Positive electrode and fluoride ion secondary battery

By forming a positive electrode composite layer with specific active materials and a solid electrolyte, the discharge capacity of fluoride ion batteries is enhanced, addressing the insufficient capacity issue in existing technologies.

JP2024136989AActive Publication Date: 2024-10-04HONDA MOTOR CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023048317
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

The fluoride ion battery described in Patent Document 1 does not have sufficient discharge capacity per unit mass of the positive electrode active material layer.

Method used

A positive electrode composite layer is formed with a first active material having a higher fluorination potential than a second active material, and optionally includes a third active material with higher fluoride ion conductivity, along with a solid electrolyte, to enhance discharge capacity.

Benefits of technology

The discharge capacity of the fluoride ion secondary battery per unit mass of the positive electrode composite material layer is improved by optimizing the composition and properties of the active materials and incorporating a solid electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136989000002
    Figure 2024136989000002
  • Figure 2024136989000003
    Figure 2024136989000003
  • Figure 2024136989000004
    Figure 2024136989000004
Patent Text Reader

Abstract

To provide a positive electrode capable of improving the discharge capacity of a fluoride ion secondary battery per unit mass of a positive electrode mixture layer.SOLUTION: The positive electrode has a positive electrode mixture layer formed on a positive electrode current collector. The positive electrode mixture layer contains a first active material that does not contain fluorine and a second active material that does not contain fluorine. The molar ratio of the first active material to the second active material is 4 or more and 35 or less. The first active material has a higher fluorine potential than the second active material.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode and a fluoride ion secondary battery. [Background technology]

[0002] In recent years, research and development of fluoride-ion secondary batteries has been conducted to contribute to energy efficiency so that many people can have access to affordable, reliable, sustainable and advanced energy.

[0003] Patent Document 1 describes a fluoride ion battery having a positive electrode active material layer containing a Cu-based active material and BiF3. Here, the positive electrode active material layer is formed by forming a precursor layer containing a Cu-based active material and Bi, and then introducing fluoride ions into the precursor layer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2022-178410 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the fluoride ion battery described in Patent Document 1 does not have a sufficient discharge capacity per unit mass of the positive electrode active material layer.

[0006] An object of the present invention is to provide a positive electrode capable of improving the discharge capacity per unit mass of a positive electrode mixture layer of a fluoride ion secondary battery. [Means for solving the problem]

[0007] (1) A positive electrode, comprising: a positive electrode composite layer formed on a positive electrode current collector; the positive electrode composite layer including a first active material not containing fluorine and a second active material not containing fluorine; a molar ratio of the first active material to the second active material being equal to or greater than 4 and equal to or less than 35; and the first active material having a higher fluorination potential than the second active material.

[0008] (2) The positive electrode according to (1), wherein the first active material and the second active material are composited.

[0009] (3) The positive electrode according to (1) or (2), wherein the positive electrode mixture layer further contains a third active material containing fluorine, and the third active material has a higher fluoride ion conductivity than the fluoride of the second active material.

[0010] (4) The first active material is copper, the second active material is bismuth, and the third active material is represented by the general formula K x Bi 1-x F 3-2x (In the formula, x is equal to or greater than 0.02 and equal to or less than 0.12.) and having a hexagonal structure.

[0011] (5) The positive electrode according to (3) or (4), wherein the first active material has a primary particle diameter of 10 nm or more and 500 nm or less, the second active material has a primary particle diameter of 10 nm or more and 500 nm or less, and the third active material has a primary particle diameter of 10 nm or more and 200 nm or less.

[0012] (6) The positive electrode according to any one of (1) to (5), wherein the positive electrode mixture layer further contains a solid electrolyte containing fluorine.

[0013] (7) The positive electrode according to (6), wherein the solid electrolyte is a metal containing cerium and strontium.

[0014] (8) A fluoride ion secondary battery comprising the positive electrode according to any one of (1) to (7). Effect of the Invention

[0015] According to the present invention, it is possible to provide a positive electrode that can improve the discharge capacity of a fluoride ion secondary battery per unit mass of the positive electrode mixture layer. [Brief description of the drawings]

[0016] [Figure 1] 1 is a graph showing the fluoride ion conductivity of K0.06Bi0.94F2.88 and BiF3. [Diagram 2] TEM image and elemental mapping of K0.06Bi0.94F2.88. [Diagram 3] This is an SEM image of K0.06Bi0.94F2.88. [Figure 4] 2 shows an SEM image and element mapping of the positive electrode composite of Example 1. [Diagram 5] 1 is an XRD spectrum of the positive electrode composite of Example 1. [Figure 6] 1 is a graph showing charge / discharge curves of the cell of Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment of the present invention will be described.

