Foam resin molding and laminated resin molding
By integrating fibrous and particulate PTFE within polycarbonate resin, the foamed resin molded products maintain lightweight properties and prevent strength loss during heat shaping processes like vacuum forming, addressing the challenge of bubble uniformity and strength retention.
Patent Information
- Application Number
- JP2023047651
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Existing foamed resin molded products face challenges in maintaining strength after heat shaping processes like vacuum forming, as the size and shape of bubbles formed during foam molding often become non-uniform, leading to irregular strength and lightness issues.
Incorporating polycarbonate resin with fibrous polytetrafluoroethylene (PTFE) and particulate PTFE, where fibrous PTFE has an average particle size of less than 40 μm, and specific content ranges of 0.1% to 1.0% by mass, and particulate PTFE has a content of 0.1% to 2.0% by mass, to stabilize fine cell formation and suppress strength loss during heat shaping.
The solution ensures lightweight properties while effectively preventing a decrease in strength after heat forming, such as vacuum forming, by stabilizing fine bubble formation and enhancing mechanical properties.
Smart Images

Figure 2024136513000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a foamed resin molded article produced by foam molding, and a laminated resin molded article in which a skin layer is laminated on a main surface of the foamed resin molded article. [Background technology]
[0002] In recent years, foamed resin molded bodies are formed into desired shapes by thermal shaping such as vacuum forming, and are used to manufacture resin products according to their applications. Resin products manufactured using foamed resin molded bodies as materials have attracted attention because they can be lightweight, making them more convenient to use, and can reduce carbon dioxide emissions.
[0003] It is difficult to control the size, shape, and other conditions of the bubbles formed during foam molding of a resin foam. If the size of the numerous bubbles becomes non-uniform and if multiple bubbles coalesce to form irregular bubbles, this affects the strength and lightness of the resin foam and its resin products. In response to this, it is known to add polytetrafluoroethylene (hereinafter referred to as PTFE) when molding a resin foam, as described in the following document.
[0004] WO 2008 / 038639 (Patent Document 1) discloses a foamed sheet containing 80-99.5% by weight of a thermoplastic resin and 0.5-20% by weight of PTFE. The foamed sheet has fine bubbles by defining the dispersed particle size and particle number of PTFE and the average bubble size in the direction perpendicular to the direction of taking the foamed sheet, thereby achieving excellent surface appearance, flexibility, light weight, formability, and high light reflectivity.
[0005] JP 2009-1674 A (Patent Document 2) discloses a foam molded article. The foam molded article is produced by foam molding a thermoplastic resin composition containing a thermoplastic resin and fluororesin particles having an average particle size of 1-100 μm, with the number ratio of particles having a particle size of 0.1 μm or more and less than 1.0 μm being 50% or less by number, and having a melt flow rate (JIS K7210) of 10-200 g / 10 min. As a result, Patent Document 2 provides a foam molded article with excellent foaming characteristics and soft feel.
[0006] Japanese Patent Laid-Open Publication No. 2000-72912 (Patent Document 3) discloses a foam containing a foaming nucleating agent. The foaming nucleating agent is composed of a fluororesin powder in which the total frequency of particles with a particle size of 0.1 to 0.5 μm is at least 50% by number, and the total frequency of particles with a particle size of 5 μm or more is 40% by number or less. This makes it possible to produce an organic polymer foam that is improved in terms of the degree of foaming, cell fineness, and foaming uniformity.
[0007] Japanese Patent Laid-Open Publication No. 2006-77218 (Patent Document 4) discloses an extruded thermoplastic resin foam to which 0.01 to 1.0 parts by weight of polytetrafluoroethylene powder is added to 100 parts by weight of the thermoplastic resin. The average particle size of the polytetrafluoroethylene powder is 0.5 μm or more and less than 1 time the average cell film thickness of the foam. This prevents a decrease in the closed cell ratio and makes the cell film uniform, improving the appearance.
[0008] Japanese Patent Application Laid-Open No. 2008-88213 (Patent Document 5) discloses a polyester foam sheet containing PTFE as a foam nucleating agent, thereby providing a foam having fine bubbles.
[0009] JP 2016-172872 A (Patent Document 6) and JP 2014-80575 A (Patent Document 7) disclose polycarbonate-based resin foam sheets for thermoforming. Each of the polycarbonate-based resin foam sheets for thermoforming has a fluororesin powder such as PTFE added thereto as a foaming regulator during foaming.
