Curable composition and cured product

The curable composition with a specific (meth)acrylic polymer and polyoxyalkylene polymer structure addresses storage stability issues, ensuring long-term stability and suitability for one-component applications.

JP2024137351APending Publication Date: 2024-10-07KANEKA CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023048844
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Conventional curable compositions containing (meth)acrylic polymers and polyoxyalkylene polymers suffer from poor storage stability, particularly when stored for extended periods.

Method used

A curable composition comprising a silyl group-containing (meth)acrylic polymer with a specific molecular structure, such as an XY diblock or XYX triblock structure, and a silyl group-containing polyoxyalkylene polymer, along with a curing catalyst, to enhance storage stability.

Benefits of technology

The composition exhibits excellent storage stability, maintaining a liquid state without gelling during prolonged storage at elevated temperatures, suitable for use as a one-component curable composition in various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137351000001
    Figure 2024137351000001
Patent Text Reader

Abstract

To provide a curable composition excellent in storage stability.SOLUTION: The curable composition of the present disclosure contains: (A) a silyl group-containing (meth)acrylic polymer; (B1) a silyl group-containing polyoxyalkylene polymer having 1.0 or more specific alkoxysilyl groups per molecule; and (C) a curing catalyst. The silyl group-containing (meth)acrylic polymer (A) contains a (meth)acrylic copolymer (A1) of a specific structure having an alkoxysilyl group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition and a cured product. [Background technology]

[0002] A curable composition containing a (meth)acrylic polymer and a polyoxyalkylene polymer has been conventionally known (see, for example, Patent Document 1). It is known that such a curable composition has high weather resistance and high heat resistance, and can therefore be used as a highly durable sealant or adhesive for outdoor applications. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2002-294022 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the above-mentioned conventional techniques have room for improvement in terms of storage stability. One aspect of the present invention aims to provide a curable composition having excellent storage stability. [Means for solving the problem]

[0005] In order to solve the above problems, a curable composition according to one aspect of the present invention is a curable composition comprising: (A) a silyl group-containing (meth)acrylic polymer; (B1) a silyl group-containing polyoxyalkylene polymer; and (C) a curing catalyst, wherein the (A) silyl group-containing (meth)acrylic polymer comprises a (meth)acrylic copolymer (A1) having an alkoxysilyl group; The (meth)acrylic copolymer (A1) contains an XY diblock structure having an X block and a Y block or an XYX triblock structure in the molecule, the number of repeating units derived from a (meth)acrylic acid ester monomer having an alkoxysilyl group contained in the X block is more than 2.0 on average, a repeating unit derived from a (meth)acrylic acid ester monomer having an alkoxysilyl group contained in the Y block is 0% by weight or more and less than 5% by weight based on the weight of all repeating units contained in the Y block, The (meth)acrylic copolymer (A1) has a molecular weight distribution (Mw / Mn) of 1.8 or less, The (B1) silyl group-containing polyoxyalkylene polymer is a curable composition having 1.0 or more alkoxysilyl groups represented by the following formula (1) per molecule: -Si(OR 1 ) 3 (1) [In formula (1), R 1 represents an alkyl group. Three R's exist in the alkoxysilyl group represented by formula (1). 1 may be the same or different. When a plurality of alkoxysilyl groups represented by formula (1) are present in the silyl group-containing polyoxyalkylene polymer (B1), R 1 may be different for each alkoxysilyl group. Effect of the Invention

[0006] According to one aspect of the present invention, a curable composition having excellent storage stability can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] Hereinafter, an embodiment of the present invention will be described in detail, but the present invention is not limited to this embodiment.

[0008] Unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more and B or less." In this specification, "(meth)acrylic" means "acrylic" and / or "methacrylic".

[0009] A curable composition according to one embodiment of the present invention comprises the following components (A), (B1) and (C). Component (A): silyl group-containing (meth)acrylic polymer Component (B1): silyl group-containing polyoxyalkylene polymer (C) Component: Curing catalyst.

[0010] For example, in applications such as sealants, there is a strong demand for improving the weather resistance of the cured product, and various studies have been conducted to increase the concentration of (meth)acrylic polymers, leading to the development of highly weather-resistant sealants. However, curable compositions with a high concentration of (meth)acrylic copolymers have room for improvement in terms of storage stability, particularly stability when stored for a long period of time.

[0011] In one embodiment of the present invention, a curable composition having excellent storage stability can be provided by using, as the (meth)acrylic polymer, a (meth)acrylic polymer (A1) having an alkoxysilyl group having a specific structure described below, and using, as the silyl group-containing polyoxyalkylene polymer, a silyl group-containing polyoxyalkylene polymer (B1) having an alkoxysilyl group having a specific structure described below.

[0012] [1. Silyl Group-Containing (Meth)acrylic Polymer] A curable composition according to one embodiment of the present invention contains a silyl group-containing (meth)acrylic polymer as the component (A).

[0013] [1.1. Main chain of (meth)acrylic polymer] The (meth)acrylic polymer contains a repeating unit (structural unit) derived from a (meth)acrylic monomer in the main chain. Only one type of (meth)acrylic monomer may be used, or two or more types of (meth)acrylic monomers may be used in combination.

[0014] The repeating units derived from the (meth)acrylic monomer contained in the (meth)acrylic polymer are preferably 50% by weight or more, more preferably 70% by weight or more, and even more preferably 90% by weight or more of the total weight of the polymer. If the content of the repeating units derived from the (meth)acrylic monomer is 50% by weight or more, good weather resistance and mechanical properties (elongation) can be obtained.

[0015] The (meth)acrylic polymer as component (A) may contain 0% by weight or more, and preferably 1% by weight or more, of repeating units derived from (meth)acrylic monomers having long side chains among all structural units contained in the (meth)acrylic polymer. By containing 1% by weight or more of repeating units derived from a (meth)acrylic monomer having a long side chain in the (meth)acrylic polymer, the compatibility of the component (A) with the component (B) and the physical properties of the cured product obtained from the curable composition containing these components can be improved. In this specification, the term "(meth)acrylic monomer having a long side chain" refers to a repeating unit derived from a (meth)acrylic monomer having a long side chain, represented by the formula "R 2 CH=CHCOOR 3 " and R 2 is a hydrogen atom or a methyl group, and R 3 represents a monomer having 9 or more carbon atoms. Of all the structural units contained in the (meth)acrylic polymer as component (A), the upper limit of the content of repeating units derived from (meth)acrylic monomers having long side chains is preferably 5% by weight or less, more preferably 3% by weight or less, and even more preferably 1% by weight or less. By limiting the amount of (meth)acrylic monomers having long side chains used to 5% by weight or less, or by not using such monomers, the production costs of the (meth)acrylic polymer can be reduced.

[0016] Examples of (meth)acrylic monomers having a long side chain include nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, icosyl (meth)acrylate, docosyl (meth)acrylate, oleyl (meth)acrylate, linoleyl (meth)acrylate, and isobornyl (meth)acrylate.

[0017] The (meth)acrylic monomer having a long side chain is, in the above formula, R 2 represents a monomer having 8 or less carbon atoms. Examples of such monomers include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, isopropoxyethyl (meth)acrylate, benzyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, glycidyl (meth)acrylate, 1-ethylcyclopentyl ether (meth)acrylate, and dimethylaminoethyl (meth)acrylate.

[0018] Among the above-mentioned monomers, one or more selected from methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are preferred. These monomers have low procurement costs and are suitable for the purpose of reducing the production costs of the (meth)acrylic polymer.

[0019] Furthermore, from the viewpoint of glass transition point, one or more selected from n-butyl acrylate and 2-ethylhexyl acrylate are preferred. (Meth)acrylic polymers obtained from these monomers have low glass transition points and low polymer viscosity. Therefore, a curable composition that is easy to use in low temperature environments can be obtained.

[0020] [1.2. Silyl Groups of (Meth)acrylic Polymers] In one embodiment, the silyl group of the (meth)acrylic polymer is represented by the following general formula (2). -[Si(R 6 ) 2-b (Y) b O] m -Si(R 7 ) 3-a (Y) a (2) In the formula, R 6 and R 7 are independently an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, or (R') 3 It is a triorganosiloxy group represented by SiO- (wherein R' is a monovalent hydrocarbon group having 1 to 20 carbon atoms, and the three R's may be the same or different). 6 or R 7 When there are two or more R 6 or R 7 may be the same or different.

