Polyamide composition, method for producing the same, and molded article

A polyamide composition with a phosphorus-based flame retardant and styrene copolymer addresses the challenge of maintaining flammability and heat resistance in non-halogen polyamide compositions, enhancing mechanical properties and flame retardancy in molded articles.

JP2024138040AActive Publication Date: 2024-10-07ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
JP2024114816
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-05-21
Filing Date
2024-07-18
Publication Date
2024-10-07
Estimated Expiration
2040-05-20

AI Technical Summary

Technical Problem

Existing polyamide compositions with non-halogen flame retardants face challenges in maintaining flammability classification V-0 according to UL94 while ensuring long-term heat resistance and mechanical properties, particularly in applications requiring both flame retardancy and heat resistance, such as in the electrical and electronic industries.

Method used

A polyamide composition containing a polyamide, a phosphorus-based flame retardant, and a styrene copolymer, with specific ratios and components, including semi-aromatic polyamides and isophthalic acid units, to enhance flame retardancy and long-term heat resistance.

Benefits of technology

The composition achieves good flame retardancy and long-term heat resistance, maintaining flammability classification V-0 and improving mechanical properties, such as tensile strength and heat resistance, in molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138040000001
    Figure 2024138040000001
  • Figure 2024138040000002
    Figure 2024138040000002
  • Figure 2024138040000003
    Figure 2024138040000003
Patent Text Reader

Abstract

To provide a polyamide composition which contains a non-halogen flame retardant and gives a molded article having good flame retardancy and long-term heat resistance, and a method for producing the polyamide composition.SOLUTION: The polyamide composition contains (A) a polyamide, (B) a phosphorus-based flame retardant, and (C) a styrene copolymer. The content of the styrene copolymer (C) is 0.1 mass% or more and 7.0 mass% or less based on the total mass of the polyamide (A), the phosphorus-based flame retardant (B), and the styrene copolymer (C). The method for producing the polyamide composition comprises melt-kneading a raw material component containing the polyamide (A), the phosphorus-based flame retardant (B), and the styrene copolymer (C).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamide composition, a method for producing the same, and a molded article. [Background technology]

[0002] Due to their excellent property profile, compositions based on aliphatic polyamides are used to manufacture molded articles in a great many applications. Polyamide compositions with flame retardant properties are required especially for components in the electrical and electronics industry to ensure adequate fire protection.

[0003] Polyamides are often flame retarded by the addition of halogen compounds. However, recently, various regulations have been established to prevent the use of products containing halogen compounds in electrical and electronic components due to hazardous substance restrictions such as RoHS (Restriction of Hazardous Substances) and PoHS (Prohibition on Certain Hazardous Substances in Consumer Products). For this reason, several non-halogen flame retardants for polyamides have been developed.

[0004] Examples of non-halogen flame retardants include phosphorus compounds. Patent Document 1 discloses the use of calcium and aluminum salts of phosphinic or diphosphinic acids as flame retardants for polyamides. Test pieces with a sample thickness of 1.2 mm made from polyamide compositions containing these non-halogen flame retardants and reinforced with 30% by weight of glass fiber based on the total weight of the composition achieve a flammability classification of V-0 according to UL94.

[0005] Patent Document 2 discloses that, in order to achieve UL94 flammability classification V-0, aluminum phosphinate is required in an amount far exceeding 20 mass % relative to the total mass of the composition in a glass fiber reinforced polyamide composition mainly composed of polyamide 6, and more than 30 mass % in a glass fiber reinforced polyamide composition mainly composed of polyamide 66. Thus, in order to achieve flammability classification V-0 using a phosphinic acid flame retardant, a large amount must be added, which causes a problem of adverse effects on mechanical properties.

[0006] Therefore, Patent Document 3 discloses a polyamide composition based on a mixture of an aliphatic polyamide containing a phosphinate as a flame retardant and a semi-aromatic polyamide. It is reported that the addition of the semi-aromatic polyamide reduces the amount of flame retardant used and improves tensile elongation.

[0007] Patent Document 4 discloses a polyamide composition based on a mixture of polyamide containing aromatic polyamide and polyphenylene sulfide, using a phosphinate as a flame retardant. It has been reported that the amount of flame retardant used can be reduced by adding polyphenylene sulfide, which has excellent flame retardancy, to polyamide containing aromatic polyamide, and the amount of outgassing derived from the flame retardant can be reduced. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 3947261 [Patent Document 2] Patent No. 4698789 [Patent Document 3] Patent No. 4614959 [Patent Document 4] JP 2009-270107 A [Patent Document 5] JP 2005-179362 A [Patent Document 6] European Patent Application Publication No. 699708 [Patent Document 7] Japanese Patent Application Publication No. 08-073720 Summary of the Invention [Problem to be solved by the invention]

[0009] However, although the polyamide composition described in Patent Document 3 has improved tensile elongation at break by reducing the amount of flame retardant used, there is still room for improvement in terms of long-term heat resistance and other properties required for automobiles and various electric parts. In addition, the polyamide composition described in Patent Document 4 reduces the amount of flame retardant used and reduces outgassing by adding polyphenylene sulfide, but there is a concern that if the ratio of aliphatic polyamide to aromatic polyamide is increased, it will become difficult to maintain the UL94 flammability classification of V-0. As described above, in the prior art, there is no known polyamide composition that uses a non-halogen flame retardant and yet has both flame retardancy and long-term heat resistance.

[0010] The present invention has been made in view of the above circumstances, and provides a polyamide composition containing a non-halogen flame retardant and capable of producing a molded article having excellent flame retardancy and long-term heat resistance, a method for producing the same, and a molded article made of the polyamide composition. Also, the present invention provides a method for adding a styrene copolymer as a flame retardant assistant. [Means for solving the problem]

[0011] That is, the present invention includes the following aspects. The polyamide composition according to a first aspect of the present invention is a polyamide composition containing (A) a polyamide, (B) a phosphorus-based flame retardant, and (C) a styrene copolymer, and the content of the (C) styrene copolymer is 0.1 mass % or more and 7.0 mass % or less with respect to the total mass of the (A) polyamide, the (B) the phosphorus-based flame retardant, and the (C) styrene copolymer.

[0012] The (A) polyamide may contain (A1) an aliphatic polyamide and (A2) a semi-aromatic polyamide containing diamine units and dicarboxylic acid units.

[0013] The (A2) semi-aromatic polyamide may contain 50 mol % or more of isophthalic acid units in all dicarboxylic acid units constituting the (A2) semi-aromatic polyamide.

[0014] The (A2) semi-aromatic polyamide may contain 75 mol % or more of isophthalic acid units in all dicarboxylic acid units constituting the (A2) semi-aromatic polyamide.

[0015] The (A2) semi-aromatic polyamide may contain 100 mol % of isophthalic acid units in all dicarboxylic acid units constituting the (A2) semi-aromatic polyamide.

[0016] The (C) styrene copolymer may contain acrylonitrile units and styrene units.

[0017] The (C) styrene copolymer may contain acrylonitrile units and styrene units, and the content of the acrylonitrile units may be 30 mass % or more based on the total mass of the constituent units of the (C) styrene copolymer.

[0018] The (B) phosphorus-based flame retardant may contain at least one phosphinate selected from the group consisting of a phosphinate represented by the following general formula (1), a diphosphinate represented by the following general formula (2), and a condensate thereof:

[0019] [ka]

[0020] (In general formula (1), R 11 and R 12 Each of M is independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. n11+is a metal ion with a valence of n11. M is an element belonging to Group 2 or Group 15 of the periodic table, a transition element, zinc, or aluminum. n11 is 2 or 3, and multiple R 11 and R 12 may be the same or different. In general formula (2), R 21 and R 22 Each of Y is independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. 21 M' is an alkylene group having 1 to 10 carbon atoms or an arylene group having 6 to 10 carbon atoms. m21+ is a metal ion having a valence of m21. M' is an element belonging to Group 2 or Group 15 of the periodic table, a transition element, zinc, or aluminum. n21 is an integer of 1 to 3. When n21 is 2 or 3, multiple R 21 , R 22 and Y 21 may be the same or different. m21 is 2 or 3. x is 1 or 2. When x is 2, multiple M' may be the same or different. n21, x, and m21 are integers that satisfy the relational formula 2×n21=m21×x.

[0021] The content of the (B) phosphorus-based flame retardant may be 0.1 mass % or more and 30 mass % or less with respect to the total mass of the (A) polyamide, the (B) phosphorus-based flame retardant, and the (C) styrene copolymer.

[0022] The polyamide composition may have a tan δ peak temperature of 90° C. or higher.

[0023] The polyamide composition may have a weight average molecular weight of 10,000 or more and 50,000 or less.

[0024] The polyamide composition according to the first embodiment may further contain at least one type of (D) filler.

[0025] A molded article according to a second aspect of the present invention is produced by molding the polyamide composition according to the first aspect.

[0026] A method for producing a polyamide composition according to a third aspect of the present invention is a method for producing the polyamide composition according to the first aspect, which comprises melt-kneading raw material components containing the (A) polyamide, the (B) phosphorus-based flame retardant, and the (C) styrene copolymer.

[0027] The method according to the fourth aspect of the present invention is a method in which a styrene copolymer is added as a flame retardant aid to a resin composition containing a polyamide and a phosphorus-based flame retardant. Effect of the Invention

[0028] According to the polyamide composition and the method for producing the same of the above-mentioned embodiment, a molded article containing a non-halogen flame retardant and having good flame retardancy and long-term heat resistance can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.

[0030] In this specification, the term "polyamide" refers to a polymer having an amide (-NHCO-) ​​group in the main chain.

[0031] <Polyamide composition> The polyamide composition of the present embodiment contains the following components (A) to (C). (A) polyamide; (B) Phosphorus-based flame retardants; (C) Styrene copolymer

[0032] In the polyamide composition of the present embodiment, the content of component (C) relative to the total mass of components (A) to (C) is 0.1 mass % or more and 7 mass % or less. The polyamide composition of the present embodiment has the above-mentioned configuration, and thus contains a non-halogen flame retardant, and a molded article having excellent flame retardancy and long-term heat resistance can be obtained.

[0033] <Characteristics of polyamide composition> The molecular weight and tan δ peak temperature of the polyamide composition of the present embodiment can be as follows, and specifically, can be measured by the method described in the examples described later.

[0034] [Weight average molecular weight (Mw) of polyamide composition] The weight average molecular weight (Mw) can be used as an index of the molecular weight of a polyamide composition. The weight average molecular weight (Mw) of the polyamide composition is preferably 10,000 or more and 50,000 or less, more preferably 17,000 or more and 45,000 or less, even more preferably 20,000 or more and 45,000 or less, even more preferably 25,000 or more and 45,000 or less, particularly preferably 30,000 or more and 42,000 or less, and most preferably 34,000 or more and 38,000 or less. When the weight average molecular weight (Mw) of the polyamide composition is within the above range, the polyamide composition has excellent mechanical properties, particularly excellent water absorption rigidity, hot rigidity, flowability, etc. Furthermore, molded articles obtained from the polyamide composition containing a component typified by the (D) filler have excellent tensile strength and long-term heat resistance.

[0035] As a method for controlling the Mw of the polyamide composition within the above range, for example, the polyamide (A) and the styrene copolymer (C) may be used whose Mw falls within the ranges described below. The weight average molecular weight (Mw) can be measured by using GPC (gel permeation chromatography) as described in the Examples below.

