purified polyimide resin A2 was filtered and then dried under heating at 80°C in a vacuum dryer to obtain 50 g of polyimide resin A2 having a structure represented by the following formula (A2). The weight average molecular weight of polyimide resin A2 was measured by gel permeation chromatography (standard polystyrene equivalent) to be 35,000.
[0337] [ka]
[0338] <Synthesis Example 3: Synthesis of polyimide resin A3> 21.2 g of 4,4'-diaminobenzophenone was placed in a 1 L separable flask, and 500 mL of N-methyl-2-pyrrolidone was placed in the separable flask and stirred at room temperature. 1 mL of triethylamine, 0.43 g of piperazine, and 21.4 g of ethylene glycol monoacetoacetate monomethacrylate were added, heated to 100°C, and stirred for 5 hours.
[0339] Next, 52.0 g of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA) was added to the reaction solution, and the reaction solution was heated to 80° C. and stirred for 10 hours. 120 mL of n-heptane was added, and azeotropic dehydration was carried out for 5 hours.
[0340] Next, the obtained reaction solution was dropped into 6 L of ultrapure water to precipitate polyimide resin A3, which was then purified. The purified polyimide resin A3 was filtered off and then dried under heating at 80°C in a vacuum dryer to obtain 70 g of polyimide A3 containing a structure represented by the following formula (A3). The weight average molecular weight of polyimide resin A3 was measured by gel permeation chromatography (standard polystyrene equivalent) to be 42,000. The infrared absorption spectrum (IR spectrum) of the obtained polyimide resin A3 was as follows. IR(cm -1): 1775, 1723, 1650, 1591, 1496, 1471, 1415, 1367, 1305, 1277, 1238, 1159, 1062, 1035, 1013, 930, 836, 766, 597, 553, 503, 430
[0341] [ka]
[0342] <Synthesis Example 4: Synthesis of Polyimide Resin A4> 21.2g of 4,4'-diaminobenzophenone was placed in a 1L separable flask, and 500mL of N-methyl-2-pyrrolidone was added to the separable flask and stirred at room temperature. 1mL of triethylamine, 0.43g of piperazine, 11.5g of Meldrum's acid, and N-methylpyrrolidone were added, and the mixture was stirred at 40°C for 5 hours. 9.3g of hydroxyethyl acrylate was added, and the mixture was stirred at 100°C for 2 hours.
[0343] Next, 52.0 g of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA) was added to the reaction solution, and the reaction solution was heated to 80° C. and stirred for 10 hours. 120 mL of n-heptane was added, and azeotropic dehydration was carried out for 5 hours.
[0344] Next, the obtained reaction solution was dropped into 6 L of ultrapure water to precipitate and purify polyimide resin A4. The purified polyimide resin A4 was filtered and then dried under heating at 80°C in a vacuum dryer to obtain 65 g of polyimide resin A4 having a structure represented by the following formula (A4). The weight average molecular weight of polyimide resin A4 was measured by gel permeation chromatography (standard polystyrene equivalent) to be 38,000.
[0345] [ka]
[0346] <Synthesis Example 5: Synthesis of Polyimide Resin A5> 21.2 g of 4,4'-diaminobenzophenone was placed in a 1 L separable flask, and 500 mL of N-methyl-2-pyrrolidone was placed in the separable flask and stirred at room temperature. 1 mL of triethylamine, 0.43 g of piperazine, and 21.4 g of ethylene glycol monoacetoacetate monomethacrylate were added, heated to 100°C, and stirred for 5 hours.
[0347] Next, 29.4 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (sBPDA) was added to the reaction solution, and the reaction solution was heated to 80° C. and stirred for 10 hours. 120 mL of n-heptane was added, and azeotropic dehydration was carried out for 5 hours.
