Microporous film and method for producing microporous film

By employing ethylene polymer particles with specific properties and a tailored production process, the challenges of moldability and stretchability in microporous membranes are addressed, resulting in a defect-free and high-performance membrane.

JP2024136962APending Publication Date: 2024-10-04MITSUI CHEMICALS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023048281
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Ultra-high molecular weight ethylene polymers exhibit poor moldability and stretchability, leading to defects such as holes and tears during the production of microporous membranes, resulting in insufficient productivity and performance.

Method used

The use of ethylene polymer particles with specific surface area between 2.00 to 30.0 m²/g, intrinsic viscosity of 5 to 50 dl/g, and bulk density of 0.01 to 0.20 g/mL, combined with a production method involving kneading, molding, stretching, and solvent removal, to create a microporous membrane with improved formability and stretchability.

Benefits of technology

The resulting microporous membrane exhibits excellent stretchability and formability, minimizing defects like holes and tears, thereby enhancing productivity and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136962000001
    Figure 2024136962000001
  • Figure 2024136962000002
    Figure 2024136962000002
  • Figure 2024136962000003
    Figure 2024136962000003
Patent Text Reader

Abstract

To provide a microporous film excellent in stretchability and moldability.SOLUTION: A microporous film obtained from ethylene-based polymer particles (A), in which the ethylene-based polymer particles (A) satisfy the following requirements (i) and (ii): (i) the specific surface area determined by a BET method from an adsorption / desorption isotherm measured by a nitrogen gas adsorption method is more than 2.00 m2 / g and 30.0 m2 / g or less; and (ii) the intrinsic viscosity [η] measured in a decalin solvent at 135°C is 5 to 50 dl / g.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a microporous membrane and a method for making a microporous membrane. [Background technology]

[0002] Ethylene polymers having extremely high molecular weights, so-called ultra-high molecular weight ethylene polymers, are superior in impact resistance, abrasion resistance, chemical resistance, and strength to general-purpose ethylene polymers, and have excellent characteristics as engineering plastics. For this reason, attempts have been made to apply them to uses such as lining materials, line parts in the food industry, machine parts, artificial joints, sporting goods, and microporous membranes by various molding methods.

[0003] In particular, microporous membranes are widely used in battery separators used in lithium secondary batteries, nickel-hydrogen batteries, nickel-cadmium batteries, polymer batteries, etc., as well as separators for electrolytic capacitors, various filters such as reverse osmosis filtration membranes, ultrafiltration membranes, and microfiltration membranes, moisture-permeable waterproof clothing, medical materials, etc.

[0004] On the other hand, ultra-high molecular weight ethylene polymers have poor fluidity when melted due to their high molecular weight, and it is said that it is difficult to perform melt molding, which is a molding method for general resins. For this reason, methods for molding ultra-high molecular weight ethylene polymers have been developed, such as a method of dissolving the ultra-high molecular weight ethylene polymer in a solvent and molding it, and a solid-phase stretch molding method of compressing ultra-high molecular weight ethylene polymer particles at a temperature below the melting point and then stretching them. For example, Patent Document 1 describes a method for producing ultra-high molecular weight ethylene polymer particles having excellent stretch moldability, and Patent Document 2 describes a polyethylene powder having excellent flowability. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 5689473 [Patent Document 2] JP 2019-038931 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, although Patent Documents 1 and 2 disclose ultra-high molecular weight ethylene polymers, as described above, these ultra-high molecular weight ethylene polymers have problems with molding processability. For this reason, when a membrane, particularly a microporous membrane, is produced, it is presumed that the membrane has poor moldability and stretchability, and even if stretching is possible, only a membrane with a low stretch ratio is produced, or the obtained membrane has molding defects (e.g., holes or tears), and thus the productivity and performance are insufficient.

[0007] The present invention has been made in view of the above, and an object of the present invention is to provide a microporous membrane that has excellent stretchability and formability, and a method for producing the microporous membrane. [Means for solving the problem]

[0008] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that the above problems can be solved by using ethylene-based polymer particles having a specific specific surface area and intrinsic viscosity, and have completed the present invention. The configuration examples of the present invention are as follows.

[0009] [1] A microporous membrane obtained from ethylene-based polymer particles (A), wherein the ethylene-based polymer particles (A) satisfy the following requirements (i) and (ii): (i) The specific surface area calculated by the BET method from the adsorption / desorption isotherm measured by the nitrogen gas adsorption method is 2.00 m 2 / g or greater than 30.0m 2 / g or less; (ii) The intrinsic viscosity [η] measured in a decalin solvent at 135° C. is 5 to 50 dl / g.

[0010] [2] The microporous membrane according to [1], wherein the ethylene polymer particles (A) satisfy the following requirement (iii): (iii) The bulk density is 0.01 to 0.20 g / mL.

[0011] [3] The microporous membrane according to [1] or [2], which is a separator.

[0012] [4] A method for producing a microporous membrane according to any one of [1] to [3], (a) preparing a kneaded mixture containing the ethylene polymer particles (A) and a solvent; (b) molding the kneaded mixture under a temperature condition higher than the dissolution temperature of the ethylene polymer particles (A) in a solvent to obtain a sheet-like molded product; (c) further stretching the sheet-like molded body; (d) removing the solvent from the sheet-like molded product; and (e) a step of heat fixing the molded body obtained through the steps (c) and (d) A method for producing a microporous membrane comprising the steps of: Effect of the Invention

[0013] According to the present invention, a microporous membrane having excellent stretchability and formability can be provided, and a microporous membrane free from forming defects such as holes during stretch forming can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will be specifically described below. In this specification, the term "to" indicating a numerical range, for example "M to N", means "greater than or equal to M and less than or equal to N" unless otherwise specified. In this specification, the term "(co)polymer" is used as a concept that encompasses both homopolymers and copolymers. In this specification, when an olefin constituting a certain (co)polymer is represented by M, the expression "structural unit derived from M" may be used, which means a "structural unit corresponding to M", that is, a structural unit having a pair of bonds formed by opening the π bond constituting the double bond of M.

[0015] <Microporous membrane> The microporous membrane of the present invention (hereinafter also referred to as "the microporous membrane") contains ethylene polymer particles (A) (hereinafter also referred to as "particles (A)") that satisfy the following requirements (i) and (ii). (i) The specific surface area calculated by the BET method from the adsorption / desorption isotherm measured by the nitrogen gas adsorption method is 2.00 m 2 / g or greater than 30.0m 2 / g or less. (ii) The intrinsic viscosity [η] measured in a decalin solvent at 135° C. is 5 to 50 dl / g.

