Thermoplastic resin composition and method for producing the same, and hot-melt adhesive

A thermoplastic resin composition with a block copolymer and α-olefin polymer improves flexibility and adhesiveness at low temperatures, addressing the limitations of conventional hot melt adhesives in automotive and industrial applications.

JP2024137160AInactive Publication Date: 2024-10-07MITSUI CHEMICALS INC

Patent Information

Application Number
JP2023048571
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional hot melt adhesives experience a significant decrease in flexibility and adhesive properties at low temperatures, limiting their effectiveness in various applications.

Method used

A thermoplastic resin composition comprising a block copolymer containing vinyl aromatic and conjugated diene compounds, an α-olefin polymer with specific properties, and optionally an adhesive resin and additives, which is used to formulate a hot melt adhesive with improved flexibility and adhesiveness at low temperatures.

Benefits of technology

The composition maintains excellent adhesion and flexibility in low temperature ranges, enhancing the performance of hot melt adhesives in automotive and industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137160000001
    Figure 2024137160000001
  • Figure 2024137160000002
    Figure 2024137160000002
  • Figure 2024137160000003
    Figure 2024137160000003
Patent Text Reader

Abstract

To provide a thermoplastic resin composition that yields a hot-melt adhesive with superior adhesion in a low temperature region, while also demonstrating superior flexibility in the low temperature region.SOLUTION: A thermoplastic resin composition comprises: a thermoplastic resin (A) comprising at least one of a block copolymer comprising a polymer block predominantly composed of a vinyl aromatic compound and a polymer block predominantly composed of a conjugated diene compound, and a hydrogenated derivative thereof; and an α-olefin polymer (B) which fulfills requirements (b-2)-(b-5). A method for producing the same and a hot-melt adhesive are provided.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic resin composition, a method for producing the same, and a hot melt adhesive. [Background technology]

[0002] Conventionally, thermoplastic resins have been used by being molded by various molding methods into various members, films, sheets, fiber adhesives, foams, crosslinked bodies, etc. In order to adapt thermoplastic resins to a wide variety of applications, material designs tailored to each application are required. When a thermoplastic resin is used as a hot melt adhesive, for example, it has been disclosed that a hot melt adhesive exhibiting good fluidity and heat resistance can be obtained by combining an amorphous poly-α-olefin with a crystalline α-olefin elastomer (for example, Patent Document 1).

[0003] As a hot melt pressure-sensitive adhesive that has adhesive properties to films, nonwoven fabrics, resin molded products, etc. even under low temperature conditions and has flexibility that does not impair the texture of the adherend, for example, a hot melt adhesive that combines a styrene-based block copolymer, a specific tackifier resin, and a specific polymer has been disclosed (for example, Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-196839 A [Patent Document 2] JP 2006-241444 A Summary of the Invention [Problem to be solved by the invention]

[0005] Conventional hot melt adhesives have a problem in that their flexibility is significantly reduced under low temperature conditions, resulting in reduced adhesiveness. However, the hot melt adhesives disclosed in Patent Documents 1 and 2 require further improvement in terms of flexibility and adhesiveness under low temperature conditions. The problem to be solved by one embodiment of the present invention is to provide a thermoplastic resin composition which provides a hot melt adhesive having excellent adhesive properties in the low temperature range and excellent flexibility in the low temperature range. [Means for solving the problem]

[0006] Means for solving the above problems include the following aspects. <1> a thermoplastic resin (A) containing at least one of a block copolymer containing a polymer block mainly made of a vinyl aromatic compound and a polymer block mainly made of a conjugated diene compound, and a hydrogenated product thereof; An α-olefin polymer (B) that satisfies the following requirements (b-2) to (b-5); A thermoplastic resin composition comprising: (b-2) No melting point is observed as measured by differential scanning calorimetry (DSC); (b-3) the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,000 to 8,700; (b-4) Density measured by pycnometer method is 810-850 kg / m 3 is; (b-5) Kinematic viscosity at 40°C is 10 to 9,800 mm 2 / s. <2> The α-olefin polymer (B) satisfies the following requirement (b-6): <1> The thermoplastic resin composition according to claim 1 ; (b-6) The pour point is less than -15°C. <3> The α-olefin polymer (B) satisfies the following requirement (b-7): <1> or <2> The thermoplastic resin composition according to claim 1 ; (b-7) Ethylene-α-olefin copolymer. <4> the thermoplastic resin (A) is a hydrogenated product of a block copolymer containing a polymer block mainly composed of the vinyl aromatic compound and a polymer block mainly composed of a conjugated diene compound; <1> ~ <3> 13. The thermoplastic resin composition according to claim 12 . <5> Further comprising an adhesive resin (C); <1> ~ <4> 13. The thermoplastic resin composition according to claim 12 . <6> Further comprising an additive (D), <1> ~ <5> 13. The thermoplastic resin composition according to claim 12 . <7> The content of the thermoplastic resin (A) is 5 to 99.99 mass%, the content of the α-olefin polymer (B) is 0.01 to 95 mass%, the content of the adhesive resin (C) is 1 to 50 mass%, and the content of the additive (D) is 0.1 to 10 mass% (the total of the thermoplastic resin (A), the α-olefin polymer (B), the adhesive resin (C), and the additive (D) is 100 mass%). <1> ~ <6> 13. The thermoplastic resin composition according to claim 12 . <8> A glass transition temperature of less than -56°C as measured by differential scanning calorimetry (DSC); <1> ~ <7> 13. The thermoplastic resin composition according to claim 12 . <9> <1> ~ <8> A hot melt adhesive comprising the thermoplastic resin composition according to any one of claims 1 to 5. <10> Used for automotive or industrial parts <9> 2. The hot melt adhesive according to claim 1 . <11> a solution polymerization step of solution polymerizing ethylene and an α-olefin in the presence of a catalyst containing a bridged metallocene compound (P) represented by the following formula (1) and at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2) and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair; a step of mixing the α-olefin polymer (B) obtained in the solution polymerization step with a thermoplastic resin (A) containing at least one of a block copolymer containing a polymer block mainly composed of a vinyl aromatic compound and a polymer block mainly composed of a conjugated diene compound and a hydrogenated product thereof; Including, The method for producing a thermoplastic resin composition, wherein the α-olefin polymer (B) satisfies the following requirements (b-2) to (b-5): (b-2) No melting point is observed as measured by differential scanning calorimetry (DSC); (b-3) the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,000 to 8,700; (b-4) Density measured by pycnometer method is 810-850 kg / m 3 is; (b-5) Kinematic viscosity at 40°C is 10 to 9,800 mm 2 / s.

[0007] [ka]

[0008] [In formula 1, R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 each independently represents a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and adjacent groups may be linked to each other to form a ring structure; R 6 and R 11 are the same group and each is a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, R 7 and R 10 are the same group and each is a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, R 6 and R 7 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 10 and R 11 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 6 , R 7 , R 10 and R11 is not a hydrogen atom at the same time, Y is a carbon atom or a silicon atom; R 13 and R 14 each independently represents a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and may be linked together to form a ring structure, M is a titanium atom, a zirconium atom, or a hafnium atom; Each Q is independently a halogen atom, a hydrocarbon group, an anionic ligand, or a neutral ligand capable of coordinating to a lone pair of electrons; j is an integer from 1 to 4. <12> R in the above (Formula 1) 13 and R 14 At least one of the groups is an aryl group; <11> A method for producing the thermoplastic resin composition according to claim 1. <13> R in the above (Formula 1) 13 and R 14 are both aryl groups, and R 2 and R 3 one of the above is a saturated hydrocarbon group having 4 carbon atoms; <12> A method for producing the thermoplastic resin composition according to claim 1. Effect of the Invention

[0009] According to one embodiment of the present invention, there is provided a thermoplastic resin composition which provides a hot melt adhesive having excellent adhesion at low temperatures and excellent flexibility in the low temperature range. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. The following description of the components may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, the term "polymer" is a concept including homopolymers and copolymers. In this specification, the use of "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower limit and upper limit. In this specification, the use of "to" indicating a numerical range means that the units written before or after it indicate the same units, unless otherwise specified. As used herein, a combination of two or more preferred embodiments is a more preferred embodiment. In this specification, when referring to the amount of each component in a composition, if multiple substances corresponding to each component are present in the composition, the amount refers to the total amount of multiple substances present in the composition, unless otherwise specified. The present invention will now be described in further detail.

[0011] <Thermoplastic resin composition> The thermoplastic resin composition according to the present invention contains a thermoplastic resin (A) including at least one of a block copolymer containing a polymer block mainly made of a vinyl aromatic compound and a polymer block mainly made of a conjugated diene compound and a hydrogenated product thereof, and an α-olefin polymer (B) satisfying requirements (b-2) to (b-5). The thermoplastic resin composition having the above-mentioned configuration has excellent flexibility in the low temperature range, and the obtained hot melt adhesive has excellent adhesion in the low temperature range. The reason for this is not clear, but the following mechanism is presumed. It is presumed that by including an α-olefin polymer (B) satisfying the requirements (b-2) to (b-5), the glass transition point of the thermoplastic resin composition can be lowered, and flexibility can be maintained down to lower temperatures. In addition, since flexibility can be maintained down to low temperatures, stress dispersion properties as an adhesive and adhesion to substrates can be maintained down to low temperatures, thereby improving adhesion at low temperatures. The term "excellent flexibility or adhesiveness in the low temperature range" means that the flexibility or adhesiveness is excellent in a temperature range of preferably -10°C or lower, more preferably -20°C or lower, and even more preferably -20°C to -30°C.

[0012] <<Thermoplastic resin (A)>> The thermoplastic resin (A) contains at least one of a block copolymer containing a polymer block mainly made of a vinyl aromatic compound and a polymer block mainly made of a conjugated diene compound, and a hydrogenated product thereof.

[0013] In this specification, the term "mainly composed of" means that the polymer block contains structural units derived from a conjugated diene compound (or a vinyl aromatic compound) in an amount of 50% by mass or more, preferably 60% by mass or more, and more preferably 80% by mass or more. For example, a polymer block mainly composed of a conjugated diene compound means that the polymer block contains structural units derived from a conjugated diene compound in an amount of preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more, based on the total mass of the polymer block. Each component contained in the block copolymer and its hydrogenated product will be described below.

[0014] [Vinyl aromatic compounds] The block copolymer contains a polymer block based on a vinyl aromatic compound. The vinyl aromatic compound is not particularly limited, and examples thereof include styrene, α-methylstyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, 3-methylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, monochlorostyrene, dichlorostyrene, methoxystyrene, indene, and acenaphthylene. Among these, from the viewpoint of economy, styrene is preferred as the vinyl aromatic compound. The vinyl aromatic compound may be contained alone or in combination of two or more kinds.

[0015] The thermoplastic resin (A) preferably contains a polymer block mainly composed of a vinyl aromatic compound, which tends to improve the affinity with non-polar resins, polar resins, and metals. Good affinity with non-polar resins, polar resins, and metals is useful, for example, when the thermoplastic resin composition is used as an adhesive such as a hot melt or heat sealant, because it can be applied to a wide range of resins and metals.

[0016] [Conjugated diene compounds] The block copolymer contains a polymer block mainly composed of a conjugated diene compound. The conjugated diene compound is not particularly limited as long as it is a diolefin having one pair of conjugated double bonds, and examples thereof include 1,3-butadiene (butadiene), 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, etc. As the conjugated diene compound, a conjugated diene compound having 4 to 20 carbon atoms is preferable, and butadiene, isoprene, and hexadiene are more preferable. One or more of the conjugated diene compounds can be used.

[0017] -Other vinyl compounds- The block copolymer containing a polymer block mainly composed of a vinyl aromatic compound and a polymer block mainly composed of a conjugated diene compound and / or a hydrogenated product thereof may be copolymerized with a vinyl compound other than the above-mentioned vinyl aromatic compound and conjugated diene compound, respectively, within the scope not impairing the object of the present invention.

[0018] Examples of vinyl compounds other than vinyl aromatic compounds and conjugated diene compounds that can be copolymerized with the block copolymer include linear α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tricene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, and 1-eicosene, and 3-methyl-1-pentene. Examples of suitable branched olefins include olefins such as α-olefins having branched chains, such as 4-methyl-1-pentene, 8-methyl-1-nonene, 7-methyl-1-decene, 6-methyl-1-undecene, and 6,8-dimethyl-1-decene, as well as cyclic olefins; vinyl carboxylic acids and vinyl carboxylates such as acrylic acid, methacrylic acid, methyl acrylate, methyl methacrylate, and ethyl methacrylate; vinyl acetate, acrylonitrile, vinyl chloride, vinylidene chloride, and vinyl alcohol. Copolymerization of any vinyl compound is useful because it makes it easier to adjust the polarity of the thermoplastic resin composition, and it may be applicable to a wider range of materials and applications, such as resins and metals.

