Particle primarily composed of polyethylene and / or polyethylene copolymer
Polyethylene particles with controlled diameter and melt flow rate, combined with specific structural units, address the clogging and penetration issues of conventional particles, achieving uniform thin film coating and improved shutdown performance in battery separator films.
Patent Information
- Application Number
- JP2023174912
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2023-10-10
- Publication Date
- 2024-10-07
AI Technical Summary
Conventional polyethylene particles used in battery separator films have large diameters and high melt viscosity, leading to clogging of surface openings and incomplete pore closure during thin film coating, compromising shutdown performance.
Development of polyethylene particles with a number average particle diameter of 0.5 μm to 5.0 μm, melt flow rate of 0.3 g/10 min to 2000 g/10 min, and inclusion of structural units derived from α,β-unsaturated carboxylic acid and α,β-unsaturated dicarboxylic acid anhydride, ensuring uniform thin film formation and effective pore closure.
The particles enable uniform thin film coating on porous substrates without pores, enhancing shutdown performance in battery separator films by preventing particle penetration and ensuring complete pore closure.
Smart Images

Figure 2024137627000001 
Figure 2024137627000002 
Figure 2024137627000003
Abstract
Description
[Technical field]
[0001] The present invention relates to particles based on polyethylene and / or polyethylene copolymers. [Background technology]
[0002] Particles mainly composed of polyethylene are used as coating agents, adhesives, resin additives, etc., taking advantage of their thermal properties and excellent water resistance and chemical resistance. In coating applications, the particles are often mixed with a solvent and used as a dispersion liquid, and are used as coating materials for a wide variety of substrates such as metals and resin films (see, for example, Patent Documents 1 and 2). In recent years, as a safety device for secondary batteries, a shutdown property has been considered, in which when the battery generates abnormal heat, a part of the separator film is melted stepwise at a temperature lower than the temperature at which the entire separator film melts, and the pores of the separator film are blocked and the current is cut off before the temperature reaches the temperature range at which thermal runaway begins. A technology has been proposed in which the shutdown property is expressed by coating the surface of a porous substrate with organic particles mainly composed of polyolefin such as polyethylene (see, for example, Patent Document 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2004-059869 A [Patent Document 2] JP 2004-051661 A [Patent Document 3] Japanese Patent Application Publication No. 9-219185 Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, the demand for thinner battery separator films has accelerated, and in order to make the coating layer of the battery separator film thinner, it is necessary to reduce the diameter of the particles contained in the coating material. However, polyethylene particle dispersions that meet the above particle size generally contain fine particles. Therefore, there is a concern that the surface openings are easily clogged when applied to porous films such as battery separator films. In addition, conventional particles have a strong tendency to penetrate into the porous structure when heated and melted, and there is a concern that the pores of the separator cannot be completely blocked during thin film coating, making it difficult to exhibit shutdown performance. Therefore, the present invention provides polyethylene particles with a small and uniform particle size and a high melt viscosity. [Means for solving the problem]
[0005] The present invention has the following configuration. (1) Particles mainly composed of polyethylene and / or polyethylene copolymers and having the following characteristics (I) to (II): (I) The number average particle diameter (D50) of the particles is 0.5 μm or more and 5.0 μm or less. (II) The polymer constituting the particles has a melt flow rate of 0.3 g / 10 min or more and 2000 g / 10 min or less at 190° C. and a load of 2160 g. (2) Particles according to (1), in which the polymer constituting the particles contains a structural unit (X) derived from an α,β-unsaturated carboxylic acid (A) and / or a structural unit (Y) derived from an anhydride of an α,β-unsaturated dicarboxylic acid (B), and the total content thereof is 1 mass % or more in 100 mass % of the structural units of the polymer constituting the particles. (3) Particles according to (1), in which the polymer constituting the particles contains a structural unit (X) derived from an α,β-unsaturated carboxylic acid (A) and / or a structural unit (Y) derived from an anhydride of an α,β-unsaturated dicarboxylic acid (B), and the total content thereof is 5% by mass or more and less than 30% by mass in 100% by mass of the structural units of the polymer constituting the particles. (4) The particles according to any one of (1) to (3), having a melting point of 90° C. or higher and 130° C. or lower. (5) Particles according to any one of (1) to (4), having a 10% particle size (D10) of 0.2 μm or more and 2.5 μm or less. (6) Particles according to any one of (1) to (5), having a number average particle size (D50) of 0.5 μm or more and 1.6 μm or less. (7) A dispersion liquid containing the particles according to any one of (1) to (6) above and a solvent. (8) The dispersion according to (7), having a solid content concentration of more than 1% by mass and not more than 50% by mass. (9) The dispersion according to (7) or (8), wherein the solvent is either water or an alcohol, or a mixture thereof. (10) The dispersion liquid according to any one of (7) to (9), wherein the solvent is water. (11) The dispersion according to any one of (7) to (10), which is used as a coating material. (12) The dispersion according to any one of (7) to (11), which is used as a coating material for film coating. (13) A film having particles according to any one of (1) to (6). (14) A battery separator film comprising particles according to any one of (1) to (6). (15) An electrode comprising the particles according to any one of (1) to (6). Effect of the Invention
[0006] The particles of the present invention have a small and uniform particle size, so that they can be coated onto various substrates to form a uniform thin film. Furthermore, when a porous film coated with the particles of the present invention is heated, a uniform thin film without holes can be formed on the porous film. Therefore, by coating the particles onto a battery separator film, the shutdown performance can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Preferred embodiments of the present invention will be described in detail below. Note that the present invention is not limited to the embodiments described below, and should be understood to include various modified examples that are implemented within the scope of the present invention.
