Thermosetting composition, sheet-like cured product, composite molding, and semiconductor device
The thermosetting composition with high inorganic filler content and specific epoxy compounds addresses the challenge of maintaining thermal conductivity and bending resistance, facilitating stable production and use in power semiconductor devices.
Patent Information
- Application Number
- JP2024046093
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-07
AI Technical Summary
Conventional thermosetting compositions face challenges in maintaining bending resistance while increasing thermal conductivity, leading to issues such as cracking during mass production when wound into rolls, particularly when using boron nitride aggregate particles as inorganic fillers.
A thermosetting composition with a high inorganic filler content of 60% by mass, containing specific epoxy compounds and boron nitride agglomerated particles with a card house structure, along with a controlled epoxy equivalent and molecular weight, ensures both high thermal conductivity and bending resistance.
The composition achieves thermal conductivity of 15 W/m·K or more in the thickness direction with bending resistance of φ<20 mm, enabling stable production and application in power semiconductor devices.
Smart Images

Figure 2024137893000010 
Figure 2024137893000001 
Figure 2024137893000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting composition having thermosetting properties, for example, a thermosetting composition whose cured product can be suitably used as a heat sink for a power semiconductor device, and to a sheet-shaped cured product, a composite molded product, and a semiconductor device using the thermosetting composition. [Background technology]
[0002] Among devices that use semiconductors, those that control and convert power from power sources and the like are called "power semiconductor devices." Power semiconductor devices are generally configured as a power module (semiconductor module) in which a power semiconductor device (semiconductor device) that converts and controls electric power and electronic components are mounted on a substrate that functions as a heat sink. In recent years, power semiconductor devices used in various fields such as railways, automobiles, industry, and general home appliances are being shifted from conventional Si power semiconductors to power semiconductors using SiC, AlN, GaN, etc. in order to achieve further miniaturization, cost reduction, and efficiency improvement.
[0003] Various issues have been pointed out for the practical application of such power semiconductor devices, one of which is the issue of heat generation from the devices. While power semiconductor devices can achieve high output and high density by operating at high temperatures, there are concerns that heat generated by device switching and other operations will reduce the reliability of the power semiconductor devices.
[0004] In recent years, heat generation due to the high density of integrated circuits has become a major problem in the electrical and electronic fields, and how to dissipate heat has become an urgent issue. For example, when semiconductor devices used to control the central processing unit of a personal computer or the motor of an electric vehicle operate stably, heat sinks, heat dissipation fins, etc. are indispensable for dissipating heat, and there is a demand for materials that can achieve both thermal conductivity and insulation as materials for connecting semiconductor devices to heat sinks, etc.
[0005] Ceramic substrates with high thermal conductivity, such as alumina substrates and aluminum nitride substrates, have traditionally been used as materials that can provide both thermal conductivity and insulation, but ceramic substrates have issues such as being easily cracked when subjected to impact, and being difficult to make thin and compact.
[0006] In order to solve the problems with ceramic substrates, many studies have been conducted on heat dissipation sheets with good thermal conductivity and excellent insulation. In particular, attempts have been made to obtain heat dissipation resin sheets that satisfy high levels of thermal conductivity and insulation by mixing fillers into resins. Various oxides and nitrides are used as fillers contained in such heat dissipation resin sheets, and many studies have been conducted on them (for example, Patent Document 1).
[0007] Attempts have been made to use hexagonal boron nitride as a filler in heat dissipation sheets. Hexagonal boron nitride is generally a thin plate crystal, and the thermal conductivity in the planar direction of the thin plate is high, but the thermal conductivity in the thickness direction of the thin plate is low. In addition, when thin plate-shaped boron nitride is mixed into a heat dissipation sheet, it is oriented parallel to the sheet surface when it is made into a sheet, so the thermal conductivity in the thickness direction of the sheet is never good.
[0008] Agglomerated boron nitride filler is one example of a material that increases the thermal conductivity in the thickness direction of a sheet. It is widely known that the use of agglomerated boron nitride filler can improve the thermal conductivity in the thickness direction of a sheet. In particular, the present applicant has previously developed a card-house structure agglomerated boron nitride filler (see, for example, Patent Document 2). Furthermore, they developed an agglomerated boron nitride filler that has a relatively large average particle size and a house-of-cards structure that is less likely to collapse even when pressure is applied (see, for example, Patent Document 3).
[0009] These agglomerated boron nitride fillers ensure a thermal conduction path due to their card-house structure, and by incorporating them into a heat dissipation sheet, the sheet has excellent thermal conductivity in the thickness direction. Furthermore, agglomerated boron nitride fillers are formed by agglomerating boron nitride particles without using a separate binder. Therefore, even if an external force is applied when forming the sheet, the card-house structure does not easily collapse, maintaining the thermal conduction path, allowing heat to be dissipated in the thickness direction of the sheet, and achieving excellent thermal conductivity (see, for example, Patent Documents 4 and 5). As a molding method for increasing the thermal conductivity in the thickness direction of a sheet, a method is known in which aggregated boron nitride fillers in a sheet are brought into surface contact with each other to increase the thermal conductivity (see, for example, Patent Document 6).
[0010] The applicant has also proposed a resin composition containing an inorganic filler and a thermosetting resin, the inorganic filler content being 50 vol% or more of the solid content of the resin composition, the boron nitride filler (A) being 82 vol% or more of the inorganic filler, the boron nitride filler including an aggregated filler, the thermosetting resin containing an epoxy resin having a mass average molecular weight of 5000 or more, the epoxy equivalent (WPE) of the resin component in the resin composition being 100≦WPE≦300, and the storage modulus E' of a cured product of the resin composition being 1≧(E' at 270°C) / (E' at 30°C)≧0.2 (Patent Document 7). [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2013-089670 A [Patent Document 2] JP 2015-006985 A [Patent Document 3] JP 2016-135730 A [Patent Document 4] International Publication No. 2015 / 119198 [Patent Document 5] JP 2017-036415 A [Patent Document 6] International Publication No. 2019 / 189746 [Patent Document 7] International Publication No. 2022 / 210686 Summary of the Invention [Problem to be solved by the invention]
[0012] The present inventors have found that, with regard to a thermosetting composition containing an inorganic filler and a thermosetting compound, when the inorganic filler content of a conventional composition is increased in order to increase the thermal conductivity after curing, the flexibility of the sheet before curing deteriorates, and the sheet may crack when wound into a roll during the mass-production process. As described above, a thermosetting composition containing an inorganic filler and a thermosetting compound has a problem in that it is difficult to ensure bending resistance while increasing thermal conductivity after curing. This problem also occurs when agglomerated particles of boron nitride are used as the inorganic filler.
[0013] Therefore, an object of the present invention is to provide a thermosetting composition that can increase thermal conductivity while ensuring bending resistance, as well as a sheet-like cured product, a composite molded product, and a semiconductor device using the thermosetting composition. [Means for solving the problem]
[0014] In order to solve the above problems, the present invention proposes a thermosetting composition, a sheet-like cured product, a composite molded article, and a semiconductor device according to the following aspects.
[0015] [1] A first aspect of the present invention is a thermosetting composition comprising an inorganic filler and a thermosetting compound, The content of the inorganic filler is 60% by mass or more relative to 100% by mass of the solid content in the thermosetting composition, The thermosetting compound includes an epoxy compound, The epoxy equivalent (WPE) of the component excluding the solvent and the inorganic filler from the thermosetting composition (referred to as the "resin component") is WPE≦250 g / eq; The thermosetting composition has a bending resistance φ of φ<20 mm, as determined by a mandrel test (JIS K5600-5-1) before curing.
[0016] [2] A second aspect of the present invention is a thermosetting composition according to the first aspect, wherein the resin component contains a polymeric epoxy compound (referred to as an "epoxy polymer") having a mass average molecular weight (Mw) of 5,000 or more in an amount of 5% by mass or more and 19% by mass or less.
[0017] [3] A third aspect of the present invention is a thermosetting composition according to the second aspect, wherein the epoxy polymer has a chemical structure represented by the following formula (1) and / or (2):
[0018] TIFF2024137893000001.tif69170
[0019] In formula (1), R 1 and R 2 Each of R represents an organic group, and at least one of them is an organic group having a molecular weight of 16 or more. 3 represents a divalent cyclic organic group.
[0020] [4] A fourth aspect of the present invention is a thermosetting composition according to the second or third aspect, wherein the epoxy polymer has a chemical structure represented by the following formula (3):
[0021] TIFF2024137893000002.tif40170
[0022] In formula (3), R 4 , R 5 , R 6 , R 7 represents an organic group having a molecular weight of 15 or more.
[0023] [5] A fifth aspect of the present invention is the thermosetting composition according to any one of the first to fourth aspects, wherein the thermal conductivity in the thickness direction after curing is 15 W / m·K or more.
[0024] [6] A sixth aspect of the present invention is a thermosetting composition according to any one of the first to fifth aspects, which contains a polyfunctional epoxy compound having three or more epoxy groups in one molecule. [7] A seventh aspect of the present invention is the thermosetting composition of the sixth aspect, wherein the multifunctional epoxy compound having three or more epoxy groups in one molecule has a mass average molecular weight (Mw) of 800 or less. [8] An eighth aspect of the present invention is the thermosetting composition according to the sixth or seventh aspect, wherein the epoxy equivalent of the multifunctional epoxy compound having three or more epoxy groups in one molecule is 50 g / equivalent or more and 200 g / equivalent or less. [9] A ninth aspect of the present invention is a thermosetting composition comprising a polyfunctional epoxy compound having four epoxy groups in one molecule in any one of the first to eighth aspects, i.e., a polyfunctional epoxy compound having four epoxy groups in one molecule as the polyfunctional epoxy compound in any one of the sixth to eighth aspects.
[10] A tenth aspect of the present invention is the thermosetting composition according to any one of the sixth to ninth aspects, wherein the content of the polyfunctional epoxy compound having three or more epoxy groups in one molecule is from 5 mass % to 50 mass % relative to 100 mass % of the solid content in the thermosetting composition excluding the inorganic filler.
[0025]
[11] An eleventh aspect of the present invention is a thermosetting composition according to any one of the first to tenth aspects, comprising a compound having a heterocyclic structure containing a nitrogen atom.
[12] A twelfth aspect of the present invention is the thermosetting composition according to any one of the first to eleventh aspects, wherein the inorganic filler is agglomerated particles of boron nitride.
[13] A thirteenth aspect of the present invention is the thermosetting composition of the twelfth aspect, wherein the boron nitride agglomerated particles have a house-of-cards structure.
[0026]
[14] A fourteenth aspect of the present invention is a sheet-shaped cured product made of the thermosetting composition according to any one of the first to thirteenth aspects.
[15] A fifteenth aspect of the present invention is a composite molded product having a cured product part made of the sheet-like cured product of the fourteenth aspect and a metal part.
