Low compression set silicone rubber composition with high temperature durability and rubber product
By using a composite modified by specific vinyl silicone oil and sulfur-containing silane compounds in silicon rubber, combined with precious metal catalysts, the problem of poor compression and permanent deformation performance of silicon rubber after long-term aging at high temperature is solved, and high temperature durability and low Cost colorless silicone rubber products.
Patent Information
- Application Number
- CN202411252112.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-12
AI Technical Summary
Existing silicone rubbers have poor compression and permanent deformation performance after long-term aging at high temperature, which is difficult to meet the requirements of high temperature durability. Common heat-resistant additives are expensive and affect color, and nitrogen and sulfur additives affect vulcanization and yellowing in platinum systems.
Use vinyl silicone oil with specific structures and a sulfur-containing silane compound modified composite, and control the ratio of silicon hydrogen group to vinyl group, combine with noble metal catalysts to form an excellent crosslinking network to improve durability, low compression and permanent Deformation performance.
The permanent deformation performance of 140℃×1000h compression is reduced to less than 30%, avoiding the use of expensive heat-resistant additives, keeping the product colorless and low cost, and at the same time, the vulcanization speed is fast, the adaptability is wide, and the second stage vulcanization is not required.
Smart Images

Figure BDA0005033054810000071 
Figure BDA0005033054810000081 
Figure BDA0005033054810000201
Abstract
Description
Technical Field
[0001] The invention relates to a silicone rubber composition and a rubber product having high temperature durability and low compression permanent deformation. Background Art
[0002] Liquid silicone rubber has good performance, good resilience, and is easy to process on a large scale, so it has been widely used in the automotive industry. However, as automobiles develop towards energy saving and low pollution, the temperature of the engine has increased by 15-50°C in recent years. At the same time, people's requirements for automobile safety, environmental protection, comfort, intelligence, etc. are getting higher and higher. It is required to ensure both the stable operation of automotive equipment and the waterproof performance of automotive equipment at work. In this case, new requirements are put forward for the performance of silicone rubber: it has excellent high-temperature durability and can still maintain low compression permanent deformation after thermal aging, so as to achieve good sealing performance. WO2019 / 175092A1 mentions that silicone rubber in American cars is divided into T3, T4, and T5 grades according to durability. At present, most silicone rubbers meet the T3 grade. In order to reach the T4 and T5 grades, the material needs better high temperature resistance and durable compression permanent deformation performance.
[0003] The general methods for improving the compression set performance of silicone rubber in the prior art are: (1) adding heat-resistant additives such as iron oxide and cerium oxide to silicone rubber to capture free radicals generated at high temperatures, thereby avoiding the attack of free radicals on polysiloxane molecular chains and improving the heat resistance stability of the material; (2) adding unsaturated bond-containing or nitrogen-sulfur-containing additives such as benzotriazole and melamine urate to neutralize the unreacted platinum catalyst after the cross-linking reaction, thereby reducing the secondary cross-linking reaction during high-temperature aging. However, these methods still have shortcomings, such as the high price of heat-resistant additives and color, and in the platinum-catalyzed liquid silicone rubber system, nitrogen-sulfur compound additives will also affect the vulcanization and yellowing of silicone rubber.
[0004] CN115895271A uses metal oxides such as nano-cerium oxide and cerium hydroxide to prepare low compression permanent deformation liquid silicone rubber. After hot air aging at 180°C×22H and aging with 25% volume compression, the compression set is ≤15%.
[0005] US5977249 uses silane containing sulfur groups to treat white carbon black and applies it to a platinum system to obtain a transparent liquid silicone rubber product with low compression set. However, the compression set of the product is tested at 175°C × 22h, and the compression set of the final product is less than 50%.
[0006] The improvement methods reported so far are mainly aimed at the compression permanent deformation after short-term aging, such as (170-180℃)×22h. However, experiments have found that materials with excellent short-term compression permanent deformation do not necessarily perform well after durability testing. There are many factors that cause silicone rubber aging. The internal factor is that the unsaturated structure in the molecular structure of silicone rubber reacts chemically with the active oxygen atoms, thereby destroying the structure of silicone rubber. Chemical and physical factors such as oxygen, ozone, heat, light, and stress are external factors that accelerate the aging of silicone rubber. During the compression permanent deformation test, the material applies external force, restricts the movement of the molecular chain, and reduces oxygen permeability. Due to the complexity of the aging mechanism, there is currently no clear mechanism to indicate what specific changes have occurred during the aging process, but some scholars have conducted research on different rubbers, and the results show that the cross-linking mechanism is different at different aging periods; some are mainly cross-linked in the early stage of aging, and mainly cracked in the later stage of aging, while others are the opposite. Due to the differences in mechanisms at different aging stages, short-term aging performance cannot represent long-term aging performance. Summary of the invention
[0007] The inventors found during the research and experimental process that a material having excellent compression set under short-time aging (177° C.×22 h) may not necessarily have excellent compression set at 140° C.×1000 h.