[0008] (1) Polymers that make up the particles The particles of the present invention are mainly composed of polyethylene and / or a polyethylene copolymer. In this specification, the term "main component" refers to a component that is contained in an amount of 80% by mass or more out of the components constituting the material.
[0009] The particles of the present invention preferably contain 1 mass % or more of the structural unit (X) derived from an α,β-unsaturated carboxylic acid (A) and / or the structural unit (Y) derived from an anhydride of an α,β-unsaturated dicarboxylic acid (B).
[0010] The structural unit (X) is a structural unit derived from an α,β-unsaturated carboxylic acid (A) and is represented by the following general formula (1).
[0011] [ka]
[0012] (In formula (1), R1, R2, and R3 are hydrogen, a methyl group, or a carboxyl group. When any one of R1, R2, and R3 is a carboxyl group, the remaining two are not carboxyl groups. a represents the degree of polymerization.) In formula (1), R1, R2, and R3 are hydrogen, methyl, or carboxyl, and when any one of R1, R2, and R3 is a carboxyl, the remaining two are not carboxyl. Examples of the α,β-unsaturated carboxylic acid (A) include acrylic acid, methacrylic acid, maleic acid, fumaric acid, crotonic acid, methylmaleic acid, methylfumaric acid, and citraconic acid.
[0013] The structural unit (Y) is a structural unit derived from an anhydride of an α,β-unsaturated dicarboxylic acid (B) and is represented by the following general formula (2).
[0014] [ka]
[0015] (In formula (2), R4 and R5 are hydrogen or a methyl group, and b represents the degree of polymerization.) In the formula (2), R4 and R5 are hydrogen or a methyl group. Examples of the anhydride of an α,β-unsaturated dicarboxylic acid (B) include maleic anhydride and citraconic anhydride. The upper limit of the total content of the structural unit (X) and the structural unit (Y) is preferably less than 30% by mass, more preferably less than 25% by mass, even more preferably less than 20% by mass, and even more preferably less than 15% by mass. The lower limit of the total content of the structural unit (X) and the structural unit (Y) is more preferably 5% by mass or more, even more preferably 6% by mass or more, even more preferably 8% by mass or more, and particularly preferably 10% by mass or more. The above is commercially available and easy to use. Since the total amount of the structural unit (X) and the structural unit (Y) is less than the above upper limit, the particles are less likely to swell in the electrolyte, so that the particles applied to the battery separator film are less likely to peel off even in the battery. Since the total content of the structural unit (X) and the structural unit (Y) is more than the above lower limit, polar groups are imparted to the particles, which reduces the affinity with the battery separator film, which is a non-polar porous film, and the particles are less likely to penetrate into the battery separator film when melted, so that the particles are more likely to block the pores of the substrate when melted.
[0016] The content of the structural unit (X) derived from an α,β-unsaturated carboxylic acid (A) or the structural unit (Y) derived from an anhydride of an α,β-unsaturated dicarboxylic acid (B) in the structural units of the polymer constituting the particles can be measured using known methods. For example, when measuring from a coated film, first, the coating layer is detached from the support using an organic solvent such as water or alcohol, and the water and the organic solvent such as alcohol are thoroughly dried to obtain a coating layer. An organic solvent that dissolves the organic resin components is added to the obtained coating layer to dissolve only the organic resin components. Next, the organic solvent is dried from the solution in which the organic resin components are dissolved, and only the organic resin components are extracted. The obtained organic resin components are used to perform nuclear magnetic resonance ( 1 H-NMR, 13 It can be calculated by C-NMR), infrared absorption spectroscopy (IR), pyrolysis gas chromatography mass spectrometry (pyrolysis GC / MS), etc. In particular, after confirming the presence or absence of α,β-unsaturated carboxylic acid (A) and / or anhydride of α,β-unsaturated dicarboxylic acid (B) by pyrolysis GC / MS, the content of structural units derived from α,β-unsaturated carboxylic acid (A) and / or anhydride of α,β-unsaturated dicarboxylic acid (B) in the structural units of the polymer constituting the particles can be determined by infrared absorption spectroscopy (IR).
