Resin composition and molding

A copolymer with carboxylic acid derivatives improves the toughness and appearance of polyester-polyolefin blends, addressing existing issues in polymer blends for molded products and promoting sustainable production.

JP2024137880APending Publication Date: 2024-10-07MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024045298
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-23
Filing Date
2024-03-21
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Polymer blends of polyester resins and polyolefin resins lack sufficient toughness and appearance when formed into molded products, despite the use of compatibilizers like carboxylic acid-modified ethylene/α-olefin copolymers, necessitating further improvements for various applications.

Method used

Incorporating a copolymer with specific structural units derived from carboxylic acid and/or carboxylic acid derivatives into the polymer blend, specifically an α-olefin copolymer with 21 or more carbon atoms, enhances compatibility and dispersibility, resulting in improved toughness and appearance.

Benefits of technology

The resin composition achieves high toughness, excellent fluidity, and enhanced appearance in molded products, contributing to sustainable production and consumption by minimizing property reductions in recycled materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137880000004
    Figure 2024137880000004
  • Figure 2024137880000001
    Figure 2024137880000001
  • Figure 2024137880000002
    Figure 2024137880000002
Patent Text Reader

Abstract

To provide a resin composition excellent in fluidity and capable of giving a molding having high toughness and excellent appearance.SOLUTION: The resin composition contains a polyolefin resin (A), a polyester resin (B), and a copolymer (C) of a carboxylic acid and / or carboxylic acid derivative and an α-olefin. A structural unit derived from the carboxylic acid and / or carboxylic acid derivative is present in the main chain of the copolymer (C).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition and a molded article. [Background technology]

[0002] Polyester resins are widely used as materials for containers of seasonings, beverages, cosmetics, etc., or food packaging films, because of their excellent mechanical properties, heat resistance, rigidity, gas barrier properties, and flavor barrier properties. On the other hand, although polyester resins have high rigidity, their high glass transition temperature of about 81°C makes them unsuitable for the manufacture of molded products that require impact resistance. In addition, polyester resins themselves have the problem of being unable to be heat sealed, and various improvements in their properties are required according to the application. For these reasons, polymer blends (including polymer alloys) of polyester resins and polyolefin resins are being actively studied.

[0003] For example, Patent Document 1 describes that by blending a polyester resin, an olefin resin, and a carboxylic acid-modified ethylene-α-olefin copolymer in a specific ratio, it is possible to produce a molded article having high low-temperature impact strength and high rigidity. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-106886 A Summary of the Invention [Problem to be solved by the invention]

[0005] Since a polymer blend of a polyester resin and a polyolefin resin is expected to be applied to various applications, it is required that the blend has properties suitable for each application and has excellent appearance when molded. However, according to the study by the present inventors, when the compatibilizer described in Patent Document 1 is used, the toughness and appearance of the obtained molded article are insufficient, and further improvement is required.

[0006] An object of one aspect of the present invention is to provide a polymer blend which is excellent in flowability and can give a molded article having high toughness and excellent appearance. [Means for solving the problem]

[0007] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by using a copolymer having a specific structure in a polymer blend of a polyester resin and a polyolefin resin, and have achieved the present invention.

[0008] [1] A resin composition comprising: a polyolefin resin (A); a polyester resin (B); and a copolymer (C) of a carboxylic acid and / or a carboxylic acid derivative and an α-olefin, wherein a structural unit derived from the carboxylic acid and / or the carboxylic acid derivative is present in the main chain of the copolymer (C). [2] The resin composition according to [1], wherein the copolymer (C) is a copolymer containing the α-olefin having 21 or more carbon atoms. [3] The resin composition according to [1] or [2], wherein the carboxylic acid and / or carboxylic acid derivative is a dicarboxylic acid anhydride. [4] The resin composition according to any one of [1] to [3], wherein the acid value of the copolymer (C) is 15 mg·KOH / g or more and 200 mg·KOH / g or less. [5] The resin composition according to any one of [1] to [4], wherein the mass average molecular weight of the copolymer (C) is 5,000 or more and 200,000 or less. [6] The resin composition according to any one of [1] to [5], wherein the content of the copolymer (C) is 0.5 parts by mass or more and less than 5 parts by mass per 100 parts by mass of the polyolefin resin (A), the polyester resin (B), and the copolymer (C) combined. [7] The resin composition according to any one of [1] to [6], wherein the content of the polyolefin resin (A) is 1 part by mass or more and 95 parts by mass or less, and the content of the polyester resin (B) is 1 part by mass or more and 95 parts by mass or less, in a total of 100 parts by mass of the polyolefin resin (A), the polyester resin (B), and the copolymer (C). [8] The resin composition according to any one of [1] to [7], wherein the polyolefin resin (A) is a propylene-based polymer. [9] The resin composition according to any one of [1] to [8], wherein the polyester resin (B) is polyethylene terephthalate.