[0008] The present invention is accomplished in view of the above problems in the prior art, and aims to provide a self-penetrating silicone rubber composition and a rubber product having high temperature durability and low compression set.
[0009] The inventors have found that the above technical problems can be solved by using vinyl silicone oil with a specific structure and a composite modified by a sulfur-containing silane compound in a silicone rubber composition and controlling the ratio of silane groups to vinyl groups, thereby completing the present invention.
[0010] Specifically, the present invention provides:
[0011] 1. A silicone rubber composition comprising:
[0012] (A) a base silicone oil comprising: a dual-end vinyl silicone oil (vinyl silicone oil I) with a viscosity of 10000-100000 mPa·s, a side-chain vinyl silicone oil (vinyl silicone oil II) with a viscosity of 500-20000 mPa·s, and a terminal vinyl silicone oil (vinyl silicone oil III) with a viscosity of 5000-20000 mPa·s, the amount of which is 100 parts by mass;
[0013] (B) a composite modified with a sulfur-containing silane compound in an amount of 0.05-0.5 parts by mass;
[0014] (C) hydrogen-containing silicone oil in an amount such that the number of silicon-hydrogen bonds / the number of vinyl groups in the silicone rubber composition = 1.2-1.5;
[0015] (D) A noble metal catalyst in an amount of 1 to 35 ppm based on the weight of the noble metal.
[0016] 2. The silicone rubber composition according to 1, further comprising at least one of the following substances: an inhibitor and a filler.
[0017] 3. The silicone rubber composition according to 1, wherein in 100 parts by mass of the base silicone oil,
[0018] Vinyl silicone oil I is 60-98 parts;
[0019] Vinyl silicone oil II is 1-20 parts;
[0020] Vinyl silicone oil III is 1-20 parts.
[0021] 4. The silicone rubber composition according to 1, wherein the base silicone oil further comprises phenyl silicone oil.
[0022] 5. The silicone rubber composition according to item 1, wherein the vinyl content of the terminal vinyl silicone oil is 1-20 wt %.
[0023] 6. The silicone rubber composition according to 1, wherein the compound comprises at least one of the following substances: silicon micropowder, clay, calcium carbonate, white carbon black, aluminum hydroxide, magnesium hydroxide, silicone oil and silicone resin.
[0024] 7. A rubber product prepared using the silicone rubber composition described in any one of 1 to 6 above.
[0025] Effects of the Invention
[0026] The silicone rubber composition according to the present invention has excellent compression permanent deformation performance, and can reduce the compression permanent deformation performance of 140℃×1000h to less than 30%. The rubber does not use expensive and easily dyed heat-resistant additives, and can reduce the compression permanent deformation after long-term aging, so that the product has the advantages of being colorless and low-cost. The silicone rubber composition has a fast vulcanization speed, and the additives used in the formula have little effect on vulcanization within a wide range of addition amounts, and the process adaptability is wide. The silicone rubber composition does not require two-stage vulcanization, and can achieve durable low compression permanent deformation. DETAILED DESCRIPTION
[0027] (Silicone rubber composition)
[0028] The silicone rubber composition of the present invention comprises: (A) base silicone oil, (B) a compound modified by a sulfur-containing silane compound, (C) hydrogen-containing silicone oil and (D) a noble metal catalyst. Among them, by using a vinyl silicone oil with a specific structure and a compound modified by a sulfur-containing silane compound in the silicone rubber composition and controlling the ratio of the silicon hydrogen group to the vinyl group, the silicone rubber composition can still have excellent compression permanent deformation performance after long-term high-temperature aging.
[0029] Hereinafter, each component of the silicone rubber composition of the present invention will be described in detail.
[0030] (Basic silicone oil)
[0031] The silicone rubber composition of the present invention comprises a base silicone oil. The base silicone oil comprises: a double-end vinyl silicone oil with a viscosity of 10000-100000 mPa·s (hereinafter sometimes referred to as vinyl silicone oil I or first vinyl silicone oil), a side-chain vinyl silicone oil with a viscosity of 500-20000 mPa·s (hereinafter sometimes referred to as vinyl silicone oil II or second vinyl silicone oil), and a terminal vinyl silicone oil with a viscosity of 5000-20000 mPa·s (hereinafter sometimes referred to as vinyl silicone oil III or third vinyl silicone oil). Preferably, the vinyl content of the vinyl silicone oil III is 1-20 wt%.
[0032] (Vinyl silicone oil Ⅰ)
[0033] Vinyl silicone oil I is a dual-end vinyl silicone oil having a dual-end vinyl structure. Its viscosity at 25°C is 10,000-100,000 mPa·s, more preferably 20,000-80,000 mPa·s, and most preferably 20,000-60,000 mPa·s. Any silicone oil having a dual-end vinyl structure and a viscosity within the above range can be used.
[0034] The vinyl group may be selected from the following groups: ethenyl, propenyl, 3-butenyl, 5-hexenyl, 9-decenyl, 10-undecenyl, 5,9-decadienyl, 6,11-dodecadienyl, and the like.
