Heat-curable composition, composition for fixing semiconductor element, and cured product
By using silicone-modified particles in a thermosetting composition with a silane compound polymer, thixotropy and coating properties are enhanced, addressing the challenge of poor performance in low-solvent curable compositions, resulting in improved semiconductor element fixation.
Patent Information
- Application Number
- JP2023047645
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Thixotropy cannot be effectively controlled in curable compositions containing silane compound polymers that are liquid at room temperature and have a low solvent content, leading to poor coating properties.
Incorporating silicone-modified particles into a thermosetting composition containing a silane compound polymer that is liquid at room temperature, which improves thixotropy and coating properties without the need for solvents.
The composition achieves excellent thixotropy and coating properties, enabling efficient application and curing of semiconductor elements with improved adhesive strength and transparency.
Smart Images

Figure 2024136509000001 
Figure 2024136509000002 
Figure 2024136509000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting composition, a composition for fixing a semiconductor element, and a cured product. [Background technology]
[0002] 2. Description of the Related Art Curable compositions have been improved in various ways depending on the intended use, and have come to be widely used industrially as raw materials for optical parts and molded articles, adhesives, coating agents, and the like. Furthermore, in recent years, curable compositions containing polysilsesquioxane compounds have been attracting attention because they form cured products that are excellent in heat resistance, transparency, and the like.
[0003] For example, Patent Documents 1 to 3 describe curable compositions containing a polysilsesquioxane compound and the use of the curable compositions as sealing materials.
[0004] When the curable component of the curable composition is a polysilsesquioxane compound that is solid at room temperature, a solvent is usually added to the curable composition in order to improve the coatability of the curable composition. However, in recent years, from the viewpoint of reducing the environmental load, etc., it is desired to reduce the amount of solvent in a curable composition or to eliminate the solvent. For this reason, various studies have been conducted so far in order to synthesize a polysilsesquioxane compound that is liquid at room temperature.
[0005] For example, Patent Document 4 describes a condensation reaction type silicone composition that contains polysilsesquioxane that is liquid at room temperature. In Production Examples 1 and 2 of Patent Document 4, methyltrimethoxysilane is used as a monomer to produce polysilsesquioxane that is liquid at room temperature. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2004-359933 A [Patent Document 2] JP 2005-263869 A [Patent Document 3] JP 2006-328231 A [Patent Document 4] WO2017 / 122762 issue Summary of the Invention [Problem to be solved by the invention]
[0007] As described above, Patent Document 4 describes a silane compound polymer that is liquid at room temperature. However, as a result of investigations by the present inventors, it was found that it is difficult to control thixotropy in a curable composition that uses a silane compound polymer that is liquid at room temperature as a curable component and does not contain a solvent or has a small solvent content. That is, in the past, the thixotropy of a curable composition has been improved by adding a filler to the curable composition, but when a filler is added to a curable composition that does not contain a solvent or has a low solvent content, the thixotropy is hardly improved or the viscosity becomes too high, resulting in poor applicability.
[0008] The present invention has been made with the aim of solving this problem, and aims to provide a thermosetting composition containing a silane compound polymer that is liquid at room temperature and has excellent thixotropy and coatability, a composition for fixing semiconductor elements comprising this thermosetting composition, and a cured product obtained by curing the thermosetting composition. In the present invention, the term "liquid at room temperature" refers to a substance that has fluidity at 25°C. The term "thermosetting" refers to a property that can be cured by heating alone, even in the absence of a curing catalyst. [Means for solving the problem]
[0009] In order to solve the above problems, the present inventors have conducted extensive research into a thermosetting composition that contains a silane compound polymer that is liquid at room temperature and a filler, and that does not contain a solvent or contains a small amount of solvent. As a result, the inventors have found that by using silicone-modified particles as a filler, it is possible to efficiently control the thixotropy of a thermosetting composition that contains a silane compound polymer that is liquid at room temperature and does not contain a solvent or has a small solvent content, and have completed the present invention.
[0010] Thus, according to the present invention, there are provided the following thermosetting compositions [1] to
[16] , a semiconductor element fixing composition
[17] , and a cured product
[18] .
[0011] [1] A thermosetting composition comprising the following component (A) and component (Bi): Component (A): a silane compound polymer that is liquid at 25°C (Bi) component: silicone-modified particles [2] The thermosetting composition according to [1], wherein the component (A) is a silane compound polymer having a viscosity of 15,000 Pa·s or less at 25°C. [3] The thermosetting composition according to [1] or [2], wherein the component (A) is a silane compound polymer having an alkoxy group. [4] The thermosetting composition according to any one of [1] to [3], wherein the component (A) is a silane compound polymer obtained by hydrolysis and polycondensation of an alkoxysilane compound. [5] The thermosetting composition according to any one of [1] to [4], wherein the component (A) is a silane compound polymer having a residual alkoxy group rate of 25% or less. [6] The thermosetting composition according to any one of [1] to [5], wherein the component (A) is a silane compound polymer having thermosetting properties. [7] The thermosetting composition according to any one of [1] to [6], wherein the component (A) is a silane compound polymer having a mass average molecular weight (Mw) of 500 to 20,000. [8] The component (A) is represented by the following formula (a-1):
[0012] [ka]
[0013] (Me represents a methyl group.) The repeating unit (1) has the following repeating unit: The following formula (a-2)
[0014] [ka]
[0015] [R 1 represents a group selected from the group consisting of an unsubstituted alkyl group having 2 to 10 carbon atoms, a substituted alkyl group having 1 to 10 carbon atoms, an unsubstituted aryl group having 6 to 12 carbon atoms, and a substituted aryl group having 6 to 12 carbon atoms. The thermosetting composition according to any one of [1] to [7], which is a silane compound polymer having or not having a repeating unit represented by the following formula (2): [9] The thermosetting composition according to [8], wherein the amount of the repeating unit (1) contained in the silane compound polymer is 70 to 100 mol % based on the total amount of the repeating unit (1) and the repeating unit (2).
[10] The thermosetting composition according to [8] or [9], wherein the total amount of the repeating unit (1) and the repeating unit (2) in the silane compound polymer is 80 to 100 mol % of all repeating units in the silane compound polymer.
[11] The thermosetting composition according to any one of [1] to
[10] , wherein the silane compound polymer has a T1 site represented by the following formula (a-3), a T2 site represented by the following formula (a-4), and a T3 site represented by the following formula (a-5), and the amount of the T1 site is 2.5 to 25 mol % based on the total amount of the T1 site, the T2 site, and the T3 site.
[0016] [ka]
[0017] [R 2represents a group selected from the group consisting of an unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted alkyl group having 1 to 10 carbon atoms, an unsubstituted aryl group having 6 to 12 carbon atoms, and a substituted aryl group having 6 to 12 carbon atoms. 1 ~X 3 each independently represents a hydrogen atom or an alkyl group. * represents a bond to another repeating unit and is directly bonded to a silicon atom of another repeating unit.
[12] The thermosetting composition according to any one of [1] to
[11] , wherein the silane compound polymer is a silane compound polymer in which an amount of T1 sites having an alkoxy group is 20 to 60 mol % of the total T1 sites.
[13] The thermosetting composition according to any one of [1] to
[12] , wherein the average particle size of the component (Bi) is 1 to 40 nm.
[14] The thermosetting composition according to any one of [1] to
[13] , wherein the component (Bi) is a silicone-modified silica particle.
[15] The thermosetting composition according to any one of [1] to
[14] , wherein the content of the (Bi) component is 0.1 to 50 parts by mass per 100 parts by mass of the (A) component.
[16] The thermosetting composition according to any one of [1] to
[15] , which may or may not contain a solvent, and in which the content of the solvent is 40 mass% or less based on the total amount of the thermosetting composition.
[17] A composition for fixing a semiconductor element, comprising the thermosetting composition according to any one of [1] to
[16] above.
[18] A cured product obtained by curing the thermosetting composition according to any one of [1] to
[16] above. Effect of the Invention
[0018] According to the present invention, there are provided a thermosetting composition containing a silane compound polymer that is liquid at room temperature and has excellent thixotropy and coatability, a composition for fixing a semiconductor element comprising this thermosetting composition, and a cured product obtained by curing the thermosetting composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] In this specification, the lower limit and upper limit described in stages for the preferred numerical range (e.g., range of content, etc.) can be independently combined. For example, the description "preferably 10 to 90, more preferably 30 to 60" can be combined with the "preferable lower limit (10)" and the "more preferable upper limit (60)" to form "10 to 60."
[0020] The present invention will be described in detail below, divided into two sections: 1) a thermosetting composition, and 2) a cured product.
[0021] 1) Thermosetting composition The thermosetting composition of the present invention is a thermosetting composition containing the following component (A) and component (Bi). Component (A): a silane compound polymer that is liquid at 25°C (Bi) component: silicone-modified particles
[0022] [Component (A): a silane compound polymer that is liquid at 25°C] The component (A) constituting the thermosetting composition of the present invention is a silane compound polymer that is liquid at 25°C. Since the thermosetting composition of the present invention contains the component (A), it has excellent coatability.
