Aqueous polyurethane dispersion for primer, primer layer, and layered product
A polyurethane aqueous dispersion with specific components addresses the adhesion and resistance issues of conventional primer layers on amorphous resins, providing improved adhesion and resistance to hot water, chemicals, and humidity.
Patent Information
- Application Number
- JP2023047158
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-23
AI Technical Summary
Conventional polyurethane resin dispersions used for primer layers exhibit poor adhesion, hot water resistance, chemical resistance, and heat and humidity resistance, particularly on amorphous resin substrates, leading to issues such as reduced adhesion under high humidity and damage from organic solvents.
A polyurethane aqueous dispersion comprising specific components like aromatic isocyanate, alkylene oxide adduct of bisphenol A, linear aliphatic polyol, diol compound with a carboxyl group, and polyol compound X, which form a primer layer with improved adhesion and resistance to hot water, chemicals, and heat and humidity.
The dispersion forms a primer layer with excellent adhesion to amorphous resin substrates, demonstrating superior hot water resistance, chemical resistance, and heat and humidity resistance, enhancing the performance of optical films and other amorphous resin materials.
Smart Images

Figure 2024136153000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous polyurethane dispersion for a primer, a primer layer, and a laminate including the primer layer. [Background technology]
[0002] A primer layer may be provided on the surface of the optical film, which can enhance the adhesion between the optical film and other substrates and can also modify the surface of the optical film. For example, the scratch resistance and mechanical strength of the optical film can be improved by providing a primer layer on the surface of the optical film.
[0003] Coating agents for forming a primer layer have been widely studied, and among them, compositions containing resin emulsions are preferably used.For example, Patent Document 1 discloses a technique for forming a primer layer by using an aqueous polyurethane resin dispersion composition containing polyurethane obtained by reacting a polycarbonate polyol having an alicyclic structure, a polyisocyanate, an acidic group-containing polyol, and a hydroxyl group-containing polyamine. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-050014 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the primer layer formed using the conventional polyurethane resin dispersion did not necessarily satisfy all the performances of adhesion to the substrate (especially the substrate formed of the amorphous resin), hot water resistance, chemical resistance, and moist heat resistance. For this reason, for example, a problem of a decrease in adhesive strength due to the intrusion of moisture under high humidity may occur, and when a coating composition containing an organic solvent is applied onto the primer layer, there is also a problem that the primer layer is destroyed by the organic solvent contained in the coating composition. From this viewpoint, a coating agent capable of forming a primer layer excellent in all performances of adhesion, hot water resistance, chemical resistance, and moist heat resistance is required.
[0006] The present invention has been made in view of the above, and has an object to provide an aqueous polyurethane dispersion for a primer, which is capable of forming a primer layer having excellent adhesion to an amorphous resin substrate and also having excellent hot water resistance, chemical resistance, and moist heat resistance, and a primer layer and a laminate. [Means for solving the problem]
[0007] Means for Solving the Problems The present inventors have conducted intensive research to achieve the above object, and as a result have found that the above object can be achieved by using a composition containing a specific isocyanate compound and a polyol compound, thereby completing the present invention.
[0008] That is, the present invention includes, for example, the subject matter described in the following sections. Item 1 A polyurethane water dispersion for a primer, which is used to form a primer layer on an amorphous resin substrate, comprising: An aromatic isocyanate; an alkylene oxide adduct of bisphenol A; A linear aliphatic polyol having 3 to 5 carbon atoms; A diol compound having a carboxyl group, A polyol compound X having a number average molecular weight of 500 to 3000; A polyurethane aqueous dispersion for a primer, comprising a polymer of a composition comprising: Section 2 Item 2. The aqueous polyurethane dispersion for a primer according to item 1, wherein the polyol compound X is at least one selected from the group consisting of polyether polyols, polyester polyols, and polycarbonate polyols. Section 3 Item 3. The aqueous polyurethane dispersion for primers according to item 1 or 2, wherein the diol compound having a carboxyl group contains dimethylolpropionic acid. Section 4 Item 4. The aqueous polyurethane dispersion for a primer according to any one of items 1 to 3, wherein the amorphous resin substrate is an optical film. Section 5 Item 5. A primer layer comprising a dried product of the aqueous polyurethane dispersion for primers according to any one of items 1 to 4. Section 6 A laminate comprising the amorphous resin substrate and the primer layer according to claim 5. Effect of the Invention
[0009] The aqueous polyurethane dispersion for a primer of the present invention can form a primer layer having excellent adhesion to an amorphous resin substrate, and can also form a primer layer having excellent resistance to hot water, chemicals, and moist heat. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expressions "containing" and "comprise" include the concepts of "containing", "comprises", "consists essentially of" and "consists only of".
