Resin particle, toner, method for manufacturing resin particle, image forming apparatus, and image forming method
The design of resin particles with a crystalline polyester resin covering mold release agent domains addresses the challenges of low-temperature fixability and heat-resistant storage stability, enhancing toner performance and image quality by preventing agent leakage and maintaining strength.
Patent Information
- Application Number
- JP2024041023
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-22
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-07
AI Technical Summary
Existing toner technologies face challenges in achieving high low-temperature fixability and heat-resistant storage stability, with conventional methods leading to mechanical fragility, contamination, and reduced image quality due to mold release agent leakage and incompatibility with crystalline polyester resin.
Resin particles are designed with a crystalline polyester resin covering 80% or more of the mold release agent domains, each with a domain diameter of 1 μm or less, ensuring the melting point of the crystalline polyester resin exceeds that of the mold release agent, enhancing compatibility and confinement of the release agent within the toner.
The solution provides resin particles with improved low-temperature fixability and heat-resistant storage stability, maintaining toner strength and preventing mold release agent leakage, thereby ensuring stable image quality.
Smart Images

Figure 2024137815000005 
Figure 2024137815000006 
Figure 2024137815000007
Abstract
Description
[Technical field]
[0001] The present invention relates to resin particles, a toner, a method for producing resin particles, an image forming apparatus, and an image forming method. [Background technology]
[0002] In recent years, toners are required to have smaller particle size and high-temperature offset resistance for improving the quality of output images, low-temperature fixability for energy saving, and heat-resistant storage stability that can withstand high temperatures and high humidity during storage and transportation after production. In particular, since the power consumption during fixation accounts for a large portion of the power consumption in the image forming process, improving the low-temperature fixability is extremely important.
[0003] Conventionally, toners produced by the kneading and pulverizing method have been used, but the toners produced by the kneading and pulverizing method have problems such as difficulty in reducing the particle size, indefinite shape, and broad particle size distribution, resulting in insufficient quality of output images and high fixing energy.
[0004] In addition, when wax (releasing agent) is added to improve fixability, the toner produced by the kneading and pulverizing method tends to be broken at the interface of the releasing agent during pulverization, so that the releasing agent tends to be present in large amounts on the toner surface. Therefore, while a releasing effect is obtained, the toner tends to adhere to the carrier, photoreceptor, and blade (filming), and there is a problem that the overall performance is not satisfactory.
[0005] In order to overcome the problems of the kneading and pulverizing method, a method for producing a toner by a polymerization method has been proposed. Furthermore, it is possible to encapsulate a release agent. As a method for producing a toner by a polymerization method, a method for producing a toner from an elongation reaction product of a urethane-modified polyester as a toner binder has been disclosed for the purpose of improving low-temperature fixing property and high-temperature offset resistance (for example, see Patent Document 1).
[0006] In addition, a method for producing a toner that has excellent powder fluidity and transferability when made into a small particle size toner, as well as excellent heat-resistant storage stability, low-temperature fixing property, and high-temperature offset resistance has been disclosed (see, for example, Patent Documents 2 and 3). Also, a method for producing a toner having an aging step for producing a toner binder with a stable molecular weight distribution and achieving both low-temperature fixability and high-temperature offset resistance has been disclosed (see, for example, Patent Documents 4 and 5). However, these proposed techniques do not satisfy the high level of low-temperature fixability required in recent years. Therefore, in order to obtain a high level of low-temperature fixability, a toner containing a resin including a crystalline polyester resin and a release agent, in which the resin and the release agent are incompatible with each other and have a sea-island phase separation structure, has been proposed (see, for example, Patent Document 6). However, there is a problem that the vicinity of the release agent is mechanically fragile, and the strength of the toner is significantly reduced, especially when stored at high temperatures. Patent Document 6 shows that the release agent is finely dispersed, but the release agent cannot be prevented from partially seeping out during high-temperature storage and reducing its strength. Therefore, a toner containing a release agent inside tends to contaminate equipment, reduce the fluidity and chargeability of the toner itself, and reduce heat-resistant storage stability and image quality. Also, a toner containing a crystalline polyester resin, a release agent and a graft polymer has been proposed (see, for example, Patent Document 7). These proposed techniques can achieve low-temperature fixation because the crystalline polyester resin melts more rapidly than the amorphous polyester resin. However, even if the crystalline polyester resin, which is an island in the sea-island phase separation structure, melts, the amorphous polyester resin, which is the majority of the sea, does not melt. In this case, the crystalline polyester resin and the amorphous polyester resin must both melt to a certain extent before fixation can occur, and these proposed techniques do not satisfy the high level of low-temperature fixability that has been increasing in recent years. In addition, toners with excellent low-temperature fixability have various problems. One of them is a trade-off with heat-resistant storage performance. When even higher low-temperature fixability is required, a means that is compatible with the contradictory heat-resistant storage performance is required. Up to now, a means has been proposed in which the surface of the toner base particles is covered with a resin to ensure heat resistance, but there are problems such as a trade-off with low-temperature fixability and a decrease in charging performance (Patent Document 8, Patent Document 9). Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide resin particles which are excellent in low-temperature fixability and heat-resistant storage stability and which can provide stable image quality. [Means for solving the problem]
[0008] In order to solve the above-mentioned problems, one aspect of the present invention has the following configuration. Resin particles containing at least a binder resin and a release agent, the binder resin contains a crystalline polyester resin, The domain diameter of the release agent is 1 μm or less, 80% or more of the surface of the release agent is covered with a crystalline polyester resin, The melting point of the crystalline polyester resin is higher than the melting point of the release agent. 2. A resin particle comprising: Effect of the Invention
[0009] According to one aspect of the present invention, there is provided resin particles which are excellent in low-temperature fixability and heat-resistant storage stability and which can provide stable image quality. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a schematic diagram illustrating another example of an image forming apparatus according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating another example of an image forming apparatus according to the present invention. [Diagram 3] FIG. 3 is a partially enlarged view of FIG. [Figure 4] FIG. 2 is a schematic diagram illustrating an example of a process cartridge. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the resin particles, the toner, the method for producing the resin particles, and the method for producing the toner according to the present invention will be described with reference to the drawings as appropriate. It should be noted that the present invention is not limited to the embodiments described below, and may be modified, added, modified, deleted, or otherwise altered within the scope of what a person skilled in the art can conceive. As long as the functions and effects of the present invention are achieved in any aspect, it is within the scope of the present invention.
[0012] <Resin particles> The resin particles according to the present invention are resin particles containing at least a binder resin and a release agent, characterized in that the binder resin contains a crystalline polyester resin, the domain diameter of the release agent is 1 μm or less, 80% or more of the surface of the release agent is covered with the crystalline polyester resin, and the melting point of the crystalline polyester resin is higher than the melting point of the release agent. Note that the "domain diameter" in the present invention means the average diameter of each domain.
[0013] <Method for confirming domains of release agent contained in toner using a transmission electron microscope> The domain of the release agent contained in the toner of the present invention is preferably evaluated by a method using a TEM (transmission electron microscope) as described below. A cross section of a toner to be observed with a transmission electron microscope (TEM) is prepared as follows. When the toner is dyed with ruthenium, the release agent contained in the toner has a high contrast and is easy to observe. When ruthenium dyeing is used, the amount of ruthenium atoms varies depending on the strength of the dyeing, so that strongly dyed areas have a large amount of these atoms, and the electron beam does not pass through them, so they appear black in the observation image, while weakly dyed areas allow the electron beam to pass through them easily, so they appear white in the observation image. The procedure for preparing a cross section of a ruthenium-dyed toner is described below. First, the toner is immersed in a 0.5% by mass solution of ruthenium tetroxide, and block dyeing is performed for 30 to 90 minutes. Next, the ruthenium-dyed toner is embedded in a resin in which an epoxy resin as a base agent and an amine as a curing agent are mixed in a mass ratio of 1:1, and left to stand for 24 hours. Next, an ultrasonic ultramicrotome (Leica, UC7) is used to cut the cylindrical resin from the outermost surface at a cutting speed of 0.6 mm / s by the length of the radius of the toner (for example, 4.0 μm when the weight average particle size (D4) is 8.0 μm) to obtain a cross section of the center of the toner. Next, the toner is cut to a film thickness of 250 nm to prepare a thin sample of the cross section of the toner. By cutting in this manner, a cross section of the center of the toner can be obtained. The obtained thin section sample is stained for 15 minutes in a RuO4 gas atmosphere of 500 Pa using a vacuum electron staining device (filgen, VSC4R1H), and a TEM image is created using a scanning transmission electron microscope (JEOL, JEM2100). The release agent is observed in the obtained TEM image using the image processing software "Image-J".
[0014] <Method of measuring domain diameter> In the present invention, the domain diameter of the release agent means the number average of the major axis of the domains of the release agent determined based on the above TEM image. Specifically, TEM images of the cross sections of 100 toner particles are prepared using the method described above, and the long diameters of all the domains of the release agent present in the cross sections of the 100 toner particles are measured using the image processing software "Image-J," and the arithmetic average value is calculated. The obtained arithmetic mean value is regarded as the domain diameter of the release agent.
[0015] In the resin particles of the present invention, the surface of the finely dispersed release agent is covered with a crystalline polyester resin having a melting point higher than that of the release agent, and therefore the finely dispersed release agent is confined inside the toner, and the toner strength can be maintained high. By finely dispersing domains of the release agent with a domain diameter of 1 μm or less in the binder resin, the strength of the resin particles as a whole can be increased. If the domain diameter exceeds 1 μm, the strength of the resin particles will decrease drastically.
[0016] In addition, since the release agent is covered with the crystalline polyester resin, the softening and exudation of the release agent during high-temperature storage is suppressed, and the heat-resistant storage stability is significantly improved. In addition, the crystalline polyester resin covering the release agent and the binder resin become compatible with each other due to heating during fixing, and the finely dispersed release agent quickly exudes, and the low-temperature fixability can be significantly improved compared to the conventional technology.
[0017] When the ratio of the surface of the release agent covered by the crystalline polyester resin is defined as the "coverage rate," by setting the coverage rate of the surface of the release agent by the crystalline polyester resin having a higher melting point than the release agent to 80% or more, the softening and exudation of the release agent due to heat is suppressed, and the resin particles can be kept stable even during storage at high temperatures. If the melting point of the crystalline polyester is lower than that of the release agent, the crystalline polyester becomes compatible with the binder resin when heated, and the bleeding of the release agent cannot be suppressed. Also, if the coverage of the release agent surface with the crystalline polyester is less than 80%, the effect of suppressing the softening and bleeding of the release agent is significantly reduced. The release agent is preferably spherical, since the spherical shape allows the release agent to easily exude during fixing.
[0018] <Domain diameter and shape of release agent> The domain size and shape of the release agent can be measured, for example, by the following method. The toner is embedded in a visible light curable embedding resin (D-800, manufactured by Nissin EM Co., Ltd.), cut to a thickness of 60 nm using an ultrasonic ultramicrotome (EM5, manufactured by Leica), and stained with RuO4 using a vacuum staining device (manufactured by Filgen Co., Ltd.). Thereafter, observation is performed using a transmission electron microscope (H7500, Hitachi) at an accelerating voltage of 120 kV. For the toner to be observed, 50 particles having a particle size within ±2.0 μm of the weight average particle size are selected and photographed. In the case of the configuration of the present invention, when RuO4 dyeing is performed, the crystalline polyester resin in the toner is projected darker, and when a release agent is used, the release agent is projected darker still more. The average major axis and the average aspect ratio of the domains made of the release agent can be determined from the observed image, but the average aspect ratio can be calculated using image processing software as necessary.
