Resin composition for photomolding, molded product, and method for producing molded product

A photomolding resin composition using high molecular weight polyfunctional (meth)acrylates and reactive diluents achieves a balance of low hardness, high strength, and high elongation at break, addressing the limitations of existing technologies.

JP2024136796AInactive Publication Date: 2024-10-04SUMITOMO CHEM CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023048045
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing resin compositions for photomolding fail to achieve a balance of moderately low hardness, high strength, and high elongation at break, particularly in applications requiring such properties.

Method used

A photomolding resin composition comprising high molecular weight polyfunctional (meth)acrylates and reactive diluents with specific glass transition temperatures, combined in specific proportions, along with a photopolymerization initiator, to form molded articles with desired mechanical properties.

Benefits of technology

The composition enables the production of flexible molded articles with suitably low hardness, high strength, and high elongation at break, suitable for applications requiring these properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136796000001
    Figure 2024136796000001
  • Figure 2024136796000002
    Figure 2024136796000002
  • Figure 2024136796000003
    Figure 2024136796000003
Patent Text Reader

Abstract

To provide a resin composition that enables a molded product with moderately low hardness as well as high strength and high elongation at break to be formed by photofabrication.SOLUTION: A resin composition for photomolding comprises a polymerizable component with a polymerizable unsaturated group. The polymerizable component comprises a high-molecular-weight polyfunctional (meth)acrylate with a molecular weight of 1000 or more and a reactive diluent that is a monofunctional monomer forming a homopolymer with a glass transition temperature of -10°C or higher.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a photomolding resin composition, a molded article, and a method for producing a molded article. [Background technology]

[0002] In the field of photomolding, such as three-dimensional photolithography using a 3D printer, compositions for forming molded articles with high breaking elongation or molded articles with a texture similar to that of an organ have been proposed (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-99750 A [Patent Document 2] Patent Publication No. 2021-146657 Summary of the Invention [Problem to be solved by the invention]

[0004] A member to which a resin molded article is applied may be required to have a moderately low hardness (for example, a hardness of about 10 to 80 measured by a type A durometer). When a molded article having such a moderately low hardness is formed by photomolding, the strength or elongation at break may be insufficient depending on the application of the member.

[0005] The present disclosure relates to a resin composition that can be photomolded to form a molded article having an appropriately low hardness while exhibiting high strength and high elongation at break. [Means for solving the problem]

[0006] The present disclosure includes at least the following: [1] Contains a polymerizable component having a polymerizable unsaturated group, The polymerizable component is A high molecular weight multifunctional (meth)acrylate having a molecular weight of 1000 or more; a reactive diluent which is a monofunctional monomer that forms a homopolymer having a glass transition temperature of -10°C or higher; A photomolding resin composition comprising: [2] The polymerizable component further comprises a monofunctional (meth)acrylate that forms a homopolymer having a glass transition temperature of less than −10° C., or does not comprise the monofunctional (meth)acrylate; a total content of the high molecular weight polyfunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate is 80 mass% or more based on the amount of the polymerizable component, the content of the high molecular weight multifunctional (meth)acrylate is 5% by mass or more and 90% by mass or less based on the total amount of the high molecular weight multifunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate; The content of the reactive diluent is 10% by mass or more and 95% by mass or less based on the total amount of the high molecular weight polyfunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate. The photomolding resin composition according to [1]. [3] The photomolding resin composition according to [1] or [2], further comprising a photopolymerization initiator. [4] The photomolding resin composition according to any one of [1] to [3], which is a composition for three-dimensional photomolding. [5] A molded article comprising a photocured product of a molding material containing the photomolding resin composition according to any one of [1] to [4]. [6] A method for producing a molded article, comprising photocuring a molding material containing the photomolding resin composition according to any one of [1] to [4]. Effect of the Invention

[0007] A resin composition is provided that can be photomolded into a flexible molded article having an appropriately low hardness and exhibiting high strength and high elongation at break. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention is not limited to the following examples.

[0009] An example of the resin composition includes a polymerizable component having a polymerizable unsaturated group. The polymerizable component includes a high molecular weight multifunctional (meth)acrylate and a reactive diluent. The resin composition can be used as a molding material for photomolding.

[0010] The high molecular weight polyfunctional (meth)acrylate is a compound having a plurality of polymerizable unsaturated groups, at least one of acryloyloxy groups and methacryloyloxy groups. The number of polymerizable unsaturated groups in the high molecular weight polyfunctional (meth)acrylate is 2 or more, and may be 30 or less, 20 or less, 10 or less, or 5 or less.

