Elastomer composition
The elastomer composition with a cyclocarbonate group-containing polymer and elastomer addresses the challenge of achieving mechanical properties and low specific gravity, offering improved strength, elongation, and recyclability.
Patent Information
- Application Number
- JP2023047334
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional elastomer compositions using inorganic or organic fillers face challenges in achieving both mechanical properties and low specific gravity, as the addition of these fillers increases weight and decreases recyclability.
An elastomer composition containing a polymer derived from a cyclocarbonate group-containing monomer and an elastomer, with specific particle sizes and ratios, which provides low specific gravity, excellent adhesion, and improved recyclability while maintaining mechanical properties.
The composition achieves both low specific gravity and enhanced mechanical properties, including strength and elongation, while maintaining good adhesion and recyclability.
Smart Images

Figure 2024136262000001 
Figure 2024136262000002 
Figure 2024136262000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an elastomer composition, and an object of the present invention is to provide an elastomer composition which has both good mechanical properties and a small specific gravity. [Background technology]
[0002] Elastomers are resins with viscoelasticity, and a method of adding a reinforcing filler is known as a method of imparting toughness to elastomers. For example, Patent Document 1 shows that the mechanical properties of elastomers are improved by adding inorganic fillers such as carbon black, silica particles, and calcium carbonate to nitrile rubber. However, the addition of these inorganic fillers increases the specific gravity, which leads to problems such as an increase in weight per unit volume and a decrease in recyclability. On the other hand, Patent Document 2 shows that the specific gravity can be reduced by using resin particles as an organic filler, but there is a problem that mechanical properties are not sufficiently obtained. As described above, it has been difficult for conventional elastomer compositions using inorganic or organic fillers to achieve both good mechanical properties and a low specific gravity. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2020-143251 [Patent Document 2] Patent Publication No. 2022-154859 Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention aims to solve the problems associated with conventional elastomer compositions using inorganic or organic fillers, and aims to provide an elastomer composition that can improve the mechanical properties of elastomers and has a small specific gravity. [Means for solving the problem]
[0005] As a result of intensive research into solving the above problems, the present inventors have found that the above problems can be solved by an elastomer composition containing a polymer containing a structure derived from a cyclocarbonate group-containing monomer in the polymer structure and an elastomer. The present invention based on this new finding includes the following aspects.
[0006] An elastomer composition comprising 1 to 90 mass% of a polymer (A) having a particle size of 10 to 1000 nm and 10 to 99 mass% of an elastomer (B), wherein the polymer (A) is a polymer obtained by polymerizing monomer components comprising 1 to 100 mass% of a cyclocarbonate group-containing monomer (A1) represented by the following formula (1) or formula (2) and 0 to 99 mass% of a copolymerizable radical polymerizable monomer (A2):
[0007] [ka] (In formula (1) and formula (2), R 1 represents a hydrogen atom or a methyl group, A represents an alkylene group having 1 to 10 carbon atoms, and X represents 0 or 1. Effect of the Invention
[0008] The elastomer composition of the present invention, like elastomer compositions using conventional organic fillers, has a small specific gravity, excellent adhesion and recyclability, and can also have improved mechanical properties. It is therefore possible to achieve both mechanical properties and a small specific gravity, which was difficult to achieve with elastomer compositions using conventional organic fillers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the embodiment described in this specification, and various modifications are possible without departing from the gist of the present invention. In this specification, a numerical range defined using the symbol "~" is intended to include both the upper and lower limits of the range. For example, "2~5" means 2 or more and 5 or less. In the present specification, in which multiple numerical ranges are described in stages, each upper limit and each lower limit can be the upper limit or lower limit of any combination of numerical ranges. For example, when the content of a certain component is described as "5-20 mass%, 10-15 mass%, "it can be each of the numerical ranges of "5-15 mass%, " "10-20 mass%, " "5-10 mass%, " and "15-20 mass%. Furthermore, in the numerical ranges described in this specification, the upper limit or lower limit of the numerical ranges can be replaced with values shown in the examples or values that are uniquely derived from the examples. In this specification, "(meth)acrylic" refers to acrylic or methacrylic, "(meth)acrylate" refers to acrylate or methacrylate, and "(meth)acrylic acid" refers to acrylic acid or methacrylic acid.
