Porous film
The porous film with inorganic and fluorine-containing polymer particles addresses blocking resistance and adhesion issues, enhancing manufacturing ease and battery performance by providing excellent adhesion to electrodes.
Patent Information
- Application Number
- JP2023169360
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2023-09-29
- Publication Date
- 2024-10-07
AI Technical Summary
Porous films used in lithium-ion secondary batteries face issues with blocking resistance and adhesion to electrodes, making them difficult to peel apart during manufacturing, which can impair their function.
A porous film configuration with a porous base material and a porous layer containing inorganic particles and fluorine-containing polymer particles, where the fluorine-containing polymer particles have specific structural units and occupy a defined percentage of the surface, providing excellent blocking resistance and adhesiveness.
The film exhibits improved blocking resistance and adhesiveness, preventing film adhesion during manufacturing and ensuring effective battery performance.
Smart Images

Figure 2024137619000014 
Figure 2024137619000015 
Figure 2024137619000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a porous film. [Background technology]
[0002] Lithium ion secondary batteries are widely used in portable digital devices such as smartphones, tablets, mobile phones, and notebook computers, as well as in automobiles such as electric vehicles, hybrid vehicles, and plug-in hybrid vehicles. The separators mounted therein are required to have various characteristics depending on the application, and various proposals have been made to satisfy the adhesive requirements between the electrodes and the porous film that is the separator (see, for example, Patent Documents 1 to 4). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 7094968 [Patent Document 2] Patent No. 6659081 [Patent Document 3] Patent No. 6051731 [Patent Document 4] Patent No. 6105816 Summary of the Invention [Problem to be solved by the invention]
[0004] However, a porous film having an adhesive function with an electrode has a problem that, in the process of manufacturing the porous film, the surfaces of the porous films tend to adhere to each other inside the rolled porous film produced, making it difficult to peel them off. This condition is called blocking. A porous film having an excellent adhesive function with an electrode without impairing blocking resistance has not yet been established.
[0005] The present invention provides a porous film having excellent blocking resistance and adhesiveness. [Means for solving the problem]
[0006] The porous film of the present invention has the following configuration. (1) A porous film having a porous layer containing inorganic particles and fluorine-containing polymer particles on at least one surface of the porous substrate, the fluorine-containing polymer particles containing 5% by mass or more and less than 30% by mass of a fluorine-containing (meth)acrylic acid ester monomer (A)-derived structural unit (X), based on 100% by mass of the monomer, a structural unit (Y-1) derived from the (meth)acrylic acid ester monomer (B), and a structural unit (Y-2) derived from the (meth)acrylic acid ester monomer (B), the structural unit (X) derived from the fluorine-containing (meth)acrylic acid ester monomer (A) being represented by the following general formula (1), and the structural units (Y-1) and (Y-2) derived from the (meth)acrylic acid ester monomer (B) being represented by the following general formula (2).
[0007] [ka]
[0008] [ka]
[0009] (In the formulas (1) and (2), R1 represents a hydrogen atom or a methyl group, R2 represents a fluorine-containing hydrocarbon group having 1 to 10 carbon atoms, R3 represents a group selected from the group consisting of alicyclic hydrocarbon groups having 5 to 10 carbon atoms, and a and b represent the degree of polymerization.) (2) The porous film according to (1), in which the occupancy rate of the fluorine-containing polymer particles on the surface of the porous layer is 60% or more and less than 95%, and when the porous layer is divided into three equal parts in the thickness direction, the region in contact with the porous substrate is designated as region A, the region in contact with region A is designated as region B, and the region in contact with region B is designated as region C, the following (a) to (c) are satisfied: (a) The content α of the fluorine-containing polymer particles in the region C is 60% or more and 90% or less of the total fluorine-containing polymer particle content in the porous film. (b) The content β of the fluorine-containing polymer particles in the region B is 10% or more and 40% or less of the total fluorine-containing polymer particle content in the porous film. (c) The content γ of the fluorine-containing polymer particles in the region A is 10% or less of the total fluorine-containing polymer particle content in the porous film. (3) The porous film according to (1) or (2), in which the indentation depth ratio h(0) shown by the following formula when the indenter is pressed in at a loading rate of 1 mN / min for 30 seconds by a nanoindentation method using a Berkovich type diamond indenter and then unloaded to 0.5 mN is 20 or more and 30 or less. h(0) = Pd(0) / d × 100 Pd(0): Indentation depth (μm) when pressed for 30 seconds at a loading rate of 1 mN / min and then unloaded to 0.5 mN d: Initial thickness of the porous layer (μm) (4) The structural unit (Y-1) derived from the (meth)acrylic acid ester monomer (B) contains at least one of cyclohexyl acrylate, cyclohexyl methacrylate, t-butylcyclohexyl acrylate, and 3,3,5-trimethylcyclohexyl acrylate, and the structural unit (Y-2) derived from the (meth)acrylic acid ester monomer (B) contains at least one of isobornyl acrylate, isobornyl methacrylate, dicyclopentanyl acrylate, and dicyclopentanyl methacrylate. The porous film according to any one of (1) to (3). (5) The porous film according to any one of (1) to (4), wherein the fluorine-containing polymer particles contain 60% by mass or more and 90% by mass or less in total of the structural unit (Y-1) derived from the (meth)acrylic acid ester monomer (B) and the structural unit (Y-2) derived from the (meth)acrylic acid ester monomer (B). (6) The porous film according to any one of (1) to (5), wherein the weight of the fluorine-containing polymer particles is from 0.01 g / m2 to 1.00 g / m2. (7) The porous film according to any one of (1) to (6), wherein the fluorine-containing polymer particles have a glass transition temperature (Tg) of 55 to 100°C. (8) The porous film according to any one of (1) to (7), wherein the fluorine-containing polymer particles have a volume average particle size of 10 nm or more and 500 nm or less. (9) The porous film according to any one of (1) to (8), wherein the thickness of the porous layer is from 0.10 μm to 5.0 μm. Effect of the Invention
[0010] According to the present invention, a porous film having excellent blocking resistance and adhesiveness can be provided. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a diagram showing a schematic diagram of an overall structure of a measuring device used in an indentation test. [Diagram 2] FIG. 13 is a diagram showing the relationship between time and load in an indentation test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Preferred embodiments of the present invention will be described in detail below. Note that the present invention is not limited to the embodiments described below, and should be understood to include various modified examples that are implemented within the scope of the present invention. (Porous base material) In the present invention, the porous substrate may be a porous membrane having pores inside, a nonwoven fabric, or a porous membrane sheet made of a fibrous material. The resin constituting the porous substrate is preferably made of a resin that is electrically insulating, electrically stable, and stable in electrolyte.
[0013] From the viewpoint of providing a shutdown function, the resin used is preferably a thermoplastic resin, and more preferably a thermoplastic resin having a melting point of 200° C. or less. The shutdown function here refers to a function that, when the lithium-ion battery generates abnormal heat, closes the porous structure by melting with heat, stops the movement of ions, and stops power generation.
[0014] The thermoplastic resin may be, for example, polyolefin, and the porous substrate is preferably a polyolefin porous substrate containing polyolefin.More preferably, the polyolefin porous substrate contains polyolefin having a melting point of 200°C or less.
[0015] Specific examples of polyolefins include polyethylene, polypropylene, copolymers thereof, and mixtures of these. Examples of polyolefin porous substrates include single-layer polyolefin porous substrates containing 90% by mass or more of polyethylene, and multi-layer polyolefin porous membrane substrates made of polyethylene and polypropylene.
[0016] Examples of methods for producing these porous substrates include a method in which a polyolefin resin is made into a sheet and then stretched to make it porous, and a method in which a polyolefin resin is dissolved in a solvent such as liquid paraffin, made into a sheet, and then the solvent is extracted to make it porous.
[0017] The polyolefin porous substrate obtained by the above method may be subjected to a surface treatment from the viewpoint of adhesion between the polyolefin porous substrate and the porous layer.
[0018] The thickness of the porous substrate is preferably 3 μm or more and 50 μm or less, more preferably 5 μm or more and 30 μm or less. By making the thickness of the porous substrate 50 μm or less, the internal resistance of the porous substrate is prevented from increasing, which is preferable. In addition, by making the thickness of the porous substrate 3 μm or more, the manufacturing becomes easy, and sufficient mechanical properties are obtained, which is preferable.
[0019] The size of the pores present in the porous substrate is preferably 0.01 to 50 μm, and the porosity of the porous substrate is preferably 10 to 95%. By having such a thickness, pore size, and porosity, it is possible to obtain sufficient ion conductivity, and also sufficient mechanical strength and insulation properties. (Porous layer) The porous film of the present invention has a porous layer containing inorganic particles and fluorine-containing polymer particles on at least one surface of a porous substrate. The porous layer has a structure in which the fluorine-containing polymer particles permeate into region C and region B when the porous layer is divided into three equal parts in the thickness direction, the region in contact with the porous substrate is region A, the region in contact with region A is region B, and the region in contact with region B is region C. The method for obtaining this structure will be described later, but a coating liquid containing inorganic particles and a coating liquid containing fluorine-containing polymer particles are separately prepared to form a porous layer containing inorganic particles and fluorine-containing polymer particles.
[0020] The porous layer can be made of at least one organic resin selected from the group consisting of acrylic acid copolymer resin, polyvinylidene fluoride resin, polyacrylamide copolymer resin, polyamideimide resin, and poly(meth)aramid resin, and in order to ensure the strength of the porous layer, it is preferable that the porous layer contains inorganic particles. Specific examples of acrylic resins contained in the porous layer include "Jurymer" (registered trademark) AT-210, ET-410, "Aron" (registered trademark) A-104, AS-2000, and NW-7060 manufactured by Toa Gosei Co., Ltd., "LIOACCUM" (registered trademark) series manufactured by Toyochem Co., Ltd., TRD202A and TRD102A manufactured by JSR Corporation, "Polystron" (registered trademark) 117, 705, and 1280 manufactured by Arakawa Chemical Industries, Ltd., "Kogam" (registered trademark) series manufactured by Showa Denko K.K., and WEM-200U and WEM-3000 manufactured by Taisei Fine Chemical Co., Ltd.
