Pressure-sensitive adhesive tape
The adhesive tape with a fluororesin base material and white particle adhesive layer addresses reflectivity and flexibility issues, ensuring effective adhesion to non-flat surfaces in optical devices.
Patent Information
- Application Number
- JP2023047131
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing adhesive tapes using fluororesin as a base material face issues with colorant shedding and are not suitable for non-flat surfaces in optical devices due to insufficient reflectivity and flexibility.
An adhesive tape with a fluororesin base material having a thickness of 90 μm or less, a reflectance of 50% or more for light with a wavelength of 550 nm, and an adhesive layer containing white particles, ensuring excellent reflectivity and flexibility for non-flat surfaces.
The adhesive tape provides high reflectivity and flexibility, suitable for optical devices with non-flat surfaces, minimizing colorant shedding and improving adhesion.
Smart Images

Figure 2024136140000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive tape. [Background technology]
[0002] Adhesive tapes with excellent light reflectivity are sometimes used inside optical devices equipped with optical members, such as liquid crystal displays (LCD) and electroluminescence (EL) displays. Patent Document 1 discloses an adhesive tape that is applied between a liquid crystal panel and a backlight housing of an LCD module. Patent Document 1 describes that an adhesive tape with excellent reflectivity can be obtained by using a tape substrate equipped with a light reflecting layer having a polyester film containing a white coloring agent. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-175328 A Summary of the Invention [Problem to be solved by the invention]
[0004] It is conceivable to use fluororesin instead of polyester resin as the tape substrate. The use of fluororesin is expected to improve the cushioning and slipperiness of the adhesive tape. However, fluororesin is generally soft, and when a white colorant is added to the substrate, the colorant is more likely to fall off during use than polyester resin. It is desirable to prevent the colorant from falling off in optical devices. In other words, there has been insufficient consideration to obtain an adhesive tape with excellent reflectivity while using fluororesin as the substrate. In addition, Patent Document 1 only considers the application of the adhesive tape to a flat surface. However, in recent optical devices that have been further thinned and highly functionalized, for example, the shapes of the components are diverse, and the application surface of the adhesive tape is not necessarily flat. It is also assumed that the adhesive tape is applied while being folded.
[0005] An object of the present invention is to provide an adhesive tape that has a substrate containing a fluororesin and is suitable for use in optical devices. [Means for solving the problem]
[0006] The present invention relates to A substrate containing a fluororesin and a pressure-sensitive adhesive layer disposed on the substrate, The reflectance of at least one surface for light with a wavelength of 550 nm is 50% or more, The thickness of the substrate is 90 μm or less. Adhesive tape, to provide. Effect of the Invention
[0007] The pressure-sensitive adhesive tape of the present invention is suitable for use in optical devices, even though it has a substrate containing a fluororesin. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an example of the pressure-sensitive adhesive tape of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates an example of the pressure-sensitive adhesive tape of the present invention. [Diagram 3] FIG. 3 is a schematic diagram for explaining the tracking test 2 carried out in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The pressure-sensitive adhesive tape according to the first aspect of the present invention comprises: A substrate containing a fluororesin and a pressure-sensitive adhesive layer disposed on the substrate, The reflectance of at least one surface for light with a wavelength of 550 nm is 50% or more, The substrate has a thickness of 90 μm or less.
[0010] In a second aspect of the present invention, for example, in the pressure-sensitive adhesive tape according to the first aspect, the substrate is a cut sheet.
[0011] In a third aspect of the present invention, for example, in the pressure-sensitive adhesive tape according to the first or second aspect, the pressure-sensitive adhesive layer contains white particles.
[0012] In a fourth aspect of the present invention, for example, in the pressure-sensitive adhesive tape according to the third aspect, the content of the white particles in the pressure-sensitive adhesive layer is 3.5% by weight or more and 30% by weight or less.
[0013] In a fifth aspect of the present invention, for example, the pressure-sensitive adhesive tape according to the third or fourth aspect contains only the fluororesin contained in the base material and the white particles contained in the pressure-sensitive adhesive layer as materials that diffuse and / or reflect light.
[0014] In a sixth aspect of the present invention, for example, in the pressure-sensitive adhesive tape according to any one of the first and third to fifth aspects, the substrate is a stretched sheet.
[0015] In a seventh aspect of the present invention, for example, in the pressure-sensitive adhesive tape according to any one of the first to sixth aspects, the base material has a single-layer structure.
[0016] In an eighth aspect of the present invention, for example, in the pressure-sensitive adhesive tape according to any one of the first to seventh aspects, the fluororesin is polytetrafluoroethylene (PTFE).
[0017] In a ninth aspect of the present invention, for example, in an adhesive tape according to any one of the first to eighth aspects, the adhesive tape is a single-sided adhesive tape, and the reflectance of the surface on the substrate side for light with a wavelength of 550 nm is 50% or more.
[0018] In a tenth aspect of the present invention, for example, in the pressure-sensitive adhesive tape according to any one of the first to ninth aspects, the reflectance of the at least one surface to light with a wavelength of 450 nm is 50% or more.
[0019] In an eleventh aspect of the present invention, for example, in the pressure-sensitive adhesive tape according to any one of the first to tenth aspects, the 180° peel adhesive strength is 0.6 N / 10 mm or more.
[0020] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The present invention is not limited to the following embodiment.
