Frosted glass-like resin composition

A thermoplastic resin composition with bead-shaped crosslinked particles addresses the challenge of achieving a frosted glass appearance in plastic molded products by maintaining transparency and luxury feel, resulting in cost-effective, transparent, and designable articles.

JP2024137616APending Publication Date: 2024-10-07SUMIKA COLOR CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023150316
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2023-09-15
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Conventional methods for achieving a frosted glass appearance in plastic molded products require additional surface treatments, which reduce versatility and are not effective in maintaining transparency and luxury feel, especially in injection molding.

Method used

A thermoplastic resin composition comprising thermoplastic resin and bead-shaped crosslinked particles with a specific refractive index difference, used in various molding methods to impart a matte feel and frosted glass look while maintaining transparency.

Benefits of technology

The solution produces molded articles that are inexpensive, highly transparent, and have a matte feel with a ground glass appearance, enhancing designability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137616000001
    Figure 2024137616000001
  • Figure 2024137616000002
    Figure 2024137616000002
  • Figure 2024137616000003
    Figure 2024137616000003
Patent Text Reader

Abstract

To enable the production of a cost-efficient molded product with high design aesthetics that features high clarity, a matte feel and a frosted glass-like appearance.SOLUTION: A thermoplastic resin composition comprises a thermoplastic resin (A) and crosslinked particles (B) with an average particle size of 50 μm or less. The difference in refractive index between the thermoplastic resin (A) and the crosslinked particles (B) is 0.005 or more and 0.08 or less. A master batch for thermoplastic resin comprises the thermoplastic resin (A) and bead-like crosslinked particles (B).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ground-glass-like composition that gives a ground-glass-like molded article having an excellent appearance. [Background technology]

[0002] Plastic containers and other molded products are widely used as a substitute for glass in terms of light weight, price, colorability, and productivity. Among them, thermoplastic resins such as acrylic resin, polyester resin, polystyrene resin, and polycarbonate resin have the characteristics of high transparency, excellent surface gloss, and excellent moldability such as injection molding, extrusion molding, and blow molding. Therefore, they are used in many fields such as cosmetics, food, medicine, health care, lighting, and signs, and the amount of use is expanding. However, their applications are generally made by utilizing their transparency, which is one of their characteristics, that is, as uncolored transparent or colored transparent molded products in which the internal filling can be seen as it is.

[0003] Although transparent plastic molded products have a beautiful appearance, they are not suitable for protecting the contents of the molded products from chemical changes because they easily transmit sunlight, which not only heats the contents but also exposes them to ultraviolet rays. In addition, transparent molded products tend to reduce the luxurious feel of the product because the contents are clearly visible.

[0004] In addition, plastic molded products are sometimes colored by blending dyes or pigments, but this does not take into consideration the texture, such as the matte feel and feel, and it is difficult to achieve a luxurious feel like frosted glass. Conventional plastic molded products are also undesirable in terms of color sense and design.

[0005] Therefore, as a method for obtaining a ground glass appearance in a plastic molded product, a method of performing surface treatment on a plastic container or a molding die is generally used. For example, Patent Document 1 discloses that a texture like a frosted glass bottle can be obtained during stretch blow molding by roughening the mold surface with sandblasting, shot blasting, etc. In addition, Patent Document 2 discloses a method of coating and baking glass powder as a method for obtaining a frosted glass product. On the other hand, Patent Document 3 discloses a technology for eliminating the gloss of plastic and imparting a matte feel by using spherical beads with high heat resistance and a high refractive index. Patent Document 4 discloses that a polyester resin composition obtained by blending a spherical fine powder of polymethyl methacrylate and a fine powder of calcium carbonate with a polyester resin causes light diffusion in the molded product, resulting in a molded product with a ground glass feel. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2000-301596 A [Patent Document 2] Japanese Patent Publication No. 60-226431 [Patent Document 3] Japanese Patent Application Publication No. 01-297465 [Patent Document 4] Japanese Patent Application Publication No. 11-001606 Summary of the Invention [Problem to be solved by the invention]

[0007] However, surface treatment of the mold or giving a ground glass appearance by labeling increases the number of steps and requires the design of a mold and layer structure suitable for the molded product, making it less versatile. In addition, molded products using conventional spherical beads or fillers were not sufficient to eliminate surface gloss and give a matte or ground glass look while maintaining the transparency of acrylic resin, polyester resin, polystyrene resin, polycarbonate resin, etc. In particular, in injection molding, the surface of the molded product is smooth, so there was no method that could give a ground glass look to the product.

