Modified ethylene-based polymer composition and production method of the same, olefin-based polymer composition containing the same, and laminate using the same

A modified ethylene polymer composition with acrylic and fluorine-containing polymers addresses fish eyes and adhesion issues, providing improved adhesive strength and appearance in laminates and packaging.

JP2024137157AInactive Publication Date: 2024-10-07MCPP INNOVATION LLC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023048565
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing modified ethylene polymer compositions suffer from the occurrence of fish eyes and inadequate adhesion to substrates, limiting their effectiveness in applications such as packaging and containers.

Method used

Incorporating a modified ethylene polymer composition comprising an acrylic polymer and a fluorine-containing polymer, with specific structural units and content percentages, to enhance adhesion and reduce fish eyes.

Benefits of technology

The modified ethylene polymer composition exhibits reduced fish eyes and improved adhesion to substrates, resulting in enhanced adhesive strength and appearance, suitable for use in laminates and packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137157000001
    Figure 2024137157000001
Patent Text Reader

Abstract

To provide a modified ethylene-based polymer composition which brings about an excellent reduction effect of fish eye generation and exhibits high adhesiveness to a base material.SOLUTION: A modified ethylene-based polymer composition contains a modified ethylene-based polymer, an acrylic polymer and a fluorine-containing polymer, wherein the modified ethylene-based polymer is a polymer formed by modifying an ethylene-based polymer with an ethylenically unsaturated compound, the acrylic polymer contains a methyl (meth-)acrylate unit and a 2-18C alkyl (meth-)acrylate unit as constitutional units, a content of the acrylic polymer in the modified ethylene-based polymer composition is 0.05-5 mass% and a content of the fluorine-containing polymer in the modified ethylene-based polymer composition is 0.005-2 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a modified ethylene polymer composition and a production method thereof. The present invention also relates to an olefin polymer composition containing the modified ethylene polymer composition, and a laminate using the modified ethylene polymer composition. [Background technology]

[0002] Modified ethylene polymer compositions modified with ethylenically unsaturated compounds, which have excellent adhesive properties, moldability, mechanical properties, and barrier properties against oxygen gas, carbon dioxide gas, etc., have been used in various packaging and container materials, etc.

[0003] In the modified ethylene polymer composition, the amount of the ethylenically unsaturated compound added can be increased by increasing the amount of the ethylenically unsaturated compound used or the amount of the radical generator used, but a large amount of fish eyes are generated due to gelation of the modified ethylene polymer composition, etc.

[0004] In response to this, for example, Patent Document 1 discloses that the occurrence of fisheyes can be reduced by using specific polymers or compounds that constitute the modified ethylene polymer composition. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2005-036221 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the modified ethylene polymer composition disclosed in Patent Document 1 has room for improvement in terms of reducing the occurrence of fisheyes, and it is also desired to achieve better adhesion to substrates.

[0007] Therefore, an object of the present invention is to provide a modified ethylene polymer composition that exhibits a favorable effect of reducing the occurrence of fisheyes and shows high adhesion to a substrate, and a method for producing the same. Another object of the present invention is to provide an olefin polymer composition containing the modified ethylene polymer composition, and a laminate using the modified ethylene polymer composition. [Means for solving the problem]

[0008] Means for Solving the Problems The present inventors have conducted intensive studies and found that the above-mentioned problems can be solved by a modified ethylene polymer composition comprising an acrylic polymer and a fluorine-containing polymer, and by using a specific structural unit for the acrylic polymer, thereby completing the present invention. That is, the gist of the present invention is as follows.

[0009] A first aspect of the present invention is a modified ethylene-based polymer composition comprising a modified ethylene-based polymer, an acrylic polymer, and a fluorine-containing polymer, wherein the modified ethylene-based polymer is an ethylene-based polymer modified with an ethylenically unsaturated compound, the acrylic polymer is a copolymer containing, as constituent units, a methyl (meth)acrylate unit and an alkyl (meth)acrylate unit having 2 to 18 carbon atoms, and the content of the acrylic polymer in the modified ethylene-based polymer composition is 0.05 to 5 mass% and the content of the fluorine-containing polymer is 0.005 to 2 mass%.

[0010] A second aspect of the present invention is the modified ethylene polymer composition of the first aspect, wherein the acrylic polymer is a copolymer containing a methyl methacrylate unit as the methyl (meth)acrylate unit and containing a butyl methacrylate unit and a butyl acrylate unit as the alkyl (meth)acrylate unit having 2 to 18 carbon atoms.

[0011] A third aspect of the present invention is the modified ethylene polymer composition of the first or second aspect, wherein the ethylenically unsaturated compound is a polar ethylenically unsaturated compound having a carboxyl group, a hydroxyl group or an amino group, an anhydride of a polar ethylenically unsaturated compound having a carboxyl group, or an aromatic vinyl compound.

[0012] A fourth aspect of the present invention relates to the modified ethylene polymer composition of the third aspect, wherein the ethylenically unsaturated compound is the polar ethylenically unsaturated compound having a carboxyl group or an anhydride thereof, and the polar ethylenically unsaturated compound having a carboxyl group or an anhydride thereof is an unsaturated dicarboxylic acid or an anhydride thereof.

[0013] A fifth aspect of the present invention relates to the modified ethylene polymer composition according to any one of the first to fourth aspects, wherein the content of the ethylenically unsaturated compound is 0.05 to 10% by mass.

[0014] A sixth aspect of the present invention relates to a modified ethylene polymer composition according to any one of the first to fifth aspects, which has a melt flow rate of 0.05 to 50 g / 10 min as measured at a temperature of 190° C. and a load of 21.2 N in accordance with JIS K 7210:2014, and a density of 0.85 to 0.97 g / cm as measured by an underwater displacement method in accordance with JIS K 7112:1999. 3 It is.

[0015] A seventh aspect of the present invention is an olefin polymer composition comprising a modified ethylene polymer composition according to any one of the first to sixth aspects and an olefin polymer, wherein the mass ratio of the modified ethylene polymer composition to the olefin polymer is 1:99 to 99:1.

[0016] An eighth aspect of the present invention is a laminate in which a layer made of the modified ethylene polymer composition according to any one of the first to sixth aspects is bonded to a layer serving as an adherend.

[0017] A ninth aspect of the present invention relates to the laminate of the eighth aspect, wherein the layer that is the adherend is at least one layer selected from the group consisting of thermoplastic resins, metal foils, paper, wood, and fibers.

[0018] A tenth aspect of the present invention is a laminate in which a layer made of the olefin polymer composition of the seventh aspect is bonded to a layer serving as an adherend.

[0019] An eleventh aspect of the present invention is the laminate of the tenth aspect, wherein the layer that is the adherend is at least one layer selected from the group consisting of thermoplastic resins, metal foils, paper, wood, and fibers.

[0020] A twelfth aspect of the present invention is a method for producing a modified ethylene polymer composition, comprising a step of melt-kneading an ethylene polymer, an ethylenically unsaturated compound, an acrylic polymer, a fluorine-containing polymer, and a radical generator, wherein the acrylic polymer is a copolymer containing, as constituent units, a methyl (meth)acrylate unit and an alkyl (meth)acrylate unit having 2 to 18 carbon atoms, the blending amount of the acrylic polymer is 0.05 to 5 parts by mass per 100 parts by mass of the ethylene polymer, and the blending amount of the fluorine-containing polymer is 0.005 to 2 parts by mass per 100 parts by mass of the ethylene polymer. Effect of the Invention

[0021] According to the present invention, a modified ethylene polymer composition can be obtained which exhibits a favorable effect of reducing the occurrence of fisheyes and which exhibits high adhesion to a substrate. Therefore, the modified ethylene polymer composition, the olefin polymer composition containing the same, and the laminate using the same are very useful because they can achieve both excellent adhesion and good appearance even when the substrate is a metal or a polar resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The following describes in detail the embodiments of the present invention, but the following embodiments are examples (representative examples) of the present invention and the present invention is not limited thereto. The present invention can be carried out in any modified form without departing from the gist of the present invention. In this specification, when "~" is used with a numerical value or a physical property value enclosed therein, the values ​​before and after the "~" are included in the expression. In this specification, "(meth)acrylate" means at least one of acrylate and methacrylate. In addition, "(meth)acrylate" may be written as "(meth)acrylic acid". In addition, in this specification, "mass %" and "weight %", and "parts by mass" and "parts by weight" have the same meaning.