[0016] <Ethylene-based polymer particles (A)> The particles (A) are not particularly limited as long as they are ethylene-based polymer particles that satisfy the above requirements (i) and (ii). The particles (A) are preferably ultra-high molecular weight ethylene-based polymer particles. The particles (A) used in the present microporous membrane may be one type or two or more types. The particles (A) used as a raw material for the present microporous membrane only need to have the following physical properties.

[0017] The content of particles (A) in the present microporous membrane is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, particularly preferably 95 to 100% by mass, and most preferably 100% by mass. When the content of the particles (A) is within the above range, a microporous membrane having excellent stretchability can be easily produced.

[0018] The ethylene-based polymer constituting the particles (A) may be an ethylene homopolymer or a copolymer of ethylene and another monomer, and among these, the ethylene-based polymer is preferably an ethylene homopolymer.

[0019] Examples of the other monomer include linear or branched α-olefins having 3 to 30 carbon atoms, preferably 3 to 20 carbon atoms, cyclic olefins having 3 to 30 carbon atoms, preferably 3 to 20 carbon atoms, polar monomers, α,β-unsaturated carboxylic acid esters, vinyl esters, unsaturated glycidyl esters, vinylcyclohexane, dienes, polyenes, and aromatic vinyl compounds. Among these, linear or branched α-olefins having 3 to 20 carbon atoms are preferred, linear or branched α-olefins having 3 to 10 carbon atoms are more preferred, and linear or branched α-olefins having 3 to 8 carbon atoms are even more preferred.

[0020] Examples of the α-olefin include propylene, 1-butene, 2-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene.

[0021] Examples of the cyclic olefin include cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, tetracyclododecene, and 2-methyl-1,4,5,8-dimethano-1,2,3,4,4a,5,8,8a-octahydronaphthalene.

[0022] Examples of the polar monomer include α,β-unsaturated carboxylic acids such as acrylic acid, methacrylic acid, fumaric acid, maleic anhydride, itaconic acid, itaconic anhydride, and bicyclo[2.2.1]-5-heptene-2,3-dicarboxylic anhydride; and metal salts of α,β-unsaturated carboxylic acids such as sodium salts, potassium salts, lithium salts, zinc salts, magnesium salts, and calcium salts thereof.

[0023] Examples of the α,β-unsaturated carboxylate ester include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, and isobutyl methacrylate.

[0024] Examples of the vinyl ester include vinyl acetate, vinyl propionate, vinyl caproate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl trifluoroacetate.

[0025] Examples of the unsaturated glycidyl ester include glycidyl acrylate, glycidyl methacrylate, and monoglycidyl itaconic acid ester.

[0026] The dienes and polyenes include cyclic or chain compounds having 4 to 30, and preferably 4 to 20, carbon atoms and two or more double bonds. Specific examples thereof include butadiene, isoprene, 4-methyl-1,3-pentadiene, 1,3-pentadiene, 1,4-pentadiene, 1,3-hexadiene, 1,4-hexadiene, 1,5-hexadiene, 1,3-octadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, ethylidenenorbornene, vinylnorbornene, dicyclopentadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, and 5,9-dimethyl-1,4,8-decatriene.

[0027] Examples of the aromatic vinyl compound include mono- or polyalkylstyrenes such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, o-ethylstyrene, m-ethylstyrene, and p-ethylstyrene; functional group-containing styrene derivatives such as methoxystyrene, ethoxystyrene, vinylbenzoic acid, methyl vinylbenzoate, vinylbenzyl acetate, hydroxystyrene, o-chlorostyrene, p-chlorostyrene, and divinylbenzene; 3-phenylpropylene, 4-phenylpropylene, and α-methylstyrene.

[0028] The content of repeating units derived from ethylene in the copolymer of ethylene and other monomers is preferably 95 mol% or more, more preferably 98 mol% or more, and even more preferably 99.5 mol% or more, relative to 100 mol% of all repeating units derived from ethylene and other monomers. The content of repeating units derived from ethylene and other monomers can be measured by known measuring methods such as nuclear magnetic resonance (NMR) spectroscopy and infrared absorption spectroscopy.

[0029] The ethylene-based polymers constituting the ethylene-based polymer may each contain at least one or more types of biomass-derived monomers (ethylene, an α-olefin having 3 to 20 carbon atoms). The same type of monomers constituting the polymer may be only biomass-derived monomers, may be only fossil fuel-derived monomers, or may contain both biomass-derived monomers and fossil fuel-derived monomers. The biomass-derived monomer is a monomer made from any renewable natural raw material or its residue, such as a plant-derived or animal-derived monomer, including fungi, yeast, algae, and bacteria, and contains as carbon 14 C isotope 1×10 -12 The biomass carbon concentration (unit: pMC) measured in accordance with ASTM D6866 is about 100 pMC. The biomass-derived monomers (ethylene, α-olefins, and other monomers) can be obtained, for example, by a conventionally known method.

[0030] It is preferable that these ethylene-based polymers contain structural units derived from biomass-derived monomers from the viewpoint of reducing the environmental load (mainly reducing greenhouse gases). If the polymer production conditions such as the polymerization catalyst, polymerization process, and polymerization temperature are the same, even if the raw material monomer is a (co)polymer containing a biomass-derived monomer, 14 C isotope 1×10 -12 ~10 -14 Other than the proportion of fossil fuel-derived monomers, the molecular structure is the same as that of (co)polymers made from fossil fuel-derived monomers. Therefore, the performance is said to be the same.

[0031] The melting point (Tm) of the particles (A) is preferably 120 to 160°C, more preferably 130 to 150°C, and even more preferably 135 to 145°C. When the melting point (Tm) is within the above range, the fluidity of the resin is maintained during molding, making molding easy. When the melting point (Tm) is below the above range, the resin may flow out during molding, making molding difficult, and the moldability (particularly the stretchability) of the obtained microporous film is reduced. When the melting point (Tm) is above the above range, the molecular fluidity is significantly reduced, and the moldability tends to be poor.

[0032] The specific surface area of ​​particle (A) calculated by the BET method from the adsorption / desorption isotherm measured by the nitrogen gas adsorption method is 2.00 m 2 / g or greater than 30.0m 2 / g or less, preferably 2.50 to 28.0 m 2 / g, more preferably 3.00 to 26.0m 2 / g, more preferably 3.00 to 20.0 m 2 / g, particularly preferably 3.00 to 18.0 m 2 When the specific surface area is within this range, a microporous membrane with excellent stretchability can be easily produced. The specific surface area means a total specific surface area obtained by adding up all the specific surface areas determined by the BET method from the adsorption / desorption isotherms measured by a nitrogen gas adsorption method, and specifically, is determined by the measurement method described in the examples below.