[0017] In order to bring the total content (X) of the structural unit (A) derived from the α,β-unsaturated carboxylic acid and the structural unit (Y) derived from the anhydride of the α,β-unsaturated dicarboxylic acid in the structural units of the polymer constituting the particles of the present invention within the above range, a commercially available copolymer of ethylene and the α,β-unsaturated carboxylic acid (A) and / or the anhydride of the α,β-unsaturated dicarboxylic acid (B) can be used as the raw material for the particles.
[0018] Commercially available copolymers of ethylene and α,β-unsaturated carboxylic acid (A) and / or α,β-unsaturated dicarboxylic anhydride (B) include, for example, Nucrel (manufactured by Mitsui Dow Polychemicals), Fusabond (manufactured by Dow Chemical Co.), Bondine (manufactured by Arkema), etc. These resins may be used alone as the raw material for the particles, or may be used in combination with other polyethylenes and / or polyethylene copolymers.
[0019] In this specification, polyethylene refers to a resin obtained by polymerizing only ethylene and a modified version of such a resin, such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, ultra-high molecular weight polyethylene, oxidized polyethylene, and polyethylene wax.
[0020] As the polyethylene, those produced by a conventionally known method or commercially available products can be used.
[0021] Specific examples of commercially available polyethylene include Evolue (manufactured by Mitsui Chemicals), Evolue H (manufactured by Mitsui Chemicals), Hi-Zex Million (manufactured by Mitsui Chemicals), LUBMER (manufactured by Mitsui Chemicals), Sanwax (manufactured by Sanyo Chemical Co., Ltd.), Sumikathene (manufactured by Sumitomo Chemical Co., Ltd.), Sumikathene-L (manufactured by Sumitomo Chemical Co., Ltd.), Sumikathene-E (manufactured by Sumitomo Chemical Co., Ltd.), Sumikathene-EP (manufactured by Sumitomo Chemical Co., Ltd.), and Excellen (manufactured by Sumitomo Chemical Co., Ltd.).
[0022] The polyethylene copolymer in this specification is a copolymer of ethylene and other monomer components, and examples of the other monomer components include α-olefins, unsaturated carboxylic acids, unsaturated dicarboxylic anhydrides, unsaturated carboxylic acid esters, vinyl acetate, etc., and it is also possible to polymerize two or more selected from these in combination. As long as the total content of the structural unit (X) and the structural unit (Y) of the particles of the present invention is within the above range, any monomer component may be included. The α-olefin is not particularly limited as long as it can be copolymerized with ethylene, and examples thereof include propylene, 1-butene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-pentene, and 1-heptene. Examples of the unsaturated carboxylic acid ester include methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, hydroxyethyl acrylate, glycidyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, and glycidyl methacrylate.
[0023] As the polyethylene copolymer, commercially available products can be used. Specific examples of commercially available polyethylene copolymers include Admer (manufactured by Mitsui Chemicals), Bondfast (manufactured by Sumitomo Chemical), Acryft (manufactured by Sumitomo Chemical), Rotader (manufactured by Arkema), and Evaflex (manufactured by Dow Mitsui Polychemicals).
[0024] In the present invention, the melt flow rate of the polymer constituting the particles at 190 ° C. and a load of 2160 g is 0.3 g / 10 min or more and 2000 g / 10 min or less. If the melt flow rate is less than 0.3 g / 10 min, the fluidity of the particles when melted is insufficient, and a thin layer without holes cannot be formed on the porous substrate. If the melt flow rate exceeds 2000 g / 10 min, the permeability into the porous substrate when the particles are melted is high, and the pores of the substrate cannot be completely blocked. The upper limit of the melt flow rate is preferably 1000 g / 10 min or less, more preferably 500 g / 10 min or less. The lower limit of the melt flow rate is preferably 10 g / 10 min or more, more preferably 50 g / 10 min or more, even more preferably 100 g / 10 min or more, and even more preferably 200 g / min or more. By setting the melt flow rate in the above range, the balance between the fluidity of the particles when melted and the permeability into the porous substrate is improved. The melt flow rate can be controlled by appropriately adjusting the molecular weight and structure of the polymer that constitutes the particles.