[0021] Y is an alkoxy group having a carbon number of 1 to 20. When there are two or more Y's, the Y's may be the same or different.

[0022] a is 0, 1, 2, or 3. b is 0, 1, or 2. m is an integer from 0 to 19, provided that the relationship a+mb≧1 is satisfied.

[0023] In general, the fewer the carbon atoms in an alkoxy group, the higher the reactivity. That is, the reactivity decreases in the order of methoxy group, ethoxy group, and propoxy group. Therefore, an appropriate alkoxy group can be selected depending on the production method and application of the (meth)acrylic polymer.

[0024] Specific examples of the silyl group include a dimethoxysilyl group, a trimethoxysilyl group, a diethoxysilyl group, a triethoxysilyl group, a triisopropoxysilyl group, a dimethoxymethylsilyl group, a diethoxymethylsilyl group, and a diisopropoxymethylsilyl group.

[0025] The number of silyl groups introduced into the (meth)acrylic polymer is, on average, more than 1 in the entire molecule. In one embodiment, the number of silyl groups is preferably 1.1 or more, more preferably 1.2 or more. In another embodiment, the number of silyl groups is preferably 2.2 or more, more preferably 2.4 or more. The upper limit of the number of silyl groups introduced into the (meth)acrylic polymer is preferably 4.0 or less, more preferably 3.5 or less.

[0026] If the number of silyl groups is within the above range, the physical properties of the curable composition and the cured product using the (meth)acrylic polymer are good. The (meth)acrylic polymer preferably has a silyl group at at least one end portion, and preferably has silyl groups at both end portions. However, some or all of the ends of the (meth)acrylic polymer molecule may not have a silyl group.

[0027] In one embodiment, the (meth)acrylic polymer includes a (meth)acrylic copolymer (A1) having an alkoxysilyl group. The (meth)acrylic copolymer (A1) has an X block having a relatively high content of alkoxysilyl groups and a Y block having a relatively low content of alkoxysilyl groups, and includes an XY diblock structure or an XYX triblock structure in the molecule.

[0028] The overall molecular structure of the (meth)acrylic polymer is not particularly limited as long as it contains an XY diblock structure or an XYX triblock structure, and may be, for example, an XYXY tetrablock structure. Here, the "XYX triblock structure" refers to the "ABA triblock structure" commonly known by those skilled in the art.

[0029] In a molecule having an XY diblock structure, the X block may be 40% or less, 30% or less, or 25% or less of the region from one end of the molecule (total units contained in the molecule is taken as 100%). In a molecule having an XYX triblock structure, the X block may be 40% or less, 30% or less, or 25% or less of the region from one end of the molecule (total units contained in the molecule is taken as 100%).

[0030] The (meth)acrylic copolymer (A1) has a repeating unit derived from a (meth)acrylic acid ester monomer having an alkoxysilyl group (hereinafter also referred to as a silyl group-containing monomer). The repeating units derived from the silyl group-containing monomer contained in the X block are more than 2.0 on average, preferably 2.1 or more, more preferably 2.2 or more. When the (meth)acrylic copolymer (A1) has two or more X blocks in one molecule, the total number of repeating units derived from the silyl group-containing monomer contained in the multiple X blocks is more than 2.0 on average. In other words, the repeating units derived from the silyl group-containing monomer contained in the X block are more than 2.0 on average per molecule of the (meth)acrylic copolymer (A1).

[0031] The repeating units derived from the silyl group-containing monomer contained in the X block are preferably more than 3% by weight, more preferably 4.5% by weight or more, and even more preferably 5% by weight or more, based on the weight of all repeating units contained in the X block. The upper limit of the repeating units derived from the silyl group-containing monomer contained in the X block is preferably 90% by weight or less, more preferably 60% by weight or less, and even more preferably 30% by weight or less.

[0032] In a preferred embodiment, the (meth)acrylic polymer is an XYX triblock polymer, and each of the blocks (X blocks) constituting the terminal portions of the (meth)acrylic polymer preferably has more than one silyl group.

[0033] On the other hand, the repeating units derived from the silyl group-containing monomer contained in the Y block are 0% by weight or more and less than 5% by weight based on the weight of all the repeating units contained in the Y block. The repeating units derived from the silyl group-containing monomer contained in the Y block are preferably 0 to 3% by weight, more preferably 0 to 2% by weight, and even more preferably 0 to 1% by weight based on the weight of all the repeating units contained in the Y block.

[0034] In a (meth)acrylic polymer containing an XY diblock structure or an XYX triblock structure in the molecule, the repeating units derived from a silyl group-containing monomer are localized in the terminal (one or both) regions.

[0035] Specific examples of silyl group-containing monomers include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane.

[0036] [1.3. Other physical properties of (meth)acrylic polymers] In one embodiment, the lower limit of the number average molecular weight of the (meth)acrylic polymer is preferably 1,200 or more, more preferably 2,000 or more, even more preferably 10,000 or more, and particularly preferably 15,000 or more. The upper limit of the number average molecular weight of the (meth)acrylic polymer is preferably 80,000 or less, more preferably 50,000 or less, and even more preferably 40,000 or less. If the number average molecular weight of the (meth)acrylic polymer is within the above range, the viscosity of the curable composition does not become too high, and sufficient workability can be ensured. For example, the number average molecular weight of the (meth)acrylic polymer is preferably 2,000 or more and 50,000 or less.

[0037] In one embodiment, the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the (meth)acrylic polymer (Mw / Mn; molecular weight distribution) is preferably 1.8 or less. The molecular weight distribution of the (meth)acrylic polymer is more preferably 1.7 or less, even more preferably 1.6 or less, even more preferably 1.5 or less, particularly preferably 1.4 or less, and most preferably 1.3 or less. If the molecular weight distribution is too large, the viscosity of the curable composition increases, and the workability tends to decrease.

[0038] In this specification, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are values ​​measured by gel permeation chromatography (GPC). For the GPC measurement, tetrahydrofuran can be used as the mobile phase, and a polystyrene gel column can be used as the stationary phase. These molecular weights can be calculated in terms of polystyrene. Such a (meth)acrylic polymer having a small molecular weight distribution can be suitably produced, for example, by living radical polymerization described later.

[0039] [1.4. Method for producing (meth)acrylic polymer] The polymerization method of the (meth)acrylic polymer is not particularly limited, and known polymerization methods can be used (radical polymerization method, cationic polymerization method, anionic polymerization method, etc.). The polymerization method called SGO (Solid Grade Oligomer; high temperature continuous bulk polymerization) is preferred because it is a method that can obtain a (meth)acrylic polymer without using a polymerization solvent, a polymerization initiator, a chain transfer agent, etc. A living polymerization method is preferred because it can introduce a functional group to the end of the polymer molecule and can synthesize a (meth)acrylic polymer with a small molecular weight distribution. Examples of living polymerization methods include living radical polymerization method, living cationic polymerization method, and living anionic polymerization method, and among them, living radical polymerization method is suitable for polymerization of a (meth)acrylic monomer. Examples of living radical polymerization methods include the following. Atom Transfer Radical Polymerization (ATRP) (see J. Am. Chem. Soc. 1995, 117, 5614; Macromolecules. 1995, 28, 1721) Single Electron Transfer Polymerization (SET-LRP (see J. Am. Chem. Soc. 2006, 128, 14156; JPSChem 2007, 45, 1607)) Reversible Chain Transfer Catalyzed Polymerization (RTCP) (see "Living Radical Polymerization Controlled by Organic Catalysts" Polymer Journal Vol. 68, 223-231 (2011); JP Patent Publication No. 2014-111798) Reversible addition-fragmentation chain transfer polymerization (RAFT polymerization) Nitroxy radical method (NMP method) Polymerization using organotellurium compounds (TERP method) · Polymerization method using organoantimony compounds (SBRP method) Polymerization method using organobismuth compounds (BIRP method) -Iodine transfer polymerization method Examples of methods for introducing a silyl group into a (meth)acrylic polymer include the method described in JP 2007-302749 A and the method described in JP 2018-162394 A. The method described in JP 2007-302749 A introduces a silyl group by converting a functional group at the end of the (meth)acrylic polymer. Specifically, the silyl group is introduced by converting the molecular end of the (meth)acrylic polymer to a hydroxyl group, an alkenyl group, and a silyl group in that order. The method described in JP 2018-162394 A introduces a silyl group by copolymerization with a silyl group-containing (meth)acrylic acid ester monomer. Specifically, a silyl group is introduced near the end of the (meth)acrylic polymer molecule by controlling the input amount of the silyl group-containing (meth)acrylic acid ester monomer according to the progress stage of the living polymerization. The silyl group-containing (meth)acrylic polymer obtained by these methods has a silyl group locally at the end or near the end of the molecule. Use of such a silyl group-containing (meth)acrylic polymer is preferable because it is effective in improving compatibility when mixed with the component (B) and also improves the elongation of the cured product.

