Method for producing resin composition and apparatus for producing resin composition

The described method and apparatus for resin composition production efficiently reduce VOCs by using a kneading extruder with strategic port and seal ring placement, ensuring high pressure and uniform aid dispersion, resulting in resin compositions with minimal residual VOCs.

JP2024137651AActive Publication Date: 2024-10-07KK TOYOTA CHUO KENKYUSHO +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023195268
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-23
Filing Date
2023-11-16
Publication Date
2024-10-07
Estimated Expiration
2043-11-16

AI Technical Summary

Technical Problem

Conventional methods for producing resin compositions fail to adequately reduce the residual amount of volatile organic compounds (VOCs), as they do not effectively disperse and remove these compounds during the devolatilization process.

Method used

A method and apparatus utilizing a kneading extruder with a specific screw configuration and seal ring arrangement, where devolatilization aid supply ports and ports are positioned upstream, and seal rings are placed between these ports, ensuring a high filling rate of raw materials (70% or more) to maintain high pressure and efficient dispersion of the aid, allowing for effective removal of VOCs.

Benefits of technology

This approach enables the production of resin compositions with significantly reduced VOC residues, achieving removal rates of 85% or more by maintaining high pressure and uniform dispersion of the devolatilization aid within the extruder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137651000001_ABST
    Figure 2024137651000001_ABST
Patent Text Reader

Abstract

To provide a method for producing a resin composition, which is capable of efficiently producing the resin composition having a sufficiently low residual amount of volatile organic compounds.SOLUTION: A method for producing a resin composition includes: a step of preparing a specific kneading extruder including a cylinder 1 in which devolatilizing agent supply ports 11A and 11B and devolatilizing ports 12A and 12B for discharging volatile components are provided so as to satisfy specific conditions, and a screw 2 having a specific screw configuration in which seal rings SR1 to SR4 are arranged at specific positions; and a conveying and kneading step of conveying and kneading a raw material fed into the cylinder 1 by using the kneading extruder. A filling rate of the raw material in at least one of the specific regions A1 and A2 in the cylinder 1 is set to 70% or more, a devolatilization agent DA is supplied to the raw material in the cylinder 1 from the devolatilization agent supply ports 11A and 11B, and the volatile components contained in the raw material are discharged from the devolatilization ports 12A and 12B to obtain the resin composition.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a resin composition and an apparatus for producing a resin composition. [Background technology]

[0002] Conventionally, in the field of resin compositions, it has been proposed to produce resin compositions using a kneading extruder capable of devolatilization in order to volatilize and remove volatile organic compounds (VOCs) such as residual solvents and residual monomers contained in the composition. In recent years, from the viewpoint of environmental protection and the like, there has been a strong social demand for the recycling of resin compositions, and there is a demand for recycling and using resin compositions. Even when producing such recycled resin compositions, it has been proposed to produce (reproduce) resin compositions using a kneading extruder capable of devolatilization in order to remove volatile organic compounds contained in the resin composition.

[0003] As a method for producing a resin composition using a kneading extruder capable of such a devolatilization process, for example, Patent Document 1 (JP 2021-62552 A) discloses a method for producing a resin composition, which includes: (a) preparing an extruder having a cylinder, a screw rotatably arranged in the cylinder, and a rotary drive mechanism for rotating the screw, in which a melt kneading section and a devolatilization section are arranged in sequence from the upstream side; (b) kneading a molten resin obtained by melting a thermoplastic resin with an additive in the melt kneading section of the extruder; (c) dispersing the devolatilization assistant in the thermoplastic resin by adding and kneading the devolatilization assistant in a first part of the devolatilization section of the extruder; and (d) removing volatile components from the kneaded product of the thermoplastic resin and the additive together with the devolatilization assistant by creating a reduced pressure state in a second part of the devolatilization section of the extruder. In addition, non-patent literature 1 (Leaflet (NL-J0014-02) of the Plastics Machinery Division of the Hiroshima Works of the Japan Steel Works, Ltd., "Introduction to the Effect of Adding Water and Devolatilizing TEX" and Internet<URL:https: / / www.jsw.co.jp / ja / product / news / details / 20211001000006.html> ) discloses a technique of using a kneading extruder equipped with seal rings before and after the hydrogenation section as a screw design suitable for low viscosity resins. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2021-62552 [Non-patent literature]

[0005] [Non-Patent Document 1] Japan Steel Works, Ltd. Hiroshima Works Plastics Machinery Division leaflet (NL-J0014-02), "Introduction to the Effect of Adding Water to TEX and Devolatilizing," Internet<URL:https: / / www.ipros.jp / catalog / detail / 557129 / > Summary of the Invention [Problem to be solved by the invention]

[0006] However, the conventional methods for producing resin compositions as described in Patent Document 1 and Non-Patent Document 1 are not sufficient in terms of reducing the amount of volatile organic compounds remaining in the obtained resin composition.

[0007] The present invention has been made in consideration of the problems associated with the above-mentioned conventional techniques, and aims to provide a resin composition manufacturing method capable of efficiently manufacturing a resin composition having a sufficiently low residual amount of volatile organic compounds, and a resin composition manufacturing apparatus that can be suitably used for the method. [Means for solving the problem]

[0008] As a result of intensive research by the inventors in order to achieve the above object, the present inventors have found a method for producing a fuel cell system comprising: a cylinder; and a screw disposed within the cylinder; the cylinder has at least one devolatilizing agent supply port and at least one devolatilizing port for discharging volatile components as openings, and has at least one structural portion in which the devolatilizing agent supply port and the devolatilizing port are provided in sequence from the upstream side with a space therebetween; the screw has at least one screw configuration in which seal rings are respectively disposed at an upstream supply port portion in the cylinder located upstream of a position where the devolatilizing agent supply port of the at least one structural portion is provided, and at a downstream supply port portion of the structural portion located between the devolatilizing agent supply port and the devolatilizing port; and the cylinder is provided with no openings other than the devolatilizing aid supply port, which serves as a reference for the position of the flow section, that connect the aforementioned region with the outside of the cylinder; and the kneading extruder is used to produce a resin composition, and the raw materials for the resin composition supplied into the cylinder by the screw are kneaded while being transported from the upstream side to the downstream side, with the raw materials being filled with 70% or more in at least one region within the cylinder between the upstream part of the supply port, where the seal ring is located, and the downstream part of the supply port, and the volatile components contained in the raw materials are discharged from the devolatilizing aid supply port while a devolatilizing aid is supplied to the raw materials in the cylinder from the devolatilizing aid supply port. This has led to the completion of the present invention.

[0009] That is, the present invention provides the following aspects.

[0010] [1] A cylinder and a screw disposed in the cylinder, the cylinder has at least one devolatilizing agent supply port and at least one devolatilizing port for discharging volatile components as openings, and has at least one structural portion in which the devolatilizing agent supply port and the devolatilizing port are arranged in sequence from the upstream side with a gap therebetween, The screw has at least one screw configuration in which a seal ring is disposed at an upstream portion of a supply port in the cylinder located upstream of a position where the devolatilizing agent supply port of at least one of the structural parts is provided, and at a downstream portion of a supply port located between the devolatilizing agent supply port and the devolatilizing port of the structural part, and in a region between the upstream portion of the supply port and the downstream portion of the supply port where the seal ring is arranged, no opening is provided that connects the region with the outside of the cylinder, other than the devolatilizing agent supply port that serves as a reference for the positions of the upstream portion of the supply port and the downstream portion of the supply port; A kneading extruder preparation step of preparing a kneading extruder; a conveying and kneading step of conveying and kneading the raw material of the resin composition supplied into the cylinder by the screw from the upstream side to the downstream side using the kneading extruder; Including, a filling rate of the raw material in at least one region in the cylinder between the upstream portion of the supply port where the seal ring is located and the downstream portion of the supply port is set to 70% or more, a devolatilizing agent is supplied to the raw material in the cylinder from the devolatilizing agent supply port, and a volatile component contained in the raw material is discharged from the devolatilizing port, thereby obtaining a resin composition.

[0011] [2] The method for producing a resin composition described in [1], in the conveying and kneading process, the filling rate of the raw material in the area within the cylinder between the upstream part of the supply port where the seal ring is located and the downstream part of the supply port is 80% or more.

[0012] [3] The method for producing a resin composition according to [1] or [2], wherein the devolatilizing aid is water.

[0013] [4] A cylinder; A screw disposed within the cylinder; a screw drive device for driving the screw; A raw material supplying device for supplying raw material into the cylinder; a devolatilization aid supplying device for supplying a devolatilization aid into the cylinder; a temperature control device for controlling the temperature of the cylinder; a control device electrically connected to the screw drive device, the raw material supply device, the devolatilization aid supply device, and the temperature adjustment device, for controlling the operation of each of the devices; The kneading extruder comprises: the cylinder has at least one devolatilizing agent supply port and at least one devolatilizing port for discharging volatile components as openings, and has at least one structural portion in which the devolatilizing agent supply port and the devolatilizing port are arranged in sequence from the upstream side with a gap therebetween, the screw has at least one screw configuration in which a seal ring is disposed at an upstream portion of a supply port in the cylinder located upstream of a position where the devolatilizing agent supply port of at least one of the structural parts is provided, and at a downstream portion of a supply port located between the devolatilizing agent supply port and the devolatilizing port of the structural part, the kneading extruder satisfies the condition that, in a region between the upstream portion of the supply port and the downstream portion of the supply port where the seal ring is arranged, no opening is provided that connects the region with the outside of the cylinder, other than the devolatilizing agent supply port that serves as a reference for the positions of the upstream portion of the supply port and the downstream portion of the supply port; The kneading extruder is a device used for producing a resin composition by conveying the raw material of the resin composition supplied into the cylinder by the screw from the upstream side to the downstream side while kneading the raw material, the control device controls operation of the screw drive device, the raw material supply device, the devolatilization aid supply device and the temperature adjustment device so that, when the raw materials are kneaded while being transported from the upstream side to the downstream side during the production of a resin composition, a devolatilization aid is supplied to the raw materials in the cylinder from the devolatilization aid supply port while maintaining a filling rate of the raw materials of 70% or more in at least one region in the cylinder between the upstream part of the supply port where the seal ring is located and the downstream part of the supply port, and volatile components contained in the raw materials are discharged from the devolatilization port.

[0014] [5] The kneading extruder further includes a pressure reducing device connected to the devolatilization port, The control device is also electrically connected to the pressure reducing device; and The apparatus for producing a resin composition according to [4], wherein the control device controls operation of the screw drive device, the raw material supply device, the devolatilization aid supply device, and the temperature control device, as well as controlling operation of the pressure reduction device, during the production of the resin composition.

