Composite filter media

The composite porous filter membrane with a polyamide coating on a hydrophobic polymeric material addresses the challenge of removing low concentration contaminants in microelectronic processing fluids, enhancing filtration efficiency and purity while maintaining high permeability and stability.

JP2024138302AInactive Publication Date: 2024-10-08ENTEGRIS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024102687
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-06-23
Filing Date
2024-06-26
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing filter membranes in microelectronic device processing struggle to effectively remove low concentrations of ionic contaminants and colloidal particles, which can adversely affect the quality and performance of microprocessors and memory devices, while maintaining high permeability and stability in acidic environments.

Method used

A composite porous filter membrane is developed, comprising a porous hydrophobic polymeric filter material coated with a polyamide polymer soluble in formic acid, which provides a semi-continuous coating to enhance non-sieve filtration performance, characterized by a surface energy greater than 30 dynes/cm and isopropanol flow time of 150 to 20,000 seconds/500 mL, and optionally includes a crosslinked polyamide coating formed through free radical polymerization.

Benefits of technology

The composite membrane achieves improved non-sieve filtration by enhancing particle retention and dye binding capacity, maintaining high permeability and stability, effectively removing ionic contaminants and colloidal particles from acidic processing liquids, thereby improving the purity of microelectronic device manufacturing fluids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138302000001_ABST
    Figure 2024138302000001_ABST
Patent Text Reader

Abstract

To provide composite membranes useful for removing various impurities from liquids.SOLUTION: In certain aspects, the composite membranes comprise a hydrophobic polymer having a polyamide as a coating thereon, and in other aspects, such composite membranes have certain acrylic polymers as coatings thereon. The composite membranes are useful in removal of various impurities in liquids, such as those encountered in industrial and life science processes.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a composite filter material or membrane comprising a porous polymeric filter coated with a layer comprising a polyamide polymer. [Background technology]

[0002] Filter products are essential tools in modern industry used to remove undesirable materials from useful fluid streams. Useful fluids treated using filters include water, liquid industrial solvents and process fluids, industrial gases used for manufacturing or processing (e.g., in semiconductor manufacturing), and liquids having medical or pharmaceutical uses. Undesirable materials removed from fluids include impurities and contaminants such as particles, microorganisms, and dissolved chemical species. Specific examples of filter applications include use with liquid materials for semiconductor and microelectronic device manufacturing.

[0003] To perform the filtering function, the filter includes a filter membrane, which serves to remove undesirable materials from the fluid passing through it. The filter membrane may be in the form of a flat sheet, which may be wound (e.g., spirally), flat, pleated, or disk-shaped, as appropriate. Alternatively, the filter membrane may be in the form of hollow fibers. The filter membrane may be contained within a housing or otherwise supported such that the fluid being filtered enters through a filtration inlet and must pass through the filter membrane before passing through a filtration outlet.

[0004] Filter membranes can be constructed from porous structures with average pore sizes that can be selected based on the application of the filter, i.e., the type of filtration performed by the filter. Typical pore sizes are in the micron or submicron range, such as from about 0.001 micron to about 10 microns. Membranes with average pore sizes of about 0.001 to about 0.05 microns are sometimes classified as ultrafilter membranes. Membranes with pore sizes between about 0.05 and 10 microns are sometimes referred to as microporous membranes.

[0005] Filter membranes with pore sizes in the micron or submicron range can be effective in removing undesirable materials from a fluid stream by either sieving or non-sieving mechanisms, or both. Sieving mechanisms are a form of filtration that removes particles from a liquid stream by mechanically retaining them on the surface of the filter membrane, which mechanically interferes with the movement of the particles and acts to retain them in the filter, mechanically impeding the flow of the particles through the filter. Typically, the particles can be larger than the pores of the filter. "Non-sieving" filtration mechanisms are forms of filtration in which the filter membrane retains suspended particles or dissolved materials contained in the fluid stream passing through the filter membrane in a non-mechanical manner, for example, an electrostatic mechanism that electrostatically attaches and retains particulate matter or dissolved impurities to the filter surface and removes them from the fluid stream, the particles may be dissolved or solid with a particle size smaller than the pores of the filter material.

[0006] Removal of ionic substances, such as dissolved anions or cations, from solutions is important in many industries, such as the microelectronics industry, where extremely low concentrations of ionic contaminants and particles can adversely affect the quality and performance of microprocessors and memory devices. The ability to make positive and negative photoresists with low levels of metal ion contaminants, or to deliver isopropyl alcohol used in Maragoni drying for wafer cleaning with low parts per billion or parts per trillion levels of metal ion contaminants, is highly desirable and are just two examples of the need for contamination prevention in semiconductor manufacturing. Colloidal particles, which can be positively or negatively charged depending on the chemistry of the colloid and the pH of the solution, can also contaminate processing fluids and need to be removed. Microporous filter membranes made of polymeric materials that attract dissolved ionic substances can remove the dissolved ionic materials by a non-sieving filtration mechanism. Examples of such microporous membranes are made from chemically inert low surface energy polymers such as ultra-high molecular weight polyethylene ("UPE"), polytetrafluoroethylene, and the like. Due to the ability of nylon to be formed into filter membranes that exhibit high permeability, and due to the excellent sieving and non-sieving filtration behavior of nylon, in particular, nylon filter membranes are used in a variety of different filtration applications in the semiconductor processing industry. Summary of the Invention

[0007] The field of microelectronic device processing requires steady improvements in processing materials and methods to sustain the parallel steady improvement in microelectronic device performance (e.g., speed and reliability). Opportunities exist to improve microelectronic device manufacturing in all aspects of the manufacturing process, including methods and systems for filtering liquid materials.

[0008] In microelectronic device fabrication, a wide variety of different liquid materials are used as process solvents, cleaning agents, and other processing solutions. Many, if not most, of these materials are used at extremely high levels of purity. As an example, the liquid materials (e.g., solvents) used in photolithographic processing of microelectronic devices must be of extremely high purity. Specific examples of liquids used in microelectronic device fabrication include spin-on-glass (SOG) technology, back surface antireflective coating (BARC) methods, and processing solutions for photolithography. Some of these liquid materials are acidic. In order to provide these liquid materials at a high level of purity for use in microelectronic device fabrication, the filtration system must be highly effective at removing various contaminants and impurities from the liquid and must be stable (i.e., do not decompose or introduce contaminants) in the presence of the liquid material (e.g., acidic material) being filtered.

[0009] In one embodiment, the composite porous filter membrane comprises: The membrane comprises a porous hydrophobic polymeric filter material having a coating thereon, the coating being a polyamide polymer that is soluble in formic acid; (i) surface energy greater than about 30 dynes / cm; (ii) Isopropanol flow rates of about 150 to about 20,000 seconds / 500 mL measured at 14.2 psi has.

[0010] The inventors believe that the polyamide coating formed on the surface of the porous hydrophobic polymeric filter material is a porous coating, thereby providing a substantially larger surface area to the polyamide coating surface. When a formic acid solution of the polyamide described herein is placed on a glass plate and the solvent is allowed to evaporate, the membrane thus formed is opaque, thus indicating that a porous membrane, rather than a non-porous membrane, is formed on the hydrophobic surface. This feature is therefore believed to provide improved non-sieving filtration performance.

[0011] In a second embodiment, a composite porous filter membrane comprises a porous hydrophobic polymeric filter membrane having coated thereon as a first coating a polyamide coating, said polyamide being soluble in formic acid, thereby providing a polyamide-coated membrane, said membrane having thereon a second coating that is the free radical reaction product of (i) at least one crosslinker and (ii) at least one monomer in the presence of a photoinitiator.

[0012] In another aspect, disclosed herein is a method for removing impurities from a liquid, the method comprising contacting the liquid with a composite membrane described herein.

[0013] The present disclosure may be more fully understood in consideration of the following description of various exemplary embodiments in conjunction with the accompanying drawings. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 (schematic and not necessarily to scale) illustrates one example of a filter product as described herein. [Diagram 2] 2 is a simplified diagram of a polyamide coated porous filter membrane, showing a base membrane (a hydrophobic polymeric filter membrane) onto which the polyamide is coated. As described below, the polyamide coating does not necessarily form a continuous coating on the base membrane as shown. [Diagram 3] Figure 3 is a graphical representation of the surface tension of mixtures of methanol and water at 20° C. The surface tension (nM / m at 20° C.) is plotted against the mass (%) of methanol in water. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] While the present disclosure is susceptible to various modifications and alternative forms, details of which have been shown by way of example in the drawings and will be described in detail. It should be understood, however, that the intention is not to limit aspects of the disclosure to the specific exemplary embodiments described. On the contrary, the intention is to cover all modifications, equivalents, and alternatives falling within the spirit and scope of the present disclosure.

[0016] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the content clearly dictates to the contrary. As used in this specification and the appended claims, the term "or" is generally used in its sense including "and / or" unless the content clearly dictates to the contrary.

[0017] The term "about" generally refers to a range of numbers that are considered equivalent to a stated value (e.g., having the same function or result). In many instances, the term "about" may include numbers that are rounded to the nearest significant figure.