[0023] Modified ethylene polymer composition The modified ethylene polymer composition according to this embodiment contains a modified ethylene polymer, an acrylic polymer, and a fluorine-containing polymer. The modified ethylene polymer is an ethylene polymer modified with an ethylenically unsaturated compound. The acrylic polymer contains, as constituent units, a methyl (meth)acrylate unit and an alkyl (meth)acrylate unit having 2 to 18 carbon atoms. The content of the acrylic polymer in the modified ethylene polymer composition is 0.05 to 5% by mass, and the content of the fluorine-containing polymer in the modified ethylene polymer composition is 0.05 to 2% by mass.

[0024] <Modified ethylene polymer> The modified ethylene polymer in this embodiment is an ethylene polymer modified with an ethylenically unsaturated compound.

[0025] The ethylene polymer before modification may be either an ethylene homopolymer or a copolymer containing ethylene units as a constituent unit.

[0026] When the ethylene polymer is a copolymer, examples of the constituent units other than the ethylene unit include α-olefins having 3 or more carbon atoms, vinyl acetate, (meth)acrylic acid, and (meth)acrylic acid esters. Examples of α-olefins having 3 or more carbon atoms include propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 4-methyl-1-pentene, 4,4-dimethyl-1-pentene, 1-hexene, 4-methyl-1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-octadecene, and the number of carbon atoms of the α-olefin is preferably 3 to 20. The ethylene and other structural units of the ethylene-based polymer may be structural units derived from biomass produced using plants as raw materials. Examples of the biomass ethylene-based polymer include biomass branched low-density polyethylene and biomass linear high-density polyethylene, which contain structural units derived from biomass such as ethylene and other structural units.

[0027] When the ethylene polymer is a homopolymer of ethylene, examples thereof include branched low density polyethylene and linear high density polyethylene.

[0028] When the ethylene polymer is a copolymer, examples thereof include linear low / medium density ethylene-α-olefin copolymers, ethylene resins, and ethylene rubbers.

[0029] Examples of linear low / medium density ethylene-α-olefin copolymers include ethylene-propylene copolymers, ethylene-1-butene copolymers, ethylene-propylene-1-butene copolymers, ethylene-4-methyl-pentene copolymers, ethylene-1-heptene copolymers, ethylene-1-hexene copolymers, and ethylene-1-octene copolymers.

[0030] Examples of ethylene-based resins include ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid copolymers, ethylene-methyl (meth)acrylate copolymers, ethylene-ethyl (meth)acrylate copolymers, and ethylene-(meth)acrylic acid-methyl (meth)acrylate copolymers.

[0031] Examples of ethylene-based rubbers include ethylene-propylene copolymers, ethylene-1-butene copolymers, and ethylene-propylene-non-conjugated diene copolymers and ethylene-1-butene-non-conjugated diene copolymers obtained by further copolymerizing these copolymers with non-conjugated dienes such as 1,4-hexadiene, dicyclopentadiene, and 5-ethylidene-2-norbornene.

[0032] Among them, the ethylene-based polymer is more preferably a branched low-density ethylene homopolymer or a linear low-density ethylene-α-olefin copolymer. The ethylene-based polymer may be used alone or in combination of two or more kinds.

[0033] The density of the ethylene polymer, as measured by the underwater displacement method in accordance with JIS K 7112:1999, is 0.85 to 0.97 g / cm 3 is preferable, and 0.86 to 0.965 g / cm 3 From the viewpoint of adhesiveness to an adherend when the modified ethylene polymer composition is prepared, the density is more preferably 0.85 g / cm. 3 More than 0.86 g / cm is preferable. 3 More preferably, 0.97 g / cm 3 Less than 0.965 g / cm is preferred. 3 The following is more preferred:

[0034] The melt flow rate (MFR) of the ethylene polymer is preferably 0.1 to 200 g / 10 min, and more preferably 0.5 to 100 g / 10 min, as measured at a temperature of 190° C. and a load of 21.2 N in accordance with JIS K 7210: 2014. From the viewpoint of moldability of the modified ethylene polymer composition, the MFR is preferably 0.1 g / 10 min or more, and more preferably 0.5 g / 10 min or more, and is preferably 200 g / 10 min or less, and more preferably 100 g / 10 min or less.

[0035] The ethylene polymer has a density of 0.85 to 0.97 g / cm 3 Furthermore, the MFR is preferably 0.1 to 200 g / 10 min, and the more preferred ranges of the density and MFR are as described above.

[0036] The modified ethylene polymer in this embodiment is a polymer obtained by modifying the above-mentioned ethylene polymer with an ethylenically unsaturated compound.

[0037] The above-mentioned ethylenically unsaturated compound is not particularly limited as long as it is a compound having an ethylenically unsaturated bond.As the ethylenically unsaturated compound, for example, the polar ethylenically unsaturated compound having a carboxyl group, a hydroxyl group or an amino group, the anhydride of the polar ethylenically unsaturated compound having a carboxyl group, etc. may be used as the ethylenically unsaturated compound. The ethylenically unsaturated compounds may be used alone or in combination of two or more.

[0038] Examples of polar ethylenically unsaturated compounds having a carboxyl group or their anhydrides include unsaturated carboxylic acids such as (meth)acrylic acid, crotonic acid, isocrotonic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, and tetrahydrophthalic acid, or their anhydrides. The above-mentioned unsaturated carboxylic acid is a concept that includes those having two or more carboxylic acids, such as unsaturated dicarboxylic acids.

[0039] Examples of the ethylenically unsaturated compound containing a hydroxyl group include p-hydroxystyrene, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, and 2-hydroxybutyl acrylate.

[0040] As the ethylenically unsaturated compound containing an amino group, for example, a primary, secondary or tertiary amino group-containing monomer can be used. More specifically, for example, monomethylaminoethyl acrylate, dimethylaminoethyl acrylate, diethylaminoethyl acrylate, monomethylaminoethyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, dimethylaminopropyl acrylamide, dimethylaminopropyl methacrylamide, allylamine, etc. can be mentioned.

[0041] Examples of the aromatic vinyl compound include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, dimethylstyrene, and chlorostyrene.

[0042] Among these, the ethylenically unsaturated compound is preferably a polar ethylenically unsaturated compound having a carboxyl group or an anhydride thereof, more preferably an unsaturated dicarboxylic acid or an anhydride thereof, from the viewpoint of adhesiveness of the modified ethylene polymer composition. Examples of the unsaturated dicarboxylic acid include maleic acid, fumaric acid, itaconic acid, citraconic acid, and tetrahydrophthalic acid. As mentioned above, from the viewpoint of adhesion, the ethylenically unsaturated compound is preferably maleic acid or maleic anhydride, and particularly preferably maleic anhydride.

[0043] In the present embodiment, the content of the ethylenically unsaturated compound in the modified ethylene polymer composition is preferably 0.05 to 10% by mass, more preferably 0.1 to 5% by mass. From the viewpoint of sufficiently modifying the ethylene polymer and obtaining better adhesiveness as the modified ethylene polymer composition, the content is preferably 0.05% by mass or more, more preferably 0.1% by mass or more. From the viewpoint of further suppressing the occurrence of fisheyes, the content is preferably 10% by mass or less, more preferably 5% by mass or less.

[0044] The density of the modified ethylene polymer in the present embodiment, in which the ethylene polymer is modified with an ethylenically unsaturated compound, measured by an underwater displacement method in accordance with JIS K 7112:1999, is 0.85 to 0.97 g / cm 3 is preferable, and 0.86 to 0.965 g / cm 3 From the viewpoint of adhesiveness to an adherend when the modified ethylene polymer composition is prepared, the density is more preferably 0.85 g / cm. 3 More than 0.86 g / cm is preferable. 3 More preferably, 0.97 g / cm 3 Less than 0.965 g / cm is preferred. 3 The following is more preferred:

[0045] The melt flow rate (MFR) of the modified ethylene polymer in this embodiment, measured in accordance with JIS K 7210: 2014 at a temperature of 190°C and a load of 21.2 N, is preferably 0.1 to 200 g / 10 min, and more preferably 0.5 to 100 g / 10 min. From the viewpoint of moldability of the modified ethylene polymer composition, the MFR is preferably 0.1 g / 10 min or more, and more preferably 0.5 g / 10 min or more, and is preferably 200 g / 10 min or less, and more preferably 100 g / 10 min or less.