[0011] The aqueous polyurethane dispersion for a primer of the present invention is used for forming a primer layer on an amorphous resin substrate, An aromatic isocyanate; an alkylene oxide adduct of bisphenol A; A linear aliphatic polyol having 3 to 5 carbon atoms; A diol compound having a carboxyl group, A polyol compound X having a number average molecular weight of 500 to 3000; The polymer comprises a composition comprising:
[0012] Hereinafter, the aqueous polyurethane dispersion for use as a primer of the present invention will be referred to simply as "aqueous polyurethane dispersion."
[0013] Since the polyurethane aqueous dispersion contains a polymer of the above composition, it is possible to form a primer layer that has excellent adhesion to amorphous resin substrates, and also has excellent resistance to hot water, chemicals, and moist heat.
[0014] (Aromatic isocyanates) The aromatic isocyanate is an isocyanate compound having at least one aromatic group and at least one isocyanate group in the molecule. The aromatic isocyanate preferably has two or more isocyanate groups.
[0015] The aromatic isocyanate may be, for example, a wide variety of known aromatic isocyanates for forming urethane resins. Examples of the aromatic isocyanate include one or more of 2,4-tolylene diisocyanate (TDI, also called 2,4-toluene diisocyanate), 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate, xylylene diisocyanate, 1,3-phenylene diisocyanate, and 1,4-phenylene diisocyanate.
[0016] The aromatic isocyanate may be a mixture of two or more isomers. For example, when the aromatic isocyanate is 2,4-tolylene diisocyanate, the aromatic isocyanate may contain its isomer, 2,6-tolylene diisocyanate.
[0017] The aromatic isocyanate can be produced by a known method, or can be obtained from a commercial product.
[0018] (Alkylene oxide adduct of bisphenol A) The alkylene oxide adduct of bisphenol A can be a compound having a structure in which two hydroxyl groups of bisphenol A are replaced with alkylene oxide moieties. That is, the alkylene oxide adduct of bisphenol A is a compound having at least two alkylene oxide moieties.
[0019] In the alkylene oxide adduct of bisphenol A, the alkylene oxide moiety preferably has two or more alkylene oxide units, and preferably has, for example, four or less.
[0020] In the alkylene oxide adduct of bisphenol A, examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, etc., with ethylene oxide and propylene oxide being preferred, and ethylene oxide being more preferred. That is, the alkylene oxide adduct of bisphenol A is preferably an ethylene oxide adduct or propylene oxide adduct of bisphenol A, and particularly preferably an ethylene oxide adduct of bisphenol A.
[0021] The weight average molecular weight of the alkylene oxide adduct of bisphenol A can be, for example, 100 to 1000. The weight average molecular weight of the alkylene oxide adduct of bisphenol A is a value measured by a GPC method (gel permeation chromatography method) and calculated using a calibration curve of standard polystyrene. The GPC conditions are, for example, column: "TSKgel GMHHR-H" manufactured by Tosoh Corporation, solvent: THF, flow rate: 0.6 mL / min, and measurement temperature: 40°C.
[0022] The hydroxyl value of the alkylene oxide adduct of bisphenol A is not particularly limited and can be, for example, 50 to 400 mgKOH / g, preferably 80 to 350 mgKOH / g, and more preferably 100 to 300 mgKOH / g.
[0023] The hydroxyl value of the alkylene oxide adduct of bisphenol A is a value measured in accordance with Method A of JIS K1557-1:2007, and is the number of milligrams of potassium hydroxide (KOH) that reacts with acetic acid to acetylate the hydroxyl groups (OH groups) in 1 g of polyol.
[0024] The alkylene oxide adduct of bisphenol A can be produced by a known method, or can be obtained from a commercial product, etc. An example of a commercial product of the alkylene oxide adduct of bisphenol A is Newpol (registered trademark) manufactured by Sanyo Chemical Industries, Ltd., and specific examples thereof include the Newpol BPE series and the Newpol BP series.
[0025] The alkylene oxide adduct of bisphenol A contained in the composition may be of one type or of two or more types.
[0026] (Straight-chain aliphatic polyol having 3 to 5 carbon atoms) The linear aliphatic polyol having 3 to 5 carbon atoms (hereinafter simply referred to as "linear aliphatic polyol") may be a compound having a linear alkyl group having 3 to 5 carbon atoms in the molecule and having two or more hydroxyl groups. The linear aliphatic polyol preferably has two hydroxyl groups.
