Method for producing silicone polymer
The method addresses resin degradation in flow synthesis by using a controlled heating and pressure process with specific solvents and resins, enabling stable and continuous silicone polymer production.
Patent Information
- Application Number
- JP2023047985
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Conventional flow synthesis methods struggle to continuously produce silicone polymers with stable molecular weight over a long period due to ion exchange resin degradation and crushing issues.
A method involving a mixed solution of silane compounds, water, and alcohol with a boiling point of 100°C or less is continuously supplied to a packed tower filled with ion exchange resin, heated at 70 to 120°C under 0.05 to 5.0 MPa gauge pressure, using cation or anion exchange resins to promote hydrolysis and condensation while maintaining resin integrity.
Enables the automatic and continuous production of silicone polymers with stable molecular weight and high polymerization rate, reducing resin degradation and allowing for long-term operation.
Smart Images

Figure 2024136756000002 
Figure 2024136756000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a silicone polymer. [Background technology]
[0002] Silicone polymers are organic-inorganic hybrid materials in which organic and inorganic compounds are combined at the molecular level. They have been the subject of intensive research in recent years because they combine the properties of organic materials, such as flexibility and processability, with the properties of inorganic materials, such as heat resistance, weather resistance, and chemical resistance.
[0003] In particular, in pattern molding for manufacturing semiconductor elements, etc., it has been proposed to use a silicone polymer as a resist underlayer film when forming a reverse pattern using lithography technology, etching technology, etc. Silicone polymers that contain a large amount of structures derived from tetramethoxysilane or tetraethoxysilane in particular have been known to have excellent embedding properties in fine resist underlayer film patterns and excellent etching resistance when the resist underlayer film pattern is removed by oxygen-based gas etching, etc.
[0004] On the other hand, the practical application of flow synthesis is being promoted. Flow synthesis is a method in which raw materials are generally continuously supplied by pumps or the like and reacted in a tubular reactor, a packed tower, or a continuous stirring tank type reactor. In particular, when a tubular reactor or a packed tower is filled with a heterogeneous catalyst and reacted, it is not necessary to remove the catalyst, so waste generated in the post-treatment process can be minimized or completely eliminated. The equipment can be designed to be smaller than the batch method, which can significantly save space and cost. Furthermore, flow reactors have a larger surface area per volume than batch reactors, and are capable of rapid mixing and stopping of solutions containing substrates, which is known to improve safety and efficiency (Non-Patent Document 1), and are expected to be the next-generation manufacturing method.
[0005] Attempts have been made to obtain silicone polymers using the flow synthesis method. It is known that after mixing alkoxysilane and ion-exchanged water in a mixer, the mixture is fed into a packed tower filled with ion-exchange resin, and the reaction liquid that flows out of the packed tower is concentrated to obtain hydrolysis products of the alkoxysilane and their condensation products (Patent Documents 1 and 2).
[0006] However, when attempting to obtain a silicone polymer with a certain degree of polymerization, there has been a problem in that it is not possible to obtain a silicone polymer automatically and continuously for a long period of time. [Prior art documents] [Non-patent literature]
[0007] [Non-Patent Document 1] Osamu Kobayashi and Toshiya Onozawa, editors and translators, Flow Chemistry for Organic Synthesis, 266p, Tokyo Kagaku Dojin (2020) [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 8-151445 [Patent Document 2] JP 2011-219647 A Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide a production method which can automatically and continuously produce a silicone polymer with a stable molecular weight over an extended period of time while obtaining a high polymerization rate. [Means for solving the problem]
[0010] The inventors have conducted extensive research into the problems associated with conventional flow synthesis methods and have found that, when a packed column is heated, the catalytic activity of the ion exchange resin deteriorates, resulting in a gradual decrease in the molecular weight obtained or the ion exchange resin is broken down, and have thus arrived at the present invention.
[0011] The present invention and its preferred embodiments comprise the following: [1] A method for producing a silicone polymer, comprising continuously supplying a mixed liquid containing at least one silane compound selected from compounds represented by the following general formula (1) and compounds represented by the following general formula (2), water, and an alcohol having a boiling point of 100°C or less to a packed tower packed with an ion exchange resin, and contacting the mixed liquid with the ion exchange resin at 70 to 120°C under a pressure indicated by a gauge pressure of 0.05 to 5.0 MPa on a pressure gauge installed on the outlet side of the packed tower. [2] The method for producing a silicone polymer according to the above [1], wherein the ion exchange resin is a cation exchange resin. [3] The method for producing a silicone polymer according to the above [1] or [2], wherein the alcohol having a boiling point of 100°C or less includes at least one selected from the group consisting of methanol, ethanol, n-propanol, and i-propanol. [4] The method for producing a silicone polymer according to any one of the above [1] to [3], wherein the amount of the alcohol having a boiling point of 100° C. or less used is 1.0 to 10 times by mass relative to the silane compound. Effect of the Invention
[0012] According to the present invention, it is possible to automatically and continuously produce a silicone polymer with a stable molecular weight for an extended period of time while obtaining a high polymerization rate. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic diagram of a flow reactor used in the method for producing a silicone polymer of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] In the method for producing a silicone polymer of the present invention, a mixed liquid containing a silane compound, water, and an alcohol is continuously supplied to a packed column packed with an ion exchange resin, and brought into contact with the ion exchange resin.