[0035] Vinyl silicone oil I may have a linear, branched, cyclic or network structure.
[0036] Examples of the vinyl silicone oil I include:
[0037] - Polydimethylsiloxanes having dimethylvinylsilyl terminal groups.
[0038] The viscosity described in the present invention is a value measured at 25° C. using a rotational viscometer (the same applies hereinafter).
[0039] Vinyl silicone oil I in the silicone rubber composition mainly plays the role of building a cross-linked network and providing elasticity and toughness of the rubber. Its content is 60-98wt%, preferably 80-98wt%, and more preferably 85-95wt% based on 100 parts by mass of the base silicone oil.
[0040] The vinyl silicone oil I can be a commercial product known in the art or a product prepared by a method known in the art. The vinyl silicone oil I can be used alone or in combination of two or more.
[0041] (Vinyl Silicone Oil Ⅱ)
[0042] Vinyl silicone oil II is a side chain vinyl silicone oil having a structure with a vinyl group in the side chain and a viscosity of 500-20000 mPa·s, preferably 1000-10000 mPa·s, more preferably 2000-5000 mPa·s. Any silicone oil having at least one vinyl group in the side chain in one molecule and a viscosity that meets the above range can be used.
[0043] The vinyl group may be selected from the group consisting of ethenyl, propenyl, 3-butenyl, 5-hexenyl, 9-decenyl, 10-undecenyl, 5,9-decadienyl and 6,11-dodecadienyl.
[0044] Examples of the vinyl silicone oil II include:
[0045] -Terminal methyl side methyl side vinyl silicone oil.
[0046] Vinyl silicone oil II in the silicone rubber composition mainly provides concentrated crosslinking points and improves strength. Its content is 1-20wt%, preferably 2-15wt%, and more preferably 2-10wt%, based on 100 parts by mass of the base silicone oil.
[0047] The vinyl silicone oil II can be a commercial product known in the art or a product prepared by a method known in the art. The vinyl silicone oil II can be used alone or in combination of two or more.
[0048] (Vinyl silicone oil Ⅲ)
[0049] Vinyl silicone oil III is a terminal vinyl silicone oil having a structure in which at least one end is capped with a vinyl group and the side chain has a vinyl group, and its viscosity is 5000-20000 mPa·s, more preferably 10000-19000 mPa·s. Any silicone oil having the above structure and a viscosity within the above range can be used.
[0050] The vinyl group may be selected from the group consisting of ethenyl, propenyl, 3-butenyl, 5-hexenyl, 9-decenyl, 10-undecenyl, 5,9-decadienyl and 6,11-dodecadienyl.
[0051] Examples of the vinyl silicone oils III include:
[0052] -Vinyl-terminated, methyl-terminated, vinyl-terminated silicone oil.
[0053] Vinyl silicone oil III is a key material of the silicone oil system of the present invention. By adding vinyl silicone oil III, durable low compression set performance can be achieved. Silicone oils with different structures / viscosities and vinyl contents can achieve an elastic cross-linked network. Its content is 1-20wt%, preferably 1-15wt%, and more preferably 1-5wt% based on 100 parts by mass of the base silicone oil. In addition, the vinyl content of vinyl silicone oil III is 1-20wt%. When the vinyl content of vinyl silicone oil III is higher than 20wt%, the vinyl as an unsaturated bond will coordinate with the metal contained in the catalyst, inhibit the catalytic efficiency of the catalyst, reduce the vulcanization rate of the system, and too much vinyl will cause the concentrated cross-linking to be too concentrated and the unreacted rate is high. More vinyl will remain in the system after thermal vulcanization, and more reaction points will be provided in the subsequent thermal aging process. The double bond unsaturated structure of the vinyl has poor aging resistance and deteriorates the compression set performance. When it is less than 1wt%, the cross-linked network of the system is difficult to form a cross-linked network with sparse and dense combination, and the concentrated cross-linking points are insufficient, so that the system has low elasticity and poor compression set. The vinyl content is more preferably 1-8 wt %, further preferably 2-4 wt %.
[0054] The vinyl silicone oil III can be a commercially available product known in the art or a product prepared by a method known in the art. The vinyl silicone oil III can be used alone or in combination of two or more.
[0055] The above-mentioned vinyl silicone oils I, II, and III may be substituted with various substituents known in the art within the scope that does not affect the effects of the present invention, and may also contain various groups known in the art in the main chain and the side chain.
[0056] (Phenyl silicone oil)
[0057] The silicone rubber composition of the present invention may optionally further contain phenyl silicone oil.
[0058] Phenyl silicone oil is a silicone oil having at least one phenyl group in one molecule, and is different from the above-mentioned base silicone oil in that it does not contain an unsaturated group in the molecule.
[0059] The phenyl silicone oil mainly plays a lubricating role in the silicone rubber composition. The viscosity of the phenyl silicone oil can be 50-300 cs. Its content can be 1-8 wt % based on 100 parts by mass of the base silicone oil.