[0010] <Elastomer composition> The elastomer composition of the present invention contains a polymer (A) and an elastomer (B). Hereinafter, the polymer (A) and the elastomer (B) will be described in order.
[0011] [Polymer (A)] The polymer (A) is a polymer obtained by polymerizing monomer components that contain at least a cyclocarbonate group-containing monomer (A1) represented by formula (1) or formula (2) and may contain a copolymerizable radically polymerizable monomer (A2).
[0012] Cyclocarbonate group-containing monomer (A1) The cyclocarbonate group-containing monomer (A1) is represented by the following formula (1) or formula (2). The monomer (A1) may be composed of only the monomer of either formula (1) or formula (2), or may be composed of both the monomer of formula (1) and the monomer of formula (2).
[0013] [ka]
[0014] In formula (1) and formula (2), R 1 represents a hydrogen atom or a methyl group. In addition, A represents an alkylene group having 1 to 10 carbon atoms. In view of availability and ease of synthesis, the number of carbon atoms in A is preferably 2 to 8, and more preferably 2 to 4. In formula (1) and formula (2), x represents 0 or 1. From the viewpoint of availability and ease of synthesis, x is preferably 0.
[0015] The cyclocarbonate group-containing monomer (A1) of formula (1) and formula (2) has a cyclocarbonate group in the molecule, which results in a cyclocarbonate structure in the polymer. The (meth)acrylate portion in the monomer (A1) contributes to the polymerization reaction. The polyoxyalkylene group portion acts as a linker between the cyclocarbonate structure and the (meth)acrylate portion.
[0016] Monomer (A1) can be produced by a known method. For example, various epoxy compounds having a (meth)acryloyl group can be used as starting materials, and carbon dioxide can be blown in at about 0.05 to 0.3 MPa to react to obtain monomer (A1). In this case, various monomers can be used as the epoxy compound having a (meth)acryloyl group. However, since it has a low viscosity, the reaction time is short, and the obtained cyclocarbonate group-containing monomer (A1) has a low hue and good transparency, it is preferable to use glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, etc. as monomer (A1) represented by formula (1), and it is preferable to use 3,4-epoxycyclohexylmethyl methacrylate, etc. as monomer (A1) represented by formula (2), and it is more preferable to use glycidyl (meth)acrylate.
[0017] The cyclocarbonate group-containing monomer (A1) can be synthesized by reacting carbon dioxide with an epoxy group to form a cyclocarbonate group. The conditions for introducing carbon dioxide into the reaction system can be selected from blowing under pressure or normal pressure, but blowing under pressure is preferred. At this time, by controlling the pressure and temperature within a certain range, the yield of the target product can be increased and the content of by-products can be kept low. In this case, the pressure is, for example, 0.05 to 0.3 MPaG, and preferably 0.1 to 0.2 MPaG. If the set pressure is too high, the yield of the cyclocarbonate body does not increase, side reactions tend to proceed, and the content of the by-product di(meth)acrylate monomer may increase.
[0018] The reaction temperature during the synthesis of the monomer (A1) varies depending on the pressure and catalyst conditions, but is, for example, in the range of 40 to 70°C, and preferably in the range of 50 to 60°C. If the reaction temperature is too low, the reaction takes too long, and unreacted raw materials tend to remain. In addition, coloring tends to occur. On the other hand, if the reaction temperature is too high, a large amount of di(meth)acrylate monomer, which is a by-product, is contained, and problems such as gelation tend to occur during polymerization. In addition, coloring tends to occur.
