Resin roll
The resin roll design addresses misalignment and damage issues by aligning core and sheet widths and adjusting solvent content, achieving precise transportation and high yield in printed wiring boards.
Patent Information
- Application Number
- JP2024009972
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2024-01-26
- Publication Date
- 2024-10-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The challenge of misalignment and damage to resin composition layers during transportation due to high inorganic filler content, which increases density differences between the resin sheet and core, is exacerbated by larger sheet widths in resin rolls used for printed wiring boards, leading to reduced yield and potential damage.
The resin roll design aligns the core and resin sheet widths closely, adjusts the residual solvent content, and includes a volatile component in the thermosetting resin composition layer, with specific density and elastic modulus ranges, to prevent misalignment and damage, using a core with a diameter of 50 mm or more and a width ratio of 0.9 to 1.1, and a density difference of 0.3 to 2.0 g/cm³.
This design effectively suppresses misalignment and damage to the resin composition layer, ensuring a good yield by maintaining precise alignment and structural integrity during transportation.
Smart Images

Figure 2024137716000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin roll on which a resin sheet having a thermosetting resin composition layer containing an inorganic filler is wound. [Background technology]
[0002] As a manufacturing technique for printed wiring boards, a manufacturing method by the build-up method in which insulating layers and conductor layers are alternately stacked is known. In the manufacturing method by the build-up method, generally, an insulating layer is formed by thermally curing a thermosetting resin composition (Patent Documents 1 to 3). The insulating layer can be formed by laminating a resin composition layer on a circuit board using a resin sheet containing a resin composition layer and curing the resin composition layer. The resin sheet generally has a three-layer structure of a base film, a resin composition layer, and a protective film, and when the resin sheet is industrially produced or used, it may be handled in the form of a resin roll in which the resin sheet is wound around a core. In the resin roll, in order to prevent the resin composition layer from being scratched, there are (1) a method in which the width of the core is made larger than the width of the resin sheet, and (2) a method in which only the base film and the protective film are provided at the end of the resin sheet (so-called "ears"). However, in the method (2), the consumption of the base film and the protective film increases only at the ears, which is not desirable from the viewpoint of cost, and therefore the method (1) is usually used. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-157027 A [Patent Document 2] JP 2020-94213 A [Patent Document 3] JP 2020-152780 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, the need for insulating layers with low dielectric tangent has been increasing for next-generation high-speed communications. Furthermore, in order to withstand the increased stress associated with the need for larger substrates, there is a demand for insulating layer materials with low thermal expansion coefficients that can reduce stress by minimizing the difference in expansion coefficient with the substrate.
[0005] As a method for ensuring low thermal expansion and excellent dielectric properties, it is considered to include a large amount of inorganic filler in the resin composition layer. However, when the resin composition layer includes a large amount of inorganic filler, when the resin sheet is transported from the resin roll, a large positional deviation may occur at the transport roll portion. This is considered to be caused by the fact that the density of the resin sheet increases due to the high filling of inorganic filler, and the density difference between the resin sheet and the core becomes large. In addition, this positional deviation is remarkable when the width of the resin sheet is large.
[0006] An object of the present invention is to provide a resin roll which is capable of suppressing misalignment during transport and suppressing damage to a resin composition layer, and which can achieve a good yield. [Means for solving the problem]
[0007] In order to achieve the object of the present invention, the inventors conducted intensive research and discovered that by aligning the width of the core and the resin sheet and adjusting the amount of residual solvent in the resin composition layer, it is possible to suppress both misalignment during transportation and damage to the resin composition layer, thereby achieving a good yield, and thus completed the present invention.
[0008] That is, the present invention includes the following. [1] A resin sheet having a base film, a thermosetting resin composition layer containing an inorganic filler provided on one surface of the base film, and a protective film provided on a surface of the thermosetting resin composition layer opposite to the base film; A core around which the resin sheet is wound; Equipped with When the thermosetting resin composition layer further contains a volatile component and the surface that does not contact the base film is exposed to the outside air after peeling the protective film, the weight loss rate of the thermosetting resin composition layer after heat treatment at 130 °C for 15 minutes is 0.7 to 5% by mass. The average density of the entire resin sheet is 1.3 g / cm 3 or more, the width of the resin sheet is 300 mm or more, Let the width of the core be W c and the width of the resin sheet be W s When W c / W s is defined as W3, the resin roll satisfies 0.9 ≦ W3 ≦ 1.1. [2] The resin roll according to [1] above, wherein 0.99 < W3 ≦ 1.1. [3] The resin roll according to [1] or [2] above, wherein the thermosetting resin composition layer further contains an epoxy resin. [4] The resin roll according to any one of [1] to [3] above, wherein the base film and the protective film are plastic films. [5] The resin roll according to any one of [1] to [4] above, wherein the film thickness of the base film is 5 μm to 75 μm, the film thickness of the thermosetting resin composition layer is 5 μm to 250 μm, and the film thickness of the protective film is 1 μm to 40 μm. [6] Let the width of the base film be W b and the width of the thermosetting resin composition layer be W r When W b / W r is defined as W1, 0.9 ≦ W1 ≦ 1.1, and let the width of the protective film be W p When W p / W r is defined as W2, 0.9 ≦ W2 ≦ 1.1. The resin roll according to any one of [1] to [5] above. [7] The resin roll according to any one of [1] to [6] above, wherein the elastic modulus of the thermosetting resin composition layer is 1 GPa to 10 GPa when measured at 23 °C. [8] The average density of the entire resin sheet is 1.8 g / cm3 The resin roll according to any one of the above [1] to [7], wherein the viscosity is less than 100 MPa. [9] The resin roll according to any one of the above [1] to [8], wherein the core has a diameter of 50 mm or more.
[10] The density of the core is 0.8 to 1.2 g / cm 3 The resin roll according to any one of the above [1] to [9],
[11] The difference between the density of the core and the average density of the entire resin sheet is 0.3 to 2.0 g / cm 3 The resin roll according to any one of the above [1] to
[10] ,
[12] The resin roll according to any one of the above [1] to
[11] , wherein the resin sheet has a width of 1000 mm or less.
[13] The resin roll according to any one of the above [1] to
[12] , wherein the resin sheet has a rolled-up length of 100 m or less.
[14] The resin roll according to any one of the above [1] to
[13] , wherein the content of the inorganic filler in the thermosetting resin composition layer is 50% by mass or more, based on 100% by mass of all non-volatile components.
[15] The resin roll according to any one of the above [1] to
[14] , wherein the content of the inorganic filler in the thermosetting resin composition layer is 80 mass% or less, when the total amount of non-volatile components is 100 mass%.
[16] The resin roll according to any one of the above [1] to
[15] , wherein the coefficient of linear thermal expansion (CTE) of the thermosetting resin composition layer after curing is 50 ppm / °C or less in the range of 25°C to 150°C.
[17] The resin roll according to any one of the above [1] to
[16] , wherein the thermosetting resin composition layer has a dielectric loss tangent (Df) after curing of 0.006 or less when measured at 5.8 GHz and 23°C.
[18] The resin roll according to any one of the above [1] to
[17] , wherein the thermosetting resin composition layer is a resin composition layer for forming an insulating layer of a printed wiring board.
[19] A resin sheet discharge device comprising a resin roll and a fixing member, The resin roll is A resin sheet including a base film, a thermosetting resin composition layer including an inorganic filler provided on one surface of the base film, and a protective film provided on a surface of the thermosetting resin composition layer opposite to the base film; A core around which the resin sheet is wound; Equipped with the thermosetting resin composition layer further contains a volatile component, and when the protective film is peeled off and the surface not in contact with the base film is exposed to the outside air, the weight loss rate of the thermosetting resin composition layer after heat treatment at 130°C for 15 minutes is 0.7 to 5% by mass; The average density of the entire resin sheet is 1.3 g / cm 3 That's all. The width of the resin sheet is 300 mm or more, The width of the core is W c The width of the resin sheet is W s And W c / W s is W3, 0.9≦W3≦1.1, The fixing member is a support portion that supports the core core; and a planar shaft stop portion that is perpendicular to the axial direction and contacts both ends of a structure consisting of the core core and the resin sheet wound around the core core to limit the axial movement of the core core and the entire resin sheet wound around the core core. The resin sheet discharge device includes:
[20] A resin sheet having a base film, a thermosetting resin composition layer containing an inorganic filler provided on one surface of the base film, and a protective film provided on a surface of the thermosetting resin composition layer opposite to the base film; A core around which the resin sheet is wound; Equipped with the thermosetting resin composition layer further contains a volatile component, and when the protective film is peeled off and the surface not in contact with the base film is exposed to the outside air, the weight loss rate of the thermosetting resin composition layer after heat treatment at 130°C for 15 minutes is 0.7 to 5% by mass; The average density of the entire resin sheet is 1.3 g / cm3 That's all. The width of the resin sheet is 300 mm or more, The width of the core is W c The width of the resin sheet is W s And W c / W s 2. A method for producing a printed wiring board, comprising the following steps (1) to (4), using a resin roll having a width W3 of 0.9≦W3≦1.1: (1) A step of removing the resin sheet from the resin roll (2) peeling the protective film from the resin sheet (3) A step of laminating the resin sheet from which the protective film has been peeled off onto an inner layer substrate such that the thermosetting resin composition layer is bonded to the inner layer substrate. (4) A step of thermally curing the thermosetting resin composition layer to form an insulating layer. Effect of the Invention
[0009] According to the present invention, it is possible to provide a resin roll which is capable of suppressing both the slippage during transport and the damage to the resin composition layer, and achieving a good yield. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view of a resin sheet carry-out device in one embodiment, in which a resin roll is installed, when carrying out a resin sheet. [Diagram 2] FIG. 2 shows a cross-sectional view taken along line AA in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below with reference to preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0012] The resin roll of the present invention comprises a resin sheet having a base film, a thermosetting resin composition layer containing an inorganic filler provided on one surface of the base film, and a protective film provided on the surface of the thermosetting resin composition layer opposite to the base film, and a core around which the resin sheet is wound, wherein the thermosetting resin composition layer further contains a volatile component, and when the protective film is peeled off and the surface not in contact with the base film is exposed to the outside air, the weight loss rate of the thermosetting resin composition layer after heat treatment at 130°C for 15 minutes is 0.7 to 5 mass%, and the average density of the entire resin sheet is 1.3 g / cm 3 The resin sheet has a width of 300 mm or more, and the difference between the width of the core and the width of the resin sheet is 10% or less. By using such a resin roll, it is possible to prevent slippage during transport and damage to the resin composition layer, and achieve a good yield.
[0013] The thermosetting resin composition layer contains a thermosetting resin. The thermosetting resin is not particularly limited, but examples thereof include epoxy resins, phenolic resins, cyanate ester resins, and benzoxazine resins.
[0014] In one embodiment, the thermosetting resin composition layer preferably contains an epoxy resin as a thermosetting resin. The epoxy resin is a curable resin having an epoxy group and an epoxy equivalent of 5,000 g / eq. or less.
[0015] Examples of epoxy resins include bixylenol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl ester type epoxy resins, and cresol novolac type epoxy resins. Resins, phenol aralkyl type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, tetraphenylethane type epoxy resins, isocyanurate type epoxy resins, phenolphthalimidine type epoxy resins, glycirol type epoxy resins, alkyleneoxy skeleton-containing epoxy resins, fluorene structure-containing epoxy resins, etc. The epoxy resins may be used alone or in combination of two or more.