[0018] [Positive electrode] The positive electrode of this embodiment has a positive electrode mixture layer formed on a positive electrode current collector, and the positive electrode mixture layer includes a first active material not containing fluorine and a second active material not containing fluorine, where the first active material has a higher fluorination potential than the second active material.

[0019] The molar ratio of the first active material to the second active material is 4 or more and 35 or less, and preferably 4 or more and 20 or less. Since the molar ratio of the first active material to the second active material is 4 or more and 35 or less, the discharge capacity of the fluoride ion secondary battery per unit mass of the positive electrode mixture layer is improved. For example, when the first active material and the second active material are Cu and Bi, respectively, if the molar ratio of Cu to Bi is less than 4, the energy density of the fluoride ion secondary battery per unit mass of the positive electrode mixture layer decreases, and if it exceeds 35, the efficiency of generating BiF3 and supplying ions to Cu during charging of the fluoride ion secondary battery decreases.

[0020] The first active material is not particularly limited as long as it is a metal having a higher fluoridation potential than the second active material, and examples thereof include Cu, Co(III), and Mo, and two or more of them may be used in combination. Among these, Cu is preferred in terms of the discharge capacity of the fluoride ion secondary battery per unit mass of the positive electrode composite layer.

[0021] The fluorination potential of the first active material is not particularly limited, but is, for example, 0.3 V (vs. Pb / PbF2) or more and 1.5 V (vs. Pb / PbF2) or less.

[0022] The primary particle diameter of the first active material is preferably 10 nm or more and 500 nm or less, and more preferably 10 nm or more and 200 nm or less. When the primary particle diameter of the first active material is 10 nm or more and 500 nm or less, the discharge capacity of the fluoride ion secondary battery per unit mass of the positive electrode mixture layer is improved.

[0023] The second active material is not particularly limited as long as it is a metal having a lower fluoridation potential than the first active material, and examples thereof include W, V, Bi, Sb, Ni, and Sn, and two or more of them may be used in combination. Among these, Bi is preferred in terms of the discharge capacity of the fluoride ion secondary battery per unit mass of the positive electrode mixture layer.

[0024] The fluorination potential of the second active material is not particularly limited, but is, for example, −0.2 V (vs. Pb / PbF2) or more and 0.5 V (vs. Pb / PbF2) or less.

[0025] The primary particle diameter of the second active material is preferably 10 nm or more and 500 nm or less, and more preferably 10 nm or more and 300 nm or less. When the primary particle diameter of the second active material is 10 nm or more and 500 nm or less, the discharge capacity of the fluoride ion secondary battery per unit mass of the positive electrode mixture layer is improved.

[0026] The first and second active materials are preferably composited together, which improves the discharge capacity of the fluoride ion secondary battery per unit mass of the positive electrode mixture layer.

[0027] The first and second active materials can be combined by mechanical force. The first and second active materials can also be combined by an aerosol process. For example, the first and second active materials are melted and then sprayed under reduced pressure.

[0028] The positive electrode mixture layer preferably further contains a third active material containing fluorine. In this case, the third active material has a higher fluoride ion conductivity than the fluoride of the second active material. This improves the discharge capacity of the fluoride ion secondary battery per unit mass of the positive electrode mixture layer.

[0029] The third active material is not particularly limited as long as it is a metal fluoride having a higher fluoride ion conductivity than the fluoride of the second active material. Among these, the third active material is preferably a metal fluoride having a higher fluoride ion conductivity than the fluoride of the second active material, which is represented by the general formula: K x Bi 1-x F 3-2x (In the formula, x is equal to or greater than 0.02 and equal to or less than 0.12.) and a compound having a hexagonal structure is preferred.

[0030] The primary particle diameter of the third active material is preferably 10 nm or more and 200 nm or less, more preferably 10 nm or more and 100 nm or less. When the primary particle diameter of the third active material is 10 nm or more and 200 nm or less, the discharge capacity of the fluoride ion secondary battery per unit mass of the positive electrode mixture layer is improved.

