Surface protective film
A polycarbonate resin-based surface protection film with specific structural units and additives addresses the brittleness and petroleum dependence of conventional films, offering enhanced transparency, heat resistance, and scratch resistance using plant-derived materials.
Patent Information
- Application Number
- JP2023047674
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Conventional protective films made from polyethylene terephthalate resin and polycarbonate resin are hard and brittle, lacking in scratch resistance and heat resistance, and are derived from petroleum resources, necessitating a shift towards plant-based materials with improved mechanical properties and optical performance.
A surface protection film composed of polycarbonate resin containing specific structural units derived from isosorbide and tricyclodecane dimethanol, with a content ratio of 65-85 mol% isosorbide and optimized thickness, transparency, and inclusion of additives to enhance scratch resistance and heat resistance.
The film achieves excellent transparency, optical properties, heat resistance, and scratch resistance while being derived from plant-based materials, suitable for display applications.
Smart Images

Figure 2024136531000001 
Figure 2024136531000002 
Figure 2024136531000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a surface protection film containing a polycarbonate resin. [Background technology]
[0002] Liquid crystal displays and organic electroluminescence displays are widely used as display devices for personal computers, smartphones, tablet terminals, and the like. Conventionally, polyethylene terephthalate resins and polycarbonate resins have been used as surface protective films for displays from the viewpoints of mechanical strength and transparency. However, these are generally manufactured using raw materials derived from petroleum resources, and there is concern about the depletion of petroleum resources, so there is a demand for the development of plastics made from carbon-neutral plant-derived monomers. In this situation, polycarbonate resins manufactured using isosorbide (hereinafter sometimes referred to as "ISB"), a plant-derived raw material, have been developed in recent years and are being applied to automotive parts and optical applications (see, for example, Patent Documents 1 and 2).
[0003] As displays become higher quality and thinner, surface protection films are required to not only prevent scratches and dirt but also to act as a support for components, and surface protection films made from biomass resources and with a high elastic modulus are being developed. Thin protective films with small optical distortion are also being developed to protect polarizers. Furthermore, protective films with excellent flexibility have also been developed for optical inspection, taking into account operability during lamination and peeling. (For example, see Patent Documents 3 to 5.) [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2004 / 111106 [Patent Document 2] International Publication No. 2007 / 148604 [Patent Document 3] JP 2009-079190 A [Patent Document 4] JP 2015-194754 A [Patent Document 5] JP 2020-33418 A Summary of the Invention [Problem to be solved by the invention]
[0005] The above-mentioned conventional protective films are hard and brittle, and therefore there is room for improvement in terms of scratch resistance as well as heat resistance.
[0006] The present invention has been made in view of the above background, and aims to provide a surface protection film that is made from plant-derived raw materials and has excellent transparency, optical properties, heat resistance, and scratch resistance. [Means for solving the problem]
[0007] That is, the present invention has the following aspects. [1] A surface protection film containing a polycarbonate resin, The polycarbonate resin contains a structural unit (A) represented by the following formula (1) and a structural unit (B) represented by the following formula (2), the content of the structural unit (A) in the polycarbonate resin is 65 mol % or more and 85 mol % or less, A surface protection film having a thickness of 21 μm or more.
[0008] [ka]
[0009] [ka]
[0010] [2] The surface protective film according to [1], which has a total light transmittance of 90% or more and a haze of 1.0% or less. [3] The surface protective film according to [1] or [2], which has a light transmittance at a wavelength of 360 nm of 60% or more. [4] The surface protection film according to any one of [1] to [3], which has a water absorption rate of 3.0% or less.
[0011] [5] The photoelastic coefficient is 14 × 10 -12 Pa -1 The surface protective film according to any one of [1] to [4], wherein [6] The surface protective film according to any one of [1] to [5], wherein the polycarbonate resin has a glass transition temperature of 125° C. or higher and 150° C. or lower. [7] The surface protective film according to any one of [1] to [6], wherein the polycarbonate resin has a reduced viscosity at 20° C. of 0.20 or more and 0.70 or less.
[0012] [8] The surface protective film according to any one of [1] to [7], wherein the content of the phosphite compound per 100 parts by weight of the polycarbonate resin is 0.04 parts by weight or less. [9] The surface protective film according to any one of [1] to [8], which is a non-stretched film. Effect of the Invention
[0013] According to the present invention, it is possible to provide a surface protection film which is made from plant-derived raw materials and has excellent transparency, optical properties, heat resistance, and scratch resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The embodiment of the present invention will be described in detail below, but the description of the configuration described below is one example (i.e., a representative example) of the embodiment of the present invention, and the present invention is not limited to the following content as long as it does not exceed the gist of the present invention. In this specification, the term "repeated structural unit" refers to a structural unit in which the same structure appears repeatedly in a resin, and each of which is linked to form the resin. For example, in the case of a polycarbonate resin, the repeating structural unit also includes a carbonyl group. In addition, the term "structural unit" refers to a partial structure that constitutes a resin, and a specific partial structure contained in the repeating structural unit. For example, it refers to a partial structure sandwiched between adjacent linking groups in a resin, or a partial structure sandwiched between a polymerizable reactive group present at the end of a polymer and a linking group adjacent to the polymerizable reactive group. More specifically, in the case of a polycarbonate resin, a carbonyl group is a linking group, and a partial structure sandwiched between adjacent carbonyl groups is referred to as a structural unit. In addition, when the expression "~" is used in this specification, it is used in a sense including the numerical value or physical value described before and after it. In addition, the numerical values or physical values described as the upper and lower limits are intended to include those values. In addition, "parts by weight" and "parts by mass," "% by weight" and "% by mass" are essentially synonymous.
[0015] The surface protective film contains a polycarbonate resin.
[0016] <Polycarbonate resin> The polycarbonate resin contains a structural unit (A) represented by the following formula (1).
[0017] [ka]
[0018] Dihydroxy compounds forming the structural unit of the formula (1) (hereinafter referred to as "first compound") include isosorbide, isomannide, and isoidet, which are stereoisomers. These may be used alone or in combination of two or more. Among these, isosorbide is most preferred in terms of availability and ease of production, optical properties, and moldability. Isosorbide is obtained by dehydration condensation of sorbitol, which is abundant as a plant-derived resource and is produced from various starches that are easily available.
[0019] In the polycarbonate resin, the content of the structural unit (A) is 65 mol% or more relative to the total structural units derived from dihydroxy compounds in the polycarbonate resin. If it is less than 65 mol%, the glass transition temperature of the polycarbonate resin is low, and the heat resistance of the surface protection film may be insufficient. From the viewpoint of further improving the heat resistance, the content of the structural unit (A) is preferably 70 mol% or more relative to the total structural units derived from dihydroxy compounds in the polycarbonate resin. In addition, the content of the structural unit (A) is 85 mol% or less relative to the total structural units derived from dihydroxy compounds in the polycarbonate resin. If it exceeds 85 mol%, the photoelastic coefficient may become too high, and the optical properties of the surface protection film may be deteriorated. In addition, in this case, the saturated water absorption rate becomes high, and the dimensional stability of the surface protection film due to water absorption may be impaired. Also, from the viewpoint of achieving a well-balanced improvement in moldability, mechanical strength, and heat resistance, which is difficult to achieve with a polycarbonate resin composed only of the repeating structural unit (A) (i.e., a polycarbonate resin composed of a polymer of the first compound), the content of the structural unit (A) is preferably 85 mol % or less based on all structural units derived from dihydroxy compounds in the polycarbonate resin. From the viewpoint of further improving optical properties and dimensional stability, and further improving moldability, mechanical strength, and heat resistance in a well-balanced manner, the content of the structural unit (A) is preferably 80 mol % or less based on all structural units derived from dihydroxy compounds in the polycarbonate resin.