[0018] Numerical ranges expressed using endpoints include all numbers subsumed within that range (eg, 1 to 5 includes 1, 1.5, 2, 2.75, 3, 3.80, 4, and 5).

[0019] As described above, in a first embodiment, the composite porous filter membrane comprises: The membrane comprises a porous hydrophobic polymeric filter material having a coating thereon, the coating being a polyamide polymer that is soluble in formic acid; i. a surface energy greater than about 30 dynes / cm; and ii. Isopropanol flow rate times of about 150 to about 20,000 seconds / 500 mL measured at 14.2 psi has.

[0020] In certain embodiments, the surface energy is from about 30 to about 100 dynes / cm, from about 30 to about 85 dynes / cm, or from about 30 to about 65 dynes / cm.

[0021] In some embodiments, the membrane has a bubble point of about 20 to 200 psi when measured using an HFE7200 at a temperature of about 22° C., and / or the membrane has a viscosity of between about 1 and about 10 μg / cm 2 Ponceau S dye binding capacity between about 1 and about 10 μg / cm 2 In one embodiment, the membrane has a methylene blue dye binding capacity (MB DBC) of between about 8 and about 10 μg / cm 2 in Ponceau S dye, and in another embodiment, the membrane has a binding capacity of about 9.2 μg / cm 2 Ponceau S dye-binding capacity of

[0022] In one embodiment, the flow rate of isopropanol is about 6,000 to about 10,000 seconds / 500 mL, and in another embodiment, about 8,000 seconds / 500 mL.

[0023] As mentioned above, the composite membranes described herein are useful as filtration media for removing impurities from various fluids. In some embodiments of the first and second aspects, the polyamide coating applied to the hydrophobic filter media or membrane does not completely cover or encapsulate the hydrophobic filter media or membrane, but rather forms a semi-continuous or partial coating on the underlying porous hydrophobic membrane. Similarly, in the second aspect where free radical polymerization is carried out in the presence of a polyamide-coated membrane, the resulting cured or crosslinked polymer coating, in some embodiments, does not completely cover or encapsulate the membrane surface, but also forms a semi-continuous or partial coating on the polyamide-coated porous hydrophobic membrane structure.

[0024] In some embodiments, the lower hydrophobic porous polymeric filter material is formed from a polymeric material, a mixture of different polymeric materials, or polymeric and non-polymeric materials. The polymeric materials forming the filter can be crosslinked together to provide a filter structure with a desired degree of integrity.

[0025] The polymeric material that can be used to form the lower porous filter membrane of the present disclosure is a hydrophobic polymer that in some embodiments has a surface energy of less than about 40 dynes / cm. In some embodiments, the filter hydrophobic polymer membrane comprises a polyolefin or a halogenated polymer. Exemplary polyolefins include polyethylene (PE), polypropylene (PP), polymethylpentene (PMP), polybutene (PB), polyisobutylene (PIB), and copolymers of two or more of ethylene, propylene, and butylene. In more specific embodiments, the filter material comprises ultra-high molecular weight polyethylene (UPE). UPE filter materials, such as UPE membranes, typically have a surface energy of about 1×10 6 More than daltons (Da), e.g., about 1 × 10 6 ~9×10 6 Da, or 1.5 × 10 6 ~9×10 6 It is formed from resins having molecular weights (viscosity average molecular weight) in the Da range. Crosslinking between polyolefin polymers such as polyethylene can be promoted by the use of heat or crosslinking chemicals such as peroxides (e.g., dicumyl peroxide or di-tert-butyl peroxide), silanes (e.g., trimethoxyvinylsilane) or azoester compounds (e.g., 2,2'-azo-bis(2-acetoxy-propane). Exemplary halogenated polymers include polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene (PCTFE), fluorinated ethylene polymers (FEP), polyhexafluoropropylene and polyvinylidene fluoride (PVDF).

[0026] In other embodiments, the filter material includes a polymer selected from polyimide, polysulfone, polyethersulfone, polyarylsulfone polyamide, polyacrylate, polyester, polyamideimide, cellulose, cellulose ester, polycarbonate, or combinations thereof.

[0027] In another embodiment, the lower hydrophobic porous filter membrane can be selected from commercially available hydrophobic membranes such as those prepared from ultra-high molecular weight polyethylene, polypropylene, polycarbonate, poly(tetrafluoroethylene), polyvinylidene fluoride, polyarylsulfone, and the like.

[0028] The composite membrane, starting from a porous hydrophobic filter membrane such as one composed of ultra-high molecular weight polyethylene, is treated with a solution of polyamide polymer in formic acid, for example. Once the membrane is coated, it is transferred to a mixing vessel containing an aqueous solution including water. The resulting membrane is then subjected to one or more washing steps including passing through washing vessels of aqueous and lower alcohols. Once dried, this process provides the composite membrane of the first aspect. In one embodiment, the washing steps include two successive vessels containing water and a vessel containing a lower, e.g. C1-C4 alcohol, between the two successive vessels of water.

[0029] Alternatively, in the second embodiment mentioned above, a composite membrane starting from a porous hydrophobic filter membrane, such as one made of ultra-high molecular weight polyethylene, is treated with a solution of polyamide polymer, for example in formic acid. Once the membrane is coated, it is transferred to a mixing vessel containing an aqueous solution comprising (i) at least one crosslinking agent, (ii) at least one monomer, and (iii) at least one photoinitiator, hereinafter referred to as "monomer solution". The membrane thus coated can then be subjected to UV light to initiate free radical polymerization at the surface of the polyamide coating with (i) at least one crosslinking agent and (ii) at least one monomer. The membrane obtained is then subjected to one or more washing steps, including passing through aqueous and lower alcohol washing vessels. Once dried, this process gives the composite membrane of the second embodiment.

[0030] In one embodiment, the composite membrane of this second aspect has the following properties: (i) isopropanol flow times of approximately 150–20,000 s / 500 mL, measured at 14.2 psi; (ii) has a bubble point of about 20 to 200 psi when measured using an ethoxy-nonafluorobutane HFE7200 at a temperature of about 22° C.; and (iii) Approximately 1 and 30 μg / cm 2 Ponceau S dye binding capacity between about 1 and 30 μg / cm 2 Methylene blue dye binding capacity (MB DBC) between has.

[0031] In certain embodiments, the surface energy is greater than 30 dynes / cm, between about 30 and 100 dynes / cm, or between about 30 and 85 dynes / cm, or between about 30 and 65 dynes / cm.

[0032] The polyamide polymers referred to above, also commonly known as "nylons", are typically understood to include copolymers and terpolymers that contain repeating amide groups in the polymer backbone. In general, nylon and polyamide resins include copolymers of diamines and dicarboxylic acids, or homopolymers of lactams and amino acids. In certain embodiments, nylons for use in the manufacture of the filter membranes described herein include copolymers of hexamethylenediamine and adipic acid (nylon 6,6), copolymers of hexamethylenediamine and sebacic acid (nylon 610), homopolymers of polycaprolactam (nylon 6), and copolymers of tetramethylenediamine and adipic acid (nylon 46). Nylon polymers are available in a wide range of grades that vary considerably in terms of molecular weight and in other properties, ranging from about 15,000 to about 42,000 (number average molecular weight). All such polyamides, as contemplated herein, are soluble in formic acid, but are generally insoluble in aqueous solutions. Such polyamides are utilized as dilute solutions in formic acid. In one embodiment, the polyamide is utilized at a concentration of about 1-4% by weight in formic acid.

[0033] The crosslinking agents are uncharged difunctional (i.e., having two carbon-carbon double bonds) vinyl, acrylic or methacrylic monomeric species, optionally with amide functionality. Non-limiting examples of such crosslinking agents include methylene bis(acrylamide), tetraethylene glycol diacrylate, tetraethylene glycol dimethacrylate, divinyl sulfone, divinylbenzene, 1,3,5-triallyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione 98%, and ethylene glycol divinyl ether.

[0034] The monomers referred to herein are of the vinyl, acrylic or methacrylic type, either charged or uncharged.

[0035] Non-limiting examples of positively charged monomers that can be used in embodiments of the present disclosure include 2-(dimethylamino)ethyl hydrochloride acrylate, [2-(acryloyloxy)ethyl]trimethylammonium chloride, 2-aminoethyl methacrylate hydrochloride, N-(3-aminopropyl)methacrylate hydrochloride, 2-(dimethylamino)ethyl methacrylate hydrochloride, [3-(methacryloylamino)propyl]trimethylammonium chloride solution, [2-(methacryloyloxy)ethyl ... Examples of monomers that may be used include, but are not limited to, acrylamidopropyl trimethylammonium chloride, 2-aminoethyl methacrylamide hydrochloride, N-(2-aminoethyl) methacrylamide hydrochloride, N-(3-aminopropyl) methacrylamide hydrochloride, diallyldimethylammonium chloride, allylamine hydrochloride, vinylimidazolium hydrochloride, vinylpyridinium hydrochloride, and vinylbenzyltrimethylammonium chloride. In certain embodiments, the positively charged monomer comprises acrylamidopropyl trimethylammonium chloride (APTAC). It should be understood that some of the positively charged monomers listed above contain quaternary ammonium groups and are naturally charged, whereas other positively charged monomers, such as those containing primary, secondary, and tertiary amines, are adjusted to generate a charge by treatment with an acid. Monomers that can be naturally or by treatment to be positively charged can be polymerized and crosslinked with a crosslinking agent to form a coating on the porous membrane.