[0016] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as “liquid epoxy resins”) and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as “solid epoxy resins”). The thermosetting resin composition layer may contain only liquid epoxy resins as the epoxy resin, or may contain only solid epoxy resins, or may contain both liquid and solid epoxy resins, but it is particularly preferable that the thermosetting resin composition layer contains both liquid and solid epoxy resins.
[0017] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.
[0018] Preferred liquid epoxy resins include glycirol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins having an ester skeleton, cyclohexane dimethanol type epoxy resins, cyclic aliphatic glycidyl ether and epoxy resins having a butadiene structure, dicyclopentadiene type epoxy resins, alkyleneoxy skeleton-containing epoxy resins, and fluorene structure-containing epoxy resins.
[0019] Specific examples of liquid epoxy resins include "EX-992L" manufactured by Nagase ChemteX Corporation, "YX7400" manufactured by Mitsubishi Chemical Corporation, "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "828EL", "825", and "Epikote 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" manufactured by Mitsubishi Chemical Corporation. " (bisphenol F type epoxy resin); "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630", "630LSD", "604" (glycidylamine type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (glycirol type epoxy resin) manufactured by ADEKA Corporation; "EP-3950L", "EP-3980S" (glycidylamine type epoxy resin) manufactured by ADEKA Corporation; "EP-4088S" (dicyclopentadiene type epoxy resin) manufactured by ADEKA Corporation; "ZX1059" (mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nippon Steel Chemical & Material Corporation; "EX-721" (glycidyl ester type epoxy resin) manufactured by Nagase ChemteX Corporation; "EX-991L" (alkyleneoxy skeleton-containing epoxy resin) manufactured by Nagase ChemteX Corporation; "Celloxide 2021P" (alicyclic epoxy resin with ester skeleton) manufactured by Daicel Corporation; Examples of such epoxy resins include "PB-3600" manufactured by Daicel Corporation, "JP-100" and "JP-200" manufactured by Nippon Soda Co., Ltd. (epoxy resins having a butadiene structure); "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resins) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "EG-280" (fluorene structure-containing epoxy resin) manufactured by Osaka Gas Chemicals Co., Ltd.; and "EX-201" (cyclic aliphatic glycidyl ether) manufactured by Nagase ChemteX Corporation.
[0020] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.
[0021] Preferred solid epoxy resins include bixylenol type epoxy resins, naphthalene type epoxy resins, naphthalene type tetrafunctional epoxy resins, naphthol novolac type epoxy resins, cresol novolac type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol type epoxy resins, biphenyl type epoxy resins, naphthylene ether type epoxy resins, anthracene type epoxy resins, bisphenol A type epoxy resins, bisphenol AF type epoxy resins, phenol aralkyl type epoxy resins, tetraphenylethane type epoxy resins, phenolphthalimidine type epoxy resins, and fluorene structure-containing epoxy resins.
[0022] Specific examples of solid epoxy resins include DIC Corporation's "HP4032H" (naphthalene type epoxy resin); DIC Corporation's "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins); DIC Corporation's "N-690" and "N-695" (cresol novolac type epoxy resins); DIC Corporation's "HP-7200", "HP-7200HH", "HP-7200H", and "HP-7200L" (dicyclopentadiene type epoxy resins); DIC Corporation's "EXA-7311", "EXA-7311-G3", and "EXA-73 11-G4", "EXA-7311-G4S", "HP6000", "HP6000L" (naphthylene ether type epoxy resin); "EPPN-502H" (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC7000L" (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC3000H", "NC3000", "NC3000L", "NC3000FH", "NC3100" (biphenyl type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "ESN475V", "ESN4100V" (naphthyl type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd. naphthalene type epoxy resin); "ESN485" (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN375" (dihydroxynaphthalene type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YX4000HK", "YL7890" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX7700" manufactured by Mitsubishi Chemical Co., Ltd. (phenol aralkyl type epoxy resin); "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals; "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical; "YL7800" (fluorene structure-containing epoxy resin) manufactured by Mitsubishi Chemical; "jER1010" (bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical; "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical; "WHR991S" (phenolphthalimidine type epoxy resin) manufactured by Nippon Kayaku Co., Ltd. These may be used alone or in combination of two or more.
[0023] When a liquid epoxy resin and a solid epoxy resin are used in combination as the epoxy resin, the mass ratio thereof (liquid epoxy resin:solid epoxy resin) is preferably 10:1 to 1:50, more preferably 5:1 to 1:20, even more preferably 2:1 to 1:10, and particularly preferably 1:1 to 1:3.
[0024] The epoxy equivalent of the epoxy resin is preferably 50 g / eq. to 5,000 g / eq., more preferably 60 g / eq. to 2,000 g / eq., even more preferably 70 g / eq. to 1,000 g / eq., and even more preferably 80 g / eq. to 500 g / eq. The epoxy equivalent is the mass of the resin per equivalent of epoxy group. This epoxy equivalent can be measured according to JIS K7236.
[0025] The weight average molecular weight of the epoxy resin is preferably 100 to 5,000, more preferably 250 to 3,000, and further preferably 400 to 1500. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.
[0026] The content of the epoxy resin in the thermosetting resin composition layer is not particularly limited, but when the total non-volatile components are taken as 100 mass%, the upper limit is preferably 50 mass% or less, more preferably 40 mass% or less, even more preferably 30 mass% or less, even more preferably 20 mass% or less, and particularly preferably 15 mass% or less, and the lower limit is, for example, 0 mass% or more, 0.1 mass% or more, preferably 0.5 mass% or more, more preferably 1 mass% or more, even more preferably 5 mass% or more, even more preferably 8 mass% or more, and particularly preferably 10 mass% or more.
[0027] When the thermosetting resin composition layer contains an epoxy resin as a thermosetting resin, it may further contain an epoxy resin curing agent as an optional component. The epoxy resin curing agent may be used alone or in any combination of two or more kinds. When the thermosetting resin contains an epoxy resin, the epoxy resin curing agent may have a function of reacting with the epoxy resin to cure it.
[0028] The epoxy resin curing agent is not particularly limited, and examples thereof include active ester curing agents, phenolic curing agents, carbodiimide curing agents, acid anhydride curing agents, amine curing agents, benzoxazine curing agents, cyanate ester curing agents, and thiol curing agents. In one embodiment, the epoxy resin curing agent preferably contains one or more epoxy resin curing agents selected from active ester curing agents, phenolic curing agents, and carbodiimide curing agents, and more preferably contains one or more epoxy resin curing agents selected from active ester curing agents and phenolic curing agents. In one embodiment, the epoxy resin curing agent is particularly preferably contains an active ester curing agent from the viewpoint of suppressing the dielectric tangent to a lower level. In one embodiment, the epoxy resin curing agent is particularly preferably contains a phenolic curing agent from the viewpoint of further improving the curability.
[0029] As the active ester curing agent, generally, compounds having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are preferably used. The active ester compound is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester compound obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester compound obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.
[0030] Specifically, the active ester curing agent is preferably a dicyclopentadiene type active ester compound, a naphthalene type active ester compound containing a naphthalene structure, an active ester compound containing an acetylated product of phenol novolac, or an active ester compound containing a benzoylated product of phenol novolac, and more preferably at least one selected from a dicyclopentadiene type active ester compound and a naphthalene type active ester compound. As the dicyclopentadiene type active ester compound, an active ester compound containing a dicyclopentadiene type diphenol structure is preferable.
[0031] Commercially available active ester curing agents include active ester compounds containing a dicyclopentadiene-type diphenol structure, such as "EXB9451", "EXB9460", "EXB9460S", "HPC-8000L-65TM", "HPC-8000-65T", "HPC-8000H", and "HPC-8000H-65TM" (manufactured by DIC Corporation); and active ester compounds containing a naphthalene structure, such as "HP-B-8151-62T", "EXB-8100L-65T", "EXB-9416-70BK", and "HPC-8150-62T". and "EXB-8" (manufactured by DIC Corporation); an active ester compound containing phosphorus, "EXB9401" (manufactured by DIC Corporation), an active ester compound which is an acetylated product of phenol novolac, "DC808" (manufactured by Mitsubishi Chemical Corporation), active ester compounds which are benzoylated products of phenol novolac, "YLH1026", "YLH1030", and "YLH1048" (manufactured by Mitsubishi Chemical Corporation), and an active ester compound containing a styryl group and a naphthalene structure, "PC1300-02-65MA" (manufactured by Air Water Corporation), etc.
[0032] As the phenol-based curing agent, from the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure is preferable. Also, from the viewpoint of adhesion to the adherend, a nitrogen-containing phenol-based curing agent is preferable, and a triazine skeleton-containing phenol-based curing agent is more preferable. Among them, from the viewpoint of highly satisfying heat resistance, water resistance, and adhesion, a triazine skeleton-containing phenol novolac resin is preferable. Specific examples of phenol-based curing agents include "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd.; "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd.; "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-375", and "SN-395" manufactured by Nippon Steel Chemical & Material Co., Ltd.; and "LA-7052", "LA-7054", "LA-3018", "LA-3018-50P", "LA-1356", "TD2090", and "KA-1160" manufactured by DIC Corporation.
[0033] Examples of the carbodiimide-based curing agent include curing agents having one or more, preferably two or more, carbodiimide structures in one molecule, such as aliphatic biscarbodiimides, such as tetramethylene-bis(t-butylcarbodiimide) and cyclohexane bis(methylene-t-butylcarbodiimide); aromatic biscarbodiimides, such as phenylene-bis(xylylcarbodiimide); and aliphatic polycarbodiimides, such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), and poly(isophoronecarbodiimide). ; polycarbodiimides such as aromatic polycarbodiimides such as poly(phenylenecarbodiimide), poly(naphthylenecarbodiimide), poly(tolylenecarbodiimide), poly(methyldiisopropylphenylenecarbodiimide), poly(triethylphenylenecarbodiimide), poly(diethylphenylenecarbodiimide), poly(triisopropylphenylenecarbodiimide), poly(diisopropylphenylenecarbodiimide), poly(xylylenecarbodiimide), poly(tetramethylxylylenecarbodiimide), poly(methylenediphenylenecarbodiimide), and poly[methylenebis(methylphenylene)carbodiimide].
[0034] Commercially available carbodiimide curing agents include, for example, "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-07", and "Carbodilite V-09" manufactured by Nisshinbo Chemical Co., Ltd.; and "Stavaxol P", "Stavaxol P400", and "Hi-Kasil 510" manufactured by LANXESS AG.
[0035] Examples of the acid anhydride curing agent include a curing agent having one or more acid anhydride groups in one molecule, and a curing agent having two or more acid anhydride groups in one molecule is preferable. Specific examples of the acid anhydride curing agent include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic dianhydride, and the like. Examples of acid anhydrides include anhydrides, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resin, which is a copolymer of styrene and maleic acid. Commercially available acid anhydride curing agents include "HNA-100", "MH-700", "MTA-15", "DDSA", and "OSA" manufactured by New Japan Chemical Co., Ltd., "YH-306" and "YH-307" manufactured by Mitsubishi Chemical Corporation, "HN-2200" and "HN-5500" manufactured by Resonaq, and "EF-30", "EF-40", "EF-60", and "EF-80" manufactured by Cray Valley Chemical Industries, Ltd.
