Resin composition for three-dimensional photofabrication, molded product, and method for producing molded product
A resin composition combining monofunctional and high molecular weight polyfunctional (meth)acrylates with a photopolymerization initiator addresses the challenge of achieving low hardness and high elongation at break in three-dimensional stereolithography, enhancing precision and reducing deformation in molded articles.
Patent Information
- Application Number
- JP2023048047
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing resin compositions for three-dimensional stereolithography fail to achieve both low hardness and high elongation at break with sufficient precision, particularly for applications requiring softness like Type A durometer hardness of 30 or less.
A resin composition comprising monofunctional (meth)acrylate and high molecular weight polyfunctional (meth)acrylate with specific viscosity and glass transition temperature ranges, along with a photopolymerization initiator, is used to form molded articles with low hardness and high elongation at break.
The resin composition enables the formation of molded articles with precise low hardness and high elongation at break, suitable for applications requiring softness, such as android skins and surgical organ models, with improved shape accuracy and reduced deformation.
Smart Images

Figure 2024136797000001 
Figure 2024136797000002 
Figure 2024136797000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a resin composition for three-dimensional stereolithography, a molded article, and a method for producing a molded article. [Background technology]
[0002] In the field of photomolding, such as three-dimensional photolithography using a 3D printer, compositions have been proposed that can form molded articles with high breaking elongation or molded articles with a texture similar to that of an organ (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-99750 A [Patent Document 2] Patent Publication No. 2021-146657 Summary of the Invention [Problem to be solved by the invention]
[0004] For components to which resin molded products are applied, softness (for example, a hardness of about 30 or less using a type A durometer) is sometimes required. However, when molded products with such low hardness are formed by stereolithography, the precision of the molded product's shape is often insufficient. In addition, there is also the problem of insufficient breaking elongation depending on the application of the component.
[0005] The present disclosure relates to a resin composition that can be used to form a molded article having a sufficiently low hardness and high elongation at break with good precision by stereolithography. [Means for solving the problem]
[0006] The present disclosure includes at least the following: [1] A resin composition comprising a polymerizable component having a polymerizable unsaturated group, The polymerizable component is A monofunctional (meth)acrylate, A high molecular weight multifunctional (meth)acrylate having a molecular weight of 1000 or more; Including, the content of the monofunctional (meth)acrylate is 80 mass% or less based on the total amount of the monofunctional (meth)acrylate and the high molecular weight polyfunctional (meth)acrylate, The viscosity of the resin composition at 25°C is 10 mPa·s or more and 9000 mPa·s or less. Resin composition for three-dimensional stereolithography. [2] The resin composition for three-dimensional optical molding according to [1], wherein the content of the monofunctional (meth)acrylate is 35% by mass or more and 80% by mass or less based on the total amount of the monofunctional (meth)acrylate and the high molecular weight polyfunctional (meth)acrylate. [3] The monofunctional (meth)acrylate is represented by the following formula (A): [ka] or an alkyl (meth)acrylate represented by the following formula (B): [ka] At least one of the alkoxy (meth)acrylates represented by R 1 represents a hydrogen atom or a methyl group, R 2 represents an alkyl group, and R 3 represents an alkanediyl group, and R 4 represents an alkyl group, n represents an integer of 1 or more, and multiple R 3 may be the same or different, The resin composition for three-dimensional optical molding according to [1] or [2]. [4] The resin composition for three-dimensional stereolithography according to any one of [1] to [3], further comprising a photopolymerization initiator. [5] A molded article comprising a photocured product of a molding material containing the resin composition for three-dimensional stereolithography according to any one of [1] to [4]. [6] A method for producing a molded product, comprising photocuring a molding material containing the resin composition for three-dimensional stereolithography according to any one of [1] to [4]. Effect of the Invention
[0007] The present invention provides a resin composition that can be used to form a molded article having a sufficiently low hardness and high elongation at break with good precision by stereolithography. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The present invention is not limited to the following examples.
[0009] An example of the resin composition includes a polymerizable component having a polymerizable unsaturated group. The polymerizable component includes a monofunctional (meth)acrylate and a high molecular weight polyfunctional (meth)acrylate having a molecular weight of 1000 or more. The resin composition can be used as a molding material for three-dimensional optical modeling.