[0036] Examples of negatively charged monomers that can be used include, but are not limited to, 2-ethylacrylic acid, acrylic acid, 2-carboxyethyl acrylate, 3-sulfopropyl acrylate potassium salt, 2-propylacrylic acid, 2-(trifluoromethyl)acrylic acid, methacrylic acid, 2-methyl-2-propene-1-sulfonic acid sodium salt, mono-2-(methacryloyloxy)ethyl maleate, 3-sulfopropyl methacrylate potassium salt, 2-acrylamido-2-methyl-1-propanesulfonic acid, 3-methacrylamidophenylboronic acid, vinylsulfonic acid, and vinylphosphonic acid, either individually or in combination of two or more of the following. In certain embodiments, the negatively charged monomer comprises a sulfonic acid moiety. It should be understood that some of the negatively charged monomers listed above contain strong acid groups and are naturally charged, while other negatively charged monomers, including weak acids, are adjusted to generate a charge by treatment with base. Monomers that are naturally or by process negatively charged can be polymerized and crosslinked with a crosslinking agent to form a coating on a porous membrane that is negatively charged in an organic solvent.

[0037] Examples of neutral monomers that can be used include, but are not limited to, acrylamide, N,N-dimethylacrylamide, N-(hydroxyethyl)acrylamide, diacetone acrylamide, N-[tris(hydroxymethyl)methyl]acrylamide, N-(isobutoxymethyl)acrylamide, N-(3-methoxypropyl)acrylamide, 7-[4-(trifluoromethyl)coumarin]acrylamide, N-isopropylacrylamide, 2-(dimethylamino)ethyl acrylate, 1,1,1,3,3,3-hexafluoroisopropyl acrylate, ethyl acrylate, 2-hydroxyethyl acrylate, butyl acrylate, ethylene glycol methyl ether acrylate, 4-hydroxybutyl acrylate, hydroxypropyl acrylate, 4-acetoxyphenethyl acrylate, benzyl acrylate, 1-vinyl-2-pyrrolidinone, vinyl acetate, ethyl vinyl ether, vinyl 4-tert-butylbenzoate, and phenyl vinyl sulfone.

[0038] In one embodiment, the photoinitiator is selected from those recognized as type I photoinitiators. Without wishing to be bound by theory, type I photoinitiators undergo unimolecular bond cleavage to generate free radicals when irradiated. Examples of suitable initiators include various persulfates such as sodium persulfate and potassium persulfate, 1-hydroxycyclohexyl phenyl ketone, (2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone) sold under the trademark Irgacure 2959, and benzoyl peroxide.

[0039] The amount of photoinitiator in the monomer solution can be any amount (i.e., concentration) high enough to affect the desired free radical reaction between the crosslinker and the monomer. Examples of useful amounts of photoinitiator in the monomer solution can range from up to 1 weight percent, such as from 0.1 or 0.5 to 4.5 weight percent, or from 1 or 2 to 3 or 4 weight percent.

[0040] The type of solvent used for the monomer solution can be any that is effective to allow the monomer solution to dissolve and deliver a useful amount of monomer to the surface of the hydrophilic polymer. A preferred solvent for the monomer solution is water or water with the addition of an organic solvent. The solvent can include an organic solvent, water, or both. Examples of organic solvents include alcohols, especially lower alcohols (e.g., C1-C6 alcohols), with isopropanol, methanol, and hexylene glycol being useful examples. The particular solvent used for a particular process, monomer solution, and monomer can be based on factors such as the type and amount of monomer in the monomer solution, the type of hydrophilic polymer, and other factors. In a solvent that contains both water and an organic solvent, the organic solvent can be included in any amount, for example, less than 90, 75, 50, 40, 30, 20, or 10% by weight. As an example, a useful solvent composition can contain 1-10% by weight hexylene glycol in water. In one embodiment, the water is deionized water.

[0041] The amount of monomer in the monomer solution, in one embodiment, is about 0.5-5 wt % based on the weight of the solution. The amount of crosslinker in the monomer solution, in one embodiment, is about 0.25-3.0 wt % based on the total weight of the monomer solution. In one embodiment, the relative amounts of monomer and crosslinker utilized, together with the relative coverage of such final crosslinked or free radical polymerized coating (on the polyamide coated hydrophobic membrane), are such that the overall, i.e., resulting membrane, has a surface energy of about 30-85 dynes / cm.

[0042] After the monomer solution has been effectively exposed or coated onto the polyamide-coated underlying porous hydrophobic membrane, the resulting membrane is exposed to electromagnetic radiation, typically in the ultraviolet portion of the spectrum, or another energy source effective to cause a photoinitiator to initiate a chemical reaction that causes the reactive moieties of the monomer to react with the crosslinker and chemically (covalently) bond to the crosslinker.

[0043] In various examples of the methods and articles described herein, the composite membrane described herein can be included in a porous filter membrane. As used herein, a "porous filter membrane" is a porous solid that contains porous (e.g., microporous) interconnected passages that extend from one surface of the membrane to the opposite surface of the membrane. The passages generally provide a tortuous tunnel or path through which the liquid being filtered must pass. Any particles contained in this liquid that are larger than the pores are prevented from entering the microporous membrane or are trapped within the pores of the microporous membrane (i.e., are removed by a sieving-type filtration mechanism) as the fluid containing these particles passes through the microporous membrane. Particles smaller than the pores can also be trapped or absorbed on the pore structure and removed, for example, by a non-sieving filtration mechanism. The liquid and possibly a reduced amount of particles or dissolved materials pass through the microporous membrane.

[0044] The exemplary porous polymeric filter membranes described herein (considered either before or after a surface coating step thereon) can be characterized by physical characteristics including pore size, bubble point, and porosity.

[0045] Porous polymeric filter membranes may have any pore size that allows the filter membrane to be effective to function as a filter membrane, including pores of a size (average pore size) that may be considered, for example, a microporous filter membrane or an ultrafilter membrane, as described herein. Examples of useful or preferred porous membranes may have an average pore size ranging from about 0.001 microns to about 1 or 2 microns, e.g., 0.01 to 0.8 microns, with the pore size being selected based on one or more factors including the particle size or type of impurity to be removed, the pressure and pressure drop requirements, and the viscosity requirements of the liquid being processed by the filter. Ultrafilter membranes may have an average pore size ranging from 0.001 microns to about 0.05 microns. Pore size is often reported as the average pore size of the porous material, which may be measured by known techniques such as mercury porosimetry (MP), scanning electron microscopy (SEM), liquid displacement (LLDP) or atomic force microscopy (AFM).

[0046] Bubble point is also a known characteristic of porous membranes. According to the bubble point test method, a sample of a porous polymeric filter membrane is immersed in a liquid having a known surface tension, wetted with a liquid having a known surface tension, and a gas pressure is applied to one side of the sample. The gas pressure is gradually increased. The minimum pressure at which gas will flow through the sample is called the bubble point. To determine the bubble point of a porous material, a sample of the porous material is immersed in ethoxy-nonafluorobutane HFE7200 (available from 3M) at a temperature of 20 to 25 degrees Celsius (e.g., 22 degrees Celsius) and wetted with ethoxy-nonafluorobutane HFE7200. Gas pressure is applied to one side of the sample by using compressed air, and the gas pressure is gradually increased. The minimum pressure at which gas will flow through the sample is called the bubble point. Examples of useful bubble points of porous polymeric filter membranes useful or preferred according to the present specification, measured using the procedure described above, can be in the range of 5 to 200 psi, for example, in the range of 20 to 200 psi.

[0047] The porous polymeric filter layer described can have any porosity that allows the porous polymeric filter layer to be effective as described herein.Exemplary porous polymeric filter layers can have relatively high porosity, for example, at least 60, 70 or 80% porosity.As used herein, and in the technical field of porous bodies, the "porosity" of a porous body (sometimes referred to as porosity) is a measure of the void (i.e., "empty") space within the porous body as a percentage of the total volume of the porous body, and is calculated as the ratio of the volume of the voids of the porous body to the total volume of the porous body.A porous body with a porosity of 0% is completely solid.

[0048] The described porous polymeric filter membranes can be in the form of sheets or hollow fibers having any useful thickness, for example, a thickness ranging from 5 to 100 microns, for example from 10 or 20 to 50 or 80 microns.

[0049] The described filter membranes can be useful for filtering liquids to remove undesirable materials (e.g., contaminants or impurities) from the liquid to produce a high purity liquid that can be used as a material in an industrial process. The filter membranes can be useful for removing dissolved or suspended contaminants or impurities from a liquid flowing through the coated filter membrane, either by sieving or non-sieving mechanisms, preferably by both combined non-sieving and sieving mechanisms. The lower porous hydrophobic filter membrane itself (before conversion to a composite hydrophobic filter membrane described herein) can exhibit effective sieving and non-sieving filtration properties, as well as desirable flow properties. The composite filter membranes described herein can exhibit at least equivalent sieving filtration properties, useful or equivalent (not excessively reduced) flow properties, and improved (e.g., substantially improved) non-sieving filtration properties, compared to the lower hydrophobic polymeric membrane utilized as a starting material.

