Aliphatic polyester resin foam sheet

By incorporating depressions on the surface of aliphatic polyester resin foam sheets, the sheets maintain biodegradability and recyclability, overcoming integration challenges with non-biodegradable laminates.

JP2024135979AInactive Publication Date: 2024-10-04SEKISUI PLASTICS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023046918
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Aliphatic polyester resin foam sheets face challenges in maintaining biodegradability and recyclability when laminated with non-biodegradable resin films, leading to difficulties in separation and recycling.

Method used

The solution involves creating an aliphatic polyester resin foam sheet with depressions on its surface, which enhances separability from other sheets by reducing excessive adhesion, allowing easy isolation and recycling.

Benefits of technology

The surface depressions facilitate easy separation of the foam sheet from laminated materials, preserving its biodegradability and recyclability, thus addressing the integration issues with non-biodegradable layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135979000001_ABST
    Figure 2024135979000001_ABST
Patent Text Reader

Abstract

To provide an aliphatic polyester resin foam sheet which facilitates isolation.SOLUTION: An aliphatic polyester resin foam sheet is composed of a resin composition containing an aliphatic polyester resin, wherein recesses are provided thereon in a ratio of 5 pieces / cm2 or more and 30 pieces / cm2 or less.SELECTED DRAWING: Figure 2A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aliphatic polyester resin foam sheet. [Background technology]

[0002] Conventionally, foamed products made of a foamed resin composition have been widely used. The foamed products are lightweight yet excellent in strength, cushioning properties, and heat insulation. As this type of foamed product, foamed sheets and foamed beads obtained by impregnating a non-foamed resin sheet or resin beads with a foaming agent such as acetone or butane and then heating to foam, as well as foamed molded articles produced by processing these into a three-dimensional shape using a mold, are known. As for the resin foamed sheet, an extruded foamed sheet is known which is obtained by melt-kneading a foaming resin composition and a foaming agent in an extruder, extruding the resulting molten mixture into a sheet shape from a sheeting die (flat die or circular die) attached to the tip of the extruder and foaming it at the same time (extrusion foaming method).

[0003] This type of extruded foam sheet is used as a cushioning sheet in the form of a sheet, or is formed into a bag and used as a packaging material, etc. This type of extruded foam sheet is also used as a raw sheet for producing a foam molded product by thermoforming, and is also widely used as a constituent member of a foam molded product such as a food tray or cup. Furthermore, in addition to being used for the above-mentioned applications by itself, the extruded foam sheet is also widely used in the form of a laminated foam sheet having a film layer (non-foamed layer) laminated on one or both sides.

[0004] In recent years, there has been a demand for biodegradable resin products that can be decomposed in the natural environment, and resin compositions based on aliphatic polyester resins have come to be used as foaming resin compositions that are raw materials for resin foam sheets. For example, Patent Document 1 below describes the production of extruded foam sheets from resin compositions containing easily recyclable polylactic acid resins. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-183098 A Summary of the Invention [Problem to be solved by the invention]

[0006] Aliphatic polyester resin foam sheets may be laminated with resin films, paper, nonwoven fabrics, etc., made of other resins before or after molding such as thermoforming, to produce final products. As described above, aliphatic polyester resin foam sheets are required to be highly biodegradable and easy to recycle. However, if the aliphatic polyester resin foam sheets are integrated with non-biodegradable resin films, etc., the inherent biodegradability of the aliphatic polyester resin foam sheets may be difficult to exhibit, and recycling may be difficult. Therefore, the present invention aims to provide an aliphatic polyester resin foam sheet that can be easily separated from other sheets even when the other sheets are laminated thereon, and to provide an aliphatic polyester resin foam sheet that can be easily isolated. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides: An aliphatic polyester resin foamed sheet composed of a resin composition containing an aliphatic polyester resin, 5 pieces / cm on surface 2 More than 30 pieces / cm 2 Provided is an aliphatic polyester resin foamed sheet having depressions in the following proportions: Effect of the Invention

[0008] According to the present invention, by providing a suitable number of depressions on the surface, excessive adhesion to other sheets can be suppressed, and an aliphatic polyester resin foam sheet having excellent separability from other sheets, etc. can be provided.

[0009] In this specification, the depression means that the cell bubble membrane located on the outermost surface of the sheet is recessed and not flush with the cell bubble membrane of the adjacent cell. Therefore, the depression in this specification means that the dimension in the planar direction (MD, TD) is about 5 times or less the size of the cell in the same direction, and the depth of the depression in the thickness direction is about 2 to 3 times or less the size of the cell in the thickness direction (VD). What specifically should be recognized as a depression will be explained in more detail in the examples. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic front view showing an example of a sheet manufacturing apparatus for producing an aliphatic polyester resin foamed sheet. [Figure 2A] FIG. 2A is a schematic perspective view (surface state diagram as viewed in the direction of block arrow IIa in FIG. 1) showing the surface state of an aliphatic polyester resin foamed sheet. [Figure 2B] FIG. 2B is a schematic cross-sectional view (cross-sectional view taken along the line IIb-IIb in FIG. 1) showing the state of a cross section when the aliphatic polyester resin foam sheet is cut along a plane parallel to the thickness direction. [Figure 3A] FIG. 3A is a schematic cross-sectional view showing a cross-section of a portion of an aliphatic polyester resin foam sheet that has no depression on its surface (a cross-sectional view of IIIA enclosed by a dashed line in FIG. 2). [Figure 3B] FIG. 3B is a schematic cross-sectional view showing a cross-section of a surface layer portion of an aliphatic polyester resin foam sheet having depressions formed on the surface (a cross-sectional view taken along the dashed line enclosure IIIB in FIG. 2). [Figure 3C] FIG. 3C is a schematic cross-sectional view showing a cross-section of a surface layer portion of an aliphatic polyester resin foam sheet having depressions formed on the surface (a cross-sectional view taken along the dashed line enclosure IIIC in FIG. 2). [Figure 4] FIG. 4 is a photograph (exterior view) showing a comparison of the state of depressions on the surface of the aliphatic polyester resin foam sheet of Example 1 and the aliphatic polyester resin foam sheet of Comparative Example 1, arranged side by side. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described. In the following, an embodiment of the present invention will be described taking as an example an aliphatic polyester resin foam sheet that is an extruded foam sheet obtained by an apparatus as shown in FIG.

[0012] The sheet manufacturing apparatus 100 illustrated in Fig. 1 includes a tandem extruder 10 and a circular die CD for discharging the aliphatic polyester resin composition melt-kneaded in the tandem extruder 10 into a cylindrical shape. The manufacturing apparatus further includes a cooling device CL for air-cooling the aliphatic polyester resin foam sheet extruded into a cylindrical shape from the circular die CD, and a mandrel MD for expanding the cylindrical aliphatic polyester resin foam sheet into a cylindrical shape of a predetermined size. The mandrel MD has a cylindrical outer peripheral surface having an outer diameter larger than the diameter of the circular die CD, and is provided so that the outer peripheral surface can be brought into sliding contact with the inner peripheral surface of the aliphatic polyester resin foam sheet extruded into a cylindrical shape to expand the aliphatic polyester resin foam sheet to a predetermined size.

[0013] The sheet manufacturing apparatus 100 is equipped with a slitting device that slits the aliphatic polyester resin foamed sheet after it has passed through the mandrel MD and become cylindrical with a predetermined diameter, and divides it into two strip-shaped sheets, and a take-up roller 22 that winds up the slit aliphatic polyester resin foamed sheet 1 after it has passed through multiple rollers 21.

[0014] The extruder upstream of the tandem extruder 10 (hereinafter also referred to as the "first extruder 10a") is provided with a hopper 11 for feeding an aliphatic polyester resin composition (hereinafter also simply referred to as the "resin composition"), which is the raw material for the aliphatic polyester resin foam sheet, and a gas inlet 12 for supplying a foaming agent such as a hydrocarbon into the cylinder.

[0015] The sheet manufacturing apparatus 100 of this embodiment is also provided with an extruder (hereinafter also referred to as "second extruder 10b") downstream of the first extruder 10a. In the second extruder 10b, melt kneading of a resin composition containing a foaming agent is performed. The aliphatic polyester resin contained in the aliphatic polyester resin foam sheet is preferably modified by crosslinking or the like so as to exhibit excellent melt tension. The modified aliphatic polyester resin (hereinafter also referred to as "modified aliphatic polyester resin") may be contained in the aliphatic polyester resin foam sheet by supplying aliphatic polyester resin that has been previously modified to the hopper 11, or may be contained in the aliphatic polyester resin foam sheet by modifying unmodified aliphatic polyester resin in the extruder used for producing the aliphatic polyester resin foam sheet.

[0016] One surface of the aliphatic polyester resin foamed sheet 1 of this embodiment obtained as described above is brought into sliding contact with a mandrel MD before the aliphatic polyester resin foamed sheet is completely cooled, and the surface is straightened to a flat state. That is, one surface of the aliphatic polyester resin foamed sheet 1 is a flattened straightened surface 1a as shown in FIG. 2B. On the other hand, the surface of the aliphatic polyester resin foamed sheet 1 opposite to the straightened surface 1a is a non-straightened surface 1b that has not been particularly straightened and remains in a freely foamed state. The aliphatic polyester resin foamed sheet 1 of this embodiment has a plurality of recesses 1p that are recessed in the straightened surface 1a.

