Porous polymeric membrane and related filters and methods

A single-step formed monolithic porous polymer membrane with non-uniform pore structure addresses the inefficiencies of layered membranes by reducing costs and enhancing capture performance in industrial filtration, particularly in semiconductor manufacturing.

JP2024138238AInactive Publication Date: 2024-10-08ENTEGRIS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024090489
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-10-10
Filing Date
2024-06-04
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing filtration membranes for industrial applications, particularly in microelectronic and semiconductor manufacturing, face challenges in achieving efficient and cost-effective manufacturing while maintaining high performance in terms of retention and capture of particles, with layered membrane techniques doubling material costs.

Method used

A single monolithic porous polymer membrane is produced in a single forming step, featuring two tight regions and an open region, by extruding a polymer solution and simultaneously exposing both sides to coagulation conditions, such as non-solvent induced phase separation or thermally induced phase separation, to create a non-uniform pore structure.

Benefits of technology

The monolithic membrane achieves improved capture performance with reduced material costs, exhibiting high retention and flow rates, and is suitable for industrial filtration applications, including semiconductor manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138238000001_ABST
    Figure 2024138238000001_ABST
Patent Text Reader

Abstract

To provide a porous polymeric membrane capable of being produced in an efficient and cost-effective, e.g., profitable, manner, and filters comprising the membrane.SOLUTION: An integral extruded porous polymeric sheet membrane comprises a first surface, a second surface, and a thickness between the first surface and the second surface, a first thickness region that includes the first surface and a portion of the membrane in a direction of the thickness, a second thickness region that includes the second surface and a portion of the membrane in the direction of the thickness, and a third thickness region extending in the direction of the thickness between the first thickness region and the second thickness region, where an average pore size of the first thickness region and an average pore size of the second thickness region are both less than an average pore size of the third thickness region.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The following description relates to a porous polymer filtration membrane having two opposing faces and a pore structure that varies across the thickness of the membrane; as well as filter elements and filters that include this type of porous polymer filtration membrane; methods of making the porous polymer filtration membranes, filter elements, and filters; and methods of using the porous polymer filtration membranes, filter elements, or filters to filter fluids, such as liquid chemicals, and remove unwanted substances from the fluids. [Background technology]

[0002] The primary application of filtration membranes is the removal of unwanted materials from useful fluid streams. Many gaseous and liquid fluids in industry are treated using filters, including environmental air, drinking water, liquid industrial solvents and process fluids, industrial gases used in manufacturing or processing (e.g., semiconductor manufacturing), and liquids for medical or pharmaceutical applications. Unwanted materials removed from the fluids include impurities and contaminants such as particles, microorganisms, dissolved chemical species, etc. Specific examples of impurity removal applications of filtration membranes include the removal of particles or bacteria from therapeutic fluids in the pharmaceutical industry, the treatment of ultrapure water and organic solvent solutions for use in microelectronics and semiconductor processing, and the use of filtration membranes in air and water purification processes.

[0003] To perform the filtration function, the filter product comprises a filtration membrane, which serves to remove unwanted materials from the fluid. The filtration membrane may be in the form of a flat sheet, which may be wound (e.g., spirally), pleated, etc., as desired. Alternatively, the filtration membrane may be in the form of hollow fibers. The filtration membrane may be contained within a housing with an inlet and an outlet, such that the fluid being filtered enters through the inlet and passes through the filtration membrane before passing through the outlet.

[0004] Filtration membranes can be constructed of porous polymeric films with an average pore size that can be selected based on the expected use of the filter, i.e., the type of filtration to be performed using the filter. Typical pore sizes are in the micron or submicron range, e.g., from about 0.001 micron to about 10 microns. Membranes with an average pore size of about 0.001 to about 0.05 microns are sometimes classified as ultrafiltration membranes. Membranes with pore sizes of 0.05 to 10 microns are sometimes classified as microporous membranes.

[0005] Commercial filtration membranes should be of a type that can be efficiently manufactured and assembled into filter products. The membranes need to be efficiently manufactured and have mechanical properties such as strength and flexibility that enable them to withstand assembly into filter cartridges or filter configurations. In addition to the mechanical properties, the membranes should have the appropriate chemical functionality and microstructure for high performance filtration.

[0006] Various techniques are known for forming porous filtration membranes. Exemplary techniques include, among others, melt extrusion (e.g., melt casting) and dip casting (phase inversion) techniques. Different techniques for forming porous materials can produce different porous membrane structures in terms of the pore size and distribution formed in the membrane. That is, different techniques produce different pore sizes and membrane structures (sometimes called morphology, which refers to the uniformity, shape and distribution of pores in the membrane).

[0007] Examples of membrane morphologies include uniform (isotropic) and asymmetric (anisotropic). Membranes with substantially uniformly sized pores distributed evenly throughout the membrane are often referred to as isotropic or "uniform". Anisotropic (also known as "asymmetric") membranes can be considered to have a morphology in which a pore size gradient exists throughout the membrane. For example, a membrane may have a porous structure with relatively large pores on one membrane surface and relatively small pores on the other membrane surface, with the pore structure varying along the thickness of the membrane. The term "asymmetric" is often used interchangeably with the term "anisotropic". The portions of the membrane that have relatively small pores (compared to other regions of the membrane) are often referred to as "tight" regions. The portions of the membrane that have larger pores are often referred to as "open" regions.

[0008] Industries that use filters, including the semiconductor material and microelectronic device fabrication and processing industries, are continually interested in discovering improved filtration membranes and filters, including new filter products with improved performance, such as improved capture performance. New filters should be capable of being manufactured in an efficient and cost-effective, e.g., profitable, manner. Summary of the Invention

[0009] The microelectronic device processing field (e.g., microelectronics and semiconductor device manufacturing) requires steady improvements in processing materials and methods to maintain a corresponding steady improvement in the performance (e.g., speed and reliability) of microelectronic devices. Opportunities for improving the manufacturing of microelectronic devices exist in all aspects of the manufacturing process, including methods and systems for filtering liquid materials used during manufacturing.

[0010] Two important aspects of commercial filtration membrane manufacturing are efficient, cost-effective production and high performance in terms of retention capacity, which refers to the amount of particles a filtration membrane can remove from a fluid stream.

[0011] An effective technique for improving capture performance is to use multiple membranes in series, such as stacking the filtration faces of two membranes together in contact and passing fluid through both membranes in series. This is sometimes called "layering" or "stacking" the filtration membranes to form a multi-layer membrane. When the layering technique is performed using asymmetric membranes, each of which has "tight" and "open" regions, fluid passing through the two membranes must pass through both "tight" regions, which may improve the capture performance of the membranes.

[0012] Although layering techniques are feasible and sometimes effective, the use of two layered membranes doubles the material cost of the membrane. It is therefore interesting to reproduce the structure of two membranes, i.e. two-layer laminated membranes, in a single integral membrane made by a single membrane forming process, i.e. to use a single manufacturing process to produce a single integral membrane with two tight layers, e.g. a "double tight" membrane. The two tight layers of the membrane are preferably not prepared using separate processes and then combined. For example, the membrane is not made by combining two separate membranes into a multilayer membrane.