[0015] The silane compound is at least one selected from the group consisting of compounds represented by the following general formula (1) and compounds represented by the following general formula (2). R a Si(OR 1 ) 4-a ...(1) In formula (1), R is a hydrogen atom or a monovalent organic group, R 1 represents a monovalent organic group, and a represents an integer of 1 or 2. Si(OR 2 )4...(2) In formula (2), R 2 represents a monovalent organic group.
[0016] R and R in the above general formula (1) 1 and R in general formula (2) 2 Examples of the monovalent organic group include an alkyl group, an aryl group, an allyl group, a glycidyl group, etc. In addition, in the general formula (1), R is preferably a monovalent organic group, particularly an alkyl group or an aryl group.
[0017] Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, and a butyl group, and preferably have 1 to 5 carbon atoms. These alkyl groups may be linear or branched, and further, hydrogen atoms may be substituted with fluorine atoms or the like.
[0018] Examples of the aryl group include a phenyl group, a naphthyl group, a methylphenyl group, an ethylphenyl group, a chlorophenyl group, a bromophenyl group, and a fluorophenyl group.
[0019] Specific examples of the compound represented by the general formula (1) include methyltrimethoxysilane, methyltriethoxysilane, methyltri-n-propoxysilane, methyltri-iso-propoxysilane, methyltri-n-butoxysilane, methyltri-sec-butoxysilane, methyltri-tert-butoxysilane, methyltriphenoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltri-n-propoxysilane, ethyltri-iso-propoxysilane, ethyltri-n-butoxysilane, and ethyltri-sec-butoxysilane. silane, ethyl tri-tert-butoxysilane, ethyl triphenoxysilane, vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tri-n-propoxysilane, vinyl tri-iso-propoxysilane, vinyl tri-n-butoxysilane, vinyl tri-sec-butoxysilane, vinyl tri-tert-butoxysilane, vinyl triphenoxysilane, n-propyl trimethoxysilane, n-propyl triethoxysilane, n-propyl tri-n-propoxysilane, n-propyl tri-iso-propoxysilane, n-propyl Tri-n-butoxysilane, n-propyl tri-sec-butoxysilane, n-propyl tri-tert-butoxysilane, n-propyl triphenoxysilane, i-propyl trimethoxysilane, i-propyl triethoxysilane, i-propyl tri-n-propoxysilane, i-propyl tri-iso-propoxysilane, i-propyl tri-n-butoxysilane, i-propyl tri-sec-butoxysilane, i-propyl tri-tert-butoxysilane, i-propyl triphenoxysilane, n-butyl trimethoxysilane, n-butyl n-butyltriethoxysilane, n-butyltri-n-propoxysilane, n-butyltri-iso-propoxysilane, n-butyltri-n-butoxysilane, n-butyltri-sec-butoxysilane, n-butyltri-tert-butoxysilane, n-butyltriphenoxysilane, sec-butyltrimethoxysilane, sec-butyltriethoxysilane, sec-butyltri-n-propoxysilane, sec-butyltri-iso-propoxysilane, sec-butyltri-n-butoxysilane, sec-butyltri-sec-butoxysilane,sec-Butyltri-tert-butoxysilane, sec-Butyltriphenoxysilane, t-Butyltrimethoxysilane, t-Butyltriethoxysilane, t-Butyltri-n-propoxysilane, t-Butyltri-iso-propoxysilane, t-Butyltri-n-butoxysilane, t-Butyltri-sec-butoxysilane, t-Butyltri-tert-butoxysilane, t-Butyltriphenoxysilane, Phenyltrimethoxysilane, Phenyltriethoxysilane, Phenyltri-n-propoxysilane, Phenyltri-iso-propoxy Silane, phenyltri-n-butoxysilane, phenyltri-sec-butoxysilane, phenyltri-tert-butoxysilane, phenyltriphenoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, gamma-aminopropyltrimethoxysilane, gamma-aminopropyltriethoxysilane, gamma-glycidoxypropyltrimethoxysilane, gamma-glycidoxypropyltriethoxysilane, gamma-trifluoropropyltrimethoxysilane, gamma-trifluoropropyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane , dimethyl-di-n-propoxysilane, dimethyl-di-iso-propoxysilane, dimethyl-di-n-butoxysilane, dimethyl-di-sec-butoxysilane, dimethyl-di-tert-butoxysilane, dimethyldiphenoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, diethyl-di-n-propoxysilane, diethyl-di-iso-propoxysilane, diethyl-di-n-butoxysilane, diethyl-di-sec-butoxysilane, diethyl-di-tert-butoxysilane, diethyldiphenoxysilane, di-n-propoxysilane