Method for producing liquid crystalline resin
By incorporating specific metal compounds in the polycondensation and acylation processes, the method enhances reaction rates, leading to more efficient production of liquid crystal resins.
Patent Information
- Application Number
- JP2023048319
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
The slow reaction rates in the acylation and subsequent solid phase polymerization of raw material monomers for liquid crystal resins lead to decreased productivity.
A method involving the use of specific metal compounds, including those from Group 3 of the periodic table and alkali metals or alkaline earth metals, in the polycondensation and acylation processes to enhance the reaction rates.
This approach significantly increases the reaction rates, allowing for more efficient production of liquid crystal resins with improved properties.
Smart Images

Figure 2024136991000001 
Figure 2024136991000002 
Figure 2024136991000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a liquid crystalline resin. [Background technology]
[0002] Liquid crystalline resins, typified by liquid crystalline polyester resins and liquid crystalline polyesteramide resins, have a good balance of excellent fluidity, mechanical strength, heat resistance, chemical resistance, electrical properties, etc., and are therefore suitably used widely as high-performance engineering plastics. Known methods for producing liquid crystal resins include a method of melt-polymerizing raw material monomers and further solid-phase polymerizing them as necessary to obtain a liquid crystal resin, and a method of melt-polymerizing raw material monomers to generate oligomers and then solid-phase polymerizing the oligomers to obtain a liquid crystal resin. For example, Patent Document 1 proposes a method of obtaining liquid crystal polyesters by two-stage polymerization of prepolymer melt polymerization and solid-phase polymerization. Before melt polymerization, the phenolic hydroxyl group or amino group of the raw material monomer may be acylated as necessary. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2001-139674 A Summary of the Invention [Problem to be solved by the invention]
[0004] If the reaction rates are slow in the acylation of the raw material monomers, the melt polymerization, and the subsequent solid-phase polymerization, the productivity decreases.
[0005] An object of the present disclosure is to provide a method for producing a liquid crystalline resin having a reaction rate improved compared to conventional methods. [Means for solving the problem]
[0006] The present disclosure has the following aspects. [1] A method for producing a liquid crystal resin, comprising: subjecting a raw material monomer containing one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof to a polycondensation reaction in the presence of at least one first metal compound containing one or more metal atoms (a) selected from Group 3 of the periodic table, and at least one second metal compound containing one or more metal atoms (b) selected from the group consisting of alkali metals, alkaline earth metals, and magnesium. [2] A method for producing a liquid crystalline resin according to [1], comprising, prior to the polycondensation reaction, acylation of the raw material monomer in the presence of at least one first metal compound containing one or more metal atoms (a) selected from Group 3 of the Periodic Table and at least one second metal compound containing one or more metal atoms (b) selected from the group consisting of alkali metals, alkaline earth metals and magnesium. [3] A method for producing a liquid crystalline resin according to [1] or [2], comprising solid-phase polymerizing the reaction product obtained by the polycondensation reaction in the presence of at least one first metal compound containing one or more metal atoms (a) selected from Group 3 of the Periodic Table, and at least one second metal compound containing one or more metal atoms (b) selected from the group consisting of alkali metals, alkaline earth metals and magnesium. [4] The method for producing a liquid crystalline resin according to any one of [1] to [3], wherein the first metal compound contains one or more selected from the group consisting of acetates, carbonates, oxides, hydroxides and chlorides of the metal atom (a). [5] The method for producing a liquid crystalline resin according to any one of [1] to [4], wherein the second metal compound contains at least one selected from the group consisting of acetates, carbonates, oxides, hydroxides and chlorides of the metal atom (b). Effect of the Invention
[0007] According to the present disclosure, it is possible to provide a method for producing a liquid crystalline resin with a reaction rate improved compared to conventional methods. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present disclosure will be described in detail, but the scope of the present disclosure is not limited to the embodiment described here, and various modifications can be made within the scope of the present disclosure. In addition, when multiple numerical ranges are described for a specific parameter, any numerical values described therein can be combined to form a suitable numerical range. In addition, the lower limit and / or upper limit of the numerical range described in this disclosure is a numerical value within that numerical range, and may be replaced with a numerical value shown in the examples. The expression "X to Y" indicating a numerical range means "X or more and Y or less". When a specific description described for one embodiment is also applicable to other embodiments, the description may be omitted in other embodiments.
[0009] [Method of manufacturing liquid crystal resin] The method for producing a liquid crystal resin according to the present embodiment includes polycondensing a raw material monomer (hereinafter, also simply referred to as "raw material monomer") containing one or more selected from the group consisting of aromatic hydroxycarboxylic acids and their polymerizable derivatives, in the presence of at least one first metal compound (hereinafter, also simply referred to as "first metal compound") containing one or more metal atoms (a) (hereinafter, also simply referred to as "metal atom (a)") selected from Group 3 of the periodic table, and at least one second metal compound (hereinafter, also simply referred to as "second metal compound") containing one or more metal atoms (b) (hereinafter, also simply referred to as "metal atom (b)") selected from the group consisting of alkali metals, alkaline earth metals, and magnesium. By polycondensing the raw material monomer in the presence of the first metal compound and the second metal compound, the time required to reach a predetermined final torque can be made shorter than in the past. As a result, the polycondensation reaction rate can be increased.
