Temporary junction method and manufacturing method of joined body

The method addresses dent defects in friction stir welding by controlling rotary tool insertion depth, ensuring airtightness and watertightness in bonded structures.

JP2024136857AInactive Publication Date: 2024-10-04MITSUBISHI ELECTRIC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023048145
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing temporary bonding methods using friction stir welding result in dent defects due to rotary tool punch holes, compromising the airtightness and watertightness of hollow containers.

Method used

A method involving friction stir welding where the rotary tool is inserted and moved from one end to the other end of the temporary joint, with decreasing insertion depth, and then pulled out at the end position, preventing the formation of holes in the temporary bonding portion.

Benefits of technology

Prevents the formation of dent defects and ensures airtightness and watertightness by avoiding rotary tool holes, enhancing the integrity of the bonded structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136857000001_ABST
    Figure 2024136857000001_ABST
Patent Text Reader

Abstract

To provide a temporary junction method capable of suppressing leaving of a pull-out hole of a rotary tool in a temporary junction part.SOLUTION: A temporary junction method includes a step of joining a first member and a second member in a temporary junction part by frictional stirring junction using a rotary tool. The rotary tool is moved from one end of the temporary junction part to the other end of the temporary junction part while being inserted in the temporary junction part, and then moved to a temporary junction ending position from the other end toward the one end. While the rotary tool is being moved to the temporary junction ending position from the other end toward the one end, an insertion depth of the rotary tool becomes smaller as it is closer to the temporary junction ending position. The rotary tool is pulled out at the temporary junction ending position.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a temporary bonding method and a method for manufacturing a bonded body. [Background technology]

[0002] For example, JP 2018-65164 A (Patent Document 1) describes a temporary joining method in which a hollow vessel body and a sealing body are temporarily spot joined at a temporary joining portion by friction stir welding using a rotary tool. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-65164 A Summary of the Invention [Problem to be solved by the invention]

[0004] After the temporary joining method described in Patent Document 1 is performed, the hollow container body and the sealing body are joined by friction stir welding using a rotary tool at the final joining portion where the hollow container body and the sealing body are arranged to pass through the temporary joining portion. According to the temporary joining method described in Patent Document 1, a punch hole of the rotary tool remains at the temporary joining portion, and therefore, a dent defect caused by the punch hole is likely to occur at the final joining portion, which may cause a loss of airtightness and watertightness of the hollow container.

[0005] The present disclosure has been made in consideration of the problems of the conventional techniques as described above. More specifically, the present disclosure provides a temporary joining method capable of suppressing a punch hole of a rotary tool from remaining in a temporary joint portion. [Means for solving the problem]

[0006] The temporary joining method of the present disclosure includes a step of joining a first member and a second member by friction stir welding using a rotating tool at a temporary joining portion. The rotating tool is inserted into the temporary joining portion and moved from one end to the other end of the temporary joining portion, and then moved from the other end toward the one end to a temporary joining end position. As the rotating tool moves from the other end toward the one end to the temporary joining end position, the insertion depth of the rotating tool decreases as it approaches the temporary joining end position. The rotating tool is withdrawn at the temporary joining end position. Effect of the Invention