[0348] Next, the obtained reaction solution was dropped into 6 L of ultrapure water to precipitate polyimide resin A5, which was then purified. The purified polyimide resin A5 was filtered off and then dried under heating at 80°C in a vacuum dryer to obtain 40 g of polyimide resin A5 containing a structure represented by the following formula (A5). The weight average molecular weight of polyimide resin A5 was measured by gel permeation chromatography (standard polystyrene equivalent) to be 32,000. The infrared absorption spectrum (IR spectrum) of the obtained polyimide resin A5 was as follows. IR(cm -1 ):1751, 1652, 1593, 1500, 1465, 1390, 1360, 1307, 1280, 1250, 1160, 1110,, 1014, 967, 940, 881, 843, 770, 698, 610, 590, 530
[0349] [ka]
[0350] <Synthesis Example 6: Synthesis of Polyimide Resin A6> 23.8 g of 1,4-diaminoanthraquinone was placed in a 1 L separable flask, and 500 mL of N-methyl-2-pyrrolidone was placed in the separable flask and stirred at room temperature. 1 mL of triethylamine, 0.43 g of piperazine, and 21.4 g of ethylene glycol monoacetoacetate monomethacrylate were added, heated to 100°C, and stirred for 5 hours.
[0351] Next, 52.0 g of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA) was added to the reaction solution, and the reaction solution was heated to 80° C. and stirred for 10 hours. 120 mL of n-heptane was added, and azeotropic dehydration was carried out for 5 hours.
[0352] Next, the obtained reaction solution was dropped into 6 L of ultrapure water to precipitate polyimide resin A6, which was then purified. The purified polyimide resin A6 was filtered and then dried under heating at 80°C in a vacuum dryer to obtain 70 g of polyimide resin A6 having a structure represented by the following formula (A6). The weight average molecular weight of polyimide resin A6 was measured by gel permeation chromatography (standard polystyrene equivalent) to be 42,000.
[0353] [ka]
[0354] <Synthesis Example 7: Synthesis of polyimide resin A7> 25.8 g of 3,3',4,4'-benzophenonetetracarboxylic dianhydride was placed in a 1 L separable flask, and 500 mL of N-methyl-2-pyrrolidone was added to the separable flask and stirred at room temperature. 26.9 g of 4,4'-diaminophenyloxide (ODA) was then added to the separable flask, and the flask was heated in an oil bath until the internal temperature reached 40°C, and polymerization was carried out for 5 hours.
[0355] Next, 10.4 g of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA) was added to the reaction solution, and the reaction solution was heated to 80° C. and stirred for 3 hours. 120 mL of n-heptane was added, and azeotropic dehydration was carried out for 5 hours.
[0356] Next, the obtained reaction solution was dropped into 6 L of ultrapure water to precipitate polyimide resin A7, which was then purified. The purified polyimide resin A7 was filtered and then dried under heating at 80°C in a vacuum dryer to obtain 65 g of polyimide resin A7 having a structure represented by the following formula (A7). The weight average molecular weight of polyimide resin A7 was measured by gel permeation chromatography (standard polystyrene equivalent) to be 31,000.
[0357] [ka]
[0358] <Synthesis Example 8: Synthesis of Polyimide A8> 52.0 g of 2,2-bis 4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA) and 300 g of gamma-butyrolactone were placed in a 1 L separable flask and dissolved. 26.9 g of 4,4'-diaminophenyloxide (ODA) was added thereto and reacted at 50°C for 20 hours to obtain polyamic acid (polyimide precursor). 55 g of toluene was added thereto and azeotropic dehydration was performed for 5 hours. After that, the reaction solution was heated until the temperature reached 204°C to remove the toluene, and a polyimide solution was obtained.
[0359] Next, the obtained polyimide solution was dropped into 6 L of ultrapure water to precipitate polyimide resin A8, which was then purified. The purified polyimide resin A8 was filtered and then dried under heating at 80°C in a vacuum dryer to obtain 65 g of polyimide resin A8 containing a structure represented by the following formula (A8). The weight average molecular weight of polyimide resin A8 was measured by gel permeation chromatography (standard polystyrene equivalent) to be 40,000.
