Recycled plastic material production method and recycled plastic material

The method adjusts resin and filler inputs to achieve desired density and strength in recycled plastics for specific uses, addressing the challenge of using recycled materials with varying specific gravities and enhancing their suitability for applications like pool floors.

JP2024137776AInactive Publication Date: 2024-10-07GIFU PLAST IND CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024032639
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-03-05
Publication Date
2024-10-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Recycled plastic materials used for specific applications, such as underwater pool floors, often contain varying materials with lower specific gravity than water, requiring different measures to ensure they do not float and meet strength requirements.

Method used

A manufacturing method that involves adjusting the input amounts of recycled resin materials and inorganic filler components to achieve a density range of 1.00g/cm³ to 1.30g/cm³, with Izod impact strength of 3.0 kJ/m² or more, by measuring and blending first and second resin materials from different recycling laws, and adding inorganic fillers as needed to meet specified physical properties.

Benefits of technology

Ensures the recycled plastic materials have the necessary density and strength for specific applications, such as pool floors, while promoting effective recycling and utilization of materials with improved physical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137776000001_ABST
    Figure 2024137776000001_ABST
Patent Text Reader

Abstract

To provide an excellent recycled plastic material production method that allows both availability expansion and environmental consideration in using recycled resin obtained from used plastic containers and packaging to which the Containers and Packaging Recycling Law is applied.SOLUTION: A first resin material 41 is obtained from used plastic containers and packaging to which the Containers and Packaging Recycling Law is applied. A second resin material 42 is obtained from any one of, or a mixture of at least two or more of, a second (home appliance) resin material 42A, a second (automobile) resin material 42B and a second (general) resin material 42C. An RP material is formed by melting, kneading and mixing after feeding the first resin material 41 and the second resin material 42 and, if necessary, also feeding an inorganic filler material 43. The RP material has a specific range in which an inorganic filler material 43 content from 10 wt.% to 43 wt.% inclusive and an Izod impact strength of 3.0 kJ / m2 or more are set.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a recycled plastic material for a specific use or purpose different from normal uses, and the recycled plastic material. [Background technology]

[0002] In the development of plastic materials, sometimes they are designed for specific or specific uses, which are different from "normal uses" that do not limit the use. For example, for the pool floor described in Patent Document 1, product development is required with the specific use in mind of use underwater. In the case of pool floors to be installed underwater, products are developed using materials with a specific gravity (density) greater than that of water, such as polyvinyl chloride resin or polycarbonate resin, so that the floor will not float underwater. Note that "specific gravity" is almost the same value as "density" in terms of physical properties, so in this application, "density" and "specific gravity" are treated as synonyms. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6431709 Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, in the development of products using plastic materials, it is desirable to use recycled materials rather than virgin materials. In particular, since the Container and Packaging Recycling Law (hereinafter referred to as the "Container and Packaging Recycling Law") was enacted, the use of recycled materials to which the Container and Packaging Recycling Law applies has been recommended. However, recycled materials to which the Container and Packaging Recycling Law applies may contain a variety of resins and other materials mixed in, and may contain many materials with a specific gravity lower than that of water. Therefore, when using recycled resins to which the Container and Packaging Recycling Law applies underwater (specific applications), such as on pool floors, various ingenuity is required that differs from the situation when using recycled materials for normal applications. The present invention has been made to solve the above-mentioned problems, and its object is to provide an excellent manufacturing method for recycled plastic materials and recycled plastic materials that can utilize recycled plastic materials to which the Containers and Packaging Recycling Law applies, even when the recycled plastic materials are used for specific uses or purposes that are different from normal uses. [Means for solving the problem]

[0005] In order to solve the above problems, the present invention has the following manufacturing method. That is, as a first means, the content of the inorganic filler is 10% by weight or more and 43% by weight or less, and the Izod impact strength is 3.0 kJ / m 2A manufacturing method for manufacturing recycled plastic materials that fall within the above-mentioned specific range, comprising a first measurement step of measuring the material properties of a first recycled resin material (which may contain an inorganic filler component, hereinafter referred to as the "first resin material") obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, and a second (home appliance recycling) resin material (which may contain an inorganic filler component, hereinafter referred to as the "second (home) resin material") obtained from used plastics to which the Home Appliance Recycling Law applies, or a second (automobile recycling) resin material (which may contain an inorganic filler component, hereinafter referred to as the "second (auto) resin material") obtained from used plastics to which the Automobile Recycling Law applies, or a second (first) resin material (which may contain an inorganic filler component, hereinafter referred to as the "first (auto) resin material") obtained from used plastics not subject to the application of the Container and Packaging Recycling Law and to which neither the Home Appliance Recycling Law nor the Automobile Recycling Law applies. The method includes a second measurement step for measuring material properties of a mixture of at least one of the second (home) resin material, the second (home) resin material, and the second (home) resin material (which may contain an inorganic filler component and will hereinafter be collectively referred to as the "second resin material"), a calculation step for calculating the input amount of the first resin material and the input amount of the second resin material based on the material properties of the first resin material and the second resin material measured in the first measurement step and the second measurement step, and an input amount calculation step for calculating the input amount of the inorganic filler material based on the calculated input amounts of the first resin material and the second resin material, so that the content of the inorganic filler material and the Izod impact strength relative to the entire recycled plastic material are within the specific ranges, based on the calculated input amounts of the first resin material and the second resin material.

[0006] As the second means, in the first means, when the inorganic filler component after melt-kneading of the recycled plastic material exceeds the upper limit of the specific range in the input amount calculation step, it is preferable to stop inputting new inorganic filler material.

[0007] As a third measure, in the first or second measure, when the material properties of the recycled plastic after molding are set within a specific range, a high or low priority application order is set, and it is preferable that the "high priority application" is set so that the polyethylene content is 30% by weight or less based on the total weight of the recycled plastic material, and that the "low priority application" includes at least an MFR of 2.0 g / 10 min or more.

[0008] As a fourth method, in any one of the first to third methods, when the polyethylene component amount of the first resin material is higher than the estimated polyethylene component value of the recycled plastic material after molding, it is preferable to provide an input amount adjustment step of reducing the input amount of the first resin material below a predetermined estimated input amount and increasing the input amounts of the second resin material and the inorganic filler material above the predetermined estimated input amounts.

[0009] The present invention, which is a product, also has the following means. That is, as means 5, a product having an inorganic filler content of 10% by weight or more and 43% by weight or less and an Izod impact strength of 3.0 kJ / m 2The recycled plastic materials falling within the above-mentioned specific range include a first recycled resin material (which may contain inorganic filler components, hereinafter referred to as the "first resin material") obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, a second (home appliance recycling) resin material (which may contain inorganic filler components, hereinafter referred to as the "second (home) resin material") obtained from used plastic to which the Home Appliance Recycling Law applies, and a second (automobile recycling) resin material (which may contain inorganic filler components, hereinafter referred to as the "second (auto) resin material") obtained from used plastic to which the Automobile Recycling Law applies, and the first recycled resin material (which may contain inorganic filler components, hereinafter referred to as the "first (home) resin material") obtained from used plastic to which the Automobile Recycling Law applies. The recycled plastic material contains a second (general recycled material) resin material (which may contain an inorganic filler component and is hereinafter referred to as the "second (first) resin material") obtained from used plastics to which the Cycle Law, the Home Appliance Recycling Law, and the Automobile Recycling Law do not apply, and a mixture of one or at least two or more of the second (home) resin material, the second (self) resin material, and the second (first) resin material (which may contain an inorganic filler component and is hereinafter collectively referred to as the "second resin material"), and the inorganic filler material, and is characterized in that the content and Izod impact strength of the inorganic filler material relative to the entire recycled plastic material are within the specified range.

[0010] As a sixth aspect of the fifth aspect, it is preferable that the first resin material and the second resin material contain at least polypropylene and polyethylene, and the polypropylene content of the second resin material is greater than the polypropylene content of the first resin material.

[0011] As a seventh aspect, in the fifth or sixth aspect, it is preferable that the first resin material and the second resin material contain at least polypropylene and polyethylene, and the polyethylene content of the first resin material is greater than the polyethylene content of the second resin material.