[0019] <<Block copolymers and their hydrogenated products>> At least one of the block copolymer containing a polymer block mainly made of a vinyl aromatic compound and a polymer block mainly made of a conjugated diene compound and its hydrogenated product (hereinafter also referred to simply as "block copolymer and / or hydrogenated product") is not particularly limited, and may be composed of a non-hydrogenated block copolymer, may be composed of a hydrogenated block copolymer, or may be a combination of a non-hydrogenated block copolymer and a hydrogenated block copolymer.

[0020] The block copolymer and / or hydrogenated product may be obtained by synthesis or may be a commercially available product. Commercially available non-hydrogenated block copolymers include, for example, Kraton's "D Series," JSR Corporation's "TR Series," and Asahi Kasei Corporation's "Tufprene" and "Asaprene" (all product names). Commercially available hydrogenated block copolymers include, for example, "Septon" and "Hybler" manufactured by Kuraray Co., Ltd., "Tuftec" manufactured by Asahi Kasei Corporation, "Dynaron" manufactured by JSR Corporation, and "G Series" manufactured by Kraton Polymers.

[0021] Of these, the thermoplastic resin (A) is preferably a hydrogenated product of a block copolymer containing a polymer block mainly made of a vinyl aromatic compound and a polymer block mainly made of a conjugated diene compound. It is preferable that the thermoplastic resin (A) is a hydrogenated product of a block copolymer containing a polymer block mainly made of a vinyl aromatic compound and a polymer block mainly made of a conjugated diene compound, since this tends to exhibit good compatibility with the α-olefin polymer (B) described later and is less susceptible to deterioration of mechanical properties and bleed-out.

[0022] The block copolymer and / or its hydrogenated product may each be modified to the extent that the object of the present invention is not impaired. The modification method is not particularly limited, and various known methods can be used. Examples of the modification method include oxidation modification, halogenation modification such as chlorosulfonation, chlorination, and bromination, and graft modification and terminal modification with a vinyl compound having an oxygen-containing group such as an acid, an acid anhydride, an ester, an alcohol, an epoxy, or an ether, a vinyl compound having a nitrogen-containing group such as an isocyanate or an amide, and a vinyl compound having a silicon-containing group such as vinyl silane.

[0023] Examples of vinyl compounds used for graft modification or terminal modification include unsaturated epoxy monomers such as unsaturated glycidyl ethers and unsaturated glycidyl esters (e.g., glycidyl methacrylate); trimethoxyvinylsilane, dimethylmethoxyvinylsilane, dimethoxymethylvinylsilane, triethoxyvinylsilane, trimethylvinylsilane, diethylmethylvinylsilane, diacetoxyethylvinylsilane, diethoxymethylvinylsilane, ethoxydimethylvinylsilane, triacetoxyvinylsilane, tris(2-methoxyethoxy)vinylsilane, triphenylvinylsilane, Monovinyl silanes such as aryl silane and triphenoxyvinyl silane, polyvinyl silanes such as diphenyldivinyl silane and allyloxydimethylvinyl silane, unsaturated carboxylic acid ester-based silane compounds such as methacryloxypropyltrimethoxysilane, methacryloxypropyltriethoxysilane and acryloxypropyltrimethoxysilane; vinyl compounds having silicon-containing groups such as styryl-based silane compounds such as styryltrimethoxysilane; acrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, and nadic acid. TM (endo-cis-bicyclo[2,2,1]hept-5-ene-2,3-dicarboxylic acid), and acid halide compounds of the above unsaturated carboxylic acids; amide compounds, imide compounds, acid anhydrides, ester compounds, and derivatives thereof.

[0024] Examples of the derivatives of the unsaturated carboxylic acid include malenyl chloride, maleimide, maleic anhydride, citraconic anhydride, monomethyl maleate, dimethyl maleate, glycidyl maleate, etc. Among these, the derivatives of the unsaturated carboxylic acid are more preferably unsaturated dicarboxylic acids and their acid anhydrides, and more preferably maleic acid, nadic acid, etc. TM and their acid anhydrides are particularly preferred.

[0025] When the thermoplastic resin (A) is a modified thermoplastic resin, it is preferable since it becomes possible to adjust the affinity with non-polar resins, polar resins, metals, carbon, silica and other inorganic materials, and the like.

[0026] <Thermoplastic resin (A) content> The content of the thermoplastic resin (A) is preferably from 5 to 99.99 mass %, more preferably from 10 to 90 mass %, and further preferably from 20 to 80 mass %, based on the total mass of the thermoplastic resin composition. When the content of the thermoplastic resin (A) is 5% by mass or more, the thermoplastic resin composition is excellent in mechanical properties, heat resistance, etc., which are characteristics of the thermoplastic resin (A), which is preferable. On the other hand, when the content of the thermoplastic resin (A) is 99.99% by mass or less, the thermoplastic resin composition can contain a suitable amount of the α-olefin polymer (B), and is excellent in flowability during molding, low-temperature flexibility, etc. The thermoplastic resin (A) may be contained either alone or in combination of two or more.

[0027] The thermoplastic resin (A) may contain thermoplastic resins other than the block copolymer containing a polymer block mainly composed of a vinyl aromatic compound and a polymer block mainly composed of a conjugated diene compound and hydrogenated products thereof (hereinafter also referred to as "other thermoplastic resins"), as necessary, within the scope that does not impair the object of the present invention.

[0028] Other thermoplastic resins include amorphous α-olefin polymers such as polypropylene, propylene-ethylene copolymers, propylene-butene-1 copolymers, propylene-butene-1-ethylene terpolymers, propylene-hexene-1-octene-1-terpolymers, propylene-hexene-1-4-methylpentene-1-terpolymers, polybutene-1, butene-1-ethylene copolymers, butene-1-propylene copolymers, butene-1-propylene-ethylene terpolymers, butene-1-hexene-1-octene-1-terpolymers, and butene-1-hexene-1-4-methylpentene-1-terpolymers; crystalline α-olefin polymers such as polyolefins, including polyethylene, polypropylene, and polybutene, and copolymers thereof; and ethylene-acetic acid. vinyl copolymers; styrene-based polymers such as polystyrene and acrylonitrile-styrene copolymers, and hydrogenated products thereof; polyvinyl chloride, polyvinylidene chloride; vinyl carboxylic acid polymers and vinyl carboxylic acid ester polymers such as polyacrylic acid, polymethacrylic acid, polymethyl acrylate, polymethyl methacrylate, and polyethyl methacrylate; ethylene-methacrylic acid copolymers, ethylene-methacrylic acid ester copolymers, ethylene-vinyl alcohol copolymers; polyesters such as polycarbonate, polyethylene terephthalate, and polybutylene terephthalate; polyamides such as nylon 6, nylon 11, nylon 12, nylon 46, nylon 66, nylon MXD6, fully aromatic polyamides, and semi-aromatic polyamides; and polyacetals.

[0029] The content of other thermoplastic resins is usually 50 mass% or less, preferably 30 mass% or less, more preferably 10 mass% or less, even more preferably 5 mass% or less, and particularly preferably 1 mass% or less, relative to the total mass of thermoplastic resin (A). It is most preferable that thermoplastic resin (A) is substantially free of other thermoplastic resins.

[0030] <α-Olefin polymer (B)> The α-olefin polymer (B) satisfies the requirements (b-2) to (b-5) described below.

[0031] The α-olefin polymer (B) may be a homopolymer of an α-olefin or a copolymer of two or more kinds of α-olefins. The α-olefin polymer (B) is preferably a homopolymer of an α-olefin having 2 to 20 carbon atoms, or a copolymer of two or more kinds of α-olefins having 2 to 20 carbon atoms.

[0032] Examples of the α-olefin having 2 to 20 carbon atoms include linear α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tricene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, and 1-eicosene, and branched α-olefins such as 3-methyl-1-pentene, 4-methyl-1-pentene, 8-methyl-1-nonene, 7-methyl-1-decene, 6-methyl-1-undecene, and 6,8-dimethyl-1-decene. These α-olefins can be used alone or in combination of two or more.

[0033] <<Requirements (b-2)>> The α-olefin polymer (B) does not show a melting point in differential scanning calorimetry (DSC). Here, "no melting point (Tm) is observed" means that the heat of fusion (ΔH) (unit: J / g) measured by differential scanning calorimetry (DSC) is not substantially measured. "no heat of fusion (ΔH) is substantially not measured" means that no peak is observed in the differential scanning calorimetry (DSC) measurement, or the observed heat of fusion is 1 J / g or less.

[0034] The melting point (Tm) and heat of fusion (ΔH) of the α-olefin polymer (B) can be measured by differential scanning calorimetry (DSC), cooling to -100°C and then heating to 150°C at a heating rate of 10°C / min, and analyzing the DSC curve with reference to JIS K7121. If the α-olefin polymer (B) has no observable melting point, it is preferred since it is easy to obtain a favorable effect of improving fluidity and imparting low-temperature flexibility.

[0035] <Requirement (b-3)> The α-olefin polymer (B) has a weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) of 1,000 to 8,700, preferably 1,200 to 7,000, and more preferably 1,500 to 5,500. A weight-average molecular weight (Mw) of 1,000 or more is preferable because the mobility of the α-olefin polymer (B) in the thermoplastic resin composition is not too high and bleeding out is unlikely to occur. On the other hand, a weight-average molecular weight (Mw) of the α-olefin polymer (B) of 8,700 or less is preferable because sufficient fluidity and flexibility improving effects are obtained and moldability is improved, and it is also preferable because it is likely to show good compatibility with the thermoplastic resin (A) and is unlikely to cause a decrease in mechanical properties or bleeding out. That is, when the weight average molecular weight (Mw) of the α-olefin polymer (B) is within the range of 1,000 to 8,700, deterioration of mechanical properties and bleed-out, etc. are suppressed, and a thermoplastic resin composition exhibiting good fluidity and flexibility is easily obtained, which is preferable. Furthermore, when the weight average molecular weight (Mw) of the α-olefin polymer (B) is 1,000 or more, the molecular chains of the α-olefin polymer (B) tend to be entangled with the molecular chains of the thermoplastic resin (A), and thus the thermoplastic resin (A) can be uniformly softened while interacting with the latter. When the thermoplastic resin composition contains various additives, this is useful because it may improve the dispersibility of the additives.

[0036] The weight average molecular weight (Mw) of the α-olefin polymer (B) can be measured by gel permeation chromatography (GPC) calibrated using a standard substance (monodisperse polystyrene) having a known molecular weight.

[0037] <<Requirements (b-4)>> The α-olefin polymer (B) has a density measured by a pycnometer method of 810 to 850 kg / m 3 and preferably 820 to 850 kg / m 3 More preferably, it is 825 to 848 kg / m 3 The above density is measured by a pycnometer method under the condition of 15°C.

[0038] The density of the α-olefin polymer (B) is 810 to 850 kg / m 3 In the case where the density of the α-olefin polymer (B) is within the range of 810 to 850 kg / m, the thermoplastic resin composition is likely to exhibit good fluidity and flexibility, which is preferable. 3 When the content is within this range, compatibility with the thermoplastic resin (A) is likely to be good, bleeding out of the thermoplastic resin composition is likely to be suppressed, and good mechanical properties and appearance can be maintained.

[0039] <<Requirements (b-5)>> The α-olefin polymer (B) has a kinetic viscosity at 40°C of 10 to 9,800 mm 2 / s, preferably 50 to 7,500 mm 2 / s, and more preferably 100 to 5,000 mm 2 / s. The kinetic viscosity of the α-olefin polymer (B) at 40°C is 10 mm 2 When the kinematic viscosity at 40° C. of the α-olefin polymer (B) is 800 mm / s or more, the content of the highly volatile low molecular weight component does not become too high, the heat resistance of the thermoplastic resin composition can be maintained, and bleeding out tends to be less likely to occur, which is preferable. 2 When the molecular weight is not more than 1 / s, the effect of improving the flowability and flexibility due to the α-olefin polymer (B) is easily obtained, which is preferable.

[0040] The α-olefin polymer (B) may further satisfy the following requirements (b-6) to (b-7).

[0041] <<Requirements (b-6)>> The pour point of the α-olefin polymer (B) is preferably lower than −15° C., more preferably −20° C. or lower, and further preferably −25° C. or lower.

[0042] When the pour point of the α-olefin polymer (B) is within the above range, the thermoplastic resin composition tends to exhibit good fluidity and flexibility, and the flexibility and adhesiveness of the thermoplastic resin (A) at low temperatures can be improved, which is preferable.

[0043] <<Requirements (b-7)>> The α-olefin polymer (B) is preferably an ethylene-α-olefin copolymer. It is preferable that the α-olefin polymer (B) is an ethylene-α-olefin copolymer, since this has the effect of effectively reducing crystallinity to make the resin composition liquid and improving fluidity, and also has the effect of improving the compatibility between the α-olefin polymer (B) and the thermoplastic resin (A) and imparting flexibility at low temperatures.