[0021] The dispersion may contain a dispersant for improving the dispersion stability of inorganic particles, and at least one of the group consisting of polyacrylic acid copolymer resin and carboxymethyl cellulose resin can be used. Representative examples of polyacrylic acid copolymer resin include DL-40 and TL-37 manufactured by Nippon Shokubai Co., Ltd., and A-6012 and A-6114 manufactured by Toa Gosei Co., Ltd. Representative examples of cellulose-based resin include carboxymethyl cellulose and its derivatives, and specifically include 1120, 1220, SP200, SE400, and DN-100L manufactured by Daicel FineChem Co., Ltd., Sunrose (registered trademark) FJ08HC and A04SH manufactured by Nippon Seishi Co., Ltd., and Cellogen (registered trademark) 7A and WS-C manufactured by Daiichi Kogyo Seiyaku Co., Ltd.
[0022] Examples of inorganic particles include inorganic oxide particles such as aluminum oxide, boehmite, silica, titanium oxide, zirconium oxide, iron oxide, and magnesium oxide, inorganic nitride particles such as aluminum nitride and silicon nitride, and sparingly soluble ion crystal particles such as calcium fluoride, barium fluoride, and barium sulfate. These particles may be used alone or in combination of two or more kinds.
[0023] The shape of the inorganic particles used may be any shape, including spherical, plate-like, needle-like, rod-like, elliptical, etc. Among these, spherical shapes are preferred from the viewpoints of surface modification, dispersibility, and coatability.
[0024] The lower limit of the content of the inorganic particles is preferably 50% by mass or more, more preferably 80% by mass or more and less than 97% by mass, based on the total of at least one organic resin selected from the group consisting of acrylic acid copolymer resin, polyvinylidene fluoride resin, polyacrylamide copolymer resin, polyamideimide resin, and poly(meth)aramid resin, and the inorganic particles. When the content of the inorganic particles is within this range, the strength of the porous layer is appropriately maintained.
[0025] The content of inorganic particles can be calculated by the following method. Using 40 g of water on a 10 cm x 10 cm porous film, the porous layer containing inorganic particles provided on the porous substrate is removed, and the water and organic solvent such as alcohol are thoroughly dried to obtain the components contained in the porous layer. After measuring the mass of all the components obtained, the components are burned at a high temperature at which the organic resin components melt and decompose, and the mass of only the inorganic particles is measured. Next, the content of inorganic particles in the porous layer is calculated in mass% using the formula (mass of inorganic particles / mass of all components) x 100.
[0026] The primary average particle diameter of the inorganic particles is preferably 0.10 μm or more and 5.0 μm or less, more preferably 0.10 μm or more and 2.5 μm or less, from the viewpoint of the strength and porosity of the porous layer. By setting the lower limit of the primary average particle diameter to 0.10 μm or more, the porous layer becomes dense, and the pores of the porous substrate are closed, which increases the air permeability and prevents the battery characteristics from deteriorating. In addition, by setting the upper limit of the primary average particle diameter to 5.0 μm or less, the porous layer is prevented from having a non-uniform structure and being unable to obtain a sufficient heat shrinkage rate, and the thickness of the porous layer is prevented from increasing and the battery characteristics are prevented from deteriorating. The primary average particle diameter is the particle diameter when the volume-based cumulative ratio is 50% calculated by the method described below.
[0027] The order of preparation of a coating liquid containing inorganic particles for forming a porous layer is not particularly limited, but from the viewpoint of uniformly dispersing the inorganic particles and making the primary average particle size of the inorganic particles in the coating liquid containing the inorganic particles uniform, it is preferable to add a dispersant to a solvent, and then add and disperse the inorganic particles in the dispersion, and then add an organic resin, additives, etc. as necessary to prepare a coating liquid containing inorganic particles.
[0028] As a solvent for dispersing the inorganic particles, a polar solvent such as water, glycerol, ethylene glycol, propylene glycol, or methanol can be used.
[0029] The method for dispersing the coating liquid containing inorganic particles is not particularly limited, but from the viewpoint of flattening and uniforming the surface shape of the porous layer, it is important that the inorganic particles in the coating liquid containing inorganic particles are uniformly dispersed and that the primary average particle size of the inorganic particles is uniform, and it is preferable to use a ball mill, a bead mill, a sand mill, a roll mill, etc. In particular, it is preferable to disperse using a bead mill, the bead diameter used in the bead mill is preferably 0.1 to 1 mm, and the material of the beads used is preferably aluminum oxide, zirconium oxide, zirconia-reinforced alumina, etc.
[0030] The viscosity of the coating liquid containing inorganic particles is preferably 3 cP or more and 200 cP or less, more preferably 5 cP or more and 150 cP or less, and even more preferably 10 cP or more and 100 cP or less. If the viscosity of the coating liquid containing inorganic particles is 200 cP or less, high-speed coating is possible and good productivity can be obtained. If the coating liquid has a low viscosity, it is preferable because it is suitable for high-speed coating, but for example, from the viewpoint of stable coating film formation, 3 cP or more is preferable. The viscosity of the coating liquid containing inorganic particles can be controlled by the solid content concentration of the coating liquid containing inorganic particles, the mixing ratio of the organic resin and the inorganic particles, and the molecular weight of the organic resin.
[0031] The porous layer contains fluorine-containing polymer particles that, in the presence of an electrolyte, penetrate into gaps between active materials of the electrode and exert an anchor effect, thereby adhering to the electrode.
[0032] By using such fluorine-containing polymer particles, a porous film that can be bonded to an electrode can be obtained, but the porous film having an adhesive function to an electrode has a problem that, in the process of producing the porous film, the surfaces of the porous films tend to adhere to each other inside the produced roll-shaped porous film, making it difficult to peel them off. This condition is called blocking.
[0033] If a roll of porous film in which blocking has occurred is used in the next process, which is the production of a battery, the function of the porous film may be impaired or the porous film may be torn. The ability to prevent this is called anti-blocking property.
[0034] Blocking is a phenomenon in which an adhesive function is expressed inside a porous film stored in a roll, and the porous films are bonded together. For the adhesive function to be expressed, the polymer particles must have an adhesive function, and the particle shape must be deformed to increase the adhesion area. Factors that cause the particle shape to deform include pressure and temperature. The pressure inside the porous film roll depends on the winding tension when the film is wound up into a roll. In other words, the pressure inside the roll increases as the winding tension increases. However, since the porous substrate of the separator is thin and has pores inside, it is stretchable, so in the manufacturing process of the porous film, it is transported and wound up at extremely low tension to prevent dimensional changes due to stretching. On the other hand, the temperature can be high enough to exceed room temperature depending on the transportation environment and transportation route. Therefore, temperature is the dominant factor that causes the particle shape to deform. This change in particle shape due to temperature can be measured using the adhesion suppression evaluation method described below, which measures the rate of change in particle diameter at any temperature. As described above, blocking resistance is a property that corresponds to the adhesion-suppressing ability of the polymer particles, and by using polymer particles having excellent adhesion-suppressing ability, a porous film having excellent blocking resistance can be obtained.
[0035] By using the polymer particles described below, a porous film having excellent adhesiveness can be obtained while suppressing blocking during the porous film production process and the battery production process using the porous film.
[0036] The polymer particles of the present invention are formed of a copolymer consisting of a structural unit (X), a structural unit (Y-1), and a structural unit (Y-2). In this specification, the structural unit (X), the structural unit (Y-1), and the structural unit (Y-2) are sometimes referred to as "polymer particle units".
[0037] The structural unit (X) is a repeating unit derived from the fluorine-containing (meth)acrylic acid ester monomer (A) and is represented by the following general formula (1).
[0038] [ka]
[0039] (In formula (1), R 1 is hydrogen or a methyl group, R 2 represents a fluorine-containing hydrocarbon group having 1 to 10 carbon atoms, and a represents the degree of polymerization. In formula (1), R 1 are each independently a hydrogen or a methyl group. 1 The monomer with hydrogen is acrylate, R 1 However, the monomer with a methyl group represents a methacrylate.
[0040] R 2 R is a fluorine-containing hydrocarbon group having 1 to 10 carbon atoms, preferably a fluorine-containing hydrocarbon group having 2 to 10 carbon atoms. The hydrocarbon group may have an unsaturated bond and may be either a linear or branched hydrocarbon group. 2 At least some of the hydrogen atoms in the hydrocarbon group are replaced with fluorine. 2 All hydrogen atoms of the hydrocarbon group may be substituted with fluorine.
[0041] R 2 For example, -CH 2 CF 3 , -CH 2 CF 2 CF 2 H, -CH 2 CF 2 CF 3 , -CH 2 CF 2 CFHCF 3 , -CH 2 (CF 2 ) 3 CF 2 H, -CH 2 CH 2 (CF 2 ) 3 CF3 , -CH 2 (CF 2 ) 5 CF 2 H, -CH 2 CH 2 (CF 2 ) 5 CF 3 , -CH 2 CH 2 (CF 2 ) 7 CF 3 , -CH(CF 3 ) 2 , -CH 2 CCH 3 (CF 3 ) 2 etc.
[0042] The fluorine-containing (meth)acrylic acid ester monomer (A) is a fluorine-containing hydrocarbon group (R 2 ).