[0010] The monofunctional (meth)acrylate is a monomer having one acryloyloxy group or methacryloyloxy group. The glass transition temperature of the homopolymer of this monofunctional (meth)acrylate may be less than 10°C, or may be -100°C or more and less than 10°C. The glass transition temperature of the homopolymer of the monofunctional (meth)acrylate may be 5°C or less, 0°C or less, -5°C or less, -10°C or less, -15°C or less, -20°C or less, -25°C or less, -30°C or less, -35°C or less, or -40°C or less. The polymerizable component may contain both a monofunctional (meth)acrylate that forms a homopolymer having a glass transition temperature of less than 10°C and a monofunctional (meth)acrylate that forms a homopolymer exhibiting a glass transition temperature of 10°C or more.
[0011] In this specification, the glass transition temperature of a homopolymer means the glass transition temperature of a homopolymer formed by homopolymerization of a monomer that is a polymerizable component. The glass transition temperature can be a midpoint glass transition temperature obtained by analyzing a melting curve measured by differential scanning calorimetry using a method in accordance with JIS K7121-1987. Literature values of homopolymers of various monomers (for example, "POLYMER HANDBOOK" (Wiley-Interscience)) can also be referenced.
[0012] The monofunctional (meth)acrylate may be, for example, at least one of an alkyl (meth)acrylate represented by formula (A) or an alkoxy (meth)acrylate represented by formula (B). [ka] [ka]
[0013] In formula (A), R 1 represents a hydrogen atom or a methyl group, R 2 R represents an alkyl group. 2 may be a linear or branched alkyl group. 1 represents a hydrogen atom or a methyl group, R 3 represents an alkanediyl group, and R 4 represents an alkyl group, and n represents an integer of 1 or more. 3 may be the same or different. 3 R may be an ethylene group or a propylene group. 4 may be a methyl group or an ethyl group. n is the number of repetitions of the oxyalkylene group and may be an integer of 1 to 20.
[0014] Examples of alkyl (meth)acrylates represented by formula (A) include ethyl acrylate (homopolymer Tg: -20°C), n-butyl acrylate (homopolymer Tg: -55°C), isobutyl acrylate (homopolymer Tg: -26°C), n-hexyl acrylate (homopolymer Tg: -65°C), n-octyl acrylate (homopolymer Tg: -70°C), 2-ethylhexyl acrylate (homopolymer Tg: -85°C), n-nonyl acrylate (homopolymer Tg: -37°C), isononyl acrylate (homopolymer Tg: -58°C), n-dodecyl acrylate (homopolymer Tg: -23°C), and isostearyl acrylate (homopolymer Tg: -18°C).
[0015] Examples of the alkoxy(meth)acrylate represented by formula (B) include methoxyethyl glycol acrylate (Tg of homopolymer: -50°C) and methoxypolyethylene glycol acrylate. The Tg of the homopolymer of methoxypolyethylene glycol acrylate is -67°C when the repeat number n of oxyethylene groups is 2, -60°C when it is 3, -50°C when it is 9, and -40°C when it is 13.
[0016] The high molecular weight polyfunctional (meth)acrylate is a compound having a plurality of polymerizable unsaturated groups, at least one of acryloyloxy groups and methacryloyloxy groups. The number of polymerizable unsaturated groups in the high molecular weight polyfunctional (meth)acrylate is 2 or more, and may be 30 or less, 20 or less, 10 or less, or 5 or less.
[0017] When the high molecular weight multifunctional (meth)acrylate is a compound that forms a homopolymer having a low glass transition temperature, a molded article having a moderately low hardness is more easily formed. The glass transition temperature of the homopolymer of the high molecular weight multifunctional (meth)acrylate may be -100°C or more and 40°C or less. The glass transition temperature of the homopolymer of the high molecular weight multifunctional (meth)acrylate may be 40°C or less, 30°C or less, 20°C or less, 10°C or less, 0°C or less, -10°C or less, -20°C or less, -25°C or less, -30°C or less, or -35°C or less.
[0018] The high molecular weight polyfunctional (meth)acrylate may be, for example, a urethane (meth)acrylate, in particular a difunctional urethane (meth)acrylate.
