Resin composition, kit, pellet, molded article, and method for manufacturing molded article
A resin composition with specific polyamide resin, perylene and green pigments, and a low-melting-point mold release agent addresses dye migration and whitening issues, ensuring effective laser weldability and mechanical strength in polyamide resin compositions.
Patent Information
- Application Number
- JP2023047172
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Polyamide resin compositions used in laser welding can experience dye migration and whitening under moist heat conditions, particularly when pigments are blended with polyamide resin.
A resin composition containing polyamide resin, perylene pigment, green pigment, and a mold release agent with a melting point lower than the polyamide resin, along with specific diamine and dicarboxylic acid-derived structural units, is used to suppress dye transfer and whitening.
The composition effectively prevents dye transfer to other members and maintains blackness even under moist heat conditions, ensuring high laser weldability and mechanical strength.
Smart Images

Figure 2024136164000001 
Figure 2024136164000002 
Figure 2024136164000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a kit, a pellet, a molded article, and a method for producing a molded article, and in particular to a resin composition containing a polyamide resin as a main component. [Background technology]
[0002] Polyamide resin, a typical engineering plastic, is easy to process and has excellent mechanical properties, electrical properties, heat resistance, and other physical and chemical properties. For this reason, it is widely used in vehicle parts, electrical and electronic equipment parts, and other precision equipment parts. Recently, parts with complex shapes have also been manufactured from polyamide resin. For example, various welding techniques, such as adhesive welding, vibration welding, ultrasonic welding, hot plate welding, injection welding, and laser welding, are used to bond parts with hollow parts such as intake manifolds.
[0003] However, welding with adhesives has problems such as the time loss required for hardening, as well as environmental impact such as pollution of the surrounding area. Problems have been pointed out with ultrasonic welding and hot plate welding, such as damage to products due to vibration and heat, and the need for post-processing due to the generation of wear powder and burrs. Injection welding often requires special molds and molding machines, and furthermore, it cannot be used unless the material has good fluidity.
[0004] On the other hand, laser welding is a method of joining a resin member (hereinafter sometimes referred to as a "transmissive resin member") that is transparent (also called non-absorbent or weakly absorbent) to laser light with a resin member (hereinafter sometimes referred to as an "absorbent resin member") that is absorbent to laser light by contacting and welding the two resin members. Specifically, this method irradiates the joining surface with laser light from the transmissive resin member side, and melts and joins the absorbing resin member that forms the joining surface with the energy of the laser light. Laser welding does not generate abrasion powder or burrs, and causes little damage to the product. Furthermore, polyamide resin itself is a material with a relatively high laser transmittance, so processing polyamide resin products using laser welding technology has recently been attracting attention.
[0005] The above-mentioned transparent resin member is usually molded from a light-transmitting resin composition. As such a light-transmitting resin composition, Patent Document 1 describes a polyamide resin composition containing 25 to 50 mass % of a semi-aromatic polyamide resin, 3 to 20 mass % of a brominated flame retardant, 1.5 to 10 mass % of zinc stannate, and a light-transmitting dye. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2020-012093 A Summary of the Invention [Problem to be solved by the invention]
[0007] As described above, a light-transmitting resin composition containing a black dye in a polyamide resin has been studied. However, such a light-transmitting resin composition may cause migration of the black dye depending on the material of the mating member or adjacent member. In order to solve this problem, it is conceivable to compound a light-transmitting resin composition by compounding a pigment instead of a dye. However, when a resin composition in which a pigment is blended with a polyamide resin was investigated, it was found that a molded article obtained from the resin composition may whiten when placed under moist and hot conditions. The present invention aims to solve such problems, and provides a resin composition capable of providing a molded article that can suppress color transfer to other components and suppress whitening even after being placed in a moist and hot condition, as well as a kit, pellets, molded article, and a method for producing a molded article. [Means for solving the problem]
[0008] As a result of the investigation by the inventors in view of the above problem, it was found that the whitening of the molded product after the wet heat test occurs depending on the type of the release agent used together with the polyamide resin and the pigment. Then, it was found that the above problem can be solved by carefully investigating the type of the release agent. Specifically, the above problems were solved by the following means. <1> A polyamide resin, a pigment, and a release agent are included. The melting point of the release agent is lower than the melting point of the polyamide resin, The pigments include a perylene pigment and a green pigment. Resin composition. <2> The polyamide resin contains diamine-derived structural units and dicarboxylic acid-derived structural units, and 70 mol % or more of the diamine-derived structural units are derived from xylylenediamine, and 70 mol % or more of the dicarboxylic acid-derived structural units are derived from an α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms. <1> The resin composition according to claim 1. <3> The xylylenediamine includes paraxylylenediamine, and the α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms includes sebacic acid. <2> The resin composition according to claim 1. <4> Further, the resin composition contains glass fibers in an amount of 20 to 60 mass %. <1> ~ <3> 10. The resin composition according to claim 9 . <5> The melting point of the release agent is equal to or higher than the melting point of the polyamide resin −150° C. and equal to or lower than the melting point of the polyamide resin −5° C. <1> ~ <4> 10. The resin composition according to claim 9 . <6> The melting point of the polyamide resin is 150 to 350°C. <1> ~ <5> 10. The resin composition according to claim 9 . <7> The melting point of the release agent is 50 to 200°C. <1> ~ <6> 10. The resin composition according to claim 9 . <8> The release agent includes a fatty acid metal salt. <1> ~ <7> 10. The resin composition according to claim 9 . <9> The perylene pigment includes at least one selected from the following: <1> ~ <8> 