[0043] As the fluorine-containing (meth)acrylic acid ester monomer (A), CH 2 =CHCOOCH 2 CF 3 (3FA), CH 2 =CHCOOCH 2 CF 2 CF 2 H(4FA), CH 2 =CHCOOCH 2 CF 2 CF 3 (5FA), CH 2 =CHCOOCH 2 CF 2 CFHCF 3 (6FA), CH 2 =CHCOOCH 2 (CF 2 ) 3 CF 2 H(8FA), CH 2 =CHCOOCH 2 CH2 (CF 2 ) 3 CF 3 (9FA)、 CH 2 =CHCOOCH 2 (CF 2 ) 5 CF 2 H(12FA)、 CH 2 =CHCOOCH 2 CH 2 (CF 2 ) 5 CF 3 (13FA)、 CH 2 =CHCOOCH 2 CH 2 (CF 2 ) 7 CF 3 (17FA)、 CH 2 =CHCOOCH(CF 3 ) 2 (HFIP-A)、 CH 2 =CHCOOCH 2 CCH 3 (CF 3 ) 2 (6FNP-A)、 CH 2 =C(CH 3 )COOCH 2 CF 3 (3FMA)、 CH 2 =C(CH 3 )COOCH 2 CF 2 CF 2 H(4FMA)、 CH 2 =C(CH 3 )COOCH 2 CF 2 CF 3 (5FMA)、 CH 2 =C(CH 3 )COOCH 2 CF 2 CFHCF 3 (6FMA)、 CH 2=C(CH 3 )COOCH 2 (CF 2 ) 3 CF 2 H(8FMA), CH 2 =C(CH 3 )COOCH 2 CH 2 (CF 2 ) 3 CF 3 (9FMA), CH 2 =C(CH 3 )COOCH 2 (CF 2 ) 5 CF 2 H(12FMA), CH 2 =C(CH 3 )COOCH 2 CH 2 (CF 2 ) 5 CF 3 (13FMA), CH 2 =C(CH 3 )COOCH 2 CH 2 (CF 2 ) 7 CF 3 (17FMA), CH 2 =C(CH 3 )COOCH(CF 3 ) 2 (HFIP-MA), CH 2 =C(CH 3 )COOCH 2 CCH 3 (CF 3 ) 2 (6FNP-MA) Examples of such compounds include:
[0044] The structural units (Y-1) and (Y-2) are repeating units derived from the (meth)acrylic acid ester monomer (B) and are represented by the following general formula (2).
[0045] [ka]
[0046] (In formula (2), R 3 represents a group selected from the group consisting of alicyclic hydrocarbon groups having 5 to 10 carbon atoms, and a and b represent the degree of polymerization. In formula (2), R 1 represents a hydrogen atom or a methyl group.
[0047] R 3 R is a group selected from the group consisting of alicyclic hydrocarbon groups having 5 to 10 carbon atoms. 3 The structural units (Y-1) and (Y-2) having the following structure are different from each other. The different structural units are R 3 are different from each other and / or are different between acrylates and methacrylates.
[0048] Examples of the alicyclic hydrocarbon group having 5 to 10 carbon atoms include a saturated monocyclic group, a polycyclic group, and a bridged ring group. Examples of the cyclic hydrocarbon group having 5 to 10 carbon atoms include a cyclohexyl group, a trimethylcyclohexyl group, a t-butylcyclohexyl group, a dicyclopentanyl group, and an isobornyl group.
[0049] The structural unit (Y-1) derived from the (meth)acrylic acid ester monomer (B) may include at least one of cyclohexyl acrylate, cyclohexyl methacrylate, t-butylcyclohexyl acrylate, and 3,3,5-trimethylcyclohexyl acrylate. The structural unit (Y-2) derived from the (meth)acrylic acid ester monomer (B) may include at least one of isobornyl acrylate, isobornyl methacrylate, dicyclopentanyl acrylate, and dicyclopentanyl methacrylate.
[0050] The copolymer forming the fluorine-containing polymer particles contains, when the monomer units thereof are taken as 100 mass%, 5 mass% or more and less than 30 mass% of the structural unit (X) derived from the fluorine-containing (meth)acrylic acid ester monomer (A) in 100 mass% of the monomer, and contains a structural unit (Y-1) derived from the (meth)acrylic acid ester monomer (B) and a structural unit (Y-2) derived from the (meth)acrylic acid ester monomer (B).
[0051] The fluorine-containing polymer particles preferably contain the structural unit (Y-1) derived from the (meth)acrylic acid ester monomer (B) in an amount of 25% by mass to 55% by mass in 100% by mass of the monomer, and the structural unit (Y-2) derived from the (meth)acrylic acid ester monomer (B) in an amount of 25% by mass to 55% by mass in 100% by mass of the monomer. In the general formulas (1) and (2), a and b are the polymerization degrees of each repeating unit and are real numbers that correspond to the above mass ratios.
[0052] The structural unit (X) derived from the fluorine-containing (meth)acrylic acid ester monomer (A) is preferably more than 5 mass%, more preferably 7 mass% or more, and even more preferably 9 mass% or more in 100 mass% of the polymer particle unit. The structural unit (X) derived from the fluorine-containing (meth)acrylic acid ester monomer (A) is preferably 28 mass% or less, more preferably 26 mass% or less, and even more preferably 24 mass% or less in 100 mass% of the polymer particle unit. By containing the structural unit (X) derived from the fluorine-containing (meth)acrylic acid ester monomer (A) in the above range, it is possible to obtain polymer particles having excellent adhesiveness and adhesion suppression properties.
[0053] The structural unit (Y-1) derived from the (meth)acrylic acid ester monomer (B) is preferably more than 25 mass%, more preferably 28 mass% or more, even more preferably 31 mass% or more, and even more preferably 34 mass% or more, based on 100 mass% of the polymer particle unit. The structural unit (Y-1) derived from the (meth)acrylic acid ester monomer (B) is preferably less than 55 mass%, more preferably 52 mass% or less, based on 100 mass% of the polymer particle unit. By containing the structural unit (Y-1) in the above range, it is possible to obtain polymer particles with excellent adhesiveness and adhesion suppression properties.
[0054] The structural unit (Y-2) derived from the (meth)acrylic acid ester monomer (B) is preferably more than 25% by mass, more preferably 28% by mass or more, based on 100% by mass of the polymer particle unit. The structural unit (Y-2) derived from the (meth)acrylic acid ester monomer (B) is preferably less than 55% by mass, more preferably 52% by mass or less, even more preferably 49% by mass or less, and even more preferably 46% by mass or less, based on 100% by mass of the polymer particle unit. By containing the structural unit (Y-2) in the above range, the effect of improving the glass transition temperature (Tg) can be obtained without impairing the degree of swelling, and thus polymer particles with excellent adhesion and adhesion can be obtained.
[0055] The total of the structural unit (Y-1) and the structural unit (Y-2) is preferably 60% by mass or more, more preferably 65% by mass or more, and even more preferably 70% by mass or more, based on 100% by mass of the polymer particle unit. The total of the structural unit (Y-1) and the structural unit (Y-2) is preferably 90% by mass or less, more preferably less than 85% by mass, and even more preferably 80% by mass or less, based on 100% by mass of the polymer particle unit. By containing the total of the structural unit (Y-1) and the structural unit (Y-2) within the above range, it is possible to obtain polymer particles with excellent adhesiveness and adhesion suppression.
[0056] The glass transition temperature (Tg) of the fluorine-containing polymer particles of the present invention is preferably 60°C or more and 100°C or less. By setting the glass transition temperature (Tg) of the fluorine-containing polymer particles to the above range, polymer particles excellent in adhesion and blocking resistance can be obtained. The upper limit of the glass transition temperature (Tg) of the fluorine-containing polymer particles is preferably less than 100°C, more preferably 90°C or less, further preferably 80°C or less, particularly preferably 70°C or less. The lower limit of the glass transition temperature (Tg) of the fluorine-containing polymer particles is preferably more than 60°C, more preferably 62°C or more. The glass transition temperature (Tg) of the fluorine-containing polymer particles can be adjusted by changing the type and composition ratio of the monomer.
[0057] In this specification, the "glass transition temperature (Tg) of the fluorine-containing polymer particles" is measured by the following method.
[0058] The aqueous dispersion of polymer particles is freeze-dried, and about 10 mg of particle powder is used to measure with a differential scanning calorimeter (DSC Pyris1 DSC, manufactured by Perkin Elmer) in accordance with JIS K7121:2012.
[0059] The polymer constituting the polymer particles can be obtained, for example, by emulsion polymerization of a monomer mixture consisting of multiple types of (meth)acrylic acid ester monomers and a radical polymerizable compound other than the (meth)acrylic acid ester monomer in an aqueous medium.
[0060] From the viewpoint of adhesion, it is preferable that the glass transition temperature (Tg) of a homopolymer composed of the polyfunctional monomer (C) having two or more olefinic double bonds per molecule is -50°C or higher and 0°C or lower.
[0061] The polyfunctional monomer (C) having two or more olefinic double bonds per molecule is preferably contained in an amount of 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 3% by mass or more, based on 100% by mass of the polymer particle unit. The polyfunctional monomer (C) having two or more olefinic double bonds per molecule is preferably contained in an amount of 10% by mass or less, more preferably 8% by mass or less, and even more preferably 6% by mass or less, based on 100% by mass of the monomer unit. By containing the polyfunctional monomer (C) having two or more olefinic double bonds per molecule in the above range, it is possible to obtain polymer particles having excellent adhesiveness and blocking resistance.