[0046] The modified ethylene polymer in the present embodiment has a density of 0.85 to 0.97 g / cm 3 Furthermore, the MFR is preferably 0.1 to 200 g / 10 min, and the more preferred ranges of the density and MFR are as described above.

[0047] <Acrylic Polymer> The acrylic polymer in this embodiment contains, as structural units, a methyl (meth)acrylate unit and an alkyl (meth)acrylate unit having 2 to 18 carbon atoms. This improves the apparent fluidity of the modified ethylene polymer composition and suppresses the occurrence of fish eyes. Furthermore, the acrylic polymer has excellent compatibility with the modified ethylene polymer, and the transparency of the modified ethylene polymer composition is also improved.

[0048] The acrylic polymer in this embodiment is a component contained as a polymer processing aid together with the fluorine-containing polymer in this embodiment, which improves the moldability and molded appearance of the resulting modified ethylene polymer composition.

[0049] The modified ethylene polymer composition according to this embodiment contains both a fluorine-based polymer processing aid composed of a fluorine-containing polymer and an acrylic polymer processing aid composed of a specific acrylic polymer, and thus exhibits a favorable effect of reducing the occurrence of fisheyes and also has excellent adhesion.

[0050] Specifically, the acrylic polymer in this embodiment contains a methyl (meth)acrylate unit as a structural unit, and thus has excellent releasability from metal, that is, excellent lubricity. In particular, from the viewpoint of effectively accumulating at the interface between the modified ethylene polymer and the metal and exhibiting lubricity, the acrylic polymer preferably contains a methyl methacrylate unit. The methyl (meth)acrylate unit may contain both a methyl methacrylate unit and a methyl acrylate unit.

[0051] The acrylic polymer in the present embodiment contains an alkyl (meth)acrylate unit having 2 to 18 carbon atoms as a constituent unit, and thus has excellent compatibility with the modified ethylene polymer.

[0052] The alkyl (meth)acrylate unit may have 2 to 18 carbon atoms, and preferably has 2 to 12 carbon atoms. From the viewpoint of compatibility with the modified ethylene polymer, the carbon number is 2 or more, and more preferably 3 or more. Furthermore, from the viewpoint of suppressing a decrease in the polymerization rate and achieving suitable polymerizability, i.e., good productivity, the carbon number is 18 or less, and preferably 12 or less. The alkyl (meth)acrylate unit having 2 to 18 carbon atoms may contain only one type, or two or more types.

[0053] The alkyl group in the alkyl (meth)acrylate unit having 2 to 18 carbon atoms may be linear or branched, or may be a cyclic alkyl group. Examples of alkyl (meth)acrylates having a linear alkyl group include ethyl (meth)acrylate, n-butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and tridecyl (meth)acrylate. Examples of alkyl(meth)acrylates having a branched alkyl group include i-butyl(meth)acrylate, t-butyl(meth)acrylate, and 2-ethylhexyl(meth)acrylate. Examples of methacrylates having a cyclic alkyl group include cyclohexyl methacrylate.

[0054] From the viewpoint of compatibility with the modified ethylene polymer, the acrylic polymer preferably contains a butyl (meth)acrylate unit, more preferably a butyl methacrylate unit and a butyl acrylate unit, and more preferably contains two or more units selected from the group consisting of an n-butyl methacrylate unit, an n-butyl acrylate unit, and an i-butyl methacrylate unit.

[0055] From the viewpoint of compatibility with the modified ethylene polymer, the acrylic polymer in the present embodiment is preferably a copolymer containing methyl methacrylate units as methyl (meth)acrylate units and containing butyl methacrylate units and butyl acrylate units as alkyl (meth)acrylate units having 2 to 18 carbon atoms.

[0056] The acrylic polymer in the present embodiment may contain, as a structural unit, a structural unit other than the methyl (meth)acrylate unit and the alkyl (meth)acrylate unit having 2 to 18 carbon atoms, as long as the effects of the present invention are not impaired. Examples of other structural units include aromatic alkenyl compounds such as styrene, α-methylstyrene, chlorostyrene, and vinyltoluene, vinyl cyanide compounds such as acrylonitrile and methacrylonitrile, vinyl esters such as vinyl acetate, and dicarboxylic acid anhydrides such as maleic anhydride. When other structural units are contained, the total unit amount of the other structural units relative to all the structural units is preferably from 0 to 30 mol %, more preferably from 0 to 25 mol %, and even more preferably from 0 to 20 mol %.

[0057] The weight average molecular weight (Mw) of the acrylic polymer in this embodiment is preferably 10,000 to 500,000. From the viewpoint of obtaining a suitable lubrication effect and obtaining high transparency of the modified ethylene polymer composition, and from the viewpoint of obtaining good adhesion, the weight average molecular weight is preferably 10,000 or more. From the viewpoint of obtaining a suitable lubrication effect and obtaining high transparency of the modified ethylene polymer composition, the weight average molecular weight is preferably 500,000 or less. The weight average molecular weight (Mw) in this specification is a value measured using gel permeation chromatography (GPC) under the following conditions. (conditions) 0.05 g of an acrylic polymer is dissolved in 10 ml of tetrahydrofuran, and the molecular weight is determined as polymethyl methacrylate equivalent molecular weight using a column (K-806L, manufactured by Showa Denko K.K.) in gel permeation chromatography (LC-10A system, manufactured by Shimadzu Corporation).

[0058] The content of the acrylic polymer in this embodiment is 0.05 to 5 parts by mass, more preferably 0.1 to 2 parts by mass, and even more preferably 0.2 to 1.8 parts by mass, per 100 parts by mass of the ethylene polymer. Here, from the viewpoint of obtaining a suitable lubrication effect and more preferably suppressing the occurrence of fisheyes in the modified ethylene polymer composition, the content is 0.05 parts by mass or more, preferably 0.1 parts by mass or more, and more preferably 0.2 parts by mass or more. In addition, from the viewpoint of ensuring higher transparency and adhesiveness of the modified ethylene polymer composition, the content is 5 parts by mass or less, preferably 2 parts by mass or less, and more preferably 1.8 parts by mass or less.

[0059] The content of the acrylic polymer in the modified ethylene polymer composition in this embodiment is preferably 0.05 to 5% by mass, more preferably 0.1 to 2% by mass, and even more preferably 0.2 to 1.8% by mass. Here, from the viewpoint of obtaining a suitable lubrication effect and more preferably suppressing the occurrence of fisheyes in the modified ethylene polymer composition, the content is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.2 parts by mass or more. In addition, from the viewpoint of ensuring higher transparency and adhesiveness of the modified ethylene polymer composition, the content is preferably 5% by mass or less, more preferably 2% by mass or less, and even more preferably 1.8% by mass or less.

[0060] The acrylic polymer in the present embodiment may be a manufactured one or a commercially available one. Examples of commercially available acrylic polymers include "Metablen (registered trademark) L type" manufactured by Mitsubishi Chemical Corporation, "PLASTISTRENGTH (registered trademark) L series" manufactured by ARKEMA, "Kane Ace (registered trademark) PA series" manufactured by Kaneka Corporation, and "PARALOID K series" manufactured by Dow Chemical Company.

[0061] <Fluorine-containing polymer> The fluorine-containing polymer in the present embodiment is a polymer containing fluorine atoms in the molecule, and is a component contained, together with the acrylic polymer in the present embodiment, as a polymer processing aid that improves the moldability of the resulting modified ethylene polymer composition. By containing a fluorine-containing polymer, the modified ethylene polymer composition according to this embodiment can reduce fisheyes and also improve the lubricity with the extruder metal, thereby exhibiting high productivity.

[0062] The ratio (molar ratio) of fluorine atoms to hydrogen atoms in the fluorine-containing polymer is preferably 1:1 or more, more preferably 1:1.5 or more, from the viewpoint of lubricity. The upper limit of the ratio of fluorine atoms is not particularly limited, but is, for example, 1:99 or less.

[0063] The fluorine-containing polymer is preferably flowable during the production of the modified ethylene polymer composition according to this embodiment, and is more preferably a fluororubber or a thermoplastic fluororesin having a melting point of 300° C. or less. The melting point of 300° C. or less provides excellent meltability during melt kneading to obtain the modified ethylene polymer composition, and the effect of reducing fisheyes can be suitably obtained. The melting point of the thermoplastic fluororesin is more preferably 230° C. or less, and even more preferably 150° C. or less. The lower limit of the melting point is not particularly limited, but is usually 100° C. or more.