[0044] The ethylene and α-olefin may be composed only of monomers derived from fossil fuels, or only of monomers derived from biomass, or may be a combination of monomers derived from fossil fuels and monomers derived from biomass. Fossil fuels are oil, coal, natural gas, shale gas, or a combination of these fuels. Biomass is any renewable natural source and its residues, such as from plants or animals, including fungi, yeasts, algae, and bacteria.

[0045] The α-olefin constituting the ethylene-α-olefin copolymer may be an α-olefin other than ethylene. Examples of α-olefins other than ethylene include linear α-olefins having 3 to 20 carbon atoms, such as propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, and 1-eicosene, and branched α-olefins having 3 to 20 carbon atoms, such as 3-methyl-1-pentene, 4-methyl-1-pentene, 8-methyl-1-nonene, 7-methyl-1-decene, 6-methyl-1-undecene, and 6,8-dimethyl-1-decene. The above α-olefins may be used alone or in combination of two or more kinds. Among the above-mentioned α-olefins, from the viewpoint of effectively reducing crystallinity to liquefy the thermoplastic resin composition and improving fluidity and flexibility, and from the viewpoint of improving compatibility between the α-olefin polymer (B) and the thermoplastic resin (A), preferred are α-olefins having 3 to 10 carbon atoms, more preferred are linear α-olefins having 3 to 10 carbon atoms, even more preferred are linear α-olefins having 3 to 6 carbon atoms, and particularly preferred is propylene.

[0046] The content of structural units derived from ethylene in the ethylene-α-olefin copolymer is preferably from 10 to 80 mol %, more preferably from 30 to 70 mol %, and even more preferably from 40 to 60 mol %. When the content of the structural units derived from ethylene is within the above range, the crystallinity is reduced, and the mechanical properties can be maintained, and good flowability improving effects and low-temperature flexibility can be obtained.

[0047] The ethylene content in ethylene-α-olefin copolymer is 13 It can be measured by C-NMR method, for example, by identifying and quantifying peaks according to the method described below and the method described in "Polymer Analysis Handbook" (published by Asakura Publishing, pp. 163-170).

[0048] The ethylene-α-olefin copolymer preferably has a blockiness (B value) measured by NMR of usually 0.9 or more, preferably 1.0 or more. The B value is a parameter indicating the randomness of the copolymerization monomer sequence distribution, and when the B value is small, the crystallinity is high, which may reduce the mechanical properties and flexibility improving effect.

[0049] [Method for producing ethylene-α-olefin copolymer] The method for producing the ethylene-α-olefin copolymer is not particularly limited, and may be any known method. For example, the method for producing the ethylene-α-olefin copolymer may be a method of copolymerizing ethylene and an α-olefin in the presence of a catalyst composed of a transition metal compound such as vanadium, zirconium, titanium, or hafnium, and an organoaluminum compound (organoaluminum oxy compound) and / or an ionizing ionic compound. A metallocene catalyst using a transition metal compound such as zirconium, titanium, or hafnium is preferable because it reduces the amount of 2,1-bonds (inversion) between two or more consecutive propylene monomers, thereby improving the low-temperature properties of the curable resin composition. Such methods are described in, for example, WO 2000 / 34420, JP 62-121710 A, WO 2004 / 29062 A, JP 2004-175707 A, WO 2001 / 27124 A, and the like.

[0050] The method for producing the ethylene-α-olefin copolymer includes a method of copolymerizing (preferably solution polymerizing) ethylene and an α-olefin in the presence of a catalyst containing a bridged metallocene compound (P) represented by the following formula (1), and at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2) and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair. Each component of the catalyst will now be described.

[0051] [Bridged metallocene compound (P)] The bridged metallocene compound (P) is a compound represented by the following formula (1).

[0052] [ka]

[0053] In formula 1, R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 each independently represents a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and adjacent groups may be linked to each other to form a ring structure; R 6 and R 11 are the same group and each is a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, R 7 and R 10 are the same group and each is a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, R 6 and R 7 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 10 and R 11 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 6 , R 7 , R 10 and R 11 is not a hydrogen atom at the same time, Y is a carbon atom or a silicon atom; R 13 and R 14 each independently represents a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and may be linked together to form a ring structure, M is a titanium atom, a zirconium atom, or a hafnium atom; Q is independently a halogen atom, a hydrocarbon group, an anionic ligand, or a neutral ligand capable of coordinating to a lone pair of electrons; j is an integer from 1 to 4. Y, M, and R in Formula 1 1 ~R 14 , Q, N and J are explained below.

[0054] < <y>> Y is a carbon atom or a silicon atom, preferably a carbon atom.

[0055] < <m>> M is a titanium atom (Ti), a zirconium atom (Zr) or a hafnium atom (Hf), and is preferably a zirconium atom.

[0056] < <R 1 ~R 14 >> R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 are each independently a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and adjacent groups may be linked to each other to form a ring structure.

[0057] Examples of the hydrocarbon group include an alkyl group having 1 to 20 carbon atoms, a cyclic saturated hydrocarbon group having 3 to 20 carbon atoms, a chain-like unsaturated hydrocarbon group having 2 to 20 carbon atoms, a cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms, an alkylene group having 1 to 20 carbon atoms, and an arylene group having 6 to 20 carbon atoms.

[0058] Examples of the alkyl group having 1 to 20 carbon atoms include linear saturated hydrocarbon groups such as methyl, ethyl, N-propyl, allyl, N-butyl, N-pentyl, N-hexyl, N-heptyl, N-octyl, N-nonyl, and N-decanyl, and branched saturated hydrocarbon groups such as isopropyl, isobutyl, S-butyl, T-butyl, T-amyl, neopentyl, 3-methylpentyl, 1,1-diethylpropyl, 1,1-dimethylbutyl, 1-methyl-1-propylbutyl, 1,1-propylbutyl, 1,1-dimethyl-2-methylpropyl, 1-methyl-1-isopropyl-2-methylpropyl, and cyclopropylmethyl. The alkyl group preferably has 1 to 6 carbon atoms.

[0059] Examples of cyclic saturated hydrocarbon groups having 3 to 20 carbon atoms include cyclic saturated hydrocarbon groups such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a norbornenyl group, a 1-adamantyl group, and a 2-adamantyl group, and groups in which a hydrogen atom of a cyclic saturated hydrocarbon group is replaced with a hydrocarbon group having 1 to 17 carbon atoms, such as a 3-methylcyclopentyl group, a 3-methylcyclohexyl group, a 4-methylcyclohexyl group, a 4-cyclohexylcyclohexyl group, and a 4-phenylcyclohexyl group. The cyclic saturated hydrocarbon group preferably has 5 to 11 carbon atoms.

[0060] Examples of chain unsaturated hydrocarbon groups having 2 to 20 carbon atoms include alkenyl groups such as ethenyl group (vinyl group), 1-propenyl group, 2-propenyl group (allyl group), and 1-methylethenyl group (isopropenyl group), and alkynyl groups such as ethynyl group, 1-propynyl group, and 2-propynyl group (propargyl group). The chain unsaturated hydrocarbon group preferably has 2 to 4 carbon atoms.

[0061] Examples of cyclic unsaturated hydrocarbon groups having 3 to 20 carbon atoms include cyclic unsaturated hydrocarbon groups such as cyclopentadienyl, norbornyl, phenyl, naphthyl, indenyl, azulenyl, phenanthryl, and anthracenyl; groups in which hydrogen atoms of cyclic unsaturated hydrocarbon groups are replaced with hydrocarbon groups having 1 to 15 carbon atoms such as 3-methylphenyl (M-tolyl), 4-methylphenyl (P-tolyl), 4-ethylphenyl, 4-t-butylphenyl, 4-cyclohexylphenyl, biphenylyl, 3,4-dimethylphenyl, 3,5-dimethylphenyl, and 2,4,6-trimethylphenyl (mesityl); and groups in which hydrogen atoms of linear hydrocarbon groups or branched saturated hydrocarbon groups are replaced with cyclic saturated hydrocarbon groups or cyclic unsaturated hydrocarbon groups having 3 to 19 carbon atoms such as benzyl and cumyl. The cyclic unsaturated hydrocarbon group preferably has 6 to 10 carbon atoms.

[0062] Examples of the alkylene group having 1 to 20 carbon atoms include a methylene group, an ethylene group, a dimethylmethylene group (an isopropylidene group), an ethylmethylene group, a methylethylene group, and an N-propylene group. The alkylene group preferably has 1 to 6 carbon atoms.

[0063] Examples of the arylene group having 6 to 20 carbon atoms include an O-phenylene group, an M-phenylene group, a P-phenylene group, and a 4,4'-biphenylylene group. The arylene group preferably has 6 to 12 carbon atoms.

[0064] Examples of silicon-containing hydrocarbon groups include alkylsilyl groups such as trimethylsilyl group, triethylsilyl group, t-butyldimethylsilyl group, and triisopropylsilyl group, which are groups in which a carbon atom in the above-mentioned hydrocarbon groups is replaced with a silicon atom; arylsilyl groups such as dimethylphenylsilyl group, methyldiphenylsilyl group, and t-butyldiphenylsilyl group; pentamethyldisilanyl group; and trimethylsilylmethyl group. The alkylsilyl group preferably has 1 to 10 carbon atoms, and the arylsilyl group preferably has 6 to 18 carbon atoms.

[0065] R 6 and R 11 are the same group and are a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group. The hydrocarbon group and the silicon-containing hydrocarbon group are defined as R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 The meanings and preferred embodiments of the hydrocarbon group and silicon-containing hydrocarbon group in the above formula are the same as those in the above formula. R 7 and R 10 are the same group and are a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group. The hydrocarbon group and the silicon-containing hydrocarbon group are defined as R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 The meanings and preferred embodiments of the hydrocarbon group and silicon-containing hydrocarbon group in the above formula are the same as those in the above formula.

[0066] R 6 and R 7 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 10 and R 11 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 6 , R 7 , R 10 and R 11 is not a hydrogen atom at the same time.

[0067] R 13 and R 14 are each independently a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and may be linked together to form a ring structure. Details of the hydrocarbon group and the silicon-containing hydrocarbon group are described above in R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 The hydrocarbon group has the same meaning as the hydrocarbon group and silicon-containing hydrocarbon group in the above formula (1). The hydrocarbon group further includes an aryl group and a substituted aryl group.

[0068] Examples of the aryl group include, but are not limited to, the above-mentioned examples of the cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms, and include substituents derived from aromatic compounds, such as a phenyl group, a 1-naphthyl group, a 2-naphthyl group, anthracenyl group, phenanthrenyl group, tetracenyl group, chrysenyl group, pyrenyl group, indenyl group, azulenyl group, pyrrolyl group, pyridyl group, furanyl group, and thiophenyl group. The aryl group is preferably a phenyl group or a 2-naphthyl group.

[0069] The aromatic compounds include aromatic hydrocarbons and heterocyclic aromatic compounds, such as benzene, naphthalene, anthracene, phenanthrene, tetracene, chrysene, pyrene, indene, azulene, pyrrole, pyridine, furan, and thiophene.

[0070] Examples of the substituted aryl group include the above-mentioned aryl group in which one or more hydrogen atoms are substituted with at least one substituent selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms, an aryl group, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a halogen atom, and a halogen-containing group. Specific examples include a 3-methylphenyl group (m-tolyl group), a 4-methylphenyl group (p-tolyl group), a 3-ethylphenyl group, a 4-ethylphenyl group, a 3,4-dimethylphenyl group, a 3,5-dimethylphenyl group, a biphenylyl group, a 4-(trimethylsilyl)phenyl group, a 4-aminophenyl group, a 4-(dimethylamino)phenyl group, a 4-(diethylamino)phenyl group, a 4-morpholinylphenyl group, a 4-methoxyphenyl group, a 4-ethoxyphenyl group, a 4-phenoxyphenyl group, a 3,4-dimethoxyphenyl group, a 3,5-dimethoxyphenyl group, a 3-methyl-4-methoxyphenyl group, a 3,5-dimethyl-4-methoxyphenyl group, a 3-(trifluoromethyl)phenyl group, a 4-(trifluoromethyl)phenyl group, a 3-chlorophenyl group, a 4-chlorophenyl group, a 3-fluorophenyl group, a 4-fluorophenyl group, a 5-methylnaphthyl group, and a 2-(6-methyl)pyridyl group.

[0071] < <q>> Each Q is independently a halogen atom, a hydrocarbon group, an anionic ligand, or a neutral ligand capable of coordinating with a lone pair of electrons. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom, with a chlorine atom being preferred. For details of the hydrocarbon group, see R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 The hydrocarbon group preferably has 1 to 7 carbon atoms.

[0072] Examples of the anionic ligand include alkoxy groups such as methoxy, t-butoxy, and phenoxy groups; carboxylate groups such as acetate and benzoate; and sulfonate groups such as mesylate and tosylate.