[0062] The volume average particle diameter of the polymer particles is preferably 100 nm or more and 500 nm or less. The volume average particle diameter of the polymer particles is preferably more than 100 nm, more preferably 120 nm or more, and even more preferably 150 nm or more. The volume average particle diameter of the polymer particles is preferably less than 500 nm, more preferably 450 nm or less, and even more preferably 400 nm or less. By making the volume average particle diameter equal to or more than the above-mentioned lower limit, the viscosity of the dispersion in which the polymer particles are dispersed is suppressed from increasing, and an aqueous dispersion with a high solid content is easily obtained. In addition, by making the volume average particle diameter equal to or less than the above-mentioned upper limit, the storage stability of the dispersion of the polymer particles can be improved, and the uniformity of the coating film formed can be improved. The volume average particle diameter of the polymer particles can be adjusted by changing the type of emulsifier and the monomer composition ratio during polymerization of the polymer particles.
[0063] The particle size distribution of the polymer particles (volume average particle size / number average particle size) is preferably 1.5 or less, more preferably 1.4 or less, even more preferably 1.3 or less, even more preferably 1.2 or less, and even more preferably 1.1 or less. By making the particle size distribution 1.5 or less, the uniformity of the coating film containing the polymer particles can be ensured, which is preferable. The particle size distribution of the polymer particles can be adjusted by changing the type of emulsifier, the monomer composition ratio, and the polymerization conditions during polymerization of the polymer particles.
[0064] The average particle size and particle size distribution of the polymer particles can be measured using a particle size distribution measuring device that uses dynamic light scattering as the measurement principle. Examples of such particle size distribution measuring devices include HORIBA LB-550, SZ-100 series (manufactured by Horiba, Ltd.), FPAR-1000 (manufactured by Otsuka Electronics Co., Ltd.), etc.
[0065] As a solvent for use in a coating liquid containing fluorine-containing polymer particles, polar solvents such as water, glycerol, ethylene glycol, propylene glycol, dimethylsulfoxide, dimethylformamide, acetonitrile, ethylene carbonate, furfuryl alcohol, and methanol can be used.
[0066] A fluororesin, acrylic resin and olefin resin may be added to the coating liquid containing the fluorine-containing polymer particles as necessary, and from the viewpoint of battery characteristics, the amount is preferably 0.5 to 15 mass %, more preferably 1 to 10 mass %.
[0067] The occupancy rate of the fluorine-containing polymer particles on the surface of the porous layer is preferably less than 95%, more preferably 90% or less, and particularly preferably 85% or less. Moreover, this occupancy rate is preferably 60% or more, more preferably 65% or more, and particularly preferably 70% or more. The occupancy rate of less than 95% is preferable from the viewpoint of increasing ion permeability and improving cycle characteristics. This ensures the life of the battery. The occupancy rate of 85% or less is preferable from the viewpoint of ensuring blocking resistance by increasing the area of contact between the part where the fluorine-containing polymer particles are not present and the inorganic particle layer is exposed and the substrate that is the back surface of the porous layer, or the fluorine-containing polymer particles occupying the porous layer surface provided on the back surface, during the production and winding of the porous film. It is also preferable from the viewpoint of suppressing the blocking of the pores on the inorganic particle surface by the fluorine-containing polymer particles and further improving ion permeability. During charging and discharging, the electrode active material expands and contracts greatly, and stress associated therewith is generated inside the battery. This stress may cause a gap to form between the electrode and the separator, which causes a technical problem of deteriorating cycle characteristics. In order to prevent the formation of such gaps, fluorine-containing polymer particles having an adhesive function can be provided on the porous surface to bond the electrode and the separator. From the viewpoint of providing this adhesiveness to the porous surface of the separator, the occupancy rate of the fluorine-containing polymer particles on the porous layer surface is preferably 60% or more, and particularly preferably 70% or more.
[0068] The occupancy rate of the fluorine-containing polymer particles on the surface of the porous layer is measured by observing the surface of the porous layer of the obtained porous film using SEM-EDX, specifically according to the method described in the examples.
[0069] The occupancy rate of the fluorine-containing polymer particles can be adjusted by changing the content of the structural unit (X) derived from the fluorine-containing (meth)acrylic acid ester monomer (A) contained in 100 mass% of the polymer particle unit and the basis weight of the fluorine-containing polymer particles.
[0070] When the porous layer is divided into three equal parts in the thickness direction, the region in contact with the porous substrate is designated as region A, the region in contact with region A is designated as region B, and the region in contact with region B is designated as region C, the content α of the fluorine-containing polymer particles in region C is preferably 90% or less, more preferably 85% or less, and particularly preferably 80% or less. The content in region C is preferably 60% or more, more preferably 65% or more. Setting the content to 90% or less is preferable from the viewpoint of increasing ion permeability and improving cycle characteristics. Stress due to expansion and contraction of the electrode active material occurs inside the battery during charging and discharging. It is known that materials required for high capacity have a large expansion and contraction rate accompanying charging and discharging, which may cause a gap to form between the electrode and the separator, resulting in a decrease in cycle characteristics. The fluorine-containing polymer particles in region C absorb the stress of this expansion and contraction, suppressing a decrease in cycle characteristics. From this viewpoint, the content of the fluorine-containing polymer particles in region C in contact with the electrode active material is preferably 60% or more, more preferably 65% or more. From the viewpoint of providing adhesiveness for bonding the electrodes and the separator, the content of the fluorine-containing polymer particles is preferably 60% or more, and from the viewpoint of improving adhesiveness, it is more preferably 65% or more.
[0071] The content β of the fluorine-containing polymer particles in region B is preferably 40% or less, more preferably 35% or less, and particularly preferably 30% or less. The content is preferably 10% or more, more preferably 15% or more. A content of 40% or less is preferable from the viewpoint of increasing ion permeability and improving cycle characteristics. On the other hand, a content of 10% or more is preferable from the viewpoint of absorbing stress due to expansion and contraction accompanying charge and discharge and suppressing deterioration of cycle characteristics.
[0072] The content γ of the fluorine-containing polymer particles in the region A is preferably 10% or less, particularly preferably 5% or less. By setting the content to 10% or less, it is preferable from the viewpoint of suppressing the blocking of the pores of the porous substrate by the fluorine-containing polymer particles, the loss of ion permeability, and the deterioration of cycle characteristics.
[0073] At a thermal shrinkage rate of 150°C, the porous substrate starts to shrink at about 130°C, and abrupt shrinkage occurs up to about 140°C. The porous layer containing inorganic particles has a function of suppressing the shrinkage of the porous substrate. When the organic resin component contained in the porous layer is not expected to have a shrinkage resistance function up to the 150°C region, it is preferable that the organic resin component contained in the porous layer is small from the viewpoint of imparting a function of suppressing the shrinkage of the porous substrate. In particular, by reducing the organic resin component present at the interface between the porous layer and the porous substrate, abrupt shrinkage of the porous substrate in the 130 to 140°C region can be suppressed. The reason why this effect is obtained is not clear, but it is presumed that the stress to withstand shrinkage inside the porous layer is the largest in the region A in contact with the porous substrate, and the shrink resistance of the porous layer is maintained high due to the small amount of organic resin component in this region. From the viewpoint of imparting this shrink resistance, the content of the fluorine-containing polymer particles in the region A is preferably 10% or less, and particularly preferably 5% or less.
[0074] By optimizing the content of fluorine-containing polymer particles in regions A, B, and C, it is possible to achieve both excellent adhesion to the electrode, a good thermal shrinkage rate at 150°C, and good cycle characteristics.
[0075] The content of the fluorine-containing polymer particles in the thickness direction of the porous layer is measured by observing the cross section of the porous layer in the obtained porous film using SEM-EDX, and in detail, is measured in accordance with the method described in the examples.
[0076] The content of the fluorine-containing polymer particles in the regions A and B can be adjusted by changing the content of the structural unit (X) derived from the fluorine-containing (meth)acrylic acid ester monomer (A) contained in 100% by mass of the polymer particle unit. The content of the fluorine-containing polymer particles in the region C can be adjusted in the manufacturing method of the porous film described later by coating a coating liquid containing inorganic particles on a porous substrate, coating a coating liquid containing fluorine-containing polymer particles before the coating liquid containing inorganic particles is dried (in a state containing a solvent), and drying the solvents at the same time.
[0077] The indentation depth ratio h(0) of the porous layer surface is preferably 20 or more, more preferably 21 or more, and particularly preferably 22 or more. The indentation depth ratio h(0) of 20 or more is preferable from the viewpoint of absorbing the stress caused by the expansion and contraction of the electrode active material during discharge in the porous layer. On the other hand, the indentation depth ratio h(0) of 30 or less is preferable from the viewpoint of suppressing insulation failure. Insulation failure occurs when, in the production process of a secondary battery, when the positive electrode and negative electrode materials and the separator are wound, minute solid matter such as foreign matter and fallen matter is mixed in during the process, and the mixed solid matter is pressed into the porous layer by the pressure during vacuum sealing or the molding pressure in the aluminum lamination process after vacuum sealing, causing damage to the separator. From this viewpoint, the indentation depth ratio h(0) is preferably 30 or less, more preferably 28 or less, and particularly preferably 25 or less.
[0078] The indentation depth ratio h(0) of the porous layer surface is measured on the surface of the porous layer of the obtained porous film by nanoindentation using a Berkovich type diamond indenter, and in detail, is measured according to the method described in the examples.