[0036] The amine-based curing agent may be a curing agent having one or more, preferably two or more, amino groups in one molecule, such as aliphatic amines, polyether amines, alicyclic amines, aromatic amines, etc., and among them, aromatic amines are preferred from the viewpoint of achieving the desired effects of the present invention. The amine-based curing agent is preferably a primary amine or secondary amine, and more preferably a primary amine. Specific examples of amine-based curing agents include 4,4'-methylenebis(2,6-dimethylaniline), 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, and 2,2-bis(3-amino-4-hydroxyphenyl)propane. propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, and the like. As the amine-based curing agent, commercially available products may be used, and examples thereof include "SEIKACURE-S" manufactured by Seika Corporation, "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", and "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd., and "Epicure W" manufactured by Mitsubishi Chemical Corporation.
[0037] Specific examples of benzoxazine-based curing agents include "JBZ-OP100D" and "ODA-BOZ" manufactured by JFE Chemical Corporation; "HFB2006M" manufactured by Showa Polymer Co., Ltd.; and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.
[0038] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include Lonza's "PT30" and "PT60" (both of which are phenol novolac-type multifunctional cyanate ester resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer).
[0039] Examples of thiol-based curing agents include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), and tris(3-mercaptopropyl)isocyanurate.
[0040] The reactive group equivalent of the epoxy resin curing agent is preferably 50 g / eq. to 3000 g / eq., more preferably 100 g / eq. to 1000 g / eq., further preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The reactive group equivalent is the mass of the epoxy resin curing agent per equivalent of reactive group.
[0041] The content of the epoxy resin curing agent in the thermosetting resin composition layer is not particularly limited, but when the total non-volatile components are taken as 100 mass%, the upper limit is preferably 50 mass% or less, more preferably 30 mass% or less, even more preferably 25 mass% or less, and particularly preferably 20 mass% or less, and the lower limit can be, for example, 0 mass% or more, 0.01 mass% or more, preferably 0.1 mass% or more, more preferably 1 mass% or more, even more preferably 5 mass% or more, and particularly preferably 8 mass% or more.
[0042] The thermosetting resin composition layer may contain a curing accelerator as an optional component. The curing accelerator functions as a curing catalyst that accelerates the curing of the thermosetting resin.
[0043] Examples of the curing accelerator include phosphorus-based curing accelerators, urea-based curing accelerators, guanidine-based curing accelerators, imidazole-based curing accelerators, metal-based curing accelerators, and amine-based curing accelerators. The curing accelerator preferably includes an amine-based curing accelerator or an imidazole-based curing accelerator. The curing accelerator may be used alone or in combination of two or more.
[0044] Examples of the phosphorus-based curing accelerator include aliphatic phosphonium salts such as tetrabutylphosphonium bromide, tetrabutylphosphonium chloride, tetrabutylphosphonium acetate, tetrabutylphosphonium decanoate, tetrabutylphosphonium laurate, bis(tetrabutylphosphonium)pyromellitate, tetrabutylphosphonium hydrogenhexahydrophthalate, tetrabutylphosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, and di-tert-butylmethylphosphonium tetraphenylborate; methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, propyltriphenylphosphonium bromide, butyltriphenylphosphonium bromide, benzyltriphenylphosphonium chloride, tetraphenylphosphonium bromide, p-tolyltriphenylphosphonium tetra-p-tolylborate ... aromatic phosphonium salts such as tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone adducts such as triphenylphosphine-p-benzoquinone adduct; aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine;Dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tris(4-ethylphenyl)phosphine, tris(4-propylphenyl)phosphine, tris(4-isopropylphenyl)phosphine, tris(4-butylphenyl)phosphine, tris(4-tert-butylphenyl)phosphine, tris(2,4-dimethylphenyl)phosphine, tris(2,5-dimethylphenyl)phosphine, tris(2,6-dimethylphenyl)phosphine Examples of aromatic phosphines include tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether.
[0045] Examples of the urea-based curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, and 3-(3,4-dimethylphenyl)-1,1-dimethylurea. aromatic dimethylureas such as butylurea, 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), and N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluene bisdimethylurea].
[0046] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.
[0047] Examples of the imidazole-based curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine. 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl- Examples of the imidazole compound include 4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins.
[0048] As the imidazole-based curing accelerator, commercially available products may be used, for example, "1B2PZ", "2MZA-PW", "2PHZ-PW", and "C11Z-A" manufactured by Shikoku Chemical Industry Co., Ltd., and "P200-H50" manufactured by Mitsubishi Chemical Corporation.
[0049] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
[0050] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene.
[0051] As the amine-based curing accelerator, a commercially available product may be used, for example, "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd.
[0052] The content of the curing accelerator in the thermosetting resin composition layer is not particularly limited, but when the total non-volatile components are taken as 100 mass%, the upper limit is preferably 5 mass% or less, more preferably 1 mass% or less, even more preferably 0.5 mass% or less, and particularly preferably 0.3 mass% or less, and the lower limit is, for example, 0 mass% or more, preferably 0.001 mass% or more, even more preferably 0.01 mass% or more, and particularly preferably 0.03 mass% or more.
[0053] The thermosetting resin composition layer contains an inorganic filler. The inorganic filler is contained in the resin composition layer in the form of particles.
[0054] As the material of the inorganic filler, an inorganic compound is used. As the material of the inorganic filler, for example, silica, alumina, aluminosilicate, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate can be mentioned. Among these, silica, alumina, and aluminosilicate are suitable, and silica is particularly suitable. As the silica, for example, amorphous silica, fused silica, crystalline silica, synthetic silica, hollow silica, etc. can be mentioned. In addition, as the silica, spherical silica is preferable. The inorganic filler may be used alone or in combination of two or more kinds in any ratio.
[0055] Examples of commercially available inorganic fillers include "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "UFP-30", "DAW-03", and "FB-105FD" manufactured by Denka Co., Ltd.; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "Cellspheres" and "MGH-005" manufactured by Pacific Cement Corporation; and "Sfereek" and "BA-1" manufactured by JGC Catalysts and Chemicals Co., Ltd.
[0056] The average particle size of the inorganic filler is not particularly limited, but is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 3 μm or less, even more preferably 2 μm or less, and particularly preferably 1 μm or less. The lower limit of the average particle size of the inorganic filler is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and particularly preferably 0.2 μm or more. The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is taken as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. The measurement sample was measured using a laser diffraction type particle size distribution measuring device with blue and red light source wavelengths, and the particle size distribution of the inorganic filler on a volume basis was measured using a flow cell method, and the average particle size was calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction type particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.
[0057] The specific surface area of the inorganic filler is not particularly limited, but is preferably 0.1 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 3m 2 The upper limit of the specific surface area of the inorganic filler is not particularly limited, but is preferably 100 m 2 / g or less, more preferably 70m 2 / g or less, more preferably 50m 2 / g or less, and even more preferably 30m 2 / g or less, particularly preferably 10m 2 The specific surface area of the inorganic filler is obtained by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.
[0058] In order to improve moisture resistance and dispersibility, the inorganic filler is preferably treated with a surface treatment agent. Examples of the surface treatment agent include fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, and titanate coupling agents. The surface treatment agent may be used alone or in any combination of two or more.
[0059] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).
[0060] From the viewpoint of improving the dispersibility of the inorganic filler, the degree of surface treatment with the surface treatment agent is preferably within a predetermined range. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2% to 5% by mass of the surface treatment agent, more preferably 0.2% to 3% by mass, and even more preferably 0.3% to 2% by mass.
[0061] The content of the inorganic filler in the thermosetting resin composition layer, when the total non-volatile components is 100 mass%, has an upper limit of preferably 90 mass% or less, more preferably 85 mass% or less, even more preferably 80 mass% or less, and particularly preferably 75 mass% or less, and has a lower limit of preferably 1 mass% or more, preferably 10 mass% or more, more preferably 30 mass% or more, even more preferably 40 mass% or more, even more preferably 50 mass% or more, even more preferably 55 mass% or more, and particularly preferably 60 mass% or more.
[0062] The thermosetting resin composition layer may contain a thermoplastic resin as an optional component. The thermoplastic resin described here is a component other than the elastomer and maleimide resin described below.
[0063] Examples of the thermoplastic resin include phenoxy resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyimide resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, polyester resin, etc. Among them, phenoxy resin is preferable from the viewpoint of obtaining the effect of the present invention remarkably. The phenoxy resin described here is a component other than those corresponding to epoxy resin. In addition, the thermoplastic resin may be used alone or in combination of two or more kinds.
[0064] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group.
[0065] Specific examples of phenoxy resins include "1256" and "4250" manufactured by Mitsubishi Chemical Corporation (both of which are phenoxy resins containing a bisphenol A skeleton); "YX8100" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol S skeleton); "YX6954" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol acetophenone skeleton); "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", "YL7482", and "YL7891BH30" manufactured by Mitsubishi Chemical Corporation.
[0066] Examples of polyvinyl acetal resins include polyvinyl formal resins and polyvinyl butyral resins, and polyvinyl butyral resins are preferred.Specific examples of polyvinyl acetal resins include S-LEC BH series, BX series (e.g., BX-5Z), KS series (e.g., KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.
[0067] Examples of polyolefin resins include ethylene-based copolymer resins such as low-density polyethylene, very low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer; and polyolefin polymers such as polypropylene and ethylene-propylene block copolymer.
[0068] Specific examples of polyimide resins include "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd.
[0069] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as "KS9100" and "KS9300" (polysiloxane skeleton-containing polyamide-imide) manufactured by Resonac Corporation.
[0070] A specific example of the polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd.
[0071] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.
[0072] Examples of the polyester resin include polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polybutylene naphthalate resin, polytrimethylene terephthalate resin, polytrimethylene naphthalate resin, and polycyclohexane dimethyl terephthalate resin.
[0073] From the viewpoint of obtaining the effects of the present invention remarkably, the weight average molecular weight of the thermoplastic resin is preferably 8,000 or more, more preferably 10,000 or more, particularly preferably 20,000 or more, and is preferably 70,000 or less, more preferably 60,000 or less, particularly preferably 50,000 or less.
[0074] The content of the thermoplastic resin in the thermosetting resin composition layer is not particularly limited, but when the total non-volatile components are 100 mass%, the upper limit is preferably 50 mass% or less, more preferably 30 mass% or less, even more preferably 10 mass% or less, even more preferably 5 mass% or less, and particularly preferably 3 mass% or less, and the lower limit is, for example, 0 mass% or more, 0.1 mass% or more, 0.5 mass% or more, 1 mass% or more, etc.
[0075] The thermosetting resin composition layer may contain an elastomer as an optional component. The elastomer described here is a component other than the maleimide resin described below.
[0076] The elastomer is a resin having flexibility, and is preferably a resin having rubber elasticity or a resin exhibiting rubber elasticity by polymerization with other components. Examples of rubber elasticity include resins exhibiting an elastic modulus of 1 GPa or less when a tensile test is performed at a temperature of 25°C and a humidity of 40% RH according to the Japanese Industrial Standards (JIS K7161).
