Fluorine-containing condensation type organosiloxane polymer precursor
A fluorine-containing condensed organosiloxane polymer precursor addresses the limitations of existing UV-resistant resins by providing high UV resistance and flexibility, ensuring effective protection for UV LEDs through thermal curing.
Patent Information
- Application Number
- JP2023047935
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Existing resin materials for UV LEDs, particularly in the deep ultraviolet region, face challenges with UV resistance, flexibility, and transmittance, and conventional methods like metallized glass sealing and adhesives fail to provide adequate protection due to material destruction and peeling.
A fluorine-containing condensed organosiloxane polymer precursor is synthesized using a specific combination of polydimethylsiloxane, tetraalkoxysilane oligomer, and an organometallic catalyst, ensuring fluorine atoms are directly bonded to silicon, allowing for thermal curing and producing a cured product with high UV resistance and flexibility.
The precursor achieves high transparency and UV resistance, particularly in the deep ultraviolet region, enabling its use as a sealant or adhesive for UV LEDs, maintaining performance over extended exposure.
Smart Images

Figure 2024136725000001 
Figure 2024136725000002 
Figure 2024136725000003
Abstract
Description
[Technical Field]
[0001] The present invention relates generally to fluorine-containing condensation-type organosiloxane polymer precursors, and more particularly to fluorine-containing condensation-type polydimethylsiloxane polymer precursors. [Background technology]
[0002] In recent years, light-emitting diodes (LEDs), which are optical components, have been shortening their emission wavelengths and increasing their output power in the sterilization and semiconductor markets, requiring improved light resistance for their components.
[0003] Conventionally, quartz glass has been used as a sealant or window material to protect LED components such as light-emitting elements, wires, and reflectors. Methods for joining quartz glass to LED elements include metallized glass sealing and gold-tin solder. This method requires a process for joining quartz glass during the manufacturing of LED elements, and this joining process requires high-temperature treatment. Furthermore, due to the hardness of the material, quartz glass and the joining material have weaknesses, such as UV (ultraviolet) resistance and thermal cycle resistance.
[0004] Another method for bonding quartz glass to LED elements is to use elastic materials such as adhesives. Especially for LEDs used in water and air sterilization, UV-resistant resins are required not only as adhesives but also as encapsulants and replacements for conventional quartz glass window materials, due to the flexibility of processing.
[0005] However, UV (ultraviolet) LEDs with wavelengths of 400 nm or less, especially in the UV-C region of 300 nm or less, have high energy even when they are low-output LEDs, making them difficult to use even with resins that have been used until now and are said to be highly heat-resistant, due to material damage and peeling from the sealing surface.
[0006] JP 2020-189964 A (Patent Document 1) describes a fluorine compound resin called Cytop manufactured by Asahi Glass Co., Ltd. This is an expensive resin intended for thin film formation, but it is recognized in the market for its light resistance to light with wavelengths in the UV range.
[0007] Japanese Patent Application Laid-Open No. 2020-9858 (Patent Document 2) describes that some silicone resins have high UV resistance and can be used in applications using deep ultraviolet rays. Silicone resins have a high degree of freedom in processing and are resins with excellent transparency and stability. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent Publication No. 2020-189964 [Patent Document 2] Japanese Patent Publication No. 2020-9858 Summary of the Invention [Problem to be solved by the invention]
[0009] However, although the fluorine compound resin described in Patent Document 1 can be used as a thin film, it cannot be used for molding a lens shape for the purpose of focusing light, or for sealing or bonding purposes on the order of millimeters or more.
[0010] Furthermore, the silicone resin described in Patent Document 2 suffers from significant reduction in transmittance and change in hardness when used in an LED with high irradiation intensity.
[0011] As such, there are few resin materials that can be used as adhesives or sealants in the UV range, especially the deep UV range, so there is a demand for materials that combine the deep UV resistance of fluororesin with the processing flexibility and high transmittance of silicone resin.
[0012] The inventors have been investigating UV-resistant materials using fluorine compounds for some time. Many of the fluorine compounds that can be synthesized and have compatibility have relatively long side chains, and many of them cause environmental problems when the fluorine atoms are released. To prevent this, it is necessary to incorporate fluorine atoms that are firmly bonded to the main chain.