[0008] The present invention has been made in consideration of the above circumstances, and has an object to provide a thermoplastic resin composition that can impart a matte finish and a ground-glass texture, regardless of the molding method, while maintaining the transparency of plastic. [Means for solving the problem]

[0009] The present inventors have conducted extensive research and have completed the present invention.

[0010] That is, the present invention relates to the following. [1] Thermoplastic resin (A) 100 parts by weight, and 0.1 to 10 parts by weight of bead-like crosslinked particles (B) having an average particle size of 50 μm or less A thermoplastic resin composition comprising: A thermoplastic resin composition, wherein the difference in refractive index between the thermoplastic resin (A) and the crosslinked particles (B) is 0.005 or more and 0.08 or less. [2] The thermoplastic resin (A) is at least one resin selected from the group consisting of a polyethylene terephthalate resin, a polystyrene resin, and a polymethyl methacrylate resin; The thermoplastic resin composition according to [1], wherein the bead-like crosslinked particles (B) are at least one resin selected from the group consisting of crosslinked polystyrene resins, methyl methacrylate-styrene copolymer crosslinked particles, crosslinked polymethyl methacrylate resins, and silicone resins. [3] The thermoplastic resin composition according to [1] or [2], wherein the thermoplastic resin (A) is a copolymerized polyethylene terephthalate resin. [4] The thermoplastic resin composition according to any one of [1] to [3], wherein the refractive index difference is 0.008 or more and 0.03 or less. [5] The thermoplastic resin composition according to any one of [1] to [4], wherein the amount of the bead-like crosslinked particles is 1.25 parts by weight or more per 100 parts by weight of the thermoplastic resin (A). [6] The thermoplastic resin composition according to any one of [1] to [5], further comprising a lubricant which is an aliphatic compound. [7] A thermoplastic resin molded article formed from the thermoplastic resin composition according to any one of [1] to [6], the thermoplastic resin molded article having a thickness of 3 mm, a total light transmittance of 60% or more, and a haze of 40 to 85. [8] Thermoplastic resin (A) 100 parts by weight, and Bead-like crosslinked particles (B) having an average particle size of 50 μm or less: 5 to 100 parts by weight A masterbatch for thermoplastic resins, comprising: The masterbatch for thermoplastic resins, wherein the difference in refractive index between the thermoplastic resin (A) and the crosslinked particles (B) is 0.005 or more and 0.08 or less. [9] The masterbatch for thermoplastic resins according to [8], wherein the thermoplastic resin (A) is a copolymerized polyethylene terephthalate resin, or the masterbatch further contains a lubricant which is an aliphatic compound.

[10] A method for producing a thermoplastic resin molded product, comprising the steps of melting and molding the resin composition according to any one of [1] to [6]. Effect of the Invention

[0011] According to the present invention, it is possible to produce a molded article which is inexpensive, has high transparency, and has a matte feel and a ground-glass texture, and is highly aesthetically pleasing (designability due to the ground-glass texture). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] [Thermoplastic resin (hereinafter sometimes referred to as "resin")] Examples of the resin include acrylonitrile-butadiene-styrene resin, low-density polyethylene resin, high-density polyethylene resin, polystyrene resin, polypropylene resin, acrylonitrile-styrene resin, cellulose acetate resin, ethylene-vinyl acetate resin, acrylic-acrylonitrile-styrene resin, acrylic-chlorinated polyethylene resin, ethylene-vinyl alcohol resin, fluororesin, polymethyl methacrylate resin, polyacetal resin, polyamide resin, polyethylene terephthalate resin, polycarbonate resin, polysulfone resin, polyethersulfone resin, methylpentene resin, polyarylate resin, polybutylene terephthalate resin, resin containing an alicyclic structure-containing ethylenically unsaturated monomer unit (e.g., cycloolefin polymer resin), polyphenylene sulfide resin, polyphenylene oxide resin, and polyether ether ketone resin.

[0013] The polyethylene terephthalate resin is preferably a copolymerized polyethylene terephthalate resin since it increases the strength of the molded product. Examples of the copolymerized polyethylene terephthalate resin include isophthalic acid copolymerized polyethylene terephthalate, adipic acid copolymerized polyethylene terephthalate, urethane-modified copolymerized polyethylene terephthalate, 1,4-cyclohexanedimethanol copolymerized polyethylene terephthalate, and neopentyl glycol copolymerized polyethylene terephthalate.