[0019] Image-Pro Plus5.1J (Media Cybernetics) can be used as image processing software. A cross-sectional image of a toner particle photographed by the above-mentioned method is used. First, to extract the toner particles to be analyzed, select the toner particle area to separate the toner particles from the background area. Select "Measurement" - "Count / Size" in Image-Pro Plus5.1J. From the "Count / Size" window, select "Measurement" - "Measurement Items." From the measurement items, select "Diameter (min)" and "Diameter (max)." In "Brightness Range Selection", it is necessary to adjust the brightness range so that only polyester resin A is selected. Depending on the RuO4 dyeing conditions, the brightness range must be changed each time, but polyester resin A can be easily identified by the difference in shade mentioned above. Select "Count" to display the measurement results. After that, the aspect ratio (long diameter / short diameter) can be calculated by taking the obtained "diameter (minimum)" as the short diameter and the "diameter (maximum)" as the long diameter. From the aspect ratio data of one toner particle obtained in this way, the average of the 10 points in order from the largest diameter (maximum) is calculated, and this is repeated for 10 toner particles to obtain the average aspect ratio. An aspect ratio of 1.4 or less was determined to be spherical. The major axis of the release agent is preferably 1.0 μm or less, more preferably 0.5 μm or less. If the major axis is too large, the release agent is easily exposed to the toner surface, the toner becomes soft, and the heat resistance storage stability deteriorates. In addition, the release effect decreases, and the low-temperature fixability deteriorates. The aspect ratio is preferably 1.4 or less, and more preferably 1.2 or less. When the aspect ratio is large (non-spherical), the coverage of the crystalline resin decreases, and the heat-resistant storage stability deteriorates.
[0020] <Crystalline polyester resin coverage> The toner is embedded in a visible light curable embedding resin (D-800, manufactured by Nissin EM Co., Ltd.), cut to a thickness of 60 nm using an ultrasonic ultramicrotome (EM5, manufactured by Leica), and stained with Ru using a vacuum staining device (manufactured by Filgen Co., Ltd.). Thereafter, observation is performed using a transmission electron microscope (H7500, Hitachi) at an accelerating voltage of 120 kV. For the toner to be observed, 50 particles having a particle size within ±2.0 μm of the weight average particle size are selected and photographed. In the case of the configuration of the present invention, when RuO4 dyeing is performed, the crystalline polyester resin in the toner is projected darker, and when a release agent is used, the release agent is projected darker still more. The average major axis and the average aspect ratio of the domains made of the release agent can be determined from the observed image, but the average aspect ratio can be calculated using image processing software as necessary.
[0021] The coverage of the crystalline polyester resin around the release agent was calculated as follows using image processing software (Image-J). (1) The periphery of all the release agent domains unevenly distributed in the cross-sectional image of one toner particle is surrounded by freehand sections, and the periphery is measured by Analyze and designated as periphery W. (2) The length of the contact portion of the crystalline polyester resin in contact with the surface of the release agent in the cross-sectional image is measured by freehand sections and is defined as the coating length C. (3) The "perimeter W" calculated in (1) above and the "covering length C" calculated in (2) above were substituted into the following formula (1) to calculate the coverage of the crystalline polyester resin on the surface of the release agent. Crystalline polyester resin coverage [%] = (Covering length C / Circumference W) × 100 Formula (1) (4) The above steps (1) to (3) were performed on 50 toner particles, and the average value of the coverage of the crystalline polyester resin on the release agent surface of the 50 toner particles was calculated, and this average value was defined as the coverage of the crystalline polyester resin.
[0022] The toner of the present invention is made as follows. (Oil phase preparation process) In the manufacturing method of the present invention, first, an oil phase is prepared by dissolving or dispersing a resin, a colorant, a prepolymer, etc. in an organic solvent. The oil phase can be prepared by gradually adding a resin, a colorant, etc. to an organic solvent while stirring, and dissolving or dispersing them. A known dispersing device can be used for dispersion, for example, a dispersing machine such as a bead mill or a disk mill. The materials used in the oil phase preparation step will be described.
[0023] (polyester resin) When used as a toner for developing electrostatic latent images in electrophotography, good fixing properties can be obtained by using a resin having a polyester skeleton. Examples of resins having a polyester skeleton include polyester resins and block polymers of polyester and resins having other skeletons, but the use of polyester resins is preferred because the uniformity of the colored resin particles obtained is high. Examples of polyester resins include ring-opening polymers of lactones, condensation polymers of hydroxycarboxylic acids, and polycondensation polymers of polyols and polycarboxylic acids. From the viewpoint of freedom in design, polycondensation polymers of polyols and polycarboxylic acids are preferred. The weight average molecular weight of the polyester resin is usually 1000 to 30000, preferably 3000 to 15000, and more preferably 5000 to 12000. If it is less than 1000, the heat resistant storage stability deteriorates, and if it exceeds 30000, the low temperature fixability deteriorates as a toner for developing electrostatic latent images. The glass transition temperature of the polyester resin is preferably in the range of 35 to 80° C., more preferably 40 to 70° C., and even more preferably 45 to 65° C. If the temperature is less than 35° C., the resulting colored resin particles may deform when placed in a high-temperature environment such as midsummer, or the colored resin particles may stick together and not be able to behave as normal particles. If the temperature exceeds 80° C., the fixing property of the colored resin particles may deteriorate when used as a toner for developing electrostatic latent images.
[0024] <Polyol> The polyol (1) may be a diol (1-1) or a trihydric or higher polyol (1-2). Preferably, (1-1) is used alone or a mixture of (1-1) and a small amount of (1-2). Diols (1-1) include alkylene glycols (ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, etc.); Alkylene ether glycols (diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, etc.); alicyclic diols (1,4-cyclohexanedimethanol, hydrogenated bisphenol A, etc.); Bisphenols (such as bisphenol A, bisphenol F, and bisphenol S); alkylene oxide (such as ethylene oxide, propylene oxide, and butylene oxide) adducts of the above alicyclic diols; 4,4'-dihydroxybiphenyls such as 3,3'-difluoro-4,4'-dihydroxybiphenyl; bis(hydroxyphenyl)alkanes such as bis(3-fluoro-4-hydroxyphenyl)methane, 1-phenyl-1,1-bis(3-fluoro-4-hydroxyphenyl)ethane, 2,2-bis(3-fluoro-4-hydroxyphenyl)propane, 2,2-bis(3,5-difluoro-4-hydroxyphenyl)propane (also known as tetrafluorobisphenol A), and 2,2-bis(3-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane; bis(4-hydroxyphenyl)ethers such as bis(3-fluoro-4-hydroxyphenyl)ether; Examples of the bisphenols include alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts. Among these, preferred are alkylene glycols having 2 to 12 carbon atoms and alkylene oxide adducts of bisphenols, and particularly preferred are alkylene oxide adducts of bisphenols and their combined use with alkylene glycols having 2 to 12 carbon atoms. Examples of the trihydric or higher polyol (1-2) include trihydric to octahydric or higher polyhydric aliphatic alcohols (such as glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and sorbitol); Examples of the phenols include trivalent or higher phenols (trisphenol PA, phenol novolac, cresol novolac, etc.); and alkylene oxide adducts of the above-mentioned trivalent or higher polyphenols.
[0025] <Polycarboxylic acid> The polycarboxylic acid (2) may be a dicarboxylic acid (2-1) or a tri- or higher polycarboxylic acid (2-2). Preferably, (2-1) is used alone or a mixture of (2-1) and a small amount of (2-2). Examples of the dicarboxylic acid (2-1) include alkylene dicarboxylic acids (succinic acid, adipic acid, sebacic acid, etc.); alkenylene dicarboxylic acids (maleic acid, fumaric acid, etc.); aromatic dicarboxylic acids (phthalic acid, isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid, etc.), 3-fluoroisophthalic acid, 2-fluoroisophthalic acid, 2-fluoroterephthalic acid, 2,4,5,6-tetrafluoroisophthalic acid, 2,3,5,6-tetrafluoroterephthalic acid, 5-trifluoro Examples of the hexafluoroisopropyl ether include methylisophthalic acid, 2,2-bis(4-carboxyphenyl)hexafluoropropane, 2,2-bis(3-carboxyphenyl)hexafluoropropane, 2,2'-bis(trifluoromethyl)-4,4'-biphenyldicarboxylic acid, 3,3'-bis(trifluoromethyl)-4,4'-biphenyldicarboxylic acid, 2,2'-bis(trifluoromethyl)-3,3'-biphenyldicarboxylic acid, and hexafluoroisopropylidenediphthalic anhydride. Among these, alkenylene dicarboxylic acids having 4 to 20 carbon atoms and aromatic dicarboxylic acids having 8 to 20 carbon atoms are preferred. Examples of the trivalent or higher polycarboxylic acid (2-2) include aromatic polycarboxylic acids having 9 to 20 carbon atoms (trimellitic acid, pyromellitic acid, etc.). The polycarboxylic acid (2) may be an acid anhydride or a lower alkyl ester (methyl ester, ethyl ester, isopropyl ester, etc.) of the above-mentioned compounds, which may be reacted with the polyol (1). The ratio of polyol to polycarboxylic acid, expressed as the equivalent ratio [OH] / [COOH] of the hydroxyl group [OH] to the carboxyl group [COOH], is usually 2 / 1 to 1 / 2, preferably 1.5 / 1 to 1 / 1.5, and more preferably 1.3 / 1 to 1 / 1.3.
[0026] (Other binder resins) The core constituting the toner of the present embodiment may contain the following binder resin. The other binder resins are not particularly limited, and examples thereof include known binder resins such as silicone resins, styrene-acrylic resins, styrene resins, acrylic resins, epoxy resins, diene resins, phenol resins, terpene resins, terpene-phenol resins, coumarin resins, amide-imide resins, butyral resins, urethane resins, and ethylene-vinyl acetate resins, which will be described later.
[0027] (Coloring agent) As the colorant of the present invention, known dyes and pigments can be used, for example, carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ochre, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, anthrazan yellow BGL, isoindolinone. Yellow, red iron oxide, red lead, vermilion, cadmium red, cadmium mercury red, antimony vermilion, permanent red 4R, para red, phisee red, parachlor orthonitroaniline red, lithol fast scarlet G, brilliant fast scarlet, brilliant carmine BS, permanent red (F2R, F4R, FRL, FRLL, F4RH), fast scarlet VD, belkan fast rubin B, brilliant scarlet G, lithol rubin GX, permanent red F5R, brilliant carmine 6B, Pogment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkaline Blue Lake, Peacock Blue - Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake, Malachite Green Lake,Phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, lithopone and mixtures thereof can be used.
[0028] (Organic solvent) The organic solvent is preferably volatile, with a boiling point of less than 100° C., from the viewpoint of facilitating subsequent removal of the organic solvent. Examples of such organic solvents include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, methanol, ethanol, and isopropyl alcohol, which may be used alone or in combination of two or more. When the resin to be dissolved or dispersed in an organic solvent is a resin having a polyester skeleton, it is preferable to use an ester-based solvent such as methyl acetate, ethyl acetate, or butyl acetate, or a ketone-based solvent such as methyl ethyl ketone or methyl isobutyl ketone, in order to obtain high solubility. Among these, methyl acetate, ethyl acetate, and methyl ethyl ketone, which have high solvent removability, are particularly preferable.
[0029] (Prepolymer) The prepolymer is a resin having a group capable of reacting with a curing agent, and in one embodiment, after the resin particles are produced, the prepolymer is contained in the resin particles as a "polyester resin (hereinafter referred to as "polyester resin A")". The prepolymer (reactive precursor) may be a polyester having a group capable of reacting with an active hydrogen group. Examples of the group capable of reacting with an active hydrogen group include an isocyanate group, an epoxy group, a carboxylic acid, and an acid chloride group. Among these, an isocyanate group is preferred because it can introduce a urethane bond or a urea bond into the amorphous polyester resin. The prepolymer may have a branched structure imparted by at least one of a trivalent or higher alcohol and a trivalent or higher carboxylic acid.