[0020] The polycarbonate resin is a polycarbonate resin containing a structural unit (B) represented by the following formula (2).
[0021] [ka]
[0022] An example of a dihydroxy compound (hereinafter referred to as a "second compound") that forms the structural unit of the formula (2) is tricyclodecane dimethanol, which is an alicyclic dihydroxy compound.
[0023] In the polycarbonate resin, the content of the structural unit (B) is preferably 20 mol% or more, more preferably 30 mol% or more, based on the total structural units derived from dihydroxy compounds in the polycarbonate resin. Also, it is preferably 15 mol% or less, more preferably 10 mol% or less. In these cases, the optical properties of the surface protection film can be improved while maintaining excellent heat resistance.
[0024] The polycarbonate resin contains a structural unit (A) derived from a first compound and a structural unit (B) derived from a second compound. The polycarbonate resin may contain a structural unit derived from a dihydroxy compound other than the first compound and the second compound (hereinafter referred to as a "third compound"), or a structural unit derived from a compound other than a dihydroxy compound. Suitable examples of the third compound include a dihydroxy compound of an aliphatic hydrocarbon, a dihydroxy compound of an alicyclic hydrocarbon, an ether-containing dihydroxy compound, and a dihydroxy compound containing an acetal ring.
[0025] Examples of aliphatic hydrocarbon dihydroxy compounds include straight-chain aliphatic dihydroxy compounds such as ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,5-heptanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol; and branched-chain aliphatic dihydroxy compounds such as 1,3-butanediol, 1,2-butanediol, neopentyl glycol, and hexylene glycol.
[0026] Examples of dihydroxy compounds of alicyclic hydrocarbons include dihydroxy compounds which are primary alcohols of alicyclic hydrocarbons, such as dihydroxy compounds derived from terpene compounds, such as 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, pentacyclopentadecane dimethanol, 2,6-decalin dimethanol, 1,5-decalin dimethanol, 2,3-decalin dimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol, 1,3-adamantanedimethanol, and limonene; and dihydroxy compounds which are secondary or tertiary alcohols of alicyclic hydrocarbons, such as 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,3-adamantanediol, hydrogenated bisphenol A, and 2,2,4,4-tetramethyl-1,3-cyclobutanediol.
[0027] Examples of the ether-containing dihydroxy compound include oxyalkylene glycols, such as diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, and polypropylene glycol.
[0028] Examples of dihydroxy compounds containing an acetal ring (i.e., a cyclic acetal structure) include spiroglycol (also known as 3,9-bis(1,1-dimethyl-2-hydroxyethyl-2,4,8,10-tetraoxaspiro[5,5]undecane) and dioxane glycol (also known as 2-(1,1-dimethyl-2-hydroxyethyl)-5-ethyl-5-hydroxymethyl-1,3-dioxane).
[0029] In addition, as the third compound, a dihydroxy compound containing an aromatic group such as a bisphenol compound, a diester compound, etc. can be used. A polycarbonate resin partially incorporating a structural unit derived from a diester compound is called a polyester carbonate resin. In other words, the polycarbonate resin in this specification is a concept that includes polyester carbonate resins.
[0030] By using a dihydroxy compound or diester compound containing an aromatic group such as a bisphenol compound as a copolymerization component, the heat resistance of the surface protective film may be improved. On the other hand, when the polycarbonate resin contains a large amount of structural units derived from a dihydroxy compound containing an aromatic group, the weather resistance tends to decrease. In addition, there is a large difference in polymerization reactivity between the dihydroxy compound or diester compound containing an aromatic group and the first and second compounds. Therefore, the dihydroxy compound or diester compound containing an aromatic group remains as an end group, making it difficult to obtain a polycarbonate resin with a high molecular weight, and the impact resistance tends to decrease. If the reaction temperature is increased to promote the reaction, the structural unit (A) is thermally decomposed, and the obtained polycarbonate resin tends to be colored. For these reasons, the content ratio of the structural unit derived from the dihydroxy compound or diester compound containing an aromatic group in the polycarbonate resin is preferably 10% by weight or less, more preferably 5% by weight or less.
[0031] Examples of dihydroxy compounds containing an aromatic group include 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, 2,2-bis(4-hydroxy-(3-phenyl)phenyl)propane, 2,2-bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, and 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane. )propane, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 1,1-bis(4-hydroxyphenyl)-2-ethylhexane, 1,1-bis(4-hydroxyphenyl)decane, bis(4-hydroxy-3-nitrophenyl)methane, 3,3-bis(4-hydroxyphenyl) 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenyl sulfone, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxy-3-methylphenyl)sulfide, bis(4-hydroxyphenyl)disulfide aromatic bisphenol compounds such as 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dichlorodiphenyl ether; dihydroxy compounds having an ether group bonded to an aromatic group such as 2,2-bis(4-(2-hydroxyethoxy)phenyl)propane, 2,2-bis(4-(2-hydroxypropoxy)phenyl)propane, 1,3-bis(2-hydroxyethoxy)benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, bis(4-(2-hydroxyethoxy)phenyl)sulfone;9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9, Examples of dihydroxy compounds having a fluorene ring include 9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, and 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene.
[0032] Examples of diester compounds include the following dicarboxylic acids. Specific examples include aromatic dicarboxylic acids such as terephthalic acid, phthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-benzophenonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid; alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid; and aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid. These dicarboxylic acid components can be used as raw materials for polyester carbonate resins as dicarboxylic acids themselves, but depending on the production method of polyester carbonate resins, dicarboxylic acid esters such as methyl esters and phenyl esters, and dicarboxylic acid derivatives such as dicarboxylic acid halides can also be used as raw materials.
[0033] The dihydroxy compound used as a raw material for the polycarbonate resin may contain various stabilizers such as a reducing agent, an antioxidant, an oxygen scavenger, a light stabilizer, an antacid, a pH stabilizer, and a heat stabilizer. In particular, since the first compound has a property of being easily degraded under acidic conditions, the degrading of the first compound can be suppressed by using a basic stabilizer in the production process of the polycarbonate resin. This can further improve the quality of the obtained polycarbonate resin.
[0034] Carbonic acid diesters used as raw materials for polycarbonate resins usually include compounds represented by the following formula (3): These carbonic acid diesters may be used alone or in combination of two or more.
[0035] [ka]
[0036] In the formula (3), A 1and A 2 are each independently a substituted or unsubstituted aliphatic hydrocarbon group having 1 to 18 carbon atoms or a substituted or unsubstituted aromatic hydrocarbon group. 1 and A 2 may be the same or different. A 1 and A 2 is preferably a substituted or unsubstituted aromatic hydrocarbon group, and more preferably an unsubstituted aromatic hydrocarbon group. Examples of the carbonic acid diester represented by formula (3) include diphenyl carbonate, substituted diphenyl carbonates such as ditolyl carbonate, dimethyl carbonate, diethyl carbonate, di-t-butyl carbonate, etc. Diphenyl carbonate and substituted diphenyl carbonates are preferred, and diphenyl carbonate is more preferred.
