Polymer foam articles and methods of making polymer foams
The method of forming a molten pneumatic mixture in an extruder with controlled pressure reduction and expansion ensures a continuous polymer matrix in large or thick foam articles, addressing structural integrity issues in conventional foam production.
Patent Information
- Application Number
- JP2024111247
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-06-27
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-06-29
AI Technical Summary
Conventional methods for producing large or thick polymer foam articles fail to maintain a continuous foam structure due to cooling gradients that cause polymer coalescence and void formation, compromising structural integrity.
A method involving the formation of a molten pneumatic mixture in an extruder, followed by pressure reduction and expansion within a collection region to allow foaming, then dispensing and cooling the molten polymer foam to maintain a continuous polymer matrix throughout the article.
The method produces polymer foam articles with a continuous polymer matrix and dispersed foams, achieving structural integrity in large or thick articles without coalescence, enabling density reduction and improved strength.
Smart Images

Figure 2024138431000001_ABST
Abstract
Description
[Background technology]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to U.S. Provisional Patent Application No. 62 / 867,516, entitled "Method for Molten Foam Injection Molding of Foamed Parts," filed June 27, 2019. U.S. Provisional Patent Application No. 62 / 867,516 is hereby incorporated by reference in its entirety as if fully set forth herein.
[0002] Foamed polymer articles have been widely adopted in industry due to the highly desirable attributes of providing the high strength associated with solid polymer articles while also providing a reduction in density and therefore the amount of polymer used to form an article of a selected volume. In addition, the industry enjoys the advantages provided by the reduction in weight of a foamed article compared to its solid counterpart, while still obtaining the advantages of strength, toughness, impact resistance, etc. provided by the polymer itself.
[0003] The industry has therefore developed several now standard methods for entraining gas into thermoplastic polymers and creating such foam articles. To mold foamed thermoplastic polymer articles using gas, commercial guidelines and industry practices employ melt mixing equipment operable to maintain pressure within the interior of the equipment to limit the expansion of the gas while melt mixing the gas or source of gas with the thermoplastic polymer, and also at a temperature above the melting temperature of the thermoplastic polymer. Such processes and equipment are designed to minimize the formation of foam, i.e. pockets of gas, that would otherwise be formed by the expansion of the gas within the molten thermoplastic polymer. Thus, while residing within and disposed within the melt mixing equipment, the thermoplastic polymer may be foam-free or substantially foam-free, including the source of gas or the gas itself dissolved or dispersed therein. A foam-free or substantially foam-free mixture of molten thermoplastic polymer and gas at or above a temperature that would form foam at atmospheric pressure may be referred to as melt pneumatic mixing. The temperature at which the gas, i.e., the physical blowing agent, will form a foam upon melt-pneumatic mixing at atmospheric pressure may be referred to as the critical temperature. Melt mixing equipment known in the art is therefore designed and adapted to create and dispense the melt-pneumatic mixture. Furthermore, such equipment is suitable for creating the melt-pneumatic mixture by adding a nascent, latent, or latent gas that is released at a characteristic temperature or formed at a characteristic temperature by an exothermic or endothermic chemical reaction. The critical temperature of the nascent, latent, or latent gas is the temperature at which the reaction occurs or the gas is released into the thermoplastic polymer. All such materials and processes are widely understood, and melt mixing equipment of various designs is widely commercially available for this purpose. The melt mixing equipment commonly employed is a single-screw or twin-screw extruder having a pressurized chamber at the distal end of the screw and modified to receive a set amount, or "shot," of melt-pneumatic mixture that proceeds while mixing and forcing the molten pneumatic mixture towards the pressurized chamber by the action of the screw.
[0004] In response to building up a set amount, or shot, in the pressurized chamber, the molten pneumatic mixture is dispensed from the melt mixing device and directed by fluidly connected tubes, pipes, etc. into the cavity of the mold, where it acquires the desired shape. Dispensing is generally performed to maximize the amount of foaming (foam formation) that occurs in the mold cavity by the release of pressure while the thermoplastic polymer is still molten. The expanded foam in the cavity is then cooled, resulting in a foamed article. Foam parts molded using this methodology are referred to in the art as injection molded foam parts. This technique is generally limited in range to making parts having a thickness of about 2 cm or less.
[0005] The injection molding process, which employs a physical blowing agent source to induce a foam structure in the molded parts, can be understood from a recent peer-reviewed journal article by Bociaga et al., “The influence of foaming agent addition, talc filler content, and injection velocity on selected properties, surface state, and structure of polypropylene injection molded parts.” Cellular Polymers 2020,39(1)3-30. In this publication, process conditions typically employed to mold standard injection molded ISO test specimens of 4.1 mm thickness were systematically varied to generate 16 different combinations of process settings and formulation variables (physical blowing agent source concentration, filler content, injection rate, injection time, hold time, and hold pressure). The authors teach that while manipulating the process and formulation will produce some variation in foam structure in the resulting foam part, not all variables will produce a part that has a "skin," a term in the art to describe a very characteristic region near the surface of an injection molded foam article that is free or substantially free of bubbles.
[0006] Inspection of the surface of an injection molded foam article and an area extending in any direction approximately 500 microns beneath the surface will reveal solid thermoplastic regions, i.e., the regions are free of or substantially free of foam. Foam parts resulting from injection molding according to conventional injection molding processes include skin layer characteristics. In addition, the skin layer of most such parts is significantly thicker than 500 μm and may be 1 mm, 2 mm, 3 mm, or even thicker depending on the method, equipment, and materials employed.
[0007] For making large foam parts (such as pallets or wheelbarrow bodies), the conventional processes described above are inadequate because large mold cavities induce excessive pressure drop as the molten pneumatic mixture flows and expands during mold filling, and foam may form but then coalesce or escape from the viscous polymer flow during filling. Thus, in some cases of "structural foam" molding, multiple nozzles are used simultaneously to rapidly fill large or thick mold cavities. In other cases, significant back pressure may be applied in the mold cavity to prevent foam formation during filling. That is, release of pressure after filling the mold acts to substantially allow foam formation within the mold cavity. Both approaches are often used in a single process.
[0008] However, the aforementioned structural foam molding process does not effectively solve the problems that have prevented the industry from making significant advances. As is widely understood, areas near the surface of a molten mass cool more rapidly than its interior, and a cooling gradient of temperature develops within the mass. The cooling rate at the deepest point within the mass is the slowest. In terms of a large mold cavity filled with a mass of molten polymer or pneumatic mixture, the interior regions of the mass may cool slowly such that the viscous flow of the thermoplastic allows the foam to coalesce, forming large polymer-free pockets and disrupting the intended continuous polymer matrix that defines such a foam. This effect may be exacerbated by the shrinkage of the polymer volume as it cools below its melt transition. For large foam parts, this effect may even lead to a complete collapse of the foam structure within the interior of the part.
[0009] The combined strength and density reduction associated with foamed articles cannot be achieved without a continuous polymer matrix throughout the entire part. Foamed parts with large polymer-free areas or voids compromise the structural integrity of the part, which makes such parts unsuitable for their intended use. These serious technical problems limit the industrial use of polymer foams to many otherwise very useful and beneficial applications. Thus, there is a continuing need to provide improved methods for making foamed articles, particularly large or thick foamed articles. There is a continuing need to obtain parts with a continuous foam structure throughout. There is a particular need to obtain parts with a thickness greater than 2 cm and with a continuous foam structure throughout. There is a continuing need in the industry to address such needs using conventional equipment and materials. Summary of the Invention [Means for solving the problem]
[0010] Described herein is a method of making a molten polymer foam. The method includes the steps of adding a thermoplastic polymer and a physical blowing agent source to an extruder, heating and mixing the thermoplastic polymer and the physical blowing agent source under pressure in the extruder to form a melt pneumatic mixture, where the temperature of the melt pneumatic mixture exceeds a critical temperature of the physical blowing agent source, collecting a quantity of the melt pneumatic mixture in a collection area of the extruder, defining an expansion volume in the collection area and allowing pressure to drop in the collection area, allowing an expansion time period to elapse after the definition, and dispensing the molten polymer foam from the collection area. In an embodiment, the expansion volume is selected to provide 10% to 300% of the total expected molten foam volume in the collection area. In an embodiment, the expansion period is 5 seconds to 600 seconds. In an embodiment, the melt pneumatic mixing is uninterrupted or substantially uninterrupted during the expansion period.
[0011] In embodiments, the dispensing is dispensing into a forming element, which in some embodiments is a die. In embodiments, there is a fluid connection between a collection area of the extruder and the die. In embodiments, the dispensing is an uninterrupted flow of the molten polymer foam. In embodiments, the dispensing is a linear flow of the molten polymer foam.
[0012] In an embodiment, the method further comprises cooling the dispensed molten polymer foam to a temperature below the melt transition temperature of the thermoplastic polymer. In an embodiment, the method further comprises adding one or more additional materials to the extruder, the one or more materials being selected from colorants, stabilizers, gloss agents, nucleating agents, fibers, particulates, and fillers. In an embodiment, the physical blowing agent source is a physical blowing agent and the addition is a pressurized addition. In another embodiment, the physical blowing agent source comprises a bicarbonate, a polycarboxylic acid or a salt or ester thereof, or a mixture thereof.
[0013] Also disclosed herein are polymeric foam articles made using the methods, materials, and apparatus described herein. In embodiments, the polymeric foam article has a foam structure throughout that is characterized as a continuous polymer matrix defining a plurality of bubbles therein. In embodiments, the surface region of the polymeric foam article comprises compressed bubbles. In embodiments, the surface region is an area that extends 500 microns from the surface of the article.
[0014] Also disclosed herein is a thermoplastic polymer foam article, the article having a foam structure throughout that is a continuous polymer matrix defining a plurality of bubbles therein, and further, a surface region of the article comprises compressed bubbles. In some embodiments, the surface region is a region of the article that extends 500 microns from its surface. In some embodiments, the article comprises compressed bubbles greater than 500 microns from its surface. In embodiments, the polymer foam article comprises a thickness greater than 2 cm, and in other embodiments, the polymer foam article comprises a thickness greater than 1,000 cm. 3 Exceeding 1,000cm 3 ~5,000cm 3 , or an additional 5,000 cm 3 and in yet other embodiments, the polymeric foam article has a volume greater than 1,000 cm 3 Volume greater than 2cm and thickness greater than 1,000cm 3 and ~5,000 cm 3 and a thickness of more than 2 cm, or 5,000 cm 3 and a thickness of more than 2 cm.
[0015] In embodiments, materials used to make polymeric foam articles include thermoplastic polymers selected from, but not limited to, polyolefins, polyamides, polyimides, polyesters, polycarbonates, poly(lactic acid), acrylonitrile-butadiene-styrene copolymers, polystyrene, polyurethanes, polyvinyl chloride, tetrafluoroethylene, polyethersulfones, polyacetals, polyaramids, polyphenylene oxides, polybutylenes, polybutadienes, polyacrylates, and methacrylate copolymers, ionomeric polymers, polyether-amide block copolymers, polyaryletherketones, polysulfones, polyphenylene sulfides, polyamide-imide copolymers, poly(butylene succinate), cellulosics, polysaccharides, and copolymers, alloys, admixtures, and mixtures thereof. In some embodiments, the thermoplastic polymer is a mixed plastic waste stream. The continuous polymer matrix optionally further comprises one or more additional materials selected from colorants, stabilizers, gloss agents, nucleating agents, fibers, particulates, and fillers.
[0016] Other objects and features will be in part apparent and in part pointed out hereinafter. The present invention provides, for example, the following: (Item 1) 1. A method comprising: adding a thermoplastic polymer and a source of a physical blowing agent to an extruder; heating and mixing the thermoplastic polymer and a physical blowing agent source under pressure in the extruder to form a melt pneumatic mix, the temperature of the melt pneumatic mix exceeding a critical temperature of the physical blowing agent source; collecting said amount of said melt pneumatic mixing in a collection area of said extruder; defining an expansion volume within the collection area and causing a pressure drop within the collection area; allowing an inflation time period to elapse after said determination; and Dispensing molten polymer foam from said collection area; A method comprising: (Item 2) 2. The method of claim 1, wherein the expansion volume is selected to provide 10% to 300% of the total expected molten foam volume within the collection area. (Item 3) 3. The method according to claim 1, wherein the expansion period is from 5 seconds to 600 seconds. (Item 4) 4. The method of any one of claims 1-3, wherein the melt pneumatic mixing is substantially uninterrupted during the expansion cycle. (Item 5) 5. The method according to any one of items 1 to 4, wherein the dispensing is dispensing into a mold. (Item 6) 6. The method of claim 5, further comprising a fluid connection between a collection area of the extruder and the die. (Item 7) 7. The method of any one of claims 1-6, wherein the dispensing comprises a linear flow of the molten polymer foam. (Item 8) 8. The method of any one of claims 1-7, further comprising cooling the dispensed molten polymer foam to a temperature below the melting transition temperature of the thermoplastic polymer. (Item 9) 9. The method of any one of items 1-8, further comprising adding one or more additional materials to the extruder, the one or more materials being selected from colorants, stabilizers, gloss agents, nucleating agents, fibers, particulates, and fillers. (Item 10) 10. The method according to any one of claims 1-9, wherein the source of physical blowing agent is a physical blowing agent and the addition is a pressurized addition. (Item 11) 10. The method according to any one of items 1-9, wherein the source of physical blowing agent comprises a bicarbonate, a polycarboxylic acid or a salt or ester thereof, or a mixture thereof. (Item 12) 1. A thermoplastic polymer foam article, the article having a foam structure throughout that is a continuous polymer matrix defining a plurality of bubbles therein, and further wherein a surface region of the article comprises compressed bubbles. (Item 13) Item 13. The polymeric foam article of item 12, wherein the surface region is a region of the article extending 500 microns from its surface. (Item 14) Item 14. The polymeric foam article of item 13, wherein the article comprises compressed foam greater than 500 microns from its surface. (Item 15) 15. The polymeric foam article of any one of items 12-14, wherein the thermoplastic polymer is selected from one or more of polyolefins, polyamides, polyimides, polyesters, polycarbonates, poly(lactic acid), acrylonitrile-butadiene-styrene copolymers, polystyrene, polyurethanes, polyvinyl chloride, tetrafluoroethylene, polyethersulfones, polyacetals, polyaramids, polyphenylene oxides, polybutylenes, polybutadienes, polyacrylates, and methacrylate copolymers, ionomeric polymers, polyether-amide block copolymers, polyaryletherketones, polysulfones, polyphenylene sulfides, polyamide-imide copolymers, poly(butylene succinate), cellulosics, polysaccharides, and copolymers, alloys, admixtures, and mixtures thereof. (Item 16) 16. The polymer foam article of any one of items 12-15, wherein the continuous polymer matrix further comprises one or more additional materials selected from colorants, stabilizers, gloss agents, nucleating agents, fibers, particulates, and fillers. (Item 17) 17. The polymeric foam article of any one of items 12-16, wherein the continuous polymer matrix further comprises talc. (Item 18) 18. The polymer foam article of any one of items 12-17, wherein the continuous polymer matrix comprises a mixed plastic waste stream. (Item 19) 19. The polymeric foam article of any one of items 12-18, wherein the polymeric foam article has a thickness greater than 2 cm. (Item 20) The polymer foam article has a thickness of 1,000 cm 3 19. The polymeric foam article of any one of items 12-18, comprising a volume greater than (Item 21) The polymer foam article has a thickness of more than 2 cm and a thickness of more than 1,000 cm 3 19. The polymeric foam article of any one of items 12-18, comprising a volume greater than [Brief description of the drawings]
[0017] [Figure 1A] 1A-1B illustrate a melt mixing apparatus useful for carrying out the methods described herein. [Figure 1B] 1A-1B illustrate a melt mixing apparatus useful for carrying out the methods described herein.
[0018] [Diagram 2] FIG. 2-1 is a photographic image of a part molded according to a standard foam molding process, as described in Example 1. FIG. 2-2 is a photographic image of a part molded according to a molten foam injection molding (MFIM) process, as described in Example 1. FIGs. 2-3 and 2-5 are photographic images of pieces cut from a part made according to a standard foam molding process, as described in Example 1. FIGs. 2-2 and 2-3 are photographic images of pieces cut from a part made according to the MFIM process, as described in Example 1.
[0019] [Diagram 3]Figure 3A is a photographic image of a cross-section of part A, made according to a standard foam molding process, as described in Example 2, cut into two pieces to reveal the cross-section, and Figure 3B is a photographic image of a cross-section of part B, made according to the MFIM process, as described in Example 2, cut into two pieces to reveal the cross-section.
[0020] [Figure 4] Figure 4A is a photographic image of a cross-section of part C, made according to the MFIM process, as described in Example 2, cut into two pieces to reveal the cross section, and Figure 4B is a photographic image of a cross-section of part D, made according to a standard foam molding process, as described in Example 2, cut into two pieces to reveal the cross section.
