Gas barrier film, laminated film, and packaging bag

The gas barrier film, comprising a liquid crystal polymer base layer and polyester resin auxiliary layer, addresses waste and tear strength issues in conventional laminated films, offering aluminum-free, recyclable, and high-strength gas barrier properties.

JP2024137283APending Publication Date: 2024-10-07FUJIMORI KOGYO CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023048748
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Conventional laminated films using aluminum-deposited polyester films generate waste with high CO2 emissions and disposal challenges, and liquid crystal polymers lack tear strength when used alone.

Method used

A gas barrier film composed of a base layer made of a liquid crystal polymer with a melting point of 230°C or less and an auxiliary layer of polyester resin, formed by polycondensation of a polyhydric carboxylic acid component and diethylene glycol, providing excellent gas barrier properties and tear strength.

Benefits of technology

The film achieves aluminum-free gas barrier properties with improved tear strength, recyclability, and reduced waste, suitable for use in production lines with metal detectors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137283000001_ABST
    Figure 2024137283000001_ABST
Patent Text Reader

Abstract

To provide an aluminum-free gas barrier film having excellent gas barrier properties and tear strength.SOLUTION: The gas barrier film according to one embodiment of the present invention includes a substrate layer and an auxiliary layer laminated on one surface of the substrate layer. The substrate layer comprises a liquid crystal polymer having a melting point of 230°C or lower and an isophthalic acid-modified polyethylene terephthalate modified with isophthalic acid. The auxiliary layer contains a polyester resin. The polyester resin is a polycondensate of a polycarboxylic acid component and a polyhydric alcohol component containing a diethylene glycol component.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas barrier film, a laminate film, and a packaging bag. [Background technology]

[0002] Conventionally, packaging bags made of a laminated film in which multiple layers are laminated on the inner surface of a base layer made of film, paper, etc., have been widely used as packaging bags for containing contents such as food, medicine, etc. Generally, the laminated film used in such packaging bags has a gas barrier property that blocks the intrusion of gases that deteriorate the contents, such as water vapor and oxygen, in order to suppress deterioration and spoilage of the contents and to maintain their functions and properties.

[0003] For example, Patent Document 1 discloses a packaging bag made by laminating a base layer / first adhesive layer / gas barrier layer / second adhesive layer / sealant layer in this order in a laminated film, with the sealant layer facing the inner surface, and then sealing to form a sealed portion. It also discloses that the gas barrier layer is a polyester film vapor-deposited with aluminum or an inorganic oxide, which provides excellent gas barrier properties and allows the quality of the fragrance to be maintained for a long time. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-5013 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in conventional laminated films, the gas barrier layer is often an aluminum-deposited polyester film or aluminum foil, and such aluminum-containing laminated films generate a large amount of CO2 during the manufacturing and disposal processes, and have the problem that they are difficult to separate and collect when disposed of. To address this problem, it is conceivable to use a liquid crystal polymer, which has excellent gas barrier properties, as the gas barrier layer, but the liquid crystal polymer has the disadvantage that it lacks tear strength when processed into a film by itself.

[0006] In view of the above, an object of one aspect of the present invention is to provide an aluminum-free gas barrier film having excellent gas barrier properties and tear strength. [Means for solving the problem]

[0007] A gas barrier film according to one embodiment of the present invention has a base layer and an auxiliary layer laminated on one side of the base layer, the base layer containing a liquid crystal polymer having a melting point of 230°C or less and an isophthalic acid-modified polyethylene terephthalate modified with isophthalic acid, and the auxiliary layer contains a polyester resin which is a polycondensate of a polyvalent carboxylic acid component and a polyhydric alcohol component containing a diethylene glycol component. Effect of the Invention

[0008] According to one aspect of the present invention, it is possible to provide an aluminum-free gas barrier film having excellent gas barrier properties and tear strength. [Brief description of the drawings]

[0009] [Figure 1] 1 is a schematic diagram showing a cross section of a gas barrier film according to one embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing a cross section of a laminated film according to one embodiment. [Diagram 3] 1 is a schematic diagram of a packaging bag according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In this specification, unless otherwise specified, the numerical range indicated by "to" means that the numerical range includes the numerical range before and after the range as the lower and upper limits.