[0012] As an eighth measure, when the material properties of recycled plastics are set to a specific range, a high or low priority application order is set, and it is preferable that a "high priority application" is set so that the polyethylene content is 30% or less by weight relative to the total weight of the recycled plastic material, and that a "low priority application" includes at least an MFR of 2.0 g / 10 min or more. As a ninth aspect, the specific range is preferably a flexural modulus of 1100 MPa or more. As a tenth aspect, the ranges of the density, MFR, flexural modulus and Izod impact strength of the first resin material are as follows: the density is 0.90 to 0.98 g / cm 3 , the MFR is 1.0 to 10.0 g / 10 min, the flexural modulus is 400 to 1200 MPa, and the Izod impact strength is 3.0 to 20.0 kJ / m 2 It is preferable that: As an eleventh aspect, when the second resin material is made of a resin material derived from recycled home appliances, the ranges of density, MFR, flexural modulus, and Izod impact strength of the second resin material are as follows: the density is 0.91 to 0.97 g / cm 3 , the MFR is 10.0 to 35.0 g / 10 min, the flexural modulus is 1000 to 1600 MPa, and the Izod impact strength is 4.0 to 15.0 kJ / m 2 It is preferable that: As a twelfth aspect, when the second resin material is made of a resin material derived from automobile recycling, the density, MFR, flexural modulus, and Izod impact strength of the second resin material are in the ranges of 0.95 to 1.10 g / cm. 3 , the MFR is 15.0 to 40.0 g / 10 min, the flexural modulus is 1500 to 2500 MPa, and the Izod impact strength is 6.0 to 35.0 kJ / m 2 It is preferable that: As a thirteenth aspect, in the case where the second resin material is made of a recycled resin material derived from a general material, the density, MFR, flexural modulus, and Izod impact strength of the second resin material are in the ranges of 0.91 to 1.0 g / cm3 , the MFR is 3.0 to 30.0 g / 10 min, the flexural modulus is 900 to 1600 MPa, and the Izod impact strength is 4.0 to 25.0 kJ / m 2 It is preferable that: Effect of the Invention

[0013] According to the present invention, it is possible to provide an excellent method for producing a recycled plastic material and a recycled plastic material that can utilize recycled plastic materials to which the Containers and Packaging Recycling Law applies, even when the recycled plastic material is used for a specific purpose different from its normal use. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a front view of a pool floor formed using recycled plastic materials according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an explanatory diagram of an extruder that melts and kneads recycled plastic material to form the material according to the present embodiment. [Diagram 3] 4 is a graph showing the relationship between the polyethylene content and the weld strength in the embodiment. [Figure 4] 4 is a flowchart showing a manufacturing process in the embodiment. [Diagram 5] FIG. 4 is an explanatory diagram showing component values ​​and physical property values ​​of a resin material in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Next, an embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a front view of a pool floor formed using recycled plastic material (hereinafter, this material will be referred to as "RP material") of this embodiment. The pool floor 10 in Fig. 1 consists of a top plate 11 on which pool users (e.g., not tall children) stand, and a number of legs 20 that support this top plate 11 from below. Note that although a pool floor has been shown as an example of using RP material for a special use (special purpose) different from normal uses, other products may also be used. The material density of the RP material from which the pool floor is formed is 1.00 g / cm 3 Above 1.30g / cm 3 The following (specific range) is desirable, but the material density may be changed to a value outside the specific range depending on the purpose, application, etc. of the product.

[0016] The extrusion molding machine 37 shown in FIG. 1 can feed pellet material 42 (comprised of a first resin material 41, a second (home appliance recycling) resin material 42A, a second (automobile recycling) resin material 42B, a second (general material recycling) resin material 42C, or an inorganic filler material 43, etc., which will be described later) into its hopper 36, and the pellet material 42 is conveyed in a conveying section 38 equipped with an internal screw. The extrusion molding machine 37 can melt-knead and mold the fed pellet material 42 inside, and discharge the pellet material 42 from a discharge port 39 as new pellet material. For the melt-kneading method, a single-screw extruder, a twin-screw extruder, a kneader, a Banbury mixer, etc. can be used. In the pellet material 42 of this embodiment, a recycled resin material 41 (hereinafter, this recycled resin material 41 will be referred to as "first resin material 41") obtained from used plastic container packaging to which the Container Recycling Law applies is an essential component. In addition, as a component of the pellet material 42, a recycled resin material obtained from used plastic to which the Home Appliance Recycling Law applies (hereinafter, this recycled resin material will be referred to as "second (home appliance recycling) resin material 42A") can be included. In addition, as another component of the pellet material 42, a recycled resin material obtained from used plastic to which the Automobile Recycling Law applies (hereinafter, this recycled resin material will be referred to as "second (automobile recycling) resin material 42B") can be included.

[0017] Furthermore, as a component of the pellet material 42, recycled resin material obtained from general used RP materials to which none of the Containers and Packaging Recycling Law, the Home Appliance Recycling Law, and the Automobile Recycling Law apply (hereinafter, this recycled resin material will be referred to as "second (general material recycled) resin material 42C") can be included. As shown in FIG. 5, the first resin material 41, the second (home appliance recycling) resin material 42A, the second (automobile recycling) resin material 42B, and the second (general material recycling) resin material 42C contain a polypropylene (hereinafter referred to as "PP") component, a polyethylene (hereinafter referred to as "PE") component, an inorganic filler component, and other components (hereinafter referred to as "others"), and are characterized by bias in the amount of components, etc. depending on the origin of the product, etc., and variations in physical properties.

[0018] In addition, an inorganic filler material 43 can be added to the pellet material 42 as an optional component to improve rigidity or increase specific gravity (density). The first resin material 41, the second (home appliance recycling) resin material 42A, the second (automobile recycling) resin material 42B, and the second (general material recycling) resin material 42C contain an inorganic filler component, and have the effect of improving rigidity according to the amount of the component. If the desired rigidity is insufficient, additional inorganic filler material 43 can be added. The inorganic filler material 43 may be any known material that does not affect the properties of the plastic material and improves rigidity. Examples of inorganic filler materials include carbonates, sulfates, silicates, phosphates, borates, oxides, and hydrates of calcium, magnesium, titanium, aluminum, iron, zinc, etc., or powders of these hydrates. Specific examples include calcium carbonate, magnesium carbonate, zinc oxide, titanium oxide, silica, alumina, clay, talc, kaolin, aluminum hydroxide, magnesium hydroxide, aluminum silicate, magnesium silicate, calcium silicate, aluminum sulfate, magnesium sulfate, calcium sulfate, magnesium phosphate, barium sulfate, silica sand, carbon black, zeolite, molybdenum, diatomaceous earth, sericite, shirasu, calcium sulfite, sodium sulfate, potassium titanate, bentonite, wollastonite, dolomite, graphite, etc. These may be contained alone or in combination of two or more kinds. The first resin material 41, the second (home appliance recycling) resin material 42A, the second (automobile recycling) resin material 42B, the second (general material recycling) resin material 42C (hereinafter, these may be collectively referred to as the second resin material 42) or the inorganic filler material 43 (a mixture of these) shown in Fig. 1 are illustrated in the form of pellets for ease of understanding, but this form is not necessarily limited to pellets. Also, the form of the resin material discharged from the discharge port 39 of the extrusion molding machine 37 may be pellets or may be other forms.

[0019] The inventors and researchers of the present application have studied the material properties, component analysis, market trends, and application fields of RP materials for many years. As a result, they have found that the presence of various resins in RP materials makes them susceptible to deterioration, deviation, bias, and variation in physical properties. They have also found that differences in the product origins of RP materials tend to cause specific trends in material properties and component analysis, which can be roughly categorized into the following (1) to (4). (1) A first resin material 41 obtained from used plastic containers and packaging to which the Containers and Packaging Recycling Law applies (in this case, the first resin material 41 (first recycled resin material) can be said to be a resin material derived from the Containers and Packaging Recycling Law). (2) A second (home appliance recycling) resin material 42A obtained from RP materials that are not subject to the Container Recycling Law but are subject to the Home Appliance Recycling Law (hereinafter, referred to as the second (home) resin material 42A, which can be said to be a resin material derived from the Home Appliance Recycling Law). (3) A second (automobile recycling) resin material 42B obtained from an RP material that is not subject to the application of the Containers and Packaging Recycling Law but is subject to the Automobile Recycling Law (hereinafter, referred to as the second (own) resin material 42B, which can be said to be a resin material derived from the Automobile Recycling Law). (4) A second (general recycled material) resin material 42C obtained from a general RP material to which none of the Container Recycling Law, the Home Appliance Recycling Law, and the Automobile Recycling Law applies (hereinafter, abbreviated as the second (first) resin material 42C, but unlike the second (home) resin material 42A and the second (self) resin material 42B, the second (first) resin material 42C can be said to be a resin material derived from a general material).