[0010] "Liquid crystallinity" refers to the property of being capable of forming an optically anisotropic molten phase. The property of an anisotropic molten phase can be confirmed by a conventional polarized light inspection method using crossed polarizers. More specifically, the anisotropic molten phase can be confirmed by observing a molten sample placed on a Leitz hot stage at a magnification of 40 times under a nitrogen atmosphere using a Leitz polarizing microscope. When a resin having liquid crystallinity is inspected between crossed polarizers, polarized light is usually transmitted even when the resin is in a molten, stationary state, and the resin is optically anisotropic.
[0011] <Raw material monomer> The raw material monomer includes one or more compounds selected from the group consisting of aromatic hydroxycarboxylic acids and their polymerizable derivatives. In the present disclosure, the term "polymerizable derivative" refers to a compound that can be polymerized by melt polymerization among compounds whose molecular structure has been partially changed. Examples of the compound include acylated compounds in which a phenolic hydroxyl group and / or an amino group is acylated with an acylating agent, halides in which one or more hydrogen atoms of an aromatic hydrocarbon group are substituted with halogen atoms, acid halides in which a carboxyl group is halogenated with a halogenating agent, acid anhydrides, and alkyl esters (having about 1 to 4 carbon atoms).
[0012] The aromatic hydroxycarboxylic acid and its polymerizable derivative are not particularly limited, and examples thereof include 4-hydroxybenzoic acid (HBA), 6-hydroxy-2-naphthoic acid (HNA), 3-hydroxybenzoic acid, 6-hydroxy-3-naphthoic acid, 6-hydroxy-4-naphthoic acid, 4-hydroxy-4'-carboxydiphenyl ether, 2,6-dichloro-p-hydroxybenzoic acid, 2-chloro-p-hydroxybenzoic acid, 2,6-dimethyl-p-hydroxybenzoic acid, 2,6-difluoro-p-hydroxybenzoic acid, 4-hydroxy-4'-biphenyl carboxylic acid, vanillic acid, and the like. At least one compound selected from these can be used. Among them, it is preferable to use at least one selected from 4-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid in terms of availability.
[0013] The content of the aromatic hydroxycarboxylic acid and its polymerizable derivative is preferably 40 to 70 mol %, more preferably 55 to 65 mol %, based on the total amount of raw material monomers.
[0014] In one embodiment, one or more of the raw material monomers may be an acylated product in which a phenolic hydroxyl group and / or an amino group is acylated with an acylation agent. The acylation reaction will be described later.
[0015] It is preferable that the raw material monomer further satisfies the following (1) or (2). (1) containing at least one compound selected from the group consisting of aromatic or alicyclic dicarboxylic acids and polymerizable derivatives thereof, or (2) At least one compound selected from the group consisting of aromatic or alicyclic dicarboxylic acids and polymerizable derivatives thereof, and at least one compound selected from the group consisting of aromatic or alicyclic diols, aromatic or alicyclic hydroxyamines, aromatic or alicyclic diamines, and polymerizable derivatives thereof.
[0016] The aromatic dicarboxylic acid is not particularly limited, and examples thereof include terephthalic acid (TA), isophthalic acid, 4,4'-diphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and compounds represented by the following general formula (I). General formula (I): TIFF2024136991000001.tif22170(Y:-(CH2) n -(n=1 to 4) and -O(CH2) n O-(n=1 to 4).
[0017] The alicyclic dicarboxylic acid is not particularly limited, and examples thereof include 1,4-cyclohexanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, etc. The polymerizable derivative is not particularly limited, and examples thereof include alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.
[0018] The total content of at least one compound selected from the group consisting of aromatic or alicyclic dicarboxylic acids and polymerizable derivatives thereof is preferably 5 to 50 mol %, more preferably 15 to 25 mol %, based on the total amount of raw material monomers.
[0019] The aromatic diol is not particularly limited, and examples thereof include 2,6-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 4,4'-dihydroxybiphenyl (BP), hydroquinone, resorcinol, a compound represented by the following general formula (II), and a compound represented by the following general formula (III).
[0020] General formula (II): TIFF2024136991000002.tif23170 (X is a group selected from alkylene (C1 to C4), alkylidene, -O-, -SO-, -SO2-, -S-, and -CO-.)