[16] A sixteenth aspect of the present invention is a semiconductor device having the composite compact of the fifteenth aspect. Effect of the Invention
[0027] The thermosetting composition proposed by the present invention can increase the thermal conductivity by making the content of inorganic filler 60 mass% or more. And, even if the content of inorganic filler is increased in this way, the thermosetting composition proposed by the present invention can obtain bending resistance, and for example, can eliminate problems such as cracking when wound into a roll in a sheet form. Therefore, a sheet-shaped thermosetting composition that can exhibit excellent thermal conductivity after curing can be mass-produced industrially. [Brief description of the drawings]
[0028] [Figure 1] FIG. 2 is a conceptual diagram of a particle cross-section according to an example of a boron nitride agglomerated particle having a house-of-card structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] An embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below, and various modifications can be made within the scope of the present invention.
[0030] <<The composition>> A composition according to an embodiment of the present invention (hereinafter referred to as "the composition") is a thermosetting composition containing a thermosetting compound and an inorganic filler.
[0031] In the present invention, the term "thermosetting composition" refers to a composition containing a compound or resin having the property of being cured by heat. That is, it is sufficient if the composition has a curing property that allows room for curing by heat, and may be one that has already been cured to a state where room for curing remains (also referred to as "temporarily cured"), or one that has not yet been cured at all (referred to as "uncured"). The present composition may be in any form, such as a powder, a slurry, a liquid, a solid, or a molded product such as a sheet. Therefore, the present composition also includes, for example, a thermosetting composition in a slurry form to be subjected to the coating step described below, a sheet that has been subjected to the coating step, a sheet that has been subjected to steps such as coating and drying, and the like.
[0032] The present composition can be cured by heating (also referred to as "cured product"). In addition, the present composition can be formed into a sheet-like thermosetting composition (also referred to as a "thermosetting sheet") by forming it into a sheet, and a sheet having thermal conductivity (referred to as the present thermally conductive sheet) can be formed by curing the thermosetting sheet. In other words, the present thermally conductive sheet is a cured product of the thermosetting sheet.
[0033] (Bending resistance) The present composition has a bending resistance φ before curing in a mandrel test (JIS K5600-5-1), i.e., in a mandrel test in accordance with JIS K5600-5-1, which is φ<20 mm, and one of its features is that it has this bending resistance. As long as the bending resistance φ of the present composition is within this range, even if the inorganic filler content is increased to increase the thermal conductivity, for example, if the inorganic filler content is set to 60 mass % or more relative to 100 mass % of the solid content in the present composition, bending resistance can be obtained, and problems such as cracking when the composition is made into a sheet and wound into a roll can be eliminated. From this viewpoint, the bending resistance φ of the present composition before curing, as determined by a mandrel test (JIS K5600-5-1), is preferably φ<20 mm, more preferably φ<19 mm, and even more preferably φ<16 mm.
[0034] In order to make the bending resistance φ of the present composition φ<20 mm, for example, methods such as adjusting the epoxy equivalent of the resin component or adjusting the content of the epoxy polymer described below can be mentioned, but the methods are not limited to these.
[0035] (Thermal Conductivity) One of the characteristics of this composition is that it can provide a cured product with a thermal conductivity in the thickness direction of 15 W / m K or more at 25°C. When the thermal conductivity in the thickness direction is within the above range, the material can be suitably used in power semiconductor devices that operate at high temperatures. From this viewpoint, the thermal conductivity in the thickness direction at 25°C of the cured product obtained by curing the composition is preferably 15 W / m·K or more, more preferably 15.5 W / m·K or more, more preferably 16 W / m·K or more, more preferably 16.5 W / m·K or more, more preferably 17 W / m·K or more, more preferably 17.5 W / m·K or more, and even more preferably 18 W / m·K or more.
[0036] The thermal conductivity can be adjusted by the type of thermosetting compound, the type and content of inorganic filler, the method of mixing the thermosetting compound and the inorganic filler, the conditions in the heating and kneading step described below, etc. Among them, by adjusting the content of the inorganic filler, particularly the boron nitride agglomerated particles, it is possible to secure a necessary and sufficient heat conduction path in the thickness direction, and the thermal conductivity can be adjusted. The thermal conductivity of the cured product in the thickness direction can be measured by the following method. For example, the thermal conductivity can be determined from the slope of a graph obtained by plotting thermal resistance against thickness using a thermal resistance measuring device (manufactured by Mentor Graphics Corporation, product name "T3ster").
[0037] (Storage modulus E') The composition can have a storage modulus E' at 30° C. after curing of 10,000 to 100,000 MPa. When the storage modulus E' at 30° C. of the cured product is within the above range, the effect of improving durability in reliability tests can be obtained. From this viewpoint, the storage modulus E' at 30°C of the cured product of the composition is preferably 10,000 MPa or more, more preferably 15,000 MPa or more, and preferably 100,000 MPa or less, more preferably 90,000 MPa or less, and even more preferably 80,000 MPa or less.
[0038] The composition can have a storage modulus E' at 200° C. after curing of 1,000 to 50,000 MPa. When the storage modulus E' at 200° C. of the cured product is within the above range, the effect of improving durability can be obtained even in reliability tests. From this viewpoint, the storage modulus E' at 200°C of the cured product of the composition is preferably 1,000 MPa or more, more preferably 2,000 MPa or more, even more preferably 3,000 MPa or more, even more preferably 4,500 MPa or more, even more preferably 5,500 MPa or more, and on the other hand, it is preferably 50,000 MPa or less, more preferably 45,000 MPa or less, even more preferably 40,000 MPa or less.
[0039] In the present composition, the storage modulus E' at 30°C or 200°C after curing can be adjusted to fall within the above range by, for example, adjusting the epoxy equivalent of the resin component, adjusting the amount of multifunctional epoxy, or adjusting the ratio of the polymer and monomer components, but is not limited to these methods. The storage modulus E' at 30°C or 200°C after curing can be measured by laminating sheets of the composition, adjusting the sample thickness to 0.1 to 1.0 mm, heating and curing the sheet, cutting the cured product into strips 4 mm wide, and subjecting the resultant to a dynamic viscoelasticity test in a tensile mode.
[0040] <Resin component> The epoxy equivalent (WPE) of the component of the present composition excluding the solvent and inorganic filler (referred to as the "resin component"), in other words, the solid content of the present composition excluding the inorganic filler, is preferably WPE≦250 g / eq. The solid content of the present composition means the components excluding the solvent from the present composition. By adjusting the epoxy equivalent (WPE) of the resin component of the present composition within the above range, the ratio of the polymer and monomer components can be adjusted, the flexibility of the present composition can be adjusted, and bending resistance can be increased. From this viewpoint, the epoxy equivalent weight (WPE) of the resin component of the present composition is preferably 250 g / equivalent or less, more preferably 245 g / equivalent or less, even more preferably 240 g / equivalent or less, even more preferably 235 g / equivalent or less, and even more preferably 230 g / equivalent or less. On the other hand, from the viewpoint of ensuring the toughness of the uncured sheet, the epoxy equivalent (WPE) of the resin component of the composition is preferably 100 g / equivalent or more, more preferably 110 g / equivalent or more, even more preferably 120 g / equivalent or more, even more preferably 150 g / equivalent or more, and even more preferably 180 g / equivalent or more. Furthermore, by adjusting the epoxy equivalent (WPE) of the resin component of the present composition within the above range, the retention force of the inorganic filler can be adjusted, and the thermal conductivity of the sheet can be improved.
[0041] In order to adjust the epoxy equivalent (WPE) of the resin component of the present composition to the above range, a method of adjusting the content ratio of an epoxy compound having a predetermined epoxy equivalent, such as an epoxy polymer and a polyfunctional epoxy compound, can be mentioned, but is not limited to these methods.
[0042] Furthermore, the resin composition obtained by removing the inorganic filler from the present composition has a storage modulus of 100 MPa or more and 1000 MPa or less after curing at 200° C. When the storage modulus E' of the cured product at 200° C. is within the above range, the effect of improving durability can be obtained even in a reliability test. From this viewpoint, the storage modulus E' at 200°C of the cured product of the resin composition excluding the inorganic filler from the present composition is preferably 100 MPa or more, more preferably 110 MPa or more, even more preferably 120 MPa or more, even more preferably 130 MPa or more, and on the other hand, it is preferably 1,000 MPa or less, more preferably 900 MPa or less, even more preferably 800 MPa or less.
[0043] <Thermosetting compounds> Examples of the thermosetting compound contained in the present composition include epoxy compounds, phenolic resins, polycarbonate resins, unsaturated polyester resins, urethane resins, melamine resins, urea resins, and benzoxazine compounds.
[0044] The content of the thermosetting compound is preferably 5 to 40% by mass relative to 100% by mass of the volatile components in the present composition, that is, the components excluding the solvent (referred to as the "solids content"). If the content of the thermosetting compound is 5% by mass or more, it is preferable because the moldability is good, while if it is 40% by mass or less, it is preferable because the content of other components can be secured and thermal conductivity can be increased. From this viewpoint, the content of the thermosetting compound is preferably 5 to 40 mass% relative to 100 mass% of the solid content in the composition, more preferably 10 mass% or more, even more preferably 20 mass% or more, and even more preferably 25 mass% or more, while it is even more preferably contained in a proportion of 40 mass% or less.
[0045] (Epoxy compounds) The composition preferably contains an epoxy compound as the thermosetting compound.
[0046] Of the thermosetting compounds contained in the present composition, the epoxy compounds preferably account for 30 to 100 mass%, and more preferably 40 mass% or more, of which 50 mass% or more, of which 60 mass% or more, and of which 70 mass% or more are epoxy compounds. The epoxy compound in this case also includes the epoxy polymer described below.
[0047] The epoxy compound as the thermosetting compound contained in the present composition may be any compound having one or more oxirane rings (epoxy groups) in one molecule.
[0048] The oxirane ring (epoxy group) contained in the epoxy compound may be either an alicyclic epoxy group or a glycidyl group, and is more preferably a glycidyl group from the viewpoint of reaction rate or heat resistance.
[0049] Examples of the epoxy compound include an epoxy group-containing silicon compound, an aliphatic epoxy compound, a bisphenol A or F type epoxy compound, a novolac type epoxy compound, an aromatic epoxy compound, an alicyclic epoxy compound, a glycidyl ester type epoxy compound, a polyfunctional epoxy compound, and a polymer type epoxy compound.