[0073] Examples of neutral ligands capable of coordinating to lone electron pairs include organic phosphorus compounds such as trimethylphosphine, triethylphosphine, triphenylphosphine, and diphenylmethylphosphine, and ether compounds such as tetrahydrofuran, diethyl ether, dioxane, and 1,2-dimethoxyethane.

[0074] < <j>> J is an integer of 1 to 4, and is preferably 2.

[0075] [Examples of bridged metallocene compounds (P)] The bridged metallocene compound (P) is represented by the formula (1) R 13 and R 14 At least one of these is preferably an aryl group.

[0076] The bridged metallocene compound (P1) is represented by the formula (1) R 13 and R 14 are both aryl groups, and R 2 and R 3 It is preferable that either one of the above is a saturated hydrocarbon group having 4 carbon atoms. In formula 1, R 13 and R 14 are both aryl groups, and R 2 and R 3 Examples of the bridged metallocene compound (P2) in which either one of R 1 ~R 4 Among these, bridged metallocene compounds in which all but the saturated hydrocarbon group having 4 carbon atoms are hydrogen atoms, and R 1 ~R 4 Among these, there can be mentioned a bridged metallocene compound in which two groups adjacent to the saturated hydrocarbon group having 4 carbon atoms are hydrogen atoms and the group that is not adjacent to the saturated hydrocarbon group having 4 carbon atoms is a methyl group.

[0077] Specific examples of the bridged metallocene compound (P) include [dimethylmethylene (η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [dimethylmethylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [dimethylmethylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [dimethylmethylene(η 5 -cyclopentadienyl)(η5-octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [dimethylmethylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -2-methyl-4-t-butylcyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylmethylene{η 5 -(2-methyl-4-i-propylcyclopentadienyl)}(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Methylphenylmethylene (η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Ethylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [ethylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [ethylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [ethylene(η 5 -cyclopentadienyl)(η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [ethylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, Ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Ethylene [η 5 -(3-tert-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Ethylene [η 5 -(3-n-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](2,7-diphenyl-3,6-di-tert-butylfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride.

[0078] Further examples of the bridged metallocene compound (P) include compounds in which the zirconium atom of the above-mentioned compound is replaced with a hafnium atom or a titanium atom, and compounds in which the chloro ligand is replaced with a methyl group. In addition, η 5 -Tetramethyloctahydrodibenzofluorenyl is 4,4,7,7-tetramethyl-(5a,5b,11a,12,12a-η 5 )-1,2,3,4,7,8,9,10-octahydrodibenzo[b,H]fluorenyl group, η 5 -Octamethyloctahydrodibenzofluorenyl is 1,1,4,4,7,7,10,10-octamethyl-(5a,5b,11a,12,12a-η 5 )-1,2,3,4,7,8,9,10-octahydrodibenzo[b,H]fluorenyl group, respectively. The bridged metallocene compounds (P) may be used alone or in combination of two or more.

[0079] [Compound (Q)] The compound (Q) is at least one compound selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2) and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair.

[0080] Specific examples of the organometallic compound (Q-1) include the following organometallic compounds (Q-1A), (Q-1B), and (Q-1C) of Groups 1, 2, 12, and 13 of the Periodic Table.

[0081] (Q-1A);General formula R A M Al(OR B ) N H P X Q An organoaluminum compound represented by the formula: (In the formula, R A and R B may be the same as or different from each other and represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms; X represents a halogen atom; M is a number where 0 < M ≤ 3, N is a number where 0 ≤ N < 3, P is a number where 0 ≤ P < 3, Q is a number where 0 ≤ Q < 3, and M + N + P + Q = 3.)

[0082] Examples of the organometallic compound (Q-1A) of Group 13 of the periodic table include tri-N-alkylaluminums such as trimethylaluminum, triethylaluminum, tri-N-butylaluminum, tri-N-hexylaluminum, and tri-N-octylaluminum, tri-branched-chain alkylaluminums such as triisopropylaluminum, triisobutylaluminum, tri-sec-butylaluminum, tri-tert-butylaluminum, tri-2-methylbutylaluminum, tri-3-methylhexylaluminum, and tri-2-ethylhexylaluminum, tricycloalkylaluminums such as tricyclohexylaluminum and tricyclooctylaluminum, triarylaluminums such as triphenylaluminum and tri(4-methylphenyl)aluminum, dialkylaluminum hydrides such as diisopropylaluminum hydride and diisobutylaluminum hydride, General formula (I-C4H9) X Al Y (C5H 10 ) Z (wherein X, Y, and Z are positive numbers and Z ≤ 2X.) Alkenylaluminums such as isoprenylaluminum represented by the formula, alkylaluminum alkoxides such as isobutylaluminum methoxide and isobutylaluminum ethoxide, dialkylaluminum alkoxides such as dimethylaluminum methoxide, diethylaluminum ethoxide, and dibutylaluminum butoxide, alkylaluminum sesquialkoxides such as ethylaluminum sesquiethoxide and butylaluminum sesquibutoxide, General formula R A 2.5 Al(OR B ) 0.5 Partially alkoxylated alkylaluminum having an average composition represented by the following formula: Alkyl aluminum aryloxides such as diethyl aluminum phenoxide and diethyl aluminum (2,6-di-tert-butyl-4-methylphenoxide); Dialkylaluminum halides such as dimethylaluminum chloride, diethylaluminum chloride, dibutylaluminum chloride, diethylaluminum bromide, and diisobutylaluminum chloride; Alkyl aluminum sesquihalides such as ethyl aluminum sesquichloride, butyl aluminum sesquichloride, and ethyl aluminum sesquibromide; partially halogenated alkylaluminums, such as alkylaluminum dihalides, such as ethylaluminum dichloride; dialkylaluminum hydrides such as diethylaluminum hydride and dibutylaluminum hydride; Alkyl aluminum dihydrides such as ethyl aluminum dihydride, propyl aluminum dihydride and other partially hydrogenated alkyl aluminums; Examples include partially alkoxylated and halogenated alkylaluminums such as ethylaluminum ethoxy chloride, butylaluminum butoxy chloride, and ethylaluminum ethoxy bromide. In addition, the above general formula R A M Al(OR B ) N H P X Q Compounds similar to the compound represented by the formula (1) can also be used, such as organoaluminum compounds in which two or more aluminum compounds are bonded via nitrogen atoms. Specific examples of such compounds include (C2H5)2AlN(C2H5)Al(C2H5)2.

[0083] Organometallic compounds of Group 13 of the Periodic Table (Q-1B); general formula M 2 AlR A A complex alkylation product of aluminum and a metal from Group 1 of the periodic table, represented by 4. (In the formula, M 2 indicates Li, Na or K, and R A represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms. Organometallic compounds in group 13 of the periodic table (Q-1B) include LiAl(C2H5)4, LiAl(C7H 15 ) 4 can be given as an example.

[0084] Organometallic compounds of Group 13 of the Periodic Table (Q-1C); general formula R A R B M 3 Dialkyl compounds of metals in Group 2 or 12 of the periodic table, represented by the formula: (In the formula, R A and R B may be the same or different and each represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms; M 3 is Mg, Zn or Cd.)

[0085] As the organoaluminum oxy compound (Q-2), a conventionally known aluminoxane can be used as it is. Specifically, the compound represented by the following general formula [III] and the compound represented by the following general formula [IV] can be mentioned.

[0086] [ka]

[0087] In the general formulas [III] and [IV], R represents a hydrocarbon group having 1 to 10 carbon atoms, and n represents an integer of 2 or more. In particular, methylaluminoxanes in which R is a methyl group and n is at least 3, preferably at least 10, are used. There is no problem if these aluminoxanes contain a small amount of an organoaluminum compound.

[0088] When copolymerization of ethylene with an α-olefin having 3 or more carbon atoms is carried out at high temperatures, benzene-insoluble organoaluminum oxy compounds as exemplified in JP-A-2-78687 can also be used. In addition, organoaluminum oxy compounds as described in JP-A-2-167305, and aluminoxanes having two or more alkyl groups as described in JP-A-2-24701 and JP-A-3-103407 can also be suitably used. The "benzene-insoluble organoaluminum oxy compounds" that may be used in the present invention are compounds that are insoluble or poorly soluble in benzene, and that have an Al component that dissolves in benzene at 60°C in terms of Al atoms of usually 10% or less, preferably 5% or less, and particularly preferably 2% or less.

[0089] Further, the organoaluminum oxy compound (Q-2) may also include modified methylaluminoxanes as represented by the following general formula [V].

[0090] [ka]

[0091] In general formula [V], Rx represents a hydrocarbon group having 1 to 10 carbon atoms, and m and n each independently represent an integer of 2 or greater. In addition, in general formula [V], "Me" represents a methyl group.

[0092] Methylaluminoxane, an example of an organoaluminum oxy compound (Q-2), is readily available and has high polymerization activity, and is therefore commonly used as an activator in polyolefin polymerization. However, since methylaluminoxane is difficult to dissolve in saturated hydrocarbons, it has been used as a solution in aromatic hydrocarbons such as toluene or benzene, which are environmentally undesirable. For this reason, flexible bodies of methylaluminoxane represented by formula [V] have been developed and used in recent years as aluminoxanes dissolved in saturated hydrocarbons. The modified methylaluminoxane represented by the general formula [V] is prepared using trimethylaluminum and alkylaluminum other than trimethylaluminum, for example, trimethylaluminum and triisobutylaluminum, as shown in, for example, U.S. Pat. No. 4,960,878 and U.S. Pat. No. 5,041,584. Aluminoxanes in which Rx in the general formula [V] is an isobutyl group are commercially available in the form of saturated hydrocarbon solutions under the trade names MMAO and TMAO (see Tosoh Finechem Corporation, Tosoh Research & Technology Review, Vol 47, 55 (2003)).

[0093] Further, the organoaluminum oxy compound (Q-2) may also include a boron-containing organoaluminum oxy compound represented by the following general formula [VI].

[0094] [ka]

[0095] In general formula [VI], R c R represents a hydrocarbon group having 1 to 10 carbon atoms. d may be the same or different and represent a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms.

[0096] Examples of the compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair (hereinafter sometimes abbreviated as "ionized ionic compound" or simply "ionic compound") include Lewis acids, ionic compounds, borane compounds, and carborane compounds described in JP-T-1-501950, JP-T-1-502036, JP-A-3-179005, JP-A-3-179006, JP-A-3-207703, JP-A-3-207704, and U.S. Pat. No. 5,321,106. Further examples include heteropoly compounds and isopoly compounds.

[0097] The ionizing ionic compound is preferably a boron compound represented by the following general formula [VII].

[0098] [ka]

[0099] In general formula [VII], R e+ As for H + , carbenium cation, oxonium cation, ammonium cation, phosphonium cation, cycloheptyltrienyl cation, ferrocenium cation having a transition metal, etc. f ~R i may be the same or different and are substituents selected from a hydrocarbon group having 1 to 20 carbon atoms, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a halogen atom and a halogen-containing group, and are preferably substituted aryl groups.

[0100] Specific examples of the carbenium cation include tri-substituted carbenium cations such as triphenylcarbenium cation, tris(4-methylphenyl)carbenium cation, and tris(3,5-dimethylphenyl)carbenium cation.

[0101] Specific examples of the ammonium cation include trialkyl-substituted ammonium cations such as trimethylammonium cation, triethylammonium cation, tri(N-propyl)ammonium cation, triisopropylammonium cation, tri(N-butyl)ammonium cation, and triisobutylammonium cation; N,N-dialkylanilinium cations such as N,N-dimethylanilinium cation, N,N-diethylanilinium cation, and N,N-2,4,6-pentamethylanilinium cation; and dialkylammonium cations such as diisopropylammonium cation and dicyclohexylammonium cation.

[0102] Specific examples of the phosphonium cation include triarylphosphonium cations such as triphenylphosphonium cation, tris(4-methylphenyl)phosphonium cation, and tris(3,5-dimethylphenyl)phosphonium cation.

[0103] R e+ Of the above specific examples, preferred are carbenium cations and ammonium cations, with triphenylcarbenium cation, N,N-dimethylanilinium cation and N,N-diethylanilinium cation being particularly preferred.

[0104] Among the ionized ionic compounds, examples of compounds containing a carbenium cation include triphenylcarbenium tetraphenylborate, triphenylcarbenium tetrakis(pentafluorophenyl)borate, triphenylcarbenium tetrakis{3,5-di-(trifluoromethyl)phenyl}borate, tris(4-methylphenyl)carbenium tetrakis(pentafluorophenyl)borate, and tris(3,5-dimethylphenyl)carbenium tetrakis(pentafluorophenyl)borate.