[0014] The melting point of the polyethylene terephthalate resin varies depending on the composition of the polyethylene terephthalate resin (particularly, depending on the type and amount of the monomer (comonomer) copolymerized with ethylene terephthalate in the copolymerized polyethylene terephthalate). The melting point of the polyethylene terephthalate resin may be 150 to 350°C, 180 to 320°C, 200 to 300°C, 210 to 290°C, 220 to 280°C, 230 to 270°C, or 240 to 260°C.

[0015] The resin is preferably a resin having excellent transparency and excellent moldability at a predetermined processing temperature, and is preferably at least one resin selected from the group consisting of polyethylene terephthalate resin, polystyrene resin, and polymethyl methacrylate resin. The resin is preferably not a polycarbonate resin. By using a thermoplastic resin with excellent transparency, the ground glass effect tends to become clearer. Two or more of these resins may be used in combination as long as the transparency and mechanical properties are not impaired.

[0016] The resin before molding (raw resin) is generally in the form of particles (pellets, granules or powder). The average particle size of the particles may be, for example, 1 μm to 10 mm or 5 μm to 5 mm. The resin is preferably in the form of particles (powder) with an average particle size of 10 μm to 2 mm or 20 μm to 1 mm. The average particle size of the particles can be measured by the same method as for the bead-like crosslinked particles.

[0017] The thickness of the molded article (i.e., the thickness of the resin) may be 0.1 mm to 30 mm or 0.3 mm to 10 mm. The thickness of the molded article may be 0.2 mm or more, 0.4 mm or more, 0.6 mm or more, 0.8 mm or more, 1 mm or more, 1.2 mm or more, 1.4 mm or more, 1.6 mm or more, 1.8 mm or more, 2 mm or more, 2.2 mm or more, 2.4 mm or more, 2.6 mm or more, 2.8 mm or more, or 3 mm or more. The thickness of the molded article may be 25 mm or less, 20 mm or less, 15 mm or less, 12 mm or less, 10 mm or less, 9 mm or less, 8 mm or less, 7 mm or less, 6 mm or less, 5 mm or less, 4 mm or less, or 3.5 mm or less.

[0018] The resin preferably has a total light transmittance of 55% or more, 60% or more, 65% or more, 70% or more, 75% or more, 80% or more, 85% or more, or 90% or more when the thickness is 2 mm to 5 mm (for example, 2 mm, 3 mm, 4 mm or 5 mm, particularly 3.0 mm). The total light transmittance may be 56% or more, 58% or more, 60% or more, 62% or more, 64% or more, 66% or more, 68% or more, 70% or more, 72% or more, 74% or more, 76% or more, 78% or more, 80% or more, 82% or more, 84% or more, 86% or more, 88% or more, 90% or more, 92% or more, or 94% or more. The total light transmittance may be 100% or less, 98% or less, 96% or less, 94% or less, 92% or less, 90% or less, or 88% or less.

[0019] The total light transmittance can be measured in accordance with JIS K 7136: 2000. For example, a haze meter (model TC-H3DPK) manufactured by Tokyo Denshoku Co., Ltd. can be used for the measurement. [Formula] Total light transmittance (Tt) = Linear transmittance (Tp) + Diffuse transmittance (Td)

[0020] [Bead-like cross-linked particles] The bead-like crosslinked particles (crosslinked polymer particles) are spherical and have an average sphericity of preferably 0.8 or more, more preferably 0.85 or more, and even more preferably 0.9 or more. Sphericity is measured by taking a photograph with a microscope, and using the observed particle area and perimeter, (sphericity) = {4π × (area) ÷ (perimeter)} 2 The closer to 1 the particle is, the closer it is to a perfect sphere. The average sphericity is preferably calculated by averaging the sphericities of 100 arbitrarily selected aggregates.

[0021] The bead-like crosslinked particles are not particularly limited, but examples thereof include crosslinked polystyrene resin, methyl methacrylate-styrene copolymer crosslinked particles, crosslinked polymethyl methacrylate resin, silicone resin, and the like, which are easy to adjust the refractive index.

[0022] The smaller the difference in refractive index between the thermoplastic resin and the particles, the more transparency can be maintained, and the easier it is to impart a ground glass look, and the difference in refractive index between the thermoplastic resin and the particles is preferably 0.005 to 0.08, more preferably 0.008 to 0.03. The difference in refractive index may be 0.006 or more, 0.007 or more, 0.008 or more, 0.009 or more, 0.01 or more, 0.011 or more, 0.012 or more, 0.013 or more, 0.014 or more, 0.015 or more, 0.02 or more, 0.025 or more, 0.03 or more, 0.035 or more, 0.04 or more, 0.045 or more, or 0.05 or more. It may be 0.07 or less, 0.065 or less, 0.06 or less, 0.055 or less, 0.05 or less, 0.045 or less, 0.04 or less, 0.035 or less, 0.03 or less, 0.025 or less, 0.02 or less, 0.019 or less, 0.018 or less, 0.017 or less, 0.016 or less, 0.015 or less, 0.014 or less, 0.013 or less, or 0.012 or less.