[10] A molded article comprising the resin composition according to any one of [1] to [9]. Effect of the Invention

[0009] According to one aspect of the present invention, it is possible to provide a resin composition containing a polyester resin and a polyolefin resin, which has excellent flowability, high toughness, and excellent appearance when formed into a molded article. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a diagram showing samples for appearance evaluation in the molded bodies according to the examples and the comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments as long as it does not deviate from the purpose. In this specification, "to" includes the lower limit and the upper limit. In addition, for each preferred range, the upper limit and the lower limit can be used in any combination.

[0012] <1.Resin composition> A resin composition according to one embodiment of the present invention contains a polyolefin resin (hereinafter, may be referred to as polyolefin resin (A)), a polyester resin (hereinafter, may be referred to as polyester resin (B)), and a copolymer of a carboxylic acid and / or a carboxylic acid derivative and an α-olefin, the copolymer having a structural unit derived from a carboxylic acid and / or a carboxylic acid derivative in the main chain (hereinafter, may be referred to as copolymer (C)).

[0013] In resin compositions of polymer blends of polyester resin and polyolefin resin, a compatibilizer may be used to improve the compatibility between the resins. As such a compatibilizer, it has been proposed to use a carboxylic acid-modified ethylene-α-olefin copolymer as described in JP-A-2001-106886. However, these polymer blends do not have sufficient toughness, such as tensile elongation at break or Charpy impact strength. In addition, molded articles of the above polymer blends may have so-called lumps due to poor dispersion of the polyester resin, and the appearance may need to be improved.

[0014] However, in one embodiment of the present invention, by using a copolymer (C) having a specific structure in the above polymer blend, it is possible to provide a molded article having high toughness and excellent appearance.

[0015] This is because, due to its structure, when the copolymer (C) is used in combination with a polymer blend of polyester resin (B) and polyolefin resin (A), the α-olefin chain penetrates into the amorphous part of the polyolefin resin (A) to maintain compatibility with the polyolefin resin. In addition, it is believed that the copolymer (C) has a carboxylic acid or a carboxylic acid derivative, which allows the copolymer (C) to react appropriately with the polyester resin (B) and impart a molecular structure that is easily compatible with the polyolefin resin (A). As a result, the resin composition according to one embodiment of the present invention can exhibit physical properties that combine the fluidity and rigidity of the polyester resin (B) and the toughness of the polyolefin resin (A) by promoting dispersion during mixing, and can obtain a molded product with excellent appearance.

[0016] Thus, according to one aspect of the present invention, when recycling waste of molded articles containing polyolefin resin (A) and polyester resin (B), a new resin composition and its molded article can be produced with high efficiency by minimizing the decrease in physical properties. Such an effect also contributes to the achievement of, for example, Goal 12 "Responsible Consumption and Production" of the Sustainable Development Goals (SDGs) advocated by the United Nations.

[0017] <1-1. Polyolefin resin (A)> As described above, the resin composition according to the present embodiment contains a polyolefin resin (A). In one aspect of the present invention, the "polyolefin resin (A)" is a resin in which the proportion of olefin units or cycloolefin units is 80 mol% or more relative to 100 mol% of all structural units constituting the resin, and which is different from the copolymer (C). In particular, the total proportion of olefin units and cycloolefin units relative to 100 mol% of all structural units constituting the polyolefin resin (A) is preferably 85 mol% or more, and particularly preferably 90 mol% or more.

[0018] Specific examples of the polyolefin resin (A) include homopolymers or copolymers of α-olefins, such as α-olefin polymers such as polyethylene, polypropylene, polybutene, poly(3-methyl-1-butene), poly(3-methyl-1-pentene), and poly(4-methyl-1-pentene); α-olefin copolymers such as ethylene-propylene block or random copolymers, α-olefin-propylene block or random copolymers having 4 or more carbon atoms, ethylene-methyl methacrylate copolymer, and ethylene-vinyl acetate copolymer; and cycloolefin polymers such as polycyclohexene and polycyclopentene.

[0019] Examples of polyethylene include low density polyethylene, linear low density polyethylene, and high density polyethylene. Examples of polypropylene include isotactic polypropylene, syndiotactic polypropylene, hemiisotactic polypropylene, and stereoblock polypropylene. In the α-olefin-propylene block or random copolymer having 4 or more carbon atoms, examples of the α-olefin having 4 or more carbon atoms include butene, 3-methyl-1-butene, 3-methyl-1-pentene, and 4-methyl-1-pentene. The resin composition may contain only one type of polyolefin resin (A), or two or more types. These may be unused polymers or recycled polymers after once being used.