10. The resin composition according to claim 9 . [ka] <10> The green pigment comprises a copper halide phthalocyanine pigment. <1> ~ <9> 10. The resin composition according to claim 9 . <11> Laser welding, <1> ~ <9> 10. The resin composition according to claim 9 . <12> the polyamide resin is composed of diamine-derived structural units and dicarboxylic acid-derived structural units, 70 mol % or more of the diamine-derived structural units are derived from xylylenediamine, and 70 mol % or more of the dicarboxylic acid-derived structural units are derived from an α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms; The xylylenediamine includes p-xylylenediamine, and the α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms includes sebacic acid, Further, the resin composition contains glass fibers in an amount of 20 to 60 mass %, The melting point of the release agent is equal to or higher than the melting point of the polyamide resin −150° C. and equal to or lower than the melting point of the polyamide resin −5° C., The melting point of the polyamide resin is 150 to 350°C. The melting point of the release agent is 50 to 200° C. The release agent includes a fatty acid metal salt, The perylene pigment includes at least one selected from the following: the green pigment comprises a copper halide phthalocyanine pigment; Laser welding, <1> ~ <11> 10. The resin composition according to claim 9 . [ka] <13> When the resin composition is molded into a test piece having a thickness of 1.5 mm, the light transmittance at a wavelength of 940 nm is 25% or more. <1> ~ <12> 10. The resin composition according to claim 9 . <14> <1> ~ <13> 13. A kit comprising the resin composition according to any one of the above items 1 to 2 and a light-absorbing resin composition comprising a thermoplastic resin and a light-absorbing dye. <15> <1> ~ <13> 2. A pellet of the resin composition according to claim 1. <16> <1> ~ <13> 2. A molded article formed from the resin composition according to claim 1. <17> <15> A molded article formed from the pellets according to claim 1. <18> Advanced driver assistance system (ADAS) related parts, <16> or <17> The molded article according to claim 1. <19> In-vehicle camera parts, <16> ~ <18> 1. The molded article according to any one of the preceding claims. <20> <1> ~ <13> 1. A method for producing a molded article, comprising laser welding a molded article formed from the resin composition according to any one of claims 1 to 9, and a molded article formed from a light-absorbing resin composition containing a thermoplastic resin and a light-absorbing dye. Effect of the Invention
[0009] The present invention makes it possible to provide a resin composition capable of providing a molded article that can suppress color transfer to other components and also suppress whitening even after being placed in a moist and hot condition, as well as a kit, pellets, molded article, and a method for producing a molded article. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the present embodiment is an example for explaining the present invention, and the present invention is not limited to the present embodiment. In this specification, the use of "to" means that the numerical values before and after it are included as the lower limit and upper limit. In this specification, various physical properties and characteristic values are those at 23° C. unless otherwise specified. In this specification, unless otherwise specified, the number average molecular weight can be measured according to the description in paragraph 0047 of JP2018-165298A, the contents of which are incorporated herein by reference. If the measurement methods, etc. described in the standards shown in this specification vary from year to year, they will be based on the standards as of January 1, 2022, unless otherwise stated.
[0011] The resin composition of the present embodiment is characterized in that it contains a polyamide resin, a pigment, and a release agent, the melting point of the release agent being lower than the melting point of the polyamide resin, and the pigment contains a perylene pigment and a green pigment. By adopting such a constitution, it is possible to obtain a resin composition capable of providing a molded article capable of suppressing migration of a colorant to other members and suppressing whitening even after being placed in a moist and hot condition. Furthermore, it is possible to obtain a resin composition having excellent blackness. The reason why whitening could be suppressed is presumably because the use of a release agent with a melting point lower than that of the polyamide resin made it possible to suppress bleeding out of the release agent even when placed in a humid and hot condition.
[0012] <Polyamide resin> The resin composition of the present embodiment contains a polyamide resin. The type of polyamide resin used in this embodiment is not particularly limited, and may be either an aliphatic polyamide resin or a semi-aromatic polyamide resin. Examples of aliphatic polyamide resins include polyamide 4, polyamide 46, polyamide 6, polyamide 66, polyamide 666, polyamide 610, polyamide 11, polyamide 12, and the like. The polyamide resin used in this embodiment preferably contains a semi-aromatic polyamide resin. For example, it is more preferable that 90% by mass or more of the polyamide resin contained in the resin composition of this embodiment is a semi-aromatic polyamide resin. Here, the semi-aromatic polyamide resin is composed of a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, and it is preferable that 20 to 80 mol % (preferably 30 to 80 mol %, more preferably 40 to 70 mol %) of the total structural units of the diamine-derived structural unit and the dicarboxylic acid-derived structural unit are structural units containing an aromatic ring. By using such a semi-aromatic polyamide resin, the mechanical strength of the obtained resin molded product can be increased. Examples of the semi-aromatic polyamide resin include terephthalic acid-based polyamide resins (polyamide 6T, polyamide 6I / 6T, polyamide 9T, polyamide 10T) and xylylenediamine-based polyamide resins described later. In addition to the above, the polyamide resins described in paragraphs 0012 to 0031 of JP 2022-139048 A can also be used, the contents of which are incorporated herein by reference.
[0013] In this embodiment, a polyamide resin containing diamine-derived structural units and dicarboxylic acid-derived structural units, in which 70 mol % or more of the diamine-derived structural units are derived from xylylenediamine and 70 mol % or more of the dicarboxylic acid-derived structural units are derived from an α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms (hereinafter sometimes referred to as a "xylylenediamine-based polyamide resin") is preferred.
[0014] The diamine-derived constituent units of the xylylenediamine-based polyamide resin are more preferably 75 mol% or more, even more preferably 80 mol% or more, even more preferably 90 mol% or more, still more preferably 95 mol% or more, and particularly preferably 99 mol% or more, derived from xylylenediamine (preferably paraxylylenediamine and / or metaxylylenediamine).