[0031] Next, Cu, Bi and K were used as the first active material, the second active material and the third active material, respectively. 0.06 Bi 0.94 F 2.88 The behavior of the positive electrode during charging and discharging of a fluoride ion secondary battery when using the following is described below. Here, the fluorination potentials of Cu and Bi are 0.65 V (vs. Pb / PbF2) and 0.31 V (vs. Pb / PbF2), respectively.

[0032] When a fluoride ion secondary battery is charged, first, Bi, which has a lower fluorination potential than Cu and is composited with Cu, is fluorinated to produce BiF3. At this time, K 0.06 Bi 0.94 F 2.88 (See Figure 1) is present, so Bi is used more effectively. Next, Cu, which has a higher fluorination potential than Bi and is composited with Bi, is fluorinated to produce CuF2. At this time, BiF3 and K, which has a higher fluoride ion conductivity than BiF3, are 0.06 Bi 0.94 F 2.88 Due to the presence of and, Cu is utilized more efficiently.

[0033] On the other hand, when a fluoride ion secondary battery is discharged, CuF2 is first defluorinated to produce Cu. At this time, BiF3, which is composited with Cu, and KF3, which has a higher fluoride ion conductivity than BiF3, are mixed. 0.06 Bi 0.94 F 2.88 The presence of , allows CuF2 to be more effectively utilized. Next, BiF3 is defluorinated to produce Bi, and K 0.06 Bi 0.94 F 2.88is defluorinated. At this time, K, which has a higher fluoride ion conductivity than BiF3, 0.06 Bi 0.94 F 2.88 Because of the presence of , BiF3 is utilized more efficiently. This improves the discharge capacity of the fluoride ion secondary battery per unit mass of the positive electrode mixture layer.

[0034] The positive electrode composite layer preferably further contains a solid electrolyte containing fluorine. As a result, when the fluoride of the second active material and the third active material are defluorinated during discharge of the fluoride ion secondary battery, the fluoride of the second active material and the third active material are effectively utilized because of the presence of the solid electrolyte containing fluorine. As a result, the discharge capacity of the fluoride ion secondary battery per unit mass of the positive electrode composite layer is improved.

[0035] The solid electrolyte is not particularly limited as long as it is a metal fluoride that has fluoride ion conductivity and is not defluorinated during discharge of the fluoride ion secondary battery. For example, Ce 0.975 Sr 0.025 F 2.975 , La 0.93 Ba 0.07 F 2.93 , Ca 0.5 Sr 0.5 F2, Sr 0.7 Y 0.3 F 2.3 , B.A. 0.7 Sb 0.3 F 2.3 , La 0.9 Sr 0.1 F 2.9 , B.A. 0.5 Ca 0.5 F2, and two or more of them may be used in combination.

[0036] The positive electrode mixture layer may further contain a conductive assistant etc. as necessary. The conductive assistant is not particularly limited as long as it has electronic conductivity, but examples thereof include acetylene black.

[0037] The positive electrode current collector is not particularly limited as long as it has electronic conductivity, and an example of the positive electrode current collector is gold foil.

[0038] [Fluoride ion secondary battery] The fluoride ion secondary battery of this embodiment includes the positive electrode of this embodiment, and for example, a solid electrolyte layer is disposed between the positive electrode of this embodiment and the negative electrode.

[0039] The negative electrode has a negative electrode mixture layer formed on a negative electrode current collector. In this case, the negative electrode mixture layer contains a negative electrode active material and may further contain a solid electrolyte, a conductive assistant, and the like, as necessary.

[0040] The negative electrode current collector is not particularly limited as long as it has electronic conductivity, but for example, aluminum foil can be used. The negative electrode active material is not particularly limited, but for example, PbSnF4 can be used. The conductive assistant is not particularly limited as long as it has electronic conductivity, but for example, acetylene black can be used.

[0041] The solid electrolyte constituting the solid electrolyte layer is not particularly limited as long as it has fluoride ion conductivity. For example, Ce 0.95 Sr 0.05 F 2.85 Examples include:

[0042] The fluoride ion secondary battery of this embodiment is obtained, for example, by sequentially laminating a positive electrode current collector and a positive electrode mixture, a solid electrolyte, a negative electrode current collector and a negative electrode mixture, and then integrally molding the resultant.