[0050] The filter membranes herein may be useful in any type of industrial or life science process that requires high purity liquid materials as input. Non-limiting examples of such processes include processes for making microelectronic or semiconductor devices, a specific example of which is a method for filtering liquid processing materials (e.g., solvents or solvent-containing liquids) used for semiconductor photolithography. Examples of contaminants present in processing liquids or solvents used to make microelectronic or semiconductor devices may include metal ions dissolved in the liquid, solid particulate matter suspended in the liquid, and gelled or solidified materials present in the liquid (e.g., produced during photolithography).

[0051] Specific examples of the described filter membranes can be used to purify liquid chemicals used or useful in semiconductor or microelectronic manufacturing applications, for example, to filter liquid solvents or other process fluids used in semiconductor photolithography processes. Some specific non-limiting examples of solvents that can be filtered using the described filter membranes include n-butyl acetate (nBA), isopropyl alcohol (IPA), 2-ethoxyethyl acetate (2EEA), xylene, cyclohexanone, ethyl lactate, methyl isobutyl carbinol (MIBC), methyl isobutyl ketone (MIBK), isoamyl acetate, undecane, propylene glycol methyl ether (PGME) and propylene glycol monomethyl ether acetate (PGMEA), and a mixture of propylene glycol monomethyl ether (PGME) and PGMEA (7:3). The exemplary filter membranes described may be effective in removing metals from solvents containing water, amines, or both, such as bases and aqueous bases, such as NH4OH, tetramethylammonium hydroxide (TMAH), and equivalent solutions that may optionally contain water. In some embodiments, a liquid containing a solvent selected from tetramethylammonium hydroxide (TMAH) or NH4OH is passed through a filter having a membrane described herein to remove metals from the solvent. In some aspects, passing the solvent-containing liquid through the membrane to remove metals from the solvent-containing liquid results in a reduction in the concentration of metals in the solvent-containing liquid.

[0052] The composite filter membrane described herein can also be characterized with respect to the dye-binding capacity of the filter membrane. Specifically, charged dyes can be bound to the surface of the filter membrane. The amount of dye that can be bound to the filter membrane can be quantitatively measured by spectroscopy based on the difference in the measured absorption readings of the membrane at the absorption frequency of the dye. Dye-binding capacity can be evaluated by using negatively charged dyes and also by using positively charged dyes.

[0053] The composite filter membrane of the first aspect, in one embodiment, has a molecular weight of at least 1 microgram per square centimeter (μg / cm) of filter membrane. 2 ), e.g., greater than 1 or 10 μg / cm 2 Alternatively or additionally, the coated filter membranes described may have a dye binding capacity for methylene blue dye of about 1-10 μg / cm 2 , for example, greater than 1 to 10 or about 5 μg / cm 2 Dye-binding capacity for Ponceau S dye at 1 and 10 μg / cm 2 The antibody may have a methylene blue dye (MB DBC) binding capacity between 100 and 150 μg / ml.

[0054] The composite filter membrane of the second aspect, in one embodiment, has a molecular weight of at least 1 microgram per square centimeter (μg / cm) of filter membrane. 2 ), for example 1, 10, 100 or 500 μg / cm 2 Alternatively or additionally, the coated filter membranes described may have a dye binding capacity for methylene blue dye of at least 1 μg / cm 2 , for example, 1, 10, 100 or 500 μg / cm 2 The dye-binding capacity of the dye may be greater than 10000000000000.

[0055] Furthermore, the filter membrane as described can be characterized by the flow rate or flux of liquid flow through the filter membrane. The flow rate must be high enough to allow the filter membrane to be efficient and effective in filtering the flow of fluid through the filter membrane. The flow rate, or, alternatively, the resistance to liquid flow through the filter membrane, can be measured in terms of flow rate or flow time. The filter membranes described herein can have relatively low flow times and excellent filtration performance (e.g., as measured by particle retention, dye binding capacity, or both), preferably in combination with a relatively high bubble point. An example of a useful or preferred isopropanol flow time can be less than about 20,000 seconds / 500 mL, such as less than about 4,000 or 2,000 seconds / 500 mL.

[0056] The membrane isopropanol (IPA) flux time reported herein is 13.8 cm when 500 ml of isopropyl alcohol (IPA) fluid is pumped at 14.2 psi and a temperature of 21 degrees Celsius. 2 The time required for a substance to pass through a membrane having an effective surface area of ​​100 μm is determined.

[0057] In some embodiments, the composite membranes described herein can have flow times approximately equal to or greater than those of the same filter membrane that does not contain the polyamide coating and the co-reacted crosslinker / monomer coating. In other words, making a composite membrane from an underlying porous hydrophobic filter membrane does not have a substantial adverse effect on the flow properties of the filter membrane, and may even improve the filtration function of the filter membrane, particularly the non-sieving filtration function of the membrane, as measured, for example, by dye binding capacity, particle retention, or both, depending on the pore size.

[0058] The described filter membranes can be included in a larger filter structure, such as a multi-layer filter assembly or filter cartridge used in a filtration system. The filtration system places the filter membrane in a filter housing, for example as part of a multi-layer filter assembly or as part of a filter cartridge, to expose the filter membrane to the flow path of the liquid chemical so that at least a portion of the liquid chemical flow passes through the filter membrane, so that the filter membrane removes a certain amount of impurities or contaminants from the liquid chemical. The structure of the multi-layer filter assembly or filter cartridge can include one or more of various additional materials and structures that support the composite filter membrane in the filter assembly or filter cartridge to allow fluid to flow from the filter inlet through the composite membrane (including the filter layer) and through the filter outlet, thereby passing the composite filter membrane as it passes through the filter. The filter membrane supported by the filter assembly or filter cartridge can be any useful shape, such as a pleated cylinder, a cylindrical pad, one or more non-pleated (flat) cylindrical sheets, a pleated sheet, among others.

[0059] An example of a filter structure comprising a filter membrane in the form of a pleated cylinder can be made to include the following components: a rigid or semi-rigid core that supports the coated pleated cylindrical filter membrane at the inner opening of the coated pleated cylindrical filter membrane; a rigid or semi-rigid cage that supports or surrounds the outside of the coated pleated cylindrical filter membrane at the outside of the filter membrane; optional end pieces or "packs" located at each of the two opposite ends of the coated pleated cylindrical filter membrane; a filter housing that includes an inlet and an outlet, any of which may be included in the filter structure but may not be required. The filter housing can be of any useful desired size, shape and material, and can preferably be made from a suitable polymeric material.

[0060] The detailed description and drawings, which are not necessarily to scale, depict exemplary embodiments and are not intended to limit the scope of the embodiments described herein. The exemplary aspects shown are intended as examples only. Selected features of any exemplary aspect may be incorporated in additional aspects, unless expressly stated to the contrary.

[0061] As an example, FIG. 1 shows a filter component 30 produced from a pleated cylindrical component 10 and an end piece 22 along with other optional components. The cylindrical component 10 includes a filter membrane 12 and is pleated as described herein. The end piece 22 is attached (e.g., "stuffed") to one end of the cylindrical filter component 10. The end piece 22 can be preferably made of a melt-processable polymeric material. A core (not shown) can be disposed in the inner opening 24 of the pleated cylindrical component 10, and a cage (not shown) can be disposed around the outside of the pleated cylindrical component 10. A second end piece (not shown) can be attached ("stuffed") to a second end of the pleated cylindrical component 30. The resulting pleated cylindrical component 30 with two opposing stuffed ends and the optional core and cage can then be placed into a filter housing including an inlet and an outlet, configured such that all of the fluid entering the inlet must pass through the filter membrane 12 before exiting the filter at the outlet.

[0062] "Particle retention" or "coverage" refers to the percentage of the number of particles that can be removed from a fluid stream by a membrane placed in the fluid path of the fluid stream. Particle retention determined according to the following procedure is referred to as the "Particle Retention Test." An aqueous feed solution of 0.1% Triton X-100 with a pH of about 5 containing 8 ppb polystyrene particles with a diameter of 25 nm (available from Duke Scientific G25B) and 0.5 M NaCl is prepared. The particle retention of a 47 mm membrane disk can be measured by passing a sufficient amount of the aqueous feed solution to achieve a monolayer coverage of 1% through the membrane at a constant flow rate of 7 mL / min and collecting the filtrate. Particle retention can be determined for different monolayer percentages such as 0.5%, 1%, 2%, 3%, 4% or 5%. To accurately determine particle retention, the process is calibrated to determine the concentration of polystyrene particles in the feed stream that do not pass through the membrane. The concentration of polystyrene particles in the filtrate and feed stream can be calculated from the absorbance of the filtrate using a fluorescence spectrophotometer. Then, the following formula: Calculate particle retention using TIFF2024138302000002.tif15170.