[0036] [Tan δ peak temperature of polyamide composition] The lower limit of the tan δ peak temperature of the polyamide composition is preferably 90°C, more preferably 105°C, and even more preferably 110°C. On the other hand, the upper limit of the tan δ peak temperature of the polyamide composition is preferably 150°C, more preferably 140°C, and even more preferably 130°C. That is, the tan δ peak temperature of the polyamide composition is preferably 90°C or higher and 150°C or lower, more preferably 105°C or higher and 140°C or lower, and even more preferably 110°C or higher and 130°C or lower. When the tan δ peak temperature of the polyamide composition is equal to or higher than the lower limit, the polyamide composition tends to have better water absorption rigidity and hot rigidity. On the other hand, when the tan δ peak temperature of the polyamide composition is equal to or lower than the upper limit, the molded article obtained from the polyamide composition containing the component represented by the (D) filler tends to have better tensile strength and long-term heat resistance.

[0037] Examples of methods for controlling the tan δ peak temperature of the polyamide composition within the above range include a method in which the polyamide composition contains (A1) an aliphatic polyamide and (A2) a semi-aromatic polyamide containing diamine units and dicarboxylic acid units, as described below, and the contents thereof are controlled within the ranges described below.

[0038] Hereinafter, each of the components of the polyamide composition of the present embodiment will be described in detail.

[0039] <(A) Polyamide> From the viewpoints of improving flame retardancy, weld strength, and laser weld strength, it is preferable that the (A) polyamide contained in the polyamide composition of the present embodiment contains (A1) an aliphatic polyamide and (A2) a semi-aromatic polyamide containing diamine units and dicarboxylic acid units.

[0040] [(A1) Aliphatic polyamide] The structural units of the aliphatic polyamide (A1) preferably satisfy at least one of the following conditions (1) and (2). (1) The polymer contains (A1-a) an aliphatic dicarboxylic acid unit and (A1-b) an aliphatic diamine unit. (2) (A1-c) Contains at least one unit selected from the group consisting of lactam units and aminocarboxylic acid units.

[0041] The polyamide composition of the present embodiment may contain, as the aliphatic polyamide (A1), one or more polyamides that satisfy at least either of the above conditions (1) and (2). In particular, it is particularly preferable that the structural unit of the aliphatic polyamide (A1) contained in the polyamide composition of the present embodiment satisfies the above condition (1).

[0042] ((A1-a) Aliphatic dicarboxylic acid unit) Examples of the aliphatic dicarboxylic acid constituting the (A1-a) aliphatic dicarboxylic acid unit include linear or branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms. Examples of linear saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms include, but are not limited to, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane dioic acid, and diglycolic acid. Examples of branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms include, but are not limited to, dimethylmalonic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid, 2,3-diethylglutaric acid, 2,2-dimethylglutaric acid, 2-methyladipic acid, and trimethyladipic acid. The aliphatic dicarboxylic acids constituting the (A1-a) aliphatic dicarboxylic acid unit may be used alone or in combination of two or more. Among these, the aliphatic dicarboxylic acid constituting the (A1-a) aliphatic dicarboxylic acid unit is preferably a linear saturated aliphatic dicarboxylic acid having 6 or more carbon atoms, since the polyamide composition tends to have better heat resistance, fluidity, toughness, low water absorption, rigidity, and the like.

[0043] Specific examples of preferred linear saturated aliphatic dicarboxylic acids having 6 or more carbon atoms include adipic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and eicosane dioic acid. Among these, from the viewpoint of the heat resistance of the polyamide composition, adipic acid, sebacic acid, or dodecanedioic acid is preferred as the linear saturated aliphatic dicarboxylic acid having 6 or more carbon atoms.

[0044] In addition, the (A1) aliphatic polyamide may further contain a unit derived from a trivalent or higher polycarboxylic acid, if necessary, within a range that does not impair the effect of the polyamide composition of the present embodiment. Examples of the trivalent or higher polycarboxylic acid include trimellitic acid, trimesic acid, and pyromellitic acid. These trivalent or higher polycarboxylic acids may be used alone or in combination of two or more.

[0045] ((A1-b) Aliphatic diamine unit) Examples of the aliphatic diamine constituting the (A1-b) aliphatic diamine unit include linear saturated aliphatic diamines having 2 to 20 carbon atoms, and branched saturated aliphatic diamines having 3 to 20 carbon atoms. Examples of linear saturated aliphatic diamines having 2 to 20 carbon atoms include, but are not limited to, ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecamethylenediamine, and the like. Examples of branched saturated aliphatic diamines having 3 to 20 carbon atoms include, but are not limited to, 2-methylpentamethylenediamine (also referred to as 2-methyl-1,5-diaminopentane), 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 2-methyl-1,8-octanediamine (also referred to as 2-methyloctamethylenediamine), 2,4-dimethyloctamethylenediamine, and the like. The aliphatic diamines constituting the (A1-b) aliphatic diamine unit may be used alone or in combination of two or more. Among these, the carbon number of the aliphatic diamine constituting the (A1-b) aliphatic diamine unit is preferably 6 or more and 12 or less, more preferably 6 or more and 10 or less. When the carbon number of the aliphatic diamine constituting the (A1-b) aliphatic diamine unit is equal to or more than the above lower limit, the heat resistance of the obtained molded article is more excellent. On the other hand, when the carbon number is equal to or less than the above upper limit, the crystallinity and releasability of the obtained molded article are more excellent.

[0046] Specific examples of preferred linear or branched saturated aliphatic diamines having 6 to 12 carbon atoms include hexamethylenediamine, 2-methylpentamethylenediamine, and 2-methyl-1,8-octanediamine. Among these, hexamethylenediamine or 2-methylpentamethylenediamine is preferred as the linear or branched saturated aliphatic diamine having from 6 to 12 carbon atoms. By containing such an aliphatic diamine unit (A1-b), the heat resistance, rigidity, etc. of a molded article obtained from the polyamide composition are more excellent.

[0047] In addition, the (A1) aliphatic polyamide may further contain a unit derived from a trivalent or higher polyvalent aliphatic amine, if necessary, within a range that does not impair the effects of the polyamide composition of the present embodiment. Examples of trivalent or higher polyvalent aliphatic amines include bishexamethylenetriamine.

[0048] ((A1-c) At least one structural unit selected from the group consisting of lactam units and aminocarboxylic acid units) The aliphatic polyamide (A1) may contain at least one structural unit (A1-c) selected from the group consisting of lactam units and aminocarboxylic acid units. By containing such units, a polyamide having excellent toughness tends to be obtained. The terms "lactam unit" and "aminocarboxylic acid unit" used herein refer to poly(condensed) lactam and aminocarboxylic acid.

[0049] Examples of lactams constituting the lactam unit include, but are not limited to, butyrolactam, pivalolactam, ε-caprolactam, caprylolactam, enantholactam, undecanolactam, laurolactam (dodecanolactam), and the like. Among them, the lactam constituting the lactam unit is preferably ε-caprolactam or laurolactam, and more preferably ε-caprolactam. By including such a lactam, the toughness of a molded article obtained from the polyamide composition tends to be superior.

[0050] Examples of aminocarboxylic acids constituting the aminocarboxylic acid unit include, but are not limited to, ω-aminocarboxylic acids, which are compounds formed by ring-opening of lactams, and α,ω-amino acids. The amino carboxylic acid constituting the amino carboxylic acid unit is preferably a linear or branched saturated aliphatic carboxylic acid having 4 to 14 carbon atoms and substituted with an amino group at the ω position. Examples of such amino carboxylic acids include, but are not limited to, 6-aminocaproic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid. Other examples of amino carboxylic acids include paraaminomethylbenzoic acid.

[0051] The lactam and aminocarboxylic acid constituting at least one structural unit selected from the group consisting of (A1-c) lactam units and aminocarboxylic acid units may each be used alone or in combination of two or more kinds.

[0052] Among them, as the (A1) aliphatic polyamide, from the viewpoints of mechanical properties, heat resistance, moldability and toughness, polyamides containing dicarboxylic acid units and diamine units are preferred, and polyamide 66 (PA66) is more preferred. PA66 is considered to be a material suitable for automobile parts because of its excellent mechanical properties, heat resistance, moldability and toughness.

[0053] The content of the (A1) aliphatic polyamide can be, for example, 50% by mass or more and 100% by mass or less, for example, 55% by mass or more and 100% by mass or less, for example, 57% by mass or more and 100% by mass or less, relative to the total mass of polyamides in the polyamide composition.

[0054] ((A1) Weight average molecular weight Mw(A1) of aliphatic polyamide) As an index of the molecular weight of the (A1) aliphatic polyamide, the weight average molecular weight Mw(A1) can be used. The weight average molecular weight Mw(A1) of the aliphatic polyamide is preferably 10,000 to 50,000, more preferably 17,000 to 45,000, even more preferably 20,000 to 45,000, even more preferably 25,000 to 45,000, particularly preferably 30,000 to 45,000, and most preferably 35,000 to 40,000. When the weight-average molecular weight Mw(A1) is within the above range, a polyamide composition having excellent mechanical properties, in particular, water absorption rigidity, hot rigidity, and fluidity, as well as tensile strength, flexural modulus when water absorbed, long-term heat resistance, tracking resistance, and the like when formed into a molded article can be obtained. The weight average molecular weight Mw(A1) can be measured by using GPC as described in the following Examples.

[0055] [(A2) Semi-aromatic polyamide] (A2) The semi-aromatic polyamide is a polyamide containing diamine units and dicarboxylic acid units. The (A2) semi-aromatic polyamide preferably contains 20 mol % or more and 80 mol % or less of aromatic structural units, more preferably 30 mol % or more and 70 mol % or less of aromatic structural units, and even more preferably 40 mol % or more and 60 mol % or less of aromatic structural units, based on the total structural units of the (A2) semi-aromatic polyamide. The term "aromatic structural units" used herein refers to aromatic diamine units and aromatic dicarboxylic acid units.

[0056] In addition, the (A2) semi-aromatic polyamide is preferably a polyamide containing (A2-a) dicarboxylic acid units containing 50 mol % or more of isophthalic acid units relative to the total dicarboxylic acid units of the (A2) semi-aromatic polyamide, and (A2-b) diamine units containing diamine units having 4 to 10 carbon atoms. In this case, the total content of isophthalic acid units and diamine units having 4 to 10 carbon atoms in the (A2) semi-aromatic polyamide is preferably 50 mol% or more, more preferably 80 mol% or more and 100 mol% or less, even more preferably 90 mol% or more and 100 mol% or less, and particularly preferably 100 mol%, based on all structural units of the (A2) semi-aromatic polyamide.

[0057] The proportion of the predetermined monomer unit constituting the semi-aromatic polyamide (A2) can be measured by nuclear magnetic resonance spectroscopy (NMR) or the like.

[0058] ((A2-a) Dicarboxylic acid unit) The dicarboxylic acid unit (A2-a) is not particularly limited, and examples thereof include an aromatic dicarboxylic acid unit, an aliphatic dicarboxylic acid unit, and an alicyclic dicarboxylic acid unit. In particular, the (A2-a) dicarboxylic acid units preferably contain isophthalic acid units in an amount of 50 mol% or more, more preferably 65 mol% or more and 100 mol% or less, even more preferably 75 mol% or more and 100 mol% or less, particularly preferably 80 mol% or more and 100 mol% or less, and most preferably 100 mol%. When the ratio of isophthalic acid units in the (A2-a) dicarboxylic acid units is equal to or greater than the above lower limit, a polyamide composition tends to be obtained that simultaneously satisfies mechanical properties, particularly rigidity when absorbing water, rigidity when hot, fluidity, etc. Furthermore, molded articles obtained from the polyamide composition tend to be superior in tensile strength, flexural modulus when absorbing water, long-term heat resistance, and tracking resistance.

[0059] (1) Aromatic dicarboxylic acid unit Examples of aromatic dicarboxylic acids constituting aromatic dicarboxylic acid units other than isophthalic acid units include, but are not limited to, dicarboxylic acids having an aromatic group such as a phenyl group, a naphthyl group, etc. The aromatic group of the aromatic dicarboxylic acid may be unsubstituted or may have a substituent.