[0030] The polyester resin containing an isocyanate group may be, for example, a reaction product of a polyester resin having an active hydrogen group and a polyisocyanate. The polyester resin having an active hydrogen group may be obtained by polycondensation of a diol, a dicarboxylic acid, and at least one of a trivalent or higher alcohol and a trivalent or higher carboxylic acid. The trivalent or higher alcohol and the trivalent or higher carboxylic acid impart a branched structure to the polyester resin containing an isocyanate group.
[0031] Examples of the diol include aliphatic diols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol; diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylol. Examples of the diol include diols having an oxyalkylene group such as ethylene glycol; alicyclic diols such as 1,4-cyclohexanedimethanol and hydrogenated bisphenol A; alicyclic diols to which alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide have been added; bisphenols such as bisphenol A, bisphenol F, and bisphenol S; and alkylene oxide adducts of bisphenols such as those to which alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide have been added. Among these, from the viewpoint of controlling the glass transition point of the polyester resin to 20° C. or less, it is preferable to use aliphatic diols having a carbon number of 3 to 10, such as 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, and 3-methyl-1,5-pentanediol, and it is more preferable to use 50 mol% or more of the alcohol component in the resin. These diols may be used alone or in combination of two or more. The polyester resin A is preferably an amorphous resin, and the melt viscosity during fixing is reduced by providing steric hindrance to the resin chain, which makes it easier to achieve low-temperature fixing properties. For this reason, the main chain of the aliphatic diol preferably has a structure represented by the following general formula (1).
[0032] [ka] [In the formula, R1 and R2 each independently represent a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and n represents an odd number from 3 to 9. However, in the n repeating units, R1 and R2 may be the same or different.]
[0033] Here, the main chain of the aliphatic diol in the present invention refers to a carbon chain that connects two hydroxyl groups of the aliphatic diol with the shortest number of carbon atoms. When the carbon number of the main chain is odd, the crystallinity decreases due to the odd-even nature, which is preferable. In addition, when the main chain has at least one alkyl group having 1 to 3 carbon atoms in the side chain, the interaction energy between the main chain molecules decreases due to the steric nature, which is more preferable.
[0034] Examples of the dicarboxylic acid include aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, dodecanedioic acid, maleic acid, and fumaric acid; and aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid. In addition, anhydrides, lower (carbon number 1 to 3) alkyl esters, and halides of these may be used. Among these, from the viewpoint of controlling the Tg of the polyester resin (A) to 20° C. or less, aliphatic dicarboxylic acids having 4 to 12 carbon atoms are preferred, and it is more preferred to use them in an amount of 50% by mass or more of the carboxylic acid component in the resin. These dicarboxylic acids may be used alone or in combination of two or more.
[0035] Examples of the trihydric or higher alcohol include trihydric or higher aliphatic alcohols such as glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and sorbitol; trihydric or higher polyphenols such as trisphenol PA, phenol novolac, and cresol novolac; and alkylene oxide adducts of trihydric or higher polyphenols, such as those obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to trihydric or higher polyphenols.
[0036] Examples of the trivalent or higher carboxylic acid include trivalent or higher aromatic carboxylic acids, and particularly preferred are trivalent or higher aromatic carboxylic acids having 9 to 20 carbon atoms, such as trimellitic acid and pyromellitic acid. In addition, anhydrides, lower (carbon number 1 to 3) alkyl esters, and halides of these may also be used.
[0037] Examples of the polyisocyanate include diisocyanates and tri- or higher valent isocyanates. The polyisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyisocyanate include 1,3- and / or 1,4-phenylene diisocyanate, 2,4- and / or 2,6-tolylene diisocyanate (TDI), crude TDI, 2,4'- and / or 4,4'-diphenylmethane diisocyanate (MDI), crude MDI [crude diaminophenylmethane [condensation product of formaldehyde and aromatic amine (aniline) or a mixture thereof; diaminodiphenylmethane and a small amount (for example, 5 to 20% by mass) of a trifunctional or more functional compound, Phosgenates of the above polyamines and mixtures thereof: polyallyl polyisocyanate (PAPI), aromatic diisocyanates such as 1,5-naphthylene diisocyanate, 4,4',4"-triphenylmethane triisocyanate, m- and p-isocyanatophenylsulfonyl isocyanate; ethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, 1,6,11-undecane triisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, etc. Aliphatic diisocyanates such as isocyanate, lysine diisocyanate, 2,6-diisocyanatomethyl caproate, bis(2-isocyanatoethyl) fumarate, bis(2-isocyanatoethyl) carbonate, and 2-isocyanatoethyl-2,6-diisocyanatohexanoate; isophorone diisocyanate (IPDI), dicyclohexylmethane-4,4'-diisocyanate (hydrogenated MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate (hydrogenated TDI), bis(2-isocyanato alicyclic diisocyanates such as m- and p-xylylene diisocyanate (XDI) and α,α,α',α'-tetramethylxylylene diisocyanate (TMXDI); trivalent or higher polyisocyanates such as lysine triisocyanate and diisocyanate-modified products of trivalent or higher alcohols; and modified products of these isocyanates, and mixtures of two or more of these may be used.Examples of the modified isocyanate include modified products containing a urethane group, a carbodiimide group, an allophanate group, a urea group, a biuret group, a uretdione group, a uretoimine group, an isocyanurate group, and an oxazolidone group.
[0038] (Charge control agent) A charge control agent and the like may be added to the oil phase. Any of the known charge control agents can be used, such as nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus simple substance or compounds, tungsten simple substance or compounds, fluorine-based activators, metal salicylic acid salts, and metal salts of salicylic acid derivatives. Specifically, these include the nigrosine dye Bontron 03, the quaternary ammonium salt Bontron P-51, the metal-containing azo dye Bontron S-34, the oxynaphthoic acid metal complex E-82, the salicylic acid metal complex E-84, the phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), the quaternary ammonium salt molybdenum complexes TP-302 and TP-415 (all manufactured by Hodogaya Chemical Co., Ltd.), the quaternary ammonium salt Copy Charge PSY VP2038, the triphenylmethane derivative Copy Blue PR, the quaternary ammonium salt Copy Charge NEG VP2036, and Copy Charge NX. Examples of the charge control agent include VP434 (all manufactured by Hoechst), LRA-901, the boron complex LR-147 (manufactured by Nippon Carlit), copper phthalocyanine, perylene, quinacridone, azo pigments, and polymeric compounds having functional groups such as sulfonic acid groups, carboxyl groups, quaternary ammonium salts, etc. The charge control agent may be used in an amount that allows the agent to exhibit its performance and does not impede fixability, etc., and is contained in the toner at 0.5 to 5 mass %, preferably 0.8 to 3 mass %.
[0039] (Phase inversion emulsification process) Next, the oil phase obtained in the oil phase preparation step is microparticulated. In this embodiment, the oil phase is neutralized with a neutralizing agent, and then an aqueous phase is added thereto, thereby obtaining a microparticle dispersion by phase inversion emulsification, in which a water-in-oil dispersion (water-in-oil emulsion) is inverted into an oil-in-water dispersion (oil-in-water emulsion).
[0040] The neutralizing agent may be either a basic inorganic compound or a basic organic compound. Examples of the basic inorganic compound include sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, sodium carbonate, sodium hydrogen carbonate, potassium carbonate, potassium hydrogen carbonate, and ammonia. Examples of the basic organic compound include N,N-dimethylethanolamine, N,N-diethylethanolamine, triethanolamine, tripropanolamine, tributanolamine, triethylamine, n-propylamine, n-butylamine, isopropylamine, monomethanolamine, morpholine, methoxypropylamine, pyridine, vinylpyridine, and isophoronediamine.
[0041] Neutralization is performed while uniformly mixing and dispersing using a normal stirrer or dispersing device. The dispersing device is not particularly limited, and examples thereof include ultrasonic dispersers, bead mills, ball mills, roll mills, homomixers, ultra mixers, dispersing mixers, penetrating type high pressure dispersing devices, collision type high pressure dispersing devices, multi-hole type high pressure dispersing devices, ultra-high pressure homogenizers, and ultrasonic homogenizers. A normal stirrer and a dispersing device may be used in combination.
[0042] The aqueous phase is ion-exchanged water or ion-exchanged water containing an organic solvent. The organic solvent may be an ester-based solvent such as methyl acetate, ethyl acetate, or butyl acetate, or a ketone-based solvent such as methyl ethyl ketone or methyl isobutyl ketone. From the viewpoint of granulation, the organic solvent concentration is preferably equal to or lower than the saturation concentration in the ion-exchanged water.
[0043] During emulsification, the mixture is uniformly mixed and dispersed using a normal stirrer or dispersing device. The dispersing device is not particularly limited, and examples thereof include ultrasonic dispersers, bead mills, ball mills, roll mills, homomixers, ultra mixers, dispersing mixers, penetrating type high-pressure dispersing devices, collision type high-pressure dispersing devices, multi-hole type high-pressure dispersing devices, ultra-high-pressure homogenizers, and ultrasonic homogenizers. A normal stirrer and a dispersing device may be used in combination.
[0044] (Solvent removal process) The organic solvent is removed from the resulting fine particle dispersion. The following four methods can be used to remove the organic solvent. (1) A method in which the temperature is gradually increased while stirring the entire system, and the organic solvent in the droplets is completely evaporated and removed. (2) A method in which the obtained fine particle dispersion is sprayed into a dry atmosphere while being stirred, to completely remove the organic solvent from the droplets. (3) A method in which the microparticle dispersion is stirred while being depressurized, and the organic solvent is evaporated and removed. (4) A method in which the organic solvent is evaporated and removed by blowing gas onto the fine particle dispersion while stirring it. The above means (2), (3), and (4) can be used in combination with the above means (1).
[0045] The drying atmosphere into which the fine particle dispersion is sprayed generally includes air, nitrogen, carbon dioxide, heated combustion gas, etc., and among these, various air streams heated to a temperature equal to or higher than the boiling point of the highest boiling point solvent used. A short treatment using a spray dryer, belt dryer, rotary kiln, etc. is sufficient to obtain the desired quality. The gas to be blown may be air, nitrogen, carbon dioxide, or heated combustion gas. By the above method, a fine particle dispersion can be obtained.
[0046] (agglomeration process) Next, the obtained colored particle dispersion is agitated to aggregate the particles to the desired particle size. To aggregate the particles, existing methods such as adding an aggregating agent or adjusting the pH can be used. When adding an aggregating agent, it may be added as is, but it is preferable to add the aggregating agent in an aqueous solution, since this can prevent localized high concentration. It is also preferable to gradually add the aggregating salt while monitoring the particle size of the colored particles. The temperature of the dispersion during aggregation is preferably near the Tg of the resin used. If the liquid temperature is too low, aggregation does not proceed very well, resulting in poor efficiency, whereas if the liquid temperature is too high, the aggregation rate increases, resulting in the generation of coarse particles and a deterioration in particle size distribution. When the target particle size is reached, aggregation is stopped by adding a salt with a low ionic valence or a chelating agent, adjusting the pH, lowering the temperature of the dispersion, or adding a large amount of aqueous medium to dilute the concentration. By the above method, a dispersion of colored aggregated particles can be obtained.
[0047] In the aggregation step, a wax may be added as a release agent, or a crystalline resin may be added for low-temperature fixability. In that case, a dispersion liquid in which a wax is dispersed in an aqueous medium or a dispersion liquid of a crystalline resin is prepared, and mixed with the colored fine particle dispersion liquid, followed by aggregation, to obtain aggregated particles in which the wax or crystalline resin is uniformly dispersed.