[0063] The number (#) of particles required to achieve 1% monolayer coverage can be calculated from the following formula: TIFF2024138302000003.tif19170 ceremony a = effective membrane surface area (mm 2 ) d p = particle diameter (mm) n=% single layer

[0064] In some embodiments, the membranes disclosed herein have a particle retention as determined by a 1% Monolayer Particle Retention Test in the ranges of about 75% to about 100%, about 75% to about 99%, about 75% to about 95%, about 75% to about 90%, about 80% to about 100%, about 80% to about 99%, about 80% to about 95%, about 80% to about 90%, about 85% to about 100%, about 85% to about 99%, about 85% to about 95%, about 85% to about 90%, about 90% to about 100%, about 90% to about 99%, about 90% to about 95% and all ranges and subranges therebetween. In some embodiments, the membranes disclosed herein have a particle retention as determined by a 3% monolayer particle retention test in the ranges of about 70% to about 100%, about 70% to about 99%, about 70% to about 95%, about 70% to about 90%, about 75% to about 100%, about 75% to about 99%, about 75% to about 95%, about 75% to about 90%, about 80% to about 100%, about 80% to about 99%, about 80% to about 95%, about 80% to about 90%, about 85% to about 100%, about 85% to about 99%, about 85% to about 95%, about 85% to about 90%, about 90% to about 100%, about 90% to about 99%, about 90% to about 95% and all ranges and subranges therebetween. EXAMPLES

[0065] Porosity Measurement Bubble Point The porosimetry bubble point test method measures the pressure required to push air through the wetted pores of a membrane. The bubble point test is a well-known method for determining the pore size of a membrane. To determine the bubble point of a porous material, a sample of the porous material is immersed in ethoxy-nonafluorobutane HFE7200 (available from 3M) at a temperature of 20-25 degrees Celsius (e.g., 22 degrees Celsius) and wetted with ethoxy-nonafluorobutane HFE7200. Gas pressure is applied to one side of the sample by using compressed air, and the gas pressure is gradually increased. The minimum pressure at which gas will flow through the sample is called the bubble point.

[0066] As used herein, the "surface energy" (surface free energy) of a surface is considered to be equal to the surface tension of the highest surface tension liquid that wets the surface within 2 seconds of contact (see Example 3, Surface Energy Measurement) (also called the "Wetting Liquid Surface Tension" test or "Standard Liquid" test), and generally corresponds to the relative hydrophobicity / hydrophilicity of the surface. In some embodiments, the membrane has a surface energy of greater than about 30 dynes / centimeter, measured as the surface tension of the highest surface tension liquid that wets the surface within 2 seconds, as described in Example 3.

[0067] Example 1 - Preparation of asymmetric 5 nm UPE membrane coated with nylon 6 A coating solution of 3 wt% nylon 6 was prepared by dissolving 3 g of nylon 6 resin in 77 g of 98% formic acid and 20 g of isopropanol. A 47 mm disk of asymmetric 5 nm UPE membrane was wetted with the coating solution for 10 seconds. The membrane disk was removed from the nylon 6 solution and placed between two polyethylene sheets. Excess solution was removed from the membrane by rolling a rubber roller over the polyethylene sandwich laid flat on a table. The membrane disk was removed from the sandwich and immediately placed in a deionized water solution where it was immersed for 2 minutes to phase separate the nylon into the asymmetric 5 nm UPE membrane. The membrane disk was removed from the DI water solution and immediately immersed in a 100% methanol solution for 2 minutes. The membrane was restrained in a holder and placed in an oven set at 60°C for 10 minutes. Prior to coating with nylon 6, the asymmetric 5 nm UPE membrane had an HFE average bubble point of 112 psi, an IPA flow time of 4,234 sec / 500 mL, a thickness of 55 um and a viscosity of 0.0 ug / cm. 2 The resulting nylon 6 coated UPE membrane had an ethoxy-nonafluorobutane HFE7200 average bubble point of 114 psi, an IPA flow time of 5,264 sec / 500 mL, a thickness of 54 um and a dye binding capacity of 2.5 ug / cm 2 Ponceau S dye-binding capacity of 1000 mg / ml.

[0068] Example 2: Retention of Nylon 6-Coated UPE Membrane 47 mm discs of asymmetric 3 nm, 5 nm and 10 nm UPE membranes were coated with the 3 wt % nylon 6 solution described in Example 1. The particle retention test described above was then run on the coated and uncoated 3 nm, 5 nm and 10 nm UPE membranes, with the results shown in Table 1 below. Table 1 TIFF2024138302000004.tif57170

[0069] As can be seen from the table, coating of 3 nm, 5 nm and 10 nm UPE membranes improved particle retention at each monolayer percentage compared to uncoated 3 nm, 5 nm and 10 nm UPE membranes.

[0070] Example 2 - Preparation of an asymmetric 5 nm UPE film coated with nylon 6 and a UV-cured monomer coating A coating solution of 3 wt% nylon 6 was prepared by dissolving 3 g of nylon 6 resin in 77 g of 98% formic acid and 20 g of isopropanol. A 47 mm disk of asymmetric 5 nm UPE membrane was wetted with the coating solution for 10 seconds. The membrane disk was removed from the nylon 6 solution and placed between two polyethylene sheets. Excess solution was removed from the membrane by rolling a rubber roller over the polyethylene sandwich laid flat on a table. The membrane disk was removed from between the polyethylene sheets and immediately placed in a deionized water solution where it was immersed for 2 minutes to phase separate the nylon into an asymmetric 5 nm UPE membrane. The membrane disk was removed from the DI water solution and immediately immersed in a monomer solution containing 0.2% Irgacure 2959, 0.2% MBAM (N,N'-methylenebis(acrylamide)), 0.5% APTAC ((3-acrylamidopropyl)trimethylammonium chloride solution, available from Sigma-Aldrich), and 5% methanol. The membrane disk was removed from the monomer solution and placed between two polyethylene sheets. Excess solution was removed from the membrane by rolling a rubber roller over the polyethylene sandwich laid flat on a table. The polyethylene sandwich was then taped to a transport unit that carried the assembly through a Fusion Systems broadband UV exposure lab unit emitting at wavelengths from 200 nm to 600 nm. The time of exposure is controlled by how fast the assembly moves through the UV unit. In this example, the assembly moved through the UV chamber at 10 feet / minute. After UV exposure, the membrane disk was removed from between the polyethylene sandwich and immediately placed in a 100% methanol solution for 2 minutes. The membrane was restrained in a holder and placed in an oven set at 60°C for 10 minutes. Prior to coating with nylon 6, the asymmetric 5 nm UPE membrane had an ethoxy-nonafluorobutane HFE7200 average bubble point of 112 psi, an IPA flow time of 4,234 seconds / 500 mL, a thickness of 55 um and a viscosity of 0.0 ug / cm. 2The resulting nylon 6 coated and UV cured monomeric UPE membrane had an HFE average bubble point of 114 psi, an IPA flow time of 10,278 sec / 500 mL, a thickness of 53 um and a dye binding capacity of 6.5 ug / cm 2 Ponceau S dye-binding capacity of 1000 mg / ml.

[0071] Example 3 - Surface Energy Measurements A liquid will wet a porous polymer membrane if the surface tension of the liquid is less than the surface free energy of the membrane. In the present disclosure, a porous membrane is wetted by a liquid when the membrane is placed in contact with the liquid with the highest surface tension in a series of inert (standard) liquids, and the membrane spontaneously wicks the liquid within 2 seconds without the application of external pressure.

[0072] In a representative example, a series of inert (standard) liquids were prepared by mixing methanol and water in different mass ratios. The surface tensions of the resulting liquids are shown in Figure 3 (plotted using surface tension data published in Lange's Handbook of Chemistry 11th edition).

[0073] A 47 mm disk of membrane prepared according to Example 1 was placed in contact with the inert liquids in a beaker, one liquid at a time. For each liquid, the amount of time required for the membrane to spontaneously wick up the liquid was recorded. The liquids of 58% methanol with a surface tension of 30.32 mN / m and 22% methanol with a surface tension of 47.86 mN / m were the highest surface tension liquids that wetted the UPE and UPE coated membranes, respectively, within 2 seconds.

[0074] A 47 mm disk of membrane prepared according to Example 2 was placed in contact with the inert liquids in a beaker, one liquid at a time. For each liquid, the amount of time required for the membrane to spontaneously wick up the liquid was recorded. The liquids of 58% methanol with a surface tension of 30.32 mN / m and 16% methanol with a surface tension of 51.83 mN / m were the highest surface tension liquids that wetted the UPE and UPE coated membranes, respectively, within 2 seconds.

[0075] Example 4 - Reduction of metals in PGMEA with nylon film, asymmetric 5nm UPE film coated with nylon 6 and asymmetric 5nm UPE film coated with nylon 6 and UV cured monomer coating This example demonstrates the ability of 5 nm asymmetric UPE membranes coated with nylon 6 or nylon 6 and UV cured monomer to reduce metals in PGMEA during filtration. Metal reduction performance is compared to a nylon 6 membrane with a 5 nm pore size.