[0060] Examples of the phenyl silicone oil include:
[0061]
[0062] Wherein m and n are each integers.
[0063] The phenyl silicone oil can be a commercially available product known in the art or a product prepared by a method known in the art. The phenyl silicone oil can be used alone or in combination of two or more.
[0064] (Compound modified with sulfur-containing silane compound)
[0065] The composite modified by sulfur-containing silane compounds of the present invention is a composite modified by sulfur-containing silane compounds including but not limited to silicon micropowder, clay, calcium carbonate, white carbon black, aluminum hydroxide, magnesium hydroxide, silicone oil, silicone resin, etc. The addition ratio of the composite modified by sulfur-containing silane compounds can be 0.05-0.5wt%, based on the base silicone oil. This component is an important component for improving durability and low compression set. The sulfur-containing groups (such as mercapto, thiocyanate, sulfoxide, sulfone, sulfide, disulfide or tetrasulfide, etc.) in the sulfur-containing silane compounds can effectively inhibit the reaction activity of the catalyst during long-term aging, reduce secondary reactions during aging, and improve pressure change, but the addition needs to be appropriate. The proportion of sulfur-containing groups is insufficient and cannot play the desired effect, but too much has an adverse effect on the system. The catalyst is sensitive to compounds containing sulfur, nitrogen, and phosphorus and is easily poisoned. Too many sulfur-containing groups will inhibit the vulcanization of the catalyst system. Therefore, the addition ratio can be 0.05-0.5wt%, preferably 0.1-0.5wt%, more preferably 0.2-0.4wt%. The content ratio of the sulfur-containing group in the composite modified by the sulfur-containing silane compound can be 0.2×10 -4 -4×10 -3 mol / g.
[0066] The sulfur-containing silane-treated composite can be obtained by uniformly mixing sulfur-containing silane with silicon powder, clay, calcium carbonate, white carbon, aluminum hydroxide, magnesium hydroxide, silicone oil, silicone resin, etc. under heating and stirring and then curing. Commercially available products can also be used.
[0067] The above-mentioned sulfur-containing silane can be used as long as it has at least one sulfur-containing group in one molecule.
[0068] Examples of the sulfur-containing silane include X b [R 2a Si(OR 1 ) 4-a ] c .
[0069] Where R 1 Each is independently an alkyl group having 1 to 10 carbon atoms, such as methyl, ethyl, propyl, butyl, etc.;
[0070] R 2 Each independently represents an alkyl group having 1 to 10 carbon atoms, such as methyl, ethyl, propyl, butyl, etc. 1 or R 2 When it is a group connected to X, it is an alkylene group;
[0071] X is a sulfur-containing group, such as a mercapto group, a thiocyano group, a sulfoxide group, a sulfone group, a sulfide group, a disulfide group, a tetrasulfide group, etc.;
[0072] a is an integer of 1-3, b is an integer of 1-3, and c is an integer of 1-3.
[0073] As specific examples thereof, the following can be cited:
[0074]
[0075] The sulfur-containing silane can be used alone or in combination of two or more thereof. The sulfur-containing silane can be commercially available or prepared by a conventional preparation method.
[0076] The silicon micropowder may have an average particle size of 20-40 microns, and may be silicon micropowder with a trade name of PGH (300 mesh).
[0077] The clay may have an average particle size of 40-60 micrometers, and specifically, may be clay with a trade name of DB-80 (manufactured by Shanxi Jinyu Kelin Technology Co., Ltd.).
[0078] The calcium carbonate may have an oil absorption value (g / 100g) ≤ 100. Specifically, calcium carbonate with a trade name of activated calcium carbonate (manufactured by Changzhou Calcium Carbonate Co., Ltd.) may be used.
[0079] The above-mentioned white carbon black can use a specific surface area of 150-300m 2 Specifically, white carbon black with a trade name of H300 (manufactured by CARBOT) can be used.
[0080] The aluminum hydroxide may have an average particle size of 2-100 micrometers, and specifically, may have a trade name of TL01-1 (manufactured by Yuxing Flame Retardant).
[0081] The magnesium hydroxide may have an average particle size of 2-100 micrometers, and specifically, may have a trade name of TM01-1 (manufactured by Yuxing Flame Retardant).
[0082] The silicone oil may be vinyl silicone oil, and specifically, silicone oil with a trade name of 621V10000 (produced by Jiangxi Xinghuo Silicone) may be used.
[0083] The silicone resin may be a vinyl silicone resin, and specifically, a silicone resin with a trade name of XJY-8206A (manufactured by Shin-Jia-Yi) may be used.
[0084] (Hydrogen silicone oil)
[0085] The hydrogen-containing silicone oil of the present invention may have a pendant hydrogen or terminal hydrogen structure, and any silicone oil having at least one silicon-hydrogen bond in one molecule may be used in the present invention.
[0086] Hydrogenated silicone oils can have linear, branched, cyclic or network structures.