[0040] 2. Silyl Group-Containing Polyoxyalkylene Polymer The curable composition according to one embodiment of the present invention contains a silyl group-containing polyoxyalkylene polymer as the component (B1). The curable composition according to one embodiment of the present invention may contain, in addition to the component (B1), a silyl group-containing polyoxyalkylene polymer having a structure different from that of the component (B1) as the component (B2).

[0041] [2.1. Main chain of polyoxyalkylene polymer] The molecular structure of the polyoxyalkylene polymer may be linear or branched. It may also be a mixture of molecules having these structures. Among these, the main chain derived from one or more selected from the group consisting of polyoxypropylene diol and polyoxypropylene triol is particularly preferred.

[0042] An example of the main chain structure of the polyoxyalkylene polymer is a structure represented by the following general formula (3): 8 is a divalent alkylene group. -R 8 -O- (3) The structure represented by formula (3) preferably accounts for 50% by weight or more of the total weight of the polyoxyalkylene polymer, more preferably 70% by weight or more, and even more preferably 90% by weight or more.

[0043] R in general formula (3) 8 The structure of R is not particularly limited as long as it is a divalent alkylene group. 8 is preferably an alkylene group having 1 to 14 carbon atoms, and more preferably a linear or branched alkylene group having 2 to 4 carbon atoms.

[0044] Specific examples of the repeating unit represented by formula (3) include -CH 2 O-, -CH 2 CH 2 O-, -CH 2 CH(CH 3 )O-, -CH 2 CH(C 2 H 5 )O-, -CH 2 C(CH 3 ) 2 O-, -CH 2 CH 2 CH 2 CH 2 Among these, the main chain of the polyoxyalkylene polymer is -CH 2 CH(CH 3 )O- The polyoxyalkylene polymer may contain a urethane bond or a urea bond in the main chain structure.

[0045] As the polyoxyalkylene polymer, commercially available products can be used. Examples of commercially available polyoxyalkylene polymers include Kaneka MS Polymer (registered trademark) S810, S257, and S327 (all manufactured by Kaneka Corporation); Silyl (registered trademark) SAX220, SAT400, SAX510, SAX520, SAX580, SAX750, and SAT145 (all manufactured by Kaneka Corporation); Exestar (registered trademark) ES-S2410, ES-S2420, and ES-S3630 (all manufactured by AGC Corporation); and HMS-1603 and HMS-1207 (all manufactured by Kouma Technology Co., Ltd.).

[0046] [2.2. Silyl group of polyoxyalkylene polymer] The structure of the silyl group contained in the polyoxyalkylene polymer that is the component (B1) is represented by the following formula (1). -Si(OR 1 ) 3 (1) In formula (1), R 1 represents an alkyl group. Three R's exist in the alkoxysilyl group represented by formula (1). 1 may be the same or different. When a plurality of alkoxysilyl groups represented by formula (1) are present in the component (B1), R 1 may be different for each alkoxysilyl group.

[0047] Examples of the alkoxysilyl group represented by formula (1) include a trimethoxysilyl group, a triethoxysilyl group, and a triisopropoxysilyl group.

[0048] The structure of the silyl group contained in the polyoxyalkylene polymer that is the component (B2) is represented by the following formula. -Si(R 4 )(OR 5 ) 2 In the formula, R 4 and R 5 represents an alkyl group. 5may be the same or different. When a plurality of alkoxysilyl groups represented by the above formula are present in (B2), R 5 may be different for each alkoxysilyl group.

[0049] Examples of the alkoxysilyl group represented by the above formula include a dimethoxymethylsilyl group, a diethoxymethylsilyl group, and a diisopropoxymethylsilyl group.

[0050] The polyoxyalkylene polymer may have, in addition to the silyl group represented by the above formula, a silyl group similar to the silyl group contained in the (meth)acrylic polymer explained in Section [1.2.].

[0051] The number of alkoxysilyl groups introduced into the polyoxyalkylene polymer is 1.0 or more, preferably 1.2 or more, more preferably 1.2 to 4.0, and even more preferably 1.5 to 2.5 per molecule. When the number of silyl groups is within the above range, good curability can be imparted to the curable composition.

[0052] In addition to the above, it is also possible to use a polyalkylene polymer having only one silyl group at the end. When used in combination with the above polymer, it is possible to replace the plasticizer component. Furthermore, it is possible to use a polyalkylene polymer obtained by the synthesis method described in JP 2021-75722 A.

[0053] The silyl group of the polyoxyalkylene polymer is preferably located at at least one end of the molecule, and more preferably located at both ends of the molecule. If the silyl group is located at the end of the molecule, good elongation can be imparted to the cured product.

[0054] [2.3. Other physical properties of polyoxyalkylene polymers] The lower limit of the number average molecular weight of the polyoxyalkylene polymer is not particularly limited, and is preferably 2,000 or more, more preferably 3,000 or more, more preferably 10,000 or more, and even more preferably 20,000 or more. The upper limit of the number average molecular weight of the polyoxyalkylene polymer is preferably 70,000 or less, more preferably 50,000 or less. For example, the number average molecular weight of the polyoxyalkylene polymer (polyoxyalkylene polymer (B1) and polyoxyalkylene polymer (B2)) is preferably 3,000 or more and 50,000 or less. By using a high molecular weight polymer having a number average molecular weight of 20,000 or more as the polyoxyalkylene polymer, the elongation of the cured product can be improved.

[0055] The molecular weight distribution of the polyoxyalkylene polymer is preferably 1.6 or less, more preferably 1.5 or less, and further preferably 1.2 or less. If the molecular weight distribution is too large, the viscosity of the curable composition increases, and the workability tends to decrease.

[0056] Such a polyoxyalkylene polymer can be obtained by the method described in

[0011] to

[0058] of JP 2021-55010 A.

[0057] [3. Curing catalyst] The curable composition according to one embodiment of the present invention includes a curing catalyst as component (C). In this specification, the term "curing catalyst" refers to a substance that catalyzes the formation of siloxane bonds by condensing silyl groups together. Examples of the curing catalyst include tin-based curing catalysts and non-tin-based curing catalysts.

[0058] Specific examples of tin-based curing catalysts include dialkyltin carboxylates (dibutyltin dilaurate, dibutyltin diacetate, dibutyltin diethylhexanolate, dibutyltin dioctate, dibutyltin dimethyl maleate, dibutyltin diethyl maleate, dibutyltin dibutyl maleate, dibutyltin diisooctyl maleate, dibutyltin ditridecyl maleate, dibutyltin dibenzyl maleate, dibutyltin maleate, dioctyltin diacetate, dioctyltin distearate, dioctyltin dilaurate, dioctyltin diethyl maleate, dioctyltin diisooctyl maleate, etc.), dialkyltin oxides (dibutyltin oxide, dioctyltin oxide, mixtures of dibutyltin oxide and phthalic acid esters, etc.), tetravalent tin compounds (dialkyltin oxide, dialkyltin diacetate, etc.) and alkoxysilyl group-containing low molecular weight ketones. Examples of the reactants include reaction products with isopropyl compounds (tetraethoxysilane, methyltriethoxysilane, diphenyldimethoxysilane, phenyltrimethoxysilane, etc.), divalent tin compounds (tin octoate, tin naphthenate, tin stearate, etc.), monoalkyltin compounds (monobutyltin compounds (monobutyltin trisoctoate, monobutyltin triisopropoxide, etc.), monooctyltin compounds), reaction products or mixtures of amine compounds and organic tin compounds (reaction products or mixtures of laurylamine and tin octoate, etc.), chelate compounds (dibutyltin bisacetylacetonate, dioctyltin bisacetylcetonate, dibutyltin bisethylacetonate, dioctyltin bisethylacetonate, etc.), and tin alcoholates (dibutyltin dimethylate, dibutyltin diethylate, dioctyltin dimethylate, dioctyltin diethylate, etc.).