[0021] General formula (III): TIFF2024136991000003.tif26170
[0022] The alicyclic diol is not particularly limited, and examples thereof include 1,4-cyclohexanedimethanol, 1,4-cyclohexanediol, etc. The polymerizable derivative is not particularly limited, and examples thereof include alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.
[0023] The aromatic hydroxyamine is not particularly limited, and examples thereof include N-acetyl-p-aminophenol (APAP), 4-aminophenol, 3-aminophenol, etc. The alicyclic hydroxyamine is not particularly limited, and examples thereof include 4-aminocyclohexanol, 3-aminocyclopentanol, etc. The polymerizable derivative is not particularly limited, and examples thereof include alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.
[0024] Examples of aromatic diamines include 1,4-phenylenediamine, etc. Examples of alicyclic diamines include, but are not limited to, 1,4-cyclohexanediamine, 1,3-cyclopentanediamine, etc. Examples of polymerizable derivatives include, but are not limited to, alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.
[0025] The total content of at least one compound selected from the group consisting of aromatic or alicyclic diols, aromatic or alicyclic hydroxyamines, aromatic or alicyclic diamines, and polymerizable derivatives thereof is preferably 5 to 50 mol %, and more preferably 15 to 25 mol %, based on the total amount of raw material monomers.
[0026] Specific examples of the combination of raw material monomers include: (I) (Ia) comprises at least one compound selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof (preferably, consists of only at least one compound selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof); (II) (IIa) at least one compound selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof, (IIb) at least one compound selected from the group consisting of aromatic or alicyclic dicarboxylic acids and polymerizable derivatives thereof, and (IIc) at least one compound selected from the group consisting of aromatic or alicyclic diols, aromatic hydroxyamines, aromatic diamines, and polymerizable derivatives thereof (preferably consisting only of the above compound (IIa), compound (IIb), and compound (IIc)); The above-mentioned components may be used in combination with a molecular weight regulator, if necessary.
[0027] <First metal compound> The first metal compound contains one or more metal atoms (a) selected from Group 3 of the periodic table. The first metal compound may be one type, or two or more types may be used in combination.
[0028] Examples of the metal atom (a) include scandium, yttrium, and lanthanoid atoms (lanthanum, cerium, samarium, europium, gadolinium, terbium, ytterbium, and lutetium).
[0029] In one embodiment, the first metal compound preferably contains one or more metal atoms (a) selected from scandium, yttrium, lanthanum, cerium, samarium, europium, gadolinium, terbium, ytterbium, and lutetium, more preferably contains one or more metal atoms (a) selected from scandium, yttrium, lanthanum, cerium, samarium, and ytterbium, and further preferably contains one or more metal atoms (a) selected from lanthanum, cerium, and samarium. In one embodiment, the first metal compound can contain lanthanum.
[0030] In one embodiment, the first metal compound preferably contains one or more selected from the group consisting of acetates, carbonates, oxides, hydroxides and chlorides of the metal atom (a), and more preferably contains one or more selected from the group consisting of acetates and oxides of the metal atom (a). In the case of a compound that generates a hydrate, it may be an anhydride or a hydrate.
[0031] Examples of acetates of the metal atom (a) include scandium acetate, yttrium acetate, lanthanum acetate, cerium acetate, samarium acetate, europium acetate, gadolinium acetate, terbium acetate, ytterbium acetate, and lutetium acetate. Examples of the carbonate of the metal atom (a) include scandium carbonate, yttrium carbonate, lanthanum carbonate, cerium carbonate, samarium carbonate, europium carbonate, gadolinium carbonate, terbium carbonate, ytterbium carbonate, and lutetium carbonate. Examples of the oxide of the metal atom (a) include scandium oxide, yttrium oxide, lanthanum oxide, cerium oxide, samarium oxide, terbium oxide, ytterbium oxide, and lutetium oxide. Examples of the hydroxide of the metal atom (a) include scandium hydroxide, yttrium hydroxide, lanthanum hydroxide, cerium hydroxide, samarium hydroxide, ytterbium hydroxide, and lutetium hydroxide. Examples of the chloride of the metal atom (a) include scandium chloride, yttrium chloride, lanthanum chloride, cerium chloride, samarium chloride, terbium chloride, dysprosium chloride, ytterbium chloride, and lutetium chloride.
[0032] The amount of the first metal compound used is preferably 0.001 to 0.2 mol %, more preferably 0.005 to 0.05 mol %, and even more preferably 0.005 to 0.01 mol %, based on the total amount of raw material monomers.
[0033] <Second metal compound> The second metal compound contains one or more metal atoms (b) selected from the group consisting of alkali metals, alkaline earth metals, and magnesium. The second metal compound may be used alone or in combination of two or more kinds.
