Method for producing carbonated slag
By crushing steelmaking slag granules during carbonation with controlled mechanical energy, the method achieves uniform and efficient carbonation, addressing incomplete carbonation and alkali elution issues in existing technologies.
Patent Information
- Application Number
- JP2023048658
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
AI Technical Summary
Existing methods for carbonating steelmaking slag face challenges in achieving uniform and efficient carbonation due to limitations in water content control, granule formation, and stirring speed, leading to incomplete carbonation and potential alkali elution.
A method involving crushing steelmaking slag granules during carbonation treatment to maintain a specific particle diameter ratio, using a cylindrical member to apply mechanical energy while controlling the rolling load, ensuring thorough carbonation without excessive particle reduction.
This approach enables uniform and efficient carbonation of steelmaking slag, reducing the risk of alkali elution and ensuring complete carbonation, thereby improving the quality and stability of the carbonated slag.
Smart Images

Figure 2024137218000001_ABST
Abstract
Description
[Technical field]
[0001] The present application discloses a method for producing carbonated slag by subjecting steelmaking slag to a carbonation treatment. [Background technology]
[0002] Steelmaking slag, such as pre-treated slag, converter slag, electric furnace slag, and casting slag, generated at steelworks, is used as a roadbed material, civil engineering and building material, and also as a base material for seaweed bed development and fertilizer in marine areas. Steelmaking slag contains water-soluble free CaO (free lime) and Ca(OH)2, so if steelmaking slag is used as it is as a material for the above, there is a problem that when it comes into contact with environmental water such as river water or seawater or rainwater, calcium ions and alkali (hydroxide ions) will be eluted, causing the water to become turbid.
[0003] To solve these problems, carbonation treatment, which involves reacting steelmaking slag with carbon dioxide, has been widely studied as a method for insolubilizing the water-soluble calcium components contained in steelmaking slag. In carbonation treatment, it is necessary to efficiently react the water-soluble calcium components contained in steelmaking slag, such as free CaO and Ca(OH)2, with carbon dioxide to generate CaCO3, and adding water is very effective in promoting the reaction. Therefore, in carbonation treatment of steelmaking slag, it is necessary to efficiently advance the carbonation reaction by controlling the supply rate of carbon dioxide-containing carbon dioxide gas, the water added to the steelmaking slag, and the relative humidity of the atmosphere. It is also known that stirring during carbonation treatment further promotes the carbonation reaction.
[0004] On the other hand, according to the findings of the present inventors, in the carbonation treatment method in which stirring is added, when the steelmaking slag is stirred, the slag particles are granulated through the water, and the gas containing carbon dioxide is less likely to penetrate into the inside of the granulated material, so that after the carbonation treatment, granulated material with the inside not carbonated is formed. In this case, a part of the granulated material may collapse during transportation or construction, and the slag that is not yet carbonated inside the granulated material may be exposed, which may cause a concern of alkali elution. In addition, if the moisture content in the steelmaking slag is increased to maximize the efficiency of the carbonation reaction, the amount of granulated material generated during and after the carbonation treatment also increases with the increase in moisture. For this reason, the increase in the amount of granulated material generated with the increase in the amount of added moisture has been an obstacle to uniformly carbonating the steelmaking slag.
[0005] Several solutions to these problems have been found. For example, Patent Document 1 proposes a method of suppressing the formation of granules during carbonation by drying steelmaking slag before carbonation to adjust the moisture content to a range of 0.5% by mass to 4% by mass. Patent Document 2 also proposes a method of suppressing the formation of granules during carbonation by adjusting the stirring Froude number in the carbonation to a certain range. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2014-234332 A [Patent Document 2] JP 2016-037409 A Summary of the Invention [Problem to be solved by the invention]
[0007] The method disclosed in Patent Document 1 has an upper limit on the amount of water added, and it is necessary to control the water during the carbonation treatment. Therefore, there is a problem that the water content is low, the carbonation reaction efficiency is low, and uniform carbonation treatment is difficult. In addition, the method disclosed in Patent Document 1 requires a complex mechanism for controlling the water content during the carbonation treatment. In the method disclosed in Patent Document 2, the stirring Froude number is stirred to a certain range in order to suppress the formation of granulated matter, so the stirring speed that would normally contribute to the carbonation reaction is limited. In other words, the fundamental inhibiting factor of the increase in the amount of granulated matter produced as the amount of water added increases cannot be eliminated, and there is room for improvement in causing the carbonation reaction to occur uniformly and efficiently.
