Antivirus processing method of resin member
The method of roughening a metal surface with a micro-etching agent and transferring the texture to resin members addresses the insufficiency of blasting, resulting in resin members with superior antiviral and antibacterial properties.
Patent Information
- Application Number
- JP2023040766
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-15
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-03-15
AI Technical Summary
Existing antiviral surface treatment methods, such as the blasting process, fail to impart sufficient antiviral properties to resin members, particularly stainless steel plates, exhibiting low antiviral activity values.
A method involving a roughening treatment of a metal member with a micro-etching agent to form a complex roughened shape, followed by transferring this shape to a resin member, using agents like organic, inorganic, or alkaline-based micro-etching agents, and thermoplastic, thermosetting, or UV curable resins.
The method achieves resin members with significantly enhanced antiviral properties, demonstrated by high antiviral activity values, and also imparts antibacterial properties due to the complex surface texture.
Smart Images

Figure 2024138211000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an antiviral treatment method for a resin member. [Background technology]
[0002] In recent years, there has been a particular demand for providing antiviral properties to surfaces that people touch with their hands in order to prevent infection with COVID-19, the so-called novel coronavirus disease.
[0003] The following Patent Document 1 describes an anti-viral surface treatment method in which a projection process (hereinafter also referred to as a "blast process") is performed in which shot material is projected onto the surface of a component, thereby randomly forming countless minute projections and recesses having a specific projection pitch width and recess depth width, thereby imparting anti-viral properties to the surface of the component. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-28394 A Summary of the Invention [Problem to be solved by the invention]
[0005] One of the evaluation criteria for antiviral properties is the "antiviral activity value," and in the technology described in Patent Document 1, the comparative object (stainless steel plate material) does not exhibit antiviral properties, but when subjected to an antiviral surface treatment method, the antiviral activity value is 0.4 to 0.7 after 24 hours at 25° C. However, as a result of studies by the present inventors, it was found that the antiviral properties obtained by the technology described in Patent Document 1 are insufficient and that further improvement of antiviral properties is necessary, since the blast treatment involves a projection treatment in which shot material is projected onto the surface of the component, and therefore only a convex shape can be imparted toward the back surface of the component.
[0006] In view of the above, an object of the present invention is to provide an antiviral treatment method for a resin member that can impart excellent antiviral properties to the resin member. [Means for solving the problem]
[0007] The above problems can be solved by the following configuration: The present invention relates to an antiviral treatment method (1) for a resin member, comprising a roughening treatment step of contacting a surface of a metal member with a microetching agent to form a roughened shape on the surface of the metal member, and a transfer step of transferring the roughened shape formed on the surface of the metal member to a surface of a resin member, thereby imparting antiviral properties to the surface of the resin member.
[0008] In the above-mentioned antiviral treatment method for a resin member (1), it is preferable that the roughening treatment process includes three steps, namely, a pretreatment step, a main treatment step, and a post-treatment step, as the antiviral treatment method for a resin member (2).
[0009] In the above-mentioned antiviral treatment method for a resin member (1) or (2), the antiviral treatment method for a resin member (3) is preferred, in which the microetching agent is at least one type of microetching agent selected from the group consisting of organic acid-based microetching agents, inorganic acid-based microetching agents, alkaline microetching agents, and hydrogen peroxide-based microetching agents.
[0010] In any one of the above antiviral treatment methods for a resin member (1) to (3), the antiviral treatment method for a resin member (4) is preferred, in which the resin member is made of a thermoplastic resin, a thermosetting resin or a UV-curable resin. Effect of the Invention
[0011] According to the method for antiviral treatment of a resin member according to the present invention, it is possible to provide a resin member that exhibits excellent antiviral properties, specifically, a high antiviral activity value. Although the reason why the method can impart superior antiviral properties to the resin member compared to blast treatment is not clear, the following reasons can be assumed.
[0012] Since the projection process involves projecting shot material onto the surface of the member, the blast process can only form a convex shape toward the back surface of the member. On the other hand, in the antiviral treatment method for a resin member according to the present invention, in the roughening process step, a microetching agent is brought into contact with the surface of the metal member to roughen the surface of the metal member, thereby forming a roughened shape on the surface of the metal member. Therefore, as shown in the experimental results described below, a much more complex shape can be formed on the surface of the metal member compared to the roughened surface formed by the blast process. Then, in the transfer process, the complex shape (roughened shape) formed on the surface of the metal member is accurately transferred to the surface of the resin member, so that a complex shape equivalent to that of the metal member can be formed on the surface of the resin member. It should be noted that the present inventors have first found that the antiviral properties obtained by the complex shape (roughened shape) formed on the surface of the resin member by the roughening process and transfer process of the present invention is significantly superior to the antiviral properties that can be imparted to a metal surface by other treatment methods, particularly blast treatment.