[0048] The flocculant, wax and crystalline resin will be described below. (Flocculant) As the flocculant, a known flocculant can be used, for example, a metal salt of a monovalent metal such as sodium or potassium, a metal salt of a divalent metal such as calcium or magnesium, or a metal salt of a trivalent metal such as iron or aluminum.
[0049] (wax) The wax is not particularly limited and can be appropriately selected depending on the purpose, but a release agent having a low melting point of 50° C. to 120° C. is preferable. The release agent having a low melting point effectively acts as a release agent between the fixing roller and the toner interface by being dispersed in the resin, and as a result, the hot offset property is good even in an oil-less case (a release agent such as oil is not applied to the fixing roller).
[0050] Suitable examples of the release agent include waxes. Examples of the waxes include natural waxes such as vegetable waxes such as carnauba wax, cotton wax, wood wax, and rice wax; animal waxes such as beeswax and lanolin; mineral waxes such as ozokerite and cerusine; and petroleum waxes such as paraffin, microcrystalline, and petrolatum. In addition to these natural waxes, synthetic hydrocarbon waxes such as Fischer-Tropsch wax and polyethylene wax; synthetic waxes such as esters, ketones, and ethers; and the like. Furthermore, fatty acid amides such as 12-hydroxystearic acid amide, stearic acid amide, phthalic anhydride, and chlorinated hydrocarbons; homopolymers or copolymers of polyacrylates such as poly-n-stearyl methacrylate and poly-n-lauryl methacrylate, which are low molecular weight crystalline polymer resins (for example, copolymers of n-stearyl acrylate and ethyl methacrylate); and crystalline polymers having long alkyl groups on the side chains may be used. These may be used alone or in combination of two or more.
[0051] The melting point of the wax is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50° C. to 120° C., and more preferably 60° C. to 90° C. If the melting point is 50° C. or higher, the wax can be prevented from adversely affecting the heat resistance storage stability, and if the melting point is 120° C. or lower, the problem of cold offset occurring during fixing at low temperatures can be effectively prevented.
[0052] The melt viscosity of the wax is preferably 5 cps to 1,000 cps, more preferably 10 cps to 100 cps, as measured at a temperature 20° C. higher than the melting point of the wax. If the melt viscosity is 5 cps or more, the release property can be prevented from decreasing, and if it is 1,000 cps or less, the effects of hot offset resistance and low-temperature fixability can be sufficiently exhibited.
[0053] The wax content in the toner is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0% by mass to 40% by mass, and more preferably 3% by mass to 30% by mass. If the wax content is 40% by mass or less, the fluidity of the toner can be prevented from deteriorating.
[0054] (Crystalline polyester resin) The crystalline polyester resin can be obtained from a polyhydric alcohol and a polycarboxylic acid or a derivative thereof, such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester. In the present invention, the crystalline polyester resin refers to a resin obtained by using a polyhydric alcohol and a polycarboxylic acid or a derivative thereof, such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester, as described above. Modified polyester resins, such as prepolymers and resins obtained by subjecting the prepolymers to a crosslinking and / or elongation reaction, do not belong to the crystalline polyester resin.
[0055] <<Polyhydric alcohol>> The polyhydric alcohol is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include diols and trihydric or higher alcohols. Examples of the diols include saturated aliphatic diols. Examples of the saturated aliphatic diols include linear saturated aliphatic diols and branched saturated aliphatic diols. Among these, linear saturated aliphatic diols are preferred, and linear saturated aliphatic diols having 2 to 12 carbon atoms are more preferred. If the saturated aliphatic diol is a branched type, the crystallinity of the crystalline polyester resin may decrease, and the melting point may decrease. In addition, if the carbon number of the saturated aliphatic diol exceeds 12, it becomes difficult to obtain a practical material.
[0056] Examples of the saturated aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanedecanediol. Among these, ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol are preferred because the crystalline polyester resin has high crystallinity and excellent sharp melting properties. Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, etc. These may be used alone or in combination of two or more.
[0057] <<Polycarboxylic acids>> The polyvalent carboxylic acid is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include divalent carboxylic acids and trivalent or higher carboxylic acids. Examples of the divalent carboxylic acids include saturated aliphatic dicarboxylic acids such as oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, and mesaconic acid; and the like. In addition, anhydrides of these and lower (1 to 3 carbon atoms) alkyl esters of these can also be mentioned.
[0058] Examples of the trivalent or higher carboxylic acid include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and the like, as well as their anhydrides and lower (carbon number 1 to 3) alkyl esters, etc. These may be used alone or in combination of two or more.
[0059] The crystalline polyester resin is preferably composed of a linear saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a linear saturated aliphatic diol having 2 to 12 carbon atoms. This provides high crystallinity and excellent sharp melting properties, and therefore excellent low-temperature fixability. In addition, as a method for controlling the crystallinity and softening point of the crystalline polyester resin, there is a method for designing and using a non-linear polyester obtained by adding a trivalent or higher polyhydric alcohol such as glycerin to the alcohol component during polyester synthesis, or a trivalent or higher polyvalent carboxylic acid such as trimellitic anhydride to the acid component and carrying out condensation polymerization.
[0060] The molecular structure of the crystalline polyester resin in the present invention can be confirmed by NMR measurement of a solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc., but it can be easily confirmed by infrared absorption spectrum at 965±10 cm -1 Or 990±10cm-1 Examples include those that have absorption due to the δCH (out-of-plane bending vibration) of olefins.
[0061] Regarding the molecular weight, from the viewpoint that a low molecular weight with a sharp molecular weight distribution has excellent low-temperature fixability, and that a large amount of low molecular weight components deteriorates heat-resistant storage stability, it has been found through extensive investigation that, in the molecular weight distribution by GPC of the o-dichlorobenzene soluble portion, the molecular weight distribution chart with the horizontal axis being log(M) and the vertical axis being weight % has a peak position in the range of 3.5 to 4.0, the half-width of the peak is 1.5 or less, the weight average molecular weight (Mw) is 3,000 to 30,000, the number average molecular weight (Mn) is 1,000 to 10,000, and Mw / Mn is 1 to 10. More preferably, the weight average molecular weight (Mw) is 5,000 to 15,000, the number average molecular weight (Mn) is 2,000 to 10,000, and Mw / Mn is 1-5.
[0062] From the viewpoint of the affinity between paper and resin, the acid value of the crystalline polyester resin is preferably 5 mgKOH / g or more to achieve the desired low-temperature fixability, more preferably 7 mgKOH / g or more to prepare fine particles by phase inversion emulsification, while it is preferably 45 mgKOH / g or less to improve hot offset properties. In addition, the hydroxyl value of the crystalline polymer is preferably 0 mgKOH / g to 50 mgKOH / g, more preferably 5 mgKOH / g to 50 mgKOH / g, to achieve a predetermined low-temperature fixability and good charging properties.
[0063] The absolute value of the difference (ΔSP value) between the SP value of the release agent and the SP value of the crystalline polyester resin is 1.1 (cal / cm 3 ) 1 / 2 It is preferable that: The SP value of a resin can be calculated by the Fedors method from the amount of monomer charged during production. When the resin monomer composition is unknown, the monomers can be identified by the following method. <Method of calculating and analyzing the composition ratio of resin monomers constituting toner> The blending amount of the monomer may be calculated by any method. For example, the toner is separated by gel permeation chromatography (GPC) or the like, and each of the separated components is subjected to the analysis method described below to calculate the mass ratio of the constituent components. In addition, gas chromatography mass spectrometry at 300°C using a reaction reagent (10% tetramethyl ammonium hydroxide (TMAH) / methanol solution) can be used to estimate the main components from the soft decomposition of the ester bonds in the resin structure through methylation, and quantitative analysis can be performed by drawing a calibration curve of TICC intensity. Separation of each component by GPC can be carried out, for example, by the following method. In GPC measurement using THF (tetrahydrofuran) as the mobile phase, the eluate is fractionated using a fraction collector or the like, and fractions corresponding to the desired molecular weight portion of the full integral of the elution curve are collected. The combined eluate is concentrated and dried using an evaporator or the like, and the solid content is dissolved in a heavy solvent such as deuterated chloroform or deuterated THF, 1 H-NMR measurement is performed, and the ratio of constituent monomers of the resin in the eluted components is calculated from the integral ratio of each element. As another method, the eluate is concentrated, hydrolyzed with sodium hydroxide or the like, and the decomposition products are qualitatively and quantitatively analyzed by high performance liquid chromatography (HPLC) or the like to calculate the ratio of constituent monomers.
[0064] (fusion process) Next, the obtained aggregated particles are fused by heat treatment to reduce unevenness. Fusion can be performed by heating the dispersion of the colored aggregated particles while stirring. The temperature of the liquid is preferably near a temperature exceeding the Tg of the resin used.
[0065] (Shelling process) The shelling step is a step of forming a shell layer on the spheronized particles obtained in the fusion step. The method for forming the shell layer is not particularly limited and can be appropriately selected depending on the purpose. For example, there can be mentioned a method in which spherical particles having a desired particle size are produced in the fusion step, the amorphous resin is added, and the aggregation step and the fusion step are repeated to form a shell layer.
[0066] (Annealing process) When a crystalline resin is added, annealing after drying causes phase separation between the amorphous resin and the crystalline resin, improving fixability. Specifically, this can be done by storing the toner at a temperature near its Tg for 10 hours or more.
[0067] (Washing and drying process) The toner particle dispersion obtained by the above method contains sub-materials such as coagulating salts in addition to the toner particles, so washing is carried out in order to extract only the toner particles from the dispersion. Methods for washing the toner particles include a centrifugation method, a vacuum filtration method, a filter press method, and the like, but are not particularly limited in the present invention.
[0068] Either method will produce a cake of toner particles, but if the toner particles cannot be sufficiently washed in one operation, the obtained cake may be dispersed again in an aqueous solvent to form a slurry, and the process of extracting the toner particles by any of the above methods may be repeated. Alternatively, if washing is performed by reduced pressure filtration or filter press, a method may be used in which the aqueous solvent is passed through the cake to wash away the secondary materials absorbed by the colored resin particles. The aqueous solvent used in this washing is water or a mixed solvent of water and an alcohol such as methanol or ethanol. Considering the cost and the environmental load due to wastewater treatment, it is preferable to use water.
[0069] Since the washed toner particles contain a large amount of the aqueous medium, the aqueous medium is removed by drying to obtain only the toner particles. As a drying method, a dryer such as a spray dryer, a vacuum freeze dryer, a reduced pressure dryer, a stationary shelf dryer, a movable shelf dryer, a fluidized bed dryer, a rotary dryer, or an agitator dryer can be used. The dried toner particles are preferably dried until the final moisture content is less than 1%. In addition, if the colored resin particles after drying are in the form of soft agglomerates and cause inconvenience in use, the soft agglomerates may be broken down by using an apparatus such as a jet mill, a Henschel mixer, a super mixer, a coffee mill, an Oster blender, or a food processor.
[0070] (External addition process) In order to impart fluidity, chargeability, cleaning properties, etc. to the toner particles obtained in the present invention, inorganic fine particles, polymeric fine particles, cleaning assistants, etc. may be added or mixed thereto. Specific mixing means include a method of applying an impact force to the mixture with blades rotating at high speed, a method of throwing the mixture into a high-speed air current, accelerating it, and causing the particles or composite particles to collide with an appropriate collision plate, etc. Examples of equipment include an Angmill (manufactured by Hosokawa Micron Corporation), a modified I-type mill (manufactured by Japan Pneumatic Co., Ltd.) with reduced grinding air pressure, a hybridization system (manufactured by Nara Machinery Works, Ltd.), a Kryptron system (manufactured by Kawasaki Heavy Industries, Ltd.), and an automatic mortar.