[0020] Among the above, the polyolefin resin (A) is preferably polyethylene, polypropylene, or polybutene, and more preferably a propylene-based polymer such as polypropylene or block polypropylene.

[0021] The melt flow rate of the polyolefin resin (A) is not particularly limited, but in order to improve mechanical properties, it is preferably 0.1g / 10min or more, more preferably 0.2g / 10min or more, and particularly preferably 0.3g / 10min or more, while in order to improve processability, it is preferably 70g / 10min or less, more preferably 60g / 10min or less, particularly preferably 50g / 10min or less, extremely preferably 30g / 10min or less, particularly preferably 25g / 10min or less, very preferably 15g / 10min or less, extremely preferably 12.5g / 10min or less, and most preferably 10g / 10min or less. The melt flow rate of the polyolefin resin (A) can be calculated according to JIS K7210.

[0022] Commercially available polyolefin resins (A) include, for example, Novatec (registered trademark) MA3, Novatec MA3H, Novatec MA1B, Novatec EA9, Novatec EA9HD, Novatec EA9FTD, Novatec EA7AD, Novatec FY6H, Novatec EA6A, Novatec FY6, Novatec FY6C, Novatec FY4, and Novatec SA3A manufactured by Japan Polypropylene Corporation, and Prime Polypro (registered trademark) J105G, Prime Polypro J106G, Prime Polypro J106MG, and Prime Polypro manufactured by Prime Polymer Co., Ltd. 107G, Prime Polypro J137G, Prime Polypro J108M, Evolue (registered trademark) SP2320, Evolue SP2520, Evolue SP2510, Evolue SP3010, Evolue SP4020, Evolue SP1071C, Hi-Zex (registered trademark) 1300J, Hi-Zex 2100J, Hi-Zex 2100JH, Hi-Zex 2200J, Hi-Zex 2208J, Hi-Zex 3300F, Hi-Zex 3600F, Hi-Zex 7000F, Hi-Zex 8000F, Novatec LL manufactured by Japan Polyethylene Co., Ltd. UF420, Novatec LL UF421, Novatec LL UF621, Novatec LL UF524, Novatec LL UF622, Novatec LL UF230, Novatec LL UF320, Novatec LL UF332, Novatec LL UA421, Novatec LL UF240, Novatec LL UF442, Novatec LL UF641, Novatec LL UF943, Novatec LL UJ960, Novatec LL UJ370, Novatec LL UJ580, Novatec LL UJ480, Novatec LL UJ990, Novatec LL UJ790, Novatec LL UE320, Novatec LL UR951, Novatec C6 SF720, Novatec C6 SF941, Novatec C6 SF8402, Novatec HD HJ360, Novatec HD 362N, Novatec HD HJ560, Novatec HD HJ580N, Novatec HD HJ490, Novatec HD HJ590N, Novatec HD HY420, Novatec HD HY530, Novatec HD HY430, Novatec HD HY331, Novatec HD HY540, Novatec HD HE122R, Novatec HD HF313, Novatec HD HF111K, Novatec HD HF560, Novatec HD HE121, Novatec HD HE212W, Novatec HD HE421, Novatec HD HB420R, Novatec HD HB338RE, Novatec HD These include Novatec HD HB332E, Novatec HD HB432E, Novatec HD HB530, Novatec HD HB216R, and Novatec HDHB111R.

[0023] <1-2. Polyester resin (B)> The resin composition according to the present embodiment contains a polyester resin (B). Here, the polyester resin (B) is a polycondensation product of an aromatic or aliphatic dicarboxylic acid and a diol, and in the production, one kind of dicarboxylic acid and one kind of diol may be selected and produced under normal polycondensation conditions, or two or more kinds may be appropriately combined and produced.

[0024] Examples of dicarboxylic acids include terephthalic acid, isophthalic acid, adipic acid, sebacic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, and diphenyl ether-4,4'-dicarboxylic acid.

[0025] Examples of diols include ethylene glycol, propylene glycol, 1,4-butylene glycol, neopentyl glycol, cyclohexanedimethanol, 2,2-bis(4-hydroxyphenyl)propane, etc. In polycondensation, a hydroxycarboxylic acid such as p-hydroxybenzoic acid may be coexisted.