[0013] The complex shape (roughened shape) formed on the surface of the metal member exhibits not only antiviral properties but also antibacterial properties. The antiviral treatment method for a resin member according to the present invention can accurately transfer the complex shape (roughened shape) formed on the surface of the metal member to the surface of the resin member, thereby forming a complex shape on the surface of the resin member equivalent to that of the metal member, and can therefore impart not only antiviral properties but also antibacterial properties to the resin member. [Brief description of the drawings]
[0014] [Figure 1] Scanning electron microscope photograph of (untreated) copper plate surface (magnification 1500x). [Diagram 2] Scanning electron microscope photograph of (untreated) copper plate surface (magnification 5000x). [Diagram 3] 1 is a scanning electron microscope photograph (magnification: 1,500 times) of the copper plate surface used in Example 1 (roughening treatment 1). [Figure 4] 1 is a scanning electron microscope photograph (magnification: 5000 times) of the copper plate surface used in Example 1 (roughening treatment 1). [Diagram 5] 1 is a scanning electron microscope photograph (magnification: 1,500 times) of the copper plate surface (roughening treatment 2) used in Example 2. [Figure 6] 1 is a scanning electron microscope photograph (magnification: 5000 times) of the copper plate surface (roughening treatment 2) used in Example 2. [Figure 7] 1 is a scanning electron microscope photograph (magnification: 1,500 times) of the surface of the (untreated) PP plate of Comparative Example 1. [Figure 8] 1 is a scanning electron microscope photograph (magnification: 5000 times) of the surface of the (untreated) PP plate of Comparative Example 1. [Figure 9] 1 is a scanning electron microscope photograph (magnification: 1,500 times) of the surface of the resin member ((transfer treatment 1) PP plate) produced in Example 1. [Figure 10] 1 is a scanning electron microscope photograph (magnification: 5,000 times) of the surface of a resin member ((transfer treatment 1) PP plate) produced in Example 1. [Figure 11] 1 is a scanning electron microscope photograph (magnification: 1,500 times) of the surface of a resin member ((transfer treatment 2) PP plate) produced in Example 2. [Figure 12] 1 is a scanning electron microscope photograph (magnification: 5,000 times) of the surface of the resin member ((transfer treatment 2) PP plate) produced in Example 2. [Figure 13] Scanning electron microscope photograph (magnification 1500x) of the surface of an untreated stainless steel component that has not been roughened. [Figure 14] Scanning electron microscope photograph (magnification 5000x) of the surface of an untreated stainless steel component that has not been roughened. [Figure 15] Scanning electron microscope photograph (magnification 1500x) of the surface of an untreated stainless steel component after blasting. [Figure 16] Scanning electron microscope photograph (magnification 5000x) of the surface of an untreated stainless steel component after blasting. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The antiviral treatment method for a resin member according to the present invention includes a roughening treatment step of contacting a surface of a metal member with a microetching agent to form a roughened shape on the surface of the metal member, and a transfer step of imparting antiviral properties to the surface of the resin member by transferring the roughened shape formed on the surface of the metal member to the surface of the resin member. First, the roughening treatment step will be described below.
[0016] <Roughening treatment process> In the roughening treatment step, a micro-etching agent is brought into contact with the surface of a metal member to form a roughened shape on the surface of the metal member. Examples of metal members that can be used in the present invention include aluminum, aluminum alloys, copper, copper alloys, nickel, nickel alloys, stainless steel, titanium, titanium alloys, iron or iron alloys. Among these, it is preferable to use aluminum, aluminum alloys, copper or copper alloys as the metal member in the present invention, and it is more preferable to use copper. The shape and size of the metal member can be designed as appropriate. In addition, in the blast treatment, since shot material is projected onto the surface of the member, it is preferable that the treated surface (surface) of the metal member to which antiviral properties are imparted is a flat surface. On the other hand, in the present invention, since a micro-etching agent is brought into contact with the surface of the metal member to roughen the surface of the metal member, the treated surface of the metal member is not limited to a flat surface, and antiviral properties can be imparted to a surface of any shape.