[0015] The reason why the resin composition manufacturing method and the resin composition manufacturing apparatus of the present invention achieve the above object is not necessarily clear, but the present inventors speculate as follows. That is, the present inventors have conducted extensive research and examined the techniques described in the above-mentioned Patent Document 1 and Non-Patent Document 1. As a result, the present inventors have concluded that the technique described in Patent Document 1 cannot sufficiently increase the pressure in the cylinder when kneading the raw material to which the devolatilizing agent has been added, and therefore the devolatilizing agent in the raw material becomes gaseous from the stage before devolatilization using a vacuum pump (reducing pump) from the devolatilization vent, and therefore the liquid devolatilizing agent cannot be sufficiently dispersed in the raw material, and the volatile organic compounds cannot be sufficiently removed. Furthermore, the present inventors have concluded that when a kneading extruder such as that described in Non-Patent Document 1 is used, depending on the operating conditions of the kneading extruder (for example, the speed at which the raw material is fed into the cylinder, etc.), the pressure in the cylinder when the devolatilizing agent is added and kneaded cannot necessarily be sufficiently increased, and therefore the volatile organic compounds cannot necessarily be sufficiently removed. As described above, the present inventors have conducted extensive research and found that the conventional resin composition manufacturing method described in Patent Document 1 and Non-Patent Document 1 has a problem with the pressure in the cylinder when adding and kneading a devolatilizing agent. In consideration of such a problem, the present invention uses the specific kneading extruder according to the present invention as described above, and sets the filling rate of the raw material to 70% or more in at least one of the regions in the cylinder between the upstream part of the supply port where the seal ring is arranged and the downstream part of the supply port (the region sandwiched between the two seal rings: the region where the devolatilizing agent is added and the raw material containing the devolatilizing agent is kneaded). As a result, when the devolatilizing agent is supplied to the raw material in the cylinder from the devolatilizing agent supply port, the pressure in the region in the cylinder is kept sufficiently high, and the occurrence of a problem such as the devolatilizing agent volatilizing in the region due to low pressure is sufficiently suppressed regardless of the speed at which the raw material is fed into the cylinder of the kneading extruder.Therefore, when the raw materials and the devolatilizing aid are kneaded, it becomes possible to knead the liquid devolatilizing aid with the raw materials under high pressure conditions, and it becomes possible to more thoroughly disperse the devolatilizing aid in the raw materials (the raw materials for the molten resin composition) and distribute it more uniformly while fully maintaining the liquid state of the devolatilizing aid. When volatile components (gas produced by volatilization of volatile organic compounds and the devolatilizing aid, etc.) are devolatilized through the devolatilizing port located in an area further downstream of the seal ring downstream of the supply port, it becomes possible to more efficiently discharge (devolatilize) the volatile organic compounds at a higher level, and the inventors presume that this makes it possible to efficiently produce a resin composition having a sufficiently low remaining amount of volatile organic compounds. Effect of the Invention

[0016] According to the present invention, it is possible to provide a resin composition manufacturing method capable of efficiently manufacturing a resin composition having a sufficiently low residual amount of volatile organic compounds, and a resin composition manufacturing apparatus that can be suitably used for the method. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a cross section of a preferred embodiment of a kneading extruder that can be used in the method for producing a resin composition of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a cross section of another preferred embodiment of a kneading extruder that can be used in the method for producing a resin composition of the present invention. [Diagram 3] FIG. 2 is a schematic cross-sectional view showing a cross section of another preferred embodiment of a kneading extruder that can be used in the method for producing a resin composition of the present invention. [Figure 4] 1 is a schematic cross-sectional view showing a cross section of a preferred embodiment of an apparatus for producing a resin composition of the present invention. [Diagram 5] 1 is a flowchart showing an example of a suitable procedure for determining necessary operating conditions using mixing simulation software (manufactured by Japan Steel Works, Ltd., product name: TEX-FAN). [Figure 6]FIG. 2 is a schematic cross-sectional view showing a cross section of a kneading extruder used in Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings. In the following description and drawings, the same or corresponding elements are designated by the same reference numerals, and duplicated explanations will be omitted.

[0019] [Preferable embodiment of the method for producing the resin composition of the present invention] First embodiment <Kneading extruder preparation step> In the present invention, a kneading extruder is prepared in the kneading extruder preparation step. Fig. 1 is a schematic cross-sectional view showing a cross section of a preferred embodiment of such a kneading extruder according to the present invention. In this specification, when describing the positional relationship of each component (screw element, etc.), the expressions "upstream" and "downstream" or "upstream side" and "downstream side" are used with respect to the conveying direction (flow direction) of the raw material (including the molten kneaded product) of the resin composition.

[0020] The kneading extruder of the embodiment shown in FIG. 1 is a twin-screw kneading extruder (screw-type kneading devolatilizing extruder) including a cylinder 1, a screw 2 disposed in the cylinder 1, and a hopper 3 for supplying raw materials connected to the upstream part of the cylinder 1 (for convenience, only the screw on one shaft side is depicted in FIG. 1). The screw 2 is connected to a rotary drive mechanism (not shown) and is in a rotatable (freely rotatable) state inside the cylinder 1. The kneading extruder shown in FIG. 1 is designed so that the downstream end of the cylinder 1 is connected to a die (not shown), and a melt-kneaded resin composition is extruded (discharged) from the die during use to obtain a resin composition from which VOCs have been devolatilized. Furthermore, in the kneading extruder of the embodiment shown in FIG. 1, a heater (not shown) is installed outside the entire region of the cylinder 1, and the cylinder is heated to a heating temperature (set temperature) appropriately set according to the type of raw material, and the raw material is melted and kneaded.

[0021] The cylinder 1 is provided with openings, devolatilization assistant supply ports (DA supply ports) 11A and 11B for supplying the devolatilization assistant DA, and devolatilization ports (vent ports) 12A and 12B for discharging the devolatilized component VOC. The DA supply ports 11A and 11B are each connected to a supply device for the devolatilization assistant DA (not shown) (for example, when the devolatilization assistant DA is water, a device capable of injecting water (water injection device)). The devolatilization ports 12A and 12B are each connected to a pressure reducing device (vacuum pump) not shown. In FIG. 1, the cylinder 1 is also provided with an opening (raw material supply port) 13 for supplying raw material (raw material for the resin composition) from the hopper 3.

[0022] In this way, the cylinder 1 is provided with two DA supply ports 11A and 11B, two devolatilization ports (vent ports) 12A and 12B, and a raw material supply port 13 as openings. In addition, the cylinder 1 has a structural portion in which the DA supply port 11A and the devolatilization port 12A are arranged in sequence from the upstream side to the downstream side with a space therebetween, and a structural portion in a region further downstream of the structural portion in which the DA supply port 11B and the devolatilization port 12B are arranged in sequence from the upstream side to the downstream side with a space therebetween. By having such a structural portion, it becomes possible to knead the devolatilization assistant DA introduced from the DA supply port and the raw material in each structural portion, and then transport the kneaded product to the region in which the devolatilization port is provided for devolatilization, and in combination with the screw configuration described later, it becomes possible to discharge (devolatilize) the volatile organic compound VOC as a volatile component from the devolatilization port at a higher level and more efficiently.

[0023] From the viewpoint of enabling more efficient removal of VOCs, the ratio of length to diameter (length / diameter) of the cylinder 1 is preferably 21 to 106. Furthermore, even when the raw material is in the form of pellets, the diameter of the cylinder 1 is preferably 12 to 90 mm from the viewpoints that no particular problem occurs in kneading the pellets and heat generation during kneading can be more sufficiently suppressed.

[0024] The screw 2 is formed by attaching various screw elements (screw segments: screw pieces) to a shaft (axis). The screw 2 is provided with a full flight screw FS and a kneading disk KD (indicated as KD in FIG. 1) on the shaft (axis). 1~3 ) and the seal ring SR (in Fig. 1, it is indicated by the symbol SR 1~4The full-flight screw FS is used mainly for the purpose of transporting the raw material of the resin composition from the upstream side to the downstream side, the kneading disk KD is used for kneading (melting and kneading) the raw material, and the seal ring SR is used to block the flow of the raw material and increase the pressure of the raw material in the cylinder.

[0025] Here, regarding the configuration of the screw 2, the positional relationship of the portions where the seal rings are arranged in the screw configuration portion in which the seal ring SR1, kneading disk KD2, and seal ring SR2 are arranged in this order will be described based on the positions of the DA supply port 11A and the devolatilization port 12A of the cylinder 1. The seal ring SR1 is arranged at a position upstream of the position where the DA supply port 11A is provided (upstream of the upstream end (upstream end) of the DA supply port 11A). The seal ring SR2 is arranged at a position downstream of the position where the DA supply port 11A is provided (downstream of the downstream end (downstream end) of the DA supply port 11A), and is arranged at a position between the DA supply port 11A and the devolatilization port 12A. In other words, when the positional relationship of the arrangement of the seal ring SR is considered, focusing on the structural portion where the DA supply port 11A and the devolatilization port 12A of the cylinder 1 are arranged side by side, the screw 2 has a screw configuration in which the seal ring SR1 is arranged upstream of the position where the DA supply port 11A of the cylinder 1 is arranged (the portion upstream of the DA supply port 11A where the seal ring SR1 in the cylinder 1 is arranged is referred to as the "upstream supply port portion"), and the seal ring SR2 is arranged between the DA supply port 11A and the devolatilization port 12A (downstream of the DA supply port 11A) (the portion downstream of the DA supply port 11A where the seal ring SR2 in the cylinder 1 is arranged is referred to as the "downstream supply port portion"). On the other hand, in the region A1 between the upstream supply port (the portion where the seal ring upstream of the reference devolatilizing agent supply port is disposed) and the downstream supply port (the portion where the seal ring downstream of the reference devolatilizing agent supply port is disposed), other than the DA supply port 11A (the opening that serves as the reference for the position of the upstream supply port and the downstream supply port), no opening is provided that connects the region A1 with the outside of the cylinder 1 (note that the "region A1" based on the DA supply port 11A here means the region within the cylinder sandwiched between a plane including the downstream end face of the seal ring SR1 and perpendicular to the axis of the cylinder (a plane including the upstream end of the kneading disc KD2 and perpendicular to the axis of the cylinder) and a plane including the upstream end face of the seal ring SR2 and perpendicular to the axis of the cylinder (a plane including the downstream end of the kneading disc KD2 and perpendicular to the axis of the cylinder).Thus, in this specification, "the region in the cylinder between the upstream portion of the supply port and the downstream portion of the supply port where the seal ring is arranged" means the region in the cylinder between a plane including the downstream end face of the seal ring (the upstream seal ring) arranged in the upstream portion of the supply port and perpendicular to the axis of the cylinder, and a plane including the upstream end face of the seal ring arranged in the downstream portion of the supply port and perpendicular to the axis of the cylinder.) Also, based on the structural portion in which the DA supply port 11B and the devolatilization port 12B of the cylinder 1 are provided side by side, the seal ring SR is provided. 3~4 Focusing on the arrangement positions, in this embodiment, the screw configuration has a seal ring SR3 and a seal ring SR4 respectively arranged at the upstream supply port portion (the portion upstream of the DA supply port 11B) upstream of the position where the DA supply port 11B is provided, and at the downstream supply port portion (the portion downstream of the DA supply port 11B) between the DA supply port 11B and the devolatilization port 12B and downstream of the DA supply port 11B. 3~4 When focusing on the above, the region A2 between the upstream part of the supply port and the downstream part of the supply port in the cylinder 1 does not have any openings other than the DA supply port 11B (an opening that serves as a reference for the positions of the upstream part of the supply port and the downstream part of the supply port). Therefore, in the embodiment of the kneading extruder shown in FIG. 1, the regions A1 and A2 are zones where a devolatilizing agent DA (preferably water) is added (supplied) and kneaded. In this way, the region (A1, A2) in the cylinder between the upstream part of the supply port and the downstream part of the supply port where the seal ring is arranged, which is the zone where the devolatilizing agent DA is added (supplied) and kneaded, will hereinafter be referred to simply as the "DA addition and kneading region" for convenience.