[0021] An example of the adhesive tape of this embodiment is shown in Fig. 1. The adhesive tape 1 in Fig. 1 includes a substrate 2 containing a fluororesin and an adhesive layer 3 disposed on the substrate 2. The adhesive tape 1 has a reflectance (hereinafter referred to as R550) of at least one surface for light with a wavelength of 550 nm of 50% or more. The substrate 2 has a thickness of 90 µm or less.
[0022] The substrate 2 containing fluororesin is more flexible than substrates made of other resins, typically polyester resins. The thickness of the substrate 2 is limited to 90 μm or less. Therefore, the adhesive tape 1 has excellent conformability to the application surface, and can improve its application even when the adhesive tape is applied to an application surface having a step due to the design of the optical device, or when the adhesive tape must be applied while being folded. Furthermore, the reflectance of at least one surface for light with a wavelength of 550 nm is equal to or greater than a predetermined value. The adhesive tape 1 is suitable for use in optical devices.
[0023] R550 may be 55% or more, 60% or more, 63% or more, 65% or more, 68% or more, 70% or more, 73% or more, 75% or more, 78% or more, 80% or more, or even 83% or more. The upper limit of R550 is, for example, 100% or less, and may be 98% or less, 95% or less, 93% or less, or even 90% or less.
[0024] The thickness of the substrate 2 may be 80 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 45 μm or less, or even 40 μm or less. The lower limit of the thickness may be 10 μm or more, 15 μm or more, 20 μm or more, 23 μm or more, 25 μm or more, 28 μm or more, 30 μm or more, 33 μm or more, or even 35 μm or more.
[0025] [Base material] The substrate 2 includes a fluororesin. The fluororesin may be the main component of the substrate 2. In this specification, the main component means a component with the largest content. The content of the main component is, for example, 50% by weight or more, and may be 60% by weight or more, 70% by weight or more, 80% by weight or more, 90% by weight or more, or even 95% by weight or more. The substrate 2 may be substantially composed of a fluororesin, and in this case, the content of the fluororesin in the substrate 2 may be, for example, 97% by weight or more, 98% by weight or more, 99% by weight or more, 99.5% by weight or more, 99.9% by weight or more, or even more than 99.9% by weight.
[0026] The fluororesin is, for example, at least one selected from polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), perfluoroalkoxyalkane (PFA), polytetrafluoroethylene-polyhexafluoropropylene copolymer (FEP), and ethylene-polytetrafluoroethylene copolymer (ETFE). The fluororesin may be PTFE. According to the study by the present inventors, the deformability and stiffness of the substrate 2 can also contribute to the conformability of the adhesive tape 1. The deformability affects, for example, the ease of folding the adhesive tape 1. The stiffness affects, for example, the suppression of wrinkles when the adhesive tape 1 is applied. The thinner the adhesive tape 1, the more likely it is that wrinkles will occur when applied. PTFE is particularly suitable for achieving a substrate 2 with good deformability and stiffness.
[0027] The substrate 2 may be a cut sheet (skive sheet). A typical example of the substrate 2 that is a cut sheet is a PTFE cut sheet. The fact that the substrate 2 is a cut sheet can be determined by observing the surface of the sheet under magnification, where linear scratches (known to those skilled in the art as cut scratches) that are characteristic of cut sheets can be confirmed. An example of a method for producing the substrate 2 that is a cut sheet is shown below, in which the fluororesin is PTFE.
[0028] PTFE powder (molding powder) is introduced into a mold, and a predetermined pressure is applied for a predetermined time to perform preforming. Preforming can be performed at room temperature. The shape of the internal space of the mold that contains the PTFE powder is preferably cylindrical in order to enable cutting by a cutting lathe, which will be described later. In this case, a cylindrical PTFE block can be formed. Next, the formed preform is removed from the mold and baked for a predetermined time at a temperature equal to or higher than the melting point of PTFE (327°C) to obtain a PTFE block. Next, the obtained PTFE block is cut to a predetermined thickness to produce a PTFE sheet, which is a cut sheet. When the PTFE block is cylindrical, it is possible to use a cutting lathe that continuously cuts the surface while rotating the block, thereby making it possible to efficiently manufacture the PTFE sheet. In addition, the cutting lathe makes it relatively easy to control the thickness of the PTFE sheet to be manufactured, and a strip-shaped PTFE sheet can also be manufactured. The PTFE sheet can be used as it is, or after various treatments such as heat treatment and surface modification treatment for removing distortion are performed, as the substrate 2.
[0029] The substrate 2 may be a stretched sheet. A typical example of the substrate 2 that is a stretched sheet is a microporous stretched PTFE sheet. In this specification, a microporous sheet means a sheet having an air permeability in the thickness direction, expressed as a Gurley number, in the range of 20 to 10,000 seconds / 100 mL. The air permeability in the thickness direction of the microporous sheet may be 20 to 5,000 seconds / 100 mL, 40 to 1,000 seconds / 100 mL, or even 50 to 300 seconds / 100 mL. The Gurley number means air permeability given by the air permeability measurement method B (Gurley type method) specified in JIS L1096 (2010).