[0010] JP 2001-187824 A (Patent Document 8) discloses a mixed resin extrusion foam board of polypropylene-based resin and polystyrene-based resin. The extrusion foam board is obtained by mixing 0.01 to 0.5 parts by weight of polytetrafluoroethylene having a primary particle diameter of 1 μm or less with respect to 100 parts by weight of polypropylene-based resin and polystyrene-based resin in an extruder, and then pressing and foaming. This increases the closed cell ratio of the polypropylene-based resin extrusion foam board, reduces the average cell diameter, and reduces the density. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] International Publication No. 2008 / 038639 [Patent Document 2] JP 2009-1674 A [Patent Document 3] JP 2000-72912 A [Patent Document 4] JP 2006-77218 A [Patent Document 5] JP 2008-88213 A [Patent Document 6] JP 2016-172872 A [Patent Document 7] JP 2014-80575 A [Patent Document 8] JP 2001-187824 A Summary of the Invention [Problem to be solved by the invention]
[0012] Usually, when a foamed resin molded body is heat-formed into a desired shape by vacuum forming or the like, the foamed resin molded body is stretched during the vacuum forming. Therefore, the strength of the resin molded product after vacuum forming of the foamed resin molded body is reduced. Therefore, in order to suppress such a decrease in the strength of the resin molded product, there is room for further consideration of the foamed resin molded body before heat forming such as vacuum forming.
[0013] Patent Documents 1 to 8 do not consider how to prevent a decrease in strength of a resin molded product after vacuum molding.
[0014] An object of the present disclosure is to provide a foamed resin molded article that ensures lightweight properties due to foaming and can suppress a decrease in strength of the resin molded article after thermal shaping such as vacuum molding. [Means for solving the problem]
[0015] In order to solve the above problems, the present disclosure provides the following solutions. That is, the foamed resin molded article according to the present disclosure may be a foamed resin molded article containing a polycarbonate resin. It may contain fibrous polytetrafluoroethylene (hereinafter referred to as PTFE) and particulate PTFE having an average particle size of less than 40 μm. The fibrous PTFE may have a content of 0.1% by mass or more and 1.0% by mass or less with respect to the foamed resin molded article. The particulate PTFE may have a content of 0.1% by mass or more and 2.0% by mass or less with respect to the foamed resin molded article. Effect of the Invention
[0016] The foamed resin molded article and laminated resin molded article according to the present disclosure ensure lightweight properties due to foaming, and can suppress a decrease in strength of the resin molded article after thermal shaping such as vacuum molding. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is an external perspective view of a foamed resin molded article according to this embodiment. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of the foamed resin molded article shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] (Configuration 1) The foamed resin molded article according to the embodiment of the present disclosure may be a foamed resin molded article containing a polycarbonate resin. It may contain fibrous polytetrafluoroethylene (hereinafter referred to as PTFE) and particulate PTFE having an average particle size of less than 40 μm. The fibrous PTFE may have a content of 0.1% by mass or more and 1.0% by mass or less with respect to the foamed resin molded article. The particulate PTFE may have a content of 0.1% by mass or more and 2.0% by mass or less with respect to the foamed resin molded article.
[0019] This makes it possible to obtain a foamed resin molded article in which finer bubbles are stably formed, thereby making it possible to suppress a decrease in strength of the foamed resin molded article after thermal shaping such as vacuum molding while ensuring the light weight achieved by foaming.
[0020] (Configuration 2) In the foamed resin molded product of Configuration 1, the fibrous PTFE may have a content of 0.2% by mass or more relative to the foamed resin molded product, which can further suppress a decrease in strength of the foamed resin molded product after thermal shaping such as vacuum molding.
[0021] (Configuration 3) In the foamed resin molded body of the configuration 1 or 2, the particulate PTFE may have a content of 0.2 mass% or more relative to the foamed resin molded body, which can further suppress a decrease in strength after the foamed resin molded body is subjected to thermal shaping such as vacuum molding.
[0022] (Configuration 4) Furthermore, the laminated resin molded product according to the embodiment of the present disclosure may have a foamed resin molded product of any one of configurations 1 to 3, and a skin layer made of a non-foamed resin laminated on one main surface of the foamed resin molded product, thereby making it possible to further suppress a decrease in strength of the foamed resin molded product after thermal shaping such as vacuum forming.
