Deproteinized crosslinked natural rubber

A rubber composition using protein-removed natural rubber and an organic peroxide crosslinking agent effectively addresses volumetric expansion and physical property deterioration in water, achieving a 4.3% or less volume change rate after 500 hours at 80°C.

JP2024138116AActive Publication Date: 2024-10-07NOK CORP +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024121903
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-07
Estimated Expiration
2039-12-12

AI Technical Summary

Technical Problem

Natural rubber's volumetric expansion and physical property deterioration during immersion in water due to its hydrophilic proteins are not adequately addressed by existing protein-free solutions.

Method used

A rubber composition comprising protein-removed natural rubber and an organic peroxide crosslinking agent, with a crosslinked product exhibiting a volume change rate of 4.3% or less after a water resistance test at 80°C for 500 hours, effectively preventing volumetric expansion and maintaining physical properties.

Benefits of technology

The crosslinked rubber composition significantly reduces volumetric expansion and maintains physical properties when immersed in water, with minimal deterioration.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a deproteinized crosslinked natural rubber that exhibits small volume expansion and little deterioration in physical properties when immersed in water.SOLUTION: A deproteinized crosslinked natural rubber is a crosslinked product of a rubber composition containing deproteinized natural rubber and an organic peroxide crosslinking agent, and has a volume change of 4.3% or less after a water resistance test at 80°C for 500 hours in accordance with JIS K-6258. This deproteinized crosslinked natural rubber is effectively used as a rubber product used in contact with water, such as a seal for a water system.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a deproteinized natural rubber. Crosslinking More specifically, the present invention relates to a method for preventing volume expansion and deterioration of physical properties when immersed in water. Low protein Removed natural rubber Crosslinking Pertaining to things. [Background technology]

[0002] The rubber materials used in wet areas are generally synthetic rubbers such as EPDM, (hydrogenated) NBR, and fluororubber, but from the perspective of resource sustainability, the use of plant-derived natural rubber is desirable.

[0003] However, because natural rubber contains hydrophilic proteins in its structure, there is a problem that its volume increases during use.

[0004] Patent Document 1 proposes protein-free natural rubber obtained by separating proteins from natural rubber, but even in this case such a tendency is still observed. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] WO 2011 / 027739 A1 Summary of the Invention [Problem to be solved by the invention]

[0006] The object of the present invention is to prevent volume expansion and deterioration of physical properties when immersed in water. Low protein Removed natural rubber Crosslinking It is to provide things. [Means for solving the problem]

[0007] The object of the present invention is to provide a rubber composition comprising a deproteinized natural rubber and an organic peroxide crosslinking agent. It is a cross-linked rubber composition, and the volume change rate after a water resistance test at 80°C for 500 hours in accordance with JIS K-6258 is 4.3% or less. Deproteinized natural rubber Crosslinking It is achieved by things. Effect of the Invention

[0008] Deproteinized natural rubber is blended with an organic peroxide crosslinking agent. A cross-linked product of a rubber composition, which has a volume change of 4.3% or less after a water resistance test at 80°C for 500 hours in accordance with JIS K-6258. Deproteinized natural rubber Crosslinking The material effectively prevents volume expansion when immersed in water with almost no deterioration in physical properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Protein-removed natural rubber according to the present invention Crosslinking The article comprises deproteinized natural rubber and an organic peroxide crosslinking agent.

[0010] In the present invention, deproteinized natural rubber is natural rubber having a nitrogen content of 0.01 to 0.01%, as measured by the Kjeldahl method (based on JIS K6451-2, which corresponds to ISO 1407; a sample is wet-decomposed using a mixed catalyst of potassium sulfate and copper (II) sulfate and sulfuric acid, the nitrogen in the sample is converted to ammonium sulfate, a strong alkali is added to the sample, and the liberated ammonia is subjected to steam distillation, introduced into an aqueous boric acid solution, and then titrated with sulfuric acid or hydrochloric acid to determine the amount of ammonia, from which the nitrogen content is calculated). Protein removal of 0.019% by weight or less It refers to natural rubber.

[0011] Such protein-removed natural rubber can be obtained by adding a urea compound, preferably urea represented by the general formula RNHCONH2 (R: hydrogen atom or an alkyl group having 1 to 5 carbon atoms) or a lower alkyl derivative thereof, an anionic, nonionic or cationic surfactant and a polar organic solvent, preferably a water-miscible polar organic solvent such as an aliphatic alcohol having an alkyl group having 1 to 5 carbon atoms, a ketone having 3 to 4 carbon atoms, an aliphatic carboxylic acid having 1 to 5 carbon atoms, or a carboxylate ester having an alkyl group having 1 to 5 carbon atoms, to natural rubber latex, and then denaturing and removing the proteins in the latex.

[0012] In addition, such protein-removed natural rubber has a protein content in the solid rubber of 0.5 μg / g or less as measured by the modified Lowry method.