[0105] Among ionized ionic compounds, compounds containing a trialkyl-substituted ammonium cation include triethylammonium tetraphenylborate, tripropylammonium tetraphenylborate, tri(N-butyl)ammonium tetraphenylborate, trimethylammonium tetrakis(4-methylphenyl)borate, trimethylammonium tetrakis(2-methylphenyl)borate, tri(N-butyl)ammonium tetrakis(pentafluorophenyl)borate, triethylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(2,4-dimethylphenyl)borate, tri(N-butyl)ammonium tetrakis(3,5-dimethylphenyl)borate, tri(N-butyl)ammonium tetrakis{4-(trifluoromethyl)phenyl} ... Examples of the ammonium tetrakis{3,5-di(trifluoromethyl)phenyl}borate include tri(N-butyl)ammonium tetrakis(2-methylphenyl)borate, dioctadecylmethylammonium tetraphenylborate, dioctadecylmethylammonium tetrakis(4-methylphenyl)borate, dioctadecylmethylammonium tetrakis(4-methylphenyl)borate, dioctadecylmethylammonium tetrakis(pentafluorophenyl)borate, dioctadecylmethylammonium tetrakis(2,4-dimethylphenyl)borate, dioctadecylmethylammonium tetrakis(3,5-dimethylphenyl)borate, dioctadecylmethylammonium tetrakis{4-(trifluoromethyl)phenyl}borate, dioctadecylmethylammonium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, and dioctadecylmethylammonium.

[0106] Among the ionized ionic compounds, examples of compounds containing an N,N-dialkylanilinium cation include N,N-dimethylanilinium tetraphenylborate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, N,N-diethylanilinium tetraphenylborate, N,N-diethylanilinium tetrakis(pentafluorophenyl)borate, N,N-diethylanilinium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, N,N-2,4,6-pentamethylanilinium tetraphenylborate, and N,N-2,4,6-pentamethylanilinium tetrakis(pentafluorophenyl)borate.

[0107] Among the ionized ionic compounds, examples of compounds containing a dialkylammonium cation include di-N-propylammonium tetrakis(pentafluorophenyl)borate and dicyclohexylammonium tetraphenylborate.

[0108] In addition, the ionic compounds exemplified in JP-A-2004-51676 can also be used without any restrictions. The above ionic compounds (Q-3) may be used alone or in combination of two or more.

[0109] Examples of the catalyst include the following [1] to [4]. [1] An embodiment including a bridged metallocene compound (P) and a compound (Q-2) [2] An embodiment including a bridged metallocene compound (P), a compound (Q-1) and a compound (Q-2) [3] An embodiment including a bridged metallocene compound (P), a compound (Q-1) and a compound (Q-3) [4] An embodiment including a bridged metallocene compound (P), a compound (Q-2) and a compound (Q-3) The bridged metallocene compound (P) and the compounds (Q-1) to (Q-3) may be introduced into the reaction system in any order.

[0110] [Carrier (R)] The catalyst comprising the bridged metallocene compound (P) and the compound (Q) may further comprise a support (R). The carrier (R) may be an inorganic or organic compound, or a granular or fine particle solid. Among these, the inorganic compound is preferably a porous oxide, an inorganic chloride, a clay, a clay mineral, or an ion-exchangeable layered compound.

[0111] As the porous oxide, specifically, SiO2, Al2O3, MgO, ZrO, TiO2, B2O3, CaO, ZnO, BaO, ThO2, etc., or a composite or mixture containing these, such as natural or synthetic zeolite, SiO2-MgO, SiO2-Al2O3, SiO2-TiO2, SiO2-V2O5, SiO2-Cr2O3, SiO2-TiO2-MgO, etc. can be used. Of these, the carrier (R) is preferably one containing SiO2 and / or Al2O3 as the main component. The properties of such porous oxides vary depending on the type and manufacturing method, but the carrier (R) preferably has a particle size of 0.5 to 300 μm, more preferably 1.0 to 200 μm, and a specific surface area of ​​50 to 1000 m. 2 / g, more preferably 100 to 700m 2 / g and the pore volume is 0.3-3.0 cm 3 / g range. Such a support (R) is calcined at 100 to 1000° C., preferably 150 to 700° C., as required, before use.

[0112] Examples of inorganic chlorides that can be used include MgCl2, MgBr2, MnCl2, and MnBr2. The inorganic chlorides can be used as they are, or can be used after being pulverized by a ball mill or a vibration mill. In addition, the inorganic chlorides can be dissolved in a solvent such as alcohol, and then precipitated into fine particles using a precipitating agent.

[0113] Clay is usually composed of clay minerals as the main component. In addition, an ion-exchangeable layered compound is a compound having a crystal structure in which the constituent faces are stacked in parallel with each other with a weak binding force due to ionic bonds, etc., and the ions contained in the compound are exchangeable. Most clay minerals are ion-exchangeable layered compounds. In addition, these clays, clay minerals, and ion-exchangeable layered compounds are not limited to natural products, and artificial synthetic products can also be used. In addition, examples of clays, clay minerals, and ion-exchangeable layered compounds include clays, clay minerals, and ionic crystalline compounds having layered crystal structures such as hexagonal close packing type, antimony type, CdCl2 type, and CdI2 type. Examples of such clays and clay minerals include kaolin, bentonite, kibushi clay, gairome clay, allophane, hisingerite, pyrophyllite, ummo group, montmorillonite group, vermiculite, ryokudeite group, palygorskite, kaolinite, nacrite, dickite, and halloysite. Examples of ion-exchangeable layered compounds include crystalline acid salts of polyvalent metals such as α-Zr(HAsO4)2·H2O, α-Zr(HPO4)2, α-Zr(KPO4)2·3H2O, α-Ti(HPO4)2, α-Ti(HAsO4)2·H2O, α-Sn(HPO4)2·H2O, γ-Zr(HPO4)2, γ-Ti(HPO4)2, and γ-Ti(NH4PO4)2·H2O. It is preferable that the clay and clay mineral are subjected to a chemical treatment. The chemical treatment is not particularly limited, and examples thereof include a surface treatment for removing impurities attached to the surface and a treatment for affecting the crystal structure of the clay. Specific examples of the chemical treatment include an acid treatment, an alkali treatment, a salt treatment, and an organic matter treatment.

[0114] The ion-exchangeable layered compound may be a layered compound in which the space between layers is expanded by utilizing the ion exchangeability and exchanging the exchangeable ions between layers with other large bulky ions. Such bulky ions play a role of supporting the layered structure and are usually called pillars. The introduction of another substance (guest compound) between the layers of the layered compound in this way is called intercalation. The guest compounds are cationic inorganic compounds such as TiCl4 and ZrCl4, metal alkoxides such as Ti(OR)4, Zr(OR)4, PO(OR)3, and B(OR)3 (R is a hydrocarbon group, etc.), [Al 13 O4(OH) 24 ] 7+ , [Zr4(OH) 14 ] 2+ , [Fe3O(OCOCH3)6] + These compounds may be used singly or in combination of two or more. In addition, when intercalating these compounds, polymers obtained by hydrolysis and polycondensation of metal alkoxides (R is a hydrocarbon group, etc.) such as Si(OR)4, Al(OR)3, Ge(OR)4, colloidal inorganic compounds such as SiO2, etc. can be coexisted. In addition, examples of pillars include oxides generated by intercalating the above metal hydroxide ions between layers and then dehydrating them with heat.

[0115] Of these, clay or clay minerals are preferred, and montmorillonite, vermiculite, pectolite, taeniolite and synthetic mica are particularly preferred. The organic compound as the carrier (R) may be a granular or fine particle solid having a particle size in the range of 0.5 to 300 μm. Specific examples include polymers produced mainly from α-olefins having 2 to 14 carbon atoms, such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene, or polymers produced mainly from vinylcyclohexane and styrene, and modified products thereof.

[0116] The method of use and order of addition of each component of the polymerization catalyst can be selected arbitrarily depending on the purpose. At least two or more of the components in the catalyst may be in contact with each other in advance. The bridged metallocene compound (P) (hereinafter also referred to as "component (P)") is usually 1 x 10 -9 ~1×10 -1 mol, preferably 1×10 -8 ~1×10 -2 It is used in amounts that equal mol.

[0117] The organometallic compound (Q-1) (hereinafter also referred to as "component (Q-1)") is used in an amount such that the molar ratio of component (Q-1) to the transition metal atom (M) in component (P) [(Q-1) / M] is generally 0.01 to 50,000, preferably 0.05 to 10,000.

[0118] The organoaluminum oxy compound (Q-2) (hereinafter also referred to as "component (Q-2)") is used in an amount such that the molar ratio [(Q-2) / M] of the aluminum atom in component (Q-2) to the transition metal atom (M) in component (P) is generally 10 to 5,000, preferably 20 to 2,000.

[0119] The ionic compound (Q-3) (hereinafter also referred to as "component (Q-3)") is used in an amount such that the molar ratio of component (Q-3) to the transition metal atom (M) in component (P) [(Q-3) / M] is generally 1 to 10,000, preferably 1 to 5,000.

[0120] The polymerization temperature is usually -50°C to 300°C, preferably 30 to 250°C, more preferably 100°C to 250°C, and further preferably 130°C to 200°C. In the polymerization temperature range, as the temperature increases, the solution viscosity during polymerization decreases and the heat of polymerization is easily removed. The polymerization pressure is usually normal pressure to 10 MPa gauge pressure (MPa-G), and preferably normal pressure to 8 MPa-G.

[0121] The polymerization reaction can be carried out in any of batch, semi-continuous and continuous systems. Furthermore, the polymerization can be carried out continuously in two or more polymerization vessels with different reaction conditions. The molecular weight of the resulting copolymer can be adjusted by changing the hydrogen concentration in the polymerization system or the polymerization temperature. It can also be adjusted by the amount of compound (Q) used. When hydrogen is added, the amount is suitably about 0.001 to 5,000 NL per kg of the resulting copolymer.

[0122] The polymerization solvent used in the liquid phase polymerization method (solution polymerization) is usually an inert hydrocarbon solvent, preferably a saturated hydrocarbon having a boiling point of 50° C. to 200° C. under normal pressure. Specific examples of the polymerization solvent include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene, and alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane, and particularly preferred are hexane, heptane, octane, decane, and cyclohexane. The α-olefin itself to be polymerized may be used as the polymerization solvent. Incidentally, aromatic hydrocarbons such as benzene, toluene, and xylene, and halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane can also be used as polymerization solvents, but from the viewpoints of reducing the burden on the environment and minimizing the effects on human health, it is preferable to reduce the amounts of these used.

[0123] The α-olefin polymer (B) may be either unmodified or modified. The modification method is the same as the modification method for the block copolymer containing a polymer block mainly composed of a vinyl aromatic compound and a polymer block mainly composed of a conjugated diene compound and / or its hydrogenated product, and the preferred embodiments are also the same.

[0124] When the α-olefin polymer (B) is a modified product, the position at which the vinyl compound or a derivative thereof is grafted is not particularly limited as long as it is bonded to any carbon atom of the α-olefin polymer. When the thermoplastic resin composition contains a modified α-olefin polymer (B), it is preferable because it is possible to adjust the affinity with non-polar resins, polar resins, metals, and inorganic materials such as carbon, silica, and silicone. Good affinity with non-polar resins, polar resins, metals, and inorganic materials is useful because it can be adapted to a wide range of resins and metals when used as an adhesive material such as a hot melt adhesive or a heat seal material.

[0125] The above-mentioned modified α-olefin polymer (B) (modified α-olefin polymer) can be prepared by various conventionally known methods, for example, the following method. (1) A method in which the above-mentioned α-olefin polymer is mixed in an extruder, a batch reactor, or the like, and a vinyl compound having a polar group or a derivative thereof is added to carry out graft copolymerization. (2) A method in which the above-mentioned α-olefin polymer is dissolved in a solvent and a vinyl compound having a polar group or a derivative thereof is added to carry out graft copolymerization. In any of the above methods, the graft reaction is preferably carried out in the presence of a radical initiator in order to efficiently graft copolymerize the graft monomer of the vinyl compound or derivative thereof having a polar group.

[0126] As the radical initiator, for example, organic peroxides, azo compounds, etc. are used. As the organic peroxides, benzoyl peroxide, dichlorobenzoyl peroxide, dicumyl peroxide, etc. are listed, and as the azo compounds, azobisisobutylnitrile, dimethylazoisobutyrate, etc. are listed. As such radical initiators, specifically, dialkyl peroxides such as dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and 1,4-bis(tert-butylperoxyisopropyl)benzene are preferably used.

[0127] The graft amount of the vinyl compound having a polar group in the thus obtained modified α-olefin polymer (B) is usually 0.01 to 30 mass%, preferably 0.1 to 20 mass%, based on 100 mass% of the mass of the modified olefin polymer.

[0128] <<Content of α-olefin polymer (B)>> The content of the α-olefin polymer (B) is preferably from 0.01 to 95 mass %, more preferably from 0.1 to 75 mass %, and further preferably from 1 to 60 mass %, based on the total mass of the thermoplastic resin composition.