[0026] Representative examples of the polyester resin (B) produced from the dicarboxylic acid and diol include polyethylene terephthalate and polybutylene terephthalate. The polyester resin (B) may be a recycled product obtained by using a molded article of the polyester resin (B) once, or may be a mixture of a virgin product and a recycled product. The polyester resin (B) is preferably one having an intrinsic viscosity (IV) of 0.30 to 0.85 (dl / g) measured at 25°C in a phenol / tetrachloroethylene=50 / 50 (weight ratio) mixed solvent.

[0027] The intrinsic viscosity of the polyester resin (B) is preferably more than 0.30 (dl / g) and less than 0.85 (dl / g). If the intrinsic viscosity of the polyester resin (B) used is 0.30 (dl / g) or less, the moldability deteriorates due to low melt tension, and the mechanical properties of the molded body such as a film become unsatisfactory, which is not preferable. If the intrinsic viscosity of the polyester resin (B) used is 0.85 (dl / g) or more, the moldability deteriorates due to high melt viscosity.

[0028] <1-3. Copolymer (C)> The resin composition according to the present embodiment contains a copolymer (C) of a carboxylic acid and / or a carboxylic acid derivative and an α-olefin, the main chain of which contains a structural unit derived from a carboxylic acid and / or a carboxylic acid derivative. The copolymer (C) may contain other components such as a diene.

[0029] The carboxylic acid is not particularly limited, but examples thereof include (meth)acrylic acid, maleic acid, methylmaleic acid, fumaric acid, methylfumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, glutaconic acid, norbornane-5-ene-2,3-dicarboxylic acid, etc. Here, "(meth)acrylic acid" refers to acrylic acid or methacrylic acid.

[0030] The carboxylic acid derivative is not particularly limited, and examples thereof include carboxylic acid esters, carboxylic acid anhydrides, and carboxylic acid imides.

[0031] The carboxylic acid ester is not particularly limited, and examples thereof include ester compounds of the above-mentioned carboxylic acids, such as (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and glycidyl (meth)acrylate.

[0032] The carboxylic acid anhydride is not particularly limited, and examples thereof include anhydrides of the above-mentioned carboxylic acids. Preferred examples include dicarboxylic acid anhydrides such as maleic anhydride, itaconic anhydride, succinic anhydride, citraconic anhydride, and 5-norbornene-2,3-dicarboxylic anhydride.

[0033] The carboxylic acid imide is not particularly limited, and examples thereof include imide compounds of the above-mentioned carboxylic acids, such as maleimide compounds such as maleimide, N-ethylmaleimide, and N-phenylmaleimide.

[0034] As the carboxylic acid and / or carboxylic acid derivative, one kind may be used alone, or two or more kinds may be used in combination. Among the above, from the viewpoint of copolymerization reactivity, carboxylic acid ester or dicarboxylic acid anhydride is preferred, dicarboxylic acid anhydride is more preferred, and maleic anhydride is particularly preferred.

[0035] When maleic anhydride is selected as the carboxylic acid derivative, the copolymer (C) has the following general formula (1) as a constituent unit.

[0036] [ka]

[0037] In formula (1), at least one of R1, R2, R3, and R4 is independently an alkyl group having one or more carbon atoms, the others are hydrogen atoms, and x and y are independently an integer of 1 or more.

[0038] The method for producing the copolymer (C) is not particularly limited, and examples thereof include (1) a method of polymerizing an α-olefin and then adding a compound or monomer having a carboxylic acid and / or a carboxylic acid derivative, and (2) a method of copolymerizing an α-olefin with a compound or monomer having an acidic group. As the polymerization method, a radical polymerization method such as solution polymerization, emulsion polymerization, suspension polymerization, or bulk polymerization, or a living polymerization method can be adopted. Furthermore, a method in which a macromonomer is once formed and then polymerized can also be adopted. The above method (2) is preferred in that it is easy to obtain a copolymer (C) having a carboxylic acid and / or a carboxylic acid derivative in the main chain.

[0039] The total proportion of carboxylic acid and / or carboxylic acid derivative in 100 mol% of copolymer (C) is not particularly limited, but in order to improve the compatibility between polyester resin (B) and polyolefin resin (A), it is preferably 20 mol% or more, and more preferably 30 mol% or more, while in order to improve the appearance of the molded article, it is preferably 80 mol% or less, and more preferably 70 mol% or less.

[0040] Although there is no particular limitation on the α-olefin, the copolymer (C) preferably contains an α-olefin having 21 or more carbon atoms. When the copolymer (C) contains an α-olefin having 21 or more carbon atoms, it tends to have excellent compatibility with the polyolefin resin (A). In 100% by mass of α-olefin, the α-olefin having 21 or more carbon atoms is preferably contained in an amount of 0.5% by mass or more, more preferably 1% by mass or more, and particularly preferably 2% by mass or more.