[0064] Examples of the fluororubber or thermoplastic fluororesin as the fluorine-containing polymer in this embodiment include homopolymers of vinylidene fluoride, hexafluoropropylene, chlorotrifluoroethylene, 1-hydropentafluoropropylene, 2-hydropentafluoropropylene, tetrafluoroethylene, perfluoroalkyl-perfluorovinyl ether, and the like, copolymers thereof, and copolymers of these monomers with α-olefins such as ethylene and propylene.

[0065] Specific examples of the fluororubber include a copolymer of vinylidene fluoride and a comonomer selected from hexafluoropropylene, chlorotrifluoroethylene, tetrafluoroethylene, 1-hydropentafluoropropylene, and 2-hydropentafluoropropylene; a terpolymer of vinylidene fluoride, tetrafluoroethylene, and a comonomer selected from hexafluoropropylene, 1-hydropentafluoropropylene, and 2-hydropentafluoropropylene; and a copolymer of tetrafluoroethylene and propylene. Among these, vinylidene fluoride-hexafluoropropylene copolymer, tetrafluoroethylene-propylene copolymer, tetrafluoroethylene-vinylidene fluoride-hexafluoropropylene copolymer, and the like are preferable.

[0066] Specific examples of thermoplastic fluororesins include tetrafluoroethylene homopolymers, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymers, tetrafluoroethylene-hexafluoropropylene copolymers, tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether copolymers, tetrafluoroethylene-ethylene copolymers, chlorotrifluoroethylene homopolymers, vinylidene fluoride homopolymers, tetrafluoroethylene-propylene copolymers, and tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymers. Among these, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer, and the like are preferable.

[0067] In the present embodiment, the critical surface tension of the fluorine-containing polymer is preferably 28 mN / m or less, more preferably 25 mN / m or less, from the viewpoint of releasability from metal. The lower limit of the critical surface tension is not particularly limited, but is, for example, 10 mN / m or more. The critical surface tension in this specification is a value determined by contact angle measurement.

[0068] The content of the fluorine-containing polymer in this embodiment is preferably 0.005 to 2 parts by mass, more preferably 0.01 to 1 part by mass, and even more preferably 0.01 to 0.5 parts by mass, per 100 parts by mass of the ethylene polymer. From the viewpoint of obtaining a favorable fisheye reduction effect, the content is preferably 0.005 parts by mass or more, and preferably 0.01 parts by mass or more. Moreover, since the fisheye reduction effect reaches a plateau, and from the viewpoint of maintaining transparency and economic efficiency, the content is preferably 2 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less.

[0069] The content of the fluorine-containing polymer in the modified ethylene polymer composition in this embodiment is 0.005 to 2 mass%, preferably 0.01 to 1 mass%, and more preferably 0.01 to 0.5 mass%. From the viewpoint of obtaining a favorable fisheye reduction effect, the content is 0.005 mass% or more, and preferably 0.01 mass% or more. Furthermore, since the fisheye reduction effect reaches a plateau, and from the viewpoint of maintaining transparency and economic efficiency, the content is preferably 2 mass% or less, more preferably 1 mass% or less, and even more preferably 0.5 mass% or less.

[0070] The fluorine-containing polymer in this embodiment may be blended with a polyalkylene glycol such as polyethylene glycol, a polyester such as polycaprolactone, or an inorganic filler such as talc, calcium carbonate, or silica.

[0071] The fluorine atom content in the fluorine-containing polymer in this embodiment is preferably 50% by mass or more, more preferably 60 to 95% by mass, and even more preferably 65 to 90% by mass. From the viewpoints of improving heat resistance and bleeding to the surface of the resulting modified ethylene polymer composition to facilitate the development of lubricity, the content is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 65% ​​by mass or more. From the viewpoints of maintaining the processability of the resulting modified ethylene polymer composition, the content is preferably 95% by mass or less, and more preferably 90% by mass or less.

[0072] The fluorine-containing polymer in the present embodiment may be a manufactured one or a commercially available one. Examples of commercially available fluorine-containing polymers include "Dynamer (registered trademark) FX series" manufactured by 3M and "Viton (registered trademark) FreeFlow series" manufactured by Chemours.

[0073] <Physical properties / applications> The melt flow rate (MFR) of the modified ethylene polymer composition according to the present embodiment, measured according to JIS K 7210:2014 at a temperature of 190°C and a load of 21.2N, is preferably 0.05 to 50g / 10min, more preferably 0.1 to 30g / 10min, and even more preferably 0.5 to 10g / 10min. Here, from the viewpoint of reducing the energy load during production and the processability of the molded product, the MFR is preferably 0.05g / 10min or more, more preferably 0.1g / 10min or more, and even more preferably 0.5g / 10min or more. From the same viewpoint, the MFR is preferably 50g / 10min or less, more preferably 30g / 10min or less, and even more preferably 10g / 10min or less.

[0074] The density of the modified ethylene polymer composition according to this embodiment, measured by the underwater displacement method in accordance with JIS K 7112:1999, is 0.85 to 0.97 g / cm 3 is preferable, and 0.87 to 0.95 g / cm 3 More preferably, 0.89 to 0.93 g / cm 3 From the viewpoint of rigidity and heat resistance, the density is more preferably 0.85 g / cm. 3 More than 0.87 g / cm is preferable. 3 More preferably, 0.89 g / cm 3 More preferably, the density is 0.97 g / cm. 3 Less than 0.95 g / cm is preferred. 3 Less than 0.93 g / cm is more preferable. 3 The following is even more preferred:

[0075] The modified ethylene polymer composition according to the present embodiment has a melt flow rate (MFR) of 0.05 to 50 g / 10 min and a density of 0.85 to 0.97 g / cm 3 More preferred ranges of MFR and density are as described above.

[0076] The modified ethylene polymer composition according to this embodiment has an effect of reducing the occurrence of fisheyes and has a good appearance. As a guideline, when the composition is made into a film having a thickness of 50 μm, the amount of fisheyes having a major axis of 0.1 mm or more and less than 0.5 mm (FE amount) is preferably 150 pieces / g or less, more preferably 135 pieces / g or less, and even more preferably 120 pieces / g or less. The smaller the amount, the better. In addition, when the film is formed, the amount of FE having a major axis of 0.5 mm or more is preferably less than 20 pieces / g, more preferably 18 pieces / g or less, and even more preferably 15 pieces / g or less, and the smaller the better. Furthermore, when the film is formed, it is more preferable that the amount of FEs having a major axis of 0.1 mm or more and less than 0.5 mm is 160 pieces / g or less, and the amount of FEs having a major axis of 0.5 mm or more is less than 20 pieces / g, and the more preferable ranges of each of the FE amounts are as described above. Here, the FE amount is a value determined by using a surface defect inspection device within an area of ​​200 mm×120 mm, and the detailed conditions can be those described in the examples described later.

[0077] The modified ethylene polymer composition according to the present embodiment may be used as it is as an adhesive composition, or another polymer composition obtained by further kneading the modified ethylene polymer composition with other optional components may be used as an adhesive composition. Another example of the polymer composition is an olefin-based polymer composition using an olefin-based polymer as the other optional component, the details of which will be described later.

[0078] The modified ethylene polymer composition according to the present embodiment can be used as an adhesive composition in the production of a laminate to form one layer of the laminate. The modified ethylene polymer composition according to the present embodiment can also be used as an adhesive composition in the production of a laminate to form one layer of the laminate by further kneading another polymer composition obtained by kneading the modified ethylene polymer composition according to the present embodiment with other optional components.

[0079] <Other ingredients> The modified ethylene polymer composition according to the present embodiment may contain any other components, as necessary, in addition to the modified ethylene polymer and the acrylic polymer, within a range that does not impair the effects of the present invention.

[0080] Examples of other components include thermoplastic resins other than the polymer in the present embodiment, tackifiers, light stabilizers, UV absorbers, nucleating agents, lubricants, antioxidants, antiblocking agents, plasticizers, release agents, flame retardants, colorants, dispersants, bulking agents, and the like, and any of these may be used that are conventionally known. These may be used alone or in combination of two or more.

[0081] Examples of thermoplastic resins include polyolefins and olefin-based elastomers, polyphenylene ethers, polycarbonates, polyamides such as nylon 66 and nylon 11, polyesters and polyester-based elastomers such as polyethylene terephthalate and polybutylene terephthalate, polystyrene and styrene copolymers or hydrogenated products thereof and styrene-based elastomers, cyclic polyolefins, and acrylics / methacrylics such as polymethyl methacrylate. In addition, some or all of the other ingredients may be produced from plant-derived raw materials.