[0020] The official name of the Packaging Recycling Law is the Law Concerning Promotion of Separate Collection and Recycling of Containers and Packaging (the provisions and definitions of the Law will be cited as necessary). Specific targets include, for example, packaging film and food trays, but the items covered by the Law are limited. (R resin materials obtained from items covered by the Law are resin materials derived from packaging recycling materials and correspond to No. 1 Resin Material 41, but the content is subject to change in accordance with amendments to the Law, etc.) The official name of the Home Appliance Recycling Law is the Law Concerning the "Law Concerning the Recycling of Specified Household Appliances" (the provisions and definitions of the law will be cited as necessary). The items covered are four types of home appliances (air conditioners, televisions, refrigerators, freezers, washing machines, and clothes dryers), but the used plastics to which the law applies are limited to those discarded from ordinary households and offices. Therefore, even if the four types of home appliances are covered by the law, there are cases in which the law does not apply due to differences in the source of disposal. (R resin materials obtained from items covered by the law are resin materials derived from home appliance materials and correspond to Type 2 (household) resin materials 42A, but the content is subject to change in accordance with amendments to the Home Appliance Recycling Law, etc.) The official name of the Automobile Recycling Law is the "Law Concerning Recycling, etc. of End-of-Life Automobiles" (the provisions and definitions of the Law will be cited as necessary). The Law defines "automobiles," and the specific objects of the Law are limited to, for example, automobile bumpers and automobile interior materials. (The R resin material obtained from the objects covered by the Law is a resin material derived from automobile materials and corresponds to the second (auto) resin material 42B, but the content is subject to change in accordance with amendments to the Automobile Recycling Law, etc.) In addition, there are R resin materials obtained from general used RP materials to which the Container Recycling Law, Home Appliance Recycling Law, and Automobile Recycling Law do not apply. For example, there are (1) R resin materials obtained from RP materials of items other than the four types of home appliances to which the Home Appliance Recycling Law applies, and (2) resin materials obtained from RP materials of motorcycles, etc. to which the Automobile Recycling Law does not apply. (These R resin materials are resin materials derived from general materials and correspond to Section 2(1) Resin Material 42C, but their contents are subject to change in accordance with changes to the Container Recycling Law, Home Appliance Recycling Law, and Automobile Recycling Law, etc.) Due to such legal treatment, while the second (home) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C have similarities in their ingredients and material properties, there are differences in their ingredients and material properties due to the origin of the products related to the applicable laws, resulting in certain trends.

[0021] 5 shows Tables 1 to 4. Table 1 shows the component values ​​by weight % of PP, the component values ​​by weight % of PE, the component values ​​by weight % of inorganic filler, and the component values ​​by weight % of other components (hereinafter referred to as "others") for four sets of materials (material 1, material 2, material 3, and material 4) of the first resin material 41, and further shows four physical property values ​​(in this case, density, melt flow rate (hereinafter referred to as "MFR"), flexural modulus, and Izod impact strength). Tables 2 to 4, like Table 1, show the weight percent values ​​of the components (PP components, PE components, inorganic filler components, other components) of each material (material 1, material 2, material 3, material 4) for the second (home) resin material 42A, the second (self) resin material 42B, and the second (first) resin material 42C, as well as four physical property values ​​(in this case, density, MFR, flexural modulus, Izod impact strength). The indication of materials 1 to 4 for each resin material (41, 42A, 42B, 42C) may be four or less or more. In addition, the four physical properties to be measured may include other physical properties as necessary.

[0022] Next, a method for measuring the material properties of a resin material will be described. The melt flow rate (hereinafter, referred to as "MFR"), which represents one of the material properties of a resin material, can be measured using a Melt Indexer G-02 (manufactured by Toyo Seiki Seisakusho Co., Ltd.) by the MFR measurement method (JIS K7210, 230 degrees Celsius, load 2.16 kg). The flexural modulus, which represents one of the material properties of a resin material, can be measured using a Bentograph B-2 (manufactured by Toyo Seiki Seisakusho Co., Ltd.) by the bending property measurement method (JIS K7171). The Izod impact strength, which represents one of the material properties of a resin material, can be measured using an impact tester IT (manufactured by Toyo Seiki Seisakusho Co., Ltd.) by the Izod impact measurement method (JIS K7110). The material density, which represents one of the material properties of a resin material, can be measured using an electronic specific gravity meter SD-200L (manufactured by Alpha Mirage Co., Ltd.) by the density and specific gravity measurement method (JIS K7112). The MFR of the material 1 of the first resin material 41 shown in the table is 3.1 g / 10 min. The flexural modulus of the material 1 of the first resin material 41 is 666 MPa. The Izod impact strength of the material 1 of the first resin material 41 is 4.6 kJ / m 2The material density of the material 1 of the first resin material 41 is 0.96 g / cm 3 The component values ​​of PP, PE, other resins, and inorganic fillers that have been analyzed are listed in the columns of Material 2, Material 3, and Material 4 of the first resin material 41. For measuring PP, PE, and other resins in the resin material, an infrared spectrophotometer FT / IR-4X manufactured by JASCO Corporation can be used, and other devices may also be used. The amount of inorganic filler is measured using the amount of combustion residue. For example, an electric crucible furnace FUC030FB manufactured by Advantec Toyo Co., Ltd. can be used. These values ​​are listed in the columns of Tables 1 to 4 (Material 1, Material 2, Material 3, and Material 4) in FIG. 5.

[0023] Next, the resin materials shown in Tables 1 to 4 in Fig. 5 will be described. First, the first resin material 41 (materials 1 to 4) will be described. The first resin material 41 is characterized in that it has a large PE content and a small PP content, and also has a small content of other substances and inorganic filler. The densities of materials 1 to 4 are 0.94 to 0.97 g / cm 3 The MFR value is in the range of 3.0 to 3.8 g / 10 min, the flexural modulus is in the range of 666 to 937 MPa, and the Izod impact strength is in the range of 4.6 to 8.4 kJ / m 2 They are scattered within a range of about The first resin material 41 has a density of 0.90 to 0.98 g / cm 3 The range of 0.93 to 0.96 g / cm is the approximate practical range. 3 A suitable practical range for the MFR of the first resin material 41 is 1.0 to 10.0 g / 10 min from the viewpoint of moldability during injection molding, and a suitable practical range is 3.0 to 7.0 g / 10 min. A suitable practical range for the flexural modulus of the first resin material 41 is 400 to 1200 MPa from the viewpoint of the rigidity (strength) of the product, and a suitable practical range is 600 to 1100 MPa. A suitable practical range for the Izod impact strength of the first resin material 41 is 3.0 to 20.0 kJ / m from the viewpoint of the impact resistance (avoidance of cracking) of the product. 2The range is roughly practical, and further, 5.0 to 15.0 kJ / m 2 This range is a suitable practical range.

[0024] The second (house) resin material 42A (materials 1 to 4) shown in Table 2 of Fig. 5 is characterized in that the PP content is extremely large and the PE content is extremely small, and the other contents and inorganic filler contents are also small. The density of the second (house) resin material 42A is 0.91 to 0.92 g / cm 3 The MFR value is in the range of 25.4 to 28.7 g / 10 min, the flexural modulus is in the range of 1259 to 1370 MPa, and the Izod impact strength is in the range of 6.0 to 7.3 kJ / m 2 As a result, the second (house) resin material 42A (materials 1 to 4) has superior values ​​of MFR, flexural modulus, and Izod impact strength compared to the first resin material 41 (materials 1 to 4). The properties of the second resin material 42A alone are density of 0.91 to 0.97 g / cm 3 The range of 0.91 to 0.94 g / cm is the approximate practical range. 3 The preferred practical range for the MFR of the second (family) resin material 42A is 10.0 to 35.0 g / 10 min from the viewpoint of moldability during injection molding, and 15.0 to 30.0 g / 10 min is a more preferred practical range. The preferred practical range for the flexural modulus of the second (family) resin material 42A is 1000 to 1600 MPa from the viewpoint of product rigidity (strength), and 1100 to 1400 MPa is a more preferred practical range. The preferred practical range for the Izod impact strength of the second (family) resin material 42A is 4.0 to 15.0 kJ / m from the viewpoint of product impact resistance (avoidance of cracking). 2 The range is the approximate practical range, and further, 6.0 to 12.0 kJ / m 2 This range is a suitable practical range.

