Aqueous secondary battery

Aqueous secondary batteries with a monoclinic MnO2-based electrode and potassium polyphosphate electrolyte enhance energy density and stability by facilitating ion insertion, addressing the limitations of cyanide-based compounds.

JP2024137744APending Publication Date: 2024-10-07TOYOTA JIDOSHA KK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024023835
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-23
Filing Date
2024-02-20
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Cyanide-based compounds used in aqueous secondary batteries can generate cyanide when malfunctioning and may not achieve sufficient energy density due to their large molecular structure.

Method used

Aqueous secondary batteries with a positive electrode active material having a monoclinic crystal structure (space group C2/m) and a composition formula of MnO2·A_xB_y(H2O)_z, where A is an alkali or alkaline earth metal, B is an anion, and the electrolyte contains potassium polyphosphate, which serves as a carrier ion, enhancing ion insertion and capacity.

Benefits of technology

The solution stabilizes the electrode structure, allowing easier insertion of carrier ions, thereby improving energy density and reducing the risk of electrolyte decomposition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137744000001
    Figure 2024137744000001
  • Figure 2024137744000002
    Figure 2024137744000002
  • Figure 2024137744000003
    Figure 2024137744000003
Patent Text Reader

Abstract

To provide a novel aqueous secondary battery.SOLUTION: An aqueous secondary battery of the present disclosure has a positive electrode active material layer, an aqueous electrolyte solution, and a negative electrode active material layer. The aqueous electrolyte solution contains an aqueous solvent, and potassium polyphosphate whose P element is 2 or more. In the aqueous electrolyte solution, any of a potassium ion, a proton, a hydroxide ion, and an anion polyphosphate serves as a carrier ion. A positive electrode active material contained in the positive electrode active material layer has a monoclinic crystal structure expressed by a space group C2 / m, and is expressed by a composition formula MnO2-AxBy(H2O)z. The A, the B, and the H2O exist in a space held between layers formed of Mn-O octahedrons. The A is an alkali metal or an alkaline earth metal, the B is an anion, and 0<x<1, 0<y<1, and 0<z<2 are satisfied.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to aqueous secondary batteries. [Background technology]

[0002] A non-aqueous battery containing a flammable non-aqueous electrolyte solution has a problem that the number of components required for safety measures is large, resulting in a low energy density per volume of the entire battery. On the other hand, an aqueous secondary battery containing a non-flammable aqueous electrolyte solution does not require the above-mentioned safety measures, and therefore has various advantages, such as a high energy density per volume. Therefore, various aqueous secondary batteries have been considered.

[0003] As an active material for aqueous secondary batteries, a cyan-based compound called Prussian blue has been proposed. For example, Non-Patent Document 1 discloses Fe-substituted Mn-rich Prussian blue K x Fe y Mn 1-y [Fe(CN)6] w A water-based secondary battery consisting of a positive electrode of zH2O is disclosed.

[0004] Patent Document 1 discloses an aqueous electrolyte solution for use in an aqueous secondary battery, the aqueous electrolyte solution containing water and potassium pyrophosphate dissolved at a concentration of 2 mol or more per kg of the water, and an aqueous secondary battery including the aqueous electrolyte solution. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-220294 A [Non-patent literature]

[0006] [Non-Patent Document 1] Nature Energy,(2019).4.495-503 Summary of the Invention [Problem to be solved by the invention]

[0007] The cyanide-based compound disclosed in Non-Patent Document 1 may generate cyanide when the battery malfunctions, and may not have sufficient energy density due to its large molecular structure.

[0008] An object of the present disclosure is to provide a novel aqueous secondary battery. [Means for solving the problem]