[0017] Both sides of the aliphatic polyester resin foam sheet 1 can be made into straightened surfaces by passing it between a pair of rollers after extrusion. For example, two straightening rollers with an adjusted surface temperature and a gap set to be equal to or less than the thickness of the extruded aliphatic polyester resin foam sheet are provided in the sheet manufacturing apparatus 100, and an aliphatic polyester resin foam sheet with straightened surfaces on both sides can be obtained by passing the aliphatic polyester resin foam sheet between the straightening rollers before it is completely cooled.

[0018] While the orthodontic surface 1a is a flat surface, the surface of the non-orthodontic surface 1b has undulations (unevenness) at a period of several millimeters, and usually has unevenness with a height difference of 30 μm or more. The height difference may be 40 μm or more, 50 μm or more, or 100 μm or more depending on the case. The height difference can be confirmed by measuring the sheet thickness at the concave and convex parts arranged side by side. The height difference is calculated as the arithmetic average value of the measured values ​​at multiple randomly selected points (for example, 10 points). The sheet thickness of the concave and convex parts can be measured, for example, on the cross section of the aliphatic polyester resin foam sheet. The height difference on the orthodontic surface 1a is usually 50 μm or less, and in many cases, 30 μm or less, except for the points where the depressions are formed.

[0019] The non-straightened surface 1b as described above is usually straightened to a flat state by contact with a molding die during molding. The aliphatic polyester resin foamed sheet 1 of the present embodiment has a surface with 5 particles / cm 2 More than 30 pieces / cm 2 It is important that the depressions 1p are provided at the following ratio, and the presence of the depressions 1p makes it easy to separate even if a resin film or the like is adhered. In this regard, the depressions provided on the non-straightening surface 1b may disappear during straightening using a molding die. Therefore, it is preferable that the aliphatic polyester resin foamed sheet 1 of this embodiment has the depressions 1p formed on the straightening surface 1a.

[0020] 5 recesses per cm 2 More than 30 pieces / cm 2 If the number of dimples is less than 30 / cm, the sheet exhibits excellent separation from other sheets. 2 If the thickness is less than or equal to the thickness, the aliphatic polyester resin foam sheet has a good appearance.

[0021] 6 recesses per cm 2 May be more than 7 pieces / cm 2 May be more than 8 pieces / cm 2 The number of depressions may be 28 / cm or more. 2May be less than 27 pieces / cm 2 May be less than 26 pieces / cm 2 It may be the following.

[0022] <Depression ratio> The ratio of dimples formed in the aliphatic polyester resin foam sheet 1 can be determined according to the following procedure. First, the surface to be measured is colored except for the depressions to enhance its identifiability. For example, the water-based dye ink impregnated in the "Sol Stamp Pad" manufactured by Shachihata Co., Ltd. can be used for coloring. For example, the coloring can be performed by lightly pressing any rubber stamp against the "Sol Stamp Pad" and rubbing the surface to be measured of the aliphatic polyester resin foam sheet with the rubber stamp to which the water-based dye ink is attached. At this time, care should be taken not to get the ink into the depressions. Next, the colored measurement surface is photographed with a digital microscope (for example, manufactured by Keyence Corporation, product name "VHX-1000ver2.3.8.2"), and the photographed image is binarized to count the number of dents. The range for measuring the number of dents is approximately 2.2 cm 2 The image is taken at a magnification of 20 times using a digital microscope. In the obtained binary image, 500 pixels (57,000 μm) were observed as white spots. 2 ) or less are removed as noise and the rest are measured as depressions. The number of measured dents is divided by the measured area to obtain the number of dents per unit area as the "dimple ratio."

[0023] The shape of the depressions 1p in a plan view (viewed in the thickness direction) of the aliphatic polyester resin foam sheet 1 is preferably a shape (linear) that extends long in one direction. When a resin film or the like is laminated on the aliphatic polyester resin foam sheet 1, depressions having the same area but with a linear shape are more likely to affect the surface condition of the resin film than depressions having a circular shape, which is advantageous in that they are less likely to impair the aesthetic appearance of the laminated foam sheet or foam molded product.

[0024] In forming the linear depressions 1p, the aliphatic polyester resin foamed sheet 1 is preferably manufactured so that the expansion ratio of the mandrel MD is high. When the diameter of the circular die CD (diameter of a circle passing through the center of the die slit = inner diameter (diameter) of the die + slit width) is "D0 (mm)" and the outer diameter of the mandrel MD is "D1 (mm)", the expansion ratio, which is the ratio (D1 / D0) of the outer diameter (D1) of the mandrel MD to the diameter (D0) of the circular die CD, is preferably 2 times or more. The expansion ratio may be 2.1 times or more, or may be 2.2 times or more. The expansion ratio (D1 / D0) is, for example, 4 times or less. The expansion ratio (D1 / D0) may be 3.8 times or less, or may be 3.6 times or less.

[0025] The depression 1p can be formed by providing a cell in which the bubble membrane is less likely to expand than other cells. The cell in which the bubble membrane is less likely to expand can be formed by including a gel-like substance in which the aliphatic polyester resin is highly polymerized in the resin composition constituting the aliphatic polyester resin foamed sheet 1. For example, if particulate gel (gel particles GP) is present in the bubble membrane that forms the outer wall of the cell, the bubble membrane containing the gel particles GP has lower extensibility than other bubble membranes when the cell is expanded by the foaming agent, so that cells that are not sufficiently expanded are formed on the surface as shown in FIG. 3B, or the bubble membrane is broken inside, causing the surface to become recessed as shown in FIG. 3C. This allows the depression 1p to be formed on the surface of the aliphatic polyester resin foamed sheet 1.

[0026] For the above reasons, the depression 1p is usually provided on the surface of the aliphatic polyester resin foamed sheet 1 with a size such that the dimensions in each of the extrusion direction (MD) and the width direction (TD) perpendicular to the extrusion direction are equal to or smaller than three bubbles. In other words, the longest dimension of the depression 1p in the planar direction is usually equal to or smaller than three times the average bubble diameter (Dmd) in the extrusion direction of the aliphatic polyester resin foamed sheet 1 and the average bubble diameter (Dtd) in the width direction. The average bubble diameter (Dmd, Dtd) of the aliphatic polyester resin foamed sheet 1 is usually equal to or smaller than 1000 μm. In many cases, the average bubble diameter (Dmd, Dtd) is equal to or smaller than 800 μm, and is equal to or smaller than 700 μm. Therefore, the dimension of the depression 1p in the planar direction is usually equal to or smaller than 3.0 mm. In many cases, the dimension of the depression 1p in the planar direction is equal to or smaller than 1.5 mm, and is equal to or smaller than 1.0 mm. The dimension of the depression 1p in the thickness direction (VD) of the aliphatic polyester resin foamed sheet 1 is usually 1.5 times or less the average bubble diameter (Dvd) in the thickness direction. The average bubble diameter (Dvd) in the thickness direction of the aliphatic polyester resin foamed sheet 1 is usually 400 μm or less. In many cases, the average bubble diameter (Dvd) in the thickness direction of the aliphatic polyester resin foamed sheet 1 is 300 μm or less, or 200 μm or less. The depth of the depression 1p, calculated as the length of a perpendicular line drawn from a straight line along the surface of the aliphatic polyester resin foamed sheet 1 in the thickness direction, is usually 600 μm or less, and in many cases, is 450 μm or less or 300 μm or less.

[0027] The average cell diameter in each direction of the aliphatic polyester resin foam sheet 1 can be determined as follows. <How to calculate the average bubble diameter> A rectangular sample is cut out from the central portion in the width direction of the aliphatic polyester resin foam sheet 1 so that the cutting directions are parallel to the MD and TD. The sample is cut in both the MD and TD directions, and the cross sections are photographed at 30x magnification using a scanning electron microscope (SU1510, Hitachi High-Technologies Corporation). At this time, the microscope images are photographed so that they will have a specified magnification when printed in a state where two images are arranged vertically and horizontally (a total of four images) on a single piece of landscape A4 paper. Next, on the image, draw arbitrary straight lines of 60 mm parallel to each of the directions MD and TD, and a straight line of 60 mm in the direction perpendicular to each direction (VD). Microscopic images of two fields of view for each cross section parallel to the MD (MD cross section) and the cross section parallel to the TD (TD cross section), totaling four fields of view, are taken and printed on A4 paper. Draw three arbitrary straight lines (60 mm long) parallel to MD on each of the two images of the MD cross section, and draw three arbitrary straight lines (60 mm long) parallel to TD on each of the two images of the TD cross section. Also, draw three straight lines (60 mm long) parallel to VD on one image of the MD cross section and one image of the TD cross section, and draw six arbitrary straight lines of 60 mm long parallel to MD, TD, and VD in each direction. It should be noted that any line should be made to avoid contact with air bubbles at its contact points as much as possible, and if any air bubbles do come into contact with the line, these air bubbles are also counted. The number of bubbles counted for six arbitrary straight lines in each of the MD, TD, and VD directions is calculated as the arithmetic average, which is the number of bubbles in each direction. The average chord length t of the bubbles in each direction is calculated from the image magnification at which the number of bubbles was counted and this number of bubbles using the following formula. Average chord length t (mm) = 60 / (number of bubbles x image magnification) (Average chord length in MD direction tM (mm) = 60 / (number of bubbles in MD direction × image magnification)) (Average chord length in TD direction tT (mm) = 60 / (number of bubbles in TD direction × image magnification)) (Average chord length in the VD direction tV (mm) = 60 / (number of bubbles in the VD direction × image magnification)) The image magnification is calculated by measuring the scale bar on the image to the nearest 1 / 100 mm using a Digimatic Caliper (Mitutoyo Corporation) and using the following formula: Image magnification = Scale bar actual value (mm) / Scale bar display value (mm) Calculate the average bubble diameter in each direction using the following formula. Average bubble diameter in MD Dmd (μm) = (tM (mm) / 0.616) × 1000 Average bubble diameter at TD Dtd (μm) = (tT (mm) / 0.616) × 1000 Average bubble diameter at VD Dvd (μm) = (tV (mm) / 0.616) × 1000