[0011] (Gas barrier film) 1 is a schematic diagram showing a cross section of a gas barrier film 1 according to one embodiment. The gas barrier film 1 of this embodiment has a base layer 2 and an auxiliary layer 3 laminated on one surface of the base layer 2.

[0012] The base layer 2 contains a liquid crystal polymer (A) having a melting point of 230° C. or less and an isophthalic acid-modified polyethylene terephthalate (B) modified with isophthalic acid, and the auxiliary layer 3 contains a polyester resin (C), which is a polycondensate of a polycarboxylic acid component and a polyhydric alcohol component containing a diethylene glycol component. With this configuration, the gas barrier film 1 can block the intrusion of gas from the outside and can exhibit excellent gas barrier properties. In addition, the polyhydric alcohol component containing a diethylene glycol component can improve the flexibility of the polyester resin (C), so the gas barrier film 1 has excellent tear strength. And, since the gas barrier film 1 has excellent tear strength, it has good processability. In this specification, the gas barrier property is a property of blocking gas, and includes water vapor barrier property that blocks water vapor and oxygen barrier property that blocks oxygen. In addition, the polyhydric alcohol component containing the diethylene glycol component can improve the flexibility of the polyester resin (C), thereby increasing the adhesive strength between the base layer 2 and the auxiliary layer 3, particularly in the width direction, and preventing the auxiliary layer 3 from peeling off from the base layer 2.

[0013] The gas barrier film 1 of this embodiment is aluminum-free (does not contain aluminum), and therefore the amount of CO2 generated during the manufacturing and disposal processes can be reduced. Furthermore, when the gas barrier film 1 is to be disposed of, it can be easily separated and collected since it can be disposed of as plastic waste. Furthermore, the liquid crystal polymer (A) and the isophthalic acid-modified polyethylene terephthalate (B) constituting the base layer 2 have good affinity and can be mixed uniformly, so that they can be mixed without adding, for example, a reactive compatibilizer. Therefore, the gas barrier film 1 of this embodiment is excellent in recyclability. Furthermore, since the gas barrier film 1 of this embodiment is aluminum-free, it can be used in a production line that uses a metal detector to detect metallic foreign matter and the like.

[0014] The melting point of the liquid crystal polymer (A) constituting the base layer 2 is preferably 220° C. or lower. When the liquid crystal polymer (A) has a melting point of 220° C. or lower, the temperature during molding can be relatively low, and the isophthalic acid-modified polyethylene terephthalate (B) can be prevented from changing due to thermal decomposition or the like. Therefore, the gas barrier film 1 can exhibit superior tear strength.

[0015] Examples of monomer components constituting the liquid crystal polymer (A) include one or more selected from terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, hydroquinone, resorcinol, 2,6-dihydroxynaphthalene, 4,4'-biphenol, p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 4-aminobenzoic acid, 4-aminophenol, 1,4-phenylenediamine, and the like.

[0016] The liquid crystal polymer (A) preferably contains a terephthalic acid component as a monomer component constituting the liquid crystal polymer (A), which allows the gas barrier film 1 to exhibit superior gas barrier properties and also has superior tear strength.

[0017] The liquid crystal polymer (A) preferably contains a hydroquinone component as a monomer component constituting the liquid crystal polymer (A), which allows the gas barrier film 1 to exhibit superior gas barrier properties and also has superior tear strength.

[0018] The liquid crystal polymer (A) preferably contains a p-hydroxybenzoic acid component and a 6-hydroxy-2-naphthoic acid component as monomer components constituting the liquid crystal polymer (A). When the liquid crystal polymer (A) contains a p-hydroxybenzoic acid component and a 6-hydroxy-2-naphthoic acid component as monomer components, the gas barrier film 1 can exhibit more excellent gas barrier properties and has excellent tear strength. From the viewpoint of improving the gas barrier properties, the liquid crystal polymer (A) more preferably contains a p-hydroxybenzoic acid component and a 6-hydroxy-2-naphthoic acid component as main monomer components. Here, the main component means that the liquid crystal polymer (A) contains 50 mol % or more of the monomer components constituting the liquid crystal polymer (A).

[0019] The monomer component constituting the liquid crystal polymer (A) is preferably an aromatic compound, which allows the gas barrier film 1 to exhibit superior gas barrier properties and also has superior tear strength.