[0026] Furthermore, the diameter D of the screw 2 is not particularly limited, but is preferably 80 to 99.5% of the diameter of the cylinder 1. When the ratio of the diameter D of the screw 2 to the diameter of the cylinder 1 is equal to or greater than the lower limit, the resin composition tends to be kneaded more thoroughly compared to when the ratio is less than the lower limit, and on the other hand, when the ratio is equal to or less than the upper limit, interference between the screw and the cylinder is less likely to occur (basically no interference occurs) compared to when the ratio exceeds the upper limit, so that more stable processing tends to be possible.

[0027] Such a screw 2 is not particularly limited, but when the length (total length) of the screw is L and the diameter (outer diameter) of the screw is D, the L / D value of the screw is preferably 20 to 105, and more preferably 25 to 100. When such an L / D value is equal to or greater than the lower limit, the resin composition tends to be kneaded more thoroughly than when it is less than the lower limit, and when it is equal to or less than the upper limit, the excessive increase in kneading torque can be suppressed compared to when it exceeds the upper limit, and more stable processing tends to be possible. Note that the "screw length" referred to here refers to the total length of the portion where the screw elements are arranged, that is, the total length in the conveying direction of the portion that functions as a screw formed by combining multiple elements.

[0028] In addition, in the screw 2, it is preferable that the ratio (L1 / D) of the screw length L1 (the length between the downstream end of the seal ring SR1 and the upstream end of the seal ring SR2) to the screw diameter D is 2 or more (more preferably 5 to 50). In addition, it is preferable that the ratio (L2 / D) of the screw length L2 (the length between the downstream end of the seal ring SR3 and the upstream end of the seal ring SR4) to the screw diameter D is also 2 or more (more preferably 2 to 50). In this way, when one DA supply port (11A or 11B) is used as a reference, the screw length (L2) of the range sandwiched between the downstream end of the seal ring (SR1 or SR3) located upstream of that supply port and the upstream end of the seal ring (SR2 or SR4) located downstream of that supply port is set to 2 or more (more preferably 2 to 50). I or L2) and the screw diameter D (L I It is preferable that L2 / D or L2 / D) is 2 or more (more preferably 2 to 50). I If the value of L2 / D or L2 / D is less than the lower limit, the mixing of the devolatilizing agent and the resin composition tends to be insufficient. I When the value of / D is equal to or less than the upper limit, an excessive increase in the kneading torque can be suppressed more effectively than when the value exceeds the upper limit, and more stable processing can be achieved.

[0029] Furthermore, in such a screw 2, the length (distance in the conveying direction) of the region where the kneading disc KD1 is located (the region where the raw materials are first kneaded) can be designed appropriately depending on the type of raw materials, etc., and is not particularly limited, but it is preferable that the length is 1 to 30 times (more preferably 2 to 25 times) the diameter D of the screw so that the molten raw materials can be more reliably supplied to the region A1 (DA addition kneading region).

[0030] In the kneading extruder of the above embodiment, the raw material (molten kneaded material) passing through the volatilization port 12A and transported downstream is blocked by the seal ring SR3 arranged downstream of the volatilization port 12A, slowing down the transport speed. However, depending on the positional relationship between the volatilization port 12A and the seal ring SR3, the feed rate of the raw material, the rotation speed of the screw, etc., problems may occur such as the material flowing out of the volatilization port 12A to the outside of the cylinder 1. Therefore, it is desirable to appropriately set the distance from the downstream end of the volatilization port 12A to the upstream end of the seal ring SR3 to a length that prevents the molten kneaded material from flowing out of the volatilization port 12A during operation of the kneader, taking into account the operating conditions actually adopted, etc., and it is preferable that the distance in the transport direction between the volatilization port and the seal ring downstream of the volatilization port (for example, the distance between the position of the downstream end of the volatilization port 12A and the position of the upstream end of the seal ring SR3) is 1 to 30 times (more preferably 3 to 25 times) the diameter D of the screw.

[0031] In addition, in the screw 2, the length (distance in the conveying direction) between the downstream end of the seal ring SR2 and the upstream end of the seal ring SR3 is preferably 2 to 30 times (more preferably 4 to 25 times) the diameter D of the screw, from the viewpoint of the removal rate of the volatile components.

[0032] Furthermore, in the screw 2, the length (distance in the conveying direction) L3 between the upstream end position of the seal ring SR1 and the downstream end position of the raw material supply port is preferably 3 to 30 times (more preferably 5 to 25 times) the diameter D of the screw.

[0033] The other components of the hopper 3, the dies, etc. are not particularly limited, and known components may be used as appropriate, and may be appropriately arranged so as to perform the functions required for the purpose.

[0034] The kneading extruder of the embodiment shown in FIG. 1 as described above uses a cylinder 1 having two devolatilizing agent supply ports (11A, 11B) and two devolatilizing ports (12A, 12B) for discharging volatile components as openings, and having two structural parts in which the devolatilizing agent supply ports and the devolatilizing ports are arranged side by side with a gap therebetween in order from the upstream side, and As the screw 1, when the screw configuration is considered based on the positions of the devolatilizing agent supply port and the devolatilizing port in each of the structural parts, respectively, two screw configurations are used in which seal rings are arranged at the upstream portion of the supply port in the cylinder located upstream of the position where the devolatilizing agent supply port is provided, and at the downstream portion of the supply port located between the devolatilizing agent supply port and the devolatilizing port.

[0035] Using such a cylinder 1, a seal ring SR 1~4 By using the screw 2 in the position as described above, and by setting the filling rate of the raw materials in at least one region (region A1 and / or A2) among the regions in the cylinder 1 where the devolatilization aid can be introduced by the DA supply port and which are sandwiched by the seal ring SR (DA addition kneading regions: regions A1 and A2) to 70% (volume %) or more, it becomes possible to knead the raw materials of the resin composition and the devolatilization aid DA under high pressure conditions in that region, and it becomes possible to highly suppress the devolatilization aid DA from becoming in a gaseous state (volatilized state) in that region during kneading. This makes it possible to knead the raw materials of the resin composition with the devolatilization aid DA that is sufficiently maintained in a liquid state in that region, and the devolatilization aid DA can be more thoroughly dispersed and spread more uniformly in the raw materials during kneading in that region, and it becomes possible to more efficiently devolatilize volatile organic compounds VOCs at a higher level in the devolatilization port located in a region further downstream of the seal ring (downstream sealing) arranged downstream of the supply port.

[0036] <Conveying and kneading process> In the first embodiment, after preparing the kneading extruder shown in FIG. 1 as described above, the conveying and kneading step is carried out using the kneading extruder.

[0037] When the kneading extruder of the embodiment shown in FIG. 1 is used and operated to carry out the conveying and kneading process, first, while heating the cylinder 1 to a set temperature, the raw material of the resin composition is charged into the cylinder through the hopper 3, and the charged raw material is conveyed in the conveying direction shown in FIG. 1 by the full-flight screw SF, reaches the area where the kneading disk KD1 is arranged, and in the area where the kneading disk KD1 is arranged, the first melt-kneading of the raw material is carried out. Next, the melt-kneaded raw material (melt-kneaded product) is conveyed by the full-flight screw SF on the downstream side adjacent to the kneading disk KD1 to the area where the seal ring SR1 is arranged (the supply port upstream part of the DA supply port 11A), passes through the area where the seal ring SR1 is arranged, and is conveyed into the area A1 (the area where the kneading disk KD2 is arranged: the first DA addition kneading area) and kneaded by the kneading disk KD2. During the kneading in the region A1, a devolatilizing agent DA (preferably water) is added from the DA supply port 11A to knead the molten raw material with the liquid devolatilizing agent DA. Then, when the molten kneaded material (molten raw material) to which the liquid devolatilizing agent DA is added and kneaded passes through the area (downstream of the supply port) where the seal ring SR2 is located downstream of the region A1, the molten raw material is conveyed further downstream by the full-flight screw SF located downstream of the seal ring SR2 adjacent to the seal ring SR2. At this time, the pressure (internal pressure of the molten kneaded material) in the area (vent part) near the devolatilizing port (vent port) 12A can be made low (preferably about 1 to 100 kPa) by operating a vacuum pump (not shown) connected to the devolatilizing port 12A, which makes it possible to vaporize the devolatilizing agent DA from the molten kneaded material present near the devolatilizing port 12A and volatilize volatile organic compounds, and the volatilized components can be discharged from the devolatilizing port 12A. In addition, by using a devolatilizing agent, the devolatilizing agent in the raw material vaporizes and expands in the vent section, increasing the surface area of ​​the raw material, thereby improving the effect of volatilizing and removing the internal volatile components from the high-temperature surface of the raw material, and making it possible to more efficiently volatilize the volatile organic compounds during devolatilization.The raw material after devolatilization is then transported to the area where the seal ring SR3 is arranged, passes through the area where the seal ring SR3 is arranged, and is transported into area A2 (area where the kneading disk KD3 is arranged: second DA addition kneading area) and kneaded by the kneading disk KD3. In area A2, a devolatilization aid DA (preferably water) is added from the DA supply port 11B, and the molten raw material and the devolatilization aid DA are kneaded. After that, when the molten kneaded product (molten raw material) to which the devolatilization aid DA has been added passes through the area where the seal ring SR4 downstream of area A2 is arranged, it is transported further downstream by the full flight screw SF arranged adjacent to and downstream of the seal ring SR4. Then, when passing through the position where the volatilization port 12B is arranged by such conveyance, the pressure in at least the region near the volatilization port 12B can be made low by operating a vacuum pump (not shown) connected to the volatilization port 12B, which makes it possible to volatilize the volatilization assistant and the volatile organic compounds from the raw materials present in the vicinity of the volatilization port 12B, and discharge them from the volatilization port 12B. In this way, after the volatile components (including volatile organic compounds) are volatilized, the molten kneaded material after volatilization is conveyed as it is to the outlet of the cylinder. After the raw materials are conveyed from the upstream side to the downstream side in the cylinder in this way and kneaded, the raw materials are conveyed to the outlet of the cylinder and extruded to the outside from a die (not shown) connected to the outlet portion to obtain a resin composition. In this way, by using and operating the kneading extruder, the raw materials of the resin composition supplied into the cylinder 1 by the screw 2 can be kneaded while being conveyed from the upstream side to the downstream side to obtain a resin composition.

