Composite cathode active material, cathode and lithium battery including the composite cathode active material, and method of preparing the composite cathode active material
A composite positive electrode active material with a lithium transition metal oxide core and a lithium nitrate-coated carbon-based shell addresses the degradation issues of nickel-based materials, improving lithium battery performance by enhancing ionic conductivity and preventing side reactions, thus increasing capacity retention and reducing resistance.
Patent Information
- Application Number
- JP2024046566
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-07
AI Technical Summary
Conventional nickel-based positive electrode active materials in lithium batteries suffer from side reactions that degrade performance and have insufficient thermal stability, necessitating a solution to prevent deterioration while maintaining high capacity.
A composite positive electrode active material is developed, comprising a lithium transition metal oxide core coated with a shell made of lithium nitrate and a conductive carbon-based composite, which includes a carbon-based material matrix and first metal oxides selected from specific groups of the periodic table, enhancing ionic conductivity and preventing side reactions.
The composite material improves initial efficiency, specific capacity, and resistance characteristics of lithium batteries, with improved capacity retention and reduced internal resistance, thereby enhancing the battery's high-rate and high-temperature cycle characteristics.
Smart Images

Figure 2024137911000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite positive electrode active material, a positive electrode and a lithium battery employing the same, and a method for producing the same. [Background technology]
[0002] In order to meet the trend of miniaturization and high performance of various devices, it is becoming important for lithium batteries to have high energy density in addition to miniaturization and weight reduction, i.e., high-capacity lithium batteries are becoming important.
[0003] In order to realize a lithium battery suitable for such applications, positive electrode active materials having high capacity are being investigated.
[0004] Conventional nickel-based positive electrode active materials have poor life characteristics due to side reactions and also lack sufficient thermal stability.
[0005] Therefore, a method is required that can prevent deterioration of battery performance while containing a nickel-based positive electrode active material. Summary of the Invention [Problem to be solved by the invention]
[0006] The problem to be solved by the present invention is to provide a new composite positive electrode active material that can suppress side reactions of the composite positive electrode active material, improve the reversibility of the electrode reaction, and prevent the deterioration of lithium performance.
[0007] Another problem to be solved by the present invention is to provide a positive electrode comprising the composite positive electrode active material.
[0008] Another problem to be solved by the present invention is to provide a lithium battery using the positive electrode.
[0009] Another object of the present invention is to provide a method for producing the composite positive electrode active material. [Means for solving the problem]
[0010] According to one aspect, a core containing a lithium transition metal oxide, and a shell disposed along the surface of the core, wherein the shell contains lithium nitrate (LiNO3) and a conductive carbon-based composite, and the conductive carbon-based composite has the chemical formula M b O b (0 < a ≤ 3, 0 < b < 4, and if a is 1, 2, or 3, then b is not an integer), one or more first metal oxides and a carbon-based material, the first metal oxide is disposed within the carbon-based material matrix, and M is one or more metals selected from Groups 2 to 13 of the Periodic Table of the Elements, Groups 15 and 16 of the Periodic Table of the Elements, a composite cathode active material is provided.
[0011] According to another aspect, a cathode including the composite cathode active material is provided.
[0012] According to still another aspect, a lithium battery including the cathode, an anode, and an electrolyte disposed between the cathode and the anode is provided.
[0013] According to still another aspect, providing a lithium transition metal oxide; providing a composite; mechanically milling the lithium transition metal oxide, the composite, and lithium nitrate, wherein the composite has the chemical formula M a O b (0 < a ≤ 3, 0 < b < 4, and if a is 1, 2, or 3, then b is not an integer), one or more first metal oxides and a carbon-based material, the first metal oxide is disposed within the carbon-based material matrix, and M is one or more metals selected from Groups 2 to 13 of the Periodic Table of the Elements, Groups 15 and 16 of the Periodic Table of the Elements, a method for manufacturing a composite cathode active material is provided. [Advantages of the Invention]
[0014] According to one embodiment, the composite positive electrode active material includes a shell containing a first metal oxide, a carbonaceous material, and lithium nitrate, thereby improving the initial efficiency, initial specific capacity, and resistance characteristics of the lithium battery, and improving the capacity retention rate. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 shows C1s X-ray photoelectron spectroscopy (XPS) spectra of the composite positive electrode active materials prepared in Example 3, Comparative Examples 1 and 2, and the bare NCA of Comparative Example 5. [Diagram 2] FIG. 1 shows O1s X-ray photoelectron spectroscopy (XPS) spectra of the composite positive electrode active materials prepared in Example 3, Comparative Examples 1 and 2, and bare NCA of Comparative Example 5. [Diagram 3] FIG. 1 shows Li1s X-ray photoelectron spectroscopy (XPS) spectra of the composite positive electrode active materials prepared in Example 3, Comparative Examples 1 and 2, and bare NCA of Comparative Example 5. [Figure 4] FIG. 1 shows Ni2p X-ray photoelectron spectroscopy (XPS) spectra of the composite positive electrode active materials prepared in Example 3, Comparative Examples 1 and 2, and bare NCA of Comparative Example 5. [Diagram 5] 1 is a graph showing the initial specific capacity and initial efficiency characteristics of lithium batteries prepared in Example 6, Comparative Examples 6 and 7, and Comparative Example 10. [Figure 6] 1 is a graph showing the capacity retention characteristics of lithium batteries produced in Example 6, Comparative Examples 6 and 7, and Comparative Example 10. [Figure 7] 1 is a schematic diagram of a lithium battery according to an embodiment. [Figure 8] FIG. 2 is a schematic diagram of a lithium battery according to another embodiment. [Figure 9] FIG. 2 is a schematic diagram of a lithium battery according to yet another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present inventive concept described below can be modified in various ways and can have various embodiments, but specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, they do not limit the present inventive concept to specific embodiments, and should be understood to include all modifications, equivalents, or alternatives that fall within the technical scope of the present inventive concept.
[0017] The terms used below are merely used to describe specific embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless otherwise clearly indicated in the context. In the following, terms such as "comprise" or "have" indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, and should be understood not to preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. In the following, " / " can be interpreted as "and" or "or" depending on the context.
[0018] In the drawings, thicknesses are exaggerated or reduced to clearly depict the various layers and regions. Similar parts are designated by the same reference numerals throughout the specification. Throughout the specification, when a part, such as a layer, film, region, or plate, is referred to as being "on" or "above" another part, this includes not only when it is directly on top of the other part, but also when there is another part between them. Throughout the specification, terms such as first and second may be used to describe various components, but the components are not limited by these terms. These terms are used only to distinguish one component from another.
[0019] Hereinafter, a composite positive electrode active material, a positive electrode and a lithium battery including the same, and a method for manufacturing the same according to exemplary embodiments will be described in more detail.
[0020] The composite positive electrode active material includes a core containing a lithium transition metal oxide and a shell disposed along the surface of the core, the shell including lithium nitrate (LiNO3) and a conductive carbon-based composite, the conductive carbon-based composite having a chemical formula M a O b (where 0 < a ≤ 3, 0 < b < 4, and if a is 1, 2, or 3, b is not an integer) and one or more first metal oxides represented by and a carbon-based material, the first metal oxide being disposed within a carbon-based material matrix, and M being one or more metals selected from Groups 2 to 13 of the periodic table of the elements, Group 15, and Group 16 of the periodic table of the elements.
[0021] Hereinafter, the theoretical basis for the excellent effects provided by the composite positive electrode active material according to one embodiment will be described, which is for the purpose of assisting the understanding of the inventive concept and is not intended to limit the inventive concept in any way.
[0022] On the core of the composite positive electrode active material, a shell including a conductive carbon-based composite containing a first metal oxide and a carbon-based material and lithium nitrate is disposed. The lithium nitrate in the shell forms a chemical bond with the carbon-based material and / or the first metal oxide included in the shell. The lithium nitrate contained in the shell increases the ion conduction of the composite positive electrode active material.
[0023] In addition to lithium nitrate, the shell may further contain one or more selected from LiNO2, Li3N, and LiN x O y (where 0.5 ≤ x ≤ 1, 2 ≤ y ≤ 3.5, for example, 3 ≤ y ≤ 3.5). LiNO2, Li3N, and LiN x O yAt least one selected from (0.5≦x≦1, 2≦y≦3.5, for example, 3≦y≦3.5) is formed by decomposition of LiNO3 through a physicochemical reaction caused by frictional energy generated during mixing with the graphene balls, and if such a component is further contained, the ion conductivity can be improved. As a result, a composite positive electrode active material with improved high rate characteristics and capacity retention, and improved specific capacity due to improved efficiency can be manufactured.
[0024] LiN x O y In the formula, the ratio of x to y is, for example, 1:2 to 1:3.
[0025] The content of lithium nitrate in the shell is 3 wt% or less, 2 wt% or less, 1 wt% or less, 0.1 to 1 wt%, 0.1 to 0.5 wt%, 0.1 to 0.3 wt%, 0.2 to 0.3 wt%, or 0.2 to 0.3 wt%, based on 100 wt% of the total weight of the composite positive electrode active material. The content of lithium nitrate in the shell is, for example, 0.2 to 0.3 wt%, or 0.25 to 0.3 wt%. When the content of lithium nitrate is within the above range, the ionic conductivity is improved without decreasing the weight and volume energy density, and a composite positive electrode active material having excellent high rate and life characteristics can be obtained.
[0026] In the shell, LiNO3, LiNO2, Li3N and LiN x O y The mixing molar ratio with one or more components selected from (0.5≦x≦1, 3≦y≦3.5) may be 10:1 to 1:1, 5:1 to 1:1, or 3:1 to 1:1.
[0027] Conventional carbon-based materials are easily aggregated, making it difficult to uniformly coat the core. In contrast, in the composite positive electrode active material, a carbon-based material matrix and a composite containing a plurality of first metal oxides disposed therein are used, and a uniform shell is disposed on the core while preventing the aggregation of the carbon-based material. Therefore, by effectively blocking the contact between the core and the electrolyte, side reactions due to the contact between the core and the electrolyte are prevented. In addition, the generation of a resistance layer is suppressed by suppressing cation mixing by the electrolyte. In addition, the elution of transition metal ions is also suppressed. The carbon-based material is, for example, a crystalline carbon-based material. The carbon-based material is, for example, a carbon-based nanostructure. The carbon-based material is, for example, a carbon-based two-dimensional nanostructure. The carbon-based material is, for example, graphene. In this case, the shell containing graphene and / or its matrix has flexibility, so that it can easily accommodate the volume change of the composite positive electrode active material during charging and discharging, thereby suppressing the occurrence of cracks inside the composite positive electrode active material. Graphene has high electronic conductivity, so that the interface resistance between the composite positive electrode active material and the electrolyte is reduced. Therefore, despite the introduction of the graphene-containing shell, the internal resistance of the lithium battery is maintained or reduced.