[0020] Examples of the liquid crystal polymer (A) include VECTORA (registered trademark) and ZENITE (registered trademark) manufactured by Celanese, LAPEROS (registered trademark) manufactured by Polyplastics, XYDAR (registered trademark) manufactured by ENEOS, Sumikasuper (registered trademark) LCP (registered trademark) manufactured by Sumitomo Chemical Co., Ltd., and UENO LCP (registered trademark) manufactured by Ueno Pharmaceutical Co., Ltd.

[0021] The isophthalic acid modified polyethylene terephthalate (B) used in the base layer 2 of this embodiment is a copolymer of linear polyester resin obtained by condensation polymerization of a dicarboxylic acid component and a diol component, in which the dicarboxylic acid component is mainly composed of terephthalic acid and further contains isophthalic acid, and the diol component is mainly composed of ethylene glycol. Here, the main component means the component with the largest content. Note that the isophthalic acid modified polyethylene terephthalate (B) is non-liquid crystal and is not included in the liquid crystal polymer (A).

[0022] The copolymerization ratio of the isophthalic acid component in the dicarboxylic acid component constituting the isophthalic acid modified polyethylene terephthalate (B) is preferably 3 mol% to 30 mol%, and more preferably 5 mol% to 25 mol%. Here, the copolymerization ratio of the isophthalic acid component in the dicarboxylic acid component is the ratio (mol percentage) of the isophthalic acid component to the dicarboxylic acid component. When the copolymerization ratio of the isophthalic acid component in the dicarboxylic acid component is 3 mol% or more, the gas barrier film 1 of the present embodiment can exhibit better gas barrier properties and tear strength, and can obtain good processability. In addition, when the copolymerization ratio of the isophthalic acid component in the dicarboxylic acid component is 30 mol% or less, it is possible to provide a gas barrier film 1 having heat resistance capable of withstanding heat when heat-sealing films having the gas barrier film 1 with each other, or the gas barrier film 1 with another film, or heat resistance capable of withstanding heat of contents when high-temperature contents are filled in a packaging bag or the like formed of a film having the gas barrier film 1.

[0023] The intrinsic viscosity (IV) of the isophthalic acid modified polyethylene terephthalate (B) is preferably 0.60 dl / g to 0.85 dl / g. Here, the intrinsic viscosity is a value measured at 30°C in a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (mass ratio 1 / 1) in accordance with JIS K 7367-5. When the intrinsic viscosity is 0.60 dl / g or more, the gas barrier film 1 of the present embodiment can exhibit more excellent gas barrier properties. In addition, when the intrinsic viscosity is 0.85 dl / g or less, the extrusion process of the base layer 2 becomes easy, and the processability of the gas barrier film 1 can be improved.

[0024] The content of the liquid crystal polymer (A) in the base layer 2 is preferably 78 parts by mass to 99 parts by mass, and the content of the isophthalic acid modified polyethylene terephthalate (B) in the base layer 2 is preferably 1 part by mass to 22 parts by mass. When the contents of the liquid crystal polymer (A) and the isophthalic acid modified polyethylene terephthalate (B) are within the above ranges, the gas barrier film 1 of the present embodiment can exhibit better gas barrier properties and tear strength. It is more preferable that the content of the liquid crystal polymer (A) in the base layer 2 is 80 parts by mass to 90 parts by mass, and the content of the isophthalic acid modified polyethylene terephthalate (B) in the base layer 2 is 10 parts by mass to 20 parts by mass.

[0025] Examples of polyvalent carboxylic acid components constituting the polyester resin (C) contained in the auxiliary layer 3 include one or more selected from terephthalic acid, isophthalic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, adipic acid, sebacic acid, etc.

[0026] Examples of the polyhydric alcohol component constituting the polyester resin (C), other than diethylene glycol, include one or more selected from ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexamethylenediol, cyclopentane dimethanol, cyclohexane dimethanol, neopentyl glycol, 2,2-diethyl-1,3-propanediol, 2,2-dipropyl-1,3-propanediol, 2-propyl-2-methyl-1,3-propanediol, 2-propyl-2-ethyl-1,3-propanediol, 2-isopropyl-2-methyl-1,3-propanediol, 2-isopropyl-2-ethyl-1,3-propanediol, 2-butyl-2-methyl-1,3-propanediol, and 2-butyl-2-ethyl-1,3-propanediol. The polyester resin (C) is non-liquid crystal and is different from the liquid crystal polymer (A).