[0025] In the present invention, the lower limit of the melting point of the polymer constituting the particles is preferably 80°C or more, more preferably 90°C or more, and even more preferably 95°C or more. The upper limit is preferably 130°C or less, more preferably 125°C or less, even more preferably 120°C or less, and even more preferably 115°C or less. By setting the melting point of the polyethylene and / or polyethylene copolymer within the above range, it becomes easier to control the temperature at which the particles melt when heated and form a thin layer without holes. Here, the melting point refers to the temperature of the melting point peak top detected during the heating process of the second run, which is measured after melting / quenching in the first run of differential scanning calorimetry (DSC) described later.
[0026] The lower limit of the weight average molecular weight (Mw) of the polymer constituting the particles is preferably 10,000 or more, more preferably 50,000 or more, and even more preferably 100,000 or more. The upper limit is preferably 1,000,000 or less. By setting the weight average molecular weight within the above range, it becomes easier to control the permeability of the particles into the porous substrate when melted.
[0027] (2) Particle characteristics The shape of the particles of the present invention is not particularly limited, but from the viewpoint of smoothness of the coating film, a true sphere is preferable.
[0028] The number average particle diameter (D50) of the particles of the present invention is 0.5 μm or more and 5.0 μm or less. If D50 exceeds 5.0 μm, the particles cannot be coated on the porous substrate in a thin film of 5 μm or less. If D50 is less than 0.5 μm, the particles tend to aggregate. The lower limit is preferably 0.7 μm or more, more preferably 0.9 μm or more, and the upper limit is preferably 2.5 μm or less, more preferably 2.0 μm or less, even more preferably 1.6 μm or less, even more preferably 1.4 μm or less, particularly preferably 1.2 μm or less, and most preferably 1.0 μm or less. By setting the number average particle diameter within the above range, the particles can be coated more thinly and densely, improving the shutdown property of the battery separator.
[0029] In addition, the lower limit of the 10% particle size (D10) in the particle size number distribution determined by the measurement method described below is preferably 0.1 μm or more, more preferably 0.2 μm or more. The upper limit of D10 is preferably 2.5 μm or less, more preferably 1.4 μm or less, even more preferably 1.2 μm or less, even more preferably 1.0 μm or less, and particularly preferably 0.8 μm or less. By having D10 within the above range, clogging of the openings can be suppressed when the particles are applied to a porous substrate.
[0030] Particles having D50 and D10 within the above ranges can be produced, for example, by a method in which a molten resin is emulsified in a solvent. (3) Dispersion liquid One embodiment of the present invention is a dispersion containing the above particles and a solvent.
[0031] The solvent in this specification may be a dispersion medium for particles mainly composed of polyethylene and / or polyethylene copolymer, and may be a solvent in which the polymer constituting the particles does not dissolve and does not easily swell. Examples include water, alcohol, ketone, DMSO, DMF, etc., and among them, water and / or alcohols are preferred because the particles in the dispersion do not swell and adhesion between the particles can be prevented. Furthermore, when the solvent is water alone, it is most preferred because there is no volatilization of the organic solvent when this dispersion is used as a coating material, which reduces the burden on the environment. Examples of alcohol include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, and 2-butapanol. Among them, methanol, ethanol, 1-propanol, and 2-propanol have a boiling point of 100°C or less under atmospheric pressure, so that the drying time is shortened when the dispersion of the present invention is used as a coating material. The solvent may be a single solvent or a mixed solvent, and when two or more types of solvents are mixed and used, there is no limit to the mixing ratio, but the higher the proportion of water, the more preferable it is.
[0032] When the solvent of the dispersion containing the particles of the present invention is water, the lower limit of the pH of the dispersion is preferably 5.0 or more, more preferably 6.0 or more, and even more preferably 7.0 or more. The upper limit is preferably 10.0 or less, more preferably 9.0 or less, and even more preferably 8.0 or less. By having the pH of the dispersion within the above range, the dispersion stability can be improved and the corrosion of the equipment used when applying the dispersion can be prevented. There is no particular restriction on the compound used to adjust the pH of the dispersion, but ammonia water or an organic amine compound with a boiling point of 100° C. or less is preferred because it can be removed by evaporation when applying the dispersion.
[0033] The dispersion containing the particles of the present invention may contain other components such as surfactants and inorganic particles in addition to the above-mentioned particles and solvent, as long as they do not interfere with solving the problems of the present invention. In particular, it is preferable that the other components are within a range that does not affect the ion permeability of the battery when the dispersion is used as a coating material for a battery separator film.