[0013] The present disclosure thus relates to a membrane integrally formed in a single forming step to have two tight regions and at least one open region, a method for preparing the membrane, and a method for using the membrane as a filtration membrane and filter product incorporating the membrane. Such porous membranes can be prepared by a novel and inventive method of extruding a polymer solution through a die in the form of a polymer solution film, followed by subjecting opposing sides of the film to conditions that solidify the polymer in the film on both sides of the film, in particular conditions that produce a tight morphology on both sides of the solidified film.

[0014] As an example of a method useful for preparing the described membranes having the described morphology, the membranes may be formed by forming an extruded liquid film of a liquid polymer solution containing a non-coagulated or partially coagulated polymer dissolved or suspended in a solvent, and coagulating the polymer within the film by simultaneously exposing two opposing surfaces of the film to conditions (e.g., temperature, non-solvent, humidity, evaporation) that cause the dissolved polymer to coagulate on both sides of the film for substantially the same time and in the same manner. In one example, the technique for inducing coagulation is by a non-solvent induced phase separation (NIPS) technique. In another example, the polymer coagulation may be caused by thermally induced phase separation (TIPS). In another example, the polymer coagulation may be caused by exposing the extruded film to humidity. In another example, the polymer coagulation may be caused by solvent evaporation from the extruded film.

[0015] In one embodiment, an extruded porous polymer sheet membrane comprises a first surface, a second surface, and a thickness between the first surface and the second surface, a first thickness region including the first surface and a portion of the membrane through the thickness, a second thickness region including the second surface and a portion of the membrane through the thickness, and a third thickness region extending through the thickness between the first thickness region and the second thickness region. The average pore size of the first thickness region and the average pore size of the second thickness region are both smaller than the average pore size of the third region.

[0016] In another aspect, a method of making an extruded porous polymer sheet membrane having first and second opposed surfaces, a thickness between the opposed surfaces, and pores having a non-uniform pore size includes forming a polymer-containing liquid comprising a polymer in a solvent; passing the polymer-containing liquid through an extrusion die to form an extruded film of the polymer-containing liquid; and exposing both sides of the extruded film to conditions that cause solidification of the polymer on both sides of the film. [Brief description of the drawings]

[0017] [Figure 1A] 1 is a cross-sectional photograph of a membrane as used herein. [Figure 1B] 1 is a cross-sectional photograph of a membrane as used herein. [Figure 2A-B] 1 is a diagram (schematic and not necessarily to scale) illustrating example methods and systems herein. [Figure 3A-B] 1 is a diagram (schematic and not necessarily to scale) illustrating example methods and systems herein. [Figure 4] FIG. 1 illustrates performance data for exemplary filtration membranes herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The following description relates to extruded porous polymeric membranes that may be effective as filtration membranes, filter products that include the filtration membranes, and related methods of preparing and using the porous membranes.

[0019] A porous polymer membrane has two opposing surfaces (or opposing "faces") and a thickness between the two opposing surfaces. The pores of the porous membrane are arranged throughout the thickness of the membrane to allow fluid to flow from one side of the membrane through the thickness of the membrane to the opposite side of the membrane and through the opposite side while removing particles or contaminants from the fluid. Thus, the membrane is permeable to fluids, such as liquids. This type of membrane is sometimes called an "open pore" membrane, as compared to a "closed pore" membrane. An open pore membrane can be in the form of a thin film or sheet of extruded porous polymer material with a relatively uniform thickness and an open pore porous structure that includes a polymer matrix that defines a large number of open "cells" that are three-dimensional void structures or pores. The open cells may be called openings, pores, channels or passages that are widely interconnected between adjacent cells to allow fluids, such as liquid fluids, to flow through the thickness of the membrane from one side to the other.

[0020] The described porous membranes contain pores of different pore sizes, and the pore size in the membrane varies along the thickness of the membrane. As used herein, "pore size" refers to the pore size (e.g., average size) in a region (or "portion") of the membrane, such as a thickness region located between two different depths of the membrane, or a specific depth in the membrane defined relative to the thickness of the membrane. For example, the region of the membrane can be the portion of the membrane between the surface of the membrane and a specific depth, such as a depth of 10 microns below the surface. As another example, the region of the membrane can be the portion located between two different depths, such as the portion of the membrane located in the middle third of the membrane thickness.

[0021] The described porous membranes have a morphology that is non-uniform (non-isotropic, non-uniform) across the membrane thickness in terms of pore size. A non-uniform morphology may be referred to as a "variable" morphology, with multiple (e.g., at least three) regions with different pore sizes at different locations along the membrane thickness. In the present context, a membrane with a "variable pore structure" is a structure that comprises pores of different sizes across the membrane thickness between two opposing surfaces of the membrane. The pore size may vary stepwise or non-stepwise across the membrane thickness (based on depth). (See, e.g., Figures 2A, 2B, 3A, and 3B.)

[0022] The membranes herein more specifically comprise two "tight" regions and at least one "open" region located between the two "tight" regions. These membranes are referred to herein as "double tight" membranes or membranes with "double tight" morphology. One region of the membrane is a region that can be referred to as a "tight region", meaning a region with relatively smaller pores throughout the thickness of the membrane. The second region of the membrane is a second tight region that also has relatively smaller pores throughout the thickness of the membrane. In the interior (or "middle") of the membrane is an "open region" located between the two opposing tight regions. The "open" region is a thickness portion that comprises pores that are relatively larger than the pores in both of the two tight regions. Due to this configuration, i.e., two tight regions and an open region in the interior of the membrane between the two tight regions, the membranes described may be referred to as "double tight" porous membranes with "variable" pore sizes.

[0023] A porous membrane having two tight regions and an internal open region is considered to be "monolithic": specifically, the entire thickness of the membrane and both opposing surfaces are formed and constructed together as a structurally single, continuous membrane by a single forming process, such as a single process including extrusion of the film and solidification of the polymers of the film (including coextrusion using a multi-slot die).

[0024] In contrast to the described integral porous membranes, other types of known porous membranes may be non-integral. These include membranes sometimes called multilayer or "composite" membranes, which are prepared by combining or placing two separate membrane layers, each having a different morphology or chemical composition, on opposing surfaces and optionally attaching or bonding them together. Such composite membranes may comprise a multilayer structure formed by combining a first porous membrane layer formed in one forming step and having a first (e.g., larger pore size) morphology with a second porous membrane layer formed in a second forming step that is different from the step of forming the first porous layer. This type of multilayer or "composite" membrane structure formed from multiple separate films made in multiple steps is not considered an "integral" membrane.