[0037] The carbonic acid diester may contain impurities such as chloride ions, which may inhibit the polycondensation reaction or deteriorate the color tone of the resulting polycarbonate resin, and therefore it is preferable to use a carbonic acid diester that has been purified by distillation or the like, as necessary.
[0038] <Production method of polycarbonate resin> The polycarbonate resin can be synthesized by polycondensing the dihydroxy compound and the carbonic acid diester through an ester exchange reaction. More specifically, the polycarbonate resin can be obtained by removing the monohydroxy compound and the like that are by-produced in the ester exchange reaction from the system during the polycondensation.
[0039] The transesterification reaction proceeds in the presence of a transesterification catalyst (hereinafter, the transesterification catalyst is referred to as a "polymerization catalyst.") The type of polymerization catalyst can have a significant effect on the reaction rate of the transesterification reaction and the quality of the resulting polycarbonate resin.
[0040] The polymerization catalyst is not particularly limited as long as it satisfies the desired transparency, color tone, heat resistance, weather resistance, and mechanical strength of the polycarbonate resin. For example, a metal compound of Group I or II (hereinafter referred to as "Group 1" and "Group 2") in the long-form periodic table, as well as a basic compound such as a basic boron compound, a basic phosphorus compound, a basic ammonium compound, or an amine compound can be used as the polymerization catalyst, and among them, a Group 1 metal compound and / or a Group 2 metal compound is preferred.
[0041] Examples of the Group 1 metal compound include sodium hydroxide, potassium hydroxide, lithium hydroxide, cesium hydroxide, sodium hydrogen carbonate, potassium hydrogen carbonate, lithium hydrogen carbonate, cesium hydrogen carbonate, sodium carbonate, potassium carbonate, lithium carbonate, cesium carbonate, sodium acetate, potassium acetate, lithium acetate, cesium acetate, sodium stearate, potassium stearate, lithium stearate, cesium stearate, sodium borohydride, potassium borohydride, lithium borohydride, cesium borohydride, sodium phenylborate, potassium phenylborate, lithium phenylborate, cesium phenylborate, sodium benzoate, potassium benzoate, lithium benzoate, cesium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, dicesium hydrogen phosphate, disodium phenylphosphate, dipotassium phenylphosphate, dilithium phenylphosphate, and dicesium phenylphosphate. Examples of Group 1 metal compounds include alcoholates or phenolates of sodium, potassium, lithium, and cesium; and disodium, dipotassium, dilithium, and dicesium salts of bisphenol A. From the viewpoints of polymerization activity and the color tone of the resulting polycarbonate resin, lithium compounds are preferred as Group 1 metal compounds.
[0042] Examples of Group 2 metal compounds include calcium hydroxide, barium hydroxide, magnesium hydroxide, strontium hydroxide, calcium hydrogen carbonate, barium hydrogen carbonate, magnesium hydrogen carbonate, strontium hydrogen carbonate, calcium carbonate, barium carbonate, magnesium carbonate, strontium carbonate, calcium acetate, barium acetate, magnesium acetate, strontium acetate, calcium stearate, barium stearate, magnesium stearate, and strontium stearate. From the viewpoint of polymerization activity and color tone of the obtained polycarbonate resin, the Group 2 metal compounds are preferably magnesium compounds, calcium compounds, and barium compounds, more preferably magnesium compounds and / or calcium compounds, and most preferably calcium compounds.
[0043] Although it is possible to use a basic compound such as a basic boron compound, a basic phosphorus compound, a basic ammonium compound, or an amine compound in combination with the Group 1 metal compound and / or the Group 2 metal compound, it is more preferable to use only the Group 1 metal compound and / or the Group 2 metal compound, and from the viewpoint of the color tone of the resulting polycarbonate resin, it is most preferable to use only the Group 2 metal compound.
[0044] Examples of basic boron compounds include metal salts of tetramethyl boron, tetraethyl boron, tetrapropyl boron, tetrabutyl boron, trimethylethyl boron, trimethylbenzyl boron, trimethylphenyl boron, triethylmethyl boron, triethylbenzyl boron, triethylphenyl boron, tributylbenzyl boron, tributylphenyl boron, tetraphenyl boron, benzyltriphenyl boron, methyltriphenyl boron, butyltriphenyl boron, etc. Examples of metal salts include sodium salt, potassium salt, lithium salt, calcium salt, barium salt, magnesium salt, strontium salt, etc.
[0045] Examples of basic phosphorus compounds include triethylphosphine, tri-n-propylphosphine, triisopropylphosphine, tri-n-butylphosphine, triphenylphosphine, tributylphosphine, and quaternary phosphonium salts.
[0046] Examples of basic ammonium compounds include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, trimethylethylammonium hydroxide, trimethylbenzylammonium hydroxide, trimethylphenylammonium hydroxide, triethylmethylammonium hydroxide, triethylbenzylammonium hydroxide, triethylphenylammonium hydroxide, tributylbenzylammonium hydroxide, tributylphenylammonium hydroxide, tetraphenylammonium hydroxide, benzyltriphenylammonium hydroxide, methyltriphenylammonium hydroxide, and butyltriphenylammonium hydroxide.
[0047] Examples of the amine compounds include 4-aminopyridine, 2-aminopyridine, N,N-dimethyl-4-aminopyridine, 4-diethylaminopyridine, 2-hydroxypyridine, 2-methoxypyridine, 4-methoxypyridine, 2-dimethylaminoimidazole, 2-methoxyimidazole, imidazole, 2-mercaptoimidazole, 2-methylimidazole, aminoquinoline, and guanidine.
[0048] The amount of the polymerization catalyst used is preferably 0.1 μmol or more, more preferably 0.3 μmol or more, and even more preferably 0.5 μmol or more per mol of the total dihydroxy compounds used in the reaction, and is preferably 300 μmol or less, more preferably 100 μmol or less, and even more preferably 50 μmol or less per mol of the total dihydroxy compounds used in the reaction.
[0049] By adjusting the amount of the polymerization catalyst used within the above-mentioned range, the polymerization rate can be increased, so that it is possible to obtain a polycarbonate resin with a desired molecular weight without necessarily increasing the polymerization temperature, and therefore deterioration of the color tone of the polycarbonate resin can be suppressed. In addition, it is possible to prevent the unreacted raw materials from volatilizing during the polymerization, which would cause the molar ratio of the dihydroxy compound and the carbonic acid diester to be lost, so that a resin with a desired molecular weight and copolymerization ratio can be obtained more reliably. Furthermore, it is possible to suppress the occurrence of side reactions, so that deterioration of the color tone of the polycarbonate resin or coloring during molding can be further prevented.
