Fiber assembly
A fiber aggregate with varying fineness and density enhances sound absorption and flame resistance in the low frequency range, addressing the limitations of conventional materials by combining flame-resistant fibers in a nonwoven fabric structure.
Patent Information
- Application Number
- JP2023049098
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-07
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024137541000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a fiber assembly having flame resistance. [Background technology]
[0002] Flame-resistant fiber nonwoven fabrics are desirable as lightweight materials with excellent flame resistance, sound absorption, and heat insulation properties, and are suitable for use in automobiles, railway vehicles, aircraft, air conditioners, building materials, and other applications. For example, in the automotive sector, there is a strong demand for parts manufacturers to develop lightweight, high-performance sound-absorbing materials in response to the worsening noise caused by the industry trend toward weight reduction.
[0003] Noises generated during acceleration or transmission fluctuations in automobiles occur in the relatively low frequency range of 100 to 2,000 Hz. Therefore, the porous materials used in conventional noise control measures are thick and heavy, and are not suitable for transportation machinery from the perspective of weight reduction. Generally, sound-absorbing materials used in automobiles are nonwoven fabrics, urethane foam, etc. These materials have good sound-absorbing properties in the high frequency range (above 2,000 Hz), but their effectiveness is reduced in the low frequency range of 100 to 2,000 Hz. In addition, with the shift to electric vehicles (EVs), noises that were previously hidden behind engine noise have become apparent. These noises include wind noise, road noise, and motor noise. The frequency range of these noises is also 100 to 2,000 Hz.
[0004] In the engine compartment of an automobile, various soundproofing materials are used under the hood, under the engine, between the engine and the cabin, in the muffler, etc., to prevent the resonance of the sound emitted from the engine or to prevent the sound itself from escaping to the outside. These engines and mufflers can reach temperatures of over 300°C during normal use, but in recent years, the temperature rise in the engine compartment has become more noticeable due to the narrowing of engine compartments and the downsizing of engine cover parts, so the sound-absorbing materials used must be heat-resistant and flame-retardant. In addition, with the shift to electric vehicles (EVs), lithium-ion batteries are becoming increasingly high-capacity, and there is a growing need to improve safety. As there have been frequent fires in electric vehicles caused by lithium-ion batteries igniting, there is a demand for flame-resistant materials that can withstand the violent ignition of lithium-ion batteries.
[0005] Conventional sound-absorbing materials made of 100% polyester fiber do not have sufficient heat resistance, and improvements are being sought. In the past, inexpensive rock wool or glass fiber was often used to manufacture these heat-resistant, flame-retardant sound-proofing materials, but heat-resistant organic fibers have gradually come to be used due to the need to make automobiles lighter and the problem of industrial waste disposal when scrapping cars.
[0006] Recently, nonwoven fabrics have been introduced as heat-resistant sound absorbing materials, which use heat-resistant organic fibers, such as aramid fibers, with a melting temperature of 350°C or higher, and which are further compounded with silicate minerals, alumina particles, mica particles, etc., as flame retardant and heat-resistant components to provide heat resistance (see, for example, Patent Documents 1 to 3). Additionally, stitch-bonded nonwoven fabrics using flame-resistant fibers obtained by oxidizing acrylic synthetic fibers (see, for example, Patent Document 4) and nonwoven fabrics made from a mixture of flame-resistant and flame-retardant fibers (see, for example, Patent Document 5) have also been introduced. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2006-138935 A [Patent Document 2] JP 2006-321053 A [Patent Document 3] Japanese Patent Application Publication No. 6-212593 [Patent Document 4] JP 2006-195104 A [Patent Document 5] JP 2003-129362 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, the former method has a problem in that a complicated process is unavoidably required to insert and adhere heat-resistant inorganic particles between heat-resistant organic fibers. The latter method has the problem that the method of making a nonwoven fabric is limited to stitch bonding because a very brittle flame-resistant fiber is used, and it is difficult to obtain a high-density nonwoven fabric. In addition, the method is very expensive. Furthermore, the latter method has the problem that it is less effective at providing the sound absorption characteristics currently required in the low frequency range of 100 to 2,000 Hz.