[0034] The lower limit of the solid content concentration of the dispersion containing the particles of the present invention is preferably more than 0.1% by mass, more preferably 1% by mass or more, even more preferably 5% by mass or more, and even more preferably 10% by mass or more. By having the solid content concentration be equal to or more than the lower limit, the drying time when applying the dispersion can be shortened. The upper limit of the solid content concentration is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less. By having the solid content concentration be equal to or less than the upper limit, the fusion of particles in the dispersion can be suppressed.
[0035] The solid content concentration is calculated from the residue when 1.0 g of the dispersion is heated at 140° C. in accordance with JIS K5601-1-2:2008.
[0036] <Production of particles> The method for producing the particles of the present invention is not particularly limited, and examples thereof include emulsion polymerization, crystallization, and a method of emulsifying a molten resin in a solvent.
[0037] Examples of methods for emulsifying a molten resin in a solvent include a method in which the raw resin, a surfactant, and water are placed in a pressure-resistant container, heated and stirred to a temperature above the melting point of the raw resin to emulsify, and then cooled to a temperature below the crystallization temperature of the raw resin to solidify the particles.
[0038] When particles are obtained in a dispersion state by the above-mentioned methods, a wet cake of polyethylene and / or polyethylene copolymer particles can be obtained by a known solid-liquid separation method such as filtration, centrifugation, or heat concentration, and then dried to obtain a particle powder.
[0039] The wet cake obtained by the above method can also be subjected to a re-dispersion step. By repeating the solid-liquid separation and dispersion steps, the solvent in the dispersion can be replaced with any solvent.
[0040] <Particle Uses> The dispersion containing the particles of the present invention is preferably used as a coating material. By applying the dispersion to a substrate such as wood, metal, ceramic, carbon material, glass, or plastic to form a coating film, the surface properties can be modified. For example, it can impart rust prevention, waterproofing, and solvent resistance, and is particularly preferably used as a coating material for films. In addition, the dispersion containing the particles of the present invention can be applied in a thin film and has an excellent balance between film-forming properties during heating and suppression of penetration into the substrate layer, so it can be applied to a battery separator film to improve shutdown performance.
[0041] As an embodiment of the present invention, a film can be mentioned in which a coating layer is provided by coating a dispersion liquid containing the particles of the present invention on a porous substrate. In such a film, even if the coating layer is thin, it has good air permeability and can be suitably used as a battery separator film. In such a film, the thickness of the coating layer is preferably 5 μm or less, more preferably 3 μm or less. In addition, such a film is preferable in that the air permeability (G25) at 25° C. determined by the measurement method described below is 200 min / 100 mL or less and the air permeability (G120) after heat treatment at 120° C. is 50,000 min / 100 mL or more, since it has excellent shutdown properties. More preferably, G25 is 150 min / 100 mL or less, and even more preferably 135 min / 100 mL or less. In addition, G120 is more preferably 80,000 min / 100 mL or more, and even more preferably 90,000 min / 100 mL or more.
[0042] The particles of the present invention can be preferably used in battery materials other than battery separator films. Specifically, they can be preferably used as a binder resin for electrodes. Here, the electrode is, for example, a positive electrode or a negative electrode of a lithium ion secondary battery. That is, the electrode of the present invention is an electrode in which a material containing a binder resin is laminated on a current collector, and the binder resin has the particles of the present invention. EXAMPLES
[0043] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. First, the measurement method will be described.
[0044] (1) Number average particle diameter (D50) Particles were observed using a scanning electron microscope (FE-SEM, JSM-6301NF manufactured by JEOL Ltd.), and the arithmetic mean value of the diameters (particle sizes) of 100 particles was measured and determined as the 50% particle size (D50). Specifically, in order to determine an accurate number-average particle size that reflects the variation in particle sizes, observations were performed at a magnification such that 2 to less than 100 fine particles were captured in one image, and the particle sizes were measured. Next, the number-average particle size was calculated by determining the arithmetic mean of the particle sizes of the 100 fine particles. The magnification of such FE-SEM was 30,000 times when the particle diameter of the particle is less than 0.1 μm, 10,000 times when it is 0.1 μm or more and less than 1 μm, 5,000 times when it is 1 μm or more and less than 3 μm, 3,000 times or more when it is 3 μm or more and less than 5 μm, 1,000 times or more when it is 5 μm or more and less than 10 μm, 500 times or more when it is 10 μm or more and less than 50 μm, 250 times or more when it is 50 μm or more and less than 100 μm, and 100 times or more when it is 100 μm or more and 200 μm or less. Note that when the particle is not perfectly circular on the image (for example, when it is elliptical), the longest diameter is measured as the particle diameter.