[0019] Copolymerizable radical polymerizable monomer (A2) The radical polymerizable monomer (A2) which can be copolymerized with the cyclocarbonate group-containing monomer (A1) is not particularly limited, and examples thereof include (meth)acrylic acid esters, aromatic vinyl compounds, amide group-containing monomers, (meth)acrylonitrile, and the like, and one or more of these may be used.
[0020] Examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, ) glyceryl acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, stearyl (meth)acrylate, and ethylene oxide adducts of (meth)acrylic acid. Of these, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and benzyl (meth)acrylate are preferred, and methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are more preferred.
[0021] Examples of aromatic vinyl compounds include styrene, α-methylstyrene, p-methylstyrene, m-methylstyrene, o-methylstyrene, p-ethylstyrene, m-ethylstyrene, o-ethylstyrene, t-butylstyrene, chlorostyrene, hydroxystyrene, t-butoxystyrene, vinyltoluene, and vinylnaphthalene, with styrene being preferred.
[0022] Examples of the amide group-containing monomer include acrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, N-isopropylacrylamide, Nt-butylacrylamide, and N-isopropylmethacrylamide.
[0023] The content ratio of the cyclocarbonate group-containing monomer (A1) and the copolymerizable radical polymerizable monomer (A2) in the monomer components constituting the polymer is 1-100% by mass:0-99% by mass, preferably 30-100% by mass:0-70% by mass, more preferably 50-100% by mass:0-50% by mass, and particularly preferably 70-100% by mass:0-30% by mass, when the total mass of the monomers (A1) and (A2) is taken as 100% by mass. If the amount of the cyclocarbonate group-containing monomer (A1) is too small, the mechanical strength of the elastomer composition may decrease. The monomer component may contain monomers other than the above monomers (A1) and (A2) within the scope that does not impede the achievement of the object of the present invention.
[0024] The particle size of the polymer (A) is 10 to 1000 nm, preferably 50 to 700 nm, more preferably 100 to 500 nm, and particularly preferably 200 to 400 nm. If the particle size is too small, it may be difficult to disperse uniformly, resulting in a decrease in mechanical strength, while if the particle size is too large, the smoothness may decrease, resulting in a decrease in adhesion. The particle size of the polymer (A) can be adjusted by the amount of surfactant added during polymerization. The particle diameter of the polymer (A) is the average particle diameter Dh measured in water at 25° C. by the cumulant method using a particle size measuring device (Zetasizer Nano S, manufactured by Malvern Instruments).
[0025] [Elastomer (B)] The elastomer (B) is a polymer obtained by polymerizing a monomer component, and can be obtained, for example, by polymerizing a monomer component containing at least one selected from the group consisting of an ethylenically unsaturated compound (B1), a conjugated diene compound (B2), and a vinyl aromatic monomer (B3).
[0026] Ethylenically unsaturated compounds (B1) Examples of the ethylenically unsaturated compound (B1) include (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, and one or more of these may be used.
[0027] Examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. Examples of the (meth)acrylic acid alkoxyalkyl ester include methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, methoxypropyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxymethyl acrylate, ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, etc. Among these, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, methoxymethyl (meth)acrylate, etc. are preferred, and methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate are more preferred.
[0028] Conjugated diene compounds (B2) Examples of the conjugated diene compound (B2) include butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 1,3-pentadiene, myrcene, ocimene, and farnacene, and one or more of these may be used.
[0029] Vinyl aromatic compounds (B3) Examples of the vinyl aromatic compound (B3) include styrene, α-methylstyrene, p-methylstyrene, m-methylstyrene, o-methylstyrene, p-ethylstyrene, m-ethylstyrene, o-ethylstyrene, t-butylstyrene, chlorostyrene, hydroxystyrene, t-butoxystyrene, vinyltoluene, vinylnaphthalene, etc., and one or more of these are used. As the vinyl aromatic compound (B3), styrene is preferred.