[0030] The average pore size of the microporous sheet is, for example, 0.01 to 1 μm. The porosity of the microporous sheet is, for example, 5 to 50%. The average pore size can be measured in accordance with ASTM (American Society for Testing and Materials) F316-86. The porosity can be calculated by substituting the mass and volume of the sheet and the true density of the material constituting the sheet into the following formula. Note that the true density of PTFE is 2.18 g / cm 3 It is. Formula: Porosity [%] = {1-(mass [g] / (thickness [cm] × area [cm 2 ] × true density [g / cm 3 ]))}×100
[0031] An example of a method for producing the substrate 2 which is a microporous stretched sheet will be described below, assuming that the fluororesin is PTFE.
[0032] A coating film is formed by applying a dispersion of PTFE powder (PTFE dispersion) to a base sheet. The base sheet can be formed from a heat-resistant material such as heat-resistant plastic (polyimide, polyether ether ketone, etc.), metal, and ceramic. The coating film can be formed by immersing the base sheet in the dispersion liquid, in addition to a method using a coater. The dispersion liquid may contain a surfactant to increase wettability to the base sheet. Next, the formed coating film is heated to remove the dispersion medium in the coating film and to bond the PTFE particles to each other, thereby obtaining a cast sheet of PTFE. In a typical example of heating, the dispersion medium is removed by heating at about 90 to 150°C (first stage), and then the PTFE particles are bonded by heating at about 350 to 400°C (second stage), which is a temperature above the melting point of PTFE. The thickness of the cast sheet may be increased by repeating the formation and heating of the coating film. A PTFE sheet, which is a cast sheet, may be used as the substrate 2.
[0033] Next, the cast sheet peeled off from the base sheet is rolled in one direction in its plane (e.g., MD; in the case of a strip, the longitudinal direction), and further stretched in one direction in its plane different from the above (e.g., TD; in the case of a strip, the width direction), to produce a PTFE sheet, which is a microporous stretched sheet. The rolling can be performed, for example, by press rolling or roll rolling. The rolling temperature is, for example, 80 to 200°C. The rolling ratio is, for example, 1.25 to 3.5 times. For stretching, various stretching machines such as a tenter stretching machine can be used. The stretching temperature is, for example, 100 to 400°C. The stretching ratio is, for example, 1.25 to 3.5 times. The PTFE sheet can be used as the substrate 2 as it is or after various treatments such as surface modification treatment are performed.
[0034] An example of the surface modification treatment is a treatment for enhancing the bondability of the PTFE sheet. This treatment can improve the anchoring property of the adhesive layer 3 to the substrate 2 including the PTFE sheet. The treatment for enhancing the bondability may be a chemical treatment or a physical treatment. An example of the chemical treatment is an alkali metal treatment using an alkali metal such as sodium. In the alkali metal treatment, for example, an etching solution containing metallic sodium is brought into contact with the PTFE sheet (sodium treatment). Examples of the etching solution are metallic sodium / liquid ammonia solution in which metallic sodium is dissolved in liquid ammonia, and metallic sodium / naphthalene solution in which metallic sodium is dissolved in naphthalene solution. An example of the physical treatment is a sputter etching treatment. The sputter etching treatment can be performed, for example, by applying a high-frequency voltage to a PTFE sheet accommodated in a reduced pressure chamber under an inert gas atmosphere such as argon or nitrogen.
[0035] Another example of the substrate 2 that is a stretched sheet is a porous stretched PTFE sheet. The porous stretched PTFE sheet can be formed, for example, by stretching a paste extrudate containing PTFE particles, or by stretching a cast sheet without rolling. The air permeability in the thickness direction of the porous sheet, expressed as the Gurley number, is usually less than 20 seconds / 100 mL.
[0036] 1, one exposed surface 11, in other words, the exposed surface of the substrate 2 opposite to the side of the pressure-sensitive adhesive layer 3, is made of the substrate 2 containing a fluororesin. The fact that the exposed surface 11 is made of the substrate 2 can contribute to improving the slipperiness of the pressure-sensitive adhesive tape 1.
[0037] The substrate 2 in Fig. 1 has a single-layer structure. The substrate 2 having a single-layer structure of a layer containing a fluororesin can particularly contribute to improving the conformability of the pressure-sensitive adhesive tape 1 and improving the slipperiness as a single-sided pressure-sensitive adhesive tape. However, the substrate 2 may have a multi-layer structure composed of two or more layers.
[0038] The substrate 2 may be a sheet having at least one main surface, particularly the main surface on the side of the pressure-sensitive adhesive layer 3, subjected to a surface modification treatment. Examples of the surface modification treatment include an alkali metal treatment and a sputter etching treatment.
[0039] The shape of the substrate 2 is, for example, a polygon such as a square or a rectangle, or a strip shape, but the shape of the substrate 2 is not limited to the above examples.
[0040] [Adhesive layer] The adhesive layer 3 is a layer formed from an adhesive composition. Examples of the adhesive composition are acrylic, silicone, urethane and rubber-based adhesive compositions. The adhesive composition may be acrylic or silicone, or may be acrylic. In other words, the adhesive layer 3 may be an acrylic adhesive layer, a silicone adhesive layer, or may be an acrylic adhesive layer. However, the adhesive composition capable of forming the adhesive layer 3 is not limited to the above examples. Examples of acrylic adhesive compositions are disclosed in JP 2005-105212 A. Examples of silicone adhesives are disclosed in JP 2003-313516 A (including those disclosed as comparative examples).
