Styrenic resin extrusion foam molding and method for manufacturing the same

By controlling the extrusion and molding processes with specific ratios, the method achieves styrenic resin foam molded articles with uniform density across the width, addressing warping and productivity issues.

JP2024137822APending Publication Date: 2024-10-07KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024041846
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-22
Filing Date
2024-03-18
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Existing styrenic resin extrusion foam molded products exhibit significant variations in density across the width direction, leading to potential warping and reduced productivity.

Method used

A method involving extrusion through a die lip with a rectangular opening followed by adjustment using a roll forming machine to control the width and thickness, with specific ratios for the width expansion and take-up speed, ensuring the density variation in the width direction is minimized.

Benefits of technology

The method produces styrenic resin extrusion foam molded articles with small density variations in the width direction, enhancing stability and productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137822000001_ABST
    Figure 2024137822000001_ABST
Patent Text Reader

Abstract

To provide a styrenic resin extrusion foam molding which has small variations in densities in a width direction, and a method for manufacturing the same.SOLUTION: A method for manufacturing a styrenic resin extrusion foam molding 100 includes Step Sa and Step Sb. Step Sa extrudes a styrenic resin composition containing a styrenic resin and a foaming agent from a high pressure area to a low pressure area through a die lip 11 having a rectangular opening, and thereby obtain an extrusion foam 20. Step Sb adjusts the width and the thickness of the extrusion foam 20 obtained in Step Sa by a roll molding machine 40, and thereby obtains the styrenic resin extrusion foam molding 100. A value obtained by dividing the width of the styrenic resin extrusion foam molding 100 obtained in Step Sb by a length in a longitudinal direction of the opening of the die lip 11 is 1.85 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an extruded styrene resin foam and a method for producing the same. [Background technology]

[0002] Since styrene-based resin extrusion foams have good heat insulating properties, they are used as heat insulating materials for houses, buildings, etc. For example, styrene-based resin extrusion foams are continuously produced by melt-kneading a styrene-based resin and a foaming agent in an extruder, optionally cooling the resulting composition, and extruding it through a die lip (e.g., a slit in a die) into a low pressure region.

[0003] For example, Patent Document 1 discloses a production method that makes it possible to obtain extruded styrene-based resin foamed articles with beautiful surfaces by controlling the pressure release rate when a composition containing a styrene-based resin and a foaming agent is extruded into a low pressure region. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-124281 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the technology described in Patent Document 1 leaves room for improvement in terms of reducing the variation in density in the width direction of the resulting styrene-based resin extrusion foam molding. If the variation in density in the width direction of the styrene-based resin extrusion foam molding is large, the styrene-based resin extrusion foam molding may warp, making it difficult to apply the styrene-based resin extrusion foam molding to a heat insulating material, etc. In addition, if the variation in density in the width direction of the styrene-based resin extrusion foam molding is large, the density may be locally high, which may reduce productivity.

[0006] In view of the above, an object of the present invention is to provide an extruded styrene resin foam having a small density variation in the width direction, and a method for producing the same. [Means for solving the problem]

[0007] <Aspects of the present invention> The present invention includes the following aspects.

[0008] [1] A step Sa of extruding a styrene-based resin composition containing a styrene-based resin and a foaming agent from a high pressure region to a low pressure region through a die lip having a rectangular opening to obtain an extruded foam; a step Sb of obtaining a styrene-based resin extruded foam by adjusting the width and thickness of the extruded foam with a roll molding machine; A method for producing an extruded styrene resin foam comprising: A method for producing a styrene-based resin extrusion foam, wherein a value obtained by dividing the width of the styrene-based resin extrusion foam obtained in the step Sb by the longitudinal length of the opening of the die lip is 1.85 or less.

[0009] [2] The method for producing a styrene-based resin extrusion foam according to [1] above, wherein a value obtained by dividing the width of the styrene-based resin extrusion foam obtained in the step Sb by the longitudinal length of the opening of the die lip is 1.50 or more.

[0010] [3] The method for producing a styrene-based resin extruded foam according to [1] or [2] above, wherein a value obtained by dividing the take-up speed of the roll molding machine by a flow rate of the extruded foam into the roll molding machine is 0.76 or less.