[0060] The substituent is not particularly limited, but examples thereof include alkyl groups having 1 to 4 carbon atoms, aryl groups having 6 to 10 carbon atoms, arylalkyl groups having 7 to 10 carbon atoms, alkylaryl groups having 7 to 10 carbon atoms, halogen groups, silyl groups having 1 to 6 carbon atoms, sulfonic acid groups and salts thereof (such as sodium salts). Examples of the alkyl group having 1 to 4 carbon atoms include, but are not limited to, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a tert-butyl group. Examples of the aryl group having 6 to 10 carbon atoms include, but are not limited to, a phenyl group, a naphthyl group, and the like. Examples of the arylalkyl group having 7 to 10 carbon atoms include, but are not limited to, a benzyl group. Examples of the alkylaryl group having 7 to 10 carbon atoms include, but are not limited to, a tolyl group, a xylyl group, and the like. Examples of the halogen group include, but are not limited to, a fluoro group, a chloro group, a bromo group, and an iodo group. Examples of the silyl group having 1 to 6 carbon atoms include, but are not limited to, a trimethylsilyl group, a tert-butyldimethylsilyl group, and the like. Among these, the aromatic dicarboxylic acid constituting the aromatic dicarboxylic acid unit other than the isophthalic acid unit is preferably an aromatic dicarboxylic acid having 8 to 20 carbon atoms which is unsubstituted or substituted with a specific substituent.

[0061] Specific examples of unsubstituted or predetermined substituent-substituted aromatic dicarboxylic acids having 8 to 20 carbon atoms include, but are not limited to, terephthalic acid, naphthalenedicarboxylic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, and 5-sodium sulfoisophthalic acid. The aromatic dicarboxylic acid constituting the aromatic dicarboxylic acid unit may be used alone or in combination of two or more kinds.

[0062] (2) Aliphatic dicarboxylic acid unit Examples of the aliphatic dicarboxylic acid constituting the aliphatic dicarboxylic acid unit include linear or branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms.

[0063] Examples of linear saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms include, but are not limited to, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane dioic acid, and diglycolic acid. Examples of branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms include, but are not limited to, dimethylmalonic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid, 2,3-diethylglutaric acid, 2,2-dimethylglutaric acid, 2-methyladipic acid, and trimethyladipic acid.

[0064] (3) Alicyclic dicarboxylic acid unit Examples of alicyclic dicarboxylic acids constituting an alicyclic dicarboxylic acid unit (hereinafter sometimes referred to as an "alicyclic dicarboxylic acid unit") include, but are not limited to, alicyclic dicarboxylic acids having an alicyclic structure with 3 to 10 carbon atoms. Among these, alicyclic dicarboxylic acids are preferably alicyclic dicarboxylic acids having an alicyclic structure with 5 to 10 carbon atoms.

[0065] Examples of such alicyclic dicarboxylic acids include, but are not limited to, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, etc. Among them, 1,4-cyclohexanedicarboxylic acid is preferred as the alicyclic dicarboxylic acid. The alicyclic dicarboxylic acid constituting the alicyclic dicarboxylic acid unit may be used alone or in combination of two or more kinds.

[0066] The alicyclic group of the alicyclic dicarboxylic acid may be unsubstituted or may have a substituent. Examples of the substituent include an alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group having 1 to 4 carbon atoms include the same as those exemplified in the above "aromatic dicarboxylic acid unit".

[0067] The dicarboxylic acid units other than the isophthalic acid units preferably contain aromatic dicarboxylic acid units, and more preferably contain aromatic dicarboxylic acids having 6 or more carbon atoms. By using such a dicarboxylic acid, a polyamide composition tends to be obtained that simultaneously satisfies mechanical properties, particularly water-absorbed rigidity, hot rigidity, fluidity, etc. Furthermore, molded articles obtained from the polyamide composition tend to be superior in tensile strength, flexural modulus when absorbing water, long-term heat resistance, and tracking resistance.

[0068] In the (A2) semi-aromatic polyamide, the dicarboxylic acid constituting the (A2-a) dicarboxylic acid unit is not limited to the compounds described above as the dicarboxylic acid, and may be a compound equivalent to the above dicarboxylic acid. The term "compound equivalent to a dicarboxylic acid" used herein means a compound that can have a dicarboxylic acid structure similar to the dicarboxylic acid structure derived from the above dicarboxylic acid. Examples of such compounds include, but are not limited to, anhydrides of dicarboxylic acids and halides of dicarboxylic acids.

[0069] Furthermore, the (A2) semi-aromatic polyamide may further contain units derived from a trivalent or higher polyvalent carboxylic acid, if necessary, within a range that does not impair the effects of the polyamide composition of the present embodiment. Examples of the trivalent or higher polyvalent carboxylic acid include trimellitic acid, trimesic acid, pyromellitic acid, etc. These trivalent or higher polyvalent carboxylic acids may be used alone or in combination of two or more.

[0070] ((A2-b) Diamine unit) The diamine unit (A2-b) constituting the semi-aromatic polyamide (A2) is not particularly limited and may be, for example, an aromatic diamine unit, an aliphatic diamine unit, an alicyclic diamine unit, etc. Among them, the diamine unit (A2-b) constituting the semi-aromatic polyamide (A2) preferably contains a diamine unit having 4 to 10 carbon atoms, and more preferably contains a diamine unit having 6 to 10 carbon atoms.

[0071] (1) Aliphatic diamine unit Examples of the aliphatic diamine constituting the aliphatic diamine unit include linear saturated aliphatic diamines having 4 to 20 carbon atoms. Examples of linear saturated aliphatic diamines having 4 to 20 carbon atoms include, but are not limited to, ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecamethylenediamine, and the like.

[0072] (2) Alicyclic diamine unit Examples of alicyclic diamines constituting the alicyclic diamine unit (hereinafter, also referred to as "alicyclic diamines") include, but are not limited to, 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, 1,3-cyclopentanediamine, and the like.

[0073] (3) Aromatic diamine unit The aromatic diamine constituting the aromatic diamine unit is not limited to the following as long as it is a diamine containing an aromatic group. Specific examples of the aromatic diamine include metaxylylenediamine.

[0074] The diamines constituting the diamine units may be used alone or in combination of two or more. Among these, the (A2-b) diamine unit is preferably an aliphatic diamine unit, more preferably a linear saturated aliphatic diamine unit having 4 to 10 carbon atoms, even more preferably a linear saturated aliphatic diamine unit having 6 to 10 carbon atoms, and particularly preferably a hexamethylenediamine unit. By using such a diamine, it is likely to be possible to obtain a polyamide composition that simultaneously satisfies mechanical properties, particularly rigidity when absorbing water, rigidity when hot, flowability, etc. Furthermore, molded articles obtained from the polyamide composition tend to be superior in tensile strength, flexural modulus when absorbing water, long-term heat resistance, and tracking resistance.

[0075] As the (A2) semi-aromatic polyamide, polyamide 6I (polyhexamethylene isophthalamide), polyamide 9I, or polyamide 10I is preferred, and polyamide 6I is more preferred. Polyamide 6I is considered to be a suitable material for automobile parts because of its excellent heat resistance, moldability, and flame retardancy.

[0076] The content of the (A2) semi-aromatic polyamide can be from 0 mass% to 50.0 mass% based on the total mass of polyamide in the polyamide composition, preferably from 10.0 mass% to 45.0 mass%, more preferably from 15.0 mass% to 43.0 mass%, and even more preferably from 20.0 mass% to 41.0 mass%. By setting the content of the (A2) semi-aromatic polyamide within the above range, the mechanical properties of the molded article obtained from the polyamide composition are more excellent. Also, by adding a component such as the (D) filler, the tensile strength, flexural modulus when absorbing water, long-term heat resistance, and tracking resistance of the molded article obtained from the polyamide composition tend to be more excellent.

[0077] ((A2) Weight average molecular weight Mw(A2) of semi-aromatic polyamide) As an index of the molecular weight of the (A2) semi-aromatic polyamide, the weight average molecular weight Mw(A2) can be used. The weight average molecular weight Mw(A2) of the semi-aromatic polyamide is preferably 10,000 to 50,000, more preferably 15,000 to 45,000, even more preferably 15,000 to 40,000, even more preferably 17,000 to 30,000, particularly preferably 17,000 to 25,000, and most preferably 18,000 to 22,000. When the weight-average molecular weight Mw(A2) is within the above range, a polyamide composition having excellent mechanical properties, in particular, water absorption rigidity, hot rigidity, and fluidity, as well as tensile strength, flexural modulus when water absorbed, long-term heat resistance, tracking resistance, and the like when formed into a molded article can be obtained. The weight average molecular weight Mw(A2) can be measured by using GPC as described in the following Examples.

[0078] [End-capping agent] The terminals of the polyamide (A) contained in the polyamide composition of the present embodiment may be capped with a known terminal capping agent. Such an end-capping agent can also be added as a molecular weight regulator when producing a polyamide from the above dicarboxylic acid and the above diamine, or from at least one member selected from the group consisting of the above lactam and the above aminocarboxylic acid.

[0079] Examples of the terminal blocking agent include, but are not limited to, monocarboxylic acid, monoamine, acid anhydride (phthalic anhydride, etc.), monoisocyanate, monoester, monoalcohol, etc. Only one type of terminal blocking agent may be used alone, or two or more types may be used in combination. Among them, the terminal blocking agent is preferably a monocarboxylic acid or a monoamine. By blocking the terminals of the polyamide with the terminal blocking agent, the thermal stability of a molded article obtained from the polyamide composition tends to be superior.

[0080] The monocarboxylic acid that can be used as the end-capping agent may be any one that is reactive with amino groups that may be present at the terminals of the polyamide. Examples of the monocarboxylic acid include, but are not limited to, aliphatic monocarboxylic acids, alicyclic monocarboxylic acids, and aromatic monocarboxylic acids. Examples of the aliphatic monocarboxylic acid include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecylic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid. An example of the alicyclic monocarboxylic acid is cyclohexanecarboxylic acid. Examples of aromatic monocarboxylic acids include benzoic acid, toluic acid, α-naphthalenecarboxylic acid, β-naphthalenecarboxylic acid, methylnaphthalenecarboxylic acid, and phenylacetic acid. These monocarboxylic acids may be used alone or in combination of two or more. In particular, from the viewpoints of fluidity and mechanical strength, it is preferred that the terminals of the semi-aromatic polyamide (A2) be blocked with acetic acid.

[0081] The monoamine usable as the end-capping agent may be any monoamine that is reactive with a carboxyl group that may be present at the end of the polyamide, and may include, but is not limited to, aliphatic monoamines, alicyclic monoamines, aromatic monoamines, etc. Examples of the aliphatic monoamine include methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine. Examples of the alicyclic monoamine include cyclohexylamine and dicyclohexylamine. Examples of aromatic monoamines include aniline, toluidine, diphenylamine, and naphthylamine. These monoamines may be used alone or in combination of two or more.

[0082] Polyamide compositions containing polyamide end-capped with an end-capping agent tend to have better heat resistance, flowability, toughness, low water absorption, and rigidity.

[0083] <(A) Method for producing polyamide> When producing the polyamide (A) (aliphatic polyamide (A1) and semi-aromatic polyamide (A2)) contained in the polyamide composition of this embodiment, the amount of dicarboxylic acid added and the amount of diamine added are preferably approximately the same molar amount. Taking into consideration the amount of diamine that escapes to the outside of the reaction system during the polymerization reaction in the molar ratio, the molar amount of the total diamine per molar amount of the total dicarboxylic acids is preferably 0.9 to 1.2, more preferably 0.95 to 1.1, and even more preferably 0.98 to 1.05.