[0027] The molecular weight (molar mass) of the linear aliphatic polyol is preferably less than 500, more preferably 400 or less, further preferably 300 or less, and particularly preferably 200 or less.
[0028] Examples of the linear aliphatic polyol include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, and 1,5-pentanediol.
[0029] The linear aliphatic polyol can be produced by a known method, or can be obtained from a commercial product.
[0030] The linear aliphatic polyol contained in the composition may be of only one type, or of two or more types.
[0031] (Diol compound having a carboxyl group) The diol compound having a carboxyl group is a compound having at least one carboxyl group and two hydroxyl groups in the molecule, and is preferably a compound having one carboxyl group and two hydroxyl groups.
[0032] Examples of the diol compound having a carboxyl group include dimethylol acetic acid, dimethylol propionic acid, and dimethylol butanoic acid. Among them, the diol compound having a carboxyl group preferably contains dimethylol propionic acid. In this case, the polyurethane resin is easily produced, so that the polyurethane water dispersion having good dispersion stability is easily produced, and a primer layer having excellent adhesion, warm water resistance, chemical resistance, and moist heat resistance is easily formed. The diol compound having a carboxyl group may be composed of only dimethylol propionic acid.
[0033] The diol compound having a carboxyl group contained in the composition may be of only one kind, or of two or more kinds.
[0034] (Polyol compound X having a number average molecular weight of 500 to 3000) The type of polyol compound X (hereinafter simply referred to as "compound X") having a number average molecular weight of 500 to 3000 (not less than 500 and not more than 3000) is not particularly limited, and a wide variety of polyols can be mentioned.
[0035] The compound X is preferably one or more selected from the group consisting of polyether polyol, polyester polyol, and polycarbonate polyol. In this case, the primer layer obtained from the polyurethane water dispersion has excellent adhesion to the amorphous resin substrate, and is particularly likely to have improved wet heat resistance. Among them, the compound X is more preferably one or more selected from the group consisting of polyether polyol and polycarbonate polyol, and is particularly preferably polyether polyol.
[0036] The type of polyether polyol is not particularly limited as long as the number average molecular weight is 500 to 3000. For example, examples of polyether polyols include polyethylene glycol, and other examples include polyhydric alcohols or derivatives thereof such as ethylene glycol, propylene glycol, propanediol, butanediol, pentanediol, 3-methyl-1,5-pentanediol, hexanediol, neopentyl glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, 1,4-cyclohexanedimethanol, bisphenol A, bisphenol F, bisphenol S, hydrogenated bisphenol A, dibromobisphenol A, 1,4-cyclohexanedimethanol, dihydroxyethyl terephthalate, hydroquinone dihydroxyethyl ether, trimethylolpropane, glycerin, and pentaerythritol; oxyalkylene derivatives such as ethylene oxide, propylene oxide, and butylene oxide; and the like.
[0037] The polyether polyol is preferably a polyethylene glycol having a number average molecular weight of 500 to 3000. In this case, the primer layer obtained from the polyurethane water dispersion has excellent adhesion to amorphous resin substrates, and further, the hot water resistance, chemical resistance, and moist heat resistance are also likely to be particularly improved.
[0038] The type of polyester polyol is not particularly limited as long as the number average molecular weight is 500 to 3000. For example, a condensation reaction product of a polyvalent carboxylic acid and a polyhydric alcohol can be mentioned.
[0039] Examples of polybasic carboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, schuberic acid, azelaic acid, sebacic acid, 1,12-dodecanedicarboxylic acid, phthalic anhydride, isophthalic acid, terephthalic acid, dimer acid, halogenated phthalic anhydride, tetrahydrophthalic acid, tetrahydrophthalic anhydride, hexahydrophthalic acid, hexahydrophthalic anhydride, hexahydroterephthalic acid, hexahydroisophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid anhydride, 4,4'-biphenyldicarboxylic acid, and dibasic acids such as dialkyl esters thereof, or the corresponding acid anhydrides thereof, and polybasic acids such as pyromellitic acid. These polybasic carboxylic acids can be used alone or in combination of two or more kinds. Examples of the α,β-unsaturated dibasic acid include maleic acid, maleic anhydride, fumaric acid, itaconic acid, and itaconic anhydride.
[0040] Examples of polyhydric alcohols include dihydric alcohols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 2-methyl-2-butyl-1,3-propanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,8-octanediol, 1,9-nonanediol, 2,4-diethyl-1,5-pentanediol, 2-ethyl-2-butyl-1,3-propanediol, diethylene glycol, dipropylene glycol, and triethylene glycol; glycerin, trimethylolpropane, pentaerythritol, and sorbitol.