[0033] For example, according to the manufacturing method of the particles (A) described later, ethylene-based polymer particles having a specific surface area in the above range can be obtained. In particular, ethylene can be polymerized using a catalyst-containing liquid for ethylene polymerization obtained by contacting an organoaluminum compound or the like with a mixture of a metal halide and an alcohol to obtain a suspension, and then contacting the suspension with a transition metal compound, thereby easily obtaining ethylene-based polymer particles having a specific surface area in the above range.

[0034] The median diameter (D50) of the particles (A) determined by a laser diffraction scattering method is preferably 20 to 700 μm, more preferably 30 to 680 μm, further preferably 40 to 660 μm, and particularly preferably 220 to 660 μm. The particles (A) having a D50 in the above range have excellent handleability (fluidity), and therefore tend to easily give a microporous film having excellent uniformity (uniformity of the mixed state and uniformity of the dimensions and surface state of the molded product).

[0035] To obtain particles (A) having a D50 in the above range, the polymerization conditions may be adjusted in the polymerization step so that particles having a D50 in the above range are obtained, or particles (A) having a D50 larger than the above range may be crushed to obtain particles (A) having a D50 in the above range. In this case, the D50 may be adjusted to be within the above range in the following step [β] or after the step [β].

[0036] The intrinsic viscosity [η] of the particles (A) measured in a decalin solvent at 135°C is 5 to 50 dl / g, preferably 10 to 50 dl / g, more preferably 15 to 45 dl / g, even more preferably 10 to 40 dl / g, particularly preferably 15 to 35 dl / g, and even more preferably 20 to 30 dl / g. When the intrinsic viscosity [η] is within the above range, a microporous film having excellent stretchability can be easily produced. When the intrinsic viscosity [η] exceeds the above range, the film may not be stretched sufficiently, resulting in a decrease in moldability. On the other hand, when the intrinsic viscosity [η] is below the above range, the polymer chain having a small molecular weight constituting the particles may not exhibit sufficient strength due to structural defects originating from the ends.

[0037] The bulk density of the particles (A) is preferably 0.01 to 0.20 g / mL, more preferably 0.02 to 0.20 g / mL, even more preferably 0.03 to 0.20 g / mL, still more preferably 0.03 to 0.18 g / mL, particularly preferably 0.03 to 0.16 g / mL, and most preferably 0.04 to 0.15 g / mL. A microporous membrane having excellent stretchability can be easily produced from the particles (A) having a bulk density in the above range. The bulk density can be determined by the measurement method specifically described in the following Examples.

[0038] The content of coarse particles in 100% by mass of particles (A) is usually 20% by mass or less, preferably 15% by mass or less, more preferably 10% by mass or less, even more preferably 7% by mass or less, particularly preferably 3% by mass or less, and most preferably 1.5% by mass or less. If the particles (A) contain a large amount of coarse particles, sufficient fluidity may not be obtained during transportation of the particles (A) after polymerization, and clogging may occur in valves, pumps, strainers, etc. In order to prevent such problems, it is preferable that the content of the coarse particles is within the above range.

[0039] When the content of the coarse particles is within the above range, the transportability of the particles (A) during the production and processing of the particles (A) is excellent, so that uniform particles can be easily obtained and a microporous membrane with excellent stretchability can be easily produced. The coarse particles referred to above are particles having a particle diameter of 1 mm or more, and refer to particles that do not pass through a 1 mm x 1 mm mesh sieve when sieved for a shaking time of 10 minutes, with an amplitude of 0.5 mm and an interval of 15 seconds.

[0040] As described later in the method for producing particles (A), by using a magnesium halide (preferably MgCl2) during the production of particles (A), ethylene polymer particles having a specific surface area within the above range tend to be easily produced. A part of the magnesium halide used during the production usually remains in the particles (A), and the Mg content in the particles (A) corresponds to the concentration of the magnesium halide during the production. The Mg content in the particles (A) is preferably from 10 to 2,000 ppm, more preferably from 20 to 1,500 ppm, and further preferably from 30 to 1,000 ppm.

[0041] It is preferable that an acetone extract of the particles (A) contains a compound (F) having a structure represented by the following formula (f) (hereinafter also referred to as "structure (f)"). When the acetone extract of the particles (A) contains the compound (F), the particles (A) tend to become uniform particles, and a binder with excellent flowability can be easily obtained. When the compound (F) is contained in the acetone extract of the particles (A), the compound (F) may be one type or two or more types. Whether or not the compound (F) is contained in the acetone extract of the particles (A) can be identified by a known analytical method such as NMR spectroscopy, and specifically, can be confirmed by the method described in the examples below.

[0042] The acetone extract of the particles (A) refers to components that are dissolved from the particles (A) into acetone after the particles (A) are brought into contact with acetone. In general, the components that are dissolved into acetone are, among the constituent components of the particles (A), catalysts and additives used in the method for producing the particles (A) described below, and also components such as additives that can be used after polymerization may be included in the acetone extract. Specifically, the compound (F) is an antistatic agent (a compound derived from an antistatic agent), which is added during the polymerization stage of the particles (A) and is one of the additives that can be added after the polymerization.

[0043] [ka] [In formula (f), R represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms.]

[0044] Examples of the alkyl group having 1 to 12 carbon atoms for R include linear or branched alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a t-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, and an n-nonyl group.

[0045] The above R is preferably a hydrogen atom or a methyl group, and more preferably a hydrogen atom. When the compound (F) in which R is such an atom or group is used in the production of the particles (A), the compound (F) has excellent polymerization activity and an effect of suppressing the generation of coarse particles.

[0046] The compound (F) is preferably a compound in which a hydrogen atom is bonded to the oxygen atom in the formula (f), and is more preferably a compound having, in the molecule, one or more structures selected from the group consisting of a structure represented by the following formula [F1], a structure represented by the following formula [F2], and a structure represented by the following formula [F3].

[0047] [ka]

[0048] R in the formulae [F1] to [F3] has the same meaning as R in the formula (f). In the formula [F2], R″ is a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, n and m are 0 or 1, p is 1 or 2, and the sum of m and p is 2. It is preferable to use the compound (F) in which m is 0 and p is 2 when producing the particles (A), since this has excellent polymerization activity and an effect of suppressing the generation of coarse particles.