[0059] Among these, a mixture of dibutyltin oxide and a phthalate ester and a reaction product of dibutyltin oxide and tetraethoxysilane are preferred because they have high activity as silanol condensation catalysts and cause little coloring of the cured product. Dibutyltin dilaurate is also preferred because it causes little coloring when added to a curable composition, is inexpensive, and is easily available. Tin compounds having a chelate (such as dibutyltin bisacetylacetonate) tend to cause the cured product to be colored yellow or orange. Therefore, it is preferred to reduce the amount of tin compounds having a chelate or not use them at all.

[0060] The amount of the tin-based curing catalyst is preferably 0.1 to 20 parts by weight, and more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the total amount of the (meth)acrylic polymer and the polyoxyalkylene polymer.

[0061] Examples of non-tin curing catalysts include potassium curing catalysts (potassium neodecanoate, potassium octylate, etc.); titanium compounds (tetrabutyl titanate, tetrapropyl titanate, titanium tetrakis(acetylacetonate), bis(acetylacetonate)diisopropoxytitanium, diisopropoxytitanium bis(ethylacetoacetate), etc.); organoaluminum compounds (aluminum tris(acetylacetonate), aluminum tris(ethylacetoacetate), diisopropoxyaluminum ethylacetoacetate, etc.); zirconium compounds (zirconium tetrakis(acetylacetonate) etc.); and bismuth compounds (bismuth octylate, bismuth neodecanoate, etc.). Potassium curing catalysts are preferred in that they can improve the transparency of the cured product.

[0062] Amidine compounds can also be used as non-tin curing catalysts (see, for example, International Publication No. 2008 / 078654). Examples of amidine compounds include 1-(o-tolyl)biguanide, 1-phenylguanidine, 1,2-dimethyl-1,4,5,6-tetrahydropyrimidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene.

[0063] The amount of the non-tin curing catalyst is preferably 0.5 to 20 parts by weight, and more preferably 1 to 10 parts by weight, per 100 parts by weight of the total amount of the (meth)acrylic polymer and the polyoxyalkylene polymer.

[0064] [4. Other Additives] The curable composition according to one embodiment of the present invention may contain various additives, including a plasticizer, in addition to the above-mentioned (meth)acrylic polymer, polyoxyalkylene polymer, and curing catalyst. By containing these additives, various physical properties of the curable composition and the cured product can be adjusted. Examples of additives include the following. These additives may be used alone or in combination of two or more.

[0065] (Filler) The curable composition according to one embodiment of the present invention may contain a filler. Examples of the filler include silica (fumed silica, precipitated silica, crystalline silica, fused silica, dolomite, silicic anhydride, silicic acid hydrate, etc.) and fibrous fillers (glass fibers, glass filaments, etc.).

[0066] The amount of the filler to be added is preferably 0 to 500 parts by weight, more preferably 1 to 200 parts by weight, and particularly preferably 2 to 50 parts by weight, based on 100 parts by weight of the total amount of the (meth)acrylic polymer and the polyoxyalkylene polymer.

[0067] (Dehydrating agent) When the curable composition according to one embodiment of the present invention is used as a one-component curable composition, it is preferable to (i) previously dehydrate and dry the blended components containing water before use, or (ii) dehydrate the composition by heating, reducing pressure, etc. while kneading the components. From this viewpoint, it is preferable to add a dehydrating agent to the curable composition.

[0068] Specific examples of the dehydrating agent include alkoxysilane compounds. The alkoxysilane compounds dehydrate the composition by reacting with water. Examples of the alkoxysilane compounds include n-propyltrimethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, methyl silicate, ethyl silicate, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, and γ-glycidoxypropyltrimethoxysilane. Among these, vinyltrimethoxysilane has a high dehydrating effect and can be preferably used.

[0069] The amount of the dehydrating agent (particularly an alkoxysilane compound capable of reacting with water, such as vinyltrimethoxysilane) is preferably 2 to 15 parts by weight, and more preferably 3 to 10 parts by weight, per 100 parts by weight of the total amount of the (meth)acrylic polymer and the polyoxyalkylene polymer.

[0070] (Adhesion promoter) An adhesion promoter may be added to the curable composition according to one embodiment of the present invention. By adding an adhesion promoter, the risk of the cured product peeling off from an adherend such as concrete can be reduced. In addition, there are cases where it is not necessary to use a primer to improve adhesion. In this case, simplification of the construction work is expected.

[0071] An example of an adhesion promoter is a silane coupling agent.Specific examples of silane coupling agents include isocyanate group-containing silanes (γ-isocyanate propyl trimethoxy silane, γ-isocyanate propyl triethoxy silane, γ-isocyanate propyl methyl diethoxy silane, γ-isocyanate propyl methyl dimethoxy silane, etc.), amino group-containing silanes (γ-aminopropyl trimethoxy silane, γ-aminopropyl triethoxy silane, γ-aminopropyl methyl dimethoxy silane, γ-aminopropyl methyl diethoxy silane, N-(β-aminoethyl)-γ-aminopropyl trimethoxy silane, Methoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldiethoxysilane, γ-ureidopropyltrimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-benzyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, etc.), mercapto group-containing silanes (γ-mercaptopropyltrimethoxysilane, γ- mercaptopropyltriethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, etc.), epoxy group-containing silanes (γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, etc.), carboxysilanes (β-carboxyethyltriethoxysilane, β-carboxyethyltriethoxysilane, Examples of silanes that can be used include silanes containing vinyl-type unsaturated groups (vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloyloxypropylmethyldimethoxysilane, γ-acroyloxypropylmethyltriethoxysilane, etc.), halogen-containing silanes (γ-chloropropyltrimethoxysilane, etc.), and isocyanurate silanes (tris(trimethoxysilyl)isocyanurate, etc.).In addition, derivatives obtained by modifying silane coupling agents, such as amino-modified silyl polymers, silylated amino polymers, unsaturated aminosilane complexes, phenylamino long-chain alkylsilanes, aminosilylated silicones, and silylated polyesters, can also be used as silane coupling agents.

[0072] The amount of the adhesion promoter is preferably 0.1 to 20 parts by weight, and more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the total amount of the (meth)acrylic polymer and the polyoxyalkylene polymer.

[0073] (Physical property adjuster) The curable composition according to one embodiment of the present invention may contain a physical property modifier that adjusts the tensile properties of the cured product. By using the physical property modifier, it is possible to increase the hardness of the cured product, or conversely, to decrease the hardness of the cured product to provide elongation.

[0074] Examples of the physical property adjuster include alkylalkoxysilanes (methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, n-propyltrimethoxysilane, etc.), alkylisopropenoxysilanes (dimethyldiisopropenoxysilane, methyltriisopropenoxysilane, γ-glycidoxypropylmethyldiisopropenoxysilane, etc.), alkoxysilanes having functional groups (γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyldimethylmethoxysilane, γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)aminopropylmethyldimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, etc.), silicone varnishes, and polysiloxanes.

[0075] The amount of the physical property adjusting agent is preferably 0.1 to 80 parts by weight, and more preferably 0.1 to 50 parts by weight, based on 100 parts by weight of the total amount of the (meth)acrylic polymer and the polyoxyalkylene polymer.

[0076] (Thixotropic agent (anti-sagging agent)) The curable composition according to one embodiment of the present invention may contain a thixotropy imparting agent (anti-sagging agent) in order to prevent sagging and improve workability.

[0077] Examples of the thixotropic agent include polyamide waxes, hydrogenated castor oil derivatives, and silicas.

[0078] The amount of the thixotropy-imparting agent is preferably 0.1 to 50 parts by weight, and more preferably 0.2 to 25 parts by weight, based on 100 parts by weight of the total amount of the (meth)acrylic polymer and the polyoxyalkylene polymer.

[0079] (light curing substance) The curable composition according to one embodiment of the present invention may contain a photocurable substance. A photocurable substance is a substance that undergoes a chemical change in a short time by the action of light, resulting in a change in physical properties (such as curing). By containing a photocurable substance, the tackiness (residual tack) of the surface of the cured product can be reduced. A typical photocurable substance can be cured by leaving it at room temperature for one day in a sunny position indoors (such as near a window). Many photocurable substances are known, such as organic monomers, oligomers, resins, and compositions containing these, and the types are not particularly limited. Examples of photocurable substances include unsaturated acrylic compounds, polyvinyl cinnamates, and azido resins.