[0034] Examples of the metal atom (b) include alkali metal atoms such as lithium, sodium, potassium, rubidium, cesium, and francium; alkaline earth metal atoms such as calcium, strontium, barium, and radium; and magnesium. In one embodiment, the metal atom (b) is preferably one or more selected from the group consisting of sodium, potassium, rubidium, cesium, calcium, strontium, barium, and magnesium, more preferably one or more selected from the group consisting of potassium, rubidium, cesium, and magnesium, and even more preferably one or more selected from the group consisting of potassium and cesium. In one embodiment, the second metal compound can include potassium. In another embodiment, the second metal compound can include cesium.
[0035] In one embodiment, the second metal compound preferably contains one or more selected from the group consisting of acetates, carbonates, oxides, hydroxides and chlorides of the metal atom (b), and more preferably contains one or more selected from the group consisting of acetates and carbonates of the metal atom (b). In the case of a compound that generates a hydrate, it may be an anhydride or a hydrate.
[0036] Examples of acetates of the metal atom (b) include lithium acetate, sodium acetate, potassium acetate, rubidium acetate, cesium acetate, calcium acetate, strontium acetate, barium acetate, and magnesium acetate. Examples of the carbonate of the metal atom (b) include lithium carbonate, sodium carbonate, potassium carbonate, rubidium carbonate, cesium carbonate; calcium carbonate, strontium carbonate, barium carbonate, radium carbonate; magnesium carbonate, and the like. Examples of the oxide of the metal atom (b) include lithium oxide, sodium oxide, potassium oxide, rubidium oxide, cesium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and the like. Examples of the hydroxide of the metal atom (b) include lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide, francium hydroxide; calcium hydroxide, strontium hydroxide, barium hydroxide, radium hydroxide; magnesium hydroxide, and the like. Examples of the chloride of the metal atom (b) include lithium chloride, sodium chloride, potassium chloride, rubidium chloride, cesium chloride; calcium chloride, strontium chloride, barium chloride, radium chloride; magnesium chloride, and the like.
[0037] The amount of the second metal compound used is preferably 0.001 to 0.2 mol %, more preferably 0.005 to 0.05 mol %, and even more preferably 0.005 to 0.01 mol %, based on the total amount of raw material monomers.
[0038] <Combination of first metal compound and second metal compound> The combination of the first metal compound and the second metal compound is not limited, and may be any of the following: a combination of a first metal compound containing one or more metal atoms selected from Group 3 of the periodic table and a second metal compound containing an alkali metal; a combination of a first metal compound containing one or more metal atoms selected from Group 3 of the periodic table and a second metal compound containing an alkaline earth metal; or a combination of a first metal compound containing one or more metal atoms selected from Group 3 of the periodic table and a second metal compound containing magnesium; and any one or more first metal compounds can be combined with any one or more second metal compounds. Although specific examples of combinations of the first metal compound and the second metal compound are not limited, preferably, the first metal compound contains one or more metal atoms (a) selected from scandium, yttrium, lanthanum, cerium, samarium, europium, gadolinium, terbium, ytterbium, and lutetium, and the second metal compound contains one or more metal atoms (b) selected from the group consisting of sodium, potassium, rubidium, cesium, calcium, strontium, barium, and magnesium. One or more first metal compounds selected from these can be combined with one or more second metal compounds. In one embodiment, the first metal compound preferably contains one or more metal atoms (a) selected from scandium, yttrium, lanthanum, cerium, samarium, and ytterbium, and the second metal compound preferably contains one or more metal atoms (b) selected from the group consisting of potassium, rubidium, cesium, and magnesium. One or more first metal compounds selected from these can be combined with one or more second metal compounds.
[0039] In one embodiment, the first metal compound can include lanthanum and the second metal compound can include potassium and / or cesium. In one embodiment, the first metal compound may include an acetate, carbonate, oxide, hydroxide, or chloride of lanthanum, and the second metal compound may include an acetate, carbonate, oxide, hydroxide, or chloride of potassium and / or cesium. In one embodiment, the first metal compound may include one or more selected from lanthanum acetate and lanthanum oxide, and the second metal compound may include one or more selected from potassium acetate, cesium acetate, and cesium carbonate.
[0040] The total amount of the first metal compound and the second metal compound used is preferably 0.002 to 0.4 mol %, more preferably 0.01 to 0.1 mol %, and even more preferably 0.01 to 0.02 mol %, based on the total amount of raw material monomers. The ratio of the amount of the first metal compound to the amount of the second metal compound used (amount of the first metal compound used / amount of the second metal compound used) is preferably 0.1 to 10, more preferably 0.5 to 5, even more preferably 0.8 to 1.2, and particularly preferably 0.9 to 1.1.
[0041] <Polycondensation reaction process (melt polymerization process)> In the polycondensation reaction step, raw material monomers containing at least one selected from the group consisting of aromatic hydroxycarboxylic acids and their polymerizable derivatives are polycondensed. The polycondensation reaction is carried out by melt polymerization. A liquid crystal resin is obtained by polycondensing the raw material monomers.