[0009] As a result of intensive research, the present inventors have found that the above problems can be solved by the following means, and have completed the present disclosure. That is, the present disclosure is as follows: <Aspect 1> A positive electrode active material layer, an aqueous electrolyte, and a negative electrode active material layer, the aqueous electrolyte solution contains an aqueous solvent and potassium polyphosphate having two or more P elements, and in the aqueous electrolyte solution, any one of potassium ions, protons, hydroxide ions, and polyphosphate anions serves as a carrier ion; The positive electrode active material contained in the positive electrode active material layer has a monoclinic crystal structure represented by the space group C2 / m and has the composition formula MnO2·A x B y (H2O) z wherein A, B, and HO are present in a space sandwiched between layers of Mn-O octahedrons, A is an alkali metal or an alkaline earth metal, B is an anion, 0 <x<1であり、 0 <y<1であり、かつ 0 <z<2である、 Water-based secondary battery. Aspect 2: The water based secondary battery according to aspect 1, wherein A contains at least Na and / or Ba. <Aspect 3> The B is at least Cl - 3. The water based secondary battery of claim 1 or 2, comprising: Aspect 4: The water based secondary battery according to any one of aspects 1 to 3, wherein the potassium polyphosphate having two or more P elements is K4P2O7. Aspect 5: The water-based secondary battery according to aspect 4, wherein the K4P2O7 is dissolved in a concentration of 2 mol or more per kg of water. Aspect 6: The water-based secondary battery according to any one of Aspects 1 to 5, wherein the aqueous electrolyte has a pH of 3 or more and 13 or less. Effect of the Invention

[0010] According to the present disclosure, a novel aqueous secondary battery can be provided. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram of an aqueous secondary battery according to one embodiment of the present disclosure. [Diagram 2] FIG. 2 is an XRD chart of the positive electrode active material of Example 1. [Diagram 3] FIG. 3 shows charge / discharge curves of a cell using the positive electrode active material of Example 1. [Figure 4] FIG. 4 is an XRD chart of the positive electrode active material of Example 2. [Diagram 5] FIG. 5 shows charge / discharge curves of a cell using the positive electrode active material of Example 2. [Figure 6] FIG. 6 is a graph showing the relationship between potassium pyrophosphate concentration and ionic conductivity. [Figure 7] FIG. 7 is a graph showing the relationship between potassium pyrophosphate concentration and pH. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] 《Water-based secondary battery》 The aqueous secondary battery of the present disclosure is A positive electrode active material layer, an aqueous electrolyte, and a negative electrode active material layer, the aqueous electrolyte solution contains an aqueous solvent and potassium polyphosphate having two or more P elements, and in the aqueous electrolyte solution, any one of potassium ions, protons, hydroxide ions, and polyphosphate anions serves as a carrier ion; The positive electrode active material contained in the positive electrode active material layer has a monoclinic crystal structure represented by the space group C2 / m and has the composition formula MnO2·A x B y (H2O) z wherein A, B, and HO are present in a space sandwiched between layers of Mn-O octahedrons, A is an alkali metal or an alkaline earth metal, B is an anion, 0 <x<1であり、 0 <y<1であり、かつ 0 <z<2である。

[0013] The present inventors have found that the positive electrode active material having the above-mentioned structure can exhibit charge / discharge behavior in a water-based potassium polyphosphate aqueous solution. Although not wishing to be bound by theory, it is believed that the structure is stabilized and the space is expanded by inserting cations such as Na and Ba, anions such as Cl, and water molecules into the space sandwiched between the layers composed of Mn-O octahedra in the monoclinic manganese oxide structure, which makes it easier for potassium ions, protons, hydroxide ions, and polyphosphate anions in the potassium polyphosphate aqueous solution to enter this space, thereby obtaining a large capacity.

[0014] Any one of the potassium ions, protons, hydroxide ions, and polyphosphate anions serves as a carrier ion in the aqueous electrolyte.

[0015] The aqueous secondary battery may have, for example, an electrolyte layer between the positive electrode and the negative electrode. The electrolyte layer may be composed of a separator and the above-mentioned aqueous electrolyte solution. As the separator, a separator known to be used in a secondary battery (e.g., nickel-metal hydride battery, zinc-air battery, etc.) may be adopted. For example, the separator may be a nonwoven fabric made of cellulose, a glass filter, etc. The thickness of the separator is not particularly limited, and may be, for example, 5 μm or more and 1 mm or less.

[0016] Each component of the aqueous secondary battery of the present disclosure will be described below.