[0023] The average particle size of the bead-like crosslinked particles is preferably 50 μm or less. When the average particle size is 50 μm or less, light scattering is sufficient, haze is high, and a good ground glass look is obtained. The average particle size of the crosslinked particles is preferably 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, 25 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. The average particle size of the crosslinked particles may be 1 μm or more, 3 μm or more, 5 μm or more, or 10 μm or more.

[0024] The average particle size can be measured using an optical microscope (200 to 500x). The median size (D50) obtained by creating a particle size distribution from the particle sizes of any number of crosslinked particles (for example, 100 or 200) can be used as the average particle size.

[0025] The HAZE of a thermoplastic resin molded article having a thickness of 3 mm may be 40-85, 45-80, or 50-75. Haze can be measured in accordance with JIS K 7136, for example, by a haze meter (model TC-H3DPK) manufactured by Tokyo Denshoku Co., Ltd. [Formula] HAZE=(Diffuse transmittance (Td) / Total light transmittance (Td))*100

[0026] In the thermoplastic resin composition, the amount of the bead-like crosslinked particles is preferably 0.1 to 10 parts by weight or 0.3 to 5 parts by weight relative to 100 parts by weight of the thermoplastic resin (A). When the amount is within the above range, the haze is high and a good ground glass texture is obtained. More preferably, it is 0.2 to 8 parts by weight or 0.3 to 3 parts by weight, for example, 1 to 2.5 parts by weight. Alternatively, the amount of the bead-like crosslinked particles relative to 100 parts by weight of the thermoplastic resin (A) is 0.1 parts by weight or more, 0.2 parts by weight or more, 0.3 parts by weight or more, 0.4 parts by weight or more, 0.5 parts by weight or more, 0.6 parts by weight or more, 0.7 parts by weight or more, 0.8 parts by weight or more, 0.9 parts by weight or more, 1 part by weight or more, 1.1 parts by weight or more, 1.2 parts by weight or more, 1.3 parts by weight or more, 1.4 parts by weight or more, 1.5 parts by weight or more, 1.6 parts by weight or more, 1.7 parts by weight or more, 1.8 parts by weight or more. The amount of the bead-like crosslinked particles may be 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, 6 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1.5 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, or 0.2 parts by weight or less. Since the ground glass property is good, the amount of the bead-like crosslinked particles is preferably 1.21 parts by weight or more, 1.22 parts by weight or more, 1.23 parts by weight or more, 1.24 parts by weight or more, or 1.25 parts by weight or more per 100 parts by weight of the thermoplastic resin (A).

[0027] In the master batch, the amount of the bead-like crosslinked particles is preferably 1 to 100 parts by weight or 5 to 20 parts by weight relative to 100 parts by weight of the thermoplastic resin (A). When the amount is within the above range, a high haze and a good ground glass texture can be obtained. The amount of the bead-like crosslinked particles relative to 100 parts by weight of the thermoplastic resin (A) may be 1 part by weight or more, 2 parts by weight or more, 3 parts by weight or more, 4 parts by weight or more, 5 parts by weight or more, 6 parts by weight or more, 7 parts by weight or more, 8 parts by weight or more, 9 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 25 parts by weight or more, 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, or 60 parts by weight or more. The amount can be 100 parts by weight or less, 90 parts by weight or less, 80 parts by weight or less, 70 parts by weight or less, 60 parts by weight or less, 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 25 parts by weight or less, 20 parts by weight or less, 19 parts by weight or less, 18 parts by weight or less, 17 parts by weight or less, 16 parts by weight or less, 15 parts by weight or less, 14 parts by weight or less, 13 parts by weight or less, 12 parts by weight or less, 11 parts by weight or less, 10 parts by weight or less, or 5 parts by weight or less.

[0028] The refractive index of thermoplastic resin was measured using a multi-wavelength Abbe refractometer (ATAGO DR-M4 model). First, a small amount of contact liquid (1-bromonaphthalene) was dropped onto the surface of a test piece made by injection molding, and the edge of the test piece was brought into contact with the surface of the prism with the light source facing the light source. After that, the field was adjusted until all colors disappeared, and the boundary between the bright field and the dark field was aligned with the intersection of the crosshairs of the eyepiece to measure the refractive index. A halogen lamp with a wavelength of 589 nm was used as the light source.