[0076] Using the same method as in Examples 1 and 2, nylon 6 coated UPE membranes were prepared and cut into 47 mm membrane strips. These membrane strips were conditioned and mounted in a clean 47 mm Filter Assembly (Savillex) by washing several times with 0.35% HCl followed by deionized water. The membrane and filter assembly were flushed with Isopropanol Gigabit (KMG) followed by PGMEA. As a control sample, a 5 nm nylon 6 membrane was also prepared and conditioned using the same method and mounted in a filter assembly. CONOSTAN Oil Analysis Standard S-21 (SCP Science) was added to the application solvent PGMEA at a target concentration of 13.59 ppb total metals. To determine the filtration metal removal efficiency, the application solvent spiked with metals was passed through the corresponding 47 mm filter assembly containing each filter at 10 mL / min and the filtrate was collected in a clean PFA jar at 50, 100 and 150 mL. ICP-MS was used to determine the metal concentrations in the applied solvent spiked with metals and each filtrate sample. The results are tabulated in Table 4.1: Metal Reduction in PGMEA. The results show that the 5 nm nylon 6 membrane can reduce total metals from 13.59 ppb to 4.79 ppb after 150 mL, the Asymmetric 5 nm UPE membrane coated with nylon 6 can reduce total metals from 13.59 ppb to 5.43 ppb after 150 mL, and the Asymmetric 5 nm UPE membrane coated with nylon 6 and a UV cured monomer coating can reduce total metals from 13.59 ppb to 3.26 ppb after 150 mL. Table 4.1: Metal reduction in PGMEA TIFF2024138302000005.tif123170

[0077] The results show that the nylon 6 coated UPE membranes generally have better metal removal than the nylon 6 control membrane, and that the nylon 6 and UV cured monomer coated UPE membranes have better metal removal than both the nylon 6 control membrane and the nylon 6 coated UPE membrane.

[0078] Aspects of the Disclosure In a first aspect, the present disclosure provides a composite porous filter membrane comprising: The membrane comprises a porous hydrophobic polymeric filter material having a coating thereon, the coating being a polyamide polymer that is soluble in formic acid; i. a surface energy greater than about 30 dynes / cm; and ii. Isopropanol flow rate times of about 150 to about 20,000 seconds / 500 mL measured at 14.2 psi The present invention provides a composite porous filter membrane having a

[0079] In a second aspect, the present disclosure provides a composite porous filter membrane comprising: The membrane comprises a porous hydrophobic polymeric filter material having a coating thereon, the coating being a polyamide polymer that is soluble in formic acid; i. a surface energy greater than about 30 dynes / cm; and ii. Particle retention in a 3% monolayer ranges from about 70% to about 100% The present invention provides a composite porous filter membrane having a

[0080] In a third aspect, the present disclosure provides a filter membrane of the first or second aspect, wherein the membrane has a 3% monolayer particle retention in the range of about 80% to about 100%.

[0081] In a fourth aspect, the present disclosure provides a filter membrane according to any of the first to third aspects, wherein said membrane has a bubble point of about 20 to about 200 psi when measured using ethoxy-nonafluorobutane HFE7200 at a temperature of about 22° C.

[0082] In a fifth aspect, the present disclosure provides a method for producing a membrane comprising the steps of: 2 Ponceau S dye binding capacity between about 1 and about 10 μg / cm 2The filter membrane of any of the first to fourth aspects is provided, having a methylene blue dye binding capacity (MB DBC) of between

[0083] In a sixth aspect, the present disclosure provides the filter membrane of any of the first to fifth aspects, wherein the hydrophobic polymeric filter material is selected from polyethylene, polypropylene, polycarbonate, poly(tetrafluoroethylene), polyvinylidene fluoride and polyarylsulfone.

[0084] In a seventh aspect, the present disclosure provides the filter membrane of any of the first to sixth aspects, wherein the hydrophobic polymeric filter material is selected from ultra-high molecular weight polyethylene and poly(tetrafluoroethylene).

[0085] In an eighth aspect, the present disclosure provides a filter membrane of any of the first to seventh aspects, having a surface energy of about 30 to about 100 dynes / cm.

[0086] In a ninth aspect, the present disclosure provides the filter membrane of any one of the first to eighth aspects, wherein the polyamide polymer is composed of at least one of: (i) a copolymer of hexamethylenediamine and adipic acid; (ii) a homopolymer of polycaprolactam; (iii) a copolymer of hexamethylenediamine and sebacic acid; and (iv) a copolymer of tetramethylenediamine and adipic acid.

[0087] In a tenth aspect, the present disclosure provides the filter membrane of any of the first to ninth aspects, wherein the polyamide polymer has a number average molecular weight of about 15,000 to about 42,000 daltons.

[0088] In an eleventh aspect, the present disclosure provides a method for producing a membrane comprising the steps of: (i) having a bubble point of about 50 to 150 psi when measured using ethoxy-nonafluorobutane HFE7200 at a temperature of about 22° C.; (ii) an isopropanol flow rate time of about 6,000 to about 10,000 seconds / 500 mL measured at 14.2 psi; and (iii) About 8 to about 10 μg / cm 2 Ponceau S dye binding capacity of 1 and 100 μg / cm 2 Methylene blue dye (MB DBC) binding capacity between A filter membrane according to any of the first to tenth aspects is provided.

[0089] In a twelfth aspect, the disclosure provides a composite porous filter membrane comprising a porous hydrophobic polymeric filter membrane having coated thereon as a first coating a polyamide coating, said polyamide being soluble in formic acid, thereby providing a polyamide-coated membrane, said polyamide-coated membrane having thereon a second coating that is the free radical reaction product of (i) at least one crosslinker and (ii) at least one monomer in the presence of a photoinitiator.

[0090] In a thirteenth aspect, the present disclosure provides the membrane of the twelfth aspect, wherein the hydrophobic polymeric filter material is selected from polyethylene, polypropylene, polycarbonate, poly(tetrafluoroethylene), polyvinylidene fluoride, and polyarylsulfone.

[0091] In a fourteenth aspect, the present disclosure provides the membrane of the twelfth or thirteenth aspect, wherein the membrane has a particle retention at 3% monolayer in the range of about 70% to about 100%, or in the range of about 80% to about 100%.

[0092] In a fifteenth aspect, the present disclosure provides a film of any one of the twelfth to fourteenth aspects, having a surface energy of about 30 to about 85 dynes / cm.

[0093] In a sixteenth aspect, the present disclosure provides the membrane of any of the twelfth to fifteenth aspects, wherein the hydrophobic polymeric filter material is selected from ultra-high molecular weight polyethylene and poly(tetrafluoroethylene).

[0094] In a seventeenth aspect, the present disclosure provides a method for producing a membrane comprising the steps of: (i) having an isopropanol flow rate time of about 150 to about 20,000 seconds / 500 mL, measured at 14.2 psi; (ii) having a bubble point of about 20 to about 200 psi when measured using an ethoxy-nonafluorobutane HFE7200 at a temperature of about 22° C.; and (iii) about 1 and about 30 μg / cm 2 Ponceau S dye binding capacity between about 1 and about 30 μg / cm 2 methylene blue dye binding capacity (MB DBC) between The membrane of any of the twelfth to seventeenth aspects is provided.

[0095] In an eighteenth aspect, the present disclosure provides the membrane of any one of the twelfth to seventeenth aspects, wherein the polyamide is composed of at least one of: (i) a copolymer of hexamethylenediamine and adipic acid; (ii) a homopolymer of polycaprolactam; (iii) a copolymer of hexamethylenediamine and sebacic acid; and (iv) a copolymer of tetramethylenediamine and adipic acid.

[0096] In a nineteenth aspect, the present disclosure provides the membrane of any one of the twelfth to nineteenth aspects, wherein the polyamide polymer has a number average molecular weight of about 15,000 to about 42,000 Daltons.

[0097] In a twentieth aspect, the present disclosure provides the membrane of any one of the twelfth to nineteenth aspects, wherein the crosslinker is selected from methylene bis(acrylamide), tetraethylene glycol diacrylate, tetraethylene glycol dimethacrylate, divinyl sulfone, divinyl benzene, 1,3,5-triallyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, and ethylene glycol divinyl ether.

[0098] In a twenty-first aspect, the present disclosure provides a process for the preparation of a methacrylic acid ester copolymer comprising the monomer selected from the group consisting of 2-(dimethylamino)ethyl hydrochloride acrylate, [2-(acryloyloxy)ethyl]trimethylammonium chloride, 2-aminoethyl methacrylate hydrochloride, N-(3-aminopropyl) methacrylate hydrochloride, 2-(dimethylamino)ethyl methacrylate hydrochloride, [3-(methacryloylamino)propyl]trimethylammonium chloride solution, [2-(methacryloyloxy)ethyl]trimethylammonium chloride, acrylamidopropyl trimethylammonium chloride, 2-aminoethyl methacrylamide hydrochloride, N-(2-aminoethyl) methacrylamide hydrochloride, N-(3-aminopropyl) methacrylamide hydrochloride, diallyldimethylammonium chloride, acrylamidopropyl tri ... and the like. The membrane of any one of the twelfth to twentieth aspects is selected from among vinylamine hydrochloride, vinylimidazolium hydrochloride, vinylpyridinium hydrochloride, vinylbenzyltrimethylammonium chloride and acrylamidopropyltrimethylammonium chloride, 2-ethylacrylic acid, acrylic acid, 2-carboxyethyl acrylate, 3-sulfopropyl acrylate potassium salt, 2-propylacrylic acid, 2-(trifluoromethyl)acrylic acid, methacrylic acid, 2-methyl-2-propene-1-sulfonic acid sodium salt, mono-2-(methacryloyloxy)ethyl maleate, 3-sulfopropyl methacrylate potassium salt, 2-acrylamido-2-methyl-1-propanesulfonic acid, 3-methacrylamidophenylboronic acid, vinylsulfonic acid, and vinylphosphonic acid.