[0025] Another example of a membrane that is not considered to be integral according to this specification is a porous membrane coated on one or both surfaces, i.e., a membrane that includes a base membrane created during the membrane formation process and one or more coatings (e.g., one or more polymer coatings) applied to one or more surfaces of the base membrane in a subsequent coating process. An exemplary membrane can be a uniform (or non-uniform) base membrane with a relatively uniform (or non-uniform) pore size throughout, and coated with a polymer on one or both surfaces after formation. The polymer coating can be the same or different from the polymer of the base membrane. The polymer coating can reduce the pore size of one or two coated surfaces.

[0026] The membranes herein can have any useful thickness, such as a thickness ranging from 10 to 300 microns, for example, from 25 or 40 microns up to 250 or 200 microns.

[0027] The membrane has two opposing, relatively parallel surfaces extending in both the length and width directions, and a thickness extending in a third direction and located between the two opposing surfaces. A location midway between the two surfaces is considered to be an imaginary "centerline" that bisects the membrane thickness, i.e., extends equidistantly in both the length and width directions from each of the two opposing surfaces.

[0028] A "thickness region" of a membrane is a portion of the membrane that extends in the length and width dimensions of the membrane over a portion of the membrane's thickness. For purposes of this specification and claims, a membrane can be considered to comprise at least three thickness regions: a first tight region, an open region, and a second tight region. The open region is located between two tight regions. One or both tight regions may include the membrane's surface, but neither tight region is required to include the surface.

[0029] In certain embodiments, the membrane may comprise a thickness region including a first thickness region that includes the membrane's first surface and extends to a depth below the first surface, but not to the membrane's centerline; a second thickness region that includes the membrane's second surface and extends to a depth below the second surface, but not to the membrane's centerline; and a third thickness region that extends through the remainder of the membrane's thickness between the first thickness region and the second thickness region, and optionally and usually includes the centerline. Examples of useful depths below the membrane's first surface that define the size (thickness) of the first thickness region relative to the membrane's total thickness include depths equal to 2, 5, 10, 20, 25, 30, or 33% of the membrane's total thickness. Similarly, examples of useful depths below the membrane's second surface that define the size (thickness) of the second thickness region relative to the membrane's total thickness include depths equal to 2, 5, 10, 20, 25, 30, or 33% of the membrane's total thickness.

[0030] According to an exemplary membrane, the double tight morphology can be defined in terms of a relatively small average pore size in each of the two tight regions compared to a relatively large pore size in the open region. The average pore size of the tight region can be any average pore size in the tight portion of a useful filtration membrane, including, but not limited to, an average pore size in the range of 1 nanometer to 10 microns, such as 1 nanometer to 5 microns, or 10 nanometers to 1 or 2 microns. The first tight region and the second tight region can each independently have the same or non-same average pore size, both average pore sizes being within one of the defined ranges. The average pore size of the open region can be any average pore size in the open portion of a useful filtration membrane, including, but not limited to, an average pore size in the range of 5 nanometers to 50 microns, such as greater than 10 microns, such as 20 nanometers to 10 microns, or 50 nanometers to 1, 2, or 5 microns. Alternatively or additionally, the average pore size of the open regions may also be at least 10, 20, 50, or 100% or more larger than the average pore size of one or both tight regions, i.e., the average pore size of the open regions may be at least 10, 20, 50, or 100% larger than the average pore size in both tight regions.

[0031] When considering the size of the thickness regions along the thickness of the membrane, the present invention does not require a specific size of each region or the relative sizes of the regions, except that the average pore size of the regions is as described, a first thickness region having a depth location of a first minimum pore size on one side of the centerline, a second thickness region having a depth location of a second minimum pore size on a second side of the centerline, and a third region having a minimum pore size larger than the first minimum pore size and larger than the second minimum pore size.

[0032] More specifically, the double tight morphology can alternatively or additionally be defined in terms of the presence of two different "minimum" pore sizes (smallest measured pore sizes), each independently located at a particular depth in the membrane, each on opposite sides of the membrane's centerline. The "minimum" pore size is the smallest pore size measured on one side of the centerline, measured at a single uniform depth below the membrane's surface and over at least a portion of the membrane's area. According to these membranes described, the membrane has a first minimum pore size at a particular depth on one side of the centerline and a second minimum pore size at a particular depth on a second side of the centerline. The depth of the first minimum pore size from the first surface may be the same or different compared to the depth of the second minimum pore size from the second surface. The first minimum pore size is the smallest pore size present at a particular depth between the centerline and the first surface. The second minimum pore size is the smallest pore size present at a particular depth between the centerline and the second surface. These two smallest pore sizes are the two smallest pore sizes in the membrane, and there are no other depths in the membrane where smaller average pore sizes exist.

[0033] According to certain exemplary embodiments, the smallest pore size (first smallest pore size or second smallest pore size) may be located at the surface (first surface or second surface) (where the depth of the location of the smallest pore size is 0) or near the surface, for example within 2, 5, 10, or 20% of the membrane thickness from the surface.

[0034] The location of the first minimum pore size and the second minimum pore size can be independently at a surface or at a depth from the surface. For example, the location of the first minimum pore size can be at the first surface (depth 0) and the location of the second minimum pore size can be at the second surface; the location of the first minimum pore size can be below the first surface and the location of the second minimum pore size can be below the second surface; the location of the first minimum pore size can be at the first surface and the location of the second minimum pore size can be below the second surface; or the location of the first minimum pore size can be below the first surface and the location of the second minimum pore size can be at the second surface.

[0035] The average pore size in a region of the membrane or at a particular depth of the membrane can be measured by any useful technique, including manual or electronic visual inspection of images produced by a scanning electron microscope (SEM). In some examples of these methods, a computer software program can be used to evaluate the pore size in a region or depth of the membrane. In other examples, a hard copy of a SEM micrograph can be visually inspected to measure the pore size in a region or depth of the membrane.

[0036] Exemplary membranes can be described in terms of asymmetry, which is the relationship between the size of the pores in the open region and the size of the pores in the tight region. The asymmetry (D) of the described membranes can be defined as follows: D = (average pore diameter of the third thickness region) / A A can be defined as one of: the average pore size of the first region; the average pore size of the second region; the first smallest pore size, or the second smallest pore size.

[0037] Preferred membranes useful herein may have a degree of asymmetry (D) of at least 5, such as at least 10, 20 or 30, calculated using at least one of the different possible pore sizes of Group A.

[0038] 1A, a cross-section of an exemplary porous membrane 10 is shown having a surface 12, a second surface 14, and a thickness between the two surfaces. A centerline 50 is located midway between surface 12 and surface 14. A first thickness region 20 is located between surface 12 and a first depth D 1 The second thickness region 40 is located in a thickness region between the second surface 14 and the second depth D 2The third thickness region 30 is located in a thickness region between the first thickness region 20 and the second thickness region 40. The average pore size in each of the first thickness region 20, the second thickness region 40, and the third thickness region 50 can be measured across the three thickness dimensions of each region. According to this specification, the average pore size of the pores in the first thickness region is substantially (e.g., measurably) smaller than the average pore size of the pores in the third thickness region, and the average pore size of the pores in the second thickness region is substantially smaller than the average pore size of the pores in the third thickness region.