[0028] In the composite positive electrode active material according to an embodiment, in the shell mainly composed of a carbon-based material, for example, a chemical bond between the carbon-based material and lithium nitrate facilitates the conduction of electrons and ions. In addition, the reversibility of the electrode reaction on the surface of the composite positive electrode active material may be increased, and the conductivity of the electrode may be increased. As a result, the cycle characteristics and charge / discharge capacity of a battery including such a composite positive electrode active material may be improved.
[0029] The carbonaceous material contained in the shell of the composite positive electrode active material is derived from a graphene matrix, and therefore has a relatively low density and a high porosity compared to conventional carbonaceous materials derived from graphite-based materials. The d002 interplanar distance of the carbonaceous material contained in the shell of the composite positive electrode active material may be, for example, 3.38 Å or more, 3.40 Å or more, 3.45 Å or more, 3.50 Å or more, 3.60 Å or more, 3.80 Å or more, or even 4.00 Å or more. The d002 interplanar distance of the carbonaceous material contained in the shell of the composite positive electrode active material may be, for example, 3.38 to 4.0 Å, 3.38 to 3.8 Å, 3.38 to 3.6 Å, 3.38 to 3.5 Å, or 3.38 to 3.45 Å. In contrast, the d002 interplanar distance of conventional carbon-based materials derived from graphite-based materials is, for example, 3.38 Å or less, or even 3.35 to 3.38 Å.
[0030] The first metal oxide has a voltage resistance and can prevent the lithium transition metal oxide contained in the core from deteriorating during charging and discharging at high voltages. The shell can contain, for example, one type of first metal oxide or two or more different types of first metal oxides.
[0031] As a result, the high rate performance of lithium batteries containing the aforementioned composite positive electrode active materials is improved, as well as the high temperature and high voltage cycling characteristics. According to one embodiment, the content of the composite is 3 wt% or less, 2 wt% or less, or 1 wt% or less based on 100 wt% of the total weight of the composite positive electrode active material. According to another embodiment, the content of the composite is 0.01 to 3 wt%, 0.1 to 2 wt%, or 0.1 to 1 wt% based on 100 wt% of the total weight of the composite positive electrode active material.
[0032] In an embodiment, the content of the composite may be 3 wt % or less, 2 wt % or less, or 1 wt % or less, based on 100 wt % of the total weight of the composite positive electrode active material.
[0033] According to another embodiment, the content of the composite may be, for example, about 0.01 wt% to about 3 wt%, about 0.1 wt% to about 2 wt%, or about 0.1 wt% to about 1 wt% based on the total weight of the composite positive electrode active material. In the composite positive electrode active material, the content of the shell may be, for example, 3 wt% or less, 2 wt% or less, 1 wt% or less, 0.1 to 1 wt%, 0.1 to 3 wt%, 0.3 to 3 wt%, 0.4 to 3 wt%, 0.3 to 3 wt%, 0.4 to 3 wt%, 0.5 wt% to 3 wt%, 0.5 wt% to 2.5 wt%, 0.5 wt% to 2 wt%, or 0.5 wt% to 1.5 wt% of the total weight of the composite positive electrode active material. The content of the first metal oxide may be, for example, 0.3 wt% to 1.8 wt%, 0.3 wt% to 1.5 wt%, 0.3 wt% to 1.2 wt%, or 0.3 wt% to 0.9 wt% of the total weight of the composite positive electrode active material. When the composite positive electrode active material contains the shell and the first metal oxide in such a content range, the cycle characteristics of the lithium battery are further improved.
[0034] The content of the first metal contained in the shell is, for example, 1 to 10 at%, 1 to 9 at%, 2 to 9 at%, 2 to 8 at%, 3 to 8 at%, 3 to 7 at%, 4 to 7 at%, or 4 to 6 at% based on the total number of atoms in the shell. When the shell contains the first metal having such a content range, the cycle characteristics of a lithium battery including the composite positive electrode active material can be further improved. The content of the first metal element contained in the shell can be determined, for example, from a peak obtained by measuring an X-ray photoelectron spectroscopy (XPS) spectrum of the surface of the composite positive electrode active material.
[0035] The oxygen (O) content of the shell is, for example, 1 to 20 at%, 1 to 18 at%, 3 to 18 at%, 3 to 16 at%, 5 to 16 at%, 5 to 14 at%, 7 to 14 at%, or 7 to 12 at% based on the total number of atoms in the shell. The oxygen content of the shell in this range can further improve the cycle characteristics of a lithium battery including the composite positive electrode active material. The oxygen (O) content of the shell can be determined, for example, from a peak obtained by measuring the X-ray photoelectron spectroscopy (XPS) spectrum of the surface of the composite positive electrode active material.
[0036] The nitrogen (N) content of the shell is, for example, 1 to 12 at%, 2 to 12 at%, 2 to 11 at%, 3 to 11 at%, 3 to 10 at%, 4 to 10 at%, 4 to 9 at%, 5 to 9 at%, 5 to 8 at%, or 5 to 7 at% based on the total number of atoms of the shell. The nitrogen content of the shell in this range can further improve the cycle characteristics of a lithium battery including the composite positive electrode active material. The nitrogen (N) content of the shell can be determined, for example, from a peak obtained by measuring the X-ray photoelectron spectroscopy (XPS) spectrum of the surface of the composite positive electrode active material.
[0037] The carbon content of the shell is, for example, 65 to 99 at%, 70 to 99 at%, 75 to 99 at%, 80 to 99 at%, 80 to 95 at%, 80 to 93 at%, 80 to 91 at%, or 83 to 90 at% based on the total number of atoms in the shell. The carbon content of the shell in this range can further improve the cycle characteristics of a lithium battery including the composite positive electrode active material. The carbon content of the shell can be determined, for example, from a peak obtained by measuring the X-ray photoelectron spectroscopy (XPS) spectrum of the surface of the composite positive electrode active material.
[0038] The metal contained in the first metal oxide is also one or more selected from, for example, Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se. The first metal oxide is, for example, Al2O z (0 < z < 3), NbO x (0 < x < 2.5), MgO x (0 < x < 1), Sc2O z (0 < z < 3), TiO y (0 < y < 2), ZrO y (0 < y < 2), V2O z (0 < z < 3), WO y (0 < y < 2), MnO y (0 < y < 2), Fe2O z (0 < z < 3), Co3O w (0 < w < 4), PdO x (0 < x < 1), CuO x (0 < x < 1), AgO x (0 < x < 1), ZnO x (0 < x < 1), Sb2O z (0 < z < 3) and SeO y (0 < y < 2) is also one or more selected from. By disposing such a first metal oxide in the matrix of the carbon-based material, the uniformity of the shell disposed on the core is improved, and the withstand voltage property of the composite positive electrode active material is further improved. For example, the shell contains Al2O x (0 < x < 3) as the first metal oxide.
[0039] The shell has the chemical formula M a O cIt may further contain one or more second metal oxides represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer). The M is one or more metals selected from Groups 2 to 13 of the periodic table, Groups 15 and 16 of the periodic table. For example, the second metal oxide contains the same metal as the first metal oxide, and the ratio c / a of a and c of the second metal oxide has a larger value than the ratio b / a of a and b of the first metal oxide. For example, c / a > b / a. The second metal oxide is selected from, for example, Al2O3, NbO, NbO2, Nb2O5, MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, and SeO2. The first metal oxide is a reduction product of the second metal oxide. The first metal oxide is obtained by reducing part or all of the second metal oxide. Therefore, the first metal oxide has a lower oxygen content and a higher oxidation number of the metal than the second metal oxide. For example, the shell is the first metal oxide Al2O x It contains (0 < x < 3) and Al2O3 which is a second metal oxide.
[0040] In the composite positive electrode active material, for example, the carbon-based material contained in the shell and the transition metal of the lithium transition metal oxide contained in the core are chemically bonded via a chemical bond. The carbon atom (C) of the carbon-based material contained in the shell and the transition metal (Me) of the lithium transition metal oxide are chemically bonded via, for example, an oxygen atom, via a C-O-Me bond (e.g., C-O-Ni bond or C-O-Co bond). The carbon-based material contained in the shell and the lithium transition metal oxide contained in the core are chemically bonded via a chemical bond, whereby the core and the shell are complexed. Therefore, it is distinguished from a mere physical mixture of the carbon-based material and the lithium transition metal oxide.
[0041] The first metal oxide and the carbon-based material contained in the shell are also chemically bonded together via a chemical bond. Here, the chemical bond is, for example, a covalent bond or an ionic bond. The covalent bond is, for example, a bond containing at least one of an ester group, an ether group, a carbonyl group, an amide group, a carbonate anhydride group, and an acid anhydride group. The ionic bond is, for example, a bond containing a carboxylate ion, an ammonium ion, an acyl cation group, or the like.
[0042] The thickness of the shell is, for example, 1 nm to 5 μm, 1 nm to 1 μm, 1 nm to 500 nm, 1 nm to 200 nm, 1 nm to 100 nm, 1 nm to 90 nm, 1 nm to 80 nm, 1 nm to 70 nm, 1 nm to 60 nm, 1 nm to 50 nm, 1 nm to 40 nm, 1 nm to 30 nm, or 1 nm to 20 nm. The conductivity of an electrode including the composite positive electrode active material is improved by having the shell have a thickness in such a range.
[0043] The composite positive electrode active material may further include, for example, a third metal doped on the core or a third metal oxide coated on the core. The shell may then be disposed on the doped third metal or on the coated third metal oxide. For example, the surface of the lithium transition metal oxide contained in the core may be doped with a third metal, or the surface of the lithium transition metal oxide may be coated with a third metal oxide, and then a shell may be disposed on the third metal and / or the third metal oxide. For example, the composite positive electrode active material may include a core, an intermediate layer disposed on the core, and a shell disposed on the intermediate layer, and the intermediate layer may include a third metal or a third metal oxide. The third metal may be one or more metals selected from Al, Zr, W, and Co, and the third metal oxide may be Al2O3, Li2O-ZrO2, WO2, CoO, Co2O3, Co3O4, etc. The shell of the composite positive electrode active material includes, for example, one or more selected from lithium nitrate, a conductive carbon composite, and a milling result of the conductive carbon composite, and the conductive carbon composite includes a first metal oxide and a carbon-based material, such as graphene, and the first metal oxide is disposed in a matrix of the carbon-based material, such as a graphene matrix. The shell is, for example, manufactured from a composite including a first metal oxide, a carbon-based material, such as graphene, and lithium nitrate. The composite may further include a second metal oxide in addition to the first metal oxide. The composite may, for example, include two or more kinds of first metal oxides. The composite may, for example, include two or more kinds of first metal oxides and two or more kinds of second metal oxides.