[0087] The amount of hydrogen-containing silicone oil added is such that the number of silicon-hydrogen bonds / number of vinyl groups (hereinafter sometimes referred to as silicon-hydrogen vinyl ratio) = 1.2-1.5. When the silicon-hydrogen vinyl ratio is less than 1.2, the degree of crosslinking is insufficient, which will lead to insufficient vinyl reactivity in the system. When it is more than 1.5, more silicon-hydrogen groups will remain after the addition reaction and participate in the secondary reaction during the aging process. When the silicon-hydrogen vinyl ratio is within this range, excellent high-temperature durability and low compression set can be achieved. The silicon-hydrogen vinyl ratio is more preferably 1.3-1.45.
[0088] The content of the hydrogen-containing silicone oil may be 0.5-3% based on 100 parts by mass of the base silicone oil.
[0089] Examples of the hydrogen-containing silicone oil include:
[0090] -Methyl-terminated silyl hydrogen siloxane.
[0091] The hydrogen-containing silicone oil can be a commercially available product known in the art or a product prepared by a method known in the art. The hydrogen-containing silicone oil can be used alone or in combination of two or more.
[0092] (catalyst)
[0093] The catalyst of the present invention is used for the addition reaction (hydrosilylation) between the alkenyl group of vinyl silicone oil and the silyl group of hydrogen-containing silicone oil. In the present invention, any hydrosilylation catalyst commonly used in the art can be used.
[0094] The catalyst of the present invention can be a noble metal catalyst, such as platinum, rhodium, palladium, ruthenium and iridium, preferably platinum, which is optionally supported on a carrier material. Among them, it is preferred to use a Karstedt platinum catalyst.
[0095] The amount of the catalyst used in the present invention depends on the desired crosslinking rate and cost factors, but can be 1-35ppm, preferably 5-25ppm, and more preferably 5-20ppm, based on the weight of the precious metal. When the amount is less than 1ppm, it is possible that the amount is too low and the reaction cannot proceed. When the amount is higher than 35ppm, the cost is too high, and in order to extend the operation time, a large amount of inhibitors need to be added, which ultimately leads to a product with too high volatile matter, which is not environmentally friendly.
[0096] (Other ingredients)
[0097] In addition to the above-mentioned main components, the silicone rubber composition of the present invention may also contain other ingredients as additives as needed. As long as it is an additive commonly used in the art, it can be used within the scope that does not affect the effect of the present invention. Specifically, the rubber composition of the present invention may also contain: inhibitors, stabilizers, fillers, adhesion promoters, metal powders, fibers, pigments, dyes, plasticizers, matting agents, delustering agents, heat and / or light stabilizers, antistatic agents, flame retardants, antibacterial agents, antifungal agents, thixotropic agents, photocuring inhibitors or delay agents, etc., which are known substances that can be conventionally used in silicone rubber compositions. The above-mentioned additives can be used within the scope that does not affect the effect of the present invention.
[0098] Specifically, examples of fillers are inorganic fillers such as white carbon (silicon dioxide). When white carbon is used, it may have a specific surface area of 200-400 m 2 / g of fumed silica, the selection range is 0-50 parts by mass (relative to 100 parts by mass of silicone oil), which mainly plays a reinforcing role. When using silica as a filler, hydroxy silicone oil, silazane and deionized water can also be added together with the silica to treat the silica.
[0099] In addition, non-reinforcing fillers, i.e., fillers with a BET surface area of less than 50 m 2 / g filler, such as quartz powder, diatomaceous earth, calcium silicate, zirconium silicate, zeolite, metal oxides, such as iron oxide, zinc oxide, titanium dioxide, aluminum oxide, metal carbonates, such as calcium carbonate, magnesium carbonate, zinc carbonate, metal sulfates, mica, silicone resin, clay, stone powder, graphite and chalk. In addition, organic fillers can also be used.
[0100] Examples of inhibitors that can be used in the present invention include acetylenic alcohols, such as ethynylcyclohexanol (e.g., 1-ethynyl-1-cyclohexanol, also referred to as ECH) and 2-methyl-3-butyn-2-ol, which are well known in the art. The inhibitor is preferably selected from acetylenic alcohols, more preferably 1-ethynyl-1-cyclohexanol (ECH).
[0101] (Method for preparing silicone rubber composition)
[0102] The silicone rubber composition of the present invention can be prepared by preparing a base rubber and then mixing the required components into the base rubber.
[0103] Specifically, vinyl silicone oil I can be mixed at a temperature of 60 to 180°C, and a base rubber mixture can be obtained according to the fillers and additives required. After vacuum treatment and dilution with vinyl silicone oil I, a base rubber can be obtained; further, vinyl silicone oil I, vinyl silicone oil II, vinyl silicone oil III and a catalyst are mixed in the base rubber to obtain component A; vinyl silicone oil I, vinyl silicone oil II, vinyl silicone oil III and a sulfur-containing siloxane-treated complex, hydrogen-containing silicone oil and additives as required are mixed in the base rubber to obtain component B. When making silicone rubber products, component A and component B are mixed, and rubber products are obtained after vulcanization. There is no particular restriction on the vulcanization conditions, as long as the vulcanization conditions commonly used in the art can be used. For example, it can be 120°C×10min or 170°C×10min.