[0071] (External additives) The primary particle size of the inorganic fine particles is preferably 5 nm to 2 μm, and particularly preferably 5 nm to 500 nm. The specific surface area according to the BET method is 20 to 500 m 2 It is preferable that the molecular weight is 1 / g. The inorganic fine particles are preferably used in an amount of 0.01 to 5% by mass of the toner.
[0072] Specific examples of inorganic fine particles include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, red iron oxide, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, and silicon nitride. Examples of polymeric fine particles include polymer particles made of polystyrene, methacrylate or acrylate copolymers obtained by soap-free emulsion polymerization, suspension polymerization, or dispersion polymerization, polycondensation systems such as silicone, benzoguanamine, and nylon, and thermosetting resins.
[0073] Such fluidizing agents can be surface-treated to increase their hydrophobicity, thereby preventing deterioration of flowability and charging properties even under high humidity conditions. Examples of preferred surface treatment agents include silane coupling agents, silylation agents, silane coupling agents having a fluoroalkyl group, organic titanate coupling agents, aluminum coupling agents, silicone oil, and modified silicone oil.
[0074] Examples of cleaning improvers for removing the developer remaining on the photoconductor or primary transfer medium after transfer include fatty acid metal salts such as zinc stearate, calcium stearate, and stearic acid, and polymer fine particles produced by soap-free emulsion polymerization, such as polymethyl methacrylate fine particles and polystyrene fine particles. The polymer particles preferably have a relatively narrow particle size distribution and a volume average particle size of 0.01 μm to 1 μm.
[0075] (Toner storage unit) The toner storage unit in the present invention refers to a unit having a function of storing toner and storing the toner. Examples of the toner storage unit include a toner storage container, a developing unit, and a process cartridge. The toner storage container refers to a container that stores toner. The developing device has a means for containing toner and developing the toner.
[0076] <Process cartridge> The process cartridge according to the present invention is formed so as to be detachably mountable to various image forming apparatuses, and has at least a photoconductor for carrying an electrostatic latent image, and a developing means for developing the electrostatic latent image carried on the photoconductor with the developer of the present invention to form a toner image. The process cartridge of the present invention may further have other means as necessary. The developing means includes at least a developer container for containing the developer of the present invention, and a developer carrier for carrying and transporting the developer contained in the developer container. The developing means may further include a regulating member for regulating the thickness of the developer carried.
[0077] By mounting the toner storage unit on an image forming apparatus and forming an image, it is possible to take advantage of the characteristics of the toner, which has excellent offset resistance, charge stability, stress resistance, and background scumming properties, and can provide high-definition, high-quality images over a long period of time, thereby forming high-quality, high-definition images with long-term image stability.
[0078] (Image forming apparatus and image forming method) The image forming apparatus of the present invention comprises at least an electrostatic latent image carrier, an electrostatic latent image forming means, and a developing means, and further comprises other means as necessary. The image forming method according to the present invention includes at least an electrostatic latent image forming step and a development step, and further includes other steps as necessary. The image forming method can be suitably performed by the image forming apparatus, the electrostatic latent image forming process can be suitably performed by the electrostatic latent image forming means, the developing process can be suitably performed by the developing means, and the other processes can be suitably performed by the other means.
[0079] More preferably, the image forming apparatus of the present invention includes an electrostatic latent image carrier, an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image carrier, a developing means provided with toner for developing the electrostatic latent image formed on the electrostatic latent image carrier with toner to form a toner image, a transfer means for transferring the toner image formed on the electrostatic latent image carrier to a surface of a recording medium, and a fixing means for fixing the toner image transferred to the surface of the recording medium. Furthermore, the image forming method of the present invention more preferably includes an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier, a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier with toner to form a toner image, a transfer step of transferring the toner image formed on the electrostatic latent image carrier to a surface of a recording medium, and a fixing step of fixing the toner image transferred to the surface of the recording medium.
[0080] The toner is used in the developing means. Preferably, the toner image is formed by using a developer containing the toner and, if necessary, other components such as a carrier.
[0081] <Electrostatic latent image carrier> The material, structure, and size of the electrostatic latent image carrier (hereinafter also referred to as "photoreceptor") are not particularly limited and can be appropriately selected from known materials. Examples of the material include inorganic photoreceptors such as amorphous silicon and selenium, and organic photoreceptors such as polysilane and phthalopolymethine.
[0082] <Electrostatic latent image forming means> The electrostatic latent image forming means is not particularly limited as long as it is a means for forming an electrostatic latent image on the electrostatic latent image carrier, and may be appropriately selected depending on the purpose. For example, there may be mentioned a means having at least a charging member that charges the surface of the electrostatic latent image carrier, and an exposure member that exposes the surface of the electrostatic latent image carrier to light in an imagewise manner.
[0083] <Developing method> As the developing means, there is no particular limitation as long as it is a developing means including toner that develops the electrostatic latent image formed on the electrostatic latent image carrier to form a visible image, and it can be appropriately selected according to the purpose.
[0084] <Cleaning means> In the image forming apparatus of the present invention, it is preferable to have a cleaning means. As described above, the toner of the present invention is excellent in cleanability. Therefore, by applying the toner to the image forming apparatus having a cleaning means, the cleanability is improved in the following points. · By improving the spacer effect of the toner, the fluidity of the toner is maintained even under stress, and the cleanability is improved. · By satisfying 0.3 < B < 2.0 for the free amount B (mass%) of the external additive (silica), the external additive sufficiently dissociates from the toner on the photoreceptor, and by forming a deposition layer (dam layer) of the external additive in the cleaning blade nip portion, high cleanability can be achieved.
[0085] As the cleaning means, there is no particular limitation as long as it can remove the toner remaining on the photoreceptor, and it can be appropriately selected according to the purpose. Examples include a magnetic brush cleaner, an electrostatic brush cleaner, a magnetic roller cleaner, a blade cleaner, a brush cleaner, a web cleaner, and the like.
[0086] <Other means> Examples of the other means include a transfer means, a fixing means, a charge removing means, a recycling means, a control means, and the like.
[0087] Next, one aspect of a method for forming an image by the image forming apparatus of the present invention will be described with reference to FIG. 1.
[0088] An example of an image forming apparatus of the present invention is shown in Fig. 1. The color image forming apparatus 100A shown in Fig. 1 includes a photoconductor drum 10 (hereinafter sometimes referred to as "photoconductor 10") as the electrostatic latent image carrier, a charging roller 20 as the charging means, an exposure device 30 as the exposure means, a developing device 40 as the developing means, an intermediate transfer body 50, a cleaning device 60 as the cleaning means having a cleaning blade, and a static elimination lamp 70 as the static elimination means.
[0089] The intermediate transfer body 50 is an endless belt, and is designed to be movable in the direction of the arrow by three rollers 51 arranged inside and stretching it. Some of the three rollers 51 also function as transfer bias rollers capable of applying a predetermined transfer bias (primary transfer bias) to the intermediate transfer body 50. A cleaning device 90 having a cleaning blade is arranged near the intermediate transfer body 50. Also, a transfer roller 80 as the transfer means capable of applying a transfer bias for transferring (secondary transfer) a developed image (toner image) to a transfer paper P as a recording medium is arranged near the intermediate transfer body 50 so as to face the intermediate transfer body 50. Around the intermediate transfer body 50, a corona charger 52 for applying a charge to the toner image on the intermediate transfer body 50 is arranged between the contact portion between the photoconductor 10 and the intermediate transfer body 50 and the contact portion between the intermediate transfer body 50 and the transfer paper 95 in the rotation direction of the intermediate transfer body 50.
[0090] Around the photosensitive drum 10, a black developing unit 45K, a yellow developing unit 45Y, a magenta developing unit 45M, and a cyan developing unit 45C are disposed directly facing each other. The black developing unit 45K includes a developer container 42K, a developer supply roller 43K, and a developing roller 44K. The yellow developing unit 45Y includes a developer container 42Y, a developer supply roller 43Y, and a developing roller 44Y. The magenta developing unit 45M includes a developer container 42M, a developer supply roller 43M, and a developing roller 44M. The cyan developing unit 45C includes a developer container 42C, a developer supply roller 43C, and a developing roller 44C. The developing belt 41 is an endless belt that is rotatably stretched around a plurality of belt rollers, and a part of the belt 41 contacts the electrostatic latent image carrier 10.
[0091] In the color image forming apparatus 100A shown in FIG. 1, for example, the charging roller 20 uniformly charges the photoconductor drum 10. The exposure device 30 exposes the photoconductor drum 10 imagewise to light to form an electrostatic latent image. The electrostatic latent image formed on the photoconductor drum 10 is developed by supplying toner from the developing device 40 to form a toner image. The toner image is transferred (primary transfer) onto the intermediate transfer body 50 by a voltage applied from the roller 51, and is further transferred (secondary transfer) onto the transfer paper 95. As a result, a transfer image is formed on the transfer paper 95. The remaining toner on the photoconductor 10 is removed by the cleaning device 60, and the charge on the photoconductor 10 is temporarily removed by the static elimination lamp 70.
[0092] Another example of the image forming apparatus of the present invention is shown in Fig. 2. The image forming apparatus 100B shown in Fig. 2 includes a copying machine main body 150, a paper feed table 200, a scanner 300, and an automatic document feeder (ADF) 400. An endless belt-like intermediate transfer body 50 is provided in the center of the copying machine main body 150. The intermediate transfer body 50 is stretched around support rollers 14, 15, and 16, and can rotate clockwise in FIG. 2. An intermediate transfer body cleaning device 17 for removing residual toner on the intermediate transfer body 50 is provided near the support roller 15. A tandem type developing device 120 is provided on the intermediate transfer body 50 stretched around the support rollers 14 and 15 along the conveying direction of the intermediate transfer body 50, in which four image forming means 18 for yellow, cyan, magenta, and black are arranged in a row facing each other. An exposure device 21, which is the exposure member, is provided near the tandem type developing device 120. A secondary transfer device 22 is provided on the side of the intermediate transfer body 50 opposite the side on which the tandem type developing device 120 is provided. In the secondary transfer device 22, a secondary transfer belt 24, which is an endless belt, is stretched around a pair of rollers 23, and the transfer paper transported on the secondary transfer belt 24 and the intermediate transfer body 50 can come into contact with each other. A fixing device 25, which is the fixing means, is disposed near the secondary transfer device 22. The fixing device 25 includes a fixing belt 26, which is an endless belt, and a pressure roller 27 disposed so as to be pressed against the fixing belt 26. In the tandem image forming apparatus, a sheet inverting device 28 is disposed near the secondary transfer device 22 and the fixing device 25 for inverting the transfer paper so that images can be formed on both sides of the transfer paper.
[0093] Next, a description will be given of the formation of a full-color image (color copy) using the tandem type developing device 120. That is, first, an original is set on the original table 130 of the automatic document feeder (ADF) 400, or the automatic document feeder 400 is opened and an original is set on the contact glass 32 of the scanner 300, and the automatic document feeder 400 is closed.
[0094] When a start switch (not shown) is pressed, the scanner 300 is driven after the original is transported and moved onto the contact glass 32 when an original is set on the automatic original transport device 400, or immediately when an original is set on the contact glass 32. Then, the first traveling body 33 and the second traveling body 34 travel. At this time, light from a light source is irradiated by the first traveling body 33, and the reflected light from the original surface is reflected by a mirror in the second traveling body 34, and is received by the reading sensor 36 through the imaging lens 35 to read the color original (color image), which is converted into image information of black, yellow, magenta, and cyan.