[0025] In addition, the second (own) resin material 42B (materials 1 to 4) shown in Table 3 of FIG. 5 is characterized by a large PP content and a small PE content, and is characterized by a large inorganic filler content compared to the first resin material 41, the second (home) resin material 42A, and the second (first) resin material 42C. Therefore, when using the second (own) resin material 42B (materials 1 to 4), since the second (own) resin material 42B (materials 1 to 4) itself contains a large amount of inorganic filler, there are cases where no additional inorganic filler material 43 is used. However, if the inorganic filler content of the second (own) resin material 42B (materials 1 to 4) itself is less than expected, a required amount of inorganic filler material 43 is added. The density of the second resin material 42B is 1.04 to 1.06 g / cm 3 The MFR value is in the range of 24.8 to 35.1 g / 10 min, the flexural modulus is in the range of 1906 to 2159 MPa, and the Izod impact strength is in the range of 17.5 to 24.6 kJ / m 2 As a result, the materials 1 to 4 of the second (own) resin material 42B are superior in MFR, flexural modulus, and Izod impact strength to the first resin material 41 (materials 1 to 4). The properties of the second (self) resin material 42B alone are density of 0.95 to 1.10 g / cm 3 is the approximate practical range, and 0.97 to 1.07 g / cm 3 A suitable practical range is 15.0 to 40.0 g / 10 min. from the viewpoint of moldability during injection molding, and a suitable practical range is 20.0 to 35.0 g / 10 min. Regarding the MFR of the second (self) resin material 42B, a rough practical range is 1500 to 2500 MPa from the viewpoint of the rigidity (strength) of the product, and a suitable practical range is 1800 to 2300 MPa. Regarding the Izod impact strength of the second (self) resin material 42B, a rough practical range is 1500 to 2500 MPa from the viewpoint of the impact resistance (avoidance of cracking) of the product, and a suitable practical range is 6.0 to 35.0 kJ / m 2 The range is the approximate practical range, and further, 10.0 to 30.0 kJ / m 2 This range is a suitable practical range. The second (first) resin material 42C (materials 1 to 4) shown in Table 4 of Fig. 5 is characterized in that the PP content is extremely large, the PE content is extremely small, and the other contents and inorganic filler content are also small. The density of the second (first) resin material 42C is 0.94 to 0.98 g / cm 3 The MFR is in the range of 9.6 to 14.0 g / 10 min, the flexural modulus is in the range of 1180 to 1324 MPa, and the Izod impact strength is in the range of 5.8 to 11.1 kJ / m 2 As a result, the second (first) resin material 42C (materials 1 to 4) has superior values ​​of MFR, flexural modulus, and Izod impact strength compared to the first resin material 41 (materials 1 to 4). The second (first) resin material 42C has a density of 0.91 to 1.0 g / cm 3 The range of 0.91 to 0.96 g / cm is the approximate practical range. 3 A suitable practical range for the MFR is 3.0 to 30.0 g / 10 min from the viewpoint of moldability during injection molding, and a suitable practical range is 4.0 to 25.0 g / 10 min. A suitable practical range for the flexural modulus of the second (first) resin material 42C is 900 to 1600 MPa from the viewpoint of the rigidity (strength) of the product, and a suitable practical range is 1100 to 1400 MPa. A suitable practical range for the Izod impact strength of the second (first) resin material 42C is 4.0 to 25.0 kJ / m from the viewpoint of the impact resistance (avoidance of cracking) of the product. 2 The range is roughly practical, and further, 5.0 to 15.0 kJ / m 2 This range is a suitable practical range.

[0026] In addition, when PP and PE components are mixed, the inventors of the present application have found that the following characteristics are obtained as a result of experiments. That is, FIG. 2 is a graph showing the relationship between the PE content ratio in an RP material (a resin material made of PP and PE) and the weld strength, with the vertical axis of FIG. 2 showing the weld strength (MPa) and the horizontal axis of FIG. 2 showing the PE content ratio. According to FIG. 2, the weld strength gradually decreases from a PE content ratio of 0% (in this case, the weld strength is 32.6 MPa) toward a PE content ratio of 50% (in this case, the weld strength is 19.0 MPa). In FIG. 2, the PE content ratio is 30% and the weld strength is about 23.0 MPa, and if the PE content ratio is in the range of 0% to 30% (preferably, in the range of 0% to 20%), it is understood that the weld strength is sufficiently maintained (i.e., the strength retention rate is 70% or more), and is a strength (allowable condition) that does not cause problems in commercialization. The weld strength was measured using a test piece of 150 x 100 x 4 mm with a weld formed in the center, under the conditions specified in JIS K7161.

[0027] The second (home) resin material 42A, second (self) resin material 42B, second (first) resin material 42C, etc. in this embodiment are resin materials mainly composed of PP (hereinafter may be referred to as "PP-mainly-component resin materials"), and when the PP-mainly-component resin material is mixed with the first resin material 41 (even if foreign matter other than PP and PE is mixed in, it can be generally ignored in terms of weld strength), it can be seen that the graph in Fig. 2 can be applied to the PE content ratio of the PP-mainly-component resin material and the first resin material 41. As a result, it can be seen that if the PE content ratio is in the range of 0 to 30%, the allowable range for the product strength of the RP material can be maintained. Next, the material properties (product properties) of products molded from RP materials will be explained using Figure 5. The material properties of the product are related to the specific ranges (amounts of components and material properties values ​​obtained by component analysis) of the RP material after melt kneading. In addition, the specific ranges of material properties can be divided into "high priority application" that is applied preferentially from the viewpoint of product usage, and "low priority application" (lower than "high" priority application). According to Table 1 below, "The amount of inorganic filler added after melt-kneading must be between 10% and 43% by weight" is "high priority application" and is important for ensuring the appropriate weight of the product. In addition, "The PE content must be 30% by weight or less" is also "high priority application". Similarly, "As the physical properties of the RP material after melt-kneading, the density must be 1.00 g / cm 3 Above 1.30g / cm 3 "Izod impact strength is 3.0 kJ / m or less" is "High priority application". 2 "Flexural modulus of elasticity is 1100 MPa or more," "MFR is 2.0 g / 10 min or more" are "low priority application." The reason why the material density is set to 1.0 or more is that it is desirable for the specific gravity to be greater than that of water so that the pool floor does not float in water. Also, the material density is set to 1.30 g / cm 3 The reason for setting the values ​​below is that the density of the resin material used in similar products is 1.35 g / cm 3 Since the density of the RP material is about the same as that of the product, it is made to be equivalent to the density of the product in order to reduce the weight (reducing the transportation cost, etc.) when transporting the finished product from the manufacturing factory to the installation site before installation and to improve convenience during construction. In this case, the conditions specified in "High priority application" are determined as the highest priority conditions in this embodiment. And, the contents specified in "Low priority application" are selected by selecting a method of appropriately setting the conditions according to the characteristics of the product within the above conditions, thereby ensuring flexibility when designing products using RP materials. Note that the high or low priority application is not uniform but may change depending on the product's usage environment and product characteristics, and in particular, the items related to "Low priority application" can be changed depending on the product's usage environment and product characteristics.