[0029] The refractive index of the bead-like crosslinked particles was measured by the Becke method. First, the polymer particles were placed on a slide glass, and a refractive index liquid (CARGILLE's standard refractive index liquid, refractive index nD25 of 1.480 to 1.596, prepared in multiple increments of 0.002) was dropped. Then, after thoroughly mixing the polymer particles and the refractive index liquid, the outline of the polymer particles was observed from above using an optical microscope while irradiating the light from a high-pressure sodium lamp "NX35" (center wavelength 589 nm) manufactured by Iwasaki Electric Co., Ltd. from below. When the outline was not visible, it was determined that the refractive index of the refractive index liquid and the polymer particles were equal.

[0030] In addition, there is no problem with the observation by the optical microscope as long as the magnification allows the outline of the polymer particles to be confirmed, but for polymer particles with a particle diameter of 5 μm, an observation magnification of about 500 times is appropriate. By the above operation, the closer the refractive index of the polymer particles and the refractive index of the refractive liquid are, the more difficult it is to see the outline of the polymer particles, so the refractive index of the refractive liquid in which the outline of the polymer particles is difficult to see is determined to be equal to the refractive index of the polymer particles.

[0031] In addition, when there is no difference in the appearance of the polymer particles between two types of refractive index liquids with a refractive index difference of 0.002, the intermediate value of these two types of refractive index liquids was determined to be the refractive index of the polymer particles. For example, when tests were performed using refractive index liquids with refractive indices of 1.554 and 1.556, if there is no difference in the appearance of the polymer particles between the two refractive index liquids, the intermediate value of these refractive index liquids, 1.555, was determined to be the refractive index of the polymer particles.

[0032] The resin and the bead-like crosslinked particles may be mixed as necessary before being melted. Alternatively, the bead-like crosslinked particles and a part of the resin may be melt-kneaded in advance to prepare a master powder or master batch having a high concentration of the bead-like crosslinked particles, and then the resin and the master powder or master batch may be melt-kneaded. Examples of the method for mixing the resin and the pigment include dry blending.

[0033] [Other agents] In addition to the resin and bead-like crosslinked particles, other agents may be added (or melted). Examples of other agents include dyes, pigments, plasticizers, antioxidants, UV absorbers, light stabilizers, flame retardants, antibacterial agents, antistatic agents, copper damage inhibitors, metal deactivators, tackifiers, antiblocking agents, lubricants, slip agents, internal release agents, anti-fogging agents (anti-drip agents, anti-fog agents), fragrances, surfactants, wetting agents, preservatives, anti-fungal agents, fillers, reinforcing agents, stabilizers, heat retaining agents, foaming agents, vibration-proofing agents, impact resistance improving agents, surface treatment agents, heat retaining agents, surface treatment agents, dispersants, water-repellent materials, etc. The amount of the other agents may be 0 to 30% by weight, 0.1 to 20% by weight, or 1 to 10% by weight relative to the resin composition.

[0034] The use of a lubricant allows the resin and the bead-like crosslinked particles to be mixed well. Examples of lubricants include amide-based lubricants such as lauric amide, palmitic amide, stearic amide, oleic amide, erucic amide, behenic amide, methylene bisstearic amide, ethylene bisstearic amide, m-xylene bisstearic amide, and methylol stearic amide; hydrocarbon-based lubricants such as paraffin wax, microcrystalline wax, and polyethylene wax; aliphatic-based lubricants such as stearic acid and behenic acid; ester-based lubricants such as stearic acid monoglyceride and pentaerythritol tetrastearate; higher alcohol-based lubricants such as stearyl alcohol; and metal soap-based lubricants such as calcium stearate, zinc stearate, and magnesium stearate.

[0035] The lubricant is preferably an aliphatic compound. The lubricant is preferably an aliphatic compound having at least one functional group selected from a carboxy group, a hydroxyl group, an amide group, and an ester bond, particularly an aliphatic alcohol, a fatty acid, a fatty acid ester, a fatty acid amide, or a fatty acid metal salt. The carbon number of the aliphatic compound (particularly, one aliphatic group) is preferably 10 or more, 12 or more, or 14 or more, and 40 or less, 32 or less, or 28 or less.