[0019] The urethane (meth)acrylate is an oligomer or polymer having at least one of an acryloyloxy group or a methacryloyloxy group and a urethane group. The urethane (meth)acrylate may be, for example, a polyester-based urethane (meth)acrylate having a soft segment derived from a polyester polyol, a polyether-based urethane (meth)acrylate having a soft segment derived from a polyether polyol, or a combination thereof.
[0020] The high molecular weight multifunctional (meth)acrylate has a molecular weight of 1000 or more. The molecular weight of the high molecular weight multifunctional (meth)acrylate may be 1000 or more and 100000 or less. The molecular weight of the high molecular weight multifunctional (meth)acrylate may be 2000 or more, 3000 or more, 4000 or more, 5000 or more, 6000 or more, 7000 or more, 8000 or more, 9000 or more, or 10000 or more, and may be 90000 or less, 80000 or less, 70000 or less, 60000 or less, or 50000 or less.
[0021] The number average molecular weight (Mn) of the high molecular weight multifunctional (meth)acrylate may be 5000 or more and 100000 or less. The number average molecular weight (Mn) of the high molecular weight multifunctional (meth)acrylate may be 6000 or more, 7000 or more, 8000 or more, 9000 or more, or 10000 or more, and may be 100000 or less, 90000 or less, 80000 or less, 70000 or less, 60000 or less, or 50000 or less. Here, Mn can be a standard polystyrene equivalent value measured by gel permeation chromatography. Usually, it is considered that the majority of the high molecular weight multifunctional (meth)acrylate with a molecular weight distribution having Mn of 5000 or more is occupied by a component having a molecular weight of 1000 or more.
[0022] The polymerizable component may further contain other compounds as necessary. For example, the polymerizable component may contain one or more monofunctional monomers (such as acryloylmorpholine) other than the monofunctional (meth)acrylate.
[0023] The resin composition may further include a photopolymerization initiator. The photopolymerization initiator may be selected from those usually used for photocuring (UV curing) of a resin composition based on the required reactivity, etc. The content of the photopolymerization initiator may be, for example, 0.1% by mass or more and 5% by mass or less based on the amount of the polymerizable component.
[0024] The resin composition may further include other components. For example, the resin composition may include a filler. The filler is a fine particle dispersed in the resin composition, and may be an inorganic filler, an organic filler, or a combination thereof. The filler may include, for example, silica particles or a pigment, and may include one or more inorganic fillers selected from silica particles, hydrotalcite particles, aluminum silicate particles, calcium oxide particles, and calcium carbonate particles.
[0025] The total content of the polymerizable components in the resin composition may be 80% by mass or more, 85% by mass or more, 90% by mass or more, or 95% by mass or more based on the total amount of the resin composition. The total content of the monofunctional (meth)acrylate and the high molecular weight multifunctional (meth)acrylate may be 80% by mass or more, 85% by mass or more, 90% by mass or more, or 95% by mass or more based on the amount of the polymerizable components, or may be substantially 100% by mass. The total content of the monofunctional (meth)acrylate and the high molecular weight multifunctional (meth)acrylate represented by formula (A) or (B) may be 80% by mass or more, 85% by mass or more, 90% by mass or more, or 95% by mass or more based on the amount of the polymerizable components, or may be substantially 100% by mass.
[0026] The content of the monofunctional (meth)acrylate may be 80% by mass or less, or 35% by mass or more and 80% by mass or less, based on the total amount of the monofunctional (meth)acrylate and the high molecular weight multifunctional (meth)acrylate. The content of the monofunctional (meth)acrylate may be 40% by mass or more, 45% by mass or more, or 50% by mass or more, and 75% by mass or less or 70% by mass or less, based on the total amount of the monofunctional (meth)acrylate and the high molecular weight multifunctional (meth)acrylate. The content of the monofunctional (meth)acrylate represented by formula (A) or (B) may be 80% by mass or less, or 35% by mass or more and 80% by mass or less, or 40% by mass or more, 45% by mass or more, or 50% by mass or more, and 75% by mass or less or 70% by mass or less, based on the total amount of the monofunctional (meth)acrylate and the high molecular weight multifunctional (meth)acrylate.
[0027] The content of the high molecular weight multifunctional (meth)acrylate may be 20% by mass or more, or 20% by mass or more and 65% by mass or less, based on the total amount of the monofunctional (meth)acrylate and the high molecular weight multifunctional (meth)acrylate. The content of the high molecular weight multifunctional (meth)acrylate may be 60% by mass or less, 55% by mass or less, or 50% by mass or less, or 25% by mass or more, or 30% by mass or more, based on the total amount of the monofunctional (meth)acrylate and the high molecular weight multifunctional (meth)acrylate.