[0023] (Configuration 5) In the laminated resin molded product of Configuration 4, the skin layer may have a melt viscosity of 5,500 Pa s or more. This makes it possible to further suppress the decrease in strength of the foamed resin molded product after thermal shaping such as vacuum molding.
[0024] Hereinafter, an embodiment of a foamed resin molded body 1 and a laminated resin molded body 10 according to the present disclosure will be specifically described with reference to Fig. 1 and Fig. 2. Note that the same or corresponding configurations in the figures are given the same reference numerals, and the same description will not be repeated. Note that, in order to make the description easier to understand, the configurations are shown in a simplified or schematic manner, and some of the components are omitted in the drawings referred to below.
[0025] The foamed resin molded body 1 contains a polycarbonate resin from the viewpoint of improving light weight and mechanical strength. However, the foamed resin molded body 1 may contain an engineering plastic and a super engineering plastic. Engineering plastics or super engineering plastics have excellent heat resistance and mechanical strength. Engineering plastics are thermoplastic resins having a deflection temperature under load of 100°C or more. Engineering plastics are thermoplastic resins having a deflection temperature under load of 100°C or more. Examples of engineering plastics include polycarbonate (PC), modified polyphenylene ether (m-PPE), and syndiotactic polystyrene (SPS). Super engineering plastics are thermoplastic resins having a deflection temperature under load of 150°C or more. Examples of super engineering plastics include polyphenylene sulfide (PPS), polysulfone (PSF), polyethersulfone (PES), polyarylate (PAR), polyamideimide (PAI), thermoplastic polyimide (PI), polyetherimide (PEI), and liquid crystal polymer (LCP). The resin material used in the foamed resin molded body 1 of the present disclosure may contain at least one selected from the group consisting of engineering plastics and super engineering plastics. For example, the polycarbonate resin is contained in an amount of 50% by mass or more, preferably 70% by mass or more, and more preferably 90% by mass or more of the resin material contained in the foamed resin molded body 1. An ultraviolet absorbing agent, an anti-aging agent, etc. may be added to the resin material of the foamed resin molded body 1. The deflection temperature under load is measured in accordance with ISO075-2B under a load of 1.81 MPa.
[0026] In this embodiment, the foamed resin molded body 1 contains fibrous PTFE and particulate PTFE. PTFE is one of various fluororesins. Therefore, the foamed resin molded body 1 may contain fibrous fluororesin and particulate fluororesin instead of fibrous PTFE and particulate PTFE. Examples of the fluororesin include ETFE resin, which is a copolymer of tetrafluoroethylene and ethylene, polyphthalamide (PPA) resin, and FEP resin, which is a copolymer of tetrafluoroethylene and hexafluoropropylene.
[0027] The fibrous PTFE has a content of 0.1% by mass or more and 1.0% by mass or less with respect to the foamed resin molded body 1. The foamed resin molded body 1 is manufactured by kneading PTFE with a molten resin material as described later. The fibrous PTFE is PTFE formed into a fibrous shape by kneading PTFE having fibril-forming ability during manufacturing and fibrillating it in the foamed resin molded body 1. Therefore, in the present disclosure, the content of the fibrous PTFE is defined as the content of PTFE having fibril-forming ability kneaded during the manufacturing of the foamed resin molded body 1. The content of the fibrous PTFE is preferably 0.1% by mass or more, preferably 0.2% by mass or more, more preferably 0.25% by mass or more, and is preferably 1.0% by mass or less, preferably 0.75% by mass or less, more preferably 0.5% by mass or less, from the viewpoint of suppressing a decrease in strength of the foamed resin molded body 1 after vacuum molding while ensuring the lightness of the foamed resin molded body 1. The fibrous PTFE has an aspect ratio of 5 or more in the foamed resin molded body 1.
[0028] The fibril-forming PTFE is preferably a high molecular weight PTFE. The fibril-forming PTFE has a number average molecular weight of preferably 1 to 10 million, more preferably 2 to 9 million, as determined from the standard specific gravity. As a result, the fibril-forming PTFE is formed into a fibrous form by bonding PTFE to each other by an external action such as shear force during kneading. The fibril-forming PTFE may be a solid or may be in the form of an aqueous dispersion. The fibril-forming PTFE may be mixed with other resins by a known method, for example, a method of mixing an aqueous dispersion of PTFE with dried organic polymer particles, in order to improve dispersibility, flame retardancy, or mechanical properties. The fibrous PTFE may be formed by kneading the fibril-forming PTFE mixed with other resins in this way. The fibrous PTFE can be produced by a known method such as an emulsion polymerization method.