[0027] The polyester resin (C) is preferably a modified polyethylene terephthalate composed of a dicarboxylic acid component composed of a terephthalic acid component and a diol component containing a diethylene glycol component, an ethylene glycol component, and a 1,4-butanediol component. This allows the gas barrier film 1 to exhibit excellent gas barrier properties and has better tear strength. In addition, the adhesive strength between the base layer 2 and the auxiliary layer 3, particularly in the width direction, can be further increased, and peeling of the auxiliary layer 3 from the base layer 2 can be further suppressed.

[0028] The glass transition temperature of the polyester resin (C) is preferably -10°C to 40°C, and more preferably 10°C to 30°C. When the glass transition temperature of the polyester resin (C) is -10°C to 40°C, the flexibility of the polyester resin (C) can be further improved, and the gas barrier film 1 has better tear strength. In addition, the adhesive strength between the base layer 2 and the auxiliary layer 3, particularly in the width direction, can be further increased, and the gas barrier film 1 can further suppress peeling of the auxiliary layer 3 from the base layer 2.

[0029] When the thickness of the base layer 2 is A and the thickness of the auxiliary layer 3 is B, B / A is preferably 0.1 to 0.4, and more preferably 0.2 to 0.3. When B / A is 0.1 to 0.4, the gas barrier film 1 can exhibit superior gas barrier properties and also has superior tear strength.

[0030] The thickness of the base layer 2 is not particularly limited, and may be 70 μm to 90 μm, and the thickness of the auxiliary layer 3 may be 10 μm to 30 μm, relative to a total thickness of 100 μm. When the base layer 2 has a thickness of 70 μm to 90 μm and the auxiliary layer 3 has a thickness of 10 μm to 30 μm, the gas barrier film 1 can exhibit better gas barrier properties and has better tear strength. Furthermore, the gas barrier film 1 can be suitably used particularly for packaging bags.

[0031] The gas barrier film 1 is preferably formed into a film shape by co-extrusion. The gas barrier film 1 can be formed into a film by co-extrusion, in which the material constituting the base layer 2 and the material constituting the auxiliary layer 3 are melt-extruded simultaneously. This can increase the adhesive strength between the base layer 2 and the auxiliary layer 3 compared to laminating the base layer 2 and the auxiliary layer 3 by a lamination method. In addition, since the liquid crystal polymer (A) constituting the base layer 2 has a melting point of 230°C or less, the heating temperature during co-extrusion can be relatively low, and the polyester resin (C) constituting the auxiliary layer 3 can be prevented from changing due to thermal decomposition or the like. Therefore, the gas barrier film 1 can exhibit excellent tear strength. Even when a long gas barrier film 1 is continuously formed and the long film is wound up after forming, the gas barrier film 1 has excellent tear strength and can be prevented from tearing.

[0032] The tear strength in the machine direction of the gas barrier film 1 is preferably 0.80 N / 100 μm or more. Here, the tear strength refers to a value measured in accordance with JIS K 7128-1. When the tear strength in the machine direction of the gas barrier film 1 is 0.80 N / 100 μm or more, even when a long gas barrier film 1 is continuously molded and the long molded film is wound up after molding, the gas barrier film 1 has superior tear strength and can be more prevented from tearing.

[0033] The adhesive strength between the base layer 2 and the auxiliary layer 3 in the machine direction and the width direction is preferably 2.0 N or more. The adhesive strength can be measured by a ring method. When the adhesive strength between the base layer 2 and the auxiliary layer 3 in the machine direction and the width direction is 2.0 N or more, the gas barrier film 1 can further suppress peeling of the auxiliary layer 3 from the base layer 2.

[0034] The adhesive strength between the base layer 2 and the auxiliary layer 3 in the width direction is preferably greater than the adhesive strength in the machine direction. In general, when a long laminate film is continuously molded and the long molded body of the film is wound along the machine direction after molding, the base layer and the auxiliary layer are likely to peel off at the ends in the width direction due to the application of a bending load. In the gas barrier film 1 of this embodiment, the adhesive strength between the base layer 2 and the auxiliary layer 3 in the width direction is greater than the adhesive strength in the machine direction, so that the auxiliary layer 3 can be prevented from peeling off from the base layer 2 even when the long molded body of the gas barrier film 1 is wound along the machine direction after molding.