[0017] As the microetching agent used in the roughening treatment step, for example, an organic acid microetching agent, an inorganic acid microetching agent, an alkali microetching agent, or a hydrogen peroxide microetching agent can be used.
[0018] Examples of organic acid-based microetching agents include microetching agents made of an aqueous solution containing an organic acid, a metal ion source, a halide ion source, and the like.
[0019] Examples of inorganic acid microetching agents include microetching agents made of an acidic aqueous solution containing an inorganic acid, a metal ion source, a halide ion source, and the like.
[0020] Examples of alkaline microetching agents include microetching agents made of an aqueous solution containing an alkali source, an amphoteric metal ion source, nitrate ions, a thio compound, and the like.
[0021] Examples of hydrogen peroxide-based microetchants include microetchants made of an aqueous solution containing hydrogen peroxide and sulfuric acid as main components.
[0022] The roughening treatment process for the metal member of the present invention may be carried out in one step, but in order to form a more complicated shape (roughened shape) on the surface of the metal member to be manufactured, it is preferable to carry out the process in two steps, and it is particularly preferable to carry out the process in three steps, including a pretreatment step, a main treatment step, and a post-treatment step. An embodiment in which the roughening treatment process is carried out in three steps will be described below.
[0023] The pretreatment step may be, for example, a step of immersing at least the surface to be treated of the metal member in an alkaline soft etching agent such as a hydrogen peroxide-based soft etching agent consisting of an aqueous solution mainly composed of dilute nitric acid, hydrogen peroxide, and sulfuric acid, or an aqueous solution containing the above-mentioned alkali source, an amphoteric metal ion source, nitrate ions, a thio compound, etc. The treatment temperature may be, for example, 15 to 40°C, and the treatment time may be, for example, about 3 seconds to 10 minutes.
[0024] In this treatment step, at least the treatment surface of the metal member is immersed in the above-mentioned organic acid microetchant, inorganic acid microetchant, alkaline microetchant, hydrogen peroxide microetchant, etc. The treatment temperature is, for example, 10 to 40°C, and the treatment time is, for example, about 5 seconds to 10 minutes.
[0025] The post-treatment step may be, for example, a step of immersing at least the treatment surface of the metal member in dilute nitric acid, etc. The treatment temperature may be, for example, 15 to 40° C., and the treatment time may be, for example, about 3 to 40 seconds.
[0026] After the roughening treatment step, a complex roughened shape is formed on the surface of the metal member. Specific examples of the complex roughened shape formed on the surface of the metal member after the roughening treatment step will be described later.
[0027] <Transfer process> Next, the transfer process will be described. In the transfer process, the roughened shape formed on the surface of the metal member is transferred to the surface of the resin member, thereby imparting antiviral properties to the surface of the resin member. In the present invention, examples of resin members that can be antivirally treated include thermoplastic resins, thermosetting resins, and UV-curable resins. Examples of thermoplastic resins include general-purpose plastics such as polypropylene, polyacrylic resins, and ABS resins; engineering plastics such as nylon 6, nylon 66, polyacetal, polycarbonate, polybutylene terephthalate, and modified polyphenylene ether; and super engineering plastics such as polyphenylene ether, liquid crystal polymer, and polyetherimide. Examples of thermosetting resins include phenolic resins, urea resins, melamine resins, epoxy resins, unsaturated polyester resins, polyurethane resins, diallyl phthalate resins, silicone resins, and alkyd resins. Examples of UV-curable resins include acrylic resins and epoxy resins.
[0028] A method for transferring the roughened shape formed on the surface of a metal member to the surface of a thermoplastic resin includes, for example, overlapping the roughened surface of the metal member with the surface of the resin member to be subjected to antiviral treatment, and heat pressing using a press. On the other hand, a method for transferring the roughened shape formed on the surface of a metal member to the surface of a thermosetting resin or UV curable resin includes, for example, forming a mold including at least the roughened surface of the metal member on which the roughened shape is formed, pouring the raw material components of the thermosetting resin or UV curable resin into it, curing it, and then demolding the resin member, thereby transferring the roughened shape formed on the surface of the metal member to the surface of the thermosetting resin or UV curable resin.
[0029] After the transfer step, a complex roughened shape is formed on the surface of the resin member. Specific examples of the complex roughened shape formed on the surface of the resin member after the transfer step will be described later.