[0084] A method for producing a polyamide includes, but is not limited to, the following polymerization step (1) or (2). (1) A step of polymerizing a combination of a dicarboxylic acid constituting a dicarboxylic acid unit and a diamine constituting a diamine unit to obtain a polymer. (2) A step of polymerizing one or more members selected from the group consisting of lactam constituting the lactam unit and aminocarboxylic acid constituting the aminocarboxylic acid unit to obtain a polymer.

[0085] The method for producing a polyamide preferably further comprises, after the polymerization step, an increasing step of increasing the degree of polymerization of the polyamide. If necessary, the method may comprise, after the polymerization step and the increasing step, a capping step of capping the ends of the resulting polymer with a terminal capping agent.

[0086] Specific methods for producing polyamide include various methods as exemplified by the following 1) to 4). 1) A method in which an aqueous solution or suspension of one or more selected from the group consisting of a dicarboxylic acid-diamine salt, a mixture of a dicarboxylic acid and a diamine, a lactam, and an aminocarboxylic acid is heated and polymerized while maintaining the molten state (hereinafter, sometimes referred to as a "thermal melt polymerization method"). 2) A method in which the degree of polymerization of polyamide obtained by hot melt polymerization is increased while maintaining the polyamide in a solid state at a temperature below the melting point (hereinafter sometimes referred to as "hot melt polymerization / solid-state polymerization method"). 3) A method of polymerizing one or more members selected from the group consisting of dicarboxylic acid-diamine salts, mixtures of dicarboxylic acids and diamines, lactams, and aminocarboxylic acids while maintaining the solid state (hereinafter, sometimes referred to as the "solid-state polymerization method"). 4) A method of polymerization using a dicarboxylic acid halide component equivalent to a dicarboxylic acid and a diamine component (hereinafter, sometimes referred to as a "solution method").

[0087] Among them, as a specific method for producing polyamide, a production method including a hot melt polymerization method is preferable. When producing polyamide by the hot melt polymerization method, it is preferable to maintain the molten state until the polymerization is completed. In order to maintain the molten state, it is necessary to produce the polyamide composition under polymerization conditions suitable for the composition. Examples of the polymerization conditions include the following conditions. First, the polymerization pressure in the hot melt polymerization method is set to 14 kg / cm. 2 More than 25kg / cm 2 Heating is continued while controlling the pressure in the vessel to below atmospheric pressure (gauge pressure is 0 kg / cm 2 ) over 30 minutes or more until the blood pressure drops to 0.

[0088] In the method for producing a polyamide, the polymerization form is not particularly limited, and may be a batch type or a continuous type. The polymerization apparatus used for producing polyamide is not particularly limited, and known apparatuses can be used. Specific examples of the polymerization apparatus include an autoclave type reactor, a tumbler type reactor, and an extruder type reactor (such as a kneader).

[0089] Hereinafter, as a method for producing polyamide, a method for producing polyamide by a batch-type hot melt polymerization method will be specifically described, but the method for producing polyamide is not limited thereto. First, an aqueous solution containing about 40% to 60% by mass of raw material components for polyamide (a combination of dicarboxylic acid and diamine, and, if necessary, at least one selected from the group consisting of lactam and aminocarboxylic acid) is prepared. The aqueous solution is then concentrated to about 65% to 90% by mass in a concentration tank operated at a temperature of 110°C to 180°C and a pressure of about 0.035 MPa to 0.6 MPa (gauge pressure) to obtain a concentrated solution. The concentrated solution obtained is then transferred to an autoclave, and heating is continued until the pressure in the autoclave reaches about 1.2 MPa or more and 2.2 MPa or less (gauge pressure). Next, in the autoclave, the pressure is maintained at about 1.2 MPa to 2.2 MPa (gauge pressure) while removing at least one of water and gas components. Next, when the temperature reaches about 220° C. to 260° C., the pressure is reduced to atmospheric pressure (gauge pressure: 0 MPa). After the pressure in the autoclave is reduced to atmospheric pressure, the pressure can be reduced as necessary to effectively remove the by-product water. The autoclave is then pressurized with an inert gas such as nitrogen, and the polyamide melt is extruded from the autoclave as a strand. The extruded strand is cooled and cut to obtain polyamide pellets.

[0090] <(A) Characteristics of polyamide> [(A) Polyamide polymer end] The polymer terminals of the polyamide (A) contained in the polyamide composition of the present embodiment are not particularly limited, but can be classified and defined as follows: 1) to 4). That is, 1) the amino terminus, 2) the carboxy terminus, 3) the terminus provided by a capping agent, and 4) other terminus. 1) The amino terminus is a polymer end having an amino group (-NH2 group) and is derived from a diamine unit. 2) The carboxyl end is a polymer end having a carboxy group (-COOH group) and is derived from a dicarboxylic acid unit. 3) The term "terminals formed by a capping agent" refers to terminals formed when a capping agent is added during polymerization. Examples of the capping agent include the above-mentioned terminal capping agents. 4) The other terminals are polymer terminals not classified into the above 1) to 3). Specific examples of the other terminals include terminals generated by deammonia reaction of amino terminals, terminals generated by decarboxylation of carboxyl terminals, etc.

[0091] [(A) Weight average molecular weight Mw(A) of polyamide] As an index of the molecular weight of the (A) polyamide, the weight average molecular weight Mw(A) can be used. The weight average molecular weight Mw(A) of the polyamide is preferably 12000 or more and 44000 or less, more preferably 17500 or more and 40000 or less, even more preferably 20000 or more and 40000 or less, even more preferably 24000 or more and 40000 or less, particularly preferably 28000 or more and 37500 or less, and most preferably 32000 or more and 36000 or less. When the weight average molecular weight Mw(A) is within the above range, a polyamide composition having excellent flame retardancy, long-term heat resistance, weld strength, and laser welding strength can be obtained. The weight average molecular weight Mw(A) can be measured by using GPC as described in the following Examples.

[0092] <(B) Phosphorus-based flame retardants> The phosphorus-based flame retardant (B) contained in the polyamide composition of the present embodiment is not particularly limited as long as it is a flame retardant containing a phosphorus element and not a halogen element. Examples of the phosphorus-based flame retardant (B) include a phosphate ester flame retardant, a melamine polyphosphate flame retardant, a phosphazene flame retardant, a phosphinic acid flame retardant, and a red phosphorus flame retardant. Among these, the (B) phosphorus-based flame retardant is preferably a phosphate-based flame retardant, a melamine polyphosphate-based flame retardant, a phosphazene-based flame retardant or a phosphinic acid-based flame retardant, and is particularly preferably a phosphinic acid-based flame retardant.

[0093] Specifically, the phosphinic acid-based flame retardant may contain at least one phosphinic acid salt selected from the group consisting of a phosphinic acid salt represented by the following general formula (1) (hereinafter, may be abbreviated as "phosphinic acid salt (1)"), a diphosphinic acid salt represented by the following general formula (2) (hereinafter, may be abbreviated as "diphosphinic acid salt (2)"), and condensates thereof.

[0094] [ka]

[0095] (In general formula (1), R 11 and R 12 Each of M is independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. n11+ is a metal ion having a valence of n11. M is an element belonging to Group 2 or Group 15 of the periodic table, a transition element, zinc, or aluminum. n11 is 2 or 3. When n11 is 2 or 3, multiple R 11 and R 12 may be the same or different. In general formula (2), R 21 and R 22 Each of Y is independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. 21 M' is an alkylene group having 1 to 10 carbon atoms or an arylene group having 6 to 10 carbon atoms. m21+ is a metal ion having a valence of m21. M' is an element belonging to Group 2 or Group 15 of the periodic table, a transition element, zinc, or aluminum. n21 is an integer of 1 to 3. When n21 is 2 or 3, multiple R 21 , R 22 and Y 21 may be the same or different. m21 is 2 or 3. x is 1 or 2. When x is 2, multiple M' may be the same or different. n21, x, and m21 are integers that satisfy the relational formula 2×n21=m21×x.

[0096] [R 11 , R 12 , R 21 and R 22 ] R 11 , R 12 , R 21 and R 22 are each independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. When n11 is 2 or 3, a plurality of R 11 and R 12may be the same or different, but are preferably the same in terms of ease of production. 21 and R 22 may be the same or different, but is preferably the same in terms of ease of production. The alkyl group may be chain-like or cyclic, but is preferably chain-like. The chain-like alkyl group may be linear or branched. Examples of the linear alkyl group include methyl, ethyl, n-propyl, n-butyl, n-pentyl, and n-hexyl groups. Examples of branched alkyl groups include a 1-methylethyl group, a 1-methylpropyl group, a 2-methylpropyl group, a 1,1-dimethylethyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 3-methylbutyl group, a 1,1-dimethylpropyl group, a 1,2-dimethylpropyl group, a 2,2-dimethylpropyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 4-methylpentyl group, a 1,1-dimethylbutyl group, a 1,2-dimethylbutyl group, a 1,3-dimethylbutyl group, a 2,2-dimethylbutyl group, a 2,3-dimethylbutyl group, a 3,3-dimethylbutyl group, a 1-ethylbutyl group, a 2-ethylbutyl group, and a 1,1,2-trimethylpropyl group. Examples of the aryl group include a phenyl group and a naphthyl group. The alkyl group and the aryl group may have a substituent. Examples of the substituent in the alkyl group include an aryl group having 6 to 10 carbon atoms. Examples of the substituent in the aryl group include an alkyl group having 1 to 6 carbon atoms. Specific examples of the alkyl group having a substituent include a benzyl group. Specific examples of the aryl group having a substituent include a tolyl group and a xylyl group. Among them, R 11 , R 12 , R 21 and R 22As the alkyl group, an alkyl group having 1 to 6 carbon atoms is preferable, and a methyl group or an ethyl group is more preferable.

[0097] [Y 21 ] Y 21 is an alkylene group having 1 to 10 carbon atoms or an arylene group having 6 to 10 carbon atoms. 21 may be the same or different, but is preferably the same in terms of ease of production. The alkylene group may be either chain-like or cyclic, but is preferably chain-like. The chain-like alkylene group may be either linear or branched. Examples of linear alkylene groups include methylene, ethylene, trimethylene, tetramethylene, pentamethylene, and hexamethylene. Examples of branched alkylene groups include 1-methylethylene and 1-methylpropylene groups. Examples of the arylene group include a phenylene group and a naphthylene group. The alkylene group and the arylene group may have a substituent. Examples of the substituent in the alkylene group include an aryl group having 6 to 10 carbon atoms. Examples of the substituent in the arylene group include an alkyl group having 1 to 6 carbon atoms. Specific examples of the alkylene group having a substituent include a phenylmethylene group, a phenylethylene group, a phenyltrimethylene group, and a phenyltetramethylene group. Specific examples of the substituted arylene group include a methylphenylene group, an ethylphenylene group, a tert-butylphenylene group, a methylnaphthylene group, an ethylnaphthylene group, and a tert-butylnaphthylene group. Among them, Y 21 As the alkyl group, an alkylene group having 1 to 10 carbon atoms is preferable, and a methylene group or an ethylene group is more preferable.

[0098] [M and M'] M and M' are each independently an ion of an element belonging to Group 2 or Group 15 of the periodic table, an ion of a transition element, a zinc ion, or an aluminum ion. Examples of the ion of an element belonging to Group 2 of the periodic table include a calcium ion and a magnesium ion. Examples of the ion of an element belonging to Group 15 of the periodic table include a bismuth ion. Furthermore, when x is 2, a plurality of M' may be the same or different, but it is preferable that they are the same in terms of ease of production. Among these, M and M' are preferably calcium, zinc or aluminum, and more preferably calcium or aluminum.

[0099] [x] x represents the number of M' and is 1 or 2. x can be appropriately selected depending on the type of M' and the number of diphosphinic acids.