[0029] The particulate PTFE has a content of 0.1% by mass or more and 2.0% by mass or less with respect to the foamed resin molded body 1. The particulate PTFE is PTFE that is kneaded with PTFE that does not have fibrillation ability during production, and maintains a particulate shape without fibrillation in the foamed resin molded body 1. Therefore, in the present disclosure, the content of the particulate PTFE is defined as the content of PTFE that does not have fibrillation ability kneaded during the production of the foamed resin molded body 1. The content of the particulate PTFE is preferably 0.1% by mass or more, preferably 0.2% by mass or more, more preferably 0.25% by mass or more, and is preferably 2.0% by mass or less, preferably 1.0% by mass or less, more preferably 0.5% by mass or less, from the viewpoint of suppressing a decrease in strength of the foamed resin molded body 1 after vacuum molding while ensuring the lightness of the foamed resin molded body 1. The particulate PTFE has an aspect ratio of less than 5 in the foamed resin molded body 1.
[0030] The PTFE that does not have the ability to form fibrils is preferably a low molecular weight PTFE. The PTFE that does not have the ability to form fibrils has a number average molecular weight calculated from the standard specific gravity of preferably several thousand to one million, more preferably 5,000 to 600,000, and most preferably 10,000 to 600,000. This means that even if an external action such as a shear force is applied during kneading, the PTFE does not have the ability to bond together and become fibrous. The PTFE that does not have the ability to form fibrils can be produced by known methods such as emulsion polymerization, suspension polymerization, telomerization of tetrafluoroethylene in a solvent, baking of low molecular weight PTFE, thermal decomposition of high molecular weight PTFE, or decomposition by radiation.
[0031] The aspect ratios of the fibrous PTFE and particulate PTFE are measured as follows. The largest diameter (major axis) and smallest diameter (minor axis) are measured in the cross section where the cross-sectional area of each of the fibrous PTFE and particulate PTFE contained in the foamed resin molded body 1 is the largest. The aspect ratios of the fibrous PTFE and particulate PTFE are calculated by dividing the major axis by the minor axis (major axis / minor axis).
[0032] More specifically, the foamed resin molded body 1 is dissolved using a solvent (tetrahydrofuran (THF)), and the dissolved residue is taken out. The dissolved residue is then washed multiple times, for example, three times, with the same solvent, and the washed residue is taken out. The above-mentioned solvent may be appropriately selected from the viewpoint of satisfactorily dissolving the engineering plastics and super-engineering plastics, such as polycarbonate resins, contained in the foamed resin molded body 1, while substantially not dissolving the fluororesin.
[0033] In addition, in the multiple washings described above, the solvent used the first time is left for two hours to obtain a washing solution. 80% of the supernatant of the washing solution is discarded. To the remaining 20% of the washing solution, a new solvent is added in the same amount as the discarded washing solution and mixed to obtain a mixed solution. The mixed solution is left for two hours, and 80% of the supernatant of the mixed solution is discarded. To the remaining 20% of the mixed solution, a new solvent is added in the same amount as the discarded mixed solution and mixed. The mixed solution is evaporated after repeating the same process multiple times, for example three times, and the volatile residue is removed.
[0034] The above-mentioned cleaning residue thus extracted is fibrous. The aspect ratio of the fibrous PTFE is calculated by dividing the major axis of the fibrous cleaning residue by the minor axis. Meanwhile, the above-mentioned volatile residue is particulate. The aspect ratio of the particulate PTFE is calculated by dividing the major axis of the particulate volatile residue by the minor axis. In addition, although fibrous residues may very rarely occur in the volatile residue, these are ignored.
[0035] The particulate PTFE has an average particle size of less than 40 μm. From the viewpoint of stably forming fine bubbles in the foamed resin molded body 1, the average particle size of the particulate PTFE is preferably less than 40 μm, more preferably less than 25 μm, and more preferably less than 10 μm, and is preferably 10 nm or more, more preferably 4 μm or more, and more preferably 8 μm or more.