[0077] In one embodiment, the elastomer is preferably a resin having, in the molecule, one or more structures selected from a polybutadiene structure, a polysiloxane structure, a poly(meth)acrylate structure, a polyalkylene structure, a polyalkyleneoxy structure, a polyisoprene structure, a polyisobutylene structure, a polycarbonate structure, and a polystyrene structure. "(Meth)acrylate" refers to methacrylate and acrylate.
[0078] In another embodiment, the elastomer is preferably one or more selected from a resin having a glass transition temperature (Tg) of 25° C. or less and a resin that is liquid at 25° C. or less. The glass transition temperature of the resin having a glass transition temperature (Tg) of 25° C. or less is preferably 20° C. or less, more preferably 15° C. or less. The lower limit of the glass transition temperature is not particularly limited, but can usually be −15° C. or more. The resin that is liquid at 25° C. is preferably a resin that is liquid at 20° C. or less, more preferably a resin that is liquid at 15° C. or less. The glass transition temperature can be measured by DSC (differential scanning calorimetry).
[0079] The elastomer is generally an amorphous resin component that can be dissolved in an organic solvent. One type of elastomer may be used alone, or two or more types may be used in combination in any ratio.
[0080] The elastomer may be, for example, a resin containing a polybutadiene structure. The polybutadiene structure may be contained in the main chain or in the side chain. The polybutadiene structure may be partially or entirely hydrogenated. A resin containing a polybutadiene structure may be called a "polybutadiene resin." Specific examples of polybutadiene resins include "Ricon 130MA8", "Ricon 130MA13", "Ricon 130MA20", "Ricon 131MA5", "Ricon 131MA10", "Ricon 131MA17", "Ricon 131MA20", and "Ricon 184MA6" (polybutadiene containing an acid anhydride group) manufactured by Cray Valley Corporation; "GQ-1000" (polybutadiene having hydroxyl groups and carboxyl groups introduced therein), "G-1000", "G-2000", and "G-3000" (polybutadiene having hydroxyl groups at both ends), "GI-1000", "GI-2000", and "GI-3000" (polybutadiene having hydrogenated hydroxyl groups at both ends) manufactured by Nippon Soda Co., Ltd.; and "FCA-061L" (hydrogenated polybutadiene skeleton epoxy resin) manufactured by Nagase ChemteX Corporation. Specific examples of polybutadiene resins include hydroxyl-terminated polybutadiene, linear polyimides made from diisocyanate compounds and tetrabasic acid anhydrides (polyimides described in JP 2006-37083 A and WO 2008 / 153208 A), and phenolic hydroxyl-containing butadiene. The content of the butadiene structure in the polyimide resin is preferably 60% by mass to 95% by mass, more preferably 75% by mass to 85% by mass. For details of the polyimide resin, refer to the descriptions in JP 2006-37083 A and WO 2008 / 153208 A, the contents of which are incorporated herein by reference.
[0081] Examples of elastomers include resins containing a poly(meth)acrylate structure. Resins containing a poly(meth)acrylate structure are sometimes called "poly(meth)acrylic resins." Specific examples of poly(meth)acrylic resins include Teisan Resin manufactured by Nagase ChemteX Corporation, and ME-2000, W-116.3, W-197C, KG-25, and KG-3000 manufactured by Negami Chemical Industries, Ltd.
[0082] Examples of elastomers include resins containing a polycarbonate structure. Resins containing a polycarbonate structure are sometimes called "polycarbonate resins". Specific examples of polycarbonate resins include "T6002" and "T6001" (polycarbonate diols) manufactured by Asahi Kasei Corporation, and "C-1090", "C-2090", and "C-3090" (polycarbonate diols) manufactured by Kuraray Co., Ltd. In addition, linear polyimides made from hydroxyl-terminated polycarbonates, diisocyanate compounds, and tetrabasic acid anhydrides can also be used. The content of the carbonate structure in the polyimide resin is preferably 60% by mass to 95% by mass, more preferably 75% by mass to 85% by mass. Details of the polyimide resin can be found in International Publication No. WO 2016 / 129541, the contents of which are incorporated herein by reference.
[0083] Examples of elastomers include resins containing a polysiloxane structure. Resins containing a polysiloxane structure are sometimes called "siloxane resins." Specific examples of siloxane resins include "SMP-2006," "SMP-2003PGMEA," and "SMP-5005PGMEA" manufactured by Shin-Etsu Silicone Co., Ltd., and linear polyimides made from amine-terminated polysiloxanes and tetrabasic acid anhydrides (see International Publication No. 2010 / 053185, JP 2002-12667 A, JP 2000-319386 A, etc.).
[0084] Examples of the elastomer include resins containing a polyalkylene structure or a polyalkyleneoxy structure. A resin containing a polyalkylene structure may be referred to as an "alkylene resin". A resin containing a polyalkyleneoxy structure may be referred to as an "alkyleneoxy resin". The polyalkyleneoxy structure is preferably a polyalkyleneoxy structure having 2 to 15 carbon atoms, more preferably a polyalkyleneoxy structure having 3 to 10 carbon atoms, and particularly preferably a polyalkyleneoxy structure having 5 to 6 carbon atoms. Specific examples of the alkylene resin and the alkyleneoxy resin include "PTXG-1000" and "PTXG-1800" manufactured by Asahi Kasei Corporation.
[0085] Examples of elastomers include resins containing a polyisoprene structure. Resins containing a polyisoprene structure are sometimes called "isoprene resins." Specific examples of isoprene resins include "KL-610" and "KL613" manufactured by Kuraray Co., Ltd.
[0086] Examples of elastomers include resins containing a polyisobutylene structure. Resins containing a polyisobutylene structure are sometimes called "isobutylene resins." Specific examples of isobutylene resins include Kaneka Corporation's "SIBSTAR-073T" (styrene-isobutylene-styrene triblock copolymer) and "SIBSTAR-042D" (styrene-isobutylene diblock copolymer).
[0087] Examples of elastomers include resins containing a polystyrene structure. Resins containing a polystyrene structure are sometimes called "styrene resins." Examples of styrene resins include styrene-butadiene-styrene block copolymers (SBS), styrene-isoprene-styrene block copolymers (SIS), styrene-ethylene-butylene-styrene block copolymers (SEBS), styrene-ethylene-propylene-styrene block copolymers (SEPS), styrene-ethylene-ethylene-propylene-styrene block copolymers (SEEPS), styrene-butadiene-butylene-styrene block copolymers (SBBS), styrene-butadiene diblock copolymers, hydrogenated styrene-butadiene block copolymers, hydrogenated styrene-isoprene block copolymers, and hydrogenated styrene-butadiene random copolymers. Specific examples of styrene resins include hydrogenated styrene-based thermoplastic elastomers "H1041", "Tuftec H1043", "Tuftec P2000", and "Tuftec MP10" (manufactured by Asahi Kasei Corporation); epoxidized styrene-butadiene thermoplastic elastomers "Epofriend AT501" and "CT310" (manufactured by Daicel Corporation); modified styrene-based elastomers having hydroxyl groups "Septon HG252" (manufactured by Kuraray Co., Ltd.); modified styrene-based elastomers having carboxyl groups "Tuftec N503M", modified styrene-based elastomers having amino groups "Tuftec N501", modified styrene-based elastomers having acid anhydride groups "Tuftec M1913" (manufactured by Asahi Kasei Co., Ltd.); unmodified styrene-based elastomers "Septon S8104" (manufactured by Kuraray Co., Ltd.); and styrene-ethylene / butylene-styrene block copolymers "FG1924" (manufactured by Kraton Co., Ltd.).
[0088] The number average molecular weight (Mn) of the elastomer is preferably 1,000 or more, more preferably 1,500 or more, even more preferably 3,000 or more, particularly preferably 5,000 or more, and is preferably 1,000,000 or less, more preferably 900,000 or less. The number average molecular weight (Mn) can be measured in terms of polystyrene using GPC (gel permeation chromatography).
[0089] The content of the elastomer in the thermoplastic resin composition layer is not particularly limited, but when the total non-volatile components are 100 mass%, the upper limit is preferably 50 mass% or less, more preferably 30 mass% or less, even more preferably 20 mass% or less, even more preferably 10 mass% or less, and particularly preferably 8 mass% or less, and the lower limit is, for example, 0 mass% or more, 0.1 mass% or more, 0.5 mass% or more, 1 mass% or more, etc.
[0090] The thermosetting resin composition layer may contain a maleimide resin as an optional component. The maleimide resin is not particularly limited, but is preferably a resin having two or more maleimide groups in one molecule, such as a dimer acid skeleton-containing maleimide resin, a trimethylindane skeleton-containing maleimide resin, or a biphenylaralkyl-type maleimide resin.
[0091] The dimer acid skeleton-containing maleimide resin is, for example, a bismaleimide compound having a hydrocarbon skeleton derived from a dimer acid. The dimer acid skeleton-containing maleimide resin is, for example, a bismaleimide compound obtained by imidizing at least a dimer acid type diamine with maleic anhydride, and further includes a bismaleimide compound obtained by imidizing a dimer acid type diamine with a tetracarboxylic dianhydride and maleic anhydride.
[0092] Commercially available dimer acid skeleton-containing maleimide resins include, for example, "BMI-689", "BMI-1500", "BMI-1700", and "BMI-3000J" manufactured by Designer Molecules Inc., and "SLK-6895-T90" manufactured by Shin-Etsu Chemical Co., Ltd. Commercially available biphenyl aralkyl type maleimide resins include "MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd. Trimethylindane skeleton-containing maleimide resins can be produced, for example, by using the method described in the Japan Institute of Invention and Innovation Disclosure Technical Bulletin No. 2020-500211 or a method equivalent thereto.
[0093] The maleimide group equivalent of the maleimide resin is preferably 30 g / eq. to 2500 g / eq., particularly preferably 75 g / eq. to 2000 g / eq. The weight average molecular weight of the maleimide resin is preferably 100 to 20,000, more preferably 150 to 10,000, particularly preferably 200 to 5,000.
[0094] The content of the maleimide resin in the thermoplastic resin composition layer is not particularly limited, but when the total non-volatile components are taken as 100 mass%, the upper limit is preferably 50 mass% or less, more preferably 30 mass% or less, even more preferably 20 mass% or less, even more preferably 10 mass% or less, and particularly preferably 5 mass% or less, and the lower limit is, for example, 0 mass% or more, 0.1 mass% or more, 0.5 mass% or more, 0.8 mass% or more, etc.
[0095] The thermosetting resin composition layer may further contain additives as optional components. Examples of additives include organic fillers, thickeners, defoamers, leveling agents, adhesion promoters, flame retardants, etc. These may be used alone or in combination of two or more at any ratio.
[0096] The thermosetting resin composition layer contains an organic solvent as a volatile component in addition to the non-volatile components described above. The type of the organic solvent is not particularly limited. Examples of the organic solvent include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, and anisole; alcohol-based solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, and methyl methoxypropionate. Examples of suitable organic solvents include ether ester solvents such as ethyl acetate, ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate, ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butyl carbitol), amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone, sulfoxide solvents such as dimethyl sulfoxide, nitrile solvents such as acetonitrile and propionitrile, aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane, and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. The organic solvent may be used alone or in any combination of two or more kinds in any ratio.