Pyrdimethoxysilane, di-n-propyldiethoxysilane, di-n-propyl-di-n-propoxysilane, di-n-propyl-di-iso-propoxysilane, di-n-propyl-di-n-butoxysilane, di-n-propyl-di-sec-butoxysilane, di-n-propyl-di-tert-butoxysilane, di-n-propyl-di-phenoxysilane, di-iso-propyldimethoxysilane, di-iso-propyldiethoxysilane, di-iso-propyl-di-n-propoxysilane, di-iso-propyl-di-iso-propoxysilane,Di-isopropyl-di-n-butoxysilane, di-isopropyl-di-sec-butoxysilane, di-isopropyl-di-tert-butoxysilane, di-isopropyl-di-phenoxysilane, di-n-butyldimethoxysilane, di-n-butyldiethoxysilane, di-n-butyl-di-n-propoxysilane, di-n-butyl-di-isopropoxysilane, di-n-butyl-di-n-butoxysilane, di-n- Butyl-di-sec-butoxysilane, di-n-butyl-di-tert-butoxysilane, di-n-butyl-di-phenoxysilane, di-sec-butyldimethoxysilane, di-sec-butyldiethoxysilane, di-sec-butyl-di-n-propoxysilane, di-sec-butyl-di-iso-propoxysilane, di-sec-butyl-di-n-butoxysilane, di-sec-butyl-di-sec-butoxysilane, di-sec-butyl di-tert-butyl-di-tert-butoxysilane, di-sec-butyl-di-phenoxysilane, di-tert-butyldimethoxysilane, di-tert-butyldiethoxysilane, di-tert-butyl-di-n-propoxysilane, di-tert-butyl-di-iso-propoxysilane, di-tert-butyl-di-n-butoxysilane, di-tert-butyl-di-sec-butoxysilane, di-tert-butyl-di-tert-butoxy Examples of the silane include di-tert-butyl-di-phenoxysilane, diphenyldimethoxysilane, diphenyl-di-ethoxysilane, diphenyl-di-n-propoxysilane, diphenyl-di-iso-propoxysilane, diphenyl-di-n-butoxysilane, diphenyl-di-sec-butoxysilane, diphenyl-di-tert-butoxysilane, diphenyldiphenoxysilane, and divinyltrimethoxysilane.
[0020] Among the compounds represented by the general formula (1), methyltrimethoxysilane, methyltriethoxysilane, methyltri-n-propoxysilane, methyltri-iso-propoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, etc. are easily available industrially and are therefore preferred. These may be used alone or in combination of two or more.
[0021] Specific examples of the compound represented by the general formula (2) include tetramethoxysilane, methoxytriethoxysilane, dimethoxydiethoxysilane, trimethoxyethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetra-iso-propoxysilane, tetra-n-butoxysilane, tetra-sec-butoxysilane, tetra-tert-butoxysilane, tetraphenoxysilane, etc. Among these, tetramethoxysilane and tetraethoxysilane are preferred because they are easily available industrially.
[0022] The water is used for hydrolysis and polycondensation of the silane compound. The type of water used may be industrial water, city water, well water, distilled water, ion-exchanged water, ultrapure water, etc. One or more of these may be used.
[0023] Among these, ion-exchanged water and ultrapure water, which have high electrical resistivity, are preferred, and ultrapure water with an electrical resistivity of 15 MΩ·cm or more is more preferred because of its low metal content.
[0024] The amount of water used is preferably 1.0 to 15.0 equivalents relative to 1.0 equivalent of the total amount of alkoxyl groups of the silane compound. When the amount of water is 1.0 equivalent or more, the hydrolysis and condensation polymerization reaction proceeds quickly, whereas when the amount of water is 15.0 equivalents or less, more preferably 10.0 equivalents or less, and even more preferably 5.0 equivalents or less, the reaction is controlled and gelation does not occur, which is preferable.
[0025] The water may be mixed with the silane compound first, or may be added to the alcohol described below. When the water is added to the alcohol, unintended hydrolysis of the silane compound can be prevented, which is preferable.
[0026] The alcohol makes it easier for the silane compound and the water to mix. It is important that the alcohol has a boiling point of 100°C or less. In the prior art, for example, when propylene glycol monoethyl ether with a boiling point of 146°C is used as a solvent, it was found that the catalytic ability of the ion exchange resin decreases and the ion exchange resin deforms and breaks. In the method for producing a silicone polymer of the present invention, since the boiling point of the alcohol is 100°C or less, even if the reaction solution containing the alcohol and the ion exchange resin are heated, the catalytic ability of the ion exchange resin does not decrease and the ion exchange resin does not deform or break, and it can be used repeatedly for a long period of time.