[0035] (Laminated film) FIG. 2 is a schematic diagram showing a cross section of a laminated film according to an embodiment. As shown in FIG. 2, the laminated film 5 of this embodiment has the gas barrier film 1 of this embodiment and a sealant layer 4 laminated on the surface of the auxiliary layer 3 of the gas barrier film 1. The sealant layer 4 contains one or more of a polyethylene resin, a polypropylene resin, a polyester resin, and a cyclic olefin resin. The sealant layer 4 is one of the outermost surfaces of the laminated film 5. Here, the sealant layer 4 is a layer used for heat sealing, and is a layer disposed as the innermost layer in contact with the contents when the laminated film 5 is used as a packaging material. This allows two laminated films 5 to be placed opposite each other and the sealant layers 4 to be bonded together by heat. The auxiliary layer 3 and the sealant layer 4 may be bonded via an adhesive layer or an anchor layer, but are preferably bonded directly to each other. The sealant layer 4 is preferably a resin film having excellent heat resistance, mechanical properties, and printability.

[0036] When the laminate film 5 is used as a packaging material, the gas barrier film 1 is located outside the sealant layer 4 that contacts the contents, so that the intrusion of gas from the outside can be blocked, and the laminate film 5 of this embodiment can exhibit excellent gas barrier properties. Furthermore, the laminate film 5 has excellent tear strength due to the presence of the gas barrier film 1. And, because the laminate film 5 has excellent tear strength, it has good processability.

[0037] The sealant layer 4 preferably contains isophthalic acid-modified polyethylene terephthalate modified with isophthalic acid. The isophthalic acid-modified polyethylene terephthalate contained in the sealant layer 4 may be the same as the isophthalic acid-modified polyethylene terephthalate contained in the above-mentioned base layer 2. When the sealant layer 4 contains isophthalic acid-modified polyethylene terephthalate, the laminate film 5 of the present embodiment can exhibit even better gas barrier properties. Furthermore, the laminate film 5 can improve the adhesion between the sealant layer 4 and the auxiliary layer 3 containing the polyester resin (C).

[0038] The thickness of the sealant layer 4 depends on the application of the packaging material and is not particularly limited, but may be, for example, 10 μm to 50 μm.

[0039] The sealant layer 4 may contain additives as components other than the resin. The additives are not particularly limited, but examples thereof include antioxidants, lubricants, antiblocking agents, stabilizers, UV absorbers, flame retardants, antistatic agents, colorants, etc.

[0040] The laminated film 5 may have another layer provided on the opposite side of the sealant layer 4 with respect to the base layer 2, and the other layer preferably contains a resin other than the liquid crystal polymer. The other layer may include, for example, an intermediate layer, an adhesive layer, an anchoring agent layer, etc. As the intermediate layer, one or more layers may be appropriately selected from a reinforcing layer, a gas barrier layer, a light-shielding layer, a printing layer, etc.

[0041] The method for producing the laminated film 5 is not particularly limited, and examples thereof include an extrusion lamination method, a dry lamination method, a coextrusion method, or a combination of these. In addition, the strength and heat deformation resistance of the film can be improved by uniaxially or biaxially stretching the formed film before lamination.

[0042] (packaging bag) Fig. 3 is a schematic diagram of a packaging bag 10 according to one embodiment. The packaging bag 10 is formed using the laminated film 5 of this embodiment. As shown in Fig. 3, the packaging bag 10 has a bag-shaped body 11 formed from the laminated film 5 and a mouth 12 joined to at least one location on the periphery of the body 11. The shape of the body 11 is not particularly limited, and examples include a three-sided bag, a four-sided bag, a seamed bag, a gusset bag, and a standing pouch. The body 11 may be a large packaging bag, such as an inner bag for a bag-in-box.

[0043] The material constituting the mouth portion 12 can be suitably used as long as it can be bonded to the sealant layer 4 of the laminated film 5 constituting the packaging bag 10 to ensure hermeticity, but it is preferably a resin that can be heat-sealed to the sealant layer 4 of the laminated film 5. This allows the mouth portion 12 and the laminated film 5 to be bonded by heat sealing. For this reason, the material constituting the mouth portion 12 is preferably polyethylene terephthalate (PET), and more preferably isophthalic acid-modified PET. This allows the mouth portion 12 to be easily heat-sealed to the sealant layer 4 of the laminated film 5, and also improves the gas barrier properties of the packaging bag 10.