[0011] [4] A styrene-based resin extrusion foam molding containing a styrene-based resin, A styrene-based resin extrusion foam molded product, in which the standard deviation of density in the width direction divided by the average density is less than 0.010. Effect of the Invention

[0012] According to the present invention, it is possible to provide an extruded styrene resin foam having a small density variation in the width direction, and a method for producing the same. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a schematic diagram for explaining an example of a method for producing an extruded styrene resin foam according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Preferred embodiments of the present invention will be described in detail below, but the present invention is not limited thereto. In addition, all academic and patent documents described in this specification are incorporated herein by reference.

[0015] Hereinafter, the compound and its derivatives may be collectively referred to by adding "based" after the compound name. In addition, when the polymer name is represented by adding "based" after the compound name, it means that the repeating unit of the polymer is derived from the compound or its derivative, unless otherwise specified. In addition, acrylic and methacrylic may be collectively referred to as "(meth)acrylic". In addition, acrylonitrile and methacrylonitrile may be collectively referred to as "(meth)acrylonitrile".

[0016] Unless otherwise specified, the components and functional groups exemplified in this specification may be used alone or in combination of two or more kinds.

[0017] The drawings referred to in the following description mainly show each component diagrammatically for ease of understanding, and the size, number, shape, etc. of each component shown in the drawings may differ from the actual ones due to the convenience of creating the drawings.

[0018] <First embodiment: Method for producing styrene-based resin extrusion foam> The manufacturing method of the styrene-based resin extrusion foam according to the first embodiment of the present invention includes steps Sa and Sb. In step Sa, a styrene-based resin composition containing a styrene-based resin and a foaming agent is extruded from a high pressure region to a low pressure region through a die lip having a rectangular opening to obtain an extruded foam. In step Sb, the width and thickness of the extruded foam obtained in step Sa are adjusted by a roll molding machine to obtain a styrene-based resin extrusion foam. In the first embodiment, the value obtained by dividing the width of the styrene-based resin extrusion foam obtained in step Sb by the longitudinal length of the opening of the die lip is 1.85 or less. According to the first embodiment, by including the above configuration, a styrene-based resin extrusion foam having a small density variation in the width direction can be obtained.

[0019] Hereinafter, the "styrene-based resin extruded foam" may be simply referred to as the "extruded foam." Furthermore, the "step Sa" may be referred to as the "extrusion step." Furthermore, the "step Sb" may be referred to as the "molding step." Furthermore, the value obtained by dividing the width (unit: mm) of the extruded foam obtained in the molding step by the longitudinal length (unit: mm) of the die lip opening may be referred to as the "width expansion ratio."

[0020] The "width of the extruded foam obtained in the molding process" refers to the width of the extruded foam before it is cut into a product. In the first embodiment, no cutting (slitting) is performed to narrow the width of the extruded foam (or extruded foam) in any of the extrusion process, molding process, and any process optionally provided between the extrusion process and the molding process.

[0021] In the first embodiment, in order to obtain an extruded foam having smaller density variation in the width direction, the width expansion ratio is preferably 1.84 or less.

[0022] In the first embodiment, in order to adjust the expansion ratio to a range suitable for a thermal insulating material or the like, the width expansion ratio is preferably 1.50 or more, more preferably 1.55 or more, and even more preferably 1.60 or more.

[0023] Hereinafter, an example of the method for producing an extruded styrene-based resin foam according to the first embodiment will be described with reference to the drawings as appropriate. Fig. 1 is a schematic diagram for explaining an example of the method for producing an extruded styrene-based resin foam according to the first embodiment.

[0024] 1, in the first embodiment, a styrene-based resin composition containing a styrene-based resin and a foaming agent is extruded through a die lip 11 of an extrusion device 10 to obtain an extruded foam 20 (extrusion step). At this time, the internal pressure of the extrusion device 10 is made higher than the pressure in the region where the styrene-based resin composition is extruded (e.g., atmospheric pressure), and the styrene-based resin composition is extruded from the high-pressure region of the extrusion device 10 to a low-pressure region, whereby the styrene-based resin composition is foamed to become the extruded foam 20.

[0025] The die lip 11 has a rectangular opening (not shown). The length of the opening of the die lip 11 in the longitudinal direction is, for example, 100 mm or more and 500 mm or less, and the length of the opening of the die lip 11 in the lateral direction is, for example, 1 mm or more and 7 mm or less.