[0027] The alcohol preferably includes at least one selected from methanol, ethanol, n-propanol, and i-propanol. Among them, methanol is preferred because it is easy to remove by distillation. Two or more kinds of the alcohol may be used.
[0028] The amount of the alcohol is preferably 0.1 to 10.0 times by mass relative to the silane compound. If the amount of the alcohol is 0.1 times by mass or more, more preferably 0.5 times by mass or more, even more preferably 1.0 times by mass or more, and even more preferably 1.2 times by mass or more, the silane compound and the water are easily mixed, and gelation of the silicone polymer is suppressed and stabilized. In addition, it is economically preferable if the amount of the alcohol is 10.0 times by mass or less, more preferably 8.0 times by mass or less, and even more preferably 5.0 times by mass or less.
[0029] In the method for producing a silicone polymer of the present invention, the silane compound, the water and the alcohol may be mixed in a mixer.
[0030] A pump is used to supply the raw materials to the mixer. Using a personal computer (PC) to control the pump pressure and flow rate is preferable as it leads to automation and labor saving.
[0031] The materials used for the mixer include stainless steels such as SUS304 and SUS316, carbon steels such as SS41, SC, and SCM, metals such as Hastelloy, titanium, Monel, nickel, Carpenter, and tantalum, resins such as Teflon (registered trademark), PFA, PVC, FRP, and CFRP, ceramics on metals, rubber linings, Teflon (registered trademark) linings, and glass linings. Teflon (registered trademark) and Teflon (registered trademark) linings are preferred because they do not dissolve metals into the mixed liquid.
[0032] As the mixer, driven mixer stirrers such as centrifugal pumps, volute pumps, in-line mixers with stirring blades, static mixers, nozzles, orifices, etc. are used. Among them, static mixers without driving parts or sliding parts, so-called static mixers, are preferred because they are suitable for the manufacture of materials for pharmaceuticals and electronic information materials, which require strict control, without the risk of dust generation or oil contamination. In addition, static mixers have a larger specific surface area than general reaction vessels, making temperature control easier, and are therefore preferred.
[0033] The flow path of the static mixer, which is made of pipes or blocks, is preferably less than 1 mm. By having the flow path be less than 1 mm, if the mixing is accompanied by a reaction, the diffusion distance of the substance is limited, so that the reaction can proceed more quickly.
[0034] The inner diameter of the pipe used in the static mixer is preferably 1 to 20 mm. If the inner diameter is 1 mm or more, the pressure loss is small and the risk of clogging is low. If the inner diameter is 20 mm or less, more preferably 10 mm or less, the specific surface area becomes larger and the reaction proceeds quickly, which is preferable.
[0035] In static mixers and micro mixers, elements consisting of rectangular plates twisted 180 degrees in opposite directions are arranged alternately inside a tube. The number of elements is preferably 12 or more. If the number of elements is 12 or more, more preferably 24 or more, sufficient mixing can be achieved regardless of the feed rate of the raw materials.
[0036] Specific examples of static mixers include Kenics mixer type, Sulzer SMV type, Sulzer SMX type, Toray Hi-mixer type, Komax mixer type, Lightnin mixer type, Ross ISG type, Bran&Lube mixer type, YMC Deneb type, YMC Spica type, YMC Hadar type, IMM CPMM-R300 type, and the like.
[0037] The time for mixing in a mixer depends on the feed rate of the raw materials and the design of the mixer, but is preferably 0.1 to 600 seconds, more preferably 1 to 300 seconds. If the mixing time is 0.1 seconds or more, more preferably 1 second or more, mixing is sufficient, and if it is 600 seconds or less, more preferably 300 seconds or less, the effect on control of the reaction time can be reduced.
[0038] In the method for producing a silicone polymer of the present invention, the mixed solution is continuously fed to a packed column packed with the ion exchange resin. That is, the method for producing a silicone polymer of the present invention uses a flow synthesis method. The flow synthesis method can produce a silicone polymer automatically and continuously for a long period of time, so that it requires less manual operation and reduces manpower compared to conventional batch reactions.
[0039] The solution may be supplied from the top of the packed tower and discharged from the bottom, or may be supplied from the bottom of the packed tower and discharged from the top.
[0040] In the method for producing a silicone polymer of the present invention, the mixed solution is brought into contact with the ion exchange resin. By bringing the mixed solution into contact with the ion exchange resin, hydrolysis and condensation of the silane compound are promoted. In addition, ionic impurities such as metals can be continuously removed. The ion exchange resin can be regenerated and used repeatedly, which is preferable in terms of resources and economy.
[0041] The ion exchange resin may be either a cation exchange resin or an anion exchange resin, because the hydrolysis and polycondensation reactions of the silane compound are promoted by either an acid or a base.