[0028] It is preferable that at least the majority (50% or more by number) of the depressions 1p on the surface of the aliphatic polyester resin foamed sheet 1 have the above-mentioned dimensions, and it is preferable that 80% or more have the above-mentioned dimensions. Almost all of the depressions 1p in the aliphatic polyester resin foamed sheet 1 of this embodiment may be of the above-mentioned dimensions. In the aliphatic polyester resin foamed sheet 1 of this embodiment, the depressions 1p of the above-mentioned dimensions are arranged at a density of 5 depressions / cm as described above. 2 More than 30 pieces / cm 2 or less, or may be provided in a ratio of 5 or more / 28 or less, or may be provided in a ratio of 5 or more / 27 or less, or may be provided in a ratio of 5 or more / 26 or less.

[0029] The frequency and size of the depressions 1p can be adjusted not only by the amount of gel particles GP, but also by, for example, the resin temperature during extrusion, the amount of foaming agent used, etc. By increasing the resin temperature during extrusion or the amount of foaming agent used, the difference in extensibility between the foam film containing gel particles GP and the foam film not containing gel particles GP can be made more noticeable.

[0030] The gel particles GP can be present in a modified aliphatic polyester resin by crosslinking the aliphatic polyester resin with a crosslinking agent to prepare the modified aliphatic polyester resin. Then, the modified aliphatic polyester resin is extrusion-foamed to obtain an aliphatic polyester resin foam sheet 1 having the gel particles GP dispersed in the bubble membrane.

[0031] The same effect can be obtained by using an aliphatic polyester resin with a high molecular weight instead of the gel particles GP. A first aliphatic polyester resin, which is the main component of the resin composition used to form the aliphatic polyester resin foamed sheet 1, and a second aliphatic polyester resin having a molecular weight much higher than that of the first aliphatic polyester resin (for example, a mass average molecular weight of one million or more) are prepared, and the ratio of the second aliphatic polyester resin to the first aliphatic polyester resin is, for example, 1 / 100 to 1 / 10 to prepare a resin composition, and the resin composition is extruded and foamed to obtain an aliphatic polyester resin foamed sheet 1 having depressions formed therein.

[0032] If the second aliphatic polyester resin has a molecular weight high enough not to show sufficient solubility in the first aliphatic polyester resin inside the extruder, fine particles of the second aliphatic polyester resin will be dispersed in the aliphatic polyester resin foam sheet 1, as in the case of containing gel particles GP. In this case, where the fine particles of the second aliphatic polyester resin are present on the surface, the expansion of the bubble film during extrusion foaming is suppressed compared to the surrounding area, and appropriate depressions are formed. The method of modifying the aliphatic polyester resin to form a gel is also effective in imparting a melt tension suitable for foaming to the resin composition.

[0033] The resin composition preferably has a gel fraction of 0.3% by mass or more when it is used to form an aliphatic polyester resin foam sheet. The gel fraction of the aliphatic polyester resin foam sheet may be 0.4% by mass or more, or may be 0.5% by mass or more. In order to obtain an aliphatic polyester resin foam sheet with a high expansion ratio, the resin composition preferably has a gel fraction of 1.2% by mass or less when it is used to form an aliphatic polyester resin foam sheet. The gel fraction of the aliphatic polyester resin foam sheet may be 1.1% by mass or less, or may be 1.0% by mass or less.

[0034] The resin composition preferably has a gel fraction of 0.4% by mass or more before being used for extrusion foaming. The gel fraction of the resin composition before extrusion foaming may be 0.5% by mass or more, or may be 0.6% by mass or more. In order to obtain an aliphatic polyester resin foamed sheet with a high expansion ratio, the gel fraction of the resin composition is preferably 2.0% by mass or less. The gel fraction of the resin composition may be 1.8% by mass or less, or may be 1.6% by mass or less. The gel fraction of the resin composition may be 1.5% by mass or less. If the gel fraction of the resin composition in the state of constituting an aliphatic polyester resin foamed sheet is within the above range, the surface of the resin foamed sheet is provided with appropriate depressions, and an aliphatic polyester resin foamed sheet having excellent separability from other sheets can be obtained.

[0035] The gel fraction (mass %) can be determined as follows. <How to calculate gel fraction> Prepare a sample of about 0.5 g from the aliphatic polyester resin foam sheet 1, and accurately weigh out the initial mass (m0(g)) of this sample. Also prepare a 200 mesh wire net (wire diameter φ0.05 mm) to filter the solution in which this sample is dissolved. The initial mass (M0(g)) of this wire net is also accurately weighed. Place the weighed measurement sample in a beaker (100 ml). Put 50 mL of chloroform as a solvent and a stir bar into the beaker, and cover with aluminum foil. Stir with a stirrer for 2 hours to dissolve at room temperature. After 2 hours, remove the aluminum foil, and filter the solution in the beaker through a 200 mesh wire net. After filtration, naturally dry the resin insoluble matter together with the mesh wire net in a draft chamber for 12 hours or more to evaporate the chloroform. Next, dry the resin insoluble matter together with the mesh wire net in a thermostatic dryer at a temperature of 120°C for 2 hours, and allow to cool in a desiccator after drying. After cooling, the wire mesh (M1(g)) to which the resin insoluble matter is attached is weighed accurately. The gel fraction is calculated using the following formula. Gel fraction (mass%) = (M1-M0) / m0 x 100

[0036] The inclusion of a high molecular weight component in a resin composition can be understood by the Z-average molecular weight, etc. The Z-average molecular weight of the aliphatic polyester resin foam sheet is preferably 400,000 or more. The Z-average molecular weight of a sample obtained by thermally melting the aliphatic polyester resin foam sheet may be 500,000 or more, or may be 600,000 or more. The Z-average molecular weight is, for example, 1,000,000 or less. The Z-average molecular weight may be, for example, 900,000 or less, or may be 800,000 or less.

[0037] The aliphatic polyester resin foam sheet preferably has a mass average molecular weight of 180,000 or more. The mass average molecular weight of a sample obtained by thermally melting the aliphatic polyester resin foam sheet may be 200,000 or more, or may be 220,000 or more. The mass average molecular weight is, for example, 350,000 or less. The mass average molecular weight may be, for example, 300,000 or less, or may be 290,000 or less.

[0038] The aliphatic polyester resin foam sheet preferably has a dispersity, which is the ratio (Mw / Mn) of the mass average molecular weight (Mw) to the number average molecular weight (Mn), of 2.4 or more. The dispersity of a sample obtained by heat-melting the aliphatic polyester resin foam sheet may be 2.5 or more, or may be 2.6 or more. The dispersity is, for example, 4.0 or less. The dispersity may be, for example, 3.8 or less, or may be 3.6 or less.

[0039] The resin composition before being used for extrusion foaming preferably has a Z-average molecular weight of 500,000 or more. The resin composition before being used for extrusion foaming may have a Z-average molecular weight of 600,000 or more, or may have a Z-average molecular weight of 650,000 or more. The Z-average molecular weight is, for example, 1.5 million or less. The Z-average molecular weight may be, for example, 1.2 million or less, or may have a Z-average molecular weight of 1 million or less.

[0040] The resin composition before being used in extrusion foaming preferably has a mass average molecular weight of 250,000 or more. The mass average molecular weight of the resin composition may be 260,000 or more, or may be 270,000 or more. The mass average molecular weight is, for example, 450,000 or less. The mass average molecular weight may be 400,000 or less, or may be 350,000 or less.

[0041] The resin composition before being used in extrusion foaming preferably has a dispersity, which is the ratio (Mw / Mn) of the mass average molecular weight (Mw) to the number average molecular weight (Mn), of 1.6 or more. The dispersity of the resin composition may be 1.8 or more, or may be 2.0 or more. The dispersity is, for example, 4.5 or less. The dispersity may be 4.0 or less, or may be 3.5 or less.