[0045] (2) 10% particle size (D10) Particles were observed using a scanning electron microscope (FE-SEM, JSM-6301NF manufactured by JEOL Ltd.), and the particle diameter at which the cumulative frequency of measuring the diameter (particle diameter) of 100 particles was 10% was determined as the 10% particle diameter (D10). Specifically, in order to determine an accurate number-average particle diameter that reflects the variation in particle diameter, observation was performed at a magnification such that 2 or more but less than 100 particles were captured in one image, and the particle diameter was measured. Next, the particle diameter at which the cumulative frequency of measuring the diameter (particle diameter) of 100 fine particles was 10% was determined as D10. Note that, when the particle was not perfectly round on the image (for example, when it was elliptical), the longest diameter was measured as the particle diameter.
[0046] (3) Melt flow rate (MFR) Using a melt indexer (F-B01 manufactured by Toyo Seiki Seisakusho), the MFR of the polymer constituting the particles was measured at a measurement temperature of 190°C and a load of 2160g according to a method conforming to JIS K7210-2014. When the MFR exceeds 2000g / 10min, accurate measurement is difficult, so measurement is not possible.
[0047] (4) Melting point of particles 7 mg of particles were weighed and measured with a differential scanning calorimeter according to the method described in JIS K7121-1987. The temperature was increased from room temperature to 150°C at a rate of 10°C / min (1st run), decreased from 150°C to room temperature at a rate of 10°C / min, and then increased from room temperature to 150°C at a rate of 10°C / min (2nd run). The peak top temperature (°C) of the endothermic peak of melting was read as the melting point from the DSC chart obtained by the temperature increase measurement of the 2nd run.
[0048] (5) Solids concentration of the dispersion containing particles According to JIS K5601-1-2:2008, 1.0 g of the particle dispersion was heated at 140° C., the residue was measured, and the particle concentration was calculated.
[0049] (6) Coating onto porous substrates An aqueous dispersion containing 15 parts by mass of particles mainly composed of polyethylene and / or polyethylene copolymer, 0.2 parts by mass of carboxymethylcellulose (high molecular weight type, manufactured by Daicel Miraizu Co., Ltd.), and 0.9 parts by mass of 2-propanol was prepared as a coating liquid. After stirring this coating liquid for 4 hours, it was applied to an olefin porous membrane "SETELA" (registered trademark) (manufactured by Toray Industries, Inc., melting point: 135°C, thickness: 9 μm, air resistance: 60 s / 100 ml) using a bar coater and dried at 50°C for 1 minute to obtain a porous film laminated with a coating layer having a coating thickness as shown in Table 1.
[0050] (7) Coating layer thickness of porous film The coating thickness of the sample was calculated by subtracting the substrate thickness from the coating thickness measured with a micrometer (Mitutoyo Corporation). The thinner the coating thickness, the better, and it was judged according to the following four criteria (SS: 3 μm or less, S: more than 3 μm and 5 μm or less, A: more than 5 μm and 10 μm or less, B: more than 10 μm).
[0051] (8) Heat treatment A SUS metal frame with outer dimensions of 140 mm x 140 mm, inner dimensions of 100 mm x 100 mm, and thickness of 2 mm was prepared. Double-sided tape (No. 501F) manufactured by Nitto Denko Corporation was attached to all four sides of the metal frame, and the porous film was attached to the metal frame without slack. The sample attached to the metal frame was heated in a hot air oven to 120°C for 10 minutes after completion of the heating, removed, cooled, and the heat-treated porous film was cut out along the inner dimensions of the metal frame to obtain a sample.
[0052] (9) Air permeability of porous film A sample of 100 mm x 100 mm size was cut out from an arbitrary part of the untreated porous film, and the air permeability (min / 100 mL) was evaluated in an environment of 25 ° C., n = 5, and was determined as G25. In addition, the sample heat-treated at 120 ° C. in (8) was also evaluated in the same manner, n = 5, to determine G120. The smaller G25 is, the better, and it was determined according to the following four criteria (SS: 135 min / 100 mL or less, S: more than 135 min / 100 mL and 150 min / 100 mL or less, A: more than 150 min / 100 mL and 200 min / 100 mL or less, B: more than 200 min / 100 mL). In addition, the larger the G120, the more preferable it is, and it was judged based on the following four criteria (SS: 90,000 min / 100 mL or more, S: 80,000 min / 100 mL or more but less than 90,000 min / 100 mL, A: 50,000 min / 100 mL or more but less than 80,000 min / 100 mL, B: less than 50,000 min / 100 mL).