[0104] The equipment used for mixing or compounding is not particularly limited, and any equipment commonly used in the art may be used, and examples thereof include a kneader, a planetary mixer, and an extruder.
[0105] (Rubber products)
[0106] The silicone rubber composition of the present invention can be used to prepare self-penetrating oil silicone rubber. The silicone rubber according to the present invention is a self-penetrating oil addition type liquid silicone rubber that meets the comprehensive properties of high tear resistance, heat resistance, oil resistance, low pressure change, etc. It belongs to a special liquid silicone rubber product and can be widely used in the fields of electricity, automobiles, medical treatment, etc. Specifically, it can be used for cable casings, automobile plug-in parts, O-rings, sealing gaskets, medical diaphragms, brakes, various joints, sealants and gaskets, etc., and can provide strong and lasting sealing.
[0107] Example
[0108] The present invention will be described in more detail below by way of examples and comparative examples, but the present invention is not limited to the following examples and comparative examples.
[0109] The viscosity in the examples is measured using a Haake tester (model TYP006-0572) at 25° C. In the examples, “%” means “% by weight” and “parts” means “parts by weight” unless otherwise specified.
[0110] Preparation Example 1: Preparation of bis-[3-(triethoxysilyl)propyl]-disulfide modified silicon micropowder
[0111] 21.68g of bis-[3-(triethoxysilyl)propyl]-disulfide was added to 100g of silicon micropowder with an average particle size of 20μm, stirred at a stirring speed of 1000rpm for 20min, then heated to 120°C, the speed was increased to 2000rpm, and maintained for 30min. Then, the reaction byproducts were removed under reduced pressure to obtain a white powder, i.e., silicon micropowder treated with bis-[3-(triethoxysilyl)propyl]-disulfide.
[0112] Preparation Example 2: Preparation of white carbon black modified with γ-thiocyanatopropyltriethoxysilane
[0113] The same method as in Preparation Example 1 was used to obtain γ-thiocyanatopropyltriethoxysilane-treated white carbon, except that 21.68 g of bis-[3-(triethoxysilyl)propyl]-disulfide was replaced by 19.54 g of γ-thiocyanatopropyltriethoxysilane and 100 g of silicon micropowder was replaced by 100 g of white carbon.
[0114] Preparation Example 3: Preparation of bis-[3-(triethoxysilyl)propyl]-disulfide-modified calcium carbonate
[0115] Calcium carbonate treated with bis-[3-(triethoxysilyl)propyl]-disulfide was obtained by the same method as in Preparation Example 1 except that 100 g of 20 μm silicon powder was replaced by 100 g of calcium carbonate.
[0116] Example 1
[0117] 100 parts of the first vinyl silicone oil (viscosity 60000mPa·s, vinyl content 0.087%), 300m 2 50 parts of fumed silica with a specific surface area of 1.377 W / g, 14 parts of hexamethyldisilazane, 0.5 parts of divinyltetramethylsilazane, and 8 parts of deionized water were mixed in a kneader at a temperature of 80°C and under the protection of an inert atmosphere, and vacuumed at a temperature of 150°C. After the vacuuming treatment, 20 parts of the first vinyl silicone oil (viscosity of 60,000 mPa·s, vinyl content of 0.087%) were added for dilution to obtain a base rubber mixture.
[0118] To 100 parts of the above-mentioned base rubber mixture, add 3 parts of vinyl silicone oil I (viscosity of 20,000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2,000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10,000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, and 0.028 parts of platinum catalyst (platinum content of 100,000 ppm) to obtain component A liquid silicone rubber.
[0119] To 100 parts of the above base rubber mixture, add 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, 0.4 parts of bis-[3-(triethoxysilyl)propyl]-disulfide treated silicon micropowder, 1.7 parts of end-side structure hydrogen-containing silicone oil with an H mass fraction of 0.75%, and 0.18 parts of inhibitor ECH to obtain component B liquid silicone rubber.
[0120] Example 2
[0121] To 100 parts of the base rubber mixture obtained in Example 1, add 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 19000 mPa·s, vinyl content of 2%), 4 parts of phenyl silicone oil, and 0.028 parts of platinum catalyst (platinum content of 100,000 ppm) to obtain component A liquid silicone rubber.
[0122] To 100 parts of the base rubber mixture obtained in Example 1, 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 19000 mPa·s, vinyl content of 2%), 4 parts of phenyl silicone oil, 0.4 parts of white carbon black treated with γ-thiocyanatopropyltriethoxysilane, 1.7 parts of hydrogenated silicone oil with an end-side structure having an H mass fraction of 0.75%, and 0.18 parts of inhibitor ECH were added to obtain component B liquid silicone rubber.