[0039] FIG. 1A also shows a first minimum pore size depth 22 located at a depth on one side of the midpoint 50. As shown, the first minimum pore size depth 22 is a depth of 0, meaning that the first minimum pore size is located at the surface 12. FIG. 1A also shows a second minimum depth 42 located on a second side of the midpoint 50, located at a depth slightly below the second surface 14. The first minimum pore size and the second minimum pore size are located at respective depths at or below the surfaces 12 and 14, respectively, and each depth is measured as the depth of the membrane where the pores running along the length and width of the membrane have the smallest average pore size for all pores on the same side of the midpoint 50, i.e., in the membrane 10 between the surface 12 and the midpoint 50 (depth 22) and in the membrane 10 between the surface 14 and the midpoint 50 (depth 42). Each minimum pore size is the smallest average pore size at any particular depth on each side of the centerline, and there are no other depths on each side of the membrane to the centerline that have an average pore size smaller than the minimum pore size.

[0040] 1B, a cross-section of a porous membrane 10 is shown having a surface 12, a second surface 14, and a thickness between the two surfaces. A centerline 50 is located halfway between surface 12 and surface 14. A first thickness region 20 is located between surface 12 and a first depth D. 1 The second thickness region 40 is located in a thickness region between the second surface 14 and the second depth D 2 The third thickness region 30 is located in a thickness region between the first thickness region 20 and the second thickness region 40, for example, at a depth D1 and depth D 2 The average pore size of the pores throughout each of the first thickness region 20, the second thickness region 40, and the third thickness region 50 can be measured across the three thickness regions. According to this specification, the average pore size of the pores in the first thickness region is substantially smaller than the average pore size of the pores in the third thickness region, and the average pore size of the pores in the second thickness region is substantially smaller than the average pore size of the pores in the third thickness region.

[0041] 1B also shows a first minimum pore size depth 22 located at or at a surface of membrane 10 on one side of midpoint 50, and a second minimum pore size depth 42 located at or at a second surface of membrane 10 on a second side of midpoint 50. In the membrane shown, the location of first minimum pore size 22 and the location of second minimum pore size 42 are at or near surface 12 and surface 14, respectively. Each of the two minimum pore sizes is the smallest average pore size on one side of the membrane relative to the centerline, and there is no other depth on each side of the membrane that has an average pore size smaller than the minimum pore size.

[0042] The described porous film can be prepared by a method of forming a polymer extrusion film, including a novel and inventive method, which includes exposing both surfaces of the film to conditions that cause the polymer of the film to solidify, the conditions being the same conditions applied in the same way to both surfaces. Because both surfaces of the extruded film are exposed to the same conditions that cause solidification in the same way and at the same time, the described method can be effective to form a solidified film with two opposing surfaces with pores that are simultaneously formed by the same solidification process; the pores in each of the two opposing surfaces can be smaller than the pores in the interior region of the film to produce a "double tight" film; the pores in the two opposing surfaces can be of comparable morphology because each surface undergoes solidification based on substantially the same or similar solidification-inducing conditions and timing. The resulting solidified film has two opposing (tight) surface or thickness regions with similar, equivalent, or substantially the same morphology, one on each side of the centerline, and an interior region with an (open) morphology that is different from the morphology of the two surfaces. An exemplary membrane may have one surface or region having a morphology with a relatively small pore size, a second (opposite) surface or region having a morphology also with a relatively small pore size, and an interior portion between the two surfaces or regions having a morphology with a relatively large pore size compared to the first and second surfaces.

[0043] As an example of a method useful for preparing the described membranes having the described morphology, the membranes can be formed by forming an extruded liquid film of a liquid polymer solution containing a non-coagulated (optionally also a certain amount of coagulated or partially coagulated) polymer dissolved (or suspended) in a solvent, and coagulating the polymer within the film by exposing the two opposing surfaces of the film to conditions (e.g., temperature, non-solvent, humidity, solvent evaporation) that coagulate the polymer on the two opposing surfaces of the film in parallel or simultaneously. In one example, the technique that induces coagulation is by a non-solvent induced phase separation (NIPS) technique. In another example, the polymer coagulation may be induced by thermally induced phase separation (TIPS).

[0044] In conventional non-solvent induced phase separation (NIPS), a polymer solution containing a polymer dissolved or suspended in a solvent is typically extruded and cast onto a support layer (e.g., a supported polymer film) to form a cast film. The cast film has one surface that is covered in contact with the support layer and another (opposite) surface that is exposed or open. The support layer and the extruded and cast film are then immersed in a coagulation bath containing a "non-solvent", i.e., a liquid in which the polymer is not substantially soluble. Immersion of the cast film in the non-solvent causes a solvent-non-solvent exchange between the non-solvent bath and the solvent of the extruded film polymer solution at the exposed surface. The solvent exchange causes the non-solvent to be present with the polymer in the cast film and precipitate the polymer from the cast polymer solution film onto the support layer. The polymer needs to be highly soluble in the solvent of the polymer solution and substantially insoluble in the "non-solvent" of the bath so that the polymer efficiently precipitates or coagulates upon contact with the non-solvent (e.g., aqueous liquid) of the coagulation bath.

[0045] According to these techniques, the liquid non-solvent contacts only one surface of the cast polymer solution film, which is the exposed surface, but not the opposite surface of the film, which is in contact with the support layer. Because the non-solvent contacts only one surface of the cast film and the solvent exchange occurs only through the one surface of the cast film, the solidified polymer film has a non-uniform, e.g., asymmetric, morphology, where one side of the film shows a different morphology compared to the other side of the film. Usually, after solidification, the film has an asymmetric morphology with a first morphology on one side of the film, a substantially different second morphology on the second side of the film, and an intermediate morphology between the two sides that varies throughout the thickness of the film, e.g., a pore size that varies stepwise over a range of pore sizes between the pore size on one surface and the pore size on the second surface. As an example, one surface may have a relatively small average pore size and an opposing surface may have a relatively large average pore size, with the average pore size at all locations (depths) between the two surfaces being between the average pore sizes at the opposing surfaces. Optionally, one surface may be considered to exhibit a "tight" morphology and the second surface may be considered to exhibit an "open" morphology.

[0046] A similar effect can be achieved using conventional thermally induced phase separation (TIPS) technology. In conventional TIPS technology, a polymer-containing liquid, typically containing non-coagulated polymer (and optionally partially coagulated polymer) in a solvent, is extruded through a slot die to form an extruded film. In conventional TIPS processes, one side of the extruded film is cooled, for example by contacting it with a low-temperature "chill roll," thereby solidifying the polymer of the extruded film.

[0047] This technique exposes one surface of the extruded film to a low temperature. The opposite surface is not directly or indirectly exposed to low temperatures, resulting in a difference in how the polymer solidifies on one surface of the extruded film compared to the opposite surface. Because only one side of the film is exposed to low temperatures, the solidified polymer film is non-uniform in morphology, with one side of the film exhibiting a substantially different morphology compared to the other side of the film. Typically, after solidification, the film has an asymmetric morphology, including a first morphology on one side of the film, a substantially different morphology on the second side of the film, and an intermediate morphology between the two sides. As an example, one surface may have a relatively small average pore size and an opposite surface may have a relatively large average pore size, with the average pore size at all positions (depths) between the two average pore sizes on the opposite surfaces. Optionally, one surface may be considered to exhibit a "tight" morphology and the second surface may be considered to exhibit an "open" morphology.