[0079] The indentation depth ratio h(0) of the porous layer surface can be adjusted by the following method for producing a porous film: mixing a coating liquid containing inorganic particles and a coating liquid containing fluorine-containing adhesive particles in advance, coating the mixture on a porous substrate, and drying the mixture; or coating a coating liquid containing inorganic particles on a porous substrate, coating a coating liquid containing fluorine-containing polymer particles before the coating liquid containing inorganic particles dries (in a state containing a solvent), and drying the solvents at the same time. (Production of a porous film) When the porous layer is divided into three equal parts in the thickness direction, the region in contact with the porous substrate is designated as region A, the region in contact with region A is designated as region B, and the region in contact with region B is designated as region C, methods for forming a structure in which the fluorine-containing polymer particles are selectively infiltrated into region C and region B include a method in which a coating liquid containing inorganic particles and a coating liquid containing fluorine-containing adhesive particles are mixed in advance, and then the mixture is applied to the porous substrate and dried; a method in which a coating liquid containing inorganic particles is applied to the porous substrate and dried to form a layer containing inorganic particles, and then a coating liquid containing fluorine-containing polymer particles is applied on the layer containing inorganic particles and dried; and a method in which a coating liquid containing inorganic particles is applied to the porous substrate, and before the coating liquid containing inorganic particles is dried, that is, before the coating liquid containing inorganic particles is dried, a coating liquid containing fluorine-containing polymer particles is applied on the coating liquid containing inorganic particles that contains a solvent, and the solvents of these coating liquids are dried at the same time.
[0080] Methods for drying the solvent include, but are not limited to, a drying method using a heated roll, a drying method using a blower, a drying oven, etc., and the drying temperature is preferably 25° C. or higher and 100° C. or lower. If the drying temperature is lower than 25° C., it may take a long time to dry the solvent, which may result in poor productivity. If the drying temperature is higher than 100° C., the porous substrate may shrink excessively.
[0081] A known method may be used for applying the coating liquid containing inorganic particles. For example, dip coating, gravure coating, chamber gravure, slit die coating, knife coating, comma coating, kiss coating, DM coater method, bar coating, screen printing, etc. Among these, gravure coating, chamber gravure, and DM coater are particularly preferred from the viewpoint of productivity.
[0082] As a method for applying a coating liquid containing fluorine-containing polymer particles, even if a method is selected in which a coating liquid containing inorganic particles is applied to a porous substrate, dried to form a layer containing inorganic particles, and then a coating liquid containing fluorine-containing polymer particles is applied on the layer containing inorganic particles, the coating liquid containing inorganic particles is applied on a porous substrate, and before the coating liquid containing inorganic particles is dried, the coating liquid containing fluorine-containing polymer particles is applied on the layer containing inorganic particles in a solvent-containing state, since there is a concern that the film structure of the layer containing inorganic particles may be destroyed, a method of coating in which a distance of several tens of μm or more is arbitrarily provided between the layer containing inorganic particles and the coating part of the coating liquid containing fluorine-containing polymer particles is preferable. For example, methods such as die coating, curtain coating, inkjet, spray coating, and rotor dampening can be mentioned. Among these, a slit die coating method using a meniscus of several tens of μm formed between the layer containing inorganic particles and the coating part of the coating liquid containing fluorine-containing polymer particles destroys the film structure containing inorganic particles to some extent. Therefore, inkjet, spray coating, and rotor dampening methods that do not use meniscus are preferable. In the inkjet, spray coating, and rotor dampening methods, the layer containing inorganic particles and the coating part of the coating liquid containing fluorine-containing polymer particles are separated by a distance of several mm or more, and since they are not coating methods that use a meniscus, there is no factor that makes the meniscus unstable as the coating speed increases, so they have excellent high-speed coating properties. Since the accompanying air current that occurs near the film as the coating speed increases prevents the droplets of the coating liquid containing fluorine-containing polymer particles discharged from the inkjet, spray coating, and rotor dampening from landing on the layer containing inorganic particles, spray coating and rotor dampening are more preferable because the flight speed of the discharged droplets is high.
[0083] The weight of the fluorine-containing polymer particles formed by the above coating method and drying is 0.2 to 1.5 g / m 2 By setting the amount of the fluorine-containing polymer particles in the above range, a porous layer having excellent adhesiveness can be formed without impairing the air permeability. The upper limit of the basis weight of the fluorine-containing polymer particles is preferably 1.2 g / m2 less than 1.0 g / m 2 It would be better if it was less than this.
[0084] The air resistance of the porous film formed by the above coating method and drying is preferably 150 sec / 100 cc or less, more preferably 140 sec / 100 cc or less. By setting the air resistance of the porous layer in this range, sufficient ion mobility is obtained, and deterioration of battery characteristics is suppressed, which is preferable.
[0085] The porous film of the present application can be suitably used as a battery separator film for a lithium ion secondary battery. A lithium ion secondary battery has a structure in which a battery separator film and an electrolyte are interposed between a positive electrode and a negative electrode.
[0086] The positive electrode is a current collector on which a positive electrode material consisting of an active material, a binder resin, and a conductive additive is laminated. 2 , LiNiO 2 , Li(NiCoMn)O 2 , LiMn 2 O 4 Spinel-type manganese oxides such as LiFePO 4 Examples of the binder resin include iron-based compounds such as fluorine resin, acrylic resin, and styrene-butadiene resin. Examples of the binder resin include fluorine resin, acrylic resin, and styrene-butadiene resin. Examples of the conductive assistant include carbon materials such as carbon black and graphite. Examples of the current collector include metal foil, and aluminum foil is particularly often used.
[0087] The negative electrode is a current collector on which negative electrode materials consisting of active materials and binder resins are laminated. Active materials include carbon materials such as artificial graphite, natural graphite, hard carbon, and soft carbon, lithium alloy materials such as tin and silicon, metal materials such as Li, and lithium titanate (Li 4 Ti 5 O 12) and the like. As the binder resin, fluororesin, acrylic resin, styrene-butadiene resin, and the like are used. As the current collector, a metal foil is suitable, and in particular, copper foil is often used.
[0088] The electrolyte is a place where ions move between the positive and negative electrodes in the secondary battery, and is composed of an electrolyte dissolved in an organic solvent. 6 , LiBF 4 , LiClO 4 and LiTFSI, but from the viewpoint of solubility in organic solvents and ionic conductivity, LiPF 6 Examples of the organic solvent include ethylene carbonate, propylene carbonate, fluoroethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate, and two or more of these organic solvents may be mixed and used. EXAMPLES
[0089] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the following description, "%" and "parts" represent "% by mass" and "parts by mass". The measurement methods used in the examples are shown below.
[0090] (1) Volume average particle size, number average particle size and particle size distribution of polymer particles The polymer particles were dispersed in water to a solid content of 0.2% by mass, and the dispersion was measured by dynamic light scattering using ELSZ (manufactured by Otsuka Electronics Co., Ltd.), analyzed by the Marquardt Method, and the volume average particle size and number average particle size were calculated. The particle size distribution (volume average particle size / number average particle size) was also calculated from the obtained values.
[0091] (2) Glass transition temperature of polymer particles The glass transition temperature (Tg) of the polymer particles was determined by measuring the intersection point between a straight line extending from the low-temperature baseline during the second heating cycle after the first heating and cooling to the high-temperature side and a tangent drawn at the point where the gradient of the curve of the stepwise change in the glass transition is maximum, using differential scanning calorimetry (DSC) in accordance with the provisions of "JIS K7121:2012 Measurement method for transition temperature of plastics."
[0092] (3) Swelling degree S of a particle film made of polymer particles in a solvent The particle film made of polymer particles was prepared by molding the polymer particles into a sheet having a thickness of about 1 to 2 mm by hot pressing. The particle film made of polymer particles was immersed in a solvent as a sample, and the swelling degree was calculated from the weight increase due to the swelling of the sample.
[0093] A particle film made of polymer particles was cut into a few mm square and 3 to 6 pieces (about 0.15 g) of sample pieces were weighed and the weight was W D Thereafter, the sample piece was immersed in about 3 mL of a mixed solvent of ethylene carbonate:ethyl methyl carbonate=3:7 (volume ratio) and left to stand at room temperature for about 20 days.
[0094] The test pieces are removed from the solvent, the test solvent adhering to the surface of each test piece is wiped off with a wipe, etc., and the weight of the test piece W W was weighed.
[0095] The swelling degree S was calculated from the following formula.
[0096]
number
[0097] Here, V D and V W are the volumes of the sample piece before and after immersion in the solvent, respectively, and were calculated using the following formula:
[0098]
number
[0099] ρ S is the density of the polymer that constitutes the sample piece, ρ L is the density of the solvent used in the test.
[0100] If the swelling degree S was 1.0 or more and less than 2.5, it was rated as "excellent," if it was 2.5 or more and less than 3.0, it was rated as "good," if it was 3.0 or more and less than 4.0, it was rated as "slightly poor," and if it was 4.0 or more (including cases where the particles dissolved in the solvent and the particle size could not be measured), it was rated as "poor." When the swelling degree S was less than 3.0, it was judged to have good swelling inhibition properties.
[0101] (4) Adhesiveness A porous film having a width of 17 mm and a length of 110 mm is obtained for evaluating adhesiveness.