[0042] The polycondensation temperature is, for example, preferably 200 to 400° C., and more preferably 240 to 380° C. The polycondensation reaction time is preferably 2 to 12 hours, more preferably 3 to 10 hours, and further preferably 4 to 7 hours.
[0043] In one embodiment, the polycondensation reaction is preferably carried out by starting decompression after the reaction system has reached a predetermined temperature, and then setting the pressure reduction level to a predetermined level. In one embodiment, the polycondensation reaction is preferably carried out under a reduced pressure of 10,000 to 133 Pa (preferably 5,000 to 1,330 Pa). In another embodiment, the polycondensation reaction is preferably carried out under normal pressure (1.013×10 5 When the polycondensation reaction is carried out under normal pressure, an oligomer (having a weight average molecular weight of less than 50,000) of the raw material monomer is obtained.
[0044] The liquid crystal resin obtained by the polycondensation reaction can be further subjected to solid-phase polymerization to increase the molecular weight, as described later.
[0045] The liquid crystal resin obtained in the polycondensation reaction step preferably has a weight average molecular weight of at least 50,000, more preferably at least 70,000. The weight average molecular weight is a value calculated by analysis using gel permeation chromatography.
[0046] <Acylation step> In one embodiment, the method for producing a liquid crystal resin may include acylation of a raw material monomer in the presence of the first metal compound and the second metal compound before the polycondensation reaction. The first metal compound and the second metal compound are as described above. By acylation of a raw material monomer in the presence of the first metal compound and the second metal compound, the acylation rate can be increased in a shorter time than in conventional methods. As a result, a method for producing a liquid crystal resin with a higher reaction rate than conventional methods can be achieved.
[0047] The first metal compound and the second metal compound used in the acylation step may be the same as or different from the first metal compound and the second metal compound used in the polycondensation reaction step. In one embodiment, when the polycondensation reaction step is carried out following the acylation step, the first metal compound and the second metal compound used in the acylation step can be used in the polycondensation reaction step.
[0048] Examples of the acylating agent include, but are not limited to, acetic anhydride, propionic anhydride, butyric anhydride, isobutyric anhydride, valeric anhydride, pivalic anhydride, 2-ethylhexanoic anhydride, monochloroacetic anhydride, dichloroacetic anhydride, trichloroacetic anhydride, monobromoacetic anhydride, dibromoacetic anhydride, tribromoacetic anhydride, monofluoroacetic anhydride, difluoroacetic anhydride, trifluoroacetic anhydride, glutaric anhydride, maleic anhydride, succinic anhydride, and β-bromopropionic anhydride. At least one selected from these can be used. Examples of suitable acylating agents from the viewpoint of cost and ease of handling include carboxylic anhydrides such as acetic anhydride, propionic anhydride, butyric anhydride, and isobutyric anhydride. Among these, acetic anhydride is preferred from the viewpoint of ease of availability. The amount of the acylating agent used is preferably 1.0 to 1.1 equivalents, more preferably 1.01 to 1.05 equivalents, based on the total amount of hydroxyl groups of the substances used in the reaction from the viewpoint of ease of reaction control.
[0049] The acylation can be carried out by a known method, for example, by mixing the raw material monomer with an acylating agent and heating at a temperature range of 120 to 160° C. for about 0.5 to 5 hours to carry out the acylation reaction, thereby obtaining a reaction product containing an acylated compound.
[0050] <Solid phase polymerization process> In one embodiment, the method for producing a liquid crystal resin may include solid-phase polymerization of a reaction product obtained by polycondensation in the presence of the first metal compound and the second metal compound. The molecular weight of the raw material resin can be increased by solid-phase polymerization, and a liquid crystal resin having excellent strength and heat resistance can be obtained. The first metal compound and the second metal compound are as described above. The molecular weight can be increased in a short time by solid-phase polymerization in the presence of the first metal compound and the second metal compound. As a result, the solid-phase polymerization rate can be increased compared to conventional methods.
[0051] The reaction product obtained by the polycondensation reaction contains a first metal compound and a second metal compound, and therefore the first metal compound and the second metal compound used in the solid-state polymerization step may be the same type as the first metal compound and the second metal compound used in the polycondensation reaction step.
[0052] The solid-phase polymerization can be carried out by a conventional method. For example, the solid-phase polymerization can be carried out by heating the raw material resin (resin obtained in the polycondensation step) at a temperature 10 to 120°C lower than the liquid crystal formation temperature of the raw material resin (resin obtained in the polycondensation step) under reduced pressure or vacuum in an inert gas stream such as nitrogen gas. Since the melting point of the liquid crystal resin increases as the solid-phase polymerization proceeds, it is also possible to carry out the solid-phase polymerization at a temperature equal to or higher than the original melting point of the raw material resin. The solid-phase polymerization can be carried out at a constant temperature or can be increased stepwise. The heating method is not particularly limited, and microwave heating, heater heating, etc. can be used.