[0023] [Physical properties and structure of component (A)] The component (A) is preferably a silane compound polymer having a viscosity at 25°C of 15,000 Pa·s or less. When the viscosity of component (A) at 25°C is 15,000 Pa·s or less, a thermosetting composition with excellent coatability is more easily obtained. For the same reasons, the viscosity of component (A) at 25°C is more preferably 4,000 Pa·s or less, even more preferably 1,000 Pa·s or less, even more preferably 500 Pa·s or less, and even more preferably 300 Pa·s or less. There is no particular lower limit for the viscosity of component (A) at 25°C, but it is usually at least 0.3 Pa·s. Therefore, the component (A) is preferably a silane compound polymer having a viscosity at 25°C of 0.3 to 15,000 Pa·s.
[0024] In this specification, the "viscosity at 25°C" of component (A) refers to the viscosity at a shear rate of 2.2 s using a cone plate with a cone radius (radius of the cone base) of 12.5 mm and a cone angle of 0.5 degree. -1 However, if the viscosity exceeds 50 Pa s in this measurement, "viscosity at 25°C" refers to the viscosity measured using parallel plates with a radius of 12.5 mm and at an angular frequency of 2.0 rad / s.
[0025] The component (A) is preferably a silane compound polymer having an alkoxy group. Since a silane compound polymer having an alkoxy group tends to be liquid at room temperature, the silane compound polymer having an alkoxy group is suitable as component (A).
[0026] The silane compound polymer having an alkoxy group can be obtained, for example, by hydrolysis and polycondensation of an alkoxysilane compound according to a conventional method (hereinafter, the component (A) obtained by this method may be referred to as the "silane compound polymer (Ai)"). The silane compound polymer (Ai) is preferably a silane compound polymer having a residual alkoxy group ratio of 25% or less.
[0027] The residual alkoxy group rate of the silane compound polymer (A-i) represents the degree to which the alkoxy group contained in the alkoxysilane compound used as a monomer remains in the silane compound polymer (Ai). The silane compound polymer (Ai) having an alkoxy group residual rate of 25% or less is a polymer in which the hydrolysis reaction of the alkoxysilane compound has progressed sufficiently, and contains a large number of Si-O-Si bonds and Si-OH bonds. Such a silane compound polymer (Ai) is a relatively large molecule and has reactivity, so that it is suitable as a curable component of a thermosetting composition. For the same reason, the residual alkoxy group ratio of the silane compound polymer (Ai) is more preferably 20% or less, further preferably 15% or less, and even more preferably 10% or less. In addition, since the silane compound polymer (Ai) easily becomes liquid at room temperature, the residual alkoxy group rate of the silane compound polymer (Ai) is preferably 2.5% or more, more preferably 3.5% or more, and even more preferably 4.5% or more. Therefore, the residual alkoxy group rate of the silane compound polymer (Ai) is preferably from 2.5 to 25%.
[0028] The residual alkoxy group rate of the silane compound polymer (Ai) 1 For example, when a silane compound polymer (Ai) is synthesized using methyltriethoxysilane, the silane compound polymer (Ai) 1 The residual alkoxy group ratio of the silane compound polymer (Ai) can be calculated by measuring H-NMR and determining the ratio of methyl groups to ethoxy groups based on the peak area ratio. Incidentally, the silane compound polymer (Ai) is usually soluble in various organic solvents such as ketone solvents such as acetone; aromatic hydrocarbon solvents such as benzene; sulfur-containing solvents such as dimethyl sulfoxide; ether solvents such as tetrahydrofuran; ester solvents such as ethyl acetate; halogen-containing solvents such as chloroform; and mixed solvents consisting of two or more of these. Therefore, NMR of the silane compound polymer (Ai) in a solution state can be measured using these solvents.
[0029] The component (A) is preferably a silane compound polymer having thermosetting properties. The component (A) having thermosetting properties is suitable as a curable component in a thermosetting composition. As described above, a silane compound polymer containing a Si-OH bond tends to have thermosetting properties. Therefore, an example of a silane compound polymer having thermosetting properties is a silane compound polymer (Ai) having an alkoxy group residual rate of 25% or less.
[0030] The component (A) is preferably a silane compound polymer having a mass average molecular weight (Mw) of 500 to 20,000. Thermosetting compositions in which the mass average molecular weight (Mw) of the component (A) is not too large tend to have excellent coatability. For the same reasons, the mass average molecular weight (Mw) of the component (A) is preferably 10,000 or less, more preferably 8,000 or less, and even more preferably 5,000 or less. A thermosetting composition in which the mass average molecular weight (Mw) of the component (A) is not too small tends to cure in a relatively short time. For the same reason, the mass average molecular weight (Mw) of the component (A) is preferably 600 or more, and more preferably 700 or more. There are no particular limitations on the molecular weight distribution (Mw / Mn) of the component (A), but it is usually from 1.00 to 10.00, preferably from 1.10 to 6.00, and more preferably from 1.15 to 4.00.
[0031] The mass average molecular weight (Mw) and number average molecular weight (Mn) can be determined, for example, as a polystyrene-equivalent value by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent.
[0032] When the silane compound polymer of component (A) is a copolymer, the silane compound polymer of component (A) may be any of a random copolymer, a block copolymer, a graft copolymer, an alternating copolymer, etc., but from the viewpoint of ease of production, etc., a random copolymer is preferred. The structure of the silane compound polymer of component (A) may be any of a ladder structure, a double-decker structure, a cage structure, a partially cleaved cage structure, a cyclic structure, and a random structure.
[0033] The component (A) is represented by the following formula (a-1):
[0034] [ka]
[0035] (Me represents a methyl group.) The repeating unit (1) has the following repeating unit: The following formula (a-2)
[0036] [ka]
[0037] [R 1 represents a group selected from the group consisting of an unsubstituted alkyl group having 2 to 10 carbon atoms, a substituted alkyl group having 1 to 10 carbon atoms, an unsubstituted aryl group having 6 to 12 carbon atoms, and a substituted aryl group having 6 to 12 carbon atoms. Hereinafter, this silane compound polymer may be referred to as "silane compound polymer (A-ii)."
[0038] R 1 The "unsubstituted alkyl group having 2 to 10 carbon atoms" represented by the following formula (I) preferably has 2 to 6 carbon atoms, and more preferably has 2 to 3 carbon atoms. Examples of the "unsubstituted alkyl group having 2 to 10 carbon atoms" include an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a s-butyl group, a t-butyl group, an n-pentyl group, an n-hexyl group, an n-octyl group, an n-nonyl group, and an n-decyl group.
[0039] R 1 The number of carbon atoms in the "alkyl group having 1 to 10 carbon atoms and a substituent" represented by the formula (I) is preferably 1 to 6, and more preferably 1 to 3. Note that this carbon number refers to the number of carbon atoms in the portion excluding the substituent (the alkyl group portion). Therefore, R 1 is a "substituted alkyl group having 1 to 10 carbon atoms", R 1 The number of carbon atoms may exceed 10. Examples of the alkyl group in the "substituted alkyl group having 1 to 10 carbon atoms" include a methyl group and the same groups as those given as the "unsubstituted alkyl group having 2 to 10 carbon atoms".
[0040] The number of atoms of the substituent in the "substituted alkyl group having 1 to 10 carbon atoms" (excluding the number of hydrogen atoms) is usually 1 to 30, and preferably 1 to 20. Examples of the substituent in the "substituted alkyl group having 1 to 10 carbon atoms" include halogen atoms such as a fluorine atom, a chlorine atom, and a bromine atom; and aryl groups such as a phenyl group.
[0041] R 1 The number of carbon atoms in the "unsubstituted aryl group having 6 to 12 carbon atoms" represented by the following formula is preferably 6. Examples of the "unsubstituted aryl group having 6 to 12 carbon atoms" include a phenyl group, a 1-naphthyl group, and a 2-naphthyl group.
[0042] R 1 The number of carbon atoms in the "aryl group having 6 to 12 carbon atoms and having a substituent" represented by the formula (I) is preferably 6. Note that this number of carbon atoms refers to the number of carbon atoms in the portion excluding the substituent (the aryl group portion). Therefore, R 1 is a "substituted aryl group having 6 to 12 carbon atoms", R 1 The number of carbon atoms may exceed 12. Examples of the aryl group in the "substituted aryl group having 6 to 12 carbon atoms" include the same groups as those exemplified as the "unsubstituted aryl group having 6 to 12 carbon atoms".