[0038] In such a process, the raw material of the resin composition to be supplied into the cylinder is not particularly limited, and may contain at least one type of resin. Such a resin is preferably a thermoplastic resin, and examples thereof include polyolefin resins (polyethylene, polypropylene, etc.), polyamide resins, polyester resins, polycarbonate resins, acrylic resins, styrene resins, vinyl chloride resins, polyphenylene sulfide, polyphenylene oxide, thermoplastic elastomers, etc. The resins contained in the resin composition may be used alone or in combination of two or more types. In addition, as the raw material of such a resin composition, a resin composition extracted from a discarded product may be used in order to reuse the resin composition. In addition, the components other than the resin in the resin composition are not particularly limited, and known components such as various fillers and pigments can be appropriately used depending on the design of the intended resin composition. In addition, the raw material may be a form consisting of a single resin that does not contain components such as fillers (because even a single resin that does not contain fillers, etc. can be recognized as a resin composition containing volatile organic compounds (volatile low molecular weight organic substances) such as monomers as impurities). Furthermore, the form of the raw material for such a resin composition is not particularly limited, but it is preferable to use a pellet or powder form, since this makes melt-kneading easier.

[0039] The devolatilizing aid DA is not particularly limited, and known components such as water, alcohol, and lower aliphatic hydrocarbons can be appropriately used, but water is more preferred from the viewpoint of improving operational safety. When water is used as the devolatilizing aid DA, the water may contain additives.

[0040] In the conveying and kneading step, in at least one region (DA-added kneading region) in the cylinder between the upstream portion of the supply port where the seal ring is arranged and the downstream portion of the supply port (in the case where there are a plurality of DA-added kneading regions, in at least one of the regions, on the other hand, in the case where there is only one DA-added kneading region in the cylinder and there are not a plurality of DA-added kneading regions, in the one DA-added kneading region), the filling rate of the raw material needs to be 70% or more (more preferably 80% or more, and even more preferably 85 to 100%). If the filling rate of the raw material is less than the lower limit, the remaining amount of volatile organic compounds cannot be sufficiently reduced, and the desired resin composition cannot be obtained. In the present invention, the "filling rate of the raw material" is the ratio of the raw material to the total volume of the DA-added kneading region (total volume of the space excluding the volume of the screw) (filling rate: volume %), which is obtained by analysis using kneading simulation software (manufactured by Japan Steel Works, Ltd., product name: TEX-FAN). In addition, such a filling rate can be adjusted by controlling the operation (including the feed rate of the raw materials, etc.) according to the design of the kneading extruder. In the present invention, it is sufficient that the filling rate of the raw materials is 70% or more in at least one DA-added kneading region in the cylinder, but since it is possible to remove (reduce) the residual volatile organic compounds at a higher level, it is more preferable to set the filling rate of the raw materials to 70% or more in all DA-added kneading regions present in the cylinder (all of regions A1 and A2 in the embodiment of FIG. 1).

[0041] Furthermore, in the conveying and kneading step, it is preferable to control the operation of the kneading extruder (including the input amount of raw materials, etc.) according to the design of the kneading extruder so that the residence time of the raw materials (molten kneaded product) of the resin composition flowing into the DA addition kneading region where the filling rate of the raw materials is 70% or more is 10 seconds or more (more preferably 20 seconds or more, and even more preferably 30 seconds or more and 600 seconds or less). By setting the residence time of the raw materials in the DA addition kneading region within the above range, it is possible to more efficiently remove VOCs while suppressing thermal decomposition of the resin composition. Note that such residence time (residence time of the raw materials from when they flow into the region until when they flow out) is a value obtained by analysis using kneading simulation software (manufactured by Japan Steel Works, Ltd., product name: TEX-FAN).

[0042] In the conveying and kneading step, the internal pressure of the raw material (molten resin composition) in the cylinder in the DA addition kneading region is preferably set to a pressure higher than the vapor pressure of the devolatilizing aid at the temperature of the DA addition kneading region, for example, when the devolatilizing aid is water and the heating temperature is 170° C., the saturated vapor pressure of water is 0.792 MPa, so it is preferable to set the pressure higher than this. In this way, by supplying (injecting) the devolatilizing aid at an internal pressure of the resin composition in the DA addition kneading region higher than the vapor pressure of the devolatilizing aid, the volatilization of the devolatilizing aid is sufficiently suppressed and the devolatilizing aid is easily maintained in a liquid state, making it possible to disperse and knead a sufficient amount of liquid devolatilizing aid in the resin composition.

[0043] The amount of degassing aid added to the raw material (molten resin composition) present in the DA addition kneading region may be appropriately adjusted depending on the type of raw material, etc., and is not particularly limited. However, from the viewpoint of enabling more efficient removal of VOCs while suppressing an excessive increase in kneading torque, it is preferable that the amount be 0.01 to 20 parts by mass (more preferably 0.01 to 15 parts by mass, even more preferably 0.01 to 0.5 parts by mass, and particularly preferably 0.02 to 0.3 parts by mass) per 100 parts by mass of the raw material in the DA addition kneading region.

[0044] In the conveying and kneading step, the supply rate of the raw material of the resin composition into the cylinder is not particularly limited, but is preferably 1 to 1000 kg / h (more preferably 2 to 800 kg / h). When the supply rate of such raw material is equal to or higher than the lower limit, a higher effect in terms of improving the treatment speed tends to be obtained compared to when it is below the lower limit, while when it is equal to or lower than the upper limit, a higher effect in terms of improving the VOC removal rate tends to be obtained compared to when it exceeds the upper limit.

[0045] In this manner, in the process of kneading the raw materials of the resin composition supplied into the cylinder 1 by the screw 2 while conveying them from the upstream side to the downstream side using the kneading extruder of the embodiment shown in FIG. 1, the filling rate of the raw materials in at least one or both of the DA addition kneading regions (regions in the cylinder between the upstream part of the supply port where the seal ring SR is located and the downstream part of the supply port: regions A1 and A2 in FIG. 1) is set to 70% or more, and a devolatilization aid DA is supplied from the devolatilization aid supply ports (11A, 11B) to the raw materials in the cylinder 1 while the volatile components contained in the raw materials are discharged from the devolatilization ports (12A, 12B), thereby obtaining a resin composition from which volatile organic compounds have been devolatilized at a sufficiently high level.

[0046] Although a preferred embodiment of the method for producing a resin composition of the present invention has been described above with reference to Fig. 1, the method for producing a resin composition of the present invention is not limited to the above embodiment. Hereinafter, other preferred embodiments of the method for producing a resin composition of the present invention will be described with reference to Figs. 2 and 3.

[0047] Second Embodiment In the second embodiment, except that a kneading extruder having a configuration as shown in FIG. 2 is prepared in the kneading extruder preparation step, the same steps as those in the first embodiment can be basically adopted, and a desired resin composition can be obtained.

[0048] The kneading extruder of the embodiment shown in Fig. 2 is basically the same as the kneading extruder of the embodiment shown in Fig. 1, except for the length (distance in the conveying direction) L3 between the upstream end position of the seal ring SR1 and the downstream end position of the raw material supply port, the positional relationship of the two DA supply ports 11A and 11B and the two devolatilization ports (vent ports) 12A and 12B, and the screw configuration in the regions A1 and A2 (DA addition kneading region) being a combination of a kneading disk KD and a flight screw. In the embodiment shown in Fig. 2, the screw configuration is a configuration in which FS, KD1, FS, SR1, KD2, FS, KD2, SR2, FS, SR3, KD3, FS, KD3, SR4, FS are arranged in this order from the upstream side to the downstream side.

[0049] Here, in the kneading extruder of the embodiment shown in Fig. 2, the length between the upstream end position of the seal ring SR1 and the downstream end position of the raw material supply port is longer than that of the embodiment shown in Fig. 1, but the length (distance in the conveying direction) L3 between the upstream end position of the seal ring SR1 and the downstream end position of the raw material supply port is configured to be within the same range as the above-mentioned range (3 to 30 times (more preferably 5 to 25 times) the diameter D of the screw), and this makes it possible to obtain a molten kneaded product in which the raw material is sufficiently melted in the region upstream of the region A1. Note that by making the length between the upstream end of the seal ring SR1 and the downstream end of the raw material supply port longer, there is an advantage in that it is possible to remove VOCs with low boiling points in advance.

[0050] In addition, in the kneading extruder of the embodiment shown in Fig. 2, the positional relationship of the two DA supply ports 11A and 11B and the two devolatilization ports (vent ports) 12A and 12B is changed compared to the first embodiment, but this is due to the fact that the length between the upstream end of the seal ring SR1 and the downstream end of the raw material supply port is longer in the embodiment shown in Fig. 2 compared to the embodiment shown in Fig. 1. In this way, it is possible to appropriately use a design in which the two DA supply ports 11A and 11B are arranged at a position where the devolatilization assistant DA can be supplied, and the two devolatilization ports (vent ports) 12A and 12B are arranged at a position where the volatile components can be exhausted (removed) (the positions of the DA supply ports 11A and 11B and the devolatilization ports 12A and 12B may be appropriately changed so as to obtain the desired function depending on the various components used).

[0051] In the embodiment of the kneading extruder shown in FIG. 2, the screw configuration is a combination of a kneading disk KD and a flight screw FS in two DA-addition kneading regions (regions A1 and A2). When two kneaders with the same L / D in the DA-addition kneading region are prepared, a kneading disk KD and a flight screw FS are combined in the screw in the region, and a kneading disk KD alone is used in the screw in the region. In the case of combining a flight screw FS, the residence time of the raw material in the DA-addition kneading region tends to be shortened and the filling rate of the raw material in the DA-addition kneading region tends to decrease, but the devolatilization aid tends to be diffused over a wide range. Therefore, the flight screw FS may be used in the screw configuration in the DA-addition kneading region in an appropriate range so long as the condition that the filling rate of the raw material in the DA-addition kneading region is 70% or more can be satisfied during the operation of the kneading extruder. In this case, it is preferable that the conditions such as the residence time of the raw material satisfy the suitable conditions described in the embodiment shown in FIG. 1.

[0052] Even when such an embodiment of the kneading extruder shown in FIG. 2 is used, the conditions (including the preferred conditions) employed in the conveying and kneading step can basically be the same as those described in the first embodiment. In the step of kneading the raw materials of the resin composition supplied into the cylinder 1 by the screw 2 while conveying them from the upstream side to the downstream side using the kneading extruder of the embodiment shown in FIG. 2, the filling rate of the raw materials in at least one or both of the DA addition kneading regions is set to 70% or more, and a devolatilization aid DA is supplied to the raw materials in the cylinder 1 from the devolatilization aid supply ports (11A, 11B) while the volatile components contained in the raw materials are discharged from the devolatilization ports (12A, 12B), thereby obtaining a resin composition from which volatile organic compounds have been devolatilized at a sufficiently high level.