[0036] The average particle size of particulate PTFE is the volume average particle size, and means the median diameter (D50) obtained by laser diffraction scattering type particle size distribution measurement. Specifically, the volume average particle size is obtained by the following measurement method. The volume-based particle size distribution of the above-mentioned volatile residue is obtained by injection type dry measurement using a laser diffraction type particle size distribution measurement device (for example, Shimadzu Corporation, model number "SALD-2300"). Using the obtained particle size distribution, the cumulative distribution for the volume is subtracted from the small particle size side, and the particle size at which the cumulative 50% of all particles is taken as D50. Note that, as mentioned above, fibrous residues may very rarely occur in the volatile residue, but this is to be ignored.
[0037] As described above, the foamed resin molding 1 contains a balanced amount of fibrous PTFE and particulate PTFE having an average particle size of less than 40 μm, thereby ensuring the lightweight properties achieved by foaming while suppressing the decrease in strength after thermal shaping such as vacuum molding.
[0038] The average fiber diameter of the fibrous PTFE is preferably less than 500 nm, and more preferably less than 100 nm. The lower limit of the average fiber diameter is not particularly limited, but is preferably 1 nm or more. This allows for more stable formation of finer bubbles, and suppresses the decrease in strength after thermal shaping such as vacuum molding. The average fiber diameter is measured as follows. First, the foamed resin molded body 1 is dissolved in tetrahydrofuran (THF) and washed, and the washing residue is taken out and dried as described above. Since the thing taken out as the washing residue is usually fibrous PTFE, an image of the washing residue is obtained by magnifying it at a magnification of 10,000 times using a scanning electron microscope (SEM), and the washing residue is observed. Then, the image is divided into squares at intervals of 5 μm, and the fiber diameter of the fiber with the smallest diameter among the fibers present in each square is measured. Finally, the average value of each fiber diameter is obtained. In this way, the average fiber diameter can be measured.
[0039] Next, an embodiment of the laminated resin molded product 10 will be specifically described with reference to Fig. 2. As shown in Fig. 2, the laminated resin molded product 10 may have a skin layer 2 on at least one of the main surfaces of the foamed resin molded product 1 described above. The skin layer 2 is made of a non-foamed resin. The non-foamed resin is a resin that does not contain bubbles caused by a foaming agent when the skin layer 2 is molded.
[0040] The skin layer 2 is made of, for example, a polycarbonate resin. The skin layer 2 may be made of a thermoplastic resin that can adhere well to the foamed resin molded body 1. More specifically, it is particularly preferable that the resin material of the skin layer 2 is the same resin material as that of the foamed resin molded body 1. The skin layer 2 may be made of a reinforced resin containing an inorganic filler in order to reinforce the skin layer 2. This configuration of the skin layer 2 makes it possible to efficiently improve the strength while reducing the weight and improving the strength. Examples of the inorganic filler include glass fiber, carbon fiber, aramid fiber, talc, and mica.
[0041] The melt viscosity of the skin layer 2 is preferably 5500 Pa·s or more, and more preferably 7000 Pa·s. The upper limit of the melt viscosity of the skin layer 2 is not particularly limited, but is preferably 10000 Pa·s. This makes it possible to suppress damage to the skin layer 2 during vacuum molding, and also to appropriately form the skin layer 2 during molding of the laminated resin molding 10. As a result, it is possible to suppress a decrease in strength of the resin molding after vacuum molding of the laminated resin molding 10. The melt viscosity is a value in accordance with ISO11443, measured at a measurement temperature of 230°C, a capillary: L / D=5 / 1, and an apparent shear rate of 91 sec-1.