[0048] The exemplary methods herein differ from prior phase separation techniques used to form porous polymeric membranes because, at least, the exemplary methods described herein expose both surfaces of an extruded (including coextruded) film to the same or similar conditions that cause solidification to a relatively similar or similar extent. The conditions may be contact with a liquid "non-solvent" or may be low temperature conditions, e.g., a low temperature liquid bath. Compared to the extruded film methods described, the methods of the present invention may not require, and preferably may not include, a step of casting an extruded film of a polymer solution onto a support layer (e.g., a polymer film or a release liner) or placing only one side of the extruded film (e.g., by a support layer) in contact with a cooled surface such as a chill roll. According to the methods of the present invention, both surfaces of the extruded film are exposed to the same conditions effective to cause solidification for the same time and optionally to the same extent (e.g., depending on the identity of the polymer on each surface), e.g., simultaneously. By subjecting both surfaces of the extruded film to the same solidification-inducing conditions in the same or equivalent manner, the conditions affect both surfaces of the film in a similar manner, causing a solidification effect on both surfaces of the film, and upon solidification, a membrane is produced that includes two opposing surfaces or faces, each having a tight morphology, and optionally two opposing equivalent or identical morphologies, relative to the interior region of the membrane.

[0049] According to examples and preferred embodiments for preparing the described membranes, a polymer can be combined with a solvent (e.g., completely dissolved in the solvent) to form a polymer-containing liquid (referred to herein as a "polymer solution" or "polymer-containing liquid") containing the polymer in a non-coagulated or partially coagulated form that can be extruded as a liquid into a sheet, after which coagulation can be induced on both sides of the sheet, such as by using an immersion precipitation method, e.g., TIPS or NIPS, or another method such as exposure to moisture or solvent evaporation. A single polymer-containing liquid may be used, or multiple polymer-containing liquids may be used in a coextruded film.

[0050] A typical method may be carried out using one or more steps including forming or otherwise preparing one or more polymer-containing liquids comprising a polymer for preparing a porous polymer membrane, dissolved or suspended in a solvent; extruding (including coextrusion) the one or more polymer-containing liquids through a die to form an extruded (including coextruded) sheet or film comprising the polymer-containing liquid; solidifying (e.g., precipitating) a polymer of the polymer-containing liquid from the polymer-containing liquid to form a solidified porous polymer membrane ("porous polymer membrane"); and, optionally, drying or otherwise further processing the formed porous polymer membrane.

[0051] An example of such a method may include the use of an extrusion die to extrude one or more polymer-containing liquids as a film. The extrusion die may be a single slot die or a multi-slot die. A single slot die may be used if only a single polymer-containing liquid is used to form the film. A multi-slot die may be used if the film is formed using two or more different polymer types or polymer-containing liquids. If a multi-slot die is used and two or more different polymers or polymer-containing liquids are used, the extruded film is considered to be a single extruded film when extruded, even if the polymers are chemically or physically different in composition; a coextruded film is considered to be a single integral film. A coextruded film from a multi-slot die is exposed to solidification-inducing conditions only on two opposing surfaces, and the resulting solidified film membrane is considered to be formed in a single extrusion step and is considered to be an integral membrane.

[0052] Any effective extrusion conditions and processing parameters can be used, including the useful draw rate of the extruded film, the useful flow rate of the polymer-containing liquid, the air gap distance (if any) between the die and the coagulation bath, the humidity of the air in the air gap region (if any), and any useful, optionally conventional, type and size die. The flow rate of the polymer-containing liquid through the die and the draw rate of the extruded film can be used to affect the thickness of the extruded film.

[0053] After being extruded, both sides of the film are exposed to conditions that solidify the polymer contained in the extruded film. For example, the extruded film can be contacted with a coagulation bath that contains a liquid that is cooler than the extruded film, or that contains a "non-solvent", or both, to solidify the polymer contained in the extruded film. An example of a coagulation bath for the TIPS process can be a liquid bath such as water that has a temperature that solidifies the (non-coagulated) polymer dissolved from the polymer-containing liquid of the extruded film, for example, a liquid that has a temperature of less than 30, 20, or 10°C. An example of a coagulation bath for NIPS can be a bath made of a non-solvent, for example, water, or a mixture of water and an organic liquid that can dissolve the polymer solution solvent.

[0054] According to a more detailed example of a particular type of film-forming technique, the extruded film (with uncoagulated or partially coagulated polymer) may be directly extruded into the coagulation bath, or may be extruded out of the coagulation bath (e.g., vertically upwards) and then immediately after extrusion into the coagulation bath. In the latter example, the film is exposed to air after being extruded from the die before the extruded (uncoagulated) film contacts the liquid of the coagulation bath. Exposing the extruded film to air before the film enters the coagulation bath ("air gap") is optional. If an air gap is present, the time that the extruded film is exposed to air before contacting the coagulation bath can be, for example, less than 2 seconds, less than 1 second, or less than 0.5 seconds, as desired. In another exemplary method, the extruded film is extruded directly into the coagulation bath without contacting air before contacting the coagulation bath.

[0055] The type of polymer in the polymer solution and the resulting porous polymer membrane can be any type of polymer known or to become known for use in forming porous membranes by NIPS or TIPS techniques. Examples of currently known or preferred polymers, particularly for the NIPS process, include polyamides, polyimides, polyamide-polyimides, polysulfones such as polyethersulfone or polyphenylsulfone, and fluoropolymers such as polyvinylidene fluoride, among others. Examples of currently known or preferred polymers, particularly for the TIPS process, include polyolefins, such as polyethylene and polypropylene, and fluorinated polymers, such as perfluoroalkoxy (PFA), among others. In a process using a single slot die, only a single polymer and a single polymer solution are necessary, although polymer mixtures can also be used. In a process using a multi-slot die, e.g., a two-slot or three-slot die, different polymer types, or polymer solutions of the same polymer but different compositions, can be run through the different slots. As an example, a first type of polymer and a first polymer solution can be used in the slots that form the film surface, and one or more different polymers (or polymer solutions) can be used in one or more slots that form the interior region of the film.

[0056] 2A, 2B, 3A, and 3B, there is shown a portion of an exemplary extrusion system that is effective for preparing the exemplary polymeric membranes described, with 2A and 3A showing a front view of the exemplary system and 2B and 3B showing a side view of the exemplary system.

[0057] 2A and 2B, system 100 includes an extrusion die 120, which may be, for example, a sheet extrusion die of the type conventionally referred to as a coat hanger manifold die. Die 120 is a single slot extrusion die with a slot 122 at the bottom of the die. Polymer solution 130 passes through the manifold interior of die 120 and then through slot 122, after which the extruded polymer solution forms an extruded film 140a that travels unsupported extending vertically downward below die 120. A liquid coagulation bath 150 having an upper surface or "bathline" 152 is located below die 120.