[0044] The conductive carbon composite and / or milled product thereof may be contained in the composite positive electrode active material in an amount of 3 wt% or less, 2 wt% or less, 1 wt% or less, 0.5 wt% or less, or 0.2 wt% or less based on the total weight of the composite positive electrode active material. The conductive carbon composite and / or milled product thereof may be contained in an amount of 0.01 wt% to 3 wt%, 0.01 wt% to 1 wt%, 0.01 wt% to 0.7 wt%, 0.01 wt% to 0.5 wt%, 0.01 wt% to 0.2 wt%, 0.01 wt% to 0.1 wt%, or 0.03 wt% to 0.07 wt% based on the total weight of the composite positive electrode active material. When the composite positive electrode active material contains one or more of the composite and / or milled product thereof in such a range, the cycle characteristics of a lithium battery including the composite positive electrode active material are further improved.
[0045] The average particle size (e.g., D50) of one or more selected from the first metal oxide and the second metal oxide contained in the composite is 1 nm to 1 μm, 1 nm to 500 nm, 1 nm to 200 nm, 1 nm to 100 nm, 1 nm to 70 nm, 1 nm to 50 nm, 1 nm to 30 nm, 3 nm to 30 nm, 3 nm to 25 nm, 5 nm to 25 nm, 5 nm to 20 nm, 7 nm to 20 nm, or 7 nm to 15 nm. The first metal oxide and / or the second metal oxide may have such a nano-range particle size, so that they can be more uniformly distributed in the carbon-based material matrix of the composite. Thus, such a composite may be uniformly coated on the core without agglomeration to form a shell. The first metal oxide and / or the second metal oxide may have such a particle size range, so that they can be more uniformly distributed on the core. Therefore, by uniformly disposing the first metal oxide and / or the second metal oxide on the core, the voltage resistance characteristic can be more effectively exhibited.
[0046] The average particle size of the first metal oxide and the second metal oxide is measured, for example, using a measuring device of the laser diffraction method or the dynamic light scattering method. The average particle size is measured, for example, using a laser scattering particle size distribution meter (e.g., LA-920 (HORIBA, Ltd.)) and is the median particle size (D50) value when 50% of the particles are accumulated from the smallest particle side in volume conversion.
[0047] The uniformity deviation of one or more of the first metal oxide and the second metal oxide contained in the composite is 3% or less, 2% or less, or 1% or less. The uniformity can be determined, for example, by X-ray photoelectron spectroscopy (XPS). Thus, in the composite, one or more of the first metal oxide and the second metal oxide may be uniformly distributed with a deviation of 3% or less, 2% or less, or 1% or less.
[0048] The carbon-based material included in the composite may have, for example, a branched structure, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed within the branched structure of the carbon-based material. The branched structure of the carbon-based material may include, for example, a plurality of carbon-based material particles that are in contact with each other. The branched structure of the carbon-based material may provide multiple conductive paths.
[0049] The carbon-based material included in the composite may be, for example, graphene. The graphene may have, for example, a branched structure, and one or more metal oxides selected from a first metal oxide and a second metal oxide may be distributed within the branched structure of the graphene. The branched structure of the graphene may include, for example, a plurality of graphene particles that are in contact with each other. The branched structure of the graphene may provide various conductive paths.
[0050] The carbon-based material contained in the composite may have, for example, a spherical structure, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of the carbon-based material may be 50 nm to 300 nm. There may be a plurality of carbon-based materials having the spherical structure. Since the carbon-based material has a spherical structure, the composite may have a robust structure.
[0051] The carbon-based material included in the composite may be, for example, graphene. The graphene may have, for example, a spherical structure, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of graphene may be 50 nm to 300 nm. There may be a plurality of graphenes having a spherical structure. Since the graphene has a spherical structure, the composite may have a robust structure.
[0052] The carbon-based material included in the composite may have a spiral structure in which a plurality of spherical structures are connected, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed within the spiral structure. The size of the spiral structure of the carbon-based material may be 500 nm to 100 μm. Since the carbon-based material has a spiral structure, the composite may have a robust structure.
[0053] The carbon-based material included in the composite may be, for example, graphene. The graphene may have a helical structure in which a plurality of spherical structures are connected, and one or more metal oxides selected from a first metal oxide and a second metal oxide may be distributed within the helical spherical structures. The helical structure of graphene may have a size of 500 nm to 100 μm. Since the graphene has a helical structure, the composite may have a robust structure.
[0054] The carbon-based material included in the composite may have a cluster structure in which a plurality of spherical structures are aggregated, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structures of the cluster structure. The size of the cluster structure of the carbon-based material may be 0.5 mm to 10 cm. Since the carbon-based material has a cluster structure, the composite may have a robust structure.
[0055] The carbon-based material included in the composite may be, for example, graphene. The graphene may have a cluster structure in which a plurality of spherical structures are aggregated, and one or more metal oxides selected from a first metal oxide and a second metal oxide may be distributed within the spherical structures of the cluster structure. The size of the graphene cluster structure may be 0.5 mm to 10 cm. Since the graphene has a cluster structure, the composite may have a robust structure.
[0056] The composite may be, for example, a wrinkled polyhedral ball structure, and one or more selected from the first metal oxide and the second metal oxide may be distributed inside or on the surface of the structure. Because the composite has such a polyhedral ball structure, the composite may be easily coated on the irregular surface irregularities of the core.
[0057] The composite may be, for example, a planar structure, and one or more selected from the first metal oxide and the second metal oxide may be distributed inside or on the surface of the structure. Because the composite has such a two-dimensional planar structure, the composite may be easily coated on the irregular surface irregularities of the core.
[0058] The carbonaceous material contained in the composite extends from the first metal oxide by a distance of 10 nm or less and includes at least 1 to 20 carbonaceous material layers. For example, a carbonaceous material having a total thickness of 12 nm or less can be disposed on the first metal oxide by stacking a plurality of carbonaceous material layers. For example, the total thickness of the carbonaceous material can be 0.6 to 12 nm.
[0059] The carbon-based material contained in the composite may be, for example, graphene. The graphene extends from the first metal oxide by a distance of 10 nm or less and includes at least 1 to 20 graphene layers. For example, a plurality of graphene layers may be stacked to provide graphene having a total thickness of 12 nm or less on the first metal oxide. For example, the total thickness of the graphene may be 0.6 to 12 nm.
[0060] The core of the composite positive electrode active material may include, for example, a lithium transition metal oxide represented by the following formula 1: [Chemical formula 1] Li a Ni x Co y M z O 2-b A b In the above Chemical Formula 1, 0.9≦a≦1.2, 0.8≦x≦0.95, 0≦y≦0.2, 0 <z≦0.2であり、x+y+z=1であり、 M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), or a combination thereof; A is F, S, Cl, Br, or a combination thereof. In chemical formula 1, 1.0≦a≦1.2, 0.8≦x≦0.95, 0≦y≦0.2, 0 <z≦0.2であり、x+y+z=1である。
[0061] The core of the composite positive electrode active material may include, for example, one or more selected from the lithium transition metal oxides represented by the following formulas 2 to 4: [Chemical formula 2] LiNi x Co y Mn z O2 [Chemical formula 3] LiNix Co y Al z O2 In the above formulas 2 and 3, 0.8≦x≦0.95, 0 <y≦0.2、0<z≦0.2であり、x+y+z=1である。 [Chemical formula 4] LiNi x Co y Mn v Al w O2 In the above formula 4, 0.8≦x≦0.95, 0 <y≦0.2、0<v≦0.2、0<w≦0.2であり、x+y+v+w=1である。
[0062] The lithium transition metal oxides of Formulas 1 to 4 may have a high nickel content of 80 mol% or more, 85 mol% or more, or 90 mol% or more based on the total transition metal moles, and may provide excellent initial capacity, room temperature life characteristics, and high temperature life characteristics. For example, in the lithium transition metal oxides of Formulas 1 to 4, the nickel content is 80 mol% to 95 mol%, 85 mol% to 95 mol%, or 90 mol% to 95 mol% based on the total transition metal moles.
[0063] The core of the composite positive electrode active material may include, for example, a lithium transition metal oxide represented by the following formulas 5 to 6: [Chemical formula 5] Li a Co x M y O 2-b A b In the above Chemical Formula 5, 1.0≦a≦1.2, 0≦b≦0.2, 0.9≦x≦1, 0≦y≦0.1, and x+y=1; M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), or a combination thereof; and A is F, S, Cl, Br, or a combination thereof. [Chemical formula 6] LiCoO2
[0064] According to another embodiment, a positive electrode includes the composite positive electrode active material, which provides improved cycle characteristics and increased conductivity.
[0065] The positive electrode can be produced, for example, by the following exemplary method, but is not necessarily limited to such a method, and can be adjusted according to required conditions.
[0066] First, the composite positive electrode active material, a conductive material, a binder, and a solvent are mixed to prepare a positive electrode active material composition. The prepared positive electrode active material composition is directly coated on a positive electrode current collector and dried to manufacture a positive electrode plate having a positive electrode active material layer. Alternatively, the positive electrode active material composition is cast on a separate support and then peeled off from the support to obtain a film, which is then laminated on the positive electrode current collector to manufacture a positive electrode plate having a positive electrode active material layer.
[0067] Examples of conductive materials that can be used include denka black, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, ketjen black, carbon fibers, carbon nanotubes, metal powders, metal fibers or metal tubes such as copper, nickel, aluminum, and silver, and conductive polymers such as polyphenylene derivatives, but are not limited to these. Any material that is used as a conductive material in the relevant technical field can be used.
[0068] Examples of binders that can be used include vinylidene fluoride / hexafluoropropylene copolymers, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the aforementioned polymers, and styrene-butadiene rubber-based polymers. Examples of solvents that can be used include, but are not limited to, N-methylpyrrolidone (NMP), acetone, and water, and any solvent that is used in the relevant technical field can be used.
[0069] It is also possible to further add a plasticizer or pore-forming agent to the positive electrode active material composition to form pores inside the electrode plate.
[0070] The contents of the composite positive electrode active material, conductive material, binder, and solvent used in the positive electrode are at levels commonly used in lithium batteries, and one or more of the conductive material, binder, and solvent may be omitted depending on the application and configuration of the lithium battery.
[0071] The positive electrode may contain a binder in an amount of 0.1 to 10 wt %, or 0.1 to 5 wt %, based on the total weight of the positive electrode active material layer. The positive electrode may contain a composite positive electrode active material in an amount of 90 to 99 wt %, or 95 to 99 wt %, based on the total weight of the positive electrode active material layer.
[0072] The positive electrode may further include, in addition to the composite positive electrode active material, other common positive electrode active materials.