[0129] The content of the α-olefin polymer (B) is preferably 0.01% by mass or more, since the effect of improving flowability and imparting flexibility due to the α-olefin polymer (B) is fully exhibited. On the other hand, the content of the α-olefin polymer (B) is preferably 95% by mass or less, since the deterioration of the mechanical properties and heat resistance of the resin composition, bleed-out, etc. are suppressed. The content of the α-olefin polymer (B) is preferably within the range of 0.01 to 95% by mass, since bleed-out is suppressed and a resin composition having excellent flowability and flexibility can be easily obtained without impairing the mechanical properties and heat resistance.

[0130] <Adhesive resin (C)> The thermoplastic resin composition may contain, in addition to the above-mentioned thermoplastic resin (A) and α-olefin polymer (B), an adhesive resin (C) as necessary. In particular, when the thermoplastic resin composition is used as a resin composition for hot melt adhesives, it is preferred that the composition contains a tackifying resin (C). When the adhesive resin (C) is contained, the viscosity of the thermoplastic resin composition during melting is adjusted, and the hot tackiness and wettability are improved. When the adhesive resin (C) is contained, the molecules of the α-olefin polymer (B) contained in the thermoplastic resin composition become entangled with the molecular chains of the thermoplastic resin (A), thereby interacting with the thermoplastic resin (A) and uniformly softening it. This makes it easier for the adhesive resin (C) to exhibit good dispersibility, and as a result, it is useful because it makes it easier to obtain a thermoplastic resin composition with excellent hot tack properties and wettability.

[0131] The adhesive resin (C) is not particularly limited, and any resin known as a tackifier can be used. Examples of the adhesive resin (C) include aliphatic hydrogenated tackifiers, rosin, modified rosin or ester compounds thereof, aliphatic petroleum resins, alicyclic petroleum resins, aromatic petroleum resins, copolymerized petroleum resins of aliphatic and aromatic components, low molecular weight styrene resins, isoprene resins, alkylphenol resins, terpene resins, hydrogenated terpene resins, coumarone-indene resins, and the like. The adhesive resin (C) may be used alone or in combination of two or more kinds.

[0132] When the thermoplastic resin composition contains an adhesive resin (C), the content of the adhesive resin (C) in the entire thermoplastic resin composition is not particularly limited, but is preferably 1 to 50 mass%, more preferably 15 to 45 mass%, and even more preferably 20 to 40 mass%. Thermoplastic resin compositions containing such an amount of adhesive resin (C) are preferred because they can be used for producing conventional molded articles, as well as for adhesives and pressure-sensitive adhesives such as hot melt adhesives, heat sealing materials, and adhesive tapes. In particular, when the thermoplastic resin composition is a resin composition for hot melt adhesives, the content of the adhesive resin (C) in the entire thermoplastic resin composition is preferably 15 to 70 mass %, more preferably 20 to 60 mass %.

[0133] The thermoplastic resin composition may contain a softener. Examples of the softener include known softeners such as process oil, lubricating oil, paraffin, liquid paraffin, polyethylene wax, polypropylene wax, petroleum-based substances including petroleum asphalt and Vaseline, coal tars including coal tar and coal tar pitch, fatty oils including castor oil, linseed oil, rapeseed oil, soybean oil and coconut oil, tall oil, beeswax, carnauba wax and lanolin, fatty acids or metal salts thereof including ricinoleic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, montanic acid, oleic acid and erucic acid, synthetic polymers including petroleum resin, coumarone-indene resin and atactic polypropylene, ester-based plasticizers including dioctyl phthalate, dioctyl adipate and dioctyl sebacate, microcrystalline wax, liquid polybutadiene or its modified or hydrogenated product, and liquid thiokol. The content of the softener is preferably 1 to 50 mass %, more preferably 5 to 40 mass %, and further preferably 10 to 30 mass %, based on the total mass of the thermoplastic resin composition. The softener may be one type alone or two or more types.

[0134] <<Additives (D)>> The thermoplastic resin composition may contain, as necessary, additives (D) such as stabilizers such as antioxidants, ultraviolet absorbers, and light stabilizers, and additives (D) such as metal soaps, fillers, flame retardants, antibacterial agents, antifungal agents, pigments, foaming agents, and crosslinking agents. Examples of the stabilizer include antioxidants such as hindered phenol compounds, phosphite compounds, and thioether compounds; ultraviolet absorbers such as benzotriazole compounds and benzophenone compounds; and light stabilizers such as hindered amine compounds. Among these, as the stabilizer, antioxidants are preferred, and hindered phenol compounds are more preferred. Examples of the metal soap include stearates such as magnesium stearate, calcium stearate, barium stearate, and zinc stearate.

[0135] Examples of the filler include glass fiber, silica fiber, metal fiber (stainless steel, aluminum, titanium, copper, etc.), natural fiber (wood flour, wood fiber, bamboo, bamboo fiber, cotton, cellulose, nanocellulose, wool, straw, hemp, flax, kenaf, kapok, jute, ramie, sisal, henequen, corn, nut shells, wood pulp, rayon, cotton, etc.), carbon black, graphite, activated carbon, graphite, single-walled carbon nanotubes, multi-walled carbon nanotubes, carbon nanofibers, carbon nanohorns, graphene nanoplatelets, nanoporous carbon, carbon fibers, silica, glass beads, and silicic acid. Examples of suitable fillers include salts (calcium silicate, talc, clay, etc.), metal oxides (iron oxide, titanium oxide, magnesium oxide, alumina, etc.), metal carbonates (calcium carbonate, barium carbonate, etc.), sulfates (calcium sulfate, barium sulfate, etc.) and various metal (magnesium, silicon, aluminum, titanium, copper, etc.) powders, mica, glass flakes, pumice powder, pumice balloons, aluminum hydroxide, magnesium hydroxide, basic magnesium carbonate, dolomite, calcium titanate, calcium sulfite, asbestos, montmorillonite, bentonite, molybdenum sulfide, organic fillers (lignin, starch, etc.), and products containing these. In particular, fillers having anisotropy in their structure, such as glass fibers, silica fibers, metal fibers, natural fibers, carbon nanotubes, carbon nanofibers, carbon nanohorns, and carbon fibers, are prone to breaking due to shear during kneading, resulting in a decrease in anisotropy and loss of their characteristics. However, the α-olefin polymer (B) is useful because it reduces shear during kneading due to its flow-improving effect, making it easier to maintain the anisotropy. In addition, the thermoplastic resin composition is useful because the molecular chains of the α-olefin polymer (B) become entangled with the molecular chains of the thermoplastic resin (A), thereby interacting with the thermoplastic resin (A) and uniformly softening the thermoplastic resin (A), which is believed to make the filler more likely to exhibit good dispersibility.

[0136] Examples of the flame retardant include halogenated diphenyl ethers such as degabromo diphenyl ether and octabromo diphenyl ether, halogenated polycarbonates, and other halogen compounds, inorganic compounds such as antimony trioxide, antimony tetraoxide, antimony pentoxide, sodium pyroantimonate, and aluminum hydroxide, and phosphorus compounds. Compounds such as tetrafluoroethylene can be added as flame retardant assistants to prevent dripping. It is believed that the thermoplastic resin composition can be uniformly softened while interacting with the thermoplastic resin (A) because the molecular chains of the α-olefin polymer (B) become entangled with the molecular chains of the thermoplastic resin (A), which makes it easier for the flame retardant to exhibit good dispersibility. As a result, it is useful because it is easier to reduce the amount of flame retardant required to be added and to obtain a good flame retardant effect.

[0137] Examples of the antibacterial and antifungal agents include organic compounds such as imidazole compounds, thiazole compounds, nitrile compounds, haloalkyl compounds, and pyridine compounds; and inorganic substances and compounds such as silver, silver-based compounds, zinc-based compounds, copper-based compounds, and titanium-based compounds.

[0138] The pigments may be any pigment that has been conventionally used to color synthetic resins. Specifically, metals such as aluminum, silver, and gold; carbonates such as calcium carbonate and barium carbonate; oxides such as ZnO and TiO2; hydroxides such as Al2O3·nH2O and Fe2O3·nH2O; sulfates such as CaSO4 and BaSO4; nitrates such as Bi(OH)2NO3; chlorides such as PbCl2; chromates such as CaCrO4 and BaCrO4; chromates, manganates, and permanganates such as CoCrO4. phosphates;borates such as Cu(BO)2;uranates such as Na2U2O7·6H2O;nitrites such as K3Co(NO2)6·3H2O;silicates such as SiO2;arsenates and arsenites such as CuAsO3·Cu(OH)2;acetates such as Cu(C2H3O2)2·Cu(OH)2;phosphates such as (NH4)2MnO2(P2O7)2;aluminates, molybdates, zincates, antimonates, tungstates, etc. Inorganic pigments such as fluorides, titanates, iron cyanides, phthalates, CaS, ZnS, CdS, graphite, and carbon black; natural organic pigments such as cochineal lake and madder lake; nitroso pigments such as naphthol green Y and naphthol green B; nitro pigments such as naphthol yellow S and pigment chlorin 2G; azo pigments such as permanent red 4R, hansa yellow, brilliant carmine 68, and scarlet 2R; basic dye lakes such as malacaine green and rhodamine B; acid dye lakes such as acid, green lake, and eosin lake; mordant dye lakes such as alizarin lake and purpurin lake; vat dye pigments such as thio-indigo red B and instanthrene orange; and phthalocyanine pigments such as phthalocyanine blue and phthalocyanine green.

[0139] It is believed that the thermoplastic resin composition can be uniformly softened while interacting with the thermoplastic resin (A) because the molecular chains of the α-olefin polymer (B) become entangled with the molecular chains of the thermoplastic resin (A), which makes it easier for the pigment to exhibit good dispersibility. As a result, it is useful because it is easier to reduce the amount of pigment required to be added and to achieve a good color development effect.

[0140] Examples of the foaming agent include azo compounds such as azodicarbonamide (ADCA), 1,1'-azobis(1-acetoxy-1-phenylethane), dimethyl-2,2'-azobisbutyrate, dimethyl-2,2'-azobisisobutyrate, 2,2'-azobis(2,4,4-trimethylpentane), 1,1'-azobis(cyclohexane-1-carbonitrile), and 2,2'-azobis[N-(2-carboxyethyl)-2-methyl-propionamidine]; nitroso compounds such as N,N'-dinitrosopentamethylenetetramine (DPT); and hydrazine derivatives such as 4,4'-oxybis(benzenesulfonylhydrazide) and diphenylsulfone-3,3'-disulfonylhydrazide. Examples of the foaming agent include organic foaming agents such as organic bodies; semicarbazide compounds such as p-toluenesulfonylsemicarbazide; organic thermal decomposition type foaming agents such as trihydrazinotriazine; bicarbonates such as sodium hydrogen carbonate and ammonium hydrogen carbonate, carbonates such as sodium carbonate and ammonium carbonate; nitrites such as ammonium nitrite, and inorganic thermal decomposition type foaming agents such as hydrogen compounds; and organic physical foaming agents such as various aliphatic hydrocarbons such as methanol, ethanol, propane, butane, pentane, hexane, etc.; various chlorinated hydrocarbons such as dichloroethane, dichloromethane, carbon tetrachloride, etc.; and various fluorinated chlorinated hydrocarbons such as fluorocarbons; and inorganic physical foaming agents such as air, carbon dioxide, nitrogen, argon, water, etc.

[0141] The foaming agent may be used together with a foaming assistant, if necessary. Specific examples of the foaming assistant include zinc oxide (ZnO), zinc stearate, organic acids such as salicylic acid, phthalic acid, stearic acid, and oxalic acid, and urea or its derivatives.

[0142] It is believed that the thermoplastic resin composition can be softened uniformly while interacting with the thermoplastic resin (A) by forming entanglements between the molecular chains of the α-olefin polymer (B) and the molecular chains of the thermoplastic resin (A), and therefore the foaming agent can be easily dispersed. As a result, it is believed that a uniform foam structure can be obtained, and a thermoplastic resin composition excellent in flexibility, light weight, resilience, and low compression set can be easily obtained, which is useful.

[0143] Examples of the crosslinking agent include organic peroxide crosslinking agents such as dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3,1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, N-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, P-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl peroxybenzoate, tert-butyl perbenzoate, tert-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.

[0144] The crosslinking agent may be used together with a crosslinking aid, if necessary. Specific examples of the crosslinking aid include organic peroxide crosslinking aids such as sulfur, p-quinone dioxime, p,p'-dibenzoylquinone dioxime, N-methyl-N-4-dinitrosoaniline, nitrosobenzene, diphenyl guanidine, and trimethylolpropane-N,N'-m-phenylenedimaleimide; or divinylbenzene, triallyl cyanurate (TAC), and triallyl isocyanurate (TAIC). In addition, polyfunctional methacrylate monomers such as ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, and allyl methacrylate, and polyfunctional vinyl monomers such as vinyl butyrate and vinyl stearate are also included.