[0100] [n11 and n21] n11 represents the number of phosphinic acids and the valence of M, and is 2 or 3. n11 can be appropriately selected depending on the type and valence of M. n21 represents the number of diphosphinic acids and is an integer of 1 to 3. n21 can be appropriately selected depending on the type and number of M'.

[0101] [m21] m21 represents the valence of M' and is 2 or 3. n21, x, and m21 are integers that satisfy the relational expression 2×n21=m21×x.

[0102] Specific examples of preferred phosphinates (1) include calcium dimethylphosphinate, magnesium dimethylphosphinate, aluminum dimethylphosphinate, zinc dimethylphosphinate, calcium ethylmethylphosphinate, magnesium ethylmethylphosphinate, aluminum ethylmethylphosphinate, zinc ethylmethylphosphinate, calcium diethylphosphinate, magnesium diethylphosphinate, aluminum diethylphosphinate, zinc diethylphosphinate, calcium methyl-n-propylphosphinate, magnesium methyl-n-propylphosphinate, aluminum methyl-n-propylphosphinate, zinc methyl-n-propylphosphinate, methane di(methylphosphinate), ) calcium, magnesium methane di(methylphosphinate), aluminum methane di(methylphosphinate), zinc methane di(methylphosphinate), calcium benzene-1,4-(dimethylphosphinate), magnesium benzene-1,4-(dimethylphosphinate), aluminum benzene-1,4-(dimethylphosphinate), zinc benzene-1,4-(dimethylphosphinate), calcium methylphenylphosphinate, magnesium methylphenylphosphinate, aluminum methylphenylphosphinate, zinc methylphenylphosphinate, calcium diphenylphosphinate, magnesium diphenylphosphinate, aluminum diphenylphosphinate, zinc diphenylphosphinate, etc. Among them, as the phosphinate (1), calcium dimethylphosphinate or aluminum dimethylphosphinate is particularly preferred because of its excellent flame retardancy.

[0103] Specific examples of preferred diphosphinates (2) include calcium methane di(methylphosphinate), magnesium methane di(methylphosphinate), aluminum methane di(methylphosphinate), zinc methane di(methylphosphinate), calcium benzene-1,4-di(methylphosphinate), magnesium benzene-1,4-di(methylphosphinate), aluminum benzene-1,4-di(methylphosphinate), and zinc benzene-1,4-di(methylphosphinate).

[0104] The method for producing phosphinates is not particularly limited, but may be, for example, the methods described in Patent Document 5, Patent Document 6, and Patent Document 7. Specifically, they are produced in an aqueous solution using phosphinic acid and a metal carbonate, metal hydroxide, or metal oxide. These are essentially monomeric compounds, but also include polymeric phosphinates that are condensates with a condensation degree of 1 to 3 depending on the reaction conditions and environment.

[0105] The content of the (B) phosphorus-based flame retardant is preferably from 0.1 to 30 mass%, more preferably from 5 to 30 mass%, even more preferably from 10 to 29 mass%, and particularly preferably from 15 to 29 mass%, based on the total mass of the (A) polyamide, the (B) phosphorus-based flame retardant, and the (C) styrene copolymer. By setting the content of the (B) phosphorus-based flame retardant to the above lower limit or more, a polyamide composition having superior flame retardancy can be obtained. On the other hand, by setting the content of the (B) phosphorus-based flame retardant to the above upper limit or less, a polyamide composition having superior flame retardancy can be obtained without impairing the properties of the polyamide copolymer.

[0106] <(C) Styrene copolymer> The (C) styrene copolymer contained in the polyamide composition of the present embodiment means a styrene copolymer having a styrene content of 10% by weight or more. Specific examples of the (C) styrene copolymer include styrene-acrylonitrile copolymer (AS resin), copolymers of a styrene monomer with a maleimide monomer such as maleimide or N-phenylmaleimide, and an acrylamide monomer such as acrylamide. Furthermore, a copolymer in which a part of the styrene in a styrene polymer is replaced with a monomer such as α-methylstyrene, p-methylstyrene, vinylxylene, monochlorostyrene, dichlorostyrene, monobromostyrene, dibromostyrene, pt-butylstyrene, ethylstyrene, and vinylnaphthalene may be used. Among them, the (C) styrene copolymer is preferably a styrene-acrylonitrile copolymer (AS resin) having a styrene unit and an acrylonitrile unit, and the content of the acrylonitrile unit is preferably 30% by mass or more, and particularly preferably 35% by mass or more, based on the total mass of the constituent units of the (C) styrene copolymer. It is believed that the addition of styrene copolymer improves fluidity and dispersibility of flame retardant, which allows for the formation of a strong and dense char (a carbonized layer formed by combustion) during combustion, improving flame retardancy. It is also believed that the addition of styrene copolymer improves fluidity and dispersibility of heat stabilizer, which increases the radical trapping efficiency of the heat stabilizer and improves long-term heat resistance.

[0107] The content of the (C) styrene copolymer is from 0.1% by mass to 7% by mass, preferably from 0.5% by mass to 6% by mass, more preferably from 1% by mass to 5% by mass, and even more preferably from 1% by mass to 3% by mass, based on the total mass of the (A) polyamide, the (B) phosphorus-based flame retardant, and the (C) styrene copolymer. By setting the content of the (C) polymer within the above range, it is possible to obtain a polyamide composition which is excellent in flame retardancy and has good weld strength and long-term heat resistance when formed into a molded product.

[0108] [(C) Weight average molecular weight of polymer Mw(C)] As an index of the molecular weight of the (C) polymer, the weight average molecular weight Mw(C) can be used. The weight average molecular weight Mw(C) of the (C) polymer is preferably 5,000 or more and 220,000 or less, more preferably 5,000 or more and 150,000 or less, even more preferably 7,000 or more and 15,000 or less, and most preferably 70,000 or more and 100,000 or less. When the weight average molecular weight Mw(C) is within the above range, it is possible to obtain a polyamide composition which has both flame retardancy and excellent weld strength and long-term heat resistance when formed into a molded article. The weight average molecular weight Mw can be measured by using GPC as described in the following Examples.

[0109] <(D) Filler> The polyamide composition of the present embodiment may further contain a filler (D) in addition to the above components (A) to (C). By containing the filler (D), the polyamide composition can have more excellent mechanical properties such as toughness and rigidity.

[0110] The filler (D) contained in the polyamide composition of the present embodiment is not particularly limited, and examples thereof include glass fibers, carbon fibers, calcium silicate fibers, potassium titanate fibers, aluminum borate fibers, glass flakes, talc, kaolin, mica, hydrotalcite, zinc carbonate, calcium hydrogen phosphate, wollastonite, zeolite, boehmite, magnesium oxide, calcium silicate, sodium aluminosilicate, magnesium silicate, ketjen black, acetylene black, furnace black, carbon nanotubes, graphite, brass, copper, silver, aluminum, nickel, iron, calcium fluoride, montmorillonite, swellable fluoromica, apatite, and the like. These (D) fillers may be used alone or in combination of two or more. Among these, the (D) filler is preferably glass fiber, carbon fiber, glass flake, talc, kaolin, mica, calcium hydrogen phosphate, wollastonite, carbon nanotube, graphite, calcium fluoride, montmorillonite, expandable fluoromica, or apatite, from the viewpoint of rigidity, strength, etc. Furthermore, the (D) filler is more preferably glass fiber or carbon fiber, and further preferably glass fiber.

[0111] When the (D) filler is glass fiber or carbon fiber, the number average fiber diameter (D) is preferably 3 μm or more and 30 μm or less. The weight average fiber length (L) is preferably 100 μm or more and 750 μm or less. Furthermore, the aspect ratio ((L) / (D)) of the number average fiber diameter (D) to the weight average fiber length (L) is preferably 10 or more and 100 or less. By using glass fiber or carbon fiber having the above configuration, higher properties can be exhibited. In addition, when the filler (D) is glass fiber, the number average fiber diameter (D) is more preferably 3 μm or more and 30 μm or less, the weight average fiber length (L) is more preferably 103 μm or more and 500 μm or less, and the aspect ratio ((L) / (D)) is more preferably 3 or more and 100 or less.

[0112] (D) The number average fiber diameter and weight average fiber length of the filler can be measured by the following method. First, a molded product of the polyamide composition is dissolved in a solvent in which the polyamide is soluble, such as formic acid. Next, from the insoluble components obtained, for example, 100 or more fillers are arbitrarily selected. Then, the fillers can be observed with an optical microscope, a scanning electron microscope, or the like to determine the number of fillers.

[0113] The content of the (D) filler in the polyamide composition is preferably from 1 mass% to 80 mass%, more preferably from 10 mass% to 70 mass%, even more preferably from 15 mass% to 60 mass%, particularly preferably from 20 mass% to 55 mass%, and most preferably from 25 mass% to 50 mass%, relative to the total mass of the polyamide composition. When the content of the (D) filler is equal to or greater than the above lower limit, the mechanical properties such as strength and rigidity of the polyamide composition tend to be improved. On the other hand, when the content of the (D) filler is equal to or less than the above upper limit, the polyamide composition tends to have better laser welding strength. In particular, when the (D) filler is glass fiber and the content of the (D) filler is within the above range relative to the total mass of the polyamide composition, the mechanical properties such as strength and rigidity of the polyamide composition tend to be further improved.

[0114] <(E) Other additives> In addition to the above components (A) to (C), the polyamide composition of this embodiment may contain (E) other additives commonly used in polyamides, provided that the effects of the polyamide composition of this embodiment are not impaired. Examples of (E) other additives include (E1) moldability improvers, (E2) deterioration inhibitors, (E3) nucleating agents, (E4) heat stabilizers, etc. The content of (E) other additives in the polyamide composition of this embodiment varies depending on the type and use of the polyamide composition, and is not particularly limited as long as it is within a range that does not impair the effects of the polyamide composition of this embodiment.

[0115] [(E1) Moldability improver] The moldability improver (E1) contained in the polyamide composition of the present embodiment is not particularly limited, but examples thereof include higher fatty acids, higher fatty acid metal salts, higher fatty acid esters, higher fatty acid amides, etc. The moldability improver is also used as a "lubricant".

[0116] (higher fatty acids) Examples of higher fatty acids include linear or branched, saturated or unsaturated aliphatic monocarboxylic acids having 8 to 40 carbon atoms. Examples of the linear saturated aliphatic monocarboxylic acid having 8 to 40 carbon atoms include lauric acid, palmitic acid, stearic acid, behenic acid, and montanic acid. Examples of branched saturated aliphatic monocarboxylic acids having 8 to 40 carbon atoms include isopalmitic acid and isostearic acid. Examples of the linear unsaturated aliphatic monocarboxylic acid having 8 to 40 carbon atoms include oleic acid and erucic acid. Examples of the branched unsaturated aliphatic monocarboxylic acid having 8 to 40 carbon atoms include isooleic acid. Among these, stearic acid or montanic acid is preferred as the higher fatty acid.

[0117] (Higher fatty acid metal salts) The higher fatty acid metal salt is a metal salt of a higher fatty acid. Examples of the metal element of the metal salt include Group 1, Group 2 and Group 3 elements of the Periodic Table, zinc, aluminum, and the like. Examples of Group 1 elements in the Periodic Table include sodium and potassium. Examples of Group 2 elements in the Periodic Table include calcium and magnesium. Examples of Group 3 elements in the periodic table include scandium and yttrium. Among these, elements of Groups 1 and 2 of the Periodic Table of the Elements or aluminum are preferred, and sodium, potassium, calcium, magnesium or aluminum is more preferred.

[0118] Specific examples of higher fatty acid metal salts include calcium stearate, aluminum stearate, zinc stearate, magnesium stearate, calcium montanate, sodium montanate, calcium palmitate, and the like. Among these, as the higher fatty acid metal salt, a metal salt of montanic acid or a metal salt of stearic acid is preferred.