[0015] The xylylenediamine is preferably paraxylylenediamine and / or metaxylylenediamine, and more preferably contains at least paraxylylenediamine. The xylylenediamine preferably contains 0 to 100 mol% metaxylylenediamine and 100 to 0 mol% paraxylylenediamine (however, the sum of metaxylylenediamine and paraxylylenediamine does not exceed 100 mol%), more preferably contains 0 to 90 mol% metaxylylenediamine and 100 to 10 mol% paraxylylenediamine, even more preferably contains 10 to 90 mol% metaxylylenediamine and 90 to 10 mol% paraxylylenediamine, still more preferably contains 20 to 90 mol% metaxylylenediamine and 80 to 10 mol% paraxylylenediamine, still more preferably contains 50 to 90 mol% metaxylylenediamine and 10 to 50 mol% paraxylylenediamine, and even more preferably contains 50 to 80 mol% metaxylylenediamine and 50 to 20 mol% paraxylylenediamine. In the xylylenediamine-based polyamide resin, the total of the constitutional units derived from paraxylylenediamine and the constitutional units derived from metaxylylenediamine preferably accounts for 80 mol % or more, more preferably 85 mol % or more, even more preferably 90 mol % or more, still more preferably 95 mol % or more, still more preferably 98 mol % or more, and still more preferably 99 mol % or more of the constitutional units derived from diamine. The upper limit of the total of the constitutional units derived from paraxylylenediamine and the constitutional units derived from metaxylylenediamine is 100 mol %.
[0016] Diamines other than metaxylylenediamine and paraxylylenediamine that can be used as the raw diamine component of the xylylenediamine-based polyamide resin include aliphatic diamines such as tetramethylenediamine, pentamethylenediamine, 2-methylpentanediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, dodecamethylenediamine, 2,2,4-trimethylhexamethylenediamine, and 2,4,4-trimethylhexamethylenediamine, 1,3-bis( Examples of the diamines include alicyclic diamines such as bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, bis(4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminomethyl)decalin, and bis(aminomethyl)tricyclodecane; and diamines having an aromatic ring such as bis(4-aminophenyl)ether, paraphenylenediamine, and bis(aminomethyl)naphthalene. These can be used alone or in combination of two or more.
[0017] On the other hand, the dicarboxylic acid-derived constituent units in the xylylenediamine-based polyamide resin are preferably 75 mol % or more, more preferably 80 mol % or more, even more preferably 90 mol % or more, even more preferably 95 mol % or more, and particularly preferably 99 mol % or more, of α,ω-straight-chain aliphatic dicarboxylic acids preferably having 4 to 20 carbon atoms (preferably α,ω-straight-chain aliphatic dicarboxylic acids having 9 to 14 carbon atoms). More specifically, the dicarboxylic acid-derived constituent units in the xylylenediamine-based polyamide resin are preferably derived from at least one of adipic acid, sebacic acid, and 1,12-dodecanedioic acid, more preferably sebacic acid and / or 1,12-dodecanedioic acid, and even more preferably sebacic acid.
[0018] Examples of dicarboxylic acid components other than those mentioned above include phthalic acid compounds such as isophthalic acid, terephthalic acid, and orthophthalic acid, and isomers of naphthalenedicarboxylic acids such as 1,2-naphthalenedicarboxylic acid, 1,3-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 1,7-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid. These can be used alone or in combination of two or more kinds.
[0019] In addition, the xylylenediamine-based polyamide resin is mainly composed of diamine-derived structural units and dicarboxylic acid-derived structural units, but does not completely exclude other structural units, and may contain lactams such as ε-caprolactam and laurolactam, and aliphatic aminocarboxylic acid-derived structural units such as aminocaproic acid and aminoundecanoic acid. Here, the main component means that the total number of diamine-derived structural units and dicarboxylic acid-derived structural units is the largest among all structural units among the structural units constituting the xylylenediamine-based polyamide resin. In this embodiment, the total of diamine-derived structural units and dicarboxylic acid-derived structural units in the xylylenediamine-based polyamide resin preferably accounts for 90% by mass or more of all structural units, more preferably accounts for 95% by mass or more, even more preferably accounts for 97% by mass or more, and even more preferably accounts for 99% by mass or more.
[0020] The melting point of the polyamide resin is preferably 150°C or higher, more preferably 180°C or higher, and even more preferably 200°C or higher, and is preferably 350°C or lower, more preferably 330°C or lower, even more preferably 300°C, even more preferably 250°C or lower, even more preferably 240°C or lower, even more preferably 230°C or lower, and particularly preferably 225°C or lower. The melting point of polyamide resin is the temperature at the top of the endothermic peak during heating observed by DSC (differential scanning calorimetry). For the measurement, a Shimadzu Corporation DSC-60 was used, the amount of sample was about 5 mg, nitrogen was flowed as the atmospheric gas at 30 mL / min, and the heating rate was 10°C / min. The melting point can be calculated from the temperature at the top of the endothermic peak observed when the sample is heated from room temperature to a temperature above the expected melting point and melted.
[0021] The lower limit of the number average molecular weight (Mn) of the polyamide resin is preferably 6,000 or more, more preferably 8,000 or more, and even more preferably 10,000 or more, and is preferably 35,000 or less, more preferably 30,000 or less, even more preferably 25,000 or less, and even more preferably 20,000 or less. When it is within such a range, the heat resistance, elastic modulus, dimensional stability, and moldability are improved.
[0022] The content of the polyamide resin in the resin composition of this embodiment is preferably 35% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and may be 60% by mass or more, based on 100% by mass of the resin composition. By making it equal to or more than the lower limit, the effects of the present invention tend to be more effectively exhibited. In addition, the content of the polyamide resin in the resin composition of this embodiment is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less, based on the resin composition. By making it equal to or less than the upper limit, the effects of the present invention tend to be more effectively exhibited. The resin composition of the present embodiment may contain only one type of polyamide resin, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0023] In the resin composition of the present embodiment, the polyamide resin and the glass fiber preferably account for 95% by mass or more of the resin composition in total, more preferably 96% by mass or more, and even more preferably 97% by mass or more. The upper limit of the total of the polyamide resin and the glass fiber is when the total accounts for 100% by mass of the resin composition.
[0024] <Pigments> The resin composition of the present embodiment contains a perylene pigment and a green pigment. By containing the perylene pigment and the green pigment, a resin composition having a high blackness can be obtained. Furthermore, a molded product having excellent laser weldability can be obtained.