[0080] Specific examples of unsaturated acrylic compounds include (meth)acrylic acid esters of low molecular weight alcohols (ethylene glycol, glycerin, trimethylolpropane, pentaerythritol, neopentyl alcohol, etc.); (meth)acrylic acid esters of alcohols obtained by modifying acids (bisphenol A, isocyanuric acid) or low molecular weight alcohols with ethylene oxide, propylene oxide, etc.; (meth)acrylic acid esters (polyether polyols whose main chain is polyether and has hydroxyl groups at the terminals, polyols whose main chain is polyether and vinyl monomers are radically polymerized in the polyols whose main chain is polyether). polymer polyols obtained by reacting an epoxy resin (such as bisphenol A type or novolak type) with (meth)acrylic acid, polyester polyols having a polyester main chain and hydroxyl groups at the terminals, and polyols having a vinyl or (meth)acrylic copolymer main chain and hydroxyl groups in the main chain; epoxy acrylate oligomers obtained by reacting an epoxy resin (such as bisphenol A type or novolak type) with (meth)acrylic acid; and urethane acrylate oligomers having urethane bonds and (meth)acrylic groups in the molecular chain obtained by reacting a polyol, a polyisocyanate, a hydroxyl group-containing (meth)acrylate, etc.

[0081] The amount of the photocurable substance to be added is preferably 0.01 to 30 parts by weight based on 100 parts by weight of the total amount of the (meth)acrylic polymer and the polyoxyalkylene polymer.

[0082] (Air oxidation curing substance) The curable composition according to one embodiment of the present invention may contain an air-oxidation curable substance. The air-oxidation curable substance refers to a compound having an unsaturated group that can be crosslinked and cured by oxygen in the air. By containing the air-oxidation curable substance, the tackiness (residual tack) of the surface of the cured product can be reduced. A typical air-oxidation curable substance can be cured by leaving it to stand in the air for one day indoors, for example.

[0083] Examples of air-oxidative curing substances include drying oils (tung oil, linseed oil, etc.); various alkyd resins obtained by modifying drying oils; substances obtained by modifying acrylic polymers, epoxy resins, silicone resins, etc. with drying oils; 1,2-polybutadiene; 1,4-polybutadiene; polymers or copolymers of C5-C8 dienes; various modified products of polymers or copolymers of C5-C8 dienes (malein modified products, boiled oil modified products, etc.). Among the above, tung oil, liquid diene polymers, and modified products thereof are preferred.

[0084] The amount of the air oxidative curing substance to be blended is preferably 0.01 to 30 parts by weight based on 100 parts by weight of the total amount of the (meth)acrylic polymer and the polyoxyalkylene polymer.

[0085] (Antioxidants and Light Stabilizers) The curable composition according to one embodiment of the present invention may contain an antioxidant and / or a light stabilizer. Various antioxidants and light stabilizers are known. For example, the substances described in [Kenichi Saruwatari et al., "Antioxidant Handbook," Taiseisha, 1976] and [Zenjiro Osawa (ed.), "Deterioration and Stabilization of Polymer Materials," CMC, 1990, pp. 235-242] can be mentioned.

[0086] Examples of the antioxidant include thioether-based antioxidants such as ADK STAB PEP-36 and ADK STAB AO-23 (all manufactured by ADEKA CORPORATION), phosphorus-based antioxidants such as Irgafos38, Irgafos168 and IrgafosP-EPQ (all manufactured by Chiba Specialty Chemicals), and hindered phenol-based antioxidants. Among the above, the hindered phenol-based antioxidants are preferred.

[0087] Specific examples of hindered phenol-based antioxidants include 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butyl-4-ethylphenol, mono (or di or tri) (α-methylbenzyl)phenol, 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), 4,4'-butylidenebis(3-methyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol), and 2,5-di-t-butylhydroquinone. , 2,5-di-t-amylhydroquinone, triethylene glycol-bis-[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylene 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,5-di-t-butyl-4-hydroxybenzyl)propionate, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 3,5-di-t-butyl-4-hydroxy-benzylphosphonate-diethyl ester, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,5-di-t-butyl-4-hydroxybenzyl)propionate ethyl benzylphosphonate) calcium, tris-(3,5-di-t-butyl-4-hydroxybenzyl) isocyanurate, 2,4-bis[(octylthio)methyl]o-cresol, N,N'-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyl]hydrazine, tris(2,4-di-t-butylphenyl)phosphite, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)-benzotriazole, methyl-3-[3-t-bu ethyl-5-(2H-benzotriazol-2-yl)-4-hydroxyphenyl]propionate-polyethylene glycol (molecular weight about 300) condensate, hydroxyphenylbenzotriazole derivatives, 2-(3,5-di-t-butyl-4-hydroxybenzyl)-2-n-butylmalonic acid bis(1,2,2,6,6-pentamethyl-4-piperidyl), 2,4-di-t-butylphenyl-3,5-di-t-butyl-4-hydroxybenzoate.

[0088] Examples of commercially available antioxidants include Nocrac 200, Nocrac M-17, Nocrac SP, Nocrac SP-N, Nocrac NS-5, Nocrac NS-6, Nocrac NS-30, Nocrac 300, Nocrac NS-7, and Nocrac DAH (all manufactured by Ouchi Shinko Chemical Industry Co., Ltd.); ADK STAB AO-30, ADK STAB AO-40, ADK STAB AO-50, ADK STAB AO-60, ADK STAB AO-616, ADK STAB AO-635, ADK STAB AO-658, ADK STAB AO-80, ADK STAB AO-15, ADK STAB AO-18, ADK STAB 328, and ADK STAB AO-37 (all manufactured by ADEKA Corporation); IRGANOX-245, IRGANOX-259, IRGANOX-565, IRGANOX-1010, IRGANOX-1024, IRGANOX-1035, IRGANOX-1076, IRGANOX-1081, IRGANOX-1098, IRGANOX-1222, IRGANOX-1330, IRGANOX-1425WL (all manufactured by Chiba Specialty Chemicals); Sumilizer GM, Sumilizer GA-80, Sumilizer GS (all manufactured by Sumitomo Chemical Co., Ltd.).

[0089] Examples of light stabilizers include ultraviolet absorbers (benzotriazole compounds such as Tinuvin P, Tinuvin 234, Tinuvin 320, Tinuvin 326, Tinuvin 327, Tinuvin 329, and Tinuvin 213 (all manufactured by BASF); triazine light stabilizers such as Tinuvin 1577, benzophenone compounds such as CHIMASSORB81; benzoate compounds such as Tinuvin 120 (manufactured by BASF); and hindered amine compounds). Of the above, hindered amine compounds are preferred.

[0090] Specific examples of the hindered amine compound include dimethyl succinate-1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate, poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}], N,N'-bis(3aminopropyl)ethylenediamine-2,4-bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino]-6-chloro-1,3,5-triazine condensate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, and bis(2,2,6,6-tetramethyl-4-piperidinyl)succinate.

[0091] Examples of commercially available light stabilizers include TINUVIN 622LD, TINUVIN 144, TINUVIN 770, TINUVIN 765, CHIMASSORB944LD, CHIMASSORB119FL (all manufactured by BASF), Adeka STAB LA-52, Adeka STAB LA-57, Adeka STAB LA-62, Adeka STAB LA-67, Adeka STAB LA-63, Adeka STAB LA-68, Adeka STAB LA-82, and Adeka STAB LA-87 (all manufactured by ADEKA).

[0092] An antioxidant and a light stabilizer may be used in combination. By using them in combination, the effect of each agent may be further improved, and the heat resistance, weather resistance, etc. of the cured product may be improved. For example, in order to improve weather resistance, an ultraviolet absorber and a hindered amine compound (HALS) may be combined. This combination is preferable because it can further improve the effect of each agent.

[0093] The amount of the antioxidant and / or the light stabilizer to be added is preferably 0.1 to 20 parts by weight, based on 100 parts by weight of the total amount of the (meth)acrylic polymer and the polyoxyalkylene polymer.

[0094] [5. Curable composition] The curable composition according to one embodiment of the present invention contains the above-described components (A), (B), and (C), and optionally other additives. The curable composition can be prepared by appropriately mixing the components (A), (B), and (C), and optionally other additives.