[0021] [Diagram 5] FIG. 5 is a graph including plots of part density versus decompression volume for various decompression times for Prototype B, as described in Example 3.
[0022] [Figure 6] FIG. 6 is a graph including plots of strain versus time for parts made in Prototypes A, B, and C, as described in Example 4.
[0023] [Figure 7] FIG. 7 shows photographic images of views of different sides of parts A, B, and C as described in Example 4.
[0024] [Figure 8] FIG. 8 shows a photographic representation of the cross-sections of parts A′, B′, C′, and D′ as described in Example 4.
[0025] [Figure 9] FIG. 9 is a depiction of two parts as described in Example 5.
[0026] [Figure 10]FIG. 10 is a conformal image of a tomographic scan of a first part fabricated according to the MFIM process, as described in Example 6.
[0027] [Figure 11] FIG. 11 is an image of the cross-sectional plane shown in FIG.
[0028] [Figure 12] FIG. 12 is a graph including a plot of average cell size and cell count versus cell circularity for a first part made as described in Example 6.
[0029] [Figure 13] FIG. 13 is a depiction of an X-ray tomography image of a cross section of the second (spherical) part as described in Example 6.
[0030] [Figure 14] FIG. 14 is a graph containing plots of average cell size and cell count versus cell circularity for the second (spherical) part, made as described in Example 6.
[0031] [Figure 15] FIG. 15 is a photomicrograph of the fracture surface of a fractured 3 inch diameter composite sphere made according to the MFIM process as described in Example 7.
[0032] [Figure 16] FIG. 16 is a photomicrograph image of the fracture surface of a fractured 3 inch diameter composite sphere made according to the MFIM process as described in Example 7.
[0033] [Figure 17] FIG. 17 is a photomicrograph image of the fracture surface of fractured 3 inch diameter composite spheres made according to the MFIM process as described in Example 7.
[0034] [Figure 18] FIG. 18 is a photomicrograph image of the fracture surface of a fractured 3 inch diameter composite sphere made according to the MFIM process as described in Example 7.
[0035] [Figure 19] FIG. 19 shows photomicrograph images of cross sections from ISO specimen parts made according to standard foam molding process steps 10, 11, 14, and 15, as described in Example 8.
[0036] [Figure 20] FIG. 20 shows photomicrograph images of cross sections from ISO specimen parts made according to MFIM process steps 9, 10, 15, and 16 as described in Example 8.
[0037] [Figure 21] FIG. 21 shows a micrograph of a cross section of an ISO specimen part made according to the MFIM process of step 9 as described in Example 8, and a stress-strain plot of a replica part made according to the MFIM process of step 9.
[0038] [Figure 22] FIG. 22 includes a cross-sectional photomicrograph of an ISO specimen part made according to the standard foam molding process of step 10, as described in Example 8, and a stress-strain plot of a replica part made according to the standard foam molding process of step 10.
[0039] [Figure 23] FIG. 23 includes two images from an X-ray tomography of an ISO specimen part made according to the standard foam molding process of step 15, as described in Example 8.
[0040] [Figure 24] FIG. 24 includes two images from an X-ray laminography of an ISO specimen part made according to the MFIM process of step 9 as described in Example 8.
[0041] [Diagram 25] FIG. 25 is an image from an X-ray scan of a large tensile specimen part made according to the MFIM process as described in Example 9.
[0042] [Figure 26] FIG. 26 includes cross sections of eight large tensile specimen parts made according to the MFIM process, as described in Example 9.
[0043] [Figure 27] FIG. 27 is an X-ray laminography image of a large tensile specimen part made according to the MFIM process as described in Example 9.
[0044] [Figure 28] FIG. 28 includes a series of X-ray tomography images at different depths within a tensile specimen part made according to the MFIM process, as described in Example 10, and a series of images at different depths within a tensile specimen part made according to a standard foam molding process.
[0045] [Figure 29] FIG. 29 is a graph including a plot of cell count versus depth for tensile specimen parts made according to the MFIM process, as described in Example 10, and a plot of cell count versus depth for tensile specimen parts made according to a standard foam molding process.
[0046] [Diagram 30] FIG. 30 is a graph including plots of cell circularity versus depth for tensile specimen parts made according to the MFIM process, as described in Example 10, and plots of cell circularity versus depth for tensile specimen parts made according to a standard foam molding process.
[0047] [Diagram 31]FIG. 31 is a graph including a plot of cell size versus depth for tensile specimen parts made according to the MFIM process, as described in Example 10, and a plot of cell size versus depth for tensile specimen parts made according to a standard foam molding process.
[0048] [Diagram 32] FIG. 32 is a photograph of Sample 20, made according to the reverse MFIM process, as described in Example 12.
[0049] FIG. 32 is a photograph of Sample 20, made according to the reverse MFIM process, as described in Example 12.
[0050] [Diagram 33] FIG. 33 is a photograph of Sample 10, made according to the MFIM process as described in Example 12.
[0051] [Diagram 34] FIG. 34 is a photograph showing a cross-section of Sample 20 made according to the reverse MFIM process as described in Example 12.
[0052] [Diagram 35] FIG. 35 is a photograph showing a cross-section of Sample 10 made according to the MFIM process as described in Example 12.
[0053] [Diagram 36] FIG. 36 is a plot of cell count versus depth (distance from surface) for Sample 10 (MFIM) and Sample 20 (reverse MFIM), as described in Example 12.
[0054] [Figure 37] FIG. 37 is a plot of cell size versus depth (distance from the surface) for Sample 10 (MFIM) and Sample 20 (reverse MFIM), as described in Example 12.
[0055] [Figure 38] FIG. 38 is a graph including averaged stress versus strain plots for Sample 10 (MFIM) and Sample 20 (inverse MFIM) from compressive modulus measurements, as described in Example 12.
[0056] [Figure 39] FIG. 39 is a graph including an averaged stress versus strain plot for Sample 10 (MFIM) and a plot for Sample 20 (inverse MFIM) from flexural modulus measurements, as described in Example 12.
[0057] [Diagram 40] FIG. 40 is a graph of stress versus strain plots from compressive modulus measurements made from three metallocene polyethylene (mPE) materials of different densities and made according to the MFIM process, as described in Example 14.
[0058] [Diagram 41] FIG. 41 illustrates a mold configuration useful for carrying out the methods described herein.
[0059] Corresponding reference characters indicate corresponding parts throughout the drawings. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0060] Detailed Description Although this disclosure provides reference to preferred embodiments, those skilled in the art will recognize that changes may be made in form and detail without departing from the spirit and scope of the invention. Various embodiments will be described in detail with reference to the drawings, in which like reference numbers represent like parts and assemblies throughout the several views. Reference to various embodiments does not limit the scope of the claims appended hereto. Additionally, any examples described herein are not intended to be limiting, but merely to describe some of the many possible embodiments for the appended claims.
[0061] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art. In case of conflict, the present specification, including definitions, will control. Preferred methods and materials are described below, although methods and materials similar or comparable to those described herein can also be used in the practice or testing of the present invention. All publications, patent applications, patents, and other references mentioned herein are incorporated by reference in their entirety. The materials, methods, and examples disclosed herein are illustrative only and are not intended to be limiting.
[0062] As used herein, "polymer matrix," including "continuous polymer matrix," "thermoplastic polymer matrix," "molten polymer matrix," and similar terms, refers to a continuous solid or molten thermoplastic polymer phase, or a quantity of solid or molten thermoplastic polymer that defines a continuous phase.
[0063] As used herein, "molten mixture" means a molten thermoplastic polymer or a mixture of molten thermoplastic polymers, optionally including one or more additional materials that are mixed with the molten thermoplastic polymer or mixtures thereof.
[0064] As used herein, a "molten pneumatic mixture" refers to a mixture of a thermoplastic polymer and a physical blowing agent source, where the polymer is at a temperature above its melting temperature, the temperature of the mixture exceeds the critical temperature of the physical blowing agent source, and the mixture is characterized as being foam-free or substantially foam-free. The molten pneumatic mixture is under sufficient pressure to prevent foam formation, or to substantially prevent foam formation, or to dissolve or disperse the physical blowing agent source as either a gas or a supercritical liquid within the thermoplastic polymer. "Substantially prevents foam formation," "substantially foam-free," and similar terms relating to the molten pneumatic mixture mean that while pressure conditions may be used to prevent foam formation in the molten mixture, defects, wear of parts, and the like within processing equipment may cause unintentional pressure losses that do not generally interfere with obtaining and maintaining a pressurized molten mixture.
[0065] As used herein, "foam," "polymer foam," "thermoplastic polymer foam," "melt foam," "molten polymer foam," and similar terms generally refer to a continuous polymer matrix defining a plurality of bubbles as intermittent phases dispersed therein.
[0066] As used herein, the term "foam" means discrete voids defined by and surrounded by a continuous thermoplastic polymer matrix.
[0067] As used herein, the term "physical blowing agent" means a gaseous compound capable of defining a foam within a molten thermoplastic polymer matrix.
[0068] As used herein, the term "critical temperature" means the temperature at which a physical blowing agent source produces a physical blowing agent at atmospheric pressure.
[0069] As used herein, the term "physical blowing agent source" refers to a latent, latent, or nascent physical blowing agent in the form of an organic compound, or combinations thereof, that is added to or present in a thermoplastic polymer matrix, such as dissolved in the matrix and / or present therein as a supercritical fluid, or that produces a physical blowing agent by chemical reaction, or the physical blowing agent source is, becomes, or produces a physical blowing agent at the critical temperature characteristic of the physical blowing agent source.
[0070] The terms "comprise," "include," "having," "has," "can," "contain," and variations thereof, as used herein, are intended to be open-ended transitional phrases, terms, or words that do not exclude the possibility of additional acts or structures. The singular forms "a," "and," and "the" include plural references unless the context clearly dictates otherwise. The present disclosure also contemplates other embodiments of "comprising," "consisting of," and "consisting essentially of" the embodiments or elements presented herein, whether or not explicitly stated.
[0071] As used herein, the terms "optional" or "optionally" mean that the event or circumstance described subsequently may, but need not, occur, and that the description includes instances in which the event or circumstance occurs and instances in which it does not occur.
[0072] As used herein, the term "about" used in describing embodiments of the present disclosure, for example, to modify amounts, concentrations, volumes, process temperatures, process times, yields, flow rates, pressures, and similar values and ranges of ingredients in a composition, refers to variations in numerical quantities that may occur, for example, through typical measuring and handling procedures used to make a compound, composition, concentrate, or formulation for use, through inadvertent errors in these procedures, through differences in the manufacture, source, or purity of the starting materials or ingredients used to carry out the method, and through similar proximate considerations. The term "about" also encompasses amounts that differ due to aging of a formulation with a particular initial concentration or mixture, and amounts that differ due to mixing or processing a formulation with a particular initial concentration or mixture. When modified by the term "about," the claims appended hereto include equivalents of these quantities. Furthermore, when "about" is employed to describe a range of values, e.g., "about 1 to 5," the recitation means "1 to 5" and "about 1 to about 5" and "1 to about 5" and "about 1 to 5," unless specifically limited by context.
[0073] As used herein, the term "substantially" means "consisting essentially of" as the term is interpreted in U.S. Patent Law, including "consisting of" as the term is interpreted in U.S. Patent Law. For example, if a specified compound or material is "substantially free," the composition may be free of that compound or material, or may have a small amount of that compound or material present through unintended contamination, side reactions, incomplete purification, or the like. A "minor amount" may be an insignificant amount, an immeasurable amount, an amount that does not interfere with the value or properties, or some other amount as provided within the context. With the provided list of components "substantially only," the composition may consist only of those components, or may have minor amounts of some other components present, or may have one or more additional components that do not significantly affect the properties of the composition. Additionally, "substantially," employed in describing embodiments of the present disclosure to modify, for example, the type or amount of an ingredient in a composition, a property, a measurable amount, a method, a value, or a range, refers to a variation that does not affect the overall recited composition, property, amount, method, value, or range in a manner that eliminates the intended composition, property, amount, method, value, or range. When modified by "substantially," the claims appended hereto include equivalents according to this definition.
[0074] As used herein, any recited range of values is to be construed as supporting a claim that contemplates every value within the range and recites any subranges with endpoints that are real values within the recited range. As a hypothetical illustrative example, the disclosure herein of a range of 1-5 is to be considered as supporting a claim to any of the following ranges: 1-5, 1-4, 1-3, 1-2, 2-5, 2-4, 2-3, 3-5, 3-4, and 4-5.
[0075] In embodiments disclosed herein, a method of extruding a molten polymer foam comprises, consists essentially of, or consists of adding a thermoplastic polymer and a physical blowing agent source to an inlet mounted on a first end of an extruder; heating and mixing the thermoplastic polymer and the physical blowing agent source in the extruder to form a molten pneumatic mixture, where the temperature of the molten pneumatic mixture exceeds a critical temperature of the physical blowing agent source; collecting a quantity of the molten pneumatic mixture in a barrel region of the extruder located proximate a second end of the extruder; forming an expanded volume in the barrel region, where the forming step involves allowing a pressure to drop in the barrel region; allowing a period of time to pass after the pressure drop; and dispensing the molten polymer foam from the extruder.
[0076] In an embodiment, an extruder is any machine designed and adapted to melt, mix, and dispense a thermoplastic polymer and mixtures thereof, optionally with one or more additional materials such as fillers, nucleating agents, diluents, stabilizers, gloss agents, and the like, and further, the extruder includes a collection area for collecting a mass of the mixed molten material, and further, is capable of forming an expansion volume within the collection area coupled with a pressure drop. Extruders are well known in the industry and are broadly used to melt, mix, and manipulate molten thermoplastic polymers. In an embodiment, the extruder is adapted and designed to melt, mix, and dispense a mixture of a thermoplastic polymer and a physical blowing agent source. Such an extruder is adapted to obtain a molten pneumatic mixture under a pressure sufficient to prevent or substantially prevent foam formation in the molten pneumatic mixture.
[0077] In an embodiment, an extruder useful for carrying out the present method includes an internal volume, referred to in the art as the "barrel" of the extruder, designed and adapted to receive the solid thermoplastic polymer and further melt and mix it. In an embodiment, the extruder defines an internal volume designed to receive the solid thermoplastic polymer and the physical blowing agent or source, and further to at least melt the polymer, and to mix the molten polymer with the physical blowing agent or source to obtain a molten pneumatic mixture. In an embodiment, the extruder further includes a collection area for collecting a mass of the molten pneumatically mixed material. In an embodiment, the extruder further includes a means for forming an expansion volume within the collection area coupled with a pressure drop.
[0078] In an embodiment, the extruder is an injection molding machine. In an embodiment, the extruder is a SODICK extruder sold by Plustech Inc. (Schaumburg, IL). TMIn some embodiments, the extruder is a single-screw extruder, which is defined as including one screw movably positioned within the barrel for rotation of a cylinder about its axis, for lateral movement of a cylinder along its axis, or for combined movement including both rotation and lateral movement. In other embodiments, the extruder is a twin-screw extruder, which is defined as including two screws movably positioned within the barrel in a generally parallel and adjacent relationship to each other, and further, each screw movably positioned within the barrel for rotation of a cylinder about its axis, for lateral movement of a cylinder along its axis, or for combined movement including both rotation and lateral movement. The screws of the twin screw extruder are further arranged such that the action of the screws, as they are orbited in a counter-rotating manner, defines a designed mixing and transport pattern of the molten thermoplastic polymer disposed within the barrel.
[0079] In an embodiment, the extruder is further adapted and designed to receive a solid thermoplastic polymer. In an embodiment, the barrel of the extruder is further adapted and designed to receive a solid thermoplastic polymer by including an inlet that is mounted near the first end of the extruder and is adapted to add the solid thermoplastic polymer to the barrel. The solid thermoplastic polymer is added to the inlet in any suitable format, for example, beads, pellets, powder, ribbons, or blocks, all of which are formats familiar to those skilled in the art. In an embodiment, the extruder includes a second, third, or even a fourth or higher inlet that is designed and adapted to add or introduce one or more additional materials, including one or more solids, liquids, or gases, into the internal volume of the extruder, and further to mix the thermoplastic polymer with one or more additional materials. The interior volume of the extruder is adapted to receive, contain, and melt the thermoplastic polymer and optionally one or more additional materials, and to expose the thermoplastic polymer and optionally one or more additional materials to heat, shear, and mixing to form a molten mixture, while simultaneously transporting the molten mixture generally in a direction proceeding from its first end to its second end. In embodiments where the extruder is a single screw extruder or a twin screw extruder, the shearing, mixing, and transporting are accomplished by rotating the screws or counter-rotating the two screws.