[0053] Third embodiment In the third embodiment, except that a kneading extruder having a configuration as shown in FIG. 3 is prepared in the kneading extruder preparation step, the same steps as those in the first embodiment can be basically adopted, and a desired resin composition can be obtained.

[0054] The kneading extruder of the embodiment shown in Fig. 3 is basically the same as the kneading extruder of the embodiment shown in Fig. 2, except that it is not provided with a devolatilizing aid supply port 11B. Since the kneading extruder of the embodiment shown in Fig. 3 is not provided with a devolatilizing aid supply port 11B, a devolatilizing aid DA is not supplied in the region A2, but the raw material from which the volatile components have been devolatilized (molten kneaded material) is caused to flow from the devolatilizing port 12A into the region A2, and the raw material can be kneaded in the region A2 under high temperature and high pressure conditions, so that the volatile components remaining in the raw material after passing through the region A2 can be removed from the devolatilizing port 12B.

[0055] Incidentally, even when such a kneading extruder of the embodiment shown in FIG. 3 is used, the conditions (including the preferred conditions) employed in the conveying and kneading step can basically be the same as those described in the first embodiment. In the step of kneading the raw material of the resin composition supplied into the cylinder 1 by the screw 2 while conveying it from the upstream side to the downstream side using the kneading extruder of the embodiment shown in FIG. 3, the filling rate of the raw material in the DA addition kneading region (region A1) is set to 70% or more, and a devolatilization aid DA is supplied from the devolatilization aid supply port (11A) to the raw material in the cylinder 1 while the volatile components contained in the raw material are discharged from the devolatilization ports (12A, 12B), thereby obtaining a resin composition from which volatile organic compounds have been devolatilized at a sufficiently high level.

[0056] Although the preferred embodiment of the method for producing a resin composition of the present invention has been described above with reference to Figs. 1 to 3, the method for producing a resin composition of the present invention is not limited to the above embodiment. For example, in the method for producing a resin composition of the above embodiment, a kneading extruder having two devolatilizing ports is used. In the present invention, the kneading extruder is A cylinder and a screw disposed within the cylinder, the cylinder has at least one devolatilizing agent supply port and at least one devolatilizing port for discharging volatile components as openings, and has at least one structural portion in which the devolatilizing agent supply port and the devolatilizing port are arranged in sequence from the upstream side with a gap therebetween, The screw has at least one screw configuration in which a seal ring is disposed at an upstream portion of a supply port in the cylinder located upstream of a position where the devolatilizing agent supply port of at least one of the structural parts is provided, and at a downstream portion of a supply port located between the devolatilizing agent supply port and the devolatilizing port of the structural part, and a region between the upstream portion of the supply port and the downstream portion of the supply port has no opening communicating the region with the outside of the cylinder, other than the devolatilizing agent supply port which serves as a reference for the positions of the upstream portion of the supply port and the downstream portion of the supply port; The number of devolatilization ports does not have to be two. That is, it is sufficient that at least one devolatilization port is provided, and the number may be one or more (two or more) depending on the type of raw material, etc. Similarly, it is sufficient that at least one devolatilization assistant supply port is provided, and the number is not particularly limited, and may be one or more (two or more).

[0057] Furthermore, the screw utilized in the present invention may have at least one screw configuration in which seal rings are disposed at the upstream portion and downstream portion of the supply port based on the devolatilizing agent supply port of at least one of the structural parts in which the devolatilizing agent supply port and the devolatilizing port are arranged in a line with a gap therebetween in order from the upstream side, and the number of such screw configuration parts is not particularly limited, but the number may be one (one in the kneading extruder of the configuration shown in FIG. 3) or two or more (two in the kneading extruder of the configuration shown in FIGS. 1 and 2).

[0058] [Preferable embodiment of the resin composition manufacturing apparatus of the present invention] The apparatus for producing a resin composition of the present invention is as described above and can be suitably used in the method for producing a resin composition of the present invention. That is, the apparatus for producing a resin composition of the present invention can be suitably used as a kneading extruder prepared in the kneading extruder preparation step in the method for producing a resin composition of the present invention.

[0059] Here, the resin composition manufacturing apparatus of the present invention is equipped with a control device for controlling, in the conveying and kneading process, the supply of a devolatilizing agent to the raw material in the cylinder from the devolatilizing agent supply port while maintaining a filling rate of the raw material of 70% or more in at least one region in the cylinder between the upstream part of the supply port and the downstream part of the supply port, where the seal ring is located, and the discharge of volatile components contained in the raw material from the devolatilizing port, and the like, and the filling rate of the raw material in at least one region in the cylinder between the upstream part of the supply port and the downstream part of the supply port, where the seal ring is located, is controlled by this control device.

[0060] A preferred embodiment of the apparatus for producing a resin composition of the present invention will now be described with reference to FIG.

[0061] The resin composition production apparatus of the embodiment shown in Fig. 4 is a suitable form of the kneading extruder of the embodiment shown in Fig. 1. The apparatus of the embodiment shown in Fig. 4 is a twin-screw kneading extruder similar to Fig. 1, and in Fig. 4, similar to Fig. 1, only the screws on one shaft side are drawn for convenience.

[0062] The resin composition manufacturing apparatus shown in FIG. 4 includes a cylinder 1, a screw 2 disposed within the cylinder 1, a hopper 3 installed at an opening of the cylinder 1 for supplying raw materials, a feeder 30 as a raw material supply device for supplying raw materials into the cylinder 1 via the hopper 3 (in this embodiment, the feeder is provided with a raw material supply screw 30a and a motor 30b for driving the screw 30a), a motor 4 as a screw drive device (a rotation drive mechanism connected to the screw 2) for driving the screw 2, and a DA supply device 5 for supplying a devolatilization aid DA into the cylinder 1 (a supply device for a devolatilization aid DA). The twin-screw kneading extruder includes a feeder 30b provided on a feeder 30, a motor 4 as a screw drive device for driving the screw 2, a DA supplying device 5, a pressure reducing device (vacuum pump) 6, a temperature adjusting device 7, a thermometer 8 for measuring the temperature of the cylinder, a pressure gauge (pressure sensor) 9 for measuring the pressure in a pipe connecting the pressure reducing device 6 and the volatilization port (12A or 12B) of the cylinder, and a control device (controller) 10 electrically connected to the motor 30b provided on the feeder 30, the motor 4 as a screw drive device for driving the screw 2, the DA supplying device 5, the pressure reducing device (vacuum pump) 6, the temperature adjusting device 7, the thermometer 8 and the pressure gauge 9. Such a twin-screw kneading extruder is a device used for producing a resin composition by conveying the raw materials of the resin composition supplied into the cylinder by the screw from the upstream side to the downstream side while kneading them.

[0063] The resin composition manufacturing apparatus of the embodiment shown in FIG. 4 is a twin-screw kneading extruder (screw-type kneading devolatilizing extruder) equipped with a cylinder 1 and a screw 2 arranged in the cylinder 1. For the cylinder 1 and the screw 2, all conditions, including the position and type of the opening of the cylinder 1, the configuration of the screw 2, etc., are the same as those described in the embodiment shown in FIG. 1 (for example, the openings of the two DA supply ports 11A and 11B, the two devolatilizing ports (vent ports) 12A and 12B, the raw material supply port 13, etc., the conditions of the regions A1 and A2, the screw configuration, etc. are the same as those in the embodiment shown in FIG. 1). Therefore, the description of the cylinder 1 and the screw 2 (including the description of the symbols) will be omitted. For the hopper 3, the same one as that described in the embodiment shown in FIG. 1 can be used.

[0064] The feeder 30 shown in FIG. 4 is used as a raw material supplying device for supplying raw material into the cylinder 1 through the hopper 3, and includes a raw material supply screw 30a (a screw for adjusting the supply speed of the raw material) and a motor 30b for driving the screw 30a. In the kneading extruder of the embodiment shown in FIG. 4, the supply speed of the raw material into the cylinder can be appropriately controlled by controlling the operation of the motor 30b of such a feeder (raw material supplying device) (controlling the rotation speed of the motor 30b). There is no particular limitation on such a feeder, and a known one can be appropriately used. A commercially available one may be used as such a feeder 30. In the kneading extruder of the embodiment shown in FIG. 4, the motor 30b of the feeder 30 is electrically connected to the control device 10, which allows the control device 10 to control the operation of the motor 30b. In addition, such a feeder 30 may be equipped with a mass meter. When a mass meter is used in this manner, the amount of raw material in feeder 30 can be managed based on the mass data, and it becomes possible to more accurately control the amount of raw material in feeder 30 and the feed rate of raw material supplied into the cylinder via hopper 3. Therefore, when a feeder 30 equipped with a mass meter is used, the mass data measured by the mass meter may be input to control device 10 in order to manage the amount of raw material in feeder 30, and the amount of raw material in the feeder may also be managed by control device 10.

[0065] The motor 4 functions as a screw drive device (rotation drive mechanism) for driving the screw 2, and is connected to the screw 2. There are no particular limitations on the motor 4 as a screw drive device, and any known motor used in the field of kneading extruders can be used as appropriate. In the embodiment shown in Fig. 4, the motor 4 is electrically connected to the control device 10, which allows the control device 10 to control the operation of the motor 4 (control the motor rotation speed).

[0066] Furthermore, the two DA supply devices 5 are used to supply the devolatilization aid DA from the DA supply port (11A or 11B) into the cylinder 1. Therefore, each DA supply device 5 is connected to the cylinder so as to be able to supply the devolatilization aid DA into the cylinder 1 via the DA supply port (11A or 11B). Such a DA supply device 5 is not particularly limited, but for example, when the devolatilization aid DA is water, a device (water injection device) equipped with a water storage container and a gear pump for injecting water connected to the container may be used. In addition, a known device may be appropriately used as the DA supply device 5. For example, when the above-mentioned gear pump is used, a known gear pump (which may be a commercially available product, etc.) may be appropriately used. When a DA supply device 5 using a gear pump is used, the amount of water injected can be controlled to a desired amount by controlling the drive (operation) of a motor that rotates the gear. 4, the DA supplying device 5 is electrically connected to the control device 10, which enables the control device 10 to control the operation of the DA supplying device 5 (for example, control of the rotation speed of the gear pump motor) and allows data (control data) relating to the operating status of the DA supplying device 5 to be input to the control device 10. Note that such data relating to the operating status can be suitably used for managing the amount of DA in the devolatilizing aid in the container.

[0067] Moreover, each of the two pressure reducing devices 6 is used to reduce the pressure in the area (vent section) near the devolatilization port (12A or 12B). Such pressure reducing devices 6 are not particularly limited, and known devices (known vacuum pumps, etc.) used in the field of so-called vent-type extruders can be used as appropriate. Here, in the embodiment shown in FIG. 4, the pressure reducing devices 6 are electrically connected to the control device 10, which enables the control device 10 to control the operation of the pressure reducing device 6 (vacuum pump, etc.) (for example, control of the rotation of the motor driving the vacuum pump, etc.).