[0042] The reduction rate ((1-Mz1 / Mz0) x 100%) of the Z-average molecular weight (Mz1) of the aliphatic polyester resin foam sheet relative to the Z-average molecular weight (Mz0) of the resin composition before use in extrusion foaming is preferably 30% or less.

[0043] The reduction rate ((1-Mw1 / Mw0) x 100%) of the mass average molecular weight (Mw1) of the aliphatic polyester resin foam sheet relative to the mass average molecular weight (Mw0) of the resin composition before being used for extrusion foaming is preferably 25% or less.

[0044] In this embodiment, the number average molecular weight (Mn), the mass average molecular weight (Mw), and the Z average molecular weight (Mz) can be determined as follows.

[0045] <Molecular weight measurement> Each average molecular weight (Mn, Mw, Mz) means an average molecular weight measured by gel permeation chromatography (GPC) in terms of polystyrene (PS). Specifically, the average molecular weight is measured as follows. 20 mg of the sample was dissolved in 6 mL of chloroform (immersion time: 6±1.0 hours (partially insoluble)) to obtain a sample solution. The sample solution is filtered through a non-aqueous 0.45 μm syringe filter manufactured by Shimadzu GLC Co., Ltd. to obtain a filtrate. The filtrate is measured using a chromatograph under the following measurement conditions. Each average molecular weight (Mn, Mw, Mz) is determined from a previously prepared calibration curve of standard polystyrene. Equipment used: Tosoh Corporation's "HLC-8320GPC EcoSEC" gel permeation chromatograph (with built-in RI and UV detectors)

[0046] (GPC measurement conditions) column Sample side Guard column = TSK guardcolumn HXL-H (6.0mm x 4.0cm) x 1, manufactured by Tosoh Corporation Measurement column: Tosoh Corporation's TSKgel GMHXL (7.8 mm I.D. x 30 cm) x 2 in series Reference Side Resistance tube (inner diameter 0.1 mm x 2 m) x 2 in series Column temperature = 40 °C Mobile phase = chloroform Mobile phase flow rate Sample pump = 1.0mL / min Reference pump = 0.5mL / min Detector = RI detector Injection volume = 50μL Measurement time = 25 min Sampling pitch = 500 msec

[0047] The standard polystyrene samples for the calibration curve are "STANDARD SM-105" and "STANDARD SH-75" manufactured by Showa Denko K.K. and have mass average molecular weights of 5,620,000, 3,120,000, 1,250,000, 442,000, 151,000, 53,500, 17,000, 7,660, 2,900, and 1,320. The above-mentioned standard polystyrene for the calibration curve is grouped into A (5,620,000, 1,250,000, 151,000, 17,000, 2,900) and B (3,120,000, 442,000, 53,500, 7,660, 1,320), and then A (2mg, 3mg, 4mg, 4mg, 4mg) is weighed and dissolved in 30mL of chloroform, and B (3mg, 4mg, 4mg, 4mg) is also weighed and dissolved in 30mL of chloroform. The standard polystyrene calibration curve is obtained by injecting 50μL of each of the prepared A and B solutions and creating a calibration curve (cubic equation) from the retention time obtained after measurement. Each average molecular weight is calculated using the calibration curve.

[0048] In order to exhibit good foaming properties, it is preferable that the resin composition (after extrusion foaming) constituting the aliphatic polyester resin foam sheet has a melt tension of 25 cN or more at 190°C and a melt mass-flow rate (MFR) of 1.9 g / 10 min or less at 190°C and a nominal load of 2.16 kg.

[0049] The melt tension of the resin composition after extrusion and foaming may be 30 cN or more, or 34 cN or more. The melt tension of the resin composition after extrusion and foaming is usually 60 cN or less.

[0050] The melt mass flow rate of the resin composition after extrusion foaming may be 1.8 g / 10 min or less, or may be 1.7 g / 10 min or less. The melt mass flow rate of the resin composition after extrusion foaming is usually 0.3 g / 10 min or more.

[0051] The melt tension of the resin composition at 190°C before being used in extrusion foaming is, for example, 40 cN or more. The melt tension of the resin composition may be 45 cN or more, or 50 cN or more. The melt tension of the resin composition may be 52 cN or more. The melt tension of the resin composition is usually 80 cN or less. The melt tension of the resin composition may be 70 cN or less. The melt tension of the resin composition may be 66 cN or less, or 62 cN or less.

[0052] The melt mass flow rate (MFR: temperature 190°C, nominal load 2.16 kg) of the resin composition before being used for extrusion foaming is, for example, 1 g / 10 min or less. The melt mass flow rate of the resin composition may be 0.8 g / 10 min or less, 0.7 g / 10 min or less, 0.6 g / 10 min or less, or 0.5 g / 10 min or less. The melt mass flow rate (MFR: temperature 190°C, nominal load 2.16 kg) of the resin composition is, for example, 0.1 g / 10 min or more.

[0053] The melt tension and the melt mass-flow rate can be measured by the following method.

[0054] <Melt tension> The melt tension can be measured using a capillary rheometer "Capillograph 1D" (special specification for heating furnace) manufactured by Toyo Seiki Seisakusho Co., Ltd., and "Rheotens 71.97" manufactured by Goettfert. The melt tension is measured under the following conditions. When using aliphatic polyester foam sheets as samples, they are defoamed by heat pressing to form non-foamed sheets with a thickness of 0.2 to 0.3 mm. At this time, the heating temperature by heat pressing is 190°C, and pressure and decompression are repeated until complete defoaming. The non-foamed sheets are vacuum-dried at 90°C for 4 hours or more, and after drying, they are vacuum-packed in nylon poly bags for vacuum packing and stored in a desiccator until immediately before measurement. Samples other than aliphatic polyester foam sheets are vacuum-dried at 90°C for 4 hours or more in advance, and after drying, they are vacuum-packed in nylon poly bags for vacuum packing and stored in a desiccator until immediately before measurement. Install the Rheotens so that the distance from the die exit of the Capillograph 1D to the measurement part is 80 mm. (Note: If the Rheotens cannot be brought close to 80 mm due to interference, take measures to avoid interference and set the Rheotens in the specified location.) First, a sample is filled into a barrel heated to a test temperature of 190° C., and then preheated for 5 minutes. The measurement time should not exceed 10 minutes, including the preheating time, after the barrel is filled. Next, a piston is inserted from the top of the barrel and the molten resin is extruded into a string-like shape. At this time, the piston descending speed (20 mm / min) is kept constant and the extruded string-like material is passed through a Rheotens wheel. The take-up speed is then gradually increased to measure the melt tension of the sample. Regarding the measurement results, the average of the maximum and minimum tension values ​​immediately before the point at which the string-like material breaks is taken as the melt tension of the sample. If there is only one maximum point on the tension chart, that maximum value is taken as the melt tension. If the string-like material becomes thin and the winding becomes idling, that point is taken as the break point, and the average of the maximum tension values ​​immediately before that point is taken as the melt tension of the sample.

[0055] (Measuring conditions for Capillograph 1D) Die: diameter 2.095mm, length 8mm, inlet angle 90 degrees (conical) Barrel diameter: 9.55mm Piston speed: 20mm / min Measurement temperature: 190℃

[0056] (Rheotensile measurement conditions) Wheel spacing: Top 0.7mm, bottom 1.0mm Acceleration: 10mm / s 2 Pulling speed: Initial speed 6.92mm / s

[0057] <Melt Mass Flow Rate (MFR)> The melt mass flow rate (MFR) of the aliphatic polyester resin or the aliphatic polyester resin composition is measured in accordance with JIS K7210:1999. The melt mass flow rate (MFR) is measured by "b) a method for measuring the time it takes for a piston to move a specified distance" described in Method B of the same standard. The melt mass flow rate (MFR) is measured using a "Melt Flow Index Tester (Automatic) 120-SAS" manufactured by Yasuda Seiki Seisakusho Co., Ltd. When using an aliphatic polyester resin foamed sheet as a sample, it is defoamed by heat pressing to form a non-foamed sheet with a thickness of 0.2 to 0.3 mm. At this time, the heating temperature by heat pressing is 190°C, and pressure decompression is repeated until complete defoaming. The non-foamed sheet is vacuum dried at 90°C for 4 hours or more, and after drying, it is placed in a nylon poly bag for vacuum packing, vacuum packed, and stored in a desiccator until immediately before measurement. Samples for measurement other than aliphatic polyester resin foamed sheets are vacuum dried at 90°C for 4 hours or more, and after drying, it is placed in a nylon poly bag for vacuum packing, vacuum packed, and stored in a desiccator until immediately before measurement, and then used for measurement.

[0058] (Measurement conditions) Sample: 3-8g Preheat 1:200 seconds Preheat 2:30 seconds Test temperature: 190℃ Test load: 2.16kgf Piston travel distance (interval): 4mm Number of tests: 3 The average of the measurements obtained from each test is taken as the MFR (g / 10 min).