[0042] The cation exchange resin may be a strong acid cation exchange resin or a weak acid cation exchange resin. A commonly used cation exchange resin, for example, a commercially available hydrogen type cation exchange resin, specifically, for example, "Amberlist" (Organo Corporation), 15DRY, 15JWET, 16WET, 35WET, "Lewatit" (manufactured by LANXESS KK), Monoplus SP112, Monoplus SP112H, CNP80WS, CNP LF, K2420, K2431, K2620, K2629, S2328, "Diaion" (manufactured by Mitsubishi Chemical Corporation), SK104H, SK110, SK110L, SK112, SK112L, SK1BH, SK1BL, SK1BLH, SKL10, SKT10L, SKT110, SKT110L, SKT20L, PK208, PK208L, PK208LH, PK212L, PK212LH, PK216, PK216L, PK216H, PK216LH, PK218, PK218L, PK220, PK220L, PK228, PK228L, PK228LH, RCP145H, RCP160M, RCP200, RCP400, RCP610, UBK04, UBK08, UBK08A, UBK08H, UBK08HUP, UBK10, UBK10H, UBK10HUP, UBK12, UBK16, UBKN1U, UBKN1UMB, UBK522M, UBK 530, UBK530J, UBK530K, UBK535, UBK535J, UBK535K, UBK535L, UBK550, UBK555, JC600, JC603, WK10, WK100, WK10S, WK11, WT01S, WK60L, WK60LA, “Monosphere” (manufactured by Dow Chemical Company), strongly acidic cation exchange resin No. 1 (crosslinking degree 2%, 50-100 mesh, H type), strongly acidic cation exchange resin No. 2 (crosslinking degree 2%, 100-200 mesh, H type), strongly acidic cation exchange resin 50W x 2 200-400 mesh (H type), strongly acidic cation exchange resin No. 4 (crosslinking degree 8%, 50-100 mesh, H type), strongly acidic cation exchange resin No. 5 (crosslinking degree 8%, 100-200 mesh, H type), strongly acidic cation exchange resin No. 6 (crosslinking degree 8%, 200-400 mesh, H type), strongly acidic cation exchange resin HCR-S (Na type), strongly acidic cation exchange resin No. 7 (H type), strongly acidic cation exchange resin C-10 (Na type), etc. can be used.
[0043] As the cation exchange resin, a strongly acidic cation exchange resin is preferred, more preferably "Amberlist" 15JWET.
[0044] The anion exchange resin may be either a strong basic anion exchange resin or a weak basic anion exchange resin, and is preferably a strong basic anion exchange resin. “Amberlist” (Organo Corporation), A21, A26, A27, "Lewatit" (manufactured by Lanxess KK), Monoplus MP800, Monoplus MP600, MP62WS, Monoplus MP64, VPOC1065, S4268, S6368, S7468, "Diamond Ion" (manufactured by Mitsubishi Chemical Corporation), NSA100, SA10A, SA10AL, SA10ALLP, SA10AOH, SA10AP, SA10DL, SA11A, SA11AL, SA12A, SA12AL, SAALL, SA20A, SA20ALL, SA20ALLP, SA20AP, SA20AP2, SAF11AL, SANUPB, SAT10L, SAT20L, UMA130J, UBA100, UBA100OH, UBA100OHUP, UBA120, UBA120A, UBA120 OH, UBA120OHUP, UBA150, UBA200, PA306S, PA308, PA308L, PA312, PA312L, PA312LOH, PA312LTU, PA312LTUMB, PA316, PA316L, PA318L, PA3 18LOH, PA408, PA412, PA418, PA418L, PA418LL, PAF308L, HPA25L, HPA25M, HPA512, HPA716, WA10, WA20, WA21J, WA30, WA30C, WA30LL, WA55, “Monosphere” (Dow Chemical), Strongly Basic Ion Exchange Resin No. 2 (2% cross-linking, 100-200 mesh, Cl type), Strongly Basic Anion Exchange Resin 1×2 200-400 mesh (Type I, Cl type), Strongly Basic Anion Exchange Resin 1×4 20-50 mesh (Type I, Cl type), Strongly Basic Anion Exchange Resin No. 3 (4% cross-linking, 50-100 mesh, Cl type), Strongly Basic Anion Exchange Resin No. 4 (4% cross-linking, 100-200 mesh, Cl type), Strongly Basic Anion Exchange Resin 1×4 200-400 mesh (Type I, Cl type), strongly basic anion exchange resin No. 5 (crosslinking degree 8%, 50-100 mesh, Cl type), strongly basic anion exchange resin No. 6 (crosslinking degree 8%, 100-200 mesh, Cl type), strongly basic anion exchange resin No. 7 (crosslinking degree 8%, 200-400 mesh, Cl type), strongly basic anion exchange resin No. 8 (OH type), strongly basic anion exchange resin 22 (Type II, Cl type), strongly basic anion exchange resin MSA-2 (Type II, Cl type), strongly basic anion exchange resin 2A (Type II, Cl type), weakly basic anion exchange resin 66 (free salt form), weakly basic anion exchange resin 77 (free salt form), etc.