[0041] The type of polycarbonate polyol is not particularly limited as long as the number average molecular weight is 500 to 3000. For example, the polycarbonate polyol may be a polycarbonate polyol obtained by reacting a polyol compound with a carbonate compound. For example, the polyol compound may be an aliphatic polyol or an alicyclic polyol. For example, the carbonate compound may be a carbonate derivative such as a carbonate ester or phosgene.
[0042] The number average molecular weight of compound X is preferably 530 or more, more preferably 550 or more, even more preferably 580 or more, and particularly preferably 600 or more. The number average molecular weight of compound X is preferably 2800 or less, more preferably 2500 or less, even more preferably 2300 or less, and particularly preferably 2000 or less.
[0043] The number average molecular weight (Mn) of compound X is a value measured by GPC (gel permeation chromatography) and calculated using a calibration curve of standard polystyrene. The GPC conditions are, for example, column: "TSKgel GMHHR-H" manufactured by Tosoh Corporation, solvent: THF, flow rate: 0.6 mL / min, and measurement temperature: 40°C.
[0044] The hydroxyl value of compound X is not particularly limited and can be, for example, 10 to 300 mgKOH / g, preferably 30 to 250 mgKOH / g, and more preferably 50 to 200 mgKOH / g.
[0045] The hydroxyl value of compound X is a value measured in accordance with Method A of JIS K1557-1:2007, and is the number of milligrams of potassium hydroxide (KOH) that reacts with acetic acid to acetylate the hydroxyl groups (OH groups) in 1 g of polyol.
[0046] Compound X can be produced by a known method, or can be obtained from a commercial source.
[0047] The compound X contained in the composition may be one type or two or more types.
[0048] (composition) As described above, the polyurethane water dispersion contains a polymer of a composition including an aromatic isocyanate, an alkylene oxide adduct of bisphenol A, a linear aliphatic polyol, a diol compound having a carboxyl group, and a compound X. Such a composition can contain other components as long as the effect of the present invention is not impaired. For example, the composition can contain an aromatic isocyanate such as an aliphatic isocyanate, and can also contain other polyols as long as the effect of the present invention is not impaired.
[0049] The composition may contain a solvent in addition to the above components. The solvent may be, for example, a wide variety of organic solvents not having an active hydrogen group that are generally used in polyurethane synthesis, such as dioxane, methyl ethyl ketone, dimethylformamide, tetrahydrofuran, N-methyl-2-pyrrolidone, toluene, and propylene glycol monomethyl ether acetate.
[0050] When the composition contains a solvent, the content thereof is not particularly limited, and can be, for example, the content of a solvent used in polymerizing a known polyurethane resin.
[0051] In the composition, the content of each component is not particularly limited.For example, when the content of the alkylene oxide adduct of bisphenol A in the composition is D moles and the content of linear aliphatic polyol is G moles, the value of the molar ratio D / G is preferably 0.5 or more, more preferably 0.6 or more, even more preferably 1 or more, even more preferably 2 or more, and particularly preferably 3 or more, and is preferably 15 or less, more preferably 12 or less, even more preferably 10 or less, even more preferably 8 or less, and particularly preferably 7 or less.
[0052] In addition, in the composition, when the content of the linear aliphatic polyol is G moles and the content of the diol compound having a carboxyl group is F moles, the molar ratio G / F is preferably 0.1 or more, more preferably 0.2 or more, even more preferably 0.25 or more, even more preferably 0.3 or more, and particularly preferably 0.4 or more, and is preferably 2.5 or less, more preferably 2 or less, even more preferably 1.5 or less, and particularly preferably 1.2 or less.
[0053] Furthermore, in the composition, when the content of the alkylene oxide adduct of bisphenol A is D moles and the content of the diol compound having a carboxyl group is F moles, the molar ratio F / D is preferably 0.1 or more, more preferably 0.2 or more, even more preferably 0.25 or more, particularly preferably 0.3 or more, and is preferably 2 or less, more preferably 1.5 or less, even more preferably 1.3 or less, and particularly preferably 1 or less. When the value of F / D is within these ranges, the dispersion stability of the polyurethane water dispersion is likely to be improved.
[0054] In the composition, the content ratio of compound X is not particularly limited. For example, the content ratio of compound X is preferably 0.1 to 30 mol%, more preferably 1 to 20 mol%, further preferably 2 to 15 mol%, and particularly preferably 3 to 10 mol% based on the total amount of the alkylene oxide adduct of bisphenol A, the linear aliphatic polyol, the diol compound having a carboxyl group, and compound X. In these cases, the adhesion of the primer layer to the amorphous resin substrate is likely to be increased.