[0026] In the example shown in Fig. 1, after the extruded foam 20 is obtained, the thickness and width of the extruded foam 20 are roughly adjusted (preliminary adjustment) by a molding die 30 placed in close contact with or close to the die lip 11. The molding die 30 includes two molding plates (not shown) placed at a predetermined distance. The thickness and width of the extruded foam 20 are roughly adjusted by passing the extruded foam 20 between the two molding plates of the molding die 30. Note that, although a molding die is used in the example shown in Fig. 1, the present invention does not require the use of a molding die.

[0027] The extruded foam 20 that has passed through the molding die 30 passes between molding rolls 41 and 42 of a roll molding machine 40 installed downstream of the molding die 30, whereby its thickness and width are adjusted (main adjustment) (molding step). The roll molding machine 40 includes at least a pair of molding rolls 41 and 42. The thickness and width of the extruded foam 20 are adjusted by the molding step, and an extruded foam 100 is obtained. In the first embodiment, the width expansion ratio is 1.85 or less.

[0028] In order to obtain an extruded foam 100 with smaller density variation in the width direction, the value obtained by dividing the take-up speed of the roll molding machine 40 by the inflow speed of the extruded foam 20 into the roll molding machine 40 is preferably 0.76 or less, and more preferably 0.75 or less. Hereinafter, the value obtained by dividing the take-up speed of the roll molding machine (unit: m / min) by the inflow speed of the extruded foam into the roll molding machine (unit: m / min) may be referred to as the "take-up / inflow speed ratio."

[0029] The inflow speed (unit: m / min) of the extruded foam 20 into the roll molding machine 40 is determined by the discharge rate (unit: kg / min) from the die lip 11 and the average density (unit: kg / m) of the extruded foam 100 obtained in the molding process. 3 ), the thickness (unit: mm) of the extruded foam molded product 100 obtained in the molding process, and the width (unit: mm) of the extruded foam molded product 100 obtained in the molding process, can be calculated using the formula "inflow rate = 1,000,000 x discharge rate / (average density x thickness x width)".

[0030] 1, the take-off speed of the roll forming machine 40 is the rotational speed (linear speed) of the forming rolls 41 and 42. When the roll forming machine 40 has two or more pairs of forming rolls, the take-off speed of the roll forming machine 40 is the rotational speed (linear speed) of the forming roll installed at the most downstream position.

[0031] In order to adjust the expansion ratio to a range suitable for use as a heat insulating material, the take-off / inlet velocity ratio is preferably 0.65 or more, more preferably 0.68 or more, and even more preferably 0.70 or more.

[0032] The width expansion rate can be adjusted, for example, by changing at least one of the amount (extrusion rate) of the styrene-based resin composition extruded from the die lip 11 per unit time, the pressure applied to the styrene-based resin composition immediately before being extruded from the die lip 11, and the take-up speed of the roll molding machine 40.

[0033] In order to obtain an extruded foam 100 having smaller density variation in the width direction while adjusting the expansion ratio to a range suitable for insulation materials, etc., it is preferable that the width expansion ratio is 1.50 to 1.85 and the take-off / inlet speed ratio is 0.65 to 0.76, it is more preferable that the width expansion ratio is 1.55 to 1.85 and the take-off / inlet speed ratio is 0.68 to 0.76, and it is even more preferable that the width expansion ratio is 1.60 to 1.85 and the take-off / inlet speed ratio is 0.70 to 0.76.

[0034] Next, each step of the method for producing a styrenic resin extrusion foam molded product according to the first embodiment will be described. The method for producing a styrenic resin extrusion foam molded product according to the first embodiment includes an extrusion step and a molding step. The method for producing a styrenic resin extrusion foam molded product according to the first embodiment may also include steps other than the extrusion step and the molding step. Steps other than the extrusion step and the molding step include a resin composition preparation step and a melt-kneading step, which will be described below.

[0035] [Resin composition preparation process] In the resin composition preparation step, each material of the extrusion foam is blended to prepare a styrene-based resin composition. The styrene-based resin composition contains at least a styrene-based resin and a foaming agent. The foaming agent may be injected into the styrene-based resin composition containing materials other than the foaming agent in the subsequent melt-kneading step. An example of the material constituting the styrene-based resin composition will be described below.

[0036] (styrene resin) Examples of the styrene resin include homopolymers of styrene monomers, copolymers of two or more styrene monomers, and copolymers of styrene monomers and other monomers. The content of structural units derived from styrene monomers in the styrene resin is preferably 70% by weight or more, more preferably 80% by weight or more, and even more preferably 90% by weight or more. Examples of the copolymer include random copolymers, block copolymers, and graft copolymers.