[0059] When the aliphatic polyester resin foamed sheet of the present embodiment is made into a non-foamed sheet by thermal melting, the non-foamed sheet preferably satisfies at least one of the following (A) and (B). (A) Maximum tensile stress is 5.0 MPa or more (B) Fracture energy is 0.05 J / g or more and 0.25 J / g or less.

[0060] The (A) maximum tensile stress may be 5.5 MPa or more, or 6.0 MPa or more. The (A) maximum tensile stress is set to, for example, 7.5 MPa or less.

[0061] (B) The breaking energy may be 0.08 J / g or more, or may be 0.1 J / g or more.(B) The breaking energy may be 0.23 J / g or less, or may be 0.2 J / g or less.

[0062] When a non-foamed sheet is made by thermal melting, the non-foamed sheet satisfies at least one of the above (A) and (B), which means that the aliphatic polyester resin is not excessively deteriorated and can be reused. Therefore, it can be said that an aliphatic polyester resin foamed sheet that satisfies at least one of the above (A) and (B) has excellent recyclability.

[0063] The maximum tensile stress and the breaking energy can be determined as follows. <Maximum tensile stress, breaking energy> The measurements are performed in accordance with JIS K7113: 1995. That is, the measurements are performed using a tensile tester (for example, Shimadzu Corporation's "Autograph AG-X plus 100kN" universal testing machine, Shimadzu Corporation's "TRAPEZIUM X" universal testing machine data processing). The test pieces are taken from a non-foamed sheet obtained by defoaming an aliphatic polyester resin foam sheet by heat pressing. The non-foamed sheet is prepared by heat pressing to a thickness of 0.2 to 0.3 mm. At this time, the heating temperature by the heat press is 190°C, and pressure reduction is repeated until complete defoaming. The non-foamed sheet thus prepared is cut into a dumbbell-shaped No. 2 specimen as specified in JIS K7113:1995. Five specimens are used. The specimens are conditioned for 16 hours in a standard atmosphere of JIS K7100:1999 code "23 / 50", class 2, before being used for measurement. Measurements are performed in the same environment, with a gripper interval of 80 mm and a test speed of 50 mm / min. Using the results obtained from the tensile test, a stress-strain curve (SS curve) is prepared, and the maximum stress in the SS curve is taken as the maximum tensile stress, and the area enclosed by the horizontal axis at the intersection of the SS curve and the vertical axis where the value is 0 is integrated to obtain the fracture energy.

[0064] The thickness of the aliphatic polyester resin foam sheet 1 of the present embodiment is not particularly limited, but may be, for example, 0.5 mm or more. The thickness of the aliphatic polyester resin foam sheet 1 may be 1 mm or more, or 1.5 mm or more. The thickness of the aliphatic polyester resin foam sheet 1 may be, for example, 8 mm or less. The thickness of the aliphatic polyester resin foam sheet 1 may be 6 mm or less, or 4 mm or less.

[0065] <Thickness> The thickness of the aliphatic polyester resin foam sheet 1 can be determined by, for example, taking an enlarged photograph of a cross section of the aliphatic polyester resin foam sheet cut along a plane perpendicular to the aliphatic polyester resin foam sheet, and is determined, for example, as the average value of multiple randomly selected locations (e.g., 20 locations).

[0066] The aliphatic polyester resin foamed sheet 1 of the present embodiment may be advantageous in terms of exhibiting excellent moldability if the open cell ratio is a certain level or less. The aliphatic polyester resin foamed sheet 1 of the present embodiment preferably has an open cell ratio of 60% or less. The open cell ratio may be 40% or less, 30% or less, or 25% or less. The aliphatic polyester resin foamed sheet 1 of the present embodiment may be advantageous in terms of exhibiting excellent cushioning properties and excellent dimensional stability by suppressing excessive secondary foaming if the open cell ratio is a certain level or more. The open cell ratio of the aliphatic polyester resin foamed sheet 1 may be 5% or more. The open cell ratio of the aliphatic polyester resin foamed sheet 1 can be measured as follows.

[0067] The aliphatic polyester resin foam sheet 1 of the present embodiment has an apparent density of 60 kg / m 3 That is all. In order to make the foamed product have high strength, it is advantageous for the apparent density to be above a certain level. The apparent density is 80kg / m 3 or more, 100 kg / m 3 On the other hand, in order to ensure light weight and cushioning properties, the apparent density is desirably equal to or less than a certain level. The apparent density of the aliphatic polyester resin foamed sheet 1 of the present embodiment is 300 kg / m 3 The apparent density is 250 kg / m 3 It may be the following.

[0068] <Apparent density> Apparent density (kg / m) of aliphatic polyester resin foam sheet 3 ) is the mass of the aliphatic polyester resin foam sheet per unit area (basis weight: g / m 2 ) by the thickness (mm) of the aliphatic polyester resin foam sheet. The basis weight can be calculated by arithmetically averaging the values ​​measured for a plurality of samples cut out from the aliphatic polyester resin foam sheet. The basis weight of the aliphatic polyester resin foam sheet can be calculated by cutting out a measurement sample from the aliphatic polyester resin foam sheet so that the dimension in the extrusion direction (MD) is 20 cm and the dimension in the transverse direction (TD) is the full width, and calculating the mass W (g) and area S (cm2 ) can be calculated from the following formula: Basis weight (g / m 2 )=W / S×10000 The apparent density can be calculated as follows: Apparent density (kg / m 3 )=Basic weight (g / m 2 ) ÷ thickness (mm)

[0069] <Open cell ratio> The open cell ratio can be determined by the following method. Cut out multiple sheet-like samples measuring 25 mm long x 25 mm wide from the aliphatic polyester resin foam sheet. The cut out samples are stacked together without leaving any gaps to make test pieces with a thickness of 21 to 23 mm, and three pieces are prepared for testing. The test pieces are conditioned for 16 hours in a JIS K7100:1999 symbol 23 / 50, class 2 environment, and the thickness (mm) is measured. For example, a "Digimatic Caliper" caliper made by Mitutoyo Corporation can be used to measure the thickness. The thickness is measured to the nearest 1 / 100 mm, and the apparent volume (cm 3 ) is required. Next, the volume (cm ) of the test piece was measured under the above environment using a dry automatic density meter (e.g., Shimadzu Corporation's "AccuPic II 1340-100cc"). 3 ) is measured. The measurement conditions are as follows. Gas used: Nitrogen Container used: 35cc Filling pressure: 0.005psig Pressure equilibrium end rate: 0.005psig / min Repeat count: 1 time Then, the open cell rate (%) of each test piece is calculated by the following formula, and the average value is regarded as the apparent density of the aliphatic polyester resin foam sheet. Open cell rate (%) = [(apparent volume - volume measured with dry-type automatic density meter) / apparent volume] x 100 (%)

[0070] The aliphatic polyester resin contained in the resin composition for forming the aliphatic polyester resin foamed sheet 1 as described above may be, for example, a hydroxy acid polycondensate, a ring-opening polymer of lactone, or a polycondensate of a polyhydric alcohol component and a polycarboxylic acid component. Examples of the hydroxy acid polycondensate include polylactic acid and a polycondensate of hydroxybutyric acid. Examples of the ring-opening polymer of lactone include polycaprolactone and polypropiolactone. Examples of the polycondensate of a polyhydric alcohol component and a polycarboxylic acid component include polyethylene succinate, polybutylene succinate, polybutylene adipate, polybutylene succinate adipate, and polybutylene adipate terephthalate. Among them, the aliphatic polyester resin is preferably polylactic acid (PLA).

[0071] In this embodiment, polylactic acid resin (PLA) refers to a polymer containing 50 mol% or more of lactic acid component units. Examples of such polymers include (1) polymers of lactic acid, (2) copolymers of lactic acid and other aliphatic hydroxycarboxylic acids, (3) copolymers of lactic acid, aliphatic polyhydric alcohols, and aliphatic polycarboxylic acids, (4) copolymers of lactic acid and aliphatic polycarboxylic acids, (5) copolymers of lactic acid and aliphatic polyhydric alcohols, and (6) mixtures of any of the above (1) to (5). Specific examples of the lactic acid include L-lactic acid, D-lactic acid, DL-lactic acid, or their cyclic dimers L-lactide, D-lactide, DL-lactide, or mixtures thereof.

[0072] Examples of the aliphatic polycarboxylic acid constituting the copolymer include oxalic acid, succinic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, undecanedioic acid, and dodecanedioic acid. The aliphatic polycarboxylic acid may be an anhydride.

[0073] Examples of the aliphatic polyhydric alcohols include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, neopentyl glycol, tetramethylene glycol, and 1,4-cyclohexanedimethanol.

[0074] Examples of the aliphatic hydroxycarboxylic acid other than lactic acid that constitutes the copolymer include glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 4-hydroxyvaleric acid, 5-hydroxyvaleric acid, and 6-hydroxycaproic acid.

[0075] The resin composition preferably contains a modified aliphatic polyester resin (modified aliphatic polyester resin), and more preferably contains a modified polylactic acid (hereinafter also referred to as "modified polylactic acid").

