Method for producing vinyl chloride resin aggregated particles
The method of applying shearing force and heat-treatment to vinyl chloride resin latex aggregates forms tertiary particles with strong primary bonds and loosely bonded secondary particles, addressing the high load issues in conventional methods and achieving suitable particle sizes for metal can coatings.
Patent Information
- Application Number
- JP2023194665
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-22
- Filing Date
- 2023-11-15
- Publication Date
- 2024-10-07
AI Technical Summary
Conventional methods for producing vinyl chloride resin agglomerated particles require high loads of pulverization and classification due to the production of aggregates larger than 100 μm, which do not meet the requirements for low sol coarse particles and low metal and salt concentrations needed for coating metal cans.
A method involving the application of shearing force to a mixture of vinyl chloride resin latex and a flocculant using a colloid mill, followed by heat-treatment at a specific temperature range, to form tertiary particles with strong primary particle bonds and loosely bonded secondary particles, which can be easily disintegrated into secondary particles using ultrasonic irradiation.
Reduces the load during pulverization and classification while achieving the necessary strength and size for vinyl chloride resin agglomerated particles suitable for metal can coatings, meeting low sol coarse particle requirements.
Smart Images

Figure 2024137650000003 
Figure 2024137650000004 
Figure 2024137650000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing polyvinyl chloride resin agglomerated particles that can be suitably used for coating the inner surface of a metal can. [Background technology]
[0002] Since vinyl chloride resin is inexpensive and has excellent processability and durability, it is widely used for coating the inner surface of metal cans. For example, Patent Document 1 describes a coating composition for metal cans that uses vinyl chloride resin aggregate particles having a particle diameter D50 of 0.5 μm to 5.0 μm at a cumulative volume percentage of 50 volume% in a volume particle size distribution, a particle diameter D90 of 8.0 μm or less at a cumulative volume percentage of 90 volume% in a volume particle size distribution, and a Na concentration of 90 ppm or less. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2019 / 159896 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0004] Resins used to coat the inside of metal cans are required to have low sol coarse particles (e.g., coarse particles of 25 μm or less according to Method A). In addition, resins used to coat the inside of metal cans are required to have low metal and salt concentrations. Therefore, in conventional methods for producing vinyl chloride resin agglomerated particles, including Patent Document 1, vinyl chloride resin latex particles are generally made into agglomerates of about 100 μm or more, and the agglomerates are washed and dehydrated to reduce the metal and salt concentrations, and then crushed and classified to produce vinyl chloride resin agglomerated particles that satisfy the low sol coarse particle characteristics, which poses a problem of high loads on the crushing and classification.
[0005] In order to solve the above-mentioned problems of the conventional art, the present invention provides a method for producing vinyl chloride resin agglomerated particles, which can produce vinyl chloride resin agglomerated particles having the strength and size required for steps such as washing, while reducing the load involved in crushing and classifying the vinyl chloride resin agglomerated particles so as to satisfy the low sol coarse particle requirement. [Means for solving the problem]
[0006] The present invention relates to a method for producing vinyl chloride resin agglomerated particles, the method comprising the steps of: applying a shear force to a mixture of vinyl chloride resin latex and an aggregating agent in a colloid mill to obtain an agglomerated latex containing vinyl chloride resin agglomerated particles; and heat-treating the agglomerated latex in a temperature range of [Tg-20°C] to [Tg+35°C], where Tg is the glass transition temperature of vinyl chloride resin, the vinyl chloride resin agglomerated particles including tertiary particles formed by further agglomeration of secondary particles formed by agglomeration of vinyl chloride resin latex particles. Effect of the Invention
[0007] According to the production method of the present invention, it is possible to obtain vinyl chloride resin agglomerated particles having the strength and size required for steps such as washing, and it is also possible to reduce the load involved in crushing and classifying the vinyl chloride resin agglomerated particles so as to satisfy the low sol coarse particle requirement. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a schematic diagram illustrating the aggregation of vinyl chloride resin latex particles to form vinyl chloride resin aggregate particles having a tertiary particle structure. [Diagram 2] FIG. 2 is a schematic diagram illustrating how tertiary particles of vinyl chloride resin agglomerated particles are disintegrated by ultrasonic irradiation to form secondary particles. [Diagram 3] 1 is a graph showing particle size distribution measured on a volume basis after irradiating the agglomerated latex (vinyl chloride resin agglomerated particles) obtained in Example 4 with ultrasonic waves. [Figure 4]1 is a graph showing particle size distribution measured on a volume basis after irradiating the agglomerated latex (vinyl chloride resin agglomerated particles) obtained in Example 3 with ultrasonic waves. [Diagram 5] 1 is a scanning electron microscope (SEM) image (3000x) of the agglomerated latex (vinyl chloride resin agglomerated particles) obtained in Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The inventors of the present invention have conducted intensive research to solve the above-mentioned problems. As a result, they have surprisingly found that in the aggregation step, by applying shear force to a mixture of vinyl chloride resin latex and aggregating agent in a colloid mill to aggregate the vinyl chloride resin latex, and then heat-treating the mixture at a predetermined temperature, vinyl chloride resin aggregated particles containing tertiary particles formed by further aggregating secondary particles formed by aggregating vinyl chloride resin latex particles (primary particles) are obtained, and that when the obtained vinyl chloride resin aggregated particles are irradiated with ultrasonic waves at 20 kHz for 3 minutes, most of the tertiary particles can be disintegrated to become secondary particles. Specifically, the vinyl chloride resin agglomerated particles obtained in the agglomeration step in which a mixture of vinyl chloride resin latex and aggregating agent is subjected to shear force in a colloid mill contain tertiary particles in which secondary particles to which primary particles are strongly bound are loosely bound, and by heat-treating the vinyl chloride resin agglomerated particles obtained in the agglomeration step, the bonds between the primary particles become stronger, and the vinyl chloride resin agglomerated particles can have the strength and size required for the washing step. In addition, since the vinyl chloride resin agglomerated particles after heat treatment are easily irradiated with ultrasonic waves at 20 kH for 3 minutes, with most of the tertiary particles collapsing to become secondary particles, the load when crushing and classifying the vinyl chloride resin agglomerated particles to satisfy the low sol coarse particle requirement can also be reduced.