[0050] The epoxy compound may be an aromatic oxirane ring (epoxy group)-containing compound.Specific examples thereof include bisphenol-type epoxy compounds obtained by glycidylating bisphenols such as bisphenol A, bisphenol F, bisphenol AD, bisphenol S, tetramethyl bisphenol A, tetramethyl bisphenol F, tetramethyl bisphenol AD, tetramethyl bisphenol S, and tetrafluorobisphenol A, biphenyl-type epoxy compounds, dihydroxynaphthalene, 9,9-bis(4-hydroxyphenyl)fluorene, and other divalent phenols, glycidylating trisphenols such as 1,1,1-tris(4-hydroxyphenyl)methane, and other epoxy compounds obtained by glycidylating tetrakisphenols such as 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, and other novolac-type epoxy compounds obtained by glycidylating novolacs such as phenol novolac, cresol novolac, bisphenol A novolac, and brominated bisphenol A novolac, and epoxy compounds having a dicyclopentadiene skeleton and epoxy compounds having a naphthalene skeleton. Among these, it is preferable to contain an epoxy compound having at least one structure selected from an epoxy compound having a biphenyl skeleton, an epoxy compound having a dicyclopentadiene skeleton, and an epoxy compound having a naphthalene skeleton.
[0051] (Epoxy Polymer) From the viewpoint of ensuring the film-forming properties of the sheet, the present composition preferably contains a high molecular weight epoxy compound (referred to as an "epoxy polymer") having a mass average molecular weight (Mw) of 5,000 or more.
[0052] Examples of the epoxy polymer include phenoxy resins having at least one skeleton selected from the group consisting of a bisphenol A type skeleton, a bisphenol F type skeleton, a bisphenol A / F mixed type skeleton, a naphthalene skeleton, a fluorene skeleton, a biphenyl skeleton, anthracene skeleton, a pyrene skeleton, a xanthene skeleton, an adamantane skeleton, and a dicyclopentadiene skeleton.
[0053] Among them, the epoxy polymer is preferably an epoxy polymer having at least one structure selected from a structure represented by the following formula (1) (also referred to as "structure (1)") and a structure represented by the following formula (2) (also referred to as "structure (2)"):
[0054] TIFF2024137893000003.tif69170
[0055] In formula (1), R 1 and R 2 Each of R represents an organic group, at least one of which is an organic group having a molecular weight of 16 or more. 3 represents a divalent cyclic organic group. The term "organic group" includes any group containing carbon atoms, and specific examples thereof include alkyl groups, alkenyl groups, and aryl groups, which may be substituted with halogen atoms, groups containing heteroatoms, or other hydrocarbon groups. The same applies hereinafter.
[0056] In the above formula (1), R 1 and R 2 At least one of R represents an organic group having a molecular weight of 16 or more, preferably a molecular weight of 16 to 1000, and examples thereof include alkyl groups such as ethyl, propyl, butyl, pentyl, hexyl, and heptyl groups, and aryl groups such as phenyl, tolyl, xylyl, naphthyl, and fluorenyl groups. 1 and R 2 may both be organic groups having a molecular weight of 16 or more, or one may be an organic group having a molecular weight of 16 or more and the other an organic group having a molecular weight of 15 or less or a hydrogen atom. Preferably, one is an organic group having a molecular weight of 16 or more and the other an organic group having a molecular weight of 15 or less, and in particular, one of them is a methyl group and the other a phenyl group, which is preferable from the viewpoints of easy control of handleability such as resin viscosity and strength of the cured product.
[0057] In the above formula (2), R 3is a divalent cyclic organic group, which may be an aromatic ring structure such as a benzene ring structure, a naphthalene ring structure, or a fluorene ring structure, or an aliphatic ring structure such as cyclobutane, cyclopentane, or cyclohexane. They may also independently have a substituent such as a hydrocarbon group or a halogen atom. The divalent bond may be a divalent group on a single carbon atom or a divalent group on different carbon atoms. Preferred examples include divalent aromatic groups having 6 to 100 carbon atoms and groups derived from cycloalkanes having 2 to 100 carbon atoms such as cyclopropane and cyclohexane. In particular, a 3,3,5-trimethyl-1,1-cyclohexylene group (also referred to as "structure (4)") represented by the following formula (4) is preferred from the viewpoints of controlling the handleability such as the resin viscosity and the strength of the cured product.
[0058] TIFF2024137893000004.tif44170
[0059] In addition, excellent heat resistance and low linear expansion are exhibited due to the rigidity of the fluorene skeleton represented by the following formula (5), and the molecular weight per unit is larger than that of ordinary epoxy resins, so that the proportion of secondary hydroxyl groups, which cause hygroscopicity, in the entire molecular structure is relatively low, which is preferable from the viewpoint of exhibiting low hygroscopicity.
[0060] TIFF2024137893000005.tif56151
[0061] Further, the epoxy polymer may include an epoxy polymer having a structure represented by the following formula (3) (also referred to as "structure (3)").
[0062] TIFF2024137893000006.tif40170
[0063] In the above formula (3), R 4 , R 5 , R 6 , R 7 Each of R is an organic group having a molecular weight of 15 or more. Preferably, R is an alkyl group having a molecular weight of 15 to 1000.4 , R 5 , R 6 , R 7 It is preferable that all of the above be methyl groups from the viewpoints of controlling the handleability of the resin, such as viscosity, and strength of the cured product.
[0064] From the viewpoint of achieving both reduced moisture absorption and strength retention of the present cured product and the present thermal conductive sheet, it is particularly preferable for the epoxy polymer to be an epoxy polymer containing either one of Structure (1) and Structure (2) and Structure (3).
[0065] Compared with typical epoxy polymers having a bisphenol A or bisphenol F skeleton, such epoxy polymers contain more hydrophobic hydrocarbon and aromatic structures, and therefore by blending the epoxy polymer, the moisture absorption amount of the resulting cured product, the thermally conductive sheet, can be reduced. From the viewpoint of reducing the amount of moisture absorption, it is preferable that the epoxy polymer contains a large amount of the hydrophobic structures (1), (2), and (3).
[0066] The weight average molecular weight of the epoxy polymer is preferably 5,000 or more, more preferably 10,000 or more, even more preferably 15,000 or more, even more preferably 20,000 or more, even more preferably 25,000 or more, even more preferably 30,000 or more. The upper limit is 100,000 or less. By being in these ranges, the film-forming property of the composition and the handling property of the uncured sheet tend to be improved. In addition, the improved film property has the effect of connecting the fillers together at the stage of the uncured sheet, so that voids are less likely to occur.
[0067] From the viewpoint of ensuring the film-forming property of the sheet and imparting flexibility, the epoxy equivalent of the epoxy polymer is preferably 5,000 g / equivalent or more, more preferably 7,000 g / equivalent or more, and even more preferably 8,000 g / equivalent or more, while from the viewpoint of solubility in a solvent, it is preferably 25,000 g / equivalent or less, and even more preferably 20,000 g / equivalent or less.
[0068] The mass average molecular weight of the epoxy polymer is a value calculated as polystyrene equivalent and measured by gel permeation chromatography. The epoxy equivalent is defined as "the mass of an epoxy polymer containing one equivalent of an epoxy group" and can be measured in accordance with JIS K7236.
[0069] The above epoxy polymers may be used alone or in combination of two or more.
[0070] (Multifunctional epoxy compound) The present composition preferably contains a polyfunctional epoxy compound, which will be described next.
[0071] The polyfunctional epoxy compound refers to an epoxy compound having two or more oxirane rings (epoxy groups) in one molecule and a mass average molecular weight of less than 5,000. By including such a polyfunctional epoxy compound, it is possible to introduce highly polar oxirane rings (epoxy groups) at a high density, which increases the effects of physical interactions such as van der Waals forces and hydrogen bonds, and for example, improves the adhesion between the thermally conductive sheet formed from the composition and a conductor. In addition, by including a polyfunctional epoxy compound, it is possible to increase the storage modulus of the thermally conductive sheet, which then exerts a strong anchor effect after the cured product of the composition penetrates into the unevenness of the conductor surface, which is the adherend, and improves the adhesion between the thermally conductive sheet and the conductor. On the other hand, the inclusion of a polyfunctional epoxy compound tends to increase the hygroscopicity of the composition, but by improving the reactivity of the oxirane ring (epoxy group), the amount of hydroxyl groups during the reaction can be reduced, thereby suppressing the increase in hygroscopicity. Furthermore, by producing the present composition by combining the above-mentioned epoxy polymer and polyfunctional epoxy compound, it is possible to achieve both high elasticity and low moisture absorption in the present thermally conductive sheet.
[0072] The polyfunctional epoxy compound may be an epoxy compound having two or more oxirane rings (epoxy groups) in one molecule, from the viewpoint of increasing the storage modulus of the cured product after thermal curing, particularly at high temperatures, which is important when the heat generation is large, such as in power semiconductors. Among them, it is preferable to include an epoxy compound having three or more oxirane rings (epoxy groups) in one molecule, and it is even more preferable to include an epoxy compound having four or more glycidyl groups in one molecule. By having multiple oxirane rings (epoxy groups), especially glycidyl groups, in one molecule, the crosslink density of the cured product is improved, and the obtained cured product, the present thermal conductive sheet, has a higher strength. As a result, when internal stress occurs in the present thermal conductive sheet during a moisture absorption reflow test, the present thermal conductive sheet does not deform or break, but maintains its shape, thereby suppressing the occurrence of voids and other voids in the present thermal conductive sheet.
[0073] From the viewpoint of adjusting the flexibility of the sheet, the molecular weight of the polyfunctional epoxy compound, particularly a polyfunctional epoxy compound having three or more epoxy groups in one molecule, is preferably 800 or less, more preferably 700 or less, even more preferably 650 or less, particularly preferably 100 or more or 630 or less, even more preferably 200 or more or 600 or less. In order to improve the handleability of the sheet, it is preferable that the compound contains one that is liquid at 25°C.
[0074] The epoxy equivalent of the polyfunctional epoxy compound having three or more epoxy groups in one molecule is preferably 25 g / equivalent or more, more preferably 50 g / equivalent or more, and even more preferably 75 g / equivalent or more, from the viewpoint of heat resistance of the sheet, while it is preferably 200 g / equivalent or less, more preferably 180 g / equivalent or less, more preferably 160 g / equivalent or less, and even more preferably 150 g / equivalent or less, from the viewpoint of solubility in a solvent. From the viewpoint of achieving lower moisture absorption and higher crosslinking, it is preferable that the polymer does not contain an amine or amide structure containing a nitrogen atom.
[0075] Specific examples of polyfunctional epoxy compounds having three or more epoxy groups in one molecule include polyfunctional epoxy compounds having three or more epoxy groups per molecule and a mass average molecular weight (Mw) of 800 or less, and preferably 650 or less. For example, EX321L, DLC301, DLC402, etc. manufactured by Nagase ChemteX Corporation can be used. These polyfunctional epoxy compounds may be used alone or in combination of two or more kinds.
[0076] (Content) The content of the epoxy polymer is preferably 5% by mass or more and 19% by mass or less based on the components (resin components) of the composition excluding the solvent and inorganic filler, in other words, 100% by mass of the solid content of the composition excluding the inorganic filler. It is preferable to contain 5% by mass or more of the epoxy polymer relative to 100% by mass of the resin component of the composition, since the film-forming properties of the sheet can be maintained, while it is preferable to contain 19% by mass or less, since the flexibility of the uncured sheet can be maintained. From this viewpoint, the content of the epoxy polymer is preferably 5% by mass or more, more preferably 6% by mass or more, more preferably 7% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more, based on 100% by mass of the resin component of the composition, while it is preferably 19% by mass or less, more preferably 18.5% by mass or less, and even more preferably 18% by mass or less.