[0009] An object of the present invention is to provide a fiber assembly having excellent flame resistance and sound absorbing properties. [Means for solving the problem]
[0010] The present invention was realized as a result of intensive research by the present inventors in order to solve the above-mentioned problems. In the present invention, the inventors discovered that the sound absorption coefficient at a specific frequency can be increased by using flame-resistant fibers with a small fiber diameter as part of the material of the nonwoven fabric, and arrived at the present invention. [1] A fiber assembly comprising a flame-resistant fiber (A) having a single fiber fineness of 1.0 dtex or more and a flame-resistant fiber (B) having a single fiber fineness of less than 1.0 dtex. [2] A fiber assembly according to [1], wherein the flame-resistant fiber (A) and the flame-resistant fiber (B) have a limiting oxygen index of 45 or more. [3] The fiber assembly according to [1] or [2], wherein the difference in fineness between the flame-resistant fiber (A) and the flame-resistant fiber (B) is 0.3 dtex or more. [4] The fiber assembly according to any one of [1] to [3], which is a nonwoven fabric. [5] The fiber assembly according to any one of [1] to [4], wherein the flame-resistant fiber (A) and the flame-resistant fiber (B) are mixed. [6] The fiber assembly according to any one of [1] to [5], which consists only of the flame-resistant fiber (A) and the flame-resistant fiber (B). [7] The fiber assembly according to any one of [1] to [6], wherein a mass ratio of the flame-resistant fiber (A) to the flame-resistant fiber (B) is 20:80 to 80:20. [8] The fiber density of the flame-resistant fiber (A) and the flame-resistant fiber (B) is 1.35 to 1.45 g / cm 3 The fiber assembly according to any one of [1] to [7], [9] Density: 0.05 to 0.2 g / cm 3 The fiber assembly according to any one of [1] to [8],
[10] Weight is 50-500g / m 2 The fiber assembly according to any one of [1] to [9],
[11] The fiber assembly according to any one of [1] to
[10] , having a thickness of 0.5 to 10 mm.
[12] A fiber assembly according to any one of [1] to
[11] , which has a sound absorption coefficient of 0.5 or more at 1000 Hz when the fiber assembly has a thickness of 30 mm.
[13] A fiber assembly according to any one of [1] to
[12] , having a strength per unit mass of 30 to 80 g / g.
[14] The fiber assembly according to any one of [1] to
[13] , wherein at least one of the flame-resistant fiber (A) and the flame-resistant fiber (B) is a carbon fiber. Effect of the Invention
[0011] According to the present invention, it is possible to provide a fiber assembly having both flame resistance and sound absorbing properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below. However, this embodiment is specifically described to allow a better understanding of the gist of the invention, and does not limit the contents of the invention unless otherwise specified. Changes, omissions, additions, and other modifications of the number, position, size, etc. are possible within the scope of the gist of the present invention.
[0013] The fiber assembly of the present invention contains flame-resistant fibers (A) having a single fiber fineness of 1.0 dtex or more, and flame-resistant fibers (B) having a single fiber fineness of less than 1.0 dtex. The strength of the fiber assembly can be increased by including fibers having a single fiber fineness of 1.0 dtex or more, whereas the sound absorption properties can be increased by including fibers having a single fiber fineness of less than 1.0 dtex. From these viewpoints, the single fiber fineness of the flame-resistant fiber (A) is preferably 1.1 dtex or more, more preferably 1.2 dtex or more, and the single fiber fineness of the flame-resistant fiber (B) is preferably 0.8 dtex or less, more preferably 0.5 dtex or less, and even more preferably 0.3 dtex or less.
[0014] (Flame-resistant fiber) The flame resistant fiber used in the present invention must have a limiting oxygen index of 45 or more. The limiting oxygen index (LOI) is a value determined by the following measurement method in accordance with JIS-K-7201, and represents the minimum volume percent of oxygen required for the fiber to sustain combustion. Specifically, about 1 g of the fiber to be measured is wound around a wire with a diameter of about 0.3 mm as a support, made into a string with a diameter of about 7 mm, and placed in a combustion cylinder with the string fixed to a frame with a diameter of 150 mm. Then, a mixed gas of oxygen and nitrogen is flowed into the cylinder at 11.4 liters / mm for about 30 seconds, and the upper end of the test piece is ignited. The minimum oxygen flow rate and the nitrogen flow rate at that time required for the test piece to continue burning for 3 minutes or more or for the burning length after ignition to be 50 mm or more are measured, and the value is calculated from the following formula. LOI = [(oxygen flow rate required to keep burning) ÷ (oxygen flow rate required to keep burning + nitrogen flow rate)] × 100 If the test piece catches fire through the fluff on its surface the moment it is ignited, it is re-ignited and the above measurements are carried out.