[0097] The organic solvent in the thermosetting resin composition layer is contained in an amount such that, when the protective film is peeled off and the surface not in contact with the base film is exposed to the outside air, the weight loss rate of the thermosetting resin composition layer after heat treatment at 130°C for 15 minutes is 0.7 to 5% by mass. The lower limit of the weight loss rate is preferably 0.8% by mass or more, more preferably 0.9% by mass or more. The upper limit of the weight loss rate is preferably 3% by mass or less, more preferably 2% by mass or less, and even more preferably 1.3% by mass or less. The weight loss rate can be measured according to the method described in the Examples below.
[0098] The elastic modulus of the thermosetting resin composition layer, when measured at 23°C, is preferably 1 GPa or more, more preferably 2 GPa or more, particularly preferably 3 GPa or more, and is preferably 10 GPa or less, more preferably 8 GPa or less, particularly preferably 7 GPa or less.
[0099] From the viewpoint of thinning the printed wiring board, the film thickness of the thermosetting resin composition layer is preferably 300 μm or less, more preferably 250 μm or less, even more preferably 200 μm or less, even more preferably 150 μm or less, even more preferably 100 μm or less, and particularly preferably 80 μm or less. The lower limit of the film thickness of the thermosetting resin composition layer is not particularly limited, but can usually be 5 μm or more, 10 μm or more, 20 μm or more, 30 μm or more, 40 μm or more, 50 μm or more, etc.
[0100] The coefficient of linear thermal expansion (CTE) of the thermosetting resin composition layer after curing is preferably 100 ppm / ° C. or less, more preferably 70 ppm / ° C. or less, even more preferably 50 ppm / ° C. or less, still more preferably 40 ppm / ° C. or less, and particularly preferably 35 ppm / ° C. or less, in the range of 25° C. to 150° C. The coefficient of linear thermal expansion (CTE) of the thermosetting resin composition layer after curing can be measured, for example, by the same method as in Test Example 6 below.
[0101] The dielectric loss tangent (Df) of the thermosetting resin composition layer after curing is preferably 0.010 or less, more preferably 0.007 or less, even more preferably 0.006 or less, still more preferably 0.005 or less, and particularly preferably 0.004 or less, when measured at 5.8 GHz and 23° C. The dielectric loss tangent (Df) of the thermosetting resin composition layer after curing can be measured, for example, by the same method as in Test Example 7 below.
[0102] The thermosetting resin composition layer can be made into an insulating material by thermal curing after removing the base film and the protective film. Therefore, the thermosetting resin composition layer can be a resin composition for forming an insulating layer (a resin composition layer for forming an insulating layer). In particular, it can be suitably used as a resin composition layer for forming an insulating layer of a printed wiring board (a resin composition layer for forming an insulating layer of a printed wiring board). It can also be suitably used as a resin composition layer for forming an insulating layer (a resin composition layer for forming an insulating layer for forming a conductor layer) for forming a conductor layer (including a rewiring layer) formed on the insulating layer.
[0103] The resin roll of the present invention may be in a form in which the resin sheet is wound around a core core so that the base film is on the outside and the protective film is on the inside, or in a form in which the resin sheet is wound around a core core so that the base film is on the inside and the protective film is on the outside. In a preferred embodiment, the resin roll of the present invention is in a form in which the resin sheet is wound around a core core so that the base film is on the outside and the protective film is on the inside.
[0104] The base film and the protective film may be, for example, a plastic film, a metal foil, a release paper, etc., and a plastic film is preferable.
[0105] Examples of plastic films include polyester resin films such as polyethylene terephthalate film and polyethylene naphthalate film; polyolefin resin films such as polyethylene film and polypropylene film; acrylic resin films such as polymethyl methacrylate film; polycarbonate resin films; triacetyl cellulose resin films; polyether sulfide resin films; polyether ketone resin films; and polyimide resin films. Of these, polyethylene terephthalate film, polyethylene naphthalate film, polyethylene film, and polypropylene film are preferred.
[0106] The plastic film used as the base film is preferably a polyester resin film, more preferably a polyethylene terephthalate film or a polyethylene naphthalate film, and the plastic film used as the protective film is preferably a polyolefin resin film, more preferably a polypropylene film or a polyethylene film.
[0107] The surface of the plastic film which is to be bonded to the thermosetting resin composition layer may be subjected to a matte treatment, a corona treatment, an antistatic treatment, or the like.
[0108] The plastic film used as the base film is preferably a plastic film with a release layer, which has a release layer on the surface to be bonded to the thermosetting resin composition layer. If the plastic film has a release layer, the base film can be efficiently removed even after the thermosetting resin composition layer is thermally cured.
[0109] Examples of release agents used in the release layer of the plastic film with a release layer include fluororesin-based release agents such as PTFE (polytetrafluoroethylene), PFA (perfluoroalkoxy fluororesin), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), ETFE (ethylene-tetrafluoroethylene copolymer), ECTFE (ethylene-chlorotrifluoroethylene copolymer), and PVDF (polyvinylidene fluoride); and non-fluorine-based release agents such as alkyd resin-based release agents, melamine resin-based release agents, polyolefin resin-based release agents, and urethane resin-based release agents. Alkyd resin-based release agents are preferred, and non-silicone alkyd resin-based release agents are more preferred.
[0110] Commercially available alkyd resin-based release agents include silicone-containing alkyd resin-based release agents such as "X" and "SK-1" manufactured by Lintec; and non-silicone alkyd resin-based release agents such as "AL-5", "AL-7", "6050", "6051", and "6052" manufactured by Lintec, and "NSP-4" manufactured by Fujimori Kogyo Co., Ltd.
[0111] The density of the base film is preferably 0.8 g / cm 3 More preferably, 1.0 g / cm 3 More preferably, 1.2 g / cm 3 More preferably, 1.3 g / cm 3 The upper limit is not particularly limited, but may be, for example, 2.5 g / cm 3 Below 2.0g / cm 3 Below 1.5g / cm 3 It can be the following:
[0112] The thickness of the base film is not particularly limited, but is preferably 100 μm or less, more preferably 75 μm or less, even more preferably 60 μm or less, and particularly preferably 50 μm or less, and the lower limit of the thickness of the base film is not particularly limited, but is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and particularly preferably 20 μm or more. When a plastic film with a release layer is used, it is preferable that the thickness of the entire plastic film with a release layer is in the above range.
[0113] The density of the protective film is preferably 2.5 g / cm 3 Less than or equal to 2.0 g / cm 3 More preferably, 1.5 g / cm 3 Less than or equal to 1.3 g / cm 3 More preferably still, 1.1 g / cm 3 Less than 1.0 g / cm, particularly preferably 1.0 g / cm 3 The lower limit is, for example, 0.8 g / cm 3 It could be more than that.
[0114] The thickness of the protective film is not particularly limited, but is preferably 100 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The lower limit of the thickness of the protective film is not particularly limited, but is preferably 0.5 μm or more, more preferably 1 μm or more, even more preferably 5 μm or more, and particularly preferably 10 μm or more.
[0115] The difference between the width of the base film and the width of the thermosetting resin composition layer is preferably 20% or less, more preferably 10% or less, and further preferably 5% or less. b The width of the thermosetting resin composition layer is W r And W b / W r is W1, preferably 0.9≦W1≦1.1, more preferably 0.93≦W1≦1.07, even more preferably 0.94≦W1≦1.06, still more preferably 0.95≦W1≦1.05, still more preferably 0.97≦W1≦1.03, and particularly preferably 0.99≦W1≦1.01.
[0116] The difference between the width of the protective film and the width of the thermosetting resin composition layer is preferably 20% or less, more preferably 10% or less, and further preferably 5% or less. p The width of the thermosetting resin composition layer is W r And W p / W rWhen W2 is taken as W2, preferably 0.9≦W2≦1.1, more preferably 0.93≦W2≦1.07, even more preferably 0.94≦W2≦1.06, even more preferably 0.95≦W2≦1.05, even more preferably 0.97≦W2≦1.03, and particularly preferably 0.99≦W2≦1.01. b , the width W of the thermosetting resin composition layer r , and the width W of the protective film p may be different from each other or may be the same.
[0117] The average density of the entire resin sheet is 1.3 g / cm 3 or more, preferably 1.35 g / cm 3 More preferably, 1.4 g / cm 3 More preferably, 1.45 g / cm 3 More preferably, 1.5 g / cm 3 More preferably, 1.55 g / cm 3 The upper limit is preferably 2.5 g / cm 3 Less than or equal to 2.0 g / cm 3 More preferably, 1.8 g / cm 3 Less than or equal to 1.8g / cm 3 less than 1.7 g / cm 3 Less than 1.65 g / cm 3 The average density of the entire resin sheet referred to here is calculated by dividing the mass (g) of the entire resin sheet including the base film, the thermosetting resin composition layer, and the protective film by the volume (cm) of the entire resin sheet. 3 ) to calculate the density (g / cm 3 ) (i.e., [average density (g / cm 3 )] = [mass of the entire resin sheet (g)] / [volume of the entire resin sheet (cm 3 )]).
[0118] The width of the resin sheet is 300 mm or more, preferably 320 mm or more, and the upper limit is preferably 2000 mm or less, more preferably 1000 mm or less, further preferably 800 mm or less, and particularly preferably 600 mm or less. The width of the resin sheet here refers to the maximum width among the width of the base film, the width of the thermosetting resin composition layer, and the width of the protective film.
[0119] The resin sheet can be produced, for example, by preparing a varnish-like resin composition as is or by dissolving the resin composition in an organic solvent, applying this onto a substrate film using a die coater or the like, and then drying the composition to form a thermosetting resin composition layer, and then pressing a protective film onto the formed thermosetting resin composition layer.
[0120] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but the content of the organic solvent in the thermosetting resin composition layer is preferably 10% by mass or less, more preferably 8% by mass or less, even more preferably 5% by mass or less, even more preferably 3% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1.3% by mass or less. Although it varies depending on the boiling point of the organic solvent in the resin composition used, for example, when a resin composition containing 30% by mass to 60% by mass of the organic solvent is used, a thermosetting resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.
[0121] The core material may be, for example, plastic, metal, etc., and is preferably plastic. The plastic material of the core is not particularly limited, but examples thereof include polyimide resin, polyester resin, nylon resin, polyether ether ketone resin, acrylic resin, ABS resin, polyvinyl chloride resin, fluororesin, urethane resin, epoxy resin, acrylic-vinyl resin, polyester melamine resin, polystyrene resin, polycarbonate resin, etc.
[0122] The diameter of the core is preferably 30 mm or more, more preferably 40 mm or more, and particularly preferably 50 mm or more, with the upper limit being, for example, 150 mm or less.
[0123] The width of the core is, for example, 300 mm or more, preferably 320 mm or more, and the upper limit is preferably 2000 mm or less, more preferably 1000 mm or less, even more preferably 800 mm or less, and particularly preferably 600 mm or less.
[0124] The difference between the width of the core and the width of the resin sheet is preferably 10% or less, or 5% or less, more preferably 3% or less, even more preferably 1% or less, particularly preferably 0.1% or less, and most preferably 0.01% or less. c The width of the resin sheet is W s And W c / W s When W3 is W3, 0.9≦W3≦1.1. The lower limit of W3 is preferably 0.95 or more or 0.97 or more, more preferably 0.98 or more or 0.99 or more, even more preferably 0.991 or more, 0.995 or more, 0.998 or more, 0.999 or more, or 1 or more. The upper limit of W3 is preferably 1.05 or less or 1.03 or less, more preferably 1.02 or less or 1.01 or less, even more preferably 1.009 or less, 1.005 or less, 1.002 or less, or 1.001 or less. The width W of the resin sheet s is the width of the base film W b , the width W of the thermosetting resin composition layer r , width of protective film W p The maximum width of the b , W r , W p If there are multiple maximum widths, the maximum width among them is W s Let us assume that.