[0025] The perylene pigment is a pigment having a perylene structure in the molecule. Specifically, the description in paragraph 0033 of JP-A-2022-139048 can be referred to, the contents of which are incorporated herein by reference. The perylene pigment is more preferably at least one selected from the following: [ka]
[0026] More preferably, the perylene pigment is the following compound: [ka]
[0027] The content of the perylene pigment in the resin composition of the present embodiment is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, even more preferably 0.04% by mass or more, and even more preferably 0.05% by mass or more, based on 100% by mass of the resin composition. The content of the perylene pigment is preferably 0.4% by mass or less, more preferably 0.3% by mass or less, even more preferably 0.2% by mass or less, even more preferably 0.18% by mass or less, and may be 0.14% by mass or less, or 0.08% by mass or less, based on 100% by mass of the resin composition. By keeping the content below the upper limit, visual blackness tends to be more effectively maintained. The resin composition of the present embodiment may contain only one type of perylene pigment, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0028] On the other hand, the type of the green pigment is not particularly limited, but examples thereof include phthalocyanine pigments and perylene pigments. Phthalocyanine pigments are preferred, copper phthalocyanine pigments are more preferred, copper halogenated phthalocyanine pigments are even more preferred, and copper chlorophthalocyanine pigments and copper fluorophthalocyanine pigments are even more preferred.
[0029] The content of the green pigment in the resin composition of this embodiment is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, even more preferably 0.04% by mass or more, may be 0.06% by mass or more, or may be 0.11% by mass or more, based on 100% by mass of the resin composition. The content of the green pigment is preferably 0.4% by mass or less, more preferably 0.3% by mass or less, even more preferably 0.2% by mass or less, and even more preferably 0.18% by mass or less, based on 100% by mass of the resin composition. By keeping the content below the upper limit, visual blackness tends to be more effectively maintained. The resin composition of the present embodiment may contain only one type of green pigment, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0030] The total amount of the perylene pigment and the green pigment in the resin composition of this embodiment is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, based on 100% by mass of the resin composition. By making it equal to or more than the lower limit, the visual blackness tends to be improved. In addition, the total amount of the perylene pigment and the green pigment is preferably 0.5% by mass or less, more preferably 0.4% by mass or less, and even more preferably 0.3% by mass or less, based on 100% by mass of the resin composition. By making it equal to or less than the upper limit, the light transmittance tends to be improved while maintaining the visual blackness.
[0031] In particular, when the total amount of the perylene pigment and the green pigment is 100 parts by mass, the mass ratio of the perylene pigment to the green pigment is preferably 10 to 90:90 to 10. By adopting such a constitution, a molded article having remarkably excellent blackness, more effectively suppressing the occurrence of sink marks, and high light transmittance over the range of 900 to 1100 nm can be obtained. The mass ratio of the perylene pigment to the green pigment is preferably 10 to 80:90 to 20, more preferably 10 to 77:90 to 23, even more preferably 10 to 75:90 to 25, and may be 15 to 75:85 to 25, or may be 20 to 75:80 to 25.
[0032] The resin composition of the present embodiment may also contain colorants other than the perylene pigment and the green pigment, but preferably does not substantially contain other colorants. "Substantially does not contain" means that the amount of colorants other than the perylene pigment and the green pigment relative to the total amount of colorants is 10% by mass or less, preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1% by mass or less, even more preferably 0.1% by mass or less, and even more preferably 0.01% by mass or less.
[0033] <Release agent> The resin composition of the present embodiment contains a release agent, and the melting point of the release agent is lower than the melting point of the polyamide resin. It is presumed that such a configuration can suppress bleeding out of the release agent and suppress whitening of the resulting molded product. The melting point of the release agent used in this embodiment is a value measured in accordance with DSC7020. In this embodiment, the melting point of the release agent is lower than the melting point of the polyamide resin, but the melting point of the release agent is preferably the melting point of the polyamide resin -150°C or more, more preferably the melting point of the polyamide resin -140°C or more, and even more preferably the melting point of the polyamide resin -130°C or more. By making it equal to or higher than the lower limit, surface whitening under high temperature and high humidity tends to be suppressed. In addition, the melting point of the release agent is lower than the melting point of the polyamide resin, but the melting point of the release agent is preferably the melting point of the polyamide resin -5°C or less, more preferably the melting point of the polyamide resin -15°C or less, even more preferably the melting point of the polyamide resin -25°C or less, even more preferably the melting point of the polyamide resin -35°C or less, and even more preferably the melting point of the polyamide resin -50°C or less. By making it equal to or lower than the upper limit, surface whitening under high temperature and high humidity tends to be suppressed. When the resin composition of the present embodiment contains two or more types of release agents, the melting point of the release agent having the highest melting point value is used.
[0034] The melting point of the release agent is preferably 50°C or higher, more preferably 65°C or higher, even more preferably 75°C or higher, even more preferably 85°C or higher, even more preferably 95°C or higher, and even more preferably 105°C or higher. By setting it to the lower limit or higher, surface whitening under high temperature and high humidity tends to be suppressed. In addition, the melting point of the release agent is preferably 215°C or lower, more preferably 205°C or lower, even more preferably 200°C or lower, even more preferably 195°C or lower, even more preferably 185°C or lower, and even more preferably 175°C or lower. By setting it to the upper limit or lower, surface whitening under high temperature and high humidity tends to be suppressed.
[0035] The type of release agent used in this embodiment is not particularly limited, but it is preferable to include at least one selected from the group consisting of aliphatic carboxylic acids, fatty acid metal salts, esters of aliphatic carboxylic acids and alcohols, aliphatic hydrocarbon compounds having a number average molecular weight of 200 to 15,000, polysiloxane-based silicone oils, and amide-based waxes, and it is more preferable to include fatty acid metal salts. For details of the release agent, please refer to the descriptions in paragraphs 0055 to 0061 of JP 2018-095706 A and the descriptions in paragraphs 0022 to 0027 of JP 2019-108526 A, the contents of which are incorporated herein by reference.
[0036] The fatty acid metal salt is preferably a metal salt of a long-chain fatty acid having 16 to 36 carbon atoms, and examples thereof include metal stearates such as calcium stearate, zinc stearate, aluminum stearate, sodium stearate, and lithium stearate, and metal montanic acids such as calcium montanate and sodium montanate, with metal montanic acids being preferred, and calcium montanate being more preferred.