[0049] Examples of the compound having the skeleton represented by the general formula [F1] include polyoxyalkylene compounds, such as polyoxyalkylene glycols and ethylenediamine-based polyoxyalkylene polyols. A preferred example of a compound having a skeleton represented by the general formula [F2] is the aliphatic diethanolamide described in Japanese Patent No. 5796797. As a preferred example of the compound having a skeleton represented by the general formula [F3], the tertiary amine compounds described in Japanese Patent No. 5796797 can be mentioned.

[0050] The weight average molecular weight (Mw) of the compound (F) measured by gel permeation chromatography (GPC) is preferably 500 to 30,000, more preferably 1,000 to 25,500, further preferably 1,500 to 20,000, particularly preferably 1,500 to 10,000. When the compound (F) having Mw in the above range is used in the production of the particles (A), the particles (A) having excellent flowability and a low content of coarse particles can be easily obtained, and a microporous membrane having uniformity and excellent stretchability can be easily produced. On the other hand, when the compound (F) having Mw smaller than the above range is used in the production of the particles (A), the compound (F) may bleed out when a molded product is produced using the obtained particles (A), resulting in poor quality. On the other hand, when the compound (F) having Mw larger than the above range is used in the production of the particles (A), the compound (F) may be incorporated as a foreign matter into the molded product obtained using the obtained particles (A).

[0051] Specific examples of compound (F) include the "ADEKA PLURONIC (registered trademark)" series manufactured by ADEKA CORPORATION. Among these, from the viewpoints of availability and ability to suppress the generation of coarse particles, "ADEKA PLURONIC (registered trademark) L-71 (Mw: 3,760)", "ADEKA PLURONIC (registered trademark) L-72 (Mw: 4,700)", "ADEKA PLURONIC (registered trademark) L-31 (Mw: 1,700)", "ADEKA PLURONIC (registered trademark) P-85 (Mw: 7,430)", "ADEKA PLURONIC (registered trademark) F-68 (Mw: 15,100)" and "ADEKA PLURONIC (registered trademark) Polyoxyalkylene glycols such as ADEKA PLURONIC (registered trademark) F-88 (Mw: 19,300) and ADEKA PLURONIC (registered trademark) 17-R2 (Mw: 3,310); and ethylenediamine-based polyoxyalkylene polyols such as ADEKA PLURONIC (registered trademark) TR-701 (Mw: 5,060), ADEKA PLURONIC (registered trademark) TR-702 (Mw: 5,390), and ADEKA PLURONIC (registered trademark) TR-913R (Mw: 4,560). Specific examples of the compound (F) other than those mentioned above include Emulgen 108 (Mw: 769) and Emulgen 109P (Mw: 970) manufactured by Kao Corporation; and Amizet (registered trademark) 5C (Mw: 647) and Acetylenol (registered trademark) E13T (Mw: 444) manufactured by Kawaken Fine Chemicals Co., Ltd.

[0052] The content of compound (F) in particles (A) is preferably 6 to 1,000 ppm, more preferably 8 to 600 ppm, and further preferably 10 to 400 ppm. Particles (A) having a content of compound (F) within the above range tend to have excellent flowability and a low content of coarse particles, and a microporous membrane with excellent stretchability can be easily produced.

[0053] The compound (F) is a compound derived from an antistatic agent, which is usually added during the polymerization stage of the particles (A) or is one of the additives that can be added after polymerization. Therefore, the content of the compound (F) in the particles (A) can be adjusted by the amount of the compound (F) added when producing the particles (A). The content of the compound (F) in the particles (A) can be calculated by liquid chromatography-mass spectrometry (LC-MS) or the like.

[0054] <Method of producing ethylene polymer particles> The method for producing the ethylene polymer particles is not particularly limited, but a method including the following steps [α] and [β] is preferred.

[0055] Step [α]: A step of obtaining a suspension, comprising: a step (1) of contacting a metal halide with an alcohol in a hydrocarbon solvent; and a step (2) of contacting the component obtained in the step (1) with an organoaluminum compound and / or an organoaluminum oxy-compound. , The above steps contacting the suspension obtained in step 2 with a transition metal compound (B) represented by the following general formula [II]: <ii>, and Adding the compound (F) <iii> The process includes the steps <iii>The process and the above process <ii>During and / or during the steps <ii>A step of producing a catalyst-containing liquid for olefin polymerization, which is carried out after

[0056] Step [β]: A step of producing ethylene-based polymer particles by homopolymerizing ethylene or copolymerizing ethylene with a linear or branched α-olefin having 3 to 20 carbon atoms in the presence of the ethylene polymerization catalyst-containing liquid.

[0057] [ka]

[0058] In formula [II], M represents titanium, zirconium, or hafnium; m represents an integer from 1 to 4; R 1 ~R 5 may be the same or different and represent a hydrogen atom, a halogen atom, a hydrocarbon group, a heterocyclic compound residue, an oxygen-containing group, a nitrogen-containing group, a boron-containing group, a sulfur-containing group, a phosphorus-containing group, a silicon-containing group, a germanium-containing group, or a tin-containing group, two or more of which may be linked to each other to form a ring, R 6 is selected from a hydrogen atom, a hydrocarbon group having 1 to 4 carbon atoms consisting only of primary or secondary carbon, an aliphatic hydrocarbon group having 4 or more carbon atoms, an aryl group-substituted alkyl group, a monocyclic or bicyclic alicyclic hydrocarbon group, an aromatic hydrocarbon group, and a halogen atom; n is a number that satisfies the valence of M, X represents a hydrogen atom, a halogen atom, a hydrocarbon group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a boron-containing group, an aluminum-containing group, a phosphorus-containing group, a halogen-containing group, a heterocyclic compound residue, a silicon-containing group, a germanium-containing group, or a tin-containing group. When n is 2 or more, the multiple groups represented by X may be the same or different, and the multiple groups represented by X may be bonded to each other to form a ring.

[0059] (Metal Halides) As the metal halide used in the step [α], a magnesium halide is preferably used in order to obtain ethylene polymer particles having the specific surface area. As the magnesium halide, MgI2 and MgCl2 are preferable, and MgCl2 is more preferable. By obtaining a suspension in this manner, it tends to be possible to produce ethylene-based polymer particles having an extremely high specific surface area.

[0060] Furthermore, the concentration of the metal halide (particularly, magnesium halide) used in the ethylene polymerization catalyst-containing liquid affects the specific surface area of ​​the ethylene polymer particles, and the specific surface area tends to increase as the concentration increases. The concentration of the metal halide (particularly, magnesium halide) in the ethylene polymerization catalyst-containing liquid is preferably 0.10 to 5.0 mmol / L, more preferably 0.20 to 3.0 mmol / L, and even more preferably 0.30 to 2.0 mmol / L.