[0080] In an embodiment, the extruder internal volume or a portion thereof is surrounded or partially surrounded by one or more heat sources. Heat sources, which are suitably adapted to heat the extruder internal volume, in various embodiments include a heated water jacket, a heated oil jacket, an electrical resistance heater, an open or jacketed flame, or another heat source. The heat source is operable to increase the temperature within the extruder internal volume. The temperature is suitably selected by an operator to melt the thermoplastic polymer and / or maintain a desired temperature within a portion of the extruder internal volume. In an embodiment, the extruder is adapted to include more than one heat source, which are independently operable to allow a person skilled in the art to provide a range of temperature "zones" within the internal volume. Additional temperature zones may be included within some extruders in association with adding one or more materials to their inlet or dispensing one or more materials from their outlet. In an embodiment, the temperature within one or more temperature zones is set by an operator for increased control and optimization of the melting, mixing, shearing, and transport of the thermoplastic polymer and, optionally, one or more additional materials.
[0081] Extruders are conventionally designed and adapted to apply and maintain a pressure within their internal volume during heating, mixing, and transporting the molten mixture. In an embodiment, the extruder is designed and adapted to apply and maintain a first pressure within an internal volume or barrel during heating, mixing, and transporting the molten mixture. In an embodiment, the pressure inside the barrel during heating, mixing, and transporting the molten pneumatic mixture is sufficient to prevent or substantially prevent leakage of the molten pneumatic mixture from the barrel. In an embodiment, the pressure inside the barrel is sufficient to prevent the molten pneumatic mixture from developing a foam when the temperature inside the barrel exceeds the critical temperature of the physical blowing agent source. In an embodiment, the pressure inside the barrel is substantially sufficient to prevent the molten pneumatic mixture from developing a foam when the temperature inside the barrel exceeds the critical temperature of the physical blowing agent source. In such embodiments described in this paragraph, "substantially" refers to inadvertent leakage of material or inadvertent loss of pressure from the barrel due to the manufacture, aging, or mode of use of the extruder and / or screw, as will be familiar to those skilled in the art. Further in such embodiments, "substantially" in the context of "sufficient to prevent the molten pneumatic mixture from developing a foam" means that a small percentage, such as up to 10%, of the physical blowing agent may inadvertently form a foam while pressure is maintained on the molten pneumatic mixture, but it is the operator's goal to maintain sufficient pressure to prevent foam from forming.
[0082] In an embodiment, the barrel of the extruder includes a collection area for collecting a quantity of the molten mixture in preparation for dispensing the molten mixture from the extruder. The mass of the molten mixture is selected by the user. In an embodiment, the molten mixture is a molten pneumatic mixture. In such an embodiment, the term in the art used to describe the collection of a mass of the molten pneumatic mixture into the collection area of the barrel of the extruder is referred to as "building a shot". As will be understood by those skilled in the art of injection molding, to build a shot, a mass of the molten pneumatic mixture is collected by conveying the molten pneumatic mixture from the first end of the extruder towards the second end, i.e. towards and into the collection area, by the rotation of a screw or screws (or another mixing element), and by allowing the molten pneumatic mixture to accumulate in the collection area until the entire desired mass of the molten pneumatic mixture is collected and disposed in the collection area of the barrel. The collection area is mounted between the screw or screws and the second end of the extruder and is in pressurized communication with the remainder of the barrel.
[0083] In conventional injection molding to form thermoplastic polymer foams, a mass of the molten pneumatic mixture, or "shot," is collected or "built" in a collection area by conveying the molten pneumatic mixture toward and into the collection area by rotation of a screw or multiple screws (or another mixing element). A shot is said to be built when the entire selected mass of the molten pneumatic mixture is disposed within the collection area. Those skilled in the art will appreciate that the foregoing description of melt mixing equipment, such as the mechanical elements and features of an extruder or other melt mixing equipment, as well as the foregoing description of the methods of creating and collecting the molten pneumatic mixture in a shot, are in accordance with conventional equipment and methods of using such equipment to create a molten pneumatic mixture and build the shot.
[0084] According to these known methods and apparatus, the shot of the molten pneumatic mixture is conventionally prevented or substantially prevented from developing foam while present in the barrel, including during mixing, heating, transport, and collection, and also while disposed in the collection area. Conventionally, once the desired shot is collected in the collection area, a gate or door, installed between the collection area and an outlet installed on the second end of the extruder, is opened to provide a fluid connection from the barrel to the outlet and dispense the shot from the extruder. In some embodiments, once the gate or door is opened, a mechanical plunger is applied to force the molten pneumatic mixture from the barrel through the outlet. In embodiments, a screw or multiple screws are suitably employed in a lateral movement in a direction toward the second end of the extruder, which in turn forces the molten pneumatic mixture from the collection area of the barrel through the outlet.
[0085] We have found that after building up a shot of molten pneumatic mixture in the collection area of the extruder, it is advantageous to form, provide or define an expansion volume in the collection area of the extruder, the defining step involving a pressure drop in the collection area, a time period, referred to herein as an expansion period, being allowed to pass after the definition, and dispensing the shot from the extruder after the expansion period. The shot is dispensed in the form of molten polymer foam in such an embodiment. In an embodiment, the expansion volume is defined in proximity to the shot, which is disposed in the collection area of the extruder. In an embodiment, the shot is not mixed or exposed to the application of shear or elongation during the process in which the expansion volume is defined. In an embodiment, the shot is not transported during the expansion period. In an embodiment, the shot is allowed to rest or reside, uninterrupted or substantially uninterrupted, in the collection area during the expansion period. In any of the foregoing embodiments, the shot may be heated during the expansion period. However, in some embodiments, heat is not added to the shot during the expansion period.
[0086] After the expansion cycle has elapsed or is transient, the molten polymer foam may be dispensed from the second end of the extruder. The molten polymer foam includes a plurality of bubbles. Without being limited by theory, it is believed that the bubbles are formed when the molten pneumatic mixture is exposed to an expanded volume and an associated pressure drop (second pressure). In accordance with known principles of physics, the formation of the bubbles is likely caused by the definition of an expanded volume and an associated pressure drop in the collection area of the barrel along with the expansion cycle, where the bubbles are formed by the action of a physical blowing agent. In some embodiments, the step of defining an expanded volume after building a shot results in better properties attributable to the dispensed molten polymer foam. In other words, we have found that forming a molten pneumatic mixture under pressure, followed by a step of lowering the pressure and an associated step of forming a defined volume prior to dispensing the mixture (such as into a mold cavity), results in a molten polymer foam that upon cooling provides a solidified polymer foam article with physical properties that are unexpected and highly beneficial.
[0087] We have found that the molten polymer foam dispensed from the extruder according to the aforementioned method obtains significant technical advantages. These advantages are observed in the solidified polymer foam resulting from cooling the molten polymer foam to a temperature below the melting transition temperature of the thermoplastic polymer. The structure of the article made using the molten polymer foam dispensed from the extruder after the expansion cycle differs from the polymer foam made by conventional methods, both macroscopically and microscopically, and exhibits superior properties suitable for, for example, structural members. The polymer foam article made using the methods, apparatus, and materials described herein is characterized as having a continuous thermoplastic matrix throughout and a plurality of bubbles dispersed throughout the polymer foam article. This characterization has been demonstrated for thicknesses of more than 2 cm, 1,000 cm 3 or a thickness of more than 2cm, plus 1,000cm 3 Exceeding 1,000cm 3 ~5,000cm 3, or an additional 5,000 cm 3 Articles with a volume exceeding 1,000 cm 3 Volume greater than 2cm and thickness greater than 1,000cm 3 ~5,000cm 3 and a thickness greater than 2 cm, or a volume greater than 5,000 cm and a thickness greater than 2 cm.
[0088] In an embodiment, the definition of the expansion volume in a single screw extruder is preferably achieved by moving the screw laterally towards the first end of the extruder and away from the collection area of the extruder where the shot is collected. In an embodiment, the definition of the expansion volume in a twin screw extruder is preferably achieved by moving both screws laterally towards the first end of the extruder and away from the area of the extruder where the shot is collected. The lateral movement is optionally accompanied by rotation of the screw or screws. That is, one or both screws may be rotated during the lateral movement, or the rotation may be stopped during the lateral movement. It should be understood that the definition of the expansion volume by the lateral movement of one or both screws is advantageously selected by the extruder operator to provide a selected expansion volume. That is, the distance of the lateral movement of the screw or screws is preferably selected by the operator to define the selected expansion volume.
[0089] Thus, in an embodiment, the expansion volume is targeted by the operator to add enough volume to the collection area to accommodate the total expected molten polymer foam volume or a percentage thereof. The total expected molten polymer foam volume of the shot may be calculated based on the amount of thermoplastic polymer and physical blowing agent source plus any additional material added to build the shot, further assuming that all of the physical blowing agent source will contribute to the formation of bubbles within the molten polymer foam to be obtained. Those skilled in the art will understand that physical blowing agent sources obtained in the industry are provided with suitable information to calculate the total expected molten polymer foam volume based on the amount of physical blowing agent source added to make the shot and other processing conditions. In an embodiment, the expansion volume is the difference between the shot volume and the expected molten polymer foam volume.In embodiments, the expansion volume is between 10% and 100% of the total expected molten polymer foam volume within the collection area, for example, between 15% and 100%, or between 20% and 100%, or between 25% and 100%, or between 30% and 100%, or between 35% and 100%, or between 40% and 100%, or between 45% and 100%, or between 50% and 50% of the difference between the shot volume and the expected molten polymer foam volume. %~100%, or 55%~100%, or 60%~100%, or 65%~100%, or 70%~100%, or 75%~100%, or 80%~100%, or 85%~100%, or 90%~100%, or 10%~95%, or 10%~90%, or 10%~85%, or 10%~80%, or 10%~75%, or 10% ~70%, or 10%~65%, or 10%~60%, or 10%~55%, or 10%~50%, or 10%~45%, or 10%~40%, or 10%~35%, or 10%~30%, or 10%~25%, or 10%~20%, or 10%~15%, or 15%~20%, or 20%~25%, or 25%~30%, or 30 % to 35%, or 35% to 40%, or 40% to 45%, or 45% to 50%, or 50% to 55%, or 55% to 60%, or 60% to 65%, or 65% to 70%, or 70% to 75%, or 75% to 80%, or 80% to 85%, or 85% to 90%, or 90% to 95%, or 95% to 100%. In yet other embodiments, the expansion volume is 100% to 300% of the difference between the shot volume and the expected molten polymer foam volume, such as 100% to 105%, or 100% to 110%, or 100% to 115%, or 100% to 120%, or 105% to 110%, or 110% to 115%, or 115% to 120%, or 120% to 125%, or 120% to 150%, or 150% to 200%, or 200% to 250%, or 250% to 300% of the difference between the shot volume and the expected molten polymer foam volume.
[0090] After the expansion volume is defined, a period of time is allowed to elapse or pass prior to dispensing the molten polymer foam from the extruder. In embodiments, the period of time is referred to as an expansion period. In some embodiments, no mixing, transport, shearing, or other physical manipulation or additional volumetric changes are performed in the collection area during the expansion period. Instead, in such embodiments, the shot is allowed to rest in the collection area during the expansion period. At the end of the expansion period, the molten polymer foam is dispensed from the extruder outlet. In embodiments, the molten polymer foam is dispensed into a mold cavity and the molten polymer foam is cooled to a temperature below the melting transition of the thermoplastic polymer to obtain a solidified polymer foam article.
[0091] In an embodiment, the expansion period is selected by the operator to be about 5 seconds to 600 seconds, depending on the mass of the sample, the source of physical blowing agent, and the amount of any additional materials present in the shot. In an embodiment, the expansion period is 5 seconds to 600 seconds, or 5 seconds to 500 seconds, or 5 seconds to 400 seconds, or 5 seconds to 300 seconds, or 20 seconds to 600 seconds, or 20 seconds to 500 seconds, or 20 seconds to 400 seconds, or 20 seconds to 300 seconds, or 10 seconds to 200 seconds, or 20 seconds to 200 seconds, or 30 seconds to 200 seconds, or 40 seconds to 200 seconds, or 50 seconds to 200 seconds, or 5 seconds to 190 seconds, or 5 seconds to 180 seconds, or 5 seconds to 170 seconds, or 5 seconds to 160 seconds, or 5 seconds to 150 seconds, or 5 seconds to 140 seconds, or 5 seconds to 130 seconds, or 5 seconds to 120 seconds, or 5 seconds to 110 seconds, or 5 seconds to 100 seconds, or 5 seconds to 90 seconds, or 5 seconds to 80 seconds, or 5 seconds to 70 seconds, or 5 seconds to 60 seconds, or 5 seconds to 50 seconds, or 5 seconds to 40 seconds, or 5 seconds to 30 seconds, or 5 seconds to 20 seconds, or 5 seconds to 10 seconds, or 10 seconds to 15 seconds, or is 15 seconds to 20 seconds, or 20 seconds to 25 seconds, or 25 seconds to 30 seconds, or 30 seconds to 35 seconds, or 35 seconds to 40 seconds, or 40 seconds to 45 seconds, or 45 seconds to 50 seconds, or 50 seconds to 55 seconds, or 55 seconds to 60 seconds, or 60 seconds to 70 seconds, or 70 seconds to 80 seconds, or 80 seconds to 90 seconds, or 90 seconds to 100 seconds, or 100 seconds to 110 seconds, or 110 seconds to 120 seconds, or 120 seconds to 130 seconds, or 130 seconds ~140 seconds, or 140 seconds to 150 seconds, or 150 seconds to 160 seconds, or 160 seconds to 170 seconds, or 170 seconds to 180 seconds, or 180 seconds to 190 seconds, or 190 seconds to 200 seconds, or 200 seconds to 250 seconds, 250 seconds to 300 seconds, or 300 seconds to 350 seconds, or 350 seconds to 400 seconds, or 400 seconds to 450 seconds, or 450 seconds to 500 seconds, or 500 seconds to 550 seconds, or 550 seconds to 600 seconds.
[0092] The use of the aforementioned method results in the formation of a molten polymer foam that obtains several significant technical advantages, as described in the following sections, when the molten polymer foam is cooled to a temperature below the melting temperature of the thermoplastic polymer, resulting in a solidified polymer foam. A polymer foam article is generally characterized as a monolithic article having a continuous polymer matrix that defines a plurality of bubbles dispersed throughout the article. In an embodiment, a polymer foam article is specifically characterized as having a continuous polymer matrix that defines a plurality of bubbles dispersed throughout the surface region of the article, where the surface region is defined as the area of the article between the article surface (polymer foam-air interface) and a distance within 500 microns of the surface.
[0093] A representative embodiment of an apparatus usefully employed to perform the aforementioned methods is shown in FIG. 1A. FIG. 1A is a schematic diagram of an exemplary single-screw injection molding apparatus 20 according to an embodiment disclosed herein for carrying out the methods described herein useful for making molten polymer foams and polymer foam articles also disclosed herein. As shown in FIG. 1A, the injection molding system 20 includes a barrel 21 attached to a motor or drive section 24 and a mold section 26. The barrel 21 includes a first end 21a and a second end 21b and defines a hollow interior barrel portion 22. The barrel portion 22 further defines a nozzle 36 proximate the barrel second end 21b. A screw 30 is disposed within the barrel portion 22 and includes a screw tip portion 34. The screw 30 is operably coupled to the motor section 24 for rotation of the screw 30 about its central axis or for lateral movement as indicated by arrow Z. The lateral movement of the screw 30 may be generally in a direction from the first end 21a of the barrel toward the second end 21b of the barrel, or from the second end 21b of the barrel toward the first end 21a of the barrel. The lateral movement of the screw 30 in either direction is optionally further coupled with a rotational movement. The screw 30 further includes one or more steps 31, which are mixing elements for mixing and transporting the material present in the barrel portion 22, generally from the first end 21a of the barrel toward the second end 21b of the barrel. The screw 30 is disposed within the barrel portion 22 in a pressurizable sealed relationship therein, allowing a pressure above atmospheric pressure to be maintained within the barrel portion 22 by the screw steps 31 within the barrel 21, and further by the installation of a check valve 32. A shutoff valve 37 is connected to the barrel 21 near the second end 20b and is operable to control a fluid connection, a pressurized connection, or both, between the nozzle 36 and the die section 26.A check valve 32, disposed within barrel portion 22 and surrounding screw 30, is operable to prevent back pressure from forcing material resident within barrel portion 22 toward first end 21 a of the barrel, thus providing a pressurizable sealed, fluidly sealed, or pressurizable fluidly sealed relationship between closure valve 37 and check valve 32.
[0094] 1A , mold section 26, as shown, includes two mold sections 38. Mold sections 38 are removably joined together to define a cavity 39. In some embodiments, one or more of mold sections 38 are movable to permit ejection of a solidified polymer foam article therefrom. In some embodiments, mold sections 38 are mounted in a touching relationship to one another, while in other embodiments, mold sections 28 are spaced apart by a gap.