[0030] The content ratio of each monomer (B1), (B2), and (B3) in the monomer components constituting the polymer is not particularly limited, but when the total mass of the monomers (B1), (B2), and (B3) is taken as 100 mass%, for example, the monomer (B1):monomer (B2):monomer (B3) is 50-100 mass%:0-50 mass:0-50 mass, preferably 60-100 mass%:0-40 mass:0-40 mass, more preferably 70-100 mass%:0-30 mass:0-30 mass, and particularly preferably 80-100 mass%:0-20 mass:0-20 mass. If the amount of the ethylenically unsaturated compound (B1) is relatively too small, flexibility may decrease.
[0031] The elastomer (B) may have a structure derived from a crosslinking agent, and the above monomer component may contain a crosslinking agent as a fourth monomer (B4). The crosslinking agent is not particularly limited, and any crosslinking agent containing two or more radical polymerizable groups in one molecule can be used. For example, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane ethoxylate tri(meth)acrylate, trimethylolpropane propoxylate tri(meth)acrylate, divinylbenzene, polyester di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol ethoxylate tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate can be used alone or in combination. From the viewpoint of polymerizability and strength of the elastomer, ethylene glycol dimethacrylate is preferred. The content of the crosslinking agent in the monomer components is not particularly limited, but is preferably 0.01 to 10 mass%, more preferably 0.05 to 5 mass%, and particularly preferably 0.1 to 1 mass%, assuming that the total mass of the monomers (B1), (B2), (B3), and (B4) is 100 mass%.
[0032] The particle size of the elastomer (B) is preferably 10 to 1000 nm, more preferably 50 to 700 nm, particularly preferably 100 to 500 nm, and even more preferably 120 to 200 nm. If the particle size is too small, the viscosity may increase, resulting in a decrease in moldability and dispersibility of the polymer particles, while if the particle size is too large, the smoothness may decrease, resulting in a decrease in adhesion. The particle size of the elastomer (B) can be adjusted by the amount of surfactant added during polymerization. The particle diameter of the elastomer (B) is the average particle diameter Dh measured in water at 25° C. by the cumulant method using a particle size measuring device (Zetasizer Nano S, manufactured by Malvern Instruments).
[0033] The polymer (A) and the elastomer (B) can each be produced by a known method, for example, emulsion polymerization.
[0034] Water is generally used as the medium used in emulsion polymerization, but other media or a mixture of water and other media can also be used. The other media other than water are not particularly limited, but for example, ethanol, n-propanol, isopropanol, n-butanol, tert-butanol, tetrahydrofuran, dioxane, ethylene glycol, glycerin, ethylene glycol monoethyl ether, acetone, acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylethanolamine, N,N-diethylethanolamine, monoethanolamine, diethanolamine, triethanolamine, morpholine, pyridine, etc. are listed, and one or more of these are used.
[0035] In the emulsion polymerization, the polymerization initiator used for the purpose of polymerizing the vinyl monomer is not particularly limited, and known azo compounds and peroxides can be used. Examples of azo compounds include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,3-dimethylbutyronitrile), 2,2'-azobis-(2-methylbutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,3,3-trimethylbutyronitrile), 2,2'-azobis(2,3,3-trimethylbutyronitrile), Examples of the azobis[N-(2-hydroxyethyl)-2-methylpropanamide], 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]tetrahydrate, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, etc., can be mentioned, and one or more of these can be used.
[0036] Examples of peroxides include di-tert-butyl peroxide, dicumyl peroxide, tert-butyl hydroperoxide, tert-butylcumyl peroxide, benzoyl peroxide, dilauryl peroxide, cumene hydroperoxide, tert-butyl peroxybenzoate, ethyl ethyl ketone peroxide, di-tert-butyl diperphthalate, cyclohexanone peroxide, diisopropylbenzene hydroperoxide, peracetic acid, sodium persulfate, potassium persulfate, and ammonium persulfate. One or more of these may be used.