[0061] As described above, a part of the magnesium halide used during production is usually contained in the ethylene-based polymer particles, and the magnesium content corresponds to the concentration of the magnesium halide during production. In order to achieve the above effects, the ethylene-based polymer particles of the present invention preferably contain 10 to 2,000 ppm of magnesium, more preferably 20 to 1,000 ppm, and even more preferably 30 to 500 ppm.

[0062] (alcohol) The alcohol used in the step [α] may be an alcohol having 1 to 25 carbon atoms. Specific examples of the alcohol include alcohols having 1 to 25 carbon atoms, such as methanol, ethanol, propanol, butanol, pentanol, hexanol, 2-ethylhexanol, octanol, dodecanol, octadecyl alcohol, oleyl alcohol, 2-butyloctanol, 2-hexyldecanol, 2-hexyldodecanol, 2-octyldecanol, 2-octyldodecanol, isohexadecanol, isoeicosanol, benzyl alcohol, phenylethyl alcohol, cumyl alcohol, isopropyl alcohol, isobutyl alcohol, and isopropylbenzyl alcohol; halogen-containing alcohols having 1 to 25 carbon atoms, such as trichloromethanol, trichloroethanol, and trichlorohexanol; and phenols having 6 to 25 carbon atoms which may have an alkyl group, such as phenol, cresol, xylenol, ethylphenol, propylphenol, nonylphenol, cumylphenol, and naphthol. The alcohol may be used alone or in combination of two or more kinds.

[0063] In addition, when an alcohol having a relatively large number of carbon atoms, such as an alcohol having 13 to 25 carbon atoms, is present in the ethylene-based polymerization catalyst-containing liquid, it is expected that the ethylene polymerization reaction will proceed mildly, and as a result, it is expected that uneven distribution of heat generation during polymerization will be suppressed. Suppression of uneven distribution of heat generation during polymerization leads to suppression of the generated polymer chains from forming an entangled structure, which is thought to result in improved performance of the obtained molded product (microporous membrane).

[0064] The amount of alcohol used is not particularly limited as long as it is an amount that dissolves the metal halide, but from the viewpoint of easily forming an alcohol complex of the metal halide, the amount is preferably 0.1 to 50 mol, more preferably 0.5 to 30 mol, further preferably 1 to 20 mol, and particularly preferably 2 to 15 mol, per mol of the metal halide.

[0065] (Hydrocarbon Solvent) The hydrocarbon solvent is not particularly limited, but specific examples thereof include aliphatic hydrocarbons such as hexane, heptane, octane, decane, dodecane, kerosene, etc., alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclopentane, etc., aromatic hydrocarbons such as benzene, toluene, xylene, etc., halogenated hydrocarbons such as ethylene chloride, chlorobenzene, dichloromethane, etc. Among these, decane, dodecane, toluene, xylene, and chlorobenzene are preferred in terms of solubility, reaction temperature, etc. The hydrocarbon solvent may be used alone or in combination of two or more kinds.

[0066] The amount of the hydrocarbon solvent used is not particularly limited as long as it is an amount that can dissolve the metal halide, but from the viewpoint of easily forming an alcohol complex of the metal halide, the amount is preferably 0.1 to 100 mol, more preferably 0.2 to 50 mol, further preferably 0.3 to 40 mol, and particularly preferably 0.5 to 30 mol, per mol of the metal halide.

[0067] (Organoaluminum Compounds) As the organoaluminum compound, a compound represented by the following formula (Al-1) can be used. R a n AIX 3-n (Al-1) (In formula (Al-1), R a is a hydrocarbon group having 1 to 12 carbon atoms, X is a halogen atom or a hydrogen atom, and n is 1 to 3.

[0068] The hydrocarbon group having 1 to 12 carbon atoms is, for example, an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 1 to 12 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms, and specific examples include a methyl group (Me), an ethyl group (Et), an n-propyl group, an isopropyl group, an isobutyl group (iso-Bu), a pentyl group, a hexyl group, a 2-ethylhexyl group, an octyl group, an isoprenyl group, a cyclopentyl group, a cyclohexyl group, a phenyl group, and a tolyl group.

[0069] Examples of the organoaluminum compound represented by the formula (Al-1) include trialkylaluminums such as trimethylaluminum, triethylaluminum, triisopropylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, and tri-2-ethylhexylaluminum; alkenylaluminums such as triisoprenylaluminum; dialkylaluminum halides such as dimethylaluminum chloride, diethylaluminum chloride, diisopropylaluminum chloride, and dimethylaluminum bromide; alkylaluminum sesquihalides such as methylaluminum sesquichloride, ethylaluminum sesquichloride, isopropylaluminum sesquichloride, butylaluminum sesquichloride, and ethylaluminum sesquibromide; alkylaluminum dihalides such as methylaluminum dichloride, ethylaluminum dichloride, isopropylaluminum dichloride, and ethylaluminum dibromide; and alkylaluminum hydrides such as diethylaluminum hydride and diisobutylaluminum hydride.

[0070] Moreover, as the organoaluminum compound, a compound represented by the following formula (Al-2) can also be used.

[0071] R a n AlY 3-n (Al-2) [In formula (Al-2), R a is the same group as in formula (Al-1), Y is -OR b , -OSiR c 3. -OAlR d 2, -NR e 2, -SiR f 3 or -N(R g )AlR h A group represented by 2, n is an integer from 1 to 2.

[0072] R b , R c , R d and R h Examples of the alkyl group include a methyl group, an ethyl group, an isopropyl group, an isobutyl group, a cyclohexyl group, and a phenyl group. R e Examples of the alkyl group include a hydrogen atom, a methyl group, an ethyl group, an isopropyl group, a phenyl group, and a trimethylsilyl group. R f and R g Examples of the alkyl group include a methyl group and an ethyl group.

[0073] As the organoaluminum compound represented by the formula (Al-2), specifically, the following compounds are used.

[0074] (i)R a n Al(OR b ) 3-n A compound represented by Examples of such compounds include alkylaluminum alkoxides such as dimethylaluminum methoxide, diethylaluminum ethoxide, diisobutylaluminum methoxide, and diethylaluminum-2-ethylhexoxide.