[0008] As described above, a new technology is needed that can uniformly and efficiently carbonate steelmaking slag. [Means for solving the problem]
[0009] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A method for producing carbonated slag, comprising: Supplying carbon dioxide gas containing carbon dioxide to the steelmaking slag to perform carbonation treatment; In the carbonation treatment, the granulated steelmaking slag is crushed so that the average particle size D1 of the carbonated slag after the carbonation treatment is not less than the average particle size D2 of the steelmaking slag before the carbonation treatment. Method for producing carbonated slag. <Aspect 2> A method for producing a carbonated slag according to embodiment 1, comprising: The average particle diameter D2 of the steelmaking slag before the carbonation treatment is 7.0 mm or less; Method for producing carbonated slag. <Aspect 3> A method for producing carbonated slag according to embodiment 1 or 2, comprising the steps of: In the carbonation treatment, the granulated steel slag is crushed so that the ratio D1 / D2 of the average particle diameter D1 of the carbonated slag after the carbonation treatment to the average particle diameter D2 of the steel slag before the carbonation treatment is 1.00 or more and 1.50 or less. Method for producing carbonated slag. <Aspect 4> A method for producing carbonated slag according to any one of aspects 1 to 3, In the carbonation treatment, the granulated steel slag is crushed by contacting the granulated steel slag with a cylindrical member. Method for producing carbonated slag. Effect of the Invention
[0010] According to the technology disclosed herein, carbonation treatment can be performed uniformly and efficiently on steelmaking slag. [Brief description of the drawings]
[0011] [Figure 1] 1 illustrates a schematic diagram of a carbonation treatment device according to one embodiment. [Diagram 2] 1 shows a schematic representation of a cylindrical member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, a method for producing carbonated slag according to one embodiment will be described with reference to the drawings. The method for producing carbonated slag according to one embodiment includes supplying carbon dioxide gas containing carbon dioxide to steelmaking slag to perform a carbonation treatment. Here, the method for producing carbonated slag according to this embodiment is characterized in that, in the carbonation treatment, granulated material of the steelmaking slag is crushed so that the average particle size D1 of the carbonated slag after the carbonation treatment is not less than the average particle size D2 of the steelmaking slag before the carbonation treatment.
[0013] 1. Steelmaking slag The steelmaking slag to be carbonated in this embodiment is a by-product generated in the steelmaking process, and has the property of being a powder or granular material. The steelmaking slag may be at least one selected from, for example, converter slag, electric furnace slag, pre-treated slag, decarburization slag, desulfurization slag, dephosphorization slag, desiliconization slag, electric furnace oxidation slag, electric furnace reduction slag, secondary refining slag, and ingot slag. The steelmaking slag may be a powder or granular material of a mixture of these slags. The particle size of the steelmaking slag is not particularly limited, but it is desirable to adjust the particle size according to the use after the carbonation treatment. Note that if the particle size of the steelmaking slag is too large, the presence of raw material particles with a large particle size may hinder the compression and destruction of the smaller granular material when the granulated material of the steelmaking slag is crushed in the carbonation treatment. From the viewpoint of enabling the granulated material to be more appropriately disintegrated in the carbonation treatment, the average particle diameter D2 of the steelmaking slag before the carbonation treatment is preferably 9.0 mm or less, more preferably 7.0 mm or less. There is no particular limit to the lower limit of the average particle diameter D2. The average particle diameter D2 may be, for example, 1.0 mm or more and 9.0 mm or less, or 2.0 mm or more and 7.0 mm or less.
[0014] In this application, the average particle diameter D2 of steelmaking slag before carbonation and the average particle diameter D1 of carbonated slag after carbonation are weighted volume-based average diameters based on the moment notation method of "Expression of particle size measurement results (JIS Z 8819)" defined in the Japanese Industrial Standards.