[0036] The aliphatic compounds include: fatty alcohols such as stearyl alcohol, cetyl alcohol, etc.; Fatty acids such as lauric acid, stearic acid, oleic acid, and behenic acid; Metal salts of fatty acids, such as calcium stearate, magnesium stearate, zinc stearate, calcium hydroxystearate, etc., and complexes of these metal salts; Aliphatic monoamides such as oleamide, erucamide, and ricinoleamide; Aliphatic alkylene bisamides such as ethylene bisstearic acid amide, ethylene bislauric acid amide, and ethylene bis12-hydroxystearic acid amide; Polyhydric alcohol fatty acid esters such as pentaerythritol sesquistearate and pentaerythritol tetrapalmitate; Examples include hydroxy fatty acid esters such as 12-hydroxystearic acid triglyceride.

[0037] The amount of the lubricant may be 0 to 10 wt%, 0.05 to 5 wt%, 0.1 to 2 wt%, or 0.2 to 1 wt% based on the resin composition, and 0 to 30 wt%, 0.1 to 20 wt%, 0.5 to 10 wt%, or 1 to 5 wt% based on the masterbatch.

[0038] <Step of melt-kneading resin and bead-like crosslinked particles> The resin and the bead-like crosslinked particles are usually melted using a kneader. Examples of the kneader for melt-kneading the resin and the bead-like crosslinked particles include various extruders such as a single screw extruder, a twin screw extruder, and a multi-screw extruder, as well as a batch type kneader such as a Banbury mixer, an intensive mixer, and a pressure kneader, a simple type kneader such as a Brabender mixer, a continuous intensive mixer, and an apparatus having a single screw extruder below these kneaders and performing kneading and extrusion simultaneously. The melting temperature (high temperature) is equal to or higher than the melting point of the resin, and may generally be 200 to 350°C, or 230 to 320°C, although it depends on the melting point of the resin.

[0039] <Step of Molding a Resin Composition Obtained by Melting and Kneading a Resin and Bead-Like Crosslinked Particles> The molding can be carried out by injection molding, extrusion molding, blow molding, etc. The molding is preferably injection molding or direct blow molding.

[0040] <Manufacturing method of injection molded products> The present invention also relates to a method for producing an injection-molded article, which comprises a step of injection-molding a resin composition obtained by melting a resin, bead-like crosslinked particles, and, if necessary, other agents at a high temperature. For the injection molding, a normal injection molding machine is used. The melt-kneaded resin and the bead-like crosslinked particles are fed into the injection molding machine. As the injection molding machine, a known one can be used, and examples thereof include a hydraulic injection molding machine, an electric injection molding machine, etc. The injection molding machine can be appropriately selected depending on the size of the injection molded article to be obtained and the size of the mold to be used. The clamping pressure can be appropriately selected depending on the size of the mold to be used and the resin capacity. The mold can be heated using an electric heater or a mold temperature regulator with a heat medium circulation. In particular, it is preferable to heat the mold by embedding a heat medium circulation pipe inside the mold, since this allows accurate and rapid control of the surface temperature of the mold and the molded body.

[0041] <Manufacturing method of extrusion molded products> The present invention also relates to a method for producing an extrusion molded product, which comprises a step of extruding a resin composition obtained by melting a resin, bead-like crosslinked particles, and, if necessary, other agents at a high temperature. For extrusion molding, a normal T-die extruder, inflation molding machine, etc. are used. These extruders are connected to a kneader. The melt-kneaded resin and bead-like crosslinked particles are fed to the extruder. Also, a device in which a kneader and an extrusion molding machine are integrated may be used. As a device in which a kneader and an extrusion molding machine are integrated, a known device may be used, and examples thereof include a continuous intensive mixer; a continuous type kneader such as a kneading type twin screw extrusion molding machine (same direction or different direction); a continuous kneading device using a rotating disk having a grinding mechanism; a single screw extrusion molding machine equipped with a kneading section (Dulmage, CTM, etc.); and a twin screw kneading extrusion molding machine having a kneading disk or a kneading rotor; but there is no particular limitation. Two or more types of kneaders may be used in combination.

[0042] <Manufacturing method of blow molded products> The present invention also relates to a method for producing a blow-molded article, which comprises a step of melting a resin, bead-like crosslinked particles, and, if necessary, other agents at a high temperature to obtain a resin composition, and then blow-molding the resulting resin composition. For the blow molding, a normal injection blow molding machine or a direct blow molding machine is used. The melt-kneaded resin and the bead-like crosslinked particles are fed to the blow molding machine. As the blow molding machine, a known one can be used and can be appropriately selected.

[0043] <Pellet manufacturing method> The case where the resin composition is in the form of pellets will be described. The melt-blended resin and bead-like crosslinked particles may be fed into a die assembly. The die device has a supply port to which the extruder is connected, and the melt-kneaded resin and the bead-like crosslinked particles are supplied from the extruder to the supply port of the die device.