[0075] (ii)R a n Al(OSiR c 3) 3-n A compound represented by Examples of such compounds include Et2Al(OSiMe3), (iso-Bu)2Al(OSiMe3), and (iso-Bu)2Al(OSiEt3).

[0076] (iii)R a n Al(OAlR d 2) 3-n A compound represented by Such compounds include, for example, Et2AlOAlEt2 and (iso-Bu)2AlOAl(iso-Bu)2.

[0077] (iv) R a n Al(NR e 2) 3-n A compound represented by Examples of such compounds include Me2AlNEt2, Et2AlNHMe, Me2AlNHEt, Et2AlN(SiMe3)2, and (iso-Bu)2AlN(SiMe3)2.

[0078] (v)R a n Al(SiR f 3) 3-n A compound represented by An example of such a compound is (iso-Bu)2AlSiMe3.

[0079] (vi)R a n Al〔N(R g )AlR h 2) 3-n A compound represented by Such compounds include, for example, Et2AlN(Me)AlEt2 and (iso-Bu)2AlN(Et)Al(iso-Bu)2.

[0080] Furthermore, as the organoaluminum compound, a compound represented by the following formula (Al-3), which is a complex alkylation product of a Group I metal and aluminum, can also be used.

[0081] M 1 AlR j 4 (Al-3) [In formula (Al-3), M 1 is a Group I metal atom such as Li, Na or K, and R j is a hydrocarbon group having 1 to 15 carbon atoms.

[0082] Specific examples of the organoaluminum compound represented by the formula (Al-3) include LiAl(C2H5)4, LiAl(C7H 15 )4 are examples.

[0083] Among the above-mentioned organoaluminum compounds, the compounds represented by the formula (Al-1) are preferred, and trimethylaluminum, triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride, ethylaluminum sesquichloride, ethylaluminum dichloride, and diisobutylaluminum hydride are particularly preferred.

[0084] (Organoaluminum oxy compound) The organoaluminum oxy compound is not particularly limited, and any conventionally known aluminoxane (including the benzene-insoluble organoaluminum oxy compounds exemplified in JP-A-2-78687 and the boron-containing organoaluminum oxy compounds exemplified in JP-A-2021-147437) can be used.

[0085] Examples of the organoaluminum oxy compound include methylaluminoxane, ethylaluminoxane, and isobutylaluminoxane. Specific examples include the organoaluminum oxy compounds described in JP-A-2021-147437. The organoaluminum oxy compounds may be used alone or in combination of two or more.

[0086] The amount of the organoaluminum compound and organoaluminum oxy-compound used is preferably 0.1 to 50 mol, more preferably 0.2 to 30 mol, further preferably 0.5 to 20 mol, and particularly preferably 1.0 to 10 mol, per mol of the metal halide.

[0087] <Other ingredients> The present microporous membrane may contain components other than the particles (A). The other components are not particularly limited, and examples thereof include conventionally known components, such as various stabilizers known per se, such as heat stabilizers, weathering stabilizers, rust inhibitors, copper damage stabilizers, and antistatic agents, as well as flame retardants, crosslinking agents, crosslinking assistants, antistatic agents, slip agents, antiblocking agents, antifogging agents, lubricants, dyes, pigments, fillers, mineral oil-based softeners, petroleum resins, and waxes. The other components may each be used alone or in combination of two or more.

[0088] The content of the other components in the present microporous membrane is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, more preferably 0 to 5% by mass, and it is particularly preferable that the present microporous membrane does not contain the other components (the content of the other components in the present microporous membrane is particularly preferably 0% by mass).

[0089] <Physical properties of this microporous membrane> The thickness of the present microporous membrane is preferably 5 to 50 μm, more preferably 10 to 40 μm, and further preferably 15 to 30 μm. From the viewpoint of obtaining good membrane strength, the thickness of the microporous membrane is preferably 5 μm or more, and from the viewpoint of obtaining good battery performance, the thickness of the microporous membrane is preferably 50 μm or less.

[0090] <Method for producing the microporous membrane> The present microporous membrane is preferably produced by a method including the following steps (a) to (e): The microporous membrane obtained by this method has excellent stretchability. (a) A step of preparing a kneaded mixture containing particles (A) and a solvent (b) A step of forming the kneaded product under a temperature condition higher than the dissolution temperature of the particles (A) in the solvent to obtain a sheet-like formed product. (c) Further stretching the sheet-like molded body (d) removing the solvent from the sheet-like molded product (e) a step of heat fixing the molded body obtained through the steps (c) and (d)

[0091] <Process (a)> Step (a) is a step of preparing a kneaded mixture containing particles (A) and a solvent, and it is preferable to prepare the kneaded mixture by melt-kneading the particles (A) and a solvent. As the solvent, any known solvent can be used as long as it is liquid or solid and becomes liquid at high temperatures, and can be extracted with a cleaning solvent described below. For example, when a solvent that is liquid at room temperature is used, it tends to be possible to stretch at a relatively high ratio. Such a liquid solvent is not particularly limited, but aliphatic or cyclic hydrocarbons such as nonane, decane, decalin, paraxylene, undecane, dodecane, and liquid paraffin, mineral oil fractions having boiling points corresponding to these, and phthalic acid esters that are liquid at room temperature, such as dibutyl phthalate and dioctyl phthalate, can be used.

[0092] In order to obtain a stable sheet-like molded product, it is preferable to use a non-volatile liquid solvent such as liquid paraffin. It is also preferable to use a solvent that is solid and becomes liquid at high temperatures. A plasticizer that is in a mixed state with the polyolefin resin composition in a heated melt-kneaded state but is solid at room temperature may be mixed with a liquid plasticizer. Examples of such plasticizers include paraffin wax, which is solid at room temperature, and higher aliphatic alcohols such as stearyl alcohol and ceryl alcohol.

[0093] The amount of the solvent used is preferably 50 to 95% by mass, more preferably 50 to 90% by mass, of the kneaded mixture of the particles (A) and the solvent. The amount of the solvent is preferably not less than the lower limit from the viewpoint of obtaining a microporous membrane with an appropriate and uniform pore size, and is preferably not more than the upper limit from the viewpoint of obtaining a uniform kneaded mixture of the particles (A) and the solvent.

[0094] If necessary, additives such as antioxidants and ultraviolet absorbers can be added to the kneaded material as long as the object of the present invention is not impaired. The method of the melt kneading is not particularly limited, but may be prepared by kneading using a known method, for example, the particles (A) and the solvent may be kneaded in a batch system using a kneader such as a Banbury mixer or a kneader, or a twin-screw extruder to obtain a kneaded product. The temperature of the melt kneading is usually 160 to 300°C, preferably 180 to 280°C.