[0011] When the high molecular weight multifunctional (meth)acrylate is a compound that forms a homopolymer having a low glass transition temperature, a molded article having a moderately low hardness is more easily formed. The glass transition temperature of the homopolymer of the high molecular weight multifunctional (meth)acrylate may be -100°C or more and 40°C or less. The glass transition temperature of the homopolymer of the high molecular weight multifunctional (meth)acrylate may be 40°C or less, 30°C or less, 20°C or less, 10°C or less, 0°C or less, -10°C or less, -20°C or less, -25°C or less, -30°C or less, or -35°C or less.

[0012] In this specification, the glass transition temperature of a homopolymer means the glass transition temperature of a homopolymer formed by homopolymerization of a monomer that is a polymerizable component. The glass transition temperature can be a midpoint glass transition temperature obtained by analyzing a melting curve measured by differential scanning calorimetry using a method in accordance with JIS K7121-1987. Literature values ​​of homopolymers of various monomers (for example, "POLYMER HANDBOOK" (Wiley-Interscience)) can also be referenced.

[0013] The high molecular weight polyfunctional (meth)acrylate may be, for example, a urethane (meth)acrylate, in particular a difunctional urethane (meth)acrylate.

[0014] The urethane (meth)acrylate is an oligomer or polymer having at least one of an acryloyloxy group or a methacryloyloxy group and a urethane group. The urethane (meth)acrylate may be, for example, a polyester-based urethane (meth)acrylate having a soft segment derived from a polyester polyol, a polyether-based urethane (meth)acrylate having a soft segment derived from a polyether polyol, or a combination thereof.

[0015] The high molecular weight multifunctional (meth)acrylate has a molecular weight of 1000 or more. The molecular weight of the high molecular weight multifunctional (meth)acrylate may be 1000 or more and 100000 or less. The molecular weight of the high molecular weight multifunctional (meth)acrylate may be 2000 or more, 3000 or more, 4000 or more, 5000 or more, 6000 or more, 7000 or more, 8000 or more, 9000 or more, or 10000 or more, and may be 90000 or less, 80000 or less, 70000 or less, 60000 or less, or 50000 or less.

[0016] The number average molecular weight (Mn) of the high molecular weight multifunctional (meth)acrylate may be 5000 or more and 100000 or less. The number average molecular weight (Mn) of the high molecular weight multifunctional (meth)acrylate may be 6000 or more, 7000 or more, 8000 or more, 9000 or more, or 10000 or more, and may be 100000 or less, 90000 or less, 80000 or less, 70000 or less, 60000 or less, or 50000 or less. Here, Mn can be a standard polystyrene equivalent value measured by gel permeation chromatography. Usually, it is considered that the majority of the high molecular weight multifunctional (meth)acrylate with a molecular weight distribution having Mn of 5000 or more is occupied by a component having a molecular weight of 1000 or more.

[0017] The reactive diluent is one or more monofunctional monomers that form homopolymers with a relatively high glass transition temperature. The combination of a high molecular weight polyfunctional (meth)acrylate and a monofunctional monomer that forms a homopolymer with a low glass transition temperature can contribute to the formation of a flexible molded product that has a moderately low hardness and exhibits high strength and high breaking elongation. The glass transition temperature of the homopolymer of the monofunctional monomer used as the reactive diluent may be -10°C or higher, or may be -10°C or higher and 200°C or lower. The glass transition temperature of the homopolymer of the monofunctional monomer used as the reactive diluent may be -5°C or higher, 0°C or higher, 5°C or higher, 10°C or higher, 15°C or higher, or 20°C or higher, or may be 190°C or lower, 180°C or lower, 170°C or lower, 160°C or lower, or 150°C or lower.

[0018] The monofunctional monomer used as the reactive diluent may be a compound having an acryloyl group or a methacryloyl group and a cyclic group. The total number of carbon atoms and heteroatoms constituting the cyclic group may be, for example, 4 to 8. The cyclic group may be an alicyclic group, a cyclic ether group, or an aromatic group, and may be an alicyclic group or a cyclic ether group. The cyclic group may have a substituent such as an alkyl group. For example, the monofunctional monomer may be at least one of a (meth)acrylamide derivative represented by the following formula (1) or a cyclic (meth)acrylate compound represented by the following formula (2). [ka]

[0019] In formula (1), R 1 represents a hydrogen atom or a methyl group, and X 1 represents a cyclic group containing a nitrogen atom bonded to a (meth)acryloyl group. 1 represents a hydrogen atom or a methyl group, R 2 represents an optionally substituted methylene group or a direct bond; X 2represents a cyclic group which may have a substituent (for example, an alkyl group). The reactive diluent may contain one or more monofunctional monomers represented by formula (1) or (2).