[0030] By the antiviral treatment method for a resin part according to the present invention, a resin part with excellent antiviral properties can be produced. The antiviral activity value, which indicates the level of antiviral properties, can be calculated by the following formula with reference to JIS R1756:2020 (visible light responsive photocatalyst, antiviral, film adhesion method). V D =Log(B D )-Log(C D ) (1) In the above formula (1), V D indicates antiviral activity value, D indicates dark place, B indicates infectivity value of unprocessed product, and C indicates infectivity value of processed product.
[0031] As described above, the antiviral treatment method for a resin member according to the present invention can produce a resin member having excellent antiviral properties. Therefore, the antiviral treatment method for a resin member according to the present invention is particularly useful as a treatment method for imparting antiviral properties to resin members used in home appliances, housing building materials / equipment, toilet-related facilities / supplies, kitchen-related facilities / supplies, bathroom-related facilities / supplies, office equipment / office supplies, printing (printed matter, laminated products and paper), transport equipment, industrial equipment / industrial supplies (films, packaging materials / films for food, etc., packaging materials, etc.), medical / nursing / health, communication-related / accessories, pet supplies, daily necessities (shoes, cleaning supplies, cosmetics, etc.), etc.
[0032] The antiviral treatment method for a resin member according to the present invention can accurately transfer a complex shape (roughened shape) formed on the surface of a metal member to the surface of the resin member, thereby forming a complex shape on the surface of the resin member equivalent to that of the surface of the metal member, and can impart not only antiviral properties but also antibacterial properties to the resin member. Therefore, it is also useful as a treatment method for imparting antibacterial properties to a resin member used in the above-mentioned applications. EXAMPLES
[0033] An example of an embodiment of the present invention will be described below, but the present invention is not limited to this description in any way.
[0034] Ref.(-) (glass plate) was prepared as an "unprocessed product". Next, an unused copper plate (100 mm x 100 mm x t1.3 mm) was prepared as an untreated copper member that had not been subjected to a roughening treatment. A scanning electron microscope photograph (magnification 1500 times) of the surface of this (untreated) copper member is shown in Figure 1, and a scanning electron microscope photograph (magnification 5000 times) is shown in Figure 2. Referring to Figures 1 and 2, and especially the photograph in Figure 2, it can be seen that the surface of the (untreated) copper member is completely free of irregularities and is close to a mirror surface.
[0035] An (untreated and unused) polypropylene (PP) plate (50 mm × 50 mm × t≦1 mm) with no roughened surface was prepared. A scanning electron microscope photograph (magnification 1500 times) of the surface of this (untreated) PP plate is shown in FIG. 7, and a scanning electron microscope photograph (magnification 5000 times) is shown in FIG. 8. Referring to FIGS. 7 and 8, and especially the photograph in FIG. 8, it can be seen that the surface of the (untreated) PP plate is completely free of irregularities and is close to a mirror surface. The (untreated) PP plate is designated as Comparative Example 1.
[0036] Example 1 An unused copper plate (100 mm × 100 mm × t1.3 mm) was subjected to a roughening treatment process (three steps: a pretreatment step, a main treatment step, and a post-treatment step) under the following conditions (hereinafter, the roughening treatment process in Example 1 will be referred to as "roughening treatment 1"). The conditions for each step are shown below. (Pre-processing step) The surface of the copper plate to be treated is sprayed with a sulfuric acid / peroxide-based soft etching agent. Treatment temperature: 25°C. Treatment time: 20 seconds. (Main processing step) Following the pretreatment, the surface of the copper plate to be treated is sprayed with an organic acid-based micro-etching agent (a micro-etching agent consisting of an aqueous solution containing an organic acid, a metal ion source, a halide ion source, etc.). Treatment temperature: 30°C. Treatment time: 50 seconds. (Post-processing step) Following this treatment, the surface of the copper plate to be treated is sprayed with dilute hydrochloric acid. Treatment temperature: 25°C. Treatment time: 15 seconds.
[0037] A scanning electron microscope photograph (magnification 1500x) of the surface of the copper plate (referred to as "(roughening treatment 1) copper plate") obtained after the roughening treatment step (roughening treatment 1) of Example 1 is shown in FIG. 3, and a scanning electron microscope photograph (magnification 5000x) is shown in FIG. 4. From the photograph in FIG. 3, it can be seen that a complex roughened shape is formed over the entire surface of the copper plate by the roughening treatment step 1. With particular reference to the photograph in FIG. 4, it can be seen that convex shapes are formed in arbitrary directions on the surface of the copper plate.