[0043] The number of atoms of the substituent in the "substituted aryl group having 6 to 12 carbon atoms" (excluding the number of hydrogen atoms) is usually 1 to 30, and preferably 1 to 20. Examples of the substituent in the "substituted aryl group having 6 to 12 carbon atoms" include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, s-butyl, isobutyl, t-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, and isooctyl; halogen atoms such as fluorine, chlorine, and bromine; and alkoxy groups such as methoxy and ethoxy.
[0044] Among these, R 1As the alkyl group, an unsubstituted alkyl group having 2 to 10 carbon atoms or an unsubstituted aryl group having 6 to 12 carbon atoms is preferable.
[0045] When the silane compound polymer (A-ii) has a repeating unit (2), the silane compound polymer (A-ii) has one kind of R 1 or may have two or more R 1 The present invention may also have the following structure.
[0046] The amount of the repeating unit (1) contained in the silane compound polymer (A-ii) is preferably 70 to 100 mol % based on the total amount of the repeating unit (1) and the repeating unit (2). When the amount of the repeating unit (1) is 70 mol % or more, the silane compound polymer (A-ii) has good curability, and the cured product thereof tends to have both suppressed cracking and high adhesive strength. For the same reason, the amount of repeating unit (1) relative to the total amount of repeating unit (1) and repeating unit (2) is more preferably 80 to 100 mol %, further preferably 90 to 100 mol %, and particularly preferably 95 to 100 mol %.
[0047] The total amount of the repeating units (1) and (2) in the silane compound polymer (A-ii) is preferably 80 to 100 mol % of all repeating units in the silane compound polymer (A-ii). A silane compound polymer (A-ii) in which the total amount of the repeating units (1) and (2) is 80 mol % or more of all the repeating units tends to be liquid at room temperature and to have thermosetting properties. For the same reason, the total amount of the repeating units (1) and (2) is more preferably from 85 to 100 mol %, and even more preferably from 90 to 100 mol %, of all the repeating units.
[0048] When the silane compound polymer (A-ii) has a repeating unit other than the repeating unit (1) or the repeating unit (2), examples of the repeating unit other than the repeating unit (1) or the repeating unit (2) include a repeating unit derived from a monofunctional silane compound such as trimethylmethoxysilane, a repeating unit derived from a difunctional silane compound such as dimethyldimethoxysilane, a repeating unit derived from a trifunctional silane compound (excluding the repeating unit (1) and the repeating unit (2)), and a repeating unit derived from a tetrafunctional silane compound such as tetramethoxysilane.
[0049] The repeating unit (1) and the repeating unit (2) described above are represented by the following formula (a-6).
[0050] [ka]
[0051] In formula (a-6), R 2 is a methyl group or R 1 It represents a group represented by the formula: O 1 / 2 indicates that the oxygen atom is shared with the adjacent repeat unit.
[0052] As shown in formula (a-6), the silane compound polymer (A-ii) has a silicon atom to which three oxygen atoms are bonded, which is generally collectively called a T site, and the other groups (R 2 The compound has a partial structure in which one Examples of the T site contained in the silane compound polymer (A-ii) include a T1 site represented by the following formula (a-3), a T2 site represented by the following formula (a-4), and a T3 site represented by the following formula (a-5).
[0053] [ka]
[0054] [R 2 is a methyl group or R 1 X represents a group represented by the formula:1 ~X 3 Each of X independently represents a hydrogen atom or an alkyl group. 1 ~X 3 Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. * is a bond to another repeating unit, and is directly bonded to the silicon atom of the other repeating unit.
[0055] As shown in formulas (a-3) to (a-5), the T3 site has three adjacent Si atoms, the T2 site has two adjacent Si atoms, and the T1 site has only one adjacent Si atom. Therefore, the T1 site tends to constitute the terminal part of the silane compound polymer (A-ii) and is an important site when interacting with other molecules. The state (liquid or solid) and thermosetting property of the silane compound polymer (A-ii) are properties expressed as a result of interaction with other molecules. Therefore, the content of T1 sites and the ratio of alkoxy group-containing T1 sites to the total amount of T1 sites, like the residual alkoxy group rate, can be indicators of a silane compound polymer that is liquid at room temperature and has thermosetting property. The content ratios of the T1 site, T2 site, and T3 site are determined by the usual method in the solution state of the silane compound polymer (A-ii). 29 It can be determined by measuring Si-NMR.
[0056] The amount of T1 sites contained in the silane compound polymer (A-ii) is preferably from 2.5 to 25 mol %, more preferably from 2.5 to 15 mol %, based on the total amount of T1 sites, T2 sites and T3 sites. In the silane compound polymer (A-ii), the proportion of alkoxy group-containing T1 sites with respect to the total amount of T1 sites is preferably from 20 to 60 mol %, more preferably from 25 to 50 mol %, of all T1 sites. The ratio of the alkoxy group-containing T1 sites to the total amount of T1 sites can be calculated according to the method described in the Examples.
[0057] [Method for producing component (A)] There are no particular limitations on the method for producing the silane compound polymer of the component (A). For example, the above-mentioned silane compound polymer (A-ii) can be produced by carrying out a step (step PO) of hydrolyzing and polycondensing methyltrialkoxysilane in the presence of water and an acid catalyst, and a step (step PU) of purifying the silane compound polymer obtained in the step PO.
[0058] The step PO is a step of hydrolyzing and polycondensing methyltrialkoxysilane in the presence of water and an acid catalyst.
[0059] In step PO, methyltrialkoxysilane is used as an essential monomer. Examples of the methyltrialkoxysilane include methyltrimethoxysilane, methyltriethoxysilane, and methyltrippropoxysilane.
[0060] In step PO, a trifunctional alkoxysilane compound other than methyltrialkoxysilane may be used as the monomer. An example of a trifunctional alkoxysilane compound other than methyltrialkoxysilane is a trifunctional alkoxysilane compound represented by the following formula (a-7).
[0061] [ka]
[0062] In formula (a-7), R 1 has the same meaning as above. OR represents an alkoxy group. OR may be the same or different.
[0063] The alkoxy group represented by OR preferably has 1 to 6 carbon atoms, and more preferably has 1 to 3 carbon atoms. Examples of the alkoxy group represented by OR include a methoxy group, an ethoxy group, and a propoxy group.
[0064] Specific examples of the trifunctional alkoxysilane compound represented by formula (a-7) include alkyltrialkoxysilane compounds such as ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrippropoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, and n-propyltrippropoxysilane; Substituted alkyltrialkoxysilane compounds such as 3,3,3-trifluoropropyltrimethoxysilane, 3,3,3-trifluoropropyltriethoxysilane, and 3,3,3-trifluoropropyltripropoxysilane; Aryltrialkoxysilane compounds such as phenyltrimethoxysilane, phenyltriethoxysilane, and phenyltripoxysilane; Substituted aryltrialkoxysilane compounds such as 4-methoxyphenyltrimethoxysilane, 4-methoxyphenyltriethoxysilane, and 4-methoxyphenyltrippropoxysilane; and the like. These trifunctional alkoxysilane compounds can be used alone or in combination of two or more.
[0065] The amount of methyltrialkoxysilane is usually 70 to 100 mol %, preferably 80 to 100 mol %, more preferably 90 to 100 mol %, and further preferably 95 to 100 mol %, based on the total amount of the trifunctional alkoxysilane compounds.
[0066] In step PO, in addition to the trifunctional alkoxysilane compound, a monofunctional alkoxysilane compound such as trimethylmethoxysilane, a difunctional alkoxysilane compound such as dimethyldimethoxysilane, or a tetrafunctional alkoxysilane compound such as tetramethoxysilane may be used as a monomer.
[0067] The amount of the trifunctional alkoxysilane compound is preferably 80 to 100 mol %, more preferably 85 to 100 mol %, and further preferably 90 to 100 mol %, based on the total amount of the alkoxysilane compounds. When the amount of the trifunctional alkoxysilane compound is 80 mol % or more based on the total amount of the alkoxysilane compounds, it becomes easier to obtain a silane compound polymer that is liquid at room temperature and has thermosetting properties.
[0068] The amount of water added to the reaction system in the step PO is preferably an amount that gives a molar ratio M of water to alkoxy groups, calculated by the following formula (F1), of 0.46 to 0.86, more preferably an amount that gives a molar ratio M of water to alkoxy groups, calculated by the following formula (F1), of 0.48 to 0.80, and further preferably an amount that gives a molar ratio M of 0.50 to 0.70.
[0069]
number
[0070] In formula (F1), M H2O is the amount of water (molar amount) added to the reaction system, and M OR is the total number of alkoxy groups (total number of moles) in the alkoxysilane compound. For example, when 1 mole of water is added to 1 mole of methyltrialkoxysilane, the value of the molar ratio M is 1 / 3 (approximately 0.33).
[0071] When the molar ratio M is 0.46 to 0.86, it becomes easy to obtain a silane compound polymer which contains an appropriate amount of alkoxy groups, is liquid at room temperature, and has thermosetting properties.