[0017] FIG. 1 is a schematic diagram showing the configuration of a water-based secondary battery 100 according to a first embodiment of the present disclosure. As shown in FIG. 1, the water-based secondary battery 100 may include a positive electrode 10, a separator 20, and a negative electrode 30. The positive electrode 10 may include a positive electrode active material layer 11 and a positive electrode current collector 12, and the negative electrode 30 may include a negative electrode active material layer 31 and a negative electrode current collector 32. In this case, the positive electrode active material layer 11 may contain the above positive electrode active material. Although not shown, the above aqueous electrolyte may be contained in the positive electrode active material layer 11 and the negative electrode active material layer 31.

[0018] <Positive electrode current collector layer> The positive electrode current collector layer may be made of a known metal that can be used as a positive electrode current collector for a secondary battery. Examples of such metals include metal materials containing at least one element selected from the group consisting of Cu, Ni, Al, V, Au, Pt, Mg, Fe, Ti, Pb, Co, Cr, Zn, Ge, In, Sn, and Zr. The form of the positive electrode current collector is not particularly limited. It may take various forms such as a foil, a mesh, or a porous form. The above metal may be vapor-deposited or plated on the surface of a substrate.

[0019] <Cathode active material layer> The positive electrode active material layer contains the positive electrode active material described above. The positive electrode active material layer may further contain an optional conductive assistant, binder, etc. The thickness of the positive electrode active material layer is not particularly limited, but may be, for example, 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0020] (Cathode active material) The positive electrode active material has a monoclinic crystal structure represented by the space group C2 / m and has the composition formula MnO2·A x B y (H2O) z The A, B and H2O exist in the space between the layers of Mn-O octahedrons.

[0021] Here, the "monoclinic crystal structure represented by the space group C2 / m" means a crystal structure in which a base-centered crystal lattice having a two-fold axis and a mirror plane is used as a unit cell. In the above crystal structure, manganese dioxide having a structure in which A, B, and H2O exist in the spaces between layers of Mn-O octahedra is also called birnessite-type manganese dioxide.

[0022] A is an alkali metal such as Li, Na, or K, or an alkaline earth metal such as Be, Mg, Ca, Sr, or Ba. In particular, it is preferable that A contains at least Na and / or Ba, and is particularly preferably composed of Na and / or Ba, from the viewpoint of battery characteristics.

[0023] B is OH - , O 2- , C.N. - , Cl - Among them, B is at least Cl - In particular, Cl - From the viewpoint of battery characteristics, it is preferable that the above-mentioned formula be used.

[0024] The value of x in the above composition formula, i.e., the composition ratio of A to Mn, may be greater than 0, 0.1 or more, or 0.2 or more, and may be 1.0 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, or 0.3 or less. When multiple substances are present as A, the above value of x may be the sum of the composition ratios of each of these substances.

[0025] The value of y in the above composition formula, i.e., the composition ratio of B to Mn, may be greater than 0 or greater than 0.01, and may be less than 1, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, 0.20 or less, 0.10 or less, 0.08 or less, 0.06 or less, 0.05 or less, 0.04 or less, 0.03 or less, or 0.02 or less. When multiple substances are present as B, the above value of y may be the sum of the composition ratios of each of these substances.

[0026] The value of z in the above composition formula, i.e., the composition ratio of HO to Mn, may be greater than 0, 0.1 or more, or 0.2 or more, and may be 2.0 or less, 1.7 or less, 1.5 or less, 1.3 or less, 1.1 or less, 1.0 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, or 0.3 or less.

[0027] The above positive electrode active material can be produced, for example, by the following method. 1. Mn 2+ An aqueous solution of the source, e.g., MnCl2 and optional alkali metal and / or alkali metal salt, is obtained and deoxygenated at low temperature. 2. To the above deoxygenated aqueous solution, an alkali metal or alkaline earth metal hydroxide, such as NaOH, is added and mixed to obtain a milky white slurry. 3. Oxygen is fed into the slurry, causing the slurry to turn black through an oxidation reaction. 4. The blackened slurry is filtered and washed with water, and the resulting precipitate is dried.

[0028] The content of the positive electrode active material is not particularly limited, and may be, for example, 20 mass% or more, 30 mass% or more, 40 mass% or more, 50 mass% or more, 60 mass% or more, or 70 mass% or more, relative to the mass of the positive electrode active material layer, and may be 99 mass% or less, 97 mass% or less, 95 mass% or less, 92 mass% or less, 90 mass% or less, 88 mass% or less, 85 mass% or less, 83 mass% or less, or 80 mass% or less.