[0055] Furthermore, in the composition, the content of aromatic isocyanate is not particularly limited. For example, when the content of aromatic isocyanate in the composition is A moles, and the total amount of the alkylene oxide adduct of bisphenol A, the linear aliphatic polyol, the diol compound having a carboxyl group, and the compound X is B moles, the molar ratio A / B (i.e., NCO / OH) can be in the range of 0.5 to 2, preferably 0.8 to 1.5, and more preferably 0.9 to 1.3.
[0056] (Polyurethane water dispersion) The polyurethane water dispersion contains a polymer of the composition. In other words, the polyurethane water dispersion is obtained by polymerizing a raw material containing the composition. Therefore, the polyurethane water dispersion can be produced by using the composition.
[0057] The polyurethane water dispersion can be prepared, for example, by reacting the composition at a predetermined temperature to produce a polyurethane resin, and then adding water and, if necessary, a neutralizing agent. An example of a method for preparing a polyurethane water dispersion using the composition will be described below.
[0058] First, a predetermined amount of the solvent is added to a raw material containing a predetermined amount of an alkylene oxide adduct of bisphenol A, a linear aliphatic polyol, a diol compound having a carboxyl group, and compound X, and then an aromatic isocyanate is added to obtain a predetermined NCO / OH value to prepare a composition. This composition is polymerized at a predetermined temperature to produce a polyurethane resin, and then water and, if necessary, a neutralizing agent are added to emulsify the resin to obtain an emulsion. The solvent is removed from the emulsion by an appropriate method to obtain a polyurethane water dispersion.
[0059] In the production of polyurethane water dispersion, a chain extender can be used to increase the molecular weight of polyurethane. The type of chain extender is not particularly limited, and a wide variety of known chain extenders can be used, including compounds having functional groups reactive to polyisocyanate compounds, specifically amine compounds, diol compounds, water, etc. The chain extender can be added, for example, simultaneously with the preparation of the above-mentioned emulsion or after the preparation of the emulsion, but is not limited thereto.
[0060] The polymerization reaction temperature is not particularly limited and can be, for example, the same temperature as that used in the synthesis of known polyurethane resins, specifically, 30 to 150°C, and preferably 40 to 100°C.
[0061] Examples of the neutralizing agent include non-volatile bases such as sodium hydroxide and potassium hydroxide, tertiary amines such as trimethylamine, triethylamine, dimethylethanolamine, methyldiethanolamine and triethanolamine, and volatile bases such as ammonia, etc. Note that the neutralization can be carried out before, during, or after the polymerization reaction.
[0062] The polyurethane water dispersion is a dispersion in which the polymer of the composition is dispersed in water, that is, a dispersion in which the polyurethane resin is dispersed in water. The solid content concentration of the polyurethane water dispersion is not particularly limited, and can be appropriately set according to the type of primer layer to be formed. For example, the solid content concentration of the polyurethane water dispersion is 1 to 50 mass%, preferably 5 to 30 mass%.
[0063] Since the polyurethane water dispersion is a polymer of the above-mentioned composition, the polyurethane resin contained in the polyurethane water dispersion is a polymer having a constituent unit derived from an aromatic isocyanate, a constituent unit derived from an alkylene oxide adduct of bisphenol A, a constituent unit derived from a linear aliphatic polyol, a constituent unit derived from a diol compound having a carboxyl group, and a constituent unit derived from compound X.
[0064] In the polyurethane water dispersion, the average particle size of the polymer (polyurethane resin) is not particularly limited and is, for example, 0.01 to 50 μm, preferably 0.015 to 10 μm, and more preferably 0.02 to 5 μm. The average particle size means the 50% cumulative value measured by dynamic light scattering.
[0065] The polyurethane water dispersion is excellent in dispersion stability, and can form a primer layer having excellent adhesion to an amorphous resin substrate, and can form a primer layer having excellent resistance to hot water, chemicals, and moist heat, and is used for a primer. Therefore, the polyurethane water dispersion is used for forming a primer layer on an amorphous resin substrate.
[0066] The amorphous resin substrate may be a substrate formed from an amorphous resin. For example, the amorphous resin substrate may be a substrate formed from an acrylic resin, a substrate formed from a polycarbonate resin, a substrate formed from a polyamide resin, a substrate formed from a polystyrene resin, a substrate formed from an amorphous olefin resin, a substrate formed from a polyether resin, etc. Among them, the amorphous resin substrate is preferably a substrate formed from an acrylic resin or a substrate formed from a polycarbonate resin. In this case, the primer layer obtained from the polyurethane water dispersion has excellent adhesion.