[0072] Examples of the acid catalyst used in step (PO) include inorganic acids such as phosphoric acid, hydrochloric acid, boric acid, sulfuric acid, and nitric acid, and organic acids such as citric acid, acetic acid, methanesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, and p-toluenesulfonic acid. Among these, at least one selected from phosphoric acid, hydrochloric acid, boric acid, sulfuric acid, citric acid, acetic acid, and methanesulfonic acid is preferred.
[0073] The amount of the acid catalyst used is usually 0.05 to 10 mol %, and preferably 0.1 to 5 mol %, based on the total amount of the alkoxysilane compounds.
[0074] Step PO can be carried out, for example, by placing an alkoxysilane compound, water, and an acid catalyst in a reaction vessel and stirring the resulting mixture. In addition to these components, an organic solvent may also be present in the reaction vessel. Examples of the organic solvent include aromatic hydrocarbons such as benzene, toluene, and xylene; esters such as methyl acetate, ethyl acetate, propyl acetate, butyl acetate, and methyl propionate; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, s-butyl alcohol, and t-butyl alcohol; etc. These solvents can be used alone or in combination of two or more. When an organic solvent is used in step PO, the amount of the organic solvent used is preferably 0.05 to 3 times, more preferably 0.1 to 1.5 times, by volume, the amount of the alkoxysilane compound.
[0075] The reaction conditions for step PO are not particularly limited. The reaction temperature in step PO is usually 0 to 85°C, preferably 15 to 75°C. The reaction time in step PO is usually from 30 minutes to 50 hours, preferably from 1 to 24 hours.
[0076] The process PO may be carried out under constant conditions from start to finish (i.e., it may have one step), or it may have multiple steps with different reaction conditions. Since a silane compound polymer having a desired molecular weight can be efficiently produced, the process PO preferably includes a step (step PO-I) of proceeding with hydrolysis of an alkoxysilane compound in the presence of water and an acid catalyst, and a step (step PO-II) of adjusting the molecular weight of the silane compound polymer.
[0077] Step PO-I is a step in which hydrolysis of an alkoxysilane compound proceeds in the presence of water and an acid catalyst. Step PO-I can be carried out, for example, by placing an alkoxysilane compound, water, and an acid catalyst in a reaction vessel and stirring the resulting mixture. In addition to these components, an organic solvent may also be present in the reaction vessel. Examples of the organic solvent include those exemplified above as the organic solvent in step PO. When an organic solvent is used in step PO-I, the organic solvent is preferably used in an amount of 0.05 to 1 time, more preferably 0.1 to 0.5 time, based on volume, relative to the alkoxysilane compound.
[0078] The reaction conditions for Step PO-I are not particularly limited. The reaction temperature in Step PO-I is usually 0 to 50°C, preferably 15 to 35°C. The reaction time for Step PO-I is usually 10 minutes to 2 hours, preferably 15 to 90 minutes.
[0079] It is preferred that the water added for the hydrolysis of the alkoxysilane compound is sufficiently consumed at the end of step PO-I. When methyltriethoxysilane is used as the monomer, the water consumption is about 100% by weight of the reaction product. 1 It can be estimated by measuring H-NMR and comparing the amount of “Si-Me” with the amount of “Si-OEt”. In step PO-I, not only the hydrolysis reaction of the alkoxysilane compound but also the polycondensation reaction may proceed.
[0080] Step PO-II is a step for adjusting the molecular weight of the silane compound polymer. That is, step PO-II is a step in which the polycondensation reaction of the reaction product of step PO-I is advanced in order to produce a silane compound polymer having a target molecular weight.
[0081] In order to adjust the molecular weight of the silane compound polymer, it is preferable to add a base to the reaction system when Step PO-II is carried out, if necessary. By adding a relatively large amount of base, by performing step PO-II at a relatively high temperature, or by extending the reaction time of step PO-II, a silane compound polymer that is liquid at room temperature, has thermosetting properties, and has a relatively large molecular weight tends to be obtained. Also, by adjusting the amount of acid catalyst or the reaction temperature in step PO-I to promote the hydrolysis reaction of the alkoxysilane compound, a silane compound polymer with a large molecular weight tends to be obtained. On the other hand, by adding a relatively small amount of base, performing step PO-II at a relatively low temperature, or shortening the reaction time of step PO-II, a silane compound polymer that is liquid at room temperature, has thermosetting properties, and has a relatively small molecular weight tends to be obtained. Also, by adjusting the amount of acid catalyst and the reaction temperature in step PO-I to allow the hydrolysis reaction of the alkoxysilane compound to proceed in a slightly suppressed manner, a silane compound polymer with a small molecular weight tends to be obtained.
[0082] When a base is added to the reaction system during Step PO-II, the amount of the base added is usually 0.05 to 10 mol %, preferably 0.1 to 5 mol %, based on the total amount of the alkoxysilane compounds. By adding the above amount of base to the reaction system, a silane compound polymer having a desired molecular weight can be efficiently produced.
[0083] Examples of the base include aqueous ammonia; organic bases such as trimethylamine, triethylamine, lithium diisopropylamide, lithium bis(trimethylsilyl)amide, pyridine, 1,8-diazabicyclo[5.4.0]-7-undecene, aniline, picoline, 1,4-diazabicyclo[2.2.2]octane, and imidazole; organic hydroxides such as tetramethylammonium hydroxide and tetraethylammonium hydroxide; metal alkoxides such as sodium methoxide, sodium ethoxide, sodium t-butoxide, and potassium t-butoxide; metal hydroxides such as sodium hydroxide, potassium hydroxide, and calcium hydroxide; metal carbonates such as sodium carbonate, potassium carbonate, and magnesium carbonate; and metal hydrogen carbonates such as sodium hydrogen carbonate and potassium hydrogen carbonate.
[0084] The reaction conditions for Step PO-II are not particularly limited. The reaction temperature in Step PO-II is usually 20 to 85°C, preferably 24 to 70°C. The reaction time for Step PO-II is usually 20 minutes to 48 hours, preferably 1 to 24 hours.
[0085] Step PO-II is preferably carried out with stirring. That is, when the reaction is carried out under conditions in which the molar ratio M of water to alkoxy groups is in the range of 0.46 to 0.86 as described above, even if the added water is completely consumed by hydrolysis, alkoxy groups remain in the reaction product of step PO-I. As described above, the reaction product of step PO-I contains a mixture of highly reactive (Si-OH) and less reactive (Si-OR) groups. Therefore, in order to efficiently carry out the polycondensation reaction of this reaction product and obtain a silane compound polymer of the desired molecular weight, it is preferable to stir the reaction system.
[0086] Step PO-II is preferably carried out in the presence of an organic solvent, which allows the reaction system to be sufficiently stirred and allows the polycondensation reaction of the reaction product of Step PO-I to proceed sufficiently. In addition, since the polycondensation reaction of the reaction product of step PO-I can be carried out under dilute conditions, the molecular weight can be adjusted with good reproducibility.
[0087] Examples of the organic solvent include those exemplified above as the organic solvent in step PO. Therefore, when step PO-I is carried out in the presence of an organic solvent, the organic solvent can be used as is to carry out step PO-II. On the other hand, when step PO-I is carried out in the absence of an organic solvent, step PO-II can be carried out in the presence of an organic solvent by adding an organic solvent to the reaction mixture obtained in step PO-I. When an organic solvent is used in Step PO-II, the organic solvent is preferably used in an amount of 0.05 to 3 times, more preferably 0.1 to 1.5 times, on a volume basis, the amount of the alkoxysilane compound used in Step PO-I.
[0088] It is preferable to carry out Step PO-II in an open system. By carrying out Step PO-II in an open system, water and alcohol, which are products of Step PO, are easily released outside the reaction system, and therefore it is possible to avoid the polycondensation reaction being inhibited by water and alcohol. In addition, when Step PO-II is carried out in the presence of an organic solvent, it is possible to prevent the polycondensation reaction from being excessively pressurized, and therefore it is possible to safely proceed with the polycondensation reaction. An open system is a system in which the reaction system and the surrounding system are not completely isolated and molecules can move between them.
[0089] [Process PU] The step PU is a step of purifying the obtained silane compound polymer. By carrying out the step PU, a high-purity silane compound polymer can be obtained. Such a silane compound polymer is more suitable as a curable component of a thermosetting composition such as a semiconductor element fixing composition.
[0090] The process PU includes a purification process using a solvent extraction method. An example of a purification process using the solvent extraction method includes the following steps. (Step PU-I) A step of adding a water-immiscible organic solvent or water to the reaction mixture obtained in step PO as necessary, stirring the mixture, and then allowing it to stand to separate into an organic phase and an aqueous phase. (Step PU-II) A step of separating the organic phase produced in step PU-I and washing the organic phase with water as necessary. (Step PU-III) A step of drying the organic phase separated in step PU-II (Step PU-IV) Removing the solvent from the organic phase dried in Step PU-III
[0091] In step PU-I, a solvent such as a water-immiscible organic solvent or water is added to the reaction mixture obtained in step PO as necessary so that the reaction mixture obtained in step PO separates into an organic phase and an aqueous phase. The amount of the solvent to be added and the type of the organic solvent are not particularly limited as long as the reaction mixture obtained in step PO separates into an organic phase and an aqueous phase.