[0073] The common positive electrode active material may be any lithium-containing metal oxide that is generally used in the art, without any limitations. For example, one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used. Specific examples thereof include Li a A 1-b B b D2 (wherein, in the formula, 0.90≦a≦1 and 0≦b≦0.5); Li a E 1-b B b O 2-c D c (wherein, 0.90≦a≦1, 0≦b≦0.5, and 0≦c≦0.05); LiE 2-b B b O 4-c D c (wherein, 0≦b≦0.5 and 0≦c≦0.05); Li a Ni 1-b-c Co b B c D α(wherein, in the formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Co b B c O 2-α F' α (wherein, in the formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Co b B c O 2-α F'2 (wherein, in the above formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c D α (wherein, in the formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Mn b B c O 2-α F' α (wherein, in the formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c O 2-α F'2 (wherein, in the above formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni b E c G d O2 (wherein the formula is 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, and 0.001≦d≦0.1); Li a Ni b Co c Mn d G e O2 (wherein the formula is 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, and 0.001≦e≦0.1); Li a NiG b O2 (wherein, in the above formula, 0.90≦a≦1, 0.001≦b≦0.1); Li a CoGb O2 (wherein, in the above formula, 0.90≦a≦1, 0.001≦b≦0.1); Li a MnG b O2 (wherein, in the above formula, 0.90≦a≦1, 0.001≦b≦0.1); Li a Mn2G b O4 (wherein the above formula is 0.90≦a≦1, 0.001≦b≦0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0≦f≦2);Li (3-f) A compound represented by any one of the chemical formulas Fe2(PO4)3(0≦f≦2);LiFePO4 can be used.
[0074] In the chemical formula representing the aforementioned compound, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F' is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; and J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof.
[0075] It is also possible to use a compound in which a coating layer is added to the surface of the aforementioned compound, and it is also possible to use a mixture of the aforementioned compound and a compound to which a coating layer is added. The coating layer added to the surface of the aforementioned compound includes, for example, a coating element compound such as an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, or a hydroxycarbonate of a coating element. The compound forming such a coating layer is amorphous or crystalline. The coating element contained in the coating layer is Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method of forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method is, for example, a spray coating method, a dipping method, etc. A detailed description of the specific coating method is omitted because it is a content that can be fully understood by those engaged in the field.
[0076] The positive electrode current collector is, for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector can be omitted. The thickness of the positive electrode current collector is, for example, 1 μm to 100 μm, 1 μm to 50 μm, 5 μm to 25 μm, or 10 μm to 20 μm.
[0077] The positive electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector may have such a structure, thereby reducing the weight of the electrode and, as a result, improving the energy density of the lithium battery.
[0078] According to still another embodiment, a lithium battery employs a positive electrode including the composite positive electrode active material described above.
[0079] A lithium battery employing a positive electrode containing the aforementioned composite positive electrode active material provides improved cycleability and thermal stability.
[0080] The lithium battery can be manufactured, for example, by the following exemplary method, but is not necessarily limited to such a method, and can be adjusted according to the required conditions.
[0081] First, the positive electrode is produced by the above-mentioned positive electrode production method.
[0082] Next, the negative electrode is prepared as follows. The negative electrode is prepared in substantially the same manner as the positive electrode, except that, for example, a negative electrode active material is used instead of the composite positive electrode active material. In addition, in the negative electrode active material composition, the conductive material, binder, and solvent can be substantially the same as those in the positive electrode.
[0083] For example, a negative active material, a conductive material, a binder, and a solvent are mixed to prepare a negative active material composition, which is then directly coated onto a negative current collector to prepare a negative plate. Alternatively, the prepared negative active material composition is cast onto a separate support, and the negative active material film peeled off from the support is laminated onto a copper current collector to prepare a negative plate.
[0084] The negative electrode active material may be any material that is used as a negative electrode active material for lithium batteries in the art, for example, at least one selected from the group consisting of lithium metal, metals that can be alloyed with lithium, transition metal oxides, non-transition metal oxides, and carbon-based materials.
[0085] Examples of metals that can be alloyed with lithium include Si, Sn, Al, Ge, Pb, Bi, Sb, Si-Y alloys (wherein Y is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, or a combination thereof, and is not Si), and Sn-Y alloys (wherein Y is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, or a combination thereof, and is not Sn). The element Y is, for example, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof.
[0086] The transition metal oxide is, for example, lithium titanium oxide, vanadium oxide, lithium vanadium oxide, or the like.
[0087] Non-transition metal oxides include, for example, SnO2, SiO x (0 <x<2)などである。
[0088] The carbon-based material may be, for example, crystalline carbon, amorphous carbon, or a mixture thereof. The crystalline carbon may be, for example, graphite, such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite. The amorphous carbon may be, for example, soft carbon (low-temperature sintered carbon) or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0089] The contents of the negative electrode active material, conductive material, binder, and solvent are at levels commonly used in lithium batteries, and one or more of the conductive material, binder, and solvent may be omitted depending on the application and configuration of the lithium battery.
[0090] The negative electrode contains a binder of, for example, 0.1 to 10 wt %, or 0.1 to 5 wt %, based on the total weight of the negative electrode active material layer. The negative electrode contains a conductive material of, for example, 0.1 to 10 wt %, or 0.1 to 5 wt %, based on the total weight of the negative electrode active material layer. The negative electrode contains a negative active material of, for example, 90 wt % to 99 wt %, or 95 wt % to 99 wt %, based on the total weight of the negative electrode active material layer. When the negative electrode active material is lithium metal, the negative electrode does not contain a binder or a conductive material.
[0091] The negative electrode current collector is, for example, made of a material that does not react with lithium, i.e., does not form any alloy or compound. The material constituting the negative electrode current collector is, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co) and nickel (Ni), but is not necessarily limited thereto, and any material that is used as an electrode current collector in the relevant technical field is possible. The negative electrode current collector may be made of one of the above-mentioned metals, or may be made of an alloy of two or more metals, or a coating material. The negative electrode current collector is, for example, in the form of a plate or foil.
[0092] The negative electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The negative electrode current collector may have such a structure, thereby reducing the weight of the electrode and, as a result, improving the energy density of the lithium battery. The metal layer may act as an electrochemical fuse and be cut off in the event of an overcurrent, thereby performing a short circuit prevention function. The thickness of the metal layer may be adjusted to adjust the limit current and maximum current. The metal layer may be electrodeposited or deposited on the base film. When the thickness of the metal layer is reduced, the limiting current and / or maximum current of the negative electrode current collector is reduced, and thus the stability of the lithium battery during a short circuit can be improved. A lead tab can be added on the metal layer for connection to the outside. The lead tab can be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, or the like. During welding, the base film and / or the metal layer can melt, and the metal layer can be electrically connected to the lead tab. To further strengthen the welding between the metal layer and the lead tab, a metal chip can be added between the metal layer and the lead tab. The metal chip can be a thin piece of the same material as the metal of the metal layer. The metal chip can be, for example, a metal foil, a metal mesh, or the like. The metal chip can be, for example, an aluminum foil, a copper foil, a SUS foil, or the like. The lead tab can be welded to the metal chip / metal layer laminate or the metal chip / metal layer / base film laminate by disposing the metal chip on the metal layer and then welding it to the lead tab.During welding, the base film, the metal layer, and / or the metal chip may be melted, and the metal layer or the metal layer / metal chip laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal layer. The thickness of the base film may be, for example, 1 to 50 μm, 1.5 to 50 μm, 1.5 to 40 μm, or 1 to 30 μm. When the base film has a thickness in such a range, the weight of the electrode assembly may be more effectively reduced. The melting point of the base film may be, for example, 100 to 300° C., 100 to 250° C., or 100 to 200° C. When the base film has a melting point in such a range, the base film may be melted during the process of welding the lead tab, and may be easily bonded to the lead tab. In order to improve the adhesion between the base film and the metal layer, a surface treatment such as a corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to 1 μm. When the metal layer has a thickness in such a range, it is possible to maintain conductivity and ensure the stability of the electrode assembly. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. When the metal piece has a thickness in such a range, it is possible to more easily connect the metal layer and the lead tab. When the negative electrode current collector 21 has such a structure, it is possible to reduce the weight of the electrode, thereby improving the energy density.
[0093] Next, a separator to be inserted between the positive electrode and the negative electrode is prepared.
[0094] The separator may be any separator that is generally used in lithium batteries. For example, the separator has low resistance to the ion movement of the electrolyte and excellent electrolyte impregnation ability. The separator is, for example, selected from glass fiber, polyester, Teflon (registered trademark), polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or a combination thereof, and is in the form of a nonwoven or woven fabric. For example, a rollable separator such as polyethylene or polypropylene is used for a lithium ion battery, and a separator excellent in organic electrolyte impregnation ability is used for a lithium ion polymer battery.
[0095] The separator is manufactured by the following exemplary method, but is not necessarily limited to such method, and may be adjusted according to the required conditions.
[0096] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated on the top of an electrode and dried to form a separator. Alternatively, the separator composition is cast on a support and dried, and the separator film is peeled off from the support and laminated on the top of an electrode to form a separator.
[0097] The polymer used for the separator is not particularly limited, and any polymer that is used as a binder for electrode plates can be used, such as vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or a mixture thereof.
[0098] Next, the electrolyte is prepared.
[0099] The electrolyte is, for example, an organic electrolytic solution, which is produced, for example, by dissolving a lithium salt in an organic solvent.
[0100] The organic solvent can be any organic solvent used in the art.The organic solvent can be, for example, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethylsulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.
[0101] The lithium salt may be any of those used as lithium salts in the art. Examples of the lithium salt include LiPF, LiBF, LiSbF, LiAsF, LiClO, LiCF, Li(CFSO)N, LiC, F, SO, LiAlO, LiAlCl, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are natural numbers from 1 to 20), LiCl, LiI, or a mixture thereof.
[0102] Alternatively, the electrolyte is a solid electrolyte, such as, but not limited to, boron oxide, lithium oxynitride, or any other solid electrolyte known in the art, which may be formed on the negative electrode by a method such as sputtering, or a separate solid electrolyte sheet may be laminated on the negative electrode.
[0103] The solid electrolyte is, for example, an oxide-based solid electrolyte, a polymer solid electrolyte, or a sulfide-based solid electrolyte.
[0104] The solid electrolyte is, for example, an oxide-based solid electrolyte. The oxide-based solid electrolyte is Li 1+x+y Al x Ti 2-x S y P 3-y O 12 (0 <x<2、0≦y<3)、BaTiO3、Pb(Zr、Ti)O3(PZT)、Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≦x<1, O≦y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2、0<y<3)、Li x Al y Ti z (PO4)3(0 <x<2、0<y<1、0<z<3)、Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x S y P 3-y O 12 (0≦x≦1, 0≦y≦1), Li x La y TiO3(0 <x<2、0<y<3)、Li2O、LiOH、Li2CO3、LiAlO2、Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2、Li 3+x La3M2O 12 (M is Te, Nb or Zr, and x is an integer from 1 to 10). The solid electrolyte is prepared by a sintering method or the like. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12(M-doped LLZO) (where M is Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10, and 0 < a < 2) is a Garnet-type solid electrolyte selected therefrom.