[0010] In this specification, when a numerical range is indicated by "~", the numerical range includes both end values (upper and lower limits). For example, a numerical range of "X~Y" includes both end values X and Y, and is the same range as "X or more and Y or less". Any number within the range and any range included within the range are specifically disclosed. In addition, when multiple numerical ranges are described in this specification, they are intended to include numerical ranges that appropriately combine the upper and lower limits of different numerical ranges.
[0011] The vinyl chloride resin latex is not particularly limited, but can be obtained, for example, by adding a polymerization initiator and an emulsifier to a vinyl chloride monomer or a mixture of a vinyl chloride monomer and a monomer copolymerizable therewith in an aqueous medium such as ion-exchanged water, and carrying out emulsion polymerization, seed emulsion polymerization, fine suspension polymerization, or seed fine suspension polymerization. In addition, in the polymerization, a dispersing aid such as a higher alcohol and a higher fatty acid, and a pH adjuster such as sodium bicarbonate and sodium carbonate may be used as necessary.
[0012] The monomer copolymerizable with the vinyl chloride monomer is not particularly limited, and may be any monomer copolymerizable with vinyl chloride, such as olefins such as ethylene, propylene, and butene; vinyl esters such as vinyl acetate, vinyl propionate, and vinyl stearate; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, octyl vinyl ether, and lauryl vinyl ether; vinylidenes such as vinylidene chloride; unsaturated carboxylic acids and their acid anhydrides such as acrylic acid, methacrylic acid, fumaric acid, maleic acid, itaconic acid, maleic anhydride, and itaconic anhydride; unsaturated carboxylic acid esters such as methyl acrylate, ethyl acrylate, monomethyl maleate, dimethyl maleate, and butylbenzyl maleate; aromatic vinyl compounds such as styrene, α-methylstyrene, and divinylbenzene; unsaturated nitriles such as acrylonitrile; and crosslinking monomers such as diallyl phthalate. These monomers may be used alone or in combination of two or more. The amount of these monomers used is preferably less than 50% by weight in the monomer mixture with vinyl chloride monomer.
[0013] The emulsifier is not particularly limited, and for example, an anionic surfactant can be used. Examples of the anionic surfactant include potassium salts, sodium salts, and ammonium salts of fatty acids, alkyl sulfuric acids, alkyl benzene sulfonic acids, alkyl sulfosuccinic acids, α-olefin sulfonic acids, and alkyl ether phosphate esters. From the viewpoint of viscosity stability of the composition containing the vinyl chloride resin aggregated particles, the emulsifier is preferably a fatty acid salt, more preferably one or more selected from the group consisting of potassium salts of fatty acids, sodium salts of fatty acids, and ammonium salts of fatty acids, and even more preferably one or more selected from the group consisting of sodium lauryl sulfate, potassium stearate, potassium myristate, and ammonium myristate.
[0014] The emulsifier can be used in an amount of, for example, about 0.1 to 3.0 parts by weight per 100 parts by weight of the total monomers. From the viewpoint of improving the stability of the resulting vinyl chloride resin latex and the transparency of films such as a can inner surface film and a marking film, the emulsifier is preferably used in an amount of 0.2 to 1.0 part by weight, more preferably 0.2 to 0.5 part by weight, per 100 parts by weight of the monomers.
[0015] The polymerization initiator may be an oil-soluble polymerization initiator or a water-soluble polymerization initiator. The oil-soluble polymerization initiator may be an organic peroxide or an azo initiator. Examples of the organic peroxide include hydroperoxides such as t-butyl hydroperoxide; diacyl peroxides such as dilauroyl peroxide and di-3,5,5-trimethylhexanoyl peroxide; peroxydicarbonates such as diisopropyl peroxydicarbonate and di-2-ethylhexyl peroxydicarbonate; and peroxyesters such as t-butyl peroxypivalate and t-butyl peroxyneodecanoate. Examples of the azo initiator include azo initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile). As the water-soluble polymerization initiator, ammonium persulfate, potassium persulfate, sodium persulfate, hydrogen peroxide water, etc. can be used. The polymerization initiator can be used alone or in combination of two or more. The polymerization initiator can be used in combination with a reducing agent such as sodium sulfite, sodium thiosulfate, sodium hydroxymethanesulfinate dihydrate (also called Rongalit), ascorbic acid, sodium ascorbate, etc., as necessary. The reducing agent can be used alone or in combination of two or more.