[0044] The resin and bead-like crosslinked particles fed from the extruder to the die device are fed to the extrusion molding section of the die device. The resin and bead-like crosslinked particles are extruded from the extrusion port of the extrusion molding section to form strands. The diameter of the strand is not particularly limited and can be appropriately changed depending on the purpose, but is, for example, in the range of 0.2 to 10 mm or 0.5 to 5 mm.

[0045] The strands can be cut into pellets after being cooled as necessary. The cutting is carried out by a pelletizer. The most commonly used cooling method is to introduce the extruded strand into a water bath and immerse the strand in the cooling water in the water bath. The strands after cooling are preferably fed to a pelletizer after removing moisture adhering to the surface with a water draining device. The pelletizer cuts the strands by driving a rotary blade or the like. The length of the strands to be cut is not particularly limited and can be appropriately changed depending on the purpose, but is, for example, in the range of 0.5 to 10.0 mm or 1.0 to 5.0 mm. The shape of the pellets includes a cylinder, a prism, etc., but a cylinder is preferred from the viewpoints of ease of production and handling.

[0046] The pellets can be used to obtain molded articles, which can be produced by the above-mentioned methods for producing injection molded articles, the above-mentioned methods for producing extrusion molded articles, blow molding, vacuum molding, inflation molding, calendar molding, slush molding, dip molding, foam molding, and the like. The resulting molded article has a matte finish and a ground glass appearance. EXAMPLES

[0047] The present invention will be specifically described below with reference to examples and comparative examples, although the present invention is not limited to these examples.

[0048] [Examples 1 to 10 and Comparative Example 1] A master batch (MB) was obtained by extruding 100 parts by weight of isophthalic acid-copolymerized polyethylene terephthalate and 34 parts by weight of bead-like crosslinked particles at a temperature of 280° C. using a twin-screw extruder. The obtained MB (amount shown in Table 1) was dry-blended with 100 parts by weight of polyethylene terephthalate copolymerized with isophthalic acid, and injection-molded at a temperature of 280°C using an injection molding machine (product name: IS55FP-1.5A, manufactured by Shibaura Machine Co., Ltd., mold clamping pressure: 55t) equipped with a three-stage molded plate mold to obtain an injection-molded product as a three-stage molded plate having a thickness of 1.0 mm / 2.0 mm / 3.0 mm. Note that, for Example 5, a plate molded product was obtained in the same manner as in Example 4, except that 0.001 parts of Pigment Black 7 was added as a coloring material.

[0049] [Table 1]

[0050] thermoplastic resin A: Isophthalic acid copolymerized polyethylene terephthalate

[0051] Bead-like cross-linked particles I: Cross-linked polystyrene 4.9μm II: Cross-linked polystyrene 8.1μm III: Cross-linked polystyrene 17μm IV: Cross-linked polystyrene 34μm V: Cross-linked polymethyl methacrylate-styrene copolymer 6.8μm VI: Cross-linked polymethyl methacrylate-styrene copolymer 9.2μm VII: Crosslinked polymethyl methacrylate-styrene copolymer 57μm VIII: Cross-linked polymethyl methacrylate 8.5μm

[0052] [Examples 11 to 12 and Comparative Example 2] A composition was obtained by dry blending 100 parts by weight of polymethyl methacrylate resin and bead-like crosslinked particles (amounts shown in Table 2). The obtained composition was injection molded at a temperature of 240°C using an injection molding machine (product name: EC75SXIII-1.5A, manufactured by Shibaura Machine Co., Ltd., mold clamping pressure: 75t) equipped with a three-stage molded plate mold, to obtain an injection molded product as a three-stage molded plate with thicknesses of 1.0 mm / 2.0 mm / 3.0 mm.

[0053] [Table 2]

[0054] thermoplastic resin B: Polymethyl methacrylate

[0055] Bead-like cross-linked particles X: Cross-linked polymethyl methacrylate styrene copolymer 13μm XI: Cross-linked polymethyl methacrylate styrene copolymer 40μm

[0056] [Examples 13 to 20] A master batch (MB) was obtained by extruding 100 parts by weight of isophthalic acid-copolymerized polyethylene terephthalate, 34 parts by weight of bead-like crosslinked particles, 0.40 parts by weight of magnesium stearate, and 0.13 parts by weight of ethylene bis(stearic acid amide) at 280°C using a twin-screw extruder. The obtained MB (amount shown in Table 3) was dry-blended with 100 parts by weight of polyethylene terephthalate copolymerized with isophthalic acid, and injection-molded at a temperature of 280°C using an injection molding machine (product name: IS55FP-1.5 A, manufactured by Shibaura Machine Co., Ltd., mold clamping pressure: 55t) equipped with a three-stage molded plate mold, to obtain an injection-molded product as a three-stage molded plate with thicknesses of 1.0 mm / 2.0 mm / 3.0 mm.