[0360] [ka]
[0361] <Synthesis Example 9: Synthesis of Polyimide Resin A9> 104g of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA) and 300g of γ-butyrolactone were placed in a 1L separable flask and dissolved. 60.1g of 5,5'-methylenebis(2-aminobenzoic acid) (MBAA) was added thereto and reacted at 50°C for 20 hours to obtain polyamic acid (polyimide precursor). 55g of toluene was added thereto and azeotropic dehydration was performed for 5 hours. Thereafter, the reaction solution was heated until the temperature reached 204°C to remove the toluene, obtaining a polyimide solution. After cooling to room temperature, 59.6g of glycidyl methacrylate and 0.45g of 4-methoxyphenol were added thereto and reacted at 100°C for 5 hours.
[0362] Next, the obtained polyimide solution was dropped into 6 L of ultrapure water to precipitate polyimide resin A9, which was purified. The purified polyimide resin A9 was filtered and then dried under heating at 80°C in a vacuum dryer to obtain 70 g of polyimide resin A9 having a structure represented by the following formula (A9). The weight average molecular weight of polyimide resin A9 was measured by gel permeation chromatography (standard polystyrene equivalent) to be 41,000.
[0363] [ka]
[0364] <Production of Photosensitive Resin Composition> Each photosensitive resin composition was prepared by dissolving each component in 400 parts by mass of γ-butyrolactone (GBL) as a solvent according to the blending amounts (unit: parts by mass) in the following Tables 1 and 2. In the tables, the blending amount of each component indicates the amount of non-volatile components.
[0365] The abbreviations in the table have the following meanings:
[0366] (Component (A): Polyimide resin) A1: Polyimide resin A1 synthesized in Synthesis Example 1 A2: Polyimide resin A2 synthesized in Synthesis Example 2 A3: Polyimide resin A3 synthesized in Synthesis Example 3 A4: Polyimide resin A4 synthesized in Synthesis Example 4 A5: Polyimide resin A5 synthesized in Synthesis Example 5 A6: Polyimide resin A6 synthesized in Synthesis Example 6 A7: Polyimide resin A7 synthesized in Synthesis Example 7 A8: Polyimide resin A8 synthesized in Synthesis Example 8 A9: Polyimide resin A9 synthesized in Synthesis Example 9
[0367] (Component (B): Crosslinking agent) B1: a compound represented by the following structural formula (B1): [ka]
[0368] (Component (C): Photoradical generator) C1: A compound represented by the following structure (C1) (Irgacure-OXE02: manufactured by BASF) [ka]
[0369] (Component (D): Sensitizer) D1: A compound represented by the following structural formula (D1): [ka]
[0370] <Production of photosensitive film> A PET film (polyethylene terephthalate film; Toray Industries, Inc., "Lumirror T6AM", thickness 38 μm) was prepared as a support. The above-mentioned photosensitive resin composition was uniformly applied to the PET film using a die coater so that the thickness of the photosensitive resin composition layer after drying was 30 μm, and the film was dried at 80° C. to 120° C. for 6 minutes to form a photosensitive resin composition layer. Next, a cover film (biaxially oriented polypropylene film, Oji F-Tex Co., Ltd., "MA-411") was placed on the surface of the photosensitive resin composition layer as a protective film, and laminated at 80° C. to produce a photosensitive film having a three-layer structure of support / photosensitive resin composition layer / cover film.
[0371] <Test 1. Measurement of dielectric constant and dielectric tangent> The photosensitive resin composition layer was peeled off from the photosensitive film and attached to a metal frame using heat-resistant tape. The photosensitive resin composition layer was irradiated with ultraviolet light (wavelength 365 nm, intensity 40 mW / cm 2 ) was exposed to light at an exposure dose of 1000 mJ. This photosensitive resin composition layer was cured under conditions of 200°C for 2 hours to obtain a film for measuring physical properties corresponding to the cured product of the photosensitive resin composition layer. A test piece having a width of 2 mm and a length of 80 mm was cut out from the film for measuring physical properties. The relative permittivity and dielectric loss tangent of the cut out test piece were measured at a measurement frequency of 5.8 GHz and a measurement temperature of 23°C by a cavity resonance perturbation method using a measuring device "HP8362B" manufactured by Agilent Technologies. Based on the measured dielectric loss tangent, the electrical properties were evaluated according to the following criteria. Dielectric tangent less than 0.01: 〇 Dielectric tangent is 0.01 or more: ×
[0372] <Test 2. Evaluation of film remaining rate> A copper plating layer was formed on a silicon wafer with a thickness of 10 μm, and the copper plating layer was subjected to a phobic treatment with a 1% hydrochloric acid aqueous solution for 10 seconds to prepare a circuit board. The above-mentioned photosensitive resin composition was applied onto the circuit board using a spin coater at a rotation speed suitable for a thickness of 15 μm, and heated on a hot plate at 120° C. for 5 minutes to form a photosensitive resin composition layer (thickness 15 μm).