[0044] When heat sealing the laminated film 5 and the mouth portion 12, the laminated film 5 may be overlapped with the sealant layer 4 on the inside, and the mouth portion 12 may be inserted between the overlapped sealant layers 4 and heat sealed. Alternatively, a flange portion or a boat-shaped fusion base may be provided at one end of the mouth portion 12, and this flange portion or fusion base may be heat sealed to the periphery of a hole provided in the laminated film 5 or the inner surface of the opening of a packaging bag. EXAMPLES

[0045] The present invention will be specifically described below with reference to examples, although the present invention is not limited to these examples.

[0046] In Examples 1 to 6 and Comparative Examples 1 to 2, the raw materials were mixed and melted in the ratios shown in Table 1, and then the molten resin constituting the base layer and the molten resin constituting the auxiliary layer were co-extruded by a T-die extruder to obtain a gas barrier film having two layers, a base layer and an auxiliary layer, and having a thickness of 100 μm. In Comparative Examples 3 to 11, the raw materials were mixed and melted in the ratios shown in Table 1, and then the molten resin constituting the base layer was extruded by a T-die extruder to obtain a gas barrier film having a thickness of 100 μm and consisting of a single layer of the base layer only. The thicknesses of the base layer and the auxiliary layer of the gas barrier films of Examples 1 to 6 and Comparative Examples 1 to 2 were as shown in Table 1. Details of each raw material are as follows.

[0047] (A) Liquid crystal polymer A-1: Low melting point liquid crystal polymer (product name "UENO LCP (registered trademark) A-8100", manufactured by Ueno Pharmaceutical Co., Ltd., density ρ = 1.40 g / cm 3 , melting point Tm=220℃)

[0048] (B) Isophthalic acid modified polyethylene terephthalate (isophthalic acid modified PET) B-1: Isophthalic acid modified polyethylene terephthalate (copolymerization ratio of isophthalic acid component in dicarboxylic acid component is 10 mol%, density ρ = 1.34 g / cm 3 , melting point Tm = 228 ° C, intrinsic viscosity IV = 0.85 dl / g) B-2: Isophthalic acid modified polyethylene terephthalate (copolymerization ratio of isophthalic acid component in dicarboxylic acid component is 12 mol%, density ρ = 1.34 g / cm 3 , melting point Tm = 224 ° C, intrinsic viscosity IV = 0.80 dl / g) B-3: Isophthalic acid modified polyethylene terephthalate (copolymerization ratio of isophthalic acid component in dicarboxylic acid component: 23 mol%, density ρ = 1.34 g / cm 3 , no melting point, intrinsic viscosity IV = 0.68 dl / g)

[0049] (C) Polyester resin C-1: Modified polyethylene terephthalate (product name "PRIT30", manufactured by Bell Polyester Products, Inc., density ρ = 1.24 g / cm 3 , melting point Tm = 188 ° C, glass transition temperature Tg = 30 ° C, intrinsic viscosity IV = 0.75 dl / g)

[0050] (D) Unmodified polyethylene terephthalate (unmodified PET) D-1: Unmodified polyethylene terephthalate (homo PET, density ρ = 1.34 g / cm 3 , melting point Tm = 255°C, intrinsic viscosity IV = 0.75 dl / g)

[0051] The liquid crystal polymer (A-1) contains, as monomer components, a p-hydroxybenzoic acid component, a 6-hydroxy-2-naphthoic acid component, a terephthalic acid component, and a hydroquinone component. The polyester resin (C-1) contains a dicarboxylic acid component consisting of a terephthalic acid component, and a diol component consisting of a diethylene glycol component, an ethylene glycol component, and a 1,4-butanediol component.

[0052] The melt flow rate (MFR) is the value (g / 10 min) at a test temperature of 190°C and a nominal load of 2.16 kg. The intrinsic viscosity is the value (dl / g) measured at 30°C in a mixed solvent of phenol / 1,1,2,2-tetrachloroethane in a mass ratio of 1 / 1.