[0057] [Table 3]

[0058] The molded articles obtained in the examples and comparative examples were evaluated for the following, and the evaluation results are shown in Table 4.

[0059] [Total light transmittance] The total light transmittance of the molded articles obtained in the examples and comparative examples was measured in accordance with JIS K 7361. In Examples 1 to 10 and Comparative Example 1, the measurement was performed on a 3.0 mm thick portion of the molded article, and in Examples 11 to 12 and Comparative Example 2, the measurement was performed on a 1.0 mm thick portion of the molded article.

[0060] [HAZE] The haze of the molded articles obtained in the examples and comparative examples was measured in accordance with JIS K 7136. Note that for Examples 1 to 10 and Comparative Example 1, the measurement was performed on a 3.0 mm thick portion of the molded article, and for Examples 11 to 12 and Comparative Example 2, the measurement was performed on a 1.0 mm thick portion of the molded article.

[0061] [Ground glass] The molded articles obtained in the Examples and Comparative Examples were visually evaluated for ground glass properties according to the following criteria: For Examples 1 to 10 and Comparative Example 1, the measurements were taken at a 3.0 mm thick portion of the molded article, and for Examples 11 to 12 and Comparative Example 2, the measurements were taken at a 1.0 mm thick portion of the molded article. ◎: More favorable ground glass properties ○: Ground glass-like ×: No ground glass properties

[0062] <Total light transmittance, haze, and ground glass properties evaluation> The molded products obtained in the examples and comparative examples were evaluated, and the results are shown in Table 4.

[0063] [Table 4] [Industrial Applicability]

[0064] According to the present invention, a molded product having a highly attractive design due to its ground glass properties can be obtained.

Claims

1. Thermoplastic resin (A) 100 parts by weight, and Bead-like crosslinked particles (B) having an average particle size of 50 μm or less: 0.1 to 10 parts by weight The thermoplastic resin composition comprises: a thermoplastic resin (A) and a crosslinked particle (B) having a refractive index difference of 0.005 or more and 0.08 or less.

2. The thermoplastic resin (A) is at least one resin selected from the group consisting of a polyethylene terephthalate resin, a polystyrene resin, and a polymethyl methacrylate resin; The thermoplastic resin composition according to claim 1, wherein the bead-like crosslinked particles (B) are at least one resin selected from the group consisting of crosslinked polystyrene resins, methyl methacrylate-styrene copolymer crosslinked particles, crosslinked polymethyl methacrylate resins, and silicone resins.

3. 3. The thermoplastic resin composition according to claim 1, wherein the thermoplastic resin (A) is a copolymerized polyethylene terephthalate resin.

4. 3. The thermoplastic resin composition according to claim 1, wherein the refractive index difference is from 0.008 to 0.

03.

5. 3. The thermoplastic resin composition according to claim 1, wherein the amount of the bead-like crosslinked particles (B) is 1.25 parts by weight or more based on 100 parts by weight of the thermoplastic resin (A).

6. The thermoplastic resin composition according to claim 1 or 2, further comprising a lubricant which is an aliphatic compound.

7. A thermoplastic resin molded article formed from the thermoplastic resin composition according to claim 1 or 2, the thermoplastic resin molded article having a thickness of 3 mm, a total light transmittance of 60% or more, and a haze of 40 to 85.

8. Thermoplastic resin (A) 100 parts by weight, and Bead-like crosslinked particles (B) having an average particle size of 50 μm or less: 5 to 100 parts by weight A masterbatch for thermoplastic resins, comprising: A masterbatch for a thermoplastic resin, wherein the difference in refractive index between the thermoplastic resin (A) and the crosslinked particles (B) is 0.005 or more and 0.08 or less.

9. 9. The masterbatch for thermoplastic resins according to claim 8, wherein the thermoplastic resin (A) is a copolymerized polyethylene terephthalate resin, or the masterbatch further contains a lubricant which is an aliphatic compound.

10. A method for producing a thermoplastic resin molded product, comprising the step of melting and molding the resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Manufacture of frost-tone glass article

    JP1985226431A

  • Molded synthetic resin article

    JP1989297465A

  • Polyester resin composition

    JP1999001606A

  • Frost-like plastic bottle

    JP2000301596A