[0053] (10) Content of structural units (X) derived from α,β-unsaturated carboxylic acid (A) and structural units (Y) derived from anhydrides of α,β-unsaturated dicarboxylic acids (B) in the structural units of the polymer constituting the particles The particle powder was processed using a pretreatment accessory (Diamond EX Press (2.0 mmΦ)) to prepare a measurement sample. IR measurement was performed using an infrared microscope system (Spectrum Spotlight 200, manufactured by PerkinElmer Japan) by the transmission method. -1 Peak / 1530~1420cm -1 The area ratio of the peaks was converted using the following formula to determine the total content of the structural unit (X) derived from the α,β-unsaturated carboxylic acid (A) and the structural unit (Y) derived from the anhydride of the α,β-unsaturated dicarboxylic acid (B).
[0054] (Total of (X) and (Y) contents) = 11.19 × (area ratio) - 4.55 Example 1 90.0 g of ethylene-methacrylic acid copolymer (manufactured by Mitsui Dow Polychemicals, MFR: 100 g / 10 mL, melting point: 95° C., methacrylic acid content: 11%), 27.0 g of polyoxyethylene polyoxypropylene block polymer (manufactured by ADEKA, melting point: 56° C., ethylene oxide ratio: 80% by mass) as a nonionic surfactant, 4.5 g of sodium lauryl sulfate as an ionic surfactant, and 328.5 g of water were placed in a pressure-resistant container and stirred at 160° C. for 30 minutes. Then, the mixture was allowed to cool to room temperature. The D50 of the obtained particles was 1.4 μm and the D10 was 0.8 μm. The obtained dispersion was applied to a porous substrate by the method (6) above, and the results of the evaluations (7) to (9) above were as shown in Table 1. The abbreviations of the components in Table 1 have the following meanings. ·LDPE: Low density polyethylene PE-WAX: Polyethylene wax E-MAA: Ethylene-methacrylic acid copolymer Example 2 A particle dispersion was obtained in the same manner as in Example 1, except that the particle raw material was changed to 90.0 g of ethylene-methacrylic acid copolymer (manufactured by Mitsui Dow Polychemicals, MFR: 500 g / 10 mL, melting point: 95° C., methacrylic acid content: 10%). The obtained particles had a D50 of 0.9 μm and a D10 of 0.6 μm. The obtained dispersion was applied to a porous substrate by the method (6) above, and the results of the evaluations (7) to (9) above are shown in Table 1.
[0055] Example 3 A particle dispersion was obtained in the same manner as in Example 2, except that the nonionic surfactant was changed to a polyoxyethylene polyoxypropylene block polymer (manufactured by Sanyo Chemical Industries, Ltd., melting point 62°C, ethylene oxide ratio 80% by mass). The obtained particles had a D50 of 0.7 μm and a D10 of 0.5 μm. The obtained dispersion was applied to a porous substrate by the method (6) above, and the results of the evaluations (7) to (9) above are shown in Table 1.
[0056] Example 4 A particle dispersion was obtained in the same manner as in Example 1, except that the raw material for the particles was changed to a 1:1 (mass ratio) mixture of ethylene-methacrylic acid copolymer (manufactured by Mitsui-Dow Polychemicals, MFR: 100 g / 10 mL, melting point: 95° C., methacrylic acid content: 11%) and ethylene-methacrylic acid copolymer (manufactured by Mitsui-Dow Polychemicals, MFR: 500 g / 10 mL, melting point: 95° C., methacrylic acid content: 10%). The obtained particles had a D50 of 1.2 μm and a D10 of 0.7 μm. The obtained dispersion was applied to a porous substrate by the method (6) above, and the results of the evaluations (7) to (9) above were as shown in Table 1.
[0057] Example 5 A particle dispersion was obtained in the same manner as in Example 1, except that the raw material for the particles was changed to an ethylene-methacrylic acid copolymer (manufactured by Mitsui Dow Polychemicals, MFR: 60 g / 10 mL, melting point: 90°C, methacrylic acid content: 15%). The obtained particles had a D50 of 1.3 μm and a D10 of 0.7 μm. The obtained dispersion was applied to a porous substrate by the method (6) above, and the results of the evaluations (7) to (9) above are shown in Table 1.
[0058] Example 6 A particle dispersion was obtained in the same manner as in Example 1, except that the raw material for the particles was changed to a 3:1 (mass ratio) mixture of ethylene-methacrylic acid copolymer (manufactured by Mitsui Dow Polychemicals, MFR: 100 g / 10 mL, melting point: 95° C., methacrylic acid content: 11%) and low-density polyethylene (manufactured by Sumitomo Chemical Co., Ltd., MFR: 200 g / 10 mL, melting point: 104° C., acid content: 0%). The obtained particles had a D50 of 1.8 μm and a D10 of 1.1 μm. The obtained dispersion was applied to a porous substrate by the method (6) above, and the results of the evaluations (7) to (9) above were as shown in Table 1.