[0016] In the vinyl chloride resin latex, the volume average particle diameter of the vinyl chloride resin latex particles is not particularly limited, but is preferably 0.1 to 2.0 μm from the viewpoint of polymerization stability. When the volume average particle diameter of the vinyl chloride resin latex particles is 0.1 μm or more, the mechanical stability during latex transfer is improved, and the productivity is improved. When the volume average particle diameter of the vinyl chloride resin latex particles is 2.0 μm or less, the polymerization stability is increased. From the viewpoint of polymerization stability, the volume average particle diameter of the vinyl chloride resin latex particles is more preferably 1.7 μm or less, and even more preferably 1.4 μm or less.
[0017] From the viewpoint of lowering the viscosity of a composition containing the vinyl chloride resin agglomerated particles and promoting gelation, the vinyl chloride resin latex preferably contains 5 to 95 volume % of vinyl chloride resin latex particles F having a volume average particle diameter of 0.5 μm or less, and 5 to 95 volume % of vinyl chloride resin latex particles R having a volume average particle diameter larger than that of the vinyl chloride resin latex particles F and 1.7 μm or less; more preferably contains 10 to 90 volume % of vinyl chloride resin latex particles F and 10 to 90 volume % of vinyl chloride resin latex particles R; even more preferably contains 15 to 85 volume % of vinyl chloride resin latex particles F and 15 to 85 volume % of vinyl chloride resin latex particles R; and even more preferably contains 20 to 50 volume % of vinyl chloride resin latex particles F and 50 to 80 volume % of vinyl chloride resin latex particles R. From the viewpoint of the stability of the polymerization of the vinyl chloride resin, the volume average particle diameter of the vinyl chloride resin latex particles R is more preferably 1.4 μm or less. From the viewpoint of low viscosity and promotion of gelation, the volume average particle diameter of the vinyl chloride resin latex particles F is more preferably 0.4 μm or less.
[0018] The solid content of the vinyl chloride resin latex is preferably 22% by weight or more, more preferably 25 to 50% by weight, and further preferably 30 to 45% by weight. When the solid content of the vinyl chloride resin latex is within the above-mentioned range, the vinyl chloride resin latex has excellent fluidity and can be easily transferred to a colloid mill.
[0019] As the flocculant, a water-soluble flocculant can be used. Examples of the water-soluble flocculant include inorganic salts, inorganic acids, organic acids, organic salts, and water-soluble polymers. Examples of the inorganic salts include, but are not limited to, sodium sulfate, aluminum sulfate, sodium chloride, potassium chloride, calcium chloride, and aluminum chloride. Examples of the inorganic acids include, but are not limited to, sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid. Examples of the organic acids include, but are not limited to, citric acid, malic acid, tartaric acid, gluconic acid, succinic acid, malonic acid, glutaric acid, maleic acid, fumaric acid, and glutaconic acid. Examples of the organic salts include, but are not limited to, sodium acetate and calcium acetate.
[0020] Examples of the water-soluble polymer include synthetic polymers, natural polymers, and semi-synthetic polymers. Examples of the synthetic polymer include polymers of acryloyl group-containing monomers, vinyl polymers, polyamidines, polyethylene oxides, and polyethyleneimines. Examples of the natural polymer include polysaccharides and proteins. Examples of the semi-synthetic polymer include cellulose ethers and starch derivatives. From the viewpoint of reducing the moisture absorption rate of the polyvinyl chloride resin agglomerated particles, the amount of the water-soluble polymer is preferably 25% by weight or less, more preferably 10% by weight or less, based on the total weight of the flocculant.
[0021] From the viewpoint of reducing the moisture absorption rate of the vinyl chloride resin agglomerated particles and stabilizing the viscosity of a composition containing the vinyl chloride resin agglomerated particles during storage, it is preferable to use, as the agglomerating agent, one or more selected from the group consisting of inorganic salts, inorganic acids, organic acids and organic salts, it is more preferable to use one or more selected from the group consisting of inorganic salts and inorganic acids, and it is even more preferable to use an inorganic salt.
[0022] The flocculant may be in the form of either a solid or an aqueous solution when added to the vinyl chloride resin latex, but is preferably in the form of an aqueous solution from the viewpoint of dispersibility, and is more preferably added to the vinyl chloride resin latex in a fluidized state. The flocculant is preferably added to the vinyl chloride resin latex after the polymerization of the vinyl chloride resin is completed.
[0023] The amount of the flocculant added is not particularly limited as long as it can flocculate the vinyl chloride resin latex, but for example, an amount of the flocculant may be added so that the concentration of the flocculant in the flocculant latex (slurry) is 1.0 to 4.0% by weight. From the viewpoint of easy flocculation of vinyl chloride resin latex particles (primary particles), an amount of the flocculant may be added so that the concentration of the flocculant in the flocculant latex is preferably 1.5% by weight or more, more preferably 2.0% by weight or more, and particularly preferably 2.5% by weight or more. In addition, from the viewpoint that the flocculant particles of the tertiary particle structure in the flocculant latex are easy to disintegrate into secondary particles but difficult to disintegrate into primary particles, the concentration of the flocculant in the flocculant latex may be 3.0% by weight or more.