[0099] In a twenty-second aspect, the present disclosure provides the membrane of any one of the twelfth to twenty-first aspects, wherein the monomer is selected from 2-ethylacrylic acid, acrylic acid, 2-carboxyethyl acrylate, 3-sulfopropyl acrylate potassium salt, 2-propylacrylic acid, 2-(trifluoromethyl)acrylic acid, methacrylic acid, 2-methyl-2-propene-1-sulfonic acid sodium salt, mono-2-(methacryloyloxy)ethyl maleate, 3-sulfopropyl methacrylate potassium salt, 2-acrylamido-2-methyl-1-propanesulfonic acid, 3-methacrylamidophenylboronic acid, vinylsulfonic acid, and vinylphosphonic acid.

[0100] In a twenty-third aspect, the present disclosure provides the membrane of any one of the twelfth to twenty-second aspects, wherein the monomer is selected from acrylamide, N,N-dimethylacrylamide, N-(hydroxyethyl)acrylamide, diacetone acrylamide, N-[tris(hydroxymethyl)methyl]acrylamide, N-(isobutoxymethyl)acrylamide, N-(3-methoxypropyl)acrylamide, 7-[4-(trifluoromethyl)coumarin]acrylamide, N-isopropylacrylamide, 2-(dimethylamino)ethyl acrylate, 1,1,1,3,3,3-hexafluoroisopropyl acrylate, ethyl acrylate, 2-hydroxyethyl acrylate, butyl acrylate, ethylene glycol methyl ether acrylate, 4-hydroxybutyl acrylate, hydroxypropyl acrylate, 4-acetoxyphenethyl acrylate, benzyl acrylate, 1-vinyl-2-pyrrolidinone, vinyl acetate, ethyl vinyl ether, vinyl 4-tert-butylbenzoate, and phenyl vinyl sulfone.

[0101] In a twenty-fourth aspect, the present disclosure provides a method for preparing a composite porous filter membrane of any one of the first to ninth aspects, comprising: a. dissolving a polyamide polymer in formic acid to form a polyamide solution; b. contacting a porous hydrophobic polymeric filter material with the polyamide solution to provide a polyamide-coated membrane; c. immersing the polyamide coated membrane in a solution comprising water; d. rinsing the polyamide coated membrane with C1-C4 alcohols and water; e. drying the polyamide coated membrane; The present invention provides a method comprising:

[0102] In a twenty-fifth aspect, the present disclosure provides a method for preparing a composite porous filter membrane of any one of the tenth to twentieth aspects, comprising: a. dissolving a hydrophilic polyamide polymer in formic acid to form a polyamide solution; b. contacting a porous hydrophobic polymeric filter material with the polyamide solution to provide a polyamide-coated membrane; c. immersing the polyamide coated membrane in a monomer solution comprising water, at least one crosslinker, at least one monomer, and at least one photoinitiator; d. removing the resulting film from the bath and exposing it to ultraviolet radiation; and then e. rinsing the polyamide-coated membrane in a rinse bath comprising a solvent selected from water and C1-C4 alcohols; f. drying the composite porous filter membrane; The present invention provides a method comprising:

[0103] In a twenty-sixth aspect, the present disclosure provides a method for removing impurities from a liquid, the method comprising contacting the liquid with a composite membrane of any one of the first to nineteenth aspects.

[0104] In a twenty-seventh aspect, the present disclosure provides the method of the twenty-sixth aspect, wherein the impurities are selected from one or more metal or metalloid ions.

[0105] In a twenty-eighth aspect, the present disclosure provides the method of the twenty-seventh aspect, wherein the impurities are selected from one or more ions of lithium, boron, sodium, magnesium, aluminum, potassium, calcium, titanium, vanadium, chromium, manganese, iron, nickel, copper, zinc, molybdenum, silver, cadmium, tin, barium, and lead.

[0106] In a twenty-ninth aspect, the present disclosure provides a filter comprising the membrane of any one of the first to eleventh aspects.

[0107] In a thirtieth aspect, the present disclosure provides a filter comprising the membrane of any one of the twelfth to twenty-third aspects.

[0108] Having thus described some exemplary aspects of the present disclosure, those skilled in the art will readily appreciate that still other aspects may be made and used within the scope of the claims appended hereto. Many advantages of the present disclosure covered by this document have been set forth in the foregoing description. It will be understood, however, that the present disclosure is in many respects merely illustrative. Changes may be made in detail without departing from the scope of the present disclosure. The scope of the present disclosure is, of course, to be defined in the language in which the appended claims are expressed.

Claims

1. 1. A composite porous filter membrane comprising: The membrane comprises a porous hydrophobic polymeric filter material having a coating thereon, the coating being a polyamide polymer that is soluble in formic acid; i. a surface energy greater than about 30 dynes / cm; and ii. An isopropanol flow time of about 150 to about 20,000 seconds / 500 mL measured at 14.2 psi A composite porous filter membrane comprising:

2. 10. The membrane of claim 1, wherein the membrane has a particle retention at 3% monolayer in the range of about 70% to about 100%.

3. 3. The membrane of claim 2, wherein the membrane has a particle retention at 3% monolayer in the range of about 80% to about 100%.

4. 4. The membrane of any one of claims 1 to 3, wherein the membrane has a bubble point of about 20 to about 200 psi when measured using ethoxy-nonafluorobutane HFE 7200 at a temperature of about 22°C.

5. The membrane is between about 1 and about 10 μg / cm 2 Ponceau S dye binding capacity between about 1 and about 10 μg / cm 2 5. The membrane of claim 1 having a methylene blue dye binding capacity (MB DBC) of between 0.1 and 0.

25.

6. 6. The membrane of any one of claims 1 to 5, wherein the hydrophobic polymeric filter material is selected from polyethylene, polypropylene, polycarbonate, poly(tetrafluoroethylene), polyvinylidene fluoride and polyarylsulfone.

7. 7. The membrane of any one of claims 1 to 6, wherein the hydrophobic polymeric filter material is selected from ultra-high molecular weight polyethylene and poly(tetrafluoroethylene).

8. The film of any one of claims 1 to 7, having a surface energy of about 30 to about 100 dynes / cm.

9. 9. The membrane of any one of claims 1 to 8, wherein the polyamide polymer is comprised of at least one of: (i) a copolymer of hexamethylenediamine and adipic acid; (ii) a homopolymer of polycaprolactam; (iii) a copolymer of hexamethylenediamine and sebacic acid; and (iv) a copolymer of tetramethylenediamine and adipic acid.

10. 10. The membrane of any one of claims 1 to 9, wherein the polyamide polymer has a number average molecular weight of about 15,000 to about 42,000 Daltons.

11. The membrane, (i) a bubble point of about 50 to about 150 psi, as measured using an ethoxy-nonafluorobutane HFE 7200 at a temperature of about 22° C.; (ii) an isopropanol flow time of about 6,000 to about 10,000 seconds / 500 mL measured at 14.2 psi; and (iii) about 8 to about 10 μg / cm 2 and the Ponceau S dye binding capacity of 1 and 100 μg / cm 2 Methylene blue dye (MBDBC) binding capacity between The membrane according to any one of claims 1 to 10, having

12. 1. A composite porous filter membrane comprising a porous hydrophobic polymeric filter membrane having coated thereon as a first coating a polyamide coating, said polyamide being soluble in formic acid, thereby providing a polyamide-coated membrane, said polyamide-coated membrane having thereon a second coating which is the free radical reaction product of (i) at least one crosslinker and (ii) at least one monomer in the presence of a photoinitiator.

13. 13. The membrane of claim 12, wherein the hydrophobic polymeric filter material is selected from polyethylene, polypropylene, polycarbonate, poly(tetrafluoroethylene), polyvinylidene fluoride, and polyarylsulfone.

14. The film of claim 12 or 13, having a surface energy of about 30 to about 85 dynes / cm.

15. 15. The membrane of any one of claims 12 to 14, wherein the membrane has a particle retention at 3% monolayer in the range of about 70% to about 100%.

16. 16. The membrane of claim 15, wherein the membrane has a particle retention at 3% monolayer in the range of about 80% to about 100%.

17. 17. The membrane of any one of claims 12 to 16, wherein the hydrophobic polymeric filter material is selected from ultra-high molecular weight polyethylene and poly(tetrafluoroethylene).