[0102] An electrode having a width of 15 mm and a length of 100 mm was obtained using graphite as an active material, vinylidene fluoride resin as a binder resin, and carbon black as a conductive assistant. This electrode is used as the negative electrode of a lithium ion secondary battery. The following evaluation sample preparation and sample measurement are performed in a dry room with a dew point of 50°C or less in order to improve measurement accuracy. The porous film and the electrode are placed in an aluminum laminate film folded in half so that the ends of the electrode and the porous film in the longitudinal direction are aligned and overlapped, and the active material of the electrode and the porous membrane of the porous film are in contact with each other. 250 μl of electrolyte is soaked into the porous film side of the test piece, and then the three pieces are closed to form a bag, and the remaining side of the aluminum laminate film is closed using a vacuum sealer to vacuum seal the test piece. This was stored under stationary conditions for 60 minutes in an environment of about 25°C. Next, a heat press was performed under conditions of 80°C, 3 MPa, and 120 seconds to bond the electrode and the porous film to prepare a test piece. After that, the test piece was taken out of the aluminum laminate film, and the end of the test piece was peeled off by about 10 mm. The electrode was held and fixed to the upper chuck of Imada Co., Ltd.'s force gauge ZP5N and MX2-500N (product name) and the separator was held and fixed to the lower chuck, and a peel test was performed at a peel speed of 300 mm / min using a peel method with a peel accuracy of 180 degrees, and the peel strength was examined. At this time, the average value of the peel strength in the peel test for a length of 60 mm performed under the above conditions was taken as the peel strength. The adhesion with the electrode was evaluated in the following three stages. Here, the electrolyte was a mixed solvent of ethylene carbonate: ethyl methyl carbonate = 3: 7 (volume ratio), and LiPF 6 The adhesive was dissolved to a concentration of 1 mol / L. If the peel strength was 1.0 N / m or more, it was determined that the adhesive had sufficient adhesion, if the peel strength was 0.5 N / m or more but less than 1.0 N / m, it was determined that the adhesive had adhesion, and if the peel strength was less than 0.5 N / m, it was determined that the adhesive had no adhesion. The "adhesion" in Table 2 shows these measured values and the criteria for evaluation.
[0103] (Judgment criteria) A :1.0N / m or more B: 0.5N / m or more, less than 1.0N / m C: Less than 0.5N / m.
[0104] (5) Content of structural units derived from (meth)acrylic acid ester monomers (A) and (B) in the structural units constituting the polymer The content of the structural units derived from the (meth)acrylic acid ester monomers (A) and (B) in the structural units constituting the polymer can be measured by the following method.
[0105] (a) For example, when measuring from a coated film, first, the coating layer is detached from the support using an organic solvent such as water or alcohol, and the water and the organic solvent such as alcohol are thoroughly dried to obtain a coating layer. An organic solvent that dissolves the organic resin components is added to the obtained coating layer to dissolve only the organic resin components. Next, the organic solvent is dried from the solution in which the organic resin components are dissolved, and only the organic resin components are extracted.
[0106] (b) Using the obtained organic resin component, the presence or absence of the (meth)acrylic acid ester monomer (A) is confirmed by pyrolysis gas chromatography / mass spectrometry (pyrolysis gas chromatography (GC) / mass spectrometry (MS)).
[0107] (c) Nuclear magnetic resonance method ( 13 The organic resin component and an appropriate amount of solvent (deuterated chloroform) are filled into a solid-state NMR sample tube, and after leaving it to stand overnight, the dipolar-decoupling (DD) / magic-angle-spinning (MAS) method is used to measure the NMR peaks. 13 The content of structural units derived from the (meth)acrylic acid ester monomers (A) and (B) in the structural units constituting the polymer is determined by C-NMR measurement.
[0108] (6) Air resistance of porous film One randomly selected spot was selected from each of three 100 mm x 100 mm porous film samples, and measured in accordance with JIS P 8117 (2009) using an Oken air permeability measuring device (EG01-5-1MR, manufactured by Asahi Seiko Co., Ltd.). The average value was calculated as the air permeability resistance (sec / 100 cm 3 ) was decided.
[0109] (7) Thickness of the porous layer The thickness of a 100 mm x 100 mm porous film sample was determined by averaging five measured values using a contact thickness meter ("Litematic" (registered trademark) series 318 manufactured by Mitutoyo Corporation). A superhard spherical probe of φ9.5 mm was used and the measurement was performed under a load of 0.01 N. Furthermore, the thickness of the porous layer was measured by washing the porous film with the same solvent as that contained in the paint containing inorganic particles and the paint containing fluorine-containing polymer particles, removing the porous layer, and measuring the porous substrate with the contact thickness meter, and the thickness was calculated according to the following formula.
[0110] Thickness of porous layer (μm) = thickness of porous film (μm) - thickness of porous substrate (μm).
[0111] (8) Weight of polymer particles Only the coating liquid containing inorganic particles was applied to a polyethylene porous substrate, and a 50 mm x 50 mm square was cut out from the dried porous film sample. The mass (g) was measured at room temperature of 25°C, and the sample was cut into 1 m 2 The basis weight of the polyethylene porous substrate and the layer containing inorganic particles is calculated by converting it into the weight per unit area. Next, the coating liquid containing inorganic particles and the coating liquid containing fluorine-containing polymer particles are applied to the polyethylene porous substrate, and the porous film sample is dried and cut into a square of 50 mm x 50 mm. The mass (g) at room temperature of 25°C is measured, and the mass per unit area is calculated by converting the basis weight of the polyethylene porous substrate and the layer containing inorganic particles into the weight per unit area. 2 The basis weights of the polyethylene porous substrate, the layer containing inorganic particles, and the layer containing fluorine-containing polymer particles were calculated in terms of basis weight per unit area. The basis weight of the polymer particles was calculated using the following formula.
[0112] Weight of polymer particles (g / m 2) = basis weight (g / m2) of the polyethylene porous substrate, the layer containing inorganic particles, and the layer containing fluorine-containing polymer particles 2 )-Polyethylene porous substrate and inorganic particle-containing layer basis weight (g / m 2 ) (9) Adhesion suppression property A dispersion of polymer particles diluted with water to a concentration of 0.01% by mass was dropped onto aluminum foil, and a sample was prepared by drying at room temperature and a sample was prepared by drying at 60°C. Then, using a scanning electron microscope (Hitachi, SU8220), two fields of view were observed at an acceleration voltage of 2.0 kV and 50,000 times magnification. The number average particle diameter of 100 particles was measured at random. The change rate of the number average particle diameter of the sample dried at 60°C relative to the number average particle diameter of the sample dried at room temperature [change rate = number average particle diameter of the sample dried at 60°C / number average particle diameter of the sample dried at room temperature] was analyzed. If the change rate is less than 1.5, it is evaluated as "excellent", if the change rate is 1.5 or more and less than 2.0, it is evaluated as "good", if the change rate is 2.0 or more and less than 3.0, it is evaluated as "slightly poor", if the change rate is 3.0 or more, it is evaluated as "poor", and if the change rate is less than 2.0, it is judged to have good adhesion inhibition. The "adhesion suppression property" shown in Table 2 is the value of the above-mentioned rate of change.
[0113] (10) Blocking resistance Two pieces of 50 mm wide x 50 mm long were cut out and placed so that the porous films were in contact with each other to obtain a porous film for evaluation of blocking resistance. This was sandwiched between two PET films of 60 mm wide x 60 mm long and 100 μm thick to create a test piece. This test piece was pressed under a condition of 0.5 MPa, and heat-treated for 48 hours at a temperature of 60°C and a relative humidity of 75% using a thermohygrostat (Espec Corporation, LHU-113). After that, the test piece was taken out, and auxiliary paper (50 mm wide x 50 mm long) was attached to each end of the two overlapping porous films. The two auxiliary papers were held and fixed in the upper and lower chucks of Imada Co., Ltd.'s force gauges ZP5N and MX2-500N (product name), and a peel test was performed at a peel speed of 300 mm / min using a peel method with a peel accuracy of 180 degrees, and the peel strength was examined. At this time, the average value of the peel strength in the peel test over a length of 30 mm conducted under the above conditions was taken as the peel strength. Blocking resistance was evaluated according to the following three stages. If the peel strength was 0.5 N / m or less, it was deemed to have sufficient blocking resistance, if the peel strength was 0.5 N / m or more but less than 1.0 N / m, it was deemed to have blocking resistance, and if the peel strength was 1.0 N / m or more, it was deemed not to have blocking resistance. The "blocking resistance" listed in Table 2 shows these measured values and the evaluation criteria.
[0114] (Judgment criteria) A: 0.5N / m or less B: 0.5N / m or more, less than 1.0N / m C:1.0N / m or more (11) Occupancy rate of fluorine-containing polymer particles on the surface of the porous layer The surface SEM-EDX images were measured by image processing, and the details are described below.
[0115] <Porous layer surface SEM-EDX measurement> A small piece of 0.5 cm×0.5 cm was cut out from the porous film, and the separator surface was subjected to SEM-EDX measurement at five different locations under atmospheric exposure under the conditions shown below.
[0116] <SEM-EDX measurement conditions> Measurement equipment: SEM: Hitachi High-Technologies Field Emission Scanning Electron Microscope FE-SEM S-4800, EDX: Bruker AXS QUANTAX FLAT QUAD System Xflash 5060FQ SEM observation accelerating voltage: 1.5 kV EDX observation accelerating voltage: 3.5 kV Emission current: 10μA ·Measurement magnification: 300x Electron beam incident angle: 0° ·X-ray extraction angle: 35°~ Dead time: 1% Mapping element: Al Measurement resolution: 600 x 450 pixels ·Measurement time: 600sec. Brightness: Adjusts brightness and contrast so that there are no pixels that reach maximum brightness and the average brightness is within the range of 40% to 60%. Image Processing The SEM-EDX image obtained above was read into the image analysis software HALCON (Ver.13.0, MVtec), and contour emphasis (differential filter (emphasize, low-pass mask width: 3 / low-pass mask height: 3 / contrast emphasis strength: 0.3), edge emphasis filter (shock_filter, time step length: 0.5 / number of repetitions: 1 / edge detection type: canny / edge detection smoothing: 1) was performed. The images were then binarized.
[0117] The differential filter "emphasize" used for contour emphasis and the edge emphasis filter "shock_filter" are image processing filters included in HALCON.
[0118] For binarization, the lower and upper thresholds for the gray value were set to 180 and 255, respectively, and the areas above 180 were determined to be areas where the fluorine-containing polymer existed. Furthermore, the gray value of the areas where the fluorine-containing polymer existed was replaced with 255 and the gray value of other areas with 0, and consecutive pixels with a gray value of 255 were linked to each other. The areas of the areas where the fluorine-containing polymer existed were extracted and integrated, and then divided by the total number of pixels in the original image to calculate the occupancy rate of the fluorine-containing polymer in the SEM-EDX image.