[0145] It is believed that the molecular chains of the α-olefin polymer (B) in the thermoplastic resin composition are entangled with the molecular chains of the thermoplastic resin (A) to uniformly soften the thermoplastic resin (A) while interacting with the thermoplastic resin (A), which makes it easier for the crosslinking agent and crosslinking aid to exhibit good dispersibility. As a result, a uniform crosslinked structure is obtained, which is useful because it makes it easier to obtain a thermoplastic resin composition that is excellent in tensile strength, heat resistance, resilience, and low compression set.

[0146] When the thermoplastic resin composition is a resin composition for hot melt adhesives, among these, the additive (D) is preferably a stabilizer, more preferably an antioxidant, and further preferably a hindered phenol compound.

[0147] The above additives can be used in any proportion and by any addition method as long as the effects of the present invention are not impaired. When the thermoplastic resin composition is a resin composition for hot melt adhesives, the content of additive (D) in the entire thermoplastic resin composition is preferably 0.1 to 10 mass%, more preferably 0.5 to 5 mass%, and even more preferably 1 to 3 mass%.

[0148] The thermoplastic resin composition preferably has a thermoplastic resin (A) content of 5 to 99.99% by mass (more preferably 10 to 90% by mass, and even more preferably 20 to 80% by mass), an α-olefin polymer (B) content of 0.01 to 95% by mass (more preferably 0.1 to 75% by mass, and even more preferably 1 to 60% by mass), an adhesive resin (C) content of 1 to 50% by mass (more preferably 15 to 45% by mass, and even more preferably 20 to 40% by mass), and an additive (D) content of 0.1 to 10% by mass (more preferably 0.5 to 5% by mass, and even more preferably 1 to 3% by mass). However, the total of the thermoplastic resin (A), the α-olefin polymer (B), the adhesive resin (C), and the additive (D) is taken as 100% by mass.

[0149] The glass transition point of the thermoplastic resin composition is preferably −56° C. or lower, more preferably −57° C. or lower, and even more preferably −58° C. or lower. There is no particular restriction on the lower limit, but it is preferably −80° C. or higher, more preferably −75° C. or higher, and even more preferably −70° C. or higher. When the pour point of the thermoplastic resin composition is within the above range, the thermoplastic resin composition tends to exhibit good low-temperature flexibility, and when used as an adhesive or pressure-sensitive adhesive such as a hot melt adhesive, a heat sealing material, or a pressure-sensitive adhesive tape, the composition can have improved conformability to uneven surfaces and adhesive properties at low temperatures. The glass transition point can be determined by differential scanning calorimetry (DSC), specifically, by the measurement method described in the examples below.

[0150] <Method of producing thermoplastic resin composition> The method for producing a thermoplastic resin composition includes a step of solution polymerizing ethylene and an α-olefin in the presence of a catalyst containing a bridged metallocene compound (P) represented by the following formula (1) and at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2) and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair (hereinafter also referred to as a "polymerization step"); a step of mixing the α-olefin polymer (B) obtained in the above step with a thermoplastic resin (A) containing at least one of a block copolymer containing a polymer block mainly composed of a vinyl aromatic compound and a polymer block mainly composed of a conjugated diene compound and a hydrogenated product thereof (hereinafter also referred to as a "mixing step"); The α-olefin polymer (B) satisfies the above requirements (b-2) to (b-5).

[0151] [ka]

[0152] In the above formula (1), R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 each independently represents a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and adjacent groups may be linked to each other to form a ring structure; R 6 and R 11 are the same group and each is a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, R 7 and R 10 are the same group and each is a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, R 6 and R 7 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 10 and R 11 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 6 , R 7 , R 10 and R 11 is not a hydrogen atom at the same time, Y is a carbon atom or a silicon atom; R 13 and R 14 each independently represents a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and may be linked together to form a ring structure, M is Ti, Zr or Hf; Q is independently a halogen atom, a hydrocarbon group, an anionic ligand, or a neutral ligand capable of coordinating to a lone pair of electrons; j is an integer from 1 to 4.

[0153] The bridged metallocene compound (P), organometallic compound (Q-1), organoaluminum oxy compound (Q-2) and compound (Q-3) which reacts with the bridged metallocene compound (P) to form an ion pair, as represented by formula 1, are the same as the bridged metallocene compound (P), organometallic compound (Q-1), organoaluminum oxy compound (Q-2) and compound (Q-3) which reacts with the bridged metallocene compound (P) to form an ion pair in the above-mentioned method for producing an ethylene-α-olefin copolymer, and preferred embodiments are also the same. The solution polymerization conditions in the solution polymerization step are the same as those in the above-mentioned method for producing an ethylene-α-olefin copolymer, and preferred embodiments are also the same.

[0154] The α-olefin polymer (B) and the thermoplastic resin (A) have the same meanings as the above-mentioned α-olefin polymer (B) and thermoplastic resin, and preferred embodiments are also the same.

[0155] [Mixing process] The mixing step is a step of mixing the α-olefin polymer (B) and the thermoplastic resin (A), and a thermoplastic resin composition containing the α-olefin polymer (B) and the thermoplastic resin (A) is obtained by the mixing step. In the mixing step, in addition to the α-olefin polymer (B) and the thermoplastic resin (A), a tackifying resin (C) and an additive (D) may be mixed.

[0156] The method for mixing the α-olefin polymer (B) and the thermoplastic resin (A) is not particularly limited, and any known method can be used. Examples of the method include a method of melt-kneading the thermoplastic resin (A), the α-olefin polymer (B), and, if necessary, the adhesive resin (C) and the additive (D) using a single-screw extruder, a twin-screw extruder, a plastomill, a Brabender, a kneader, a roll mixer, a Banbury mixer, or the like. For example, there may be mentioned a method in which the thermoplastic resin (A) and the α-olefin polymer (B) are dry-blended using a high-speed mixer such as a Henschel mixer, a tumbler, or the like, and then melt-kneaded using an extruder, or a method in which the α-olefin polymer (B) is added directly from an open part while the thermoplastic resin (A) is being melt-kneaded using an extruder, and then melt-kneaded by inserting it using a side feeder, a liquid feed pump, or the like. In addition, there may be mentioned a method in which the α-olefin polymer (B) is added using a master batch produced by melt-kneading a part of the thermoplastic resin (A) or other resins in advance, or a method in which the thermoplastic resin (A), the α-olefin polymer (B), or the like is filled into a melt bag made of polyethylene, ethylene-vinyl acetate copolymer, polybutene, polybutadiene, or the like.

[0157] The method for producing a thermoplastic resin composition may further include steps other than the above solution polymerization step and the mixing step (hereinafter, also referred to as "other steps"). Examples of the other steps include a step of preparing a thermoplastic resin (A) and a step of molding the obtained thermoplastic resin composition.

[0158] The hot melt adhesive of the present invention contains the above-mentioned thermoplastic resin composition. Among these, the thermoplastic resin composition of the present invention exhibits good fluidity and excellent flexibility in the low temperature range, and is therefore particularly suitable for applications such as hot melt adhesives used in automobile parts and industrial parts, heat sealing materials, adhesive tapes, and the like.

[0159] The thermoplastic resin composition of the present invention can be used for various purposes without any particular limitation. Specifically, the thermoplastic resin composition can be used for various purposes, such as hot melt adhesives, heat seal materials, adhesive tapes and other adhesives and pressure sensitive adhesives, sealants, electric wires, wires, cables, wire harnesses, linings, hoses, tubes, pipes, bottles, separators, molding materials, mandrels, belts, shock absorbing pads, protectors, helmets, guards and other protective equipment, golf clubs, tennis rackets, bats, tools and other various grip members, mouth guards, baseballs, tennis balls, golf balls and other various balls, vibration control pallets, shock absorbing dampers, insulators, shock absorbing materials for footwear, shock absorbing foams, toothbrushes, flooring materials, power tool members, agricultural equipment members, heat dissipation materials, transparent substrates. , soundproofing materials, cushioning materials, gaskets, caps, medicine stoppers, packing materials, cap liners, shoe soles, soles, midsoles, innersoles, soles and other shoe and sandal components, leather, nonwoven fabrics, fibers, cloth materials, films and sheets used for various purposes such as packaging, optics, release, heat transfer, electrical conductivity, dust prevention, transfer, protection, and shock absorption, bumpers, door trims, rear package trims, seat back garnishes, instrument panels, interior materials, exterior materials, masterbatches such as pellets, powders, and pastes containing fillers, pigments, oils, fibers, etc., extrusion molded products, injection molded products, hollow molded products, foam molded products, various molded products such as crosslinked molded products, building materials, automobile components, home appliance components, industrial components, clothing components, daily necessities components, kitchenware components, and sporting goods components. EXAMPLES

[0160] The present invention will be described in more detail below with reference to examples. In the following examples and comparative examples, the physical properties were measured or evaluated by the following methods.

[0161] [Melting Point] Measurements were performed using a differential scanning calorimetry (DSC) analyzer (Seiko Instruments Inc., model number: X-DSC-7000). Approximately 8 mg of the sample was placed in a sealable aluminum sample pan and placed in a DSC cell, and the DSC cell was heated from room temperature to 150°C at a rate of 10°C / min under a nitrogen atmosphere, then held at 150°C for 5 minutes, and then cooled at a rate of 10°C / min until the DSC cell was cooled to -100°C (cooling down process). Next, after keeping at -100°C for 5 minutes, the temperature was raised to 150°C at 10°C / min, and the temperature at which the enthalpy curve obtained during the heating process showed a maximum value was taken as the melting point (Tm), and the sum of the endothermic heats associated with melting was taken as the heat of fusion. If no peak was observed or the value of the heat of fusion was 1 J / g or less, it was considered that the melting point (Tm) was not observed. The melting point and heat of fusion were determined in accordance with JIS K7121.

[0162] [Weight average molecular weight (Mw)] The determination was made using the following high-speed GPC (gel permeation chromatography) measuring device. Measuring device: Tosoh Corporation, model number: HLC8320GPC Mobile phase: Tetrahydrofuran: THF (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., stabilizer-free, liquid chromatography grade) Column: Two TSKgel Super MultiporeHZ-M columns manufactured by Tosoh Corporation were connected in series. Sample concentration: 5mg / mL Mobile phase flow rate: 0.35mL / min Measurement temperature: 40℃ Standard sample for calibration curve: PStQuick MP-M, manufactured by Tosoh Corporation

[0163] 〔density〕 The density at 15°C was determined by the pycnometer method in accordance with JIS K2249-3.

[0164] [Kinematic viscosity] Based on ASTM D 445, the measurements were carried out using a viscometer for measuring dynamic viscosity (Canon Inc., product name: fully automatic viscometer CAV-4).

[0165] [Pour point] Based on JIS K2269, the measurement was carried out using an automatic pour point measuring device (manufactured by Tanaka Scientific Instruments Manufacturing Co., Ltd., model number: MPC-302).

[0166] [Glass transition temperature] The measurement was performed using a differential scanning calorimetry (DSC) analyzer (Seiko Instruments, model number: X-DSC-7000). Approximately 8 mg of the sample was placed in a simple, sealable aluminum sample pan and placed in a DSC cell. The DSC cell was heated from room temperature to 150°C at 10°C / min under a nitrogen atmosphere, then held at 150°C for 5 minutes, and then cooled at 10°C / min to -100°C (cooling down process). Next, the sample was held at -100°C for 5 minutes, and then heated to 150°C at 10°C / min, and the glass transition point was determined from the endothermic curve obtained during the heating process.

[0167] [Flexibility evaluation] The obtained thermoplastic resin composition was cut into a rectangular shape of 30 mm length × 10 mm width to prepare a test piece. Next, the dynamic viscoelasticity of the obtained test piece was measured in a nitrogen atmosphere at a temperature range of -70°C to 100°C using a viscoelasticity measuring device (manufactured by TA Instruments, model number: RSA-III) under conditions of a frequency of 1 Hz, a heating rate of 3°C / min, and a tensile mode. The obtained storage modulus was evaluated for flexibility according to the following evaluation criteria: When the storage modulus at temperature conditions of -30°C and -20°C is A or B, it can be said that the flexibility in the low temperature range is excellent. -Evaluation criteria- A: The storage modulus is 1 MPa or less. B: The storage modulus is more than 1 MPa and 50 MPa or less. C: The storage modulus is more than 50 MPa and is 100 MPa or less. D: The storage modulus exceeds 100 MPa.

[0168] The smaller the storage modulus value, the more excellent the flexibility, and therefore the adhesive or pressure-sensitive adhesive can conform even when the substrate is bent, and peeling of the adhesive or pressure-sensitive adhesive can be suppressed. Therefore, it can be said that the thermoplastic resin composition can be suitably used as an adhesive or pressure-sensitive adhesive for hot melt adhesives, heat seal materials, adhesive tapes, and the like.