[0082] The amount of the thermoplastic resin used in the present embodiment varies depending on the type of resin used, but is, for example, preferably 0 to 49 parts by mass, more preferably 0 to 20 parts by mass, relative to 100 parts by weight of the ethylene polymer. From the viewpoints of ensuring higher transparency and adhesiveness of the modified ethylene polymer composition, the amount used is preferably 49 parts by mass or less, more preferably 20 parts by mass or less.

[0083] Examples of the tackifier include amorphous resins that are solid at room temperature, such as petroleum resins, rosin resins, terpene resins, and hydrogenated products thereof.

[0084] Among the above, examples of the petroleum resin include aliphatic petroleum resin, aromatic petroleum resin, or copolymers thereof, and hydrogenated products thereof. Examples of the petroleum resin skeleton include C5 resin, C9 resin, C5 / C9 copolymer resin, cyclopentadiene resin, polymer of vinyl-substituted aromatic compound, copolymer of olefin / vinyl-substituted aromatic compound, copolymer of cyclopentadiene compound / vinyl-substituted aromatic compound, etc. In addition, as mentioned above, hydrogenated products of these can also be used as tackifiers.

[0085] Among the above, the rosin resin is a natural resin containing abietic acid as a main component, and examples thereof include natural rosin, polymerized rosin derived from natural rosin, stabilized rosin obtained by disproportionating natural rosin or polymerized rosin, unsaturated acid modified rosin obtained by adding unsaturated carboxylic acids to natural rosin or polymerized rosin, natural rosin ester, modified rosin ester, polymerized rosin ester, etc. Furthermore, examples of the above hydrogenated products include stabilized rosin obtained by hydrogenating natural rosin or polymerized rosin.

[0086] Among the above, examples of the terpene resin include aromatic terpene resins such as polyterpene resins, terpene phenol resins, and aromatic modified terpene resins. As described above, hydrogenated products of these resins can also be used as tackifiers.

[0087] The amount of the tackifier used in the present embodiment varies depending on the type of resin used, but is preferably 1 to 40 parts by mass, and more preferably 5 to 30 parts by mass, relative to 100 parts by weight of the ethylene polymer. From the viewpoint of ensuring adhesiveness, the amount is preferably 1 part by mass or more, and more preferably 5 parts by mass or more. Also, from the viewpoint of productivity of the modified ethylene resin, that is, suppressing blocking during pelletization, the amount is preferably 40 parts by mass or less, and more preferably 30 parts by mass or less.

[0088] Examples of antioxidants include phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants. Among these, phenol-based antioxidants are preferred, and the combined use of a phenol-based antioxidant with a phosphorus-based antioxidant or a sulfur-based antioxidant is also preferred.

[0089] Examples of phenol-based antioxidants include 2,4-dimethyl-6-t-butylphenol, 2,6-di-t-butylphenol, 2,6-di-t-butyl-p-cresol, 2,6-di-t-butyl-4-ethylphenol, 2,4,6-tri-t-butylphenol, 2,5-di-t-butylhydroquinone, butylated hydroxyanisole, n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, and butyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate. phenyl)propionate and other monophenols, 4,4'-dihydroxydiphenyl, 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-butylidenebis(3-methyl-6-t-butylphenol), 2,6-bis(2'-hydroxy-3'-t-butyl-5'-methylbenzyl)-4-methylphenol and other bisphenols, 1,1,3- Tris(2'-methyl-4'-hydroxy-5'-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3',5'-di-t-butyl-4'-hydroxybenzyl)benzene, tris(3,5-di-t-butyl-4-hydroxyphenyl)isocyanurate, tris[β-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxyethyl]isocyanurate, tetrakis[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate] Polyphenols of tri- or higher order such as methane, thiobisphenols such as 2,2'-thiobis(4-methyl-6-t-butylphenol), 4,4'-thiobis(2-methyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol), naphthylamines such as aldol-α-naphthylamine, phenyl-α-naphthylamine, phenyl-β-naphthylamine, diphenylamines such as p-isopropoxydiphenylamine, N,N'-diphenyl-p-phenylenediamine, N,Examples of the phenylenediamine-based compounds include N'-di-β-naphthyl-p-phenylenediamine, N-cyclohexyl-N'-phenyl-p-phenylenediamine, and N-isopropyl-N'-phenyl-p-phenylenediamine. Among these, monophenol-based compounds, bisphenol-based compounds, tri- or higher polyphenol-based compounds, and thiobisphenol-based compounds are preferred.

[0090] The phosphorus-based antioxidant preferably has a basic skeleton of a phosphite ester in which three alkoxy groups are bonded to a phosphorus atom, and at least one of the alkoxy groups is a bulky group having three or more carbon atoms. Examples include phenyldiisoalkyl (C1-C10) phosphite, diphenylisoalkyl (C1-C10) phosphite, and tris-(2,4-di-t-butylphenyl) phosphite.

[0091] Examples of sulfur-based antioxidants include dilauryl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, pentaerythritol-tetrakis-(β-lauryl-thiopropionate), 2-mercapto-5-methylbenzimidazole, and the like.

[0092] The amount of the antioxidant used in the present embodiment varies depending on the type of antioxidant used, but is, for example, preferably 0.001 to 2 parts by mass, more preferably 0.005 to 1 part by mass, and even more preferably 0.007 to 0.8 parts by mass, relative to 100 parts by mass of the ethylene polymer. Here, from the viewpoint of obtaining a better fisheye reduction effect, the amount used is preferably 0.001 parts by mass or more, more preferably 0.005 parts by mass or more, and even more preferably 0.007 parts by mass or more. In addition, from the viewpoint of suppressing the antioxidant from bleeding out from the modified ethylene polymer composition, the amount used is preferably 2 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.8 parts by mass or less.

[0093] Examples of the filler include inorganic fillers such as calcium carbonate, talc, and silica. In addition, a filler may be blended with the fluorine-containing polymer of the present embodiment, and then both the fluorine-containing polymer and the filler may be contained in the modified ethylene polymer composition of the present embodiment. In this case, in addition to the inorganic fillers described above, organic fillers such as polyalkylene glycols such as polyethylene glycol and polyesters such as polycaprolactone may also be used.

[0094] <Manufacturing method> The method for producing the modified ethylene polymer composition according to the present embodiment includes a step of melt-kneading an ethylene polymer, an ethylenically unsaturated compound, an acrylic polymer, a fluorine-containing polymer, and a radical generator.

[0095] Here, the ethylene-based polymer, the ethylenically unsaturated compound, the acrylic polymer, and the fluorine-containing polymer can be the ethylene-based polymer and the ethylenically unsaturated compound described in the above-mentioned <Modified ethylene-based polymer>, the acrylic polymer, and the fluorine-containing polymer, respectively, and preferred embodiments are also the same. In addition to the above, the optional components described in the above <Other Components> may be melt-kneaded together.

[0096] The radical generator in this embodiment is preferably, for example, an organic peroxide. Specifically, for example, dialkyl peroxides such as di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, 1,4-bis(t-butylperoxyisopropyl)benzene, 1,1-bis(t-butylperoxy)cyclohexane, n-butyl-4,4-bis(t-butylperoxy)valerate, 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, 2,2-bis(t-butylperoxy)butane, and 1,1-bis(t-butylperoxy)cyclododecane, t-butylperoxyacetate, t-butylperoxy-2-ethylhexanoate, t-butylperoxypivalate, t-butylperoxylaurate, t-butylperoxybenzoate, t-butylperoxyphenyl per ... peroxy esters such as di-t-butylperoxyisopropyl carbonate, t-butylperoxymaleic acid, di-t-butylperoxyisophthalate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(toluylperoxy)hexane, diacyl peroxides such as 3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, benzoyl peroxide, hydroperoxides such as t-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, p-mentha hydroperoxide, 2,5-dimethyl-2,5-di(hydroperoxy)hexane, ketone peroxides such as methyl ethyl ketone peroxide, cyclohexanone peroxide, etc. These may be used alone or in combination of two or more.

[0097] Among these, radical generators having a 1-minute half-life temperature of 140°C or higher are preferred, and for example, dialkyl peroxides such as di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, and peroxy esters such as t-butyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexyne-3, are particularly preferred.