[0095] In an embodiment, the methods disclosed herein are preferably carried out using an apparatus such as the system 20 shown in Figures 1A-1B. In Figure 1A, a selected mass of mixture 42A comprising a thermoplastic polymer, a physical blowing agent source, and optionally a selected amount of one or more additional materials is added to the barrel section 22 through the inlet 28 as indicated by arrow A. In some embodiments, the physical blowing agent source is a physical blowing agent, and the inlet 28 or another inlet (not shown) is a pressurized gas inlet relative to the barrel section 22, and the physical blowing agent is added to the gas inlet at a selected pressure while a non-gaseous material is added to the inlet 28. During the addition of the mixture 42A to the barrel section 22 through the inlet 28, the motor 24 is operable to rotate the screw 30. The rotation of the screw 30 transports and mixes the mixture 42A to the screw tip 34. A heat source (not shown) is preferably employed to add heat to the mixture 42A in the barrel section 22. The motor 24 rotates the screw 30 to transport the mixture 42A present in the barrel portion 22 in a direction generally proceeding from the first end 21a toward the second end 21b of the barrel 21 until the screw tip 34 is reached. In addition, the rotation of the screw 30 provides mixing of the mixture 42A during transport. A heating element or heating zone (not shown) proximate the barrel portion 22 operates to heat the mixture 42A as it is transported and mixed by the rotation of the screw 30. Multiple heating zones may be present proximate the barrel portion 22 to vary the temperature inside the barrel portion 22 between the first end 21a and the second end 21b of the barrel 21. During transport, the screw 30 rotating within the barrel portion 22 is operable to mix the mixture 42A and heat is added to the mixture as it is transported, thereby raising the temperature of the mixture above the melting point of the thermoplastic polymer and converting the mixture 42A into a molten pneumatic mixture 42B at least by the time it reaches the second end 21b of the barrel 21.Additionally, the positioning of the screw 30 within the barrel section 22, further with the step 31 in contact with the barrel 21 during rotation of the screw 30, combined with the check valve 32, the shut-off valve 37 in the closed position, or both, provides a pressurizable sealed relationship within the barrel section 22, whereby the molten pneumatic mixture 42B exists within the barrel section 22 under pressure above atmospheric pressure. The pressure within the barrel section 22 is sufficient to prevent or substantially prevent foam formation even when the physical blowing agent source is above its critical temperature.
[0096] Rotation of the screw 30 further operates to transport the pressurized molten pneumatic mixture toward the screw tip 34 and to transport or build up a selected mass of the pressurized molten pneumatic mixture 42B into a collection area 40 of the barrel section 22. The collection area 40 is defined as the area within the volume of the barrel section 22 that extends between the check valve 32 and the shutoff valve 37 in FIG. 1A and further as the area of the barrel section 22 that is mounted along the X distance of the barrel 21. The selected mass or "shot" of the pressurized molten pneumatic mixture 42B is collected, i.e., accumulated, in the collection area 40 of the barrel section 22. The pressure in the collection area 40 is sufficient to prevent or substantially prevent foam formation in the molten pneumatic mixture. In an embodiment, the shot substantially fills the collection area 40.
[0097] The construction of the shot of molten pneumatic mixture 42B is accomplished using conventional methods familiar to those skilled in the art. Conventional and known variations in methods and materials employed to construct the shot for injection molding are encompassed by the methods described herein. Once the shot is constructed, it may be subjected to the methods disclosed herein to obtain all of the technical advantages disclosed herein for forming polymeric foams and polymeric foam articles. For example, to form the shot, a method such as the MUCELL® high pressure process employed by Trexel Inc. (Wilmington, MA) is preferably employed, which includes the direct addition of a source of physical blowing agent as a gas to an extruder, with pressurized mixing to prevent or substantially prevent foam formation, followed by shot collection. Various patents and trademark publications further describe specialized melt mixing and conveying designs for obtaining the molten pneumatic mixture and forming the shot, such as specialized screw designs for mixing and counterflow patterns and the like. Any of these may be usefully employed in conjunction with the shot formation methods and apparatus described above to form a shot as described herein and collect the shot under pressure in a collection area of a melt mixing device.
[0098] Once the shot is formed and collected in the collection area, an expansion volume is defined therein, and the expansion is accompanied by a drop in pressure in the collection area and adjacent to the shot. Thus, FIG. 1A depicts the molten pneumatic mixing apparatus 20 with the screw 30 positioned to collect the shot in the collection area 40. The shot comprises a selected mass of the molten pneumatic mixture 42B and is disposed under pressure in the collection area 40. At this stage of the process, and still with reference to FIG. 1A, FIG. 1B depicts the apparatus 20 with the screw 30 positioned to define an expansion volume 44 in the collection area 40. In somewhat more detail, FIG. 1B shows the screw 30 in a position resulting from a lateral movement of the screw 30 toward the first end 21a of the barrel, i.e., the screw 30 is retracted in FIG. 1B relative to FIG. 1A. The retraction and resulting partial displacement of the screw 30 from the collection area 40 defines an expansion volume 44 in the collection area 40 and also causes pressure to drop in the collection area 40. In some embodiments, the rotation of the screw 30 is stopped prior to retraction. In some embodiments, the rotation of the screw 30 is stopped during retraction or after retraction is completed. The retraction distance of the screw 30, i.e., the distance of lateral movement of the screw 30 towards the first end 21a of the barrel, is selected by the operator to provide a suitable expansion volume 44.
[0099] In some embodiments depicted in FIG. 1B, the expansion volume 44 is selected by the operator to provide a collection area 40 having a total volume that matches the total expected molten polymer foam volume of the shot, and in such embodiments, the total volume within the collection area 40 after the addition of the expansion volume 44 is the total expected molten polymer foam volume of the molten pneumatic mixture 42B of FIG. 1B. In other embodiments, the expansion volume 44 is selected by the operator to provide a collection area 40 having a total volume that is a percentage of the total expected molten polymer foam volume of the molten pneumatic mixture or shot residing within the collection area 40. That is, the total volume within the collection area 40 after the addition of the expansion volume 44 is equal to about 50%-120% of the total expected molten polymer foam volume. In some embodiments, the expansion volume is set to provide a total volume within the collection area to accommodate 100% of the total expected molten polymer foam volume. The total expected molten polymer foam volume of the shot may further be calculated based on the amounts of thermoplastic polymer and physical blowing agent source, plus any additional materials added to construct the shot, assuming that all of the physical blowing agent source contributes to the formation of bubbles within the molten polymer foam to be obtained.
[0100] After retracting the screw 30 and defining the expansion volume 44, as shown in FIG. 1B, a period of time, referred to as an "expansion period," is allowed to elapse or transition while the shot is held within the collection area 40, as shown in FIG. 1B, specifically, the collection area 40 includes the expansion volume 44. The expansion period is selected by the operator to be between 5 seconds and 200 seconds. In an embodiment, during the expansion period, the shot is allowed to sit uninterrupted or substantially uninterrupted within the collection area 40. In an embodiment, "uninterrupted" means that the shot is not exposed to any process that causes mixing, shearing, or transport (flow) of the shot during the expansion period. In an embodiment, "substantially uninterrupted" means that the shot is not intentionally perturbed by the mixing, shearing, or transporting processes performed during the expansion period, but for example, thermal differentials, leakage, and other manufacturing issues may lead to inadvertent stresses or strains on the shot residing within the collection area during the expansion period.
[0101] After the expansion cycle has elapsed, the nozzle shutoff valve 37 as shown in Figure 1B is opened and the molten polymer foam is dispensed from the barrel 22. In the embodiment as shown in Figures 1A-1B, the molten polymer foam flows into the cavity 39. The dispensing step may be pressurized dispensing by mechanical means such as pushing using lateral movement of a screw or by applying pressurized gas to a collection area, although application of pressure is not required to dispense the molten polymer foam in some embodiments. In embodiments, the pressure at the nozzle 36 as shown in Figures 1A-1B during dispensing of the molten polymer foam exceeds gravity by 1 psi to 20 psi, e.g., 3 psi to 20 psi, 5 psi to 20 psi, 7 psi to 20 psi, 10 psi to 20 psi, 15 psi to 20 psi, 1 psi to 15 psi, 1 psi to 10 psi, 1 psi to 7 psi, 1 psi to 5 psi, 2 psi to 5 psi, 5 psi to 10 psi, 10 psi to 15 psi, or 15 psi to 20 psi, without the addition of an external pressure source, such as by forcing the molten polymer foam using additional lateral movement of the screw 30 toward the second end 21b of the barrel in Figures 1A-1B. In embodiments, the dispensing step is accomplished by maintaining a fluid connection between the nozzle 36 and the cavity 39. In some such embodiments, the fluid connection is further a pressurized connection.
[0102] Once placed within the cavity 39 defined by the mold portion 38 shown in Figures 1A-1B, the molten polymer foam is cooled or allowed to cool until it reaches a temperature below the melt transition of the thermoplastic polymer, such as the temperature present in the ambient conditions of the surrounding environment. In some embodiments where the expansion volume is set to provide a total volume in the collection area that is less than 100% of the total expected molten polymer foam volume, the foam may continue to nucleate and / or develop (grow in size) after the molten polymer foam is dispensed and before the temperature has cooled sufficiently to reach the melt transition temperature of the thermoplastic polymer. Cooling of the molten polymer foam is accomplished using conventional methods for cooling injection molded articles, including, but not limited to, immersing the mold in a liquid coolant having a set temperature, or spraying the mold with a liquid coolant such as liquid water, impinging a stream of air onto the mold, cooling the ambient air, and the like.
[0103] In an alternative embodiment of the aforementioned method, an apparatus 20 configured as shown in FIG. 1B is employed to form a molten polymer foam. FIG. 1B shows the screw 30 in a position resulting from a lateral movement of the screw 30 toward the first end 21a of the barrel, i.e., the screw 30 is retracted in FIG. 1B relative to FIG. 1A. The retraction and resulting partial displacement of the screw 30 from the collection area 40 defines an expansion volume 44 in the collection area 40, further causing a pressure drop in the collection area 40. The apparatus 20 configured as shown in FIG. 1B is employed to mix, heat, and transport the molten pneumatic mixture 42B toward the second end 21b of the barrel 21 in substantially the same manner as described above. Additionally, the positioning of the screw 30 within the barrel section 22, where the step 31 contacts the barrel 21 during rotation of the screw 30, in combination with the check valve 32, the shutoff valve 37 in a closed position, or both, provides a pressurizable sealed relationship within the barrel section 22, whereby the molten pneumatic mixture 42B exists within the barrel section 22 under pressure above atmospheric pressure. The pressure within the barrel section 22 is sufficient to prevent or substantially prevent foam formation even when the physical blowing agent source is above its critical temperature. However, in this alternative embodiment, the molten pneumatic mixture is transported through the check valve 32 into the collection area 40, which is further augmented by the expansion volume 44.
[0104] It is an advantage of the disclosed method that conventional materials and equipment for extrusion and injection molding are useful for carrying out the method.No special equipment or material requirements are required for carrying out the disclosed method.Thus, any thermoplastic polymer or mixtures thereof that are useful for injection molding and / or for forming polymer foams can be usefully combined with any commercially useful physical blowing agent source using conventional techniques such as standard injection molding equipment, optionally with one or more additional materials as selected by the equipment operator.
[0105] In embodiments, thermoplastic polymers useful in conjunction with the methods, apparatus, and articles described herein include any thermoplastic or mixtures thereof known in the industry to be useful for injection molding or injection molding of polymer foam articles, and mixtures of such polymers. Useful polymers are characterized as having a melt flow viscosity suitable for use in injection molding, such as shot forming. Thus, thermoplastic polymers may contain a degree of crosslinking that is thermoreversible or does not otherwise prevent sufficient viscous melt flow for the injection molding process.
[0106] In embodiments, thermoplastic polymers useful in conjunction with the methods, apparatus, and articles described herein include olefins, such as polyethylene, polypropylene, polyα-olefins and various copolymers and branched / crosslinked variations thereof, including, but not limited to, low density polyethylene (LDPE), high density polyethylene (HDPE), linear low density polyethylene (LLDPE), thermoplastic polyolefin elastomers (TPE), ultra-high molecular weight polyethylene (UHMWPE), and the like; polyamides (PA), polyimides (PI), polyesters, such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), polyhydroxyalkanoates (PHAs), such as polyhydroxybutyrate (PHB), polycarbonates (PC), poly(lactic acid) (PLA), acrylonitrile-butadiene-styrene copolymers (ABS), polystyrene, thermal Polyurethanes, including thermoplastic polyurethane elastomers (PU, TPU), polycaprolactone, polyvinyl chloride (PVC), tetrafluoroethylene, polyethersulfone (PES), polyacetal, polyaramid, polyphenylene oxide (PPO), polybutylene, polybutadiene, polyacrylate, and methacrylate (acrylic) copolymers, ionomeric polymers (SURLYN® and similar ionically functionalized olefin copolymers), polyether-amide block copolymers (PEBAX®), polyaryletherketone (PAEK), polysulfone, polyphenylene sulfide (PPS), polyamide-imide copolymers, poly(butylene succinate), cellulosics, polysaccharides, and copolymers, alloys, admixtures, and mixtures thereof, without limitation, are usefully employed in conjunction with the methods described herein.
[0107] Regarding non-limiting uses of polymer blends and mixtures, we have found that mixed streams of recycled plastics are useful as thermoplastic polymers in embodiments. Thus, in embodiments, marine waste plastics are mixed streams of polymer waste collected from oceans and shorelines, with exemplary contents of 10%-90% polyolefin content, 10%-90% PET content, 1%-25% polystyrene content, and 1%-50% unknown polymer content. Such mixed plastic streams and waste plastic streams, including but not limited to those collected from oceans and shorelines, are also useful for forming molten polymer foams and polymer foam articles using the methods and apparatus described herein.
[0108] Physical blowing agent sources are widely available in the industry, and conditions useful for developing physical blowing agents during melt mixing are well understood and widely reported. Thus, any physical blowing agent source useful for injection molding, reaction injection molding, or other methods of making polymeric foams is useful herein for forming molten polymeric foams and solidified polymeric foam articles according to the methods, apparatus, and polymeric foam articles described herein. Physical blowing agents useful in connection with the methods and apparatus described herein include air, CO2, and N2, either in the form of beads, pellets, and the like, or in covert form, encapsulated within a thermoplastic material, and a chemical reaction generates CO2 or N2 when heated in a melt mixing apparatus. Such chemical reactions are preferably, but not limited to, exothermic or endothermic for their use in conjunction with the methods and apparatus disclosed herein. Suitable physical blowing agent sources include sodium bicarbonate, polycarboxylic acids such as citric acid or salts or esters thereof, such as compounds based on sodium citrate or the trimethyl ester of sodium citrate, mixtures of sodium bicarbonate and polycarboxylic acids such as citric acid, sulfonyl hydrazides including p-toluenesulfonyl hydrazide (p-TSH) and 4,4'-oxybis-(benzenesulfonyl hydrazide) (OBSH), pure and modified azodicarbonamide, semicarbazide, tetrazole, and diazinon. In any of the foregoing, the physical blowing agent source is optionally further encapsulated within a carrier resin designed to melt during heating, mixing, and collection of the shot.
[0109] In embodiments, useful physical blowing agent sources include commercially available compositions, such as those available from Clariant AG, Switzerland; HYDROCEROL® BIH70, HYDROCEROL® BIH CF-40-T, or HYDROCEROL® XH-901, available from RTP Company, Winona, MN; FCX7301, available from RTP Company, Winona, MN; FCX27314, available from CelChem LLC, Naples, FL; CELOGEN® 780, available from Galata Chemicals, Southbury, CT; ACTAFOAM® 780, available from Galata Chemicals, Southbury, CT; ACTAFOAM® AZ, available from ADEKA Polymer Additives Europe, Mulhouse, France; ORGATERMB.BA.20, available from Endex International, Rockford, IL; ENDEX1750 TM and FOAMAZOL, available from Bergen International, East Rutherford, NJ. TM Includes 57.
[0110] In some embodiments, the physical blowing agent source is a physical blowing agent, which is applied as a gas to a melt mixing device, such as a device similar to the extruder shown in Figures 1A-1B. In such embodiments, the gas is dissolved in the thermoplastic polymer by direct pressurized addition and mixing in the melt mixing device. In some embodiments, the gas is made a supercritical fluid by pressurization either prior to or simultaneously with dissolution into the molten thermoplastic polymer. The step of applying a physical blowing agent directly to an injection molding device is referred to in the industry as the MUCELL® process, as employed by Trexel Inc. (Wilmington, DE). Specialized equipment is required for this process, such as a regulated, pressurized fluid connection from a gas reservoir (tank, cylinder, etc.) to the inlet of the extruder device to form a pressurized relationship with the barrel as the thermoplastic polymer is also added to the barrel and melted. Where such specialized equipment is available, physical blowing agents are usefully employed as a source of physical blowing agent in conjunction with the methods described herein by direct application of the physical blowing agent to a thermoplastic polymer and one or more additional materials to form a molten pneumatic mixture.