[0068] Moreover, the temperature adjustment device 7 is used to heat or cool the cylinder at each of the positions. Such a temperature adjustment device 7 is disposed outside the cylinder 1 so as to be able to heat the cylinder. Such a temperature adjustment device 7 is not particularly limited, and known heating / cooling means used in the field of extruders (for example, a device consisting of a heater (which may be used as a heating / cooling means by heating when the heater is in operation and allowing it to cool naturally when the heater is stopped), a device consisting of a heating means such as a heater and a cooling means such as a heat dissipation fin, a device configured to circulate a heat medium (heating liquid or cooling liquid) so as to heat or cool a desired location, etc.) can be appropriately used.

[0069] Furthermore, the thermometer 8 is used to measure the temperature of the cylinder. There are no particular limitations on the type of thermometer 8, and any known temperature measuring device (which may be a commercially available product) can be used as appropriate. The thermometer 8 is connected to the control device 10, which allows the temperature data obtained by the thermometer to be input to the control device 10.

[0070] In addition, the pressure gauge (pressure sensor) 9 is used to measure the pressure state in the pipe connecting the volatilization port (12A or 12B) and the pressure reducing device 6 (vacuum pump). There are no particular limitations on such pressure gauge 9, and any known pressure gauge can be used as appropriate.

[0071] The control device 10 is electrically connected to the feeder 30 (particularly the motor 30b in the feeder 30), the motor 4, the DA supply device 5, the pressure reducing device (vacuum pump) 6, the temperature adjusting device 7, and the thermometer 8. Such a control device 10 is a device used to control the operation of the motor 4 which is a screw drive device, the feeder 30 (more specifically the motor 30b in the feeder 30) which is a raw material supply device, the DA supply device 5, and the temperature adjusting device 7 so that, when raw materials are kneaded while being conveyed from the upstream side to the downstream side in the production of a resin composition, the devolatilizing agent DA is supplied to the raw materials in the cylinder 1 from the devolatilizing agent supply port while keeping the filling rate of the raw materials in at least one or both of the DA addition kneading regions (regions in the cylinder between the upstream part of the supply port where the seal ring SR is arranged and the downstream part of the supply port: region A1, region A2) at 70% or more, and the volatile components contained in the raw materials are discharged from the devolatilizing port.

[0072] Such a control device 10 may be any device capable of controlling the operation of each of the above devices as desired, and may be, for example, a computer configured by appropriately combining known peripheral devices such as a necessary CPU, ROM, RAM, and programs required for various calculations required for control (such programs may be recorded in the ROM and used, or may be recorded in another recording medium and used). The specific configuration is not particularly limited, and a device equipped with hardware consisting of a CPU and memory, etc., and a computer program (software) stored (installed) in the memory, etc., for executing the control of the operation of each of the above devices may be used. Examples of such a CPU include a central processing unit, a processing unit, an arithmetic unit, a processor, a microprocessor, a microcomputer, a DSP (Digital Signal Processor), etc.

[0073] Here, the control device 10 may have a computer program (software) for executing calculations necessary for controlling the operation of the motor 4, which is a screw drive device, the feeder 30 (more specifically, the motor 30b in the feeder 30), which is a raw material supply device, the DA supply device 5, and the temperature adjustment device 7. For example, when raw materials are conveyed from the upstream side to the downstream side during the production of a resin composition and kneaded, at least one or both of the DA addition kneading regions (regions within the cylinder between the upstream part of the supply port where the seal ring SR is arranged and the downstream part of the supply port: region A1, region A2) may be selected depending on the type of raw materials, the screw configuration, etc. A suitable example of the present invention is to use a computer program which is programmed to operate various devices so as to satisfy the predetermined conditions during actual operation by inputting temperature data measured by thermometer 8 and the like into the computer, the computer determining in advance the operating conditions of motor 4, the operating conditions of motor 30b related to the feed rate of the raw material, the temperature conditions of the cylinder, and the like which are required for supplying devolatilizing agent DA from the devolatilizing agent supply port to the raw material in cylinder 1 and discharging the volatile components contained in the raw material from the devolatilizing port while maintaining a filling rate of the raw material of 70% or more. The method for determining the necessary conditions in advance is not particularly limited. For example, a kneading simulation software (manufactured by Japan Steel Works, Ltd., product name: TEX-FAN) may be used to determine the necessary operating conditions for supplying the devolatilizing agent DA to the raw material in the cylinder 1 from the devolatilizing agent supply port while setting the filling rate of the raw material in at least one or both of the DA addition kneading regions (regions in the cylinder between the upstream portion of the supply port and the downstream portion of the supply port where the seal ring SR is arranged: region A1, region A2) to 70% or more, and for discharging the volatile components contained in the raw material from the devolatilizing port, depending on the structure of the kneading extruder. A specific method for determining such necessary operating conditions (control conditions) will be briefly described below with reference to FIG. 5. The flow shown in FIG. 5 is an example of a suitable procedure for determining the operating conditions when the filling rate of the raw material in both the region A1 and region A2, which are the DA addition kneading regions in the cylinder of the kneading extruder shown in FIG. 4, is set to 70% or more.

[0074] Fig. 5 is a diagram (flowchart) showing a preferred embodiment of a procedure for determining the operating conditions of various devices in the kneading extruder required when, in the production of a resin composition, the raw materials are kneaded while being conveyed from the upstream side to the downstream side using the kneading extruder shown in Fig. 4, the devolatilization aid DA is supplied from the devolatilization aid supply port to the raw materials in the cylinder 1 while keeping the filling rate of the raw materials in both of the DA addition kneading regions (regions in the cylinder between the upstream part of the supply port where the seal ring SR is arranged and the downstream part of the supply port: region A1, region A2) at 70% or more, and the volatile components contained in the raw materials can be discharged from the devolatilization port. In the flow shown in Fig. 5, the calculations for determining such operating conditions are performed using a computer capable of calculations using kneading simulation software (manufactured by Japan Steel Works, Ltd., product name: TEX-FAN).

[0075] In the flow shown in FIG. 5, in step S101, first, information on the device configuration of the kneading extruder (cylinder configuration, screw diameter, screw configuration, etc.) is input to a calculation unit in a computer that performs calculations using kneading simulation software, and the physical properties of the components that are the raw materials of the resin composition (PVT properties of the resin) are also input.

[0076] Next, in step S102, the following conditions (A) to (C) are input to the calculation unit as conditions (kneading conditions) to be adopted in order to achieve a desired filling rate in a desired region when using a kneading extruder: [Condition (A)] Screw 2 rotation speed (motor 4 rotation speed, a value that affects the residence time of the raw material in a specific area during mixing and transport of the raw material) [Condition (B)] Rotational speed of the feeder motor 30b (rotational speed of the raw material supply screw 30a: value for controlling the raw material supply speed) [Condition (C)] Temperature of cylinder 1 The values ​​are input, and the calculation unit executes the calculation of the kneading simulation using kneading simulation software (manufactured by Japan Steel Works, Ltd., product name: TEX-FAN). The input values ​​of the conditions (A) to (C) in step S102 are not particularly limited, and a person skilled in the art may input values ​​that are estimated to be necessary to set the filling rate of the raw material in the DA addition kneading region to a desired value (70% or more).

[0077] Next, in step S103, it is judged whether the filling rates of the raw material in the DA addition kneading areas (area A1, area A2) are both the desired value of 70% or more in the conveying and kneading process based on the result (content) of the simulation output as the calculation result. If the filling rates of the raw material are not the desired value as a result of the judgment in step S103, the process proceeds to step S104, and if they are the desired value, the process proceeds to step S105.

[0078] Here, if the process proceeds to step S104 as a result of the determination in step S103, in step S104, a new value different from the value adopted (input) in the previous simulation (calculation) is input for at least one of the input values ​​of the above conditions (A) to (C) based on the previous simulation result (calculation result), and the calculation of the kneading simulation is performed. The input of a new value for at least one of the input values ​​of the above conditions (A) to (C) may be a value that is estimated to be an optimal value for making the filling rate of the raw material a desired value (70% or more) based on the result of the kneading simulation. The input of such a new value may be performed by inputting a value calculated by a person skilled in the art from the calculation result of the kneading simulation so as to obtain the desired result, or a separate calculation unit that analyzes the calculation results so far and calculates a value that will be required to make the filling rate of the raw material in the DA addition kneading region (region A1, region A2) a desired value may be provided in the computer, and the value obtained by the separate calculation unit may be input to the calculation unit that performs the calculation by the kneading simulation software.

[0079] Then, if the result of the judgment in step S103 is that the filling rates of the raw materials in the DA addition kneading areas (area A1, area A2) are both the desired value of 70% or more, the operating conditions of the motor 4 which is the screw drive device, the feeder 30 which is the raw material supply device (more specifically, the motor 30b in the feeder 30), the DA supply device 5 and the temperature control device 7 are obtained from the conditions adopted at that time, and the calculation is terminated.

[0080] In addition, the flow as shown in Fig. 5 can be executed for the same raw material by appropriately changing the set value of the desired filling rate of the raw material in the DA addition kneading region, and the operating conditions for satisfying various filling rate conditions can be obtained in advance. In this way, when the operating conditions for satisfying various filling rate conditions are obtained in advance, when the desired filling rate value is input to the control device 10 based on the data of those operating conditions, the control device 10 automatically calculates the operating conditions of each device required to satisfy the filling rate value, and a computer program that controls the operation of each device to satisfy the operating conditions may be created and stored in the memory of the computer that constitutes the control device 10. As a result, it is possible to efficiently control each device by inputting the desired filling rate value to the control device 10.

[0081] In this way, if the control device 10 is made of a computer having stored therein a computer program for controlling the operation of each device so as to satisfy the operating conditions obtained as described above, the control device 10 can control the operation of each device so that the filling rates of the raw materials in the DA addition kneading regions (regions A1 and A2) are all the desired values ​​of 70% or more during the production of the resin composition. When controlling the operation of each device, for example, cylinder temperature data obtained by the thermometer 8 may be automatically input to the control device 10, and the operation of the temperature adjustment device 7 may be controlled so that the cylinder temperature becomes the required temperature according to the temperature change state.

[0082] In controlling the operation of each of these devices, the control device 10 also controls the operation of the DA supply device 5 and the pressure reducing device 6 so that the filling rate of the raw material in the DA addition kneading region is set to a desired value of 70% or more, the devolatilization aid DA is supplied from the devolatilization aid supply port to the raw material in the cylinder 1, and the volatile components contained in the raw material are discharged from the devolatilization port. In order to control the operation of the DA supply device 5 and the pressure reducing device 6, it is preferable that the control device 10 is equipped with a computer program programmed to control the operation of the DA supply device 5 and the pressure reducing device 6 so as to satisfy the set conditions of the desired supply amount and supply rate of the devolatilization aid and the desired pressure (internal pressure of the molten kneaded material) of the region (vent portion) in the vicinity of the devolatilization ports (12A and 12B) by the pressure reducing device 6. The computer program for such operation control may be appropriately created so as to adjust the supply amount and pressure to the desired amount by applying a known method for controlling the DA supply device 5 (e.g., a gear motor) or a known method for controlling the pressure reducing device 6, which are used in the field of vented extruders. Also, for example, the operation of the pressure reducing device 6 may be controlled so that the pressure can be maintained at the desired value by configuring a calculation unit in the control device 10 to input pressure data measured by a pressure gauge (pressure sensor) 9 to change the operating conditions of the pressure reducing device 6 (e.g., the number of revolutions of the driving motor of the vacuum pump) so that the pressure at the measurement site becomes the desired value according to the input pressure data.