[0053] [Liquid crystal resin] The liquid crystal resin obtained by the method for producing a liquid crystal resin according to the present embodiment preferably contains at least one selected from liquid crystal polyesters and liquid crystal polyesteramides. The liquid crystal polyesters and liquid crystal polyesteramides are not particularly limited, but are preferably aromatic polyesters or aromatic polyesteramides. In addition, polyesters that partially contain aromatic polyesters or aromatic polyesteramides in the same molecular chain may also be used. In one embodiment, the liquid crystal resin obtained preferably contains one or more selected from fully aromatic polyesters and fully aromatic polyesteramides. "Fully aromatic" means that all raw material monomers have aromatic rings.
[0054] The aromatic polyester or aromatic polyester amide contains at least a structural unit derived from an aromatic hydroxycarboxylic acid or a polymerizable derivative thereof, and more specifically, (1) (1a) polyesters consisting essentially of one or more aromatic hydroxycarboxylic acids and their derivatives; (2) polyesters consisting essentially of (2a) one or more aromatic hydroxycarboxylic acids and their derivatives, and (2b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives; (3) polyesters consisting essentially of (3a) one or more aromatic hydroxycarboxylic acids and their derivatives, (3b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives, and (3c) one or more aromatic diols, alicyclic diols, aliphatic diols, and their derivatives; (4) polyesteramides consisting essentially of (4a) one or more aromatic hydroxycarboxylic acids and their derivatives, (4c1) one or more aromatic hydroxyamines, aromatic diamines, and their derivatives, and (4c2) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives; (5) polyesteramides mainly composed of (5a) one or more aromatic hydroxycarboxylic acids and their derivatives, (5b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives, (5c1) one or more aromatic hydroxyamines, aromatic diamines, and their derivatives, and (5c2) one or more aromatic diols, alicyclic diols, and their derivatives.
[0055] The molecular weight (weight average molecular weight Mw) of the liquid crystal resin is not particularly limited, and for the resin obtained in the polycondensation reaction (melt polymerization) step, it is preferably 50,000 to 500,000, more preferably 75,000 to 400,000. For the resin obtained in the solid phase polymerization step, it is preferably 60,000 to 600,000, more preferably 75,000 to 500,000. The weight average molecular weight Mw can be calculated by analysis using gel permeation chromatography.
[0056] The melting point of the liquid crystal resin is not particularly limited and can be 250 to 380° C. The melt viscosity of the liquid crystal resin is not particularly limited and the resin obtained in the polycondensation reaction (melt polymerization) step can be obtained at a cylinder temperature 10 to 30° C. higher than the melting point of the liquid crystal resin and a shear rate of 1000 sec -1 The melt viscosity measured at a shear rate of 1000 sec is preferably 5 Pa·s or more and 150 Pa·s or less, more preferably 10 Pa·s or more and 100 Pa·s or less. Furthermore, when the solid-state polymerization step is performed, the resin is polymerized at a cylinder temperature 10 to 30°C higher than the melting point of the liquid crystal resin and at a shear rate of 1000 sec -1The melt viscosity measured by is preferably 5 Pa·s or more and 200 Pa·s or less, more preferably 10 Pa·s or more and 150 Pa·s or less. "Cylinder temperature 10 to 30°C higher than the melting point of the liquid crystal resin" means a cylinder temperature at which the liquid crystal resin can be melted to a degree at which the melt viscosity can be measured, and the cylinder temperature higher than the melting point varies depending on the type of raw material resin within the range of 10 to 30°C. The liquid crystal resin can be in the form of a powder / granule mixture, or in the form of a molten mixture (melt-kneaded product) such as pellets. In the present disclosure, the melt viscosity refers to the melt viscosity measured in accordance with ISO11443. EXAMPLES
[0057] The present disclosure will be described in more detail below by showing examples, but interpretation of the present disclosure is not limited to these examples.
[0058] [Example 1] After the following raw materials were charged into a polymerization vessel, the temperature of the reaction system was raised to 140°C and the reaction was carried out at 140°C for 3 hours (acylation reaction). The acylation rate (acetylation rate) was calculated as follows. The results are shown in Table 1.