[0098] The melt-kneading in the manufacturing method according to the present embodiment is usually performed by uniformly mixing each component and then melt-kneading. Here, the ethylenically unsaturated compound and the radical generator may be added during the melt-kneading. In addition, the ethylenically unsaturated compound and the radical generator may be added in a state of being dissolved in an organic solvent or the like.

[0099] The fluorine-containing polymer may be added in a state where a master batch is produced from an ethylene polymer or a thermoplastic resin other than the polymer in the present embodiment, which is another component, and then subjected to melt kneading. In this case, the amount of each component such as the fluorine-containing polymer added is adjusted so that the final blend amount falls within a desired range.

[0100] As the mixing device, for example, a tumbler blender, a ribbon blender, a V-type blender, a Henschel mixer, or the like can be used. The mixing time is usually 0.1 to 30 minutes, preferably 0.5 to 5 minutes.

[0101] As a kneading device for carrying out the melt kneading, for example, a mixing roll, a kneader, a Banbury mixer, a Brabender Plastograph, a single-screw or twin-screw extruder, or the like is used.

[0102] The temperature for melt kneading is usually 120 to 300° C., preferably 150 to 280° C., and the kneading time is usually 0.1 to 30 minutes, preferably 0.5 to 10 minutes.

[0103] The amount of the ethylenically unsaturated compound in this embodiment is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the ethylene polymer. From the viewpoint of sufficiently modifying the ethylene polymer and obtaining better adhesiveness as a modified ethylene polymer composition, the amount is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more. From the viewpoint of further suppressing the occurrence of fisheyes, the amount is preferably 10 parts by mass or less, more preferably 5 parts by mass or less.

[0104] The amount of the radical generator in this embodiment is preferably 0.01 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, and even more preferably 0.01 to 1 part by mass, relative to 100 parts by mass of the ethylene-based polymer. From the viewpoint of obtaining a sufficient graft amount, the amount is preferably 0.01 parts by mass or more. From the viewpoint of suppressing side reactions such as crosslinking of the ethylene-based polymer, the amount is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 1 part by mass or less.

[0105] The amount of the acrylic polymer in this embodiment is 0.01 to 10 parts by mass, preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 2 parts by mass, per 100 parts by mass of the ethylene polymer. Here, from the viewpoint of obtaining a suitable lubrication effect and more preferably suppressing the occurrence of fisheyes in the modified ethylene polymer composition, the amount is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more. In addition, from the viewpoint of ensuring higher transparency and adhesiveness of the modified ethylene polymer composition, the amount is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 2 parts by mass or less.

[0106] The amount of the fluorine-containing polymer in this embodiment is 0.005 to 2 parts by mass, preferably 0.01 to 1 part by mass, and more preferably 0.01 to 0.5 parts by mass, per 100 parts by mass of the ethylene polymer. From the viewpoint of obtaining a favorable fisheye reduction effect, the content is 0.005 parts by mass, and preferably 0.01 parts by mass. Furthermore, the fisheye reduction effect reaches a plateau, and from the viewpoint of maintaining transparency and economic efficiency, the content is preferably 2 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less.

[0107] With regard to the blending amounts of the acrylic polymer and the fluorine-containing polymer relative to the ethylene polymer, the blending amount of the acrylic polymer is preferably greater than the blending amount of the fluorine-containing polymer, from the viewpoints of maintaining transparency and reducing the occurrence of fisheyes.

[0108] Olefin Polymer Composition The olefin polymer composition according to the present embodiment contains a modified ethylene polymer composition and an olefin polymer. Here, the modified ethylene polymer composition may be one described in the above "Modified ethylene polymer composition", and preferred embodiments are also the same.

[0109] Use of the olefin polymer composition according to the present embodiment as an adhesive composition is preferable from the viewpoint of stabilizing the modification amount in the polymer composition and the effect of reducing the occurrence of fisheyes, as well as from the viewpoint of productivity, as compared with the use of the modified ethylene polymer composition as it is as an adhesive composition.

[0110] The olefin-based polymer in this embodiment may be a homopolymer or a copolymer. As the homopolymer, for example, a homopolymer of ethylene or a homopolymer of an α-olefin having 3 to 20 carbon atoms is preferable, and a homopolymer of ethylene or a homopolymer of propylene is more preferable. The olefin-based polymer in this embodiment may be a biomass polyolefin containing structural units derived from biomass produced using plants as raw materials.

[0111] As the copolymer, a copolymer obtained from two or more monomers selected from the group consisting of ethylene and an α-olefin having 3 to 20 carbon atoms, a copolymer of ethylene and vinyl acetate, (meth)acrylic acid, a (meth)acrylic acid ester, or the like is preferred, and a copolymer obtained from two or more monomers selected from ethylene and an α-olefin having 3 to 10 carbon atoms, or a copolymer obtained from two or more monomers selected from the group consisting of ethylene and vinyl acetate and a (meth)acrylic acid ester is more preferred.

[0112] Examples of α-olefins having 3 to 20 carbon atoms include propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 4-methyl-1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-octadecene. Among these, α-olefins having 3 to 10 carbon atoms are more preferred.

[0113] The olefin polymer in the present embodiment is preferably a homopolymer of ethylene, a homopolymer of propylene, a copolymer obtained from two or more monomers selected from ethylene and an α-olefin having 3 to 10 carbon atoms, or a copolymer obtained from ethylene and two or more monomers selected from the group consisting of vinyl acetate and a (meth)acrylic acid ester, and even more preferably a homopolymer of ethylene, or a copolymer of two or more monomers selected from ethylene, propylene, 1-butene, 1-hexene, and 1-octene.

[0114] In the olefin polymer composition according to this embodiment, the mass ratio (modified ethylene polymer composition:olefin polymer) of the modified ethylene polymer composition and the olefin polymer is preferably 1:99 to 99:1, more preferably 2:98 to 98:2. That is, the content of the olefin polymer relative to the total content of the modified ethylene polymer composition and the olefin polymer is preferably 1 to 99 mass%, more preferably 2 to 98 mass%. The content of the modified ethylene polymer composition relative to the total content is preferably 1 to 99 mass%, more preferably 2 to 98 mass%.

[0115] From the viewpoint of obtaining good adhesion, the content of the olefin polymer is preferably 99% by mass or less, more preferably 98% by mass or less, and the content of the modified ethylene polymer composition is preferably 1% by mass or more, more preferably 2% by mass or more. From the viewpoint of the effect of reducing the occurrence of fisheyes and productivity, the content of the olefin polymer is preferably 1% by mass or more, more preferably 2% by mass or more, and the content of the modified ethylene polymer composition is preferably 99% by mass or less, more preferably 98% by mass or less.

[0116] The method for producing the olefin polymer composition according to the present embodiment is not particularly limited, and a conventionally known method can be used. For example, a method of mechanically blending the modified ethylene polymer composition, the olefin polymer, and other components added as necessary using an extruder, kneader, or the like, or a method of dissolving and mixing in a suitable good solvent and then removing the solvent, or the like, can be used.

[0117] The mechanical blending method includes, for example, a melt kneading method. The temperature for melt kneading is usually 120 to 300° C., preferably 150 to 280° C., and the kneading time is usually 0.1 to 30 minutes, preferably 0.5 to 10 minutes.

[0118] <Laminate> One aspect of the laminate according to this embodiment is one in which a layer made of a modified ethylene polymer composition and a layer serving as an adherend are bonded and laminated. Another aspect of the laminate according to this embodiment is one in which a layer made of an olefin polymer composition and a layer serving as an adherend are bonded and laminated.

[0119] The modified ethylene polymer composition may be one described in the above section "Modified ethylene polymer composition", and the preferred embodiments are the same. The olefin polymer composition may be one described in the above section "Olefin polymer composition", and the preferred embodiments are the same.

[0120] The layer that is the adherend in this embodiment may be at least one layer selected from the group consisting of thermoplastic resin, metal foil, paper, wood, and fiber.

[0121] The modified ethylene polymer composition and the olefin polymer composition in the present embodiment both exhibit better adhesion than conventional polymer compositions and can therefore be suitably used as an adhesive composition layer, and are also excellent in adhesion to the above-mentioned thermoplastic resins, metal foils, paper, wood, and fibers.