[0095] Then, the image information for black, yellow, magenta, and cyan is transmitted to the image forming means 18 (image forming means for black, image forming means for yellow, image forming means for magenta, and image forming means for cyan) in the tandem developing device 120. Then, in each image forming means 18, a toner image for black, yellow, magenta, and cyan is formed. That is, as shown in FIG. 3, each image forming means 18 (image forming means for black, image forming means for yellow, image forming means for magenta, and image forming means for cyan) in the tandem developing device 120 includes an electrostatic latent image carrier 10 (electrostatic latent image carrier for black 10K, electrostatic latent image carrier for yellow 10Y, electrostatic latent image carrier for magenta 10M, and electrostatic latent image carrier for cyan 10C), a charging device 20 which is the charging means for uniformly charging the electrostatic latent image carrier 10, and a charging device 21 which charges the electrostatic latent image carrier 10 based on each color image information. The image forming apparatus includes an exposure device that exposes the electrostatic latent image carrier to light (L in FIG. 3) in the form of an image corresponding to each color image to form an electrostatic latent image corresponding to each color image on the electrostatic latent image carrier, a developing device 61 that is the developing means that develops the electrostatic latent image with each color toner (black toner, yellow toner, magenta toner, and cyan toner) to form a toner image with each color toner, a transfer charger 62 for transferring the toner image onto the intermediate transfer body 50, a cleaning device 63, and a charge remover 64. Each image forming means 18 is capable of forming a single color image (black image, yellow image, magenta image, and cyan image) based on image information of the respective color. The black image formed on the black electrostatic latent image carrier 10K, the yellow image formed on the yellow electrostatic latent image carrier 10Y, the magenta image formed on the magenta electrostatic latent image carrier 10M, and the cyan image formed on the cyan electrostatic latent image carrier 10C are sequentially transferred (primary transfer) onto the intermediate transfer body 50 which is rotated by the support rollers 14, 15, and 16. Then, the black image, the yellow image, the magenta image, and the cyan image formed on the cyan electrostatic latent image carrier 10C are superimposed on the intermediate transfer body 50 to form a composite color image (color transfer image).
[0096] On the other hand, in the paper feed table 200, one of the paper feed rollers 142 is selectively rotated to feed a sheet (recording paper) from one of the paper feed cassettes 144 provided in multiple stages in the paper bank 143. The sheets are separated one by one by the separation roller 145 and sent to the paper feed path 146, then conveyed by the conveyance roller 147 and guided to the paper feed path 148 in the copying machine main body 150, where they are stopped by striking against the registration roller 49. Alternatively, the paper feed roller 142 is rotated to feed the sheets (recording paper) on the manual feed tray 54, and the sheets are separated one by one by the separation roller 52 and placed in the manual feed path 53, where they are also stopped by striking against the registration roller 49. The registration roller 49 is generally used while being grounded, but may be used with a bias applied to remove paper dust from the sheets. Then, the registration roller 49 is rotated in synchronization with the composite color image (color transfer image) composited on the intermediate transfer body 50, a sheet (recording paper) is sent between the intermediate transfer body 50 and the secondary transfer device 22, and the composite color image (color transfer image) is transferred (secondary transfer) onto the sheet (recording paper) by the secondary transfer device 22. In this way, a color image is transferred and formed on the sheet (recording paper). Note that residual toner on the intermediate transfer body 50 after the image transfer is cleaned by the intermediate transfer body cleaning device 17.
[0097] The sheet (recording paper) on which the color image has been transferred and formed is transported by the secondary transfer device 22 and sent to the fixing device 25, where the composite color image (color transfer image) is fixed onto the sheet (recording paper) by heat and pressure. Thereafter, the sheet (recording paper) is switched by a switching claw 55, discharged by discharge rollers 56, and stacked on a paper output tray 57. Alternatively, the sheet is switched by a switching claw 55, inverted by a sheet inverting device 28, and guided to the transfer position again, an image is also recorded on the back side, and then the sheet is discharged by discharge rollers 56 and stacked on a paper output tray 57.
[0098] An example of a process cartridge according to the present invention is shown in Fig. 4. The process cartridge 110 has the photosensitive drum 10, a corona charger 52, a developing device 40, a transfer roller 80 and a cleaning device 90. EXAMPLES
[0099] Examples of the present invention will be described below, but the present invention is not limited to these examples. In the following description, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0100] <Example 1> (Preparation of polyester resin 1) In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 2 mol ethylene oxide adduct of bisphenol A / 3 mol propylene oxide adduct of bisphenol A (molar ratio 40 / 60) as a diol component, terephthalic acid / adipic acid (molar ratio 85 / 15) as a dicarboxylic acid component, and 3.5 mol% trimethylolpropane based on the total monomer amount were added so that the molar ratio of hydroxyl group to carboxylic acid (OH / COOH) was 1.2. Furthermore, 1,000 ppm of tetrabutyl orthotitanate based on the total monomer amount was added as a condensation catalyst, and the temperature was raised to 230°C over 2 hours under a nitrogen stream, and the reaction was carried out for 5 hours while distilling off the generated water. After that, the mixture was reacted for 4 hours under a reduced pressure of 5 mmHg to 15 mmHg, and cooled to 180°C. After that, 1.0 mol% of trimellitic anhydride based on the total monomer amount and 200 ppm of tetrabutyl orthotitanate based on the total monomer amount were added, and the mixture was reacted at normal pressure at 180°C for 1 hour, and then further reacted for 3 hours under a reduced pressure of 5 mmHg to 20 mmHg, to obtain [Polyester Resin 1] having a glass transition point of 57°C and a weight average molecular weight of 7,700, as determined from the DSC curve of the first heating cycle by DSC.
[0101] (Preparation of prepolymer 1) In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen inlet tube, 3-methyl-1,5-pentanediol as a diol component, terephthalic acid / adipic acid (molar ratio 55 / 45) as a dicarboxylic acid component, 1.0 mol% trimethylolpropane with respect to the total monomer amount, and 0.5 mol% trimellitic anhydride with respect to the total monomer amount were added so that the molar ratio of hydroxyl group to carboxylic acid (OH / COOH) was 1.5. Furthermore, 1,000 ppm of tetrabutyl orthotitanate with respect to the total monomer amount was added as a condensation catalyst, and the temperature was raised to 200°C over 2 hours under a nitrogen stream, and the temperature was further raised to 230°C over 2 hours, and the reaction was carried out for 3 hours while distilling off the generated water. After that, the reaction was carried out for 5 hours under a reduced pressure of 5 mmHg to 15 mmHg to obtain [intermediate polyester 1] with a weight average molecular weight of 18,000.
[0102] Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [intermediate polyester 1] and isophorone diisocyanate (IPDI) were placed in amounts such that the molar ratio (NCO / OH) of the isocyanate groups of IPDI to the hydroxyl groups of [intermediate polyester 1] was 2.0, and ethyl acetate was added to dissolve so as to obtain a 50% ethyl acetate solution. The mixture was then heated to 80°C under a nitrogen stream and reacted for 5 hours to obtain an ethyl acetate solution of [prepolymer 1], a reactive precursor of polyester resin (A). The glass transition temperature of the obtained amine-extended product of [Prepolymer 1] was −37° C. as determined from the DSC curve of the first heating run by DSC.
[0103] The amine extension product of the [prepolymer 1] is obtained by first adding ethyl acetate to adjust [prepolymer 1] to a 20% ethyl acetate solution, dropping a 20% ethyl acetate solution of isophorone diamine (IPDA) while stirring in an amount such that the molar ratio (NH2 / NCO) of the isocyanate group of [prepolymer 1] to the amino group of IPDA is 1.1, and thoroughly stirring. The obtained ethyl acetate solution of the amine extension product is cast on a Teflon (registered trademark) petri dish, dried in an environment of 80°C for 10 hours, and further dried under reduced pressure at 120°C and 10 kPa or less to thoroughly remove the solvent, thereby obtaining an amine extension product of [prepolymer 1].
[0104] (Preparation of Crystalline Polyester Resin Dispersion C-1) <Synthesis of crystalline polyester resin C-1> In a 5L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, 1,6-hexanediol and sebacic acid were charged so that the ratio of OH groups to COOH groups (OH / COOH) was 1.1. The mixture was reacted while discharging water together with 500 ppm titanium tetraisopropoxide relative to the mass of the charged raw materials, and finally heated to 235°C and reacted for 1 hour. Then, the mixture was reacted for 6 hours under reduced pressure of 10 mmHg or less. Then, the temperature was set to 185°C, trimellitic anhydride was added so that the molar ratio with COOH groups was 0.053, and the mixture was reacted for 2 hours with stirring to obtain [Crystalline polyester resin C-1]. [Crystalline polyester resin C-1] (55 parts), methyl ethyl ketone (35 parts), and 2-propyl alcohol (10 parts) were added to a four-neck flask. Then, the mixture was stirred while being heated at the melting point of the [Crystalline polyester resin C-1] to dissolve the [Crystalline polyester resin C-1]. The SP value of [Crystalline polyester resin C-1] is 10.2 (cal / cm 3 ) 1 / 2 It was.
[0105] <Preparation of Crystalline Polyester Resin Dispersion C-1> In a container equipped with a stirring rod and a thermometer, 45 parts of [Crystalline polyester resin C-1] and 450 parts of ethyl acetate were charged, and the temperature was raised to 80°C under stirring, and the temperature was kept at 80°C for 5 hours, after which the temperature was cooled to 30°C in 1 hour. Dispersion was performed using a bead mill (Ultraviscomill, manufactured by Imex) under conditions of a liquid delivery rate of 1 kg / hr, a disk peripheral speed of 6 m / sec, 80% by volume of zirconia beads with a diameter of 0.5 mm, and 3 passes to obtain [Crystalline polyester resin dispersion C-1]. The volume average particle size of the obtained crystalline polyester resin particles was 450 nm, and the solid concentration of the resin particles was 10%. The melting point of [Crystalline polyester resin C-1] is 74.9°C, and the SP value is 10.2 (cal / cm3 ) 1 / 2 It was.
[0106] <Synthesis of crystalline polyester resin C-2> Ethylene glycol and sebacic acid were charged into a 5L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple so that the ratio of OH groups to COOH groups (OH / COOH) was 1.1. The mixture was reacted while discharging water together with 500 ppm titanium tetraisopropoxide relative to the mass of the charged raw materials, and finally heated to 235°C and reacted for 1 hour. Then, the mixture was reacted for 6 hours under reduced pressure of 10 mmHg or less. Then, the temperature was set to 185°C, trimellitic anhydride was added so that the molar ratio with COOH groups was 0.053, and the mixture was reacted for 2 hours with stirring to obtain [Crystalline polyester resin C-2]. [Crystalline polyester resin C-2] (55 parts), methyl ethyl ketone (35 parts), and 2-propyl alcohol (10 parts) were added to a four-neck flask. Then, the mixture was stirred while being heated at the melting point of [Crystalline polyester resin C-2] to dissolve the [Crystalline polyester resin C-2]. The SP value of [Crystalline polyester resin C-2] is 10.0 (cal / cm 3 ) 1 / 2 It was.
[0107] <Synthesis of crystalline polyester resin C-3> In a 5L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, 1,6-hexanediol and 1,10-decanedicarboxylic acid were charged so that the ratio of OH groups to COOH groups (OH / COOH) was 1.1. The mixture was reacted while discharging water together with 500 ppm of titanium tetraisopropoxide relative to the mass of the charged raw materials, and finally heated to 235°C and reacted for 1 hour. Then, the mixture was reacted for 6 hours under reduced pressure of 10 mmHg or less. Then, the temperature was set to 185°C, trimellitic anhydride was added so that the molar ratio with COOH groups was 0.053, and the mixture was reacted for 2 hours with stirring to obtain [Crystalline polyester resin C-3]. [Crystalline polyester resin C-3] (55 parts), methyl ethyl ketone (35 parts), and 2-propyl alcohol (10 parts) were added to a four-neck flask. Then, the mixture was stirred while being heated at the melting point of [Crystalline polyester resin C-3] to dissolve the [Crystalline polyester resin C-3]. The SP value of [Crystalline polyester resin C-3] is 9.7 (cal / cm 3 ) 1 / 2 It was.