[0037] The content of the release agent in the resin composition of this embodiment is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.2% by mass or more in the resin composition. By making it equal to or more than the lower limit, the releasability tends to be further improved. In addition, the content of the release agent is preferably 3% by mass or less, more preferably 2% by mass or less, even more preferably 1% by mass or less, even more preferably 0.8% by mass or less, and even more preferably 0.6% by mass or less. By making it equal to or less than the upper limit, the difference in transmittance due to the mold temperature tends to be smaller. The resin composition of the present embodiment may contain only one type of release agent, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0038] <Glass fiber> The resin composition of the present embodiment preferably contains glass fibers in a ratio of 20 to 60 mass % in the resin composition. By containing the glass fibers in this ratio, high mechanical strength can be achieved for the obtained molded article. The glass fiber that can be used in the resin composition of the present embodiment is preferably surface-treated with a surface treatment agent such as a coupling agent. Glass fibers to which a surface treatment agent is attached are preferred because they have excellent durability, moist heat resistance, hydrolysis resistance, and heat shock resistance.
[0039] The glass fibers are made of a glass composition such as A-glass, C-glass, E-glass, S-glass, R-glass, M-glass, or D-glass, with E-glass (alkali-free glass) being particularly preferred.
[0040] The glass fiber used in the resin composition of the present embodiment may be a single fiber or a plurality of single fibers twisted together. The form of the glass fiber may be any of "glass roving" which is a single fiber or a plurality of single fibers twisted together and wound continuously, "chopped strand" which is cut to a length of 1 to 10 mm, and "milled fiber" which is pulverized to a length of 10 to 500 μm. Such glass fibers are commercially available under the trade names "Glaslon Chopped Strand" and "Glaslon Milled Fiber" from Asahi Fiber Glass Co., Ltd. and "E Glass Fiber Chopped Strand" from Nippon Electric Glass Co., Ltd., and are easily available. Glass fibers of different forms can also be used in combination.
[0041] The glass fiber used in this embodiment may have a circular or noncircular cross section. By using glass fiber having a noncircular cross section, warping of the obtained molded product can be more effectively suppressed. In this embodiment, even if glass fiber having a circular cross section is used, warping can be effectively suppressed by using a polyamide resin that crystallizes sufficiently even at a low mold temperature.
[0042] The content of glass fibers in the resin composition of this embodiment is preferably 20 mass% or more, and more preferably 25 mass% or more, and is preferably 60 mass% or less, and more preferably 55 mass% or less, and may further be 50 mass% or less, 45 mass% or less, 40 mass% or less, or 35 mass% or less. The resin composition of the present embodiment may contain only one type of glass fiber, or may contain two or more types. When two or more types are contained, the total amount is within the above range. Note that the content of the glass fiber in the present embodiment is intended to include the amount of the bundling agent and the surface treatment agent.
[0043] <Copper iodide, potassium iodide and cerium oxide> The resin composition of the present embodiment preferably contains at least one of copper iodide, potassium iodide, and cerium oxide, and more preferably contains at least one of copper iodide and potassium iodide. By containing copper iodide, the heat resistance of the resulting molded product tends to be improved. In addition, by containing potassium iodide, a complex is easily formed in the polyamide resin, and decomposition of the resin tends to be more effectively suppressed. In other words, by blending these components, it is possible to impart performance according to the application.
[0044] The proportion of copper iodide in the resin composition of this embodiment is preferably 0.01 mass% or more, and more preferably 0.02 mass% or more, and is preferably 2 mass% or less, more preferably 1 mass% or less, even more preferably 0.5 mass% or less, and even more preferably 0.3 mass% or less. The proportion of potassium iodide in the resin composition of this embodiment is preferably 0.01 mass% or more, and more preferably 0.02 mass% or more, and is preferably 2 mass% or less, more preferably 1 mass% or less, even more preferably 0.5 mass% or less, and even more preferably 0.3 mass% or less. The proportion of cerium oxide in the resin composition of this embodiment is preferably 0.01 mass% or more, and more preferably 0.02 mass% or more, and is preferably 2 mass% or less, more preferably 1 mass% or less, even more preferably 0.5 mass% or less, and even more preferably 0.3 mass% or less.
[0045] <Nucleating agent> The resin composition of the present embodiment may contain a nucleating agent. There are no particular limitations on the nucleating agent, so long as it remains unmelted during melt processing and can become a crystal nucleus during the cooling process. Among these, talc and calcium carbonate are preferred, and talc is more preferred. The lower limit of the number average particle size of the nucleating agent is preferably 0.1 μm or more, more preferably 1 μm or more, and even more preferably 3 μm or more.The upper limit of the number average particle size of the nucleating agent is preferably 40 μm or less, more preferably 30 μm or less, even more preferably 28 μm or less, even more preferably 15 μm or less, and even more preferably 10 μm or less.
[0046] The content of the nucleating agent in the resin composition of the present embodiment is preferably 0.01 to 1 mass %, more preferably 0.1 mass % or more, and more preferably 0.5 mass % or less. The resin composition of the present embodiment may contain only one type of nucleating agent, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0047] <Other ingredients> The resin composition of the present embodiment may contain other components within the scope of the present invention, such as flame retardants, flame retardant assistants, light stabilizers, antioxidants, ultraviolet absorbers, fluorescent brighteners, anti-dripping agents, antistatic agents, anti-fogging agents, anti-blocking agents, flow improvers, plasticizers, dispersants, antibacterial agents, etc. In the resin composition of this embodiment, the contents of the polyamide resin, perylene pigment, green pigment, and release agent, as well as other components that are blended as necessary, are adjusted so that the total of each component is 100 mass %. In this embodiment, an embodiment in which the total of the polyamide resin, perylene pigment, green pigment, release agent, copper iodide, and potassium iodide accounts for 98 mass % or more of the resin composition is exemplified.