[0105] Sulfide-based solid electrolytes also include, for example, those containing lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or combinations thereof. The sulfide-based solid electrolyte particles may also include Li2S, P2S5, SiS2, GeS2, B2S3, or combinations thereof. The sulfide-based solid electrolyte particles may also be Li2S or P2S5. The sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte contains Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte contains Li2S-P2S5, the mixed molar ratio of Li2S and P2S5 is also, for example, in the range of about 50:50 to about 90:10. Also, Li3PO4, halogen, halogen compounds, Li 2+2x Zn 1x GeO4 (LISICON) (0 ≤ x < 1), Li 3+y PO 4-x N x (LIPON) (0 < x < 4, 0 < y < 3), Li 3.25 Ge 0.25 P 0.75 S4 (ThioLISICON), Li2O-Al2O3-TiO2-P2O5 (LATP), etc., are inorganic solid electrolytes produced by adding to inorganic solid electrolytes of Li2S-P2S5, SiS2, GeS2, B2S3, or combinations thereof, and can be used as the sulfide solid electrolyte. Non-limiting examples of the sulfide solid electrolyte material are Li2S-P2S5; Li2S-P2S5-LiX (where X is a halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S-P2S5-Z m Sn (0 < m < 10, 0 < n < 10, Z = Ge, Zn or Ga); Li2S - GeS2; Li2S - SiS2 - Li3PO4; and Li2S - SiS2 - Li p MO q (0 < p < 10, 0 < q < 10, M is P, Si, Ge, B, Al, Ga or In). Accordingly, the sulfide - based solid electrolyte material can be produced by treating starting materials of the sulfide - based solid electrolyte substance (e.g., Li2S, P2S5, etc.) by a melt quenching method, a mechanical milling method, etc. Further, a firing step can be carried out after the treatment. The sulfide - based solid electrolyte can be amorphous, crystalline, or in a state where they are mixed. The polymer solid electrolyte is, for example, an electrolyte containing a mixture of a lithium salt and a polymer, or a polymer having an ion-conductive functional group. The polymer solid electrolyte is, for example, a polymer electrolyte that does not contain a liquid electrolyte.Examples of the polymer contained in the polymer solid electrolyte include polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene oxide (PEO), poly(styrene-b-ethylene oxide) block copolymer (PS-PEO), poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, polystyrene sulfonate (PSS), polyvinyl fluoride (PVF, Polyvinyl Fluoride), poly(methylmethacrylate) (PMMA), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyacrylonitrile (PAN), polyaniline, polyacetylene, Nafion, Aquivion, Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone), SPEEK, sulfonated poly(arylene ether ketone ketone), SPAEKKS, sulfonated poly(aryl ether ketone), ketone, SPAEK), poly[bis(benzimidazobenzisoquinolinones)], SPBIBI, poly(styrene sulfonate), PSS, and lithium 9,10-diphenylanthracene-2-sulfonate, DPASLi. +) or a combination thereof, but is not limited thereto, and any of those usable as a polymer electrolyte in the art can be used. Any of those usable as a lithium salt in the art can be used. Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (x and y are each 1 to 20), LiCl, LiI, or a mixture thereof. The gel electrolyte is, for example, a gel polymer electrolyte. The gel polymer electrolyte is, for example, an electrolyte including a liquid electrolyte and a polymer, or including an organic solvent and a polymer having an ion-conductive functional group. The liquid electrolyte is, for example, an ionic liquid, a mixture of a lithium salt and an organic solvent, a mixture of an ionic liquid and an organic solvent, or a mixture of a lithium salt, an ionic liquid and an organic solvent. The polymer may be selected from the polymers used in the solid polymer electrolyte. The organic solvent may be selected from the organic solvents used in the liquid electrolyte. The lithium salt may be selected from the lithium salts used in the solid polymer electrolyte. The ionic liquid refers to a salt that has a melting point below room temperature and is in a liquid state at room temperature, or a room temperature molten salt, which is composed of only ions. The ionic liquid may, for example, comprise: a) one or more cations selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazolium, and mixtures thereof; and b) BF4 - , PF6 - , AsF6 - , SbF6 - , AlCl4 - , HSO4 - , ClO4 - , CH3SO3 - , CF3CO2 - , Cl - , Br -, I - , SO4 - , CF3SO3 - , (FSO2)2N - , (C2F5SO2)2N - , (C2F5SO2)(CF3SO2)N - , and (CF3SO2)2N - and one or more compounds containing the anion. The solid polymer electrolyte may be impregnated with an electrolytic solution in a lithium battery to form a gel polymer electrolyte. The gel electrolyte may further include inorganic particles.
[0106] 7, a lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The positive electrode 3, the negative electrode 2, and the separator 4 are wound or folded to form a battery structure. The formed battery structure is housed in a battery case 5. An organic electrolyte is injected into the battery case 5, and the battery case 5 is sealed with a cap assembly 6 to complete the lithium battery 1. The battery case 5 is cylindrical, but is not necessarily limited to such a shape, and may be, for example, a square type, a thin film type, etc.
[0107] Referring to FIG. 8, a lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The separator 4 is disposed between the positive electrode 3 and the negative electrode 2, and the positive electrode 3, the negative electrode 2, and the separator 4 are wound or folded to form a battery structure 7. The formed battery structure 7 is housed in a battery case 5. The battery structure 7 also includes electrode tabs 8 that serve as electrical paths for conducting current generated in the battery structure 7 to the outside. An organic electrolyte is injected into the battery case 5 and sealed, completing the lithium battery 1. The battery case 5 is rectangular, but is not necessarily limited to such a shape, and may be, for example, cylindrical or thin-film type.
[0108] Referring to FIG. 9, a lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The separator 4 is disposed between the positive electrode 3 and the negative electrode 2 to form a battery structure. The battery structure 7 is stacked in a bi-cell structure and then housed in a battery case 5. The battery structure 7 also includes electrode tabs 8 that act as electrical paths for directing current generated in the battery structure 7 to the outside. An organic electrolyte is injected into the battery case 5 and sealed to complete the lithium battery 1. The battery case 5 is rectangular, but is not necessarily limited to such a shape and may be, for example, cylindrical or thin-film type.
[0109] The pouch-type lithium battery corresponds to the lithium batteries of FIGS. 7 to 9, in which a pouch is used as a battery case. The pouch-type lithium battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are stacked in a bi-cell structure, impregnated with an organic electrolyte, and housed in the pouch and sealed to complete the pouch-type lithium battery. For example, although not shown in the drawings, the above-mentioned positive electrode, negative electrode, and separator are simply stacked and housed in a pouch in the form of an electrode assembly, or wound into an electrode assembly in the form of a jelly roll, or folded and then housed in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed to complete the lithium battery.
[0110] Lithium batteries have excellent life characteristics and high rate characteristics, and are therefore used, for example, in electric vehicles (EVs), hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs), and fields requiring large amounts of power storage, such as electric bicycles and power tools.
[0111] Lithium batteries are stacked in multiple numbers to form a battery module, and multiple battery modules form a battery pack. Such a battery pack can be used in all devices that require high capacity and high output. For example, it can be used in notebook computers, smartphones, electric vehicles, etc. The battery module includes, for example, a plurality of batteries and a frame for positioning them. The battery pack includes, for example, a plurality of battery modules and a bus bar for connecting them. The battery module and / or the battery pack may further include a cooling device. A plurality of battery packs are regulated by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.
[0112] According to still another embodiment, a method for manufacturing a composite cathode active material includes providing a lithium transition metal oxide, providing a composite, and mechanically milling the lithium transition metal oxide, the composite, and lithium nitrate, where the composite has the chemical formula M a O b (where 0 < a ≤ 3, 0 < b < 4, and if a is 1, 2, or 3, b is not an integer), and includes one or more first metal oxides and a carbon-based material, the first metal oxide being disposed within a carbon-based material matrix, and M being one or more metals selected from Groups 2 to 13 of the Periodic Table of the Elements, Group 15, and Group 16 of the Periodic Table of the Elements. In the step of mechanical milling, the milling method is not particularly limited, and any method that can be used in the art as a method of bringing the lithium transition metal oxide and the composite into contact using a machine is possible.
[0113] A lithium transition metal oxide is provided. The lithium transition metal oxide is, for example, a compound represented by the aforementioned Chemical Formulas 1 to 6.
[0114] The step of providing the composite includes, for example, supplying a reaction gas composed of a carbon source gas to a structure containing a metal oxide and performing heat treatment to provide the composite.
[0115] The step of providing the composite includes, for example, M a O c supplying a reaction gas composed of a carbon source gas to one or more second metal oxides represented by (0 < a ≤ 3, 0 < c ≤ 4, and when a is 1, 2, or 3, b is an integer) and performing heat treatment to produce an undoped composite, wherein the M is one or more metals selected from Groups 2 to 13 of the Periodic Table of the Elements, Group 15, and Group 16 of the Periodic Table of the Elements. The reaction temperature can be raised to the heat treatment temperature (T). The time taken to raise the reaction temperature to the heat treatment temperature T can also be from 10 minutes to 4 hours. The heat treatment temperature (T) can also be from 700 °C to 1100 °C. The reaction time can be, for example, in the range of 4 hours to 8 hours. Subsequently, the heat-treated product can be cooled to room temperature to produce a composite material. The time taken to lower the reaction temperature from the heat treatment temperature T to room temperature can also be, for example, in the range of 1 hour to 5 hours.
[0116] The carbon source gas is a compound represented by the following Chemical Formula 7, or a mixed gas selected from one or more of the compound represented by the following Chemical Formula 7, the compound represented by the following Chemical Formula 8, and the oxygen-containing gas represented by the following Chemical Formula 9.
[0117] [Chemical Formula 7] CnH (2n+2-a) [OH] a In the above Chemical Formula 7, n is from 1 to 20, a is 0 or 1, [Chemical Formula 8] CnH 2n In the above Chemical Formula 8, n is from 2 to 6, [Chemical Formula 9] C x H y O z In the above Chemical Formula 9, x is 0, or an integer from 1 to 20, y is 0, or an integer from 1 to 20, and z is 1 or 2.
[0118] The compound represented by Chemical Formula 7 and the compound represented by Chemical Formula 8 are one or more selected from the group consisting of methane, ethylene, propylene, methanol, ethanol, and propanol. The oxygen-containing gas represented by Chemical Formula 9 includes, for example, carbon dioxide (CO2), carbon monoxide (CO), water vapor (H2O), or a mixture thereof.
[0119] M a O c After the step of supplying a reaction gas composed of a carbon source gas to the second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer) and performing heat treatment, a cooling step using one or more inert gases selected from the group consisting of nitrogen, helium, and argon can be further carried out. The cooling step refers to the step of adjusting to room temperature (20 - 25°C). The carbon source gas may also contain one or more inert gases selected from the group consisting of nitrogen, helium, and argon.
[0120] In the method for producing a composite, the process of growing a carbon-based material, such as graphene, by a gas-phase reaction can be carried out under various conditions.
[0121] According to the first condition, for example, M a O c First, methane is supplied to a reactor in which a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer) is arranged, and the temperature is raised to the heat treatment temperature (T). The temperature rising time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 700°C to 1,100°C. At the heat treatment temperature (T), heat treatment is carried out for a certain reaction time. The reaction time is, for example, 4 hours to 8 hours. The heat-treated product is cooled to room temperature to produce a composite. The time taken during the process of cooling from the heat treatment temperature (T) to room temperature is, for example, 1 hour to 5 hours.