[0050] Considering the adverse effect of sodium, potassium, cesium, and iron on the color tone of the polycarbonate resin, the total content of sodium, potassium, cesium, and iron in the polycarbonate resin is preferably 1 weight ppm or less. In this case, the deterioration of the color tone of the polycarbonate resin can be further prevented, and the color tone of the polycarbonate resin can be further improved. From the same viewpoint, the total content of sodium, potassium, cesium, and iron in the polycarbonate resin is more preferably 0.5 weight ppm or less. These metals may be mixed not only from the catalyst used, but also from raw materials or reaction equipment. Regardless of the source, the total amount of these metals and compounds containing these metals in the polycarbonate resin is preferably within the above-mentioned range as the total content of sodium, potassium, cesium, and iron.
[0051] It is preferable that the dihydroxy compound and the carbonic acid diester are melted separately or mixed uniformly before the transesterification reaction. The melting or mixing temperature is usually 80°C or higher, preferably 90°C or higher, and usually 200°C or lower, preferably 150°C or lower, more preferably 120°C or lower. In this case, the dissolution rate can be increased and the solubility can be sufficiently improved, and problems such as solidification can be sufficiently avoided. Furthermore, in this case, the thermal deterioration of the dihydroxy compound can be sufficiently suppressed, and the quality, represented by the color tone, of the obtained polycarbonate resin can be further improved.
[0052] The dihydroxy compound and the carbonic acid diester are melted or mixed in an atmosphere with an oxygen concentration within a predetermined range. The oxygen concentration is preferably 10 vol% or less. More preferably, the oxygen concentration is 0.0001 vol% or more and 10 vol% or less, even more preferably, the oxygen concentration is 0.0001 vol% or more and 5 vol% or less, and even more preferably, the oxygen concentration is 0.0001 vol% or more and 1 vol% or less. In this case, the color tone can be improved and the reactivity can be increased.
[0053] The method of polycondensing a dihydroxy compound and a carbonic acid diester is carried out in multiple stages using multiple reactors in the presence of the above-mentioned catalyst. The reaction may be carried out in a batchwise manner, a continuous manner, or a combination of a batchwise manner and a continuous manner, but it is preferable to adopt a continuous manner from the viewpoint of obtaining a polycarbonate resin with less heat history and excellent productivity.
[0054] From the viewpoint of controlling the polymerization rate and the quality of the resulting polycarbonate resin, it is preferable to appropriately select the jacket temperature, the internal temperature, and the pressure in the reaction system according to the reaction stage. Specifically, it is preferable to obtain a prepolymer at a relatively low temperature and low vacuum in the early stage of the polycondensation reaction, and to increase the molecular weight to a predetermined value at a relatively high temperature and high vacuum in the later stage of the reaction. In this case, the distillation of unreacted monomers is suppressed, and it becomes easier to adjust the molar ratio of the dihydroxy compound and the carbonate diester to a desired ratio. As a result, it is possible to suppress a decrease in the polymerization rate. In addition, it becomes possible to more reliably obtain a polymer having a desired molecular weight and terminal group.
[0055] The polymerization catalyst can be added to a raw material preparation tank or a raw material storage tank, or can be added directly to a polymerization reactor. From the viewpoint of supply stability and control of the polycondensation reaction, it is preferable to install a catalyst supply line in the raw material line before the raw material is supplied to the polymerization reactor, and supply the polymerization catalyst in the form of an aqueous solution.
[0056] By adjusting the temperature of the polycondensation reaction, it is possible to improve productivity and prevent the increase of the heat history of the product. Furthermore, it is possible to further prevent the volatilization of the monomer and the decomposition and coloration of the polycarbonate resin. Specifically, the following conditions can be adopted as the reaction conditions in the first stage reaction. That is, the maximum temperature inside the polymerization reactor is set in the range of usually 160 to 230°C, preferably 170 to 220°C, and more preferably 180 to 210°C. In addition, the pressure of the polymerization reactor (hereinafter, pressure refers to absolute pressure) is set in the range of usually 1 to 110 kPa, preferably 5 to 50 kPa, and more preferably 7 to 30 kPa. In addition, the reaction time is set in the range of usually 0.1 to 10 hours, preferably 1 to 5 hours. It is preferable that the first stage reaction is carried out while distilling off the generated monohydroxy compound outside the reaction system.
[0057] From the second stage onwards, it is preferable to gradually reduce the pressure of the reaction system from the pressure of the first stage, and to finally reduce the pressure (absolute pressure) of the reaction system to 1 kPa or less while removing the monohydroxy compound that is subsequently generated from the reaction system. The maximum internal temperature of the polymerization reactor is usually set in the range of 200 to 260° C., preferably 210 to 240° C., and more preferably 215 to 230° C. The reaction time is usually set in the range of 0.1 to 10 hours, preferably 0.5 to 5 hours, and more preferably 1 to 3 hours.
[0058] After the polycarbonate resin is polymerized as described above, it can usually be cooled and solidified, and pelletized with a rotary cutter, etc. The pelletization method is not limited, but examples thereof include a method in which the polycarbonate resin is withdrawn in a molten state from the final polymerization reactor, cooled and solidified in the form of a strand, and pelletized, a method in which the polycarbonate resin in a molten state is supplied from the final polymerization reactor to a single-screw or twin-screw extruder, extruded, cooled and solidified, and pelletized, and a method in which the polycarbonate resin in a molten state is withdrawn from the final polymerization reactor, cooled and solidified in the form of a strand, pelletized once, and then supplied to the single-screw or twin-screw extruder again, melt-extruded, cooled and solidified, and pelletized.
[0059] In order for the polycarbonate resin to be suitably used for the surface protection film, it is preferable that the polycarbonate resin contains little foreign matter. Therefore, in order to remove foreign matter such as discolored parts and gels in the polycarbonate resin obtained by melt polycondensation as described above, it is preferable to perform filtration using a filter. More specifically, it is preferable to remove residual monomers, by-product phenols, etc. by devolatilization under reduced pressure, and to mix additives such as heat stabilizers, by melt extruding the polycarbonate resin using the vented twin-screw extruder described above, and then filtering it with a filter.
[0060] The filter may be of any known shape, such as a candle type, a pleat type, or a leaf disk type. In order to obtain a filtration accuracy of 99%, the filter aperture is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 20 μm or less. When it is particularly desired to reduce foreign matter, the filter aperture is particularly preferably 10 μm or less. However, if the aperture is small, the pressure loss in the filter increases, which may lead to damage to the filter or deterioration of the polycarbonate resin due to shear heat generation, so even if a filtration accuracy of 99% is required, the filter aperture is preferably 1 μm or more. The filter aperture is determined in accordance with ISO16889:1999.
[0061] The polycarbonate resin filtered through the filter is discharged from the die head in the form of strands, cooled and solidified, and pelletized with a rotary cutter, etc. Stranding and pelletization, in which the polycarbonate resin comes into direct contact with the outside air, are preferably carried out in a clean room with a cleanliness level higher than Class 7, more preferably Class 6, defined in JIS B 9920-1:2019, in order to prevent contamination from the outside air.
[0062] In pelletizing, it is preferable to use a cooling method such as air cooling or water cooling. In the case of air cooling, it is preferable to use air from which foreign matter in the air has been removed in advance using a HEPA filter or the like, in order to prevent re-adhesion of foreign matter in the air. In the case of water cooling, it is preferable to use water from which metals in the water have been removed using an ion-exchange polycarbonate resin or the like, and from which foreign matter in the water has been removed using a water filter. In order to obtain a filtration accuracy of 99% removal, it is preferable that the mesh size of the water filter is 10 to 0.45 μm.