[0092] The silane compound polymer is usually contained in the organic phase. Therefore, in step PU-II, the organic phase produced in step PU-I is separated. Thereafter, the organic phase may be washed with water according to a conventional method.
[0093] In step PU-III, the organic phase is dried by conventional methods, such as by addition of magnesium sulfate.
[0094] In step PU-IV, the solvent is removed from the organic phase. The removal of the solvent can be carried out by a conventional method such as concentration using an evaporator or vacuum drying.
[0095] [Content of component (A)] The content of the component (A) in the thermosetting composition of the present invention is preferably 50% by mass or more, more preferably 60% by mass or more, based on the total amount of the components constituting the thermosetting composition (excluding the solvent). There is no particular upper limit, but it is usually 95% by mass or less, more preferably 90% by mass or less. Therefore, the content of the component (A) is preferably 50 to 95 mass % based on the total amount of the components (excluding the solvent) constituting the thermosetting composition. Thermosetting compositions having a content of component (A) within the above range tend to have better thixotropy and coatability.
[0096] [Component (Bi): Silicone-modified particles] The component (Bi) that constitutes the thermosetting composition of the present invention is silicone-modified particles. Since the thermosetting composition of the present invention contains the component (Bi), even a thermosetting composition that does not contain a solvent or has a small amount of solvent will have excellent thixotropy and coatability. In other words, in paints and adhesives, hydrophobic particles are generally added to improve thixotropy, but as shown in the examples, even when particles having alkyl groups on their surfaces (alkyl-modified particles) were added to a thermosetting composition that contains a silane compound polymer that is liquid at room temperature as a curable component and does not contain a solvent, the thixotropy was not significantly improved. On the other hand, the addition of silicone-modified particles to this thermosetting composition improved the thixotropy. This difference in the thixotropy-improving effect is presumably due to the fact that the alkyl-modified particles have a high affinity with component (A) in the thermosetting composition, which weakens the interaction between the alkyl-modified particles and makes it difficult for the thixotropy-improving effect to be expressed, whereas the silicone-modified particles have a low affinity with component (A) in the thermosetting composition, which weakens the interaction between the silicone-modified particles and makes it possible for the silicone-modified particles to interact sufficiently with each other to express the thixotropy-improving effect.
[0097] The average particle size of the silicone modified particles is preferably 1 to 40 nm, more preferably 5 to 30 nm, and further preferably 9 to 20 nm. By using silicone-modified particles having an average particle size within the above range, it becomes easier to obtain a thermosetting composition having superior thixotropy. The average particle size of the silicone-modified particles can be determined by observing the silicone-modified particles using a transmission electron microscope (TEM) and calculating the average particle size of a number of arbitrarily selected particles (e.g., 1,000 particles).
[0098] Examples of silicone-modified particles include particles obtained by contacting particles (core particles) having reactive groups such as hydroxyl groups on the surface with silicone oil.
[0099] Examples of the core particles include inorganic oxide particles such as aluminum oxide particles, zirconium oxide particles, silicon oxide particles, and titanium oxide particles. Among these inorganic oxide particles, silicon oxide particles are preferred because they are easily available. Therefore, silicone-modified silica particles are preferred as the (Bi) component.
[0100] The inorganic oxide particles used as the core particles can be synthesized, for example, by a fumed method. The fumed method is a known manufacturing method, and fumed silica can be synthesized, for example, by carrying out a step of introducing a silicon compound such as silicon tetrachloride or metallic silicon into an oxygen-hydrogen flame to cause a hydrolysis reaction.
[0101] The silicone oil used in producing the silicone-modified particles includes reactive silicone oil and non-reactive silicone oil.
[0102] The reactive silicone oil may be a silicone oil having a reactive group at the end of the main chain or at a side chain formed by siloxane bonds. An example of the main chain composed of siloxane bonds contained in the reactive silicone oil is a poly(dimethylsiloxane) chain. Examples of the reactive group contained in the reactive silicone oil include a hydroxyl group, an amino group, an epoxy group, and a carboxyl group.
[0103] Examples of non-reactive silicone oils include dimethyl silicone oil and methyl phenyl silicone oil.
[0104] The method for producing the silicone-modified particles is not particularly limited. For example, the silicone-modified particles can be obtained by mixing the core particle powder with silicone oil and heating the resulting mixture. The heating conditions are not particularly limited, but are, for example, 80 to 380° C. for 5 to 80 minutes.
[0105] The content of the (Bi) component in the thermosetting composition of the present invention is preferably 0.1 to 50 parts by mass per 100 parts by mass of the (A) component. The thixotropy improving effect is sufficiently exhibited when the content of the (Bi) component is 0.1 parts by mass or more per 100 parts by mass of the (A) component, and for the same reason, the content is preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more, per 100 parts by mass of the (A) component. By setting the content of the (Bi) component to 50 parts by mass or less per 100 parts by mass of the (A) component, the thermosetting composition does not become too viscous and has excellent coatability. For the same reason, the content of the (Bi) component is more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less per 100 parts by mass of the (A) component.
[0106] [Component (B-ii): Particles other than component (Bi)] The thermosetting composition of the present invention may contain particles other than the component (Bi) as the component (B-ii). Examples of the component (B-ii) include particles used for the purpose of relieving stress in the cured product of the thermosetting composition and suppressing the occurrence of cracks. Examples of the component (B-ii) include particles having an average primary particle size of more than 0.04 μm and not more than 8 μm, preferably 0.06 to 7 μm, more preferably 0.3 to 6 μm, and even more preferably 0.5 to 4 μm. The average primary particle size of component (B-ii) can be determined by measuring the particle size distribution by a laser scattering method using a laser diffraction / scattering particle size distribution analyzer (e.g., product name "LA-920" manufactured by Horiba, Ltd.).
[0107] The shape of component (B-ii) may be any of spherical, chain-like, needle-like, plate-like, flake-like, rod-like, fibrous, etc., but spherical is preferred. Here, spherical means substantially spherical, including true spherical, spheroidal, ovoid, confetti-like, cocoon-like, and other polyhedral shapes that can approximate a sphere.
[0108] The constituents of the component (B-ii) are not particularly limited, and examples thereof include inorganic oxides, metals, metal carbonates, metal sulfates, metal hydroxides, metal silicates, minerals, silicon-containing polymers, and the like.
[0109] Examples of inorganic oxides include aluminum oxide, silicon oxide, titanium oxide, chromium oxide, nickel oxide, copper oxide, zirconium oxide, indium oxide, zinc oxide, and composite oxides of these.
[0110] Metal refers to an element belonging to Group 1 (excluding H), Group 2 to 11, Group 12 (excluding Hg), Group 13 (excluding B), Group 14 (excluding C and Si), Group 15 (excluding N, P, As, and Sb), or Group 16 (excluding O, S, Se, Te, and Po) in the periodic table.
[0111] Examples of the metal carbonate include calcium carbonate and magnesium carbonate. Examples of the metal sulfate include calcium sulfate and barium sulfate. The metal hydroxide may, for example, be aluminum hydroxide. Examples of the metal silicate include aluminum silicate, calcium silicate, and magnesium silicate. Examples of minerals include smectite and bentonite. Examples of silicon-containing polymers include silicone and polysilsesquioxane.
[0112] The component (B-ii) may be used alone or in combination of two or more. Of these, silicon-containing polymers are preferred as the constituent component of component (B-ii), and polysilsesquioxanes are more preferred, as they tend to give cured products with excellent transparency.
[0113] When the thermosetting composition of the present invention contains the component (B-ii), the content of the component (B-ii) is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, per 100 parts by mass of the component (A). By having the content of the component (B-ii) be 40 parts by mass or less, per 100 parts by mass of the component (A), it becomes easier to obtain a thermosetting composition that becomes a cured product having sufficient adhesive strength. There is no particular lower limit for the content of the component (B-ii), but it is preferably at least 0.1 part by mass, more preferably at least 0.2 part by mass, and even more preferably at least 0.5 part by mass, per 100 parts by mass of the component (A). Therefore, the content of the component (B-ii) is preferably 0.1 to 40 parts by mass per 100 parts by mass of the component (A).
[0114] [Component (C): Silane coupling agent] The thermosetting composition of the present invention may contain a silane coupling agent as component (C). The cured product of the thermosetting composition containing component (C) has excellent adhesive strength at room temperature and at high temperatures.