[0015] In the fiber assembly of the present invention, the flame-resistant fiber (A) and the flame-resistant fiber (B) preferably have a limiting oxygen index of 45 or more. The limiting oxygen index is the minimum concentration of oxygen required for combustion, expressed as a percentage. A limiting oxygen index of 45 or more is sufficient as flame resistance. A limiting oxygen index of 46 or more is preferable, and a limiting oxygen index of 47 or more is more preferable.
[0016] In the fiber assembly of the present invention, the difference in single fiber fineness between the flame-resistant fiber (A) and the flame-resistant fiber (B) is preferably 0.3 dtex or more. The difference in fineness allows both sound absorption properties and strength of the assembly to be improved in a well-balanced manner. From this viewpoint, the difference in single fiber fineness is more preferably 0.5 dtex or more, and even more preferably 0.7 dtex or more.
[0017] The fiber assembly of the present invention is preferably a nonwoven fabric. Nonwoven fabric has a moderate amount of space, which makes it easy to achieve high sound absorption, and because it combines strength and flexibility, it is easy to use on curved or uneven surfaces. The method for producing the nonwoven fabric is not particularly limited, and may be columnar flow (water jet) or needle punch. Needle punching is more preferred because it makes it easier to form spaces within the nonwoven fabric. The fiber assembly thus produced can also be made into a laminate depending on the required performance.
[0018] The fiber assembly of the present invention preferably contains a mixture of the flame-resistant fiber (A) and the flame-resistant fiber (B). In the fiber assembly of the present invention, the flame-resistant fiber (A) and the flame-resistant fiber (B) may be laminated separately, but it is preferable that the flame-resistant fiber (A) and the flame-resistant fiber (B) are mixed, since this makes it easier to increase the space within the nonwoven fabric and improve the sound absorption properties.
[0019] The fiber assembly of the present invention preferably consists of only the flame-resistant fiber (A) and the flame-resistant fiber (B). Since the fiber assembly is used around things that generate heat, it is preferable not to mix in combustible fibers. However, as long as the fiber assembly has flame resistance, it is possible to mix other fibers, resins, ceramics, and metals. The flame-resistant fiber (A) and the flame-resistant fiber (B) are preferably acrylic fibers, and at least one of them may be a carbon fiber.
[0020] In the fiber assembly of the present invention, the mass ratio of the flame-resistant fiber (A) to the flame-resistant fiber (B) is preferably 20:80 to 80:20. This ratio makes it easy to achieve both good sound absorption properties and good strength of the fiber aggregate. From the viewpoint of sound absorbing properties, the mass ratio of the flame-resistant fiber (A) to the flame-resistant fiber (B) is more preferably 20:80 to 50:50, and further preferably 20:80 to 40:60.
[0021] In the fiber assembly of the present invention, the fiber density of the flame-resistant fiber (A) and the flame-resistant fiber (B) are each 1.35 to 1.45 g / cm 3 It is preferable that: The fiber density is 1.35 g / cm 3 Above this, the flame resistance is good, and the resistance is 1.37g / cm 3 More preferably, 1.39 g / cm 3 The above is even more preferable.
[0022] The fiber assembly of the present invention has a density of 0.05 to 0.2 g / cm 3 It is preferable that: The density of the fiber assembly is 0.05g / cm 3 If the density is more than 0.2g / cm, the strength of the fiber assembly is easily increased. 3 If it is below this level, it is easy to achieve high sound absorption characteristics. From these viewpoints, the density is 0.06 to 0.17 g / cm 3 More preferably, 0.07 to 0.13 g / cm 3 is more preferred.