[0119] (Higher fatty acid ester) The higher fatty acid ester is an ester of a higher fatty acid and an alcohol. As the higher fatty acid ester, an ester of an aliphatic carboxylic acid having 8 to 40 carbon atoms and an aliphatic alcohol having 8 to 40 carbon atoms is preferred. Examples of the aliphatic alcohol having 8 to 40 carbon atoms include stearyl alcohol, behenyl alcohol, and lauryl alcohol. Specific examples of higher fatty acid esters include stearyl stearate and behenyl behenate.

[0120] (Higher fatty acid amide) Higher fatty acid amides are amide compounds of higher fatty acids. Examples of higher fatty acid amides include stearic acid amide, oleic acid amide, erucic acid amide, ethylene bisstearylamide, ethylene bisoleylamide, N-stearyl stearic acid amide, and N-stearyl erucic acid amide. These higher fatty acids, higher fatty acid metal salts, higher fatty acid esters and higher fatty acid amides may each be used alone or in combination of two or more.

[0121] [(E2) Deterioration inhibitor] The deterioration inhibitor (E2) contained in the polyamide composition of the present embodiment is used for the purposes of preventing thermal deterioration and discoloration when heated, and improving heat aging resistance. The deterioration inhibitor (E2) is not particularly limited, but examples thereof include copper compounds, phenol-based stabilizers, phosphite-based stabilizers, hindered amine-based stabilizers, triazine-based stabilizers, benzotriazole-based stabilizers, benzophenone-based stabilizers, cyanoacrylate-based stabilizers, salicylate-based stabilizers, and sulfur-based stabilizers. Examples of the copper compound include copper acetate and copper iodide. Examples of the phenol-based stabilizer include hindered phenol compounds. These deterioration inhibitors (E2) may be used alone or in combination of two or more.

[0122] [(E3) Nucleating agent] (E3) Nucleating agent means a substance that, when added, provides at least one of the following effects (1) to (3). (1) The effect of increasing the crystallization peak temperature of the polyamide composition. (2) The effect of reducing the difference between the extrapolated onset temperature and the extrapolated end temperature of the crystallization peak. (3) The effect of making the spherulites in the resulting molded product finer or more uniform in size.

[0123] (E3) Nucleating agents include, but are not limited to, talc, boron nitride, mica, kaolin, silicon nitride, carbon black, potassium titanate, molybdenum disulfide, and the like. The nucleating agent (E3) may be used alone or in combination of two or more kinds. Among these, as the nucleating agent (E3), talc or boron nitride is preferred from the viewpoint of nucleating agent effect.

[0124] In addition, since the effect of the nucleating agent is high, the number average particle size of the nucleating agent (E3) is preferably 0.01 μm or more and 10 μm or less. The number average particle size of the nucleating agent can be measured by the following method. First, the molded product is dissolved in a solvent in which polyamide is soluble, such as formic acid. Next, from the insoluble components obtained, nucleating agents having, for example, 100 or more particles are arbitrarily selected. Then, the particle size can be determined by observing the particles with an optical microscope, a scanning electron microscope, or the like.

[0125] The content of the nucleating agent in the polyamide composition of the present embodiment is preferably 0.001 parts by mass or more and 1 part by mass or less, more preferably 0.001 parts by mass or more and 0.5 parts by mass or less, and even more preferably 0.001 parts by mass or more and 0.09 parts by mass or less, relative to 100 parts by mass of polyamide ((A) aliphatic polyamide and (B) semi-aromatic polyamide). By setting the content of the nucleating agent to be equal to or more than the above lower limit per 100 parts by mass of polyamide, the heat resistance of the polyamide composition tends to be further improved, and by setting the content of the nucleating agent to be equal to or less than the above upper limit per 100 parts by mass of polyamide, a polyamide composition having superior toughness can be obtained.

[0126] [(E4) Heat stabilizer] (E4) Heat stabilizers include, but are not limited to, phenol-based heat stabilizers, phosphorus-based heat stabilizers, amine-based heat stabilizers, and metal salts of elements in Groups 3, 4, and 11 to 14 of the Periodic Table of the Elements.

[0127] (Phenol-based heat stabilizer) Examples of the phenol-based heat stabilizer include, but are not limited to, hindered phenol compounds, etc. Hindered phenol compounds have the property of imparting excellent heat resistance and light resistance to resins such as polyamides and fibers. Examples of the hindered phenol compound include, but are not limited to, N,N'-hexane-1,6-diylbis[3-(3,5-di-t-butyl-4-hydroxyphenylpropionamide), pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], onate], 3,9-bis{2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propynyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, 3,5-di-t-butyl-4-hydroxybenzylphosphonate-diethyl ester, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid, and the like. These hindered phenol compounds may be used alone or in combination of two or more.

[0128] When a phenol-based heat stabilizer is used, the content of the phenol-based heat stabilizer in the polyamide composition is preferably 0.01 mass % or more and 1 mass % or less, and more preferably 0.05 mass % or more and 1 mass % or less, relative to the total mass of the polyamide composition. When the content of the phenol-based heat stabilizer is within the above range, the heat aging resistance of the polyamide composition can be further improved, and the amount of gas generation can be further reduced.

[0129] (Phosphorus-based heat stabilizer) Examples of phosphorus-based heat stabilizers include, but are not limited to, pentaerythritol-type phosphite compounds, trioctyl phosphite, trilauryl phosphite, tridecyl phosphite, octyl diphenyl phosphite, trisisodecyl phosphite, phenyl diisodecyl phosphite, phenyl di(tridecyl) phosphite, diphenyl isooctyl phosphite, diphenyl isodecyl phosphite, diphenyl (tridecyl) phosphite, triphenyl phosphite, tris(nonylphenyl) phosphite, Tris(2,4-di-t-butylphenyl)phosphite, tris(2,4-di-t-butyl-5-methylphenyl)phosphite, tris(butoxyethyl)phosphite, 4,4'-butylidene-bis(3-methyl-6-t-butylphenyl-tetra-tridecyl)diphosphite, tetra(C12-C15 mixed alkyl)-4,4'-isopropylidene diphenyl diphosphite, 4,4'-isopropylidenebis(2-t-butylphenyl)-di(nonylphenyl)phosphite, tris(biphenyl)phosphite, tetra(tridecyl) sil)-1,1,3-tris(2-methyl-5-t-butyl-4-hydroxyphenyl)butane diphosphite, tetra(tridecyl)-4,4'-butylidenebis(3-methyl-6-t-butylphenyl)diphosphite, tetra(C1-C15 mixed alkyl)-4,4'-isopropylidene diphenyl diphosphite, tris(mono, di mixed nonylphenyl)phosphite, 4,4'-isopropylidenebis(2-t-butylphenyl)-di(nonylphenyl)phosphite, 9,10-dihydro-9-oxa-10-phosphaphenan Threonine-10-oxide, tris(3,5-di-t-butyl-4-hydroxyphenyl)phosphite, hydrogenated-4,4'-isopropylidene diphenyl polyphosphite, bis(octylphenyl)-bis(4,4'-butylidenebis(3-methyl-6-t-butylphenyl))-1,6-hexanol diphosphite, hexatridecyl-1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)diphosphite, tris(4,4'-isopropylidenebis(2-t-butylphenyl))phosphite, tris(1,3-stearoyloxyisopropyl)phosphite, 2,2-methylenebis(4,6-di-t-butylphenyl)octylphosphite, 2,2-methylenebis(3-methyl-4,6-di-t-butylphenyl)2-ethylhexylphosphite, tetrakis(2,4-di-t-butyl-5-methylphenyl)-4,4'-biphenylene diphosphite, tetrakis(2,4-di-t-butylphenyl)-4,4'-biphenylene diphosphite, etc. These phosphorus-based heat stabilizers may be used alone or in combination of two or more.

[0130] Examples of the pentaerythritol type phosphite compound include, but are not limited to, 2,6-di-t-butyl-4-methylphenyl-phenyl-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-methyl-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-2-ethylhexyl-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-isodecyl-pentaerythritol diphosphite, 2,6-di-t-butyl- 4-Methylphenyl-lauryl-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-isotridecyl-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-stearyl-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-cyclohexyl-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-benzyl-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl- Ethyl cellosolve-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-butylcarbitol-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-octylphenyl-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-nonylphenyl pentaerythritol diphosphite, bis(2,6-di-t-butyl-4-methylphenyl) pentaerythritol diphosphite, bis(2,6-di-t-butyl-4-ethylphenyl) Pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-2,6-di-t-butylphenyl-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-2,4-di-t-butylphenyl-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-2,4-di-t-octylphenyl-pentaerythritol diphosphite, 2,6-di-t-butyl-4-methylphenyl-2-cyclohexylphenyl-pentaerythritol diphosphite, 2,Examples include 6-di-t-amyl-4-methylphenyl-phenyl pentaerythritol diphosphite, bis(2,6-di-t-amyl-4-methylphenyl) pentaerythritol diphosphite, and bis(2,6-di-t-octyl-4-methylphenyl) pentaerythritol diphosphite. These pentaerythritol-type phosphite compounds may be used alone or in combination of two or more.

[0131] When a phosphorus-based heat stabilizer is used, the content of the phosphorus-based heat stabilizer in the polyamide composition is preferably 0.01 mass % or more and 1 mass % or less, and more preferably 0.05 mass % or more and 1 mass % or less, based on the total mass of the polyamide composition. When the content of the phosphorus-based heat stabilizer is within the above range, the heat aging resistance of the polyamide composition can be further improved, and the amount of gas generation can be further reduced.

[0132] (Amine-based heat stabilizer) Examples of the amine-based heat stabilizer include, but are not limited to, 4-acetoxy-2,2,6,6-tetramethylpiperidine, 4-stearoyloxy-2,2,6,6-tetramethylpiperidine, 4-acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(phenylacetoxy)-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 4-methoxy-2,2,6,6-tetramethylpiperidine, 4-stearyloxy-2,2,6,6-tetramethylpiperidine, and the like. 4-cyclohexyloxy-2,2,6,6-tetramethylpiperidine, 4-benzyloxy-2,2,6,6-tetramethylpiperidine, 4-phenoxy-2,2,6,6-tetramethylpiperidine, 4-(ethylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, 4-(cyclohexylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, 4-(phenylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, bis(2,2,6,6-tetramethyl-4-piperidyl)-carbonate, bis (2,2,6,6-tetramethyl-4-piperidyl)-oxalate, bis(2,2,6,6-tetramethyl-4-piperidyl)-malonate, bis(2,2,6,6-tetramethyl-4-piperidyl)-sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)-adipate, bis(2,2,6,6-tetramethyl-4-piperidyl)-terephthalate, 1,2-bis(2,2,6,6-tetramethyl-4-piperidyloxy)-ethane, α,α'-bis(2,2,6,6-tetramethyl-4-piperidyloxy)-p-xylene , bis(2,2,6,6-tetramethyl-4-piperidyltolylene-2,4-dicarbamate, bis(2,2,6,6-tetramethyl-4-piperidyl)-hexamethylene-1,6-dicarbamate, tris(2,2,6,6-tetramethyl-4-piperidyl)-benzene-1,3,5-tricarboxylate, tris(2,2,6,6-tetramethyl-4-piperidyl)-benzene-1,3,4-tricarboxylate, 1-[2-{3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxy}butyl]-4-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxy]2,2,6,6-tetramethylpiperidine, a condensation product of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol, and β,β,β',β'-tetramethyl-3,9-[2,4,8,10-tetraoxaspiro(5,5)undecane]diethanol, etc. These amine-based heat stabilizers may be used alone or in combination of two or more.

[0133] When an amine-based heat stabilizer is used, the content of the amine-based heat stabilizer in the polyamide composition is preferably 0.01 mass % or more and 1 mass % or less, and more preferably 0.05 mass % or more and 1 mass % or less, based on the total mass of the polyamide composition. When the content of the amine-based heat stabilizer is within the above range, the heat aging resistance of the polyamide composition can be further improved, and the amount of gas generation can be further reduced.