[0077] The content of the polyfunctional epoxy compound is preferably 5% by mass or more and 95% by mass or less, based on 100% by mass of the solid content in the composition excluding the inorganic filler. When the content of the polyfunctional epoxy compound is 5% by mass or more, the curability can be maintained, and when the content is 95% by mass or less, other components for maintaining the film-forming property can be included. From this viewpoint, the content of the polyfunctional epoxy compound is preferably 5% by mass or more, more preferably 10% by mass or more, more preferably 15% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less. In particular, the content of the polyfunctional epoxy compound having three or more epoxy groups in one molecule is preferably 5% by mass or more and 50% by mass or less relative to 100% by mass of the solid content in the present composition excluding the inorganic filler. If the content of the polyfunctional epoxy compound having three or more epoxy groups in one molecule is 5% by mass or more, the elastic modulus of the cured product of the thermosetting composition can be maintained. From this viewpoint, the content of the polyfunctional epoxy compound having three or more epoxy groups in one molecule is preferably 5% by mass or more, more preferably 6% by mass or more, and even more preferably 7% by mass or more, based on 100% by mass of the solid content of the solid content of the present composition excluding the inorganic filler. On the other hand, if the content of the polyfunctional epoxy compound having three or more epoxy groups in one molecule is 50% by mass or less, the toughness of the uncured sheet can be maintained and the water absorption rate of the cured sheet can be suppressed, which is preferable. From this viewpoint, the content of the polyfunctional epoxy compound having three or more epoxy groups in one molecule is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less, based on 100% by mass of the solid content of the solid content of the present composition excluding the inorganic filler. In particular, from the viewpoint of adjusting the epoxy equivalent (WPE) of the resin component of the composition within a suitable range, the content of the polyfunctional epoxy compound having three or more epoxy groups in one molecule and an epoxy equivalent of 25 to 200 is preferably from 5 mass% to 50 mass% relative to 100 mass% of the solid content in the composition excluding the inorganic filler, and more preferably from 6 mass% to 45 mass%, and even more preferably from 7 mass% to 40 mass%.
[0078] As described later, when an epoxy polymer and a polyfunctional epoxy compound are used in combination, from the viewpoints of the film-forming properties of the sheet and the elastic modulus of the cured sheet, the content of the polyfunctional epoxy compound having three or more epoxy groups in one molecule is preferably 20 parts by mass or more and 500 parts by mass or less, more preferably 30 parts by mass or more or 400 parts by mass or less, and even more preferably 40 parts by mass or more or 350 parts by mass or less, per 100 parts by mass of the epoxy polymer.
[0079] The content ratio of the inorganic filler to the epoxy polymer (epoxy polymer / inorganic filler) is preferably 0.01 or more, more preferably 0.02 or more, and even more preferably 0.03 or more, from the viewpoint of maintaining the film formability of the uncured sheet. On the other hand, from the viewpoint of improving the bending resistance of the uncured sheet, it is preferably less than 0.1, more preferably 0.095 or less, and even more preferably 0.09 or less.
[0080] The content ratio of the inorganic filler to the polyfunctional epoxy compound having three or more epoxy groups in one molecule (polyfunctional epoxy compound having three or more epoxy groups in one molecule / inorganic filler) is preferably 0.02 or more, more preferably 0.03 or more, and even more preferably 0.04 or more, from the viewpoint of improving the retention of the inorganic filler. On the other hand, from the viewpoint of improving the thermal conductivity of the sheet, it is preferably 0.2 or less, more preferably 0.18 or less, and even more preferably 0.15 or less.
[0081] The content ratio of the inorganic filler to the epoxy compound (epoxy compound / inorganic filler) is preferably 0.2 or more, more preferably 0.22 or more, and even more preferably 0.25 or more, from the viewpoint of improving the sheet handling property, while it is preferably 0.53 or less, more preferably 0.52 or less, and even more preferably 0.51 or less, from the viewpoint of improving the thermal conductivity of the sheet.
[0082] <Inorganic filler> The inorganic filler contained in the present composition preferably has a thermal conductivity of 2.0 W / m·K or more, particularly preferably 3.0 W / m·K or more, particularly preferably 5.0 W / m·K or more, and particularly preferably 10.0 W / m·K or more.
[0083] Examples of inorganic fillers include electrically insulating fillers consisting only of carbon, fillers consisting of metal carbides or semi-metal carbides, metal oxides or semi-metal oxides, and metal nitrides or semi-metal nitrides.
[0084] An example of the electrically insulating filler made only of carbon is diamond (thermal conductivity: approximately 2000 W / m·K). Examples of the metal carbide or semi-metal carbide include silicon carbide (thermal conductivity: about 60 to 270 W / m·K), titanium carbide (thermal conductivity: about 21 W / m·K), and tungsten carbide (thermal conductivity: about 120 W / m·K).
[0085] Examples of the metal oxide or semi-metal oxide include magnesium oxide (thermal conductivity: about 40 W / m·K), aluminum oxide (thermal conductivity: about 20 to 35 W / m·K), zinc oxide (thermal conductivity: about 54 W / m·K), yttrium oxide (thermal conductivity: about 27 W / m·K), zirconium oxide (thermal conductivity: about 3 W / m·K), ytterbium oxide (thermal conductivity: about 38.5 W / m·K), beryllium oxide (thermal conductivity: about 250 W / m·K), and "sialon" (ceramics composed of silicon, aluminum, oxygen, and nitrogen, thermal conductivity: about 21 W / m·K). Examples of the metal nitride or semi-metal nitride include boron nitride (thermal conductivity in the plane direction of a plate-like particle of hexagonal boron nitride (h-BN): approximately 200 to 500 W / m K), aluminum nitride (thermal conductivity: approximately 160 to 285 W / m K), and silicon nitride (thermal conductivity: approximately 30 to 80 W / m K).
[0086] These inorganic fillers may be used alone or in combination of two or more.
[0087] From the viewpoint of electrical insulation, the volume resistivity of inorganic fillers at 20°C is 10 13 It is preferable that the resistivity is 10 Ω·cm or more, and particularly 10 14 It is more preferable that the resistivity is Ω·cm or more. Among them, metal oxides, semi-metal oxides, metal nitrides, and semi-metal nitrides are preferred because they can easily provide the thermally conductive sheet with sufficient electrical insulation. Specific examples of such inorganic fillers include aluminum oxide (Al 2 O 3, Volume resistivity:>10 14 Ω·cm), Aluminum Nitride (AlN, volume resistivity:>10 14 Ω·cm), Boron Nitride (BN, volume resistivity:>10 14 Ω·cm), silicon nitride (Si 3 N 4 , Volume resistivity:>10 14 Ω cm), silica (SiO 2 , Volume resistivity:>10 14 Examples include the surface area (Ω·cm). Among these, aluminum oxide, aluminum nitride, and boron nitride are preferred, with aluminum oxide and boron nitride being particularly preferred since they can impart high insulating properties to the present thermally conductive sheet.
[0088] The conductive filler may be in the form of irregular particles, spheres, whiskers, fibers, plates, or aggregates or mixtures thereof. Among these, the inorganic filler of the present invention is preferably in the form of spheres.
[0089] In the present invention, "spherical" generally means that the aspect ratio (ratio of major axis to minor axis) is 1 or more and 2 or less, preferably 1 or more and 1.75 or less, more preferably 1 or more and 1.5 or less, and further preferably 1 or more and 1.4 or less. The aspect ratio can be determined by randomly selecting 10 or more particles from an image of a cross section of the composition or the thermally conductive sheet taken with a scanning electron microscope (SEM), determining the ratio of the long axis to the short axis of each particle, and calculating the average value.
[0090] (Boron nitride agglomerated particles) The inorganic filler contained in the present composition preferably contains "boron nitride agglomerated particles" formed by agglomeration of primary particles of boron nitride, because this has fewer problems with moisture absorption during heat molding, is less toxic, can efficiently increase thermal conductivity, and can impart high insulating properties to the present thermally conductive sheet.
[0091] In addition, the boron nitride agglomerated particles may be used in combination with other inorganic fillers. However, the heat transfer behavior in the present thermal conductive sheet does not depend solely on the thermal conductivity inside the inorganic filler, as described below. Therefore, even if diamond particles or the like, which have extremely high thermal conductivity but are also extremely expensive, are used among the particles exemplified above, the thermal conductivity in the thickness direction of the present thermal conductive sheet does not increase extremely. Therefore, when using boron nitride agglomerated particles in combination with other inorganic fillers, the main focus is on reducing the cost of the composition. Therefore, it is preferable to appropriately select from magnesium oxide, aluminum oxide, tungsten carbide, silicon carbide, aluminum nitride, etc., as the inorganic filler to be used in combination with boron nitride, in terms of being relatively inexpensive and having a relatively high thermal conductivity.
[0092] In particular, from the viewpoint of high thermal conductivity, it is preferable that boron nitride agglomerated particles account for 75 mass% or more of the inorganic filler, more preferably 80 mass% or more, and even more preferably 85 mass% or more (including 100 mass%) of the inorganic filler.
[0093] The boron nitride agglomerated particles are preferably spherical in shape.
[0094] From the viewpoint of improving thermal conductivity, the agglomerated structure of the boron nitride agglomerated particles is preferably a card house structure. The aggregate structure of the boron nitride aggregated particles can be confirmed by a scanning electron microscope (SEM).
[0095] The house-of-cards structure is a structure in which plate-shaped particles are stacked in a complex manner without being oriented, and is described in "Ceramics 43 No. 2" (published by the Ceramic Society of Japan in 2008). More specifically, it refers to a structure in which the flat surface of a primary particle forming an aggregate particle is in contact with the end surface of another primary particle present within the aggregate particle. A schematic diagram of the house of cards structure is shown in Figure 1. The card-house structured aggregated particles have a very high breaking strength due to their structure, and do not break even during the pressurizing process performed during sheet molding of the thermal conductive sheet. Therefore, the primary particles that are usually oriented in the longitudinal direction of the thermal conductive sheet can be made to exist in a random direction. Therefore, by using the card-house structured aggregated particles, the proportion of the primary particles that have the ab plane oriented in the thickness direction of the thermal conductive sheet can be increased, so that heat can be effectively conducted in the thickness direction of the sheet, and the thermal conductivity in the thickness direction can be further increased.
[0096] Incidentally, boron nitride agglomerated particles having a house-of-cards structure can be produced, for example, by the method described in International Publication No. 2015 / 119198.
[0097] When using boron nitride agglomerated particles having a house-of-card structure, the particles may be surface-treated with a surface treatment agent. As the surface treatment agent, for example, a known surface treatment agent such as a silane coupling treatment can be used. It is considered that the attenuation of thermal conductivity at the interface between the inorganic filler and the matrix resin can be further reduced by increasing the adhesion at the interface between the inorganic filler and the matrix resin by chemical treatment.