[0023] The fiber assembly of the present invention has a basis weight of 50 to 500 g / m 2 It is preferable that: The fiber aggregate has a basis weight of 50g / m 2 If the density is more than 500g / m, the strength of the fiber assembly is easily increased. 2 If it is below this, it can be made lightweight and flexible, making it easy to handle. From these viewpoints, the basis weight is 70 to 450 g / m 2 More preferably, 100 to 300 g / m2 is more preferred.
[0024] The fiber assembly of the present invention preferably has a thickness of 0.5 to 10 mm. If the thickness of the fiber assembly is 0.5 mm or more, it can have high sound absorption properties, and if it is 10 mm or less, it can be made lightweight and flexible, making it easy to handle. From these viewpoints, the thickness is more preferably from 1 to 8 mm, and more preferably from 1.5 to 6 mm.
[0025] The fiber assembly of the present invention preferably has a sound absorption coefficient of 0.5 or more at 1000 Hz when the fiber assembly has a thickness of 30 mm. If the thickness is less than 30 mm, stack multiple pieces together and measure it to be 30 mm. If the sound absorption coefficient of a fiber assembly at 1000 Hz is 0.5 or more, it will easily absorb the sound of an automobile engine.
[0026] The fiber assembly of the present invention preferably has a strength per unit mass of 30 to 80 g / g. If the strength per unit mass of the fiber assembly is 30 g / g, it will not break and will be easy to handle, and if it is 80 g / g or less, the fiber assembly will be flexible and easy to handle.
[0027] (Method of manufacturing flame-resistant fiber) The flame-resistant fiber is produced by heating an acrylic fiber bundle in air at 200 to 300° C. while applying tension to the bundle. The density of the fiber can be adjusted by adjusting the heating temperature and heating time, and the limit oxygen index can also be adjusted.
[0028] (Method of manufacturing fiber assembly) The obtained flame-resistant fiber is cut to a length of 20 to 150 mm, and a fiber assembly can be produced by using a known needle punch method or columnar flow method.
[0029] (Flame-resistant fiber precursor acrylic fiber bundle) The flame-resistant fiber precursor acrylic fiber of the present invention is obtained by spinning an acrylonitrile polymer solution in which an acrylonitrile polymer is dissolved in a solvent. The acrylonitrile polymer used in the present invention is a polymer obtained by polymerizing acrylonitrile as a main monomer. The acrylonitrile polymer may be a homopolymer obtained only from acrylonitrile, or a copolymer in which other monomers are copolymerized in addition to acrylonitrile as the main component.
[0030] The content of acrylonitrile units in the acrylonitrile polymer can be determined taking into consideration the quality required for the resulting flame-resistant fiber bundle, and is preferably 90% by mass or more and 97.5% by mass or less, and more preferably 95% by mass or more and 97% by mass or less. If the content of acrylonitrile units is 90% by mass or more, fusion between single fibers can be prevented in the flame-resistant process for converting the flame-resistant fiber precursor acrylic fiber into a flame-resistant fiber. Furthermore, adhesion between single fibers can be avoided in treatments such as drawing with a heated roller or pressurized steam. If the content of acrylonitrile units is 97% by mass or less, the solubility in a solvent does not decrease, and precipitation and solidification of the acrylonitrile polymer can be prevented, so that the flame-resistant fiber precursor acrylic fiber can be stably produced.
[0031] The monomer units other than acrylonitrile in the acrylonitrile copolymer can be appropriately selected from vinyl monomers copolymerizable with acrylonitrile, and vinyl monomers that improve the hydrophilicity of the acrylonitrile polymer and vinyl monomers that promote the flame retardancy reaction are preferred. Examples of the monomer include (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, and hexyl (meth)acrylate; vinyl halides such as vinyl chloride, vinyl bromide, and vinylidene chloride; unsaturated carboxylic acids and salts thereof such as (meth)acrylic acid, itaconic acid, and crotonic acid; maleimide, phenylmaleimide, (meth)acrylamide, styrene, α-methylstyrene, and vinyl acetate; polymerizable unsaturated monomers containing sulfonic groups such as sodium styrenesulfonate, sodium allylsulfonate, sodium β-styrenesulfonate, and sodium methallylsulfonate; and polymerizable unsaturated monomers containing pyridine groups such as 2-vinylpyridine and 2-methyl-5-vinylpyridine. It is desirable to remove unreacted monomers, polymerization catalyst residues, and other impurities as much as possible from the acrylonitrile polymer obtained by polymerization. The acrylonitrile copolymer may be synthesized by any polymerization method, and the present invention is not limited by the difference in the polymerization method.