[0122] Examples of the thermoplastic resin in this embodiment include polyamide-based resins, polyester-based resins, saponified ethylene-vinyl acetate copolymers, polycarbonate-based resins, polystyrene-based resins, acrylic resins, polyolefin-based resins, and ethylene-vinyl alcohol copolymers. Examples of polyamide resins include nylon 6, nylon 11, nylon 12, nylon 6-6, nylon 6-10, and nylon 6-12.

[0123] Examples of the metal foil include aluminum, copper, and stainless steel foils. Examples of wood include veneer, plywood, and wood fiberboard. Examples of the fibers include woven fabrics and nonwoven fabrics.

[0124] Among the above, laminates having layers made of saponified ethylene-vinyl acetate copolymer, polyamide resin, polyester resin or metal foil have excellent gas barrier properties and are suitably used as food storage containers, packaging materials and the like.

[0125] The laminate according to the present embodiment may be in the form of a film, plate, tube, foil, or woven fabric, as well as a bottle, a container, or an injection-molded product. In particular, from the viewpoint of more suitably utilizing the effect of reducing fisheyes, the laminate is preferably in the form of a film or plate, and more preferably in the form of a film. When the laminate is in the form of a film, the thickness is preferably 2 mm or less, and more preferably 1 mm or less.

[0126] The method for producing the laminate according to this embodiment is not particularly limited. For example, a method of laminating another layer onto a previously molded film or sheet by a lamination method such as extrusion lamination, dry lamination, sandwich lamination, etc. Other examples include a multi-layer inflation method in which a resin molten in an extruder is bonded at the tip of a multi-layer die to form a laminate, a co-extrusion molding method such as a multi-layer T-die co-extrusion molding method, a multi-layer blow molding method, an injection molding method, and other conventional molding methods.

[0127] When the layer to be adherend is a layer of a saponified ethylene-vinyl acetate copolymer, a polyamide-based resin, or a polyester-based resin, and is to be laminated with an adhesive composition layer made of the modified ethylene-based polymer composition or the olefin-based polymer composition in this embodiment, the method for producing the laminate is preferably coextrusion molding.

[0128] When a laminate is to be prepared by combining a metal foil or the like with an adhesive composition layer comprising the above-mentioned modified ethylene polymer composition or olefin polymer composition, the laminate is preferably produced by a lamination method.

[0129] Specific examples of the layer structure of the laminate according to this embodiment include a gas barrier layer / modified ethylene polymer composition layer, a gas barrier layer / modified ethylene polymer composition layer / polyolefin layer, a polyolefin layer / modified ethylene polymer composition layer / gas barrier layer / modified ethylene polymer composition / polyolefin layer, etc. Here, the gas barrier layer is a layer made of a saponified ethylene-vinyl acetate copolymer, a metal foil, etc. Furthermore, the modified ethylene polymer composition layer in the above layer structure can be replaced with the olefin polymer composition of the present embodiment.

[0130] The laminate according to this embodiment has excellent adhesion due to the layer made of the modified ethylene polymer composition or the olefin polymer composition, and has excellent surface smoothness with reduced occurrence of fisheyes.

[0131] Furthermore, laminates using polyamide resins, polyester resins, saponified ethylene-vinyl acetate copolymers, and metal foils as constituent layers as adherend layers have good gas barrier properties, and therefore, by forming a laminate together with the olefin polymer composition of the present embodiment or an olefin polymer composition, the laminate has good processability, water resistance, chemical resistance, flexibility, and other properties.

[0132] Furthermore, laminates using polycarbonate resins, polystyrene resins, metal foils, and wood as constituent layers as adherend layers have excellent rigidity, while laminates using paper, wood, and fiber as constituent layers have excellent mechanical strength. EXAMPLES

[0133] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the invention. Note that the values ​​of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values ​​in the embodiments of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​of the following examples or values ​​of the examples.

[0134] "raw materials" In the following examples, the following raw materials were used:

[0135] <Component (A): Ethylene-based polymer> (A)-1 Linear ethylene-1-butene copolymer [density: 0.92 g / cm 3 , MFR (190℃, load 21.2N): 30.0g / 10min, melting point: 123℃] (A)-2 Linear ethylene-1-butene copolymer [density: 0.92 g / cm 3 , MFR (190℃, load 21.2N): 2.1g / 10min, melting point: 123℃]

[0136] <Component (B): Fluorine-based polymer processing aid> (B)-1 Vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer [3M: Dynamer(registered trademark) FX5911] (B)-2 Vinylidene fluoride-hexafluoropropylene copolymer + antiblocking agent mixture [3M: Dynamer(registered trademark) FX9613]

[0137] <Component (C): Acrylic polymer processing aid> (C)-1 Acrylic polymer [copolymer consisting of methyl methacrylate units, butyl methacrylate units, and butyl acrylate units, weight average molecular weight: approximately 250,000 g / mol, glass transition temperature: approximately 25°C]

[0138] <Component (D): Ethylenically unsaturated compound> (D)-1 Maleic anhydride [NOF Corporation]

[0139] <Component (E): Radical generator) (E)-1 2,5-Dimethyl-2,5-bis(t-butylperoxy)hexane [Perhexa 25B (registered trademark), manufactured by NOF Corporation]

[0140] <Ingredient (F): Antioxidant> (F)-1 Phenol-based antioxidant [BASF: IRGANOX (registered trademark) 1010]

[0141] <Component (G): Olefin-based polymer> (G)-1 Linear ethylene-1-butene copolymer [Saudi Petrochemical Company, QAMAR (trademark) FD18N, MFR: 2.0 g / 10 min, density: 0.92 g / cm 3 ]

[0142] Examples 1-1 to 1-2, Comparative Examples 1-1 to 1-5, and Reference Examples 1-1 to 1-3 The components described in the above "Raw Materials" were mixed for 1 minute using a super mixer in the amounts shown in Table 1. The resulting mixture was melt-kneaded using a twin-screw extruder (manufactured by Japan Steel Works, Ltd.: TEX25αIII, diameter 25 mm, L / D 43) under conditions of a kneading temperature of 240°C, a screw rotation speed of 300 rpm, and a discharge rate of 20 kg / hour, and extruded through a die into a strand shape and cut to obtain modified ethylene polymer compositions. When the obtained modified ethylene polymer composition was subjected to each evaluation, the modified ethylene polymer composition was used within 30 minutes to 1 hour after the start of strand cut granulation. In addition, blank spaces in Table 1 indicate that no compound was added.

[0143] 《Examples 2-1a to 2-2a, Comparative Examples 2-1a to 2-3a, Reference Examples 2-2a to 2-3a》 A mixture of 10 parts by mass of each modified ethylene polymer composition obtained in Examples 1-1 to 1-2, Comparative Examples 1-1 to 1-3, and Reference Examples 1-2 to 1-3 and 90 parts by mass of an olefin polymer was melt-kneaded at a kneading temperature of 210°C using a single-screw extruder (PSM50-32(1V), manufactured by IKG, D=50 mmφ, L / D=32), and then extruded through a die into a strand shape and cut to obtain each modified olefin polymer.

[0144] 《Examples 2-1b to 2-2b, Comparative Examples 2-1b to 2-3b, Reference Examples 2-2b to 2-3b》 A mixture of 15 parts by mass of each of the modified ethylene polymer compositions obtained in Examples 1-1 to 1-2, Comparative Examples 1-1 to 1-3, and Reference Examples 1-2 to 1-3 and 85 parts by mass of an olefin polymer was melt-kneaded at a kneading temperature of 210°C using a single-screw extruder (PSM50-32(1V), manufactured by IKG, D=50 mmφ, L / D=32) to obtain each modified olefin polymer.

[0145] Measurement and evaluation methods <Component (D); Content of ethylenically unsaturated compound> The content of ethylenically unsaturated compounds, that is, the graft ratio, was determined using an infrared spectrometer. Specifically, the amount of ethylenically unsaturated compounds in the modified ethylene polymer was determined in advance as a standard sample by nuclear magnetic resonance measurement, and a calibration curve was prepared from the quantitative values. Next, pellets of each of the modified ethylene polymer compositions obtained in Examples 1-1 to 1-2, Comparative Examples 1-1 to 1-5, and Reference Examples 1-1 to 1-3 were press-molded into a film having a thickness of 100 μm at 200° C. Using this as a sample, the absorption characteristic of the ethylenically unsaturated compound in the sample, i.e., the absorption at 1900 to 1600 cm, was measured with an FT-IR device (JASCO FT / IR610, manufactured by JASCO Corporation). -1 The carbonyl characteristic absorption observed in the (C=O stretching vibration band) was measured, and the carbonyl content was calculated using the calibration curve prepared above. In addition, in the modification with an ethylenically unsaturated compound, not all of the ethylenically unsaturated compound, i.e. 100%, is subjected to the reaction, and the ethylenically unsaturated compound that has not reacted with the ethylenic polymer may remain in the modified ethylenic polymer composition. However, the content of the ethylenically unsaturated compound (graft ratio) in this specification means the value measured by the above method. The results are shown in Table 1.