[0037] Examples of styrene-based monomers include styrene, methylstyrene, dimethylstyrene, ethylstyrene, diethylstyrene, isopropylstyrene, bromostyrene, dibromostyrene, tribromostyrene, chlorostyrene, dichlorostyrene, trichlorostyrene, vinyltoluene, and vinylxylene. Examples of other monomers include polyfunctional vinyl compounds such as divinylbenzene; (meth)acrylic acid; (meth)acrylic acid ester compounds such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, and butyl methacrylate; cyanide vinyl compounds such as (meth)acrylonitrile; diene compounds such as butadiene; unsaturated carboxylic acid anhydrides such as maleic anhydride and itaconic anhydride; and N-alkyl-substituted maleimide compounds such as N-methylmaleimide, N-butylmaleimide, N-cyclohexylmaleimide, and N-phenylmaleimide. These may be used alone or in combination of two or more.

[0038] The styrene resin may be a blend of a homopolymer or copolymer of the above-mentioned styrene monomer and a homopolymer or copolymer of the above-mentioned other monomer. For example, the styrene resin may be blended with rubber-reinforced polystyrene (e.g., diene-rubber-reinforced polystyrene, acrylic-rubber-reinforced polystyrene, etc.), polyphenylene ether resin, etc.

[0039] As the styrene-based resin, polystyrene (a homopolymer of styrene), a styrene-acrylonitrile copolymer, a styrene-(meth)acrylic acid copolymer, a styrene-maleic anhydride copolymer, and a styrene-diene compound copolymer (for example, a styrene-butadiene copolymer) are preferred from the viewpoints of being relatively inexpensive and suitable for extrusion foam molding, etc. From the viewpoint of cost, polystyrene is particularly preferred.

[0040] The styrene resin may have a branched structure for the purpose of adjusting the melt flow rate, melt viscosity during molding, melt tension, etc. Hereinafter, the melt flow rate is referred to as MFR. The MFR of the styrene resin is preferably 40 g / 10 min or less, more preferably 1 g / 10 min or more and 30 g / 10 min or less. If the MFR of the styrene resin is 40 g / 10 min or less, it is easy to uniformly disperse the foaming agent in the styrene resin in the extrusion device, so that extrusion and foam molding can be performed stably, and as a result, production stability is improved. In this specification, the MFR of the styrene resin is a value measured according to the measurement method specified in JIS K7210 under conditions of a temperature of 200 ° C. and a load of 5 kg.

[0041] (foaming agent) Examples of the blowing agent include carbon dioxide, water, dimethyl ether, saturated hydrocarbons having 3 to 5 carbon atoms, alcohols having 1 to 4 carbon atoms, inorganic gases (more specifically, nitrogen, etc.), and organic fluorine compounds having a small global warming potential (more specifically, hydrofluoroolefins, hydrochlorofluoroolefins, etc.). These may be used alone or in combination of two or more.

[0042] Examples of saturated hydrocarbons having 3 to 5 carbon atoms include propane, normal butane, isobutane, normal pentane, isopentane, and neopentane. From the viewpoint of foamability, propane, normal butane, isobutane, and mixtures thereof are preferred. Also, from the viewpoint of heat insulating performance of extrusion foamed products, normal butane, isobutane, and mixtures thereof are preferred.

[0043] Examples of the alcohol having 1 to 4 carbon atoms include ethanol, methanol, propyl alcohol, isopropyl alcohol, butyl alcohol, isobutyl alcohol, and tert-butyl alcohol.

[0044] The amount of the foaming agent used (when multiple types of foaming agents are used, the total amount used) is preferably 1 part by weight or more and 20 parts by weight or less, and more preferably 5 parts by weight or more and 10 parts by weight or less, per 100 parts by weight of the styrene-based resin. When the amount of the foaming agent used is 1 part by weight or more and 20 parts by weight or less, the foaming power of the styrene-based resin composition is ensured, and it becomes easier to stably obtain an extruded foam molded article having a desired thickness.

[0045] (Flame retardant) As the flame retardant, a bromine-based flame retardant is preferably used. Specific examples of the bromine-based flame retardant include brominated bisphenol-based compounds such as tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl)ether and tetrabromobisphenol A-bis(2,3-dibromopropyl)ether; bromine-containing polymers such as brominated styrene-butadiene block copolymers, brominated styrene-butadiene random copolymers, and brominated styrene-butadiene graft copolymers; tetrabromocyclooctane; hexabromocyclododecane; tris(2,3-dibromopropyl)isocyanurate; and the like. These may be used alone or in combination of two or more.