[0115] The silane coupling agent refers to a silane compound having a silicon atom, a functional group, and a hydrolyzable group bonded to the silicon atom. The functional group refers to a group having reactivity with other compounds (mainly organic substances), and examples thereof include a vinyl group, an allyl group, an epoxy group, an amino group, a substituted amino group, an acrylic group, a methacrylic group, a mercapto group, an isocyanate group, a group having an isocyanurate structure, a group having a urea structure, and a group having an acid anhydride structure. The component (C) can use either a single compound, or a combination of two or more different compounds.
[0116] When the thermosetting composition of the present invention contains the component (C), the content of the component (C) is preferably 70 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less, per 100 parts by mass of the component (A). By having the content of the component (C) be 70 parts by mass or less per 100 parts by mass of the component (A), it becomes easier to obtain a thermosetting composition that is less likely to crack in the cured product. There is no particular lower limit for the content of the component (C), but it is preferably at least 0.1 part by mass, more preferably at least 1 part by mass, and even more preferably at least 5 parts by mass per 100 parts by mass of the component (A). Therefore, the content of the component (C) is preferably 0.1 to 70 parts by mass per 100 parts by mass of the component (A).
[0117] As the silane coupling agent, a silane coupling agent having a nitrogen atom in the molecule and a silane coupling agent having an acid anhydride structure in the molecule are preferable.
[0118] Examples of the silane coupling agent having a nitrogen atom in the molecule include a trialkoxysilane compound represented by the following formula (c-1), a dialkoxyalkylsilane compound or a dialkoxyarylsilane compound represented by the following formula (c-2), and the like.
[0119] [ka]
[0120] In the above formula, R a represents an alkoxy group having 1 to 6 carbon atoms, such as a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, or a t-butoxy group. a They may be the same or different. R b represents an alkyl group having 1 to 6 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, or a t-butyl group; or an aryl group having or having no substituent, such as a phenyl group, a 4-chlorophenyl group, a 4-methylphenyl group, or a 1-naphthyl group.
[0121] R c represents an organic group having 1 to 10 carbon atoms and a nitrogen atom. c may further be bonded to another group containing a silicon atom. R c Specific examples of the organic group having 1 to 10 carbon atoms include an N-2-(aminoethyl)-3-aminopropyl group, a 3-aminopropyl group, an N-(1,3-dimethyl-butylidene)aminopropyl group, a 3-ureidopropyl group, and an N-phenyl-aminopropyl group.
[0122] Among the compounds represented by the above formula (c-1) or (c-2), R c In the case where the silane coupling agent is an organic group bonded to another silicon atom-containing group, examples of the compound include an isocyanurate-based silane coupling agent bonded to another silicon atom via an isocyanurate skeleton, and a urea-based silane coupling agent bonded to another silicon atom via a urea skeleton.
[0123] Among these, as silane coupling agents having a nitrogen atom in the molecule, isocyanurate-based silane coupling agents and urea-based silane coupling agents are preferred because they tend to give cured products with superior adhesive strength, and furthermore, those having four or more alkoxy groups bonded to silicon atoms in the molecule are preferred. "Having four or more alkoxy groups bonded to a silicon atom" means that the total number of alkoxy groups bonded to the same silicon atom and alkoxy groups bonded to different silicon atoms is four or more.
[0124] An example of an isocyanurate-based silane coupling agent having four or more alkoxy groups bonded to a silicon atom is a compound represented by the following formula (c-3): An example of an urea-based silane coupling agent having four or more alkoxy groups bonded to a silicon atom is a compound represented by the following formula (c-4):
[0125] [ka]
[0126] In the formula, R a has the same meaning as above. t1 to t5 each independently represent an integer of 1 to 10, preferably an integer of 1 to 6, and particularly preferably 3.
[0127] Among these, as the silane coupling agent having a nitrogen atom in the molecule, it is preferable to use 1,3,5-N-tris(3-trimethoxysilylpropyl)isocyanurate, 1,3,5-N-tris(3-triethoxysilylpropyl)isocyanurate (hereinafter referred to as "isocyanurate compound"), N,N'-bis(3-trimethoxysilylpropyl)urea, N,N'-bis(3-triethoxysilylpropyl)urea (hereinafter referred to as "urea compound"), and combinations of the above-mentioned isocyanurate compounds and urea compounds.
[0128] When the thermosetting composition of the present invention contains a silane coupling agent having a nitrogen atom in the molecule, the content thereof is not particularly limited, but the amount thereof is preferably 65 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less, per 100 parts by mass of the above component (A). There is no particular lower limit for the content of the silane coupling agent having a nitrogen atom in the molecule, but it is preferably at least 0.1 part by mass, more preferably at least 0.3 part by mass, and even more preferably at least 1 part by mass, per 100 parts by mass of component (A). Therefore, the content of the silane coupling agent having a nitrogen atom in the molecule is preferably 0.1 to 65 parts by mass per 100 parts by mass of the component (A).
[0129] Silane coupling agents having an acid anhydride structure in the molecule are organosilicon compounds having both a group having an acid anhydride structure and a hydrolyzable group in one molecule.Specific examples include compounds represented by the following formula (c-5).
[0130] [ka]
[0131] In the formula, Q represents a group having an acid anhydride structure, R d represents an alkyl group having 1 to 6 carbon atoms or a phenyl group having or without a substituent, R e represents an alkoxy group having 1 to 6 carbon atoms or a halogen atom, i and k represent integers of 1 to 3, j represents an integer of 0 to 2, and i+j+k=4. When j is 2, R d may be the same or different. When k is 2 or 3, multiple R e When i is 2 or 3, multiple Q's may be the same or different. Q is expressed by the following formula:
[0132] [ka]
[0133] (wherein h represents an integer of 0 to 10), and the group represented by (Q1) is particularly preferred.
[0134] Examples of silane coupling agents having an acid anhydride structure in the molecule include tri(C1-6)alkoxysilyl(C2-8)alkyl succinic anhydrides such as 2-(trimethoxysilyl)ethyl succinic anhydride, 2-(triethoxysilyl)ethyl succinic anhydride, 3-(trimethoxysilyl)propyl succinic anhydride, and 3-(triethoxysilyl)propyl succinic anhydride; Di(C1-6)alkoxymethylsilyl(C2-8)alkyl succinic anhydrides, such as 2-(dimethoxymethylsilyl)ethyl succinic anhydride; (C1-6)alkoxydimethylsilyl(C2-8)alkyl succinic anhydrides, such as 2-(methoxydimethylsilyl)ethyl succinic anhydride;
[0135] Trihalogenosilyl (C2-8) alkyl succinic anhydrides, such as 2-(trichlorosilyl)ethyl succinic anhydride and 2-(tribromosilyl)ethyl succinic anhydride; Dihalogenomethylsilyl (C2-8) alkyl succinic anhydrides, such as 2-(dichloromethylsilyl)ethyl succinic anhydride; halogenodimethylsilyl (C2-8) alkyl succinic anhydrides such as 2-(chlorodimethylsilyl)ethyl succinic anhydride; and the like.
[0136] Among these, as the silane coupling agent having an acid anhydride structure in the molecule, tri(C1-6)alkoxysilyl(C2-8)alkyl succinic anhydride is preferred, and 3-(trimethoxysilyl)propyl succinic anhydride or 3-(triethoxysilyl)propyl succinic anhydride is particularly preferred.
[0137] When the thermosetting composition of the present invention contains a silane coupling agent having an acid anhydride structure in the molecule, the content thereof is not particularly limited, but the amount thereof is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less, per 100 parts by mass of the above component (A). There is no particular lower limit for the content of the silane coupling agent having an acid anhydride structure in the molecule, but it is preferably 0.1 part by mass or more, more preferably 0.3 part by mass or more, and even more preferably 0.5 part by mass or more, per 100 parts by mass of component (A). Therefore, the content of the silane coupling agent having an acid anhydride structure in the molecule is preferably 0.1 to 30 parts by mass per 100 parts by mass of the component (A).
[0138] [solvent] The thermosetting composition of the present invention may contain a solvent. However, since the thermosetting composition of the present invention has excellent thixotropy and coatability even without containing a solvent, it is preferable that the composition does not contain a solvent in consideration of the environmental load and the like. The content of the solvent is preferably 40% by mass or less, more preferably 20% by mass or less, further preferably 5% by mass or less, and particularly preferably 0% by mass, based on the total amount of the thermosetting composition.
[0139] [Other ingredients] The thermosetting composition of the present invention may contain components other than those described above, provided that the object of the present invention is not impaired. Examples of components other than those mentioned above include additives such as antioxidants, ultraviolet absorbers, and light stabilizers. The content of these additives can be appropriately determined depending on the purpose.
[0140] [Thermosetting composition] The thermosetting composition of the present invention can be prepared, for example, by mixing the above-mentioned components (A) and (B) and, if desired, other components in a predetermined ratio, followed by degassing. The mixing method and the degassing method are not particularly limited, and known methods can be used.