[0020] An example of the acrylamide derivative represented by formula (1) is acryloylmorpholine represented by the following formula (Tg of homopolymer: 145° C.). [ka]

[0021] Examples of the cyclic (meth)acrylate compound represented by formula (2) include isobornyl acrylate (homopolymer Tg: 97°C), cyclic trimethylolpropane formal acrylate (homopolymer Tg: 10°C), and 2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl acrylate (homopolymer Tg: -7°C) represented by the following formula.

[0022] [ka]

[0023] The polymerizable component may further contain other compounds as necessary. For example, the polymerizable component may contain one or more monofunctional (meth)acrylates different from the reactive diluent. The glass transition temperature of the homopolymer of the monofunctional (meth)acrylate may be less than -10°C, or may be -100°C or more and less than -10°C. The glass transition temperature of the homopolymer of the monofunctional (meth)acrylate may be -15°C or less, -20°C or less, -25°C or less, -30°C or less, -35°C or less, or -40°C or less.

[0024] The monofunctional (meth)acrylate that forms a homopolymer at less than −10° C. may be, for example, at least one of an alkyl (meth)acrylate represented by formula (A) or an alkoxy (meth)acrylate represented by formula (B). [ka] [ka]

[0025] In formula (A), R 1 represents a hydrogen atom or a methyl group, R 2 R represents an alkyl group. 2 may be a linear or branched alkyl group. 1 represents a hydrogen atom or a methyl group, R 3 represents an alkanediyl group, and R 4 represents an alkyl group, and n represents an integer of 1 or more. 3 may be the same or different. 3 R may be an ethylene group or a propylene group. 4 may be a methyl group or an ethyl group. n is the number of repetitions of the oxyalkylene group and may be an integer of 1 to 20.

[0026] Examples of alkyl (meth)acrylates represented by formula (A) include ethyl acrylate (homopolymer Tg: -20°C), n-butyl acrylate (homopolymer Tg: -55°C), isobutyl acrylate (homopolymer Tg: -26°C), n-hexyl acrylate (homopolymer Tg: -65°C), n-octyl acrylate (homopolymer Tg: -70°C), 2-ethylhexyl acrylate (homopolymer Tg: -85°C), n-nonyl acrylate (homopolymer Tg: -37°C), isononyl acrylate (homopolymer Tg: -58°C), n-dodecyl acrylate (homopolymer Tg: -23°C), and isostearyl acrylate (homopolymer Tg: -18°C).

[0027] Examples of the alkoxy(meth)acrylate represented by formula (B) include methoxyethyl acrylate (Tg of homopolymer: -50°C) and methoxypolyethylene glycol acrylate. The Tg of the homopolymer of methoxypolyethylene glycol acrylate is -67°C when the repeat number n of oxyethylene groups is 2, -60°C when it is 3, -50°C when it is 9, and -40°C when it is 13.

[0028] The resin composition may further include a photopolymerization initiator. The photopolymerization initiator may be selected from those usually used for photocuring (UV curing) of a resin composition based on the required reactivity, etc. The content of the photopolymerization initiator may be, for example, 0.1% by mass or more and 5% by mass or less based on the amount of the polymerizable component.

[0029] The resin composition may further include other components. For example, the resin composition may include a filler. The filler is a fine particle dispersed in the resin composition, and may be an inorganic filler, an organic filler, or a combination thereof. The filler may include, for example, silica particles or a pigment, and may include one or more inorganic fillers selected from silica particles, hydrotalcite particles, aluminum silicate particles, calcium oxide particles, and calcium carbonate particles.

[0030] The total content of the polymerizable components in the resin composition may be 80% by mass or more, 85% by mass or more, 90% by mass or more, or 95% by mass or more based on the total amount of the resin composition. The total content of the high molecular weight polyfunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate that forms a homopolymer at less than -10°C may be 80% by mass or more, 85% by mass or more, 90% by mass or more, or 95% by mass or more based on the amount of the polymerizable components, or may be substantially 100% by mass.

[0031] The content of the high molecular weight multifunctional (meth)acrylate may be 5% by mass or more and 90% by mass or less based on the total amount of the high molecular weight multifunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate forming a homopolymer at less than -10°C. The content of the high molecular weight multifunctional (meth)acrylate may be 10% by mass or more, 15% by mass or more, 20% by mass or more, 25% by mass or more, or 30% by mass or more based on the total amount of the high molecular weight multifunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate forming a homopolymer at less than -10°C, and may be 85% by mass or less, 80% by mass or less, 75% by mass or less, or 70% by mass or less.