[0046] From the viewpoint of economic efficiency and its influence on other required physical properties, the amount of the flame retardant used is preferably 0.5 parts by weight or more and 10 parts by weight or less, and more preferably 0.5 parts by weight or more and 7 parts by weight or less, per 100 parts by weight of the styrene-based resin.

[0047] The styrene-based resin composition may contain, as other additives, water-absorbing substances (bentonite, silica, etc.), cell size regulators (talc, etc.), lubricants (sodium stearate, calcium stearate, etc.), radical generators (2,3-dimethyl-2,3-diphenylbutane, poly-1,4-diisopropylbenzene, etc.), flame retardant assistants (triphenylphosphine oxide, etc.), stabilizers (epoxy compounds, polyhydric alcohol ester compounds, phenolic stabilizers, phosphite stabilizers, etc.), surfactants, flame retardant regulators (iron oxide, iron complexes, diphenylalkanes, diketones, etc.), processing aids (fatty acid metal salts, fatty acid amides, fatty acid esters, liquid paraffin, olefin waxes, etc.), antistatic agents, colorants (pigments, dyes, etc.), ultraviolet absorbers, fluorescent brighteners, plasticizers, fillers, etc.

[0048] [Melting and kneading process] In the melt-kneading step, the styrene-based resin composition is supplied to an extrusion device, and the styrene-based resin composition is melt-kneaded in the extrusion device. The extrusion device may be, for example, an extrusion device equipped with an extruder using a screw. The extruder using a screw may be, for example, a single-screw extruder or a twin-screw extruder. The L / D (effective length of the screw / diameter of the screw) of the extruder is, for example, 10 or more and 50 or less. When a twin-screw extruder is used, the rotation directions of the screws may be the same or different.

[0049] The extrusion device may also include a first extruder for melt-kneading the foaming agent and a material other than the foaming agent, and a second extruder for further melt-kneading and cooling the melt-kneaded product obtained in the first extruder. When the extrusion device includes the second extruder, the foaming agent may be supplied to the second extruder. The type of the first extruder and the type of the second extruder may be the same or different. Furthermore, the extrusion device may include a cooler downstream of the extruder for the purpose of adjusting the temperature to a temperature suitable for foaming the styrene-based resin composition. At the most downstream of the extrusion device, a die lip is provided as an opening for extruding the styrene-based resin composition.

[0050] The temperature when the styrene-based resin composition is melt-kneaded is, for example, 150° C. or more and 250° C. or less. When a cooler is used, the melt-kneaded product is preferably cooled in the cooler to a temperature of, for example, 100° C. or more and 140° C. or less.

[0051] [Extrusion process] In the extrusion step, the styrene-based resin composition (e.g., the molten mixture obtained in the melt-kneading step) is extruded from a high-pressure region through a die lip to a low-pressure region (e.g., into the atmosphere) to foam the styrene-based resin composition and obtain an extruded foam. The pressure (pressure in the high-pressure region) applied to the styrene-based resin composition immediately before it is extruded through the die lip is, for example, 1.5 MPa or more and 15 MPa or less. Hereinafter, the pressure applied to the styrene-based resin composition immediately before it is extruded through the die lip may be referred to as "foaming pressure".

[0052] [Molding process] In the molding step, the width and thickness of the extruded foam obtained in the extrusion step are adjusted by a roll molding machine to obtain a styrene-based resin extruded foam. The inflow speed of the extruded foam into the roll molding machine is, for example, 2.00 m / min to 8.00 m / min, preferably 3.00 m / min to 7.00 m / min. The take-up speed of the roll molding machine is, for example, 1.00 m / min to 6.00 m / min, preferably 2.00 m / min to 5.00 m / min.

[0053] In the first embodiment, after the molding step, a step of cutting the obtained extruded foam according to the application may be provided.

[0054] [Extruded styrene resin foam obtained by the manufacturing method according to the first embodiment] Next, the extruded styrene resin foam molded product (hereinafter, sometimes referred to as "extruded foam molded product FM") obtained by the production method according to the first embodiment will be described.

[0055] The extruded foam FM is produced by the production method according to the first embodiment, and therefore has small variation in density in the width direction.

[0056] In order to obtain an extruded foam FM with smaller density variation in the width direction, the standard deviation of the density of the extruded foam FM in the width direction (unit: kg / m 3 ) to the average density of the extruded foam FM (unit: kg / m 3 ) is preferably less than 0.010.