[0015] 2. Carbonation treatment In this embodiment, carbon dioxide gas containing carbon dioxide is supplied to the steelmaking slag as described above, thereby subjecting the steelmaking slag to a carbonation treatment. In this embodiment, the conditions of the carbonation treatment may be the same as those of the conventional treatment, except that the granulated material described later is crushed. For example, in order to promote the carbonation treatment, water may be added to the steelmaking slag before or during the carbonation treatment. Furthermore, moisture may be supplied to the steelmaking slag together with carbon dioxide. The amount of carbon dioxide gas supplied, the amount of moisture added to the steelmaking slag, the relative humidity during the carbonation treatment, the carbonation treatment temperature, the carbonation treatment time, and the like are not particularly limited. For example, the amount of carbon dioxide gas supplied per 1 kg of steelmaking slag may be 0.1 liters / minute or more and 2.0 liters / minute or less. Furthermore, the amount of moisture per 1 kg of steelmaking slag may be 30 g or more and 120 g or less. Furthermore, the carbon dioxide gas supplied to the steelmaking slag may contain 50% to 99.9% carbon dioxide, and the water vapor in the carbonation treatment atmosphere may be 1.5 vol% or more. The carbonation temperature may be 5° C. or more and 40° C. or less. The carbonation time may be 30 minutes or more and 3.0 hours or less.
[0016] 3. Crushing of granulated material As described above, in the carbonation process, water is added to the steelmaking slag to promote the carbonation reaction. Here, the steelmaking slag to which water has been added is easily granulated through the water. According to the knowledge of the present inventor, if the steelmaking slag is granulated during the carbonation process, it becomes difficult to uniformly and efficiently proceed with the carbonation reaction. In order to solve such a problem, in this embodiment, the carbonation process of the steelmaking slag is progressed while the granulated steelmaking slag is crushed. For example, the granulated steelmaking slag can be crushed by applying mechanical energy to the granulated steelmaking slag. However, if the mechanical energy applied to the granulated steelmaking slag is too large, not only the granulated steelmaking slag is crushed, but also the raw material particles of the steelmaking slag are crushed and pulverized, and new surfaces that are not carbonated are exposed. As a result, even after the carbonation process of the steelmaking slag, the surfaces that are not carbonated remain, and there is a concern that calcium ions and alkali (hydroxide ions) may be eluted. In contrast, in this embodiment, while crushing the granulated steel slag, the raw material particles of the steel slag are prevented from being crushed or pulverized as much as possible in order to suppress exposure of the newly formed surfaces of the raw material particles of the steel slag. Specifically, in this embodiment, it is important to crush the granulated steel slag so that the average particle diameter D1 of the carbonated slag after the carbonation treatment is not less than the average particle diameter D2 of the steel slag before the carbonation treatment. Note that the "crushing of the granulated steel slag" in this application means a phenomenon in which mechanical energy is applied to the granulated steel slag composed of a plurality of slag particles (raw material particles) to break down the aggregation between the slag particles and disintegrate or break down (disintegrate (loosen)) the relatively large granulated steel slag particles into those having a relatively small particle size, and does not mean crushing or pulverizing the steel slag particles (raw material particles) themselves that constitute the granulated steel slag. In order to realize such "crushing of the granulated steel slag," it is effective to devise a means for crushing the granulated steel slag, as described later. Specifically, the granulated material can be "crushed" by applying a predetermined pressing load to the granulated material using a cylindrical member described below, for example.
[0017] As described above, in this embodiment, it is important to disintegrate the granulated steel slag so that the average particle diameter D1 of the carbonated slag after the carbonation treatment is not less than the average particle diameter D2 of the steel slag before the carbonation treatment. That is, the ratio D1 / D2 of the average particle diameter D1 of the carbonated slag after the carbonation treatment to the average particle diameter D2 of the steel slag before the carbonation treatment is 1.00 or more. The upper limit of the ratio D1 / D2 is not particularly limited. In one embodiment, the ratio D1 / D2 may be 1.00 or more and 1.50 or less. When the ratio D1 / D2 is 1.00 or more and 1.50 or less, the granulated steel slag is disintegrated more appropriately and reliably in the carbonation treatment. Note that, in this embodiment, it is sufficient that the granulated steel slag is disintegrated during the carbonation treatment, and it does not matter if the average particle diameter D1 of the carbonated slag increases as granulation progresses after the carbonation treatment. In this regard, in this embodiment, the ratio D1 / D2 may exceed 1.50.