[0098] By using agglomerated particles of boron nitride as the inorganic filler used in the present thermally conductive sheet, the particle size can be made larger than that of an inorganic filler that uses primary particles as they are. By increasing the particle size of the inorganic filler, the number of heat transfer paths between the inorganic fillers via the thermosetting compound having low thermal conductivity can be reduced, and therefore the increase in thermal resistance in the heat transfer paths in the thickness direction can be reduced.
[0099] From the above viewpoints, the lower limit of the maximum particle size of the boron nitride agglomerated particles is preferably 20 μm or more, more preferably 30 μm or more, and even more preferably 40 μm or more, while the upper limit of the maximum particle size is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and even more preferably 90 μm or less.
[0100] The average particle size of the boron nitride agglomerated particles is not particularly limited. Among them, 5 μm or more is preferable, 10 μm or more is more preferable, and particularly 15 μm or more is even more preferable. Also, 100 μm or less is preferable, and 90 μm or less is more preferable. When the average particle size of the boron nitride agglomerated particles is 5 μm or more, the number of particles in the composition and the cured product of the composition is relatively small, and the number of interparticle interfaces is reduced, so that the thermal resistance is reduced, and the thermal conductive sheet may have a high thermal conductivity. When the average particle size is equal to or less than the upper limit, the surface smoothness of the cured product using the composition tends to be obtained.
[0101] By having the average particle size or maximum particle size of the boron nitride agglomerated particles be equal to or less than the above upper limit, when the boron nitride agglomerated particles are contained in a matrix resin, a high-quality film without surface roughness, etc. By having the average particle size or maximum particle size be equal to or more than the above lower limit, the interface between the matrix resin and the boron nitride agglomerated particles is reduced, resulting in lower thermal resistance and achieving high thermal conductivity, while also providing a sufficient thermal conductivity improvement effect as an inorganic filler required for power semiconductor devices.
[0102] It is also considered that the effect of the thermal resistance at the interface between the matrix resin and the boron nitride agglomerated particles on the thickness of the thermal conductive sheet becomes significant when the size of the boron nitride agglomerated particles is 1 / 10 or less of the thickness of the thermal conductive sheet. In particular, in the case of power semiconductor devices, the thermal conductive sheet has a thickness of 100 μm to 300 μm, and therefore, from the viewpoint of thermal conductivity, it is preferable that the maximum particle size of the boron nitride agglomerated particles is larger than the above lower limit. Furthermore, by having the maximum particle size of the boron nitride agglomerated particles be equal to or greater than the above lower limit, not only is the increase in thermal resistance caused by the interface between the boron nitride agglomerated particles and the matrix resin suppressed, but the number of required thermal conduction paths between particles is reduced, increasing the probability that they will connect from one side to the other in the thickness direction of the thermally conductive sheet. On the other hand, by having the maximum particle size of the boron nitride agglomerated particles be equal to or less than the above upper limit, protrusion of the boron nitride agglomerated particles onto the surface of the thermal conductive sheet is suppressed, and a good surface shape without surface roughness is obtained. Therefore, when a sheet is produced by bonding it to a copper substrate, sufficient adhesion is obtained and excellent voltage resistance characteristics can be obtained.
[0103] The ratio of the size (maximum particle diameter) of the boron nitride agglomerated particles to the thickness of the thermally conductive sheet (maximum particle diameter / thickness) is preferably 0.3 or more and 1.0 or less, and more preferably 0.35 or more or 0.95 or less, and even more preferably 0.4 or more or 0.9 or less.
[0104] The maximum particle size and average particle size of the boron nitride agglomerated particles can be measured, for example, by the following method. The maximum particle size and average particle size of the boron nitride agglomerated particles used as the raw material can be determined as the maximum particle size Dmax and average particle size D50 of the boron nitride agglomerated particles from the obtained particle size distribution by measuring the particle size distribution of a sample in which boron nitride agglomerated particles are dispersed in a solvent, specifically, a sample in which boron nitride agglomerated particles are dispersed in a pure water medium containing a dispersion stabilizer, using a laser diffraction / scattering particle size distribution measuring device. Here, Dmax and D50 are the maximum particle size and the cumulative volume 50% particle size in a volume-based particle size distribution obtained by measurement using a laser diffraction / scattering particle size distribution measurement method. The maximum particle size and the average particle size can also be determined using a dry particle size distribution measuring device such as Morphologi G3 (manufactured by Malvern Instruments).
[0105] On the other hand, the maximum particle size and average particle size of the boron nitride agglomerated particles in this composition or this thermally conductive sheet can also be measured in the same manner as above by dissolving and removing the resin component containing the curable compound in a solvent (including a heated solvent), or by swelling the resin component to reduce the adhesive strength with the boron nitride agglomerated particles and then physically removing it, and further by heating the resin component in the atmosphere to incinerate it and remove it. In addition, regarding the maximum particle size of the boron nitride agglomerated particles in the present composition or the present thermally conductive sheet, it is also possible to directly observe any 10 or more boron nitride agglomerated particles on a cross-section of the present composition or the present thermally conductive sheet using a scanning electron microscope, a transmission electron microscope, a Raman microspectrometer, an atomic force microscope or the like, and determine the maximum particle size among them. The average particle diameter of the boron nitride agglomerated particles in the present composition or present thermally conductive sheet can also be determined by directly observing a cross section of the present composition or present thermally conductive sheet using a scanning electron microscope, a transmission electron microscope, a Raman microspectrometer, an atomic force microscope or the like to observe any 10 or more boron nitride agglomerated particles, and calculating the arithmetic average value of the particle diameters. When the particles are non-spherical, the longest and shortest diameters are measured, and the average value thereof is regarded as the particle diameter of the particle.
[0106] (Inorganic filler content) The content of the inorganic filler is preferably 60% by mass or more relative to 100% by mass of the solid content in the composition. If the content of the inorganic filler is 60% by mass or more relative to 100% by mass of the solid content in the composition, the insulating property and thermal conductivity can be improved. From this viewpoint, the content of the inorganic filler is preferably 60% by mass or more relative to 100% by mass of the solid content in the composition, more preferably 63% by mass or more, and even more preferably 65% by mass or more. On the other hand, if the content is 85% by mass or less, the handling property and film-forming property can be maintained. From this viewpoint, the content of the inorganic filler is preferably 85% by mass or less, more preferably 83% by mass or less, and even more preferably 81% by mass or less.
[0107] The content of the boron nitride agglomerated particles is preferably 50% by mass or more relative to 100% by mass of the total inorganic filler. When the content of the boron nitride agglomerated particles is 50% by mass or more relative to 100% by mass of the total inorganic filler, the insulating property and thermal conductivity can be improved. From this viewpoint, the content of the boron nitride agglomerated particles is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on 100% by mass of the total inorganic filler.
[0108] <Hardening agent> The present composition preferably contains a curing agent, if necessary. Examples of the curing agent include phenol resins, compounds having a heterocyclic structure containing a nitrogen atom (referred to as "nitrogen-containing heterocyclic compounds"), acid anhydrides having an aromatic skeleton or an alicyclic skeleton, water additives of the acid anhydrides, or modified products of the acid anhydrides, etc. Only one type of curing agent may be used, or two or more types may be used in combination. By using these preferable curing agents, it is possible to obtain a cured product having an excellent balance of heat resistance, moisture resistance, and electrical properties.
[0109] Examples of the phenolic resin include phenolic novolac, o-cresol novolac, p-cresol novolac, t-butylphenol novolac, dicyclopentadiene cresol, polyparavinylphenol, bisphenol A type novolac, xylylene modified novolac, decalin modified novolac, poly(di-o-hydroxyphenyl)methane, poly(di-m-hydroxyphenyl)methane, or poly(di-p-hydroxyphenyl)methane. Among them, in order to further improve the flexibility and flame retardancy of the present composition, the present cured product, and the present thermal conductive sheet, and to improve the mechanical properties and heat resistance of the cured product, novolac type phenolic resins having a rigid main chain skeleton and phenolic resins having a triazine skeleton are preferred. In addition, in order to improve the flexibility of the uncured thermosetting composition and the toughness of the resin cured product, phenolic resins having an allyl group are preferred.
[0110] Examples of the heterocyclic structure of the nitrogen-containing heterocyclic compound include structures derived from imidazole, triazine, triazole, pyrimidine, pyrazine, pyridine, and azole. From the viewpoint of improving the insulating properties and adhesion to metals of the cured product, imidazole-based compounds and triazine-based compounds are preferred. Preferable imidazole compounds and triazine compounds include, for example, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,4-diamino-6-vinyl-s-triazine, 2,4-diamino-6-vinyl-s-triazine isocyanuric acid adduct, 2,4-diamino-6-methacryloyloxyethyl-s-triazine, 2,4-diamino-6-methacryloyloxyethyl-s-triazine isocyanuric acid adduct, and the like can be mentioned.
[0111] Among these, those having a structure derived from imidazole and those having a structure derived from triazine are particularly preferred, since they have high resin compatibility and a high reaction activation temperature, and thus the curing speed and physical properties after curing can be easily adjusted, thereby enabling improvement in the storage stability of the composition and further improvement in the adhesive strength after heat molding to be realized. Therefore, those having a structure derived from imidazole and those having a structure derived from triazine are particularly preferred. As the heterocyclic structure of the nitrogen-containing heterocyclic compound, a structure derived from 1,3,5-triazine is particularly preferable, and the compound may have a plurality of the structural moieties exemplified above.
[0112] Depending on the structure, the nitrogen-containing heterocyclic compound may contain a thermosetting catalyst, which will be described later, and therefore the present composition may contain a nitrogen-containing heterocyclic compound as a thermosetting catalyst. The nitrogen-containing heterocyclic compound may be used alone or in combination of two or more kinds, and may have a plurality of heterocyclic structures simultaneously in one molecule. The molecular weight of the nitrogen-containing heterocyclic compound is preferably 1,000 or less, and more preferably 500 or less.
[0113] The acid anhydride having an aromatic skeleton, the water-added product of the acid anhydride, or the modified product of the acid anhydride is not particularly limited.
[0114] The acid anhydride having an alicyclic skeleton, a water adduct of the acid anhydride, or a modified product of the acid anhydride is preferably an acid anhydride having a polyalicyclic skeleton, a water adduct of the acid anhydride, or a modified product of the acid anhydride, or an acid anhydride having an alicyclic skeleton obtained by an addition reaction of a terpene compound with maleic anhydride, a water adduct of the acid anhydride, or a modified product of the acid anhydride.
[0115] The curing agent is preferably contained in an amount of 0 to 70% by mass, particularly 0 to 55% by mass, based on 100% by mass of the solid content of the composition excluding the inorganic filler. If the content of the curing agent is equal to or more than the lower limit, sufficient curing performance can be obtained, and if it is equal to or less than the upper limit, the reaction proceeds effectively, the crosslinking density can be improved, the strength can be increased, and the film formability can be improved.