[0125] The density of the core is preferably 0.8 to 1.4 g / cm 3 , more preferably 0.8 to 1.3 g / cm 3 , and more preferably 0.8 to 1.2 g / cm 3 , particularly preferably 0.9 to 1.1 g / cm3 It is.
[0126] The difference between the density of the core in the resin roll and the average density of the entire resin sheet is preferably 0.1 g / cm 3 More preferably, 0.2 g / cm 3 More preferably, 0.3 g / cm 3 More preferably, 0.4 g / cm 3 More preferably, 0.5 g / cm 3 The upper limit is preferably 2.0 g / cm 3 Less than or equal to 1.5 g / cm 3 More preferably, 1.0 g / cm 3 Less than or equal to 0.8 g / cm 3 Less than 0.7 g / cm, particularly preferably 0.7 g / cm 3 The difference between the density of the core and the average density of the entire resin sheet is the average density of the entire resin sheet (g / cm 3 ) to the density of the core (g / cm 3 ) to obtain the density difference (g / cm 3 )
[0127] The winding length of the resin sheet around the core in the resin roll is preferably 300 m or less, more preferably 100 m or less, even more preferably 50 m or less, and particularly preferably 30 m or less. The lower limit is not particularly limited, but may be 1 m or more, 5 m or more, etc.
[0128] The resin roll is used by being installed in, for example, a resin sheet discharge device.
[0129] Fig. 1 is a schematic cross-sectional view of a resin sheet discharge device 100 in one embodiment when a resin roll is installed and a resin sheet is discharged. The cross-sectional view of Fig. 1 is a cross-sectional view of a surface perpendicular to the axial direction. Fig. 2 is a cross-sectional view taken along line AA of Fig. 1.
[0130] The resin sheet discharge device 100, in a form in which a resin roll 10 is installed, includes, as shown in Figures 1 and 2, the resin roll 10 having a core core 12 and a resin sheet 11a wound around the core core 12 as described above, a fixing member 20 having a support portion 21 and a stop portion 22, a conveying roll 30, etc.
[0131] 1, the resin sheet 11a wound around the core 12 is unwound from the resin roll 10 of the resin sheet unloading device 100. The unwound resin sheet 11b is unloaded from the resin roll 10 to the transport roll 30 and changes the unloading direction so as to come into contact with the transport roll 30.
[0132] 2, the axial support portion 21 of the fixing member 20 has a shape that protrudes perpendicularly to the plane of the shaft stop portion 22, and the axial support portions 21 of a pair of fixing members 20 are fitted into recesses formed in the center of both ends of the cylindrical core core 12, respectively, to rotatably fix the core core 12, thereby axially supporting the core core 12. The shape of the axial support portion 21 is not particularly limited as long as it can axially support the core core 12.
[0133] As shown in Figure 2, the axial stop portion 22 of the fixing member 20 is planar and perpendicular to the axial direction, and contacts both ends of the structure consisting of the core core 12 and the resin sheet 11a wound around the core core 12, thereby functioning as a so-called flange that limits the axial movement of the core core 12 and the resin sheet 11a wound around the core core 12 as a whole.
[0134] The resin roll of the present invention can be used in a method for producing a printed wiring board, which includes the following steps (1) to (4). (1) A process for removing a resin sheet from a resin roll (2) Peeling the protective film off the resin sheet (3) A step of laminating the resin sheet after peeling off the protective film onto the inner layer substrate so that the thermosetting resin composition layer is bonded to the inner layer substrate. (4) A step of thermally curing the thermosetting resin composition layer to form an insulating layer.
[0135] The protective film in step (2) may be peeled off manually or mechanically by an automatic peeling device. The method of peeling off the protective film in step (2) may include, for example, a method of conveying the thermosetting resin composition layer and the base film while the protective film is fixed, and peeling off the protective film, a method of pulling the protective film while the thermosetting resin composition layer and the base film are fixed, and a method of conveying the thermosetting resin composition layer and the base film while pulling the protective film, and peeling off the protective film, but is not limited thereto as long as the protective film can be peeled off from the thermosetting resin composition layer without damaging the thermosetting resin composition layer.
[0136] The inner layer substrate used in step (3) is a member that becomes the substrate of the printed wiring board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The substrate may have a conductor layer on one or both sides, and the conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate may be called an inner layer circuit substrate. In addition, an intermediate product on which an insulating layer and / or a conductor layer is to be further formed during the manufacture of a printed wiring board is also included in the inner layer substrate of the present invention. When the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components may be used.
[0137] The lamination of the resin sheet to the inner layer substrate after peeling off the protective film in step (3) can be carried out, for example, by thermocompression bonding the resin sheet to the inner layer substrate from the base film side. Examples of the member for thermocompression bonding the resin sheet to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression bonding member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the inner layer substrate.
[0138] The lamination in step (3) may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination in step (3) may be performed under reduced pressure conditions, preferably at a pressure of 26.7hPa or less.
[0139] The lamination in step (3) can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.
[0140] In step (3), after lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the substrate film side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. Note that the lamination and the smoothing treatment may be performed successively using the commercially available vacuum laminator.
[0141] The base film may be removed between step (3) and step (4), or may be removed after step (4).
[0142] In step (4), the thermosetting resin composition layer is thermally cured to form an insulating layer made of a cured product of the resin composition. The conditions for thermally curing the thermosetting resin composition layer are not particularly limited, and conditions that are usually adopted when forming an insulating layer for a printed wiring board may be used.
[0143] For example, the heat curing conditions of the thermosetting resin composition layer vary depending on the types of components contained in the resin composition layer, but in one embodiment, the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and even more preferably 170° C. to 210° C. The curing time can be preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.
[0144] Before the thermosetting resin composition layer is thermally cured, the thermosetting resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the thermosetting resin composition layer, the thermosetting resin composition layer may be preheated at a temperature of 50°C to 120°C, preferably 60°C to 115°C, more preferably 70°C to 110°C for 5 minutes or more, preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes.
[0145] In manufacturing a printed wiring board, in addition to the above steps (1) to (4), a step (5) of drilling holes in the insulating layer, a step (6) of roughening the insulating layer, and a step (7) of forming a conductor layer may be further carried out. These steps (5) to (7) may be carried out according to various methods used in manufacturing printed wiring boards and known to those skilled in the art. Furthermore, if necessary, the formation of the insulating layer and the conductor layer in steps (1) to (7) may be repeated to form a multilayer wiring board.
[0146] Step (5) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (5) may be performed using, for example, a drill, a laser, plasma, or the like, depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined depending on the design of the printed wiring board.
[0147] Step (6) is a step of roughening the insulating layer. Usually, smears are also removed in this step (6). The procedure and conditions of the roughening treatment are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer of a printed wiring board can be adopted. For example, the insulating layer can be roughened by carrying out a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order.
[0148] The swelling liquid used in the roughening treatment is not particularly limited, but includes an alkaline solution, a surfactant solution, etc., and is preferably an alkaline solution, and more preferably a sodium hydroxide solution or a potassium hydroxide solution. Examples of commercially available swelling liquids include "Swelling Dip Securigans P" and "Swelling Dip Securigans SBU" manufactured by Atotech Japan. The swelling treatment using the swelling liquid is not particularly limited, but can be performed by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes, for example. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes.
[0149] The oxidizing agent used in the roughening treatment is not particularly limited, but examples thereof include an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 minutes to 30 minutes. The concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan.
[0150] The neutralizing solution used in the roughening treatment is preferably an acidic aqueous solution, and a commercially available product such as "Reduction Solution Securigant P" manufactured by Atotech Japan can be mentioned.
[0151] The treatment with the neutralizing solution can be carried out by immersing the surface that has been roughened with an oxidizing agent in a neutralizing solution at 30° C. to 80° C. for 5 to 30 minutes. From the viewpoint of workability, etc., a method in which the object that has been roughened with an oxidizing agent is immersed in a neutralizing solution at 40° C. to 70° C. for 5 to 20 minutes is preferred.
[0152] In one embodiment, the arithmetic mean roughness (Ra) of the insulating layer surface after the roughening treatment is not particularly limited, but is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, and may be, for example, 1 nm or more, 2 nm or more, etc. The root mean square roughness (Rq) of the insulating layer surface after the roughening treatment is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, and may be, for example, 1 nm or more, 2 nm or more, etc. The arithmetic mean roughness (Ra) and root mean square roughness (Rq) of the insulating layer surface can be measured using a non-contact surface roughness meter.
[0153] Step (7) is a step of forming a conductor layer, and the conductor layer is formed on the insulating layer. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among these, from the viewpoints of versatility in forming the conductor layer, cost, ease of patterning, and the like, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.
[0154] The conductor layer may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.
[0155] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.
[0156] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method, and from the viewpoint of ease of production, it is preferable to form the conductor layer by the semi-additive method. An example of forming the conductor layer by the semi-additive method will be described below.
[0157] First, a plating seed layer is formed on the surface of an insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.
[0158] The printed wiring board described above can be used in a semiconductor device including a printed wiring board.
[0159] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft). EXAMPLES
[0160] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Unless otherwise specified, the temperature and pressure conditions are room temperature (25°C) and normal pressure (1 atm), respectively.
[0161] <Synthesis Example 1: Synthesis of Elastomer A> In a reaction vessel, 69 g of bifunctional hydroxyl-terminated polybutadiene ("G-3000" manufactured by Nippon Soda Co., Ltd., number average molecular weight = 3000, hydroxyl group equivalent = 1800 g / eq.), 40 g of aromatic hydrocarbon mixed solvent ("IPZOL 150" manufactured by Idemitsu Petrochemical Co., Ltd.), and 0.005 g of dibutyltin laurate were placed and mixed to dissolve uniformly. When the mixture became uniform, the temperature was raised to 60°C, and 8 g of isophorone diisocyanate ("IPDI" manufactured by Evonik Degussa Japan Co., Ltd., isocyanate group equivalent = 113 g / eq.) was added while stirring, and the reaction was carried out for about 3 hours.
[0162] Next, 23 g of cresol novolac resin (DIC "KA-1160", hydroxyl equivalent = 117 g / eq.) and 60 g of ethyl diglycol acetate (Daicel) were added to the reaction mixture, and the mixture was heated to 150°C while stirring, and reacted for about 10 hours. The disappearance of the NCO peak at 2250 cm-1 was confirmed by FT-IR. The disappearance of the NCO peak was regarded as the end point of the reaction, and the reaction mixture was cooled to room temperature. The reaction mixture was then filtered through a 100-mesh filter cloth to obtain an elastomer having a butadiene structure and a phenolic hydroxyl group (phenolic hydroxyl group-containing butadiene resin: non-volatile component 50% by mass). The number average molecular weight of elastomer A was 5900, and the glass transition temperature was -7°C.