[0028] The viscosity of the resin composition or molding material at 25°C may be 10 mPa·s or more and 9000 mPa·s or less. When the viscosity of the resin composition is within this range, a molded product with little deformation such as depressions and warping is easily formed by three-dimensional stereolithography. From the same viewpoint, the viscosity of the resin composition or molding material at 25°C may be 50 mPa·s or more, or 100 mPa·s or more, or 8000 mPa·s or less, 7000 mPa·s or less, 6000 mPa·s or less, 5000 mPa·s or less, 4000 mPa·s or less, or 3000 mPa·s or less. The viscosity at 25°C may be a value measured at 25°C at a rotation speed of 4 to 200 rpm using a Brookfield type viscometer (B type viscometer).
[0029] The resin compositions exemplified above can be used to manufacture various molded products by three-dimensional stereolithography. For stereolithography, the resin composition may be used as a molding material as it is. Alternatively, a molding material prepared by mixing other components (e.g., a photopolymerization initiator) with the resin composition as necessary may be used.
[0030] Three-dimensional photo-molding includes, for example, repeatedly photo-curing a film of a molding material. The method of three-dimensional photo-molding is not particularly limited, and the molding material can be applied for three-dimensional photo-molding by, for example, a pull-up method or a pull-down method. By three-dimensional photo-molding, a molded product that is a photo-cured product of the molding material can be obtained. The shape of the molded product to be formed can be appropriately selected based on the desired application, etc., and is not particularly limited.
[0031] The molded article (molded article) formed by stereolithography of the resin composition according to the present disclosure can be used as a member that requires a molded article exhibiting sufficiently low hardness and high elongation at break. The hardness of the photocured product (molded article) of the resin composition by a type A durometer may be 0 or more and 40 or less, or 20 or less. The elongation at break of the photocured product (molded article) of the resin composition may be 50% or more, 75% or more, or 500% or less. The tensile strength of the photocured product (molded article) of the resin composition may be 0.01 MPa or more and 5.0 MPa or less.
[0032] Examples of components to which molded articles are applied include skins for robots such as androids, organ models for surgical training, pads, grippers, grommets, bellows, packings, and gaskets.
[0033] [Example] The present invention is not limited to the following examples.
[0034] 1.Material The following materials were prepared: (A) Monofunctional (meth)acrylate A1: 2-Ethylhexyl acrylate (molecular weight: 184, homopolymer Tg: -85°C) A2: Methoxyethylene glycol acrylate (molecular weight: 130, homopolymer Tg: -50°C, number of repeating oxyethylene groups: 1) A3: Methoxypolyethylene glycol acrylate (molecular weight: 218, homopolymer Tg: -60°C, number of repeating oxyethylene groups: 3) A4: Methoxypolyethylene glycol acrylate (molecular weight: 483, homopolymer Tg: -50°C, number of repeating oxyethylene groups: 9) A5: Methoxypolyethylene glycol acrylate (molecular weight: 659, homopolymer Tg: -40°C, number of repeating oxyethylene groups: 13) (B) High molecular weight multifunctional (meth)acrylate B1: Urethane acrylate (Mn: approx. 35,000, homopolymer Tg: -43°C, bifunctional) B2: Urethane acrylate (Mn: 5000, Tg of homopolymer: 35°C, bifunctional) (C) Photopolymerization initiator C1: Omnirad TPO H (trade name): 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (IGM Resins BV)
[0035] 2.Resin composition (molding material) The materials were mixed in the mass ratios shown in Table 1 or Table 2, and the mixture was stirred using a planetary centrifugal mixer. The mixture after stirring was degassed to obtain a uniform liquid resin composition. For the resin composition containing a filler, the content of each monomer relative to the total amount of the monofunctional (meth)acrylate and the high molecular weight polyfunctional (meth)acrylate is shown in parentheses. The obtained resin composition was used as a molding material for photomolding or photolithography. The viscosity of each resin composition was measured at 25°C and a rotation speed of 4 to 200 rpm using a B-type viscometer (LVDV2T, manufactured by AMETEK BROOKFIELD).