[0037] In the polymerization of a vinyl monomer, the method of adding the vinyl monomer and the polymerization initiator is not particularly limited, and they may be added all at once, or may be added in several divided portions, or may be added dropwise. The polymerization atmosphere for the vinyl monomer is not particularly limited, but from the viewpoint of suppressing polymerization inhibition due to oxygen, an inert gas atmosphere such as nitrogen is preferable. The polymerization temperature of the vinyl monomer is preferably 30 to 160° C., more preferably 50 to 100° C. If the polymerization temperature is too low, the polymerization rate may decrease, which is not preferable from the viewpoint of productivity. If the polymerization temperature is too high, the molecular weight of the resulting vinyl polymer tends to be small, which may result in a decrease in the strength of the resulting polymer.
[0038] During the emulsion polymerization, a surfactant and / or a dispersion stabilizer can also be used. The method of using a surfactant and a dispersion stabilizer includes, for example, a method of including both in an aqueous dispersion, and a method of chemically bonding a surfactant or a dispersion stabilizer to a resin. The mode of bonding between the surfactant and the resin is not particularly limited, but for example, a mode in which a so-called reactive surfactant having an unsaturated bond capable of radical polymerization in the molecule is copolymerized with a resin by radical polymerization, etc. In addition, the mode of bonding between the dispersion stabilizer and the resin is also not particularly limited, but for example, a mode in which a dispersion stabilizer is graft-copolymerized with a resin, etc. are included.
[0039] Examples of the surfactant that can be used during emulsion polymerization include anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants.
[0040] Examples of the anionic surfactant include alkyl sulfate salts such as sodium dodecyl sulfate, polyoxyethylene alkyl ether sulfate salts, alkyl benzene sulfonates, alkyl naphthalene sulfonates, alkyl sulfosuccinates, alkyl diphenyl ether disulfonates, naphthalene sulfonate-formaldehyde condensates, polyoxyethylene polycyclic phenyl ether sulfate salts, polyoxyethylene distyrenated phenyl ether sulfate salts, fatty acid salts, alkyl phosphates, and polyoxyethylene alkyl phenyl ether sulfate salts. One or more of these may be used.
[0041] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyalkylene alkyl ethers, polyoxyethylene polycyclic phenyl ethers, polyoxyethylene distyrenated phenyl ethers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene alkylamines, alkyl alkanolamides, polyoxyethylene alkyl phenyl ethers, and the like. One or more of these may be used.
[0042] Examples of the cationic surfactant include quaternary ammonium salts such as alkyltrimethylammonium bromide, alkylpyridinium bromide, imidazolinium laurate, pyridinium salts, imidazolinium salts, etc., and one or more of these may be used.
[0043] Examples of amphoteric surfactants include lauryl betaine, lauryl dimethylamine oxide, etc., and one or more of these may be used.
[0044] The surfactant that can be used during emulsion polymerization is preferably an anionic surfactant or a nonionic surfactant, more preferably an anionic surfactant, and particularly preferably an alkyl sulfate such as sodium dodecyl sulfate.
[0045] The dispersion stabilizer is not particularly limited, but examples thereof include polyether, polyvinyl alcohol, polyvinylpyrrolidone, poly(vinylpyrrolidone-vinyl acetate) copolymer, polyacrylic acid, starch, gum arabic, gum tragacanth, casein, gelatin, dextrin, carboxylated starch, cationized starch, dextrin, ethyl cellulose, carboxylated methyl cellulose, hydroxyethyl cellulose, cationized cellulose, and the like, and one or more of these may be used.
[0046] The polymer (A) and elastomer (B) obtained by emulsion polymerization may be subjected to centrifugal purification or dialysis, if necessary, to remove unreacted residual monomers and surfactants, and may further be subjected to concentration or drying after removing the medium.
[0047] [Preparation of Elastomer Composition] The elastomer composition of the present invention contains a polymer (A) and an elastomer (B). When the total mass of the polymer (A) and the elastomer (B) is taken as 100 mass%, the content ratio of the polymer (A):elastomer (B) is 1 to 90 mass%:10 to 99 mass, preferably 5 to 60 mass%:40 to 95 mass, and more preferably 10 to 50 mass%:50 to 90 mass. If the amount of polymer (A) is relatively too large, the elongation may decrease, whereas if the amount of elastomer (B) is relatively too large, the mechanical strength may decrease.