[0058] A source (not shown) of polymer solution 130 is provided at a constant and regular rate by a pump or other flow device so that it flows continuously through the die 120. After exiting the slot 122 downward, the extruded film 140a enters and is immersed in the liquid in the coagulation bath 150. The extruded film 140a exits the die slot 122 as a thin continuous film of polymer solution 130 with any non-coagulated polymer present in the polymer solution. The film 140a with the non-coagulated polymer is then contacted with the liquid of the coagulation bath 150 to coagulate the dissolved polymer of the polymer solution 130 in the film 140a.

[0059] Starting from the bus line 152, the liquid in the coagulation bath 150 contacts the two opposing surfaces of the film 140a, coagulating the dissolved polymer on both surfaces of the film 140a. The polymer of the film 140a precipitates (e.g., coagulates) out of solution to form a porous polymer film membrane 140b containing the polymer in a coagulated form. Because the liquid in the coagulation bath 150 contacts the two opposing surfaces of the film 140a simultaneously, both surfaces are equally susceptible to the liquid coagulating the polymer, producing a film 140b with two opposing surfaces having the same or identical morphology.

[0060] Optionally, as shown in Figures 2A and 2B, the film 140a made of the non-coagulated polymer solution 130 passes through an air space ("air gap") after exiting the die slot 122 and before contacting the liquid in the coagulation bath 150. Upon entering the coagulation bath 150, the liquid in the coagulation bath 150 causes phase separation in the polymer solution 130 to form a filtration membrane 140b. Alternatively, according to other exemplary systems and methods, such as those shown in Figures 3A and 3B, there is no air gap between the die slot 122 and the liquid in the coagulation bath 150, and phase separation (coagulation) of the polymer of the film 140a occurs immediately in the coagulation bath 150 as the polymer solution 130 exits the die slot 122 to form the membrane 140b.

[0061] Note that these figures show extruded films formed from a single polymer solution using a single slot die. In alternative methods and systems, two or more different polymer solutions (optionally one or more different types of polymers) can be run through different slots of a multi-slot extrusion die.

[0062] One or more optional subsequent steps, such as a washing tank, a heating step, a drying step, or a winding section, can be used to further treat or process the membrane 140b. For example, after the phase separation (coagulation) step in the coagulation bath 150, the membrane 140b can be directed through a washing tank to extract residual solvent. The washed (still wet) membrane 140b can then be collected on a roll, optionally before or after a post-processing drying step.

[0063] As shown in Figures 2A, 2B, 3A, and 3B, the extruded film undergoes a reduction in film width, film thickness, or both immediately after it leaves the die. This phenomenon is sometimes referred to as "necking". That is, after the film leaves the die, the film "necks down" to reduce in width, thickness, or both. Alternatively, this phenomenon is sometimes referred to as the "dog-bone" effect. Due to this necking effect, the thickness of the extruded film measured across the width of the film and at the edges of the film may also exhibit reduced uniformity - the film thickness may become less uniform. That is, it may exhibit increased variability across the width and at the edges. Particular locations of reduced uniformity may occur at both ends (ends) of the film, with an increased thickness at each end (like a dog bone). A further potential advantage of the present system and method is the desired high uniformity in film thickness across the width of the film, including the ends, i.e., reduced dog-bone effect.

[0064] The described filtration membranes may be useful for producing a filtered liquid by passing a liquid through the filtration membrane to remove one or more contaminants from the liquid, the filtered liquid containing a reduced level of one or more contaminants or particulate matter compared to the level of the contaminants or particulate matter present in the liquid before the liquid passes through the filtration membrane.

[0065] The described polymeric membranes can provide a combination of useful, desirable, or advantageous physical properties, including performance (filtration performance as measured by "retention performance"), pore size or bubble point (related to pore size), flow, and mechanical properties (flexibility and durability, or reduced brittleness).

[0066] The level of effectiveness of a filtration membrane in removing unwanted substances (i.e., "impurities") from a liquid can be measured in one way as "retention performance". Retention performance, in terms of the effectiveness of a filtration membrane (e.g., a filtration membrane as described), generally refers to the total amount of impurities (actual or during a performance test) removed from a liquid relative to the total amount of impurities present in the liquid containing the impurities when the liquid is passed through the filtration membrane. Thus, the "retention performance" value of a filtration membrane is a percentage, and a filter with a high retention performance value (high percentage) is relatively effective at removing particles from a liquid, and a filter with a low retention performance value (low percentage) is relatively ineffective at removing particles from a liquid.

[0067] Particle capture performance can be measured by measuring the number of test particles removed from a fluid stream by a membrane placed in the middle of the fluid stream. In one method, particle capture performance can be measured by passing a sufficient amount of an aqueous feed solution of 0.1% Triton X-100 containing 8 ppm polystyrene particles (e.g., G25 polystyrene round particles with a nominal diameter of 5 to 15 nanometers) to achieve 1% monolayer coverage through a 47 millimeter diameter membrane specimen at a constant flow rate of 7 milliliters per minute and collecting the permeate. The concentration of polystyrene particles in the permeate can be calculated from the absorbance of the permeate. The particle capture performance is then calculated using the following equation: TIFF2024138238000002.tif15170

[0068] As used herein, the "nominal diameter" is the diameter of a particle determined by photon correlation spectroscopy (PCS), laser diffraction, or optical microscopy. Usually, the calculated diameter, or nominal diameter, is expressed as the diameter of a sphere having the same projected area as the projected image of the particle. PCS, laser diffraction, and optical microscopy techniques are well known in the art (see, for example, Jillavenkatesa, A., et al.; "Particle Size Characterization;" NIST Recommended Practice Guide; National Institute of Standards and Technology Special Publication 960-1; January 2001).

[0069] In the preferred embodiment of the described membrane, the membrane can exhibit a retention performance of more than 90% at 0.5%, 1.0%, 1.5% and 2.0% monolayer coverage, and can also exhibit a retention performance of more than 95, 96 or 97% at 0.5%, 1.0%, 1.5% and 2.0% monolayer coverage. With this level of retention performance, these examples of the membrane of the present invention show a higher retention performance level compared to many currently commercially available filtration membranes, such as comparable flat sheet and hollow fiber filtration membranes made with UPE. These exemplary membranes also provide useful, good or very good flow rates (short flow times) and exhibit mechanical properties that allow the membrane to be prepared and assembled into filter cartridges or filter products.