[0045] The contact time of the mixed liquid with the ion exchange resin is preferably a space velocity (SV) of 0.05 to 5. If the space velocity (SV) is 0.05 or more, more preferably 0.1 or more, the reaction amount per unit time is large and is economically preferable, whereas if it is 5 or less, more preferably 2 or less, the hydrolysis and condensation polymerization proceed sufficiently and therefore it is preferable.
[0046] In the method for producing a silicone polymer of the present invention, the reaction is carried out under a pressure such that the gauge pressure of a pressure gauge installed on the outlet side of the packed tower indicates a pressure of 0.05 to 5.0 MPa. By setting the gauge pressure at 0.05 MPa or more, more preferably at 0.10 MPa or more, the mixed liquid containing the alcohol with a boiling point of 100° C. or less can be heated to above the boiling point. By increasing the temperature in the system while suppressing the boiling of the alcohol, the ion exchange resin can function as a heterogeneous catalyst. In this way, the reaction rate can be increased to quickly complete the reaction, and a silicone polymer with a high degree of polymerization can be obtained. If the gauge pressure is 5.0 MPa or less, more preferably 3.0 MPa or less, the reaction can be carried out safely without leakage even in a simple device.
[0047] The method for adjusting the pressure is not particularly limited, but the pressure can be adjusted by installing a back pressure valve on the discharge side of the packed tower packed with the ion exchange resin. The back pressure valve is preferably one that can arbitrarily adjust the pressure inside the reactor.
[0048] In the method for producing a silicone polymer of the present invention, the mixed liquid is contacted with an ion exchange resin at 70 to 120°C. If the temperature is 70°C or higher, the ion exchange resin functions as a heterogeneous catalyst, hydrolysis and condensation proceed quickly, and a silicone polymer is obtained in a short time. If the temperature is 120°C or lower, more preferably 100°C or lower, the reaction can be easily controlled, which is preferable. In order to proceed with the reaction at a predetermined temperature, the mixed liquid or its components may be heated in advance, or the packed tower may be heated. To heat the packed tower, a jacket may be installed on the packed tower and heated with hot water or steam.
[0049] The ion exchange resin can be reused repeatedly. After use, it may be washed with a solvent that dissolves the silicone polymer and reused, or it may be regenerated with hydrochloric acid, an aqueous solution of sodium hydroxide, or the like.
[0050] In the silicone polymer manufacturing method of the present invention, the pump operation and the temperature control of the static mixer and packed tower can be controlled by a program using a PC or the like, allowing automatic operation. By utilizing an information transmission network, the operation of the equipment can be remotely controlled, further improving the safety of the work. Furthermore, automatic operation eliminates the variation caused by manual operation, allowing for highly reproducible production.
[0051] The weight average molecular weight of the silicone polymer produced by the production method of the present invention is preferably 300 to 100,000. If the weight average molecular weight of the silicone polymer is 300 or more, more preferably 500 or more, and even more preferably 1,000 or more, it can form a coating film. If the weight average molecular weight of the silicone polymer is 100,000 or less, more preferably 50,000 or less, and even more preferably 20,000 or less, it is soluble in an organic solvent.
[0052] The silicone polymer preferably has a polydispersity (Mw / Mn) calculated by dividing the weight average molecular weight (Mw) by the number average molecular weight (Mn) of 1 to 20, and more preferably 1 to 5. In the present invention, the weight average molecular weight (Mw), number average molecular weight (Mn) and Z average molecular weight (Mz) of the silicone polymer can be measured by gel permeation chromatography (GPC) and calculated in terms of standard polystyrene.
[0053] The silicone polymer may have a cage-type higher-order structure.
[0054] The silicone polymer may be dissolved in a solvent, such as an alcohol solvent or a high boiling point solvent. Examples of alcohol solvents include methanol, ethanol, and isopropanol. As the high boiling point solvent, for example, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether, propylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether, ethyl lactate, etc. can be preferably used.
[0055] The silicone polymer composition can be applied by a general coating method such as spin coating, etc. When the silicone polymer composition is applied to a substrate by, for example, spin coating, it can form a thin film on the substrate, and when heated, the solvent can be removed and the silicone polymer can be hydrolyzed and polycondensed to form a thermoset film.
[0056] Examples of the substrate include glass, silicon wafers, and resins such as polyethylene, polypropylene, and polypropylene terephthalate.
[0057] The thin film formed on the substrate can be heated using a hot plate or an incubator.
[0058] The heating temperature is preferably 80° C. or higher, and more preferably 100° C. or higher.
[0059] The thermoset film thus formed has excellent properties of transparency and heat resistance, and can therefore be used as a protective film for semiconductors or displays, a resist underlayer film, and the like.