[0134] (Metal salts of elements in groups 3, 4, and 11 to 14 of the periodic table) There are no particular limitations on the metal salts of elements in Groups 3, 4, and 11 to 14 of the periodic table, so long as they are salts of metals belonging to these groups. Among these, copper salts are preferred from the viewpoint of further improving the heat aging resistance of the polyamide composition, and examples of such copper salts include, but are not limited to, copper acetate, copper propionate, copper benzoate, copper adipate, copper terephthalate, copper isophthalate, copper salicylate, copper nicotinate, copper stearate, and copper complex salts in which copper is coordinated with a chelating agent. Examples of the chelating agent include ethylenediamine and ethylenediaminetetraacetic acid. These copper salts may be used alone or in combination of two or more. Among them, copper acetate is preferred as the copper salt. When copper acetate is used, a polyamide composition having excellent heat aging resistance and capable of more effectively suppressing metal corrosion of the screw and cylinder part during extrusion (hereinafter, may be simply referred to as "metal corrosion") can be obtained.

[0135] When a copper salt is used as the heat stabilizer (E4), the content of the copper salt in the polyamide composition is preferably from 0.01 to 0.60 mass%, more preferably from 0.02 to 0.40 mass%, relative to the total mass of the polyamide (A). When the content of the copper salt is within the above range, the heat aging resistance of the polyamide composition can be further improved, and copper precipitation and metal corrosion can be more effectively suppressed.

[0136] In addition, the content of copper element derived from the above copper salt is, from the viewpoint of improving the heat aging resistance of the polyamide composition, (A) polyamide 10 6 The amount is preferably from 10 to 2000 parts by mass, more preferably from 30 to 1500 parts by mass, and even more preferably from 50 to 500 parts by mass, based on parts by mass (1 million parts by mass).

[0137] The components of the heat stabilizer (E4) explained above may be used alone or in combination of two or more.

[0138] <Method for producing polyamide composition> The method for producing the polyamide composition of the present embodiment is not particularly limited, so long as it is a method of mixing polyamide (A) with each of the components (B) to (C) and, if necessary, each of the components (D) and (E).

[0139] Examples of a method for mixing the above components (A) to (C) and, if necessary, the components (D) and (E) include the following method (1) or (2). (1) The above components (A) to (C), and, if necessary, components (D) and (E), are mixed using a Henschel mixer or the like, and then fed to a melt kneader for kneading. (2) A method in which the above-mentioned components (A) to (C) and, if necessary, component (D) are mixed in advance using a Henschel mixer or the like in a single-screw or twin-screw extruder to prepare a mixture containing the components (A) to (C) and, if necessary, component (E), and the mixture is fed to a melt kneader and kneaded, and then, optionally, component (D) is blended in through a side feeder.

[0140] The components constituting the polyamide composition may be supplied to the melt kneader by supplying all of the components to the same supply port at once, or by supplying each of the components from a different supply port.

[0141] When the (A) polyamide contains the (A1) aliphatic polyamide, the melt-kneading temperature is preferably at least about 1°C and not more than about 100°C higher than the melting point of the (A1) aliphatic polyamide, and more preferably at least about 10°C and not more than about 50°C higher than the melting point of the (A1) aliphatic polyamide. The shear rate in the mixer is 100 sec -1 The average residence time during kneading is preferably about 0.5 minutes or more and 5 minutes or less. The melt-kneading apparatus may be any known apparatus, and for example, a single-screw or twin-screw extruder, a Banbury mixer, a melt-kneader (mixing roll, etc.), etc. are preferably used. The blending amount of each component when producing the polyamide composition of the present embodiment is the same as the content of each component in the polyamide composition described above.

[0142] ≪Molded products≫ The molded article of the present embodiment is produced by molding the polyamide composition of the above embodiment. The molded article of the present embodiment contains a non-halogen flame retardant and yet has excellent flame retardancy and long-term heat resistance.

[0143] The method for obtaining the molded product is not particularly limited, and any known molding method can be used. Examples of known molding methods include extrusion molding, injection molding, vacuum molding, blow molding, injection compression molding, decorative molding, other material molding, gas-assisted injection molding, foam injection molding, low-pressure molding, ultra-thin-wall injection molding (ultra-high-speed injection molding), and in-mold composite molding (insert molding, outsert molding).

[0144] <Application> The molded article of the present embodiment contains the polyamide composition of the above embodiment, has excellent flame retardancy and long-term heat resistance, and can be used for various applications. The molded article of the present embodiment can be suitably used in, for example, the automotive field, the electrical and electronic field, the mechanical and industrial field, the office equipment field, and the aviation and space field.

[0145] ≪Addition method≫ The method of the present embodiment is a method of adding (C) a styrene copolymer as a flame retardant auxiliary to a resin composition containing (A) a polyamide and (B) a phosphorus-based flame retardant. As described above, by adding (C) a styrene copolymer to a resin composition containing (A) a polyamide and (B) a phosphorus-based flame retardant, the fluidity of the resin composition is improved, and the dispersibility of the flame retardant (B) a phosphorus-based flame retardant is improved. Therefore, it is presumed that a strong and dense char (a carbonized layer formed by combustion) can be formed during combustion, and the flame retardancy is improved. In addition, by adding (C) a styrene copolymer to a resin composition containing (A) a polyamide and (B) a phosphorus-based flame retardant, the fluidity of the resin composition is improved, and the dispersibility of the heat stabilizer is improved, and therefore it is presumed that the radical trapping efficiency of the heat stabilizer is increased, and the long-term heat resistance is improved.

[0146] The resin composition may contain the components (D) and (E) in addition to the components (A) and (B). The components (A) to (E) may be the same as those exemplified for the polyamide composition. EXAMPLES

[0147] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples.

[0148] Each of the components of the polyamide composition used in the present examples and comparative examples will be described below.

[0149] <Components> [(A1) Aliphatic polyamide] A1-1: Polyamide 66

[0150] [(A2) Semi-aromatic polyamide] A2-1: Polyamide 6I A2-2: Polyamide 6I / 6T (manufactured by EMS Co., Ltd., model number: G21, content of isophthalic acid units in all dicarboxylic acid units is 70 mol%, molecular weight: 27,000)

[0151] [(B) Phosphorus-based flame retardants] B-1: Phosphinic acid flame retardant Aluminum diethylphosphinate (manufactured by Clariant, product name: "Exolit OP1230") B-2: Phosphinic acid flame retardant Calcium diethylphosphinate (manufactured by Taihei Chemical Industry Co., Ltd.)

[0152] [(B') Flame retardants other than phosphorus-based] B'-1: Nitrogen-based flame retardant Melamine cyanurate (Nissan Chemical Industries, Ltd.)

[0153] [(C) Styrene copolymer] C-1: Styrene-acrylonitrile copolymer (AS) (manufactured by Asahi Kasei Corporation) (acrylonitrile content 40% by weight, molecular weight: 80,000) C-2: Styrene-acrylonitrile copolymer (AS) (manufactured by Asahi Kasei Corporation) (acrylonitrile content: 25% by weight, molecular weight: 140,000) C-3: Styrene-acrylonitrile copolymer (AS) (manufactured by Asahi Kasei Corporation) (acrylonitrile content 30% by weight, molecular weight: 130,000)

[0154] [(D) Filler] D-1: Glass fiber (GF) (manufactured by Nippon Electric Glass, product name "ECS03T275H", average fiber diameter 10 μmφ, cut length 3 mm)

[0155] [(E) Other additives] E-1: Phenol-based heat stabilizer (manufactured by Ciba Specialty Chemicals, product name: "Irganox 1098")

[0156] <Production of polyamide> The production methods of the aliphatic polyamide A1-1 and the semi-aromatic polyamide A2-1 are described in detail below. The aliphatic polyamide A1-1 and the semi-aromatic polyamide A2-1 obtained by the production methods described below were dried in a nitrogen stream to adjust the moisture content to about 0.2% by mass, and then used as raw materials for the polyamide compositions in the examples and comparative examples described below.

[0157] [Synthesis Example 1] Synthesis of aliphatic polyamide A1-1 (polyamide 66) The polymerization reaction of polyamide was carried out by the "thermal melt polymerization method" as follows. First, 1500 g of an equimolar salt of adipic acid and hexamethylenediamine was dissolved in 1500 g of distilled water to prepare a homogeneous aqueous solution of 50% by mass of the raw material monomers. This aqueous solution was charged into an autoclave with an internal volume of 5.4 L and substituted with nitrogen. Next, the solution was concentrated by gradually removing steam to a solution concentration of 70% by mass while stirring at a temperature of about 110°C to 150°C. Next, the internal temperature was raised to 220°C. At this time, the autoclave was pressurized to 1.8 MPa. The reaction was continued for 1 hour while gradually removing steam and maintaining the pressure at 1.8 MPa until the internal temperature reached 245°C. Next, the pressure was lowered over 1 hour. Next, the inside of the autoclave was maintained under a reduced pressure of 650 torr (86.66 kPa) for 10 minutes using a vacuum device. At this time, the final internal temperature of the polymerization was 265°C. The mixture was then pressurized with nitrogen to form a strand from the lower spinneret (nozzle), cooled with water, cut, and discharged in pellet form. The pellets were then dried at 100°C under a nitrogen atmosphere for 12 hours to obtain aliphatic polyamide A1-1 (polyamide 66). The resulting aliphatic polyamide A1-1 (polyamide 66) had Mw(A1)=40,000.

[0158] [Synthesis Example 2] Synthesis of semi-aromatic polyamide A2-1 (polyamide 6I) The polymerization reaction of polyamide was carried out by the "thermal melt polymerization method" as follows. First, 1500 g of an equimolar salt of isophthalic acid and hexamethylenediamine, 1.5 mol % excess adipic acid relative to the total equimolar salt components, and 0.5 mol % acetic acid were dissolved in 1500 g of distilled water to prepare a 50 mass % equimolar homogeneous aqueous solution of the raw material monomers. Next, the solution was concentrated by gradually removing steam to a solution concentration of 70 mass % while stirring at a temperature of about 110°C to 150°C. Next, the internal temperature was raised to 220°C. At this time, the autoclave was pressurized to 1.8 MPa. The reaction was continued for 1 hour while gradually removing steam and maintaining the pressure at 1.8 MPa until the internal temperature reached 245°C. Next, the pressure was reduced over 30 minutes. Next, the inside of the autoclave was maintained at a reduced pressure of 650 torr (86.66 kPa) for 10 minutes using a vacuum device. At this time, the final internal temperature of the polymerization was 265°C. The mixture was then pressurized with nitrogen to form a strand from the lower spinneret (nozzle), cooled with water, cut, and discharged in pellet form. The pellets were then dried at 100°C under a nitrogen atmosphere for 12 hours to obtain semi-aromatic polyamide A2-1 (polyamide 6I). The resulting semi-aromatic polyamide A2-1 (polyamide 6I) had a content of isophthalic acid units in dicarboxylic acid units of 100 mol % and Mw(A2)=20,000.

[0159] <Physical properties and evaluation> First, the pellets of the polyamide compositions obtained in the Examples and Comparative Examples were dried in a nitrogen stream to reduce the moisture content in the polyamide compositions to 500 ppm or less. Next, the pellets of each polyamide composition with the adjusted moisture content were used to measure various physical properties and perform various evaluations using the following methods.

[0160] [Physical property 1] tan δ peak temperature Using a PS40E injection molding machine manufactured by Nissei Kogyo Co., Ltd., a molded product was molded according to JIS-K7139 under the injection molding conditions of a cylinder temperature of 290°C, a mold temperature of 100°C, injection for 10 seconds, and cooling for 10 seconds. The molded product was measured under the following conditions using a dynamic viscoelasticity evaluation device (EPLEXOR500N manufactured by GABO Co., Ltd.).