[0059] [Acylation (acetylation) rate] After the acylation reaction, 10 mg of the sample was dissolved in 0.5 mL of DMSO-d6. The resulting solution was analyzed using a nuclear magnetic resonance device (AVANCEIII400 manufactured by Bruker). 1 H-NMR measurement was performed to obtain the integral values of the aromatic ring 3-position proton of the unreacted monomer and the aromatic ring 3-position proton of the acylated (acetylated) monomer, and the acylation (acetylation) rate was calculated using the following formula. Acetylation rate = [(proton integral value of acetylated monomer) / ((proton integral value of unreacted monomer)+(proton integral value of acetylated monomer))] × 100 Thereafter, the temperature was further increased to 340°C over 4.5 hours, and the pressure was then reduced to 10 Torr (i.e., 1330 Pa) over 15 minutes, and polycondensation was carried out while distilling off acetic acid, excess acetic anhydride, and other low boiling points (polycondensation step). After the stirring torque reached a predetermined value (0.7 V), nitrogen was introduced to change the pressure from reduced pressure to normal pressure and then to pressurized state, and the polymer was discharged from the bottom of the polymerization vessel. The strands were then pelletized to obtain liquid crystalline resin pellets. The time required from the start of pressure reduction until the stirring torque reached a predetermined value (0.7 V) (time to final torque) was measured. The results are shown in Table 1. The weight average molecular weight (Mw) of the obtained liquid crystalline resin pellets was calculated as follows and was 131,000 (prepolymer). (raw materials) 4-Hydroxybenzoic acid (HBA): 188.3 g (60 mol%) 6-Hydroxy-2-naphthoic acid (HNA): 21.4 g (5 mol%) Terephthalic acid (TA): 66.0 g (17.5 mol%) 4,4'-Dihydroxybiphenyl (BP): 52.9 g (12.5 mol%) N-acetyl-p-aminophenol (APAP): 17.2 g (5 mol%) Lanthanum acetate sesquihydrate (La(OAc)3·1.5H2O): 51.5 mg (0.0068 mol%) Potassium acetate (KOAc): 14.7 mg (0.0068 mol%) Acylating agent (acetic anhydride): 226.9g
[0060] [Weight average molecular weight (Mw)] The obtained liquid crystal resin was dissolved in 3,5-bistrifluoromethylphenol as a solvent by stirring at room temperature for 6 hours. The solution was analyzed by gel permeation chromatography (Tosoh Corporation, "HLC-8320GPC", differential refractometer detector) to calculate the weight average molecular weight (Mw) in terms of standard polystyrene.
[0061] The obtained liquid crystal resin pellets (prepolymer) were subjected to solid phase polymerization as follows. In a solid-phase polymerization vessel equipped with a nitrogen inlet / outlet, 10 g of the liquid crystal resin pellets (prepolymer) obtained above was charged and placed under a nitrogen atmosphere. The reaction system was heated to 295°C and reacted for 2 hours (solid-phase polymerization step). The temperature was then lowered to room temperature and the liquid crystal resin pellets were taken out. The weight-average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 172,000. The solid-state polymerization rate was calculated as follows, and the results are shown in Table 1. [Solid phase polymerization rate] The solid-state polymerization rate was calculated by dividing the difference in weight-average molecular weight (Mw) of the liquid crystal resin obtained before and after the solid-state polymerization by the solid-state polymerization time. The shear rate of the obtained liquid crystal resin was 1000 sec -1 The melt viscosity measured at a cylinder temperature of 350°C was 23 Pa·s.
[0062] [Example 2] Liquid crystal resin pellets were obtained in the same manner as in Example 1, except that 28.8 mg (0.0068 mol%) of cesium acetate (CsOAc) was used instead of potassium acetate. The acylation rate (acetylation rate) was calculated and the time to reach the final torque was measured in the same manner as in Example 1. The results are shown in Table 1. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 129,000 (prepolymer). The obtained liquid crystal resin pellets (prepolymer) were subjected to solid-phase polymerization in the same manner as in Example 1 to obtain liquid crystal resin pellets. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 242,000. The solid-phase polymerization rate was calculated in the same manner as in Example 1. The results are shown in Table 1. The shear rate of the obtained liquid crystal resin was 1000 sec -1 The melt viscosity measured at a cylinder temperature of 350°C was 21 Pa·s.
[0063] [Example 3] Liquid crystal resin pellets were obtained in the same manner as in Example 1, except that 48.9 mg (0.0068 mol%) of lanthanum oxide (La2O3) was used instead of lanthanum acetate, and 48.9 mg (0.0068 mol%) of cesium carbonate (CsCO3) was used instead of potassium acetate. The acylation rate was calculated and the time to reach the final torque was measured in the same manner as in Example 1. The results are shown in Table 1. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 123,000 (prepolymer). The obtained liquid crystal resin pellets (prepolymer) were subjected to solid-phase polymerization in the same manner as in Example 1 to obtain liquid crystal resin pellets. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 185,000. The solid-phase polymerization rate was calculated in the same manner as in Example 1. The results are shown in Table 1. The shear rate of the obtained liquid crystal resin was 1000 sec -1 The melt viscosity measured at a cylinder temperature of 350°C was 24 Pa·s.