[0013] On the other hand, such compounds tend to have poor reactivity due to the steric hindrance of the fluorine atoms, and require high temperatures and long curing times.
[0014] Therefore, an object of the present invention is to provide a fluorine-containing condensation-type organosiloxane polymer precursor that has little fluorine desorption and can be thermally cured to give a cured product that is UV-resistant, particularly resistant to the deep ultraviolet region. [Means for solving the problem]
[0015] The fluorine-containing condensation organosiloxane polymer precursor according to the present invention is a condensation reaction product of a mixture containing at least a condensation reaction product of at least the following (A) and (B), the following (C), and the following (D) as a catalyst, and contains one or more fluorine atoms directly bonded to silicon. (A) Polydimethylsiloxane having silanol groups at both ends, with a number average molecular weight (Mn) of more than 10,000 and less than 60,000. (B) A tetraalkoxysilane oligomer, which is a linear tetramer to decamer and has a methoxy group or an ethoxy group as an alkoxy group. (C) Silane compounds having fluorine and alkoxy groups directly bonded to silicon. (D) a condensation and cure-accelerating catalyst which is an organometallic compound.
[0016] This makes it possible to provide a fluorine-containing condensation organosiloxane polymer precursor that has little fluorine desorption and that can be thermally cured to give a cured product that is UV-resistant, particularly resistant to the deep ultraviolet region. DETAILED DESCRIPTION OF THE INVENTION
[0017] The materials used in the present invention will be described in detail below.
[0018] <Polydimethylsiloxane (A) having silanol groups at both ends> The fluorine-containing condensation organosiloxane polymer precursor of the present invention is made from polydimethylsiloxane (PDMS) with reactive silanol groups at both ends. Various raw materials were considered, including those with silanol groups at both ends, branched molecular chains, or those with multiple silanol groups at the ends, as well as those with other reactive functional groups. However, when considering incorporating fluorine through the reaction of fluorine-containing compounds, the steric hindrance of the fluorine atoms made these difficult to synthesize. Consequently, a linear PDMS with silanol groups at both ends was found to be optimal for creating a fluorine-containing condensation polydimethylsiloxane polymer precursor. The general chemical formula is shown in Formula (1). H-(O-Si(CH3)2) m -OH (Formula 1)
[0019] The polydimethylsiloxane having silanol groups at both ends is linear and has a number average molecular weight (Mn) of more than 10,000 and less than 60,000, and m in the formula (1) is 134-810.
[0020] If the number-average molecular weight is 10,000 or less, the fluorine-containing condensation-type polydimethylsiloxane cured body obtained by curing the synthesized fluorine-containing condensation-type polydimethylsiloxane polymer precursor becomes hard, making it difficult to relieve thermal stress. As a result, UV resistance is reduced. On the other hand, if the number-average molecular weight is 60,000 or more, the steric hindrance of fluorine makes the fluorine incorporation reaction very difficult. Therefore, the number-average molecular weight of the raw material PDMS with terminal silanol groups is preferably greater than 10,000 and less than 60,000, and more preferably greater than 20,000 and less than 60,000.
[0021] The molecular weight distribution index Mw / Mn (Mw / Mn; Mw is the weight-average molecular weight) is preferably greater than 1.3, and more preferably 1.5 or greater. The molecular weight distribution index Mw / Mn is generally 1.3 or greater for general-purpose silicones, and 1.5 or greater for those with high molecular weights. Although products with a molecular weight distribution index Mw / Mn of 1.1 or less are commercially available using highly homogeneous living polymerization, in order to obtain UV resistance, a high molecular weight distribution index Mw / Mn is preferable, rather than such highly homogeneous PDMS.