[0095] [5.1. Composition and properties of the curable composition] In the curable composition, the lower limit of the content of the polyoxyalkylene polymer is preferably 5 parts by weight or more, more preferably 30 parts by weight or more, and even more preferably 40 parts by weight or more, when the content of the (meth)acrylic polymer is 100 parts by weight. The upper limit of the content of the polyoxyalkylene polymer is preferably 300 parts by weight or less, more preferably 280 parts by weight or less, and even more preferably 250 parts by weight or less, when the content of the (meth)acrylic polymer is 100 parts by weight. If the content ratio of the (meth)acrylic polymer to the polyoxyalkylene polymer is within the above range, a cured product with excellent weather resistance can be obtained. In order to ensure weather resistance for a longer period of time, it is preferable to mix more (meth)acrylic polymer than polyoxyalkylene polymer.

[0096] The curable composition preferably has excellent storage stability. In this specification, "excellent storage stability" means that the curable composition after preparation can maintain a liquid state without gelling after storing (standing) at 50°C for a sufficient time (for example, 1 week, 2 weeks, 3 weeks, or 4 weeks). For more details on the method for evaluating storage stability, see the examples described below.

[0097] [5.2. Form and Use of Curable Composition] The curable composition according to one embodiment of the present invention is a one-component type curable composition. The one-component type curable composition is a composition in which all the blending components are blended in advance and then sealed and stored. The one-component type curable composition is usually cured by moisture in the air after use (after opening), but in the conventional curable composition, the curing reaction proceeds even during storage (sealed), and problems such as gelation of the curable composition may occur. On the other hand, the curable composition according to one embodiment of the present invention has excellent storage stability due to the above-mentioned configuration. That is, there is no risk of gelation during storage (sealed), and it can be stored stably for a long time. Therefore, the curable composition according to one embodiment of the present invention can be suitably used as a one-component type curable composition.

[0098] The use of the curable composition is not particularly limited. Examples include architectural and industrial sealants, electrical and electronic component materials (such as solar cell back sealants), electrical insulating materials (such as wire and cable insulating coating materials), pressure sensitive adhesives, adhesives, elastic adhesives, contact adhesives, tile adhesives, paints, coating materials, sealing materials for can lids, etc., electrical and electronic potting agents, films, gaskets, casting materials, various molding materials, artificial marble, rust-proofing and waterproofing sealants for cut parts of wire-reinforced glass or laminated glass, and waterproofing agents.

[0099] Examples of the method of applying the curable composition include hand application (using a trowel, etc.), bead application, and application by roller or spray. In order to increase strength, it is preferable to apply the curable composition so as to obtain a cured product having a thickness of 2 to 20 mm. In this case, it is preferable to adjust the viscosity of the curable composition to a certain level or higher. On the other hand, when applying to a complex surface or when it is desired to improve workability, it is preferable to spray apply a curable composition having a low viscosity. In this case, it is preferable to perform spray application several times since it is possible to adjust the thickness to the desired thickness.

[0100] One embodiment of the present invention also includes a cured product obtained by curing the above-mentioned curable composition. The shape of the cured product is not limited, and may be, for example, a film (cured film). The thickness of the cured film may be 2 to 20 mm.

[0101] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in the different embodiments are also included in the technical scope of the present invention.

[0102] An embodiment of the present invention may include the following features. <1> A curable composition comprising (A) a silyl group-containing (meth)acrylic polymer, (B1) a silyl group-containing polyoxyalkylene polymer, and (C) a curing catalyst, wherein the (A) silyl group-containing (meth)acrylic polymer comprises a (meth)acrylic copolymer (A1) having an alkoxysilyl group, the (meth)acrylic copolymer (A1) having an XY diblock structure or an XYX triblock structure having an X block and a Y block in the molecule, and the X block is comprised of an alkoxysilyl group-containing (meth)acrylic acid ester monomer derived therefrom. a repeating unit derived from a (meth)acrylic acid ester monomer having an alkoxysilyl group contained in the Y block is 0% by weight or more and less than 5% by weight based on the weight of all repeating units contained in the Y block; the molecular weight distribution (Mw / Mn) of the (meth)acrylic copolymer (A1) is 1.8 or less; and the silyl group-containing polyoxyalkylene polymer (B1) has 1.0 or more alkoxysilyl groups represented by the following formula (1) per molecule: -Si(OR 1 ) 3 (1) [In formula (1), R 1 represents an alkyl group. Three R's exist in the alkoxysilyl group represented by formula (1). 1 may be the same or different. When a plurality of alkoxysilyl groups represented by formula (1) are present in the silyl group-containing polyoxyalkylene polymer (B1), R 1 may be different for each alkoxysilyl group. <2> The (A) silyl group-containing (meth)acrylic polymer is 2 CH=CHCOOR 3 (In the formula, R 2 is a hydrogen atom or a methyl group, and R 3 is a group having 9 or more carbon atoms), <1> The curable composition according to claim 1. <3> The number average molecular weight of the (A) silyl group-containing (meth)acrylic polymer is 2,000 or more and 50,000 or less. <1> or <2> The curable composition according to claim 1. <4> The (B1) silyl group-containing polyoxyalkylene polymer has a number average molecular weight of 3,000 or more and 50,000 or less. <1> ~ <3> 13. The curable composition according to claim 12 . <5> The composition further comprises (B2) a silyl group-containing polyoxyalkylene polymer, the (B2) silyl group-containing polyoxyalkylene polymer having 1.0 or more alkoxysilyl groups represented by the following formula per molecule: <1> ~ <4> The curable composition according to any one of the above: -Si(R 4 )(OR 5 ) 2 [In the formula, R 4 and R 5 represents an alkyl group. 5 may be the same or different. When a plurality of alkoxysilyl groups represented by the above formula are present in the silyl group-containing polyoxyalkylene polymer (B2), R 5 may be different for each alkoxysilyl group. <6> The (B2) silyl group-containing polyoxyalkylene polymer has a number average molecular weight of 3,000 or more and 50,000 or less. <5> The curable composition according to claim 1. <7> <1> ~ <6> 2. A cured product obtained by curing the curable composition according to claim 1. EXAMPLES

[0103] An embodiment of the present invention will now be described.

[0104] [Measurement method] [Number average molecular weight] The following device was used to measure the number average molecular weight. The measured value is a polystyrene-equivalent molecular weight. Liquid delivery system: HLC-8120GPC (Tosoh Corporation) Column: TSK-GEL H type (Tosoh Corporation) Solvent: THF.

[0105] [Terminal silyl group introduction rate] 1 The introduction rate of terminal silyl groups was calculated from the results of H-NMR measurement. 1 The following equipment was used for H-NMR measurements. Measuring instrument: JNM-LA400 (manufactured by JEOL Ltd.) Solvent: CDCl 3 .

[0106] [material] <(A) Silyl Group-Containing (Meth)Acrylic Polymer> As the (A) silyl group-containing (meth)acrylic polymer, a silyl group-containing (meth)acrylic polymer ((A1) silyl group-containing (meth)acrylic polymer) obtained by the method described in Production Example 1 below was used.

[0107] [Production Example 1] (preparation) A 2000 mL three-neck flask was prepared, and 108 g of ethyl acrylate, 707 g of n-butyl acrylate, and 186 g of octadecyl acrylate were added to the flask and mixed to obtain a mixture. Hereinafter, this mixture is referred to as a "(meth)acrylic acid ester monomer mixture."

[0108] Next, a stirring vessel is prepared, and cupric bromide (CuBr 2 ) 52.7mg, Hexamethyltris(2-aminoethyl)amine (Me 6 54.4 mg of TREN and 1.82 g of methanol were added and stirred under a nitrogen stream until a homogeneous solution was obtained. Hereinafter, the homogeneous solution obtained is referred to as a "copper solution." The amount of copper contained in the obtained copper solution was equivalent to 15 ppm with respect to the total amount of the (meth)acrylic acid ester monomer mixture.

[0109] In addition, a separate stirring vessel was prepared, and 30.8 mL of methanol, 1.0 g of ascorbic acid, and 1.6 mL of triethylamine were charged into the stirring vessel, and stirred under a nitrogen stream until a homogeneous solution was obtained. The resulting homogeneous solution is referred to as the "ascorbic acid solution."

[0110] (1st step) 5.60g (0.029 mol) of α-ethyl bromobutyrate (initiator), 20% by weight of the total amount of the (meth)acrylic acid ester monomer mixture obtained by the above operation, 10g (0.045 mol; 1.5 molar equivalent to the initiator) of 3-methacryloxypropylmethyldimethoxysilane, 107.68g of methanol (manufactured by Wako Pure Chemical Industries, Ltd.), and the total amount of the copper solution obtained by the above operation were charged into a stirrer, and stirred for 30 minutes under a nitrogen gas flow to obtain a homogeneous solution. The stirrer used in the first step was a stirrer with a jacket temperature control, and the jacket temperature was set to 45°C.