[0064] [Comparative Example 1] Liquid crystalline resin pellets were obtained in the same manner as in Example 1, except that the first metal compound, the second metal compound and other catalysts were not used. The acylation rate (acetylation rate) was calculated and the final torque arrival time was measured in the same manner as in Example 1. The results are shown in Table 1. The weight average molecular weight (Mw) of the obtained liquid crystalline resin pellets was calculated to be 129,000 (prepolymer). The obtained liquid crystal resin pellets (prepolymer) were subjected to solid-phase polymerization in the same manner as in Example 1 to obtain liquid crystal resin pellets. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 159,000. The solid-phase polymerization rate was calculated in the same manner as in Example 1. The results are shown in Table 1. The shear rate of the obtained liquid crystal resin was 1000 sec -1 The melt viscosity measured at a cylinder temperature of 350°C was 20 Pa·s.
[0065] [Comparative Example 2] Liquid crystalline resin pellets were obtained in the same manner as in Example 1, except that only 51.5 mg (0.0068 mol%) of lanthanum acetate 1.5 hydrate was used, and potassium acetate was not used. The acylation rate was calculated and the time to reach the final torque was measured in the same manner as in Example 1. The results are shown in Table 1. The weight average molecular weight (Mw) of the obtained liquid crystalline resin pellets was calculated to be 133,000 (prepolymer). The obtained liquid crystal resin pellets (prepolymer) were subjected to solid-phase polymerization in the same manner as in Example 1 to obtain liquid crystal resin pellets. The weight average molecular weight (Mw) of the obtained liquid crystal resin pellets was calculated to be 151,000. The solid-phase polymerization rate was calculated in the same manner as in Example 1. The results are shown in Table 1. The shear rate of the obtained liquid crystal resin was 1000 sec -1 The melt viscosity measured at a cylinder temperature of 350°C was 20 Pa·s.
[0066] [Table 1]
[0067] As shown in Examples 1 to 3 in Table 1, by polycondensing raw material monomers in the presence of the first metal compound and the second metal compound, the time required to reach the final torque in the polycondensation reaction can be shortened and the polycondensation reaction rate can be increased compared to Comparative Examples 1 and 2. In addition, the acylation rate can be increased compared to Comparative Examples 1 and 2. Furthermore, the solid-phase polymerization rate can be increased compared to Comparative Examples 1 and 2. As shown in Comparative Example 2, when only one of the first metal compound and the second metal compound is used, the time to reach the final torque in the polycondensation reaction is longer than in the conventional method (Comparative Example 1), and the solid-phase polymerization rate is also lower. In Comparative Example 2, the acylation rate can be increased more than in the conventional method (Comparative Example 1), but the result is lower than in Examples 1 to 3. [Industrial Applicability]
[0068] The method for producing a liquid crystalline resin according to the present embodiment has an improved reaction rate compared to conventional methods, and therefore can produce a liquid crystalline resin efficiently, and has industrial applicability.
Claims
1. A method for producing a liquid crystal resin, comprising: subjecting a raw material monomer containing one or more selected from the group consisting of aromatic hydroxycarboxylic acids and polymerizable derivatives thereof to a polycondensation reaction in the presence of at least one first metal compound containing one or more metal atoms (a) selected from Group 3 of the Periodic Table, and at least one second metal compound containing one or more metal atoms (b) selected from the group consisting of alkali metals, alkaline earth metals, and magnesium.
2. 2. The method for producing a liquid crystalline resin according to claim 1, further comprising, prior to the polycondensation reaction, acylation of the raw material monomer in the presence of at least one first metal compound containing one or more metal atoms (a) selected from Group 3 of the Periodic Table and at least one second metal compound containing one or more metal atoms (b) selected from the group consisting of alkali metals, alkaline earth metals and magnesium.
3. 3. A method for producing a liquid crystalline resin according to claim 1 or 2, comprising solid-phase polymerizing the reaction product obtained by the polycondensation reaction in the presence of at least one first metal compound containing one or more metal atoms (a) selected from Group 3 of the Periodic Table, and at least one second metal compound containing one or more metal atoms (b) selected from the group consisting of alkali metals, alkaline earth metals and magnesium.
4. 3. The method for producing a liquid crystalline resin according to claim 1, wherein the first metal compound contains at least one selected from the group consisting of acetates, carbonates, oxides, hydroxides and chlorides of the metal atom (a).
5. 3. The method for producing a liquid crystalline resin according to claim 1, wherein the second metal compound contains at least one selected from the group consisting of acetates, carbonates, oxides, hydroxides and chlorides of the metal atom (b).
Citation Information
Patent Citations
Biodegradable polyester composite catalyst, as well as preparation method and using method thereof
CN103333328A
Thermotropic liquid crystal aromatic polyester
JP1989221420A
Biaxially oriented polyester film
JP2000309649A
Method for producing glycolic acid copolymer
JP2003113228A
Preparation process of thermotropic liquid crystalline polymer
JP2005272776A