[0116] <Curing accelerator> The present composition may contain a thermosetting catalyst as a curing accelerator, if necessary, in order to adjust the curing rate and the physical properties of the cured product.
[0117] It is preferable to appropriately select the thermosetting catalyst depending on the type of thermosetting compound and curing agent. Specific examples of the thermosetting catalyst include linear or cyclic tertiary amines, organic phosphorus compounds, diazabicycloalkenes such as quaternary phosphonium salts or organic acid salts, and imidazoles. In addition, organic metal compounds, quaternary ammonium salts, metal halides, and the like can also be used. Examples of the organic metal compounds include zinc octylate, tin octylate, and aluminum acetylacetone complexes. Furthermore, the nitrogen-containing heterocyclic compound described above as a curing agent also functions as a thermosetting catalyst, and therefore may be blended as a thermosetting catalyst.
[0118] Among these, compounds having imidazole (referred to as "imidazole-based compounds") are preferred, particularly from the viewpoints of storage stability, heat resistance, and curing speed. Preferred imidazole compounds include, for example, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2, Examples of the compound include 4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. In particular, by using an imidazole compound having a melting point of 100° C. or higher, and more preferably 200° C. or higher, a cured product having excellent storage stability and adhesion can be obtained. Furthermore, those containing a nitrogen-containing heterocyclic compound other than the above-mentioned imidazole ring are more preferred from the viewpoint of adhesiveness. The thermosetting catalyst may be used alone or in combination of two or more kinds.
[0119] The thermosetting catalyst is preferably contained in an amount of 0.1 to 10 mass%, particularly 0.1 to 5 mass%, based on 100 mass% of the solid content of the solid content of the composition excluding the inorganic filler. When the content of the thermosetting catalyst is equal to or more than the lower limit, the progress of the curing reaction can be sufficiently promoted to achieve good curing, and when it is equal to or less than the upper limit, the curing speed is not too fast, and therefore the storage stability of the composition can be improved.
[0120] <Organic solvent> The present composition may contain an organic solvent as necessary, for example, to improve the coatability when forming a sheet-like cured product through a coating step. Examples of organic solvents that may be contained in the present composition include methyl ethyl ketone, cyclohexanone, propylene glycol monomethyl ether acetate, butyl acetate, isobutyl acetate, propylene glycol monomethyl ether, etc. These organic solvents may be used alone or in combination of two or more.
[0121] When the composition contains an organic solvent, the content is appropriately determined depending on the handling property during the preparation of the thermally conductive sheet, etc. Usually, the organic solvent is preferably used so that the solid content (total of components other than the solvent) in the composition is 10 to 90 mass%, particularly 40 mass% or more or 80 mass% or less. In addition, when formed into a sheet, the organic solvent is preferably used so that the solids concentration (total of components other than the solvent) in the composition is 95 mass % or more, more preferably 97 mass % or more, even more preferably 98 mass % or more, and even more preferably 99 mass % or more.
[0122] <Other ingredients> The present composition may contain other ingredients in addition to the above ingredients. Examples of the other components include additives such as dispersants, thermoplastic resins, organic fillers, inorganic fillers, and silane coupling agents that improve the interfacial adhesive strength between inorganic fillers and resin components, additives that can be expected to have the effect of increasing the adhesive strength between a resin sheet and a metal plate-shaped material, insulating carbon components such as reducing agents, viscosity adjusters, thixotropic agents, flame retardants, colorants, various antioxidants such as phosphorus-based and phenol-based, process stabilizers such as phenol acrylate-based, heat stabilizers, hindered amine radical scavengers (HAAS), impact modifiers, processing aids, metal deactivators, copper inhibitors, antistatic agents, extenders, etc. The amount of these additives added when used may usually be within the range of the amount used for these purposes.
[0123] <<Uses of this composition>> The present composition can be made into a present cured product by heating, and the present cured product can be made into a sheet-like cured product to form the present thermal conductive sheet. That is, the present thermal conductive sheet, which is a sheet-like cured product, is made of the present composition.
[0124] <Thermal conductive sheet> The present thermally conductive sheet according to one embodiment of the present invention may be a thermally conductive sheet formed from a cured product of the present composition.
[0125] The thermal conductivity of this thermal conductive sheet in the thickness direction at 25°C is preferably 15 W / m·K or more, more preferably 15.5 W / m·K or more, more preferably 16 W / m·K or more, more preferably 16.5 W / m·K or more, more preferably 17 W / m·K or more, particularly preferably 17.5 W / m·K or more, and of these, more preferably 18 W / m·K or more. Since the thermal conductivity in the thickness direction is equal to or more than the above lower limit, the sheet can be suitably used in power semiconductor devices that operate at high temperatures. The thermal conductivity can be adjusted by the type of thermosetting compound, the type and content of inorganic filler, the method of mixing the thermosetting compound and the inorganic filler, the conditions in the heating and kneading step described below, and the like.
[0126] The thermal conductivity of the thermally conductive sheet in the thickness direction can be measured by the following method. For example, the thermal conductivity can be determined from the slope of a graph obtained by plotting thermal resistance against thickness using a thermal resistance measuring device (manufactured by Mentor Graphics Corporation, product name "T3ster").
[0127] (Breakdown voltage (BDV)) The present thermally conductive sheet preferably has a dielectric breakdown voltage of 50 kV / mm or more. If the thermal conductive sheet has a dielectric breakdown voltage of 50 kV / mm or more, sufficient insulation performance can be obtained, and the sheet can be used in applications such as power semiconductor devices, industrial equipment, automotive equipment, and power generation energy. From this viewpoint, the thermally conductive sheet preferably has a breakdown voltage of 50 kV / mm or more, more preferably 53 kV / mm or more, and even more preferably 55 kV / mm or more.
[0128] In order to prepare the composition of the present invention so that the breakdown voltage of the thermal conductive sheet falls within the above range, for example, the type of thermosetting compound, the type and content of the inorganic filler, the method of mixing the thermosetting compound and the inorganic filler, the conditions in the heating and kneading step described below, etc. may be adjusted, but the method is not limited to these. For the method of measuring the dielectric breakdown voltage, see the method in the Examples described below.
[0129] (Thickness) The lower limit of the thickness of the thermally conductive sheet is preferably 50 μm or more, more preferably 60 μm or more, and even more preferably 70 μm or more, while the upper limit of the thickness is preferably 400 μm or less, more preferably 300 μm or less, and even more preferably 250 μm or less. By making the thickness of this thermally conductive sheet 50 μm or more, sufficient voltage resistance characteristics can be ensured. On the other hand, by making the thickness 400 μm or less, it is possible to achieve a smaller and thinner device, particularly when the thermally conductive sheet is used in a power semiconductor device, and the thin film can reduce the thermal resistance in the thickness direction compared to insulating thermally conductive layers made of ceramic materials.
[0130] <Method of manufacturing thermally conductive sheet> An example of the method for producing the thermally conductive sheet will now be described.
[0131] The present thermally conductive sheet is prepared by forming the present composition into a sheet (this process is referred to as the "film-forming process"), drying the composition as necessary (this process is referred to as the "drying process"), and further applying pressure as necessary (this process is referred to as the "pressing process"). The sheet-like composition thus obtained is then cured to produce the present thermally conductive sheet as a sheet-like cured product (this process is referred to as the "curing process").
[0132] (Film forming process) For example, the present composition in a slurry form can be formed into a sheet by a coating method such as a blade method, a solvent casting method, or an extrusion film forming method.
[0133] When forming a film in a sheet form by the above coating method, the present composition in a slurry form is first coated on the surface of a substrate to form a coating film, that is, the present composition in a slurry form is used to form a coating film on the substrate by a dip method, a spin coating method, a spray coating method, a blade method, or any other method. The present composition in a slurry form can be applied using a coating device such as a spin coater, a slit coater, a die coater, a blade coater, etc. Such a coating device can uniformly form a coating film of a predetermined thickness on a substrate. As the substrate, a copper plate or copper foil or a PET film, which will be described later, is generally used, but there is no limitation thereto.
[0134] (drying process) The composition formed into a sheet as described above is dried usually at a temperature of 10 to 150°C, preferably 25 to 120°C, more preferably 30 to 110°C to remove the solvent and low molecular weight components. By keeping the drying temperature at or below the upper limit, curing of the resin in the composition is suppressed, and the resin in the sheet-shaped composition tends to flow in the subsequent pressurizing step, making it easier to remove voids. By keeping the drying temperature at or above the lower limit, the solvent can be effectively removed, and productivity tends to improve. The drying time is not particularly limited, and can be appropriately adjusted depending on the state of the composition, the drying environment, etc. The drying time is preferably 1 minute or more, more preferably 2 minutes or more, and even more preferably 5 minutes or more. The drying time is preferably 24 hours or less, more preferably 10 hours or less, even more preferably 4 hours or less, and particularly preferably 2 hours or less. By setting the drying time to the above lower limit or more, the solvent can be sufficiently removed, and the residual solvent tends to be prevented from forming voids in the cured resin. By setting the drying time to the above upper limit or less, the productivity tends to be improved, and the production cost tends to be reduced.
[0135] (Pressure process) After the drying step, it is desirable to apply pressure to the obtained sheet-like composition for the purposes of bonding inorganic fillers together to form a heat conduction path, eliminating voids and gaps in the sheet, improving adhesion to the substrate, etc. However, depending on the purpose, pressure may not be applied.
[0136] In the pressing step, it is desirable to apply a load of 2 MPa or more to the sheet-like composition on the substrate. The load is preferably 5 MPa or more, more preferably 7 MPa or more, and even more preferably 9 MPa or more. The load is preferably 1500 MPa or less, more preferably 1000 MPa or less, and even more preferably 800 MPa or less. By setting the load during pressing to the above upper limit or less, the secondary particles of the boron nitride agglomerated particles are not destroyed, and a sheet having high thermal conductivity without voids in the sheet-like composition of the present invention can be obtained. By setting the load to the above lower limit or more, contact between the inorganic fillers becomes good, making it easier to form a thermal conduction path, and therefore a thermally conductive sheet having high thermal conductivity can be obtained.
[0137] The heating temperature of the sheet-like composition on the substrate in the pressurizing step is not particularly limited. The heating temperature is preferably 10° C. or higher, more preferably 20° C. or higher, and even more preferably 30° C. or higher. The heating temperature is preferably 300° C. or lower, more preferably 250° C. or lower, even more preferably 200° C. or lower, even more preferably 100° C. or lower, and particularly preferably 90° C. or lower. By carrying out the pressurization step within this temperature range, the melt viscosity of the resin in the sheet-shaped composition can be reduced, and voids and gaps in the thermal conductive sheet can be further reduced. In addition, by heating at or below the upper limit, decomposition of organic components in the sheet-shaped composition and the cured product and voids caused by residual solvent tend to be suppressed.