[0041] The pressure-sensitive adhesive layer 3 may contain white particles. The pressure-sensitive adhesive layer 3 containing white particles can contribute to improving the reflectance of the pressure-sensitive adhesive tape 1.
[0042] An example of the white particles is an inorganic particle. An example of the inorganic particle is a particle composed of a metal oxide such as titanium oxide (typically titanium dioxide), zinc oxide, aluminum oxide, calcium oxide, tin oxide, barium oxide, and cesium oxide, a particle composed of a metal carbonate such as calcium carbonate and barium carbonate, and a particle composed of a metal hydroxide such as aluminum hydroxide, calcium hydroxide, and zinc hydroxide. The white particles may be organic particles such as resin particles. The white particles may be titanium oxide particles.
[0043] The content of the white particles in the pressure-sensitive adhesive layer 3 containing the white particles is, for example, 0.1% by weight or more and 90% by weight or less. The lower limit of the content of the white particles may be 0.5% by weight or more, 0.9% by weight or more, 1% by weight or more, 3% by weight or more, 3.5% by weight or more, 4% by weight or more, 5% by weight or more, 6% by weight or more, 8% by weight or more, 10% by weight or more, 12% by weight or more, or even 13% by weight or more. The upper limit of the content may be 80% by weight or less, 70% by weight or less, 60% by weight or less, 50% by weight or less, 45% by weight or less, 40% by weight or less, 35% by weight or less, 30% by weight or less, 25% by weight or less, or even 20% by weight or less. The content of the white particles may be 3.5% by weight or more and 30% by weight or less.
[0044] The thickness of the pressure-sensitive adhesive layer 3 is, for example, 1 to 50 μm. The lower limit of the thickness of the pressure-sensitive adhesive layer 3 may be 3 μm or more, 5 μm or more, 7 μm or more, 10 μm or more, or even 12 μm or more. The upper limit of the thickness of the pressure-sensitive adhesive layer 3 may be 45 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, 23 μm or less, 20 μm or less, or even 18 μm or less.
[0045] The adhesive layer 3 may contain other materials than those mentioned above. The other materials may be materials contained in the adhesive composition capable of forming the adhesive layer 3. Examples of other materials are additives such as crosslinking agents, crosslinking assistants, leveling agents, plasticizers, softeners, antistatic agents, ultraviolet absorbers, antioxidants, and light stabilizers. However, the adhesive layer 3 may be substantially free of fluorescent agents and metal particles. The adhesive layer 3 substantially free of fluorescent agents and metal particles can contribute to suppressing the difference in reflectance due to the wavelength of light in the adhesive tape 1, for example, reducing the absolute value of the difference between R550 and the reflectance of at least one surface for light with a wavelength of 450 nm (hereinafter referred to as R450). An example of a fluorescent agent is a fluorescent brightening agent. In this specification, substantially free means that the content is, for example, 0.1% by weight or less, preferably 0.05% by weight or less, more preferably 0.03% by weight or less, and particularly preferably less than 0.01% by weight.
[0046] [Adhesive tape] The adhesive tape 1 in Fig. 1 includes a substrate 2 and an adhesive layer 3. Examples of combinations of the substrate 2 and the adhesive layer 3 include a combination of the substrate 2 which is a cut sheet or a cast sheet, particularly a cut sheet, with the adhesive layer 3 which contains white particles, and a combination of the substrate 2 which is a stretched sheet with the adhesive layer 3 which does not substantially contain white particles. The substrate 2 may not substantially contain white particles.
[0047] The pressure-sensitive adhesive tape 1 may contain only the fluororesin contained in the substrate 2 and the white particles contained in the pressure-sensitive adhesive layer 3 as materials that diffuse and / or reflect light. This embodiment is particularly suitable for improving the conformability to the application surface. This embodiment is also suitable for suppressing the difference in reflectance of the pressure-sensitive adhesive tape 1 depending on the wavelength of light.
[0048] The R450 of the pressure-sensitive adhesive tape 1 is, for example, 50% or more, and may be 55% or more, 60% or more, 63% or more, 65% or more, 68% or more, 70% or more, 73% or more, 75% or more, 78% or more, 80% or more, 83% or more, or even 85% or more. The upper limit of R450 is, for example, 100% or less, and may be 98% or less, 95% or less, 93% or less, or even 90% or less.
[0049] The reflectance of at least one surface of the pressure-sensitive adhesive tape 1 to light having a wavelength of 630 nm (hereinafter referred to as R630) is, for example, 45% or more, and may be 50% or more, 55% or more, 60% or more, 63% or more, 65% or more, 68% or more, 70% or more, 73% or more, 75% or more, 78% or more, or even 80% or more. The upper limit of R630 is, for example, 100% or less, and may be 98% or less, 95% or less, 93% or less, or even 90% or less.
[0050] The absolute value of the difference between R450 and R550 may be 6% or less, 5.5% or less, 5% or less, 4.5% or less, 4% or less, 3.5% or less, 3% or less, 2.5% or less, or even 2% or less. The pressure-sensitive adhesive tape 1 having a small absolute value is particularly suitable for use in optical devices. R450 may be smaller or larger than R550.
[0051] The absolute value of the difference between R630 and R550 may be 5% or less, 4.5% or less, 4% or less, 3.5% or less, or even 3% or less. The pressure-sensitive adhesive tape 1 having the small absolute value is particularly suitable for use in optical devices. R630 may be smaller or larger than R550.