[0060] As described above, the silicone polymer obtained by the production method of the present invention can be easily used to obtain a coating film, and is therefore suitable for use in semiconductors, displays, etc. Furthermore, the silicone polymer can be used not only in the field of electronic information materials, but also in a wide range of fields such as paints and adhesives. EXAMPLES
[0061] The present invention will be described in detail below with reference to examples and comparative examples. In the following examples, the following apparatuses were used for analysis, and general reagents purchased from reagent manufacturers were used as raw materials unless otherwise specified. The following methods were used for analysis.
[0062] ·Molecular weight measurement The gel permeation chromatography device used was a Tosoh HLC-8220GPC system, and the columns were Tosoh "TSKgel" SuperHZ3000, "TSKgel" SuperHZ2000, and "TSKgel" SuperHZ1000, all connected in series, for analysis. Detection was performed with a refractometer (RI), and one "TSKgel" SuperH-RC was used as the reference column. Tetrahydrofuran manufactured by Wako Pure Chemical Industries was used as the developing solvent, and the flow rate of the column and reference column was 0.35 mL / min. The measurement temperature was 40°C for both the plunger pump and the column. The sample was prepared by diluting approximately 0.025 g of silicone polymer with 10 mL of tetrahydrofuran, and then injecting 25 μL of the diluted solution. For molecular weight distribution calculations, Tosoh Corporation's "TSKgel" standard polystyrene (A-500, A-1000, A-2500, A-5000, F-1, F-2, F-4, F-10, F-20, F-40, F-80) was used as the standard substance.
[0063] [Example 1] (Flow reactor) The flow reactor used was "KeyChem-Integral" (manufactured by YMC Corporation), which consists of two dual plunger pumps, a micromixer, a controller, and a control PC. Each of the dual plunger pumps was connected to a micromixer. The micromixer was further connected to a 60 ml column. The 60 ml column was packed with 53 ml of pretreated strong acid cation exchange resin ("Amberlist" 15JWET, manufactured by Organo). The 60 ml column was equipped with a hot water jacket and heated to 70°C so that the ion exchange resin could function as a heterogeneous catalyst. The reaction liquid that passed through the 60 ml column was collected in an eggplant flask.
[0064] (Monomer solution) 54.48 g (0.400 mol) of tetramethoxysilane, 60.88 g (0.400 mol) of methyltrimethoxysilane, and 115.36 g of methanol as a solvent were weighed into a 100 ml plastic container and stirred with a magnetic stirrer to prepare a monomer solution.
[0065] (ion-exchanged water) 100.92 g of ion-exchanged water was weighed into a 100 ml plastic container and used as ion-exchanged water.
[0066] (mixed liquid) The plastic container containing the monomer solution was connected to a dual plunger pump A, and the plastic container containing the ion-exchanged water was connected to a dual plunger pump B. The liquid was delivered to a micromixer set at a temperature of 25° C., with pump A delivering speed of 3.07 ml / min and pump B delivering speed of 0.135 ml. The monomer solution and ion-exchanged water were mixed in the micromixer to obtain a mixed liquid.
[0067] (Flow reaction) The above mixture was fed into a 60 ml column packed with ion exchange resin by adjusting the pump so that the space velocity (SV) was 0.5. The back pressure valve installed on the outlet side of the column was adjusted so that the gauge pressure measured by the pressure gauge was within the range of 0.2 to 0.3 MPa. The solution after the reaction was collected in a flask from the outlet side of the column.
[0068] (concentrated) While collecting the solution after the reaction, 177.8 g of propylene glycol monoethyl ether was added to the solution using a plunger pump. The solution was concentrated under reduced pressure to obtain a colorless, transparent silicone polymer solution. The operation up to the concentration under reduced pressure was carried out automatically using a control PC.
[0069] The amount of the obtained silicone polymer solution was 177.5 g, and the weight average molecular weight (Mw) of the silicone polymer was 1,400.
[0070] (First cleaning of ion exchange resin) Next, 87.6 g of methanol was weighed into a plastic container as a cleaning solution, and was supplied from pumps A and B to a 60 ml column packed with ion exchange resin in the same manner to clean the ion exchange resin. When the appearance of the ion exchange resin in the column was visually checked, no deformation or fracture was observed.
[0071] (Second production) Subsequently, the above-mentioned "monomer solution" to "concentration" steps were repeated under the same conditions using the washed ion exchange resin (first recycling), to obtain a colorless and transparent silicone polymer solution.
[0072] The amount of the obtained silicone polymer solution was 176.2 g, and the weight average molecular weight (Mw) of the silicone polymer was 1,360.
[0073] (Second washing of ion exchange resin) Next, the ion exchange resin was washed in the same manner as in “First washing of ion exchange resin.” When the ion exchange resin in the column was visually inspected, no deformation or fracture was observed.
[0074] (3rd production) Subsequently, the above-mentioned "monomer solution" to "concentration" steps were repeated under the same conditions using the washed ion exchange resin (second recycling), to obtain a colorless and transparent silicone polymer solution.