[0146] <Melt Flow Rate (MFR)> The melt flow rate (MFR) of each of the modified ethylene polymer compositions obtained in Examples 1-1 to 1-2, Comparative Examples 1-1 to 1-5, and Reference Examples 1-1 to 1-3 was measured at a temperature of 190° C., a load of 21.2 N, and for 10 minutes in accordance with JIS K 7210: 2014. The results are shown in Table 1.

[0147] <density> The density of each of the modified ethylene polymer compositions obtained in Examples 1-1 to 1-2, Comparative Examples 1-1 to 1-5, and Reference Examples 1-1 to 1-3 was measured by the underwater displacement method in accordance with JIS K 7112: 1999. The results are shown in Table 1.

[0148] <Fisheye (FE)> For each of the modified ethylene polymer compositions obtained in Examples 1-1 to 1-2, Comparative Examples 1-1 to 1-5, and Reference Examples 1-1 to 1-3, a monolayer film molding machine having a T-die with a width of 300 mm (GSI Creos Corporation) was used to obtain a monolayer film having a layer thickness of 50 μm under conditions of a T-die temperature of 200° C., a molding speed of 5 m / min, and a cast roll temperature of 30° C. The obtained monolayer film was cut to a length of 200 mm and a width of 120 mm, which was used as the inspection area. Then, using a compact digital surface defect inspection device (GX-70LT, manufactured by Mamiya-OP Co., Ltd.), the number of FEs with a major axis of 0.1 mm or more and less than 0.5 mm, and the number of FEs with a major axis of 0.5 mm or more were counted. The number of FEs counted was divided by the mass of the monolayer film in the inspection area to determine the amount of fisheyes (FEs) per unit mass (pieces / g). In this evaluation, if the amount of FE with a major axis of 0.1 mm or more and less than 0.5 mm is 150 pieces / g or less, the appearance is evaluated as good. In addition, the amount of FE with a major axis of 0.5 mm or more is more preferably 15 pieces / g or less. The results are shown in Table 1.

[0149] <Adhesive strength> A multilayer film molding machine (manufactured by Labtech Engineering Co.) with a 350 mm wide three-type five-layer feedblock type T-die was used to produce a five-layer film consisting of an ethylene-based polymer layer / adhesive resin layer / ethylene-vinyl alcohol copolymer (EVOH) layer / adhesive resin layer / ethylene-based polymer layer. Here, the adhesive resin layers were made of the olefin polymer compositions obtained in Examples 2-1a to 2-2a, Comparative Examples 2-1a to 2-3a, and Reference Examples 2-2a to 2-3a, as well as Examples 2-1b to 2-2b, Comparative Examples 2-1b to 2-3b, and Reference Examples 2-2b to 2-3b. The ethylene polymer layers were made of Novatec (registered trademark) SF8402 (manufactured by Japan Polyethylene Corporation). The ethylene-vinyl alcohol copolymer layer was made of Soarnol (registered trademark) DC3203RB (manufactured by Mitsubishi Chemical Corporation). The specific conditions were a T-die temperature of 240°C, a molding speed of 5 m / min, and a cast roll temperature of 80°C. The thicknesses of the individual layers were 30 μm / 10 μm / 20 μm / 10 μm / 30 μm, respectively, resulting in a five-layer film laminate with a total thickness of 100 μm.

[0150] The five-layer film obtained above was cut into 15 mm-wide strips parallel to the molding direction to prepare test pieces. A T-peel test was performed on each test piece at a constant temperature of 23°C and a speed of 300 mm / min to measure the adhesive strength at the interface between the adhesive resin layer and the EVOH layer. Generally, if the interlayer strength of a laminate is 2N / 15mm or more, it is considered to be sufficient for practical use, so in this evaluation, if the adhesive strength at the interface between the adhesive resin layer and the EVOH layer is 2N / 15mm or more, the adhesion is evaluated as good. The results are shown in Table 1.

[0151] [Table 1]

[0152] The results in Table 1 show that the modified ethylene polymer composition according to this embodiment exhibits a good effect of reducing the occurrence of fisheyes and also exhibits high adhesion to substrates. In particular, it was found that the olefin polymer composition including the modified ethylene polymer composition according to this embodiment contains both a fluorine-based polymer processing aid and an acrylic polymer processing aid as polymer processing aids, and thus exhibits a remarkable effect in both reducing the occurrence of fisheyes and adhesion to substrates, compared with the case where one of them is contained alone or neither is contained.

Claims

1. The polymers include modified ethylene polymers, acrylic polymers, and fluorine-containing polymers, The modified ethylene polymer is an ethylene polymer modified with an ethylenically unsaturated compound, The acrylic polymer is a copolymer containing, as structural units, a methyl (meth)acrylate unit and an alkyl (meth)acrylate unit having 2 to 18 carbon atoms; A modified ethylene-based polymer composition, wherein the content of the acrylic polymer is 0.05 to 5% by mass and the content of the fluorine-containing polymer is 0.005 to 2% by mass.

2. The modified ethylene polymer composition according to claim 1, wherein the acrylic polymer is a copolymer containing a methyl methacrylate unit as the methyl (meth)acrylate unit and containing a butyl methacrylate unit and a butyl acrylate unit as the alkyl (meth)acrylate unit having 2 to 18 carbon atoms.

3. The modified ethylene polymer composition according to claim 1, wherein the ethylenically unsaturated compound is a polar ethylenically unsaturated compound having a carboxyl group, a hydroxyl group or an amino group, an anhydride of a polar ethylenically unsaturated compound having a carboxyl group, or an aromatic vinyl compound.

4. the ethylenically unsaturated compound is the polar ethylenically unsaturated compound having a carboxyl group or an anhydride thereof, The modified ethylene polymer composition according to claim 3, wherein the polar ethylenically unsaturated compound having a carboxyl group or an anhydride thereof is an unsaturated dicarboxylic acid or an anhydride thereof.

5. The modified ethylene-based polymer composition according to claim 1, wherein the content of the ethylenically unsaturated compound in the modified ethylene-based polymer composition is 0.05 to 10% by mass.

6. The melt flow rate measured in accordance with JIS K 7210:2014 under conditions of a temperature of 190°C and a load of 21.2N is 0.05 to 50 g / 10 min, and Density measured by underwater displacement method according to JIS K 7112:1999 is 0.85 to 0.97 g / cm 3 The modified ethylene polymer composition according to claim 1,

7. The modified ethylene polymer composition according to any one of claims 1 to 6 and an olefin polymer are contained therein, The mass ratio of the modified ethylene polymer composition to the olefin polymer is 1:99 to 99:

1.

8. A laminate comprising a layer made of the modified ethylene polymer composition according to any one of claims 1 to 6 and a layer serving as an adherend bonded thereto.

9. 9. The laminate according to claim 8, wherein the layer that is the adherend is at least one layer selected from the group consisting of thermoplastic resins, metal foils, paper, wood, and fibers.

10. A laminate comprising a layer made of the olefin polymer composition according to claim 7 and a layer serving as an adherend bonded to each other.

11. The laminate according to claim 10, wherein the layer that is the adherend is at least one layer selected from the group consisting of thermoplastic resins, metal foils, paper, wood, and fibers.

12. A method for producing a modified ethylene polymer composition, comprising the steps of: The method includes a step of melt-kneading an ethylene-based polymer, an ethylenically unsaturated compound, an acrylic polymer, a fluorine-containing polymer, and a radical generator, The acrylic polymer is a copolymer containing, as structural units, a methyl (meth)acrylate unit and an alkyl (meth)acrylate unit having 2 to 18 carbon atoms; the amount of the acrylic polymer is 0.05 to 5 parts by mass per 100 parts by mass of the ethylene polymer, The amount of the fluorine-containing polymer blended is 0.005 to 2 parts by mass per 100 parts by mass of the ethylene polymer.

Citation Information

Patent Citations

  • Modified ethylene-based polymer composition and laminated product given by using the same

    JP2005036221A