[0070] Bubble point is a known property of porous materials, including the composite filtration membrane described. Bubble point may correspond to pore size, and pore size may correspond to filtration performance. Smaller pore size may be associated with higher bubble point, and possibly with higher filtration performance (higher capture performance). However, higher bubble point is usually also associated with relatively higher resistance to flow through the porous material, and lower flux. According to certain exemplary dual tight membranes herein, bubble points may be equivalent when measured in either direction of flow through the membrane. If the higher of the two bubble points is not more than 20% greater than the lower, for example, if the higher of the two bubble points is not more than 10, 5, 2, or 1% greater than the lower, the bubble point measured in one direction is considered equivalent to the bubble point measured in the opposite direction. Equivalent bubble points in this way may indicate that the film has a high degree of symmetry with respect to the centerline of the membrane.

[0071] One method for determining the bubble point of a porous material is to wet a sample of the porous material by immersion in a liquid with a known surface tension and apply gas pressure to one side of the sample. The gas pressure is increased in steps. The minimum pressure at which the gas will flow through the sample is called the bubble point. A Novec HFE 7200, IPA, or water, compressed air, or compressed N 2 Examples of useful bubble points of the described porous filtration membranes, measured using a gas at a temperature of 20-30°C (usually 25°C), can be in the range of 2-400 psi, for example in the range of 135-185 psi.

[0072] The filtration membranes described herein, or filters or filter components containing the filtration membranes described herein, may be useful in methods of filtering liquid chemicals to purify the liquid chemicals or remove unwanted substances from the liquid chemicals, particularly to produce high purity liquid chemicals useful in industrial processes that require very high purity chemical inputs. In general, the liquid chemicals may be any of a variety of useful commercially available substances, and may be liquid chemicals that are useful or used for any application, any industrial or commercial use. Particular embodiments of the filters described may be used to filter liquid solvents or other process liquids used in semiconductor photolithography or cleaning methods or steps for processing semiconductor wafers or microelectronic devices, to purify liquid chemicals that are used or are useful in semiconductor or microelectronic manufacturing applications.

[0073] Some specific non-limiting examples of solvents (including cleaning solutions) that can be filtered using the described filtration membranes include n-butyl acetate (nBA), isopropyl alcohol (IPA), 2-ethoxyethyl acetate (2EEA), xylene, cyclohexanone, ethyl lactate, methyl isobutyl carbinol (MIBC), methyl isobutyl ketone (MIBK), isoamyl acetate, undecane, propylene glycol methyl ether (PGME), propylene glycol monomethyl ether acetate (PGMEA), or a mixture of any of these, such as a mixture of PGME and PGMEA; or concentrated or diluted ammonium hydroxide, hydrogen peroxide, hydrochloric acid, HF, sulfuric acid, another peroxide solution, or a combination of these, such as a combination of ammonium hydroxide and hydrogen peroxide, or a combination of hydrochloric acid and hydrogen peroxide.

[0074] The membrane can be contained within a larger filter structure, such as a filter or filter cartridge for use in a filtration system. A filtration system places the composite filtration membrane in a liquid chemical flow path, for example as part of a filter or filter cartridge, such that at least a portion of the liquid chemical flow passes through a filter layer of the composite filtration membrane, which removes a certain amount of impurities or contaminants from the liquid chemical. The filter or filter cartridge structure may include one or more of a variety of additional materials and structures that support the composite filtration membrane within the filter, such that the fluid flows from the filter inlet, through the membrane (including the filter layer), through the filter outlet, and thereby through the composite filtration membrane as it passes through the filter. EXAMPLES

[0075] Referring to FIG. 4, FIG. 4 shows a comparison of three filtration membranes made of polyethersulfone, prepared by different methods, and having different structures or morphologies.

[0076] One membrane is a "single-layer PES membrane." This membrane was prepared by conventional phase separation methods such as NIPS. The single-layer PES membrane has asymmetric properties, with one side having a tight surface and the other side having an open surface.

[0077] One membrane is a "bilayer PES membrane," which is made by laminating two single-layer PES membranes together, creating a multilayer membrane in which the two membranes are used in series.

[0078] One membrane is a "double tight layer PES membrane" prepared according to the present specification.

[0079] As shown in FIG. 4, the double tight layer PES membrane of the present invention exhibits significantly improved capture performance compared to other membranes made of the same materials but with different morphologies or structures.

[0080] In a first embodiment, an integral extruded porous polymer sheet membrane comprises a first surface, a second surface, and a thickness between the first surface and the second surface, a first thickness region including the first surface and a portion of the membrane in the thickness direction, a second thickness region including the second surface and a portion of the membrane in the thickness direction, and a third thickness region extending in the thickness direction between the first thickness region and the second thickness region, wherein the average pore size of the first thickness region and the average pore size of the second thickness region are both smaller than the average pore size of the third region.

[0081] A second embodiment according to the first embodiment, wherein the membrane has a centerline between the first and second surfaces, the first thickness region includes a depth location having a minimum pore size on a first side of the centerline, and the second thickness region includes a depth location having a minimum pore size on a second side of the centerline.

[0082] A third aspect according to the second aspect, wherein the first minimum pore size is in the range of 1 nanometer to 10 microns and the second minimum pore size is in the range of 1 nanometer to 10 microns.

[0083] A fourth aspect according to the second or third aspect, wherein the first minimum pore size is between the first surface and a third thickness depth from the first surface, the second minimum pore size is between the second surface and a third thickness depth from the second surface, and the average pore size of the third thickness region is measured in the central third of the thickness.

[0084] The degree of asymmetry (D) is at least 5. D = (average pore diameter of the third thickness region) / A where A is one of the average pore size of the first region; the average pore size of the second region; the first minimum pore size, or the second minimum pore size. A fifth aspect according to any one of the first to fourth aspects, wherein

[0085] A sixth aspect according to any one of the first to fifth aspects, wherein the membrane comprises a polymer selected from polyethersulfone and polyamideimide.

[0086] A seventh embodiment according to any one of the first to sixth embodiments, having a thickness in the range of 40 to 300 microns.

[0087] An eighth embodiment according to any one of the first to seventh embodiments, having a capture performance of at least 90% as measured based on a 1% monolayer using G25 polystyrene round particles having a nominal diameter of 5 to 15 nanometers.

[0088] A ninth aspect according to any one of the first to eighth aspects, prepared by a process of non-solvent induced phase separation whereby the first thickness region, the second thickness region, and the third thickness region are formed using the same phase separation process.

[0089] A tenth embodiment according to any one of the first to ninth embodiments, consisting essentially of an extruded porous polymer sheet membrane having first and second surfaces, a thickness between the surfaces, a first thickness region, a second thickness region, and a third thickness region.

[0090] An eleventh embodiment according to any one of the first to tenth embodiments, comprising an extruded porous polymer sheet membrane having first and second surfaces, a thickness between the surfaces, a first thickness region, a second thickness region, and a third thickness region.

[0091] In a twelfth aspect, a filter comprises a membrane according to any one of the first to eleventh aspects.

[0092] A thirteenth embodiment, comprising a membrane encased in a housing in a pleated configuration.

[0093] In a fourteenth embodiment, a method of filtering a fluid comprises passing the fluid through the filter of the eleventh embodiment.

[0094] A fifteenth embodiment according to the fourteenth embodiment, wherein the fluid is a semiconductor photolithography solvent, a cleaning fluid, or an etching fluid.