[0138] The time of the pressurizing step is not particularly limited. The time of the pressurizing step is preferably 30 seconds or more, more preferably 1 minute or more, even more preferably 3 minutes or more, and particularly preferably 5 minutes or more. The time of the pressurizing step is preferably 1 hour or less, more preferably 30 minutes or less, and even more preferably 20 minutes or less. By keeping the pressurizing time below the upper limit, the manufacturing time of the thermally conductive sheet can be reduced, and the production cost tends to be reduced. By keeping the pressurizing time above the lower limit, the gaps and voids in the thermally conductive sheet can be sufficiently removed, and the heat transfer performance and the voltage resistance characteristics tend to be improved.
[0139] (hardening process) The composition can be cured by heating. In this case, the heating temperature is preferably 30 to 400° C., more preferably 50° C. or higher, and even more preferably 90° C. or higher, while it is preferably 300° C. or lower, and even more preferably 250° C. or lower.
[0140] The curing step for completely curing the composition may be carried out under pressure or without pressure. When pressure is applied, it is preferable to carry out the step under the same conditions as the above-mentioned pressurizing step for the same reasons as above. The pressurizing step and the curing step may be carried out simultaneously. In particular, in the sheet forming process which involves a pressing step and a hardening step, it is preferable to apply a load within the above range and carry out the pressing and hardening.
[0141] The load when the pressing step and the curing step are performed simultaneously is not particularly limited. In this case, it is preferable to apply a load of 5 MPa or more to the sheet-like composition on the substrate, more preferably 7 Pa or more, even more preferably 9 MPa or more, and particularly preferably 20 MPa or more. In addition, the load is preferably 2000 MPa or less, more preferably 1500 MPa or less. By setting the load when the pressing step and the curing step are carried out simultaneously to the above upper limit value or less, the secondary particles of the boron nitride agglomerated particles are not destroyed, and a sheet-like cured product having high thermal conductivity and no voids in the sheet-like present composition can be obtained. In addition, by setting the load to the above lower limit value or more, contact between the inorganic fillers becomes good, making it easier to form a thermal conductive path, and therefore the present thermal conductive sheet having high thermal conductivity can be obtained.
[0142] When the pressing step and the curing step are performed simultaneously, the pressing time is not particularly limited. The pressing time is preferably 30 seconds or more, more preferably 1 minute or more, even more preferably 3 minutes or more, and particularly preferably 5 minutes or more. The pressing time is preferably 1 hour or less, more preferably 30 minutes or less, and even more preferably 20 minutes or less. By keeping the pressurizing time at or below the upper limit, the manufacturing time of the thermally conductive sheet can be reduced, and production costs tend to be reduced.By keeping the pressurizing time at or above the lower limit, voids and gaps in the sheet-like cured product, i.e., the thermally conductive sheet, can be sufficiently removed, and heat transfer performance and voltage resistance tend to be improved.
[0143] <<Composite molded body>> A composite molded product (referred to as "the present composite molded product") as an example of an embodiment of the present invention is a sheet-like cured product of the present composition, i.e., a cured product part made of the present thermally conductive sheet and a metal part that are laminated together. That is, the composite molded product has a cured product part made of the present thermally conductive sheet and a metal part. In this case, the metal part may be provided on only one surface of the cured product part made of the thermally conductive sheet, or on two or more surfaces. For example, the thermally conductive sheet may have a metal part on only one surface, or on both surfaces. The metal part may be patterned.
[0144] Such a composite molded product can be produced by using a metal part as the substrate and forming a sheet of the composition or the thermally conductive sheet on the substrate according to the method described above. Alternatively, the composite molded product can be produced by peeling the sheet of the composition or the thermally conductive sheet formed on a substrate other than the metal part from the substrate, and then heat-pressing the sheet onto a metal member that will become the metal part.
[0145] In this case, a sheet-like composition or thermally conductive sheet of the present invention is formed in the same manner as described above, except that it is applied onto a substrate such as PET which may be treated with a release agent, and then peeled off from the substrate. This sheet-like composition or thermally conductive sheet of the present invention is then placed on another metal plate, or sandwiched between two metal plates and pressed to be integrated.
[0146] In this case, the metal plate may be a metal plate having a thickness of about 10 μm to 10 cm and made of copper, aluminum, nickel-plated metal, etc. The surface of the metal plate may be physically roughened or chemically treated with a surface treatment agent, etc. From the viewpoint of adhesion between the thermosetting composition and the metal plate, it is more preferable that the surface of the metal plate is subjected to such treatment.
[0147] Specific examples of the present composite molded article include a heat dissipating laminate, a heat dissipating circuit board, a semiconductor device, a power module, etc. These will be described below in order, but the present invention is not limited to these.
[0148] <Heat dissipation laminate> A heat dissipation laminate according to one embodiment of the present invention (referred to as "the present heat dissipation laminate") may be a laminate including the present thermally conductive sheet.
[0149] An example of the present heat dissipating laminate is one in which a heat dissipating metal layer containing a heat dissipating material is laminated on one surface of the present heat conductive sheet.
[0150] The heat dissipating material is not particularly limited as long as it is made of a material having good thermal conductivity. In particular, in order to increase the thermal conductivity in the laminated structure, it is preferable to use a heat dissipating metal material, and more preferably to use a flat metal material. The type of metal material is not particularly limited, but among them, a copper plate, an aluminum plate, an aluminum alloy plate, etc. are preferable because they have good thermal conductivity and are relatively inexpensive.
[0151] The thermal conductive sheet and the heat dissipation metal layer can be laminated and integrated by press molding, which is a batch process. In this case, the press equipment and press conditions are the same as those for obtaining the thermal conductive sheet.
[0152] <Heat dissipation circuit board> A heat dissipation circuit board according to one embodiment of the present invention (hereinafter referred to as "the present heat dissipation circuit board") may be any circuit board provided with the present thermally conductive sheet. An example of the present heat dissipating circuit board is one in which the above-mentioned heat dissipating metal layer is laminated on one surface of the present heat conductive sheet, and a circuit board is formed on the surface of the heat conductive sheet opposite the heat dissipating metal layer, for example, by etching or the like. Specifically, an integrated structure of "heat dissipating metal layer / heat conductive sheet / conductive circuit" is more preferable. The state before the circuit etching can be, for example, an integrated structure of "heat dissipating metal layer / heat conductive sheet / conductive circuit forming metal layer" in which the conductive circuit forming metal layer is flat and formed on the entire surface of one side of the heat conductive sheet, or formed on a partial area.
[0153] The material of the conductive circuit-forming metal layer is not particularly limited. In particular, it is generally preferable to form the conductive circuit-forming metal layer from a copper thin plate having a thickness of 0.05 mm to 1.2 mm in terms of electrical conductivity, etching properties, cost, and the like.
[0154] <Semiconductor devices> A semiconductor device according to an example of an embodiment of the present invention (hereinafter referred to as "the present semiconductor device") may be any device that includes the present heat dissipation circuit board. An example of the present semiconductor device is one having a configuration in which a silicon wafer or a rewiring layer on which a pre-diced semiconductor chip is mounted is formed on the present heat dissipation circuit board.
[0155] <Power module> A power module according to an example of an embodiment of the present invention (hereinafter referred to as "the present power module") may be any module that includes the present thermally conductive sheet. An example of the present power module is one in which the present thermally conductive sheet is mounted on a power semiconductor device as a heat dissipating circuit board. In this power semiconductor device, conventionally known materials can be appropriately used for the materials other than the thermally conductive sheet or laminated heat dissipation sheet, such as aluminum wiring, sealing material, packaging material, heat sink, thermal paste, and solder.
[0156] <<Explanation of terms>> In the present invention, when it is written "α to β" (α and β are arbitrary numbers), unless otherwise specified, it includes the meaning of "α or more and β or less", as well as "preferably larger than α" or "preferably smaller than β". In addition, when it is stated that "α or more" or "α≦" (α is any number), it also means "preferably greater than α" unless otherwise specified, and when it is stated that "β or less" or "≦β" (β is any number), it also means "preferably smaller than β" unless otherwise specified. In the present invention, the term "sheet" conceptually encompasses a sheet, a film, and a tape. In addition, in this specification, the expression "and / or" means "and / or." EXAMPLES
[0157] An example of the present invention will be described below, however, the present invention is not limited to the example described below.
[0158] <Ingredients> The raw materials used in the examples and comparative examples are as follows.
[0159] (Inorganic filler) Inorganic filler 1: boron nitride agglomerated particles having a house-of-cards structure, produced according to the method for producing boron nitride agglomerated particles disclosed in the examples of WO 2015 / 561028. Maximum particle size: 90μm Average particle size (D50): 45μm Inorganic filler 2: Admatechs Spherical Alumina Particles Average particle size (D50): 7~13μm
[0160] (Epoxy compounds) Resin component 1: Biphenyl-type solid epoxy compound manufactured by Mitsubishi Chemical Corporation, with two glycidyl groups per molecule Molecular weight: approx. 400 Epoxy equivalent: 200g / equivalent Resin component 2: Nagase ChemteX Corporation, a multifunctional epoxy compound containing a structure with four or more glycidyl groups per molecule Does not contain amine or amide structures containing nitrogen atoms Molecular weight: approx. 400 Epoxy equivalent: 100g / equivalent
[0161] (hardening agent) Hardener 1: Meiwa Kasei's "MEH-8000H", a phenolic resin hardener Hardener 2: Yamada Chemical Industry Co., Ltd. 2,7-DHN 2,7-Dihydroxynaphthalene Hardener 3: UBE H-4 phenolic resin hardener
[0162] (polymer) Epoxy polymer 1: a bifunctional epoxy polymer manufactured by Mitsubishi Chemical Corporation and disclosed as resin component 1 in JP2020-63438A, having the structures of the above formulas (2) and (3) Polystyrene equivalent weight average molecular weight: 30,000 Epoxy equivalent: 9,000g / equivalent Epoxy polymer 2: a bifunctional epoxy polymer manufactured by Mitsubishi Chemical Corporation and disclosed in Japanese Patent No. 6497292, having the structures of the above formulas (1), (2), and (3) Polystyrene equivalent weight average molecular weight: 40,000 Epoxy equivalent: 11,000g / equivalent
[0163] (Thermosetting catalyst) -Thermosetting catalyst 1: 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine. Contains both a structure derived from imidazole and a structure derived from triazine in one molecule ("Curesol 2E4MZ-A" manufactured by Shikoku Kasei Co., Ltd.) -Thermal curing catalyst 2: 2-phenyl-4,5-dihydroxymethylimidazole (Shikoku Kasei Corporation "Curezol 2PHZ-PW")
[0164] <Examples 1 to 5 and Comparative Examples 1 to 4> Each raw material was weighed out so as to obtain the composition (parts by mass) shown in Table 1, and mixed using a planetary stirring device to obtain a mixture. When preparing this mixture, a slurry-like thermosetting composition was prepared using 20% by mass each of methyl ethyl ketone and cyclohexanone so that the mixture constituted 60% by mass (solid content concentration) of the coating slurry.