[0123] Example 3
[0124] To 100 parts of the base rubber mixture obtained in Example 1, add 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, and 0.028 parts of platinum catalyst (platinum content of 100,000 ppm) to obtain component A liquid silicone rubber.
[0125] To 100 parts of the base rubber mixture obtained in Example 1, 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, 0.1 part of silicon micropowder treated with bis-[3-(triethoxysilyl)propyl]-disulfide, 1.7 parts of hydrogenated silicone oil with an end-side structure having an H mass fraction of 0.75%, and 0.18 parts of inhibitor ECH were added to obtain liquid silicone rubber of component B.
[0126] Example 4
[0127] To 100 parts of the base rubber mixture obtained in Example 1, add 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, and 0.028 parts of platinum catalyst (platinum content of 100,000 ppm) to obtain component A liquid silicone rubber.
[0128] To 100 parts of the base rubber mixture obtained in Example 1, 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, 0.077 parts of bis-[3-(triethoxysilyl)propyl]-disulfide-treated silicon micropowder, 1.7 parts of hydrogenated silicone oil with an end-side structure having an H mass fraction of 0.75%, and 0.18 parts of inhibitor ECH were added to obtain component B liquid silicone rubber.
[0129] Example 5
[0130] To 100 parts of the base rubber mixture obtained in Example 1, add 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, and 0.028 parts of platinum catalyst (platinum content of 100,000 ppm) to obtain component A liquid silicone rubber.
[0131] To 100 parts of the base rubber mixture obtained in Example 1, 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, 0.77 parts of bis-[3-(triethoxysilyl)propyl]-disulfide-treated silicon micropowder, 1.7 parts of hydrogenated silicone oil with an end-side structure having an H mass fraction of 0.75%, and 0.18 parts of inhibitor ECH were added to obtain component B liquid silicone rubber.
[0132] Example 6
[0133] To 100 parts of the base rubber mixture obtained in Example 1, add 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, and 0.028 parts of platinum catalyst (platinum content of 100,000 ppm) to obtain component A liquid silicone rubber.
[0134] To 100 parts of the base rubber mixture obtained in Example 1, 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, 0.77 parts of calcium carbonate treated with bis-[3-(triethoxysilyl)propyl]-disulfide, 1.7 parts of hydrogenated silicone oil with an end-side structure having an H mass fraction of 0.75%, and 0.18 parts of inhibitor ECH were added to obtain liquid silicone rubber of component B.
[0135] Comparative Example 1
[0136] To 100 parts of the base rubber mixture obtained in Example 1, add 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 4 parts of phenyl silicone oil, and 0.028 parts of platinum catalyst (platinum content of 100,000 ppm) to obtain component A liquid silicone rubber.
[0137] To 100 parts of the base rubber mixture obtained in Example 1, 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 4 parts of phenyl silicone oil, 0.4 parts of bis-[3-(triethoxysilyl)propyl]-disulfide-treated silicon micropowder, 1.1 parts of end-side structure hydrogenated silicone oil with an H mass fraction of 0.75%, and 0.18 parts of inhibitor ECH were added to obtain component B liquid silicone rubber.
[0138] Comparative Example 2
[0139] To 100 parts of the base rubber mixture obtained in Example 1, add 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, and 0.028 parts of platinum catalyst (platinum content of 100,000 ppm) to obtain component A liquid silicone rubber.
[0140] To 100 parts of the base rubber mixture obtained in Example 1, 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, 1.7 parts of hydrogenated silicone oil with an end-side structure having an H mass fraction of 0.75%, and 0.18 parts of inhibitor ECH were added to obtain component B liquid silicone rubber.
[0141] Comparative Example 3
[0142] To 100 parts of the base rubber mixture obtained in Example 1, add 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 4 parts of phenyl silicone oil, and 0.028 parts of platinum catalyst (platinum content of 100,000 ppm) to obtain component A liquid silicone rubber.
[0143] To 100 parts of the base rubber mixture obtained in Example 1, 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 4 parts of phenyl silicone oil, 1.1 parts of hydrogenated silicone oil with an end-side structure having an H mass fraction of 0.75%, and 0.18 g of inhibitor ECH were added to obtain liquid silicone rubber of component B.
[0144] Comparative Example 4
[0145] To 100 parts of the base rubber mixture obtained in Example 1, add 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 19000 mPa·s, vinyl content of 2%), 4 parts of phenyl silicone oil, and 0.028 parts of platinum catalyst (platinum content of 100,000 ppm) to obtain component A liquid silicone rubber.
[0146] To 100 parts of the base rubber mixture obtained in Example 1, 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2%), 4 parts of phenyl silicone oil, 0.4 parts of bis-[3-(triethoxysilyl)propyl]-disulfide-treated silicon micropowder, 2.5 parts of hydrogenated silicone oil with an end-side structure having an H mass fraction of 0.75%, and 0.18 parts of inhibitor ECH were added to obtain component B liquid silicone rubber.