[0067] The amorphous resin substrate may be, for example, a film, and is preferably an optical film. The thickness and shape of the optical film are not particularly limited, and any known optical film may be widely used.
[0068] (Primer layer and laminate) A primer layer can be formed using the polyurethane water dispersion. For example, the polyurethane water dispersion is applied to the above-mentioned amorphous resin substrate to form a coating film, and the coating film is dried to form the primer layer. That is, the primer layer contains a dried product of the polyurethane water dispersion. The dried product of the polyurethane water dispersion is, for example, a product in which volatile components such as water in the polyurethane water dispersion have been dried.
[0069] The thickness of the primer layer is not particularly limited, and may be, for example, the same thickness as that of a known primer layer.
[0070] The method for forming a primer layer from the polyurethane water dispersion is not particularly limited, and any of the known methods for forming a primer layer can be widely used.
[0071] The primer layer obtained from the polyurethane water dispersion not only has excellent adhesion to the amorphous resin substrate such as the optical film, but also can modify the surface of the optical film to have higher performance. For example, the primer layer obtained from the polyurethane water dispersion can improve the hot water resistance, chemical resistance, and moist heat resistance of the amorphous resin substrate (optical film, etc.).
[0072] Therefore, the polyurethane water dispersion is suitable as a coating agent (or a primer composition) for forming a primer layer, and can be particularly suitable for use as a coating agent for amorphous resin substrates (or a primer composition for amorphous resin substrates). Such a coating agent may contain known additives such as an ultraviolet absorber, an antioxidant, a discoloration inhibitor, and a pH adjuster, as necessary, and the coating agent may consist of the polyurethane water dispersion alone. The coating agent may contain 50% by mass or more of the polyurethane water dispersion, preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.
[0073] A laminate containing a primer layer made of a polyurethane water dispersion and the amorphous resin substrate can be widely used in various optical applications, and is particularly suitable as a component for display devices such as liquid crystal displays and touch panels.
[0074] In specifying the invention included in the present disclosure, the configurations (properties, structures, functions, etc.) described in each embodiment of the present disclosure may be combined in any manner. In other words, the present disclosure includes all subject matter consisting of all combinations of the configurations that can be combined as described in this specification. EXAMPLES
[0075] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples.
[0076] (raw materials) Appropriate raw materials were selected from the raw materials shown below to produce the polyurethane water dispersions of the respective Examples.
[0077] <Aromatic isocyanate (A)> A mixture consisting of 80% by mass of 2,4-tolylene diisocyanate and 20% by mass of 2,6-tolylene diisocyanate (Coronate T-80) ·4,4'-Diphenylmethane diisocyanate (MDI)
[0078] <Alkylene oxide adduct of bisphenol A (D)> Bisphenol A with 4 moles of ethylene oxide (Sanyo Chemical Industries, Ltd. "Newpol BPE-40", weight average molecular weight 400, hydroxyl value 281 mgKOH / g) Bisphenol A with 2 moles of ethylene oxide (Sanyo Chemical Industries, Ltd. "Newpol BPE-20NK") Bisphenol A propylene oxide 2 mole adduct (ADEKA "BPX-11")
[0079] <Straight-chain aliphatic polyol (G)> 1,4-Butanediol (Mitsubishi Chemical Corporation) 1,3-Propanediol 1,5-Pentanediol
[0080] <Diol compound having a carboxyl group (F)> Dimethylolpropionic Acid
[0081] <Compound X> Polyethylene glycol 1 (number average molecular weight 600, Sanyo Chemical Industries, Ltd. "PEG-600") Polyethylene glycol 2 (number average molecular weight 1000, Sanyo Chemical Industries, Ltd. "PEG-1000") Polyethylene glycol 3 (number average molecular weight 2000, Sanyo Chemical Industries, Ltd. "PEG-2000") Polyester polyol (number average molecular weight 2000, Kuraray "P-2010") Polycarbonate polyol (number average molecular weight 1000, Asahi Kasei Corporation "T-5651")
[0082] Example 1 A polyurethane water dispersion was produced by selecting each raw material at the blending ratio (molar ratio) shown in Example 1 of the blending table in Table 1. The blending conditions column in Table 1 shows the molar ratio of each raw material with aromatic isocyanate (A) as the standard (1 mole). First, a 4-mol ethylene oxide adduct of bisphenol A, 1,4-butanediol, dimethylolpropionic acid, polyethylene glycol 1 as compound X, and methyl ethyl ketone were added to a four-neck flask equipped with a stirrer, a reflux condenser, a thermometer, and a nitrogen blowing tube, and a raw material was obtained by thoroughly stirring and dissolving. To this raw material, Coronate T-80 was added to prepare a composition, and the polymerization reaction was carried out at 75°C until the NCO content reached 1.20% by mass. Thereafter, triethylamine as a neutralizing agent and water were added and emulsified to obtain an emulsion, and the emulsion was heated under reduced pressure to distill off the solvent methyl ethyl ketone. As a result, a polyurethane water dispersion with a solid content of 25% by mass was obtained.