[0022] A small molecular weight distribution index (Mw / Mn) is advantageous in that it provides good transparency and homogeneity to light and allows the curing reaction to be completed quickly. However, a polymer with a small molecular weight distribution has low toughness against deformation and a reduced thermal stress relaxation capacity. The inventors believe that this is because the presence of molecules with a certain degree of molecular weight difference acts as a cushion, absorbing the impact associated with thermal deformation. In terms of optical properties, a molecular weight distribution index (Mw / Mn) of 1.3 or less is desirable. However, in terms of resistance to UV rays, a molecular weight distribution index (Mw / Mn) of greater than 1.3 is preferable, with 1.5 or greater being more preferable.
[0023] <Silane oligomer (B) having an alkoxy group> Silane oligomers with alkoxy groups are generally known as compounds such as methyl silicate and ethyl silicate, and are easily available. The general structural formula of these oligomers, alkyl silicates, is shown below in formula (2). (RO)3Si-O-(Si(OR)2-O) n -Si-(OR)3 formula (2)
[0024] Here, R is a methyl or ethyl group. In the case of a methyl group, the reaction proceeds rapidly, but methanol may be generated as a by-product, so it is preferable to use an ethyl group. n can be an integer greater than or equal to 1, but commercially available products generally have n = 4 to 10 (tetramer to decamer). Although synthesis is theoretically possible with n greater than 10, oligomers to be reacted with polymers with long molecular chains do not harden, so n = 4 to 10 is practical. Note that commercially available products often contain unreacted raw materials, so it is desirable to purify them using distillation or other methods.
[0025] <Silane compound (C) having fluorine and alkoxy groups directly bonded to silicon> Silane compound (C) having fluorine and alkoxy groups directly bonded to silicon is a silane compound with one fluorine atom and three alkoxy groups directly bonded to the silicon atom. There are no restrictions on the alkoxy group, but an ethoxy group is preferred from the standpoint of ease of reaction control. This compound is highly reactive and volatile, and it is expected that it would be difficult to control the reaction with a methoxy group, which generally has high reactivity. The general structural formula of this silane compound (C) is shown below in formula (3). F-Si(OC n H m )3 (n is an integer greater than or equal to 1, m = 2n + 1) Equation (3)
[0026] <Organometallic compound (D)> The fluorine-containing condensation-type organosiloxane polymer precursor of the present invention is synthesized using an organometallic compound condensation and curing-accelerating catalyst. There are no limitations on the metal-based catalyst, but Sn-based catalysts are the most effective because they are easy to use and can be added in small amounts. Metal-based catalysts include organometallic compounds other than Sn, such as Ti-based, Al-based, Zn-based, Zr-based, and Bi-based compounds. However, these have low reactivity and can cause problems such as reduced heat resistance and discoloration of the cured product if they remain. Therefore, Sn-based catalysts are the most effective, despite their environmental and safety issues.
[0027] Common Sn-based catalysts include dibutyltin dilaurate, dibutyltin diacetate, dibutyltin bisacetylacetonate, etc. Depending on the synthesis conditions, a small amount of Sn-based catalyst can effectively promote condensation reactions, and the amount can be kept below 500 ppm.
[0028] <Measurement of average molecular weight> The average molecular weight of the PDMS (A) was measured by gel permeation chromatography (GPC), and the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) was used as the molecular weight distribution index. Polystyrene was used as a standard sample to measure the molecular weight in terms of polystyrene. The measurement of the molecular weight in terms of polystyrene by GPC was carried out under the following measurement conditions. a) Measuring equipment: Tosoh GPC HLC-8320PC b) Columns with Mn of 30,000 or less: TSKgel guardColumn Super HZ-H, TSKgel Super HZM-H x 2 c) Columns with Mn of 30,000 or more: TSKgel guardColumn Super MP(HZ)-N, TSKgel Multipore HZ-N x 3 d) Oven temperature: 40℃ e) Eluent: tetrahydrofuran (THF) 1.0 mL / min f) Standard sample: polystyrene g) Injection volume: 100μL h) Concentration: 0.05g / 10mL i) Sample preparation: THF containing 0.2% by mass of 2,6-di-tert-butyl-p-phenol (BHT) was used as a solvent, and the sample was dissolved by stirring at room temperature. j) Correction: The deviation of the BHT peak between the calibration curve measurement and the sample measurement is corrected, and the molecular weight is calculated.