[0036] 3.Light molding (1) Sheet-shaped molded products A DLP (registered trademark) type 3D printer (ML-100, manufactured by Muto Industries, Ltd.) was used to form a dumbbell-shaped molded product (thickness 1.7 mm) conforming to ASTM D638 by photo-curing 0.1 mm-thick films of the molding material (resin composition) in sequence. For comparison, a molded product was produced in the same manner using a commercially available photo-curing composition (Elastic 50A resin, product name, Formlabs). The exposure time for photo-curing each film was set to the time shown in Table 1 or Table 2.
[0037] JIS-A hardness The hardness (Duro-A) of the test specimen (molded product) was measured in an atmosphere at a temperature of 23° C. using an automatic hardness tester equipped with a durometer type A (RH-105A, manufactured by Excel Corporation).
[0038] Tensile Test A tensile test was performed on the test pieces using a tensile tester (Ueshima Seisakusho Co., Ltd., QUICK READER P-57) at a temperature of 23°C and a tensile speed of 500 mm / min. From the measurement results, the breaking strength (TB) and breaking elongation (EB) of the molded product were obtained.
[0039] (2) Three-dimensional stereolithography A DLP (registered trademark) type 3D printer (ML-100, manufactured by Muto Industries, Ltd.) was used to form a dumbbell-shaped molded product (thickness 1.7 mm) conforming to ASTM D638 by photo-curing 0.1 mm-thick films of the molding material (resin composition) in sequence. For comparison, a molded product was produced in the same manner using a commercially available photo-curing composition (Elastic 50A resin, product name, Formlabs). The exposure time for photo-curing each film was set to the time shown in Table 1 or Table 2.
[0040] The appearance of the molded product was visually evaluated according to the following criteria. No uneven thickness: No uneven thickness was observed. Uneven thickness: Areas with uneven thickness (such as a depression in the center of the molded product) are visually confirmed. The molded product was placed on a flat metal plate, and the presence or absence of warping was evaluated by visually checking whether or not there was a gap between the molded product and the metal plate.
[0041] [Table 1] [Table 2]
[0042] From the evaluation results shown in Tables 1 and 2, it was confirmed that the photomolding compositions of the examples could be used to form molded articles having sufficiently low hardness and high breaking elongation with good precision by stereolithography.
Claims
1. A resin composition comprising a polymerizable component having a polymerizable unsaturated group, The polymerizable component is A monofunctional (meth)acrylate, A high molecular weight multifunctional (meth)acrylate having a molecular weight of 1000 or more; Including, the content of the monofunctional (meth)acrylate is 80 mass% or less based on the total amount of the monofunctional (meth)acrylate and the high molecular weight polyfunctional (meth)acrylate, The viscosity of the resin composition at 25°C is 10 mPa·s or more and 9000 mPa·s or less. Resin composition for three-dimensional stereolithography.
2. 2. The resin composition for three-dimensional optical molding according to claim 1, wherein the content of the monofunctional (meth)acrylate is 35% by mass or more and 80% by mass or less based on the total amount of the monofunctional (meth)acrylate and the high molecular weight polyfunctional (meth)acrylate.
3. The monofunctional (meth)acrylate is represented by the following formula (A): 【Chemistry 1】 or an alkyl (meth)acrylate represented by the following formula (B): 【Chemistry 2】 At least one of alkoxy (meth)acrylates represented by the formula: R 1 represents a hydrogen atom or a methyl group; R 2 represents an alkyl group; R 3 represents an alkanediyl group, R 4 represents an alkyl group, n represents an integer of 1 or more, and a plurality of R 3 may be the same or different, The resin composition for three-dimensional stereolithography according to claim 1 or 2.
4. The resin composition for three-dimensional stereolithography according to claim 1 or 2, further comprising a photopolymerization initiator.
5. A molded article comprising a photocured product of a molding material comprising the resin composition for three-dimensional stereolithography according to claim 1 or 2.
6. A method for producing a molded product, comprising photocuring a molding material containing the resin composition for three-dimensional stereolithography according to claim 1 or 2.
Citation Information
Patent Citations
Resin composition for optical molding
JP2019099750A
Composition for three-dimensional forming, high molecular weight body, three-dimensional formed article, and manufacturing method of three-dimensional formed article
JP2021146657A