[0108] <Synthesis of crystalline polyester resin C-4> Ethylene glycol and adipic acid were charged into a 5L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple so that the ratio of OH groups to COOH groups (OH / COOH) was 1.1. The reaction was carried out while discharging water together with 500 ppm titanium tetraisopropoxide relative to the mass of the charged raw materials, and the temperature was finally raised to 235°C and the reaction was carried out for 1 hour. After that, the reaction was carried out for 6 hours under a reduced pressure of 10 mmHg or less. After that, the temperature was set to 185°C, trimellitic anhydride was added so that the molar ratio with COOH groups was 0.053, and the reaction was carried out for 2 hours with stirring to obtain [Crystalline polyester resin C-4]. Into a four-neck flask, 55 parts of [Crystalline polyester resin C-4], 35 parts of methyl ethyl ketone, and 10 parts of 2-propyl alcohol were added. Then, the mixture was stirred while being heated at the melting point of the [Crystalline polyester resin C-4] to dissolve the [Crystalline polyester resin C-4]. The SP value of [Crystalline polyester resin C-4] is 10.9 (cal / cm 3 ) 1 / 2 It was.
[0109] <Synthesis of crystalline polyester resin C-5> 1,6-hexanediol and sebacic acid were charged into a 5L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple so that the ratio of OH groups to COOH groups (OH / COOH) was 1.1. The reaction was carried out while discharging water together with 500 ppm of titanium tetraisopropoxide relative to the mass of the charged raw materials, and the temperature was finally raised to 235°C and the reaction was carried out for 1 hour. After that, the reaction was carried out for 6 hours under a reduced pressure of 10 mmHg or less. After that, the temperature was set to 185°C, trimellitic anhydride was added so that the molar ratio with COOH groups was 0.053, and the reaction was carried out for 2 hours with stirring to obtain [Crystalline polyester resin C-5]. [Crystalline polyester resin C-5] (55 parts), methyl ethyl ketone (35 parts), and 2-propyl alcohol (10 parts) were added to a four-neck flask. Then, the mixture was stirred while being heated at the melting point of [Crystalline polyester resin C-5] to dissolve the [Crystalline polyester resin C-5]. The SP value of [Crystalline polyester resin C-5] is 9.8 (cal / cm 3 ) 1 / 2 It was.
[0110] <Synthesis of crystalline polyester resin C-6> 1,6-hexanediol and oxalic acid were charged into a 5L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple so that the ratio of OH groups to COOH groups (OH / COOH) was 1.1. The mixture was reacted while draining water together with 500 ppm titanium tetraisopropoxide relative to the mass of the charged raw materials, and finally heated to 235°C and reacted for 1 hour. Then, the mixture was reacted for 6 hours under reduced pressure of 10 mmHg or less. Then, the temperature was set to 185°C, trimellitic anhydride was added so that the molar ratio with COOH groups was 0.053, and the mixture was reacted for 2 hours with stirring to obtain [Crystalline polyester resin C-6]. Into a four-neck flask, 55 parts of [Crystalline polyester resin C-6], 35 parts of methyl ethyl ketone, and 10 parts of 2-propyl alcohol were added. Then, the mixture was heated and stirred at the melting point of [Crystalline polyester resin C-6] to dissolve the [Crystalline polyester resin C-6]. The SP value of [Crystalline polyester resin C-6] was 10.8 (cal / cm 3 ) 1 / 2 It was.
[0111] <Synthesis of amorphous polyester resin (MB) for masterbatches> In a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, bisphenol A ethylene oxide 2 mole adduct, bisphenol A propylene oxide 2 mole adduct, terephthalic acid, and adipic acid were added to obtain a mixture of bisphenol A propylene oxide 2 mole adduct and bisphenol A ethylene oxide 2 mole adduct in a molar ratio of 60 / 40 (bisphenol A propylene oxide 2 mole adduct / bisphenol A ethylene oxide 2 mole adduct). The molar ratio (terephthalic acid / adipic acid) was 97 / 3, and the molar ratio of hydroxyl groups to carboxyl groups, OH / COOH, was 1.3. This was reacted with titanium tetraisopropoxide (500 ppm relative to the resin components) at normal pressure and 230°C for 8 hours, and then reacted for a further 4 hours at a reduced pressure of 10 mmHg to 15 mmHg. After that, trimellitic anhydride was added to the reaction vessel so that the amount was 1 mol% relative to the total resin components, and this was reacted at 180°C, normal pressure, for 4 hours to obtain [Amorphous polyester resin MB for master batches].
[0112] <Preparation of Masterbatch 1> 1,200 parts of water, 500 parts of carbon black (Printex35, manufactured by Dexa) [DBP oil absorption=42 mL / 100 mg, pH=9.5], and 500 parts of [amorphous polyester resin MB for master batches] were added and mixed in a Henschel mixer (manufactured by Nippon Coke and Engineering Co., Ltd.). The mixture was kneaded using two rolls at 150° C. for 30 minutes, then rolled to cool and pulverized in a pulverizer to obtain [master batch 1].
[0113] (Preparation of WAX dispersion 1) To 720 parts of ion-exchanged water, 180 parts of ester wax (NOF Corporation, WE-11, synthetic wax made from plant-derived monomers, melting point 67°C) and 17 parts of an anionic surfactant (Dai-ichi Kogyo Seiyaku, Neogen SC, sodium dodecylbenzenesulfonate) were added. This was dispersed in a homogenizer while heated to 90°C, yielding [WAX Dispersion 1]. The volume average particle size of the resulting wax particles was 300 nm, and the solid concentration of the resin particles was 25%. The SP value of the above ester wax is 9.5 (cal / cm 3 ) 1 / 2 It was.
[0114] (Preparation of WAX dispersion 2) [WAX Dispersion 2] was obtained in the same manner as WAX Dispersion 1, except that in the preparation of WAX Dispersion 1, the ester wax (NOF Corporation, WE-11, melting point 67°C) was replaced with ester wax (NOF Corporation, WE-10, melting point 70.4°C). The SP value of the above ester wax is 9.7 (cal / cm 3 ) 1 / 2 It was.
[0115] <Toner production> <Preparation of oil phase> 50 parts of [amine-extended product of prepolymer 1], 50 parts of [crystalline polyester resin dispersion C-1], 50 parts of [wax dispersion 1], 550 parts of [polyester resin 1], and 100 parts of [master batch 1] were placed in a container and mixed at 5,000 rpm for 60 minutes using a TK homomixer (manufactured by Primix Corporation) to obtain [oil phase 1]. The above blend amounts indicate the blend amounts of solid content in each raw material.
[0116] <Preparation of aqueous phase> 990 parts of water, 20 parts of sodium dodecyl sulfate, and 90 parts of ethyl acetate were mixed and stirred to obtain a milky white liquid, which was designated as [aqueous phase 1].
[0117] <Emulsification> 700 parts of [Oil Phase 1] was stirred at 8,000 rpm with a TK homomixer, and 20 parts of 28% aqueous ammonia was added so that the neutralization rate was 400%, and after mixing for 10 minutes, 1,200 parts of [Aqueous Phase 1] was gradually added dropwise to obtain [Emulsified Slurry 1]. The particle size of [Emulsified Slurry 1] was measured to be 0.50 μm. The solid content concentration was also measured to be 23.0%.
[0118] <Agglomeration / fusion process> 100 parts of [Emulsified slurry 1] and 300 parts of ion-exchanged water were placed in a container and stirred for 1 minute. Next, 100 parts of 3% magnesium chloride solution was added dropwise and the mixture was stirred for an additional 5 minutes, and then heated to 60°C. Thereafter, when the particle size reached 5.0 μm, 50 parts of sodium chloride was added to terminate the flocculation step, and [flocculated slurry 1] was obtained. The [aggregated slurry 1] was heated to 70° C. while being stirred, and cooled when the desired circularity of 0.957 was reached, to obtain [resin particle dispersion 1].
[0119] <Annealing process, cleaning process, drying process> [Resin particle dispersion 1] was stored at 45° C. for 10 hours, filtered under reduced pressure, and washed and dried as follows. (1) 100 parts of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (at 12,000 rpm for 10 minutes), and then filtered. (2): 900 parts of ion-exchanged water was added to the filter cake of (1), and ultrasonic vibration was applied and mixed with a TK homomixer (rotation speed 12,000 rpm for 30 minutes), and then the mixture was filtered under reduced pressure. This operation was repeated until the electrical conductivity of the reslurry liquid became 10 μC / cm or less, and then the mixture was filtered to obtain [Filter cake 1]. The [filter cake 1] was dried in a circulating air dryer at 45° C. for 48 hours and sieved through a 75 μm mesh to obtain [resin particles 1].
[0120] <External attachment> 2.5 parts of inorganic fine particles, TS530 manufactured by Cabosil Corporation, were added to 100 parts of [Resin particles 1], and mixed for 10 minutes at 40 m / s in a Henschel mixer to obtain [Toner 1].
[0121] <Example 2> [Toner 2] was obtained in the same manner as in Example 1, except that in the preparation of [Crystalline Polyester Resin Dispersion C-1] in Example 1, [Crystalline Polyester Resin C-1] was changed to [Crystalline Polyester Resin C-2], [WAX Dispersion 1] was changed to [WAX Dispersion 2], and the heating temperature of the aggregated slurry in the aggregation and fusion process was changed to 68°C.
[0122] <Example 3> [Toner 3] was obtained in the same manner as in Example 1, except that in the preparation of [Crystalline Polyester Resin Dispersion C-1] in Example 1, [Crystalline Polyester Resin C-1] was changed to [Crystalline Polyester Resin C-3], [WAX Dispersion 1] was changed to [WAX Dispersion 2], and the heating temperature of the aggregated slurry 1 in the aggregation and fusion process was changed to 75°C.
[0123] <Example 4> [Toner 4] was obtained in the same manner as in Example 1, except that in the preparation of [Crystalline polyester resin dispersion C-1] in Example 1, [Crystalline polyester resin C-1] was changed to [Crystalline polyester resin C-2].
[0124] <Example 5> [Toner 5] was obtained in the same manner as in Example 1, except that in the preparation of [Crystalline Polyester Resin Dispersion C-1] in Example 1, [Crystalline Polyester Resin C-1] was changed to [Crystalline Polyester Resin C-2] and [WAX Dispersion 1] was changed to [WAX Dispersion 2].
[0125] <Example 6> [Toner 6] was obtained in the same manner as in Example 1, except that in the preparation of [Crystalline Polyester Resin Dispersion C-1] in Example 1, [Crystalline Polyester Resin C-1] was changed to [Crystalline Polyester Resin C-2], [WAX Dispersion 1] was changed to [WAX Dispersion 2], and the heating temperature of the aggregated slurry in the aggregation and fusion process was changed to 72°C.
[0126] <Example 7> [Toner 7] was obtained in the same manner as in Example 1, except that in the preparation of [Crystalline Polyester Resin Dispersion C-1] in Example 1, [Crystalline Polyester Resin C-1] was changed to [Crystalline Polyester Resin C-6], [WAX Dispersion 1] was changed to [WAX Dispersion 2], and the heating temperature of the aggregated slurry in the aggregation and fusion process was changed to 72°C.
[0127] <Comparative Example 1> [Toner 8] was obtained in the same manner as in Example 1, except that in the preparation of [Crystalline Polyester Resin Dispersion C-1] in Example 1, [Crystalline Polyester Resin C-1] was changed to [Crystalline Polyester Resin C-4], [WAX Dispersion 1] was changed to [WAX Dispersion 2], and the heating temperature of the aggregated slurry in the aggregation and fusion process was changed to 72°C.