[0052] R450, R550 and R630 can be determined from the reflection spectrum of the pressure-sensitive adhesive tape 1 evaluated using an optical property evaluation device such as a spectrophotometer. The reflection spectrum is evaluated in a state where the pressure-sensitive adhesive tape 1 is attached to a mirror-finished surface of a stainless steel plate. At this time, light for evaluating the reflection spectrum is incident on the pressure-sensitive adhesive tape 1 from the exposed surface opposite to the stainless steel plate. The pressure-sensitive adhesive layer 3 of the pressure-sensitive adhesive tape 1 can be used for attachment to the stainless steel plate, and in this case, the substrate side reflectance can be determined for the pressure-sensitive adhesive tape 1, which is a single-sided pressure-sensitive adhesive tape.
[0053] The pressure-sensitive adhesive tape 1 in Fig. 1 is a single-sided pressure-sensitive adhesive tape. For the pressure-sensitive adhesive tape 1 which is a single-sided pressure-sensitive adhesive tape, each of the reflectances R450, R550, and R630 may be the reflectance when light is incident from the side of the substrate 2 (substrate-side reflectance). In other words, the pressure-sensitive adhesive tape 1 may be a single-sided pressure-sensitive adhesive tape, and the reflectance of the surface on the substrate 2 side for light with a wavelength of 550 nm may be 50% or more.
[0054] The adhesive tape 1 of the present embodiment is not limited to a single-sided adhesive tape, and may be a double-sided adhesive tape. The adhesive tape 1, which is a double-sided adhesive tape, comprises a base material 2 and a pair of adhesive layers respectively disposed on both main surfaces of the base material 2. At least one of the adhesive layers may be adhesive layer 3, and both adhesive layers may be adhesive layer 3. For the adhesive layer other than adhesive layer 3, an adhesive layer provided in a known adhesive tape may be applied.
[0055] The thickness of the pressure-sensitive adhesive tape 1 is, for example, 6 to 400 μm. The upper limit of the thickness of the pressure-sensitive adhesive tape 1 may be 350 μm or less, 300 μm or less, 250 μm or less, 200 μm or less, 150 μm or less, 125 μm or less, 100 μm or less, 85 μm or less, 75 μm or less, 70 μm or less, 65 μm or less, 60 μm or less, or even 55 μm or less. The lower limit of the thickness of the pressure-sensitive adhesive tape 1 may be 10 μm or more, 15 μm or more, 20 μm or more, 25 μm or more, 30 μm or more, or even 35 μm or more.
[0056] The pressure-sensitive adhesive tape 1 may be a white pressure-sensitive adhesive tape having a white appearance on at least one side selected from the substrate 2 and the pressure-sensitive adhesive layer 3, typically the substrate 2 side. In this specification, white refers to a whiteness having a whiteness of, for example, L * a * b * Color space L * It means that the value is 70 or more. * a * b * The color system was established in 1976 by the International Commission on Illumination (CIE) and is also known as "CIELAB". * a * b * In the color system, L corresponds to lightness. * The higher the value, the higher the whiteness.
[0057] The 180° peel adhesive strength of the adhesive tape 1 may be, for example, 0.6 N / 10 mm or more, 0.8 N / 10 mm or more, 1.0 N / 10 mm or more, 1.2 N / 10 mm or more, 1.4 N / 10 mm or more, 1.5 N / 10 mm or more, 1.6 N / 10 mm or more, or even 1.7 N / 10 mm or more. The upper limit of the 180° peel adhesive strength may be, for example, 6.0 N / 10 mm or less, less than 5.5 N / 10 mm, 5.0 N / 10 mm or less, 4.5 N / 10 mm or less, 4.0 N / 10 mm or less, 3.5 N / 10 mm or less, 3.2 N / 10 mm or less, 2.5 N / 10 mm or less, 2.0 N / 10 mm or less, or even 1.8 N / 10 mm or less. The 180° peel adhesive strength can be measured in accordance with the method for measuring 180° peel adhesive strength for adhesive tape defined in Japanese Industrial Standards (formerly Japanese Industrial Standards; JIS) Z0237: 2009. The 180° peel adhesive strength is the adhesive strength (initial adhesive strength) before the heating test described later.
[0058] The adhesive tape 1 has a 180° peel adhesion (adhesive strength after heat test) after a heat test (left in an atmosphere at 60° C. for one week) of, for example, 1.0 N / 10 mm or more, 1.2 N / 10 mm or more, 1.3 N / 10 mm or more, 1.4 N / 10 mm or more, 1.5 N / 10 mm or more, 1.8 N / 10 mm or more, 2.0 N / 10 mm or more, 2.5 N / 10 mm or more, 3.0 N / 10 mm or more, 3.5 N / 10 mm or more, or even 3.8 N / 10 mm or more. The upper limit of the adhesive strength after heat test is, for example, 6.0 N / 10 mm or less, and may be less than 5.5 N / 10 mm, 5.0 N / 10 mm or less, 4.5 N / 10 mm or less, or even 4.3 N / 10 mm or less. The adhesive strength after the heat test can be measured in the same manner as the initial adhesive strength, except that the adhesive tape 1 after the heat test is used as the evaluation object. The heat test corresponds to an accelerated test assuming long-term storage of the adhesive tape 1.