[0141] The thermosetting composition of the present invention is subjected to a shear rate of 2s at a temperature of 25°C. -1 In this case, the viscosity is preferably from 20 to 100 Pa·s, and more preferably from 20 to 45 Pa·s. The thermosetting composition of the present invention is subjected to a shear rate of 200 s -1 In this case, the viscosity is preferably from 3 to 30 Pa·s, and more preferably from 3 to 12 Pa·s. The thixotropy index of the thermosetting composition of the present invention is preferably 3 or more, and more preferably 4 or more. The viscosity and thixotropy index of the thermosetting composition of the present invention can be determined according to the method described in the Examples.
[0142] As described above, the thermosetting composition of the present invention uses a combination of the components (A) and (B), and therefore has excellent thixotropy and coatability even if it does not contain a solvent or contains a small amount of solvent. Therefore, by using the thermosetting composition of the present invention, operations such as repeated microdispensing can be carried out efficiently without contaminating the surroundings.
[0143] Because of the above-mentioned characteristics, the thermosetting composition of the present invention is suitably used as a composition for fixing a semiconductor element. Examples of the semiconductor element fixing composition include an adhesive for fixing a semiconductor element and a sealant for fixing a semiconductor element. Examples of semiconductor elements include light-emitting elements such as light-emitting diodes (LEDs) and laser diodes (LDs); light-receiving elements such as photodiodes, solar cells, and CMOS image sensors; composite optical elements; integrated circuits; and large-scale integrated circuits.
[0144] When the thermosetting composition of the present invention is used as a semiconductor element fixing composition, the thermosetting composition of the present invention is usually cured by heating. The heating temperature when the thermosetting composition of the present invention is heat-cured is usually 100 to 200° C. The heating time is usually 10 minutes to 20 hours, preferably 30 minutes to 10 hours.
[0145] [Adhesive for fixing semiconductor elements] When the thermosetting composition of the present invention is used as an adhesive for fixing a semiconductor element, a predetermined amount of the thermosetting composition of the present invention is usually applied to one or both of the adhesive surfaces of the materials to be bonded (such as a semiconductor element and a substrate), pressed together, and then cured by heating. This process makes it possible to firmly bond the materials to be bonded together.
[0146] Materials that can be used to form the substrate include glasses such as soda lime glass and heat-resistant hard glass; ceramics; sapphire; metals such as iron, copper, aluminum, gold, silver, platinum, chromium, titanium, and alloys of these metals, and stainless steel (SUS302, SUS304, SUS304L, SUS309, etc.); and synthetic resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, ethylene-vinyl acetate copolymer, polystyrene, polycarbonate, polymethylpentene, polysulfone, polyether ether ketone, polyether sulfone, polyphenylene sulfide, polyetherimide, polyimide, polyamide, acrylic resin, norbornene resin, cycloolefin resin, and glass epoxy resin.
[0147] [Sealant for fixing semiconductor elements] When the thermosetting composition of the present invention is used as a sealant for fixing a semiconductor element, the thermosetting composition of the present invention is usually molded into a desired shape to obtain a molded body containing a semiconductor element, which is then cured by heating to obtain a semiconductor element encapsulated body containing the semiconductor element. The method for molding the thermosetting composition of the present invention into a desired shape is not particularly limited, and any known molding method such as a typical transfer molding method or a casting method can be used.
[0148] 2) Cured product The cured product of the present invention is obtained by curing the thermosetting composition of the present invention. The thermosetting composition of the present invention can be cured by heat curing. The heating temperature when the thermosetting composition of the present invention is heat-cured is usually 100 to 200° C. The heating time is usually 10 minutes to 20 hours, preferably 30 minutes to 10 hours.
[0149] When the cured product of the present invention is an adhesive cured product used as an adhesive for fixing semiconductor elements, the cured product of the present invention preferably has excellent adhesive strength. For example, when the die shear strength was measured in the examples, the cured product of the present invention had a strength of 80N / 4mm at 23°C. 2 More preferably, 100N / 4mm 2 More preferably, it is 30N / 4mm or more at 100°C. 2 More than 50N / 4mm is preferable. 2 More preferably, it is 60N / 4mm or more. 2 Even more preferably, this is the case. In this specification, "4 mm 2 " means "2mm square," that is, 2mm x 2mm (a square with each side measuring 2mm). EXAMPLES
[0150] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples in any way.
[0151] [Production Example 1] A 300 ml eggplant-shaped flask was charged with 23.71 g (133 mmol) of methyltriethoxysilane, and then an aqueous solution (H2O: 266 mmol) of 35 mass% hydrochloric acid (HCl: 0.133 mmol, 0.1 mol% relative to methyltriethoxysilane) was added to 4.782 g of distilled water while stirring, and the entire volume was stirred for 1 hour at 24° C. The system was heated to 70° C., and 15.3 g of propyl acetate and 0.020 g of 28% aqueous ammonia solution (NH3: 0.333 mmol, 0.25 mol% relative to methyltriethoxysilane) were added thereto, and the entire volume was stirred at 70° C. for 4 hours. After the reaction solution was cooled to room temperature (25°C), 100g of propyl acetate and 200g of water were added thereto to carry out a liquid separation treatment, and an organic phase containing the reaction product was separated. Magnesium sulfate was added to this organic phase and a drying treatment was carried out. After removing magnesium sulfate by filtration, the organic phase was concentrated with an evaporator, and the obtained concentrate was then vacuum dried to obtain a silane compound polymer.
[0152] [Production Examples 2 to 4] A silane compound polymer was obtained in the same manner as in Production Example 1, except that the conditions were changed to those shown in Table 1.
[0153] [Table 1]
[0154] The following measurements were carried out on the silane compound polymers obtained in Production Examples 1 to 3. The results are shown in Table 2.
[0155] [Viscosity measurement] In Production Examples 1 and 3, a rheometer (machine name "MCR301", manufactured by Anton Paar) was used, and the cone plate had a cone radius of 12.5 mm and a cone angle of 0.5°. The cone radius was 12.5 mm and the cone angle was ... -1 The viscosity of the mixture was measured. In Production Example 2, the viscosity was measured at 25° C. and 2.0 rad / s using parallel plates with a radius of 12.5 mm. In Production Example 4, since it was a solid, the viscosity could not be measured.
[0156] [Average molecular weight measurement] The mass average molecular weight (Mw) of the silane compound polymer was measured using the following device and conditions. Device name: HLC-8220GPC, manufactured by Tosoh Corporation Column: "TSK guard column SuperH-H", "TSK gel SuperHM-H", "TSK gel SuperHM-H", and "TSK gel SuperH2000" connected in sequence Solvent: Tetrahydrofuran Standard material: polystyrene Injection volume: 20μl Measurement temperature: 40℃ Flow rate: 0.6ml / min Detector: Differential refractometer
[0157] [ 1 H-NMR measurement] Device name: Bruker Biospin AV-500 1 H-NMR resonance frequency: 500MHz Probe: 5mmφ solution probe Measurement temperature: room temperature (25℃) Repeat time: 1s Number of times: 16
[0158] < 1 H-NMR sample preparation method Silane compound polymer concentration: 3% Measurement solvent: acetone-d6 Internal standard: TMS
[0159] [Alkoxy group residual ratio] 1 Based on the results of H-NMR measurement, the ratio of alkoxy groups to methyl groups was obtained, and the residual ratio of alkoxy groups in the silane compound polymer was calculated.
[0160] [ 29 Si-NMR measurement] Device name: Bruker Biospin AV-500 29 Si-NMR resonance frequency: 99.352MHz Probe: 5mmφ solution probe Measurement temperature: room temperature (25℃) Sample rotation speed: 20kHz Measurement method: Inverse gate decoupling method 29 Si flip angle: 90° 29 Si 90°Pulse width: 8.0μs Repeat time: 5s Accumulation count: 9200 times Observation width: 30kHz
[0161] < 29 Si-NMR sample preparation method In order to shorten the relaxation time, Fe(acac)3 was added as a relaxation reagent and measurements were performed. Silane compound polymer concentration: 15% Fe(acac)3 concentration: 0.6% Measurement solvent: acetone Internal standard: TMS
[0162] Waveform processing analysis For each peak in the spectrum after Fourier transformation, the chemical shift was determined from the peak top position, and each peak was integrated in the following range. T1 site: -52.0 to -45.0 ppm T2 site: -60.7 to -52.0 ppm T3 site: -71.5 to -60.7 ppm Based on the obtained values, the proportions of T1 sites, T2 sites, and T3 sites were calculated.
[0163] [Ratio of alkoxy-containing T1 sites to the total amount of T1 sites] 29 Si-NMR measurement was carried out, and the amount of T1 sites having one or two alkoxy groups was determined based on the integral value in the range of −52.0 to −50.0 ppm. Next, based on this integral value, the ratio of alkoxy group-containing T1 sites to the total amount of T1 sites (T1(OR) / T1(total)) was calculated.