[0024] Specifically, the aggregation of the vinyl chloride resin latex is carried out by feeding an aqueous solution of the vinyl chloride resin latex and an aggregating agent such as an inorganic salt to a colloid mill, mixing the vinyl chloride resin latex and the aqueous solution of the aggregating agent at the inlet of the colloid mill, and applying a shear force to the mixture inside the colloid mill. The conditions for applying the shear force are not particularly limited, and from the viewpoint of forming secondary particles in which the primary particles are strongly bonded and the secondary particles are easily bonded to form a tertiary particle structure, the frequency may be 20 to 60 Hz and the clearance may be 40 to 1240 μm. The frequency may be 40 to 60 Hz. The temperature may be 20 to 50° C. The residence time may be 1.5 to 10 seconds. The colloid mill is not particularly limited, but for example, “Type-K120” manufactured by PUC Co., Ltd. may be appropriately used.
[0025] In the coagulated latex (slurry) obtained in the coagulation step, the concentration of the resin solid content is preferably 22% by weight or more, more preferably 25 to 50% by weight, and further preferably 30 to 45% by weight. When the concentration of the resin solid content in the coagulated latex is within the above-mentioned range, the coagulated latex has excellent fluidity and is easily transported.
[0026] The agglomerated latex is heat-treated at a temperature range of [Tg-20°C] to [Tg+35°C], where Tg is the glass transition temperature of the vinyl chloride resin. This makes the bond between the primary particles stronger, and the strength of both the secondary particles and the tertiary particles is also stronger, making it possible to obtain vinyl chloride resin agglomerated particles having the strength and size required for the washing process. Note that, before the heat treatment, the concentration of the resin solid content in the agglomerated latex may be adjusted to 10 to 50% by weight. In addition, by performing the agglomeration process under the above-mentioned conditions, the vinyl chloride resin agglomerated particles after the heat treatment are likely to be disintegrated into secondary particles by irradiation with ultrasonic waves at 20 kH for 3 minutes, and therefore the load when crushing and classifying the vinyl chloride resin agglomerated particles to satisfy the low sol coarse particle requirement can also be reduced. From the viewpoint of further increasing the strength of the vinyl chloride resin agglomerated particles, the heat treatment is preferably carried out in the range of [Tg-10°C] to [Tg+35°C], and more preferably in the range of Tg to [Tg+35°C], where Tg is the glass transition temperature of the vinyl chloride resin. In addition, the heat treatment time is not particularly limited, but after reaching a predetermined temperature, from the viewpoint of industrial implementation, it may be held for 30 seconds to 300 minutes, 3 to 120 minutes, or 5 to 30 minutes.
[0027] The heat-treated agglomerated latex (slurry containing vinyl chloride resin agglomerated particles) contains tertiary particles formed by further agglomeration of secondary particles formed by agglomeration of vinyl chloride resin latex particles (primary particles). That is, the obtained vinyl chloride resin agglomerated particles contain tertiary particles 3 formed by further agglomeration of secondary particles 2 formed by agglomeration of vinyl chloride resin latex particles (primary particles) 1, as shown in FIG. 1. In the vinyl chloride resin agglomerated particles, the tertiary particles have a structure in which secondary particles strongly bonded to primary particles are loosely bonded, and the secondary particles have a structure in which primary particles are strongly bonded. This can be confirmed, for example, by irradiating the agglomerated latex with ultrasonic waves at 20 kHz for 3 minutes, whereby the tertiary particles 3 are mostly disintegrated to become secondary particles 2, as shown in FIG. 2. In the agglomerated latex, the vinyl chloride resin agglomerated particles may contain secondary particles in addition to tertiary particles.
[0028] In the heat-treated agglomerated latex, the vinyl chloride resin agglomerated particles have a tertiary particle structure in which the primary particles are strongly bonded to the secondary particles and the secondary particles are somewhat loosely bonded to each other, i.e., the bond strength between the primary particles is high and the bond strength between the secondary particles is relatively low, so that the load when pulverizing and classifying the particles to meet the low sol coarse particle requirement is reduced while maintaining the strength and size (particle diameter) required for processes such as washing. In particular, by applying shear force to a mixture of the vinyl chloride resin latex and the agglomerating agent in a colloid mill to cause agglomeration and then heat-treating the mixture, the vinyl chloride resin agglomerated particles in the heat-treated agglomerated latex tend to have a D50 of 10 μm or more and a D90 of 110 μm or less, and the secondary particles in the vinyl chloride resin agglomerated particles tend to have a D90 of 10.5 μm or less, so that the load when pulverizing and classifying the particles to meet the low sol coarse particle requirement is reduced while maintaining the strength and size (particle diameter) required for processes such as washing.
[0029] The vinyl chloride resin agglomerated particles preferably have a (tertiary particle) median diameter (D50) of 10 to 60 μm and a D90 of 20 to 110 μm, more preferably a median diameter (D50) of 10 to 50 μm and a D90 of 20 to 100 μm, and even more preferably a median diameter (D50) of 30 to 50 μm and a D90 of 50 to 100 μm. In the vinyl chloride resin agglomerated particles, the secondary particle median diameter (D50) is preferably 2.0 to 6.5 μm and more preferably 2.0 to 6.0 μm. In addition, in the vinyl chloride resin agglomerated particles, the secondary particle D90 is preferably 11 μm or less, more preferably 10.5 μm or less, even more preferably less than 10 μm, and even more preferably 9 μm or less. This makes it easier for the composition containing the vinyl chloride resin agglomerated particles to satisfy the requirement of low sol coarse particles (e.g., 25 μm or less coarse particles according to Method A) when used to coat the inner surface of a metal can. In the vinyl chloride resin agglomerated particles, the upper limit of D90 of the secondary particles is preferably within the above-mentioned range, and the lower limit is not particularly limited, but may be, for example, 5 μm or more from the viewpoint of powder handling. In this specification, the particle size of the tertiary particles in the vinyl chloride resin agglomerated particles is measured using vinyl chloride resin agglomerated particles (agglomerated latex after heat treatment) as a sample, and the particle size of the secondary particles in the vinyl chloride resin agglomerated particles can be measured using vinyl chloride resin agglomerated particles (agglomerated latex after heat treatment) after ultrasonic irradiation under conditions of 20 kHz and 3 minutes as a sample. In this specification, D50 and D90 are based on volume, and are measured specifically as described in the Examples.