[0048] The elastomer composition of the present invention is prepared by mixing the dispersions of the polymer (A) and the elastomer (B) in the above-mentioned ratio, and if necessary, the pH is adjusted with a 100 mM aqueous sodium hydroxide solution or the like.
[0049] The elastomer composition of the present invention can be placed in a mold having a desired shape and dried to obtain a molded product. The shape of the molded product is not particularly limited, and examples thereof include a sheet, a film, a hollow body, a block body, a plate-like body, a cylinder, a complex-shaped body, a foam, and the like.
[0050] The molded article obtained from the elastomer composition of the present invention has both good mechanical properties and a small specific gravity, and can be used for a wide variety of products and semi-finished products in a wide range of fields, such as automobile parts, electrical appliances, building materials, and miscellaneous goods. EXAMPLES
[0051] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.
[0052] Table 1 shows the content (mass%) of each monomer in the monomer components constituting the polymer (A) used in the examples and comparative examples, and the particle size of the polymer (A). Table 2 shows the content (mass%) of each monomer in the monomer components constituting the elastomer (B) used in the examples and comparative examples, and the particle size of the elastomer (B). The abbreviations in Tables 1 and 2 are as follows. DOMA: (2-oxo-1,3-dioxolan-4-yl)-methyl methacrylate (R 1 is a methyl group, and X is 0. MMA: Methyl methacrylate MEA: Methoxyethyl acrylate
[0053] (Production method of polymer (A-1)) DOMA (5.6 g) and ion-exchanged water (24 g) were added to a four-necked round-bottom flask (50 mL) and placed in an oil bath set at 70 °C. A reflux condenser was attached, and the solution was stirred (250 rpm) with a glass stirrer while bubbling with nitrogen for 30 minutes to remove dissolved oxygen. After switching to nitrogen flow, sodium dodecyl sulfate dissolved in ion-exchanged water (5 g) was added, and the solution was stirred for 5 minutes to maintain thermal equilibrium. Then, potassium persulfate (0.016 g) dissolved in ion-exchanged water (1 g) was added to initiate the polymerization reaction. The nitrogen flow was stopped one hour after the start of polymerization, and the dispersion obtained after 24 hours was collected in a sample tube. The sample tube containing the dispersion was quenched with tap water to terminate the polymerization. After that, centrifugal purification and dialysis were performed to remove residual monomers and surfactants, and an aqueous dispersion of polymer microparticles (A-1) was obtained.
[0054] (Production method of polymers (A-2) to (A-6)) Similarly to the polymer (A-1), the monomer components were polymerized in the proportions shown in Table 1 to obtain aqueous dispersions of polymers (A-2) to (A-6).
[0055] [Table 1]
[0056] (Production method of elastomer (B-1)) Ion-exchanged water (95 g) was added to a four-necked round-bottom flask (400 mL) and placed in an oil bath set at 70°C. A reflux condenser was attached, and the solution was stirred (300 rpm) with a glass stirrer while bubbling with nitrogen for 30 minutes to remove dissolved oxygen from the solution. After switching to nitrogen flow, methoxyethyl acrylate (19.5015 g, 99.9 mass%), ethylene glycol dimethacrylate (0.0297 g, 0.1 mass%), and sodium dodecylbenzenesulfonate (0.0348 g, 1 mM) dissolved in ion-exchanged water (2 g) were added, and the flask was allowed to thermally equilibrate for 5 minutes. Then, potassium persulfate (0.0541 g) dissolved in ion-exchanged water (3 g) was added to start the polymerization reaction. The nitrogen flow was stopped one hour after the start of polymerization, and the dispersion obtained after 12 hours was collected in a sample tube. The sample tube containing the dispersion was quenched with tap water to stop the polymerization. After that, the remaining monomers and surfactants were removed by dialysis, and an aqueous dispersion of elastomer (B-1) was obtained.