[0164] [Table 2]
[0165] The compounds used in the Examples, Comparative Examples, and Reference Examples are shown below.
[0166] (Silane compound polymer) PSQ(A1): silane compound polymer obtained in Production Example 1 PSQ (A2): silane compound polymer obtained in Production Example 2 PSQ (A3): silane compound polymer obtained in Production Example 3 PSQ (A4): silane compound polymer obtained in Production Example 4
[0167] (particle) Particles (B1): (manufactured by Nippon Aerosil Co., Ltd., product name "AEROSIL RY200", silica particles surface-modified with polydimethylsiloxane, average primary particle diameter: 12 nm) Particles (B2): (manufactured by Nippon Aerosil Co., Ltd., product name "AEROSIL RY300", silica particles surface-modified with polydimethylsiloxane, average primary particle diameter: 7 nm) Particles (B3): (manufactured by Nippon Aerosil Co., Ltd., product name "AEROSIL RX300", silica particles having trimethylsilyl groups as surface modification groups, average primary particle diameter: 7 nm) Particles (B4): (manufactured by Nikko Rica Corporation, product name "MSP-SN08", polymethylsilsesquioxane particles, average primary particle diameter: 0.8 μm)
[0168] (Silane coupling agent) SCA(C1): 1,3,5-N-tris[3-(trimethoxysilyl)propyl]isocyanurate SCA(C2): 3-(trimethoxysilyl)propylsuccinic anhydride
[0169] Example 1 5 parts by mass of particles (B1) and 10 parts by mass of particles (B4) were added to 100 parts by mass of PSQ (A1), and the whole was stirred. After dispersion treatment with a triple roll mill, 30 parts by mass of silane coupling agent (C1) and 3 parts by mass of silane coupling agent (C2) were added, and the whole was thoroughly mixed and degassed to obtain a thermosetting composition.
[0170] [Examples 2 and 3, Comparative Examples 1 to 3] A thermosetting composition was obtained in the same manner as in Example 1, except that the composition was changed to that shown in Table 3.
[0171] [Reference example 1] 25 parts by mass of particles (B3) and 10 parts by mass of particles (B4) were added to 100 parts by mass of polysilsesquioxane compound (A4), and 60 parts by mass of a mixed solvent of diethylene glycol monobutyl ether acetate: tripropylene glycol-n-butyl ether = 40:60 (mass ratio) was further added, and the whole was stirred. After dispersion treatment with a three-roll mill, 30 parts by mass of silane coupling agent (C1) and 3 parts by mass of silane coupling agent (C2) were added, and the whole was thoroughly mixed and defoamed to obtain a thermosetting composition.
[0172] The following measurements were carried out on the thermosetting compositions obtained in Examples 1 to 3, Comparative Examples 1 to 3, and Reference Example 1. The results are shown in Table 3.
[0173] [Viscosity evaluation] The rheometer (Anton Paar, MCR301) was used with a cone plate having a radius of 12.5 mm and a cone angle of 0.5°, and the shear rate was 2 s at 25°C. -1 and the shear rate is 200 s -1 The viscosity of each was measured. The thixotropic index (when the shear rate is 2s -1 Viscosity / shear rate of 200s -1 The viscosity of the solution was calculated.
[0174] [Die shear strength test] 4mm 2 The thermosetting composition was applied to the mirror surface of a silicon chip (2 mm x 2 mm) to a thickness of approximately 2 μm, and the applied surface was placed on an adherend (silver-plated copper plate) and pressed. The composition was then heat-treated at 170°C for 2 hours to harden the material, yielding an adherend with a test piece attached. The adherend with the test piece attached was left for 30 seconds on the measurement stage of a bond tester (Dage, Series 4000) that had been preheated to a predetermined temperature (23°C, 100°C), and a stress was applied to the adhesive surface in the horizontal direction (shear direction) at a speed of 200 μm / s from a position 100 μm above the adherend, and the adhesive strength (N / 4 mm) between the test piece and the adherend at 23°C and 100°C was measured. 2 ) was measured.
[0175] [Table 3]
[0176] The following can be seen from Table 3: The thermosetting compositions obtained in Examples 1 to 3 contain the component (A) and the component (Bi), and therefore have excellent thixotropy and coatability. On the other hand, in Comparative Example 1, when alkyl-modified particles were used instead of component (Bi) [silicone-modified particles], the thixotropic index decreased. In Comparative Example 2, in which no alkyl-modified particles were added, the thixotropy index was lower than that of Comparative Example 1. In addition, in Comparative Example 3 in which an excess of alkyl-modified particles was used, the thixotropy index was about the same as in Comparative Example 1, but the viscosity was too high and the coatability was poor. Even when alkyl-modified particles are used, in Reference Example 1 in which a solvent is present, sufficient performance is achieved in terms of both viscosity and thixotropy.
Claims
1. A thermosetting composition comprising the following component (A) and component (Bi): Component (A): a silane compound polymer that is liquid at 25°C Component (Bi): Silicone-modified particles
2. 2. The thermosetting composition according to claim 1, wherein the component (A) is a silane compound polymer having a viscosity of 15,000 Pa·s or less at 25°C.
3. The thermosetting composition according to claim 1 , wherein the component (A) is a silane compound polymer having an alkoxy group.
4. The thermosetting composition according to claim 3 , wherein the component (A) is a silane compound polymer obtained by hydrolysis and polycondensation of an alkoxysilane compound.
5. The thermosetting composition according to claim 4, wherein the component (A) is a silane compound polymer having a residual alkoxy group ratio of 25% or less.
6. 2. The thermosetting composition according to claim 1, wherein the component (A) is a silane compound polymer having thermosetting properties.
7. 2. The thermosetting composition according to claim 1, wherein the component (A) is a silane compound polymer having a mass average molecular weight (Mw) of 500 to 20,000.
8. The component (A) is represented by the following formula (a-1): 【Chemistry 1】 (Me represents a methyl group.) The repeating unit (1) has a repeating unit represented by the formula: The following formula (a-2) 【Chemistry 2】 [R 1 represents a group selected from the group consisting of an unsubstituted alkyl group having 2 to 10 carbon atoms, a substituted alkyl group having 1 to 10 carbon atoms, an unsubstituted aryl group having 6 to 12 carbon atoms, and a substituted aryl group having 6 to 12 carbon atoms. The thermosetting composition according to claim 1, which is a silane compound polymer having or not having a repeating unit represented by the following formula (2):
9. 9. The thermosetting composition according to claim 8, wherein the amount of the repeating unit (1) contained in the silane compound polymer is 70 to 100 mol % based on the total amount of the repeating unit (1) and the repeating unit (2).
10. 9. The thermosetting composition according to claim 8, wherein the total amount of the repeating units (1) and (2) in the silane compound polymer is 80 to 100 mol % of all repeating units in the silane compound polymer.
11. The thermosetting composition according to claim 8, wherein the silane compound polymer has a T1 site represented by the following formula (a-3), a T2 site represented by the following formula (a-4), and a T3 site represented by the following formula (a-5), and the amount of the T1 site is 2.5 to 25 mol % based on the total amount of the T1 site, the T2 site, and the T3 site. 【Chemistry 3】 [R 2 represents a group selected from the group consisting of an unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted alkyl group having 1 to 10 carbon atoms, an unsubstituted aryl group having 6 to 12 carbon atoms, and a substituted aryl group having 6 to 12 carbon atoms. 1 ~X 3 each independently represents a hydrogen atom or an alkyl group. * represents a bond to another repeating unit and is directly bonded to a silicon atom of the other repeating unit.
12. The thermosetting composition according to claim 11, wherein the silane compound polymer is a silane compound polymer in which the amount of T1 sites having an alkoxy group is 20 to 60 mol % of the total T1 sites.
13. 2. The thermosetting composition according to claim 1, wherein the average particle size of the component (Bi) is 1 to 40 nm.
14. The thermosetting composition according to claim 1, wherein the component (Bi) is a silicone-modified silica particle.
15. 2. The thermosetting composition according to claim 1, wherein the content of the component (Bi) is 0.1 to 50 parts by mass per 100 parts by mass of the component (A).
16. 2. The thermosetting composition according to claim 1, which may or may not contain a solvent, and the content of the solvent is 40 mass % or less based on the total amount of the thermosetting composition.
17. A composition for fixing a semiconductor element, comprising the thermosetting composition according to claim 1 .
18. A cured product obtained by curing the thermosetting composition according to claim 1.
Citation Information
Patent Citations
Surface-protective water-repellent agent for exterior surface
JP2010202717A
Organopolysiloxane and coating composition containing the same
JP2021080307A
Curable composition, method for producing curable composition, cured object, method for using curable composition, and optical device
WO2016031728A1
Curable composition, method for producing curable composition, cured product, and use of curable composition
WO2017110947A1
Condensation reaction-type die bonding agent, LED light emitting device and method for manufacturing same
WO2017122796A1