[0042] Next, a method for manufacturing the foamed resin molded body 1 and the laminated resin molded body 10 will be described (not shown). First, resin pellets and powdered PTFE, which are resin materials, are charged into the screw cylinder of the main extruder. The resin pellets are made of, for example, polycarbonate resin. The resin pellets and powdered PTFE are heated in the screw cylinder to generate a molten resin. The powdered PTFE contains PTFE with fibril-forming ability and PTFE without fibril-forming ability in the above-mentioned content ratios. Next, a foaming agent is injected into the molten resin from a foaming agent injection cylinder attached to the screw cylinder of the main extruder. The foaming agent is dissolved in the molten resin by the above-mentioned screw cylinder, and is kneaded and uniformly dispersed. In this way, a mixed molten resin is generated. By this kneading, a shear force is applied to the powdered PTFE through the polycarbonate resin in the mixed molten resin, and as a result, the PTFE with fibril-forming ability among the powdered PTFE is stretched by the shear force and formed into a fibrous form, becoming fibrous PTFE. At that time, the PTFE that does not have fibril forming ability among the powdered PTFE becomes particulate PTFE. The mixed molten resin is discharged from the die outlet to form the foamed resin molded body 1. In addition, when the skin layer 2 is provided, that is, when the laminated resin molded body 10 is manufactured, at the same time, resin pellets that are the resin material are charged into each of the screw cylinders of the two sub-extruders, and heated and melted to generate two molten resins. One of the two molten resins is discharged from the die outlet to form the skin layer 2 provided on one main surface of the foamed resin molded body 1, and the other is discharged from the die outlet to form the skin layer 2 provided on the other main surface of the foamed resin molded body 1. The mixed molten resin and the two molten resins are merged in the die from each extruder, and discharged from the die outlet so that the skin layer 2 is laminated on one and the other main surfaces of the foamed resin molded body 1. The mixed molten resin is foamed when extruded from the die outlet into the atmosphere. In this way, the foamed resin molded body 1 can be manufactured. The foaming method may be a physical foaming method using an inert gas such as nitrogen or carbon dioxide as a foaming agent, or a chemical foaming method. The foamed resin molded body 1 or laminated resin molded body 10 extruded in this manner is transported to a cutting machine by a take-up machine.The cutter cuts the foamed resin molded body 1 or the laminated resin molded body 10 into a desired shape. The method for producing the foamed resin molded body 1 and the laminated resin molded body 10 is not particularly limited and may be injection molding or the like.
[0043] The foamed resin molded body 1 and laminated resin molded body 10 thus manufactured can be shaped into a desired shape by thermal shaping such as vacuum molding and used in the following applications: For example, wide products and parts such as mobility materials, such as signs or automobile exterior materials, which require comparative strength, products and parts that require heat resistance and strength, such as batteries or trays for heat-generating components used in manufacturing processes involving heating steps, or products and parts that require weight reduction. The foamed resin molded body 1 contains polycarbonate resin and is foam-molded by co-extrusion molding, making it suitable as a material for molding these products and parts.
[0044] Products and parts made from the foamed resin molded body 1 and the laminated resin molded body 10 can reduce the amount of resin used. As a result, the foamed resin molded body 1 according to this embodiment can contribute to improving resource utilization efficiency, reducing the burden of transportation, reducing energy consumption, and reducing CO2 emissions. By providing the foamed resin molded body 1 to society, it is possible to contribute to achieving Goal 7 (Affordable and Clean Energy), Goal 9 (Industry, Innovation and Infrastructure), and Goal 11 (Sustainable Cities and Communities) out of the 17 Sustainable Development Goals (SDGs) established by the United Nations.
[0045] Although the embodiments have been described above, the present disclosure is not limited to the above-described embodiments, and various modifications are possible without departing from the spirit of the present disclosure.
[0046] (Example) As shown in Table 1 below, foamed resin molded bodies of Examples 1 to 11 and Comparative Examples 1 to 8 were prepared, and the density of each foamed resin molded body and the reduction rate of the yield point stress of the resin molded article relative to the yield point stress of the foamed resin molded body were measured to evaluate the light weight due to foaming of the foamed resin molded body and the decrease in strength of the resin molded article after vacuum molding. In order to measure the yield point stress of each of the foamed resin molded bodies in the MD (extrusion) direction and TD (width) direction, two foamed resin molded bodies were prepared for each of Examples 1 to 11 and Comparative Examples 1 to 8, and test pieces were cut out from each of the two foamed resin molded bodies using a punching machine. Specifically, one test piece was cut out from the center of the width direction of each sheet-like foamed resin molded body to have a size of 80 mm x 10 mm in the MD (extrusion) direction in order to measure the yield point stress in the MD direction, and the other test piece was cut out to have a size of 80 mm x 10 mm in the TD (width) direction in order to measure the yield point stress in the TD direction. The resin molded product is a molded product obtained by vacuum molding a foamed resin molded product. Note that the present disclosure is not limited to these examples.