[0013] Kjeldahl method (JIS K6451-2): 0.1g of rubber, 0.65g of catalyst (potassium sulfate: copper(II) sulfate pentahydrate: selenium = weight ratio 15:2:1), and 2.5ml of concentrated sulfuric acid were weighed and placed in a Kjeldahl flask, and heated with a gas burner for about 30 minutes until the solution turned green. A steam distillation apparatus was assembled, and an appropriate amount of distilled water was placed in a 1L flask, which was then heated in an oil bath, and the 300ml two-neck flask and Liebig condenser were washed with steam. The contents of the Kjeldahl flask were transferred into the two-neck flask using 20ml of distilled water, and 10ml of 67w / v% sodium hydroxide aqueous solution and 10ml of distilled water were added to the two-neck flask, and steam was passed through. Ammonia was captured using an Erlenmeyer flask containing 10ml of 2w / v% boric acid aqueous solution as a receiver. The distillation was stopped when the content of the Erlenmeyer flask in the steam distillation apparatus reached about 20ml. The inside of the Liebig condenser was washed with distilled water, and the washings were poured into an Erlenmeyer flask. The nitrogen content in the rubber sample was determined by titration with 0.005 mol / L sulfuric acid using methyl red as an indicator. The nitrogen content was calculated using the following formula. Nitrogen content (%) = V / 1000(L)×N(molL -1 )×14×2(gmol -1 )×1 / w(g -1 ) x 100 Here, V is the titration amount of 0.005 mol / L sulfuric acid, w is the mass of rubber, and N is the concentration of 0.005 mol / L sulfuric acid used in the titration multiplied by a factor (1.004).

[0014] Examples of organic peroxide crosslinking agents include dicumyl peroxide, di-tert-butyl peroxide, and 2,5-dimethyl-2,5-di(tert-butyl peroxide). Hexine-3Examples of the peroxides that can be used include dialkyl peroxides such as 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and 1,3-bis(tert-butylperoxyisopropyl)benzene, diacyl peroxides such as benzoyl peroxide, and peroxy esters such as 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane and tert-butylperoxyisopropyl carbonate, and preferably dicumyl peroxide.

[0015] These organic peroxide crosslinking agents are used in a ratio of about 0.1 to 10 parts by weight, preferably about 0.2 to 5 parts by weight, per 100 parts by weight of the protein-removed natural rubber.

[0016] Triallyl isocyanurate, triallyl cyanurate along with organic peroxide crosslinkers A polyfunctional unsaturated compound such as trimethylolpropane trimethacrylate may be used in combination in an amount of about 10 parts by weight or less, preferably about 0.2 to 5 parts by weight, per 100 parts by weight of the protein-removed natural rubber.

[0017] Furthermore, a crosslinking aid such as zinc oxide, magnesium oxide, litharge, stearic acid, zinc stearate, etc. may be added in an amount of about 0.1 to 10 parts by weight, preferably about 0.2 to 5 parts by weight, per 100 parts by weight of the protein-removed natural rubber.

[0018] In addition, anti-aging agents such as p-phenylenediamines such as N-isopropyl-N'-phenyl-p-phenylenediamine, N-octyl-N'-phenyl-p-phenylenediamine, N,N'-diallyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, and N,N'-di(1,4-dimethylpentyl)-p-phenylenediamine, and ketone-amine reaction products such as 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, as well as other optional ingredients may be appropriately blended and used.

[0019] Rubber compositionVarious reinforcing agents or fillers can be used in an amount of about 90 parts by weight or less, preferably about 35 to 60 parts by weight, per 100 parts by weight of the protein-removed natural rubber. The proportion of the reinforcing agent or filler improves the breaking strength and modulus of the crosslinked product, but a larger proportion may impair the breaking elongation and compression set properties.

[0020] As the reinforcing agent or filler, generally, various grades of carbon black, preferably FEF carbon black, white filler such as silica produced by dry method or wet method is used. When silica is used, it is preferable to use a silane coupling agent in combination.

[0021] Rubber composition The preparation of the rubber composition is carried out by kneading the protein-removed natural rubber and other compounding ingredients in a sealed kneader or an open roll.

[0022] Rubber composition The crosslinking is carried out by heating in a hot press at about 140 to 200° C. for about 3 to 30 minutes depending on the type of crosslinking agent used.

[0023] Obtained Protein-removed cross-linked natural rubber The rubber composition is effectively used as a rubber product which is used in contact with water, particularly as a sealing material for water systems, for example, a sealing material for water supply systems. EXAMPLES

[0024] The present invention will now be described with reference to examples.

[0025] Reference example To 100 parts by weight of natural rubber latex (product of Malaysia Golden Hope Pvt. Ltd., imported by Toyotsu Chemiplas; rubber concentration 60.2% by weight, ammonia content 0.7% by weight), 1 part by weight of sodium dodecyl sulfate and 0.1 part by weight of urea were added and stirred at room temperature for 90 minutes.

[0026] The latex was then centrifuged at 15°C and 9000 rpm for 30 minutes to separate the upper cream layer. Distilled water was added to the cream layer, and 0.5 parts by weight of sodium dodecyl sulfate and 2.5 parts by weight of acetone were added, followed by stirring for 1 hour.