[0059] The surface resistivity of the exposed surface 11 on the substrate 2 side of the adhesive tape 1, which is a single-sided adhesive tape, is 1×10 11 Ω / sq or more, 1×10 12 Ω / sq or more, 1×10 13 Ω / sq or more, even 1×1014 The upper limit of the surface resistivity is not limited, and may be, for example, 1×10 18 It is less than Ω / sq.
[0060] The shape of the adhesive tape 1 is, for example, a polygon such as a square or a rectangle, or a strip. However, the shape of the adhesive tape 1 is not limited to the above examples. The polygonal adhesive tape 1 can be distributed as a sheet, and the strip-shaped adhesive tape 1 can be distributed as a roll wound around a core. The width of the strip-shaped adhesive tape 1 and the width of the roll formed by winding the strip-shaped adhesive tape 1 can be freely set.
[0061] The pressure-sensitive adhesive tape 1 can exhibit properties derived from the fluororesin contained in the substrate 2. Examples of the properties include heat resistance, moisture resistance, solvent resistance, chemical resistance, flame resistance, and weather resistance.
[0062] The adhesive tape 1 may include materials and / or layers other than the substrate 2 and the adhesive layer 3. An example of an adhesive tape 1 having an additional layer is shown in FIG. 2. The adhesive tape 1 of FIG. 2 further includes a release liner (separator) 4 arranged on the adhesive layer 3 so as to cover the adhesive layer 3. The release liner 4 has a function of protecting the adhesive layer 3 during distribution and storage of the adhesive tape 1. The release liner 4 is usually peeled off when the adhesive tape 1 is used. The surface of the release liner 4 facing the adhesive layer 3 may be subjected to a release treatment. Examples of the release liner 4 include a sheet of polyester resin such as polyethylene terephthalate (PET), and a sheet of polyolefin resin such as polyethylene and polypropylene. The release liner 4 may be the same as a release liner that may be included in a known adhesive tape.
[0063] The adhesive tape 1 can be used in optical devices such as LCD and EL display devices. The adhesive tape 1 may be attached to a member used in the optical device. In the manufacturing process of the optical device, the member may be attached to the optical device with the adhesive tape 1 attached. However, the applications and modes of use of the adhesive tape 1 are not limited to the above examples.
[0064] The pressure-sensitive adhesive tape 1 can be produced, for example, by forming a pressure-sensitive adhesive layer 3 on a substrate 2. The pressure-sensitive adhesive layer 3 can be formed, for example, by forming a coating film of a pressure-sensitive adhesive composition on the substrate 2 and drying and / or curing the coating film. A pressure-sensitive adhesive composition containing white particles can be used to form the pressure-sensitive adhesive layer 3 containing white particles. Known methods can be used for coating the pressure-sensitive adhesive composition and drying and curing the coating film. EXAMPLES
[0065] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.
[0066] In this example, a single-sided adhesive tape was prepared. The method for evaluating the prepared adhesive tape will be described below.
[0067] [Reflectance] The reflectance of the adhesive tape was evaluated as follows. The adhesive tape to be evaluated was cut into a size of 2 cm x 2 cm to prepare a test piece. A stainless steel plate (Nihon Kinzoku, SUS304 BA plate) having a mirror-finished surface was prepared, and the cut test piece was attached to the surface via the adhesive layer. Next, the attached test piece together with the stainless steel plate was set in a spectrophotometer (Nihon Bunko, UV-Visible Spectrophotometer V-560), and the substrate side of the test piece was set as the light irradiation side, and the reflection spectrum of the test piece for light with wavelengths of 200 to 800 nm was obtained. From the obtained reflection spectrum, the reflectance of the test piece for each light with wavelengths of 450 nm, 550 nm, and 630 nm was obtained.
[0068] [Initial adhesive strength] The initial adhesive strength of the adhesive tape (unit: N / 10mm) was measured in accordance with the method for measuring 180° peel adhesive strength of adhesive tape as defined in JIS Z0237:2009. The size of the test piece was 10mm wide and 150mm long. The stainless steel plate (SUS304) as the adherend and the test piece were pressed together by moving a roller of mass 2kg back and forth once in a test atmosphere of 23°C temperature and 50% relative humidity. In order to stabilize the bond between the adherend and the test piece, the test piece was left for at least 30 minutes after the above pressing, and then a 180° peel test was performed in which the test piece was peeled off from the adherend at a peel angle of 180° and a peel speed of 300mm / min. After the start of the test, the measured value of the first 40mm length peeled off was ignored, and the average of the measured values of the subsequent 100mm length peeled off was taken as the initial adhesive strength of the adhesive tape.
[0069] [Adhesive strength after heat test] The adhesive strength after the heating test was evaluated in the same manner as the evaluation of the initial adhesive strength, except that the adhesive tape used for the evaluation was subjected to a heating test in which the tape was left in an atmosphere at a temperature of 60° C. for one week. A hot air dryer was used for the heating test.
[0070] [Follow-up test] The adhesive tape conformability test was carried out as follows. Each test was carried out in an atmosphere with a temperature of 23° C. and a relative humidity of 50%. (Test 1) A test piece with a width of 10 mm was obtained according to the test piece preparation method (item 4.1) described in JIS Z0237:2009. Next, a stainless steel round bar (diameter 8 mm) was prepared, and the test piece was wrapped around the round bar from one end in the length direction. The wrapping was performed in the circumferential direction of the periphery of the round bar while pulling the other end of the test piece by hand. The test piece was cut in the width direction when it was wrapped about one and a half times while aligning both ends in the width direction with the already wrapped test piece, and a light force was applied perpendicular to the surface so that the cut end was in close contact. After that, the test piece was left in an environment of 40°C temperature and 95% RH for 3 hours, and the case where the cut end did not float was designated as A, and the case where the cut end floated was designated as B.