[0083] (Examples 2 to 17) A polyurethane water dispersion was obtained in the same manner as in Example 1, except that the raw materials and blending amounts were changed as shown in Table 1.
[0084] (Comparative Examples 1 to 4) A polyurethane water dispersion was obtained in the same manner as in Example 1, except that the raw materials and blending amounts were changed as shown in Table 1.
[0085] (Reference example 1) The same polyurethane water dispersion as in Example 1 was prepared.
[0086] (Evaluation method) <Adhesion to substrate> As the amorphous resin substrate, either a polymethylmethacrylate film (PMMA film; Technoloy S000#75) or a polycarbonate (PC film; "Elmec" manufactured by Kaneka Corporation) was used. After the substrate was degreased with isopropyl alcohol, a polyurethane water dispersion was applied to the substrate with a bar coater so that the dry film thickness was 10 μm to form a coating film. This coating film was dried at 80°C for 10 minutes, then dried at 120°C for 10 minutes, and left overnight to form a primer layer on the substrate. A 100-square grid peel test (JIS-K5400) was performed on this primer layer, and the number of remaining squares was counted and evaluated according to the following criteria. [Judgment criteria] A: No peeling at all, extremely excellent adhesion to the substrate. B: The remaining mass was 80% or more, and the adhesion to the substrate was excellent. C: The remaining mass was less than 80%, and the adhesion to the substrate was poor.
[0087] <Formulation stability> A sample was prepared by adding 6 parts by mass of a carbodiimide crosslinking agent (product name: Carbodilite V-02-L2, manufactured by Nisshinbo Chemical Co., Ltd.) to 50 parts by mass of a polyurethane water dispersion. The sample was stored at 20°C for one week, and the viscosity was measured before and after storage, and the blend stability was evaluated based on the change in viscosity. The viscosity was measured at 20°C using a single cylindrical rotational viscometer (JIS Z-8803:2011), and evaluated according to the following criteria. [Judgment criteria] A: The viscosity change was less than 100 mPa·s, and the compounding stability (dispersion stability) was excellent. B: The viscosity change was 100 mPa·s or more, or gelation occurred after storage, and the compounding stability (dispersion stability) was poor.
[0088] <Hot water resistance> The polyurethane water dispersion was applied onto a substrate so as to have a dry thickness of approximately 200 to 300 μm, and then dried at 40° C. for 15 hours, then at 80° C. for 6 hours, and then at 120° C. for 30 minutes to produce a coating. A Teflon (registered trademark)-coated metal plate was used as the substrate. A 2×2 cm test piece was cut from the coating formed on the substrate, and the test piece was immersed in warm water at 40° C. for 24 hours. The mass of the test piece before immersion (W0) (g) and the mass of the test piece after immersion (Wn) (g) were measured, and the mass was calculated using the following formula (1): Mass increase rate (%) ={(Wn(g)-W0(g)) / W0(g)}×100 (1) The mass increase rate (%) of the test piece was calculated based on the above and evaluated according to the following criteria. [Judgment criteria] A: The mass increase rate was 50% or less, and the warm water resistance was extremely excellent. B: The mass increase rate was more than 50% and not more than 200%, and the hot water resistance was excellent. C: The mass increase rate exceeded 200%, and the warm water resistance was poor.
[0089] <Chemical resistance> The polyurethane water dispersion was applied to a substrate so that the dry thickness was about 200 to 300 μm, and the substrate was dried at 40° C. for 15 hours, then dried at 80° C. for 6 hours, and further dried at 120° C. for 30 minutes to prepare a coating. A metal plate processed with Teflon (registered trademark) was used as the substrate. A test piece of 2×2 cm was cut from the coating formed on the substrate, and the test piece was immersed in a 1:1 (mass ratio) mixed solvent of ethyl acetate / toluene or isopropyl alcohol at 40° C. for 24 hours. The mass (W0) (g) of the test piece before immersion and the mass (Wn) (g) of the test piece after immersion were measured, and the mass increase rate (%) of the test piece was calculated based on the above formula (1), and the evaluation was performed according to the following criteria. [Judgment criteria] A: The mass increase rate was 50% or less, and the chemical resistance was extremely excellent. B: The mass increase rate was more than 50% and not more than 200%, and the chemical resistance was excellent. C: The mass increase rate exceeded 200%, and the chemical resistance was poor.