[0032] When the content of the reactive diluent is large, the strength and breaking elongation of the molded article tend to be improved. The content of the reactive diluent may be 10% by mass or more and 95% by mass or less based on the total amount of the high molecular weight multifunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate that forms a homopolymer at less than -10°C. The content of the reactive diluent based on the total amount of the high molecular weight multifunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate that forms a homopolymer at less than -10°C may be 11% by mass or more, 12% by mass or more, 13% by mass or more, 14% by mass or more, 15% by mass or more, 16% by mass or more, 17% by mass or more, 18% by mass or more, 19% by mass or more, 20% by mass or more, 21% by mass or more, 22% by mass or more, 23% by mass or more, 24% by mass or more, 25% by mass or more, or 30% by mass or more, or may be 90% by mass or less, 85% by mass or less, 80% by mass or less, 75% by mass or less, 70% by mass or less, 45% by mass or less, 40% by mass or less, or 30% by mass or less.

[0033] The content of the monofunctional (meth)acrylate forming a homopolymer below -10°C may be 0% by mass or more and 85% by mass or less based on the total amount of the high molecular weight multifunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate forming a homopolymer below -10°C. The content of the monofunctional (meth)acrylate forming a homopolymer below 10°C may be 5% by mass or more, 10% by mass or more, 15% by mass or more, 20% by mass or more, 25% by mass or more, 30% by mass or more, 35% by mass or more, 40% by mass or more, or 45% by mass or more based on the total amount of the high molecular weight multifunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate forming a homopolymer below -10°C, and may be 80% by mass or less, 75% by mass or less, 70% by mass or less, 65% by mass or less, 60% by mass or less, 55% by mass or less, or 50% by mass or less.

[0034] The viscosity of the resin composition or molding material at 25°C may be 10 mPa·s or more and 9000 mPa·s or less. When the viscosity of the resin composition is within this range, a molded product with little deformation such as depressions and warping is easily formed by three-dimensional stereolithography. From the same viewpoint, the viscosity of the resin composition or molding material at 25°C may be 50 mPa·s or more, or 100 mPa·s or more, or 8000 mPa·s or less, 7000 mPa·s or less, 6000 mPa·s or less, 5000 mPa·s or less, 4000 mPa·s or less, 3000 mPa·s or less, or 2000 mPa·s or less. The viscosity at 25°C may be a value measured at 25°C at a rotation speed of 4 to 200 rpm using a Brookfield type viscometer (B type viscometer).

[0035] The resin compositions exemplified above can be used to manufacture various molded products by photomolding. For photomolding, the resin composition may be used as a molding material as it is. Alternatively, a molding material prepared by mixing other components (e.g., a photopolymerization initiator) with the resin composition as necessary may be used.

[0036] Photomolding is a molding method including a photocuring step. For example, photomolding may be a molding method including photocuring a molding material in a mold, or may be three-dimensional photomolding including repeated photocuring of a film of the molding material. The method of three-dimensional photomolding is not particularly limited, and the molding material can be applied for three-dimensional photomolding by, for example, a pull-up method or a pull-down method. Photomolding can produce a molded product that is a photocured product of the molding material. The form of the molded product formed can be appropriately selected based on the desired application, etc., and is not particularly limited.

[0037] The molded article formed by photomolding of the resin composition according to the present disclosure can be used as a member that requires high strength and high breaking elongation together with moderately low hardness. The hardness of the photocured product (molded article) of the resin composition by a type A durometer may be 10 or more or 20 or more, and may be 80 or less. The tensile strength of the photocured product (molded article) of the resin composition may be 1.0 MPa or more or 1.3 MPa or more, and may be 15.0 MPa or less. The breaking elongation of the photocured product (molded article) of the resin composition may be 100% or more or 150% or more, and may be 1500% or less or 500% or less.

[0038] Examples of components to which molded articles are applied include skins for robots such as androids, organ models for surgical training, pads, grippers, grommets, bellows, packings, and gaskets.