[0032] First, the polyacrylonitrile copolymer of the present invention described above is dissolved in a solvent to prepare a spinning solution. That is, the spinning solution used in the present invention can be composed of a polyacrylonitrile copolymer and a solvent. As the solvent, an organic solvent such as dimethylacetamide, dimethylsulfoxide, or dimethylformamide, or an aqueous solution of an inorganic compound such as zinc chloride or sodium thiocyanate can be used. However, an organic solvent is preferred in that the precursor fiber obtained does not contain metal and the process is simplified, and among them, it is preferred to use dimethylacetamide as the solvent in that the coagulated yarn and the wet heat drawn yarn have high density.
[0033] The spinning dope must have the proper viscosity and fluidity to obtain dense coagulated yarn. It is preferable that the concentration of the copolymer in the spinning solution is equal to or higher than the concentration of the copolymer in the spinning solution. The concentration of the copolymer is preferably 15% by mass or more and 30% by mass or less, and more preferably The content is preferably 18% by mass or more and 25% by mass or less.
[0034] The spinning solution is then spun to obtain a solidified yarn. Specifically, the wet spinning method, the dry wet spinning method, the dry spinning method, etc. can be mentioned. Among these, the wet spinning method and the dry-wet spinning method are preferably used from the viewpoint of spinning productivity.
[0035] (Description of the method for producing flame-resistant fiber precursor acrylic fiber bundle) The method for producing a flame-resistant fiber precursor fiber bundle of the present invention includes a first cleaning and drawing step of cleaning and drawing a fiber bundle discharged from a coagulation bath, an oil agent application step, a drying and densifying step, and a second drawing step, in that order, In the first washing and stretching step, the stretching is preferably performed by air stretching and / or hot water stretching at a stretch ratio of 4.1 times or more, and in the second stretching step, the stretching is preferably performed by dry heat stretching at a stretch ratio of 1.1 to 2.0 times.
[0036] (First washing and stretching process) In the first washing and stretching step, the film is preferably stretched at a stretch ratio of 4.1 times or more by air stretching and / or hot water stretching. The upper limit of the draw ratio is preferably 6.0 times or less from the viewpoint of preventing single fiber breakage. If the draw ratio is 4.1 times or more, the drawability in the second drawing step can be improved, and stable production can be facilitated. From this viewpoint, the stretching ratio is more preferably 4.2 to 5.8 times, and further preferably 4.5 to 5.5 times. The hot water drawing may be performed simultaneously with washing in a bath for washing the solvent contained in the coagulated yarn with boiling water, or may be performed separately. The hot water temperature for hot water drawing is preferably 80 to 100°C. If it is 80°C or higher, drawing can be easily performed. 100°C means a boiling water state. From this viewpoint, the hot water temperature is more preferably 85 to 99°C, and further preferably 90 to 98°C. The distance between the rollers for hot water stretching is preferably 1000 to 10000 mm. If it is 1000 mm or more, stretching becomes easy. It is preferable that the hot water is applied so as to penetrate the fiber bundle. By passing the hot water through the fiber bundle, the hot water can reach the inside of the fiber bundle, thereby reducing unevenness in stretching.
[0037] (Oil application process) After the first washing and stretching step, an oil is applied. The oil is not particularly limited and can be appropriately selected in consideration of the ease of passing through the subsequent steps.
[0038] (drying densification process) In the step of drying and densifying the fiber bundle after the first drawing step, a heated roll, a hot plate, hot air, infrared rays, microwaves, etc., can be used. The heated roll may be one or more. The temperature for drying and densifying must be higher than the glass transition temperature of the fiber, which is 60 to 90°C, but may vary depending on the state from the water-containing state to the dry state, and a heated roll temperature of about 100 to 200°C is preferred.