[0047] Each foamed resin molded body was produced under the conditions shown in Table 1 below. Each foamed resin molded body was made of polycarbonate resin having a melt viscosity of 7738 Pa·s as a resin material, but the melt viscosity changed due to the inclusion of fibrous PTFE. Therefore, when the foamed resin molded body is 100 mass%, the content excluding the content of fibrous PTFE and particulate PTFE is the content of polycarbonate resin. In addition, in the foamed resin molded body having a skin layer except for Example 10, the resin material of the skin layer was all polycarbonate resin. Each foamed resin molded body was produced by an extrusion molding method in which molten resin is extruded and cooled and solidified. At this time, the molten resin was kneaded to such an extent that the fibrous PTFE and particulate PTFE were not fibrillated. The "average particle diameter" is the average particle diameter of particulate PTFE. In addition, in the "foamed resin molded body", the one having a skin layer among Examples 1 to 11 is the laminated resin molded body described above.
[0048] [Table 1]
[0049] (Resin molded product after vacuum forming) A sheet-like foamed resin molded body was vacuum molded at a heating temperature of 190°C using a box-shaped mold. The mold was box-shaped with a width of 100 mm, a length of 200 mm, and a depth of 40 mm, and a box-shaped resin molded product having a bottom surface with a width of 100 mm and a length of 200 mm was obtained. The bottom surface of the resin molded product was cut out using a punching machine from the center of the width direction of the bottom surface in the longitudinal direction in the TD (width) direction or in the longitudinal direction in the MD (extrusion) direction, avoiding the portion up to 10 mm from the end in the MD direction, to have a size of 80 mm x 10 mm. Similarly to the test pieces of the foamed resin molded body described above, test pieces for measuring the yield point stress in the MD direction and the TD direction were prepared.
[0050] (Evaluation method) In the evaluation method for the reduction rate of yield stress, if the average reduction rate of yield stress in the extrusion direction (MD) and transverse direction (TD) of the foamed resin molded product is less than 40%, it is rated as "A"; If it was more than 50% but less than 50%, it was rated as "B", and if it was 50% or more, it was rated as "C".
[0051] (Yield stress of foamed resin molding) The yield stress of the foamed resin molded body was measured by performing a three-point bending test (based on ISO 178) on the test piece of the foamed resin molded body described above. The three-point bending test was performed in air using a bench-top precision universal testing machine (Shimadzu Corporation, model number "AGS-J") at a test speed of 10 mm / min and a support distance of 32 mm.
[0052] (Yield stress of resin molded products) The yield stress of the resin molded product was measured by carrying out a three-point bending test (based on ISO 178) on the test piece of the above-mentioned resin molded product. The measurement conditions were the same as those for measuring the yield stress of the foamed resin molded product.
[0053] The density of the foamed resin molded body was measured using a submerged displacement densitometer DSGI manufactured by Toyo Seiki Seisakusho.
[0054] (evaluation) In Examples 1 to 11, the density of each foamed resin molded body was relatively low, and each yield point stress reduction rate was 50% or less, and was rated as "A" or "B." On the other hand, in Comparative Examples 1 to 5, 7, and 8, the density of each foamed resin molded body was relatively low, but the yield point stress of the resin molded product after vacuum molding was significantly lower than the yield point stress of the foamed resin molded body, and was rated as "C." In Comparative Example 6, the yield point stress reduction rate was highly rated, but the density was relatively high and lightweight properties could not be obtained.