[0048] <Physical properties of resin composition> The resin composition of the present embodiment preferably has a high light transmittance at wavelengths of 940 to 1100 nm. For example, when the resin composition of the present embodiment is molded into a test piece having a thickness of 1.5 mm, the light transmittance at a wavelength of 940 nm is preferably 25% or more, more preferably 29% or more. The upper limit of the light transmittance at a wavelength of 940 nm of the test piece having a thickness of 1.5 mm is, for example, 90% or less, and may be 70% or less. When a pigment is blended into a polyamide resin, the light transmittance is usually reduced, but in the present embodiment, the light transmittance can be maintained at a high level by using a perylene pigment and a green pigment in combination as the pigment. The light transmittance is measured by preparing a test piece for measuring light transmittance (ASTM D638 standard No. 4 dumbbell piece, 1.5 mm thick) from the resin composition, and measuring the light transmittance on the side opposite the gate using a transmittance measuring device. The transmittance measuring device may be UV-3600 manufactured by Shimadzu Corporation. The resin composition of the present embodiment preferably has excellent blackness. For example, when the resin composition of the present embodiment is molded into a test piece having a thickness of 1.5 mm, the L value is preferably less than 20, more preferably 19 or less, and even more preferably 18 or less. The lower limit of the L value is ideally 0, but even if it is 1 or more, the required performance is sufficiently satisfied. Such a high blackness is achieved by using a perylene pigment and a green pigment in combination.
[0049] <Method of producing resin composition> The method for producing the resin composition of the present embodiment is not particularly limited, but a method using a single-screw or twin-screw extruder having a vent port for volatilization as a kneader is preferred. The polyamide resin, perylene pigment, green pigment, release agent, and other additives to be mixed as necessary may be fed to the kneader all at once, or the polyamide resin component may be fed, and then the other blended components may be fed sequentially. The glass fiber is preferably fed from the middle of the extruder in order to prevent it from being crushed during kneading. Two or more components selected from each component may be mixed and kneaded in advance. In this embodiment, the pigment may be a polyamide resin or the like that is prepared in advance as a master batch, and then kneaded with other components to obtain the resin composition in this embodiment.
[0050] The method for producing a molded product using the resin composition of the present embodiment is not particularly limited, and molding methods generally used for thermoplastic resins, such as injection molding, blow molding, extrusion molding, and press molding, can be applied. In this case, the particularly preferred molding method is injection molding because of its good fluidity. In injection molding, it is preferable to control the resin temperature to 250 to 310°C.
[0051] <Application> The resin composition of the present embodiment is preferably used for laser welding, in particular, as a light-transmitting resin composition for laser welding. One embodiment of the resin composition of the present embodiment is in the form of pellets. In the present embodiment, the molded article is preferably formed from a resin composition or pellets.
[0052] <Kit> The resin composition of this embodiment and a light-absorbing resin composition containing a thermoplastic resin and a light-absorbing dye are preferably used as a kit for producing a molded article by laser welding. That is, the resin composition of the present embodiment included in the kit serves as a light-transmitting resin composition, and a molded article formed from such a light-transmitting resin composition serves as a transmissive resin member for laser light during laser welding, whereas a molded article formed from a light-absorbing resin composition serves as an absorbing resin member for laser light during laser welding.
[0053] <<Light-absorbing resin composition>> The light absorbing resin composition used in this embodiment contains a thermoplastic resin and a light absorbing dye, and may further contain other components such as a reinforcing filler. Examples of the thermoplastic resin include polyamide resin, olefin resin, vinyl resin, styrene resin, acrylic resin, polyphenylene ether resin, polyester resin, polycarbonate resin, polyacetal resin, etc., and from the viewpoint of good compatibility with the light-transmitting resin composition (the resin composition of the present embodiment), polyamide resin, polyester resin, and polycarbonate resin are particularly preferred, and polyamide resin is more preferred. The thermoplastic resin may be one type or two or more types. The type of polyamide resin used in the light absorbing resin composition is not limited, but the above-mentioned xylylenediamine polyamide resin is preferred. Examples of the reinforcing filler include glass filler (preferably glass fiber), carbon fiber, silica, alumina, carbon black, and fillers capable of absorbing laser light, such as inorganic powder coated with a material that absorbs laser light, and glass fiber is preferred. The glass fiber is synonymous with the glass fiber that may be blended in the resin composition of the present embodiment, and the preferred range is also the same. The content of the reinforcing filler is preferably 20 to 70 mass%, more preferably 25 to 60 mass%, and further preferably 30 to 55 mass%. The light absorbing dye includes a dye having an absorption wavelength in the range of the wavelength of the irradiated laser light, for example, in the range of 900 nm to 1100 nm in this embodiment. The light absorbing dye also includes a dye having a transmittance of less than 30%, or even 10% or less, when mixed in an amount of 0.3 parts by mass with respect to 100 parts by mass of polyamide resin and the light transmittance is measured. Specific examples of light absorbing pigments include inorganic pigments (black pigments such as carbon black (e.g., acetylene black, lamp black, thermal black, furnace black, channel black, ketjen black, etc.), red pigments such as iron oxide red, orange pigments such as molybdate orange, and white pigments such as titanium oxide), and organic pigments (yellow pigments, orange pigments, red pigments, blue pigments, green pigments, etc.). Among them, inorganic pigments are generally preferred because of their strong hiding power, and black pigments are more preferred. Two or more of these light absorbing pigments may be used in combination. The content of the light absorbing pigment is preferably 0.01 to 30 parts by mass relative to 100 parts by mass of the polyamide resin.
[0054] In the above kit, it is preferable that 80% by mass or more of the components in the resin composition other than the light-transmitting pigment and reinforcing filler are common to the components in the light-absorbing resin composition other than the light-absorbing pigment and reinforcing filler, more preferably 90% by mass or more of the components in the light-absorbing resin composition other than the light-absorbing pigment and reinforcing filler, and even more preferably 95 to 100% of the components in the light-absorbing resin composition other than the light-transmitting pigment and reinforcing filler are common to the components in the above kit.