[0111] The physical blowing agent source is added to the thermoplastic polymer and any optional one or more additional materials in an amount that targets the selected density reduction of the thermoplastic polymer according to the conventional techniques associated with the desired polymer foam density and the operation of the physical blowing agent and the physical blowing agent source to form the thermoplastic polymer foam. The amount of the physical blowing agent source added to the thermoplastic polymer is not particularly limited. Thus, we have found that a density reduction of up to 85% is achieved without the use of polymer or glass bubbles or equivalents, providing a polymer foam article having unique and surprising properties as reported below, and further having a targeted density reduction of up to 85%. As used herein, "density reduction" refers to the percent mass reduction in a polymer foam article compared to the same article without the addition of a physical blowing agent (source) to make the article (i.e., a polymer article that excludes or substantially excludes foam). Thus, in embodiments, the molten polymer foams and polymer foam articles described herein suitably provide a selected density reduction of up to 85%, e.g., 30%-85%, e.g., 35%-85%, 40%-85%, 45%-85%, 50%-85%, 55%-85%, 60%-85%, 65%-85%, 70%-85%, 75%-85%, 30%-35%, 35%-40%, 40%-50%, 50%-55%, 55%-60%, 60%-65%, 65%-70%, 70%-75%, 75%-80%, or 80%-85%, while excluding glass or polymer bubbles. The inclusion of glass or polymer bubbles further expands the available density reduction of polymer foam articles made according to the methods herein. In some embodiments, density reductions of greater than 85% may be achieved. Polymeric foam articles that benefit from density reduction may nevertheless be capable of withstanding temperatures up to 1,000 cm 3 Exceeding 1,000cm 3 ~5,000cm 3 , or an additional 5,000 cm 3 and molded articles having a volume exceeding 1,000 cm 3 Volume greater than 2cm and thickness greater than 1,000cm 3 ~5,000cm 3and a thickness of more than 2 cm, or 5,000 cm 3 The foam has been characterized as having a continuous polymer matrix throughout, including molded articles with volumes of greater than 100 mm and thicknesses of greater than 2 cm, with the foam being dispersed throughout.
[0112] As stated above, the amount of the physical blowing agent source added to the thermoplastic polymer is not particularly limited. Thus, we have found that up to 70% of the total volume of the polymer foam article comprises foam. The total volume of the foam as a percentage of the total volume of the polymer foam article is referred to as the "porosity" of the article. Thus, a porosity of up to about 70% is achieved without including polymer or glass bubbles or equivalents, providing a polymer foam article having unique and surprising properties reported below and further having a targeted porosity of up to 70% of the volume of the polymer foam article. Thus, in embodiments, the molten polymer foams and polymer foam articles described herein preferably provide a porosity of up to 70%, e.g., 5%-70%, 10%-70%, 15%-70%, 20%-70%, 25%-70%, 30%-70%, 35%-70%, 40%-70%, 45%-70%, 50%-70%, 55%-70%, 60%-70%, 5%-10%, 10%-15%, 15%-20%, 20%-25%, 25%-30%, 30%-35%, 35%-40%, 40%-50%, 50%-55%, 55%-60%, 60%-65%, or 65%-70%, while excluding glass or polymer bubbles. The inclusion of glass or polymer foam further expands the available porosity of polymer foam articles made according to the methods herein. In some embodiments, sections of greater than 70% porosity can be achieved. Polymer foam articles having 70% porosity can nevertheless be 5,000 cm 3 volume greater than 2cm, thickness greater than 5,000cm 3 The foam has been characterized as having a continuous polymer matrix throughout, with the foam dispersed therein, including molded articles having both a volume of greater than 100 mm and a thickness of greater than 2 cm.
[0113] In some embodiments, the thermoplastic polymer and the physical blowing agent source are admixed prior to application of the admixture to a melt mixing device for heating and mixing. In other embodiments, the thermoplastic polymer and the physical blowing agent source are added separately to the melt mixing device, such as by two different inlets or ports available for adding materials to the melt mixing device. In yet other embodiments, a solid mixture including both the thermoplastic polymer and the physical blowing agent source is added as a single input to a melt mixing device for heating and mixing.
[0114] In an embodiment, one or more additional materials are included or added to the melt mixing device along with the thermoplastic polymer and the physical blowing agent source. Such additional materials are preferably mixed or blended with the thermoplastic polymer, the physical blowing agent source, or both, or the one or more additional materials are added separately, such as by individual ports or inlets to the melt mixing device. Examples of suitable additional materials include colorants (dyes and pigments), stabilizers, brighteners, nucleating agents, fibers, particulates, and fillers. Specific examples of some suitable materials include talc, titanium dioxide, glass bubbles or beads, thermoplastic polymer particles, fibers, beads, or bubbles, and thermoset polymer particles, fibers, beads, or bubbles. Additional examples of suitable materials include fibers, such as glass fibers, carbon fibers, cellulose fibers and fibers containing cellulose, natural fibers such as cotton or wool fibers, and synthetic fibers, such as polyester, polyamide, or aramid fibers, including microfibers, nanofibers, crimped fibers, crushed or chopped fibers, phase separated and mixed fibers, such as bicomponent fibers containing any of the previously mentioned polymers, and thermosets formed from any of the previously mentioned polymers. Further examples of suitable additional materials are waste materials, sand, gravel, crushed stone, slag, recycled concrete and geosynthetic aggregates, and other biological, organic, and mineral waste streams and mixtures thereof, optionally further crushed or chopped, including woven or nonwoven fabrics, textiles, or papers. Further examples of suitable additional materials are minerals such as calcium carbonate and dolomite, clays such as montmorillonite, sepiolite, and bentonite, mica, wollastonite, hydromagnesium / huntite mixtures, synthetic minerals, silica agglomerates or colloids, aluminum hydroxide, alumina-silica composite colloids and particulates, halloysite nanotubes, magnesium hydroxide, basic magnesium carbonate, precipitated calcium carbonate, and antimony oxide. Further examples of suitable additional materials are carbonaceous fillers such as graphite, graphene, graphene quantum dots, carbon nanotubes, and C 60Further examples of suitable additional materials include thermally conductive fillers, such as boron nitride (BN) and surface treated BN.
[0115] In an embodiment, the one or more additional materials, along with the thermoplastic polymer and the source of physical blowing agent, comprise about 0.1% to 50% of the mass of the thermoplastic polymer, e.g., 0.1% to 45%, 0.1% to 40%, 0.1% to 35%, 0.1% to 30%, 0.1% to 25%, 0.1% to 20%, 0.1% to 15%, 0.1% to 10%, 0.1% to 9%, 0.1% to 8%, 0.1% to 7%, 0.1% to 6%, 0.1% to 5%, 0.1% to 4%, 0.1% to 3%, 0.1% to 2%, 0.1% to 1%, 1% to 50%, 2% to 50%, 3% to 50%, 4% of the mass of the thermoplastic polymer added to the melt mixing device. ~50%, 5%-50%, 6%-50%, 7%-50%, 8%-50%, 9%-50%, 10%-50%, 11%-50%, 12%-50%, 13%-50%, 14%-50%, 15%-50%, 20%-50%, 25%-50%, 30%-50%, 35%-50%, 40%-50%, 45%-50%, 0.1%-2%, 2%-5%, 5%-10%, 10%-15%, 15%-20%, 20%-25%, 25%-30%, 30%-35%, 35%-40%, 40%-45%, or 45%-50% is included or added to a melt mixing device to form a shot.
[0116] Thus, it will be appreciated by those skilled in the art that in a melt mixing device that is not an extruder, the following method will result in a molten polymer foam that possesses significant technical advantages as described in the following sections. A method of forming and collecting a molten polymer foam includes the steps of: heating and mixing a thermoplastic polymer and a physical blowing agent source to form a molten pneumatic mixture, where the temperature of the molten pneumatic mixture exceeds a critical temperature of the physical blowing agent source and the pressure applied to the molten pneumatic mixture is sufficient to substantially prevent the formation of bubbles; collecting a selected amount of the molten pneumatic mixture in a collection area; defining an expansion volume in the collection area adjacent to the molten pneumatic mixture that creates a pressure drop; maintaining the expansion volume for an expansion time period; and collecting the molten polymer foam from the collection area. In an embodiment, the molten pneumatic mixture is uninterrupted or substantially uninterrupted during the expansion period.
[0117] In some embodiments, collecting the molten polymer foam includes applying the molten polymer foam to a cavity defined by a mold and cooling the molten polymer foam below the melting temperature of the thermoplastic polymer to obtain a polymer foam article. In embodiments where the molten polymer foam is applied to the mold cavity, the cooled polymer foam article acquires the shape and dimensions of the mold, and the polymer foam is further characterized as a continuous polymer matrix with bubbles dispersed throughout the article. In embodiments, the molten polymer foam is applied to the mold cavity by allowing the molten polymer foam to flow and enter the mold cavity by gravity, and in some such embodiments, the flow is allowed to fall uninterrupted into the open cavity. In other embodiments, the molten polymer foam is applied to the forming element under pressurized flow. In embodiments, the molten polymer foam is delivered to the mold cavity by a fluid connection thereto from a nozzle or other means of delivery of the molten polymer foam from the collection area of the melt mixing device.
[0118] For example, in an embodiment, the extruder is adapted and designed to dispense the molten mixture from an outlet into a forming element, which is a die, defining a cavity therein and designed and adapted to receive a molten polymer mixture, such as a molten pneumatic mixture. In an embodiment, the forming element is a die, configured and adapted to receive the molten thermoplastic polymer dispensed from the outlet, and further, the die is generally characterized as defining a void or cavity having a selected shape and dimensions of a desired article.
[0119] In embodiments, dispensing from the extruder is accomplished by mechanical pushing, by applying gaseous pressure from within the barrel of the extruder, or a combination thereof. In other embodiments, the outlet, valve, gate, nozzle, or door to the collection area is simply opened after the expansion cycle has passed, and the molten polymer foam is allowed to flow uninterrupted through the outlet, and the melt flow is then directed to cooling or other processing equipment, or the melt flow is allowed to be poured into a forming element. In other embodiments, the forming element is fluidly connected to the outlet, and further designed and adapted to be filled with the molten mixture such that the molten mixture acquires a selected shape upon cooling and solidification. In some embodiments, the forming element is fluidly connected to the extruder outlet such that pressure is maintained between the collection area, the outlet, and the forming element or mold. Any conventional thermoplastic molding or forming process associated with injection molding of polymeric articles, such as polymeric foam articles, is suitably employed to mold the molten polymer foam described herein.
[0120] In embodiments where the molten polymer foam is allowed to flow uninterrupted through the outlet, or is forced under pressure out of the outlet without further impediment to the flow, the melt flow eventually impinges on a surface, such as a surface that is approximately perpendicular to the direction of the melt flow. We have found that flow under such circumstances then impinges on a surface, such as a surface that is approximately perpendicular to the direction of the melt flow, as described by Batty and Bridson, “Accurate Viscous Free Surfaces for Buckling, As reported by the “Computer Animation of Continuous Melt Flows” Symposium on Computer Animation, Dublin, July 2008, the molten polymer foam has been observed to acquire roughly cylindrical (coiled) and planar (folded) patterns during continuous melt flow. In embodiments, the molten polymer foam is allowed to flow, or “poured”, uninterrupted from the outlet of the melt mixing device into a mold configured as an open container. In embodiments, the open container mold is completely filled with the molten polymer foam, and in other embodiments, the open container mold is partially filled with the molten polymer foam.
[0121] In some embodiments related to the coiled melt flow described above, a substantially shear-free melt flow, or a substantially linear melt flow, or a melt flow that is substantially linear and shear-free, is provided by the fluid connection between the extruder outlet and the die cavity. In some such embodiments, the melt flow may obtain a coiled melt flow either by impinging on the vertical surface thereof, or by flowing down a substantially vertical wall or side of the die cavity and collecting at the bottom of the die cavity. A schematic of one such embodiment is shown in FIG. 41, which shows a variation of the extruder of FIGS. 1A-1B, where the die 26 of the apparatus 20 is mounted on a substantially horizontal surface 100. With reference to the elements as shown in FIGS. 1A-1B, the shutoff valve 37 is not present at the distal end 21b of the barrel 21; instead, in FIG. 41, the collection area 40 extends to a die valve 137 that is mounted proximate to the die cavity 39 defined in the die 26. The mold valve 137 is thus operable to define the collection area 40 or provide an outlet for dispensing the molten polymer foam via the generally linear horizontal flow 110 into the mold cavity 39. The mold valve 137 is mounted at a height H above the horizontal surface 100, i.e., a height H2 above the floor or bottom 120 of the mold 26 as mounted on the horizontal surface 100. Referring to FIG. 41 , the mold valve 137 is selectively opened to provide a fluid connection between the collection area 40 and the mold cavity 39. The mold valve 137 is thus selectively opened to provide a generally linear horizontal flow 110 of molten polymer foam entering the mold cavity 39. In response to entering the mold cavity 39, the linear flow flows downwardly over a distance H2, and in some embodiments acquires a coiled melt flow as it proceeds to fill the mold cavity 39. Other related variations of the methods and apparatus for providing a coiled melt flow as described herein are also contemplated.
[0122] In an embodiment, upon cooling the polymeric foam article and removing it from the open container or mold in which it is mounted, as shown in FIG. 41, coiled and folded flow patterns become visible on the surface of the article. Examples of such visible flow patterns can be seen, for example, in FIGS. 2-2 and 2-4. Upon cryogenic fracturing and microscopic inspection of the interior of a polymeric foam article formed using coiled and folded flow, the interior of the article is free or substantially free of flow patterns, interfaces, or other evidence of coils and folds. For example, cryogenic fracturing of such a polymeric foam article does not result in fracturing at any discernible interfaces between the coils and folds, and both macroscopic and microscopic inspection of the interior of such a polymeric foam article obtains a homogenous appearance to the flow patterns. The physical properties of such polymeric foam articles are consistent with those obtained by exposing a molten polymeric foam to a directed fluid flow or exposing a molten polymeric foam to a pressurized and directed fluid flow via a fluid connection between the outlet of a melt mixing device and a mold.
[0123] In some embodiments, the method herein includes substantially filling a mold formed according to the method described above with molten polymer foam, then cooling the molten polymer foam to form a solidified polymer foam, and in embodiments, further removing the solidified polymer foam article from the mold. In embodiments, the cooling step is to a temperature below the melting transition temperature of the thermoplastic polymer. In embodiments, the cooling step is to a temperature equilibrated with the ambient temperature of the surrounding environment. In some embodiments, the mold further includes one or more vents for pressure equalization within the mold while filling it with molten polymer foam, while in other embodiments, no vents are present. After cooling, the polymer foam article may be removed from the mold for further modification or use.
[0124] In accordance with any of the foregoing descriptions, Table 1 provides useful, but non-limiting examples of processing conditions that may be employed to make molten polymer foams using a conventional single screw extruder type reaction injection molding apparatus by further employing one or more representative thermoplastic polymers and a citric acid-based physical blowing agent source as indicated.
[0125] Table 1. Representative thermoplastic polymers and conditions useful for making and molding molten polymer foams. [Table 1]
[0126] In embodiments, mold dimensions usefully employed to form polymer foam articles made using the methods and materials disclosed herein include molds that define a cavity, or a series of cavities, that can be filled by a single shot of molten polymer foam. Thus, the size of the mold cavity is limited only by the size of the shot that can be constructed in the melt mixing device employed by the user. Up to 1×10 5 cm 3A representative mold cavity having a volume of 100 mm to 150 mm is useful for making large parts, such as automobile interior or exterior parts, I-beam structural parts, and other large plastic items that suitably employ polymer foam. Furthermore, the shape of the mold cavity is not particularly limited and may be complicated in terms of overall shape and even surface patterns and features, such as dumbbells, tableware, decorative globes with raised geographical features, human or animal or insect shapes, framework or packaging shapes for framing or encasing electronic items, appliances, automobiles, and the like, shapes for later placement and fitting of screws, bolts, and other non-thermoplastic items into or through the polymer foam article, and shapes recognizable as the like are all suitable mold shapes for molding polymer foam articles as described herein. In some embodiments, the cavity includes a thickness gradient of up to 300% for one or more regions of the cavity.