[0083] The resin composition production method of the present invention can be carried out by using the resin composition production apparatus of the embodiment shown in Fig. 4. Therefore, as described above, the resin composition production apparatus of the present invention can be suitably used for the resin composition production method of the present invention. The resin composition manufacturing apparatus of the embodiment shown in FIG. 4 is one of the preferred embodiments of the apparatus for manufacturing the resin composition of the embodiment shown in FIG. 1. During the raw material conveying and kneading process, the operation of each device constituting the kneading extruder (including the amount of raw material input, etc.) is controlled by the control device 10 as described above. Except for this, the resin composition can be manufactured under the same conditions as those described in the method for manufacturing a resin composition using the device of the embodiment shown in FIG. 1. Therefore, the description of the specific method for manufacturing a resin composition using the apparatus for manufacturing a resin composition of the embodiment shown in FIG. 4, such as the raw material conveying and kneading process, is omitted. (Note that the feeder 30, motor 4, DA supply device 5, pressure reducing device 6, temperature control device 7, etc. specifically described in FIG. 4 are used, and the operation of these devices is controlled by the control device 10 as described above. Basically, the conveying and kneading process can be performed under the same conditions as those used when the kneading extruder of the embodiment shown in FIG. 1 is used, and the preferred conditions of the process can be similar to those described in the process when the device of the embodiment shown in FIG. 1 is used.)

[0084] The resin composition production apparatus of the embodiment shown in FIG. 4 has been described above, but the resin composition production apparatus of the present invention is not limited to the above embodiment, and may include any kneading extruder including: a cylinder; a screw disposed in the cylinder; a screw drive device for driving the screw; a raw material supply device for supplying raw materials into the cylinder; a devolatilization aid supply device for supplying a devolatilization aid into the cylinder; a temperature adjustment device for adjusting the temperature of the cylinder; and a control device electrically connected to the screw drive device, the raw material supply device, the devolatilization aid supply device and the temperature adjustment device and for controlling the operation of each of the devices, the cylinder has at least one devolatilizing agent supply port and at least one devolatilizing port for discharging volatile components as openings, and has at least one structural portion in which the devolatilizing agent supply port and the devolatilizing port are arranged in sequence from the upstream side with a gap therebetween, the screw has at least one screw configuration in which a seal ring is disposed at an upstream portion of a supply port in the cylinder located upstream of a position where the devolatilizing agent supply port of at least one of the structural parts is provided, and at a downstream portion of a supply port located between the devolatilizing agent supply port and the devolatilizing port of the structural part, the kneading extruder satisfies the condition that, in a region between the upstream portion of the supply port and the downstream portion of the supply port where the seal ring is arranged, no opening is provided that connects the region with the outside of the cylinder, other than the devolatilizing agent supply port that serves as a reference for the positions of the upstream portion of the supply port and the downstream portion of the supply port; The kneading extruder is a device used for producing a resin composition by conveying the raw material of the resin composition supplied into the cylinder by the screw from the upstream side to the downstream side while kneading the raw material, The control device is not particularly limited as long as it controls the operation of the screw drive device, the raw material supply device, the devolatilization aid supply device, and the temperature adjustment device so that, when the raw materials are kneaded while being transported from the upstream side to the downstream side during production of a resin composition, a devolatilization aid is supplied to the raw materials in the cylinder from the devolatilization aid supply port while maintaining a filling rate of the raw materials of 70% or more in at least one region within the cylinder between the upstream part of the supply port where the seal ring is located and the downstream part of the supply port, and volatile components contained in the raw materials are discharged from the devolatilization port. EXAMPLES

[0085] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the following examples and comparative examples, the same recycled polypropylene pellets (separated and recovered from automobiles and home appliances) were used as the raw material.

[0086] Example 1 The recycled polypropylene raw material was kneaded using a twin-screw extruder (manufactured by Japan Steel Works, Ltd., product name: TEX30, ratio of screw length L to screw diameter (outer diameter) D (L / D) = 77, maximum screw outer diameter (screw diameter): 30 mm (nominal value), cylinder inner diameter (cylinder diameter): 32 mm) to obtain a resin composition (pellet-shaped). The cylinder and screws were designed to be similar to those shown in Figure 1 (the screws were arranged in the order FS, KD1, FS, SR1, KD2, SR2, FS, SR3, KD3, SR4, FS from the upstream side to the downstream side), and a seal ring SR 1~4The diameter of the screw SR1 was 30 to 31 mm, and the gap between the seal ring and the inner diameter of the cylinder at the position where the seal ring was arranged was 0.5 to 1 mm. In the twin-screw extruder, the ratio (L1 / D) of the screw length L1 to the screw diameter (outer diameter) D in the region A1 shown in FIG. 1 was set to 7, the ratio (L2 / D) of the screw length L2 to the screw diameter (outer diameter) D in the region A2 was set to 7, and the length L3 between the upstream end of the seal ring SR1 and the downstream end of the raw material supply port was set to 847.5 mm. Furthermore, in the screw 2, the length between the downstream end of the seal ring SR2 and the upstream end of the seal ring SR3 was set to 465 mm, and the ratio (length / diameter) of the screw length to the diameter of the portion constituted by the kneading disk KD1 was set to 7.5. In addition, when kneading the raw materials, the temperature of the cylinder was set to 170°C, the screw rotation speed was set to 150 rpm, the supply rate of the raw materials to the cylinder was set to 5 kg / h, water was used as the devolatilization aid DA, the amount of water injected from the devolatilization aid supply port 11A was set to 14 parts by mass relative to 100 parts by mass of the raw materials in the cylinder 1, and the amount of water injected from the devolatilization aid supply port 11B was set to 14 parts by mass relative to 100 parts by mass of the raw materials in the cylinder 1 (the amount of water injected was determined from the ratio of the supply rate of the resin composition to the supply rate of water). In addition, when kneading the raw materials, the pressure inside the cylinder was reduced by a water-sealed vacuum pump connected to the devolatilization ports (vent ports) 12A and 12B, and the volatile components were removed from the devolatilization ports. The two DA-added mixing regions (regions A1 and A2) were analyzed using mixing simulation software (manufactured by Japan Steel Works, Ltd., product name: TEX-FAN) to determine the filling rate of the raw materials. The filling rate (volume %) of the raw materials in each region (A1 and A2) was 100%.

[0087] In Example 1, the mixing conditions adopted for mixing the raw materials, such as a cylinder temperature of 170° C., a screw rotation speed of 150 rpm, and a supply rate of the raw materials to the cylinder of 5 kg / h, were determined by analyzing the mixing conditions (such as the supply rate of the raw materials) required to achieve a filling rate (volume %) of the raw materials of 100% in both of the two DA addition mixing regions (regions A1 and A2) using mixing simulation software (manufactured by Japan Steel Works, Ltd., product name: TEX-FAN) according to the procedure (flowchart) shown in FIG. 5 . During kneading of the raw materials, the operation of a raw material supply device (not shown in FIG. 1: with reference to FIG. 4, a device corresponding to the feeder 30 shown in FIG. 4) for supplying the raw materials, a screw drive device (a rotary drive mechanism for rotating the screw: not shown in FIG. 1: with reference to FIG. 4, a device corresponding to the motor 4 shown in FIG. 4), and a heater for adjusting the temperature inside the cylinder (not shown in FIG. 1: with reference to FIG. 4, a device corresponding to the temperature control device 7 shown in FIG. 4) was controlled by a computer (not shown in FIG. 1: with reference to FIG. 4, a device corresponding to the control device 10 shown in FIG. 4) electrically connected to these devices so that the cylinder temperature was 170°C, the screw rotation speed was 150 rpm, and the supply rate of the raw materials to the cylinder was 5 kg / h. In addition, the operation of an apparatus for supplying the devolatilizing aid, not shown in Fig. 1 (with reference to Fig. 4, this apparatus corresponds to the DA supply apparatus 5 shown in Fig. 4) was also controlled by a computer (not shown in Fig. 1: with reference to Fig. 4, this apparatus corresponds to the control device 10 shown in Fig. 4) electrically connected to the apparatus so that the amount of water injected from the devolatilizing aid supply port 11A satisfied the above-mentioned condition. Furthermore, when kneading the raw materials, the operation of a water ring vacuum pump (not shown in Fig. 1: with reference to Fig. 4, this apparatus corresponds to the pressure reducing device 6 shown in Fig. 4) connected to the devolatilizing ports (vent ports) 12A and 12B was also controlled by a computer (not shown in Fig. 1: with reference to Fig. 4, this apparatus corresponds to the control device 10 shown in Fig. 4) electrically connected to the water ring vacuum pump, thereby reducing the pressure in the cylinder.

[0088] Example 2 The design of the cylinder and screws was changed to be similar to that shown in Figure 2 (note that the screw configuration was arranged in the following order from upstream to downstream: FS, KD1, FS, SR1, KD2, FS, KD2, SR2, FS, SR3, KD3, FS, KD3, SR4, FS), the ratio (L1 / D) of the screw length (corresponding to L1 in Figure 1) to the screw diameter (outer diameter) D in the region A1 was changed to 8.25, and the ratio (L2 / D) of the screw length (corresponding to L2 in Figure 1) to the screw diameter (outer diameter) D in the region A2 was changed to The raw material was kneaded in the same manner as in Example 1 to obtain a resin composition, except that the length between the upstream end of the seal ring SR1 and the downstream end of the raw material supply port (the length of the portion corresponding to L3 in FIG. 1) was changed to 1267.5 mm, the length to diameter ratio (length / diameter) of the flight screw FS arranged in the region A1 was set to 1.25, the length to diameter ratio of the flight screw FS arranged in the region A2 was set to 1.25, and the length to diameter ratio (length / diameter) of the screw of the portion constituted by the kneading disk KD1 was set to 8. The filling rate (volume%) of the raw material in the regions A1 and A2 was determined in the same manner as in Example 1, and the filling rate of the raw material in the region A1 was 93%, and the filling rate of the raw material in the region A2 was 87%.

[0089] Example 3 The design of the cylinder and screw was changed to be the same as that shown in Fig. 3 (note that the design was the same as that shown in Fig. 2 except that the devolatilizing agent supply port 11B was not formed), and the raw materials were kneaded in the same manner as in Example 2 to obtain a resin composition, except that water was injected only from the devolatilizing agent supply port 11A. The filling rate (volume %) of the raw materials in the region A1 where water was injected was determined in the same manner as in Example 1, and the filling rate was 93%.