[0053] [Table 1]

[0054] Next, the obtained gas barrier films were evaluated as follows: For the gas barrier films of Comparative Examples 3 to 11, evaluation was performed on properties other than adhesive strength since no auxiliary layer was provided.

[0055] (tear strength) In accordance with JIS K 7128-1, a trouser tear method was used to measure the tear strength in the machine direction by making a 75 mm long slit in the center of a sample cut to 150 mm x 50 mm, with a chuck width of 50 mm and a pulling speed of 200 mm / min.

[0056] (Adhesive strength) The adhesive strength of a sample cut to 25.4 mm x 200 mm was measured by the ring method, with the auxiliary layer clamped between grippers at a peel distance of 30 mm and a peel speed of 5 mm / min. An adhesive strength of 2.2 N or more in the machine direction (MD) and an adhesive strength of 2.5 N or more in the cross direction (TD) were evaluated as pass, and an adhesive strength of less than 2.2 N in the machine direction (MD) and less than 2.5 N in the cross direction (TD) were evaluated as fail.

[0057] (Oxygen gas permeability, water vapor permeability) The oxygen gas permeability and water vapor permeability of the prepared film were measured in accordance with JIS K 7126-2 and JIS K 7129-2.

[0058] The evaluation results are shown in Table 2.

[0059] [Table 2]

[0060] As shown in Table 2, the gas barrier films of Examples 1 to 6 had oxygen permeability and water vapor permeability equal to or greater than those of the gas barrier film of Comparative Example 11 made of a liquid crystal polymer alone, and were confirmed to have excellent gas barrier properties. In addition, the gas barrier films of Examples 1 to 6 were confirmed to have excellent tear strength compared to Comparative Examples 2 to 11. Furthermore, the gas barrier films of Examples 1 to 6 were confirmed to have excellent adhesive strength that met the pass criteria. The gas barrier film of Comparative Example 1 had excellent tear strength, but failed the adhesive strength and was not suitable for practical use.

[0061] Furthermore, a three-layer laminate film was produced by co-extrusion molding using each of the raw materials of Example 1 shown in Table 1 and isophthalic acid-modified PET as the raw material for the sealant layer, in which a base layer of 80 μm in thickness, an auxiliary layer of 20 μm in thickness, and a sealant layer of 50 μm in thickness were laminated in that order. A three-pack sealed bag was then produced at a heat seal temperature of 170° C., a sealing pressure of 0.2 MPa, and a sealing time of 1 sec, and it was confirmed that the packaging bag could be produced without any problems.

[0062] (Embodiments of the present invention) The present invention includes the following aspects. <Aspect 1> A base layer and an auxiliary layer laminated on one surface of the base layer, The base layer contains a liquid crystal polymer having a melting point of 230° C. or less and an isophthalic acid-modified polyethylene terephthalate modified with isophthalic acid, The auxiliary layer contains a polyester resin, The polyester resin is a polycondensate of a polyvalent carboxylic acid component and a polyhydric alcohol component containing a diethylene glycol component. <Aspect 2> The gas barrier film according to embodiment 1, wherein a copolymerization ratio of an isophthalic acid component in a dicarboxylic acid component constituting the isophthalic acid-modified polyethylene terephthalate is 3 mol % to 30 mol %. <Aspect 3> The gas barrier film according to aspect 1 or 2, wherein the content of the liquid crystal polymer relative to the base layer is 78 parts by mass to 99 parts by mass, and the content of the isophthalic acid-modified polyethylene terephthalate relative to the base layer is 1 part by mass to 22 parts by mass. <Aspect 4> The gas barrier film according to any one of Aspects 1 to 3, wherein the polyester resin is a modified polyethylene terephthalate consisting of a dicarboxylic acid component consisting of a terephthalic acid component and a diol component consisting of a diethylene glycol component, an ethylene glycol component, and a 1,4-butanediol component. <Aspect 5> Aspects 5. The gas barrier film according to any one of aspects 1 to 4, wherein the liquid crystal polymer contains a terephthalic acid component as a monomer component constituting the liquid crystal polymer. <Aspect 6> 6. The gas barrier film according to any one of aspects 1 to 5, wherein the liquid crystal polymer contains a hydroquinone component as a monomer component constituting the liquid crystal polymer. <Aspect 7> 7. The gas barrier film according to any one of aspects 1 to 6, wherein the liquid crystal polymer contains a p-hydroxybenzoic acid component and a 6-hydroxy-2-naphthoic acid component as monomer components constituting the liquid crystal polymer. <Aspect 8> A gas barrier film according to any one of aspects 1 to 7, in which B / A is 0.1 to 0.4, where A is the thickness of the base layer and B is the thickness of the auxiliary layer. <Aspect 9> 9. The gas barrier film according to any one of aspects 1 to 8, wherein the base layer and the auxiliary layer are formed into a film by coextrusion molding. <Aspect 10> A gas barrier film according to any one of aspects 1 to 9; a sealant layer laminated on a surface of the auxiliary layer, The sealant layer is a laminated film containing at least one of a polyethylene resin, a polypropylene resin, a polyester resin, and a cyclic olefin resin. <Aspect 11> 11. The laminate film according to claim 10, wherein the sealant layer contains isophthalic acid-modified polyethylene terephthalate modified with isophthalic acid. <Aspect 12> a layer provided on the opposite side of the sealant layer with respect to the gas barrier film; 12. The laminate film according to embodiment 10 or 11, wherein the other layer contains a resin other than the liquid crystal polymer. <Aspect 13> A packaging bag formed using the laminate film according to any one of aspects 10 to 12. [Explanation of symbols]