[0007] According to the temporary joining method of the present disclosure, it is possible to prevent a punch hole from the rotary tool from remaining in the temporary joined portion. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a perspective view of a joint body 100. [Diagram 2] FIG. 2 is an exploded perspective view of the joined body 100. [Diagram 3] 1 is a manufacturing process diagram of the bonded body 100. FIG. [Figure 4] FIG. 11 is a plan view illustrating the temporary bonding step S1. [Diagram 5] FIG. 5 is an enlarged view of V in FIG. [Figure 6] FIG. 6 is a cross-sectional view taken along line VI-VI in FIG. [Figure 7] 1 is an enlarged plan view of the vicinity of a temporary bonded portion 40 after completion of a temporary bonding step S1. [Figure 8] FIG. 11 is a plan view illustrating the main bonding step S2. [Figure 9] FIG. 13 is an enlarged plan view illustrating a first modified example of the temporary joining step S1. [Figure 10] FIG. 11 is an enlarged plan view illustrating a second modified example of the temporary joining step S1. [Figure 11] FIG. 11 is an enlarged plan view illustrating a third modified example of the temporary joining step S1. [Figure 12] FIG. 11 is an enlarged plan view illustrating a fourth modified example of the temporary joining step S1. [Figure 13] FIG. 11 is a plan view illustrating a modified example of the main bonding step S2. [Figure 14] FIG. 2 is a perspective view of a joined body 100A. [Figure 15] FIG. 2 is an exploded perspective view of the joined body 100A. [Figure 16] 10 is an enlarged plan view illustrating a temporary bonding step S1 in the manufacturing method of the bonded body 100A. FIG. [Figure 17] FIG. 17 is a cross-sectional view taken along line XVII-XVII in FIG. [Figure 18] FIG. 2 is a perspective view of a joint body 200. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The details of the embodiments of the present disclosure will be described with reference to the drawings. In the following drawings, the same or corresponding parts are designated by the same reference numerals, and redundant description will not be repeated.

[0010] Embodiment 1 A description will be given of a bonded body according to embodiment 1. The bonded body according to embodiment 1 is designated as a bonded body 100.

[0011] (Configuration of the joint assembly 100) The structure of the bonded body 100 will be described below.

[0012] Fig. 1 is a perspective view of a bonded body 100. Fig. 2 is an exploded perspective view of the bonded body 100. As shown in Figs. 1 and 2, the bonded body 100 has a first member 10 and a second member 20. The first member 10 is a box-shaped member 11. The second member 20 has a sealing body 21. The bonded body 100 is a hollow container.

[0013] The constituent material of the first member 10 (box-shaped member 11) is a metallic material capable of friction stirring. Specific examples of the constituent material of the first member 10 (box-shaped member 11) include aluminum, aluminum alloy, copper, copper alloy, titanium, titanium alloy, magnesium, magnesium alloy, etc. The constituent material of the second member 20 (sealing body 21) is a metallic material capable of friction stirring. Specific examples of the constituent material of the second member 20 (sealing body 21) include aluminum, aluminum alloy, copper, copper alloy, titanium, titanium alloy, magnesium, magnesium alloy, etc. The constituent material of the second member 20 (sealing body 21) may be the same as or different from the constituent material of the first member 10 (box-shaped member 11).

[0014] The box-shaped member 11 has a side wall portion 11a and a bottom wall portion 11b. The side wall portion 11a has a rectangular ring shape in a plan view. The bottom wall portion 11b is continuous with the lower end of the side wall portion 11a. As a result, the lower end side of the side wall portion 11a is closed. The box-shaped member 11 has an opening portion 11c. The opening portion 11c is defined by the upper end of the side wall portion 11a. As the side wall portion 11a has a rectangular ring shape in a plan view as described above, the opening portion 11c is rectangular.

[0015] The sealing body 21 is a flat plate-shaped member. The sealing body 21 is disposed on the upper end of the side wall portion 11a so as to close the opening 11c. The sealing body 21 has, for example, a rectangular shape in a plan view.

[0016] The first member 10 (box-shaped member 11) and the second member 20 (sealing body 21) are joined at a permanent joint 30. The permanent joint 30 is located at a position where the box-shaped member 11 (the upper end of the side wall portion 11a) and the sealing body 21 overlap. The permanent joint 30 is, for example, annular in plan view. More specifically, the permanent joint 30 is a rectangular annular shape that follows the opening edge of the opening 11c. By joining the box-shaped member 11 and the sealing body 21, a closed space defined by the side wall portion 11a, the bottom wall portion 11b, and the sealing body 21 is formed inside the joined body 100.

[0017] (Method of Manufacturing Bonded Body 100) A method for producing the bonded body 100 will now be described.

[0018] Fig. 3 is a manufacturing process diagram of the bonded body 100. As shown in Fig. 3, the manufacturing method of the bonded body 100 includes a temporary bonding step S1 and a main bonding step S2.