[0165] The obtained slurry-like thermosetting composition was applied to a PET substrate by a doctor blade method and dried by heating at 60°C for 120 minutes to obtain a sheet-like thermosetting composition. The total content of methyl ethyl ketone and cyclohexanone in the sheet-like thermosetting composition was 1 mass% or less. The thickness of this sheet after pressing was 150 μm.
[0166] For the sheet-like thermosetting compositions obtained in the Examples and Comparative Examples, WPE measurement, evaluation of bending resistance of the sheets, storage modulus E' measurement of the cured thermosetting composition, thermal conductivity measurement, and BVD measurement were performed as follows. The results of each Example and Comparative Example are shown in Table 1.
[0167] In Table 1, the "proportion of polymer in resin component" refers to the proportion (mass%) of the total content of the epoxy polymer relative to 100 mass% of the components (resin component) excluding the solvent and inorganic filler from the thermosetting composition, i.e., 100 mass% of the total amount of the resin component, curing agent, epoxy polymer, and thermosetting catalyst. In Table 1, "WPE of resin component excluding filler" is the epoxy equivalent (g / equivalent) of the component excluding the solvent and inorganic filler from the thermosetting composition.
[0168] <Measurement and Evaluation> The raw materials used in the Examples and Comparative Examples, and the sheet-shaped thermosetting compositions produced in the Examples and Comparative Examples were measured and evaluated for their physical properties as follows.
[0169] (Measurement of epoxy equivalent (WPE) of resin component) The resin components (excluding the solvent and inorganic filler) used in each of the Examples and Comparative Examples, i.e., resin component 1-2, epoxy polymer 1-2, curing agent 1-3, and thermosetting catalyst 1-2, were mixed in the mass ratio shown in Table 1 below to obtain a resin composition, which was measured by potentiometric titration and converted into the value of the entire resin components to obtain the epoxy equivalent (g / equivalent).
[0170] (Evaluation of sheet bending resistance (mandrel test)) The sheet-shaped thermosetting composition prepared in each of the Examples and Comparative Examples was cut into a piece having a width of 2 cm and a length of 15 cm or more, and bending resistance was evaluated according to the test method of JIS K5600-5-1. ◎ (Pass): The diameter of the jig where the sheet broke is less than 16 mm 〇 (Pass): The diameter of the jig where the sheet broke is less than 20 mm and 16 mm or more × (Fail): The diameter of the jig where the sheet broke is 20 mm or more.
[0171] (Measurement of storage modulus (E') of cured product of thermosetting composition) Three sheets of the sheet-like thermosetting composition prepared in each Example and Comparative Example were stacked, and while applying a load of 10 MPa from above and below, they were heated and cured at 175°C (product temperature) for 30 minutes and at 200°C for 30 minutes to obtain a cured product of the thermosetting composition. This cured product was cut into test pieces of approximately 4 mm width and 50 to 60 mm length to be used as evaluation samples. The storage modulus (E') of this evaluation sample was measured under the following conditions using a measuring device: Hitachi High-Tech Science Corporation "DMS6100". Measurement temperature conditions: -110~270℃ Measurement mode: Tensile mode Measurement frequency: 1Hz Chuck distance: 35mm Distortion amplitude (μm): 5μm Initial force amplitude (mN): 50mN
[0172] (Measurement of thermal conductivity in the thickness direction of the thermosetting composition layer) The sheet-shaped thermosetting compositions prepared in each of the Examples and Comparative Examples were cured by heating at 175°C (product temperature) for 30 minutes and at 200°C for 30 minutes while applying a load of 10 MPa to obtain a sheet-shaped cured product having a thickness of 150 μm. In addition, two, three, or four sheets of the sheet-like thermosetting composition prepared in each Example and Comparative Example were stacked and pressed in the same manner as above to obtain four types of sheet-like cured products (filler-containing sheets) of the thermosetting composition with different thicknesses. The following measurements were carried out on these four types of sheet-like cured products with different thicknesses, and the thermal conductivity at 25°C in the sheet thickness direction using a steady state method was measured from the slope represented by the thermal resistance value versus sheet thickness (in accordance with ASTM D5470). (1) Thickness: Thickness (μm) when pressed at a pressure of 3400 kPa using a Mentor Graphics T3Ster-DynTIM (2) Measurement area: The area (cm) of the part that transfers heat when measuring using a Mentor Graphics T3Ster-DynTIM 2 ) (3) Thermal resistance value: Thermal resistance value (K / W) when pressed at a pressure of 3400 kPa using Mentor Graphics T3Ster-DynTIM. (4) Thermal conductivity: The thermal resistance of four sheets of different thicknesses was measured, and the thermal conductivity (W / m K) was calculated using the following formula. Formula: Thermal conductivity (W / m K) = 1 / ((slope (thermal resistance value / thickness): K / (W μm)) × (area: cm 2 ))×10 -2
[0173] (Measurement of BDV (dielectric breakdown voltage) of cured thermosetting composition) The sheet-like thermosetting composition prepared in each Example and Comparative Example was laid on a 2 mm thick copper plate, and while applying a pressure of 10 MPa, it was heated at 175°C (product temperature) for 30 minutes and then at 200°C for 30 minutes to bond the sheets together through heat-pressure curing. The cured product of the sheet-like thermosetting composition was laminated on the copper plate to prepare a composite molded body (evaluation sample). The composite molding (evaluation sample) was immersed in insulating oil (Fluorinert FC-40 manufactured by 3M), and using an ultra-high voltage withstand voltage tester 7470 (manufactured by Keisoku Gijutsu Kenkyusho), electrodes were placed on the patterned copper of φ25 mm, a voltage of 0.5 kV was applied, and the voltage was increased by 500 V every minute, and the voltage until the cured thermosetting composition was destroyed (BDV: dielectric breakdown voltage) was measured. In addition, the thermosetting composition after the bending resistance test was adhered to a copper plate by heat and pressure curing in the same manner as above, and the BDV of the composite molded article (BDV after bending test) was measured.
[0174] [Table 1]
[0175] A comparison between Examples 1 to 5 and Comparative Examples 1 to 4, as well as the results of tests conducted by the inventors thus far, reveals that by setting the WPE of the resin component within a specified range, the crosslink density is increased, making it possible to maintain contact between the inorganic filler particles, and by reducing the thermal resistance between the fillers, the thermal conductivity is increased. It was also found that by having the ratio of the polymer component fall within a specific range, the flexibility of the sheet before curing can be maintained, and bending resistance is improved. Furthermore, by having the WPE of the resin component fall within a prescribed range, the elastic modulus of the resin component tends to be high, leading to improved heat resistance. It was also found that the insulating properties of the cured product were maintained by increasing the bending resistance before curing. Furthermore, it was found that the insulation of the sheet of Comparative Example 2, which cracked in the bending test (BDV of a composite molding evaluation sample hardened on a copper plate in a similar manner using the sheet after the bending test) was lower than the insulation of the sheet before the bending test and Examples 1 to 5, which did not crack in the bending test.
[0176] It has been confirmed that the thermosetting composition of the present invention, which contains a specific filler and resin, can provide a cured sheet that has high thermal conductivity, high insulation properties, and high heat resistance while maintaining the bending resistance of the uncured sheet.
Claims
1. A thermosetting composition containing an inorganic filler and a thermosetting compound, The content of the inorganic filler is 60% by mass or more relative to 100% by mass of the solid content in the thermosetting composition, The thermosetting compound includes an epoxy compound, the epoxy equivalent (WPE) of the component (referred to as the "resin component") excluding the solvent and the inorganic filler from the thermosetting composition is WPE≦250 g / eq; The thermosetting composition has a bending resistance φ of φ<20 mm, as determined by a mandrel test (JIS K5600-5-1) before curing.
2. 2. The thermosetting composition according to claim 1, wherein the resin component contains a polymeric epoxy compound (referred to as an "epoxy polymer") having a mass average molecular weight (Mw) of 5,000 or more in an amount of 5% by mass or more and 19% by mass or less.
3. 3. The thermosetting composition according to claim 2, wherein the epoxy polymer has a chemical structure represented by the following formula (1) and / or (2): (In formula (1), R 1 and R 2 Each of R represents an organic group, and at least one of them is an organic group having a molecular weight of 16 or more. 3 represents a divalent cyclic organic group.
4. 3. The thermosetting composition of claim 2, wherein the epoxy polymer has a chemical structure represented by the following formula (3): (In formula (3), R 4 , R 5 , R 6 , R 7 Each represents an organic group having a molecular weight of 15 or more.
5. 2. The thermosetting composition according to claim 1, which has a thermal conductivity in the thickness direction after curing of 15 W / m·K or more.
6. The thermosetting composition according to claim 1 , comprising a polyfunctional epoxy compound having three or more epoxy groups in one molecule.
7. The thermosetting composition according to claim 6, wherein the polyfunctional epoxy compound having three or more epoxy groups in one molecule has a mass average molecular weight (Mw) of 800 or less.
8. 7. The thermosetting composition according to claim 6, wherein the epoxy equivalent of the polyfunctional epoxy compound having three or more epoxy groups in one molecule is 50 g / equivalent or more and 200 g / equivalent or less.
9. The thermosetting composition according to claim 6, wherein the polyfunctional epoxy compound having three or more epoxy groups in one molecule is a polyfunctional epoxy compound having four epoxy groups in one molecule.
10. 7. The thermosetting composition according to claim 6, wherein a content ratio of the polyfunctional epoxy compound having three or more epoxy groups in one molecule is 5 mass% or more and 50 mass% or less with respect to 100 mass% of a solid content excluding the inorganic filler from the solid content of the thermosetting composition.
11. The thermosetting composition of claim 1 , comprising a compound having a heterocyclic structure containing a nitrogen atom.
12. 10. The thermosetting composition of claim 1, wherein the inorganic filler is agglomerated particles of boron nitride.
13. 13. The thermosetting composition of claim 12, wherein the boron nitride agglomerated particles have a house of cards structure.
14. A sheet-like cured product comprising the thermosetting composition according to any one of claims 1 to 13.
15. A composite molded article having a cured part made of the sheet-like cured product according to claim 14 and a metal part.
16. A semiconductor device comprising the composite compact of claim 15.
Citation Information
Patent Citations
Heat dissipation member, and manufacturing method of semiconductor module
JP2013089670A
Boron nitride aggregated particle, composition containing boron nitride aggregated particle, and three-dimensional integrated circuit having layer comprising the composition
JP2015006985A
Boron nitride aggregated particle, and method for producing the same, composition containing the same, and molding containing the same
JP2016135730A
Heat release resin sheet and device containing heat release resin sheet
JP2017036415A
Agglomerated boron nitride particles, production method for agglomerated boron nitride particles, resin composition including agglomerated boron nitride particles, moulded body, and sheet
WO2015119198A1