[0063] 1 Gas barrier film 2 Base material layer 3 Auxiliary layer 4 Sealant Layer 5. Laminated Film 10 packaging bags 11 Torso 12 Mouth

Claims

1. A base layer and an auxiliary layer laminated on one surface of the base layer, The base layer contains a liquid crystal polymer having a melting point of 230° C. or less and an isophthalic acid-modified polyethylene terephthalate modified with isophthalic acid, The auxiliary layer contains a polyester resin, The polyester resin is a polycondensate of a polycarboxylic acid component and a polyhydric alcohol component containing a diethylene glycol component.

2. 2. The gas barrier film according to claim 1, wherein a copolymerization ratio of an isophthalic acid component in a dicarboxylic acid component constituting the isophthalic acid-modified polyethylene terephthalate is 3 mol % to 30 mol %.

3. 3. The gas barrier film according to claim 2, wherein the content of the liquid crystal polymer relative to the base layer is 78 parts by mass to 99 parts by mass, and the content of the isophthalic acid-modified polyethylene terephthalate relative to the base layer is 1 part by mass to 22 parts by mass.

4. 4. The gas barrier film according to claim 3, wherein the polyester resin is a modified polyethylene terephthalate comprising a dicarboxylic acid component comprising a terephthalic acid component and a diol component comprising a diethylene glycol component, an ethylene glycol component, and a 1,4-butanediol component.

5. The gas barrier film according to claim 4 , wherein the liquid crystal polymer contains a terephthalic acid component as a monomer component constituting the liquid crystal polymer.

6. The gas barrier film according to claim 5 , wherein the liquid crystal polymer contains a hydroquinone component as a monomer component constituting the liquid crystal polymer.

7. 7. The gas barrier film according to claim 6, wherein the liquid crystal polymer contains a p-hydroxybenzoic acid component and a 6-hydroxy-2-naphthoic acid component as monomer components constituting the liquid crystal polymer.

8. 8. The gas barrier film according to claim 7, wherein the thickness of the base layer is A and the thickness of the auxiliary layer is B, and B / A is 0.1 to 0.

4.

9. The gas barrier film according to claim 8 , wherein the base layer and the auxiliary layer are formed into a film by coextrusion molding.

10. A gas barrier film according to any one of claims 1 to 9, a sealant layer laminated on a surface of the auxiliary layer, The sealant layer is a laminated film containing at least one of a polyethylene resin, a polypropylene resin, a polyester resin, and a cyclic olefin resin.

11. The laminated film according to claim 10 , wherein the sealant layer comprises an isophthalic acid-modified polyethylene terephthalate modified with isophthalic acid.

12. a layer provided on the opposite side of the sealant layer with respect to the gas barrier film; The laminate film according to claim 11 , wherein the other layer contains a resin other than a liquid crystal polymer.

13. A packaging bag formed using the laminated film according to claim 10.

Citation Information

Patent Citations

  • Packaging bag

    JP2014005013A