[0038] For reference, a scanning electron microscope photograph (magnification 1500x) of the surface of an untreated stainless steel member that has not been roughened is shown in FIG. 13, a scanning electron microscope photograph (magnification 5000x) is shown in FIG. 14, a scanning electron microscope photograph (magnification 1500x) of the surface of the untreated stainless steel member after blasting is shown in FIG. 15, and a scanning electron microscope photograph (magnification 5000x) is shown in FIG. 16. As is clear from comparing FIG. 13 with FIG. 15 and FIG. 14 with FIG. 16, it can be seen that the blasting process can only form a convex shape toward the back surface of the member, and therefore a complex roughened shape cannot be formed on the stainless steel surface. On the other hand, referring to FIG. 3 and FIG. 4, especially the photograph in FIG. 4, it can be seen that a much more complex roughened shape is formed on the surface of the copper plate (roughened treatment 1) compared to the stainless steel surface that has been blasted.
[0039] Next, the roughened surface of the copper plate (roughening treatment 1) was overlapped with the surface of the (untreated) PP plate to be subjected to antiviral treatment, and the surface was hot-pressed using a press machine to transfer the roughened surface formed on the surface of the copper plate (roughening treatment 1) to the surface of the (untreated) PP plate (transfer process). Hereinafter, the transfer process in Example 1 is referred to as "transfer process 1." Table 1 shows the hot-press conditions.
[0040] [Table 1]
[0041] FIG. 9 shows a scanning electron microscope photograph (magnification 1500 times) of the surface of the PP plate (referred to as "(transfer treatment 1) PP plate") obtained after the transfer step (transfer treatment 1) of Example 1, and FIG. 10 shows a scanning electron microscope photograph (magnification 5000 times). From the photograph in FIG. 9, it can be seen that a complex roughened shape is formed on the entire surface of the PP plate by the transfer treatment 1. With particular reference to the photograph in FIG. 10, it can be seen that a convex shape is formed in any direction on the surface of the PP plate. In other words, it can be seen that a much more complex roughened shape is formed on the surface of the PP plate compared to the blast treatment, which can only form a convex shape toward the back surface of the member.
[0042] Example 2 An unused copper plate (100 mm × 100 mm × t1.3 mm) was subjected to a roughening treatment process (three steps: pretreatment step, main treatment step, and post-treatment step) under the following conditions (hereinafter, the roughening treatment process in Example 2 is referred to as "roughening treatment 2"). The conditions for each step are shown below. (Pre-processing step) The surface of the copper plate to be treated is sprayed with a sulfuric acid / peroxide-based soft etching agent. Treatment temperature: 25°C. Treatment time: 20 seconds. (Main processing step) Following the pretreatment, the surface of the copper plate to be treated is sprayed with an organic acid-based micro-etching agent (a micro-etching agent consisting of an aqueous solution containing an organic acid, a metal ion source, a halide ion source, etc.). Treatment temperature: 30°C. Treatment time: 150 seconds. (Post-processing step) Following this treatment, the surface of the copper plate to be treated is sprayed with dilute hydrochloric acid. Treatment temperature: 25°C. Treatment time: 15 seconds.
[0043] A scanning electron microscope photograph (magnification 1500x) of the surface of the copper plate (referred to as "(roughening treatment 2) copper plate") obtained after the roughening treatment step (roughening treatment 2) of Example 2 is shown in FIG. 5, and a scanning electron microscope photograph (magnification 5000x) is shown in FIG. 6. From the photograph in FIG. 5, it can be seen that a complex roughened shape is formed on the entire surface of the copper plate by the roughening treatment step 2. With particular reference to the photograph in FIG. 6, it can be seen that a convex shape is formed in any direction on the surface of the copper plate. In other words, it can be seen that a much more complex roughened shape is formed on the surface of the copper plate compared to blast treatment, which can only form a convex shape toward the back surface of the member.
[0044] Next, the roughened surface of the (roughening treatment 2) copper plate and the surface of the (untreated) PP plate to be subjected to the antiviral treatment were overlapped and hot-pressed using a press machine to transfer the roughened surface formed on the surface of the (roughening treatment 2) copper plate to the surface of the (untreated) PP plate (transfer process). Note that the transfer process was carried out under the same hot-press conditions except that a (roughening treatment 2) copper plate was used instead of the (roughening treatment 1) copper plate. The transfer process in Example 2 is referred to as "transfer process 2").