[0018] 4. Specific examples of methods for crushing granulated materials Below, an example will be given of a form in which the steelmaking slag granules are crushed by contacting them with a cylindrical member during the carbonation treatment, but the crushing means used in this embodiment is not limited to the following.
[0019] 4.1 Drum Mixer FIG. 1 shows a schematic diagram of a carbonation treatment apparatus according to an embodiment. The carbonation treatment apparatus 10 shown in FIG. 1 is a drum mixer in which rolls or rods are installed as cylindrical members 2 inside the drum 1. When carbonation treatment of steelmaking slag is performed using such a carbonation treatment apparatus 10, first, steelmaking slag is put into the drum 1. Next, the steelmaking slag is stirred by the rotation of the drum 1 while continuously introducing carbon dioxide gas into the drum 1. During stirring, the rolls or rods as the cylindrical members 2 continue to rotate by the rotation of the drum 1 at the lower part inside the drum mixer. The granulated steelmaking slag formed during stirring is compressed and crushed by the rolls or rods. In the carbonation treatment apparatus 10 shown in FIG. 1, the granulated steelmaking slag can be crushed so that the average particle diameter D1 of the carbonated slag after carbonation treatment is not less than the average particle diameter D2 of the steelmaking slag before carbonation treatment by adjusting the rotation speed of the drum 1, the material of the rolls or rods as the cylindrical members 2, the size of the rolls or rods, and the number of rolls or rods.
[0020] For example, if the rotation speed of the drum 1 is slow, the granulated material does not enter the lower part of the roll or rod and is not crushed. Therefore, it is necessary to put a sufficient amount of steelmaking slag into the inside of the drum 1 and to make the granulated material flow vigorously inside the drum 1 under stirring. It is desirable to adjust the rotation speed of the drum so that the granulated material is in the normal cascade region or the lower discharge flow region described in Non-Patent Document 1 below. For example, when the Froude number is 15×10 -3 When the drum 1 is rotated so that the volume ratio of the raw material inside the drum is adjusted to about 8-13%, the normal cascade region is formed, and when the volume ratio is set to about 14% or more, the discharge flow lower region is formed.
[0021] [Non-patent document 1] Katsuhiko Sato: Fukisen, 28 (1981), p.99
[0022] 4.2 Mixmuller Kneader In the Mix-Muller type kneader, the steel slag can be carbonated while crushing the granulated steel slag. The Mix-Muller kneader is a device that stirs powdered raw materials with a wheel as a cylindrical member that rotates in conjunction with the stirrer, and can efficiently and uniformly mix liquid and powder. However, this device, which aims for uniform mixing, has a small compression area by the wheel and low crushing efficiency of the granulated material. In addition, it is generally known that the raw material particles are also crushed and pulverized at the same time, and when the Mix-Muller kneader is used under normal conditions, there is a risk that the raw material particles of the steel slag will be crushed and pulverized. Therefore, when using the Mix-Muller kneader, it is necessary to appropriately change the wheel dimensions and rolling load so that the raw material particles of the steel slag are not crushed and pulverized. Specifically, it is preferable to adjust the total rolling load of the wheel (cylindrical member) per 1 kg of slag to 0.5 to 5.0 (kgf / kg slag). In addition, the ratio of the side length to the bottom diameter of the wheel (cylindrical member) (side length ÷ bottom diameter) is preferably in the range of 0.5 to 7.0. Note that some Mixmuller kneaders have a device that increases the rolling load by hydraulic pressure or a spring, and in that case, the rolling load must be calculated taking into account the effect of the spring.