[0029] (Conductive assistant) The conductive assistant optionally contained in the positive electrode active material layer can be any of those known as conductive assistants used in aqueous secondary batteries. For example, carbon materials can be used. Specifically, they include ketjen black (KB), vapor grown carbon fiber (VGCF), acetylene black (AB), carbon nanotubes (CNT), carbon nanofibers (CNF), carbon black, coke, graphite, etc. Alternatively, they may be metal materials that can withstand the environment during use of the battery. Only one type of conductive assistant may be used alone, or two or more types may be used in combination. The conductive assistant may be in various shapes, such as powder and fiber.

[0030] The amount of the conductive assistant contained in the positive electrode active material layer is not particularly limited, and may be, for example, 1 mass% or more, 3 mass% or more, 5 mass% or more, 7 mass% or more, 10 mass% or more, or 15 mass% or more, and may be 30 mass% or less, 28 mass% or less, or 25 mass% or less.

[0031] (binder) The binder optionally contained in the positive electrode active material layer may be any binder known to be used in aqueous secondary batteries. For example, styrene butadiene rubber (SBR)-based binders, carboxymethyl cellulose (CMC)-based binders, acrylonitrile butadiene rubber (ABR)-based binders, butadiene rubber (BR)-based binders, polyvinylidene fluoride (PVDF)-based binders, polytetrafluoroethylene (PTFE)-based binders, etc. Only one type of binder may be used alone, or two or more types may be used in combination.

[0032] The amount of binder contained in the positive electrode active material layer is not particularly limited and may be, for example, 1 mass % or more, 2 mass % or more, 3 mass % or more, or 4 mass % or more, and may be 20 mass % or less, 18 mass % or less, 15 mass % or less, 12 mass % or less, 10 mass % or less, or 7 mass % or less.

[0033] <Aqueous electrolyte> The aqueous electrolyte contains an aqueous solvent and potassium polyphosphate having two or more P elements. In the aqueous electrolyte, any one of potassium ions, protons, hydroxide ions, and polyphosphate anions serves as a carrier ion.

[0034] The pH of the aqueous electrolyte may be 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, or 10 or more, and may be 13 or less, 12 or less, or 11 or less.

[0035] (Water-based solvent) The aqueous solvent is a solvent containing water. The aqueous solvent may contain water as a main component. That is, based on the total amount of the aqueous solvent constituting the electrolytic solution (100 mol%), water may account for 50 mol% or more, 70 mol% or more, 90 mol% or more, or 95 mol% or more. The upper limit of the proportion of water in the aqueous solvent is not particularly limited, and the aqueous solvent may be 100 mol%, that is, the entire amount of the aqueous solvent may be water.

[0036] The aqueous solvent may consist of water alone, but may further contain other components, such as one or more organic solvents selected from ethers, carbonates, nitriles, alcohols, ketones, amines, amides, sulfur compounds, and hydrocarbons. The solvent other than water may account for 50 mol% or less, 30 mol% or less, 10 mol% or less, or 5 mol% or less based on the total amount of the aqueous solvent constituting the electrolyte (100 mol%).

[0037] (Potassium polyphosphate) Potassium polyphosphate is an electrolyte dissolved in an aqueous solvent. This potassium polyphosphate is a potassium polyphosphate with a P element of 2 or more.

[0038] Such potassium polyphosphate may be, for example, potassium pyrophosphate.

[0039] Here, in order for an electrolyte to be "dissolved" in an aqueous solvent, it is not necessary for the electrolyte to be completely ionized. For example, in the case of potassium polyphosphate, potassium polyphosphate does not have to be completely ionized into potassium ions and polyphosphate ions in the aqueous electrolyte. That is, if potassium polyphosphate is potassium pyrophosphate, "dissolved potassium pyrophosphate" in the aqueous electrolyte is K + , P2O7 4- , KP2O7 3- , K2P2O7 2- , K3P2O7 - Ions derived exclusively from the ionization of potassium pyrophosphate such as HP2O7 3- , H2P2O7 2- , H3P2O7 - , HKP2O7 2- , H2KP2O7 - , HK2P2O7 - The aqueous electrolyte may be present as ions derived from ionization such as those described above and interactions between water molecules, or as associations of these ions. In addition, in the aqueous electrolyte, the "dissolved potassium pyrophosphate" does not have to be derived from a salt of potassium and pyrophosphate (K4P2O7) (obtained by adding K4P2O7 to water). For example, the aqueous electrolyte may include an electrolyte in which a potassium ion source (KOH, CH3COOK, etc.) and a pyrophosphate ion source (H4P2O7, etc.) are separately added to water and dissolved therein, resulting in the formation of the above ions or associations in the water.