[0063] <Additives> The surface protective film may contain other components such as additives in addition to the polycarbonate resin.
[0064] The polycarbonate resin may contain a catalyst deactivator as an additive. The catalyst deactivator is not particularly limited as long as it is an acidic substance that has a function of deactivating the polymerization catalyst. From the viewpoint of excellent effects of catalyst deactivation and coloration suppression, the catalyst deactivator is preferably a phosphorus-based acidic compound, more preferably phosphonic acid (phosphorous acid) and phosphonic acid ester, and even more preferably phosphonic acid (phosphorous acid).
[0065] By adjusting the content of the phosphorus-based acidic compound according to the amount of the polymerization catalyst, the effect of catalyst deactivation and coloring inhibition can be obtained more reliably, and the optical properties of the surface protective film can be further improved. The content of the phosphorus-based acidic compound is preferably 0.5 times mol or more, more preferably 0.7 times mol or more, and even more preferably 0.8 times mol or more, in terms of the amount of phosphorus atoms, relative to 1 mol of the metal atoms of the polymerization catalyst. In addition, it is preferably 5 times mol or less, more preferably 3 times mol or less, and even more preferably 1.5 times mol or less.
[0066] Examples of additives other than the catalyst deactivator include antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, fillers and other fillers, neutralizers, lubricants, antifogging agents, antiblocking agents, slip agents, dispersants, colorants, flame retardants, antistatic agents, conductivity imparting agents, crosslinking agents, crosslinking assistants, metal deactivators, molecular weight regulators, antibacterial agents, antifungal agents, fluorescent brighteners, light diffusing agents such as organic diffusing agents and inorganic diffusing agents, etc. These additives can be used within a range that does not impair the effects of the present disclosure.
[0067] One or more types of heat stabilizers may be blended to prevent a decrease in molecular weight or deterioration in color during molding, etc. As the heat stabilizer, phosphite compounds and phenol compounds are preferred, and phosphite compounds are more preferred. Examples of the phosphite compounds include triphenyl phosphite, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tridecyl phosphite, trioctyl phosphite, trioctadecyl phosphite, didecyl monophenyl phosphite, dioctyl monophenyl phosphite, diisopropyl monophenyl phosphite, monobutyl diphenyl phosphite, monodecyl diphenyl phosphite, monooctyl diphenyl phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, bis(nonylphenyl)pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, and the like. Among these, trisnonylphenyl phosphite, tris(2,4-di-tert-butylphenyl) phosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, and bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphite are preferably used. These compounds may be used alone or in combination of two or more.
[0068] However, since the phosphite compound, which is a heat stabilizer, may bleed out during molding and contaminate the film-forming roll or the film surface, the content of the phosphite compound in 100 parts by weight of polycarbonate resin is preferably 0.04 parts by weight or less, more preferably 0.02 parts by weight or less, and even more preferably 0.01 parts by weight or less.
[0069] In addition, within a range that does not impair the effects of the present disclosure, the above-mentioned polycarbonate resin may be kneaded with one or more selected from synthetic resins such as aromatic polyesters, aliphatic polyesters, polyamides, polystyrenes, polyolefins, amorphous polyolefins, acrylonitrile-butadiene-styrene copolymers (ABS resins), and acrylonitrile-styrene copolymers (AS resins); elastomers such as acrylic rubbers and butadiene rubbers; and biodegradable resins such as polylactic acid and polybutylene succinate. In other words, the polycarbonate resin may be a polymer alloy.
[0070] <Physical properties of polycarbonate resin> (glass transition temperature) The glass transition temperature of the polycarbonate resin is preferably 125°C or higher and 150°C or lower, more preferably 127°C or higher and 145°C or lower. In this case, the surface protection film exhibits sufficient heat resistance. The glass transition temperature of the polycarbonate resin is controlled by the monomer composition (i.e., the composition of the structural units) constituting the polycarbonate resin. For example, the glass transition temperature tends to increase as the content ratio of the structural unit A in the polycarbonate resin increases.
[0071] (Molecular weight: reduced viscosity) The molecular weight of the polycarbonate resin is represented by, for example, the number average molecular weight measured by reduced viscosity. The values obtained by these measuring methods indicate that the molecular weight is larger as the numerical value is higher. The reduced viscosity of the polycarbonate resin is preferably 0.20 dL / g or more, more preferably 0.30 dL / g or more. In this case, the mechanical strength of the surface protection film can be further improved. On the other hand, the reduced viscosity is preferably 0.70 dL / g or less, more preferably 0.65 dL / g or less. In this case, the fluidity during molding can be improved, and the productivity and moldability can be further improved. The details of the method for measuring the reduced viscosity will be described in the examples.
[0072] <Method of manufacturing surface protection film> The method of forming a surface protection film using polycarbonate resin can be a casting method in which polycarbonate resin is dissolved in a solvent and cast, and then the solvent is removed, or a melt film-forming method in which polycarbonate resin is melted without using a solvent to form a film.Specific examples of the melt film-forming method include melt extrusion using a T-die, calendar molding, heat pressing, co-extrusion, co-melting, multilayer extrusion, and inflation molding.The film-forming method is not particularly limited, but is preferably a melt film-forming method, and more preferably a melt extrusion method using a T-die.
[0073] When forming a film by the melt film-forming method, the forming temperature is preferably 280°C or less, more preferably 270°C or less, and even more preferably 265°C or less. If the forming temperature is too high, foreign matter or bubbles may occur in the film, and defects in the film may increase or the film may become discolored. On the other hand, if the forming temperature is too low, the melt viscosity of the polycarbonate resin may become too high, making it difficult to form the film, and it may be difficult to produce a film with a uniform thickness. In order to avoid this, the lower limit of the forming temperature is usually 200°C or more, preferably 210°C or more, and more preferably 220°C or more. Here, the forming temperature of the film is the temperature during forming in the melt film-forming method, and is usually the value measured by measuring the polycarbonate resin temperature at the die outlet from which the molten polycarbonate resin is extruded.
[0074] In addition, if foreign matter is present in the film, when the film is used as an optical film such as a surface protection film, it is recognized as a defect such as light leakage, and the visibility is reduced. In order to remove foreign matter in the polycarbonate resin, it is preferable to attach a polymer filter after the extruder, filter the polycarbonate resin, and then extrude it through a die to form a film. In this case, it is necessary to connect the extruder, the polymer filter, and the die with piping to transfer the molten polycarbonate resin, but in order to minimize thermal deterioration in the piping, it is preferable to arrange each facility so that the residence time is minimized. In addition, the process of transporting and winding the film after extrusion is performed in a clean room, and great care is required to prevent foreign matter from adhering to the film.
[0075] <Properties of surface protection film> The thickness of the surface protection film is 21 μm or more. If the thickness is less than 21 μm, the scratch resistance may be insufficient. From the viewpoint of further improving the scratch resistance of the surface protection film, the thickness is preferably 30 μm or more, more preferably 50 μm or more. In addition, from the viewpoint of reducing the occurrence of flatness defects due to rolling habits when wound into a roll and stored, the thickness of the surface protection film is preferably 300 μm or less, more preferably 250 μm or less, and even more preferably 200 μm or less.