[0041] Copolymer (C) more preferably contains an α-olefin having 21 or more carbon atoms, even more preferably contains an α-olefin having 24 or more carbon atoms, particularly preferably contains an α-olefin having 26 or more carbon atoms, and most preferably contains an α-olefin having 30 or more carbon atoms. On the other hand, in terms of dispersibility in resin, the number of carbon atoms of the α-olefin is preferably 150 or less, more preferably 130 or less, and particularly preferably 100 or less.

[0042] The copolymer (C) is dissolved in an organic solvent, and the solution is subjected to pyrolysis GC-MS (gas chromatography mass spectrometer, using a non-polar column), whereby the molecular weight of the copolymer (C) can be obtained, and the number of carbon atoms and the content of α-olefin can be calculated. An example of the organic solvent that dissolves the copolymer (C) is THF (tetrahydrofuran), but is not limited thereto.

[0043] The proportion of α-olefin units in 100 mol% of copolymer (C) is not particularly limited, but in order to improve the compatibility between polyester resin (B) and polyolefin resin (A), it is preferably 20 mol% or more, and more preferably 30 mol% or more, while in order to improve the appearance of molded articles, it is preferably 80 mol% or less, and more preferably 70 mol% or less.

[0044] In order to improve the appearance of the molded article, the acid value of the copolymer (C) is preferably 15 mg KOH / g or more, more preferably 31 mg KOH / g or more, more preferably 53 mg KOH / g or more, even more preferably 57 mg KOH / g or more, even more preferably 65 mg KOH / g or more, particularly preferably 80 mg KOH / g or more, and most preferably 85 mg KOH / g or more.

[0045] On the other hand, if the acid value of the copolymer (C) is too high, the copolymer (C) may react excessively with the polyester resin (B), making it difficult for the copolymer (C) to obtain suitable compatibility with the polyester resin (B) and the polyolefin resin (A). Therefore, the acid value is preferably 200 mg KOH / g or less, more preferably 140 mg KOH / g or less, even more preferably 135 mg KOH / g or less, and particularly preferably 130 mg KOH / g or less.

[0046] Determination of Acid Number: The acid value of copolymer (C) can be measured by titration. 2.0 g of copolymer (C) is dissolved in a solvent (a 3 / 7 mixture of ethanol / toluene) at 90°C. After cooling, three drops of phenolphthalein solution are added to the solution, which is then titrated with a 0.5 mol / L KOH ethanol solution. If copolymer (C) is insoluble in the solvent (a 3 / 7 mixture of ethanol / toluene), the acid value can be measured by FT-IR measurement. Copolymer (C) is heat pressed at 5 MPa for 5 minutes at or above its melting temperature to produce a molded product. FT-IR measurement is performed on this molded product, and an acid value of 1780 cm is obtained. -1 The modification rate of carboxylic acid and / or carboxylic acid derivatives is quantified based on the absorption of 11.44. The modification rate is multiplied by the coefficient 11.44 to calculate the acid value.

[0047] The mass average molecular weight of the copolymer (C) is not particularly limited, but is preferably 2,000 or more, more preferably 3,000 or more, and even more preferably 5,000 or more in order to improve impact resistance, while being preferably 1,000,000 or less, more preferably 750,000 or less, even more preferably 500,000 or less, and particularly preferably 250,000 or less. In addition, if the mass average molecular weight is too high, the dispersibility in the resin is deteriorated, so the mass average molecular weight is extremely preferably 200,000 or less, particularly preferably 100,000 or less, very preferably 50,000 or less, and most preferably 30,000 or less. The mass average molecular weight of the copolymer (C) may be, for example, 2,000 or more and 50,000 or less, 3,000 or more and 30,000 or less, or 5,000 or more and 200,000 or less. The mass average molecular weight of the copolymer (C) is a value calculated as standard polystyrene by dissolving the copolymer (C) in an organic solvent such as THF and measuring the resultant by gel permeation chromatography.

[0048] An example of a commercially available product of the copolymer (C) is Diacalna (registered trademark) 30M (manufactured by Mitsubishi Chemical Corporation).

[0049] <1-4. Composition of Resin Composition> In the resin composition, the content of polyester resin (B) in a total of 100 parts by mass of polyolefin resin (A) and polyester resin (B) is not particularly limited, but in order to improve the heat resistance of the obtained molded article, it is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 7.5 parts by mass or more, and particularly preferably 10 parts by mass or more; on the other hand, in order to reduce the weight of the obtained molded article, it is preferably 99 parts by mass or less, more preferably 95 parts by mass or less, even more preferably 92.5 parts by mass or less, and particularly preferably 90 parts by mass or less.