[0040] The concentration of potassium polyphosphate in the aqueous electrolyte is not particularly limited and may be appropriately selected depending on the intended performance of the battery.

[0041] In the aqueous electrolyte, potassium polyphosphate may be dissolved in water at a concentration of 2.0 mol or more, 3.0 mol or more, 4.0 mol or more, or 5.0 mol or more per 1.0 kg of water. Such a concentration is preferable from the viewpoint of expressing the characteristic of improving oxidation / reduction resistance peculiar to a concentrated aqueous solution system called water-in-salt.

[0042] According to the new findings of the present inventors, the higher the concentration of potassium polyphosphate in the aqueous electrolyte, the smaller the hysteresis of the positive electrode active material during charging and discharging, and the easier it is to obtain high performance as an aqueous secondary battery. In addition, the higher the concentration of potassium polyphosphate in the aqueous electrolyte, the lower the overvoltage, and the easier it is to develop a good charge and discharge plateau. Furthermore, it is considered that the higher the concentration of potassium polyphosphate in the aqueous electrolyte, the easier it is for polyphosphate ions and potassium ions to approach each other and form an association. Therefore, for example, it is considered that polyphosphate ions are easily moved to the negative electrode side by being dragged by potassium ions when charging an aqueous secondary battery. The polyphosphate ions that reach the negative electrode interact with each other at the high work function site on the surface of the negative electrode, and as a result, direct contact between the aqueous electrolyte and the high work function site on the surface of the negative electrode is suppressed, and electrolysis of the aqueous electrolyte is easily suppressed.

[0043] The concentration of "dissolved potassium polyphosphate" in the aqueous electrolyte can be determined as follows. For example, elements and ions contained in the aqueous electrolyte are determined by elemental analysis or ion analysis, and the potassium ion concentration and polyphosphate ion concentration in the aqueous electrolyte are determined, and the determined ion concentration is converted into the potassium polyphosphate concentration. Alternatively, the solvent is removed from the aqueous electrolyte, and the solid content is chemically analyzed and converted into the potassium polyphosphate concentration.

[0044] In the aqueous electrolyte, the entire amount of potassium ions contained in the electrolyte does not have to be calculated as "dissolved potassium polyphosphate". That is, the aqueous electrolyte may contain more potassium ions than the concentration that can be calculated as potassium polyphosphate. For example, when producing an aqueous electrolyte, if a potassium ion source other than the potassium polyphosphate source (e.g., KOH, CH3COOK, K3PO4, etc.) is added and dissolved in water together with the potassium polyphosphate source, the aqueous electrolyte will contain more potassium ions than the concentration that can be calculated as potassium polyphosphate.

[0045] The aqueous electrolyte may contain cations other than potassium ions. For example, alkali metal ions, alkaline earth metal ions, transition metal ions, etc. other than potassium ions may be contained. The aqueous electrolyte may also contain anions other than those bound to cations. For example, when the potassium polyphosphate is potassium pyrophosphate, as described above, such anions are P2O7 4- In addition, KP2O7 3- , K2P2O7 2- , K3P2O7 - , HP2O7 3- , H2P2O7 2- , H3P2O7 - , HKP2O7 2- , H2KP2O7 - , HK2P2O7 - The aqueous electrolyte may contain, for example, anions derived from other electrolytes, which will be described later.

[0046] Other electrolytes may be dissolved in the aqueous electrolyte solution of the present disclosure. For example, KPF6, KBF4, K2SO4, KNO3, CH3COOK, (CF3SO2)2NK, KCF3SO3, (FSO2)2NK, K2HPO4, KH2PO4, etc. may be dissolved. The other electrolytes may account for 50 mol% or less, 30 mol% or less, 10 mol% or less, 5 mol% or less, or 1 mol% or less based on the total amount of electrolytes dissolved in the electrolyte solution (100 mol%).