[0090] <Moisture and heat resistance> As the amorphous resin substrate, either the PMMA film or the PC film described above was used. After the substrate was degreased with isopropyl alcohol, a polyurethane water dispersion was applied to the substrate with a bar coater so that the dry film thickness was 10 μm to form a coating film. This coating film was dried at 80° C. for 10 minutes, then dried at 120° C. for 10 minutes, and left overnight to form a primer layer on the substrate. This primer layer was stored for one week in an environment of a temperature of 85° C. and a humidity of 85% RH, and then a 100-square grid peel test (JIS-K5400) was performed to count the number of remaining squares, and evaluation was performed according to the following criteria. [Judgment criteria] A: No peeling at all, extremely excellent resistance to moist heat. B: The remaining mass was 80% or more, and the moist heat resistance was excellent. C: The remaining mass was less than 80%, and the moist heat resistance was poor.
[0091] Table 1 shows the compounding conditions and evaluation results in the production of polyurethane water dispersions of each Example and Comparative Example. In the compounding conditions in Table 1, a blank means that the raw material was not used. In Table 1, "type of substrate" means the type of amorphous substrate used in the evaluation of adhesion to the substrate, hot water resistance, chemical resistance, and moist heat resistance. In Table 1, 4EO adduct, 2EO adduct, and 2PO adduct mean 4 mol ethylene oxide adduct of bisphenol A, 2 mol ethylene oxide adduct of bisphenol A, and 2 mol propylene oxide adduct of bisphenol A, respectively.
[0092] In Table 1, "(D) / (G)", "(G) / (F)", and "(F) / (D)" all mean molar ratios, and are specifically as follows: (D) / (G): Alkylene oxide adduct of bisphenol A / linear aliphatic polyol (G) / (F): Linear aliphatic polyol / diol compound having a carboxyl group (F) / (D): Diol compound having a carboxyl group / alkylene oxide adduct of bisphenol A
[0093] The "NCO / OH" in Table 1 is the ratio of the number of moles of aromatic isocyanate to the total number of moles of the alkylene oxide adduct of bisphenol A, the linear aliphatic polyol, the diol compound having a carboxyl group, and the compound X (i.e., the value of A / B described above).
[0094] In Reference Example 1 of Table 1, a PET (polyethylene terephthalate) film was used as the substrate instead of a PMMA film or PC film, and the results of evaluations of adhesion to the substrate, hot water resistance, chemical resistance, and moist heat resistance are shown.
[0095] It is clear from Table 1 that the polyurethane water dispersion obtained from the composition containing an aromatic isocyanate, an alkylene oxide adduct of bisphenol A, a linear aliphatic polyol having 3 to 5 carbon atoms, a diol compound having a carboxyl group, and polyol compound X can form a primer layer that has excellent adhesion to an amorphous resin substrate (amorphous optical film) and also has excellent hot water resistance, chemical resistance, and moist heat resistance.
[0096] [Table 1]
Claims
1. A polyurethane water dispersion for a primer, which is used to form a primer layer on an amorphous resin substrate, comprising: An aromatic isocyanate; an alkylene oxide adduct of bisphenol A; a linear aliphatic polyol having 3 to 5 carbon atoms; A diol compound having a carboxyl group, A polyol compound X having a number average molecular weight of 500 to 3,000; A polyurethane aqueous dispersion for a primer, comprising a polymer of a composition comprising:
2. 2. The aqueous polyurethane dispersion for a primer according to claim 1, wherein the polyol compound X is at least one selected from the group consisting of polyether polyols, polyester polyols, and polycarbonate polyols.
3. The aqueous polyurethane dispersion for a primer according to claim 1 , wherein the diol compound having a carboxyl group comprises dimethylolpropionic acid.
4. The aqueous polyurethane dispersion for a primer according to claim 1 , wherein the amorphous resin substrate is an optical film.
5. A primer layer comprising a dried product of the aqueous polyurethane dispersion for primers according to any one of claims 1 to 4.
6. A laminate comprising the amorphous resin substrate and the primer layer according to claim 5 .
Citation Information
Patent Citations
Primer composition and laminate
JP2013227520A
Aqueous resin composition, laminate produced using same, and image display device
WO2015019899A1
Primer composition
WO2021065325A1
Aqueous polyurethane resin dispersion composition
JP2022050014A
WO2015208284A1