[0057] (Production method of elastomer (B-2)) Similarly to the elastomer (B-1), the monomer components were polymerized in the content ratios shown in Table 2 to obtain an aqueous dispersion of elastomer (B-2).
[0058] [Table 2]
[0059] (Evaluation of particle size by dynamic light scattering (DLS)) The hydrodynamic diameter (Dh) of all microparticles was determined by dynamic light scattering (DLS) measurement (Malvern, Zetasizer Nano S). The concentration of all dispersions was approximately 0.005% by mass, and the NaCl concentration was adjusted to 1 mM, and measurements were performed at 25°C. The diameter of the microparticles was calculated from the measured diffusion coefficient using the Stokes-Einstein equation (Zetasizer software ver.8.02). Before measurement, an equilibration time of 300 seconds was allowed to elevate the sample solution temperature to a uniform temperature.
[0060] (Preparation of filled elastomers and measurement of their mechanical properties) Each aqueous dispersion of fine particles of elastomers (B-1) and (B-2) was adjusted to a neutral condition of pH 7 with a 100 mM aqueous sodium hydroxide solution. Then, polymers (A-1) to (A-6) were mixed at the weight fractions (mass %, solid content equivalent) shown in Tables 3 and 4. After mixing several times with a pipetter, the solution was poured into a 3.5 cm square silicon sheet and dried in an incubator set at 25°C. At this time, the solid weight of the film was 48 mg / cm. 3The amount of the dispersion liquid poured into the mold was adjusted so as to obtain the following: After drying for 72 hours, the pieces were cut into JIS No. 7 dumbbell pieces and subjected to uniaxial extension tests at a pulling speed of 1000 mm / min using a Tensilon tensile testing machine (STB-1225L, manufactured by A&D Co., Ltd., equipped with a 50N load cell) to calculate the strength and elongation. In addition, "Silica" in Table 4 is "Snowtex (registered trademark)-YL" manufactured by Nissan Chemical Industries, Ltd. (particle size according to the BET method: 60 nm).
[0061] [Table 3]
[0062] [Table 4]
[0063] The evaluation criteria in Tables 3 and 4 are as follows: Strength (MPa): △ (unacceptable) less than 2.0, ○ (acceptable) 2.0 or more, less than 5.0, ◎ (good) 5.0 or more Elongation (%): △ (unacceptable) less than 400, ○ (acceptable) 400 or more, less than 650, ◎ (good) 650 or more Specific gravity: △ (unacceptable) over 1.0, ○ (acceptable / good) 1.0 or less
[0064] As shown in Table 3, the filler-containing elastomer obtained from the elastomer composition satisfying the requirements of the present invention not only has good mechanical properties such as strength and elongation, but also can suppress an increase in specific gravity. On the other hand, as shown in Table 4, Comparative Example 1, which did not use the polymer (A) of the present invention, and Comparative Example 2, which did not use the cyclocarbonate group-containing monomer (A1) of the present invention, had insufficient strength. Also, Comparative Examples 3 and 4, which used silica as a filler, had high specific gravity even though they had good mechanical properties.
Claims
[Claim 1] The polymer (A) has a particle size of 10 to 1000 nm, and the elastomer (B) is contained in an amount of 1 to 90% by mass. The polymer (A) is an elastomer composition obtained by polymerizing monomer components containing 1 to 100 mass % of a cyclocarbonate group-containing monomer (A1) represented by the following formula (1) or formula (2) and 0 to 99 mass % of a copolymerizable radically polymerizable monomer (A2): [Formula 1] (In formula (1) and formula (2), R 1 represents a hydrogen atom or a methyl group, A represents an alkylene group having 1 to 10 carbon atoms, and X represents 0 or 1.
Citation Information
Patent Citations
Nitrile rubber composition and rubber crosslinked product
JP2020143251A