[0057] Hereinafter, the value obtained by dividing the standard deviation of the density in the width direction of the extruded foam molded product by the average density of the extruded foam molded product may be referred to as the "deviation / average density ratio". The lower limit of the deviation / average density ratio is not particularly limited and may be 0.000. The method for measuring the standard deviation of the density in the width direction of the extruded foam molded product and the method for measuring the average density of the extruded foam molded product are both the same as or similar to the methods described in the examples below.

[0058] The thickness of the extruded foam FM is not particularly limited and is appropriately selected depending on the application. For example, in the case of a heat insulating material used for applications such as building materials, in order to impart preferable heat insulating properties, bending strength, and compressive strength, the thickness of the extruded foam FM is preferably 10 mm or more, more preferably 20 mm or more. In addition, from the viewpoint of the processability of the extruded foam FM, the thickness of the extruded foam FM is preferably 150 mm or less, more preferably 100 mm or less.

[0059] In addition, in the case of extruded styrene-based resin foam molded products, after foam molding to give them a shape, the surface layer (skin layer) that was in contact with the mold may be removed by about 5 mm in the thickness direction to produce the final product, and the thickness of the extruded foam molded product FM is the thickness of the extruded foam molded product before the skin layer is removed.

[0060] In order to obtain an extruded foam molded product FM that is lightweight while having excellent heat insulation, bending strength, and compressive strength, the density of the extruded foam molded product FM is 15 kg / m 3 More than 60kg / m 3 It is preferable that the thickness is less than 20 kg / m 3 More than 40kg / m 3 It is more preferable that:

[0061] In order to obtain an extruded foam FM having excellent heat insulation, bending strength, and compressive strength, the average cell diameter of the extruded foam FM is preferably 0.05 mm or more and 1.00 mm or less, more preferably 0.10 mm or more and 1.00 mm or less, even more preferably 0.20 mm or more and 0.80 mm or less, and particularly preferably 0.20 mm or more and 0.60 mm or less. In order to obtain an extruded foam FM having high heat insulation, the closed cell ratio of the extruded foam FM is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more.

[0062] <Second embodiment: styrene-based resin extrusion foam> Next, a styrene-based resin extruded foam according to a second embodiment of the present invention will be described. In the following description, the description of the same content as in the first embodiment may be omitted.

[0063] The styrene-based resin extrusion foam according to the second embodiment contains a styrene-based resin and has a deviation / average density ratio of less than 0.010. Since the styrene-based resin extrusion foam according to the second embodiment has a deviation / average density ratio of less than 0.010, the density variation in the width direction is small.

[0064] The method for producing the styrene-based resin extrusion foam according to the second embodiment is not particularly limited as long as it is a method capable of adjusting the deviation / average density ratio to less than 0.010. However, in order to easily adjust the deviation / average density ratio to less than 0.010, the method for producing the styrene-based resin extrusion foam according to the second embodiment is preferably the method for producing the styrene-based resin extrusion foam according to the first embodiment. When the styrene-based resin extrusion foam according to the second embodiment is produced by the production method according to the first embodiment, the deviation / average density ratio can be adjusted, for example, by changing at least one of the width expansion rate and the take-up / inflow speed ratio.

[0065] Other points of the second embodiment are the same as those described in the section [Extruded styrene resin foam obtained by the production method according to the first embodiment] above. EXAMPLES

[0066] Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0067] <Material preparation> The following materials were prepared as materials for producing extruded foam molded articles of the Examples and Comparative Examples.

[0068] [Styrene-based resin] Styrene resin (PS Japan "680", MFR: 7.0g / 10min)

[0069] [Flame retardant] Brominated styrene-butadiene block copolymer (LANXESS "EMERALD INNOVATION 3000", bromine content: 65% by weight)

[0070] [Water-absorbing substance] Bentonite (BYK "Bentolite L") Silica (Evonik Degussa Japan "Carplex BS-304F")

[0071] [Radical generator] Poly-1,4-diisopropylbenzene (United Initiators "CUROX CC-P3")

[0072] [Stabilizer] Bisphenol A diglycidyl ether (ADEKA "EP-13") Reaction mixture of dipentaerythritol and adipic acid (Ajinomoto Fine-Techno Co., Ltd. "Plenriser ST210") Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)] (Rianlon "RIANOX 1010FF") 3,9-bis(2,4-di-tert-butylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane (SONGWON "SONGNOX 6260FF") Orthocresol novolac epoxy resin (DIC "EPICLON N-680")

[0073] [Lubricant] Calcium stearate ("SC-P" manufactured by Sakai Chemical Industry Co., Ltd.)