[0119] The above processing was performed on all five SEM-EDX images obtained, and five occupancies of the fluorine-containing polymer were obtained for each image. The average of these was taken as the occupancy rate of the fluorine-containing polymer relative to the entire surface of the porous layer.
[0120] (12) Occupancy rate of fluorine-containing polymer particles in the cross section of the porous layer A cross section of a sample was cut out from the porous film using a microtome, and the cross section was subjected to SEM-EDX measurement at five different locations in an exposed atmosphere under the conditions shown below.
[0121] <SEM-EDX measurement conditions> Measurement equipment: SEM: Hitachi High-Technologies Field Emission Scanning Electron Microscope FE-SEM S-4800, EDX: Bruker AXS QUANTAX FLAT QUAD System Xflash 5060FQ SEM observation accelerating voltage: 1.5 kV EDX observation accelerating voltage: 3.5 kV Emission current: 10μA ·Measurement magnification: 10000x Electron beam incident angle: 0° ·X-ray extraction angle: 35°~ Dead time: 1% Mapping element: Al Measurement resolution: 600 x 450 pixels ·Measurement time: 600sec. Brightness: Adjusts brightness and contrast so that there are no pixels that reach maximum brightness and the average brightness is within the range of 40% to 60%. Image Processing The cross-sectional SEM-EDX image obtained above was read into the image analysis software HALCON (Ver.13.0, MVtec), and contour emphasis (differential filter (emphasize, low-pass mask width: 3 / low-pass mask height: 3 / contrast emphasis strength: 0.3), edge emphasis filter (shock_filter, time step length: 0.5 / number of repetitions: 1 / edge detection type: canny / edge detection smoothing: 1) was performed. The images were then binarized.
[0122] The differential filter "emphasize" used for contour emphasis and the edge emphasis filter "shock_filter" are image processing filters included in HALCON.
[0123] For binarization, the lower and upper thresholds for the gray value were set to 180 and 255, respectively, and the areas above 180 were determined to be areas where fluorine-containing polymers were present. Furthermore, the gray values of the areas where the fluorine-containing polymers were present were replaced with 255 and the gray values of other areas were replaced with 0, and consecutive pixels with a gray value of 255 were linked to extract the areas where the fluorine-containing polymers were present. The obtained areas where the fluorine-containing polymers were present were superimposed on the cross-sectional SEM image, and the fluorine-containing polymers were mapped on the cross-sectional SEM image.
[0124] The cross-sectional SEM image onto which the fluorine-containing polymer region was mapped was divided into 50 in the row direction, and the fluorine-containing polymer area in each divided row region was integrated to calculate the fluorine-containing polymer content in each divided cross-sectional SEM image region in the row direction.
[0125] The row region representing the bottom surface of the porous layer, which is on the porous substrate side, is determined from a cross-sectional SEM image on which the fluorine-containing polymer is mapped, and the row region representing the top surface of the porous layer is determined as the highest row in which the fluorine-containing polymer content is less than 30% in each divided row region divided into 50 columns in the row direction.
[0126] The row region from the bottom surface to the top surface of the obtained porous layer was divided into three, and the region in contact with the porous substrate was determined as region A, the region in contact with region A as region B, and the region in contact with region B as region C. The fluorine-containing polymer area in each region was calculated and divided by the total number of pixels in the three regions to calculate the fluorine-containing polymer content in each region.
[0127] The above processing was carried out for all the obtained SEM-EDX images and five SEM images, and the average values thereof were taken as the content of the fluorine-containing polymer in each of the regions A, B, and C.
[0128] (13) Indentation depth rate The measurement was performed by a nanoindentation method in accordance with ISO14577. The measurement will be explained using the schematic diagram of FIG. 1. First, both ends in the MD direction were fixed with the gripping parts 2 and 3 so that the porous film 1 would not wrinkle. Next, the screw 5 was turned so that the length of the porous film 1 from the gripping parts 2 to the gripping parts 3 was stretched by 1%, and the porous film 1 was fixed to a mirror-finished SUS pedestal 4 with a curvature radius of 300 mm. Next, a Berkovich-type diamond indenter 6 was brought into contact with the porous film 1 fixed to the SUS pedestal 4, and the load was increased at a loading rate of 1 mN / min for 30 seconds. After the load reached 0.5 mN (FIG. 2(A)), the load was held at 0.5 mN for 60 seconds (FIG. 2(B)), and then the load was removed to 0 mN at an unloading rate of 1 mN / min (FIG. 2(C)). At this time, the indentation depth of the Berkovich type diamond indenter 6 pressed into the porous film 1 was measured using an Anton Paar UNHT3. Indentation tests were performed at 5 points at 50 μm intervals in the TD direction and 5 points at 50 μm intervals in the MD direction from there, for a total of 25 points, and Pd(0) was calculated from the average curve of the 25 measurements. h(0) was calculated from the obtained Pd(0) and the thickness of the porous layer. h(0) = Pd(0) / d × 100 Pd(0): Indentation depth (μm) when pressed for 30 seconds at a loading rate of 1 mN / min and then unloaded to 0.5 mN d: Initial thickness of the porous layer (μm) The grade was A (good): h(0) was 20 or more, and B (unacceptable): h(0) was 5 or more and less than 20.
[0129] (14)Heat shrinkage rate at 150℃ The amount required for measurement was cut out from the porous film roll, and after leaving it for 24 hours without load, it was cut into a 95mm x 95mm square, a 50mm cross was drawn from the center so that it was parallel to each side of the square, and the dimensions of the two sides of the 50mm cross were measured using a glass scale (measurement accuracy 0.1mm) (α), and the sample was sandwiched between clean paper (Sakurai Co., Ltd., NEWSTACLEAN) and heat treated at 150°C for 1 hour using a low-temperature incubator (Yamato Scientific Co., Ltd., DKN602). Note that the load and stress applied to the test sample piece during the heat treatment were nothing other than a slight load caused by overlapping with clean paper. After removing the evaluation sample from the low-temperature incubator and cooling it, the dimensions of the two sides of the 50mm cross after heat treatment were measured using a glass scale (β), and the thermal shrinkage was calculated using the following formula (8), and the average value of the three samples was taken as the thermal shrinkage at 150°C. 150℃ heat shrinkage rate (%)=(α-β) / α×100...(8) The rating was A (good): the heat shrinkage rate at 150°C was less than 5%, B (passable): the heat shrinkage rate at 150°C was 5% or more but less than 10%, C (unacceptable): the heat shrinkage rate at 150°C was 10% or more.
[0130] (15) Cycle characteristics (Battery construction) The positive electrode sheet contains Li(Ni 5 / 10 Mn 2 / 10 Co 3 / 10 )O 2A positive electrode slurry was prepared by dispersing 92 parts by mass of the above, 2.5 parts by mass each of acetylene black and graphite as a positive electrode conductive assistant, and 3 parts by mass of polyvinylidene fluoride as a positive electrode binder in N-methyl-2-pyrrolidone using a planetary mixer, and then coating the resulting slurry on aluminum foil, drying, and rolling to prepare a positive electrode (coating weight: 9.5 mg / cm). 2 ).
[0131] This positive electrode sheet was cut to a size of 40 mm x 40 mm. At this time, the current collecting tab adhesive part without the active material layer was cut out to a size of 5 mm x 5 mm outside the active material surface. An aluminum tab with a width of 5 mm and a thickness of 0.1 mm was ultrasonically welded to the tab adhesive part.
[0132] The negative electrode sheet was prepared by dispersing 98 parts by mass of natural graphite as the negative electrode active material, 1 part by mass of carboxymethyl cellulose as a thickener, and 1 part by mass of a styrene-butadiene copolymer as a negative electrode binder in water using a planetary mixer, applying the resulting negative electrode slurry onto copper foil, drying, and rolling (coating weight: 5.5 mg / cm). 2 ).
[0133] The negative electrode sheet was cut to a size of 45 mm x 45 mm. At this time, the current collecting tab adhesive part without the active material layer was cut out to a size of 5 mm x 5 mm outside the active material surface. A copper tab of the same size as the positive electrode tab was ultrasonically welded to the tab adhesive part.
[0134] Next, the porous film was cut to 55 mm x 55 mm, and the positive and negative electrodes were placed on both sides of the porous film with the active material layer separating the porous film, and the positive electrode coating was arranged so that all the positive electrode coating parts faced the negative electrode coating parts to obtain an electrode group. The positive electrode, negative electrode, and porous film were sandwiched between a single 90 mm x 200 mm aluminum laminate film, the long side of the aluminum laminate film was folded, and the two long sides of the aluminum laminate film were heat-sealed to form a bag shape.
[0135] Diethyl carbonate: Diethyl carbonate = 1:1 (volume ratio) mixed solvent, LiPF as solute 6The electrolyte solution was prepared by dissolving the above in an aluminum laminate film so as to have a concentration of 1 mol / L. 1.5 g of the electrolyte solution was poured into a bag-shaped aluminum laminate film, and the short sides of the aluminum laminate film were heat-sealed while the electrolyte solution was being impregnated under reduced pressure to prepare a laminated battery.
[0136] The discharge rate characteristics of the prepared laminated battery were tested according to the following procedure, and evaluated in terms of the discharge capacity retention rate.
[0137] The charging conditions were a constant current charge of 3C and 4.25V, and the discharging conditions were a constant current discharge of 3C and 2.7V, which were repeated 500 times.