[0095] A sixteenth aspect according to the fifteenth aspect, wherein the fluid is selected from propylene glycol methyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), cyclohexanone, and n-butyl acetate.

[0096] A seventeenth aspect according to the fifteenth aspect, wherein the fluid comprises a dilute or concentrated solution comprising ammonium hydroxide, hydrogen peroxide, hydrochloric acid, HF, sulfuric acid, a peroxide solution, or a combination thereof.

[0097] In an eighteenth embodiment, a method of making an extruded porous polymer sheet membrane having first and second opposed surfaces, a thickness between the opposed surfaces, and pores having a non-uniform pore size includes forming a polymer-containing liquid comprising a polymer in a solvent, passing the polymer-containing liquid through an extrusion die to form an extruded film of the polymer-containing liquid, and exposing both sides of the extruded film to conditions that cause solidification of the polymer on both sides of the film.

[0098] A nineteenth embodiment according to the eighteenth embodiment, further comprising inducing solidification on both sides of the extruded film by a thermally induced phase separation technique.

[0099] A twentieth embodiment according to the eighteenth embodiment, further comprising inducing solidification on both sides of the extruded film by a non-solvent induced phase separation technique.

[0100] A 21st embodiment according to the 18th embodiment, further comprising inducing solidification on both sides of the extruded film by exposing both sides of the extruded film to moisture.

[0101] A twenty-second embodiment according to the eighteenth embodiment, further comprising causing solidification on both sides of the extruded film by evaporating liquid on both sides of the extruded film.

[0102] A 23rd embodiment according to the 18th embodiment, comprising contacting the first surface and the second surface of the extruded film with a coagulation bath to coagulate the dissolved polymer of the polymer solution and form an extruded porous polymer membrane comprising the coagulated polymer of the polymer solution.

[0103] A 24th aspect according to any one of the 18th to 23rd aspects, wherein the membrane comprises a first surface, a second surface, and a thickness between the first and second surfaces, a first thickness region including the first surface and a portion of the membrane in the thickness direction, a second thickness region including the second surface and a portion of the membrane in the thickness direction, and a third thickness region extending in the thickness direction between the first thickness region and the second thickness region, wherein an average pore size of the first thickness region and an average pore size of the second thickness region are both smaller than an average pore size of the third region.

[0104] A 25th embodiment according to the 23rd or 24th embodiment, wherein the extruded film exits the die through a die opening, and the die opening is immersed in the coagulation liquid.

Claims

1. 1. An integral extruded porous polymer sheet membrane comprising: a first surface, a second surface, and a thickness between the first surface and the second surface; a first thickness region including the first surface and a portion of the membrane through the thickness; a second thickness region including the second surface and a portion of the membrane through the thickness; and a third thickness region extending in a thickness direction between the first thickness region and the second thickness region; A membrane, wherein the average pore size of the first thickness region and the average pore size of the second thickness region are both smaller than the average pore size of the third thickness region.

2. the membrane has a centerline between the first surface and the second surface; the first thickness region has a minimum pore size at a location between the first surface and the centerline; 10. The membrane of claim 1, wherein the second thickness region has a minimum pore size at a location between the second surface and the centerline.

3. a first minimum pore size in the range of 1 nanometer to 10 microns; 3. The membrane of claim 2, wherein the second minimum pore size is in the range of 1 nanometer to 10 microns.

4. a first minimum pore size is at a depth of one-third the thickness from the first surface; 5. The membrane of claim 2, wherein the second smallest pore size is at a depth of one-third the thickness from the second surface.

5. The asymmetry degree (D) is at least 5, D = (average pore diameter of the third thickness region) / A [wherein A is one of the average pore size of the first region; the average pore size of the second region; the first minimum pore size, or the second minimum pore size.] The membrane according to any one of claims 1 to 4, wherein said membrane is defined as:

6. 6. The membrane of claim 1 , wherein the membrane comprises a polymer selected from polyethersulfone and polyamideimide.

7. A membrane according to any one of claims 1 to 6, having a thickness in the range of 40 to 300 microns.

8. 8. The membrane of any one of claims 1 to 7, prepared by a process of non-solvent induced phase separation whereby the first thickness region, the second thickness region and the third thickness region are formed using the same phase separation process.

9. A filter comprising a membrane according to any one of claims 1 to 8.

10. 1. A method of filtering a fluid, comprising passing the fluid through an integral extruded porous polymer sheet membrane, the membrane comprising: a first surface, a second surface, and a thickness between the first surface and the second surface; a first thickness region including the first surface and a portion of the membrane through the thickness; a second thickness region including the second surface and a portion of the membrane through the thickness; and a third thickness region extending in a thickness direction between the first thickness region and the second thickness region; The method, wherein the average pore size of the first thickness region and the average pore size of the second thickness region are both smaller than the average pore size of the third thickness region.

11. The method of claim 10 , wherein the fluid is a semiconductor photolithography solvent, a cleaning fluid, or an etching fluid.

12. The method according to claim 10 or claim 11, wherein the fluid is selected from propylene glycol methyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), cyclohexanone, n-butyl acetate.

13. 13. The method of any one of claims 10 to 12, wherein the fluid comprises a dilute or concentrated solution comprising ammonium hydroxide, hydrogen peroxide, hydrochloric acid, HF, sulfuric acid, a peroxide solution, or a combination thereof.

14. 1. A method for making an integral extruded porous polymer sheet membrane, comprising: forming a polymer-containing liquid comprising a polymer in a solvent; passing the polymer-containing liquid through an extrusion die to form an extruded film of the polymer-containing liquid; and subjecting both sides of the extruded film to conditions that cause solidification of the polymer on both sides of the film; A one-piece extruded porous polymer sheet membrane, a first surface, a second surface, and a thickness between the first surface and the second surface; a first thickness region including the first surface and a portion of the membrane through the thickness; a second thickness region including the second surface and a portion of the membrane through the thickness; and a third thickness region extending in a thickness direction between the first thickness region and the second thickness region; The method, wherein the average pore size of the first thickness region and the average pore size of the second thickness region are both smaller than the average pore size of the third thickness region.

15. 15. The method of claim 14, further comprising inducing solidification on both sides of the extruded film by a thermally induced phase separation technique.

16. 16. The method of claim 14 or claim 15, further comprising inducing solidification on both sides of the extruded film by a non-solvent induced phase separation technique.

17. 17. The method of any one of claims 14 to 16, further comprising inducing solidification on both sides of the extruded film by exposing both sides to moisture.

18. 18. The method of any one of claims 14 to 17, further comprising causing solidification on both sides of the extruded film by evaporating liquid on both sides of the extruded film.

19. 19. The method of any one of claims 14 to 18, further comprising inducing coagulation on both sides of the extruded film by contacting the first surface and the second surface with a coagulation bath.

20. The extruded film exits the extrusion die through a die opening; 20. The method of any one of claims 14 to 19, wherein the die opening is immersed in the coagulation liquid.