[0127] In accordance with any of the foregoing descriptions, Table 2 provides useful, but non-limiting examples of mold cavity volumes and mold dimensions useful for shaping molten polymer foam, either by pressurized flow or by uninterrupted flow of the molten polymer foam into a mold. In addition, mold cavity volumes and mold dimensions useful for shaping molten polymer foam, either by pressurized flow or by uninterrupted flow of the molten polymer foam into a mold, are also provided. 3 Larger mold volumes such as 150 mm or larger are also useful if the shot mass is suitably increased.
[0128] Table 2. Representative mold cavity volumes and dimensions useful for molding molten polymer foams. [Table 2-1] [Table 2-2]
[0129] Any of the methods, processes, uses, machines, devices, or individual features thereof described above can be freely combined with each other to form polymer foams and polymer foam articles having unique and surprising properties. Thus, in an embodiment, a polymer foam article is formed using the methods, materials, and devices described above. The polymer foam article is a discrete monolithic object made by forming or molding a molten polymer foam according to any of the methods and materials disclosed above and variations thereof, which can be combined in any part and in any manner to form a molten polymer foam as described above.
[0130] Thus, the terminology used to refer to the methods, materials, and apparatus in the foregoing discussion will be used below to refer to articles made using one or more of the methods, materials, and apparatus encompassed in the foregoing discussion.
[0131] In an embodiment, any combination of the foregoing methods results in the formation of a polymeric foam article comprising, consisting essentially of, or consisting of a continuous thermoplastic polymer matrix that defines a plurality of bubbles. The continuous thermoplastic polymer matrix comprises, consists of, or consists essentially of a solid thermoplastic polymer, i.e., the thermoplastic polymer is at a temperature below its melting transition temperature. In an embodiment, the continuous thermoplastic polymer matrix further comprises one or more additional materials dispersed in the solid thermoplastic polymer.
[0132] The polymeric foam article obtains a selected percentage density reduction based on the amount of physical blowing agent source added to the shot based on the density of the thermoplastic polymer and any other materials added to form the polymeric foam. In embodiments, density reductions of 30%, 40%, 50%, 60%, 70% and even up to 80%-85% are selected by the user. In embodiments, density reductions of up to 85% are achieved solely through the presence of bubbles intermittently dispersed within the polymer matrix. In embodiments, the polymeric foam article excludes hollow particulates, such as polymer or glass bubbles, that are added to the shot prior to forming the polymeric foam article using the methods and apparatus described herein.
[0133] Further, in conjunction with the reduced density, as noted above, the polymeric foam articles herein are characterized as having a continuous thermoplastic polymer matrix throughout, or substantially throughout, the entirety of the polymeric foam articles. We have found that large-sized polymeric foam articles may be suitably formed from the molten polymeric foams disclosed herein to include a continuous polymer matrix that defines a plurality of cells. A "large-sized" article is one that is larger than 1,000 cm 3 More than, for example, 2,000 cm 3 Over 3,000cm 3 Over 4,000cm 3 or more than 5,000 cm 3 or more than 1,000cm 3 ~5,000cm 3 Any volume up to 10,000cm 3 , up to 20,000cm 3 , up to 50,000cm 3 , or even up to 100,000 cm 3, or greater. Thus, large polymer foam articles may be suitably formed to include a continuous polymer matrix that defines multiple bubbles throughout. The volume of the article is limited only by the size of the mold cavity and the size of the shot that may be collected in the melt mixing device. In embodiments, large articles are formed from a single shot dispensed from a single outlet of the melt mixing device, i.e., without splitting into multiple simultaneous distribution pipes, nozzles, or other methods of directing multiple melt streams simultaneously into a single mold cavity.
[0134] In addition, we have found that thick polymeric foam articles can be suitably formed to include a continuous polymeric matrix that defines a plurality of bubbles. Thickness, as used herein, refers to the linear distance through the interior of a polymeric foam article between any two points on its surface. A "thick" article is defined as having a thickness of 2 cm or more, for example, 3 cm, 4 cm, 5 cm, 6 cm, 7 cm, 8 cm, 9 cm, 10 cm, 15 cm, 20 cm, 25 cm, 30 cm, 35 cm, 40 cm, 45 cm, or even 50 cm or more. In some embodiments, polymeric foam articles that are characterized as both large and thick are formed using the methods and materials described herein, and further, large and thick polymeric foam articles are nevertheless characterized as having a continuous polymeric matrix that defines a plurality of bubbles throughout the article. In embodiments, large, thick articles are formed from a single shot dispensed from a single outlet of the melt mixing device, i.e., without splitting the molten polymer foam stream into multiple simultaneous distribution pipes, nozzles, or other methods of directing multiple melt streams simultaneously into a single mold cavity.
[0135] The manufacture of large, thick, or large and thick polymeric foam articles is problematic in the industry due to the cooling gradient of the molten foam after being dispensed into a cavity having such dimensions. The interior of such articles tends to cool very slowly, and a portion of the thermoplastic polymer disposed in the mold cavity may remain above its melting temperature, allowing significant coalescence of the foam to occur before the thermoplastic solidifies (reaches a temperature below its melting transition temperature). In sharp contrast, we have found that large, thick, and large and thick articles are successfully formed using the methods, materials, and apparatus disclosed herein, and further, the formed polymeric foam articles are characterized by a continuous polymeric matrix with bubbles dispersed throughout the article. Cooling the interior of larger articles at a slower rate shows little or no evidence of foam coalescence during cooling. The bubbles remain intact or substantially intact during cooling of the molten polymeric foam and do not coalesce during cooling, resulting in a continuous polymeric matrix regardless of the size, thickness, or volume of the polymeric foam article formed.
[0136] This feature of the polymer foam articles described herein is surprising and unexpected, as prior art methods result in foams that tend to undergo foam coalescence during cooling. Thus, prior art molten polymer foams placed within the interior volume of a mold may cool slowly enough to allow the foam to completely coalesce, such that the interior of a large or thick article formed using conventional polymer foaming methods may acquire very large voids or even completely collapsed structures therein. In sharp contrast, molten polymer foams formed according to the present method do not undergo substantial foam coalescence or collapse of the continuous polymer matrix during cooling of the molten polymer foam. Thus, large and thick polymer foam articles with a continuous polymer matrix throughout are achieved using the methods, materials, and apparatus described herein.
[0137] The continuous polymer matrix as a structural feature of the polymer foam article according to the above-mentioned method, apparatus, and material is characterized as existing throughout the entire polymer foam article, including its surface area. The surface area may be preferably characterized as the interior area of the polymer foam article that is 500 microns or less from the surface. The surface area as defined herein is the portion of the foam article's area, conventionally referred to as the "skin layer", which is the area that is free or substantially free of foam in the polymer foam article made using conventional methods. Conventionally formed foam articles include a skin layer that is at least as thick as the surface area, i.e., 500 microns thick, but in many cases the skin layer is much thicker and may extend as far as 1 mm, 1.5 mm, 2 mm, 2.5 mm, or even 3 mm away from the surface of the article. However, the polymer foam article formed using the method of the present disclosure obtains a true foam structure from its surface through its entire thickness and volume. In embodiments, microscopic inspection reveals evidence of bubbles on the surface of polymeric foam articles formed using the conditions, processes, and materials disclosed herein. Thus, the methods disclosed herein obtain unexpected results in view of the continuous nature of the polymeric matrix structure throughout the entirety of a polymeric foam article, in any direction and within the interior of a very large and / or thick polymeric foam article, and also in all of its areas, including within the surface and surface regions of the article.
[0138] The following examples include an analysis of the surface regions of several polymeric foam articles made using the methods disclosed herein and exhibiting the present continuous foam structure. Macroscopically, the polymeric foam articles made using the methods disclosed herein may appear to have a skin layer, i.e., the surface region of the article may appear different from the interior region of the article. However, we have found that the surface region of the polymeric foam articles made by the present methods contains a plurality of compressed bubbles, in sharp contrast to the skin layer, which is characterized by the absence of bubbles. Macroscopically, the compressed bubbles produce an appearance suggestive of a skin layer. However, microscopic inspection reveals that the visually apparent difference results from a "flattening" or compressed arrangement of the continuous polymer matrix near the surface of the article.
[0139] Thus, as seen, for example, in Figures 17 and 18, there is a gradual transition from spherical to compressed foam moving toward the surface of a polymeric foam article formed by employing the conditions, processes, and materials disclosed herein. Thus, in an embodiment, the surface region of a polymeric foam article made using the methods disclosed herein comprises a plurality of compressed foams. In an embodiment, the compressed foam is present within the surface region of a polymeric foam article made using the methods disclosed herein. In some such embodiments, the compressed foam is present within an interior area of the polymeric foam article that is 500 microns or less from the surface. In some such embodiments, the compressed foam is present within an interior area of the polymeric foam article that is as far away as 2 cm from the surface. Compressed foam is defined as a foam having a circularity of less than 1, with a circularity value of zero representing a completely non-spherical foam and a value of 1 representing a perfectly spherical foam. In embodiments, bubbles having a circularity of less than 0.9 are observed within a surface region of the foamed polymer article, and further, 10% to 90%, or 10% to 80%, or 10% to 70%, or 10% to 60%, or 10% to 50%, or 10% to 40%, or 10% to 30%, or 10% to 20%, or 20% to 80%, or 20% to 70%, or 20% to 60%, or 20% to 50%, or 20% to 40%, or 20% to 30%, or 30% to 70%, or 30% to 60%, or 30% to 50%, or 30% to 40% of the bubbles within the surface region have a circularity of 0.9 or less. In an embodiment, the average circularity within a surface region of the foamed polymer article is from 0.70 to 0.95, e.g., from 0.75 to 0.95, or from 0.80 to 0.95, or from 0.85 to 0.95, or from 0.90 to 0.95, or from 0.70 to 0.90, or from 0.70 to 0.85, or from 0.70 to 0.80, or from 0.70 to 0.75, or from 0.70 to 0.75, or from 0.75 to 0.80, or from 0.80 to 0.85, or from 0.85 to 0.90, or from 0.90 to 0.95.
[0140] In embodiments, the compressed foam is present within the polymeric foam article greater than 500 microns from its surface. For example, in embodiments, the compressed foam is present up to 1 mm from the surface of the polymeric foam article, or up to 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 1 cm, or more from its surface. In some embodiments, the area of compressed foam within a polymeric foam article is between 0.01% and 70% of the total volume of the article, e.g., between 0.1% and 70%, or between 0.5% and 70%, or between 1% and 70%, or between 2% and 70%, or between 3% and 70%, or between 4% and 70%, or between 5% and 70%, or between 6% and 70%, or between 7% and 70%, or between 8% and 70%, or between 9% and 70%, or between 10% and 70%, or between 15% and 70%, or between 20% and 70%, or between 30% and 70%, or between 40% and 70%, or between 50% and 60%. % to 70%, or 60% to 70%, or 0.01% to 60%, or 0.01% to 60%, or 0.01% to 50%, or 0.01% to 40%, or 0.01% to 30%, or 0.01% to 20%, or 0.01% to 10%, or 0.01% to 9%, or 0.01% to 8%, or 0.01% to 7%, or 0.01% to 6%, or 0.01% to 5%, or 0.01% to 4%, or 0.01% to 3%, or 0.01% to 2%, or 0.01% to 1%, or 0.01% to 0.1%.
[0141] 12 and 14 show plots of average bubble size and average bubble count versus average bubble circularity for two polymeric foam articles made using the methods of the present disclosure. Quantitative analysis of bubble size and distribution reveals an inverse relationship between average bubble size and bubble circularity, and an inverse relationship between average bubble size and bubble count.
[0142] FIG. 18 additionally shows visual evidence that bubbles are present at the surface of a polymeric foam article formed using the methods, materials, and apparatus as described herein. FIG. 18 additionally shows visual evidence that a plurality of compressed bubbles are present substantially 500 microns from the surface of a polymeric foam article formed using the methods, materials, and apparatus as described herein. In this sense, the polymeric foam article of the present disclosure obtains a significant difference from prior art foam articles. The "skin layer," i.e., the first 500 microns of the thickness of a foam article made by a conventional process, is free of bubbles or substantially free of bubbles, whereas it is characteristic of prior art foam articles that the bubbles are generally spherical, regardless of where they are located. Thus, at thicknesses within a conventional foam article where bubbles are observed, they are generally spherical, with a circularity of approximately or about 1. Compressed bubbles are not formed using conventional methodologies for making foam articles, and therefore, a distribution of foam circularity is not observed in such conventional foam articles. Furthermore, foam is not even formed within the first 500 microns thickness of foam articles made by conventional processes, therefore no comparison with respect to foam is drawn with respect to the surface area of foamed polymer articles as described herein and foam articles made using conventional injection molding methods.
[0143] Moreover, the conditions, processes, and materials disclosed herein are preferably optimized to form polymeric foam articles with different physical properties depending on the targeted end use or application. For example, the density of the polymeric foam article is preferably varied as a function of expansion volume. By lowering the expansion volume, the density of the resulting polymeric foam article is reduced in a generally linear manner, for example, as shown in FIG. 5. Also, as can be seen in FIG. 5, increasing the expansion time period results in a denser polymeric foam article. Such conditions and other variables, all within the scope of the conditions, methods, and materials disclosed herein, are preferably used to vary the physical properties of the resulting polymeric foam article.
[0144] In one variation of the conditions, processes, and materials disclosed herein, the molten polymer foam is preferably dispensed by splitting the molten polymer foam stream into two, three, four, or more paths toward multiple molds or mold sections for forming multiple polymer foam articles from a single shot. In another variation of the conditions, processes, and materials disclosed herein, two shots are used to fill a single mold, the first shot differing from the second shot in terms of thermoplastic polymer content or ratio of mixed polymers, source of physical blowing agent, optionally one or more additional materials, density, porosity, depth of compressed foam region, or some other material or physical property difference.
[0145] In another variation of the conditions, processes, and materials disclosed herein, polymeric foam articles made using the methods disclosed herein were subjected to fastener pull-out testing in accordance with ASTM D6117. The polymeric foam articles obtain superior pull-out strength to foam articles made using traditional foaming methods. Furthermore, the polymeric foam articles formed using the materials, methods, and apparatus disclosed herein do not require pre-drilling, tapping, or engineering of fastener locations.
[0146] In yet another variation of the conditions, processes, and materials disclosed herein, polymeric foam articles made using the methods disclosed herein were subjected to impact testing. Using the guidelines of the National Institute of Justice (NIJ) "Ballistic Resistance of Body Armor NIJ Standard-0101.06", a series of 3-inch thick polymeric foam articles were formed from polyether-amide block copolymer (PEBAX®), linear low density polyethylene (LLDPE), and polypropylene using a citric acid-based physical blowing agent source. Polymeric foam articles made using all three of these thermoplastic polymers were found to stop .22 caliber LR handgun bullets and pass NIJ Level I, and to stop 9mm LUGER® handgun bullets and pass NIJ Level II and IIA. EXAMPLES
[0147] Experimental Section
[0148] The following examples are intended to further illustrate the present invention and are not intended to limit the scope of the present invention in any manner. Examples 1 and 11 were performed on an Engel Duo 550 Ton injection molding machine (available from Engel Machinery Inc., York, PA, USA). Examples 2-4 were performed on a Van Dorn 300 injection molding machine (available from Van Dorn Demag, Strongsville, Ohio, USA). Unless otherwise indicated, the remaining examples were performed on an Engel Victory 340 Ton injection molding machine (available from Engel Machinery Inc., York, PA, USA).
[0149] In the examples of this specification, "cc" means "cubic centimeter" (cm 3 ) and "sec" means "seconds." Standard Foam Molding and MFIM
[0150] In the examples herein, two direct injection expanded foam molding techniques were employed, referred to herein as "standard foam molding" and "molten foam injection molding" ("MFIM").
[0151] In standard foam molding, the following general procedure was used: A) A mixture was prepared by blending the polymer (which may be in the form of pellets, powder, beads, granules, and the like) with the blowing agent (expanding agent) and any other additives such as fillers. The mixture was introduced into the injection unit, and the rotating injection unit screw moved the mixture forward in the injection unit barrel, thus forming a heated fluid material, usually according to an injection molding process. B) A set volume of material was dosed at the front of the injection unit barrel by the rotation of the screw, thus moving the set volume from the feed zone to the front of the screw. During this feed step, the screw was rotated, translating the molten mixture forward into the space in the barrel between the screw and the nozzle, thereby providing the set volume. C) The molten mixture was injected into the mold cavity by the forward translation of the screw and / or the rotation of the screw.