[0074] [Bubble size adjuster] Talc (Hayashi Kasei "KHP-400")

[0075] [Foaming agent] Odorless butane (Iwatani Corporation, a mixture of isobutane and normal butane, weight ratio: isobutane / normal butane = 30 / 70) Dimethyl ether (manufactured by Iwatani Corporation) Water (tap water)

[0076] <Preparation of extruded foam> The methods for producing the extruded foams of Examples 1 to 4 and Comparative Examples 1 and 2 will be described below.

[0077] [Example 1] (Resin composition preparation process) A mixture of 100 parts by weight of a styrene-based resin, 2.50 parts by weight of a brominated styrene-butadiene block copolymer, 0.20 parts by weight of poly-1,4-diisopropylbenzene, 0.20 parts by weight of a reaction mixture of dipentaerythritol and adipic acid, 0.25 parts by weight of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)], and 3,9-bis(2,4-di-tert-butylphenoxy)phenyl ether was added. A resin composition was prepared by dry blending 0.0125 parts by weight of (oxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 0.125 parts by weight of orthocresol novolac epoxy resin, 0.15 parts by weight of bisphenol A diglycidyl ether, 0.10 parts by weight of talc, 0.20 parts by weight of calcium stearate, 0.40 parts by weight of bentonite, and 0.10 parts by weight of silica.

[0078] (Melting and kneading process) The obtained resin composition was fed into the first extruder of an extrusion device in which a twin screw extruder (first extruder) with a diameter of 40 mm and L / D 32, a single screw extruder (second extruder) with a diameter of 90 mm and L / D 30, and a cooler were connected in series in this order, so that the discharge rate from the die lip (amount extruded from the die lip) described below was 50 kg / hour. Then, the resin composition was melt-kneaded in the first extruder while being heated at a temperature of 200°C to obtain a melt-kneaded product. Next, 3.50 parts by weight of odorless butane, 3.00 parts by weight of dimethyl ether, and 0.50 parts by weight of water were pressed into the melt-kneaded product near the center of the first extruder with respect to 100 parts by weight of styrene-based resin. Then, the mixture was kneaded in the second extruder connected to the first extruder, and the temperature (resin temperature) of the melt-kneaded product was cooled to 120°C by a cooler connected to the second extruder.

[0079] (Extrusion process) Next, the molten mixture (styrene-based resin composition) was extruded into the atmosphere at a foaming pressure of 2.1 MPa from a die lip having a rectangular opening (longitudinal length of opening: 150 mm, lateral length of opening: 1.9 mm) provided at the tip of the cooling machine, and foamed.

[0080] (molding process) The obtained extruded foam was then molded using a molding die (distance between two molding plates: 25 mm) placed in close contact with the die lip and a roll molding machine (distance between upper and lower rolls: 15 mm, take-up speed: 2.44 m / min) placed downstream of the molding die, to obtain an extruded foam having a rectangular cross-sectional shape of 30.5 mm in thickness and 276 mm in width (extruded foam of Example 1).

[0081] [Examples 2 to 4 and Comparative Examples 1 and 2] The extruded foam molded articles of Examples 2 to 4 and Comparative Examples 1 and 2 were obtained in the same manner as in Example 1, except that the discharge rate from the die lip, the foaming pressure, and the take-up speed of the roll molding machine were set as shown in Table 1 below.

[0082] <Measurement method> The methods for measuring the thickness, width, average density, and standard deviation of the density in the width direction of the extruded foam are described below. For each measurement method, the extruded foam was used after being left to stand for 16 hours or more in a standard atmosphere of JIS K 7100:1999 Class 3 (temperature 23±5°C, relative humidity 40-70%) for conditioning.

[0083] [Thickness of extruded foam] For each extruded foam, the thickness was measured at three locations, namely, the center in the width direction, a location 50 mm from one end in the width direction toward the center, and a location 50 mm from the other end in the width direction toward the center, using a caliper ("M-type standard caliper" manufactured by Mitutoyo Corporation). The average value was calculated from the measurements at the three locations, and the average value was defined as the thickness of each extruded foam.