[0023] 4.3 Supplementary information for cylindrical members As described above, the cylindrical member is used to compress and crush the granulated material produced during the carbonation treatment of steel slag. As shown in FIG. 2, the cylindrical member 2 may have both bottom surfaces that are circular and have a certain length (side length) between the two bottom surfaces. As described above, the cylindrical member 2 may be any member that can crush the granulated material by contacting its side surface with the granulated material while rotating, and in this respect, the term "circle" does not necessarily have to be a perfect circle, and is a concept that includes an ellipse and the like. As described above, the cylindrical member 2 may be at least one type selected from a roll, a rod, a wheel, and the like.
[0024] As described above, under conditions where the mechanical compressive force of the cylindrical member 2 is too high, or under conditions where the cylindrical member 2 collides violently with the raw material particles at high speed, the raw material particles are crushed and pulverized, generating a large amount of new surfaces of uncarbonated steelmaking slag, which cause alkali elution. On the other hand, when the rolling load of the cylindrical member 2 is low, the granulated material cannot be crushed, resulting in a problem of reduced carbonation efficiency. In order to crush the granulated material while suppressing the crushing and pulverization of the raw material particles, for example, it is advisable to adjust the rolling load of the cylindrical member 2 per 1 kg of slag. The total rolling load of the cylindrical member 2 per 1 kg of slag is preferably, for example, 0.5 to 5.0 (kgf / kg slag). By adjusting the rolling load in this way, it is possible to control the average particle diameter D1 of the carbonated slag after the carbonation treatment not to be less than the average particle diameter D2 of the steelmaking slag before the carbonation treatment. The rolling load is a concept defined in the present application and is a load (force) applied in the vertical direction (gravity direction) by the cylindrical member 2 in a stationary state placed on a flat surface. The rolling load is gravity calculated by multiplying the mass of the cylindrical member 2 by the gravitational acceleration.
[0025] The material of the cylindrical member 2 is preferably determined so as to appropriately control the rolling load of the cylindrical member 2. The material of the cylindrical member 2 is not particularly limited, but considering the acquisition cost, ease of handling, wear resistance, and drop resistance (impact resistance), it is preferable to use a metal, and more preferably, a spheroidal graphite cast iron material in consideration of the balance between acquisition cost and wear resistance.
[0026] The dimensions of the cylindrical member 2 are preferably appropriately determined taking into consideration the rolling load, maximum speed, and actual workability. Although not particularly limited, it is preferable that the ratio of the side length to the bottom diameter (side length ÷ bottom diameter) is in the range of 0.5 to 7.0.
[0027] When the carbonation treatment device is provided with a plurality of cylindrical members 2, the raw material particles of the steelmaking slag may be crushed or pulverized due to collisions between the cylindrical members 2. In this regard, for example, when the above-mentioned drum mixer is used as the carbonation treatment device, the number of cylindrical members 2 (rolls or rods) provided in the drum mixer is preferably two or less, and more preferably one. On the other hand, in the case of a Mixmuller kneader, there is no particular limit to the number of cylindrical members 2 (wheels).
[0028] In addition, the steel slag granules may be broken down by the high-speed rotation of the stirring blades. However, in this case, since the steel slag is relatively hard, the stirring blades wear out quickly, and the stirring blades deteriorated by wear must be replaced frequently. This leads to an increase in downtime due to the replacement of the stirring blades, which may result in a significant decrease in processing efficiency. In addition, when using stirring blades or other stirring blades, the raw material particles of the steel slag may be crushed or pulverized by shearing. In this regard, in order to break down the granules while suppressing the generation of new surfaces caused by the crushing or pulverization of the raw material particles of the steel slag as much as possible without decreasing the average particle size of the steel slag in the carbonation process, it is better to break down the steel slag granules by bringing them into contact with a cylindrical member as described above, rather than breaking down the granules by the high-speed rotation of the stirring blades.
[0029] 5. Carbonated slag The above carbonation treatment can carbonate the particle surfaces of steelmaking slag to produce carbonated slag. As described above, according to the production method of this embodiment, the surface of the steelmaking slag can be uniformly and efficiently carbonated during the carbonation treatment while crushing the steelmaking slag granules, with as little generation of new surfaces of the raw material particles of the steelmaking slag as possible. In this embodiment, the carbonated slag is preferably carbonated over its entire surface.