[0152] In the molten foam injection molding (MFIM) process, the following general procedure was used: A) A mixture was prepared by blending the polymer (which may be in the form of plastic particles, pellets, powder, beads, granules, and the like) with chemical foaming agents and any other additives such as fillers. The mixture was introduced into the injection unit, and the rotating injection unit screw moved the material forward in the injection unit barrel, thus forming a heated fluid material, usually according to an injection molding process. B) A set volume of material was dosed at the front of the injection unit barrel by the rotation of the screw, thus moving the set volume from the feed zone to the front of the screw. During this feed step, the screw was rotated, moving the material between the screw and the nozzle, thereby providing the set volume. C) Once the material was moved to the front of the screw, in a step referred to herein as "depressurization", the screw was moved backwards away from the nozzle without rotation, or substantially without rotation, to avoid more of the material moving to the front of the screw.
[0153] A mixture-free space between the screw and nozzle was created in the barrel, the intentional space having a volume, referred to herein as the "decompression volume." D) Material was placed in the barrel between the screw and nozzle for a period of time, referred to herein as the "decompression time." During the decompression time, the material foamed due to the pressure drop created by the space added in step (C). E) The molten foam was injected into the mold cavity by forward translation of the screw and / or rotation of the screw.
[0154] Example 1 Two parts were foam molded using a blend of low density polyethylene blended with 2% by weight Hydrocerol® BIH70 blowing agent available from Clariant AG, Muttenz, Switzerland. Molding was performed using an Engel Duo 550 Ton injection molding machine available from Engel Machinery Inc., York, PA, USA. The mold cavity was (nearly) spherical in shape with a diameter of 6 inches (15.24 cm). The first part was molded using the standard foam molding process and the second part was molded using the MFIM process. An aluminum mold with a cold sprue and runner system feeding a 6 inch diameter spherical cavity was employed for both parts. The melt delivery system for each part was identical for the majority of processing conditions. The process settings for the MFIM process and the standard foam molding process used as controls are detailed in Table 3. Parts were produced from each process of approximately equal mass. [Table 3]
[0155] The first and second parts were photographed. Figure 2-1 is a photographic image of the first part molded using a standard foam molding process. As can be seen in the image, the standard foam process did not result in the part filling the mold cavity, and the part did not conform to the shape of the spherical cavity of the mold.
[0156] Figure 2-2 is a photographic image of a second part molded using the MFIM process. As can be seen in the image, the MFIM process resulted in a part that completely or substantially filled the spherical mold cavity, and the part conformed or substantially conformed to the shape of the spherical cavity of the mold.
[0157] The first part, molded using a standard foam molding process, was cut into two pieces. Figures 2-3 and 2-5 are photographic images of one of the pieces of the part made according to the standard foam molding process. As can be seen in the images, the first part contained a large hollow cavity.
[0158] The second part, molded according to the MFIM process, was cut into two pieces. Figures 2-4 and 2-6 are photographic images of one of the pieces of the second part. As can be seen in the images, the second part lacked the large hollow cavities of the standard foam process part. The MFIM part had a cellular structure throughout.
[0159] Example 2 Two parts were formed by foam injection molding, part A followed the standard foam molding process and part B followed the MFIM process. In both processes, LDPE / talc pellets were dry blended with the blowing agent and mixed during loading into the molding machine.
[0160] For part B, a mixture of low density polyethylene (LDPE), talc, and Hydrocerol® BIH70 was formed and fed into a Van Dorn 300 injection molding machine to provide a polymer shot inside the barrel. After the shot was accumulated in front of the screw, the screw was translated backwards away from the injection nozzle without rotating, according to the MFIM method, creating a space between the screw and the nozzle, which has a vacuum volume. The mixture was then foamed into the space prior to injection into the mold.
[0161] The same procedure was used for part A, except that the screw was not retracted away from the nozzle after the shot was accumulated in front of the screw, i.e., the vacuum volume was zero. The shot was timed to fill the mold cavity under standard foam molding conditions with a target of 10% weight reduction for a solid part.
[0162] Tables 4-7 below show the polymer, mold, machine, and processing settings used in Example 2. [Table 4] [Table 5] [Table 6] [Table 7]
[0163] Parts A and B were each cut in half to reveal the cross section. Figures 3A and 3B show the resulting cross sections of Parts A and B, respectively. As shown in Figure 3A, Part A had a thick outer region extending approximately 0.8 inches (20.3 mm) from the surface, indicating that over 50% of the molded part was completely solid. The density of Part A was 0.84 g / cc.
[0164] Figure 3B shows a cross section of part B, which was molded according to the MFIM process using the settings shown in Tables 4 and 5. As can be seen in Figure 3B, part B had a foam structure, including a distribution of cell sizes and shapes. Solid non-foamed outer regions were nearly absent in part B. The density of part B was 0.35 g / cc.
[0165] A spherical cavity mold was used to form two more parts, part C and part D, by foam injection molding. The same mixture composition of LDPE, talc, Hydrocerol® BIH70 was used to form parts C and D. Part C was made by the MFIM process and part D by a standard foam molding process. Both processes produced spherical or near-spherical parts with a 6 inch (15.24 cm) diameter. Parts C and D were cut through the middle (widest part) into two pieces to expose the cross-sections of the parts. FIG. 4A is a photographic image of the cross-section of part C (471 g, required 160 seconds cooling time) made by the MFIM process. FIG. 4B is a photographic image of part D (1,360 g, required 800 seconds cooling time) molded using the standard foaming process target. This is a photographic image of a cross section of the endothelial cell (requested).
[0166] Similar results were obtained with the block mold. Part C, made according to the MFIM process, exhibited cells throughout the part, while Part D, made according to the standard foam molding process, exhibited areas adjacent the outer surface of the part that were free of cells or substantially free of cells ("solid"). Part C was less dense than Part D.
[0167] Example 3 In Example 3, block parts were molded using the MFIM process at various vacuum volumes (Prototype A) and various vacuum volumes and vacuum times (Prototype B).
[0168] Tables 8-10 show the material compositions, mold geometry information, and processing settings used for Prototypes A and B. [Table 8] [Table 9]
[0169] The composite LDPE / talc pellets were mixed with the blowing agent immediately prior to molding.
[0170] Prototype A
[0171] In Prototype A, all variables were held constant except for the volume ratio of polymer to vacuum volume (empty space) in the barrel prior to injection. The sample run-by-run settings for Prototype A are shown in Table 10. [Table 10]
[0172] The volume of molten foam injected into the polymer cavity was constant, but the density of the molten foam was a function of the polymer shot / vacuum volume ratio, which was varied to give the parts weights and densities as shown in Table 11. [Table 11]
[0173] The results in Table 11 show that by decreasing the mass and volume of polymer within the molten foam shot with a corresponding increase in vacuum volume, the density of the resulting part can be varied.
[0174] Prototype B
[0175] For Prototype B, five molds under the same conditions as Prototype A were performed three times, one using a decompression time of 20 seconds (same as Prototype A), one using a decompression time of 70 seconds, and one using a decompression time of 120 seconds. The 15 resulting foam molded parts were weighed and density calculated using the volume of the mold cavity. Part density was plotted as a function of decompression volume for each of the three decompression times. The plot is shown in FIG. 5. As can be seen in FIG. 5, part density varied as a function of decompression volume. Additionally, as shown in FIG. 5, the longer the decompression time, the denser the part.
[0176] Example 4 In Example 4, two series of prototypes, Series I and Series II, were run using the MFIM process. In Series I, a constant injection rate was used, but the mold closure height was varied. In Series II, the mold closure height was increased with increasing injection rate. In Series II, all conditions were kept constant except for the injection rate (cc / sec) and the mold closure height. In the prototypes, LDPE / talc pellets were dry blended with the blowing agent and mixed during loading into the molding machine.
[0177] Tables 12-13 below show the material composition of the composites to be injected and the basic mold configuration used for prototyping. [Table 12] [Table 13]
[0178] Series I
[0179] In Series I, an injection rate of 394 cubic centimeters per second was used and three prototypes were run: Prototype A had a mold closure height of 1.02 mm and produced part A, Prototype B had a mold closure height of 0.76 mm and produced part B, and Prototype C had a mold closure height of 0.51 mm and produced part C. The settings for the Series I prototypes are shown in Table 14. [Table 14]
[0180] During each molding cycle (each of Prototype A, Prototype B, and Prototype C), a strain gauge (Kistler surface strain sensor type 9232A, available from Kistler Holding AG, Winterthur, Switzerland) was mounted directly on or inside the mold cavity. The strain sensor contained two piezoelectric sensors that measured the strain of the aluminum cavity as a function of time during the molding cycle. The strain measurements were used as an indirect measure of the forces acting on the surface of the mold cavity resulting from the injection of the molten foam and any subsequent additional foaming that occurred within the mold cavity. The cavity strain measurements are shown in FIG. 6, where for Prototype A, there is a 1.02 mm gap height (line A), for Prototype B, there is a 0.76 mm mold closure height (line B), and for Prototype C, there is a 0.51 mm mold closure height (line C). In FIG. 6, the strain (unit extension per unit length) is plotted against time in seconds. The strain curves show that the pressure was higher in prototype C than prototype B, which was higher than prototype A.
[0181] 7 includes photographic images showing side, top, perspective, and bottom views of parts A, B, and C. Parts A and B showed evidence of crushing because the parts did not adequately conform to the mold cavity shape. Part A showed more crushing than part B. Part C was more fully formed than either part A or B in that the edges of part C were better defined, part C conformed better to the mold cavity shape, and the interior of the part appeared more homogeneous.
[0182] It was believed that the part could partially collapse within the cavity during molding if sufficient pressure was not provided to stabilize the foam within the cavity during solidification. Therefore, in Series II, the mold was closed more tightly at a slower injection rate to maintain sufficient pressure to prevent the part from collapsing during molding.
[0183] Series II
[0184] In Series II, the gap between the mold halves, i.e., the mold closure height, was systematically decreased as the pour rate was decreased. The molding conditions used were the same as in Series I, but the pour rates and mold closure heights used were as shown in Table 15. [Table 15]
[0185] Four parts were produced as parts A', B', C', and D' in prototypes A', B', C', and D', respectively.
[0186] Parts A', B', C', and D' were each cut in two and the cross sections were photographed. The photographic images are shown in Figure 8. In order to produce parts that would not collapse before solidifying, the mold halves had to be gradually closed until they were actually pressed together (as indicated by the negative dimensions), as shown in Table 15.
[0187] Parts A', B', C', and D' showed no evidence of crushing and appeared fairly uniform with well-defined edges and surfaces. Thus, parts were made using the MFIM process using significantly different injection rates by controlling the pressure within the cavity during injection, for example, by varying the mold closure height.
[0188] Example 5 In Example 5, the same LDPE composite material as in Examples 1-3 was used in a non-standard two cavity mold with molding parameters as shown in Tables 16-18. [Table 16] [Table 17] [Table 18]
[0189] Example 5 produced part 51 shown in Figure 9. During injection, the melted molten foam enters through sprue 52 and splits into two separate channels, filling part 51 substantially simultaneously. Thus, the MFIM process can be used to form parts by splitting the melt into multiple channels in a mold.
[0190] Example 6 The first part was molded using a 15 wt% talc / 85 wt% polycarbonate composite formulation and compounded with 3 wt% Hydrocerol® XH-901 prior to loading into the injection molding machine. The first part was formed using the MFIM process. Process details are provided in Tables 19 and 20. The part was made using a 4×2×2 block mold (5.08×10.16×10.16 cm) with a mold cavity volume of 524.4 cc and a sprue volume of 17.4 cc. The sprue was cut from the part and the part was then subjected to x-ray laminography to quantify the cell structure formed within the 5.08×10.16×10.16 cm geometry. [Table 19] [Table 20]
[0191] X-ray tomography was performed using a Zeiss Metrotom 800 130 kV imaging system (available from Carl Zeiss AG, Oberkochen, Germany). The instrument measured the attenuation of X-ray radiation due to the component geometry and the density of the materials used. Column data was calculated using the Feldkamp reconstruction algorithm, which is a standard technique in the industry. The instrument had a 1,536 x 1,920 pixel flat panel detector for an ultimate resolution of 3.5 μm under the conditions of the measurements.
[0192] A conformal image of a full Zeiss 3D tomographic scan of the first part is shown in Figure 10, where the solid polymer section is shown as transparent, the cells are shaded for visualization, and the cutting plane AA for a single cross section is indicated. Figure 11 is a single plane cross section AA selected from the X-ray data where threshold analysis has been applied to enable discrete cell identification and subsequent quantitative analysis.
[0193] The circularity of the cross sections of the cells was obtained. These cross-sectional circularities were used as a measure of the sphericity of the cells. Hence, circularity and sphericity are used synonymously in the examples. Quantitative analysis, shown in FIG. 12, revealed the cell distribution of both count and average size as a function of the circularity of each cell. A circularity value of zero represents a perfectly non-spherical cell, and a value of one represents a perfectly spherical cell. The data showed the distribution of cell sizes and shapes. Except for the most deformed cells (indicated by 0.1-0.2 on the circularity scale), there was an inverse relationship between the average cell size and the number of cells for a given circularity. Furthermore, there is also an inverse relationship between the average cell size and the number of cells.
[0194] Using the MFIM process, a second spherical part with a diameter of 6 inches (15.24 cm) was molded from low density polyethylene (LDPE) using the polymer formulation and processing parameters as outlined in Tables 21 and 22. The LDPE / talc pellets were dry blended with the blowing agent Hydrocerol® BIH70 and mixed during loading into the molding machine. [Table 21] [Table 22]
[0195] Figure 13 is an X-ray tomography image of a cross-section of a sphere. As can be seen in Figure 13, the outer region contained numerous smaller cell sizes with larger cells in the central region.
[0196] FIG. 14 shows a plot of average cell size and average cell count against average cell circularity, revealing an inverse relationship between average cell size and circularity, and between average cell size and number of cells.
[0197] Example 7 The MFIM process produced LDPE composite spheres (92% by weight polymer, 5% by weight talc, and 3% by weight Hydrocerol®) with a diameter of 3 inches (7.62 cm). BIH70) and the resulting foam cell structure is detailed in Figures 15-18. Molding conditions are provided in Table 23. Parts were molded on an Engel Victory 340 Ton injection molding press in a custom designed water-cooled aluminum mold. The mold cavity volume was 15.38 in. 3 (252cc) and the shot size is 5 inches 3 (82cc) and the reduced pressure volume in the barrel is 5 inches 3 (82 cc). Decompression time was 77 seconds. The molded part weight was 80.31 g, resulting in a final part density of 0.32 g / cc. [Table 23]
[0198] After removal from the mold, the parts were aged under ambient conditions for 24 hours, then scored and submerged in liquid nitrogen for 2 minutes. After removal from the liquid nitrogen, the spheres were fractured along the scored surface lines and the fracture surfaces were imaged using an Environmental Scanning Electron Microscope (ESEM) (FEI Quanta FEG650). The images shown in Figures 15-18 are photomicrographs at various magnifications taken of the fracture surfaces of the sphere parts using a large electric field detector, i.e., 5.0 kV and 40 Pa pressure.
[0199] The white boxes in Figure 15 indicate areas detailed in Figure 16. The white boxes in Figure 16 indicate areas detailed in Figure 17.
[0200] In FIG. 17, the cells on the left of the image are larger and relatively spherical, while those cells on the right side of the picture appear increasingly flattened as they approach the surface of the sphere.
[0201] The image in Figure 18 details the area indicated by the white box in Figure 17. As can be seen in Figure 18, there is a gradual transition from spherical to "flattened" or compressed cells moving towards the surface of the part.
[0202] Example 8 To establish baseline differences between standard thickness parts produced under standard foam molding conditions, a recently published study of standard foam injection molding (Paultkiewicz et al, Cellular Polymers 39,3-30(2020)) was used to establish molding parameter baselines using a 16-step statistical analysis design of experiment (DOE) approach. Materials (standard molding grade polypropylene with 0, 10, and 20 wt% talc and 0, 1, and 2 wt% Hydrocerol® BIH70 (blowing agent)) were compounded to specifications outlined in the publication to closely mimic the baseline study. The study was designed to investigate the effect of blowing agent concentration, talc content, and process conditions on selected properties of injection molded foam parts. A standard ISO tensile specimen mold was used with cavity dimensions of 4.1 mm thickness, 10 mm width at gauge length, and 170 mm length. No special venting was developed for the O specimen mold. After ensuring that the injection molding machine, material formulation, and process window were capable of replicating the results published by Paultkiewicz et al., a second study was conducted using process variables specific to MFIM, specifically, decompression volume and decompression time, while pressure and hold time (critical variables in the published study) were set to constant values of zero kN and zero seconds, respectively.