[0043] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and the above embodiment may be modified as appropriate within the scope of the spirit of the present invention. EXAMPLES

[0044] Examples of the present invention will be described below, but the present invention is not limited to these examples.

[0045] [K 0.06 Bi 0.94 F 2.88 Preparation of Potassium fluoride (manufactured by Kojundo Chemical Laboratory) and bismuth fluoride (manufactured by Kojundo Chemical Laboratory) were weighed out, and then premixed for about 1 hour using an agate mortar and pestle to obtain a raw material mixed powder.

[0046] The obtained raw material mixed powder was classified using a stainless steel mesh with 500 μm openings. Next, the raw material mixed powder that did not pass through the mesh was mixed using an agate mortar and pestle and then classified, and this operation was repeated until all the raw material mixed powder passed through the mesh.

[0047] The weighing, pre-mixing and classification of the raw materials were carried out in a purged (DBO type) glove box (manufactured by Miwa Seisakusho) to prevent moisture absorption by the fluoride.

[0048] The sealed powder hopper containing the classified raw material mixed powder was removed from the glove box and connected to a high-frequency induction thermal plasma nanoparticle synthesis device TP-40020NPS (manufactured by JEOL Ltd.). Next, argon gas was supplied to the plasma torch, and the raw material mixed powder was melted by thermal plasma to form a raw material melt, which was then sprayed into a chamber in a reduced pressure environment. The raw material melt sprayed into the chamber was cooled and turned into nanoparticles, and the K 0.06 Bi 0.94 F 2.88 Next, the exhaust filter was 0.06 Bi 0.94 F 2.88 After collecting the K, the exhaust filter was closed off at both the upstream and downstream with valves and the exhaust was transported into a glove box. 0.06 Bi 0.94 F 2.88 was collected. Here, K 0.06 Bi 0.94 F 2.88 The composition was analyzed by ICP atomic emission spectrometry.

[0049] In Figure 2, 0.06 Bi 0.94 F 2.88The TEM image and elemental mapping are shown in Fig. 1. The TEM image and elemental mapping were analyzed by TEM-EELS.

[0050] In Figure 3, 0.06 Bi 0.94 F 2.88 The SEM image is shown.

[0051] From Figure 3, K 0.06 Bi 0.94 F 2.88 It can be seen that the primary particle diameter is 10 nm or more and 100 nm or less.

[0052] [Ce 0.92 Sr 0.08 F 2.92 Preparation of Cerium fluoride (manufactured by Kojundo Chemical Laboratory) and strontium fluoride (manufactured by Kojundo Chemical Laboratory) were weighed out, and then premixed for about 1 hour using an agate mortar and pestle to obtain a raw material mixed powder.

[0053] The obtained raw material mixed powder was classified using a stainless steel mesh with 500 μm openings. Next, the raw material mixed powder that did not pass through the mesh was mixed using an agate mortar and pestle and then classified, and this operation was repeated until all the raw material mixed powder passed through the mesh.

[0054] The weighing, pre-mixing and classification of the raw materials were carried out in a purged (DBO type) glove box (manufactured by Miwa Seisakusho) to prevent moisture absorption by the fluoride.

[0055] The sealed powder hopper containing the classified raw material powder mixture was removed from the glove box and connected to a high-frequency induction thermal plasma nanoparticle synthesis device TP-40020NPS (manufactured by JEOL Ltd.). Next, argon gas was supplied to the plasma torch, and the raw material powder mixture was melted by thermal plasma to produce a raw material melt, which was then sprayed into a chamber in a reduced pressure environment. The raw material melt sprayed into the chamber was cooled and turned into nanoparticles, resulting in the release of Ce. 0.92 Sr0.08 F 2.92 Next, Ce was detected in the exhaust filter. 0.92 Sr 0.08 F 2.92 After collecting the Ce, the exhaust filter was blocked off at both the upstream and downstream with valves and the exhaust was transported into a glove box. 0.92 Sr 0.08 F 2.92 Here, Ce 0.92 Sr 0.08 F 2.92 The composition was analyzed by ICP atomic emission spectrometry.