[0055] <<Laser welding method>> Next, the laser welding method will be described. In this embodiment, a molded article (transmissive resin member) formed from the resin composition of this embodiment and a molded article (absorbent resin member) formed from the light-absorbing resin composition can be laser-welded to produce a molded article (laser-welded body). By laser welding, the transmissive resin member and the absorbent resin member can be firmly welded together without using an adhesive. The shape of the member is not particularly limited, but since the members are used by joining them together by laser welding, the shape usually has at least a surface contact portion (flat surface, curved surface). In laser welding, the laser light transmitted through the transparent resin member is absorbed by the absorbing resin member, melts, and the two members are welded together. The molded product formed from the resin composition of this embodiment has high transparency to laser light, so it can be preferably used as a transparent resin member. Here, the thickness of the member through which the laser light transmits (thickness in the laser transmission direction at the part through which the laser light transmits) can be appropriately determined taking into consideration the application, the composition of the resin composition, and other factors, and is, for example, 5 mm or less, preferably 4 mm or less.
[0056] The laser light source used in laser welding can be determined according to the transmission wavelength of the light of the light-transmitting dye, and is preferably a laser with a wavelength in the range of 900 to 1100 nm. For example, a semiconductor laser or a fiber laser can be used.
[0057] More specifically, for example, when welding a transparent resin member and an absorbing resin member, first, the parts to be welded of both are brought into contact with each other. At this time, it is preferable that the welded parts of both are in surface contact, and they may be flat surfaces, curved surfaces, or a combination of flat surfaces and curved surfaces. Next, laser light is irradiated from the transparent resin member side. At this time, if necessary, a lens may be used to focus the laser light at the interface between the two. The focused beam passes through the transparent resin member and is absorbed near the surface of the absorbing resin member, generating heat and melting it. Next, the heat is transmitted to the transparent resin member by thermal conduction and melts it, forming a molten pool at the interface between the two, and after cooling, the two are joined together. The molded product in which the transmissive resin member and the absorptive resin member are welded in this manner has high weld strength. Note that the molded product in this embodiment is intended to include not only finished products and parts, but also members that form part of these products and parts.
[0058] The molded article obtained by laser welding in this embodiment can be applied to various uses, for example, various storage containers, electrical and electronic equipment parts, office automation (OA) equipment parts, household appliance parts, mechanical mechanism parts, vehicle mechanism parts, etc. In particular, it can be suitably used for food containers, medicine containers, oil and fat product containers, hollow parts for vehicles (various tanks, intake manifold parts, camera housings, etc.), electrical parts for vehicles (various control units, ignition coil parts, etc.), advanced driver assistance system (ADAS) related parts, motor parts, various sensor parts, connector parts, switch parts, breaker parts, relay parts, coil parts, transformer parts, lamp parts, etc. In particular, the resin composition or kit of this embodiment is suitable for advanced driver assistance system (ADAS) related parts (especially in-vehicle camera parts). Examples of related parts used in ADAS (Advanced Driver Assistance System) include cameras for image data, lidars and millimeter-wave radar parts for distance data, GPS and odometer parts for position data, and IMU (Inertial Measurement Unit) parts for speed, acceleration, and attitude data, etc.
Examples
[0059] The present invention will be described more specifically with reference to the following examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed as long as they do not depart from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. When the measuring instruments used in the examples are difficult to obtain due to being obsolete, etc., measurements can be made using other devices having equivalent performance.
[0060] 1. Raw materials <Polyamide resin> MP10: The molar ratio of metaxylylenediamine / paraxylylenediamine (M / P) = 7:3, synthesized according to the following synthesis example. <<Synthesis example of MP10 (M / P molar ratio = 7:3)>> Sebacic acid was dissolved by heating in a reaction vessel under a nitrogen atmosphere, and then a mixed diamine of paraxylylenediamine (manufactured by Mitsubishi Gas Chemical Co., Ltd.) and metaxylylenediamine (manufactured by Mitsubishi Gas Chemical Co., Ltd.) in a molar ratio of 3:7 was gradually added dropwise under pressure (0.35 MPa) so that the molar ratio of diamine to sebacic acid became approximately 1:1, while the temperature was raised to 235°C. After the addition was completed, the reaction was continued for 60 minutes, and the amount of components with a molecular weight of 1,000 or less was adjusted. After the reaction was completed, the contents were taken out in the form of strands and pelletized with a pelletizer to obtain a polyamide resin (MP10).
[0061] <Talc> #5000S: Hayashi Kasei, Micron White <Copper iodide (CuI)> Cuprous iodide, manufactured by Nippon Chemical Industries Co., Ltd. <Potassium iodide> Fujifilm Wako Pure Chemical Industries, Ltd.
[0062] <Release agent> Zinc stearate (II): Fujifilm Wako Pure Chemical Industries, Ltd. CS8CP: Calcium montanate, manufactured by Nitto Kasei Kogyo Co., Ltd. Light Amide WH-255: Kyoeisha Chemical Co., Ltd., higher fatty acid amide LICOLUB WE 4: Clariant Chemical Company, Montan acid ester LICOWAX E: Clariant Chemical Company, Montan acid ester
[0063] <Glass fiber (GF)> ECS03T-756H: Nippon Electric Glass Co., Ltd., glass fiber
[0064] <Pigments> Red-purple pigment: Paliogen Red violet K5411, Manufacturer: Color & Effect Japan Co., Ltd. Green pigment: Heliogen Green K9362, Manufacturer: Color & Effect Japan Co., Ltd.
[0065] Examples 1 to 9, Comparative Examples 1 to 3 <Compound> The components other than the glass fiber were weighed and dry-blended so as to have the compositions shown in Tables 1 to 4 below (each component in Tables 1 to 4 is expressed in parts by mass), and then, after being dry-blended, they were introduced from the screw root of a twin-screw extruder (manufactured by Shibaura Machine Co., Ltd., TEM26SS) using a twin-screw cassette weighing feeder (manufactured by Kubota Corporation, CE-W-1-MP). For the glass fiber, it was introduced into the above-mentioned twin-screw extruder from the side of the extruder using a vibratory cassette weighing feeder (manufactured by Kubota Corporation, CE-V-1B-MP), and melt-kneaded with the resin components, etc., to obtain resin composition pellets. The temperature setting of the extruder was 280 °C.