[0019] Fig. 4 is a plan view illustrating the temporary joining step S1. Fig. 5 is an enlarged view of V in Fig. 4. Fig. 6 is a cross-sectional view of VI-VI in Fig. 5. As shown in Figs. 4 to 6, in the temporary joining step S1, a first member 10 (box-shaped member 11) and a second member 20 (sealing body 21) are temporarily joined at a temporary joining portion 40 by friction stir welding using a rotary tool 50.

[0020] The temporary joint 40, or the permanent joint 30, is located at a position where the box-shaped member 11 (the upper end of the side wall portion 11a) and the sealing body 21 overlap. The number of temporary joints 40 is, for example, multiple. The multiple temporary joints 40 are arranged at intervals in a rectangular ring shape along the opening edge of the opening 11c in a plan view. The temporary joints 40 have one end 40a and the other end 40b. The other end 40b is the end opposite to the one end 40a.

[0021] In the temporary joining step S1, first, the sealing body 21 is placed on the upper end of the side wall portion 11a. Second, the rotating rotation tool 50 is inserted into one end 40a. At this time, the rotation tool 50 is inserted so that its tip (tip 50a) reaches the boundary surface between the side wall portion 11a and the sealing body 21. In other words, the rotation tool 50 is inserted so as to penetrate the sealing body 21. Third, the rotation tool 50 is moved from one end 40a to the other end 40b. As the rotation tool 50 moves, the constituent material of the box-shaped member 11 and the constituent material of the sealing body 21 at the temporary joining portion 40 plastically flows, and the upper end of the side wall portion 11a and the sealing body 21 are friction stir joined.

[0022] Fourth, the rotating tool 50 is moved from the other end 40b toward the one end 40a to the temporary joining end position 40c. At this time, the insertion depth of the rotating tool 50 becomes smaller as it approaches the temporary joining end position 40c, and the rotating tool 50 is withdrawn at the temporary joining end position 40c. FIG. 7 is an enlarged plan view of the temporary joining portion 40 and its vicinity after the temporary joining step S1 is completed. As shown in FIG. 7, a groove 40d is formed on the surface of the temporary joining portion 40 after the temporary joining step S1 is completed. The groove 40d extends between the other end 40b and the temporary joining end position 40c in a plan view. The width of the groove 40d becomes smaller as it approaches the temporary joining end position 40c.

[0023] The trajectory of the rotary tool 50 from one end 40a to the other end 40b in a plan view is defined as trajectory L1, and the trajectory of the rotary tool 50 from the other end 40b to the temporary joining end position 40c in a plan view is defined as trajectory L2. The trajectory L2 overlaps with the trajectory L1, for example. The moving distance of the rotary tool 50 from one end 40a to the other end 40b in a plan view is defined as moving distance DIS1, the moving distance of the rotary tool 50 from the other end 40b to the temporary joining end position 40c is defined as moving distance DIS2, and the tool diameter of the rotary tool 50 is defined as tool diameter D. The moving distance DIS2 is preferably smaller than the moving distance DIS1 and larger than the tool diameter D.

[0024] The rotary tool 50 is, for example, a shoulderless tool that does not have a shoulder. The length of the tip 50a is greater than the thickness of the sealing body 21. The surface of the tip 50a is inclined with respect to the central axis of the rotary tool 50 so that the outer diameter becomes smaller as it approaches the tip. The inclination angle of the surface of the tip 50a is, for example, 20° or more and 40° or less. Although not shown, a spiral groove is machined on the surface of the tip 50a. It is preferable that the spiral groove is machined in the opposite direction to the rotation direction of the rotary tool 50. For example, when the rotary tool 50 is rotated counterclockwise, the spiral groove is formed clockwise toward the tip.

[0025] The main joining process S2 is performed after the temporary joining process S1. Fig. 8 is a plan view illustrating the main joining process S2. As shown in Fig. 8, the first member 10 (box-shaped member 11) and the second member 20 (sealing body 21) are friction stir welded at the main joining portion 30 using a rotary tool 50. The main joining portion 30 passes through the temporary joining portion 40 in a plan view.