[0050] In the resin composition, the content of polyolefin resin (A) in a total of 100 parts by mass of polyolefin resin (A) and polyester resin (B) is not particularly limited, but in order to reduce the weight of the resulting molded article, it is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 7.5 parts by mass or more, and particularly preferably 10 parts by mass or more; on the other hand, in order to improve the heat resistance of the resulting molded article, it is preferably 99 parts by mass or less, more preferably 95 parts by mass or less, even more preferably 92.5 parts by mass or less, and particularly preferably 90 parts by mass or less.

[0051] In the resin composition, the content of copolymer (C) per 100 parts by mass of the total of polyolefin resin (A) and polyester resin (B) is not particularly limited, but in order to increase the affinity of polyolefin resin (A) and polyester resin (B) with other components described later, it is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and particularly preferably 0.5 parts by mass or more; on the other hand, in order to improve the appearance of the molded article, it is preferably 10 parts by mass or less, more preferably 7.5 parts by mass or less, and particularly preferably less than 5 parts by mass.

[0052] There is no particular limitation on the ratio of the total amount of polyolefin resin (A) and polyester resin (B) in 100 parts by mass of the resin composition, but in order to improve processability, it is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and particularly preferably 30 parts by mass or more, while in order to improve the appearance of the molded product, it is preferably 99.9 parts by mass or less, more preferably 99.8 parts by mass or less, and particularly preferably 99.7 parts by mass or less.

[0053] The resin composition may contain other components in addition to the polyester resin (B), the polyolefin resin (A), and the copolymer (C).

[0054] Examples of other components include fillers. In one embodiment of the present invention, the filler refers to a component that is added for the purpose of imparting mechanical strength, light reflection / scattering, flame retardancy, sound insulation, vibration damping, etc., and has a melting point equal to or higher than the processing temperature of the resin composition.

[0055] The filler is not particularly limited, but may be an inorganic filler or an organic filler.

[0056] There are no particular limitations on the inorganic filler, and examples thereof include glass fiber, glass beads, talc, barium sulfate, wollastonite, kaolin, finely powdered silica, mica, calcium silicate, aluminum oxide, and magnesium oxide.

[0057] There are no particular limitations on the organic filler, and examples thereof include wood powder, paper powder, cellulose fiber, and carbon fiber.

[0058] Among the above, the filler is preferably an inorganic filler, paper powder, or cellulose fiber, and more preferably a glass filler such as glass beads, paper powder, or cellulose fiber.

[0059] When the resin composition contains a filler, the proportion thereof is not particularly limited, but from the viewpoint of mechanical strength, the proportion is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and particularly preferably 20 parts by mass or more, relative to 100 parts by mass of the resin composition; on the other hand, from the viewpoint of moldability, the proportion is preferably 70 parts by mass or less, more preferably 60 parts by mass or less, and particularly preferably 50 parts by mass or less.

[0060] In addition, examples of other components other than the filler include other resins other than the polyolefin resin (A) and the polyester resin (B), flame retardants (phosphorus-based, bromine-based, silicone-based, organic metal salt-based, etc.), anti-drip agents (e.g., fluorinated polyolefin, silicone, and aramid fiber), lubricants (e.g., long-chain fatty acid metal salts such as magnesium stearate, etc.), release agents (e.g., pentaerythritol tetrastearate, etc.), nucleating agents, antistatic agents, stabilizers (e.g., phenol-based stabilizers, sulfur-based stabilizers, phosphorus-based stabilizers, ultraviolet absorbers, amine-based light stabilizers, etc.), plasticizers, dyes, pigments, etc. In addition, these other components can be well-known materials, and can be arbitrarily selected and used according to the application of the resin composition, and each other component in the resin composition can also be arbitrarily selected.

[0061] The proportion of other components in 100 parts by mass of the resin composition is not particularly limited, but is usually 0.1 parts by mass or more, and preferably 60 parts by mass or less, and more preferably 50 parts by mass or less.

[0062] Any method can be used to produce the resin composition. For example, the polyolefin resin (A), the polyester resin (B), the copolymer (C), and other components as necessary are thoroughly mixed using a premixing means such as a V-type blender, a Henschel mixer, a mechanochemical device, or an extrusion mixer, and optionally granulated using an extrusion granulator or a briquetting machine, and then melt-kneaded and extruded using a melt mixer.