[0076] The starting material for the modified aliphatic polyester resin (hereinafter also referred to as "unmodified aliphatic polyester resin") is preferably a plant-derived diol or dicarbonate, which is a constituent unit of the unmodified aliphatic polyester resin. That is, it is preferable that at least a part of the unmodified aliphatic polyester resin, such as polylactic acid (PLA), polybutylene succinate (PBS), and polybutylene succinate adipate (PBSA), is plant-derived.

[0077] The unmodified aliphatic polyester resin preferably has a melt mass flow rate (MFR) of 1 g / 10 min or more and 15 g / 10 min or less, measured under conditions of 190° C. and a nominal load of 2.16 kg. The MFR of the unmodified aliphatic polyester resin may be 2 g / 10 min or more, or 3 g / 10 min or more. The MFR of the unmodified aliphatic polyester resin may be 10 g / 10 min or less, or 8 g / 10 min or less.

[0078] The MFR of the unmodified aliphatic polyester resin can be measured by the same method as that for the MFR of the resin composition.

[0079] As a method for modifying such an unmodified polyester resin, there is a method of crosslinking (partial crosslinking) with an organic peroxide.

[0080] Examples of the organic peroxide include peroxy esters, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxydicarbonates, peroxyketals, and ketone peroxides.

[0081] Examples of the peroxy ester include t-butylperoxy 2-ethylhexyl carbonate, t-hexylperoxy isopropyl monocarbonate, t-hexylperoxybenzoate, t-butylperoxybenzoate, t-butylperoxylaurate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxyacetate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, and t-butylperoxyisopropyl monocarbonate.

[0082] Examples of the hydroperoxide include permethane hydroperoxide, diisopropylbenzene hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide.

[0083] Examples of the dialkyl peroxide include dicumyl peroxide, di-t-butyl peroxide, and 2,5-dimethyl-2,5-di(t-butylperoxy)-hexyne-3.

[0084] Examples of the diacyl peroxide include dibenzoyl peroxide, di(4-methylbenzoyl) peroxide, and di(3-methylbenzoyl) peroxide.

[0085] Examples of the peroxydicarbonate include di(2-ethylhexyl) peroxydicarbonate and diisopropyl peroxydicarbonate.

[0086] Examples of the peroxyketals include 1,1-di-t-butylperoxy-3,3,5-trimethylcyclohexane, 1,1-di-t-butylperoxycyclohexane, 2,2-di(t-butylperoxy)-butane, n-butyl 4,4-di-(t-butylperoxy)valerate, and 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane.

[0087] Examples of the ketone peroxide include methyl ethyl ketone peroxide and acetylacetone peroxide.

[0088] In this embodiment, it is preferable to use an organic peroxide that has a mild reactivity and has a high half-life temperature. The one-minute half-life temperature of the organic peroxide is preferably 150° C. or more and 200° C. or less.

[0089] The one-minute half-life temperature can be measured using a 0.1 mol / L solution in benzene as the solvent. Since the decomposition reaction in a dilute solution of organic peroxide can be regarded as a first-order reaction, the decomposition reaction can be expressed as the following formulas (1) and (2) where C is the initial concentration of organic peroxide, ΔC is the amount decomposed, k is the decomposition rate constant, and t is the time. Equation (1): dx / dt=k(C-ΔC) Equation (2): ln C / (C-ΔC)=kt Half-life time is t 1 / 2 Then (C-ΔC) becomes C / 2, so the above formula becomes as follows. Equation (3): k·t 1 / 2 =ln2 Therefore, if an organic peroxide is thermally decomposed at a certain temperature (T) and the relationship between time (t) and "ln C / (C-ΔC)" is plotted on a graph, the decomposition rate constant (k) can be calculated from the slope of the approximate line, and the half-life time (t 1 / 2 ) is obtained. The decomposition rate constant k is expressed by the Arrhenius equation as follows: Equation (4): k=Aexp(-ΔE / RT) Equation (5): lnk=lnA-ΔE / RT (A: frequency factor, ΔE: activation energy, R: gas constant, T: absolute temperature) The decomposition rate constant k at each temperature is calculated at several points, and the activation energy ΔE is calculated from the slope of the straight line obtained by plotting "lnk" and "1 / T". The activation energy ΔE is used to replace "lnk" with "lnt 1 / 2 The one-minute half-life temperature can be calculated from the approximate straight line obtained by plotting the relationship between " and "1 / T".

[0090] As organic peroxides having the above half-life temperatures, t-butylperoxyisopropyl carbonate (1-minute half-life temperature: 156° C.) and t-butylperoxy-3,5,5-trimethylhexanoate (1-minute half-life temperature: 159° C.) are preferred.

[0091] The organic peroxide is preferably used in an amount of 0.02 parts by mass or more and 1.0 parts by mass or less when the amount of the unmodified aliphatic polyester resin to be modified is taken as 100 parts by mass. The amount of the organic peroxide may be 0.05 parts by mass or more, or 0.08 parts by mass or more. The amount of the organic peroxide may be 0.8 parts by mass or less, or 0.6 parts by mass or less.

[0092] As a method for modifying the non-modified polyester resin, it is preferable to use a crosslinking aid together with an organic peroxide. Examples of the crosslinking aid include divinylbenzene, diallylbenzene, divinylnaphthalene, divinylphenyl, divinylcarbazole, and divinylpyridine. The crosslinking aid may be a multifunctional acrylic acid compound such as ethylene glycol diacrylate, butylene glycol diacrylate, triethylene glycol diacrylate, 1,6-hexanediol diacrylate, and tetramethylolmethane tetraacrylate; or a multifunctional methacrylic acid compound such as ethylene glycol dimethacrylate, butylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, 1,10-decanediol dimethacrylate, trimethylolpropane trimethacrylate, and tetramethylolmethane tetramethacrylate. Examples of the crosslinking aid that can be used include polyvinyl esters, polyallyl esters, polyacryloyloxyalkyl esters, polymethacryloyloxyalkyl esters of aliphatic and aromatic polyvalent carboxylic acids such as divinyl phthalate, diallyl phthalate, diallyl maleate, and bisacryloyloxyethyl terephthalate, polyvinyl ethers and polyallyl ethers of aliphatic and aromatic polyhydric alcohols such as diethylene glycol divinyl ether, hydroquinone divinyl ether, and bisphenol A diallyl ether; allyl esters of cyanuric acid or isocyanuric acid such as triallyl cyanurate and triallyl isocyanurate; triallyl phosphate; trisacryloxyethyl phosphate; maleimide compounds such as N-phenylmaleimide and N,N'-m-phenylene bismaleimide; and compounds having two or more triple bonds such as dipropargyl phthalate and dipropargyl maleate.

[0093] The crosslinking aid may be a polymer type having an epoxy group capable of bonding with a hydroxyl group or a carboxyl group of an aliphatic polyester resin. This type of polymer type crosslinking aid is also suitable in that it has a chain extension function. Examples of the polymer type crosslinking aid include epoxy group-containing (meth)acrylic polymers. Examples of the epoxy group-containing (meth)acrylic polymers include styrene-glycidyl (meth)acrylate copolymers. The styrene-glycidyl (meth)acrylate copolymer is preferably one in which the proportion of glycidyl methacrylate in the copolymer exceeds 20% by mass. The proportion of glycidyl methacrylate in the copolymer is more preferably more than 30% by mass, and particularly preferably more than 50% by mass. The epoxy equivalent in this copolymer is, for example, 150 to 3000 g / eq. The epoxy equivalent may be 200 to 500 g / eq. The mass average molecular weight (Mw) of the styrene-glycidyl (meth)acrylate copolymer is, for example, 2000 to 25000. The mass average molecular weight (Mw) may be 3000 to 8000. The number average molecular weight (Mn) of the styrene-glycidyl (meth)acrylate copolymer may be, for example, 400 to 6000. The number average molecular weight (Mn) may be 1000 to 4000. The dispersity (Q value=Mw / Mn) of the styrene-glycidyl (meth)acrylate copolymer is, for example, 1.5 to 5.

[0094] As the epoxy group-containing (meth)acrylic polymer, a commercially available product sold under the trade name "Joncryl" by BASF, a commercially available product sold under the trade name "ARUFON" by Toagosei Co., Ltd., or a commercially available product sold under the trade name "Marproof" by NOF Corporation may be used.

[0095] The modified aliphatic polyester resin is preferably prepared by melt-kneading a mixture containing 0.02 to 1.0 parts by mass of the organic peroxide as described above relative to 100 parts by mass of unmodified aliphatic polyester resin, and further containing 0.1 to 1.2 parts by mass of a crosslinking aid such as the epoxy group-containing (meth)acrylic polymer. The ratio of the crosslinking aid to 100 parts by mass of unmodified aliphatic polyester resin may be 0.2 parts by mass or more, or 0.3 parts by mass or more. The ratio of the crosslinking aid to 100 parts by mass of unmodified aliphatic polyester resin may be 1.1 parts by mass or less, or 1.0 parts by mass or less. By carrying out such modification, a modified aliphatic polyester resin suitable as a main component of a resin composition having a gel fraction suitable for producing an aliphatic polyester resin foamed sheet having moderate depressions can be obtained.