[0111] Next, when the temperature in the polymerization system reached 40° C. or higher, the ascorbic acid solution obtained by the above-mentioned operation was continuously added dropwise to initiate the polymerization reaction. The rate at which the ascorbic acid solution was added was set to a rate at which 144 mg of ascorbic acid was added to the polymerization system per hour.

[0112] When the temperature in the polymerization system was monitored, it rose at the same time as the drop of the ascorbic acid solution started, and after reaching the maximum temperature, the temperature gradually decreased. When the temperature difference between the temperature in the polymerization system and the jacket temperature reached 1°C, a small amount of the reaction solution in the polymerization system was sampled and analyzed by gas chromatography. As a result, 90% by weight of the (meth)acrylic acid ester monomer mixture initially charged was consumed by the polymerization reaction.

[0113] (2nd process) Next, the remaining (meth)acrylic acid ester monomer mixture that was not added in the first step (80% by weight of the total amount) was continuously dropped into the above polymerization system over a period of 90 minutes. During this time, the ascorbic acid solution was continuously dropped. The dropping rate of the ascorbic acid solution was set to a rate at which 48 mg of ascorbic acid solution was added to the polymerization system per hour, and the dropping rate of the (meth)acrylic acid ester monomer mixture was set to 334 g. In addition, the reaction solution in the polymerization system was successively sampled and analyzed by gas chromatography. Then, polymerization was continued until 88% by weight of the total amount (100% by weight) of the (meth)acrylic acid ester monomer mixture added to the polymerization system was consumed by the polymerization reaction.

[0114] (3rd step) Next, 11 g (0.049 mol; 1.6 molar equivalents relative to the initiator) of 3-methacryloxypropylmethyldimethoxysilane was added to the polymerization system to continue polymerization. During this time, the ascorbic acid solution was continuously added dropwise until 98% by weight of the total amount of the (meth)acrylic acid ester monomer mixture added to the polymerization system was consumed. Thereafter, the addition of the ascorbic acid solution was stopped to terminate the polymerization.

[0115] After the polymerization was completed, the jacket temperature was changed to 80° C., and the solvent was then removed from the polymerization system. A diaphragm pump was used first, and then a vacuum pump was used for the removal of the solvent. After the removal of the solvent, the jacket temperature was cooled to 60° C. or less.

[0116] (purification) 1000g of butyl acetate was added to a jacket temperature-controlled stirring device and mixed with the polymer after devolatilization until a homogeneous solution was obtained. An adsorbent was added to the homogeneous solution obtained and stirred for 1 hour. As the adsorbent, 10g of Kyoward 500SH (manufactured by Kyowa Chemical Industry Co., Ltd.) and 10g of Kyoward 700SEN-S (manufactured by Kyowa Chemical Industry Co., Ltd.) were used.

[0117] After the stirring was completed, the mixture was filtered through a filter equipped with a bag filter cloth. This resulted in a clear polymer solution. 1.5 g of an antioxidant (Sumilizer GS; manufactured by Sumitomo Chemical) was added to the solution and mixed until homogenous. The solvent was then removed from the solution to obtain a silyl group-containing (meth)acrylic polymer (A1). For the removal of the volatilization, a diaphragm pump was used first, followed by a vacuum pump. The obtained (A1) silyl group-containing (meth)acrylic polymer contained an XYX triblock structure in the molecule having an X block derived from 3-methacryloxypropylmethyldimethoxysilane and a Y block derived from ethyl acrylate, n-butyl acrylate, and octadecyl acrylate, the repeating units derived from the (meth)acrylic acid ester monomer having an alkoxysilyl group contained in the X block were 304 on average, the repeating units derived from the (meth)acrylic acid ester monomer having an alkoxysilyl group contained in the Y block were 1.1% by weight based on the weight of all the repeating units contained in the Y block, and the molecular weight distribution (Mw / Mn) was 1.11. In the following, the (A1) silyl group-containing (meth)acrylic polymer may be simply referred to as "(A1)".

[0118] <(A') Silyl Group-Containing (Meth)Acrylic Polymer> As the silyl group-containing (meth)acrylic polymer (A'), a silyl group-containing (meth)acrylic polymer obtained by the method described in the following Comparative Production Example 1 was used. Note that the silyl group-containing (meth)acrylic polymer (A') does not contain X blocks as a whole molecule, and therefore does not correspond to the silyl group-containing (meth)acrylic copolymer (A) in one embodiment of the present invention.

[0119] [Comparative Production Example 1] A (meth)acrylic polymer having a methyldimethoxysilyl group introduced at the molecular end (another silyl group-containing (meth)acrylic polymer) was synthesized by the following procedure. 1. The inside of a stainless steel reaction vessel equipped with a stirrer was deoxidized, and 7.7 g of cuprous bromide and 200 g of butyl acrylate were placed in the reaction vessel and stirred while heating. 2. 90 g of acetonitrile and 17.6 g of diethyl 2,5-dibromoadipate (initiator) were added to the reaction vessel and mixed. The temperature of the mixture was adjusted to about 80° C., and then pentamethyldiethylenetriamine was added to initiate the polymerization reaction. 3. 800 g of butyl acrylate was gradually added to the reaction vessel to proceed with the polymerization reaction. During the polymerization reaction, pentamethyldiethylenetriamine was appropriately added to adjust the polymerization rate. The total amount of pentamethyldiethylenetriamine used during the polymerization was 1.4 g. During the polymerization reaction, the internal temperature of the reaction vessel was adjusted to about 80°C to about 90°C. 4. When the monomer conversion rate (polymerization reaction rate) reached about 95% or more, the volatile matter was removed by devolatilization under reduced pressure to obtain a concentrated (meth)acrylic polymer. 5. To the reaction vessel (i.e., to the polymer concentrate obtained in step 4) were added 200 g of 1,7-octadiene, 260 g of acetonitrile, and 3.1 g of pentamethyldiethylenetriamine. 6. The reaction vessel was heated and stirred for several hours while controlling the internal temperature to about 80° C. to about 90° C. As a result, the polymer terminals of the (meth)acrylic polymer were reacted with 1,7-octadiene, and an alkenyl group was introduced into the terminals of the (meth)acrylic polymer. 7. Acetonitrile and unreacted 1,7-octadiene were removed by volatilization under reduced pressure to obtain a concentrated (meth)acrylic polymer having alkenyl groups at its ends. 8. The concentrate obtained in step 7 was diluted with butyl acetate, and a filter aid and an adsorbent (Kyoward 700SEN and Kyoward 500SH, manufactured by Kyowa Chemical Industry) were added. 9. The mixture obtained in step 8 was heated and stirred at about 80° C. to 100° C., and the solid components were then filtered off. The filtrate was then concentrated to obtain a crude polymer. 10. To the resulting crude polymer, a heat stabilizer (Sumilizer GS, manufactured by Sumitomo Chemical Co., Ltd.) and an adsorbent (Kyoward 700SEN and Kyoward 500SH) were added. 11. The temperature of the crude polymer was increased while the volatilization under reduced pressure and the heating and stirring were continued at about 170° C. to about 200° C. for several hours. 12. To the crude polymer, adsorbents (Kyoward 700SEN and Kyoward 500SH) and butyl acetate in an amount approximately 10 times by weight relative to the crude polymer were added, and the mixture was heated and stirred at approximately 170°C to approximately 200°C for several hours to obtain a treated liquid. 13. The treated liquid obtained in step 12 was further diluted with butyl acetate, and the adsorbent was filtered off. The filtrate was concentrated to obtain a polymer having alkenyl groups at both ends. 14. 500 g of the polymer having alkenyl groups at its ends obtained in step 13 was mixed with 7.7 g of methyldimethoxysilane, 2.5 g of methyl orthoformate, and 50 mg of platinum catalyst, and the mixture was heated and stirred at about 100° C. for about 1 hour. An isopropanol solution of bis(1,3-divinyl-1,1,3,3-tetramethyldisiloxane) platinum complex catalyst was used as the platinum catalyst. 15. After heating and stirring, volatile components (unreacted methyldimethoxysilane, etc.) were distilled off under reduced pressure to obtain a (meth)acrylic polymer ((A') silyl group-containing (meth)acrylic polymer) having methyldimethoxysilyl groups introduced at the molecular ends. The obtained (meth)acrylic polymer (A') had a number average molecular weight of 27,000, a molecular weight distribution of 1.2, and the number of silyl groups introduced per molecule was 2.0.