[0028] [Table 1]

[0029] Next, the manufacturing method of this embodiment will be described with reference to the flow chart shown in FIG. 3. In FIG. 3, the material properties of the product to be commercialized, which will be molded from the final RP material, are grasped in advance. First, the material properties of the product to be commercialized are grasped, and the material properties (density, MFR, flexural modulus, Izod impact strength) are grasped in addition to the component analysis (in this case, the component ratio of "PP component, PE component, other components, inorganic filler material") that constitutes the material properties. Hereinafter, this step will be referred to as product property grasping step S1, and abbreviated as "S1" in FIG. 3. Both the component analysis values ​​and the material property values ​​will be collectively referred to as product properties (material properties). Next, the components of the first resin material 41 are analyzed, and furthermore, the material physical properties are measured (Step S2). Hereinafter, this step is referred to as the component analysis / material physical property measurement step S2, and is abbreviated as "S2" in FIG. 3. In this case, the first resin material 41 is melt-kneaded, and in addition to the component analysis of the "PP component, PE component, other components, inorganic filler material" of the first resin material 41, the material physical properties "density, MFR, flexural modulus, Izod impact strength" are measured (Step S2). The material property measurement step of measuring the material properties in Step S2 corresponds to the "first measurement step" in the claims. Next, the results of the component analysis and material properties of the first resin material 41 are compared with the results of the component analysis and material properties grasped in the product characteristic grasping step S1 to verify (step S3). Hereinafter, such a comparison verification step is referred to as the comparison verification step S3, and is abbreviated as "S3" in FIG. 3. In step S4, the components of the second (household) resin material 42A are analyzed, and further the material properties are measured. Hereinafter, the step of measuring the component analysis values ​​and material properties of the second (household) resin material 42A is referred to as the component analysis and material property measurement step S4, and is abbreviated as "S4" in FIG. 3. In this case, the second (household) resin material 42A alone is melt-kneaded, and in addition to the component analysis of the "PP component, PE component, other components, inorganic filler material" of the second (household) resin material 42A after kneading, the material properties "density, MFR, flexural modulus, Izod impact strength" are measured. The material characteristic measuring step of measuring the material characteristic of the second (house) resin material 42A in step S4 corresponds to the "second measuring step" in the claims. If there is no plan to use the second (house) resin material 42A, it is not necessary to measure the material characteristic of the second (house) resin material 42A.

[0030] In step S5, the second (own) resin material 42B is subjected to component analysis and further to measurement of material property values. Hereinafter, the step of measuring the component analysis value and material property value of the second (own) resin material 42B is referred to as component analysis and material property measurement step S5, and is abbreviated as "S5" in FIG. 3. In this case, the second (own) resin material 42B alone is melted and kneaded, and in addition to the component analysis of "PP component, PE component, other components, inorganic filler material" of the second (own) resin material 42B after kneading, the material properties "density, MFR, flexural modulus, Izod impact strength" are measured. If there is no plan to use the second (own) resin material 42B, it is not necessary to measure the material properties of the second (own) resin material 42B. The material property measurement step of measuring the material properties of the second (own) resin material 42B in step S5 corresponds to the "second measurement step" in the claims. In step S6, the second (first) resin material 42C is subjected to component analysis and further to measurement of material property values. Hereinafter, the step of measuring the component analysis value and material property value of the second (first) resin material 42C is referred to as component analysis and material property measurement step S6, and is abbreviated as "S6" in FIG. 3. In this case, the second (first) resin material 42C alone is melted and kneaded, and in addition to the component analysis of "PP component, PE component, other components, inorganic filler material" of the kneaded second (first) resin material 42C, the material properties "density, MFR, flexural modulus, Izod impact strength" are measured. The material property measurement step of measuring the material property of the second (first) resin material 42C in step S6 corresponds to the "second measurement step" in the claims. Note that if there is no plan to use the second (first) resin material 42C, it is not necessary to measure the material property of the second (first) resin material 42C.

[0031] In step S7, based on the material properties of the first resin material 41 measured in step S2 and the material properties of the second (home) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C measured in steps S4 to S6, the input amount of the first resin material 41 and the input amount of any one of the second (home) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C (a mixture of two or more types, if necessary) are calculated. Hereinafter, the step of calculating the input amount is referred to as the input amount calculation step S7, and is abbreviated as "S7" in FIG. 3.) The input amount calculation step S7 corresponds to the "calculation step" in the claims. In addition, for a resin material obtained by melt-kneading and molding any one of the second (home) resin material 42A, the second (own) resin material 42B and the second (first) resin material 42C (a mixture of two or more types is also called a mixed second resin material, but these may be collectively referred to as the second resin material 42), whose input amount has been calculated, if the PE component amount of the first resin material 41, whose component analysis value and material property value have been measured in step S6, is higher than the assumed PE component value of the RP material, it is preferable to carry out a process of reducing the input amount of the first resin material 41 from a predetermined assumed input amount and increasing the input amount of the second resin material 42 from a predetermined assumed input amount. In step S8, both the first resin material 41, the amount of which was calculated in S7, and the mixed second resin material, the amount of which was calculated in S7, are added, and the first resin material 41 and the second resin material 42 (including the mixed second resin material) that are melt-kneaded and molded (hereinafter referred to as "molded first and second resin materials 45") are subjected to component analysis and further material property values ​​are measured (hereinafter this step is referred to as component analysis / material property measurement step S8, abbreviated as "S8" in FIG. 3). In this case, in addition to component analysis of "PP component, PE component, other components, inorganic filler material" of the first and second molded resin materials 45, the material properties "density, MFR, flexural modulus, Izod impact strength" are measured. If the inorganic filler component of the material properties after melt-kneading (molded first and second resin materials 45) falls within a specific range, additional addition of inorganic filler material 43 is not required.

[0032] In step S9, for the first and second molding resin materials 45, the amount of inorganic filler material 43 to be added is calculated so that the material properties after melt-kneading of the RP material are within the target (specific range) product properties (material properties) grasped in S1. Hereinafter, the step of calculating the amount of inorganic filler material 43 to be added is referred to as calculation step S9, and is abbreviated as "S9" in FIG. 3. If the inorganic filler component is within the specific range and exceeds the upper limit of the specific range, the addition of new inorganic filler material 43 is eliminated (stopped). The input amount calculation step S9 corresponds to the "input amount calculation step" in the claims. In step S10, the inorganic filler material 43 whose amounts were calculated in S9 and the first and second molding resin materials 45 whose amounts were calculated are added, and the inorganic filler material 43 and the first and second molding resin materials 45 are melt-kneaded and molded to produce a molded product (hereinafter referred to as the "final molded body 46"), and the material properties of the molded product are measured. (Hereinafter, the step of measuring the component analysis values ​​and material physical properties of the final molded body 46 is referred to as the component analysis / material physical property measurement step S10, and abbreviated as "S10" in FIG. 3. In this case, in addition to the component analysis of the "PP component, PE component, other components, and inorganic filler material" of the final molded body 46, the material properties of "density, MFR, flexural modulus, and Izod impact strength" are measured.) In step S11, the results of the component analysis and material properties of the final molded body 46 are compared with the results of the component analysis and material properties grasped in the product characteristic grasping step S1 to verify the results. Hereinafter, such a comparison verification step is referred to as the comparison verification step S11, and is abbreviated as "S11" in Fig. 3. If it is determined as a result of the comparison verification that the components of the material of the final molded body 46 are inappropriate, for example, a process of readjusting the amounts of the inorganic filler material 43 and the first and second molding resin materials 45 is performed. In step S11, if it is determined that the final molded body 46 that is melt-kneaded and molded can achieve the target product characteristics (material characteristics) identified in S1, the process proceeds to the next step S12. In step S12, the process proceeds to a manufacturing process in which products similar to the final molded body 46 are mass-produced.

[0033] The first resin material 41 shown in Table 1 is widely distributed in the market, but its flexural modulus is 1000 MPa or less, and does not reach the flexural modulus of 1100 MPa (see Table 1). Therefore, the quality of the recycled product using the RP material cannot be maintained by the first resin material 41 alone. On the other hand, the "density, MFR, flexural modulus, and Izod impact strength" shown by the second (family) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C (see Tables 2 to 4 in FIG. 4) are often at the levels shown in FIG. 5, and it can be seen that the second (family) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C can be used to manufacture lightweight recycled products. However, with regard to the distribution of second (household) resin material 42A, second (own) resin material 42B, and second (one) resin material 42C, the commercial relationships between the companies wishing to purchase RP materials and the sales companies have become deep, and if the distribution volume of second (household) resin material 42A, second (own) resin material 42B, and second (one) resin material 42C decreases, it will be difficult for companies wishing to purchase that do not have such commercial relationships to obtain the desired quantity of second (household) resin material 42A, second (own) resin material 42B, and second (one) resin material 42C from the market when desired.