[0373] The photosensitive resin composition layer was irradiated with ultraviolet light (wavelength 365 nm, intensity 40 mW / cm 2 The exposure was 50 mJ / cm 2 to 1000mJ / cm 2 The optimal value was set in the range of
[0374] Next, the entire surface of the photosensitive resin composition layer was spray-developed with cyclopentanone as a developer at a spray pressure of 0.2 MPa for 120 seconds, followed by spray rinsing with 2-methoxy-1-methylethyl acetate (PGMEA) at a spray pressure of 0.2 MPa for 30 seconds. Thereafter, the thickness of the photosensitive resin composition was measured. The thickness was measured using a small film thickness meter "mini-lab film-150" manufactured by Avantes. The thickness of the photosensitive resin composition layer after development (film thickness after development) was divided by the thickness of the photosensitive resin composition layer before exposure (initial film thickness) to calculate the remaining film ratio. The obtained remaining film ratio was evaluated according to the following criteria. Remaining film rate is 70% or more: 〇 Residual film rate is less than 70%: ×
[0375] <Result> The results of the above-mentioned Examples and Comparative Examples are shown in the following Tables 1 and 2. In the following tables, the meanings of the abbreviations are as follows. Dk: relative dielectric constant. Df: Dielectric tangent.
[0376] [Table 1]
[0377] [Table 2]
Claims
1. A polyimide resin comprising a repeating unit represented by the following formula (1): [Formula 1] (In formula (1), X 1 represents a tetravalent organic group, Y 1 represents a divalent organic group, X 1 and Y 1 At least one of the above contains at least two benzene rings and a divalent group represented by formula (1-1) linking the two benzene rings. [chemical 2] (In formula (1-1), R 1 and R 2 is a hydrogen atom, -CN, -NO 2 , -COH, -R, -OR, -COR, -COOR, -CONHR, -CONR 2 , -SR, -SOR, or -SO 2 Indicates R, R 1 and R 2 At least one of the above contains an ethylenically unsaturated bond, R 1 and R 2 may be joined together to form a non-aromatic ring which may have a substituent; Each R independently represents an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent. * represents a bond.)
2. In formula (1), X 1 The polyimide resin according to claim 1, wherein the polyimide resin comprises one or more structures selected from the group consisting of a structure represented by the following formula (X1-1) and a structure represented by the following formula (X1-2): [C3] (In formula (X1-1) and formula (X1-2), R 11 and R 12is a hydrogen atom, -CN, -NO 2 , -COH, -R, -OR, -COR, -COOR, -CONHR, -CONR 2 , -SR, -SOR, or -SO 2 Indicates R, R 11 and R 12 At least one of the above contains an ethylenically unsaturated bond, R 11 and R 12 may be joined together to form a non-aromatic ring which may have a substituent; R each independently represents an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent; R 13 and R 14 each independently represents a substituent; L 1 represents a divalent organic group; n 11 and n 12 each independently represents an integer of 0 or more and 3 or less; n 13 and n 14 each independently represents an integer of 0 or more and 2 or less. * represents a bond.)