[0026] In the main welding process S2, first, the rotating tool 50 is inserted into the main welding start position 30a. At this time, the rotating tool 50 is inserted so that the tip 50a reaches the boundary surface between the side wall portion 11a and the sealing body 21. That is, the rotating tool 50 is inserted so as to penetrate the sealing body 21. Third, the rotating tool 50 is moved from the main welding start position 30a to circle the main welding portion 30 and return to the main welding start position 30a again. As a result, the constituent material of the box-shaped member 11 and the constituent material of the sealing body 21 in the main welding portion 30 plastically flows, and the upper end of the side wall portion 11a and the sealing body 21 are friction stir welded.

[0027] The rotation tool 50 is moved from the main welding start position 30a to the main welding end position 30b. The main welding end position 30b is in the main welding part 30. At this time, the insertion depth of the rotation tool 50 decreases as it approaches the main welding end position 30b, and the rotation tool 50 is pulled out at the main welding end position 30b. In this manner, the structure of the joined body 100 shown in FIG. 1 is formed.

[0028] (Modification of temporary joining step S1) Fig. 9 is an enlarged plan view illustrating a first modified example of the temporary joining step S1. As shown in Fig. 9, the temporary joint 40 does not have to be linear in plan view. For example, the temporary joint 40 near the corner of the edge of the opening 11c may be curved along the corner of the edge of the opening 11c. In this case, the locus L1 and the locus L2 are also curved in the same manner.

[0029] FIG. 10 is an enlarged plan view illustrating a modified example 2 of the temporary joining step S1. FIG. 11 is an enlarged plan view illustrating a modified example 3 of the temporary joining step S1. As shown in FIG. 10 and FIG. 11, the trajectory L2 may not overlap with the trajectory L1. More specifically, the trajectory L2 may be non-parallel to the trajectory L1 as shown in FIG. 10. That is, the rotation tool 50 may be moved obliquely from the other end 40b toward the one end 40a to the temporary joining end position 40c. Also, as shown in FIG. 11, the trajectory L2 may be parallel to the trajectory L1, but may be shifted from the trajectory L1 in a direction perpendicular to the extension direction of the temporary joint 40. That is, the rotation tool 50 may be turned back in a curved shape in a plan view after reaching the other end 40b, and then moved linearly again.

[0030] Fig. 12 is an enlarged plan view illustrating a fourth modified example of the temporary joining step S1. As shown in Fig. 12, the temporary joint 40 may extend in a spiral shape in a plan view. In this case, the one end 40a and the other end 40b are, for example, at the outermost and innermost peripheries, respectively, of the spiral-shaped temporary joint 40 in a plan view.

[0031] (Modification of Main Joining Step S2) Fig. 13 is a plan view illustrating a modified example of the main welding step S2. As shown in Fig. 13, in the main welding step S2, the main welding end position 30b may be outside the main welding part 30 in a plan view. In this case as well, the insertion depth of the rotation tool 50 decreases as it approaches the main welding end position 30b, and the rotation tool 50 is pulled out at the main welding end position 30b.

[0032] (Effects of the manufacturing method of the bonded body 100) The effects of the method for producing the bonded body 100 will be described below.

[0033] In the manufacturing method of the joined body 100, a temporary joining step S1 is performed. In the temporary joining step S1, the insertion depth of the rotating tool 50 gradually decreases while the rotating tool 50 is moved from the other end 40b toward the one end 40a to the temporary joining end position 40c, and then the rotating tool 50 is pulled out at the temporary joining end position 40c. Therefore, in the manufacturing method of the joined body 100, after the temporary joining step S1 is performed, a punch hole of the rotating tool 50 is unlikely to remain. As a result, after the main joining step S2 is performed, a dent defect caused by the punch hole of the rotating tool 50 remaining in the temporary joining step S1 is unlikely to be formed, and it is possible to ensure the airtightness and watertightness of the joined body 100 (hollow container).