[0056] [Example 1] Copper (manufactured by High Purity Chemical Laboratory), Bismuth (manufactured by High Purity Chemical Laboratory), K 0.06 Bi 0.94 F 2.88 and acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) were weighed to a mass ratio of 50.0:16.7:31.1:2.2, and then placed in a 45 mL silicon nitride pot. Next, a silicon nitride ball with a diameter of 2 mm and cyclohexane were placed in the pot to crush the raw material. At this time, the pot was rotated at 200 rpm for 15 minutes, and then the rotation was stopped for 5 minutes, and this operation was repeated 40 times. Next, the crushed raw material was dried to obtain a positive electrode composite material.

[0057] The weighing and crushing of the raw materials were carried out in a purged (DBO type) glove box (manufactured by Miwa Seisakusho) to prevent moisture absorption by the fluoride and oxidation of the copper.

[0058] FIG. 4 shows an SEM image and element mapping of the positive electrode composite.

[0059] From FIG. 4, it can be seen that the primary particle diameter of copper and bismuth is 10 nm or more and 500 nm or less, and that they are composited.

[0060] Figure 5 shows the XRD spectrum of the positive electrode composite. 0.06 Bi 0.94 F 2.88The XRD spectra of BiF3 and Bi2O3 are also shown. The X-ray energy used for measuring the XRD spectra was 25 keV (λ=0.496 Å).

[0061] As can be seen from FIG. 5, the positive electrode mixture does not contain BiF3 and is made of K with a hexagonal structure. 0.06 Bi 0.94 F 2.88 It can be seen that it includes.

[0062] [Example 2] Copper (manufactured by High Purity Chemical Laboratory), Bismuth (manufactured by High Purity Chemical Laboratory), K 0.06 Bi 0.94 F 2.88 A positive electrode mixture was obtained in the same manner as in Example 1, except that the powdered tantalum oxide and acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) were weighed out so that the mass ratio was 53.2:17.8:26.8:2.2.

[0063] [Example 3] Copper (manufactured by High Purity Chemical Laboratory), Bismuth (manufactured by High Purity Chemical Laboratory), K 0.06 Bi 0.94 F 2.88 , Ce 0.92 Sr 0.08 F 2.92 A positive electrode mixture was obtained in the same manner as in Example 1, except that the powdered tantalum oxide and acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) were weighed out so that the mass ratio was 53.2:17.8:14.4:12.4:2.2.

[0064] [Example 4] Copper (manufactured by High Purity Chemical Laboratory), Bismuth (manufactured by High Purity Chemical Laboratory), K 0.06 Bi 0.94 F 2.88 and acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) were weighed out to give a mass ratio of 37.3:29.3:31.2:2.2, and then premixed for about 1 hour using an agate mortar and pestle to obtain a raw material mixed powder.

[0065] The obtained raw material mixed powder was classified using a stainless steel mesh with 500 μm openings. Next, the raw material mixed powder that did not pass through the mesh was mixed using an agate mortar and pestle and then classified, and this operation was repeated until all the raw material mixed powder passed through the mesh.

[0066] The weighing, pre-mixing and classification of the raw materials were carried out in a purged (DBO type) glove box (manufactured by Miwa Seisakusho) to prevent moisture absorption of the fluoride and oxidation of the copper.

[0067] The sealed powder hopper containing the classified raw material mixed powder was removed from the glove box and connected to a high-frequency induction thermal plasma nanoparticle synthesis device TP-40020NPS (manufactured by JEOL Ltd.). Next, argon gas was supplied to the plasma torch, and the raw material mixed powder was melted by thermal plasma to form a raw material melt, which was then sprayed into a chamber in a reduced pressure environment. The raw material melt sprayed into the chamber was cooled and turned into nanoparticles, producing composites (Cu-Bi), K 0.06 Bi 0.94 F 2.88 The positive electrode mixture was collected using an exhaust filter, and the positive electrode mixture was then transported into a glove box with the upstream and downstream of the exhaust filter blocked off using valves, and the positive electrode mixture was collected.

[0068] [Example 5] K 0.06 Bi 0.94 F 2.88 Instead of Ce 0.92 Sr 0.08 F 2.92 A positive electrode mixture was obtained in the same manner as in Example 1, except that the above was used.

[0069] [Comparative Example 1] A positive electrode mixture was obtained in the same manner as in Example 5, except that bismuth (manufactured by Kojundo Chemical Laboratory) was used instead of copper (manufactured by Kojundo Chemical Laboratory).