[0163] <Synthesis Example 2: Synthesis of Maleimide A> Maleimide A (n = 1.47, Mw / Mn = 1.81) represented by the following formula was synthesized in the same manner as in Synthesis Example 1 of the Japan Institute of Invention and Innovation Disclosure Technical Journal Publication No. 2020-500211, and a MEK solution of maleimide A (70% by mass of non-volatile components) was obtained.
[0164] [ka]
[0165] <Example 1> (1) Preparation of resin varnish Bisphenol A epoxy resin (Mitsubishi Chemical "828EL", epoxy equivalent approx. 180g / eq.) 3 parts, naphthylene ether epoxy resin (DIC "HP-6000L", epoxy equivalent approx. 213g / eq.) 4 parts, bixylenol epoxy resin (Mitsubishi Chemical "YX4000H", epoxy equivalent 190g / eq.) 3 parts, phenolic hardener (DIC "KA-1160", cresol novolac resin, hydroxyl equivalent 117g / eq.) 3 parts, active ether A mixture of 11 parts of steric curing agent (DIC "HPC-8000-65T", active group equivalent 223 g / eq., toluene solution with solid content of 65% by mass), 1 part of carbodiimide curing agent (Nisshinbo Chemical "Carbodilite V-03", active group equivalent approximately 216 g / eq., toluene solution with solid content of 50% by mass), and spherical silica (Admatechs "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m) surface-treated with an aminosilane coupling agent (Shin-Etsu Chemical "KBM-573"). 2 A varnish-like resin composition was prepared by uniformly dispersing 50 parts of a methyl ketone (1:1 solution of MEK and cyclohexanone with a solid content of 30 mass %), 50 parts of a methyl ketone (1:1 solution of MEK and cyclohexanone with a solid content of 30 mass %), and 0.05 parts of a curing accelerator (4-dimethylaminopyridine, DMAP), in a high-speed rotating mixer.
[0166] (2) Preparation of resin sheet As the base film, a biaxially oriented polyethylene terephthalate (PET) film (Toray Industries, Inc., "Lumirror T6AM", thickness 38 μm) that had been subjected to release treatment with a non-silicone release agent (Lintec Corporation, "AL-5") was prepared. The varnish-like resin composition prepared in the above step (1) was applied to the release surface of the base film using a die coater, and dried at 80°C to 110°C (average 100°C) for 5 minutes to form a resin composition layer. The resin composition layer had a thickness of 70 μm. Next, a protective film was provided so as to be bonded to the resin composition layer. As the protective film, a biaxially oriented polypropylene (OPP) film (Oji F-Tex Co., Ltd., "HS413", thickness 15 μm) with rough surfaces on both sides was used. Then, it was cut to a width of 350 mm to obtain a resin sheet.
[0167] (3) Preparation of resin roll The resin sheet obtained in the above step (2) was wound around an ABS core (diameter 70 mm, width 350 mm) with the protective film facing inward to obtain a resin roll (winding length 20 m).
[0168] <Example 2> In step (2), a resin sheet having a resin composition layer width of 480 mm and a base film and protective film width of 500 mm (same as the resin sheet in Example 1 step (2) except for the width) was used as the resin sheet, and in step (3), the core width was changed from 350 mm to 500 mm. Except for this, a resin roll was obtained in the same manner as in Example 1.
[0169] <Example 3> In step (1), 0.05 parts of a curing accelerator (1-benzyl-2-phenylimidazole, "1B2PZ" manufactured by Shikoku Chemical Industry Co., Ltd.) was used instead of 0.05 parts of a curing accelerator (4-dimethylaminopyridine (DMAP)), and 1 part of a bismaleimide resin ("BMI-689" manufactured by Designer Molecules Inc.) was further added. A resin roll was obtained in the same manner as in Example 1.
[0170] <Example 4> In step (1), instead of 0.05 parts of the curing accelerator (4-dimethylaminopyridine (DMAP)), 0.05 parts of the curing accelerator (1-benzyl-2-phenylimidazole, Shikoku Chemical Industry Co., Ltd.'s "1B2PZ") were used, instead of 3 parts of the phenoxy resin (Mitsubishi Chemical Corporation's "YX7553BH30", solid content 30 mass%), 2 parts of the elastomer A (solid content 50 mass%) obtained in Synthesis Example 1 were used, and 1 part of the bismaleimide resin (Designer Molecules Inc.'s "BMI-689") was further added. Except for this, a resin roll was obtained in the same manner as in Example 1.
[0171] <Example 5> In step (1), instead of 0.05 parts of the curing accelerator (4-dimethylaminopyridine (DMAP)), 0.05 parts of the curing accelerator (1-benzyl-2-phenylimidazole, Shikoku Chemical Industry Co., Ltd. "1B2PZ") were used, instead of 3 parts of the phenoxy resin (Mitsubishi Chemical Corporation "YX7553BH30", solid content 30 mass%), 14 parts of the elastomer A (solid content 50 mass%) obtained in Synthesis Example 1 were used, 1 part of the maleimide compound (Designer Molecules Inc. "BMI-689") was further added, and the amount of surface-treated spherical silica (Admatechs Co., Ltd. "SO-C2") was changed from 50 parts to 80 parts, except that the resin roll was obtained in the same manner as in Example 1.
[0172] <Example 6> In step (1), instead of 0.05 parts of the curing accelerator (4-dimethylaminopyridine (DMAP)), 0.05 parts of a curing accelerator (1-benzyl-2-phenylimidazole, Shikoku Chemical Industry Co., Ltd.'s "1B2PZ") was used, 4 parts of a maleimide compound (Designer Molecules Inc.'s "BMI-689") was further added, and the amount of surface-treated spherical silica (Admatechs Co., Ltd.'s "SO-C2") used was changed from 50 parts to 60 parts. Except for this, a resin roll was obtained in the same manner as in Example 1.
[0173] <Example 7> In step (1), instead of 0.05 parts of the curing accelerator (4-dimethylaminopyridine (DMAP)), 0.05 parts of a curing accelerator (1-benzyl-2-phenylimidazole, Shikoku Chemical Industry Co., Ltd.'s "1B2PZ") were used, 2 parts of a biphenylaralkyl-type maleimide resin (Nippon Kayaku Co., Ltd.'s "MIR-3000-70MT", a MEK / toluene mixed solution with a solid content of 70%) was further added, and the amount of surface-treated spherical silica (Admatechs Co., Ltd.'s "SO-C2") used was changed from 50 parts to 52 parts. Except for this, a resin roll was obtained in the same manner as in Example 1.
[0174] <Example 8> In step (1), instead of 0.05 parts of the curing accelerator (4-dimethylaminopyridine (DMAP)), 0.05 parts of the curing accelerator (1-benzyl-2-phenylimidazole, Shikoku Chemical Industry Co., Ltd.'s "1B2PZ") were used, 2 parts of the maleimide A (solid content 70%) obtained in Synthesis Example 2 were further added, and the amount of surface-treated spherical silica (Admatechs Co., Ltd.'s "SO-C2") used was changed from 50 parts to 52 parts. Except for this, a resin roll was obtained in the same manner as in Example 1.
[0175] <Example 9> In step (1), instead of 0.05 parts of the curing accelerator (4-dimethylaminopyridine (DMAP)), 0.05 parts of a curing accelerator (1-benzyl-2-phenylimidazole, Shikoku Chemical Industry Co., Ltd.'s "1B2PZ") was used, 1 part of a bismaleimide resin (Designer Molecules Inc.'s "BMI1500") was further added, and the amount of surface-treated spherical silica (Admatechs Co., Ltd.'s "SO-C2") used was changed from 50 parts to 52 parts. Except for this, a resin roll was obtained in the same manner as in Example 1.
[0176] <Example 10> A resin roll was obtained in the same manner as in Example 1, except that in step (1), the amount of surface-treated spherical silica ("SO-C2" manufactured by Admatechs) was changed from 50 parts to 30 parts, and in step (3), the core width was changed from 350 mm to 380 mm.
[0177] <Example 11> A resin roll was obtained in the same manner as in Example 1, except that in step (1), 2 parts of the elastomer A (solid content 50% by mass) obtained in Synthesis Example 1 were used instead of 3 parts of the phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, solid content 30% by mass), and in step (2), a low-density polyethylene (PE) film ("GF-1" manufactured by Tamapoly Co., Ltd., thickness 25 μm) was used as the protective film instead of the biaxially oriented polypropylene (OPP) film ("HS413" manufactured by Oji F-Tex Co., Ltd., thickness 15 μm).
[0178] <Example 12> A resin roll was obtained in the same manner as in Example 1, except that in step (1), 2 parts of the elastomer A (solid content 50% by mass) obtained in Synthesis Example 1 were used instead of 3 parts of the phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, solid content 30% by mass), and in step (2), a biaxially oriented polypropylene (OPP) film ("HS413" manufactured by Oji F-Tex Co., Ltd., thickness 15 μm) was used as the protective film.
[0179] <Comparative Example 1> A resin roll was obtained in the same manner as in Example 1, except that in the step (3), the core width was changed from 350 mm to 400 mm.
[0180] <Comparative Example 2> A resin roll was obtained in the same manner as in Example 1, except that in step (1), the amount of surface-treated spherical silica ("SO-C2" manufactured by Admatechs) was changed from 50 parts to 5 parts, and in step (3), the core width was changed from 350 mm to 400 mm.
[0181] <Comparative Example 3> A resin roll was obtained in the same manner as in Example 1, except that in the step (1), the amount of surface-treated spherical silica ("SO-C2" manufactured by Admatechs Co., Ltd.) used was changed from 50 parts to 100 parts.
[0182] <Test Example 1: Measurement of weight loss rate of resin composition layer due to heat treatment> The resin sheet prepared in step (2) of the examples and comparative examples was cut into 10 cm x 10 cm pieces, which were placed in a desiccator together with thoroughly dried silica gel and left for 30 minutes. Thereafter, the mass (g) of the resin sheet was measured with the protective film peeled off, and the value was taken as α1 (g). Next, the resin sheet was heated in an oven at 130 ° C for 15 minutes, and after cooling in a desiccator together with silica gel for 30 minutes as before, the mass (g) of the resin sheet was measured again, and the value was taken as α2 (g). In addition, only the substrate film was cut into 10 cm x 10 cm pieces, which were left in a desiccator for 30 minutes, and the mass (g) of the substrate film was measured, and the value was taken as β (g). The value of the weight reduction rate A (mass%) of the resin composition layer when the resin sheet was heat-treated at 130 ° C for 15 minutes was calculated from the following formula (A).
[0183]
number
[0184] <Test Example 2: Measurement of density of resin sheet> The average density (g / cm) of the entire resin sheet produced in step (2) of the examples and comparative examples 3 ), and the density (g / cm ) of the core used in step (3) 3 ) were measured using a Mettler Toledo analytical balance XP105 (using a specific gravity measurement kit). The resin sheet was cut into 3 cm x 3 cm pieces, and the core was cut into 2 cm x 2 cm pieces. N=3 pieces were measured, and the average value was used.
[0185] <Test Example 3: Measurement of Elastic Modulus of Resin Composition Layer> The protective film and the substrate film were peeled off from the resin sheet produced in step (2) of the examples and comparative examples to obtain a resin composition layer. A tensile test was performed using a tensile tester "RTC-1250A" manufactured by Orientec Co., Ltd., and the elastic modulus of the resin composition layer at 23°C was measured. The measurement was performed five times, and the average value was calculated.