[0034] In the temporary joining step S1, the rotary tool 50 is folded back and moved toward the one end 40a after reaching the other end 40b, so that the temporary joint 40 can be shortened. In addition, since the rotary tool 50 is folded back and moved in this manner, the first member 10 (box-shaped member 11) and the second member 20 (sealing body 21) can be firmly temporarily joined over the entire length of the temporary joint 40. If the rotary tool 50 is moved without changing direction after reaching the other end 40b, and the insertion depth is gradually reduced before the rotary tool 50 is pulled out, a groove 40d is formed in the unjoined region (outside the temporary joint 40), which may cause defects when the main joining step S2 is performed.

[0035] By making the travel distance DIS2 larger than the tool diameter D, the depth of the groove 40d can be reduced. By making the travel distance DIS2 smaller than the travel distance DIS1, the rotary tool 50 can be pulled out from the firmly joined temporary joint 40. If a spiral groove is machined on the surface of the tip 50a, it is possible to reduce the load on the joining device that drives the rotary tool 50 when inserting the rotary tool 50. In this case, it is possible to keep the metallic material that flows during friction stir welding in the temporary joint 40 (main joint 30).

[0036] Embodiment 2 A bonded body according to embodiment 2 will be described. The bonded body according to embodiment 2 is designated as bonded body 100A. Here, differences from bonded body 100 will be mainly described, and overlapping descriptions will not be repeated.

[0037] (Configuration of Joint 100A) The structure of the bonded body 100A will be described below.

[0038] Fig. 14 is a perspective view of the joined body 100A. Fig. 15 is an exploded perspective view of the joined body 100A. As shown in Figs. 14 and 15, the joined body 100A has a first member 10 (box-shaped member 11) and a second member 20 (sealing body 21). In the joined body 100A, the first member 10 (box-shaped member 11) and the second member 20 (sealing body 21) are joined at a main joint 30 by friction stir welding using a rotary tool 50. In these respects, the configuration of the joined body 100A is common to the configuration of the joined body 100.

[0039] In the bonded body 100A, a recess 11d is formed at the upper end of the side wall 11a. The recess 11d has a step bottom surface 11da and a step side surface 11db. The step bottom surface 11da is adjacent to the opening 11c in a plan view. The lower end of the step side surface 11db is continuous with the end of the step bottom surface 11da on the opposite side to the opening 11c. The upper end of the step side surface 11db is continuous with the upper end of the side wall 11a around the recess 11d.

[0040] In the joined body 100A, the sealing body 21 is disposed on the step bottom surface 11da so as to close the opening 11c. When the sealing body 21 is disposed on the step bottom surface 11da, the side surface of the sealing body 21 preferably contacts the step side surface 11db. In the joined body 100A, the main bonding portion 30 overlaps the upper end of the side wall portion 11a around the recess 11d and the outer periphery of the sealing body 21 in a plan view. In these respects, the configuration of the joined body 100A is different from that of the joined body 100.

[0041] (Method of Manufacturing Bonded Body 100A) A method for producing the bonded body 100A will be described below.

[0042] The manufacturing method of the bonded body 100A includes a temporary bonding step S1 and a main bonding step S2. In this respect, the manufacturing method of the bonded body 100A is common to the manufacturing method of the bonded body 100. The manufacturing method of the bonded body 100A differs from the manufacturing method of the bonded body 100 in the details of the temporary bonding step S1.

[0043] Fig. 16 is an enlarged plan view illustrating a temporary bonding step S1 in the manufacturing method of the bonded body 100A. Fig. 17 is a cross-sectional view taken along line XVII-XVII in Fig. 16. As shown in Figs. 16 and 17, in the manufacturing method of the bonded body 100A, the temporary bond 40 overlaps the upper end of the side wall 11a around the recess 11d and the outer periphery of the sealing body 21 in a plan view. In other respects, the temporary bonding step S1 in the manufacturing method of the bonded body 100A is similar to the temporary bonding step S1 in the manufacturing method of the bonded body 100.

[0044] (Effects of the manufacturing method of the bonded body 100A) The effects of the manufacturing method of the bonded body 100A will be described below.