[0039] (Second stretching process) The second drawing step is a step of hot drawing the fiber bundle after the drying and densifying step. In the hot drawing, a hot roll, a hot plate, hot air, infrared rays, microwaves, etc. can be used. The draw ratio in the hot drawing is preferably 1.1 to 2.0 times, more preferably 1.3 to 1.5 times. If the draw ratio in the hot drawing is 1.1 times or more, the fiber orientation can be increased, and if it is 1.5 times or less, the generation of fluff can be easily reduced.
[0040] In the method for producing a flame-resistant fiber precursor acrylic fiber bundle of the present invention, the product of the first draw ratio and the second draw ratio is preferably 7.0 to 9.0. When the product of the first draw ratio and the second draw ratio is 6.0 to 9.0, the fiber orientation can be sufficiently increased while suppressing fluffing of the flame-resistant fiber precursor acrylic fiber bundle. From this viewpoint, the product of the first stretching ratio and the second stretching ratio is more preferably from 6.5 to 8.5, and further preferably from 7.0 to 8.0.
[0041] (Total fineness of fiber bundles after drying and densification process) In the method for producing a flame-resistant fiber precursor acrylic fiber bundle of the present invention, the total fineness of the fiber bundle after the drying and densifying step is preferably 8,000 to 120,000 dtex. If it is 10,000 to 60,000 dtex, it can be produced efficiently. More preferably, it is 12,000 to 30,000 tex. Even more preferably, it is 15,000 to 24,000 dtex.
[0042] In the method for producing a flame-resistant fiber precursor acrylic fiber bundle of the present invention, the fiber bundle temperature during dry heat drawing is preferably set to 100 to 200°C in the second drawing step. If the fiber bundle temperature is 100° C. or higher, it is effective for stretchability because it is a temperature above the glass transition point, and if it is 200° C. or lower, the effect on stretchability can be made highly reproducible. From these viewpoints, the fiber bundle temperature is more preferably 120 to 190°C, and further preferably 150 to 180°C.
[0043] The method for producing the flame-resistant fiber precursor acrylic fiber bundle of the present invention is preferably a wet spinning method. The wet spinning method allows for high productivity. EXAMPLES
[0044] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. The measurements in the examples were carried out by the following methods.
[0045] (Method of measuring limiting oxygen index (LOI)) Measurements were performed in accordance with JIS-K-7201.
[0046] (Method of measuring basis weight) Measurement was performed according to JIS-L-1096.
[0047] (Thickness measurement method) Measurement was performed according to JIS-L-1096.
[0048] (Method of measuring density) It was calculated by dividing the basis weight by the thickness.
[0049] (Method of measuring the strength of fiber assembly) Measurement was performed according to JIS-L-1096. The strength in the warp and weft directions was averaged to calculate the value.
[0050] (Method of measuring strength per unit weight) The strength was calculated by dividing the average value of the warp and weft directions by the weight of a 5 cm x 10 cm square sample.
[0051] (Method of evaluating strength characteristics) The strength properties of the flame-resistant fiber nonwoven fabric were evaluated as follows: less than 30 strength per unit weight (g / g) is marked "x", 30 or more but less than 45 is marked "◯", and 45 or more is marked "◎".
[0052] (Method of measuring normal incidence sound absorption coefficient) The required number of flame-resistant nonwoven fabrics were stacked to obtain a measurement sample with a thickness of approximately 30 mm. In accordance with JIS-A-1405-2, the normal incidence sound absorption coefficient was measured at a frequency of 1000 Hz using a thin tube with an inner diameter of 29 mm in contact with a rigid wall.
[0053] (10) Sound absorption properties The sound absorption properties of the flame-resistant fibrous nonwoven fabric were evaluated by assigning the following criteria to the normal incidence sound absorption coefficient: less than 0.5 is marked "x", 0.5 or more and less than 0.6 is marked "◯", and 0.6 or more is marked "◎".
[0054] (Preparation of flame-resistant fiber (A)) An acrylic fiber bundle having a single fiber fineness of 1.3 dtex and a total fiber fineness of 65,000 dtex was heated under tension in air at 200 to 300°C for 70 minutes to obtain a flame-resistant fiber (A) having a thick fiber fineness. The density of the flame-resistant fiber was 1.405 g / cm. 3 The limiting oxygen index (LOI value) was 49. The fiber bundle of the flame-resistant fiber (A) was cut to a length of 70 mm.