[0122] According to the second condition, for example, M a O cFirst, hydrogen is supplied to a reactor in which a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer) is disposed, and the temperature is raised to a heat treatment temperature (T). The temperature rising time to the heat treatment temperature (T) is from 10 minutes to 4 hours, and the treatment temperature (T) is in the range of 700°C to 1,100°C. After heat treatment for a certain reaction time at the heat treatment temperature (T), methane gas is supplied, and heat treatment is carried out for the remaining reaction time. The reaction time is, for example, from 4 hours to 8 hours. The heat-treated product is cooled to room temperature to produce a composite. During the cooling process, nitrogen is supplied. The time taken for cooling from the heat treatment temperature (T) to room temperature is, for example, from 1 hour to 5 hours.
[0123] According to the third condition, for example, M a O c First, hydrogen is supplied to a reactor in which a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer) is disposed, and the temperature is raised to a heat treatment temperature (T). The temperature rising time to the heat treatment temperature (T) is from 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 700°C to 1,100°C. After heat treatment for a certain reaction time at the heat treatment temperature (T), a mixed gas of methane and hydrogen is supplied, and heat treatment is carried out for the remaining reaction time. The reaction time is, for example, from 4 hours to 8 hours. The heat-treated product is cooled to room temperature to produce a composite. During the cooling process, nitrogen is supplied. The time taken for cooling from the heat treatment temperature (T) to room temperature is, for example, from 1 hour to 5 hours.
[0124] In the process of producing the composite, when the carbon source gas contains water vapor, a composite having very excellent conductivity can be obtained. The content of water vapor in the gas mixture is not limited. For example, based on 100% by volume of the entire carbon source gas, it is from 0.01% to 10% by volume. The carbon source gas is, for example, methane, a mixed gas containing methane and an inert gas, or a mixed gas containing methane and an oxygen-containing gas.
[0125] The carbon source gas can be, for example, methane, a mixture of methane and carbon dioxide, or a mixture of methane, carbon dioxide, and water vapor. In the mixture of methane and carbon dioxide, the molar ratio of methane to carbon dioxide is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. In the mixture of methane, carbon dioxide, and water vapor, the molar ratio of methane to carbon dioxide to water vapor is about 1:0.20 to 0.50:0.01 to 1.45, about 1:0.25 to 0.45:0.10 to 1.35, or about 1:0.30 to 0.40:0.50 to 1.0.
[0126] The carbon source gas is, for example, carbon monoxide or carbon dioxide. The carbon source gas is, for example, a mixture of methane and nitrogen. In the mixture of methane and nitrogen, the molar ratio of methane to nitrogen is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, about 1:0.30 to 1:0.40. The carbon source gas does not include an inert gas such as nitrogen.
[0127] The heat treatment pressure can be selected taking into consideration the heat treatment temperature, the composition of the gas mixture, the amount of carbon coating desired, etc. The heat treatment pressure can be controlled by adjusting the amount of the gas mixture flowing in and the amount of the gas mixture flowing out. The heat treatment pressure is, for example, 0.5 atm or more, 1 atm or more, 2 atm or more, 3 atm or more, 4 atm or more, or 5 atm or more.
[0128] The heat treatment time is not particularly limited and can be appropriately adjusted according to the heat treatment temperature, the pressure during heat treatment, the composition of the gas mixture, and the amount of the desired carbon coating. For example, the reaction time at the heat treatment temperature is, for example, from 10 minutes to 100 hours, from 30 minutes to 90 hours, or from 50 minutes to 40 hours. For example, the greater the heat treatment time, the greater the amount of carbon deposited, for example, the amount of graphene (carbon), and thereby the electrical properties of the composite can be improved. However, such a tendency is not necessarily directly proportional to time. For example, after a predetermined time has elapsed, carbon deposition, for example, graphene deposition, may no longer occur or the deposition rate may decrease.
[0129] Through the gas-phase reaction of the aforementioned carbon source gas, even at a relatively low temperature, M a O c (where 0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, then c is an integer), and the reduced product thereof, M a O b (where 0 < a ≤ 3, 0 < b < 4, A is 1, 2, or 3, and b is not an integer), by providing a uniform carbon-based material coating, for example, a graphene coating, on one or more selected from the first metal oxides represented thereby, an undoped composite is obtained.
[0130] The composite has, for example, a matrix of a carbon-based material having one or more structures selected from a spherical structure, a helical structure in which a plurality of spherical structures are connected, a cluster structure in which a plurality of spherical structures are aggregated, and a sponge structure, for example, a graphene matrix, and M arranged within the matrix of the carbon-based material a O b (where 0 < a ≤ 3, 0 < b < 4, A is 1, 2, or 3, and b is not an integer), and the first metal oxide represented thereby, and M a O c (where 0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, then c is an integer), and one or more selected from the second metal oxides represented thereby.
[0131] Next, the lithium transition metal oxide, the composite, and the lithium nitrate are mechanically milled. A Nobilta mixer or the like can be used for milling. The rotation speed of the mixer during milling is, for example, 1,000 rpm to 2,500 rpm. If the milling speed is less than 1,000 rpm, the shear force applied to the lithium transition metal oxide, the composite, and the lithium nitrate is weak, so that the lithium transition metal oxide, the composite, and the lithium nitrate are unlikely to form a chemical bond. If the milling speed is too fast, the composite is carried out in an excessively short time, so that the composite and lithium nitrate are uniformly coated on the lithium transition metal oxide, and it is difficult to form a uniform and continuous shell. The milling time is, for example, 5 minutes to 100 minutes, 5 minutes to 60 minutes, or 5 minutes to 30 minutes. If the milling time is too short, the composite and lithium nitrate are uniformly coated on the lithium transition metal oxide, and it is difficult to form a uniform and continuous shell. If the milling time is too long, the production efficiency may be reduced.
[0132] The content of lithium nitrate is 3 wt% or less, 2 wt% or less, 1 wt% or less, 0.1 to 1 wt%, 0.1 to 0.5 wt%, 0.1 to 0.3 wt%, 0.2 to 0.3 wt%, or 0.25 to 0.3 wt%, based on 100 wt% of the total weight of the lithium transition metal oxide, the composite, and the lithium nitrate.
[0133] The content of the complex may be 3 wt% or less, 2 wt% or less, or 1 wt% or less of the total weight of the lithium transition metal oxide, the complex, and the lithium nitrate. The content of the complex may be, for example, 0.01 to 3 wt%, 0.1 to 2 wt%, or 0.1 to 1 wt% of the total weight of the lithium transition metal oxide, the complex, and the lithium nitrate. For example, the content of the complex may be 0.01 to 3 parts by weight, 0.1 to 3 parts by weight, 0.1 to 2 parts by weight, or 0.1 to 1 part by weight per 100 parts by weight of the mixture of the lithium transition metal oxide, the complex, and the lithium nitrate.
[0134] According to one embodiment, the total weight of lithium nitrate and the composite is, for example, 3% by weight or less, 2% by weight or less, 1% by weight or less, 0.1 to 1% by weight, or 0.1 to 0.5% by weight based on 100% by weight of the total weight of the lithium transition metal oxide, the composite, and lithium nitrate, and the mixing weight ratio of lithium nitrate and the composite is 1:3 to 3:1, 1:2 to 2:1, or 1:1.
[0135] The average particle size (D50) of the composite used for mechanical milling of the lithium transition metal oxide, the composite, and lithium nitrate is, for example, 1 μm to 20 μm, 3 μm to 15 μm, or 5 μm to 10 μm. And the average particle size of lithium nitrate is 10 to 2,000 nm, or 50 to 1,500 nm.
[0136] The present invention will be described in more detail through the following examples and comparative examples. However, these examples are for illustrative purposes only, and the scope of the present invention is not limited thereby.
[0137] (Production of Composite) Production example 1: Al 2 O 3 @Gr complex After placing Al2O3 particles (average particle size: about 20 nm) in the reactor, the internal temperature of the reactor was raised to 1,000 °C under the condition that CH4 was supplied at about 300 sccm and 1 atm for about 30 minutes in the reactor.
[0138] Subsequently, it was maintained at the above temperature for 7 hours for heat treatment. Subsequently, the internal temperature of the reactor was adjusted to room temperature (20 - 25 °C) to obtain a composite in which Al2O3 particles and Al2Oz (0 < z < 3) particles, which are reduction products thereof, were embedded in graphene.
[0139] The content of aluminum oxide (Al2O3 particles and Al2Oz (0 < z < 3) particles, which are reduction products thereof) contained in the composite was 60 wt%.
[0140] (Production of Composite Positive Electrode Active Material) Example 1: Al 2 O 3 @Gr composite 0.2wt% (aluminum oxide 0.12wt%) and LiNO 3 0.1wt% coating NCA91 LiNi 0.91 Co 0.05 Al 0.04 O2 (hereinafter referred to as NCA91 or NCA), lithium nitrate, and the composite obtained in Production Example 1 were milled for about 5 to 30 minutes at a rotation speed of about 1,000 to 2,000 rpm using a Nobilta Mixer (Hosokawa, Japan) to obtain a composite positive electrode active material.
[0141] The mixing weight ratio of NCA91, lithium nitrate, and the composite obtained in Production Example 1 was 99.7:0.1:0.2.
[0142] Example 2: Al 2 O 3 @Gr composite 0.2wt% (aluminum oxide 0.12wt%) and LiNO 3 0.2wt% coating NCA91 A composite positive electrode active material was prepared in the same manner as in Example 1, except that the mixing weight ratio of NCA91, lithium nitrate, and the composite obtained in Preparation Example 1 was changed to 99.6:0.2:0.2.
[0143] Example 3: Al 2 O 3 @Gr composite 0.2wt% (aluminum oxide 0.12wt%) and LiNO 3 0.3wt% coating NCA91 A composite positive electrode active material was prepared in the same manner as in Example 1, except that the mixing weight ratio of NCA91, lithium nitrate, and the composite obtained in Preparation Example 1 was changed to 99.5:0.3:0.2.
[0144] Comparative example 1: Al 2 O 3 @Gr complex 0.2wt% coating NCA91 LiNi 0.91 Co 0.05 Al 0.04 Instead of O2 (NCA91), lithium nitrate, and the composite obtained in Example 1, LiNi 0.91 Co 0.05 Al 0.04A composite positive electrode active material was prepared in the same manner as in Example 1, except that Al2O3@Gr@Gr composite was used. The mixing weight ratio of NCA91 to Al2O3@Gr composite was 99.8:0.2.
[0145] Comparative example 2: LiNO 3 Coating NCA91 LiNi 0.91 Co 0.05 Al 0.04 O2 (NCA91) and lithium nitrate were milled for about 5 to 30 minutes at a rotation speed of about 1,000 to 2,000 rpm using a Nobilta Mixer (Hosokawa, Japan) to obtain a composite positive electrode active material.
[0146] The mixing weight ratio of NCA91 to lithium nitrate was 99.7:0.3.