[0039] [Example] The present invention is not limited to the following examples. 1.Material The following materials were prepared: (A) Monofunctional (meth)acrylate A1: 2-Ethylhexyl acrylate (molecular weight: 184, homopolymer Tg: -85°C) A2: Methoxyethylene glycol acrylate (molecular weight: 130, homopolymer Tg: -50°C, number of ethylene glycol repeats: 1) A3: Methoxypolyethylene glycol acrylate (molecular weight: 483, homopolymer Tg: -50°C, number of ethylene glycol repeats: 9) (B) High molecular weight multifunctional (meth)acrylate B1: Urethane acrylate (Mn: approx. 15,000, homopolymer Tg: 43°C, bifunctional) B2: Urethane acrylate (Mn: approx. 35,000, homopolymer Tg: -43°C, bifunctional) B3: Polybutadiene diacrylate (Mn: approx. 10,000, bifunctional) B4: Modified polyisoprene with methacryloyloxy groups (Mn: approx. 35,000, 3 or more functional groups) B5: Urethane acrylate (Mn: 5000, homopolymer Tg: 35°C, bifunctional) (C) Reactive diluent C1: Acryloylmorpholine (molecular weight: 145, homopolymer Tg: 145°C) C2: Isobornyl acrylate (molecular weight: 208, homopolymer Tg: 97°C) C3: Cyclic trimethylolpropane formal acrylate (molecular weight: 200, homopolymer Tg: 10°C) (D) Photopolymerization initiator D1: Omnirad 1173 (trade name): 2-hydroxy-2-methyl-1-phenyl-1-propanone (IGM Resins BV)

[0040] 2.Resin composition (molding material) The materials were mixed in the mass ratios shown in Table 1, and the mixture was stirred using a planetary centrifugal mixer. The mixture after stirring was degassed to obtain a homogeneous liquid resin composition. This resin composition was used as a molding material for photomolding.

[0041] 3.Light molding The molding material was cast on a Teflon petri dish to form a resin film with a thickness of 2 mm. The resin film was irradiated with ultraviolet light using a conveyor-type UV irradiation device (I-Grandage ECS-4011GX, manufactured by I-Graphics Co., Ltd.) to form a sheet-shaped molded product that was a photocured product of the molding material (resin composition). The conditions for ultraviolet light irradiation were as follows. For comparison, a sheet-shaped molded product was produced in the same manner using a commercially available photopolymerization composition (Elastic 50A resin, product name, Formlabs). Lamp: High pressure mercury lamp Lamp output: 4kW Lamp height: 130mm Conveyor speed: 84m / min Accumulated light output: 5J / cm 2 (UVICURE PLUS II UV meter, UV-A measurement value, FusionUV Systems Japan KK) Dumbbell-shaped No. 3 test pieces for evaluating physical properties were cut out from the sheet-like molded product.

[0042] 4. Evaluation of molded products JIS-A hardness The hardness (Duro-A) of the test specimen (molded product) was measured in an atmosphere at a temperature of 23° C. using an automatic hardness tester equipped with a durometer type A (RH-105A, manufactured by Excel Corporation).

[0043] Tensile Test A tensile test was performed on the test pieces using a tensile tester (Ueshima Seisakusho Co., Ltd., QUICK READER P-57) at a temperature of 23°C and a tensile speed of 500 mm / min. From the measurement results, the breaking strength (TB) and breaking elongation (EB) of the molded product were obtained.

[0044] [Table 1]

[0045] [Table 2]

[0046] From the evaluation results shown in Tables 1 and 2, it was confirmed that the photomolding compositions of the Examples exhibited appropriately low hardness, high strength, and high elongation at break.

Claims

1. Contains a polymerizable component having a polymerizable unsaturated group, The polymerizable component is A high molecular weight multifunctional (meth)acrylate having a molecular weight of 1000 or more; a reactive diluent which is a monofunctional monomer that forms a homopolymer having a glass transition temperature of −10° C. or higher; A photomolding resin composition comprising:

2. The polymerizable component further comprises a monofunctional (meth)acrylate that forms a homopolymer having a glass transition temperature of less than −10° C., or does not comprise the monofunctional (meth)acrylate; a total content of the high molecular weight polyfunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate is 80 mass% or more based on the amount of the polymerizable component, the content of the high molecular weight multifunctional (meth)acrylate is 5% by mass or more and 90% by mass or less based on the total amount of the high molecular weight multifunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate, The content of the reactive diluent is 10% by mass or more and 95% by mass or less based on the total amount of the high molecular weight polyfunctional (meth)acrylate, the reactive diluent, and the monofunctional (meth)acrylate. The photomolding resin composition according to claim 1 .

3. The photomolding resin composition according to claim 1 or 2, further comprising a photopolymerization initiator.

4. The photomolding resin composition according to claim 1 or 2, which is a composition for three-dimensional photomolding.

5. A molded article comprising a photocured product of a molding material comprising the photomolding resin composition according to claim 1 or 2.

6. A method for producing a molded article, comprising photocuring a molding material containing the photomolding resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Resin composition for optical molding

    JP2019099750A

  • Composition for three-dimensional forming, high molecular weight body, three-dimensional formed article, and manufacturing method of three-dimensional formed article