[0045] In the manufacturing method of the bonded body 100A, the temporary bonding step S1 is performed as in the manufacturing method of the bonded body 100. Therefore, in the manufacturing method of the bonded body 100A, after the temporary bonding step S1 is performed, the punching hole of the rotation tool 50 is unlikely to remain, and after the main bonding step S2 is performed, a dent defect caused by the punching hole of the rotation tool 50 remaining in the temporary bonding step S1 is unlikely to be formed.

[0046] Embodiment 3 A bonded body according to embodiment 3 will be described. The bonded body according to embodiment 3 is designated as bonded body 200. Here, differences from bonded body 100 will be mainly described, and overlapping descriptions will not be repeated.

[0047] (Configuration of the joint body 200) The structure of the bonded body 200 will be described below.

[0048] Fig. 18 is a perspective view of a joined body 200. As shown in Fig. 18, the joined body 200 has a first member 10 and a second member 20. In the joined body 100A, the first member 10 and the second member 20 are joined at a main weld 30 by friction stir welding using a rotary tool 50, and the main weld 30 is located at a position where the first member 10 and the second member 20 overlap. In these respects, the configuration of the joined body 200 is common to the configuration of the joined body 100.

[0049] In the joined body 200, the first member 10 is not a box-shaped member 11, and the second member 20 is not a sealing body 21. The joined body 200 is not a hollow container. In the joined body 200, the main joint 30 is linear rather than annular in plan view. In these respects, the configuration of the joined body 200 is different from that of the joined body 100.

[0050] (Method of Manufacturing Bonded Body 200) A method for producing the bonded body 200 will now be described.

[0051] The manufacturing method of the bonded body 200 includes a temporary bonding step S1 and a main bonding step S2. In this respect, the manufacturing method of the bonded body 200 is common to the manufacturing method of the bonded body 100. The manufacturing method of the bonded body 200 differs from the manufacturing method of the bonded body 100 in terms of the details of the temporary bonding step S1.

[0052] In the temporary bonding step S1 in the manufacturing method of the bonded body 200, the multiple temporary bonded portions 40 are arranged linearly at intervals in a plan view, not in a ring shape (see FIG. 18). In other respects, the temporary bonding step S1 in the manufacturing method of the bonded body 200 is similar to the temporary bonding step S1 in the manufacturing method of the bonded body 100.

[0053] (Effects of the manufacturing method of the bonded body 200) The effects of the manufacturing method of the bonded body 200 will be described below.

[0054] In the manufacturing method of the bonded body 200, the temporary bonding step S1 is performed as in the manufacturing method of the bonded body 100. Therefore, in the manufacturing method of the bonded body 200, after the temporary bonding step S1 is performed, a punch hole of the rotation tool 50 is unlikely to remain, and after the main bonding step S2 is performed, a dent defect caused by the punch hole of the rotation tool 50 remaining in the temporary bonding step S1 is unlikely to be formed.

[0055] [Note] Aspects of the present disclosure are summarized in the appendix.

[0056] <Appendix 1> The method includes a step of joining a first member and a second member at a temporary joint by friction stir welding using a rotary tool, The rotating tool is inserted into the temporary joint and moved from one end of the temporary joint to the other end of the temporary joint, and then moved from the other end toward the one end to a temporary joining end position; When the rotation tool moves from the other end toward the one end to the temporary joining end position, an insertion depth of the rotation tool becomes smaller as the rotation tool approaches the temporary joining end position, The temporary joining method, wherein the rotating tool is withdrawn at the temporary joining completion position.

[0057] <Appendix 2> 2. The temporary joining method according to claim 1, wherein a movement distance of the rotating tool from the other end to the temporary joining end position is smaller than a movement distance of the rotating tool from the one end to the other end and is larger than a tool diameter of the rotating tool.

[0058] <Appendix 3> A step of temporarily joining a first member and a second member at a temporary joining portion by friction stir welding using a rotary tool; and joining the first member and the second member by friction stir welding using the rotary tool at a main joint that passes through the temporary joint, The rotating tool is inserted into the temporary joint and moved from one end of the temporary joint to the other end of the temporary joint, and then moved from the other end toward the one end to a temporary joining end position; When the rotation tool moves from the other end toward the one end to the temporary joining end position, an insertion depth of the rotation tool becomes smaller as the rotation tool approaches the temporary joining end position, The method for manufacturing a joint body, wherein the rotating tool is withdrawn at the temporary joining completion position.