[0055] In addition, since Comparative Example 1 does not contain fibrous PTFE and particulate PTFE, the bubbles contained in the foamed resin molding became large and proper vacuum molding was not possible, and damage was confirmed in the resin molded product. The reason why the yield stress reduction rate of Comparative Examples 2 and 3 was high is thought to be due to the fact that the bubbles contained in the foamed resin molding became large because either fibrous PTFE or particulate PTFE was not contained. The reason why the yield stress reduction rate of Comparative Example 4 was high is thought to be due to the fact that the content of particulate PTFE was small, so the number of bubbles contained in the foamed resin molding was reduced and the bubbles became larger accordingly. The reason why the yield stress reduction rate of Comparative Example 5 was high is thought to be due to the fact that the content of fibrous PTFE was small, so the bubbles contained in the foamed resin molding became larger. The reason why the density of Comparative Example 6 was high is thought to be due to the fact that the foamed resin molding contained a large amount of fibrous PTFE, so the number of bubbles contained in the foamed resin molding was reduced, resulting in a structure similar to that of a non-foamed resin. The reason why the yield stress reduction rate of Comparative Example 7 was high is considered to be due to the fact that the number of bubbles contained in the foamed resin molding increased excessively due to the inclusion of a large amount of particulate PTFE, resulting in a thinning of the bubble walls, or the number of particulate PTFE contributing to the increase in the number of bubbles decreased due to secondary aggregation of particulate PTFE, resulting in a decrease in the number of bubbles and the coarsening of each bubble. Also, the reason why the yield stress reduction rate of Comparative Example 8 was high is considered to be due to the fact that the particulate PTFE itself became a foreign matter, causing damage to the bubble walls during extrusion molding of the foamed resin molding, or the particulate PTFE, which has a relatively large average particle size, became defective in the bubble walls, resulting in a decrease in mechanical properties.
[0056] As a result, it was confirmed that by taking into consideration the balance between the contents of fibrous PTFE and particulate PTFE as in Examples 1 to 11, and setting the content of fibrous PTFE to 0.1% by mass or more and 1.0% by mass or less, and the content of particulate PTFE having an average particle size of less than 40 μm to 0.1% by mass or more and 2.0% by mass or less, finer bubbles can be stably formed, and the reduction in strength of the resin molded product after thermal shaping such as vacuum molding can be suppressed while ensuring the lightweight properties achieved by foaming.
[0057] In addition, comparing Examples 1 to 8, 10, and 11, which have the same average particle size of particulate PTFE, when the content of fibrous PTFE and the content of particulate PTFE are 0.2 mass% or more, particularly 0.25 mass% or more, the reduction rate of yield stress could be rated "A". Furthermore, among them, when the content of fibrous PTFE and the content of particulate PTFE are 0.50 mass% or less as in Examples 2 and 3, the value of the reduction rate of yield stress (average) was 30% or less, and the reduction rate of yield stress could be further reduced.
[0058] In addition, comparing Examples 1 to 9 and 11 with Example 10, it was found that when a skin layer was provided on the main surface of the foamed resin molded body, i.e., when it was a laminated resin molded body, the yield stress reduction rate tended to be relatively small. Furthermore, comparing Examples 1 to 8 and 11 with Example 9, the tendency for the yield stress reduction rate to be relatively small by setting the melt viscosity of the skin layer to 5500 Pa s or more became more pronounced.
[0059] In this example, tests were conducted using PTFE as the material for the fibrous fluororesin and particulate fluororesin, but it is believed that similar results would be obtained even if fluororesins such as ETFE resin, PPA resin, and FEP resin were used as the material. [Explanation of symbols]
[0060] 1 foamed resin molded body, 2 skin layer, 10 laminated resin molded body
Claims
1. A foamed resin molded article containing a polycarbonate resin, The present invention includes fibrous polytetrafluoroethylene (hereinafter referred to as PTFE) and particulate PTFE having an average particle size of less than 40 μm, The fibrous PTFE has a content of 0.1% by mass or more and 1.0% by mass or less with respect to the foamed resin molding, The particulate PTFE has a content of 0.1% by mass or more and 2.0% by mass or less relative to the foamed resin molded product.
2. The foamed resin molded article according to claim 1, The foamed resin molded product has a content of the fibrous PTFE of 0.2 mass% or more relative to the foamed resin molded product.
3. The foamed resin molded article according to claim 1 or 2, The particulate PTFE has a content of 0.2 mass% or more relative to the foamed resin molded product.
4. The foamed resin molded article according to claim 1 , a skin layer made of a non-foamed resin and laminated on one main surface of the foamed resin molding;
5. The laminated resin molding according to claim 4, A laminated resin molding, wherein the skin layer has a melt viscosity of 5,500 Pa·s or more.
Citation Information
Patent Citations
Foaming nucleating agent, foam and production of foam
JP2000072912A
Fiber-reinforced hollow material and method for producing fiber-reinforced hollow material
JP2020152051A
Foam sheet of thermoplastic resin composition and process for producing the same
WO2008038639A1
Extrusion-foamed board of mixture of polypropylene and polystyrene resins
JP2001187824A
Thermoplastic resin extruded foam and method for producing the same
JP2006077218A