[0076] The length of the surface protective film in the longitudinal direction is preferably 500 m or more, more preferably 1000 m or more, and even more preferably 1500 m or more. From the viewpoint of productivity and quality, it is preferable that the production of the surface protective film is carried out continuously. In this specification, "long length" means that the longitudinal dimension of the film is sufficiently larger than the width direction of the film, and essentially means that it can be wound in the longitudinal direction to form a coil. More specifically, it means that the longitudinal dimension of the film is 10 times or more larger than the width direction. In addition, the obtained film may be stretched within a range that does not impair the object of the present invention. As the stretching method, a known method is used, for example, longitudinal uniaxial stretching, transverse uniaxial stretching using a tenter or the like, and fixed-end uniaxial stretching are used. In addition, simultaneous biaxial stretching, sequential biaxial stretching, etc., which are combinations of these stretching methods, are used. The stretching may be carried out in a batch manner, but it is preferable to carry out it continuously in terms of productivity.
[0077] The surface protection film is preferably a non-stretched film. For example, in the case of a stretched film produced by a stretching method, rainbow unevenness may occur due to birefringence, which may reduce visibility.
[0078] The surface protective film has a total light transmittance of preferably 90% or more, more preferably 91% or more, and even more preferably 92% or more. The surface protective film also has a light transmittance of preferably 60% or more, more preferably 70% or more, and even more preferably 80% or more at a wavelength of 360 nm. In these cases, the light emission amount of the light source of the liquid crystal display or the organic EL display can be reduced, power consumption can be reduced, heat generation of the display device can be suppressed, and durability can be improved. Therefore, the surface protective film becomes more suitable for display applications. The upper limit of the total light transmittance of the film is not particularly limited, but is usually 99% or less.
[0079] The haze of the surface protection film is preferably 1.0% or less, more preferably 0.5% or less, and even more preferably 0.1% or less. In this case, the surface protection film has sufficiently excellent transparency. For example, in a melt extrusion method using a T-die, a molten resin is extruded from a T-die into a film shape, and a mirror surface such as a mirror roll or a mirror belt is brought into contact with at least one side of the extruded film-like material, so that the surface smoothness of the surface protection film is improved and a mirror gloss is obtained, and the haze of the surface protection film can be reduced to the above range. The mirror surface is preferably a metal mirror surface. Examples of the metal of the mirror surface include chromium.
[0080] The surface protective film preferably has a total light transmittance of 90% or more and a haze of 1.0% or less. In this case, the surface protective film has excellent transparency and visibility, and is more suitable for the above-mentioned display applications. From the same viewpoint, the surface protective film more preferably has a total light transmittance of 90% or more and a haze of 0.5% or less, and further preferably has a total light transmittance of 92% or more and a haze of 0.1% or less.
[0081] The water absorption rate of the surface protective film is preferably 3.0% or less, more preferably 2.5% or less, and even more preferably 2.0% or less. In this case, it is possible to suppress changes in optical properties due to water absorption and deformation of the film. The water absorption rate is measured, for example, by a method described in detail in the Examples. The water absorption rate of the surface protective film is controlled by adjusting the monomer composition (i.e., the composition of the structural units) constituting the polycarbonate resin. For example, the water absorption rate of the surface protective film tends to increase as the content ratio of the structural unit A in the polycarbonate resin increases.
[0082] If the photoelastic coefficient of the surface protection film is high, rainbow interference fringes may occur when stress is applied to the film, resulting in poor visibility. To prevent this, the photoelastic coefficient of the surface protection film is set to 14×10 -12 Pa -1 Less than or equal to 12×10 is preferred-12 Pa -1 Less than or equal to 10x10 is preferable. -12 Pa -1 The following is more preferable. The photoelastic coefficient is measured, for example, by a method described in detail in the Examples. The photoelastic coefficient of the surface protective film is controlled by adjusting the monomer composition (i.e., the composition of the structural unit) constituting the polycarbonate resin. For example, the photoelastic coefficient tends to increase as the content ratio of the structural unit A in the polycarbonate resin increases. EXAMPLES
[0083] Hereinafter, the present disclosure will be described in more detail using examples, but the present disclosure is not limited to the following examples as long as it does not depart from the gist of the disclosure.
[0084] [Measurement method] Various physical properties of the polycarbonate resin were measured according to the following methods.
[0085] (reduced viscosity) A polycarbonate resin sample was dissolved in a solvent (specifically, methylene chloride) to prepare a polycarbonate resin solution with a precise concentration of 0.6 g / dL. The reduced viscosity was measured at a temperature of 20.0°C ± 0.1°C using an Ubbelohde type viscometer manufactured by Moritomo Rika Kogyo Co., Ltd. The transit time t0 of the solvent and the transit time t of the solution were measured, and the relative viscosity η was calculated from the values of t0 and t using the following formula (i). rel Calculate the relative viscosity η rel From the following formula (ii), the specific viscosity η sp In the formula (ii), η0 is the viscosity of the solvent. sp By dividing by the concentration c [g / dL] of the polycarbonate resin solution, the reduced viscosity η (η = η sp / c) was calculated. A higher reduced viscosity means a higher molecular weight. η rel =t / t0 (i) η sp =(η-η0) / η0=η rel -1 (ii)
[0086] (Glass transition temperature: Tg) The glass transition temperature was measured using a differential scanning calorimeter DSC6220 manufactured by SII NanoTechnology. Specifically, about 10 mg of a polycarbonate resin sample was placed in an aluminum sample pan manufactured by SII NanoTechnology, and sealed. The sample was heated from 30°C to 250°C at a heating rate of 20°C / min under a nitrogen gas flow of 50 mL / min. After holding at this temperature for 3 minutes, it was cooled to 30°C at a rate of 20°C / min. Next, it was held at 30°C for 3 minutes and heated again to 200°C at a rate of 20°C / min. The differential scanning calorimetry curve (DSC data) obtained in the second heating (i.e., heating) was analyzed as the measurement curve. In the measurement curve, the temperature at the intersection of a straight line extending the baseline on the low temperature side to the high temperature side and a tangent drawn at the point where the gradient of the curve of the stepwise change part of the glass transition is maximum (i.e., the extrapolated glass transition onset temperature) was obtained, and this was taken as the glass transition temperature.
[0087] (Total light transmittance, haze measurement) The total light transmittance and haze of the surface protection film were measured using a turbidity meter COH400 manufactured by Nippon Denshoku Industries Co., Ltd.
[0088] (Transmittance measurement at 360 nm) The transmittance of the surface protection film at 360 nm was measured using a UV-visible spectrophotometer V-730 manufactured by JASCO Corporation.