[0161] (Measurement conditions) Measurement mode: Tensile Measurement frequency: 8.00Hz Heating rate: 3℃ / min Temperature range: -100℃ to 250℃

[0162] The ratio of the storage modulus E1 to the loss modulus E2 (E2 / E1) was defined as tan δ, and the highest temperature was defined as the tan δ peak temperature.

[0163] [Physical Property 2] Molecular weight of polyamide composition (Mw) The weight average molecular weight (Mw) of the polyamide compositions obtained in the Examples and Comparative Examples was measured using GPC under the following measurement conditions.

[0164] (Measurement conditions) Measuring device: Tosoh Corporation, HLC-8020 Solvent: Hexafluoroisopropanol solvent Standard sample: PMMA (polymethyl methacrylate) (Polymer Laboratory) GPC columns: TSK-GEL GMHHR-M and G1000HHR

[0165] [Rating 1] Flame retardant Measurements were performed using the method of UL94 (a standard established by Underwriters Laboratories Inc., USA). The test pieces (length 127 mm, width 12.7 mm, thickness 1.6 mm) were prepared by attaching a mold for UL test pieces (mold temperature = 100 ° C.) to an injection molding machine (PS40E manufactured by Nissei Kogyo Co., Ltd.) and molding each polyamide composition at a cylinder temperature of 290 ° C. The injection pressure was set at a pressure of + 2% of the full filling pressure when molding the UL test pieces. The flame retardant grade was evaluated according to the UL94 standard (vertical flame test) to see whether it was V-0, V-1, or V-2. The smaller the grade number, the higher the flame retardant.

[0166] [Evaluation 2] Weld strength Molding was performed using an injection molding machine (PS40E manufactured by Nissei Kogyo Co., Ltd.) equipped with a mold in which molten resin flows from both ends of the length direction of a shape of 127 mm in length, 12.7 mm in width, and 1.6 mm in thickness, and a test specimen was obtained. The specific molding conditions were set to injection + pressure holding time 25 seconds, cooling time 15 seconds, mold temperature 80°C, and molten resin temperature at the melting peak temperature (Tm2) + 20°C on the high temperature side of polyamide. A tensile test was performed on this molded test specimen in accordance with the method of ASTM D638, except that the chuck distance was 50 mm and the tensile speed was 50 mm / min, and the tensile strength was determined.

[0167] [Evaluation 3] Long-term heat resistance The multipurpose test piece (A type) for the above tensile strength was heated at 120°C in a hot air circulating oven to cause thermal degradation. After 1000 hours in the oven, the specimen was removed from the oven and cooled at 23°C for at least 24 hours. The cooled multipurpose test specimen (A type) was then subjected to a tensile test at a tensile speed of 5 mm / min in accordance with ISO 527 in the same manner as described above to measure each tensile strength. The heat aging retention rate was calculated using the following formula.

[0168] Heat resistance retention rate (%) = tensile strength after aging / tensile strength before aging x 100

[0169] [Evaluation 4] Laser weld strength Each polyamide resin composition was dry-blended with a colored masterbatch for laser welding (Orient Chemical Industry: eBIND ACW-9871, hereinafter simply referred to as ACW) at a dilution ratio of 60 times, molded into a flat plate of 60 mm × 60 mm × plate thickness 2.0 mm, and cut into a flat plate of 28 mm × 60 mm × plate thickness 2.0 mm to produce the component A. The specific molding conditions were set as follows: the mold temperature was 80°C, and the molten resin temperature was set to the melting peak temperature (Tm2) + 20°C on the high-temperature side of the polyamide. In addition, 1,500 ppm of carbon black (primary particle size 27 nm) was dry blended with 100 parts by mass of the polyamide resin composition, and a flat plate of 60 mm x 60 mm x 2.0 mm thickness was molded and cut into a flat plate of 25 mm x 60 mm x 2.0 mm thickness to prepare member B. With part A and part B overlapping and fixed in place by 20 mm in the long side direction of each part, the head of the laser welding machine was used to irradiate the laser from part A side to one end of the test piece parallel to the short side of the test piece with a scanning speed of 50.0 mm / sec and an output of 150 W, and at the same time, that part was cooled with air to prepare the test piece. The prepared test piece was subjected to a tensile test using an Instron universal testing machine with a 30 kN load cell, with both ends of member A and member B of the test piece being clamped in chucks at a chuck distance of 30 mm and a tensile test speed of 5.0 mm / min, to measure the maximum point load.

[0170] <Production of polyamide composition> [Example 1] Using a TEM 35mm twin-screw extruder (set temperature: 280°C, screw rotation speed: 300 rpm) manufactured by Toshiba Machine Co., Ltd., (A) polyamide A1-1, (C) styrene copolymer C-1, and (E) other additives E-1 were blended in advance and fed from the top feed port provided at the most upstream part of the extruder. In addition, (B) phosphorus-based flame retardant B-1 and (D) filler D-1 were fed from the side feed port on the downstream side of the extruder (in a state where the resin fed from the top feed port was fully melted). Next, the molten kneaded product extruded from the die head was cooled in a strand shape and pelletized to obtain pellets of a polyamide composition. The blending amounts were as shown in Table 1. Furthermore, a molded article was produced by using the obtained pellets of the polyamide composition according to the above-mentioned method, and various physical properties were measured and evaluated. The evaluation results are shown in Table 1.

[0171] [Examples 2 to 12, Comparative Examples 1 to 6] The composition of components (A) to (E) was as shown in Table 1, and the production method was the same as that of Example 1. The evaluation results are shown in Tables 1 and 2. In Table 2, "ND" stands for No Data, and indicates that the strength of the produced test piece was so low that it could not be measured.

[0172] [Table 1]

[0173] [Table 2]

[0174] As shown in Table 1, in the polyamide compositions (Examples 1 to 12) containing (A) a polyamide, (B) a phosphorus-based flame retardant, and (C) a styrene copolymer, in which the content of the styrene copolymer (C) relative to the total mass of the components (A) to (C) was in the range of 0.1 mass % or more and 7 mass % or less, molded articles that were compatible with flame retardancy and long-term heat resistance were obtained.

[0175] Furthermore, the polyamide compositions (Examples 2 to 12) containing (A1) aliphatic polyamide A1-1 and (A2) semi-aromatic polyamide A2-1 or A2-2 gave molded articles with particularly good laser weld strength. Furthermore, in the polyamide compositions (Examples 2, 3, and 6 to 10) containing the styrene copolymer C-1 having a high acrylonitrile content, molded articles having particularly good flame retardancy and long-term heat resistance were obtained.

[0176] On the other hand, in the polyamide compositions (Comparative Examples 1 to 6) that did not contain the (C) styrene copolymer or in which the content of the (C) styrene copolymer exceeded 7 mass% relative to the total mass of the (A) to (C) components, no molded articles that achieved both flame retardancy and long-term heat resistance were obtained.

[0177] From the above, it has become clear that the polyamide composition of the present embodiment can provide a molded article that has both flame retardancy and long-term heat resistance while containing a non-halogen flame retardant. [Industrial Applicability]

[0178] According to the polyamide composition of the present embodiment, a molded article having both flame retardancy and long-term heat resistance can be obtained while containing a non-halogen flame retardant. The molded article of the present embodiment can be suitably used in the fields of automobiles, electrical and electronics, machinery and industry, office equipment, and aviation and space.

Claims

1. (A) polyamide, (B) a phosphorus-based flame retardant, and (C) Styrene copolymer A polyamide composition comprising: The polyamide composition, wherein the content of the styrene copolymer (C) is 0.1 mass % or more and 7.0 mass % or less based on the total mass of the polyamide (A), the phosphorus-based flame retardant (B), and the styrene copolymer (C).

2. 2. The polyamide composition according to claim 1, wherein the polyamide (A) comprises: (A1) an aliphatic polyamide; and (A2) a semi-aromatic polyamide containing diamine units and dicarboxylic acid units.

3. 3. The polyamide composition according to claim 2, wherein the semi-aromatic polyamide (A2) contains 50 mol % or more of isophthalic acid units in all dicarboxylic acid units constituting the semi-aromatic polyamide (A2).

4. 4. The polyamide composition according to claim 2, wherein the semi-aromatic polyamide (A2) contains 75 mol % or more of isophthalic acid units in all dicarboxylic acid units constituting the semi-aromatic polyamide (A2).

5. The polyamide composition according to any one of claims 2 to 4, wherein the semi-aromatic polyamide (A2) contains 100 mol% of isophthalic acid units in all dicarboxylic acid units constituting the semi-aromatic polyamide (A2).

6. The polyamide composition according to any one of claims 1 to 5, wherein the styrene copolymer (C) contains acrylonitrile units and styrene units.

7. The (C) styrene copolymer contains acrylonitrile units and styrene units, The polyamide composition according to any one of claims 1 to 6, wherein the content of the acrylonitrile units is 30 mass% or more based on the total mass of the constituent units of the styrene copolymer (C).

8. The polyamide composition according to any one of claims 1 to 7, wherein the (B) phosphorus-based flame retardant comprises at least one phosphinate selected from the group consisting of a phosphinate represented by the following general formula (1), a diphosphinate represented by the following general formula (2), and a condensate thereof: [Formula 1] (In general formula (1), R 11 and R 12 Each of M is independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. n11+ is a metal ion having a valence of n11. M is an element belonging to Group 2 or Group 15 of the Periodic Table, a transition element, zinc, or aluminum. n11 is 2 or 3. When n11 is 2 or 3, a plurality of R 11 and R 12 may be the same or different. In general formula (2), R 21 and R 22 Each of Y is independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. 21 M' is an alkylene group having 1 to 10 carbon atoms or an arylene group having 6 to 10 carbon atoms. m21+ is a metal ion having a valence of m21. M' is an element belonging to Group 2 or Group 15 of the Periodic Table, a transition element, zinc, or aluminum. n21 is an integer of 1 to 3. When n21 is 2 or 3, a plurality of R 21 , R 22 and Y 21 may be the same or different. m21 is 2 or 3. x is 1 or 2. When x is 2, multiple M' may be the same or different. n21, x, and m21 are integers that satisfy the relational expression 2×n21=m21×x.

9. The polyamide composition according to any one of claims 1 to 8, wherein the content of the phosphorus-based flame retardant (B) is 0.1 mass% or more and 30 mass% or less with respect to the total mass of the polyamide (A), the phosphorus-based flame retardant (B), and the styrene copolymer (C).

10. The polyamide composition according to any one of claims 1 to 9, wherein the polyamide composition has a tan δ peak temperature of 90°C or higher.

11. The polyamide composition according to any one of claims 1 to 10, wherein the polyamide composition has a weight average molecular weight of 10,000 or more and 50,000 or less.

12. The polyamide composition according to any one of claims 1 to 11, further comprising at least one (D) filler.

13. A molded article obtained by molding the polyamide composition according to any one of claims 1 to 12.

14. A method for producing the polyamide composition according to any one of claims 1 to 12, comprising the steps of: A method for producing a polyamide composition, comprising melt-kneading raw material components containing the polyamide (A), the phosphorus-based flame retardant (B), and the styrene copolymer (C).

15. A method of adding a styrene copolymer as a flame retardant auxiliary to a resin composition containing a polyamide and a phosphorus-based flame retardant.

Citation Information

Patent Citations

  • Preparation method of semi-aromatic polyamide alloy

    CN102796368A

  • Flame-retardant resin composition

    JP2005336473A

  • Flame-retardant polyamide molding compound and its use

    JP2007507566A

  • Polyamide resin composition and molded article comprising the same

    JP2010037372A

  • Flame retardant composition containing a polymer dispersant

    JP2012500877A