[0029] <Preparation of Fluorine-Containing Condensed Polydimethylsiloxane Polymer Precursor (E)> The fluorine-containing condensation-type organosiloxane polymer precursor of the present invention, i.e., a fluorine-containing condensation-type polydimethylsiloxane polymer precursor, is synthesized by a condensation reaction of dehydration and dealcoholization by heating a mixture of the condensation reaction product of (A) and (B) above with (C) above in the presence of an organometallic compound (D) as a catalyst.
[0030] Polydimethylsiloxane (A) with silanol groups at both ends and silane oligomer (B) with alkoxy groups are mixed in a molar ratio and undergo a condensation reaction through dehydration and dealcoholization by heat treatment. This reaction is controlled over a period of several to several tens of hours, yielding a condensation-type polydimethylsiloxane polymer precursor. For synthesis, a reaction vessel (a flask with multiple openings) equipped with a stirrer, thermometer, and drip line is used. Any stirring device can be used, including a rotary stirrer with impellers, a magnetic stirrer, a two-axis planetary stirrer, or an ultrasonic cleaner, as long as it is effective in homogeneously mixing the highly viscous liquid raw materials involved in the reaction. However, rotary stirrers and magnetic stirrers are preferred, as they require temperature control, atmosphere control, and drip lines for the components. Uniformity of the synthesis temperature is important. The synthesis temperature is preferably set between 60 and 140°C. The synthesis atmosphere is individually set depending on the type of raw materials, the blending ratio, the synthesis equipment, etc., such as when the reaction is carried out at a low temperature for a long period of time or when the synthesis is carried out at a high temperature for a short period of time. The synthesis atmosphere uses, for example, nitrogen gas as an inert gas, and the reaction vessel is sufficiently filled with nitrogen gas with a constant moisture content. In this case, the nitrogen gas can be obtained from a nitrogen gas production device, a cylinder, or liquid nitrogen.
[0031] The molar ratio (compounding ratio) of polydimethylsiloxane (A) having silanol groups at both ends to silane oligomer (B) having alkoxy groups is preferably adjusted to (A) / (B) in the range of 0.1 to 4. By maintaining the (A) / (B) molar ratio in the above range and conducting the condensation reaction under conditions suitable for condensation, gelation during or after the reaction is less likely to occur, and a stable sol can be obtained without residual low-molecular-weight siloxane. The (A) / (B) molar ratio is preferably 0.1 to 4, more preferably 1 to 2.
[0032] The molar ratio referred to here is the molar ratio calculated based on the number average molecular weight (Mn) of PDMS measured by gel permeation chromatography (GPC) using polystyrene as the standard substance and tetrahydrofuran as the eluent, and the purity and average molecular weight of the tetraalkoxysilane oligomer.
[0033] The synthesized condensation-type polydimethylsiloxane polymer precursor is heated with a silane compound (C) having fluorine and an alkoxy group directly bonded to silicon in the presence of an organometallic compound (D) to cause a condensation reaction through dehydration and dealcoholization. The organometallic compound (D) is used here as a condensation-promoting catalyst. The synthesis temperature is preferably set appropriately between 60 and 140°C.
[0034] Silane compound (C), which has fluorine and alkoxy groups directly bonded to silicon, is highly reactive, making temperature control important. This compound reacts with the condensation-type polydimethylsiloxane polymer precursor prepared earlier via the alkyl group, but the precursor's functional groups must be hydrolyzed to leave reactive silanol groups. For this reason, some kind of hydrolysis treatment is desirable, but since hydrolysis generally occurs during the synthesis process due to atmospheric water vapor, it is not necessarily necessary to incorporate a hydrolysis treatment.
[0035] The amount of the silane compound (C) having fluorine and an alkoxy group directly bonded to silicon is adjusted to 0.5 to 10 moles per mole of the polydimethylsiloxane (A) having silanol groups at both ends. If the amount is less than 0.5 moles per mole of polydimethylsiloxane (A), resistance to deep ultraviolet light is not obtained, and if the amount is more than 10 moles per mole of polydimethylsiloxane (A), gelation occurs. The amount of the silane compound (C) having fluorine and an alkoxy group directly bonded to silicon is preferably 0.5 to 10 moles, more preferably 4 to 8 moles, per mole of polydimethylsiloxane (A).