[0084] [Width of extruded foam] The width of each extruded foam was measured using a caliper ("M-type standard caliper" manufactured by Mitutoyo Corporation). The width of each extruded foam was measured at one location for each extruded foam.

[0085] [Average density of extruded foam] First, each extruded foam was cut so that the length in the longitudinal direction (extrusion direction in the extrusion process) was 50 mm, and then the surface layers (skin layers) on both sides of the extruded foam were removed so that 10 mm regions remained above and below the center of the thickness direction of the extruded foam. Next, the obtained rod-shaped extruded foam (length in the extrusion direction: 50 mm, thickness: 20 mm, width: width shown in Table 1 below) was cut at 20 mm intervals in the width direction of the extruded foam to obtain multiple test pieces (about 10 to 12 pieces for each extruded foam). The length, thickness, and width of each test piece obtained were measured using a caliper ("M-type standard caliper" manufactured by Mitutoyo Corporation) to determine the volume. Next, the weight of each test piece was measured, and the density of each test piece was calculated from the obtained weight and the above volume. Then, for each extruded foam, the average value of the density of the multiple test pieces was calculated, and the obtained average value was taken as the average density of each extruded foam.

[0086] [Standard deviation of density in the width direction of extruded foam] For each extruded foam, the standard deviation of the densities of the test pieces obtained in the measurement of the [average density of the extruded foam] was calculated. 3 In the following cases, the extruded foam molding was evaluated as having "small density variation in the width direction." On the other hand, the standard deviation of the density in the width direction of the extruded foam molding was 0.30 kg / m 3 When the density variation in the width direction was larger than 100%, the extruded foam was evaluated as "having a large density variation in the width direction".

[0087] <Result> Table 1 shows the discharge rate from the die lip, the foaming pressure, the thickness of the extruded foam, the width of the extruded foam, the width expansion rate, the inflow speed of the extruded foam into the roll molding machine, the take-up speed of the roll molding machine, the take-up / inflow speed ratio, the average density of the extruded foam, the standard deviation of the density in the width direction of the extruded foam, and the deviation / average density ratio for Examples 1 to 4 and Comparative Examples 1 and 2.

[0088] [Table 1]

[0089] As shown in Table 1, the width expansion ratio was 1.85 or less in Examples 1 to 4. In Examples 1 to 4, the standard deviation of the density in the width direction of the extruded foam molded product was 0.30 kg / m 3 Thus, the extruded foams obtained in Examples 1 to 4 had small variation in density in the width direction.

[0090] As shown in Table 1, the width expansion ratio exceeded 1.85 in Comparative Examples 1 and 2. In Comparative Examples 1 and 2, the standard deviation of the density in the width direction of the extruded foam molded product was 0.30 kg / m 3 Therefore, the extruded foams obtained in Comparative Examples 1 and 2 had a large variation in density in the width direction.

[0091] The above results demonstrate that the present invention can provide an extruded styrene resin foam having a small density variation in the width direction. [Explanation of symbols]

[0092] 11: Die Lip 20: Extruded foam 40: Roll forming machine 100: Extruded foam (styrene-based resin extruded foam)

Claims

1. A step Sa of extruding a styrene-based resin composition containing a styrene-based resin and a foaming agent from a high pressure region to a low pressure region through a die lip having a rectangular opening to obtain an extruded foam; a step Sb of adjusting the width and thickness of the extruded foam by a roll molding machine to obtain a styrene-based resin extruded foam; A method for producing an extruded styrene resin foam comprising: A method for producing a styrene-based resin extrusion foam, wherein a value obtained by dividing the width of the styrene-based resin extrusion foam obtained in the step Sb by the longitudinal length of the opening of the die lip is 1.85 or less.

2. 2. The method for producing a styrene-based resin extrusion foam according to claim 1, wherein a value obtained by dividing the width of the styrene-based resin extrusion foam obtained in the step Sb by the length of the opening of the die lip in the longitudinal direction is 1.50 or more.

3. 3. The method for producing a styrene-based resin extrusion foam according to claim 1, wherein a value obtained by dividing a take-up speed of the roll molding machine by an inflow speed of the extruded foam into the roll molding machine is 0.76 or less.

4. A styrene-based resin extrusion foam molding containing a styrene-based resin, A styrene-based resin extrusion foam molded product, in which the standard deviation of density in the width direction divided by the average density is less than 0.010.

Citation Information

Patent Citations

  • Method for producing polystyrene-based resin extruded foam

    JP2013124281A