[0034] Incidentally, the present inventors have derived from the experimental data and knowledge they have accumulated thus far, a component analysis of the first resin material 41 and the second resin material 42 and measurement of the material properties. As a result, it has been found that the amount of the second resin material 42 added relative to the first resin material 41 is adjusted to mix, melt and knead the molded first and second resin materials 45, etc., to have an increased PP component and a higher flexural modulus, and that the final molded body 46, etc. can be used for commercialization. As a result of component analysis and measurement of the material properties of the first resin material 41, the second (household) resin material 42A, the second (own) resin material 42B, and the second (one) resin material 42C, it is found that the first resin material 41, the second (household) resin material 42A, the second (own) resin material 42B, and the second (one) resin material 42C contain at least PP, PE, and inorganic filler components, and that the PP content of the second (household) resin material 42A, the second (own) resin material 42B, and the second (one) resin material 42C is greater than the PE content of the first resin material 41, and the PE content of the first resin material 41 is greater than the PE content of the second (household) resin material 42A, the second (own) resin material 42B, and the second (one) resin material 42C. In addition, when it is assumed that the amount of PE in the first resin material 41 is higher than the assumed amount of PE in the RP material after melt-kneading, it was found that a method of reducing the amount of the first resin material 41 from the assumed amount and increasing the amount of the second (home) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C mixed and added from the assumed amount is effective. As a result, although the first resin material 41 alone has a large distribution volume, its use applications are limited because its flexural modulus is 1000 MPa or less. However, by adopting a measure of mixing the second (home) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C with the first resin material 41 and appropriately setting the compounding ratio, the amount of PE components after melt-kneading is reduced while the amount of PP components is increased, and further, the values ​​of the flexural modulus and the like are increased, so that the use applications of the first resin material 41 are now in a promising situation. In other words, in the case of a manufacturing method in which the amounts of second (household) resin material 42A, second (own) resin material 42B, and second (first) resin material 42C added to the first resin material 41 are adjusted and melt-kneaded, it is found that the properties of the first resin material 41 can be improved and it can be used more effectively by adding the second (household) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C to the first resin material 41 in the compounding ratios shown in Examples 1 and 2 (described later), mixing them, and melt-kneading them.

[0035] Specific examples will be described below. Comparative Example 1 and Example 1 use material 2 of the first resin material 41 in Table 1 of Fig. 5, and use material 3 of the second (first) resin material 42C in Table 4 of Fig. 5. However, a material other than material 2 of the first resin material 41 in Table 1 of Fig. 5 may be used, and a material other than material 3 of the second (first) resin material 42C in Table 4 of Fig. 5 may be used. First, we disclose a manufacturing method for an RP material in which the compounding ratio is changed based on component detection of the first resin material 41 and the second (first) resin material 42C in a situation where inorganic filler 43, second (home) resin material 42A, and second (self) resin material 42B are not available in sufficient quantities and only the first resin material 41 and the second (first) resin material 42C are used.

[0036] TIFF2024137776000003.tif3073

[0037] In the above Comparative Example 1, the second resin material 42 obtained by melt-kneading the second (first) resin material 42C alone and the first resin material 41 are melt-kneaded to form the molded first and second resin materials 45, which become the final molded body 46. The components (ratios) and material properties of Comparative Example 1 are as described above. In Comparative Example 1, the PE component is 30.9% by weight (background colored), which does not satisfy the condition that the PE component is 30% by weight or less, which is the specific range. Similarly, the density is 0.98 g / cm 3 (With background color) indicates that the specific density range is 1.00 g / cm 3 Above 1.30g / cm 3 Similarly, since the inorganic filler 43 is 7.0% by weight (background color), the specific range of the condition "the amount of inorganic filler material added after melt kneading is 10% by weight or more and 43% by weight or less" is not satisfied. In order to solve this situation, measures are taken to change the ratio between the first resin material 41 and the second resin material 42 (adjusting the amounts of materials added, etc.). That is, in the case of Comparative Example 1, the mixture was 40% by weight of the first resin material 41, 55% by weight of the second resin material 42, and 5% by weight of the inorganic filler. In Example 1, the mixture is changed to 35% by weight of the first resin material 41, 56% by weight of the second resin material 42, and 9% by weight of the inorganic filler. This adjustment of the amounts of materials added is performed based on the results of component analysis and measurement of the material properties, with the premise derived from accumulated experimental data and knowledge. As a result, when the final molded body 46 was subjected to component analysis and measurement of the material properties, it was as shown in Example 1 below.

[0038] TIFF2024137776000004.tif3073

[0039] As a result, the PE component was 27.9% by weight, which satisfied the specific range condition of "PE component is 30% by weight or less". In addition, the inorganic filler 43 was 10.9% by weight, which satisfied the specific range condition of "the amount of inorganic filler material added after melt kneading is 10% by weight or more and 43% by weight or less". Similarly, the density was 1.00 g / cm 3 Therefore, the specific density range is 1.00 g / cm 3 Above 1.30g / cm3 The condition below is met. Also, since the MFR is 7.1g / 10min, it is understood that the specific range of "MFR is 3.0g / 10min or more" is met. Also, the Izod impact strength is 8.3kJ / m 2 Therefore, the Izod impact strength is 3.0 kJ / m 2 In addition, the inorganic filler is 10.9 g / cm or more. 3 Therefore, the specific range of "the inorganic filler is 10 to 43% by weight based on the total weight" is satisfied. From the results of Comparative Example 1 and Example 1, it can be seen that even in a situation where the second (home) resin material 42A and the second (self) resin material 42B are not available in sufficient quantities, by reducing the input amount of the first resin material 41 and increasing the input amount of the second (first) resin material 42C containing a large amount of PP components, the first resin material 41 can be effectively utilized. By taking this measure, the PE components after melt kneading are reduced while the PP components are increased, improving the rigidity and impact resistance of the RP material, and it can be seen that such a method of changing the compounding ratio is effective.

[0040] Next, a manufacturing method for an RP material is disclosed in which the compounding ratio is changed based on component detection of the first resin material 41, the second (first) resin material 42C and the inorganic filler 43 in a situation where sufficient amounts of the second (home) resin material 42A and the second (self) resin material 42B cannot be obtained and only the first resin material 41, the second (first) resin material 42C and the inorganic filler 43 are used.

[0041] TIFF2024137776000005.tif3076

[0042] In Comparative Example 2 and Example 2, the second (home) resin material 42A and the second (self) resin material 42B are not used, so the second resin material 42 is melt-kneaded with the second (first) resin material 42C alone, and the first resin material 41 and the inorganic filler 43 are melt-kneaded to form a molded final body 46 of the molded first and second resin materials 45. The components (ratios) of Comparative Example 2 are the first resin material 41 (45% by weight), the second resin material 42 (10% by weight) melt-kneaded with the second (first) resin material 42C, and the inorganic filler 43 (45% by weight). In Comparative Example 2, the inorganic filler 43 is 45.9% by weight (with background color), which does not satisfy the specific range of "the inorganic filler is 10 to 43% by weight or less with respect to the total weight". Similarly, the density is 1.33 g / cm 3 (With background color) indicates that the specific density range is 1.00 g / cm 3 Above 1.30g / cm 3 The Izod impact strength is 2.7 kJ / m or less. 2 (With colored background) "Izod impact strength is 3.0 kJ / m 2 In order to solve this condition, a measure (adjustment of input amount, etc.) is taken to change the ratio of the first resin material 41 and the second resin material 42. That is, in the case of Comparative Example 2, the mixture of the first resin material 41 (45% by weight), the second (first) resin material 42C (10% by weight), and the inorganic filler 43 (45% by weight) is changed to the mixture of the first resin material 41 (45% by weight), the second (first) resin material 42C (13% by weight), and the inorganic filler 43 (42% by weight) in Example 2 by changing and adjusting the input amount. This input amount adjustment is performed based on the results of component analysis and measurement of material properties, based on the premise derived from accumulated experimental data, knowledge, etc. When the final molded body 46 is component analyzed and the material properties are measured, the breakdown values ​​are as follows.