[0169] [Adhesion Evaluation] A thermoplastic resin composition was applied onto a PP (polypropylene) film as an adherend to form an adhesive layer. Then, the PP (polypropylene) film as an adherend was placed on the adhesive layer and heat-sealed at 180°C and 1 MPa using a heat sealer to prepare a laminated sample consisting of the PP (polypropylene) film as an adherend / adhesive layer / PP film as an adherend. The laminated samples prepared above were subjected to T-peel tests (peel speed: 300 mm / min, width: 25 mm) at temperature conditions of -30°C, -20°C, 0°C, and 25°C. The obtained average peel strength (N / cm) was used to evaluate the adhesion according to the following evaluation criteria. When the average peel strength under temperature conditions of -30°C and -20°C is A or B, it can be said that the adhesiveness in the low temperature range is excellent. -Evaluation criteria- A: The average peel strength exceeds 6N / cm. B: Average peel strength is 6N / cm or less and exceeds 3N / cm. C: Average peel strength is 3N / cm or less and exceeds 1N / cm. D: The average peel strength is 1 N / cm or less.

[0170] The higher the average peel strength (i.e., adhesive strength), the more the substrates are prevented from peeling from each other, and therefore the thermoplastic resin composition can be suitably used as an adhesive or pressure-sensitive adhesive for hot melt adhesives, heat seal materials, adhesive tapes, etc. In particular, if the adhesive strength is excellent in the low temperature range, it can be said that the composition can be suitably used as an adhesive or pressure-sensitive adhesive even in a cold environment.

[0171] <Thermoplastic resin (A)> As the thermoplastic resin (A), a styrene-ethylene / butylene-styrene copolymer (manufactured by Kraton Polymers, product name: Kraton G1657) was used.

[0172] <α-Olefin polymer (B)> The α-olefin polymer (B) was produced by the following method.

[0173] [Production Example 1-1] (α-Olefin polymer (B-1)) In a 2-liter continuous polymerization reactor equipped with an agitator and thoroughly purifying the atmosphere with nitrogen, 1 liter of dehydrated and purified hexane was placed, and ethylaluminum sesquichloride (Al(C2H5) 1.5 ·Cl 1.5 ) in hexane at a rate of 500mL / h for 1 hour, and then a hexane solution of VO(OC2H5)Cl2 adjusted to 16mmol / L as a catalyst at a rate of 500mL / h and hexane at a rate of 500mL / h were continuously fed. Meanwhile, the polymerization solution was continuously extracted from the top of the reactor so that the polymerization solution in the reactor was always 1L. Next, ethylene gas was fed at a rate of 18L / h, propylene gas at a rate of 18L / h, and hydrogen gas at a rate of 120L / h using a bubbling tube. The copolymerization reaction was carried out at 35°C by circulating a coolant through a jacket attached to the outside of the reactor. As a result, a polymerization solution containing an ethylene-propylene copolymer was obtained. The obtained polymerization solution was washed three times with 500mL of 0.2mol / L hydrochloric acid per 1L of the polymerization solution, and then three times with 500mL of distilled water per 1L of the polymerization solution, dried over magnesium sulfate, and the solvent was distilled off under reduced pressure. The resulting viscous liquid was dried under reduced pressure at 130° C. for 24 hours to obtain an α-olefin polymer (B-1). The resulting α-olefin polymer (B-1) had a weight average molecular weight (Mw) of 1820 and a density of 833 kg / m 3 , Kinematic viscosity at 40°C: 155mm 2 / s, pour point: -50°C, and no melting point was observed.

[0174] [Production Example 1-2] (α-Olefin polymer (B-2)) 250 mL of decane was charged into a 1 L glass polymerization vessel that had been thoroughly purged with nitrogen, and the temperature inside the system was raised to 130°C. Then, ethylene was continuously fed into the vessel at a flow rate of 25 L / hr, propylene at 75 L / hr, and hydrogen at 360 L / hr, and the vessel was stirred at a rotation speed of 600 rpm. Next, 0.2 mmol of triisobutylaluminum was charged into the vessel, followed by 0.688 mmol of MMAO in terms of aluminum atom and [methylphenylmethylene (η 5 -cyclopentadienyl)(η 5 Polymerization was started by charging the mixture obtained by mixing 0.0023 mmol of 1,2-di-tert-butylfluorenyl)zirconium dichloride with toluene for 15 minutes or more into the polymerization vessel. Then, ethylene, propylene, and hydrogen were continuously fed, and polymerization was carried out at 130°C for 15 minutes. After stopping the polymerization by adding a small amount of isobutyl alcohol to the system, the unreacted monomers were purged. The obtained polymer solution was washed three times with 100 mL of 0.2 mol / L hydrochloric acid and then three times with 100 mL of distilled water, dried over magnesium sulfate, and the solvent was distilled off under reduced pressure. The obtained polymer was dried overnight under reduced pressure at 80°C to obtain α-olefin polymer (B-2). The obtained α-olefin polymer (B-2) had a weight average molecular weight (Mw): 2620 and a density: 837 kg / m 3 , Kinematic viscosity at 40°C: 380mm 2 / s, pour point: -40°C, and no melting point was observed.

[0175] [Production Example 1-3] (α-Olefin polymer (B-3)) 25 mL of decane was charged into a 1 L glass polymerization vessel that had been thoroughly purged with nitrogen, and the temperature inside the system was raised to 130°C. Then, ethylene was continuously fed into the vessel at a flow rate of 25 L / hr, propylene at 75 L / hr, and hydrogen at 360 L / hr, and the vessel was stirred at a rotation speed of 600 rpm. Next, 0.2 mmol of triisobutylaluminum was charged into the vessel, followed by 0.688 mmol of MMAO in terms of aluminum atom and [diphenylmethylene (η 5 -3-N-butylcyclopentadienyl)(η 5 Polymerization was started by charging the mixture obtained by mixing 0.0023mmol of 1,7-di-tert-butylfluorenyl)zirconium dichloride with toluene for 15 minutes or more into the polymerization vessel. Then, ethylene, propylene, and hydrogen were continuously fed, and polymerization was carried out at 130°C for 15 minutes. After stopping the polymerization by adding a small amount of isobutyl alcohol to the system, the unreacted monomer was purged. The obtained polymer solution was washed three times with 100mL of 0.2mol / L hydrochloric acid, then three times with 100mL of distilled water, dried over magnesium sulfate, and the solvent was distilled off under reduced pressure. The obtained polymer was dried overnight under reduced pressure at 80°C to obtain α-olefin polymer (B-3). The resulting α-olefin polymer (B-3) had a weight average molecular weight (Mw) of 2700 and a density of 838 kg / m 3 , Kinematic viscosity at 40°C: 400mm 2 / s, pour point: -39°C, and no melting point was observed.

[0176] <<Mineral oil>> The following mineral oils were used: (Z-1): Paraffin-based process oil, Diana Process Oil PW-90 (weight average molecular weight (Mw): 830, density: 872 kg / m, manufactured by Idemitsu Kosan Co., Ltd. 3 , Kinematic viscosity at 40°C: 90mm 2 / s, pour point: -15℃, melting point: -20℃) (Z-2): Paraffin-based process oil, Diana Process Oil PW-380 (weight average molecular weight (Mw): 1300, density: 879 kg / m, manufactured by Idemitsu Kosan Co., Ltd. 3 , Kinematic viscosity at 40°C: 390mm 2 / s, pour point: -15℃, melting point: -10℃)

[0177] <<Adhesive resin (C)>> As the adhesive resin (C), a C5C9 petroleum resin (manufactured by Eastman Chemical Company, trade name: Regalite C6100) was used.

[0178] <<Additives (D)>> As the additive (D), a hindered phenol-based antioxidant (manufactured by BASF Japan, trade name: Irganox 1010) was used.

[0179] Example 1 According to the compounding amounts shown in Table 1, the thermoplastic resin (A), α-olefin polymer (B) or mineral oil, adhesive resin (C), and antioxidant were melt-mixed in a separable glass flask equipped with a stirrer to obtain a thermoplastic resin composition (mixing conditions: 180°C, 60 minutes, 150 rpm). The obtained thermoplastic resin composition was subjected to measurement of physical properties and evaluation of flexibility and adhesion. The results are shown in Table 1.

[0180] [Examples 2-3 and Comparative Examples 1-2] A thermoplastic resin composition was obtained by mixing the components in the same manner as in Example 1, except that the composition was changed to that shown in Table 1. The physical properties of the obtained thermoplastic resin composition were measured, and the flexibility and adhesiveness were evaluated. The results are shown in Table 1.

[0181] [Table 1]

[0182] It can be seen that the thermoplastic resin compositions of Examples 1 to 3 are superior in flexibility in the low temperature range compared to the thermoplastic resin compositions of Comparative Examples 1 and 2, and the resulting hot melt adhesives have superior adhesive properties at low temperatures.< / j> < / q> < / m> < / y>

Claims

1. a thermoplastic resin (A) containing at least one of a block copolymer containing a polymer block mainly composed of a vinyl aromatic compound and a polymer block mainly composed of a conjugated diene compound, and a hydrogenated product thereof; An α-olefin polymer (B) that satisfies the following requirements (b-2) to (b-5); A thermoplastic resin composition comprising: (b-2) No melting point is observed as measured by differential scanning calorimetry (DSC); (b-3) the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,000 to 8,700; (b-4) Density measured by pycnometer method is 810 to 850 kg / m 3 is; (b-5) Kinematic viscosity at 40 ° C. is 10 to 9,800 mm 2 / s.

2. The thermoplastic resin composition according to claim 1, wherein the α-olefin polymer (B) satisfies the following requirement (b-6): (b-6) The pour point is less than -15°C.

3. The thermoplastic resin composition according to claim 1, wherein the α-olefin polymer (B) satisfies the following requirement (b-7): (b-7) Ethylene / α-olefin copolymer.

4. The thermoplastic resin composition according to claim 1, wherein the thermoplastic resin (A) is a hydrogenated product of a block copolymer containing a polymer block mainly composed of the vinyl aromatic compound and a polymer block mainly composed of a conjugated diene compound.

5. The thermoplastic resin composition according to claim 1 , further comprising a tackifying resin (C).

6. The thermoplastic resin composition of claim 1 further comprising an additive (D).

7. The thermoplastic resin composition according to claim 1, wherein the content of the thermoplastic resin (A) is 5 to 99.99% by mass, the content of the α-olefin polymer (B) is 0.01 to 95% by mass, the content of the adhesive resin (C) is 1 to 50% by mass, and the content of the additive (D) is 0.1 to 10% by mass (wherein the total of the thermoplastic resin (A), the α-olefin polymer (B), the adhesive resin (C), and the additive (D) is 100% by mass).

8. 2. The thermoplastic resin composition according to claim 1, which has a glass transition point of less than −56° C. as measured by differential scanning calorimetry (DSC).

9. A hot melt adhesive comprising the thermoplastic resin composition according to any one of claims 1 to 8.

10. 10. The hot melt adhesive of claim 9 for use in automotive or industrial parts.

11. a solution polymerization step of solution polymerizing ethylene and an α-olefin in the presence of a catalyst containing a bridged metallocene compound (P) represented by the following formula (1) and at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2) and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair; a step of mixing the α-olefin polymer (B) obtained in the solution polymerization step with a thermoplastic resin (A) containing at least one of a block copolymer containing a polymer block mainly composed of a vinyl aromatic compound and a polymer block mainly composed of a conjugated diene compound and a hydrogenated product thereof; Including, The method for producing a thermoplastic resin composition, wherein the α-olefin polymer (B) satisfies the following requirements (b-2) to (b-5): (b-2) No melting point is observed as measured by differential scanning calorimetry (DSC); (b-3) the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,000 to 8,700; (b-4) Density measured by pycnometer method is 810 to 850 kg / m 3 is; (b-5) Kinematic viscosity at 40 ° C. is 10 to 9,800 mm 2 / s. [Formula 1] [In formula 1, R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 each independently represents a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and adjacent groups may be linked to each other to form a ring structure; R 6 and R 11 are the same group and each is a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, R 7 and R 10 are the same group and each is a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, R 6 and R 7 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 10 and R 11 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 6 , R 7 , R 10 and R 11 is not a hydrogen atom at the same time, Y is a carbon atom or a silicon atom; R 13 and R 14 each independently represents a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and may be linked together to form a ring structure, M is a titanium atom, a zirconium atom, or a hafnium atom; Each Q is independently a halogen atom, a hydrocarbon group, an anionic ligand, or a neutral ligand capable of coordinating to a lone pair of electrons; j is an integer from 1 to 4.

12. R in the above (Formula 1) 13 and R 14 The method for producing a thermoplastic resin composition according to claim 11, wherein at least one of the following is an aryl group.

13. R in the above (Formula 1) 13 and R 14 are both aryl groups, and R 2 and R 3 The method for producing a thermoplastic resin composition according to claim 12, wherein either one of the above is a saturated hydrocarbon group having 4 carbon atoms.

Citation Information

Patent Citations

  • Hot melt hardenable pressure-sensitive adhesive

    JP2006241444A

  • Thermoplastic resin composition and use thereof

    JP2020196839A

Cited By