[0089] (Photoelastic Coefficient) For details of the measurement using a combination of a birefringence measuring device equipped with a He-Ne laser, a polarizer, a compensator, an analyzer, and a vibration type viscoelasticity measuring device (DVE-3 manufactured by Rheology Co., Ltd.), see Journal of the Society of Rheology, Japan, Vol. 19, p. 93-97 (1991). Specifically, a test piece with a width of 5 mm and a length of 20 mm was cut out from the film produced by the above-mentioned melt extrusion method. The test piece was fixed to the viscoelasticity measuring device, and the storage modulus E' was measured under the conditions of room temperature (specifically, 25°C) and a frequency of 96 Hz. During this measurement, the emitted laser light was passed through the polarizer, test piece, compensator, and analyzer in this order, and detected by a photodetector (specifically, a photodiode), and a waveform of angular frequency ω or 2ω was obtained by a lock-in amplifier. The amplitude and phase difference relative to the strain were obtained, and the strain optical coefficient O' was calculated. At this time, the directions of the absorption axes of the polarizer and the analyzer were adjusted to be perpendicular to each other and to form an angle of π / 4 with respect to the elongation direction of the test piece. The photoelastic coefficient C was calculated from the storage modulus E' and the strain optical coefficient O' by the following formula (iii). C=O' / E' (iii)
[0090] (Water absorption measurement) A square test piece measuring 10 cm in length and 10 cm in width was cut out from the film. The test piece was dried for 24 hours or more at a temperature of -10°C (Tg-10°C), which is the glass transition temperature of the polycarbonate resin constituting the test piece, under a reduced pressure of 200 Pa or less. The weight of the test piece after drying was measured to the order of 0.1 mg, and this value was taken as the dry weight. Next, the dried sample was immersed in demineralized water adjusted to 23°C for 72 hours or more. After the immersion, the test piece was taken out of the demineralized water, and all moisture on the surface was wiped off with a clean, dry cloth or filter paper, and then the weight of the test piece was measured to the order of 0.1 mg, and this value was taken as the water absorption weight. The water absorption weight was measured within 1 minute after taking it out of the water. The water absorption rate (%) was calculated from the water absorption weight and the dry weight according to the following formula (iv). Here, the calculated water absorption rate is the saturated water absorption rate. (Water absorption weight - dry weight) / dry weight x 100 = water absorption rate...(iv)
[0091] (Scratch resistance) In an environment where the temperature and humidity were adjusted to 25°C ± 5 and humidity 50% ± 5, a conical brass protrusion was placed on the surface protection film, and a weight was set on the conical brass so that the load was 100 g. In this state, the protrusion was moved at a speed of 1 mm / sec over a width of 1 cm. After that, the surface of the film was visually observed, and the case where no scratches were visible was evaluated as "○", and the case where scratches were visible was evaluated as "×".
[0092] Tables 1 and 2 show the physical properties of the polycarbonate resins and films in the examples and comparative examples described below.
[0093] [Raw materials used] The abbreviations and manufacturers of the compounds used in the Preparation Examples and Examples are as follows:
[0094] <Dihydroxy compounds> ISB: Isosorbide (manufactured by Rocket Fleuret) TCDDM: Tricyclodecane dimethanol (Oxea) CHDM: 1,4-cyclohexanedimethanol (SK Chemicals) SPG: Spiroglycol (manufactured by Mitsubishi Gas Chemical Co., Ltd.) ND: 1,9-nonanediol (Tokyo Chemical Industry Co., Ltd.)
[0095] <Carbonate diester> DPC: Diphenyl carbonate (Mitsubishi Chemical)
[0096] <Catalyst deactivator> Phosphonic acid (Tokyo Chemical Industry Co., Ltd.)
[0097] <Heat stabilizer (antioxidant)> Irganox 1010: Pentaerythritol-tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) (BASF)
[0098] (Production Example 1) Production of polycarbonate resin Polycarbonate resin was polymerized using a continuous polymerization facility consisting of three vertical stirring reactors, one horizontal stirring reactor, and a twin-screw extruder. The three vertical stirring reactors are called the first vertical stirring reactor, the second vertical stirring reactor, and the third vertical stirring reactor, respectively, and the horizontal stirring reactor is called the fourth horizontal stirring reactor. Specifically, ISB, TCDDM, and DPC were melted in tanks, respectively, and continuously fed to the first vertical stirring reactor at flow rates of 27.3 kg / hr for ISB, 15.7 kg / hr for TCDDM, and 57.6 kg / hr for DPC (molar ratio ISB / TCDDM / DPC=0.700 / 0.300 / 1.010). At the same time, an aqueous solution of calcium acetate monohydrate, which is a polymerization catalyst, was supplied to the first vertical stirring reactor in an amount such that calcium acetate monohydrate was 1.5 μmol per 1 mol of all dihydroxy compounds. The internal temperature, internal pressure, and residence time of each reactor were as follows: first vertical stirring reactor: 190°C, 25 kPa, 120 minutes, second vertical stirring reactor: 195°C, 10 kPa, 90 minutes, third vertical stirring reactor: 205°C, 4 kPa, 45 minutes, fourth horizontal stirring reactor: 220°C, 0.1 to 1.0 kPa, 120 minutes. The internal pressure of the fourth horizontal stirring reactor was finely adjusted during operation so that the reduced viscosity of the resulting polycarbonate resin was 0.38 dL / g to 0.40 dL / g.
[0099] The polycarbonate resin extracted from the fourth horizontal stirred reactor was fed in a molten state to a vented twin-screw extruder TEX30α manufactured by Japan Steel Works, Ltd. The extruder had three vacuum vents (i.e., the first vent, the second vent, and the third vent), where the remaining low molecular weight components in the resin were removed by volatilization, and phosphonic acid was added as a catalyst deactivator just before the first vent at 1.3 ppm by weight relative to the polycarbonate resin, and Irganox1010 was added just before the third vent at 1000 ppm by weight relative to the polycarbonate resin. The polycarbonate resin that had passed through the extruder was still in a molten state and passed through a 10 μm Ultipleats candle filter [manufactured by PALL] to filter out foreign matter. The polycarbonate resin was then extruded in a strand shape from the die, cooled with water, solidified, and cut with a rotary cutter to pelletize the polycarbonate resin.
[0100] (Production Example 2) Production of polycarbonate resin ISB 77.0 parts by mass (0.527 mol), TCDDM 25.9 parts by mass (0.132 mol), DPC 141.1 parts by mass (0.659 mol), and calcium acetate monohydrate 3.48 x 10 -4 Part of mass (1.98×10 -6 mol) was put into the reactor, and the inside of the reactor was replaced with reduced pressure nitrogen. Under a nitrogen atmosphere, the raw materials were dissolved while stirring the inside of the reactor at 150 ° C for about 10 minutes. In the first stage of the reaction, the temperature inside the reactor was raised to 220 ° C over 30 minutes, and the raw materials were reacted at normal pressure for 60 minutes. Next, the pressure was reduced from normal pressure to 13.3 kPa over 90 minutes, and the pressure was kept at 13.3 kPa for 30 minutes, and the generated phenol was extracted outside the reaction system. Next, in the second stage of the reaction, the heat medium temperature was raised to 220 ° C over 15 minutes, while the pressure was reduced to 0.10 kPa or less over 15 minutes, and the generated phenol was extracted outside the reaction system. After reaching a predetermined stirring torque, the pressure was returned to normal pressure with nitrogen to stop the reaction, and the generated polycarbonate resin was extruded into water, and the strands were cut to obtain pellets. The above-mentioned various evaluations were performed using the polycarbonate resin pellets obtained in this way.
[0101] (Production Example 3) Production of polycarbonate resin ISB 89.1 parts by mass (0.610 mol), TCDDM 13.3 parts by mass (0.068 mol), DPC 145.1 parts by mass (0.677 mol), and calcium acetate monohydrate 3.58 x 10 -4 Part of mass (2.03×10 -6 The procedure of Production Example 2 was repeated except that the compound was changed to (mol).