[0030] As described above, in this embodiment, the average particle diameter D1 of the carbonated slag after the carbonation treatment is not less than the average particle diameter D2 of the steelmaking slag before the carbonation treatment. The average particle diameter D1 of the carbonated slag after the carbonation treatment is preferably 9.0 mm or less, more preferably 7.0 mm or less, depending on the average particle diameter D2 of the steelmaking slag before the carbonation treatment. There is no particular limit to the lower limit of the average particle diameter D1. The average particle diameter D1 may be, for example, 1.0 mm or more and 9.0 mm or less, or 2.0 mm or more and 7.0 mm or less. EXAMPLES
[0031] As described above, one embodiment of the present invention has been described. However, the present invention is not limited to the above embodiment, and various modifications are possible. For example, an embodiment obtained by appropriately combining the technical means disclosed in the above description is also included in the technical scope of the present invention. Below, the effects of the technology of the present disclosure will be described in more detail while showing examples, but the technology of the present disclosure is not limited to the following examples.
[0032] 1. Preparation of steel slag As the steelmaking slag before carbonation treatment, those classified into particle sizes of 10 mm or less after crushing and those classified into particle sizes of 7 mm or less were used.
[0033] 2. Carbonation treatment Carbonated slag was obtained by subjecting the steelmaking slag to a carbonation treatment. The carbonation treatment was carried out under the conditions shown in Table 1 below. A drum mixer, a rod mill tester, and a Mix Muller kneader were used as carbonation treatment devices. The drum mixer, the rod mill tester, and the Mix Muller kneader are all batch-type agitation treatment devices.
[0034] After the steelmaking slag was charged into the stirring vessel (drum), water was added to the steelmaking slag before stirring. When the grain size of the steelmaking slag was 10 mm or less, 7 mass% of the steelmaking slag mass was added, and when the grain size was 7 mm or less, 10 mass% of the steelmaking slag mass was added. During stirring, an acrylic lid was attached to the drum mixer and a stainless steel lid was attached to the rod mill tester, both of which were fixed with bolts to prevent the steelmaking slag from leaking out of the vessel during stirring. The Mixmuller kneader is originally a sealed stirring device, and the raw material inlet was closed and sealed.
[0035] In the mixing treatment using the drum mixer and rod mill tester, a hose was inserted through the circular opening in the center of the lid, and carbon dioxide gas (concentration 99.5 vol% or more) was allowed to flow in at a flow rate of 14 L / min. In the mixing treatment using the Mixmuller kneader, a hose was inserted through the opening (for adding liquid raw materials) at the top of the device, and carbon dioxide gas (concentration 99.5 vol% or more) was allowed to flow in at a flow rate of 30 L / min. The dimensions of the opening in the lid were 80 mmφ for the drum mixer and 30 mmφ for the rod mill tester. The mixing and carbonation treatment was carried out for 1.0 hour.
[0036] [Table 1]
[0037] 3. Evaluation of Carbonated Slag 3.1 pH measurement The pH of steelmaking slag before carbonation and the carbonated slag after carbonation were measured. Specifically, 150g of steelmaking slag or carbonated slag was placed in a 2.0L beaker containing 1.5L of pure water, then manually stirred with a stirring rod for 10 seconds and allowed to stand for 1 hour. After 1 hour, the mixture was manually stirred again with a stirring rod for 10 seconds, and the pH immediately after stirring was measured with a glass electrode pH meter. The stirring rod was rotated along the inner surface of the beaker at a stirring speed of 1 revolution per second. The pH of steelmaking slag before carbonation was 11.1 for slag with a particle size of 10mm or less, and 11.2 for slag with a particle size of 7mm or less.
[0038] 3.2 Measurement of average particle size The average particle size of the steelmaking slag before carbonation and the carbonated slag after carbonation was measured. Specifically, the particles were classified and weighed using mesh sieves with openings of 16.0 mm, 13.2 mm, 9.5 mm, 8.0 mm, 6.7 mm, 4.0 mm, 2.0 mm, 1.0 mm, 0.6 mm, 0.3 mm, 0.1 mm, and 0.053 mm, and the average particle size was calculated based on the weighted volume-based average size according to the moment notation method of the Japanese Industrial Standard "Expression of particle size measurement results (JIS Z 8819)".