[0047] <Negative electrode current collector layer> The negative electrode current collector layer may be made of a known metal that can be used as a negative electrode current collector for an aqueous secondary battery. Examples of such metals include metal materials containing at least one element selected from the group consisting of Cu, Ni, Al, V, Au, Pt, Mg, Fe, Ti, Pb, Co, Cr, Zn, Ge, In, Sn, and Zr. In particular, when considering stability in an aqueous electrolyte, the negative electrode current collector may contain at least one element selected from the group consisting of Al, Ti, Pb, Zn, Sn, Mg, Zr, and In, may contain at least one element selected from the group consisting of Ti, Pb, Zn, Sn, Mg, Zr, and In, or may contain Ti. All of Al, Ti, Pb, Zn, Sn, Mg, Zr, and In have low work functions, and it is considered that even if they come into contact with an aqueous electrolyte, electrolysis of the aqueous electrolyte is unlikely to occur.

[0048] The form of the negative electrode current collector is not particularly limited. It may be in various forms such as foil, mesh, porous, etc. It may be a substrate having the above-mentioned metal plated or vapor-deposited on its surface.

[0049] The surface of the negative electrode current collector may be coated with a carbon material. That is, the negative electrode may further include a negative electrode current collector and a coating layer provided on the surface of the negative electrode current collector on which the aqueous electrolyte is disposed (between the negative electrode current collector and the negative electrode active material layer), and the coating layer may contain a carbon material. Examples of the carbon material include Ketjen Black (KB), vapor grown carbon fiber (VGCF), acetylene black (AB), carbon nanotubes (CNT), carbon nanofibers (CNF), carbon black, coke, graphite, etc.

[0050] The thickness of the coating layer is not particularly limited. The coating layer may be provided on the entire surface of the negative electrode current collector, or may be provided on only a part of the surface.

[0051] The coating layer may contain a binder for binding the carbon materials together and between the carbon materials and the negative electrode current collector.

[0052] When a coating layer containing a carbon material is provided on the surface of a negative electrode current collector, the withstand voltage of the reduction side of the aqueous electrolyte is likely to be improved. Since the edge portion of the carbon material has high reaction activity, it is considered that the adsorption and decomposition of anions, such as polyphosphate ions, contained in the aqueous electrolyte is likely to occur, and that the anions are likely to interact with each other. Therefore, when the above-mentioned aqueous electrolyte is used in a potassium ion secondary battery, the edge portion of the carbon material is inactivated, and the electrolysis of the aqueous electrolyte at the edge portion can be suppressed, and as a result, the reduction side potential window of the aqueous electrolyte is considered to be expanded.

[0053] <Negative electrode active material layer> The negative electrode active material layer includes a negative electrode active material. The negative electrode active material layer may include a conductive assistant and a binder in addition to the negative electrode active material. The thickness of the negative electrode active material layer is not particularly limited, but may be, for example, 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0054] The negative electrode active material contained in the negative electrode active material layer may be selected from active materials having a charge / discharge potential of carrier ions lower than that of the positive electrode active material, taking into consideration the potential window of the aqueous electrolyte. For example, potassium-transition metal complex oxide; titanium oxide; metal sulfides such as Mo6S8; elemental sulfur; KTi2(PO4)3; NASICON type compounds; WO3; hydrogen storage alloys; inorganic compounds having a crystal structure belonging to space group I23, etc. Here, the inorganic compound having a crystal structure belonging to space group I23 may be an inorganic compound containing element A, element M, and O, in which the element A is at least one of Bi and La, and the element M is at least one of Bi, Mn, Fe, Co, and Ni. Only one type of negative electrode active material may be used alone, or two or more types may be used in combination.

[0055] The shape of the negative electrode active material is not particularly limited, and may be, for example, particulate. In this case, the particle size is not particularly limited, and an appropriate size may be selected according to the design of the battery. The negative electrode active material may have a primary particle size of 1 nm or more, 5 nm or more, 10 nm or more, 50 nm or more, or 100 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, 30 μm or less, or 10 μm or less. In addition, the negative electrode active material may be formed by aggregation of primary particles. In this case, the particle size of the secondary particles is not particularly limited, and may be, for example, 100 nm or more, 500 nm or more, or 1 μm or more, and may be 1000 μm or less, 500 μm or less, 100 μm or less, 50 μm or less, 30 μm or less, or 20 μm or less.