[0096] The resin composition of the present embodiment exhibits good foamability by being melt-kneaded and extruded in an extruder together with a component for foaming the resin composition. Examples of the components for foaming that are supplied to the extruder together with the resin composition include a bubble adjuster and a foaming agent. In addition to the components, various additives may be added to the resin composition during extrusion foaming. Examples of the additives include a filler, a colorant, a flame retardant, an antibacterial agent, a weather resistance agent, and a surfactant. The proportion of additives other than the resin in the resin composition of the present embodiment is usually 10% by mass or less. The proportion of additives may be 8% by mass or less, or 6% by mass or less.

[0097] The aliphatic polyester resin foam sheet 1 in this embodiment can be produced by carrying out a modification step in which an aliphatic polyester resin, an organic peroxide, and a crosslinking aid are melt-kneaded to obtain a modified aliphatic polyester resin, and a sheet production step in which a resin composition containing the modified aliphatic polyester resin is extruded together with a foaming agent into a sheet to produce a foam sheet. The resin composition may be prepared only from the modified aliphatic polyester resin obtained in the modification step, or may be prepared by blending two or more modified aliphatic polyester resins, or blending one or more modified aliphatic polyester resins with one or more non-modified aliphatic polyester resins.

[0098] In this embodiment, the modification process, the resin composition preparation process for preparing a resin composition containing a modified aliphatic polyester resin, and the sheet production process using the resin composition obtained in the resin composition preparation process may each be carried out in a batchwise manner, or may be carried out continuously.

[0099] When the above-mentioned steps are carried out continuously, all the steps may be carried out in one extrusion line. For example, the above-mentioned steps can be carried out continuously using a tandem line equipped with a first extruder provided on the upstream side in the moving direction of the material, a second extruder connected on the downstream side of the first extruder, and a sheeting die (flat die, circular die) attached to the tip of the second extruder. In that case, for example, the modification step can be carried out by supplying the unmodified aliphatic polyester resin, the organic peroxide, and the crosslinking aid to the first extruder, and melt-kneading the unmodified aliphatic polyester resin, the organic peroxide, and the crosslinking aid in the first extruder.

[0100] In the present embodiment, a lamination step of laminating a non-foamed layer on one or both sides of the aliphatic polyester resin foamed sheet can be carried out after the sheet preparation step to prepare a laminated foamed sheet in which a foamed layer and a non-foamed layer made of the aliphatic polyester resin foamed sheet are laminated. This lamination step can also be carried out in a batchwise manner or continuously.

[0101] The non-foamed layer is laminated, for example, on the corrective surface 1a of the aliphatic polyester resin foam sheet 1. The non-foamed layer may be formed of a resin film composed of a resin composition different from the resin composition constituting the foam layer. Even if the resin film is poorly biodegradable, in this embodiment, since the aliphatic polyester resin foam sheet 1 has a depression, the foamed layer and the non-foamed layer can be easily separated. For example, a very small gap may be formed inside the non-foamed layer at the location where the depression occurs. Therefore, by applying hot air to the laminated foam sheet or its molded product from the non-foamed layer side, a bulge can be generated in the resin film forming the non-foamed layer at the portion corresponding to the depression, and the peeling between the foamed layer and the non-foamed layer can be advanced in the surface direction. In addition, even if a visible gap is not formed between the foamed layer and the non-foamed layer, the adhesive strength between the non-foamed layer and the portion corresponding to the depression is low, so the non-foamed layer can be easily peeled off from the portion.

[0102] The aliphatic polyester resin foamed sheet thus produced can be suitable as a raw sheet for producing a foamed molded body (thermoformed body) by thermoforming or the like. As a thermoforming method for obtaining a thermoformed body, a conventionally known method such as vacuum forming, pressure forming, and vacuum pressure forming can be adopted. In addition, a surface material such as paper, nonwoven fabric, or resin film can be adhered to the thermoformed body using the aliphatic polyester resin foamed sheet, and the surface material can be easily separated after use.

[0103] As described above, the aliphatic polyester resin foam sheet of the present embodiment is suitable as a resin foam sheet for a laminated foam sheet to form a laminated foam sheet in which a resin foam sheet is laminated with another sheet material, and has a corrected surface that has been corrected so that the unevenness of the surface formed by extrusion foaming is made flat, the corrected surface being a laminated surface on which another sheet material is laminated, and is suitable as a resin foam sheet for a laminated foam sheet having the above-mentioned depressions on the laminated surface.

[0104] The aliphatic polyester resin foam sheet of this embodiment is also suitable as a thermoforming resin foam sheet used for producing a thermoformed product with a surface material, which is a thermoformed product having a thermoformed product and a sheet-like surface material bonded to the surface of the thermoformed product. More specifically, the aliphatic polyester resin foam sheet of this embodiment is suitable as a thermoforming resin foam sheet having at least one surface that is flatly corrected and has the above-mentioned depressions formed on the corrected surface, which is thermoformed so that the corrected surface is an adhesive surface for the surface material.

[0105] The use of the aliphatic polyester resin foam sheet of the present embodiment is not limited to the above. In addition, in the present embodiment, an extruded foam sheet produced by an extrusion foaming method is exemplified as the aliphatic polyester resin foam sheet, but the aliphatic polyester resin foam sheet of the present embodiment does not have to be an extruded foam sheet. For example, even in the case where a foam sheet is produced by impregnating a non-foamed aliphatic polyester resin sheet having gel particles dispersed therein with a foaming agent under pressure and then releasing the pressure, an aliphatic polyester resin foam sheet having depressions formed on the surface can be obtained, and the aliphatic polyester resin foam sheet can be easily separated and collected.

[0106] As described above, the examples in this embodiment are limited, and the aliphatic polyester resin foamed sheet of this embodiment, its manufacturing method, applications, etc. are not limited to the above examples. As described above, this embodiment includes the following disclosures.

[0107] (1) An aliphatic polyester resin foamed sheet composed of a resin composition containing an aliphatic polyester resin, 5 pieces / cm on surface 2 More than 30 pieces / cm 2 An aliphatic polyester resin foam sheet having depressions in the following proportions:

[0108] (2) The aliphatic polyester resin foam sheet according to (1), wherein the resin composition has a melt tension of 25 cN or more at 190° C. and a melt mass-flow rate of 1.9 g / 10 min or less under a nominal load of 2.16 kg.

[0109] (3) 1. An aliphatic polyester resin foamed sheet according to claim 1, which, when made into a non-foamed sheet by thermal melting, satisfies at least one of the following (A) and (B): (A) Maximum tensile stress is 5.0 MPa or more (B) Fracture energy is 0.05 J / m 3 More than 0.25J / m 3 below

[0110] (4) The aliphatic polyester resin foam sheet according to any one of (1) to (3), wherein the aliphatic polyester resin is a polylactic acid resin.

[0111] (5) The aliphatic polyester resin foam sheet according to any one of (1) to (4), wherein the resin composition contains an epoxy group-containing acrylic-modified styrene resin.

[0112] (6) The aliphatic polyester resin foam sheet according to any one of (1) to (5), having a gel fraction of 0.3% by mass or more and 1.2% by mass or less. EXAMPLES

[0113] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these. <Example 1> (1) Preparation of modified aliphatic polyester resin A mixture was obtained by stirring and mixing 100 parts by mass of polylactic acid resin ("FY804" manufactured by Toyohara Group Co., Ltd., D content: 4%), 0.3 parts by mass of organic peroxide: t-butylperoxy-3,5,5-trimethylhexanoate ("Trigonox 42" manufactured by Kayaku Nouryon Co., Ltd., 1-minute half-life temperature T1: 159°C), and 0.5 parts by mass of epoxy group-containing acrylic modified styrene resin ("Joncryl ADR 4468" manufactured by BASF) in a ribbon blender. The resulting mixture was fed into a twin-screw extruder with a diameter of 57 mm (L / D=31.5). The mixture was melt-kneaded in a twin-screw extruder with the feed section set at 170°C and the subsequent temperatures set at 200°C and the rotation speed at 100 rpm, and the kneaded material was extruded in the form of strands at an output of 30 kg / h from a die with an orifice diameter of 3 mm and 18 holes attached to the tip of the extruder. The extruded strand-like kneaded product was then cooled by passing it through a 2 m long cooling water tank containing water at 30° C. The cooled strand was cut with a pelletizer to obtain pellets of the modified polylactic acid resin.