[0055] (Preparation of flame-resistant fiber (B)) An acrylic fiber bundle having a single fiber fineness of 0.13 dtex and a total fineness of 65,000 dtex was heated under tension in air at 200 to 300°C for 70 minutes to obtain a fine flame-resistant fiber (B). The density of the flame-resistant fiber (B) was 1.401 g / cm 3 The limiting oxygen index (LOI value) was 47. The fiber bundle of the flame-resistant fiber (B) was cut to a length of 70 mm.
[0056] Example 1 The thick flame-resistant fiber (A) and the fine flame-resistant fiber (B) prepared above were mixed in a weight ratio of 75 / 25 and passed through a card to prepare a web. There was no particular problem with the carding properties. The resulting web was folded over using a cross layer, and then two folded webs were stacked together and spun at 300 points / cm using a 3-barb, No. 40 needle. 2 The fibers were entangled by needle punching to obtain a flame-resistant fiber nonwoven fabric. The physical properties of the obtained nonwoven fabric are shown in Table 1. The normal incident sound absorption coefficient was measured by stacking 16 sheets of the obtained nonwoven fabric to prepare a measurement sample.
[0057] Example 2 A flame-resistant fibrous nonwoven fabric was obtained in the same manner as in Example 1, except that the mixing ratio of the flame-resistant fiber (A) and the flame-resistant fiber (B) was changed to 50 / 50. The physical properties of the obtained nonwoven fabric are shown in Table 1. The normal incident sound absorption coefficient was measured by stacking 16 sheets of the obtained nonwoven fabric to prepare a measurement sample.
[0058] Example 3 A flame-resistant fibrous nonwoven fabric was obtained in the same manner as in Example 1, except that the mixing ratio of the flame-resistant fiber (A) and the flame-resistant fiber (B) was changed to 25 / 75. The physical properties of the obtained nonwoven fabric are shown in Table 1. The normal incident sound absorption coefficient was measured by stacking 16 sheets of the obtained nonwoven fabric to prepare a measurement sample.
[0059] Example 4 A flame-resistant fiber nonwoven fabric was obtained in the same manner as in Example 1, except that the mixing ratio of the flame-resistant fiber (A) and the flame-resistant fiber (B) was changed to 50 / 50 and the number of overlapping folded webs was changed to three. The physical properties of the obtained nonwoven fabric are shown in Table 1. The normal incident sound absorption coefficient was measured by stacking nine sheets of the obtained nonwoven fabric as a measurement sample.
[0060] Example 5 A flame-resistant fiber nonwoven fabric was obtained in the same manner as in Example 1, except that the mixing ratio of the flame-resistant fiber (A) and the flame-resistant fiber (B) was changed to 50 / 50 and the number of overlapping folded webs was changed to 5. The physical properties of the obtained nonwoven fabric are shown in Table 1. The normal incident sound absorption coefficient was measured by stacking six of the obtained nonwoven fabrics as a measurement sample.
[0061] Example 6 The flame-resistant fiber (A) and the flame-resistant fiber (B) were mixed in a weight ratio of 70 / 30 and passed through a card to prepare a web. There was no particular problem with the carding properties. The obtained web was folded using a cross layer and then subjected to a pressure of 50 kg / cm 2 The fibers were entangled by a columnar water jet treatment using a group of nozzles with a diameter of 0.15 mm and a pitch of 0.4 mm, using high-pressure water of 1000 gage pressure. The fibers were then dried to obtain a flame-resistant fiber nonwoven fabric. The physical properties of the obtained nonwoven fabric are shown in Table 1. The normal incident sound absorption coefficient was measured by stacking 37 pieces of the obtained nonwoven fabric as a measurement sample.
[0062] Example 7 A flame-resistant fibrous nonwoven fabric was obtained in the same manner as in Example 6, except that the mixing ratio of the flame-resistant fiber (A) and the flame-resistant fiber (B) was changed to 30 / 70. The physical properties of the obtained nonwoven fabric are shown in Table 1. The normal incident sound absorption coefficient was measured by stacking 37 pieces of the obtained nonwoven fabric as a measurement sample.