[0039] 4. Evaluation Results Table 2 below shows the average particle diameter D2 of the steelmaking slag before the carbonation treatment, the average particle diameter D1 of the carbonated slag after the carbonation treatment, and the pH of the carbonated slag after the carbonation treatment.
[0040] [Table 2]
[0041] As shown in Table 2, the pH of the carbonated slag was 10.0 or less in all of Examples 1 to 5. In contrast, the pH of Comparative Examples 3, 6, and 7 was higher than that of Examples 1 to 5, specifically, the pH was 10.3 or more. In Comparative Examples 3, 6, and 7, the average particle size D1 of the carbonated slag after carbonation was smaller than the average particle size D2 of the steelmaking slag before carbonation, which is considered to be because the raw material particles of the steelmaking slag were crushed and pulverized in the carbonation, resulting in a large amount of new surfaces that were not carbonated.
[0042] Comparative Examples 1, 2, 4, and 5 had a higher pH than Examples 1 to 5, specifically, a pH of 10.2 or more. In Comparative Examples 1, 2, 4, and 5, the steelmaking slag was not subjected to pressure reduction during the carbonation treatment, and the steelmaking slag granules were not crushed, which is thought to be why carbonation did not progress inside the granules.
[0043] It is obvious that if the granulated steelmaking slag is crushed during the carbonation treatment of the steelmaking slag, the same effects as those of the above-mentioned Examples 1 to 5 can be obtained. In this regard, it does not matter if the average particle diameter D1 of the carbonated slag increases due to, for example, the progress of granulation after the carbonation treatment.
[0044] 5. Summary From the above results, it can be said that according to the manufacturing method of carbonated slag that satisfies the following (1) and (2), it is possible to uniformly and efficiently carbonate steelmaking slag. (1) A method for producing carbonated slag includes supplying carbon dioxide gas containing carbon dioxide to steelmaking slag to perform a carbonation treatment. (2) In the carbonation treatment, the granulated steelmaking slag is crushed so that the average particle diameter D1 of the carbonated slag after the carbonation treatment is not less than the average particle diameter D2 of the steelmaking slag before the carbonation treatment. [Explanation of symbols]
[0045] 1 drum 2 Cylindrical member 10 Carbonation treatment device (drum mixer)
Claims
1. A method for producing carbonated slag, comprising: Supplying carbon dioxide gas containing carbon dioxide to the steelmaking slag to perform carbonation treatment; In the carbonation treatment, the average particle diameter D of the carbonated slag after the carbonation treatment 1 is the average particle diameter D of the steelmaking slag before the carbonation treatment 2 The steel slag granules are crushed so that the particle size is not less than 1 / 2. Method for producing carbonated slag.
2. A method for producing carbonated slag according to claim 1, The average particle diameter D of the steelmaking slag before the carbonation treatment 2 is 7.0 mm or less; Method for producing carbonated slag.
3. A method for producing carbonated slag according to claim 1, In the carbonation treatment, the average particle diameter D of the carbonated slag after the carbonation treatment 1 and the average particle diameter D of the steelmaking slag before the carbonation treatment 2 Compared to D 1 / D 2 The steelmaking slag granules are crushed so that the ratio of the granules to the total granules is 1.00 or more and 1.50 or less. Method for producing carbonated slag.
4. A method for producing carbonated slag according to any one of claims 1 to 3, In the carbonation treatment, the granulated steel slag is crushed by contacting the granulated steel slag with a cylindrical member. Method for producing carbonated slag.
Citation Information
Patent Citations
Carbonization method for seel making slag
JP2014234332A
Carbonation treatment method of steelmaking slag
JP2015205794A
Carbonation treatment method of steel slag
JP2016037409A
Steel slag grain, steel slag, and method for producing steel slag grain
JP2016094664A
Processing method of steelmaking slags, manufacturing method of slag products, and processing system of steelmaking slags
JP2022038784A