[0045] FIG. 11 shows a scanning electron microscope photograph (magnification 1500 times) of the surface of the PP plate (referred to as "(transfer treatment 2) PP plate") obtained after the transfer step (transfer treatment 2) of Example 2, and FIG. 12 shows a scanning electron microscope photograph (magnification 5000 times). From the photograph in FIG. 11, it can be seen that a complex roughened shape is formed on the entire surface of the PP plate by transfer treatment 2. With particular reference to the photograph in FIG. 12, it can be seen that a convex shape is formed in any direction on the surface of the PP plate. In other words, it can be seen that a much more complex roughened shape is formed on the surface of the PP plate compared to blast treatment, which can only form a convex shape toward the back surface of the member.
[0046] [Antiviral evaluation] Using Ref.(-) (glass plate) as an unprocessed product, the antiviral properties of the (untreated) PP plate of Comparative Example 1 and the PP plates subjected to the antiviral treatment methods for resin members of Examples 1 and 2 ((Transfer Treatment 1) PP Plate and (Transfer Treatment 2) PP Plate) were evaluated under the following conditions. [Test Standards] Refer to JIS R1756:2020 (visible light responsive photocatalyst, anti-virus, film adhesion method) [Unprocessed product name] Ref.(-)(Glass plate) [Test item name] (Untreated) PP plate (Comparative Example 1), (Transfer treatment 1) PP plate (Example 1), (Transfer treatment 2) PP plate (Example 2) [Size of test sample (PP board)] 50mm×50mm×t≦1mm [n number] n=1 [Test phage] bacteriophage Qβ (NBRC 20012) [host E. coli (NBRC 106373)]; the results are shown in Table 2. Bacteriophage φ6 (NBRC 105899, not JIS standard) [host Pseudomonas syringae (NBRC 14084)]; the results are shown in Table 3. [Dilution of test phage] 1 / 500NB [Sterilization of test samples] Sterilization with UV254nm (15 minutes on each side) [Conditions for operation] Temperature 25℃, dark place, action time 0 hours, 8 hours [Adhesive film] Polypropylene film (VF-10, KOKUYO), 40mm x 40mm
[0047] [Table 2]
[0048] As shown in Table 2, the (Transfer Treatment 1) PP plate and (Transfer Treatment 2) PP plate obtained in Example 1 and Example 2 showed a significant decrease in infectivity titer after 8 hours in a dark place at 25°C. Similarly, the antiviral activity value increased to 4.9 or 5.3 after 8 hours in a dark place at 25°C. From these results, it can be seen that the resin members produced by the antiviral treatment methods for resin members in Examples 1 and 2 have a remarkable effect on antiviral properties due to the formation of a very complex roughened shape on the surface of the resin member.
[0049] [Table 2]
[0050] As shown in Table 3, the infectivity titer of the (transfer treatment 1) PP plate and the (transfer treatment 2) PP plate obtained in Example 1 and Example 2 significantly decreased after 8 hours in a dark place at 25°C. Similarly, the antiviral activity value increased to 3.4 or 4.9 after 8 hours in a dark place at 25°C. From these results, it can be understood that the resin members produced by the antiviral treatment methods for resin members in Examples 1 and 2 have a significant effect on antiviral properties regardless of the test phage, that is, regardless of the norovirus, influenza virus, or even coronavirus, due to the formation of a very complex roughened shape on the surface of the resin member.
Claims
1. a roughening treatment step of contacting a surface of a metal member with a microetching agent to form a roughened shape on the surface of the metal member; and a transfer step of transferring the roughened shape formed on the surface of the metal member to a surface of a resin member, thereby imparting antiviral properties to the surface of the resin member.
2. 2. The anti-viral treatment method for a resin member according to claim 1, wherein the roughening treatment step comprises three steps: a pretreatment step, a main treatment step, and a post-treatment step.
3. 2. The anti-viral treatment method for a resin member according to claim 1, wherein the microetching agent is at least one type of microetching agent selected from the group consisting of organic acid-based microetching agents, inorganic acid-based microetching agents, alkali-based microetching agents, and hydrogen peroxide-based microetching agents.
4. 2. The antiviral treatment method for a resin member according to claim 1, wherein the resin member is made of a thermoplastic resin, a thermosetting resin or a UV-curable resin.
Citation Information
Patent Citations
Synthetic polymer film with surface having bactericidal action
JP2016153510A
Fine rugged structure, and production method of fine convex structure and fine concave structure
JP2018030334A
Mold propagation suppressing member
JP2020033700A
Production method and mold for antibacterial member
JP2023060950A
Non-conductive antibacterial sheet, process for manufacturing same and method for inhibiting the growth of bacteria
WO2015072364A1