[0043] TIFF2024137776000006.tif3176

[0044] As a result, in Example 2, the inorganic filler 43 is 43.0% by weight, which satisfies the specific range condition of "the inorganic filler is 10 to 43% by weight relative to the total weight". Similarly, the Izod impact strength is 3.0 kJ / m 2 Therefore, the Izod impact strength is 3.0 kJ / m 2 The specific range of "flexural modulus is 1100 MPa or more" is met because the flexural modulus is 2646 MPa. The specific range of "flexural modulus is 1100 MPa or more" is met because the MFR is 2.8 g / 10 min., and the specific range of "MFR is 2.0 g / 10 min. or more" is met. Similarly, the density is 1.30 g / cm. 3 Therefore, "density is 1.00 g / cm 3 Above 1.30g / cm 3 The Izod impact strength is 3.0 kJ / m or less. 2 Therefore, the Izod impact strength is 3.0 kJ / m 2 Meets the specific range of "equal to or greater than." From the results of Comparative Example 2 and Example 2, it can be seen that even in a situation where the second (house) resin material 42A, the second (own) resin material 42B, and the second (first) resin material 42C are not available in sufficient amounts and only the first resin material 41, the second (first) resin material 42C, and the inorganic filler 43 are used, the first resin material 41 can be effectively utilized by reducing the amount of the first resin material 41 input and increasing the amount of the second (first) resin material 42C that contains a large amount of PP components. By taking this measure, the PE components after melt-kneading decreased while the PP components increased, and the values ​​of the flexural modulus and the like increased, so it can be seen that such a method of changing the compounding ratio is effective.

[0045] As described above in detail, the manufacturing method of the present embodiment includes the following components: 3 Above 1.30g / cm 3 The material performance is specified as density 1.00g / cm3 to be within the following range: 3 Above 1.30g / cm 3a first measurement step (S2) of measuring material performance of a first resin material 41 (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law is applied; a second measurement step (S4 to S6) of measuring material performance of a second resin material 42 (which may contain an inorganic filler component) obtained from used plastic mainly composed of polypropylene; a calculation step (S7) of calculating input amounts of the first resin material 41 and the second resin material 42 (which may contain an inorganic filler component) based on the material performances of the first resin material 41 and the second resin material 42 (which may contain an inorganic filler component) measured in the first measurement step and the second measurement step; and a calculation step (S8) of calculating input amounts of the first resin material 41 and the second resin material 42 (which may contain an inorganic filler component) based on the calculated input amounts of the first resin material 41 and the second resin material 42 (which may contain an inorganic filler component) after melt-kneading the recycled plastic material so that the material performance is within the specified range (density is 1.00 g / cm 3 Above 1.30g / cm 3 and an input amount calculation step (S9) for calculating the input amount of the inorganic filler material 43 so that the amount of the inorganic filler material 43 is calculated ... That is, while the second resin material 42 can be recycled by itself, the first resin material 41, which has a large inflow, is currently difficult to recycle by itself. Furthermore, among the second resin materials 42, the resin materials derived from the Automobile Recycling Law and the Home Appliance Recycling Law, in particular, are less in circulation than the first resin material 41. Furthermore, the business ties between the purchasing companies and the selling companies of RP materials are strong, making it difficult to obtain them from the distribution market and making it difficult to advance recycling. Under the current circumstances, however, by mixing an appropriate amount of the second resin material 42 with the first resin material 41 and melt-kneading it, the melt-kneaded resin material has physical properties superior to those of the first resin material 41, opening the way for recycling. Therefore, there is a high possibility that recycling will progress significantly for the first resin material 41, which has a large inflow. As recycling as a whole progresses, it can be said that the industrial effects will be extremely large.

[0046] The RP material of this embodiment contains the following components: 3 Above 1.30g / cm 3 The recycled plastic material is manufactured so that the specific range is that the density is 1.00 g / cm or less, and the recycled plastic material is obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law is applied, and the input amount is calculated based on the measured material performance. The recycled plastic material is a first resin material 41 (which may contain an inorganic filler component) obtained from used plastic mainly composed of polypropylene, and the input amount is calculated based on the measured material performance. The recycled plastic material is manufactured so that the specific range (density is 1.00 g / cm or less) is the specific range (density is 1.00 g / cm or less) based on the calculated input amounts of the first resin material 41 and the second resin material 42. 3 Above 1.30g / cm 3The inorganic filler material 43, the amount of which is calculated so as to be within the range below, and the first resin material 41, the second resin material 42, and the inorganic filler material 43, the amounts of which are calculated, are melted and kneaded to form the RP material. In the case of the RP material of this embodiment, the first resin material 41 alone has limited uses, whereas in the case of the final molded body 46 in which the second resin material 42 is mixed into the first resin material 41 and melted and kneaded, the values ​​of the flexural modulus and Izod impact strength increase, and the melted and kneaded resin material can be used in a wide range of applications, unlike the case of the first resin material 41 alone. As a result, the first resin material 41, which is widely distributed, can be used in an environmentally friendly manner, and the use of the RP material to which the Container Recycling Law is applied can be effectively promoted. In addition, according to the present embodiment, a method of adjusting the input amount is adopted in which the second resin material 42 is used to adjust the input amount relative to the first resin material 41. However, it is not necessary to adopt the input amount adjustment method, and a method of setting an appropriate mixing ratio from the beginning may be adopted. The second resin material 42 that is added to improve the physical properties of the first resin material 41 may be virgin material other than recycled material, or may be second (home) resin material 42A, second (own) resin material 42B, or second (first) resin material 42C that has not yet been released to the market.

[0047] The following supplementary notes are provided. Supplementary Note 1 is as follows: The material properties are as follows: Density is 1.00 g / cm 3 Above 1.30g / cm 3The manufacturing method for producing a recycled plastic material having a specific range of not more than 100% is characterized by comprising: a first measurement step (S2) for measuring the material performance of a first recycled resin material (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies; a second measurement step (S4 to S6) for measuring the material performance of a second recycled resin material (which may contain an inorganic filler component) obtained from used plastic mainly composed of polypropylene; a calculation step (S7) for calculating the input amounts of the first recycled resin material and the second recycled resin material (which may contain an inorganic filler component) based on the material performances of the first recycled resin material and the second recycled resin material (which may contain an inorganic filler component) measured in the first measurement step and the second measurement step; and an input amount calculation step (S9) for calculating the input amount of inorganic filler material based on the calculated input amounts of the first recycled resin material and the second recycled resin material (which may contain an inorganic filler component) so that the material performance of the recycled plastic material after melt-kneading is within the specific range. Supplementary Note 2 is as follows: That is, in the manufacturing method of the recycled plastic material described in Supplementary Note 1, in the input amount calculation step, when the inorganic filler component after melt-kneading of the recycled plastic material exceeds the upper limit of a specific range, the input of new inorganic filler material is eliminated. Supplementary Note 3 is as follows: That is, in the manufacturing method of the recycled plastic material described in Supplementary Note 1 or 2, when the material properties of the recycled plastic after molding are set to a specific range, a high or low priority application order is set, and the "high priority application" specifies that the polyethylene content is 30% by weight or less (15% by weight when the recycled plastic material is welded) relative to the total weight of the recycled plastic material, and the "low priority application" includes at least that the MFR is 3.0 g / 10 min or more. Supplementary Note 4 is as follows: That is, in the method for producing a recycled plastic material according to any one of Supplementary Note 1 to 3, the first and second recycled resin materials contain at least polypropylene and polyethylene, and the polypropylene content of the second recycled resin material is greater than the polypropylene content of the first recycled resin material, and the polyethylene content of the first recycled resin material is greater than the polyethylene content of the second recycled resin material. Supplementary Note 5 is as follows: That is, in the method for producing a recycled plastic material according to any one of Supplementary Note 1 to 4, when it is expected that the content of polyethylene in the first recycled resin material is higher than the expected content value of polyethylene in the recycled plastic material, the method is characterized by including an input amount adjustment step of reducing the input amount of the first recycled resin material below a predetermined expected input amount and increasing the input amount of the second recycled resin material above a predetermined expected input amount. Appendix 6 is as follows: The material properties are density 1.00g / cm 3 Above 1.30g / cm 3 The recycled plastic material is manufactured so that the specific range is below the specified range, and is characterized in that it comprises a first recycled resin material (which may contain an inorganic filler component) obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies, and whose input amount is calculated based on measured material performance; a second recycled resin material (which may contain an inorganic filler component) obtained from used plastic whose main component is polypropylene, and whose input amount is calculated based on measured material performance; and an inorganic filler material whose input amount is calculated based on the calculated input amounts of the first recycled resin material and the second recycled resin material so that the material performance after melt-kneading of the recycled plastic material falls within the specific range, and the first recycled resin material, the second recycled resin material, and the inorganic filler material whose input amounts are calculated are melt-kneaded together. Supplementary Note 7 is as follows: That is, in the recycled plastic material described in Supplementary Note 6, the polyethylene content in the molded recycled plastic material is adjusted and blended to be 30% by weight or less with respect to the total weight of the recycled plastic material. Supplementary Note 8 is as follows: That is, in the recycled plastic material described in Supplementary Note 6 and Supplementary Note 7, when the recycled plastic material is welded, the polyethylene content in the recycled plastic material after molding is adjusted and blended to be 15% by weight or less with respect to the total weight of the recycled plastic material. Supplementary Note 9 is as follows: That is, in the recycled plastic material described in any one of Supplementary Notes 6 to 8, the specific range of the material performance satisfies all of the following conditions (1) to (4). (1) Density (based on JIS standard K 7112) is 1.00 g / cm 3 The compressive strength (based on JIS standard K 7171) is 1100MPa or more, (2) MFR (based on JIS standard K 7210) is 2.0g / 10min or more, (3) Flexural modulus (in accordance with JIS standard K 7171) of 1100 MPa or more; (4) Izod impact strength (JIS standard K 7110 compliant) is 3.0 kJ / m 2 End [Explanation of symbols]