[0095] <Process (b)> Step (b) is a step of forming the kneaded mixture under a temperature condition higher than the dissolution temperature of the particles (A) in the solvent to obtain a sheet-like formed product. The melt-kneaded mixture may be formed into a sheet-like molded product by hot pressing, or may be formed into a sheet-like molded product by using an extruder equipped with a T-die or the like, or may be formed into a sheet-like molded product by cooling once, pelletizing, and then extruding again through a die via an extruder into a sheet-like molded product. Alternatively, the mixture may be kneaded using a twin-screw extruder or a continuous kneader, and then formed into a sheet-like molded product using a die attached to the tip of the kneader.

[0096] The temperature during the heat pressing or extrusion is preferably higher than the dissolution temperature of the particles (A) in the solvent, and is usually 140 to 280°C. As the die, a sheet die is usually used, but a double cylindrical hollow die, an inflation die, etc. can also be used.

[0097] When forming into a sheet, the sheet-shaped product obtained by the above method may be further quenched. In this case, it is more preferable to quench under conditions where the degree of supercooling (ΔT) is 20° C. or more. By carrying out the quenching operation, the phase separation structure in which the phase of the particles (A) is microphase separated by the solvent can be fixed, and the film strength can be further increased.

[0098] The thickness of the obtained sheet-like molded product is not particularly limited, but is preferably 0.1 to 30 mm, more preferably 0.2 to 20 mm.The sheet-like molded product is preferably in a gel state.

[0099] <Process (c)> Step (c) is a step of further stretching the sheet-like molded body. This step may be performed before or after step (d) described later, or may be further performed on the molded body obtained through steps (c) and (d) in this order. That is, the solvent may be removed after the sheet-like molded body is stretched, the solvent may be removed from the sheet-like molded body and then the sheet-like molded body is stretched, or the solvent may be removed from the sheet-like molded body and then the sheet-like molded body is stretched and then further stretched.

[0100] The stretching is performed at a predetermined magnification by a normal tenter method, roll method, inflation method, rolling method, or a combination of these methods after heating the sheet-like molded body. The stretching may be uniaxial or biaxial, but biaxial stretching is preferred. In the case of biaxial stretching, simultaneous biaxial stretching, sequential stretching, or multi-stage stretching (for example, a combination of simultaneous biaxial stretching and sequential stretching) may be used, but simultaneous biaxial stretching is particularly preferred. Stretching tends to improve the mechanical strength of the resulting microporous membrane.

[0101] The stretching ratio varies depending on the thickness of the sheet, but in the case of uniaxial stretching, it is preferably 2 times or more, and more preferably 3 to 30 times. In the case of biaxial stretching, it is at least 3 times or more in either direction, and the areal ratio is preferably 9 times or more, and more preferably 25 times or more. By making the areal ratio 9 times or more, the pin puncture strength and the like are improved. The stretching temperature is usually in the range of 100 to 140°C, and preferably 110 to 120°C.

[0102] <Process (d)> Step (d) is a step of removing the solvent from the sheet-like molded product. As described above, this step may be performed before or after step (c). Moreover, this step may be further performed to remove the remaining solvent from the molded product obtained through steps (d) and (c) in this order. A washing solvent is used to remove (wash) the solvent. The phase of the particles (A) is microphase-separated from the solvent used in step (a), so a porous film is obtained by extracting and removing the solvent. The washing solvent may be a known washing solvent, and examples of such solvent include chlorinated hydrocarbons such as methylene chloride and carbon tetrachloride, hydrocarbons such as pentane, hexane, and heptane, fluorinated hydrocarbons such as trifluoroethane, ethers such as diethyl ether and dioxane, and easily volatile solvents such as methyl ethyl ketone.

[0103] The solvent can be removed (washed) by immersing the stretched membrane or sheet in a washing solvent, showering the stretched membrane or sheet with the washing solvent, or a combination of these methods. Washing with the washing solvent is preferably carried out until the amount of remaining solvent is less than 1 part by mass relative to the amount added.

[0104] <Process (e)> Step (e) is a step of heat-setting the molded article having a microporous structure obtained through steps (c) and (d) for the purpose of preventing shrinkage of the microporous membrane in the stretching direction due to residual stress acting during stretching.

[0105] The heat setting temperature is preferably 80°C or higher and lower than 160°C. The heat setting method may be a known method, and specific examples include a method of passing the microporous membrane through a continuous hot air oven to heat shrink the membrane to a length reduction of 10 to 50% after heat setting (this method is also called "relaxation"), and a method of fixing the membrane so that the dimension in the stretching direction does not change.

[0106] In addition, before the heat setting, it is also preferable to dry the molded body obtained through the steps (c) and (d) by a heat drying method, an air drying method, etc. The drying temperature is preferably a temperature equal to or lower than the crystal dispersion temperature of the particles (A), and more preferably a temperature 5° C. or more lower than the crystal dispersion temperature.

[0107] There are no particular limitations as long as the drying treatment dries the molded body to an extent that does not impair the object of the present invention, but the content of the washing solvent remaining in the microporous membrane is preferably 5 parts by mass or less, and more preferably 3 parts by mass or less, per 100 parts by mass of the molded body after drying. If a large amount of washing solvent remains in the membrane due to insufficient drying, the porosity may decrease during subsequent heat setting, and permeability may deteriorate.

[0108] <separator> Due to its excellent stretchability and other characteristics, the microporous membrane is useful as a raw material for films, microporous membranes, and separators, and is particularly useful as a battery separator for lithium secondary batteries, nickel-hydrogen batteries, nickel-cadmium batteries, polymer batteries, and the like. The battery separator obtained from the microporous membrane is considered to have higher permeability, better heat shrinkage, and higher safety than battery separators obtained from microporous membranes made of ethylene-based polymer particles that do not satisfy the requirements of the present invention, since the polymer is less likely to melt during the membrane drying process. Therefore, the battery separator obtained from the microporous membrane is very useful in terms of safety, and is particularly suitable as a lithium battery separator.

[0109] When used as a separator, it is preferable to form a porous resin film having a single layer or multilayer structure composed of one or more types of particles (A). The separator has a thickness of, for example, 5 to 30 μm. EXAMPLES

[0110] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0111] <Specific surface area> The adsorption and desorption isotherms of the ethylene polymer particles were measured by the nitrogen gas adsorption method using a high-precision gas adsorption apparatus (Microtrack Bell, LA-950). As an analytical method, the specific surface area of ​​the ethylene polymer particles was determined from the adsorption / desorption isotherm by the BET method. Before measuring the adsorption / desorption isotherm, degassing was performed using a pretreatment device (Microtrack-Bel, BELPREP VAC-II).