[0186] <Test Example 4: Evaluation of conveyance deviation> The resin rolls prepared in step (3) of the examples and comparative examples were placed in a resin sheet discharge device equipped with a fixing member for restricting the axial movement of the core and the entire resin sheet as shown in FIG. 2. The resin sheet was unwound from the resin roll of the resin sheet discharge device at a speed of 15 cm per second and placed on a conveying roll. The position of the end of the resin sheet in the conveying roll portion when it was placed on the conveying roll as shown in FIG. 2 was confirmed. When it had been unwound a further 10 m, the position of the end of the resin sheet in the conveying roll portion was confirmed and evaluated based on the following evaluation criteria.
[0187] Evaluation criteria "Good": The axial deviation of the position of the end of the resin sheet when it was first placed on the transport roll and when it was pulled out 10 m was less than 5 mm. "△": The axial deviation of the position of the end of the resin sheet when it was first applied to the conveying roll and then pulled out 10 m was 5 mm or more but less than 10 mm. "X": The axial deviation of the position of the end of the resin sheet when it was pulled out 10 m from the position of the end of the resin sheet in the transport roll when it was first placed on the transport roll was 10 mm or more.
[0188] <Test Example 5: Evaluation of susceptibility to scratches of resin composition layer> The resin rolls prepared in step (3) of the examples and comparative examples were placed in a resin sheet discharge device equipped with a fixing member for restricting the axial movement of the core and the entire resin sheet as shown in FIG. 2. The resin sheet was unwound from the resin roll of the resin sheet discharge device at a speed of 15 cm per second and placed on a conveying roll. When the resin sheet had been unwound by 10 m, the resin sheet in the conveying roll portion shown in FIG. 2 was observed with the naked eye and evaluated based on the following evaluation criteria.
[0189] Evaluation criteria "Good": No visible chipping occurred at the end of the resin composition layer of the resin sheet "X": When chipping occurred on the edge of the resin composition layer of the resin sheet
[0190] <Test Example 6: Measurement and Evaluation of Coefficient of Linear Thermal Expansion (CTE)> The resin sheet prepared in step (2) of the examples and comparative examples was heated at 200°C for 90 minutes to thermally cure the resin composition layer, and then the substrate film was peeled off to obtain a cured product for evaluation. The cured product for evaluation was cut into a test piece having a width of 5 mm and a length of 15 mm. The test piece was subjected to a thermomechanical analysis by a tensile load method using a thermomechanical analyzer ("Thermo Plus TMA8310" manufactured by Rigaku Corporation). In detail, the test piece was mounted on the thermomechanical analyzer, and then measured twice consecutively under the measurement conditions of a load of 1 g and a heating rate of 5°C / min (the first time was heated to 200°C, and the second time was heated to 260°C). In the second measurement, the linear thermal expansion coefficient (ppm / °C) in the planar direction in the range from 25°C to 150°C was calculated and evaluated based on the following evaluation criteria.
[0191] Evaluation criteria "Good": Coefficient of linear thermal expansion is 35 ppm / ℃ or less "△": When the linear thermal expansion coefficient is more than 35 ppm / ℃ and less than 50 ppm / ℃ "X": When the linear thermal expansion coefficient exceeds 50 ppm / °C, or when the cured product is brittle and cannot be measured (Comparative Example 3)
[0192] <Test Example 7: Measurement and evaluation of dielectric tangent (Df)> The resin sheet prepared in step (2) of the examples and comparative examples was heated at 200°C for 90 minutes to thermally cure the resin composition layer. The substrate film was then peeled off to obtain a cured product of the resin composition. This cured product was cut into a test piece having a width of 2 mm and a length of 80 mm. The dielectric loss tangent (Df) of the test piece was measured at a measurement frequency of 5.8 GHz and a measurement temperature of 23°C by a cavity resonance perturbation method using an "HP8362B" manufactured by Agilent Technologies. Measurements were performed on three test pieces.
[0193] Evaluation criteria "X": When the dielectric tangent exceeds 0.006, or when the cured product is brittle and cannot be measured (Comparative Example 3) "△": When the dielectric tangent is greater than 0.004 and less than or equal to 0.006 "Good": Dielectric tangent is 0.004 or less
[0194] Details of the resin rolls obtained in the examples and comparative examples, as well as the measurement results and evaluation results of the test examples, are summarized in Table 1 below.
[0195] [Table 1]
[0196] As shown in Table 1, a resin sheet having a base film, a thermosetting resin composition layer containing an inorganic filler provided on one side of the base film, and a protective film provided on the side of the thermosetting resin composition layer opposite to the base film, and a core around which the resin sheet is wound, the thermosetting resin composition layer further contains a volatile component, and when the protective film is peeled off and the side not in contact with the base film is exposed to the outside air, the weight loss rate of the thermosetting resin composition layer after heat treatment at 130°C for 15 minutes is 0.7 to 5 mass%, and the average density of the entire resin sheet is 1.3 g / cm 3 As described above, by using a resin roll in which the width of the resin sheet is 300 mm or more and the difference between the width of the core and the width of the resin sheet is 10% or less, it is possible to suppress both slippage during transport and damage to the resin composition layer, thereby achieving a good yield. [Explanation of symbols]
[0197] 10 Resin roll 11a Rolled resin sheet 11b Unrolled resin sheet 12 Core 20 Fixing member 21 axis branch 22 Shaft stop part 30 Transport roll 100 Resin sheet discharge device
Claims
1. A resin sheet including a base film, a thermosetting resin composition layer including an inorganic filler provided on one surface of the base film, and a protective film provided on a surface of the thermosetting resin composition layer opposite to the base film; A core around which the resin sheet is wound; Equipped with the thermosetting resin composition layer further contains a volatile component, and when the protective film is peeled off and the surface not in contact with the base film is exposed to the outside air, the weight loss rate of the thermosetting resin composition layer after heat treatment at 130°C for 15 minutes is 0.7 to 5 mass%, The average density of the entire resin sheet is 1.3 g / cm 3 That's all. The width of the resin sheet is 300 mm or more, The width of the core is W c The width of the resin sheet is W s And, W c / W s W 3 In this case, 0.9≦W 3 A resin roll having a viscosity of ≦1.
1.
2. 0.99<W 3 2. The resin roll according to claim 1, wherein the viscosity is ≦1.
1.
3. The resin roll according to claim 1 , wherein the thermosetting resin composition layer further comprises an epoxy resin.
4. The resin roll according to claim 1 , wherein the base film and the protective film are plastic films.
5. The resin roll according to claim 1, wherein the base film has a thickness of 5 μm to 75 μm, the thermosetting resin composition layer has a thickness of 5 μm to 250 μm, and the protective film has a thickness of 1 μm to 40 μm.
6. The width of the base film is W b and the width of the thermosetting resin composition layer is W r And, W b / W r W 1 In this case, 0.9≦W 1 ≦1.1, and the width of the protective film is W p And, W p / W r W 2 In this case, 0.9≦W 2 The resin roll according to claim 1, wherein the viscosity is ≦1.
1.
7. The resin roll according to claim 1, wherein the elastic modulus of the thermosetting resin composition layer is 1 GPa to 10 GPa when measured at 23°C.
8. The average density of the entire resin sheet is 1.8 g / cm 3 The resin roll according to claim 1 , wherein the thickness of the resin roll is less than 1 mm.
9. The resin roll according to claim 1 , wherein the core has a diameter of 50 mm or more.
10. The density of the core is 0.8 to 1.2 g / cm 3 The resin roll according to claim 1 .
11. The difference between the density of the core and the average density of the entire resin sheet is 0.3 to 2.0 g / cm 3 The resin roll according to claim 1 .
12. The resin roll according to claim 1 , wherein the resin sheet has a width of 1000 mm or less.
13. The resin roll according to claim 1 , wherein the resin sheet has a rolled-up length of 100 m or less.
14. The resin roll according to claim 1 , wherein the content of the inorganic filler in the thermosetting resin composition layer is 50% by mass or more, based on 100% by mass of all non-volatile components.
15. The resin roll according to claim 1 , wherein the content of the inorganic filler in the thermosetting resin composition layer is 80% by mass or less, based on 100% by mass of all non-volatile components.
16. The resin roll according to claim 1, wherein the thermosetting resin composition layer has a coefficient of linear thermal expansion (CTE) after curing of 50 ppm / °C or less in the range of 25°C to 150°C.
17. The resin roll according to claim 1, wherein the thermosetting resin composition layer has a dielectric loss tangent (Df) after curing of 0.006 or less when measured at 5.8 GHz and 23°C.
18. The resin roll according to claim 1 , wherein the thermosetting resin composition layer is a resin composition layer for forming an insulating layer of a printed wiring board.
19. A resin sheet discharge device including a resin roll and a fixing member, The resin roll is A resin sheet including a base film, a thermosetting resin composition layer including an inorganic filler provided on one surface of the base film, and a protective film provided on a surface of the thermosetting resin composition layer opposite to the base film; A core around which the resin sheet is wound; Equipped with the thermosetting resin composition layer further contains a volatile component, and when the protective film is peeled off and the surface not in contact with the base film is exposed to the outside air, the weight loss rate of the thermosetting resin composition layer after heat treatment at 130°C for 15 minutes is 0.7 to 5 mass%, The average density of the entire resin sheet is 1.3 g / cm 3 That's all. The width of the resin sheet is 300 mm or more, The width of the core is W c The width of the resin sheet is W s And, W c / W s W 3 In this case, 0.9≦W 3 ≦1.1, The fixing member is a support portion that supports the core core; and a planar shaft stop portion that is perpendicular to the axial direction and contacts both ends of a structure consisting of the core core and the resin sheet wound around the core core to limit the axial movement of the core core and the entire resin sheet wound around the core core. The resin sheet discharge device includes:
20. A resin sheet including a base film, a thermosetting resin composition layer including an inorganic filler provided on one surface of the base film, and a protective film provided on a surface of the thermosetting resin composition layer opposite to the base film; A core around which the resin sheet is wound; Equipped with the thermosetting resin composition layer further contains a volatile component, and when the protective film is peeled off and the surface not in contact with the base film is exposed to the outside air, the weight loss rate of the thermosetting resin composition layer after heat treatment at 130°C for 15 minutes is 0.7 to 5 mass%, The average density of the entire resin sheet is 1.3 g / cm 3 That's all. The width of the resin sheet is 300 mm or more, The width of the core is W c The width of the resin sheet is W s And, W c / W s W 3 In this case, 0.9≦W 3 A method for producing a printed wiring board, comprising the following steps (1) to (4), using a resin roll having a viscosity of ≦1.1: (1) A step of carrying out the resin sheet from the resin roll (2) Peeling off the protective film from the resin sheet (3) A step of laminating the resin sheet from which the protective film has been peeled off onto the inner layer substrate so that the thermosetting resin composition layer is bonded to the inner layer substrate. (4) A step of thermally curing the thermosetting resin composition layer to form an insulating layer.
Citation Information
Patent Citations
JP1976105992U
Laminate element having improved preservable stability
JP1988063032A
Photosensitive resin composition
JP2021039202A
Thermosetting resin composition, resin film for interlayer insulation, composite film, printed wiring board and method for producing the same
JP2019157027A
Resin material and multilayer printed wiring board
JP2020094213A