[0063] Examples of the melt kneader include twin-screw extruders such as vented twin-screw extruders, Banbury mixers, kneading rolls, single-screw extruders, and multi-screw extruders having three or more screws. The temperature during melt kneading is, for example, 200 to 320° C. The resin composition extruded as described above is directly cut and pelletized by a device such as a pelletizer, or cooled to form strands, and then the strands are cut and pelletized by a device such as a pelletizer.

[0064] <2. Molded body> A molded article can be obtained by molding the resin composition according to one embodiment of the present invention. Examples of applications of the resin composition include molded articles obtained by recycling automobile, motorcycle, and ship parts, electrical and electronic parts, miscellaneous goods, fibers, films, and molded articles, and molded articles useful in other fields.

[0065] The molded article contains the resin composition. That is, the molded article contains the polyolefin resin (A), the polyester resin (B), and the copolymer (C). The preferred ratio of each component in the molded article is the same as the preferred ratio described in the above-mentioned resin composition. The shape of the molded article is not particularly limited, and may be various shapes such as a resin plate, a sheet, a film, a cable, a fiber, or an irregular shape.

[0066] The film and sheet obtained from the resin composition according to one embodiment of the present invention may be laminated with two or more other substrates, such as polyolefins such as polyethylene or polypropylene, polyvinyl chloride, polyamide, ethylene-vinyl alcohol copolymer, aluminum foil, paper, etc., depending on the application.

[0067] The fiber obtained from the resin composition according to one embodiment of the present invention may have two or more layers with other substrates such as polyolefins such as polyethylene or polypropylene, polyvinyl chloride, polyamide, ethylene-vinyl alcohol copolymer, polyester, etc., depending on the application.

[0068] The molding method for obtaining the molded product is not particularly limited, and examples thereof include extrusion processing, calendar processing, injection molding, rolling, compression molding, blow molding, etc. The temperature when molding the resin composition according to one embodiment of the present invention is, for example, 200 to 320°C. EXAMPLES

[0069] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the following examples. In the following examples, % is by weight unless otherwise specified.

[0070] [Examples 1 to 10, Comparative Examples 1 to 11] The raw materials were blended in the ratios shown in Tables 1 and 2 and mixed by hand blending. Then, using a φ30 mm counter-rotating twin screw extruder (model name "PCM-30", manufactured by Ikegai Corporation), the mixture was melt-kneaded at a screw rotation speed of 150 rpm and a cylinder temperature of 250 to 270°C to obtain a resin composition. Using pellets of the obtained resin composition, the MFR (melt mass flow rate) or MVR (melt volume rate) was measured at a temperature of 270°C and a load of 21.2 N.

[0071] The details of each raw material shown in Tables 1 and 2 are as follows.

[0072] (Polyolefin resin (A-1)) Polypropylene resin (Japan Polypropylene Corporation, Novatec PP МA1B, melt mass flow rate 21.0g / 10min) (Polyolefin resin (A-2)) Polypropylene resin (Japan Polypropylene Corporation, Novatec PP FY-4, melt mass flow rate 5.0g / 10min)

[0073] (Polyester resin (B-1)) Polyethylene terephthalate resin (Bellpet (registered trademark) EFG70, manufactured by Bell Polyester Products Co., Ltd., intrinsic viscosity (IV) = 0.75 dl / g)

[0074] (Copolymer (C-1)) Diacaluna 30M (manufactured by Mitsubishi Chemical Corporation, copolymer of α-olefin and maleic anhydride, acid value 80 mg KOH / g, mass average molecular weight 10,000) (Copolymer (C-2)) UMEX (registered trademark) 1010 (Sanyo Chemical Industries, Ltd., maleic anhydride modified polyolefin, acid value 52 mg KOH / g, mass average molecular weight 30,000) (Copolymer (C-3)) Modic (registered trademark) P908 (manufactured by Mitsubishi Chemical Corporation, maleic anhydride modified polyolefin, acid value 10 mg KOH / g, mass average molecular weight 150,000)

[0075] The copolymer (C-1) is a copolymer containing at least 0.5% by mass of an α-olefin having 21 to 100 carbon atoms, based on 100% by mass of the contained α-olefins.

[0076] The obtained resin composition was injection molded using a 100t injection molding machine (model name "SE-100DU", manufactured by Sumitomo Heavy Industries, Ltd.) under the condition of a molding temperature of 250 to 270°C to obtain molded bodies (Charpy impact strength test pieces) of length 80 mm x width 10 mm x thickness 4 mm, tensile test pieces specified in JIS-7139, and flat plates of length 100 mm x width 50 mm x thickness 2 mm. The molded bodies were used to carry out the evaluations described below. The obtained results are shown in Tables 1 and 2. In Tables 1 and 2, items marked with "-" indicate that they were not measured or evaluated.