[0147] Comparative Example 5
[0148] To 100 parts of the base rubber mixture obtained in Example 1, add 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 19000 mPa·s, vinyl content of 2%), 4 parts of phenyl silicone oil, and 0.028 parts of platinum catalyst (platinum content of 100,000 ppm) to obtain component A liquid silicone rubber.
[0149] To 100 parts of the base rubber mixture obtained in Example 1, 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 19000 mPa·s, vinyl content of 2%), 4 parts of phenyl silicone oil, 0.4 parts of bis-[3-(triethoxysilyl)propyl]-disulfide, 1.7 parts of hydrogenated silicone oil with an end-side structure having an H mass fraction of 0.75%, and 0.18 parts of inhibitor ECH were added to obtain component B liquid silicone rubber.
[0150] Comparative Example 6
[0151] To 100 parts of the base rubber mixture obtained in Example 1, add 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, and 0.028 parts of platinum catalyst (platinum content of 100,000 ppm) to obtain component A liquid silicone rubber.
[0152] To 100 parts of the base rubber mixture obtained in Example 1, 3 parts of vinyl silicone oil I (viscosity of 20000 mPa·s, vinyl content of 0.09%), 4 parts of vinyl silicone oil II (viscosity of 2000 mPa·s, vinyl content of 0.55%), 2.5 parts of vinyl silicone oil III (viscosity of 10000 mPa·s, vinyl content of 2.2%), 4 parts of phenyl silicone oil, 1.49 parts of bis-[3-(triethoxysilyl)propyl]-disulfide-treated silicon micropowder, 1.7 parts of hydrogenated silicone oil with an end-side structure having an H mass fraction of 0.75%, and 0.18 parts of inhibitor ECH were added to obtain component B liquid silicone rubber.
[0153] Comparative Example 7
[0154] According to Example 7 of US5977249, a rubber sample was prepared.
[0155] Rubber synthesis and testing
[0156] The prepared A and B components of each embodiment and comparative example were mixed in a weight ratio of 1:1, and then a vulcanization test was performed. The molding conditions were 170° C.×10 min, and two-stage vulcanization was not required.
[0157] Afterwards, the obtained rubber sample slices were tested for hardness, tensile strength / elongation at break, tear strength, rebound, compression set, scorch time T10, vulcanization time T90, and maximum torque MH. The hardness was measured according to ASTM D 2240. The tensile strength / elongation at break was measured according to ASTM D 412. The tear strength was measured according to ASTM D 624B. The rebound was measured according to ASTM D 1054. The compression set was measured according to ASTM D 395. The scorch time T10, the vulcanization time T90, and the maximum torque MH were measured according to the group standard "T / FSI 076-2022 Self-lubricating liquid silicone rubber for connectors".
[0158]
[0159] It can be seen from the data in Table 1 that even the comparative examples with low short-term compression set do not perform well after long-term durability tests. In contrast, the rubber product of the present invention can achieve low compression set with high temperature durability without affecting mechanical properties.
Claims
1. A silicone rubber composition comprising: (A) a base silicone oil comprising: a dual-end vinyl silicone oil (vinyl silicone oil I) with a viscosity of 10000-100000 mPa·s, a side-chain vinyl silicone oil (vinyl silicone oil II) with a viscosity of 500-20000 mPa·s, and a terminal vinyl silicone oil (vinyl silicone oil III) with a viscosity of 5000-20000 mPa·s, the amount of which is 100 parts by mass; (B) a composite modified with a sulfur-containing silane compound in an amount of 0.05-0.5 parts by mass; (C) hydrogen-containing silicone oil in an amount such that the number of silicon-hydrogen bonds / the number of vinyl groups in the silicone rubber composition = 1.2-1.5; (D) A noble metal catalyst in an amount of 1 to 35 ppm based on the weight of the noble metal. 2 . The silicone rubber composition according to claim 1 , further comprising at least one of the following substances: an inhibitor and a filler.
3. The silicone rubber composition according to claim 1, wherein in 100 parts by mass of the base silicone oil, Vinyl silicone oil I is 60-98 parts; Vinyl silicone oil II is 1-20 parts; Vinyl silicone oil III is 1-20 parts.
4. The silicone rubber composition according to claim 1, wherein the composition further comprises phenyl silicone oil.
5. The silicone rubber composition according to claim 1, wherein the vinyl content of the terminal vinyl silicone oil is 1-20 wt%. 6 . The silicone rubber composition according to claim 1 , wherein the compound comprises at least one of the following substances: silicon micropowder, clay, calcium carbonate, white carbon black, aluminum hydroxide, magnesium hydroxide, silicone oil, and silicone resin.
7. A rubber product prepared using the silicone rubber composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Silicone rubber composition with low compression set and preparation method thereof
CN115895271A
Liquid silicone rubber with improved compression set
US5977249A
Low compression set silicon rubber composition
WO2019175092A1
Cited By
Self-healing single-component heat-conducting gel and method for preparing same
CN122832514A
Low-compression-set silicone rubber composition having high-temperature durability, and rubber product
WO2026052062A1