[0063] Comparative Example 1 A flame-resistant fibrous nonwoven fabric was obtained in the same manner as in Example 1, except that only the thick flame-resistant fiber (A) was used. The physical properties of the obtained nonwoven fabric are shown in Table 1. The normal incident sound absorption coefficient was measured by stacking 16 sheets of the obtained nonwoven fabric to prepare a measurement sample. The lack of fine flame-resistant fiber (B) resulted in poor sound absorption properties.
[0064] Comparative Example 2 A flame-resistant fibrous nonwoven fabric was obtained in the same manner as in Example 1, except that only the fine flame-resistant fiber (B) was used. The physical properties of the obtained nonwoven fabric are shown in Table 1. The normal incident sound absorption coefficient was measured by stacking 16 sheets of the obtained nonwoven fabric to prepare a measurement sample. Since it was made only of fine flame-resistant fiber (B), the sound absorption characteristics were good, but the strength was poor.
[0065] Example 8 The flame-resistant fiber nonwoven fabric obtained in Example 2 was heat-treated at 1400° C. in a nitrogen atmosphere to obtain a carbon fiber nonwoven fabric. The physical properties of the obtained nonwoven fabric are: basis weight: 94 (g / m 2 ), Thickness: 0.15 (cm), Density: 0.06 (g / cm 3 ), strong warp / weft average: 50.8 (g / 5cm), 5 x 10 cm weight: 0.48 (g), strength per unit weight: 106 (g / g), normal incidence sound absorption coefficient: 0.72 (-), and both strength and sound absorption properties were good. The normal incidence sound absorption coefficient was measured by stacking 20 sheets of the obtained nonwoven fabric to prepare a measurement sample.
[0066] [Table 1]
Claims
1. A fiber assembly comprising a flame-resistant fiber (A) having a single fiber fineness of 1.0 dtex or more and a flame-resistant fiber (B) having a single fiber fineness of less than 1.0 dtex.
2. 2. The fiber assembly according to claim 1, wherein the flame-resistant fiber (A) and the flame-resistant fiber (B) have a limiting oxygen index of 45 or more.
3. 2. The fiber assembly according to claim 1, wherein the difference in single fiber fineness between the flame-resistant fiber (A) and the flame-resistant fiber (B) is 0.3 dtex or more.
4. 2. The fiber assembly according to claim 1, which is a nonwoven fabric.
5. 2. The fiber assembly according to claim 1, wherein the flame-resistant fiber (A) and the flame-resistant fiber (B) are mixed.
6. 2. The fiber assembly according to claim 1, which consists of only the flame-resistant fiber (A) and the flame-resistant fiber (B).
7. The fiber assembly according to claim 1, wherein the mass ratio of the flame-resistant fiber (A) to the flame-resistant fiber (B) is 20:80 to 80:
20.
8. The fiber density of the flame-resistant fiber (A) and the flame-resistant fiber (B) is 1.35 to 1.45 g / cm 3 The fiber assembly according to claim 1,
9. Density: 0.05 to 0.2 g / cm 3 The fiber assembly according to claim 1,
10. Weight per unit area: 50 to 500 g / m 2 The fiber assembly according to claim 1,
11. 2. The fiber assembly according to claim 1, which has a thickness of 0.5 to 10 mm.
12. 2. The fiber assembly according to claim 1, which has a sound absorption coefficient of 0.5 or more at 1000 Hz when the fiber assembly has a thickness of 30 mm.
13. 2. The fiber assembly according to claim 1, which has a strength per unit mass of 30 to 80 g / g.
14. 2. The fiber assembly according to claim 1, wherein at least one of the flame-resistant fiber (A) and the flame-resistant fiber (B) is a carbon fiber.
Citation Information
Patent Citations
Wholly aromatic polyamide structural material
JP1994212593A
Flame-resistant staple fiber nonwoven fabric and method for producing the same
JP2003129362A
Heat-resistant acoustic material
JP2006138935A
Fire-retardant sound absorbing heat insulating material
JP2006195104A
Heat-resistant sound-absorbing and heat insulating material
JP2006321053A