18. The membrane, (i) having an isopropanol flow time of about 150 to about 20,000 seconds / 500 mL, measured at 14.2 psi; (ii) having a bubble point of about 20 to about 200 psi when measured using an ethoxy-nonafluorobutane HFE 7200 at a temperature of about 22° C.; and (iii) between about 1 and about 30 μg / cm 2 Ponceau S dye binding capacity between about 1 and about 30 μg / cm 2 having a methylene blue dye binding capacity (MB DBC) of between 18. A membrane according to any one of claims 12 to 17.

19. 19. The membrane of any one of claims 12 to 18, wherein the polyamide is comprised of at least one of: (i) a copolymer of hexamethylenediamine and adipic acid; (ii) a homopolymer of polycaprolactam; (iii) a copolymer of hexamethylenediamine and sebacic acid; and (iv) a copolymer of tetramethylenediamine and adipic acid.

20. 20. The membrane of any one of claims 12 to 19, wherein the hydrophilic polyamide polymer has a number average molecular weight of about 15,000 to about 42,000 Daltons.

21. 21. The membrane according to any one of claims 12 to 20, wherein the crosslinking agent is selected from methylene bis(acrylamide), tetraethylene glycol diacrylate, tetraethylene glycol dimethacrylate, divinyl sulfone, divinyl benzene, 1,3,5-triallyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione and ethylene glycol divinyl ether.

22. The monomer is 2-(dimethylamino)ethyl hydrochloride acrylate, [2-(acryloyloxy)ethyl]trimethylammonium chloride, 2-aminoethyl methacrylate hydrochloride, N-(3-aminopropyl)methacrylate hydrochloride, 2-(dimethylamino)ethyl methacrylate hydrochloride, [3-(methacryloylamino)propyl]trimethylammonium chloride solution, [2-(methacryloyloxy)ethyl]trimethylammonium chloride, acrylamidopropyltrimethylammonium chloride, 2-aminoethyl methacrylamide hydrochloride, N-(2-aminoethyl)methacrylamide hydrochloride, N-(3-aminopropyl)methacrylamide hydrochloride, diallyldimethylammonium chloride, allylamine hydrochloride 22. The membrane according to any one of claims 12 to 21, wherein the acrylic acid is selected from the group consisting of acrylic acid, vinylimidazolium hydrochloride, vinylpyridinium hydrochloride, vinylbenzyltrimethylammonium chloride and acrylamidopropyltrimethylammonium chloride, 2-ethylacrylic acid, acrylic acid, 2-carboxyethyl acrylate, 3-sulfopropyl acrylate potassium salt, 2-propylacrylic acid, 2-(trifluoromethyl)acrylic acid, methacrylic acid, 2-methyl-2-propene-1-sulfonic acid sodium salt, mono-2-(methacryloyloxy)ethyl maleate, 3-sulfopropyl methacrylate potassium salt, 2-acrylamido-2-methyl-1-propanesulfonic acid, 3-methacrylamidophenylboronic acid, vinylsulfonic acid and vinylphosphonic acid.

23. 23. The membrane of any one of claims 12 to 22, wherein the monomer is selected from 2-ethylacrylic acid, acrylic acid, 2-carboxyethyl acrylate, 3-sulfopropyl acrylate potassium salt, 2-propylacrylic acid, 2-(trifluoromethyl)acrylic acid, methacrylic acid, 2-methyl-2-propene-1-sulfonic acid sodium salt, mono-2-(methacryloyloxy)ethyl maleate, 3-sulfopropyl methacrylate potassium salt, 2-acrylamido-2-methyl-1-propanesulfonic acid, 3-methacrylamidophenylboronic acid, vinylsulfonic acid and vinylphosphonic acid.

24. 24. The membrane of any one of claims 12 to 23, wherein the monomer is selected from acrylamide, N,N-dimethylacrylamide, N-(hydroxyethyl)acrylamide, diacetoneacrylamide, N-[tris(hydroxymethyl)methyl]acrylamide, N-(isobutoxymethyl)acrylamide, N-(3-methoxypropyl)acrylamide, 7-[4-(trifluoromethyl)coumarin]acrylamide, N-isopropylacrylamide, 2-(dimethylamino)ethyl acrylate, 1,1,1,3,3,3-hexafluoroisopropyl acrylate, ethyl acrylate, 2-hydroxyethyl acrylate, butyl acrylate, ethylene glycol methyl ether acrylate, 4-hydroxybutyl acrylate, hydroxypropyl acrylate, 4-acetoxyphenethyl acrylate, benzyl acrylate, 1-vinyl-2-pyrrolidinone, vinyl acetate, ethyl vinyl ether, vinyl 4-tert-butyl benzoate and phenyl vinyl sulfone.

25. 1. A composite porous filter membrane comprising: The membrane comprises a porous hydrophobic polymeric filter material having a coating thereon, the coating being a polyamide polymer that is soluble in formic acid; A surface energy greater than about 30 dynes / cm; and Particle retention in a 3% monolayer ranges from about 70% to about 100% A composite porous filter membrane comprising:

26. 26. The membrane of claim 25, wherein the membrane has a particle retention at 3% monolayer in the range of about 80% to about 100%.

27. 27. The membrane of claim 25 or 26, wherein the membrane has a bubble point of about 20 to about 200 psi when measured using ethoxy-nonafluorobutane HFE 7200 at a temperature of about 22°C.

28. The membrane is between about 1 and about 10 μg / cm 2 Ponceau S dye binding capacity between about 1 and about 10 μg / cm 2 28. The membrane of any one of claims 25 to 27, having a methylene blue dye binding capacity (MB DBC) of between.

29. 29. The membrane of any one of claims 25 to 28, wherein the hydrophobic polymeric filter material is selected from polyethylene, polypropylene, polycarbonate, poly(tetrafluoroethylene), polyvinylidene fluoride and polyarylsulfone.

30. 30. The membrane of any one of claims 25 to 29, wherein the hydrophobic polymeric filter material is selected from ultra-high molecular weight polyethylene and poly(tetrafluoroethylene).

31. The film of any one of claims 25 to 30, having a surface energy of about 30 to about 100 dynes / cm.

32. 32. The membrane of any one of claims 25 to 31, wherein the polyamide polymer is comprised of at least one of: (i) a copolymer of hexamethylenediamine and adipic acid; (ii) a homopolymer of polycaprolactam; (iii) a copolymer of hexamethylenediamine and sebacic acid; and (iv) a copolymer of tetramethylenediamine and adipic acid.

33. 33. The membrane of any one of claims 25 to 32, wherein the polyamide polymer has a number average molecular weight of about 15,000 to about 42,000 Daltons.

34. The membrane, (iv) a bubble point of about 50 to about 150 psi, as measured using an ethoxy-nonafluorobutane HFE 7200 at a temperature of about 22° C.; (v) an isopropanol flow time of about 6,000 to about 10,000 seconds / 500 mL measured at 14.2 psi; and (vi) About 8 to about 10 μg / cm 2 and the Ponceau S dye binding capacity of 1 and 100 μg / cm 2 Methylene blue dye (MBDBC) binding capacity between 34. The membrane of any one of claims 25 to 33, having

35. A method for preparing a composite porous filter membrane according to any one of claims 1 to 11 or 25 to 34, comprising the steps of: a. dissolving a polyamide polymer in formic acid to form a polyamide solution; b. contacting a porous hydrophobic polymeric filter material with the polyamide solution to provide a polyamide-coated membrane; c. immersing the polyamide coated membrane in a solution comprising water; d.C 1 ~C 4 rinsing the polyamide coated membrane with alcohol and water; e. drying the polyamide coated membrane; A method comprising:

36. 25. A method for preparing a composite porous filter membrane according to any one of claims 12 to 24, comprising the steps of: a. dissolving a hydrophilic polyamide polymer in formic acid to form a polyamide solution; b. contacting a porous hydrophobic polymeric filter material with the polyamide solution to provide a polyamide-coated membrane; c. immersing the polyamide coated membrane in a monomer solution comprising water, at least one crosslinking agent, at least one monomer, and at least one photoinitiator; d. removing the resulting film from the bath and applying ultraviolet radiation, followed by e. Water and C 1 ~C 4 rinsing the polyamide coated membrane in a rinse bath comprising a solvent selected from an alcohol; f. drying the composite porous filter membrane; A method comprising:

37. 35. A method for removing impurities from a liquid comprising contacting the liquid with the composite membrane of any one of claims 1 to 34.

38. 38. The method of claim 37, wherein the impurities are selected from one or more metal or metalloid ions.

39. 39. The method of claim 38, wherein the impurities are selected from one or more ions of lithium, boron, sodium, magnesium, aluminum, potassium, calcium, titanium, vanadium, chromium, manganese, iron, nickel, copper, zinc, molybdenum, silver, cadmium, tin, barium, and lead.

40. A filter comprising a membrane according to any one of claims 1 to 34.

Citation Information

Patent Citations

  • Porous hollow yarn membrane

    JP1986283305A

  • Conjugated fiber and multi-slit fiber

    JP2008007902A

  • Composite material comprising a multilayer hydrophilic coating layer

    JP2008520403A

  • Highly retentive polyamide hollow fiber membranes produced by controlled shrinkage

    JP2019526431A

  • Polyamide coated filter membrane, filters, and methods

    WO2019212707A1