[0203] Molding was completed using an Engel Victory 340 Ton machine equipped with water cooling. The constant and variable process conditions used are shown in Table 24 for both the "standard" foam molding process and the MFIM molding process. [Table 24]
[0204] The designed studies called for 16 combinations of processing conditions / polymer formulations (16 runs) for each standard and MFIM molding study. Multiple replicates of each run were performed to produce replicate parts for each run. Table 25 outlines the variations between runs in both the standard and MFIM designed runs. The runs were performed in a random order to avoid bias. The L / T ratio for the ISO tensile specimens is 40.5. [Table 25-1] [Table 25-2]
[0205] After molding the 32 unique process combinations of the two 16-step DOE studies, five samples from each series were mechanically tested for tensile strength and the fracture surfaces were imaged after fracture. A representative selection of ISO specimen cross sections from steps 10, 11, 14, and 15 of the standard foam molding process are shown in Figure 19, and a representative selection of ISO specimen cross sections from steps 9, 10, 15, and 16 of the MFIM process are shown in Figure 20.
[0206] The differences between standard foam molding techniques as adopted from recent literature and the MFIM process are evident when examining the cross-sectional images. The structure in the standard process specimen consists of relatively few, but well-defined, spherical cells flanked on all sides by thick regions of polymer that are devoid of cells. The cross-sectional images obtained from the standard foam molding process are in good agreement with those in the publication by Paultkiewicz et al. and represent the current industry standard. In contrast, typical cross-sections of MFIM molded ISO specimens show a cellular structure with more asymmetrically deformed cells.
[0207] The cells in the MFIM cross section also progress to regions adjacent to the surface in nearly all cases, albeit in a much thinner part with a much larger L / T ratio (40.5) than previously described, similar to the previous examples described herein. The results clearly show that the employment of a decompression step in MFIM, combined with the elimination of the standard foam molding process variables of hold pressure and time, results in a significantly different cell structure within the molded part.
[0208] Tensile testing of five replicate parts from MFIM process 9 was performed. Figure 21 shows a representative cross section and a series of stress / strain plots for the five tested parts from MFIM process 9.
[0209] Tensile testing of five replicate parts from step 10 made using the standard foam molding process was performed. Figure 22 shows a representative cross section and a series of stress / strain plots for the five parts tested from the standard foam process step 10.
[0210] The average tensile strength of the five parts from MFIM step 9 was less than the average of the five parts from the standard foam molding process step 10. However, the MFIM parts showed greater strain (elongation) at failure.
[0211] Many more cells were visible in the cross section of the MFIM part from step 9 (102 cells) than in the standard foam molding process part from step 10 (19 cells).
[0212] X-ray tomography scans (completed under conditions described in Example 5) were completed on randomly selected replica parts from step 15 of the standard foam molding process (shown in FIG. 23), and on randomly selected replica parts produced during step 9 of the MFIM process (shown in FIG. 24). Both FIG. 23 and FIG. 24 show a "top" view taken at 50% depth, and a "side" view also taken at 50% depth.
[0213] In the developed cell structure of the standard foam molding process ISO specimen (FIG. 23), the cells were circular in shape and the area adjacent to the surface of the specimen was devoid of cells.
[0214] In contrast, as shown in FIG. 24, the ISO specimens produced via the MFIM process contain multiple elongated cell populations, with the cells being found in areas adjacent to the surface of the part.
[0215] Example 9 To explore the dependence of the final cell structure on the MFIM processing conditions, eight tensile specimens of LDPE were molded on an Engel Victory 340 Ton injection molding machine using the MFIM process. The mold contained an aluminum material modified tensile specimen cavity with dimensions of 24 cm long, 2.54 cm thick, and variable width with a gauge length of 6 cm and a gauge width of 2.54 cm tapering to a flange with a width of 3.5 cm. The large tensile specimens were fed from a cold sprue and runner system through a 1.0 cm diameter gate. The material mix consisted of LDPE with and without talc, always containing 2 wt% blowing agent Clariant Hydrocerol® BIH70. The melt temperature was set to the profile detailed in Table 26, and the residence time in the barrel was 13 minutes before building the shot for injection. After building up the shot, the screw was backed off to give a reduced pressure volume of either 4.0 in 3 (66 cc) or 6.0 in 3 (98 cc) and the LDPE blowing agent mixture was allowed to foam into the empty barrel space prior to injection for either 15 or 45 seconds. The study was completed on both unfilled LDPE and 15% talc filled LDPE. Detailed process conditions are shown in Table 26. [Table 26]
[0216] FIG. 25 shows an x-ray scan of one of the parts from this study, showing the overall shape of each part.
[0217] FIG. 26 depicts the cross-sections of each specimen molded in this study and cut from the middle of the gauge length with the variable parameters indicated. The sample set includes two primary groups: samples made with talc and samples made without talc. In FIG. 26, the sample set on the left depicts those parts made without talc. These parts exhibit a smaller cellular structure within the core of the part, indicating that the integrity of the developed cellular structure was largely unaffected by changes in decompression ratio and decompression time, which were all within acceptable ranges.
[0218] The sample set on the right depicts those specimens containing 15 wt% talc. Some smearing on the part surface resulted from knife damage on the low modulus LDPE but is not representative of part quality. The cell structure in the talc parts was consistently larger and the cell circularity was slightly below the equivalent without talc.
[0219] X-ray tomography images of 15% talc, 6 in. 3 The image was taken from a cross section approximately 50% in from the major surface of the MFIM part, created using a (98cc) vacuum volume and a 15 second vacuum time. The image is shown in FIG.
[0220] Example 10 Tensile specimen parts were made using a standard foam molding process from LDPE loaded with 15 wt% talc and 2 wt% Hydrocerol® BIH70 using processing parameters as described for Example 9, but without the decompression step of the MFIM process. The standard foam molded parts were made from the 15% talc, 6 inch foam from Example 9. 3 (98 cc) vacuum volume, and 15 second vacuum time. Using the method as described in Example 6, X-ray laminography images were taken from the center of each of the parts (MFIM molded and standard foam molded) at various depths from the major surfaces. Cross-sectional images were also recorded. The images are shown in FIG.
[0221] X-ray laminographic analysis of cell count, cell circularity, and average cell size (longest dimension of the cells) was performed on images of each tensile specimen part (MFIM and standard process material) at each depth from the major surface. Cell count, cell circularity, and average cell size were each plotted against cross-sectional depth, and individual plots are shown in Figures 29-31, respectively.
[0222] As shown in Figure 29, the cell counts are higher at all depths than the MFIM molded parts. As can be seen throughout the examples and figures, parts molded using standard foam molding processes appear to have no, or substantially no, cells in the region or "skin" adjacent to the surface, for example, within about the first 2.5 mm depth from the major surface, while cells are present in parts molded using the MFIM process in the region between about 2.5 mm below the surface and the surface.
[0223] As shown in FIG. 30, in general, cell circularity is higher in the standard foam molding process samples than in the MFIM shaped parts, except towards the center of the MFIM parts, where circularity is also higher in the MFIM molded samples.
[0224] As shown in Figure 31, cell size was generally larger for the standard foam molded tensile bar parts, but dropped off sharply to zero in the region close to the outer surface (e.g., within 2.5 mm of the surface). In contrast, cell size was more uniform through the depth of the MFIM molded parts, with cells continuing right to the surface.
[0225] The same trend was noted by visual inspection of the cross-sections shown in Figure 28. Within 2.5 mm of any outer surface, standard foam molded parts appear to be devoid of cells, while cells are visible all the way to the outer surface in the MFIM parts.
[0226] Example 11 A large sample of the recovered marine plastic was analyzed using differential scanning calorimetry and estimated to consist of approximately 85% HDPE by weight, with the remainder including polypropylene and contaminants.
[0227] Two parts, a 4" x 4" x 2" brick and a 15.24 cm diameter sphere, were successfully molded from marine plastic using the MFIM process. Molding was done using an Engel Duo 550 Ton injection molding machine (available from Engel Machinery Inc., York, PA, USA). Both parts were opened and closed at the center and filled by viscous coil-fold flow.
[0228] The processing parameters and properties of the resulting parts are listed in Tables 27 and 28, respectively. [Table 27] [Table 28]
[0229] Example 12 A 9 inch (22.86 cm) diameter sphere, "Sample 10," was molded using the MFIM process described herein. In addition, a second 9 inch (22.86 cm) diameter sphere, "Sample 20," was molded using a modified process. The modified process, referred to herein as the "reverse MFIM" process, was as follows.
[0230] A) A mixture was prepared by blending a polymer (which may be in the form of pellets, powder, beads, granules, and the like) with chemical foaming agents and any other additives such as fillers. The mixture was introduced into an injection unit, where a rotating injection unit screw moved the material forward in the injection molding machine barrel, thus forming a heated fluid material, according to a normal injection molding process. B) The screw was moved backwards towards the hopper, creating an intentional space in the barrel between the screw and the nozzle. C) A set volume of material was dosed at the front of the barrel of the injection unit by the rotation of the screw, thus moving the set volume from the feed zone to the front of the screw and into the intentional space created in step B. During this feed step, the screw was rotated, moving the molten material into the space in the barrel between the screw and the nozzle, thereby providing the set volume. However, the set volume occupied only a part of the intentional space, thereby providing a volume for the shot to foam and expand, i.e., a decompression volume. D) The material remained in the barrel between the screw and the nozzle for a period of time, referred to herein as the "decompression time." During the decompression time, the material expanded due to foaming, filling or partially filling the space created in step (B). E) The molten foam was injected into the mold cavity by forward translation of the screw and / or rotation of the screw.
[0231] Thus, the normal and reverse MFIM processes differed from one another in that in the MFIM process, the screw is rotated to introduce a shot into the front of the barrel before it is translated backwards to allow for a vacuum space, whereas in the reverse process, the screw is translated backwards to allow for a vacuum space before it is rotated and introduces a shot of material into the intentionally created space.
[0232] Both Sample 10 and Sample 20 were molded from virgin LDPE containing 2% Hydrocerol® BIH70, 2% talc, and 1% yellow colorant. Molding was performed on an Engel Duo 550 Ton injection molding machine (available from Engel Machinery Inc., York, PA, USA). The mold was a spherical cavity in an aluminum mold fed by a cold runner and sprue.
[0233] The processing parameters are shown in Table 29. [Table 29-1] [Table 29-2]
[0234] The density of the parts for both Sample 10 and Sample 20 was 0.214 g / cc, with a density reduction of 77% in both cases.
[0235] A photograph of Sample 20 is shown in FIG. 32 and a photograph of Sample 10 is shown in FIG. 33, where each spherical part is mounted on a stand. As can be seen, Sample 20, made using the "reverse MFIM process", exhibited a non-uniform surface, while the surface of Sample 10, made using the MFIM process, was much more uniform. The average wrinkle depth was estimated using optical microscopy and X-ray tomography. The average wrinkle depth was measured to be less than 50 microns for Sample 10, but 565 microns for Sample 20.
[0236] Samples 10 and 20 were each cut in half to provide a cross section at the largest diameter. The cross sections of the four pieces were photographed. The half of Sample 20 made by the reverse MFIM method is shown in FIG. 34 and the half of Sample 10 is shown in FIG. 35. Close inspection of the edges showed that in Samples 10 and 20, unlike parts produced in any of the examples by the standard foam method, cells were found right up to the surface, e.g., within 2.5 mm of the surface.
[0237] X-ray tomography was performed on the first inch depth of the samples for Sample 10 and Sample 20 using the method described in Example 6, and cell counts and cell sizes were measured for different distances from the surface of each sample. The plots are provided in Figures 36 and 37, where "MFIM" refers to Sample 10 and "Reverse MFIM" refers to Sample 20.
[0238] Two additional sphere parts, namely parts 6 and 7, were prepared under the same conditions as sample 10 using the same polymer / talc / colorant / blowing agent mixture, i.e., by the MFIM method. Five cuboid parts, each approximately 2 inches by 2 inches by 1 inch, were cut from each of parts 6 and 7 and the compressive modulus (stress vs. strain) was tested. The average stress vs. average strain (MFIM method) was plotted and is shown in FIG. 38.
[0239] Two additional sphere parts, parts 22 and 24, were prepared under the same conditions as sample 20 using the same polymer / talc / colorant / blowing agent mixture. Five cuboid parts, each approximately 2 inches by 2 inches by 1 inch (approximately 5.1 cm by 5.1 cm by 5.1 cm), were cut from each of parts 22 and 24 and the compressive modulus (stress vs. strain) was tested. The average stress vs. average strain (inverse MFIM method) was plotted and is shown in FIG. 38. As can be seen in FIG. 38, the compressive modulus of the parts made by the MFIM process (average of parts 6 and 7) and the parts made by the inverse MFIM process (average of parts 22 and 24) are similar.
[0240] Five strips were cut from each of parts 6 and 7 (MFIM) and 22 and 24 (reverse MFIM). Each strip was approximately 1 inch by 1 inch by 8 inches. The flexural modulus (stress vs. strain) was tested for all of the strips and the results were averaged for the 10 MFIM produced strips and the results were averaged for the 10 reverse MFIM strips. The results are plotted in Figure 39.
[0241] Example 13 Parts of various geometries and materials, as shown in Table 30, were processed using the MFIM method as described herein. The parts were sectioned. In all cases, the regions close to the surface contained smaller sized cells, but as one moved away from the surface, the cell size increased. The regions of reduced cell size closer to the surface transitioned to larger cell sizes as one moved further away from the surface. The transition was gradual, so there were not distinct layers of smaller and larger sizes, but using microscopy, the relative areas of the regions of smaller or "compressed" cells and larger cells were estimated by visual inspection and confirmed by light microscopy, and are shown in Table 30. While the numbers are estimates only, inspection of the images showed that the depth of the area and percent area occupied by the "compressed" cells varied widely, likely depending on the part geometry, material, and / or process conditions. [Table 30]
[0242] Example 14 The first part molded using a formulation of 98 wt% metallocene polyethylene was compounded with 2 wt% Hydrocerol® BIH70 prior to loading into the injection molding machine. The first part was formed using the MFIM process. Process details are provided in Tables 31 and 32. The part was made using a 2" x 4" x 4" block mold (5.08 x 10.16 x 10.16 cm) with a mold cavity volume of 524.4 cc and a sprue volume of 17.4 cc. The sprue was cut from the part and the part was then subjected to a compressive load test to quantify the compressive strength properties of the cellular structure formed in the 2" x 4" x 4" geometry. [Table 31] [Table 32]
[0243] Compression tests were performed on an Instron Universal Testing System (available from Instron USA, Norwood, Massachusetts, USA). Each molded foam block was placed between the test platens and stabilized in an environmental chamber at 30° C. for 5 minutes prior to testing. The instrument was equipped with a 250 kN load cell. The compression test rate was 5 mm / min.
[0244] The results showed that the compressive modulus was 19 MPa for Sample A (0.37 g / cc), 39 MPa for Sample B (0.45 g / cc), and 55 MPa for Sample C (0.57 g / cc). As shown in Figure 40, the compressive strength of the metallocene polyethylene (mPE) blocks increases with increasing density.
Claims
1. A method for forming a polymeric foam article, the method comprising: forming a molten pneumatic mixture by heating and mixing a thermoplastic polymer with a physical blowing agent source, the temperature of the molten pneumatic mixture exceeding a temperature at which the physical blowing agent source produces a physical blowing agent at atmospheric pressure, and a pressure applied to the molten pneumatic mixture is sufficient to substantially prevent the formation of a foam; collecting a selected amount of the molten pneumatic mixture in a collection area; forming a molten polymer foam from the molten pneumatic mixture by defining an expanded volume in the collection area adjacent to the molten pneumatic mixture; dispensing the molten polymer foam from the collection area into a cavity defined by a mold, the molten polymer foam contacting a surface of the mold defining the cavity; cooling the molten polymer foam within the mold cavity to form a solidified polymer foam article. A method comprising:
2. The method of claim 1, wherein the dispensing includes partially filling the mold cavity.
3. The method of claim 1, wherein the dispensing includes substantially filling the mold cavity.
4. The method of claim 1, wherein the dispensing includes completely filling the mold cavity.
5. A method according to any one of claims 1 to 4, wherein the heating, mixing, collecting, defining and dispensing are performed using an injection moulding machine.
6. The method of claim 1, wherein the physical foaming agent source is an organic compound.
7. The method of claim 1, wherein the physical foaming agent source is a physical foaming agent.
8. The method according to claim 1, wherein the physical blowing agent is CO 2 or N 2 .
9. A method for forming a polymeric foam article, the method comprising: forming a molten polymer foam in a barrel region of an extruder; dispensing the molten polymer foam from the extruder into a cavity defined by a die, the cavity being fluidly connected to the extruder, the dispensing including an uninterrupted flow of the molten polymer foam into the cavity, the uninterrupted flow capturing one or more of a coiled melt flow or a folded melt flow inside the cavity; A method comprising:
10. The method of claim 9, wherein the uninterrupted flow is a pressurized flow.
11. The method described in claim 9 or claim 10, wherein the mold is an aluminum mold.
Citation Information
Patent Citations
Method for manufacturing foamed molding
JP2009096139A