[0071] (Test 2) A test piece 21 having a width of 10 mm and a length of 200 mm was obtained according to the test piece preparation method (item 4.1) described in JIS Z0237:2009. Next, a stainless steel plate 51 (a strip having a length of 200 mm, a width of 15 mm, and a thickness of 2 mm) was prepared, and the test piece 21 was attached to one end 52 in the width direction of the plate 51 so that the long sides were parallel to each other. The attachment was performed so that, when the cross section of the plate 51 and the test piece 21 in the width direction is viewed, the test piece 21 surrounds the one end 52 in a U-shape, and the width W of the part of the test piece 21 that is joined to each of the main surfaces 53A and 53B of the plate 51 is constant over the length L of the test piece 21 (see FIG. 3). When the test piece 21 is attached to the plate 51 without any lifting or wrinkles over the width direction, the width W is 4 mm on each of the main surfaces 53A and 53B of the plate 51. The attachment was performed by attaching the test piece 21 with a width of 4 mm to one main surface 53A of plate 51, and then folding the test piece 21 in the width direction so as to surround the U-shape. When the attached test piece was checked, the case where neither wrinkles nor lifting from the plate at the folded-back part of the U-shape were observed was rated A, the case where wrinkles were observed but no lifting was observed was rated B, and the case where lifting was observed but no wrinkles was observed was rated C.
[0072] [Preparation of substrate] (Production Example 1) PTFE powder (Teflon (registered trademark) PTFE molding powder 7A-J, manufactured by Mitsui DuPont Fluorochemicals) was introduced into a cylindrical mold and preformed under the conditions of a temperature of 23°C, a pressure of 60 MPa, and a pressure application time of 1 hour. Next, the preform was removed from the mold and baked at 375°C for 3 hours to obtain a cylindrical PTFE block with a height of 100 mm and an outer diameter of 50 mm. Next, the obtained PTFE block was cut by a cutting lathe to form a PTFE cut sheet with a thickness of 38 μm. Next, the PTFE cut sheet was subjected to a sodium treatment to improve the bonding with the adhesive layer, and the treated sheet was used as the substrate A. The sodium treatment was performed by immersing the sheet in a treatment liquid (Fluorobonder E, manufactured by Technos).
[0073] (Production Example 2) A fluorosurfactant (MEGAFAC F-142D, manufactured by DIC) was added in an amount of 1 part by mass per 100 parts by mass of PTFE to a dispersion of PTFE particles (PTFE particle concentration 40% by mass, average particle size of PTFE particles 0.2 μm, containing 6 parts by mass of nonionic surfactant per 100 parts by mass of PTFE). Next, a coating film (thickness 20 μm) of the above PTFE dispersion to which a fluorosurfactant was added was formed on the surface of a strip-shaped polyimide substrate (thickness 125 μm). The coating film was formed by immersing the polyimide substrate in the PTFE dispersion and then pulling it up. Next, the entire substrate and coating film were heated to form a cast sheet of PTFE. The heating was performed in two stages: a first heating (100° C., 1 minute) and a second heating (390° C., 1 minute). The first heating removed the dispersion medium contained in the coating film, and the second heating promoted the formation of a cast sheet based on the binding of the PTFE particles contained in the coating film. After repeating the above immersion and subsequent heating two more times, the formed cast sheet (thickness 25 μm) was peeled off from the polyimide substrate. Next, the peeled cast sheet was rolled in the MD direction (longitudinal direction) and further stretched in the TD direction (width direction). The rolling in the MD direction was performed by roll rolling. The rolling ratio (area ratio) was 2.0 times, and the temperature (roll temperature) was 170 ° C. The stretching in the TD direction was performed by a tenter stretching machine. The stretching ratio was 2.0 times, and the temperature (temperature of the stretching atmosphere) was 300 ° C. In this way, a PTFE microporous sheet (thickness 10 μm) having countless pores (average pore diameter 0.1 μm) formed by rolling and stretching was formed, and this was used as the substrate B.
[0074] (Production Example 3) 100 parts by weight of PTFE fine powder (F104, manufactured by Daikin Industries) and 20 parts by weight of n-dodecane (manufactured by Japan Energy) as a molding aid were uniformly mixed. The obtained mixture was compressed by a cylinder and then ram extrusion molded into a sheet. Next, the sheet-like mixture was rolled to a thickness of 0.12 mm through a pair of metal rolls, and the molding aid was dried and removed by heating at 150°C to obtain a sheet molded body. Next, the sheet molded body was stretched in the longitudinal direction (rolling direction) at a stretching temperature of 280°C and a stretching ratio of 10 times to form a PTFE stretched porous sheet (thickness 25 μm, average pore size 1 μm), which was used as the substrate C.
[0075] (Production Example 4) Substrate D, which was a sodium-treated cut PTFE sheet, was obtained in the same manner as in Production Example 1, except that the cutting thickness was changed to 100 μm.