[0048] 41 First recycled resin material (first resin material) 42 PP main component resin material Secondary resin material 42A 2nd (house) resin material (derived from recycled home appliance materials) 42B Second (self) resin material (derived from recycled automobile materials) 42C 2nd (first) resin material (derived from general recycled materials) 43 Inorganic filler materials S2 First measurement step S4 to S6 Second measurement step S7 Calculation step S9 Input amount calculation step

Claims

1. The content of inorganic filler is 10% by weight or more and 43% by weight or less, and the Izod impact strength is 3.0 kJ / m 2 A manufacturing method for producing recycled plastic materials within the above specific range, A first measurement step of measuring material properties of a first recycled resin material (which may contain an inorganic filler component, hereinafter referred to as the "first resin material") obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies; a second measurement step of measuring material properties of a mixture of at least one of the second (household) resin material, the second (owner) resin material, and the second (first) resin material (which may contain an inorganic filler component, hereinafter collectively referred to as the "second (household) resin material"), which may be obtained from used plastic to which the Home Appliance Recycling Law applies, or the second (automobile recycling) resin material (which may contain an inorganic filler component, hereinafter collectively referred to as the "second (automobile) resin material") obtained from used plastic to which the Automobile Recycling Law applies, or the second (general recycling material) resin material (which may contain an inorganic filler component, hereinafter collectively referred to as the "second (first) resin material") obtained from used plastic to which neither the Container and Packaging Recycling Law applies nor the Automobile Recycling Law applies; a calculation step of calculating an input amount of the first resin material and an input amount of the second resin material based on material properties of the first resin material and the second resin material measured in the first measurement step and the second measurement step; and an input amount calculation step of calculating an input amount of the inorganic filler material based on the calculated input amounts of the first resin material and the second resin material, so that the content of the inorganic filler material and the Izod impact strength relative to the entire recycled plastic material are within the specific range.

2. 2. The method for producing recycled plastic material according to claim 1, characterized in that, in the input amount calculation step, if the inorganic filler component after melt-kneading of the recycled plastic material exceeds the upper limit of the specific range, the input of new inorganic filler material is stopped.

3. 3. The method for producing a recycled plastic material according to claim 1 or 2, characterized in that, when the material properties of the recycled plastic after molding are within a specific range, a high or low priority application order is set, where a "high priority application" specifies that the polyethylene content is 30% by weight or less based on the total weight of the recycled plastic material, and a "low priority application" includes at least an MFR of 2.0 g / 10 min or more.

4. A method for producing recycled plastic material as described in claim 1 or 2, characterized in that it includes an input amount adjustment step of reducing the input amount of the first resin material below a predetermined estimated input amount and increasing the input amounts of the second resin material and the inorganic filler material above the predetermined estimated input amounts when the polyethylene component amount of the first resin material is higher than the estimated polyethylene component value of the recycled plastic material after molding.

5. The content of inorganic filler is 10% by weight or more and 43% by weight or less, and the Izod impact strength is 3.0 kJ / m 2 A recycled plastic material that is within the above specific range, A first recycled resin material (which may contain an inorganic filler component, hereinafter referred to as the "first resin material") obtained from used plastic containers and packaging to which the Container and Packaging Recycling Law applies; A second (home appliance recycling) resin material (which may contain an inorganic filler component, hereinafter referred to as the "second (home) resin material") obtained from used plastics to which the Home Appliance Recycling Law applies, a second (automobile recycling) resin material (which may contain an inorganic filler component, hereinafter referred to as the "second (home) resin material") obtained from used plastics to which the Automobile Recycling Law applies, a second (general recycling material) resin material (which may contain an inorganic filler component, hereinafter referred to as the "second (first) resin material") obtained from used plastics to which none of the Container and Packaging Recycling Law, the Home Appliance Recycling Law, and the Automobile Recycling Law applies, and a mixture of at least one or two or more of the second (home) resin material, the second (first) resin material, and the second (first) resin material (which may contain an inorganic filler component, hereinafter collectively referred to as the "second resin material"); The inorganic filler material is contained, A recycled plastic material, characterized in that the content of inorganic filler material relative to the entire recycled plastic material and the Izod impact strength are within the above-mentioned specific ranges.

6. The recycled plastic material according to claim 5, characterized in that the first resin material and the second resin material contain at least polypropylene and polyethylene, and the polypropylene content of the second resin material is greater than the polypropylene content of the first resin material.

7. The recycled plastic material according to claim 5 or 6, characterized in that the first resin material and the second resin material contain at least polypropylene and polyethylene, and the polyethylene content of the first resin material is greater than the polyethylene content of the second resin material.

8. The recycled plastic material according to claim 6 or 7, characterized in that, when the material properties of the recycled plastic are within a specific range, a high or low priority application order is set, in which the "high priority application" specifies that the polyethylene content is 30% by weight or less based on the total weight of the recycled plastic material, and the "low priority application" includes at least an MFR of 2.0 g / 10 min or more.

9. The recycled plastic material according to claim 5 or 6, characterized in that the specific range is a flexural modulus of 1100 MPa or more.

10. The ranges of density, MFR, flexural modulus and Izod impact strength of the first resin material are as follows: density: 0.90 to 0.98 g / cm 3 , the MFR is 1.0 to 10.0 g / 10 min, the flexural modulus is 400 to 1200 MPa, and the Izod impact strength is 3.0 to 20.0 kJ / m 2 7. The recycled plastic material according to claim 5 or 6,

11. When the second resin material is made of the resin material derived from the home appliance recycling, the density, MFR, flexural modulus, and Izod impact strength of the second resin material are in the ranges of 0.91 to 0.97 g / cm 3 , the MFR is 10.0 to 35.0 g / 10 min, the flexural modulus is 1000 to 1600 MPa, and the Izod impact strength is 4.0 to 15.0 kJ / m 2 7. The recycled plastic material according to claim 5 or 6,

12. When the second resin material is made of the resin material derived from the automobile recycling, the density, MFR, flexural modulus, and Izod impact strength of the second resin material are in the ranges of 0.95 to 1.10 g / cm. 3, the MFR is 15.0 to 40.0 g / 10 min, the flexural modulus is 1500 to 2500 MPa, and the Izod impact strength is 6.0 to 35.0 kJ / m 2 7. The recycled plastic material according to claim 5 or 6,

13. When the second resin material is made of a recycled resin material derived from the general material, the density, MFR, flexural modulus, and Izod impact strength of the second resin material are in the ranges of 0.91 to 1.0 g / cm 3 , the MFR is 3.0 to 30.0 g / 10 min, the flexural modulus is 900 to 1600 MPa, and the Izod impact strength is 4.0 to 25.0 kJ / m 2 7. The recycled plastic material according to claim 5 or 6,

Citation Information

Patent Citations

  • Preparation of molding resin material

    JP1995233263A

  • Manufacture of instrument panel

    JP2000007792A

  • Polypropylene resin composition that is superiorly resistant to injury

    JP2002003692A

  • Method and apparatus for manufacture of recycle plastic panel

    JP2007112028A

  • Method for modifying waste composite resin composition

    JP2008184534A