[0120] <(B1) Silyl Group-Containing Polyoxyalkylene Polymer> ((B1-1) Silyl Group-Containing Polyoxyalkylene Polymer) As the (B1-1) silyl group-containing polyoxyalkylene polymer, which is the (B1) silyl group-containing polyoxyalkylene polymer, a polymer obtained by the method described in paragraphs

[0175] (Synthesis Example 4) and

[0176] (Synthesis Example 5) of JP 2021-55010 A was used. The obtained (B1-1) silyl group-containing polyoxyalkylene polymer had 1.6 trimethoxysilyl groups per molecule and was a silyl group-containing polyoxyalkylene polymer having a number average molecular weight of 28,500.

[0121] ((B1-2) Silyl Group-Containing Polyoxyalkylene Polymer) As the (B1-2) silyl group-containing polyoxyalkylene polymer, which is the (B1) silyl group-containing polyoxyalkylene polymer, a polymer obtained by the method described in paragraphs

[0175] (Synthesis Example 4) and

[0178] (Synthesis Example 7) of JP 2021-55010 A was used. The obtained (B1-2) silyl group-containing polyoxyalkylene polymer had 2.1 trimethoxysilyl groups per molecule and was a silyl group-containing polyoxyalkylene polymer having a number average molecular weight of 26,200.

[0122] <(B2) Silyl Group-Containing Polyoxyalkylene Polymer> ((B2-1) Silyl Group-Containing Polyoxyalkylene Polymer) As the (B2) silyl group-containing polyoxyalkylene polymer, a silyl group-containing polyoxyalkylene polymer (B2-1), a polymer obtained by the method described in

[0166] (Synthesis Example 1-2) and paragraph

[0176] (Synthesis Example 2-8) of JP 2020-158733 A was used. The obtained (B2-1) silyl group-containing polyoxyalkylene polymer had 1.4 methyldimethoxysilyl groups per molecule and was a silyl group-containing polyoxyalkylene polymer having a number average molecular weight of 28,000.

[0123] [Example] Example 1 50g of (A1) was mixed with 50g of (B1-1), 1g of Siluest_A171 as a dehydrating agent, and 2g of Siluest_A1120 as an adhesion promoter (both manufactured by Momentive Performance Materials Japan, LLC), and mixed uniformly with a spoon. 1.5g of the reaction product of dibutyltin oxide and dioctyl acid phthalate (No. 918 (old) manufactured by Sankyoki Synthetic Co., Ltd.) as a curing catalyst (C) was added thereto, and mixed thoroughly with a stirring defoamer (Awatori Rentaro ARE250 manufactured by Thinky Corporation) to obtain a one-liquid curable composition.

[0124] The viscosity of the obtained curable composition immediately after preparation (initial viscosity) and after standing at 50°C for 1 week, 2 weeks, 3 weeks or 4 weeks (viscosity when stored at 50°C) were measured using a cone-plate type E-type viscometer (TVB-25, manufactured by Toki Sangyo Co., Ltd.). Furthermore, the viscosity increase rate (viscosity increase rate when stored at 50°C) was calculated based on the following formula. The results are shown in Table 1: Viscosity increase rate when stored at 50°C = viscosity when stored at 50°C / initial viscosity.

[0125] Example 2 A curable composition was prepared in the same manner as in Example 1, except that (B1-2) was used instead of (B1-1), and the initial viscosity and the viscosity when stored at 50° C. were measured, and the viscosity increase rate when stored at 50° C. was calculated. The results are shown in Table 1.

[0126] Example 3 A curable composition was prepared in the same manner as in Example 1, except that the amount of (B1-1) was changed to 30 g and 20 g of (B2-1) was newly added, and the initial viscosity and the viscosity when stored at 50° C. were measured, and the viscosity increase rate when stored at 50° C. was calculated. The results are shown in Table 1.

[0127] Comparative Example 1 A curable composition was prepared in the same manner as in Example 1, except that the silyl group-containing (meth)acrylic polymer (A') prepared in Comparative Production Example 1 was used instead of (A1), and the initial viscosity and the viscosity after storage at 50°C were measured, and the viscosity increase rate after storage at 50°C was calculated. The results are shown in Table 1.

[0128] Comparative Example 2 A curable composition was prepared in the same manner as in Example 2, except that the silyl group-containing (meth)acrylic polymer (A') prepared in Comparative Production Example 1 was used instead of (A1), and the initial viscosity and the viscosity after storage at 50°C were measured, and the viscosity increase rate after storage at 50°C was calculated. The results are shown in Table 1.

[0129] Comparative Example 3 A curable composition was prepared in the same manner as in Example 3, except that the silyl group-containing (meth)acrylic polymer (A') prepared in Comparative Production Example 1 was used instead of (A1), and the initial viscosity and the viscosity after storage at 50°C were measured, and the viscosity increase rate after storage at 50°C was calculated. The results are shown in Table 1.

[0130] [Table 1]

[0131] <Result> The curable compositions of Comparative Examples 1 to 3 using the silyl group-containing (meth)acrylic polymer (A') obtained by Comparative Production Example 1 gelled after 3 weeks of storage at 50°C, indicating that they have problems with storage stability. In contrast, the curable compositions of Examples 1 to 3 using (A1) showed low viscosity increase rates and maintained a liquid state even after storage at 50°C for 4 weeks. In other words, it was demonstrated that the curable composition according to one embodiment of the present invention has good storage stability. [Industrial Applicability]

[0132] One aspect of the present invention provides a curable composition having excellent storage stability.

Claims

1. (A) a silyl group-containing (meth)acrylic polymer; (B1) a silyl group-containing polyoxyalkylene polymer; (C) a curing catalyst, The (A) silyl group-containing (meth)acrylic polymer contains a (meth)acrylic copolymer (A1) having an alkoxysilyl group, The (meth)acrylic copolymer (A1) contains, in a molecule, an XY diblock structure having an X block and a Y block or an XYX triblock structure, the number of repeating units derived from a (meth)acrylic acid ester monomer having an alkoxysilyl group contained in the X block is more than 2.0 on average, a repeating unit derived from a (meth)acrylic acid ester monomer having an alkoxysilyl group contained in the Y block is 0% by weight or more and less than 5% by weight based on the weight of all repeating units contained in the Y block, The (meth)acrylic copolymer (A1) has a molecular weight distribution (Mw / Mn) of 1.8 or less, The silyl group-containing polyoxyalkylene polymer (B1) is a curable composition having 1.0 or more alkoxysilyl groups represented by the following formula (1) per molecule: -Si(OR 1 ) 3 ...(1) [In formula (1), R 1 represents an alkyl group. Three R's exist in the alkoxysilyl group represented by formula (1). 1 may be the same or different. When a plurality of alkoxysilyl groups represented by formula (1) are present in the silyl group-containing polyoxyalkylene polymer (B1), R 1 may be different for each alkoxysilyl group.

2. The (A) silyl group-containing (meth)acrylic polymer is R 2 CH=CHCOOR 3 (In the formula, R 2is a hydrogen atom or a methyl group, R 3 The curable composition according to claim 1 , comprising 1% by weight or more of repeating units derived from (wherein

3. The curable composition according to claim 1, wherein the number average molecular weight of the silyl group-containing (meth)acrylic polymer (A) is 2,000 or more and 50,000 or less.

4. The curable composition according to claim 1, wherein the number average molecular weight of the silyl group-containing polyoxyalkylene polymer (B1) is 3,000 or more and 50,000 or less.

5. Further, (B2) a silyl group-containing polyoxyalkylene polymer is contained, The curable composition according to claim 1, wherein the silyl group-containing polyoxyalkylene polymer (B2) has 1.0 or more alkoxysilyl groups represented by the following formula per molecule: -Si(R 4 ) (OR 5 ) 2 [In the formula, R 4 and R 5 represents an alkyl group. 5 may be the same or different. In addition, when a plurality of alkoxysilyl groups represented by the above formula are present in the silyl group-containing polyoxyalkylene polymer (B2), R 5 may be different for each alkoxysilyl group.

6. The curable composition according to claim 5, wherein the number average molecular weight of the silyl group-containing polyoxyalkylene polymer (B2) is 3,000 or more and 50,000 or less.

7. A cured product obtained by curing the curable composition according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Water crosslinking encapsulant

    JP2011525201A

  • Curable composition

    JP2002294022A