[0128] <Comparative Example 2> [Toner 9] was obtained in the same manner as in Example 1, except that in the preparation of [Crystalline Polyester Resin Dispersion C-1] in Example 1, [Crystalline Polyester Resin C-1] was changed to [Crystalline Polyester Resin C-4], [WAX Dispersion 1] was changed to [WAX Dispersion 2], and the heating temperature of the aggregated slurry in the aggregation and fusion process was changed to 75°C.
[0129] <Comparative Example 3> [Toner 10] was obtained in the same manner as in Example 1, except that in the preparation of [Crystalline Polyester Resin Dispersion C-1] in Example 1, [Crystalline Polyester Resin C-1] was changed to [Crystalline Polyester Resin C-5], [WAX Dispersion 1] was changed to [WAX Dispersion 2], and the heating temperature of the aggregated slurry in the aggregation and fusion process was changed to 65°C.
[0130] <Comparative Example 4> [Toner 11] was obtained in the same manner as in Example 1, except that in the preparation of [Crystalline Polyester Resin Dispersion C-1] in Example 1, [Crystalline Polyester Resin C-1] was changed to [Crystalline Polyester Resin C-4], [WAX Dispersion 1] was changed to [WAX Dispersion 2], and the heating temperature of the aggregated slurry in the aggregation and fusion process was changed to 65°C.
[0131] <Comparative Example 5> [Toner 12] was obtained in the same manner as in Example 1, except that in the preparation of [Crystalline Polyester Resin Dispersion C-1] in Example 1, [Crystalline Polyester Resin C-1] was replaced with [Crystalline Polyester Resin C-4], and the heating temperature of the aggregated slurry in the aggregation and fusion process was changed to 68°C.
[0132] The compositions of the oil phases in Examples 1 to 7 and Comparative Examples 1 to 5 are shown in Table 1. In Table 1, "↑" means "the same as that shown in the upper column."
[0133] [Table 1]
[0134] Table 2 shows the physical properties of the wax in Examples 1 to 7 and Comparative Examples 1 to 5, the shapes measured by the above-mentioned measuring method, the physical properties of the crystalline polyester resin, the coverage of the crystalline polyester resin measured by the above-mentioned measuring method, and the conditions of the aggregated slurry.
[0135] [Table 2]
[0136] <Preparation of carrier> To 100 parts of toluene, 100 parts of silicone resin (organo straight silicone), 5 parts of γ-(2-aminoethyl)aminopropyltrimethoxysilane, and 10 parts of carbon black were added, and dispersed for 20 minutes with a homomixer to prepare a resin layer coating liquid. Using a fluidized bed type coating device, the resin layer coating liquid was applied to the surface of 1,000 parts of spherical magnetite having a volume average particle size of 50 μm to prepare a [carrier].
[0137] <Preparation of developer> Using a ball mill, 5 parts of each toner and 95 parts of carrier were mixed to prepare each developer.
[0138] Next, the various properties of each of the toners and developers obtained were evaluated as follows.
[0139] <Low temperature fixability> Composite resin particles are applied to the paper surface at 0.8 mg / cm 2 The powder is applied evenly to the paper surface using a printer with the heat fixing unit removed. Other methods may be used as long as they can uniformly deposit the powder at the above weight density. The paper is then fixed to the pressure roller at a fixing speed (heat roller peripheral speed) of 213 mm / sec and a fixing pressure (pressure roller pressure) of 10 kg / cm. 2 The temperature at which cold offset occurs (MFT) was measured when the paper was passed through the above conditions. The lower the temperature at which cold offset occurs, the better the low-temperature fixing property.
[0140] [Evaluation Criteria] ◎: Minimum fixing temperature is 130℃ or less ○: The minimum fixing temperature is greater than 130°C and less than or equal to 135°C. △: The minimum fixing temperature is greater than 135°C and less than 140°C ×: The minimum fixing temperature is higher than 140° C.
[0141] <Heat-resistant storage stability> The toner was filled into a 50 mL glass container and left in a thermostatic chamber at 50° C. for 24 hours, and then cooled to 24° C. Next, the penetration [mm] was measured by a penetration test (JIS K2235-1991) to evaluate the heat resistance storage stability. [Evaluation Criteria] ◎: Penetration 20mm or more ○: Penetration 15mm or more and less than 20mm △: Penetration 10mm or more and less than 15mm ×: Penetration less than 10mm
[0142] <Image quality> A 400 dpi standard line chart image for evaluation (output image) was formed on coated paper (POD gloss coated paper, Oji Paper Co., Ltd.) using a color production printer (RICOH Pro C7210S, manufactured by Ricoh Co., Ltd.). The output image was formed so that a line image of a black solid image was created. The formed thin line portion was compared with the original file image, and reproducibility was evaluated according to the criteria in the table below. Note that an evaluation result of "3" or more is at a practically usable level.
[0143] [Evaluation Criteria] 5: Even when the image of the continuous lines in the original image is viewed through a magnifying glass, there are no missing high-brightness lines and they are reproduced. 4: When observed with a loupe at 100x magnification, slight partial loss of the line image is observed. 3: When observed with a loupe at 100x magnification, partial loss of the line image is evident. 2: Partial loss of line image is visible to the naked eye. 1: Continuous missing parts of the line image are clearly visible to the naked eye.
[0144] The evaluation results of Examples 1 to 7 and Comparative Examples 1 to 5 are shown in Table 3.
[0145] [Table 3]
[0146] From the results in Table 3, it is clear that Examples 1 to 7 of the present invention exhibit excellent performance in all of low-temperature fixing property, heat-resistant storage stability, and image quality. On the other hand, it was found that Comparative Examples 1 to 5 had deteriorated low-temperature fixability, heat-resistant storage stability, and image quality.
[0147] Examples of aspects of the present invention include the following. (1) Resin particles containing at least a binder resin and a release agent, the binder resin contains a crystalline polyester resin, The domain diameter of the release agent is 1 μm or less, 80% or more of the surface of the release agent is covered with a crystalline polyester resin, The melting point of the crystalline polyester resin is higher than the melting point of the release agent. 2. A resin particle comprising: (2) The absolute value of the difference (ΔSP value) between the SP value of the release agent and the SP value of the crystalline polyester resin is 1.1 (cal / cm 3 ) 1 / 2 The resin particles according to the above (1), which are: (3) The resin particles according to (1) or (2) above, wherein the binder resin is an amorphous polyester resin containing an aliphatic alcohol monomer. (4) The resin particles according to any one of (1) to (3) above, wherein the release agent is spherical. (5) A toner comprising the resin particles according to any one of (1) to (4) above. (6) an oil phase preparation step of preparing an oil phase by dissolving or dispersing at least a binder resin containing a crystalline polyester resin and a release agent in an organic solvent; a phase inversion emulsification step of adding an aqueous phase to the oil phase to invert the water-in-oil dispersion into an oil-in-water dispersion; a desolvation step of removing an organic solvent from the oil-in-water dispersion to obtain a fine particle dispersion; an aggregating step of aggregating the microparticles in the microparticle dispersion; The method for producing resin particles according to any one of (1) to (5) above, comprising: (7) an electrostatic latent image carrier; an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image bearing member; a developing unit which develops the electrostatic latent image formed on the electrostatic latent image carrier to form a toner image, and which is provided with a toner; An image forming apparatus, wherein the toner is the toner described in (5) above. (8) forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier with a toner to form a toner image, The image forming method, wherein the toner is the toner described in (5) above. [Explanation of symbols]
[0148] 10 Electrostatic latent image carrier (photoconductor drum) 10K Black Electrostatic Latent Image Carrier 10Y Yellow electrostatic latent image carrier 10M Magenta electrostatic latent image carrier 10C Cyan electrostatic latent image carrier 14 Support roller 15 Support roller 16 Support roller 17 Cleaning equipment 18 Image forming means 20 Charging roller 21 Exposure equipment 22 Secondary transfer device 23 Laura 24 Secondary transfer belt 25 Fixing device 26 Fixing belt 27 Pressure roller 28 Sheet reversing device 30 Exposure equipment 32 Contact Glass 33 First Running Body 34 Second Running Body 35 Imaging Lens 36 Reading sensor 40 Developer 41 Developing belt 42K Developer compartment 42Y Developer storage unit 42M Developer compartment 42C Developer container 43K Developer supply roller 43Y Developer supply roller 43M Developer supply roller 43C Developer supply roller 44K developing roller 44Y Developing roller 44M Developing roller 44C Developing roller 45K Black Development Unit 45Y Yellow Development Unit 45M Magenta Development Unit 45C Cyan Development Unit 49 Registration roller 50 Intermediate transfer body 51 Lola 52 Corona charger 53 Manual feed path 54 Manual feed tray 55 Switching claw 56 Discharge roller 57 Output Tray 58 Corona charging device 60 Cleaning Equipment 61 Developing device 62 Transfer charger 63 Cleaning Equipment 64 Static electricity removal lamp 70 Static electricity removal lamp 80 Transfer roller 90 Cleaning Equipment 95 Transfer paper 100A, 100B, 100C image forming device 110 Process cartridge 120 Tandem type developer 130 Manuscript stand 142 Paper feed roller 143 Paper Bank 144 Paper feed cassette 145 Separation roller 146 Paper feed path 147 Transport roller 148 Paper feed path 150 Copying device body 160 Charging device 200 Paper feed table 300 Scanner 400 Automatic Document Feeder (ADF) L exposure light [Prior art documents] [Patent documents]
[0149] [Patent Document 1] Japanese Patent Application Publication No. 11-133665 [Patent Document 2] JP 2002-287400 A [Patent Document 3] JP 2002-351143 A [Patent Document 4] Patent No. 2579150 [Patent Document 5] JP 2001-158819 A [Patent Document 6] JP 2004-46095 A [Patent Document 7] JP 2007-271789 A [Patent Document 8] Patent No. 6024276 [Patent Document 9] Patent No. 4873734
Claims
1. Resin particles containing at least a binder resin and a release agent, the binder resin contains a crystalline polyester resin, The domain diameter of the release agent is 1 μm or less, 80% or more of the surface of the release agent is covered with a crystalline polyester resin, The melting point of the crystalline polyester resin is higher than the melting point of the release agent.
1. A resin particle comprising:
2. The absolute value of the difference between the SP value of the release agent and the SP value of the crystalline polyester resin (ΔSP value) is 1.1 (cal / cm 3 ) 1/2 The resin particles according to claim 1, wherein:
3. 3. The resin particles according to claim 1, wherein the binder resin is an amorphous polyester resin containing an aliphatic alcohol monomer.
4. The resin particles according to claim 1 or 2, wherein the release agent is spherical.
5. A toner comprising the resin particles according to claim 1 or 2.
6. an oil phase preparation step of preparing an oil phase by dissolving or dispersing at least a binder resin containing a crystalline polyester resin and a release agent in an organic solvent; a phase inversion emulsification step of adding an aqueous phase to the oil phase to invert the water-in-oil dispersion into an oil-in-water dispersion; a desolvation step of removing an organic solvent from the oil-in-water dispersion to obtain a fine particle dispersion; an aggregating step of aggregating the microparticles in the microparticle dispersion; The method for producing resin particles according to claim 1 , comprising:
7. An electrostatic latent image carrier; an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image bearing member; a developing unit which develops the electrostatic latent image formed on the electrostatic latent image carrier to form a toner image, and which is provided with a toner; 6. An image forming apparatus, comprising: the toner according to claim 5.
8. an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier with a toner to form a toner image, 6. An image forming method, comprising the toner according to claim 5.
Citation Information
Patent Citations
JP1973073734A
Welding wire feeder
JP1985024276A
Dry toner
JP1999133665A
Method for producing polyester-based polymer
JP2001158819A
Dry toner, manufacturing method for the toner and image forming apparatus using the toner
JP2002287400A