3. L 1 is a methylene group, -C(=O)-, or -C(=CR 11 R 12 3. The polyimide resin according to claim 2, wherein
4. In formula (1), Y 1 contains one or more structures selected from the group consisting of a structure represented by the following formula (Y1-1), a structure represented by the following formula (Y1-2), a structure represented by the following formula (Y1-3), and a structure represented by the following formula (Y1-4). [C4] (In the formulas (Y1-1), (Y1-2), (Y1-3) and (Y1-4), R 21 and R 22 is a hydrogen atom, -CN, -NO 2 , -COH, -R, -OR, -COR, -COOR, -CONHR, -CONR 2 , -SR, -SOR, or -SO 2 Indicates R, R 21 and R 22 At least one of the above contains an ethylenically unsaturated bond, R 21 and R 22 may be joined together to form a non-aromatic ring which may have a substituent; R each independently represents an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent; R 23 and R 24 each independently represents a substituent; L 2 represents a divalent organic group; n 21 and n 22 each independently represents an integer of 0 to 4; n 23 and n 24 each independently represents an integer of 0 or more and 3 or less; n 25 represents an integer of 0 to 3; n 26 represents an integer of 0 to 5; n 27 represents an integer of 0 or more and 2 or less; n 28 represents an integer of 0 or more and 4 or less. * represents a bond.)
5. L 2 is a methylene group, -C(=O)-, or -C(=CR 21 R 22 5. The polyimide resin according to claim 4, wherein
6. R 1 and R 2The polyimide resin according to claim 1, wherein at least one of the following is represented by the following formula (1-2): [C5] (In formula (1-2), R 15 , R 16 and R 17 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms; p 1 represents an integer from 0 to 10; * represents a bond.)
7. 2. The polyimide resin according to claim 1, having a weight average molecular weight of 5,000 or more.
8. A photosensitive resin composition comprising the polyimide resin according to any one of claims 1 to 7, a crosslinking agent, and a photoradical generator.
9. The photosensitive resin composition according to claim 8 , further comprising a sensitizer.
10. 9. The photosensitive resin composition according to claim 8, wherein the amount of the polyimide resin is 40% by mass or more and 95% by mass or less based on 100% by mass of non-volatile components of the photosensitive resin composition.
11. A support and a photosensitive resin composition layer formed on the support, A photosensitive film, wherein the photosensitive resin layer comprises the photosensitive resin composition according to claim 8.
12. A semiconductor package substrate comprising a cured product of the photosensitive resin composition according to claim 8.
13. A semiconductor device comprising the semiconductor package substrate according to claim 12.
14. A step of forming a photosensitive resin composition layer containing the photosensitive resin composition according to claim 8 on a circuit board; A step of irradiating the photosensitive resin composition layer with actinic rays; developing the photosensitive resin composition layer; A method for manufacturing a semiconductor package substrate, comprising:
15. 2. A method for producing a polyimide resin according to claim 1, comprising reacting a precursor resin containing a repeating unit represented by the following formula (1') with a Wittig reagent or a phosphonic acid diester compound: [C6] (In formula (1'), X 2 represents a tetravalent organic group, Y 2 represents a divalent organic group, X 2 and Y 2 At least one of the above contains at least two benzene rings and a carbonyl group connecting the two benzene rings.
16. 2. A method for producing a polyimide resin according to claim 1, comprising reacting a precursor resin containing a repeating unit represented by the following formula (1′) with a β-dicarbonyl compound: [C7] (In formula (1'), X 2 represents a tetravalent organic group, Y 2 represents a divalent organic group, X 2 and Y 2 At least one of the above contains at least two benzene rings and a carbonyl group connecting the two benzene rings.
17. 2. A method for producing a polyimide resin according to claim 1, comprising reacting a precursor resin containing a repeating unit represented by the following formula (1') with Meldrum's acid, and then reacting the precursor resin with an alcohol compound. [C8] (In formula (1'), X 2 represents a tetravalent organic group, Y 2 represents a divalent organic group, X 2 and Y 2 At least one of the above contains at least two benzene rings and a carbonyl group connecting the two benzene rings.
18. 2. A method for producing the polyimide resin according to claim 1, comprising reacting a tetracarboxylic dianhydride represented by the following formula (1'-a) with a diamine compound represented by the following formula (1'-b): [C9] (In formula (1'-a), X 1 represents a tetravalent organic group. 1 represents a divalent organic group. 1 and Y 1 At least one of the above contains at least two benzene rings and a divalent group represented by formula (1-1) linking the two benzene rings.
Citation Information
Patent Citations
Negative photosensitive resin composition, method for producing pattern and electronic parts
JP2003084435A