[0030] The pH of the heat-treated aggregated latex may be adjusted, if necessary, to a range of 4 to 11, preferably 5 to 10, and more preferably 6 to 9. By adjusting the pH within the above range, the moisture absorption rate of the obtained vinyl chloride resin aggregated particles is low, and the storage stability of the composition containing the vinyl chloride resin aggregated particles is improved. The pH adjustment can be performed using a compound capable of adjusting the pH to within the above range, and is not particularly limited, but for example, sodium hydroxide can be used.
[0031] It is preferable to dehydrate the heat-treated coagulated latex or the pH-adjusted coagulated latex, and then add water to wash it. The dehydration can be performed by filtration, although not limited thereto. Washing can reduce the concentrations of metals and salts.
[0032] The washed aggregated latex is dehydrated and then dried to obtain vinyl chloride resin aggregated particles. If necessary, the washed aggregated latex is dehydrated and dried, and then pulverized and / or classified. The dehydration is not particularly limited, but can be performed by filtration. The drying temperature is not particularly limited, but can usually be performed at a resin temperature in the range of 35 to 100°C. The pulverizer or crusher is also not particularly limited, and for example, a roller mill, a high-speed rotary crusher, a ball mill, a jet mill, etc. can be used.
[0033] The vinyl chloride resin aggregate particles obtained after drying tend to have the characteristics of low sol coarse particles (25 μm or less by Method A) and low metal / salt concentration (90 ppm or less), and can be suitably used in a metal can coating composition. From the viewpoints of the processability, retort resistance, and tearability of the coating film, the metal can coating composition preferably contains (A) 20 to 80 parts by weight of the vinyl chloride resin aggregate particles, (B) 1 to 30 parts by weight of one or more resins selected from the group consisting of phenolic resins, epoxy resins, and acrylic resins, (C) 1 to 60 parts by weight of a polyester resin, and (D) an organic solvent, and the total amount of (A), (B), and (C) is preferably 100 parts by weight. The metal can coating composition may be a can inner surface coating composition used on the inner surface of a metal can, or may be a can outer surface coating composition used on the outer surface of a metal can. The composition containing the vinyl chloride resin aggregate particles may be used as a marking film composition. From the viewpoint of the transparency, water resistance, and weather resistance of the marking film, it is preferable that the composition for the marking film contains (a) 50 to 90 parts by weight of the vinyl chloride resin aggregate particles, (b) 10 to 50 parts by weight of a plasticizer, and (c) an organic solvent, the total amount of (a) and (b) being 100 parts by weight. EXAMPLES
[0034] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0035] First, the measurement and evaluation methods used in the examples and comparative examples will be described.
[0036] (Volume average particle size of polyvinyl chloride resin latex particles) The polyvinyl chloride resin latex was used as a measurement sample, and in accordance with JIS Z 8823-2:2016, a disk centrifugal particle size distribution measuring device (CPS Instruments.Inc., "Disk Centrifuge Model DC18000") was used to create a particle concentration gradient by centrifugation based on the sedimentation method, and the volume average particle size (peak particle size) of the polyvinyl chloride resin latex particles was obtained from the weight distribution based on each volume standard. The measurement conditions were as follows: the disk rotation speed was set to 12,000 rpm, and then 8 mL of an 8 wt% sucrose aqueous solution and a 24 wt% sucrose aqueous solution were injected to create a sucrose concentration gradient. The measurement sample was prepared by adding ion-exchanged water filtered through a 0.2 μm filter to polyvinyl chloride resin latex filtered through a 350 mesh wire net, and 0.1 mL of the sample was added and measured using a 470 nm detector.
[0037] (Average degree of polymerization of vinyl chloride resin) The average degree of polymerization of vinyl chloride resin was measured in accordance with JIS K 7367-2:1999. First, 2.5 mg of vinyl chloride resin aggregate particles or dried vinyl chloride resin latex and 50 mL (47.1 g) of cyclohexanone were placed in a 100 ml beaker, and dissolved in a shaker at 25°C for 1 hour to prepare a sample solution. Next, the average (n=2) of the falling seconds of the sample solution and cyclohexanone was calculated, and the viscosity ratio (VR) = falling seconds of the sample solution / falling seconds of cyclohexanone was calculated. Next, the K value corresponding to the viscosity ratio (VR) was measured based on the conversion table of JIS K 7367-2:1999. Next, the average degree of polymerization was calculated based on the K value.
[0038] (Glass transition temperature of polyvinyl chloride resin) The glass transition temperature Tg of vinyl chloride resin was measured by weighing 5 mg of vinyl chloride resin into an aluminum container, putting a lid on it and crimping it, and then setting the empty aluminum container together with a reference substance in a differential scanning calorimeter (DSC7020, Hitachi High-Tech Science Corporation) and performing differential scanning calorimetry in a nitrogen gas atmosphere at a temperature rise rate of 10°C / min in the range of 30°C to 200°C to calculate Tg. Note that the vinyl chloride resin sample used was a resin spray-dried from the vinyl chloride resin latex obtained in each production example at an inlet temperature of 105°C and an outlet temperature of 55°C.