[0075] The amount of the obtained silicone polymer solution was 177.2 g, and the weight average molecular weight (Mw) of the silicone polymer was 1,360.
[0076] (Third washing of ion exchange resin) Next, the ion exchange resin was washed in the same manner as in “First washing of ion exchange resin.” When the ion exchange resin in the column was visually inspected, no deformation or fracture was observed.
[0077] In Example 1, a silicone polymer was obtained automatically and continuously for an extended period of time.
[0078] [Comparative Example 1] (Flow reactor) A flow reactor similar to that used in Example 1 was used.
[0079] (Monomer solution) Propylene glycol monoethyl ether (boiling point 146.4° C.) was used as the solvent instead of methanol.
[0080] (ion-exchanged water) The same ion-exchanged water as used in Example 1 was used.
[0081] (mixture) A mixed solution was prepared in the same manner as in Example 1, except that the above monomer solution was used.
[0082] (Flow reaction) The above mixed solution was used, and the back pressure valve was adjusted so that the gauge pressure measured by the pressure gauge was 0.0 MPa. Other than that, the same procedure as in Example 1 was followed to collect the solution after the reaction.
[0083] (concentrated) To the solution after the above reaction, propylene glycol monoethyl ether was added in the same manner as in Example 1, and the solution was then concentrated under reduced pressure to obtain a colorless and transparent silicone polymer.
[0084] The amount of the obtained silicone polymer solution was 176.2 g, and the weight average molecular weight (Mw) of the silicone polymer was 1,900.
[0085] (First cleaning of ion exchange resin) Next, except that propylene glycol monoethyl ether was used as the washing liquid, the ion exchange resin was washed in the same manner as in Example 1. When the ion exchange resin in the column was visually inspected, no deformation or fracture was found.
[0086] (Second production) Subsequently, the above-mentioned "monomer solution" to "concentration" steps in this comparative example were repeated under the same conditions using the washed ion exchange resin (first recycling), to obtain a colorless and transparent silicone polymer solution.
[0087] The amount of the obtained silicone polymer solution was 178.8 g, and the weight average molecular weight (Mw) of the silicone polymer was 1,780.
[0088] (Second washing of ion exchange resin) Next, the ion exchange resin was washed in the same manner as in "First washing of ion exchange resin" in this comparative example. When the ion exchange resin in the column was visually inspected, some of the resin was partially cracked or changed in shape.
[0089] (3rd production) Subsequently, the above-mentioned "monomer solution" to "concentration" steps in this comparative example were repeated under the same conditions using the washed ion exchange resin (second recycled), to obtain a colorless and transparent silicone polymer solution.
[0090] The amount of the obtained silicone polymer solution was 178.2 g, and the weight average molecular weight (Mw) of the silicone polymer was 1560. The weight average molecular weight (Mw) gradually decreased, suggesting a decrease in the catalytic activity of the ion exchange resin.
[0091] (Third washing of ion exchange resin) Next, the ion exchange resin was washed in the same manner as in "First washing of ion exchange resin" in this comparative example. When the ion exchange resin in the column was visually inspected, some of the resin was partially cracked or changed in shape.
[0092] [Table 1] [Explanation of symbols]
[0093] 1: Monomer tank 2: Ion exchange tank 3: Pump 4: Mixer 5: Packed tower 6: Hot water jacket 7: Pressure gauge 8: Back pressure valve 9: Receiver
Claims
1. A method for producing a silicone polymer, comprising continuously supplying a solution containing at least one silane compound selected from compounds represented by the following general formula (1) and compounds represented by the following general formula (2), water, and an alcohol having a boiling point of 100°C or less to a packed tower packed with an ion exchange resin, and contacting the solution with the ion exchange resin at 70 to 120°C under a pressure indicated by a gauge pressure of 0.05 to 5.0 MPa on a pressure gauge installed on the outlet side of the packed tower. R a Si(OR 1 ) 4-a ....(1) In formula (1), R is a hydrogen atom or a monovalent organic group, R 1 represents a monovalent organic group, and a represents an integer of 1 or 2. Si(OR 2 ) 4 ....(2) In formula (2), R 2 represents a monovalent organic group.
2. The method for producing a silicone polymer according to claim 1, wherein the ion exchange resin is a cation exchange resin.
3. 3. The method for producing a silicone polymer according to claim 1, wherein the alcohol having a boiling point of 100° C. or less includes at least one selected from the group consisting of methanol, ethanol, n-propanol, and i-propanol.
4. The amount of alcohol used, which has a boiling point of 100°C or less, The method for producing a silicone polymer according to claim 1 or 2, wherein the amount of the compound is 1.0 to 10 times by mass relative to the silane compound.
Citation Information
Patent Citations
Production of silanolated organosilane or siloxane
JP1996151445A
Method for producing organosilane having silanol group and low molecular weight organopolysiloxane
JP2011219647A