[0066] <Manufacture of ASTM D638 standard No. 4 dumbbell piece (1.5 mm thick)> After drying the pellets of the resin composition obtained by the above manufacturing method at 120 °C for 3 hours, an ASTM D638 standard No. 4 dumbbell piece (1.5 mm thick) was injection-molded using an injection molding machine (manufactured by Nissei Plastic Industrial Co., Ltd., "NEX140III") under the conditions of a cylinder temperature of 260 °C, a mold temperature of 110 °C, and a molding cycle of 50 seconds.
[0067] <Whitening after the damp heat test> The surface state of an ASTM D638 standard No. 4 dumbbell piece (1.5 mm thick) placed under high temperature and high humidity (85 °C, 85%) was confirmed when a 50-hour test was conducted, and the presence or absence of whitening was confirmed.
[0068] <L* value before the damp heat test> Regarding the test piece for measuring the linear transmittance before the damp heat test (ASTM D638 standard No. 4 dumbbell piece, 1.5 mm thick), in accordance with JIS K7105, the L* value was measured using a color difference meter (SE6000 manufactured by Nippon Denshoku Industries Co., Ltd.) under the following measurement conditions. Measurement conditions: Reflectance measurement, C light source / 2°, field of view 30Φ, using a white plate
[0069] <L* value before the damp heat test> For the test pieces for measuring the linear transmittance after the wet heat test (ASTM D638 standard No. 4 dumbbell pieces, 1.5 mm thick), the L* value was measured under the following measurement conditions using a color difference meter (SE6000 manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K7105. Measurement conditions: Reflection measurement, C light source / 2°, field of view 30Φ, white plate used
[0070] <Light transmittance> The light transmittance was measured using a transmittance measuring device on the side of a test piece for measuring light transmittance (ASTM D638 standard No. 4 dumbbell piece, 1.5 mm thick) opposite the gate. The transmittance measurement device used was a UV-3600 Plus manufactured by Shimadzu Corporation.
[0071] [Table 1]
[0072] [Table 2]
[0073] [Table 3]
[0074] [Table 4]
[0075] As is clear from the above results, the molded article formed from the resin composition of the present invention is inhibited from whitening after the wet heat test, and the L * value and L after damp heat test * The light transmittance was low and the blackness was excellent (Examples 1 to 9). In contrast, when a release agent having a melting point higher than that of the polyamide resin was used, whitening occurred after the wet heat test and the blackness was poor (Comparative Examples 1 to 3).
Claims
1. A polyamide resin, a pigment, and a release agent are included. The melting point of the release agent is lower than the melting point of the polyamide resin, The pigments include a perylene pigment and a green pigment. Resin composition.
2. The polyamide resin comprises a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, and 70 mol % or more of the diamine-derived structural unit is derived from xylylenediamine, and 70 mol % or more of the dicarboxylic acid-derived structural unit is derived from an α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms. The resin composition according to claim 1.
3. 3. The resin composition according to claim 2, wherein the xylylenediamine comprises paraxylylenediamine, and the α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms comprises sebacic acid.
4. The resin composition according to claim 1 or 2, further comprising glass fibers in an amount of 20 to 60 mass % in the resin composition.
5. 3. The resin composition according to claim 1, wherein the melting point of the release agent is not less than the melting point of the polyamide resin minus 150° C. and not more than the melting point of the polyamide resin minus 5° C.
6. The resin composition according to claim 1 or 2, wherein the melting point of the polyamide resin is 150 to 350°C.
7. The resin composition according to claim 1 or 2, wherein the melting point of the release agent is 50 to 200°C.
8. The resin composition according to claim 1 , wherein the release agent comprises a fatty acid metal salt.
9. The resin composition according to claim 1 or 2, wherein the perylene pigment comprises at least one selected from the following: 【Chemistry 1】
10. The resin composition according to claim 1 or 2, wherein the green pigment comprises a copper halide phthalocyanine pigment.
11. The resin composition according to claim 1 or 2, which is used for laser welding.
12. the polyamide resin is composed of diamine-derived structural units and dicarboxylic acid-derived structural units, 70 mol % or more of the diamine-derived structural units are derived from xylylenediamine, and 70 mol % or more of the dicarboxylic acid-derived structural units are derived from an α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms; The xylylenediamine includes p-xylylenediamine, and the α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms includes sebacic acid, Further, the resin composition contains glass fibers in an amount of 20 to 60% by mass, The melting point of the release agent is equal to or higher than the melting point of the polyamide resin −150° C. and equal to or lower than the melting point of the polyamide resin −5° C., The melting point of the polyamide resin is 150 to 350° C. The melting point of the release agent is 50 to 200° C. The release agent includes a fatty acid metal salt, The perylene pigment includes at least one selected from the following: the green pigment comprises a copper halide phthalocyanine pigment; Laser welding, The resin composition according to claim 1. 【Chemistry 2】
13. 13. The resin composition according to claim 1, 2 or 12, wherein the resin composition has a light transmittance of 25% or more at a wavelength of 940 nm when molded into a test piece having a thickness of 1.5 mm.
14. A kit comprising the resin composition according to claim 1, 2 or 12, and a light-absorbing resin composition comprising a thermoplastic resin and a light-absorbing dye.
15. A pellet of the resin composition according to claim 1, 2 or 12.
16. A molded article formed from the resin composition according to claim 1, 2 or 12.
17. 16. A molded article formed from the pellets of claim 15.
18. 17. The molded article according to claim 16, which is an advanced driver assistance system (ADAS)-related part.
19. The molded article according to claim 16, which is an in-vehicle camera part.
20. A method for producing a molded article, comprising laser welding a molded article formed from the resin composition according to claim 1, 2 or 12 and a molded article formed from a light-absorbing resin composition comprising a thermoplastic resin and a light-absorbing dye.
Citation Information
Patent Citations
Polyamide resin composition, kit, method for producing molding and molding
JP2020012093A