[0036] The synthesized fluorine-containing condensation polydimethylsiloxane polymer precursor (E) becomes a highly transparent and UV-resistant fluorine-containing condensation polydimethylsiloxane cured body through heat treatment. It also has adhesive properties, making it possible to fill UV-LED packages and use it as an encapsulant. Because it also has adhesive properties, it can be used to fixate quartz window materials for UV-LEDs and as a coating film. Because of its high UV resistance, it can be applied to optical components that use light in the deep ultraviolet region, particularly around 265 nm.
[0037] An organometallic compound (D) can be used as a catalyst to obtain a cured product. Here, the organometallic compound (D) is used as a curing-accelerating catalyst. The organometallic compound (D) is added during the synthesis of the fluorine-containing condensation-type polydimethylsiloxane polymer precursor (E), but further organometallic compound (D) may be added before thermal curing. It is desirable to use an appropriate curing agent depending on the shape, size, thickness, etc. of the resulting cured product.
[0038] Furthermore, the fluorine-containing condensation type organosiloxane polymer precursor of the present invention can be placed in a mold material that has been processed in the depth direction, and then thermally cured to obtain a resin molded product.
[0039] Fluorine-containing condensation polydimethylsiloxane polymer precursor (E) can be used as a coating, potting, or adhesive layer, and can also be placed in a mold that allows shape transfer and processed into a resin molded body. For coating or potting, it can be cured by degassing and desolvating at around 100°C, and then baking at 150-200°C. When used as an adhesive layer, it can be primarily cured at around 150°C, retaining its viscosity and adhesiveness, allowing the objects to be bonded together. To obtain a resin molded body, it can be poured into a mold and shaped.
[0040] The fluorine-containing condensation polydimethylsiloxane polymer precursor (E) contains hydroxyl groups and alkoxy groups that react with hydroxyl groups within its molecule. These functional groups undergo dealcoholization and dehydration reactions when the reaction by-products are removed from the system at temperatures above 100°C. Therefore, when obtaining a resin molded product, if functional groups such as hydroxyl groups are present on the surface of the mold material, a condensation reaction will occur, bonding the material to the mold and making it difficult to demold. While it is possible to make demolding easier by treating the mold surface with fluorine, this is expensive, and the resulting film often lacks durability and requires maintenance.
[0041] In the case of mold molding, demolding is facilitated by using a mold shaped using an acrylic resin, fluororesin, or olefin resin, which has a relatively low surface functional group and can be mirror-finished. By pouring a fluorine-containing condensation polydimethylsiloxane polymer precursor (E) into the mold and holding it at 100°C or less for a certain period of time, a demoldable fluorine-containing condensation polydimethylsiloxane polymer cured product (F) can be obtained. In mold molding, the thermosetting temperature is preferably 60°C to 100°C, more preferably 80°C to 100°C, and even more preferably a temperature above 80°C but below 100°C. Subsequently, secondary curing, if necessary, can be performed to obtain a resin molded product with light resistance in the deep ultraviolet region.
[0042] The present invention provides a material that can be used as a sealing layer or adhesive layer, window material, or lens that has excellent light resistance in the UV region, particularly the deep UV region, and that does not experience deterioration in properties such as deformation, breakage, discoloration, or peeling due to deep UV light over a long period of time. UV-LEDs made from resin materials, particularly resin materials that can be used in the deep UV region, can promote the use of ultraviolet light in the medical, optical, and industrial fields, providing significant benefits.
[0043] The present invention can be summarized as follows.
[0044] (1) The fluorine-containing condensation organosiloxane polymer precursor according to the present invention is a condensation reaction product of a mixture containing at least a condensation reaction product of the following (A) and (B), the following (C), and the following (D) as a catalyst, and contains one or more fluorine atoms directly bonded to silicon: (A) Polydimethylsiloxane having silanol groups at both ends, with a number average molecular weight (Mn) of more than 10,000 and less than 60,000. (B) A tetraalkoxysilane oligomer, which is a linear tetramer to decamer and has a methoxy group or an ethoxy group as an alkoxy group. (C) Silane compounds having fluorine and alkoxy groups directly bonded to silicon. (D) Organometallic compounds.