[0077] [Charpy impact test] Measurements were made in accordance with ISO-179-1 and with a TYPE A notch in accordance with ISO2818.

[0078] [Tensile test] The test was performed in accordance with ISO-527, and the tensile speed was set to 5 mm / min.

[0079] [Appearance evaluation] The resulting molded product (a flat plate with a thickness of 2 mm) was irradiated with light from the back, and the presence of color unevenness, as shown in FIG. 1, was judged as "unacceptable," and the absence of color unevenness was judged as "acceptable."

[0080] [Transmittance] The transmittance of the obtained molded product (a flat plate having a thickness of 2 mm) was measured in accordance with JIS K-7361.

[0081] [Table 1]

[0082] [Table 2]

[0083] As can be seen by comparing Examples 1-2 with Comparative Examples 1-2, and Example 3 with Comparative Example 7, in a resin composition containing a polyolefin resin and a polyester resin, by using a copolymer (C-1) which is a copolymer of a carboxylic acid and / or a carboxylic acid derivative and an α-olefin and has a structural unit derived from a carboxylic acid and / or a carboxylic acid derivative in the main chain, the toughness represented by the tensile elongation at break and the Charpy impact strength was greatly improved. The flowability represented by MVR and MFR was also improved, and a molded product with high total light transmittance and excellent appearance without color unevenness was obtained.

[0084] In addition, as can be seen by comparing Examples 1-2 with Comparative Examples 3-6, and Example 3 with Comparative Examples 8-9, in a resin composition containing a polyolefin resin and a polyester resin, when a polymer having a carboxylic acid and / or a carboxylic acid derivative in a graft chain rather than in a main chain, such as copolymer (C-2) or (C-3), is used in combination, the toughness and fluidity represented by tensile elongation at break and Charpy impact strength are insufficient, and the total light transmittance is also reduced, so that the appearance of the molded article is also insufficient. In contrast, when copolymer (C-1) having a carboxylic acid and / or a carboxylic acid derivative in the main chain is used in combination, it was confirmed that the toughness represented by tensile elongation at break and Charpy impact strength is significantly improved, the total light transmittance is high, and the appearance of the molded article is also excellent. [Industrial Applicability]

[0085] In the resin composition according to one aspect of the present invention, the polyester resin and the polyolefin resin are compatible with each other and have excellent flowability. By using such a resin composition, a molded article having high toughness and excellent appearance can be obtained.

[0086] The molded article obtained by using the resin composition according to one embodiment of the present invention can be suitably used as a molded article obtained by recycling automobile, motorcycle, and ship parts, electric and electronic parts, miscellaneous goods, fibers, films, molded articles, and the like, and a molded article useful in other fields.

Claims

1. A polyolefin resin (A), A polyester resin (B), (C) a copolymer of a carboxylic acid and / or a carboxylic acid derivative and an α-olefin, A resin composition, wherein the structural unit derived from the carboxylic acid and / or a carboxylic acid derivative is present in the main chain of the copolymer (C).

2. The resin composition according to claim 1, wherein the copolymer (C) is a copolymer containing the α-olefin having 21 or more carbon atoms.

3. The resin composition according to claim 1 , wherein the carboxylic acid and / or carboxylic acid derivative is a dicarboxylic acid anhydride.

4. The resin composition according to claim 1, wherein the acid value of the copolymer (C) is 15 mg·KOH / g or more and 200 mg·KOH / g or less.

5. The resin composition according to claim 1, wherein the mass average molecular weight of the copolymer (C) is 5,000 or more and 200,000 or less.

6. 2. The resin composition according to claim 1, wherein the content of the copolymer (C) in a total of 100 parts by mass of the polyolefin resin (A), the polyester resin (B), and the copolymer (C) is 0.5 parts by mass or more and less than 5 parts by mass.

7. The content of the polyolefin resin (A) is 1 part by mass or more and 95 parts by mass or less, and the content of the polyester resin (B) is 1 part by mass or more and 95 parts by mass or less, in a total of 100 parts by mass of the polyolefin resin (A), the polyester resin (B), and the copolymer (C). The resin composition according to claim 1, wherein the content of the polyolefin resin (A) is 1 part by mass or more and 95 parts by mass or less.

8. The resin composition according to claim 1 , wherein the polyolefin resin (A) is a propylene-based polymer.

9. The resin composition according to claim 1 , wherein the polyester resin (B) is polyethylene terephthalate.

10. A molded article comprising the resin composition according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Polyester polymer alloy

    JP2001106886A