[0147] Comparative example 3: Al 2 O 3 @Gr composite coating NCA91 and LiNO 3 Coating NCA91 Blend The NCA91 and the composite obtained in Production Example 1 were milled for about 5 to 30 minutes at a rotation speed of about 1,000 to 2,000 rpm using a Nobilta Mixer (Hosokawa, Japan) to obtain a first composite positive electrode active material. Here, the mixing weight ratio of NCA91 and the composite obtained in Production Example 1 was 99.6:0.4.
[0148] The first composite positive electrode active material and the composite positive electrode active material obtained in Comparative Example 2 were mixed in a 1:1 mixing ratio by weight to obtain a composite positive electrode active material.
[0149] Comparative example 4: Al 2 O 3 @Gr and LiBr coated NCA91 A composite positive electrode active material was obtained in the same manner as in Example 1, except that LiBr was used instead of lithium nitrate.
[0150] Comparative example 5: bare NCA91 NCA91 was used as it is as the positive electrode active material.
[0151] (Manufacture of lithium batteries (half cells)) Example 4 (Production of positive electrodes) The composite positive electrode active material prepared in Example 1, a carbon conductive material (Denka Black), and polyvinylidene fluoride (PVdF) were mixed in a weight ratio of 96:2:2, and the mixture was mixed with N-methylpyrrolidone (NMP) in an agate mortar to prepare a slurry.
[0152] The slurry was bar coated on an aluminum current collector having a thickness of 15 μm, dried at room temperature, and then dried once more under vacuum at 120° C., followed by rolling and punching to prepare a positive electrode plate having a thickness of 55 μm.
[0153] Electrode loading level 10.5mg / cm 2 and the electrode mixture density was 3.6 g / cc.
[0154] (Coin cell manufacturing) Using the positive electrode plate prepared as described above, lithium metal was used as a counter electrode, a polytetrafluoroethylene (PTFE) separator was used as a separator, and a solution of 1.15M LiPF6 and 1.5wt% vinylene carbonate (VC) dissolved in ethylene carbonate (EC) + ethyl methyl carbonate (EMC) + dimethyl carbonate (DMC) (volume ratio of 2:4:4) was used as an electrolyte to prepare coin cells.
[0155] Examples 5 and 6 Coin cells were prepared in the same manner as in Example 4, except that the composite positive electrode active materials prepared in Examples 2 and 3 were used instead of the composite positive electrode active material prepared in Example 1.
[0156] Comparative Examples 6 to 10 A coin cell was fabricated in the same manner as in Example 4, except that the composite cathode active materials prepared in Comparative Examples 1 to 5 were used instead of the composite cathode active material produced in Example 1.
[0157] Evaluation example 1: X-ray photoelectron spectroscopy (XPS) spectrum evaluation In the manufacturing process of the undoped composite produced in Production Example 1, X-ray photoelectron spectroscopy (XPS) spectra were measured using Quantum 2000 (Physical Electronics) over time. X-ray photoelectron spectroscopy (XPS) spectra of the C 1s orbital and Al 2p orbital were measured for samples before heating, after 1 minute, after 5 minutes, after 30 minutes, after 1 hour, and after 4 hours, respectively. At the initial stage of heating, only the peak related to the Al 2p orbital was shown, and the peak related to the C 1s orbital was not shown. After 30 minutes, the peak related to the C 1s orbital was clearly shown, and the magnitude of the peak related to the Al 2p orbital was significantly reduced.
[0158] After 30 minutes, a peak related to the C 1s orbital due to C-C bonds and C=C bonds caused by graphene growth was clearly shown in the vicinity of 284.5 eV.
[0159] As the reaction time elapsed, the peak position of the Al 2p orbital shifted to the side of lower binding energy (eV (binding energy)) due to the reduction of the oxidation number of aluminum.
[0160] Therefore, it was confirmed that graphene grew on the Al2O3 particles and Al2O x (0 < x < 3), which is the reduction product of Al2O3, was generated.
[0161] The average carbon and aluminum contents were measured through X-ray photoelectron spectroscopy (XPS) in 10 regions of the composite sample prepared in Preparation Example 1. From the measurement results, the deviation of the aluminum content in each region was calculated. The deviation of the aluminum content was expressed as a percentage of the average value, which is defined as the uniformity. The percentage of the deviation of the aluminum content to the average value, i.e., the uniformity of the aluminum content, was 1%. Therefore, it was confirmed that aluminum oxide was uniformly distributed in the composite prepared in Preparation Example 1.
[0162] Evaluation example 2: X-ray photoelectron spectroscopy (XPS) spectrum and residual lithium evaluation X-ray photoelectron spectroscopy (XPS) spectra of the composite positive electrode active materials prepared in Example 3, Comparative Examples 1 and 2, and bare NCA91 of Comparative Example 5 are shown in Figures 1 to 4, respectively. In Figures 1 to 4, bare, NCA_GB, NCA_LiNO3, and NCA_GB_LiNO3 respectively represent X-ray photoelectron spectroscopy (XPS) spectra of bare NCA91 of Comparative Example 5; composite positive electrode active materials prepared in Comparative Examples 1, 2, and Example 3, and Figures 1 to 4 respectively represent XPS spectra of C 1s, O 1s, Li 1s, and Ni 2p.
[0163] X-ray photoelectron spectroscopy (XPS) was carried out to understand the reason why the electrochemical properties of the sample with LiNO3 added were improved. When analyzing the C 1s and O 1s peaks shown in Figures 1 and 2, it was shown that the amount of carbonate groups on the surface of the NCA particles was reduced after Al2O3@Gr and LiNO3 coating. Furthermore, together, the Al2O3@Gr-LiNO3 coating provided the most significant reduction of CO3 groups, and at the same time, the Li 1s peak was shifted to a higher binding energy, implying the formation of Li3N phase, which is responsible for the improved ionic conductivity of the NCA cathode material.
[0164] The X-ray photoelectron spectroscopy (XPS) peaks of carbonate groups are mainly due to the residual Li2CO3 remaining on the surface of the NCA anode particles after synthesis. Therefore, the amount of residual lithium determined by titration of LiOH with Li2CO3 was measured, proving that the amount of residual lithium compounds on the surface of the NCA particles after coating with the composite (GB)-LiNO3 was reduced (Table 1). In Table 1 below, the content of residual lithium compounds was evaluated by the following method.
[0165] Residual lithium content The sample was titrated in a 1N HCl solution, and the amount of lithium in the sample solution was measured. The sample was titrated in a 1N HCl solution, and the amount of lithium in the solution was measured.
[0166] The amount of lithium in the sample solution was measured using an automatic titrator, measuring the first inflection point (EP1) where the pH changes rapidly from pH 7 to 9, and the endpoint (FP) where the pH reaches 5, and calculating the Li2CO3 content and LiOH content using the following Equations 1 and 2.
[0167] [Formula 1] Li2CO3 content (%): (FP-EP1) x 0.1 x 0.001 x (Li2CO3 Mw (73.89) / 5) x 100
[0168] [Formula 2] LiOH content (%): (2 x EP1-FP) x 0.1 x 0.001 x (LiOH Mw (23.94) / 5) x 100
[0169] The calculated Li2CO3 content and LiOH content were combined to measure the content of lithium remaining on the final surface, and the content of lithium remaining on the surface was converted to wt% based on the total weight of the positive electrode active material. The results are shown in Table 1 below.
[0170] [Table 1]
[0171] As can be seen from Table 1, the content of residual lithium in the composite cathode active material of Example 3 was reduced as compared with Comparative Examples 1, 2 and 5.
[0172] Evaluation example 3: SEM, HR-TEM and SEM-EDAX analysis Scanning electron microscopy, high-resolution transmission electron microscopy and EDAX analysis were performed on the composite cathode active material produced in Example 1 and the bare NCA of Comparative Example 5.
[0173] During SEM-EDAX analysis, FEI Titan 80-300 of Philips was used.
[0174] The composite produced in Production Example 1 has a structure in which Al2O3 particles and Al2O z (0 < z < 3) particles are embedded in graphene. It was confirmed that a graphene layer is arranged on the outer contour of one or more particles selected from Al2O3 particles and Al2O z (0 < z < 3). One or more of the Al2O3 particles and Al2O z (0 < z < 3) particles are uniformly dispersed in the graphene matrix. One or more of the particle sizes of the Al2O3 particles and Al2O z (0 < z < 3) particles were about 20 nm. The particle size of the composite produced in Production Example 1 was about 100 nm to 200 nm. The composite cathode active material produced in Example 1 also showed a structure and particle size similar to those of the composite produced in Production Example 1.
[0175] In the composite cathode active material produced in Example 1, it was confirmed that a shell formed by a composite containing lithium nitrate and graphene was arranged on the NCA core.
[0176] SEM-EDAX analysis was performed on the bare NCA of Comparative Example 5 and the composite cathode active material produced in Example 1.
[0177] It was confirmed that the concentration of aluminum (Al) distributed on the surface of the composite positive electrode active material of Example 1 was increased compared to that of the bare NCA composite positive electrode active material of Comparative Example 5.
[0178] Therefore, it was confirmed that in the composite positive electrode active material of Example 1, the composite prepared in Preparation Example 1 was uniformly coated on the NCA core to form a shell.
[0179] Evaluation example 4: Normal temperature (25°C) charge / discharge characteristic evaluation The lithium batteries prepared in Examples 4 to 6, Comparative Examples 6, 7, and 10 were charged at a constant current of 0.1 C rate at 25° C. until the voltage reached 4.4 V (vs. Li), and then cut off at a current of 0.05 C rate while maintaining 4.4 V in constant voltage mode. Then, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 2.8 V (vs. Li) (formation cycle).
[0180] The lithium battery that had undergone the chemical cycle was charged at a constant current of 0.2C rate at 25°C until the voltage reached 4.4V (vs. Li), and then cut off at a current of 0.05C rate while maintaining 4.4V in constant voltage mode. It was then discharged at a constant current of 0.2C rate until the voltage reached 2.8V (vs. Li) (first cycle). Such cycles were repeated under the same conditions up to the 50th cycle (50 repetitions).
[0181] In all charge / discharge cycles, a rest time of 10 minutes was allowed after one charge / discharge cycle. Some of the results of the room temperature charge / discharge experiments are shown in Table 2 below and Figure 5. Figure 5 shows the initial specific capacity and initial efficiency characteristics of the lithium batteries prepared in Example 6, Comparative Examples 6, 7, and 10. Here, the initial efficiency is defined by the following Equation 3.
[0182] [Formula 3] Initial efficiency [%] = [discharge capacity in formation cycle / charge capacity in formation cycle] x 100
[0183] Evaluation example 5: High temperature (45℃) charge / discharge characteristic evaluation The lithium batteries prepared in Examples 4 to 6, Comparative Examples 6, 7, and 10 were charged at a constant current of 0.1 C rate at 45° C. until the voltage reached 4.4 V (vs. Li), and then cut off at a current of 0.05 C rate while maintaining 4.4 V in constant voltage mode. Then, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 2.8 V (vs. Li) (formation cycle).