[0076] [Preparation of adhesive composition] (Production Example 5) To a mixture of 100 parts by weight of 2-ethylhexyl acrylate (2-EHA) and 5 parts by weight of acrylic acid (AA), 0.1 parts by weight of 2,2'-azobisisobutyronitrile (AIBN) as a polymerization initiator and 100 parts by weight of toluene as a polymerization solvent were added. 2 After the substitution for 2 hours, polymerization was allowed to proceed at 60° C. for 6 hours to obtain an acrylic copolymer. Next, 1 part by weight of an isocyanate-based crosslinking agent (Coronate-L, manufactured by Nippon Polyurethane) was added to 100 parts by weight of the obtained acrylic copolymer, and the mixture was diluted with toluene to obtain a transparent pressure-sensitive adhesive composition A, which was a solution with a solid content concentration of 40% by weight.
[0077] (Production Example 6) A white adhesive composition B was obtained in the same manner as in Production Example 5, except that a white pigment containing titanium oxide particles at a solid content concentration of 75 wt % (OT-906, manufactured by Resinocolor Industries Co., Ltd.) was added together with the isocyanate-based crosslinking agent. The white pigment was added so that the content in the formed adhesive layer was 0.9 wt %.
[0078] (Examples 7 to 13) White adhesive compositions C to I were obtained in the same manner as in Production Example 6, except that the white pigment was added so that the above content was 3 wt%, 3.6 wt%, 6 wt%, 15 wt%, 30 wt%, 60 wt%, or 90 wt%.
[0079] [Preparation of adhesive sheet] (Sample 1) The adhesive composition B prepared in Production Example 6 was applied to one main surface of the substrate A and heated at a temperature of 100° C. for 3 minutes to obtain an adhesive tape that was a single-sided adhesive tape. A roll coater was used to apply the adhesive composition, and the coating thickness was adjusted so that the adhesive layer after heating had a thickness of 15 μm.
[0080] (Samples 2-13) A single-sided adhesive tape was obtained in the same manner as in Sample 1, except that the substrate and adhesive composition were changed as shown in Table 1 below.
[0081] The configurations and evaluation results of each of the prepared pressure-sensitive adhesive tapes are shown in Tables 1 and 2 below, respectively.
[0082] [Table 1]
[0083] [Table 2]
[0084] The light reflection from sample 13 was poor.
[0085] Sample 12, which had poor results in the conformability test, was evaluated for its adherence to a flat surface as follows.
[0086] For sample 12, a test piece 21 with a width of 10 mm and a length of 200 mm was obtained in the same manner as in the followability test 2. Next, a stainless steel plate (a strip of 200 mm in length, 15 mm in width, and 2 mm in thickness) was prepared, and the test piece 21 was attached to one of the flat main surfaces so that the long sides were parallel to each other. The attachment was performed by bringing one end of the test piece 21 in the length direction into contact with the plate, applying a light force with a hand perpendicular to the surface of the test piece 21, and then sliding the hand while applying a force from the end toward the other end in the length direction of the test piece 21. As a result, no wrinkles were observed in the attached test piece 21. For sample 12, although the attachment to a flat surface could be performed without any problems, it was confirmed that the results were inferior to those of followability tests 1 and 2, which are intended for use in optical devices. [Industrial Applicability]
[0087] The pressure-sensitive adhesive tape of the present invention can be used in optical devices such as LCD and EL display devices, as well as in various other applications. [Explanation of symbols]
[0088] 1 adhesive tape 2 Base material 3 Adhesive layer 4 Release Liner 11 Exposed surface
Claims
1. A substrate containing a fluororesin and a pressure-sensitive adhesive layer disposed on the substrate, The reflectance of at least one surface for light having a wavelength of 550 nm is 50% or more; The thickness of the substrate is 90 μm or less. Adhesive tape.
2. The adhesive tape according to claim 1 , wherein the substrate is a cut sheet.
3. The adhesive tape according to claim 1 , wherein the adhesive layer comprises white particles.
4. The pressure-sensitive adhesive tape according to claim 3 , wherein the content of the white particles in the pressure-sensitive adhesive layer is 3.5% by weight or more and 30% by weight or less.
5. The pressure-sensitive adhesive tape according to claim 3 , comprising only the fluororesin contained in the substrate and the white particles contained in the pressure-sensitive adhesive layer as materials that diffuse and / or reflect light.
6. The pressure-sensitive adhesive tape according to claim 1 , wherein the substrate is an oriented sheet.
7. The pressure-sensitive adhesive tape according to claim 1 , wherein the substrate has a single-layer structure.
8. The pressure-sensitive adhesive tape according to claim 1 , wherein the fluororesin is polytetrafluoroethylene (PTFE).
9. The adhesive tape is a single-sided adhesive tape, The pressure-sensitive adhesive tape according to claim 1 , wherein the reflectance of the surface on the substrate side to light having a wavelength of 550 nm is 50% or more.
10. The pressure-sensitive adhesive tape according to claim 1 , wherein the reflectance of the at least one surface to light with a wavelength of 450 nm is 50% or more.
11. 2. The pressure-sensitive adhesive tape according to claim 1, which has a 180° peel adhesion of 0.6 N / 10 mm or more.
Citation Information
Patent Citations
Light shielding reflective tape and LCD module
JP2009175328A
Cited By
Method for forming molten glass, forming apparatus, and method for producing glass product
US12291475B2