[0045] (2) In the fluorine-containing condensation-type organosiloxane polymer precursor according to the present invention, the mixture preferably contains 0.5 to 10 moles, more preferably 4 to 8 moles, of (C) per mole of (A).
[0046] (3) The cured product according to the present invention is a cured product obtained by thermally curing the fluorine-containing condensation-type organosiloxane polymer precursor described in (1) or (2) above, and preferably has a light transmittance of 80% or more at a wavelength of 200 to 300 nm.
[0047] (4) A method for producing a cured product according to the present invention includes the steps of placing the fluorine-containing condensation-type organosiloxane polymer precursor described in (1) or (2) above in a mold formed from an acrylic resin, a fluororesin, or an olefin-based resin, and thermally curing the polymer at a temperature of 100°C or less. [Example]
[0048] The present invention will be explained in more detail below using examples, but the present invention is not limited to these examples in any way.
[0049] <Preparation of Fluorine-Containing Condensed Polydimethylsiloxane Polymer Precursor (E)> A reaction vessel equipped with a stirrer, a thermometer, and a dropping line was filled with nitrogen gas. The nitrogen gas used was produced by a nitrogen gas production apparatus (UNX-200 manufactured by Japan Unix Corporation).
[0050] Next, PDMS (A) with silanol groups at both ends, tetraalkoxysilane oligomer (B), and solvent were added to the reaction vessel filled with nitrogen gas. After stirring until (A) and (B) were homogeneous, a condensation catalyst was added and the mixture was allowed to react at 120°C for 1 hour. The mixture was then allowed to cool naturally to room temperature, yielding a condensation-type polydimethylsiloxane polymer precursor. To this precursor, a silane compound (C) with fluorine and alkoxy groups directly bonded to silicon and an organometallic compound (D) as a catalyst were added. The mixture was then filled with nitrogen in the same way as before, mixed until transparent, reacted at 120°C for 30 minutes, and then allowed to cool naturally to room temperature, yielding a fluorine-containing condensation-type polydimethylsiloxane polymer precursor (E).
[0051] The masses of the raw materials used and their respective molar ratios (number of moles per mole of polydimethylsiloxane (A)) are shown in Table 1 (Examples 1 to 9) and Table 2 (Comparative Examples 1 to 3).
[0052] [Table 1]
[0053] [Table 2]
[0054] The materials used were as follows:
[0055] PDMS(A): Nusil PLY2-7630 (number average molecular weight (Mn) 27100, molecular weight distribution index Mw / Mn = 2.21), Nusil PLY1-7630 (number average molecular weight (Mn) 18800, molecular weight distribution index Mw / Mn = 1.87), Nusil PRO-2369 (number average molecular weight Molecular weight (Mn) 54300, molecular weight distribution index Mw / Mn=1.94), JNC FM-9927 (number average molecular weight (Mn) 35000, molecular weight distribution index Mw / Mn=1.10), JNC FM-9925A (number average molecular weight (Mn) 10000, molecular weight distribution index Mw / Mn=1.10).
[0056] Silicate oligomer (B): Ethyl silicate, manufactured by Tama Chemicals Co., Ltd., silicate 40 (a linear tetra- to hexamer oligomer of tetraethoxysilane, average molecular weight 745. Distilled at 130°C for 2 hours before use.)
[0057] Fluoroalkylsilane (C): Triethoxyfluorosilane (Azmak The materials used were nonafluorohexyltrimethoxysilane (fluorine is not directly bonded to silicon, manufactured by Azmax Corporation).
[0058] Tertiary butanol manufactured by Wako Pure Chemical Industries was used as the solvent.
[0059] <Preparation of Fluorine-Containing Condensation-Type Polydimethylsiloxane Polymer Cured Material (F)> A dome-shaped depression measuring 2 cm in diameter and 1 cm in depth was created in acrylic resin, and the surface was polished to create a mold. The fluorine-containing condensation-type polydimethylsiloxane polymer precursor (E) from Example 1 was poured into this mold, and the temperature and time conditions under which it could be demolded were determined. The results are shown in Table 3.