[0138] <Calculation of Discharge Capacity Retention Rate> The discharge capacity retention rate was calculated by (discharge capacity after 500 cycles) / (first discharge capacity) x 100. Five laminated batteries were produced, and the average value was taken as the discharge capacity retention rate.
[0139] The ratings were A (good): discharge capacity retention rate of 80% or more, B (passable): discharge capacity retention rate of 60% or more but less than 80%, and C (unacceptable): discharge capacity retention rate of less than 60%.
[0140] Example 1 The coating liquid containing inorganic particles is prepared by preparing 0.5 parts by weight (active ingredient) of a polyacrylic acid-based dispersant ("Aron" (registered trademark) A-6114, manufactured by Toa Gosei Co., Ltd.) for 100 parts by weight of barium sulfate (average particle size = 1.2 μm) and adding it to water. Next, the entire amount of barium sulfate is added while stirring using a Three-One Motor (manufactured by Toki Sangyo Co., Ltd.) equipped with a disperser-type blade. Next, the mixture is stirred at 1000 rpm for 60 minutes to obtain a mixed liquid with a solid content of 60% by weight.
[0141] The resulting mixture was milled once using a bead mill disperser (Picomiru PCM-LR, manufactured by Asada Iron Works Co., Ltd.) and zirconia beads with a bead diameter of 0.5 mm (Toray Ceram φ0.5 mm, manufactured by Toray Industries, Inc.) under conditions of a bead filling rate of 55 volume%, a peripheral speed of 6 m / sec, and a flow rate of 16 kg / hr to obtain a master batch liquid.
[0142] To the obtained master batch liquid, 3.5 parts by weight (active ingredient) of acrylic emulsion (Polysol AP-4735, manufactured by Showa Denko K.K.) was added as a binder, and water was then added. Next, 0.5 parts by weight of a wetting agent (SN Wet 366, manufactured by San Nopco Ltd.) was added, and the mixture was stirred at 500 rpm for 10 minutes with a Three-One Motor (manufactured by Toki Sangyo Co., Ltd.) equipped with a dispersing blade to produce a coating liquid containing inorganic particles with a solid content of 55% by weight.
[0143] A coating liquid containing fluorine-containing polymer particles was prepared by the following procedure. 120 parts of ion-exchanged water and 1 part of Adeka Reasorb SR-1025 (emulsifier manufactured by Adeka Corporation) were charged into a reactor, and stirring was started. The reactor was placed under a nitrogen atmosphere, and 0.4 parts of 2,2'-azobis(2-(2-imidazolin-2-yl)propane) (manufactured by Wako Pure Chemical Industries, Ltd.) was added. A mixture consisting of 26 parts of 2,2,2-trifluoroethyl methacrylate (3FMA), 41 parts of cyclohexyl acrylate (CHA), 30 parts of isobornyl methacrylate (IBOMA), 2 parts of 4-hydroxybutyl acrylate (4HBA), 1 part of polyalkylene glycol dimethacrylate (Blenmer (registered trademark) PDE-600 (manufactured by NOF Corp.)), 9 parts of Adeka Reasorb SR-1025 (emulsifier manufactured by Adeka Corp.) and 115 parts of ion-exchanged water was continuously dropped at 60 ° C. for 2 hours, and after the end of the dropping, polymerization was carried out at 60 ° C. for 4 hours to obtain polymer particles. The polymer particles were mixed with pure water to be 3 mass %, and dispersed with a stirrer to produce a coating liquid containing fluorine-containing polymer particles.
[0144] A coating solution containing inorganic particles was applied to one side of a polyethylene porous substrate (thickness 9 μm, air permeability 100 sec / 100 cc) by chamber gravure and dried in a hot air oven at 50°C until the solvent evaporated, obtaining a layer containing inorganic particles. A coating solution containing two fluorine-containing polymer particles was sprayed onto this layer containing inorganic particles using an external mixing two-fluid spray nozzle (nozzle diameter: 0.1 mm) at an air pressure of 0.04 MPa, resulting in a polymer particle basis weight of 1.0 g / m 2Thereafter, the mixture was dried in a hot air oven at 50° C. until the pure water evaporated, thereby obtaining a porous film having a porous layer formed thereon.
[0145] The evaluation results of the obtained polymer particles and porous film are shown in Tables 1 and 2.
[0146] (Examples 2 to 7, Comparative Examples 1 to 4) A porous film was obtained in the same manner as in Example 1, except for the changes shown in Table 1. The obtained evaluation results and the like are as shown in Table 2.
[0147] [Table 1]
[0148] [Table 2]
[0149] The composition ratio of the monomers shown in Table 1 is the ratio of each component when the total amount of the monomer components is 100 parts by mass. The abbreviations of the components in Table 1 have the following meanings. 3FMA: 2,2,2-trifluoroethyl methacrylate (in formula (1), R 1 :-CH 3 , R 2 :-CH 2 CF 3 , a is the degree of polymerization) CHA: cyclohexyl acrylate (wherein R 1 :-H, R 3 : cyclohexyl group, b is the degree of polymerization) IBOMA: isobornyl methacrylate (R 1 :-CH 3 , R 2 : isobornyl group, b is the degree of polymerization) IBOA: isobornyl acrylate (wherein R 1 :-H, R 2 : isobornyl group, b is the degree of polymerization) 4HBA: 4-Hydroxybutyl acrylate MMA: Methyl methacrylate
[0150] [ka]
[0151] [ka] [Explanation of symbols]
[0152] 1: Separator 2, 3: Grip part 4: SUS base 5: Screw thread 6: Berkovich type diamond indenter
Claims
1. A porous substrate and a porous layer containing inorganic particles and fluorine-containing polymer particles on at least one surface of the porous substrate, the fluorine-containing polymer particles contain 5% by mass or more and less than 30% by mass of a structural unit (X) derived from a fluorine-containing (meth)acrylic acid ester monomer (A) in 100% by mass of the monomer, and a structural unit (Y-1) derived from a (meth)acrylic acid ester monomer (B), and a structural unit (Y-2) derived from a (meth)acrylic acid ester monomer (B), the structural unit (X) derived from the fluorine-containing (meth)acrylic acid ester monomer (A) being represented by the following general formula (1), and the structural units (Y-1) and (Y-2) derived from the (meth)acrylic acid ester monomer (B) being represented by the following general formula (2). A porous film. 【Chemistry 1】 【Chemistry 2】 (In formulas (1) and (2), R1 represents a hydrogen atom or a methyl group, R2 represents a fluorine-containing hydrocarbon group having 1 to 10 carbon atoms, R3 represents a group selected from the group consisting of alicyclic hydrocarbon groups having 5 to 10 carbon atoms, and a and b represent the degree of polymerization.)
2. 2. The porous film according to claim 1, wherein the occupancy rate of the fluorine-containing polymer particles on the surface of the porous layer is 60% or more and less than 95%, and the porous layer is divided into three equal parts in the thickness direction, and a region in contact with the porous substrate is designated as region A, a region in contact with region A is designated as region B, and a region in contact with region B is designated as region C, the porous film satisfies the following (a) to (c): (a) The content α of the fluorine-containing polymer particles in the region C is 60% or more and 90% or less of the total fluorine-containing polymer particle content in the porous film. (b) the content β of the fluorine-containing polymer particles in the region B is 10% or more and 40% or less of the total fluorine-containing polymer particle content in the porous film. (c) The content γ of the fluorine-containing polymer particles in the region A is 10% or less of the total fluorine-containing polymer particle content in the porous film.
3. 3. The porous film according to claim 1 or 2, wherein the indentation depth ratio h(0) is 20 or more and 30 or less when the indentation is performed for 30 seconds at a loading rate of 1 mN / min using a nanoindentation method using a Berkovich diamond indenter and then unloaded to 0.5 mN, as shown in the following formula. h(0)=Pd(0) / d×100 Pd(0): Indentation depth (μm) when pressed at a loading rate of 1 mN / min for 30 seconds and then unloaded to 0.5 mN d: initial thickness of the porous layer (μm)
4. The structural unit (Y-1) derived from the (meth)acrylic acid ester monomer (B) includes at least one of cyclohexyl acrylate, cyclohexyl methacrylate, t-butyl cyclohexyl acrylate, and 3,3,5-trimethylcyclohexyl acrylate, and the structural unit (Y-2) derived from the (meth)acrylic acid ester monomer (B) includes at least one of isobornyl acrylate, isobornyl methacrylate, dicyclopentanyl acrylate, and dicyclopentanyl methacrylate. The porous film according to claim 1 or 2.
5. The fluorine-containing polymer particles contain a total of 60% by mass or more and 90% by mass or less of the structural unit (Y-1) derived from the (meth)acrylic acid ester monomer (B) and the structural unit (Y-2) derived from the (meth)acrylic acid ester monomer (B). The porous film according to claim 1 or 2.
6. The weight of the fluorine-containing polymer particles is 0.01 g / m 2 1.00g / m or more 2 The porous film according to claim 1 or 2, wherein:
7. 3. The porous film according to claim 1, wherein the glass transition temperature (Tg) of the fluorine-containing polymer particles is 55 to 100° C.
8. 3. The porous film according to claim 1, wherein the fluorine-containing polymer particles have a volume average particle size of 10 nm or more and 500 nm or less.
9. 3. The porous film according to claim 1, wherein the thickness of the porous layer is from 0.10 μm to 5.0 μm.
Citation Information
Patent Citations
Sliding resin material
JP1985051731A
Name flag detachment preventing apparatus in carp streamer pole
JP1986005816A
Separator, lithium battery including the same, method for manufacturing the separator, and method for manufacturing the lithium battery
JP6659081B2
Separator and electrochemical element including same
JP7094968B2
Cited By
Electrolyte-resistant acrylate pressure-sensitive adhesive and preparation method thereof
CN120843020A