[0027] This centrifugation and redispersion process (rubber concentration was adjusted to 30% by weight using 1% anionic surfactant-0.025% ethanol aqueous solution) was repeated a total of three times to prepare protein-removed natural rubber latex, which was then dried to obtain protein-removed natural rubber.

[0028] The obtained natural rubber (PFNR) was Subject to the above conditions The measured nitrogen content was 0.001, which is the detection limit. weight %, and the protein amount measured by the modified Lowry method was at a level of 0.5 μg / g or less, which is the detection limit.

[0029] Example 1 PFNR obtained in the reference example 100 parts by weight FEF Carbon Black 50% Dicumyl peroxide 2.5 〃 Crosslinking agent zinc oxide 5 〃 Crosslinking agent stearic acid 1 〃 Anti-aging agent (Kawaguchi Chemical Industry Products Antage RD) 2 Same Of the above components, PFNR was masticated in a closed kneader, and then the compounding components other than dicumyl peroxide were added and kneaded at 120° C. Furthermore, dicumyl peroxide was added and kneaded using an open roll to obtain a protein-removed natural rubber composition.

[0030] The resulting protein-removed natural rubber composition was thermally crosslinked at 170°C for 7 minutes, and crosslinked until the time corresponding to t90 on the vulcanization curve, to obtain a crosslinked sheet having a thickness of 2 mm. The crosslinked sheet was subjected to the following tests. Normal values ​​(hardness, tensile strength, elongation at break): Compliant with JIS K-6253 and K-6251 Water immersion test : JIS K-6258 compliant 80℃ , 500 hours Measure the change in normal value and the volume change rate after immersion in water JIS No. 6 test pieces and 2 x 5 cm test pieces for measuring volume change were cut from the rubber sheet. Each set consisted of three pieces. Then, 100 ml of ion-exchanged water was poured in and the container was covered with aluminum foil. After the test, the test tube was placed in a thermostatic chamber at a specified temperature. The volume was measured by placing the test piece in water. Calculate the weight of the suspended object using Archimedes' principle. The percentage change in volume was calculated.

[0031] Example 2 In Example 1, instead of the PFNR obtained in the Reference Example, the same amount (100 parts by weight) of deproteinized NR (imported by Toyotsu Chemiplas; nitrogen content 0.019% by weight) was used.

[0032] Comparative Example In Example 1, the same amount (100 parts by weight) of natural rubber (imported by Toyotsu Chemiplas; nitrogen content: 0.480% by weight) was used in place of the PFNR obtained in the Reference Example.

[0033] The results obtained in the above examples and comparative examples are shown in the following table. table Measurement items Example 1 Example 2 Comparative Example [Normal value] Hardness (Durometer A) 53 59 61 Tensile strength (MPa) 20.3 23.4 24.5 Elongation at break (%) 340 380 350 [After immersion in water for 500 hours at 80℃] Hardness change rate (%) -6 -14 -10 Tensile strength change rate (%) -10 -16 -32 Elongation change at break (%) +3 -8 -14 Volume change rate (%) +4.1 +4.3 +9.1

[0034] The above results show that when PFNR or deproteinized NR is used instead of natural rubber, the volume change after immersion in water at 80°C for 500 hours is small, and in the case of PFNR in particular, the rates of change in various physical properties are also kept small.

Claims

1. A cross-linked product of a rubber composition comprising protein-removed natural rubber and an organic peroxide cross-linking agent, said cross-linked product having a volume change of 4.3% or less after a water resistance test at 80°C for 500 hours in accordance with JIS K-6258.

2. 2. The cross-linked protein-removed natural rubber according to claim 1, wherein the protein-removed natural rubber has a nitrogen content of 0.019% by weight or less as measured by the Kjeldahl method specified in JIS K-6451, which corresponds to ISO 1407.

3. The protein-removed natural rubber cross-linked product according to claim 1, wherein the rubber composition further comprises a reinforcing agent or a filler.

4. The cross-linked product of protein-removed natural rubber according to claim 3, wherein the reinforcing agent or filler is blended in an amount of 90 parts by weight or less per 100 parts by weight of the protein-removed natural rubber.

5. The cross-linked product of protein-removed natural rubber according to claim 3, wherein the reinforcing agent or filler is blended in a ratio of 35 to 60 parts by weight per 100 parts by weight of the protein-removed natural rubber.

6. The protein-removed natural rubber cross-linked product according to claim 1, which is a rubber product used in contact with water.

7. The protein-removed natural rubber cross-linked product according to claim 6, which is used as a seal for an aqueous system.

Citation Information

Patent Citations

  • Sealant for preventing corrosion of aperture of stainless steel

    JP1982055981A

  • Rubber composition

    JP1984100148A

  • Deproteinized natural rubber

    JP1994056902A

  • Method for removing allergen from natural rubber latex and production of molded natural rubber article

    JP1994256404A

  • Rubber composition

    JP1994329838A