[0039] (Particle size distribution of polyvinyl chloride resin agglomerated particles) Using the aggregated latex as a sample, a laser diffraction / scattering type particle size distribution analyzer (Horiba, Partica LA-950) was used to measure the particle size distribution of vinyl chloride resin aggregated particles (tertiary particles) in the aggregated latex on a volume basis, and the particle size (median size) D50 at which the cumulative volume percentage in the volumetric particle size distribution is 50 volume% and the particle size D90 at which the cumulative volume percentage in the volumetric particle size distribution is 90 volume% were obtained. The measurement conditions were: temperature 25°C, material information transparent with refractive index 1.51, no check for spherical particles, carrier water with refractive index 1.33. In addition, set zero was set for 10 seconds, measurement was performed for 10 seconds, and no calculation was performed for dry cut. In addition, using the ultrasonic irradiation function of a laser diffraction / scattering type particle size distribution analyzer (Horiba, Partica LA-950), the aggregated latex samples were irradiated at 20 kHz for 3 minutes and the particle size distribution was measured on a volume basis. In the particle size distribution of the agglomerated latex after irradiation at 20 kHz for 3 minutes, when the histogram has one peak, it means that all of the vinyl chloride resin agglomerated particles (tertiary particles) have disintegrated into secondary particles and have not disintegrated into primary particles. Based on the histogram, D50 and D90 of the secondary particles in the agglomerated latex were calculated. In the particle size distribution of the aggregated latex after irradiation at 20 kHz for 3 minutes, if the histogram has two peaks, it means that the vinyl chloride resin aggregated particles (tertiary particles) have collapsed into secondary particles and primary particles. In this case, the obtained particle size distribution was fitted using a log-normal distribution, and the peaks were separated to separate the histogram into peaks corresponding to secondary particles and peaks corresponding to primary particles, and the collapse ratio of the vinyl chloride resin aggregated particles (tertiary particles) into secondary particles and the collapse ratio into primary particles were obtained. In addition, the D50 and D90 of the secondary particles were obtained based on the histogram corresponding to the secondary particles.
[0040] (Observation of the shape of polyvinyl chloride resin aggregate particles) The aggregated latex was used as a sample, and the shape of the polyvinyl chloride resin aggregated particles was observed under a scanning electron microscope (Hitachi High-Technologies Corporation, S-4800).
[0041] (Production Example 1) A 300L jacketed pressure vessel was charged with 136.4 kg of vinyl chloride monomer, 150 kg of ion-exchanged water, 16.7 g of sodium lauryl sulfate, 127.5 g of sodium hydroxymethanesulfinate dihydrate (Rongalite), and 60 g of sodium hydrogen carbonate, and the temperature was raised to 50°C. Polymerization was carried out by continuously adding 3.2 kg of 0.3 wt% t-butyl hydroperoxide aqueous solution and 7.9 kg of 4 wt% sodium lauryl sulfate aqueous solution while stirring. After polymerization was continued until the polymerization pressure was reduced by 0.35 MPa from the initial pressure (0.7 MPa), the remaining monomer was recovered to obtain a vinyl chloride resin latex. In the finally obtained vinyl chloride resin latex, the polymerization conversion rate relative to the total amount of vinyl chloride monomer charged was 90%. In the obtained vinyl chloride resin latex, the volume average particle diameter of the vinyl chloride resin latex particles was 0.45 μm, and the average polymerization degree was 1480. The concentration of the resin solid content in the vinyl chloride resin latex was 38% by weight.
[0042] (Production Example 2) A 300L jacketed pressure vessel was charged with 150 kg of vinyl chloride monomer, 150 kg of ion-exchanged water, 14.6 kg of vinyl chloride resin latex obtained in Production Example 1, 83.3 g of potassium myristate aqueous solution (0.06 parts by weight relative to 100 parts by weight of the total amount of vinyl chloride monomer charged), 127.5 g of sodium hydroxymethanesulfinate dihydrate (Rongalite), and 15 g of potassium phosphate, and the mixture was heated to 48°C. While stirring, 5.44 kg of 0.4% by weight t-butyl hydroperoxide aqueous solution and 6.8 kg of 10% by weight potassium myristate aqueous solution (0.45 parts by weight relative to 100 parts by weight of the total amount of vinyl chloride monomer charged) were continuously added to perform polymerization. After polymerization was continued until the polymerization pressure was reduced by 0.3 MPa from the initial pressure (0.65 MPa), the remaining monomer was recovered to obtain a vinyl chloride resin latex. In the finally obtained vinyl chloride resin latex, the polymerization conversion rate of the total amount of vinyl chloride monomer charged was 90%. The obtained vinyl chloride resin latex contained 80 volume % of vinyl chloride resin latex particles having a volume average particle diameter of 1.24 μm and 20 volume % of vinyl chloride resin latex particles having a volume average particle diameter of 0.45 μm, and the average polymerization degree of the vinyl chloride resin was 1640. In addition, the concentration of the resin solid content in the vinyl chloride resin latex was 40 weight %, and the Tg of the vinyl chloride resin was 80° C.