[0060] [Table 3]
[0061] The results shown in Table 3 show that adhesion to the mold can be avoided by heat curing at a temperature of 100°C or less. The heat curing temperature is preferably 60°C or more and 100°C or less, more preferably 80°C or more and 100°C or less, and even more preferably a temperature higher than 80°C and 100°C or less.
[0062] <Evaluation of light transmittance> <Preparation of evaluation samples> A fluorine-containing condensed polydimethylsiloxane polymer precursor (E) was applied to a 10 mm x 20 mm, 0.5 mm thick quartz substrate, and vacuum degassed for 15 minutes. Another quartz substrate of the same size was placed on top of the coating, and the coating was then heated at 80°C for 30 minutes and then baked at 220°C for 3 hours.
[0063] <Exposure test at 258 nm> The example and comparative example samples prepared by the above method were illuminated with a low-pressure mercury lamp at 258 nm and an output of 17 mW / m using an SSP16-110 manufactured by Sen Special Light Sources Co., Ltd. 2 The changes in appearance and transmittance at 265 nm were compared from the initial time point to 500 hours and 1000 hours later. The results are shown in Table 4.
[0064] [Table 4]
[0065] The results in Table 4 show that all Examples exhibited high transmittance of 90% or more at 265 nm. Even after 500 hours of irradiation testing, all Examples still exhibited transmittance of 90% or more, and even after 1000 hours of irradiation testing, almost all Examples still exhibited transmittance of 90% or more. On the other hand, Comparative Example 1 gelled, and Comparative Example 2 had an initial transmittance of 100% but developed cracks after 500 hours of irradiation testing. Comparative Example 3 had an initial transmittance of over 90%, but after 500 hours of irradiation testing, the transmittance decreased to 87.6%.
[0066] [Example of change] The present invention is not limited to the above examples, and modifications, deletions, and additions are possible as long as they do not violate the technical concept of the present invention, which can be recognized by those skilled in the art from the claims and the description of the specification. Furthermore, the above examples are not limited to these, and organometallic compounds of different types and characteristics may be used.
Claims
1. A condensation reaction product of at least the following (A) and the following (B): The following (C) and A fluorine-containing condensation-type organosiloxane polymer precursor, which is a condensation reaction product of a mixture containing at least the following (D) as a catalyst, and which contains one or more fluorine atoms directly bonded to silicon: (A) A polydimethylsiloxane having silanol groups at both ends and having a number average molecular weight (Mn) of more than 10,000 and less than 60,000. (B) A tetraalkoxysilane oligomer which is linear and has a methoxy group or an ethoxy group as an alkoxy group. (C) A silane compound having a fluorine atom and an alkoxy group directly bonded to silicon. (D) Organometallic compound.
2. 2. The fluorine-containing condensation type organosiloxane polymer precursor according to claim 1, wherein the mixture contains 0.5 to 10 moles of the (C) per mole of the (A).
3. A fluorine-containing condensation-type organosiloxane polymer, which is a cured product obtained by thermally curing the fluorine-containing condensation-type organosiloxane polymer precursor according to claim 1 or 2, and has a light transmittance of 80% or more at a wavelength of 200 to 300 nm.
4. A method for producing a cured product, comprising the steps of placing the fluorine-containing condensation-type organosiloxane polymer precursor according to claim 1 or 2 in a mold formed of an acrylic resin, a fluororesin, or an olefin-based resin, and thermally curing the precursor at a temperature of 100° C. or less.
Citation Information
Patent Citations
Composition for sealant, and light-emitting device and solar cell module using the composition for sealant
JP2012116990A
Fluorine-containing condensed type organopolysiloxane prepolymer and cured product thereof
JP2020158692A
Light-emitting device and sterilizer
JP2020009858A
Resin composition and ultraviolet light-emitting device
JP2020189964A
Cited By
Organopolysiloxane prepolymer and cured body of said organopolysiloxane prepolymer
WO2026042613A1