[0059] Example 7 The particle dispersion was prepared in the same manner as in Example 1, except that the raw material for the particles was changed to a 55:45 (mass ratio) mixture of ethylene-methacrylic acid copolymer (manufactured by Mitsui Dow Polychemicals, MFR: 100 g / 10 mL, melting point: 95°C, methacrylic acid content: 11%) and low-density polyethylene (manufactured by Sumitomo Chemical Co., Ltd., MFR: 200 g / 10 mL, melting point: 104°C, acid content: 0%). The D50 of the particles was 2.2 μm and the D10 was 1.3 μm. The obtained dispersion was applied to a porous substrate by the method (6) above, and the results of the evaluations (7) to (9) above were as shown in Table 1.
[0060] (Comparative Examples 1 to 2) A dispersion of polyethylene wax particles (manufactured by Mitsui Chemicals, Inc., solid content: 40% by mass, D50: 0.2 μm, melting points: 87° C. and 107° C.) was applied to a porous substrate by the method (6) above, and the results of the evaluations (7) to (9) above are shown in Table 1. It can be seen that when the MFR of the polymer constituting the particles is large, the pores of the porous substrate cannot be completely blocked by thin film coating.
[0061] (Comparative Examples 3 to 4) Low-density polyethylene particles (Sumitomo Seika Chemicals, D50: 6.6 μm, melting point: 107° C.) were applied to a porous substrate by the method (6) above, and the evaluations (7) to (9) above were carried out, with the results shown in Table 1. Note that because the particles had a large D50 of more than 5 μm, they could not be applied to a thin film of 5 μm or less. Furthermore, it was found that even when the particles were applied to a thickness of 10 μm, the pores in the substrate could not be completely blocked.
[0062] [Table 1] [Industrial Applicability]
[0063] The particles of the present invention can be coated on various substrates to form a uniform thin film. Furthermore, when a porous film coated with the particles of the present invention is heated, a uniform thin film without holes can be formed on the porous film. Therefore, by applying the particles of the present invention as a coating material for forming a shutdown layer on the surface of a battery separator film used in lithium ion batteries, it is expected to contribute to improving the safety of the battery.
Claims
1. Particles mainly composed of polyethylene and / or a polyethylene copolymer and having the following characteristics (I) to (II). (I) The number average particle diameter (D50) of the particles is 0.5 μm or more and 5.0 μm or less. (II) The polymer constituting the particles has a melt flow rate at 190° C. under a load of 2160 g of 0.3 g / 10 min or more and 2000 g / 10 min or less.
2. 2. The particle according to claim 1, wherein the polymer constituting the particle contains a structural unit (X) derived from an α,β-unsaturated carboxylic acid (A) and / or a structural unit (Y) derived from an anhydride of an α,β-unsaturated dicarboxylic acid (B), and the total content thereof is 1 mass % or more in 100 mass % of the structural units of the polymer constituting the particle.
3. 2. The particle according to claim 1, wherein the polymer constituting the particle contains a structural unit (X) derived from an α,β-unsaturated carboxylic acid (A) and / or a structural unit (Y) derived from an anhydride of an α,β-unsaturated dicarboxylic acid (B), and the total content thereof is 5% by mass or more and less than 30% by mass in 100% by mass of the structural units of the polymer constituting the particle.
4. The particles according to any one of claims 1 to 3, having a melting point of 90°C or higher and 130°C or lower.
5. The particles according to any one of claims 1 to 3, wherein the 10% particle size (D10) of the particles is 0.2 µm or more and 2.5 µm or less.
6. The particles according to any one of claims 1 to 3, wherein the number average particle diameter (D50) of the particles is 0.5 µm or more and 1.6 µm or less.
7. A dispersion comprising the particles according to any one of claims 1 to 3 and a solvent.
8. The dispersion according to claim 7 , having a solids concentration of more than 0.1% by mass and not more than 50% by mass.
9. 8. The dispersion of claim 7, wherein the solvent is either water or an alcohol, or a mixture thereof.
10. The dispersion of claim 7 wherein the solvent is water.
11. The dispersion according to claim 7, which is used as a coating material.
12. 8. The dispersion according to claim 7, which is used as a coating material for film coating.
13. A film comprising the particles according to any one of claims 1 to 3.
14. A battery separator film comprising the particles of any one of claims 1 to 3.
15. An electrode comprising the particles according to any one of claims 1 to 3.
Citation Information
Patent Citations
Diaphragm for battery and its manufacture
JP1997219185A
Aqueous dispersion, coating film, and laminate film
JP2004051661A
Process for manufacturing polyethylene wax particle, and polyethylene wax particle
JP2004059869A