[0114] (2) Preparation of foam 100 parts by mass of the modified aliphatic polyester resin obtained by the above-mentioned method and 1.0 part by mass of a cell regulator ("Crown Talc" manufactured by Matsumura Sangyo Co., Ltd.) were dry blended to prepare a mixture. In a tandem extruder equipped with a first extruder (upstream) having a diameter of φ50 mm and a second extruder (downstream) having a diameter of φ65 mm, the obtained mixture was supplied to the first extruder having a diameter of φ50 mm through a hopper and heated to melt it. Thereafter, butane (isobutane / normal butane=70 / 30) as a foaming agent was pressure-fed into the first extruder and melt-mixed together with the above mixture. Next, this molten mixture was transferred to a second extruder with a diameter of 65 mm and uniformly cooled to a temperature suitable for extrusion foaming, and then extrusion foaming was performed through a circular die with a diameter of 70 mm at a discharge rate of 30 kg / h to obtain a cylindrical foam. The obtained cylindrical foam was placed on a φ206 mm mandrel whose inside was cooled with water at about 20°C, and its outer surface was cooled and molded by blowing air onto it using an air ring larger in diameter than the mandrel. It was then cut at one point on the circumference with a cutter to obtain a strip-shaped aliphatic polyester resin foam sheet.

[0115] <Example 2> An aliphatic polyester resin foamed sheet was produced in the same manner as in Example 1, except that 0.6 parts of t-butylperoxy-3,5,5-trimethylhexanoate was used in the production method of the aliphatic polyester resin foamed sheet.

[0116] <Example 3> In the manufacturing method of the aliphatic polyester resin foam sheet, an aliphatic polyester resin foam sheet was produced in the same manner as in Example 1, except that the type of organic peroxide used was 0.3 parts by mass of t-butylperoxyisopropyl monocarbonate ("Trigonox BPIC-75" manufactured by Nouryon Chemical Industry Co., Ltd., 1-minute half-life temperature T1: 156°C).

[0117] <Comparative Example 1> An aliphatic polyester resin foam sheet was produced in the same manner as in Example 1, except that in the manufacturing method of the aliphatic polyester resin foam sheet, no epoxy group-containing acrylic-modified styrene-based resin was added, and only 0.5 parts by mass of t-butylperoxyisopropyl monocarbonate was used.

[0118] The properties of the modified aliphatic polyester resin used for producing the aliphatic polyester resin foam sheet and the obtained aliphatic polyester resin foam sheet were measured. The results are shown in Table 2. The results for each evaluation item in the table represent the results measured by the methods described above. The following items were evaluated as follows:

[0119] <Depression formation ratio> The percentage of dents was measured using the method described above, and the number of dents per unit area was 30 / cm 2The number of depressions per unit area was 30 / cm or less, and the rest was judged as "x". 2 It was visually confirmed that a beautiful appearance could be obtained if the thickness was less than 100 mm. Photographs of the appearance of the aliphatic polyester foam sheet of Example 1 and the aliphatic polyester foam sheet of Comparative Example 1 are shown in FIG. 4. This figure also shows that dimples were formed at an appropriate rate in the examples. Coarse dimples were observed in the aliphatic polyester foam sheet of Comparative Example 1. This is because the number of dimples per unit area was 30 / cm. 2 This is thought to be because, once the thickness exceeds this value, multiple depressions that should otherwise be individual depressions merge together.

[0120] <Removability> (Film peeling test) A laminated foam sheet was produced by passing an aliphatic polyester resin foam sheet and a 20 μm-thick polybutylene adipate terephthalate resin film, which were superimposed, through a heated roll (diameter: 150 mm, heating temperature: 140° C.) at 2.0 m / min and immediately thereafter through a cooling roll with a surface temperature of 25° C. A rectangular test piece with a width of 15 mm and a length of 100 mm was cut from the laminated foam sheet so that the longitudinal direction was the extrusion direction (MD) of the foam sheet. The polybutylene adipate terephthalate resin film was peeled off over a small section (less than 20 mm) from one end of the longitudinal direction of this rectangular sample toward the other end, and the end of the polybutylene adipate terephthalate resin film where the peeling began was set in a tensile testing machine (manufactured by Orientec Corporation, "Tensilon RTM-500"), and while holding the rectangular sample so that the peeling direction was 90 degrees, a peeling test of the polybutylene adipate terephthalate resin film was performed at a tensile speed of 200 mm / min. In the test, it was confirmed whether peeling was possible at the interface between the polybutylene adipate terephthalate resin film and the aliphatic polyester resin foam sheet. If peeling was possible at the interface but the polybutylene adipate terephthalate resin film peeled off easily without making any noise during peeling, it was judged that the adhesive strength was insufficient and was judged as "X". If peeling was possible at the interface and the polybutylene adipate terephthalate resin film peeled off with a sound during peeling, it was judged that the adhesive strength was at an acceptable level and was judged as "O".

[0121] <Dimensional change rate due to heating> Three flat square test pieces with sides of about 10 cm each were cut out from the aliphatic polyester resin foam sheet of each example so that each side was parallel to the extrusion direction (MD) or width direction (TD) of the aliphatic polyester resin foam sheet. Next, two straight lines were drawn in a cross shape on the aliphatic polyester resin foam sheet of each test piece, connecting the centers of the opposing sides. At this time, the length of the straight line in the extrusion direction (MD1), the length of the straight line in the width direction (TD1), and the thickness of the foam sheet at the intersection of the cross (VD1) were measured before heating. Next, each test piece was placed on a flat platform in an oven with no humidity control set at 70°C and heated for 150 seconds, then removed from the oven and cooled at room temperature for 30 minutes. Thereafter, the straight line length in each direction (MD2, TD2) and the thickness (VD2) of each test piece after heating were measured. The thermal deformation rate (%) of each test piece was calculated by the following formula (s), and the arithmetic mean value was taken as the thermal deformation rate (%) of the foamed sheet, which was used as the evaluation standard for heat resistance. The evaluation was made as follows: "Good" was given to those whose thermal dimensional change rate was 25% or less, and "Poor" was given to others. Heat deformation rate (%) = (MDr + TDr + VDr) / 3 (s) MD transformation rate (MDr) (%) = (|MD2-MD1| / MD1) × 100 TD deformation rate (TDr) (%) = (|TD2-TD1| / TD1) × 100 VD deformation rate (VDr) (%) = (|VD2-VD1| / VD1) × 100

[0122] <Moldability> A flat rectangular test piece measuring 700 mm in length and 640 mm in width was cut out from each of the extruded foam sheets produced. Next, a single-shot molding machine (manufactured by Tosei Sangyo Co., Ltd., product name "Unic Automatic Molding Machine FM-3A") was prepared, and the average temperature of the upper heater of this single-shot molding machine was set to 272°C, the average temperature of the lower heater was set to 240°C, the upper atmospheric temperature was set to 183°C, and the lower atmospheric temperature was set to 180°C. Next, the above test pieces were introduced into a single-shot molding machine and heated for 5 seconds each, and then heat molding was performed using a mold containing 22 truncated cones of different heights, each measuring 10 mm in diameter (top surface) and 35 mm in diameter (bottom surface). The mold surface temperature was adjusted to 50°C. The heat molding was carried out three times for each heating time. The heights of the 22 truncated cones are as shown in Table 1. Thereafter, the molded products molded after each heating time were visually inspected, and the number of the tallest truncated cone among those that had no tears in each cone shape was recorded as the score for that molding. The same molding was performed two more times, and the scores from the three moldings were averaged to obtain the elongation value. An elongation value of 16 or more was rated as "good", and anything else was rated as "poor".

[0123] [Table 1]

[0124] <Overall rating> As an overall judgment, for all the evaluations of the physical properties of the aliphatic polyester foam sheet, those that were all "good" were judged as "good", those with one "bad" were judged as "good", and those with two or more "bad" were judged as "bad".

[0125] [Table 2]

[0126] In the aliphatic polyester resin foamed sheets of the Examples, even if a non-foamed layer was formed on the surface on which the depressions were formed, the non-foamed layer was relatively easy to peel off. From the above, it can be seen that the present invention provides an aliphatic polyester resin foamed sheet which is suitable for use in thermoforming and is easy to isolate. [Explanation of symbols]

[0127] 1: Aliphatic polyester resin foam sheet, 1a: Correction surface, 1p: Recess

Claims

1. An aliphatic polyester resin foamed sheet composed of a resin composition containing an aliphatic polyester resin, 5 particles / cm on surface 2 More than 30 pieces / cm 2 An aliphatic polyester resin foam sheet having depressions in the following proportions:

2. 2. The aliphatic polyester resin foam sheet according to claim 1, wherein the resin composition has a melt tension of 25 cN or more at 190° C. and a melt mass flow rate of 1.9 g / 10 min or less under a nominal load of 2.16 kg.

3. 3. The aliphatic polyester resin foamed sheet according to claim 1, which, when made into a non-foamed sheet by thermal melting, satisfies at least one of the following (A) and (B): (A) Maximum tensile stress is 5.0 MPa or more (B) Fracture energy is 0.05 J / m 3 0.25J / m or more 3 below

4. 3. The aliphatic polyester resin foam sheet according to claim 1, wherein the aliphatic polyester resin is a polylactic acid resin.

5. 3. The aliphatic polyester resin foam sheet according to claim 1, wherein the resin composition comprises an epoxy group-containing acrylic-modified styrene resin.

6. 3. The aliphatic polyester resin foam sheet according to claim 1, having a gel fraction of 0.3% by mass or more and 1.2% by mass or less.

Citation Information

Patent Citations

  • Method for producing modified polylactic resin, polylactic resin and polylactic resin foam sheet

    JP2019183098A