[0102] (Production Example 4) Production of polycarbonate resin ISB 56.9 parts by mass (0.389 mol), TCDDM 46.8 parts by mass (0.239 mol), DPC 134.5 parts by mass (0.628 mol), and calcium acetate monohydrate 3.31 x 10 -4 Part of mass (1.88×10-6 The procedure of Production Example 2 was repeated except that the compound was changed to (mol).
[0103] (Production Example 5) Production of polycarbonate resin The TCDDM in Production Example 2 was changed to ND and SPG was added, resulting in 71.8 parts by mass (0.491 mol) of ISB, 16.2 parts by mass (0.101 mol) of ND, 24.6 parts by mass (0.081 mol), 144.8 parts by mass (0.676 mol) of DPC, and 1.78 x 10 calcium acetate monohydrate as a catalyst. -4 Part of mass (1.01×10 -6 The procedure of Production Example 2 was repeated except that the compound was changed to (mol).
[0104] (Production Example 6) Production of polycarbonate resin The same procedure as in Production Example 1 was repeated, except that the TCDDM in Production Example 1 was changed to CHDM, the ISB was 29.8 kg / hr, the CHDM was 12.6 kg / hr, the DPC was 63.1 kg / hr (molar ratio ISB / CHDM / DPC = 0.700 / 0.300 / 1.010), and the phosphonic acid was 0.63 ppm by weight relative to the polycarbonate resin.
[0105] <Example 1> The polycarbonate resin pellets obtained in Production Example 1 were vacuum dried at 90°C for 5 hours or more. Next, using a single-screw extruder (screw diameter: 30 mm, cylinder set temperature: 220°C to 270°C) manufactured by Technobel Co., Ltd., the polycarbonate resin was extruded into a film shape from a T-die (width: 400 mm, set temperature: 200 to 270°C) by melt extrusion. The extruded film was wound into a roll shape using a winding machine while being cooled by a chill roll (set temperature: 100 to 170°C). In this way, a non-stretched film (surface protection film) with a predetermined thickness was produced. Using this film, the above-mentioned various measurements and evaluations were performed. The results are shown in Table 1.
[0106] <Example 2> Except for changing the thickness of the film, the same procedure as in Example 1 was carried out. The results are shown in Table 1.
[0107] <Example 3> The same procedure as in Example 1 was carried out except that the polycarbonate resin obtained in Production Example 2 was used and the film thickness was changed. The results are shown in Table 1.
[0108] <Comparative Example 1> Except for changing the thickness of the film, the same procedure as in Example 1 was carried out. The results are shown in Table 2.
[0109] <Comparative Example 2> The same procedure as in Example 1 was carried out except that the polycarbonate resin obtained in Production Example 3 was used and the film thickness was changed. The results are shown in Table 2.
[0110] <Comparative Example 3> The same procedure as in Example 1 was carried out except that the polycarbonate resin obtained in Production Example 4 was used and the film thickness was changed. The results are shown in Table 2.
[0111] <Comparative Example 4> The same procedure as in Example 1 was carried out except that the polycarbonate resin obtained in Production Example 5 was used and the film thickness was changed. The results are shown in Table 2. As shown in.
[0112] <Comparative Example 5> The same procedure as in Example 1 was carried out except that the polycarbonate resin obtained in Production Example 6 was used and the film thickness was changed. The results are shown in Table 2.
[0113] [Table 1]
[0114] [Table 2]
[0115] Suitable surface protection films are those that have no "x" in any of the above-mentioned characteristic evaluation items. The films of Examples 1 to 3 contain a structural unit (A) represented by formula (1) and a structural unit (B) represented by the following formula (2), the content of the structural unit (A) in the polycarbonate resin is 65 mol% or more and 85 mol% or less, and the thickness is 21 μm or more. Therefore, the films of Examples 1 to 3 were superior to the films shown in the comparative examples in terms of the overall evaluation items such as transparency, optical properties, heat resistance, and scratch resistance.
[0116] On the other hand, in Comparative Example 1, the film thickness was too thin, resulting in poor scratch resistance. Therefore, Comparative Example 1 is not suitable as a surface protection film. Comparative Example 2 has a high photoelastic coefficient and a high water absorption rate because the content of the structural unit represented by formula (1) (specifically, the structural unit derived from ISB) is too high. Therefore, Comparative Example 2 has a large optical distortion and poor dimensional stability.
[0117] Comparative Example 3 has a low Tg and poor heat resistance because the content of the structural unit represented by formula (1) (specifically, the structural unit derived from ISB) is too small. Comparative Example 4 has a low Tg because it does not have a structural unit represented by formula (2) (specifically, the structural unit derived from TCDDM). Therefore, Comparative Example 4 has poor heat resistance. Comparative Example 5 also has a high photoelastic coefficient and a low Tg because it does not have a structural unit represented by formula (2) (specifically, the structural unit derived from TCDDM). Therefore, Comparative Example 5 has a large optical distortion and poor heat resistance.
[0118] From the above results, it can be seen that a surface protection film containing a polycarbonate resin, which contains a structural unit (A) represented by formula (1) and a structural unit (B) represented by formula (2), in which the content of structural unit (A) in the polycarbonate resin is 65 mol % or more and 85 mol % or less, and has a thickness of 21 μm or more, can provide a surface protection film that is made from plant-derived raw materials and has excellent transparency, optical properties, heat resistance, and scratch resistance.
Claims
1. A surface protection film containing a polycarbonate resin, The polycarbonate resin contains a structural unit (A) represented by the following formula (1) and a structural unit (B) represented by the following formula (2), The content of the structural unit (A) in the polycarbonate resin is 65 mol % or more and 85 mol % or less, A surface protection film having a thickness of 21 μm or more. 【Chemistry 1】 【Chemistry 2】
2. 2. The surface protective film according to claim 1, which has a total light transmittance of 90% or more and a haze of 1.0% or less.
3. 3. The surface protective film according to claim 1, having a light transmittance of 60% or more at a wavelength of 360 nm.
4. 3. The surface protective film according to claim 1, which has a water absorption rate of 3.0% or less.
5. Photoelastic coefficient is 14 x 10 -12 P -1 The surface protective film according to claim 1 or 2, wherein the thickness is less than 1 mm.
6. 3. The surface protective film according to claim 1, wherein the polycarbonate resin has a glass transition temperature of 125°C or higher and 150°C or lower.
7. 3. The surface protective film according to claim 1, wherein the polycarbonate resin has a reduced viscosity at 20°C of 0.20 or more and 0.70 or less.
8. 3. The surface protective film according to claim 1, wherein the content of the phosphite compound in 100 parts by weight of the polycarbonate resin is 0.04 parts by weight or less.
9. The surface protective film according to claim 1 or 2, which is a non-stretched film.
Citation Information
Patent Citations
Base material for surface protective film, production method of the base material, surface protective film using the base material, and optical film with surface productive film
JP2020033418A
METHOD OF MANUFACTURING FILM HAVING NEGATIVE THICKNESS RETARDATION (Rth)
JP2020181204A
Polycarbonate copolymer and process for production thereof
WO2007148604A1
Surface protective film or sheet
JP2009079190A
Polarizer protective film
JP2015194754A