[0043] Example 1 The vinyl chloride resin latex obtained in Production Example 2 was diluted with pure water so that the resin solid concentration was 36.5% by weight. The diluted vinyl chloride resin latex and sodium sulfate (20% by weight aqueous solution) as a flocculant were sent to a colloid mill (PUC, Type-K120), and the vinyl chloride resin latex and sodium sulfate were mixed at the inlet of the colloid mill. The mixture was subjected to shear force inside the colloid mill under the conditions of a temperature of 30°C, a frequency of 60Hz, a clearance of 40μm, and a residence time of 6 seconds to flocculate the vinyl chloride resin latex. Sodium sulfate was added so that the flocculated latex (total amount of the vinyl chloride resin latex and the aqueous solution of sodium sulfate) was 2.0% by weight. The obtained flocculated latex was diluted with pure water so that the solid concentration was 20% by weight, and the diluted flocculated latex was heat-treated by holding it at 60°C for 10 minutes to produce vinyl chloride resin flocculated particles.
[0044] (Examples 2 to 4) A vinyl chloride resin agglomerated particles were prepared in the same manner as in Example 1, except that the temperature during the heat treatment was changed as shown in Table 1 below.
[0045] (Examples 5 to 6) A vinyl chloride resin agglomerated particles were produced in the same manner as in Example 4, except that the frequency was changed as shown in Table 1 below.
[0046] (Examples 7 to 10) Vinyl chloride resin agglomerated particles were prepared in the same manner as in Example 4, except that the clearance was changed as shown in Table 1 below.
[0047] (Examples 11 to 12) Vinyl chloride resin aggregated particles were prepared in the same manner as in Example 4, except that the concentration of the flocculant (sodium sulfate) was changed as shown in Table 1 below.
[0048] Comparative Example 1 The vinyl chloride resin latex obtained in Production Example 2 was diluted with pure water to a solid content concentration of 36.5% by weight, and sodium sulfate (20% by weight aqueous solution) was added as a coagulant to the diluted vinyl chloride resin latex so that the concentration was 2.0% by weight in the coagulated latex. The mixture was placed in a 50 mL vial and stirred for 10 minutes using a magnetic stirrer to coagulate the vinyl chloride resin latex. The coagulated latex was subjected to a heat treatment by keeping it at 90°C for 10 minutes.
[0049] Comparative Example 2 The vinyl chloride resin latex obtained in Production Example 2 was diluted with pure water to a solid content concentration of 36.5% by weight, and sodium sulfate (20% by weight aqueous solution) was added as a coagulant to the diluted vinyl chloride resin latex so that the coagulated latex had a concentration of 2.0% by weight. The resulting mixture was mixed in a MULTI STAGE MIXER (clearance 8500 μm) at a temperature of 30° C. and agitation power of 10 kW / m 3 The mixture was stirred for a residence time of 6 seconds under the above conditions to coagulate the vinyl chloride resin latex. The coagulated latex was then subjected to a heat treatment by being held at 90°C for 10 minutes.
[0050] [Table 1]
[0051] The volume average particle size of the vinyl chloride resin latex particles, the average polymerization degree of the vinyl chloride resin, and the glass transition temperature of the vinyl chloride resin latexes obtained in Production Examples 1 and 2 were measured and calculated as described above.
[0052] The D50 and D90 of the tertiary particles and secondary particles of the vinyl chloride resin agglomerated particles obtained in the Examples and Comparative Examples were measured and calculated as described above, and the results are shown in Table 2 below. In addition, the disintegration ratio of the vinyl chloride resin agglomerated particles obtained in the Examples and Comparative Examples to secondary particles disintegrated into secondary particles by ultrasonic irradiation, and the disintegration ratio of the vinyl chloride resin agglomerated particles to primary particles disintegrated into primary particles were measured and calculated as described above, and the results are shown in Table 2 below. In addition, the shapes of the vinyl chloride resin agglomerated particles obtained in the Examples and Comparative Examples were observed using an SEM as described above.
[0053] [Table 2]
[0054] 3 and 4 show examples of particle size distributions measured on a volume basis after irradiating the agglomerated latexes (vinyl chloride resin agglomerated particles) obtained in Examples 3 and 4, respectively, with ultrasonic waves. As can be seen from Fig. 3, the histogram has one peak, and the vinyl chloride resin agglomerated particles (tertiary particles) obtained in Example 4 are only disintegrated into secondary particles by ultrasonic irradiation, and are not disintegrated into primary particles. Although not shown, the histogram of particle size distribution measured on a volume basis after ultrasonic irradiation of the agglomerated latexes (vinyl chloride resin agglomerated particles) obtained in Examples 5 to 11 had one peak. As can be seen from Fig. 4, the histogram has two peaks, and most of the vinyl chloride resin agglomerated particles (tertiary particles) obtained in Example 3 are disintegrated into secondary particles by ultrasonic irradiation, but some are disintegrated into primary particles. Although not shown, the histogram of particle size distribution measured on a volume basis after ultrasonic irradiation of the agglomerated latexes (vinyl chloride resin agglomerated particles) obtained in Examples 1, 2, and 12 had two peaks.
[0055] Fig. 5 shows an SEM image of the vinyl chloride resin agglomerated particles of Example 4. Fig. 5 shows that the vinyl chloride resin agglomerated particles of Example 4 contain tertiary particles formed by further agglomeration of secondary particles which are agglomerates of primary particles (vinyl chloride resin latex particles). Although not shown in the figures for Examples 1 to 3 and 6 to 12, it was confirmed that, like Example 4, the vinyl chloride resin agglomerated particles contain tertiary particles formed by further agglomeration of secondary particles which are agglomerates of primary particles (vinyl chloride resin latex particles).