[0112] <Intrinsic viscosity [η]> The intrinsic viscosity [η] of the ethylene polymer particles was measured in decalin at a temperature of 135° C. by dissolving the particles in decalin and using a fully automatic viscosity measuring device (VMR-053UPC, manufactured by Rigo Co., Ltd.).

[0113] <Bulk density> The bulk density of the ethylene polymer particles was measured using a standard bulk specific gravity measuring instrument (manufactured by Tsutsui Rikagaku Kikai Co., Ltd., JIS K 6720 for vinyl chloride resins). Specifically, the attached 100 mL SUS container, the mass of which had been measured in advance, was set, and ethylene-based polymer particles were filled from the funnel of a standard bulk specific gravity measuring instrument (manufactured by Tsutsui Rikagaku Kikai Co., Ltd., JIS K-6720 for polyvinyl chloride resin). Excess ethylene-based polymer particles on the SUS container were removed with a spatula to adjust the volume to exactly 100 mL, and the mass was measured again to calculate the bulk density.

[0114] <Melting point> Using a differential scanning calorimeter (Discovery DSC2500 manufactured by TA Instruments), a sample (about 5 mg) in a nitrogen atmosphere was (1) heated from 30° C. to 200° C. at 10° C. / min and held for 10 minutes, (2) cooled to 30° C. at 10° C. / min and held at 30° C. for 1 minute, and then (3) heated to 200° C. at 10° C. / min. The temperature at the apex of the crystal melting peak during the heating process in (1) was taken as the melting point.

[0115] [Synthesis Example 1] Preparation of component (i) 66.1 g (0.694 mol) of anhydrous magnesium chloride, 246 g of dehydrated decane, and 271 g (2.08 mol) of 2-ethylhexanol were placed in a 1 L glass vessel equipped with a stirrer and thoroughly purged with nitrogen, and the mixture was reacted at 145°C for 4 hours to obtain a homogeneous and transparent component (i') of 1.0 mol / L in terms of Mg atom. The component (i') was diluted with dehydrated decane to obtain a homogeneous and transparent component (i) having a concentration of 0.25 mol / L calculated as Mg atom.

[0116] [Synthesis Example 2] Production of ethylene-based polymer particles (A-1) Capacity 1.6m with agitator, fully substituted with nitrogen 3 Into the reactor, 721 kg of dehydrated decane and 2.7 mol of triisobutylaluminum in terms of Al atoms were charged. After heating to 60°C, 0.86 mol of the component (i) in terms of Mg atoms were charged and stirred for 15 minutes. After that, it was cooled to 40°C, and ethylene gas was blown in until the pressure inside the reactor became 0.1 MPaG. Next, 4.3 mmol of the transition metal compound (B-1) in terms of Ti atoms was charged, followed by 5.8 g of Adeka Pluronic (registered trademark) L-71 (manufactured by ADEKA Corporation) and 7.2 NL of hydrogen, and then polymerization reaction was carried out at 50°C for 119 minutes while supplying ethylene gas so that the total pressure became 0.6 MPaG. After the polymerization was completed, the mixture was filtered and washed with decane, washed with hexane, and dried under reduced pressure at 80°C for 18 hours to obtain 52.5 kg of ethylene-based polymer particles (A-1). The intrinsic viscosity [η] of the obtained ethylene polymer particles was 22 dl / g, the bulk density was 0.065 g / mL, and the specific surface area was 3.3 m 2 / g and the melting point was 140.3°C.

[0117] [ka] [In formula (B-1), t Bu represents a tert-butyl group.

[0118] [Ethylene-based polymer particles (CA-1)] As the ethylene-based polymer particles (CA-1), a polymer having the following physical properties was used. ·Intrinsic viscosity [η]: 22dl / g ·Specific surface area: 0.9m 2 / g Bulk density: 0.42g / mL Melting point: 135.7℃

[0119] [Example 1] The ethylene polymer particles (A-1) obtained in Production Example 2 and liquid paraffin were melt-kneaded at a mass ratio of 20 / 80 at 200°C using a batch kneader (manufactured by Toyo Seiki Co., Ltd.). The kneaded mixture was heat-pressed at 200°C to obtain a sheet-like molded product having a thickness of 0.5 mm. The obtained sheet-like molded product was simultaneously biaxially stretched 6x6 times at a stretching temperature of 115°C using a batch biaxial stretching machine. After stretching, the liquid paraffin was extracted and removed using hexane, and dried at room temperature. Next, heat setting was performed at 125°C for 1 minute to obtain a microporous film having a thickness of 15 μm. The microporous film was formed without any holes.

[0120] [Comparative Example 1] A microporous membrane was produced in the same manner as in Example 1, except that the ethylene-based polymer particles (CA-1) were used instead of the ethylene-based polymer particles (A-1). The obtained microporous membrane had holes (breaks). < / ii> < / ii> < / iii> < / iii> < / ii>

Claims

1. A microporous membrane obtained from ethylene-based polymer particles (A), wherein the ethylene-based polymer particles (A) satisfy the following requirements (i) and (ii): (i) The specific surface area calculated by the BET method from the adsorption / desorption isotherm measured by the nitrogen gas adsorption method is 2.00 m 2 / g or more, 30.0 m 2 / g or less; (ii) The intrinsic viscosity [η] measured in a decalin solvent at 135° C. is 5 to 50 dl / g.

2. The microporous membrane according to claim 1, wherein the ethylene-based polymer particles (A) satisfy the following requirement (iii): (iii) The bulk density is 0.01 to 0.20 g / mL.

3. The microporous membrane of claim 1 which is a separator.

4. A method for producing the microporous membrane according to any one of claims 1 to 3, comprising the steps of: (a) preparing a kneaded mixture containing the ethylene polymer particles (A) and a solvent; (b) forming the kneaded mixture under a temperature condition higher than the dissolution temperature of the ethylene polymer particles (A) in a solvent to obtain a sheet-like formed product; (c) further stretching the sheet-like molded body; (d) removing the solvent from the sheet-like molded body; and (e) a step of heat fixing the molded body obtained through the steps (c) and (d) A method for producing a microporous membrane comprising the steps of:

Citation Information

Patent Citations

  • Lapping machine

    JP1981089473A

  • Polyethylene powder, sintered porous sheet, adsorption buffer material and battery separator

    JP2019038931A