[0059] <Appendix 4> a movement distance of the rotating tool from the other end to the temporary joining end position is smaller than a movement distance of the rotating tool from the one end to the other end and is larger than a tool diameter of the rotating tool.

[0060] <Appendix 5> the first member is a box-shaped container having an opening, the second member is a sealing body disposed on the box-shaped container so as to close the opening, The method for producing a bonded body according to claim 3 or 4, wherein the temporary bonded portion is located at an overlapping portion of the box-shaped container and the sealing body.

[0061] <Appendix 6> The main joint is annular along an edge of the opening, the rotating tool is inserted into the main welding portion, moved from a welding start position to the main welding portion while circling the main welding portion to the welding start position, and then moved to a welding end position; When moving from the welding start position to the welding end position, an insertion depth of the rotation tool becomes smaller as the rotation tool approaches the welding end position, The method for manufacturing a joined body described in Appendix 5, wherein the rotating tool is withdrawn at the joining completion position.

[0062] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of this application is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]

[0063] 100, 100A, 200 joint body, 10 first member, 11 box-shaped member, 11a side wall portion, 11b bottom wall portion, 11c opening, 11d recessed portion, 11da step bottom surface, 11db step side surface, 20 second member, 21 sealing body, 30 actual joint portion, 30a actual joint start position, 30b actual joint end position, 40 temporary joint portion, 40a one end, 40b the other end, 40c temporary joint end position, 40d groove, 50 rotating tool, 50a tip portion, D tool diameter, DIS1, DIS2 travel distance, L1, L2 trajectory, S1 temporary joint process, S2 actual joint process.

Claims

1. The method includes a step of joining a first member and a second member at a temporary joint by friction stir welding using a rotary tool, The rotating tool is inserted into the temporary joint and moved from one end of the temporary joint to the other end of the temporary joint, and then moved from the other end toward the one end to a temporary joining end position; When the rotation tool moves from the other end toward the one end to the temporary joining end position, an insertion depth of the rotation tool becomes smaller as the rotation tool approaches the temporary joining end position, The temporary joining method, wherein the rotating tool is withdrawn at the temporary joining completion position.

2. The temporary joining method according to claim 1 , wherein a moving distance of the rotating tool from the other end to the temporary joining end position is smaller than a moving distance of the rotating tool from the one end to the other end and is larger than a tool diameter of the rotating tool.

3. A step of temporarily joining a first member and a second member at a temporary joining portion by friction stir welding using a rotary tool; and joining the first member and the second member by friction stir welding using the rotary tool at a main joint that passes through the temporary joint, The rotating tool is inserted into the temporary joint and moved from one end of the temporary joint to the other end of the temporary joint, and then moved from the other end toward the one end to a temporary joining end position; When the rotation tool moves from the other end toward the one end to the temporary joining end position, an insertion depth of the rotation tool becomes smaller as the rotation tool approaches the temporary joining end position, The method for manufacturing a joint body, wherein the rotating tool is withdrawn at the temporary joining completion position.

4. 4. The method for manufacturing a joined body according to claim 3, wherein a movement distance of the rotating tool from the other end to the temporary joining end position is smaller than a movement distance of the rotating tool from the one end to the other end and is larger than a tool diameter of the rotating tool.

5. the first member is a box-shaped container having an opening, the second member is a sealing body disposed on the box-shaped container so as to close the opening, The method for manufacturing a bonded body according to claim 3 , wherein the temporary bonded portion is located at a portion where the box-shaped container and the sealing body overlap each other.

6. The main joint is annular along an edge of the opening, the rotating tool is inserted into the main welding portion, moved from a welding start position to the main welding position while circling the main welding portion, and then moved to a welding end position; When moving from the welding start position to the welding end position, an insertion depth of the rotation tool becomes smaller as the rotation tool approaches the welding end position, The method for manufacturing a joint body according to claim 5 , wherein the rotation tool is withdrawn at the joining completion position.