[0090] Comparative Example 1 The design of the cylinder and the screw were changed to be similar to that shown in FIG. 6 (note that the screw configuration was arranged in the order of FS, KD1, FS, SR1, KD2, FS, SR2, FS, SR3, KD3, FS, SR4, FS from the upstream side to the downstream side. Here, the screw length and diameter ratios (corresponding to L1 / D and L2 / D) of the regions A1 and A2 were not changed compared to Example 1, but the screw configuration in region A1 was changed to one consisting of a kneading disk KD2 and a flight screw FS, and the screw configuration in region A2 was changed to one consisting of a kneading disk KD3 and a flight screw FS). The ratio of the length and diameter (length / diameter) of the flight screw FS arranged in region A1 was set to 6.5, and the ratio of the length and diameter (length / diameter) of the flight screw FS arranged in region A2 was set to 6.5. Except for this, the raw materials were kneaded in the same manner as in Example 1 to obtain a resin composition. The filling rate (volume %) of the raw material in the regions A1 and A2 was determined in the same manner as in Example 1, and the filling rate of the raw material in the region A1 was 34%, and the filling rate of the raw material in the region A2 was 34%.

[0091] Comparative Example 2 Except for changing the supply rate of the raw materials to the cylinder to 15 kg / h, the raw materials were kneaded in the same manner as in Comparative Example 1 to obtain a resin composition. The filling rates (volume %) of the raw materials in areas A1 and A2 were determined in the same manner as in Example 1, and the filling rate of the raw materials in area A1 was 48%, and the filling rate of the raw materials in area A2 was 48%.

[0092] [Evaluation of properties of resin compositions obtained in Examples 1 to 3 and Comparative Examples 1 and 2] The raw material recycled polypropylene (pellet-like) and the resin compositions (pellet-like) obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were used as they were to prepare samples (20 to 50 mg) for measurement. Then, using a thermal desorption (TD)-gas chromatograph mass spectrometer (instrument configuration: TDU manufactured by Gestell, and product name: 7890B GC-5977B MSD manufactured by Agilent), the gas components (volatilized organic compounds: volatile organic compounds) generated when the samples were heated at 80°C for 10 minutes were analyzed. The gas generated by heating with TD was concentrated and collected at a cooling inlet (CIS, Tenax-TA filled in the insert, temperature: -50°C), and then the CIS was rapidly heated from -50°C to 300°C at a heating rate of 720°C / min, and separated with a column (manufactured by Agilent, product name: HP-5MS UI, length 30 m, inner diameter 0.25 mm, film thickness 0.25 μm). He (flow rate: 1.5 mL / min) was used as the carrier gas for the column, and the column temperature was raised from 0°C to 300°C at a heating rate of 10°C / min. The components separated in the column were detected by a mass spectrometer (electron ionization method, ion source temperature: 230°C, MS quadrupole temperature: 150°C, scan range of m / z value: 28.7-600). The integral value of the total ion current (TIC) chromatogram in the range of m / z values ​​from 33 to 600 was defined as the amount of volatile organic compounds contained in the sample, and the amount of volatile organic compounds contained per mg of each sample of the raw material (pellets before kneading) and the resin composition (pellets after kneading) obtained in each Example was calculated, and the removal rate of volatile organic compounds (the proportion of volatile organic compounds removed from the raw material) was calculated using the following calculation formula (1): [Volatile organic compound removal rate (%)] = (M1-M2) / M1(1) (In formula (1), M1 represents the amount of volatile organic compounds contained per 1 mg of a raw material sample (the amount of volatile organic compounds in the raw material before devolatilization), and M2 represents the amount of volatile organic compounds contained per 1 mg of a sample of the kneaded resin composition (pellets after kneading) obtained in the Examples, etc. (the amount of volatile organic compounds remaining in the resin composition obtained after devolatilization).) The results are shown in Table 1.

[0093] Table 1 also shows the ratio (L1 / D) of the length to the screw diameter D of the screw L1 located in the water-injected area A1, and the ratio (L2 / D) of the length to the screw diameter D of the screw L2 located in the water-injected area A2, as well as the filling rate (volume %) of the raw material in the water-injected area A1 and the water-injected area A2.

[0094] [Table 1]

[0095] As is clear from the results shown in Table 1, in Examples 1 to 3, which adopted a method corresponding to the method for producing a resin composition of the present invention in which the filling rate of the raw material (melt-kneaded product) in the region where the devolatilizing aid (water) is added and kneaded (Examples 1 to 2: Regions A1 and A2, Example 3: Region A1) is 70% or more, the volatile organic compounds (VOCs) in the raw material were efficiently removed at a high level (a high level of removal rate of 85% or more) in the devolatilizing step, and it was confirmed that such a method makes it possible to efficiently produce a resin composition with a sufficiently low residual amount of VOC. In contrast, in the methods adopted in Comparative Examples 1 and 2, in which the filling rate of the raw material (melt-kneaded product) in the region where the devolatilizing aid (water) is added and kneaded is less than 70%, the VOC removal rate was 48% or less, and the volatile organic compounds (VOCs) could not be sufficiently devolatilized and removed. [Industrial Applicability]

[0096] As described above, according to the present invention, it is possible to provide a method for producing a resin composition capable of efficiently producing a resin composition having a sufficiently low residual amount of volatile organic compounds, and a resin composition production apparatus that can be suitably used for the method. Therefore, the method for producing a resin composition of the present invention is useful, for example, as a method for producing a recycled resin composition from which VOCs have been removed, or a method for obtaining a deodorized resin composition from which VOCs have been removed, etc. [Explanation of symbols]

[0097] 1...cylinder, 2...screw, 3: hopper, 4...motor for driving screw 2, 5...devolatilization aid supply device, 6...pressure reducing device (vacuum pump), 7...temperature adjusting device, 8...thermometer, 9...pressure gauge (pressure sensor), 10...controller, 11A and B...devolatilization aid supply port, 12A and B...devolatilization port for discharging volatile components, 13...opening for supplying raw material (raw material supply port), 30...feeder, 30a...screw for supplying raw material, 30b...motor for driving screw for supplying raw material, FS...full flight screw, KD 1~3 ...Kneading disc, SR 1~4 ...sealing ring, DA...devolatilization aid, VOC...volatile organic compounds.

Claims

1. The present invention relates to a cylinder and a screw disposed in the cylinder, the cylinder has at least one devolatilizing agent supply port and at least one devolatilizing port for discharging volatile components as openings, and has at least one structural portion in which the devolatilizing agent supply port and the devolatilizing port are arranged side by side with a gap therebetween in that order from the upstream side, The screw has at least one screw configuration in which a seal ring is disposed at an upstream portion of a supply port in the cylinder located upstream of a position where the devolatilizing agent supply port of at least one of the structural parts is provided, and at a downstream portion of a supply port located between the devolatilizing agent supply port and the devolatilizing port of the structural part, and in a region between the upstream portion of the supply port and the downstream portion of the supply port where the seal ring is arranged, no opening is provided that connects the region with the outside of the cylinder, other than the devolatilizing agent supply port that serves as a reference for the positions of the upstream portion of the supply port and the downstream portion of the supply port; A kneading extruder preparation step of preparing a kneading extruder; a conveying and kneading step of conveying and kneading the raw material of the resin composition supplied into the cylinder by the screw from the upstream side to the downstream side using the kneading extruder; Including, a devolatilization agent is supplied from the devolatilization agent supply port to the raw material in the cylinder, and a volatile component contained in the raw material is discharged from the devolatilization port to obtain a resin composition, the method comprising the steps of: in the conveying and kneading step, setting a filling rate of the raw material in at least one region in the cylinder between the upstream portion of the supply port where the seal ring is located and the downstream portion of the supply port to be 70% or more;

2. A method for producing a resin composition, characterized in that, in the conveying and kneading process, the filling rate of the raw material in the area within the cylinder between the upstream portion of the supply port where the seal ring is located and the downstream portion of the supply port is 80% or more.

3. 2. The method for producing a resin composition according to claim 1, wherein the devolatilizing aid is water.

4. A cylinder; A screw disposed within the cylinder; a screw drive device for driving the screw; A raw material supplying device for supplying raw material into the cylinder; a devolatilization aid supplying device for supplying a devolatilization aid into the cylinder; a temperature control device for controlling the temperature of the cylinder; a control device electrically connected to the screw drive device, the raw material supply device, the devolatilization aid supply device, and the temperature adjustment device, for controlling the operation of each of the devices; The kneading extruder comprises: the cylinder has at least one devolatilizing agent supply port and at least one devolatilizing port for discharging volatile components as openings, and has at least one structural portion in which the devolatilizing agent supply port and the devolatilizing port are arranged side by side with a gap therebetween in that order from the upstream side, the screw has at least one screw configuration in which a seal ring is disposed in an upstream portion of a supply port in the cylinder located upstream of a position where the devolatilizing agent supply port of at least one of the structural parts is provided, and in a downstream portion of a supply port located between the devolatilizing agent supply port and the devolatilizing port of the structural part, the kneading extruder satisfies the condition that, in a region between the upstream portion of the supply port and the downstream portion of the supply port where the seal ring is arranged, no opening is provided that connects the region with the outside of the cylinder, other than the devolatilizing agent supply port that serves as a reference for the positions of the upstream portion of the supply port and the downstream portion of the supply port; The kneading extruder is a device used for producing a resin composition by conveying and kneading raw materials of the resin composition supplied into the cylinder by the screw from the upstream side to the downstream side, the control device controls the operation of the screw drive device, the raw material supply device, the devolatilization aid supply device and the temperature adjustment device so that, when the raw materials are kneaded while being transported from the upstream side to the downstream side in the production of a resin composition, a devolatilization aid is supplied to the raw materials in the cylinder from the devolatilization aid supply port while a filling rate of the raw materials in at least one region in the cylinder between the upstream part of the supply port where the seal ring is arranged and the downstream part of the supply port is kept at 70% or more, and volatile components contained in the raw materials are discharged from the devolatilization port; An apparatus for producing a resin composition comprising:

5. The kneading extruder further includes a pressure reducing device connected to the devolatilization port, The control device is also electrically connected to the pressure reducing device; and the control device controls operations of the screw drive device, the raw material supply device, the devolatilization aid supply device, and the temperature adjustment device, and also controls operation of the pressure reduction device, during the production of the resin composition; The apparatus for producing a resin composition according to claim 4,

Citation Information

Patent Citations

  • Removal of volatile substance from thermoplastic resin and vent type twin-screw extruder

    JP1996207118A

  • Manufacture of polycarbonate resin pellet

    JP1997066524A

  • Method for devolatilization treatment of polymer resin raw material and devolatilization kneading extruder

    JP2000309019A

  • Method of producing resin composition and screw type kneading devolatilization extruder

    JP2021062552A

  • Process for production of polycarbonate resin pellets

    WO2012108245A1