[0056] The amount of the negative electrode active material contained in the negative electrode active material layer is not particularly limited. For example, the amount of the negative electrode active material may be 20 mass% or more, 40 mass% or more, 60 mass% or more, or 70 mass% or more, or 99 mass% or less, 97 mass% or less, or 95 mass% or less, based on the entire negative electrode active material layer (100 mass%).

[0057] The type of conductive assistant or binder optionally contained in the negative electrode active material layer is not particularly limited, and may be appropriately selected from, for example, those exemplified as the conductive assistant or binder optionally contained in the positive electrode active material layer. The amount of conductive assistant or binder contained in the negative electrode active material layer is not particularly limited, and the amount mentioned for the positive electrode active material layer may be referred to.

[0058] <Other configurations> In addition to the above-mentioned components, the aqueous secondary battery may also have obvious components for a battery, such as terminals and a battery case.

[0059] An aqueous secondary battery having the above configuration can be manufactured, for example, by forming a positive electrode active material layer on the surface of a positive electrode current collector by a dry or wet process to obtain a positive electrode, forming a negative electrode active material layer on the surface of a negative electrode current collector by a dry or wet process to obtain a negative electrode, disposing a separator between the positive electrode and the negative electrode, and impregnating them with an aqueous electrolyte solution. EXAMPLES

[0060] The present disclosure will be specifically described with reference to examples and comparative examples, but the present disclosure is not limited thereto.

[0061] <<Preparation of Positive Electrode Active Material>> Example 1 Ion-exchanged water was added to 19.8 g of manganese(II) chloride tetrahydrate to prepare 200 ml of a 0.5 mol / L manganese chloride aqueous solution. Ion-exchanged water was added to 109 g of a 50 w / w% aqueous sodium hydroxide solution to prepare 250 ml of a 5.5 mol / L aqueous sodium hydroxide solution.

[0062] The manganese chloride aqueous solution was transferred to a 1 L stirring vessel capable of gas flow, and further placed in a cooling bath to cool the temperature to 10°C or less, and Ar gas was bubbled in while stirring to expel the air from within the vessel. While maintaining the temperature and bubbling gas, the sodium hydroxide aqueous solution prepared above was added and mixed with a roller pump over a period of 15 minutes to produce a milky white slurry.

[0063] Thereafter, the gas pipe was reconnected to the air pump, and air was pumped in at 6 L / min. Bubbling was continued for more than 20 hours, turning the slurry black and promoting the oxidation reaction.

[0064] After the reaction was completed, the mixture was filtered using a Buchner funnel and washed with an aqueous AgNO3 solution until no white precipitate of AgCl was formed.

[0065] The obtained wet cake was thoroughly dried for one day in a hot air dryer at 80° C., and classified using a standard sieve with 38 μm openings to obtain an active material powder.

[0066] By XRD measurement, it was identified as MnO2 having a layered structure represented by the space group C2 / m. The XRD chart of the positive electrode active material of Example 1 is shown in FIG.

[0067] ICP measurement revealed that Na was present at a composition ratio of Na / Mn=0.27 and that Cl was present at 0.4 mass %.

[0068] Example 2 An active material powder of Example 2 was obtained in the same manner as in Example 1, except that 200 mL of a 0.5 mol / L manganese / barium chloride mixed aqueous solution obtained by adding 17.8 g of manganese(II) chloride tetrahydrate and 2.44 g of barium chloride dihydrate to ion-exchanged water was used instead of the 200 mL of the manganese chloride aqueous solution described above.

[0069] The XRD measurement identified the material as MnO2 having a layered structure represented by the space group C2 / m. The XRD chart of the positive electrode active material of Example 2 is shown in FIG.

[0070] ICP measurement revealed that Ba was present in a composition ratio of Ba / Mn=0.11, Na was present in a composition ratio of Na / Mn=0.09, and Cl was present at 0.5 mass %.