[0056] Also, as can be seen from Tables 1 and 2, the vinyl chloride resin agglomerated particles obtained in Examples 1 to 12 in which shear force by a colloid mill was applied during aggregation of the vinyl chloride resin latex by the aggregating agent have most of the tertiary particles having a D50 of 10 to 60 μm disintegrated by ultrasonic irradiation to form secondary particles having a D90 of 10.5 μm or less, which makes it easier to meet the characteristic of low sol coarse particles (e.g., A-method coarse particles of 25 μm or less) required for resins for coating metal cans. Also, in the examples, it can be seen that the proportion of particles disintegrated into primary particles by ultrasonic irradiation is low, and the primary particles are strongly bonded to each other to form secondary particles, but the secondary particles are relatively loosely bonded to each other to form tertiary particles. Therefore, it is possible to provide vinyl chloride resin agglomerated particles that have a low load of pulverization and classification while maintaining the strength and size required for processes such as washing.
[0057] On the other hand, in the case of Comparative Examples 1 and 2 in which no shear force was applied by a colloid mill during aggregation of the polyvinyl chloride resin latex by the coagulant, the polyvinyl chloride resin agglomerated particles had a D90 of more than 20 μm even when irradiated with ultrasonic waves, and the load of crushing and classification to obtain low sol coarse particles (e.g., Method A coarse particles of 25 μm or less) required for metal can coating resins is high.
[0058] The present invention is not particularly limited, but may include, for example, the following embodiments. [1] A method for producing polyvinyl chloride resin agglomerated particles, comprising the steps of: A step of applying a shear force to the mixture of the polyvinyl chloride resin latex and the coagulant in a colloid mill to obtain an agglomerated latex containing polyvinyl chloride resin agglomerated particles; The coagulated latex is heat-treated at a temperature in the range of [Tg-20°C] to [Tg+35°C], where Tg is the glass transition temperature of the vinyl chloride resin; The vinyl chloride resin agglomerated particles include tertiary particles formed by further agglomeration of secondary particles formed by agglomeration of vinyl chloride resin latex particles. [2] The method for producing polyvinyl chloride resin agglomerated particles according to [1], wherein the agglomerating agent is an inorganic salt. [3] The method for producing vinyl chloride resin aggregated particles according to [1] or [2], wherein the median diameter of the secondary particles is 2.0 to 6.5 μm. [4] The method for producing vinyl chloride resin aggregated particles according to any one of [1] to [3], wherein the secondary particles have a D90 of 10.5 μm or less. [5] The method for producing vinyl chloride resin agglomerated particles according to any one of [1] to [4], wherein the vinyl chloride resin agglomerated particles include secondary particles formed by agglomeration of vinyl chloride resin latex particles. [6] The method for producing vinyl chloride resin agglomerated particles according to any one of [1] to [5], wherein the heat treatment is carried out at a temperature of Tg to [Tg+35° C.], where Tg is the glass transition temperature of the vinyl chloride resin. [7] The method for producing vinyl chloride resin agglomerated particles according to any one of [1] to [6], wherein the vinyl chloride resin agglomerated particles have a median diameter of 10 to 60 μm. [Explanation of symbols]
[0059] 1. Polyvinyl chloride resin latex particles 2 Secondary particles (polyvinyl chloride resin agglomerated particles) 3. Tertiary particles (polyvinyl chloride resin agglomerated particles)
Claims
1. A method for producing vinyl chloride resin agglomerated particles, comprising the steps of: A step of applying a shear force to the mixture of the polyvinyl chloride resin latex and the flocculant in a colloid mill to obtain an agglomerated latex containing polyvinyl chloride resin agglomerated particles; The coagulated latex is heat-treated at a temperature in the range of [Tg-20°C] to [Tg+35°C], where Tg is the glass transition temperature of the vinyl chloride resin; The vinyl chloride resin agglomerated particles include tertiary particles formed by further agglomeration of secondary particles formed by agglomeration of vinyl chloride resin latex particles.
2. The method for producing polyvinyl chloride resin aggregated particles according to claim 1 , wherein the aggregating agent is an inorganic salt.
3. 2. The method for producing vinyl chloride resin aggregated particles according to claim 1, wherein the median diameter of the secondary particles is 2.0 to 6.5 μm.
4. The method for producing vinyl chloride resin agglomerated particles according to claim 1 , wherein the secondary particles have a D90 of 10.5 μm or less.
5. The method for producing vinyl chloride resin agglomerated particles according to claim 1 , wherein the vinyl chloride resin agglomerated particles include secondary particles formed by agglomeration of vinyl chloride resin latex particles.
6. 2. The method for producing vinyl chloride resin agglomerated particles according to claim 1, wherein the heat treatment is carried out at a temperature of Tg to [Tg+35° C.], where Tg is the glass transition temperature of the vinyl chloride resin.
7. The method for producing vinyl chloride resin agglomerated particles according to any one of claims 1 to 6, wherein the vinyl chloride resin agglomerated particles have a median diameter of 10 to 60 µm.
Citation Information
Patent Citations
Vinyl chloride resin aggregate particles, production method therefor, coating composition for metal can, composition for marking film, and coating film