[0070] [Fabrication of fluoride ion secondary battery] The positive electrode mixtures of Examples 1 to 5 and Comparative Example 1 were used to fabricate fluoride ion secondary batteries.

[0071] PbSnF4 as the negative electrode active material and acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd.) as the conductive additive were mixed in a mass ratio of 70:5 to obtain a negative electrode mixture.

[0072] The cell was fabricated using an alumina tube with an inner diameter of 10 mm. 0.95 Sr 0.05 F 2.85 A pressure of 740 MPa was applied to 150 mg of the solid electrolyte layer to form a solid electrolyte layer. Next, 10 mg of the positive electrode composite and gold foil as a positive electrode current collector were placed on one side of the solid electrolyte layer, and 20 mg of the negative electrode composite and aluminum foil as a negative electrode current collector were placed on the other side of the solid electrolyte layer, and then the mixture was uniaxially pressed at a pressure of 185 MPa to obtain a cell. Next, the cell was sealed in a sealed glass container with a confining pressure of about 340 MPa applied.

[0073] [Charge / discharge capacity] The inside of the glass container was depressurized by a vacuum pump, and a constant current charge / discharge test of the cell was performed at a cell temperature of 140°C. Specifically, using a potentio / galvanostat SI1287 / 1255B (manufactured by Solartron), the cell was charged at a current value of 120μA until the voltage reached 1.5V (vs. Pb / PbF2), and then charged again at a current value of 40μA until the voltage reached 1.5V. Next, the cell was discharged at a current value of 120μA until the voltage reached -0.5V, and then discharged again at a current value of 40μA until the voltage reached -0.5V. At this time, in order to control the cell temperature during charging and discharging, the cell was placed in a small environmental tester SU261 (manufactured by Espec) and a constant current charge / discharge test was performed.

[0074] FIG. 6 shows the charge / discharge curves of the cell of Example 3.

[0075] The evaluation results of the cell discharge capacity per unit mass of the positive electrode mixture layer are shown in Table 1. In Table 1, AB means acetylene black.

[0076] [Table 1]

[0077] It can be seen from Table 1 that the discharge capacity per unit mass of the positive electrode mixture layer is high in the cells of Examples 1 to 5. In contrast, the discharge capacity per unit mass of the positive electrode mixture layer in the cell of Comparative Example 1 is low because the positive electrode mixture layer does not contain the first active material.

Claims

1. A positive electrode mixture layer is formed on the positive electrode current collector, the positive electrode mixture layer includes a first active material not containing fluorine and a second active material not containing fluorine, and a molar ratio of the first active material to the second active material is 4 or more and 35 or less; The first active material has a higher fluorination potential than the second active material.

2. The positive electrode of claim 1 , wherein the first active material and the second active material are composited.

3. The positive electrode mixture layer further includes a third active material containing fluorine, The positive electrode according to claim 1 , wherein the third active material has a higher fluoride ion conductivity than the fluoride of the second active material.

4. the first active material is copper; the second active material is bismuth; The third active material is represented by the general formula K x Bi 1-x F 3-2x (In the formula, x is 0.02 or more and 0.12 or less.) The positive electrode according to claim 3 , which is a compound having a hexagonal structure and represented by the following formula:

5. The first active material has a primary particle diameter of 10 nm or more and 500 nm or less, The second active material has a primary particle diameter of 10 nm or more and 500 nm or less, The positive electrode according to claim 3 , wherein the third active material has a primary particle diameter of 10 nm or more and 200 nm or less.

6. The positive electrode according to claim 1 or 2, wherein the positive electrode mixture layer further comprises a solid electrolyte containing fluorine.

7. 7. The positive electrode of claim 6, wherein the solid electrolyte is a metal fluoride containing cerium and strontium.

8. A fluoride ion secondary battery comprising the positive electrode according to claim 1 or 2.

Citation Information

Patent Citations

  • Nonaqueous electrolyte battery

    JP1980111067A

  • Positive electrode active material and fluoride ion battery

    JP2019200852A

  • Fluoride ion battery and manufacturing method thereof

    JP2022178410A

  • Positive electrode active material for fluoride ion secondary batteries, positive electrode using said active material, fluoride ion secondary battery, and method for producing said active material

    WO2019187942A1