[0071] <<Preparation of the positive electrode>> About 75 parts by mass of the positive electrode active material powder of Example 1, about 20 parts by mass of acetylene black as a conductive assistant, and about 5 parts by mass of polyvinylidene fluoride (PVDF) as a binder were mixed to prepare a positive electrode active material mixture. Next, the positive electrode active material mixture was uniformly coated on the surface of Ni foil using a doctor blade, and dried to obtain a positive electrode for evaluation. That is, the positive electrode is a positive electrode in which a positive electrode active material layer containing a positive electrode active material and the like is formed on the surface of Ni foil as a positive electrode current collector. For Example 2, a positive electrode for evaluation was also prepared in the same manner.

[0072] <<Preparation of evaluation cell>> An evaluation cell having the following configuration was fabricated. Cell: VM4 (EC Frontier) Working electrode: Positive electrode coating film Counter electrode: Pt mesh Reference electrode:Ag / AgCl Electrolyte: 5.0 mol / kg potassium pyrophosphate (K4P2O7) aqueous solution

[0073] Cell evaluation The evaluation cell was charged and discharged under the following conditions to evaluate the charge and discharge characteristics. Charge / discharge current value: 0.2mA / cm 2 Cutoff voltage: -0.5~0.95V vs. Ag / AgCl Measurement temperature: 25℃

[0074] The charge / discharge curves of Examples 1 and 2 are shown in Figures 3 and 5, respectively.

[0075] Reference Examples 1 and 2 <Reference example 1> The relationship between the concentration of the potassium pyrophosphate aqueous solution and the ionic conductivity is shown in FIG.

[0076] When the potassium pyrophosphate concentration in the aqueous potassium pyrophosphate solution was in the range of more than 0 mol / kg to 8 mol / kg or less, the aqueous potassium pyrophosphate solution had ionic conductivity.

[0077] <Reference example 2> The relationship between the concentration and pH of the aqueous potassium pyrophosphate solution is shown in FIG.

[0078] When the potassium pyrophosphate concentration in the aqueous potassium pyrophosphate solution was more than 0 mol / kg and not more than 8 mol / kg, the pH of the aqueous potassium pyrophosphate solution was 10.0 to 12.0. [Explanation of symbols]

[0079] 10 positive electrode 11 Cathode active material layer 12 Positive electrode current collector 20 Separator 30 Negative electrode 31 Negative electrode active material layer 32 Negative electrode current collector 100 Aqueous secondary battery

Claims

1. A positive electrode active material layer, an aqueous electrolyte, and a negative electrode active material layer, the aqueous electrolyte solution contains an aqueous solvent and potassium polyphosphate having two or more P elements, and in the aqueous electrolyte solution, any one of potassium ions, protons, hydroxide ions, and polyphosphate anions serves as a carrier ion; The positive electrode active material contained in the positive electrode active material layer has a monoclinic crystal structure represented by the space group C2 / m and has the composition formula MnO 2 ・A x B y (H 2 O) z and A, B and H 2 O exists in the space between the layers of Mn-O octahedrons. A is an alkali metal or an alkaline earth metal, B is an anion, 0<x<1, 0<y<1, and 0<z<2; Water-based secondary battery.

2. The water-based secondary battery according to claim 1 , wherein A contains at least Na and / or Ba.

3. The B is at least Cl - The aqueous secondary battery according to claim 1 or 2, comprising:

4. The potassium polyphosphate having two or more P elements is 4 P 2 O 7 3. The aqueous secondary battery according to claim 1 or 2,

5. The above K 4 P 2 O 7 The aqueous secondary battery according to claim 4 , wherein the above is dissolved in a concentration of 2 mol or more per kg of water.

6. 3. The aqueous secondary battery according to claim 1, wherein the aqueous electrolyte has a pH of 3 or more and 13 or less.

Citation Information

Patent Citations

  • Sodium ion-based aqueous electrolyte electrochemical secondary energy storage device

    JP2011519122A

  • Aqueous electrolyte solution and aqueous potassium ion battery

    JP2019220294A

  • Bis(pyridinium)-naphthalene diimide redox ionic compounds as electrode active materials

    US20200028172A1

  • Layered electrode materials and methods for rechargeable zinc batteries

    US20200395606A1

  • Secondary cell and device including secondary cell

    WO2018221309A1