[0184] The lithium battery that had undergone the chemical cycle was charged at a constant current of 0.2C rate at 45°C until the voltage reached 4.4V (vs. Li), and then cut off at a current of 0.05C rate while maintaining 4.4V in constant voltage mode. It was then discharged at a constant current of 0.2C rate until the voltage reached 2.8V (vs. Li) (first cycle). Such cycles were repeated under the same conditions up to the 50th cycle (50 repetitions).
[0185] In all charge / discharge cycles, a 10-minute rest period was allowed after one charge / discharge cycle. Some of the results of the high-temperature charge / discharge experiments are shown in Table 2 below and Figure 6. Figure 6 shows the capacity retention characteristics of the lithium batteries prepared in Example 6, Comparative Examples 6, 7, and Comparative Example 10.
[0186] The capacity retention rate is defined by the following formula 4.
[0187] [Formula 4] Capacity retention rate [%] = [discharge capacity at 50th cycle / discharge capacity at first cycle] x 100
[0188] Evaluation Example 6: Resistance The internal resistance of the lithium batteries of Examples 6 to 10 and Comparative Example 10 was measured at 25°C, and the results are shown in Table 3. For the measurement of the internal resistance, five batteries were manufactured for each lithium battery, and the batteries were charged and discharged at 1 / 3C for 10 seconds, while the internal resistance at SOC 50% was measured. At this time, SOC 50% means a state where the battery is charged to 50% charge capacity when the total charge capacity of the battery is 100%. Some of the results are shown in Table 2 below.
[0189] Evaluation example 7: Room temperature high rate characteristic evaluation The lithium batteries of Examples 6 to 10 and Comparative Example 10 were charged at a constant current of 0.1 C rate at 25° C. until the voltage reached 4.4 V (vs. Li), and then cut off at a current of 0.05 C rate while maintaining 4.4 V in constant voltage mode. Subsequently, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 2.80 V (vs. Li) (chemical formation cycle).
[0190] The lithium battery after the formation cycle was charged at 25°C at a constant current rate of 0.2 C until the voltage reached 4.4 V (vs. Li), and then cut off at a current rate of 0.05 C while maintaining 4.4 V in constant voltage mode. It was then discharged at a constant current rate of 0.2 C until the voltage reached 2.8 V (vs. Li) (first cycle).
[0191] The lithium battery that had undergone the first cycle was charged at 25°C at a constant current rate of 0.2 C until the voltage reached 4.4 V (vs. Li), then cut off at a current rate of 0.05 C while maintaining 4.4 V in constant voltage mode, and discharged at a constant current rate of 0.5 C until the voltage reached 2.8 V (vs. Li) (second cycle).
[0192] The lithium battery after the second cycle was charged at 25°C at a constant current of 0.2 C rate until the voltage reached 4.4 V (vs. Li), then cut off at a current of 0.05 C rate while maintaining 4.4 V in constant voltage mode, and discharged at a constant current of 1.0 C rate until the voltage reached 2.8 V (vs. Li) (third cycle).
[0193] The lithium battery after the third cycle was charged at 25°C at a constant current of 0.2 C rate until the voltage reached 4.4 V (vs. Li), then cut off at a current of 0.05 C rate while maintaining 4.4 V in constant voltage mode, and discharged at a constant current of 2.0 C rate until the voltage reached 2.8 V (vs. Li) (fourth cycle).
[0194] In all charge / discharge cycles, a 10-minute rest period was allowed after each charge / discharge cycle. Some of the results of the room temperature charge / discharge experiments are shown in Table 2 below. The high rate characteristic is defined by the following Equation 5.
[0195] [Formula 5] High rate characteristic [%] = [2.0C rate discharge capacity (4th cycle discharge capacity) / 0.2C rate discharge capacity (first cycle discharge capacity)] × 100
[0196] [Table 2]
[0197] As can be seen from Table 2, the lithium batteries of Examples 4 to 6 have improved initial efficiency, specific capacity, and capacity retention while reducing internal resistance, compared to the lithium batteries of Comparative Examples 6, 7, and 10. It was found that adding lithium nitrate to the shell helps increase the initial cycle discharge capacity and coulombic efficiency, and improves the capacity retention after 50 cycles at 45°C and reduces the DCIR after 50 cycles. [Explanation of symbols]
[0198] 1 Lithium battery 2 negative electrode 3 Positive electrode 4. Separator 5 Battery case 6 Cap Assembly 7 Battery structure 8 Electrode tab
Claims
1. a core comprising a lithium transition metal oxide; a shell disposed along a surface of the core; The shell is made of lithium nitrate (LiNO 3 ) and a conductive carbon-based composite, the conductive carbon-based composite being represented by the chemical formula M a O b (where 0<a≦3, 0<b<4, and if a is 1, 2, or 3, then b is not an integer), and a carbon-based material; the first metal oxide is disposed in a carbon-based material matrix, and M is one or more metals selected from Groups 2 to 13 of the Periodic Table, Groups 15 and 16 of the Periodic Table.
2. 2. The composite positive electrode active material of claim 1, wherein the content of lithium nitrate in the shell is 3 wt% or less, based on 100 wt% of the total weight of the composite positive electrode active material.
3. The shell is Li 3 N, LiNO 2 , and LiN x O y 2. The composite positive electrode active material of claim 1, further comprising one or more selected from (0.5≦x≦1, 2≦y≦3.5).
4. 2. The composite positive electrode active material of claim 1, wherein the shell comprises a first metal in an amount of 1 to 10 at% based on the total number of atoms in the shell, an oxygen in an amount of 1 to 20 at% based on the total number of atoms in the shell, and a nitrogen in an amount of 1 to 12 at% based on the total number of atoms in the shell.
5. 2. The composite positive electrode active material of claim 1, wherein the shell has a carbon content of 65 to 99 at % based on the total number of atoms in the shell.
6. 2. The composite positive electrode active material of claim 1, wherein the metal contained in the first metal oxide is one or more metals selected from the group consisting of Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se.
7. The first metal oxide is Al 2 O z (0<z<3), NbO x (0<x<2.5), MgO x (0<x<1), Sc 2 O z (0<z<3), TiO y (0<y<2), ZrO y (0<y<2), V 2 O z (0<z<3), WO y (0<y<2), MnO y (0<y<2), Fe 2 O z (0<z<3), Co 3 O w (0<w<4), PdO x (0<x<1), CuO x (0<x<1), AgO x (0<x<1), ZnO x (0<x<1), Sb 2 O z (0<z<3) and SeO y 2. The composite positive electrode active material of claim 1 , wherein y is one or more selected from (0<y<2).
8. 2. The composite cathode active material of claim 1, wherein the shell has a thickness of 1 nm to 5 μm.
9. 10. The composite cathode active material of claim 1 , wherein the carbon-based material is graphene.
10. 2. The composite positive electrode active material of claim 1, wherein the shell comprises lithium nitrate, and at least one selected from the group consisting of a conductive carbon composite including the first metal oxide and a carbon-based material, and a milling product of the conductive carbon composite, and a content of the at least one selected from the group consisting of the conductive carbon composite and the milling product of the conductive carbon composite is 3 wt % or less of a total weight of the composite positive electrode active material.
11. the carbon-based material has a branched structure, and the metal oxide is distributed within the branched structure; 10. The composite active cathode material of claim 9, wherein the branched structure comprises a plurality of carbon-based material particles in contact with one another.
12. The carbon-based material has at least one structure selected from a spherical structure, a helical structure in which the spherical structures are connected, and a cluster structure in which the spherical structures are aggregated, the first metal oxide is distributed within the spherical structures, the size of the spherical structures is 50 nm to 300 nm, the size of the helical structures is 500 nm to 100 μm, and the size of the cluster structures is 0.5 mm to 10 cm; The composite is a wrinkled polyhedral ball structure or a planar structure, and at least one selected from a first metal oxide and a second metal oxide is distributed inside or on a surface of the structure; 10. The composite positive electrode active material of claim 9, wherein the carbon-based material extends from the first metal oxide by a distance of 10 nm or less, includes at least 1 to 20 carbon-based material layers, and has a total thickness of 0.6 to 12 nm.
13. 2. The composite positive electrode active material according to claim 1, wherein the lithium transition metal oxide is at least one selected from the group consisting of compounds represented by the following Formulas 1 to 6: [Chemical formula 1] Li a Ni x Co y M z O 2-b A b In the above Chemical Formula 1, 1.0≦a≦1.2, 0≦b≦0.2, 0.8≦x<1, 0<y≦0.3, 0<z≦0.3, and x+y+z=1; M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), or a combination thereof; A is F, S, Cl, Br, or a combination thereof; [Chemical formula 2] L)) x Co y Mn z O 2 [Chemical formula 3] L)) x Co y Al z O 2 In the formulas 2 and 3, 0.8≦x≦0.95, 0<y≦0.2, 0<z≦0.2, and x+y+z=1; [Chemical formula 4] L)) x Co y Mn v Al w O 2 In the formula 4, 0.8≦x≦0.95, 0<y≦0.2, 0<v≦0.2, 0<w≦0.2, and x+y+v+w=1; [Chemical formula 5] Li a Co x M y O 2-b A b In the above Chemical Formula 5, 1.0≦a≦1.2, 0≦b≦0.2, 0.9≦x≦1, 0≦y≦0.1, and x+y=1; M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), or a combination thereof; A is F, S, Cl, Br, or a combination thereof; [Chemical formula 6] LiCoO 2 。
14. A positive electrode comprising the composite active positive electrode material of claim 1.
15. The positive electrode according to claim 14 ; A negative electrode; and an electrolyte disposed between the positive electrode and the negative electrode.
16. The positive electrode includes a positive electrode current collector, and the negative electrode includes a negative electrode current collector, and at least one of the positive electrode current collector and the negative electrode current collector includes a base film and a metal layer disposed on one surface or both surfaces of the base film; the base film comprises a polymer, the polymer comprising polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof; 16. The lithium battery of claim 15, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
17. providing a lithium transition metal oxide; Providing a complex; and mechanically milling the lithium transition metal oxide, the composite, and the lithium nitrate; The complex has the formula M a O b (where 0<a≦3, 0<b<4, and if a is 1, 2, or 3, then b is not an integer), and a carbon-based material, the first metal oxide is disposed in a carbon-based material matrix, and M is one or more metals selected from Groups 2 to 13 of the Periodic Table, Groups 15 and 16 of the Periodic Table.
18. providing the complex, M a O c (where 0<a≦3, 0<c≦4, and if a is 1, 2, or 3, then c is an integer) is supplied with a reaction gas comprising a carbon source gas to heat-treat one or more second metal oxides, thereby providing an undoped composite; and contacting the undoped composite with lithium nitrate to provide a composite, 18. The method of claim 17, wherein M is at least one metal selected from the group consisting of metals of Groups 2 to 13, 15 and 16 of the periodic table.
Citation Information