Fluorine resin

A fluororesin with a residue unit in a specific formula is produced using a controlled polymerization and precipitation process, addressing high haze issues in melt-molded products, resulting in transparent and heat-resistant optical applications.

JP2024138550AActive Publication Date: 2024-10-08TOSOH CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024117036
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-03-27
Filing Date
2024-07-22
Publication Date
2024-10-08
Estimated Expiration
2039-10-04

AI Technical Summary

Technical Problem

The existing fluororesins containing oxolane rings have a high haze value in melt-molded products, which affects their transparency and performance in optical applications.

Method used

A fluororesin containing a residue unit represented by a specific general formula with a haze value of 2% or less in a hot press molded product, produced through a method involving polymerization, insoluble matter removal, and precipitation steps, using specific solvents and conditions to achieve low haze and high transparency.

Benefits of technology

The fluororesin achieves a haze value of 2% or less in melt-molded products, ensuring excellent transparency and performance as optical members with high heat resistance and chemical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138550000001
    Figure 2024138550000001
  • Figure 2024138550000002
    Figure 2024138550000002
  • Figure 2024138550000003
    Figure 2024138550000003
Patent Text Reader

Abstract

To provide a fluorine resin containing an oxolane ring having a small haze value of a molding.SOLUTION: A fluorine resin includes a residue unit represented by general formula (1), and has yellowness of a heated, melted and molded article (thickness of 3 mm) at 280°C for 24 hours of 2 or less, wherein the fluorine resin has an insoluble content when the fluorine resin is dissolved in 1,1,1,2,3,4,4,5,5,5-decafluoro-3-methoxy-2-(trifluoromethyl)pentane of 0.2 wt.% or less. In the formula (1), Rf1, Rf2, Rf3 and Rf4 each independently represents one kind of the group consisting of a fluorine atom, a linear perfluoroalkyl group having 1 to 7 carbon atoms, a branched perfluoroalkyl group having 3 to 7 carbon atoms and a cyclic perfluoroalkyl group having 3 to 7 carbon atoms, the perfluoroalkyl group may have an ethereal oxygen atom, Rf1, Rf2, Rf3 and Rf4 may be bonded to each other to form a ring having 4 or more and 8 or less carbon atoms, and the ring may be a ring containing an ethereal oxygen atom.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fluororesin and a method for producing the same. [Background technology]

[0002] Amorphous fluororesins are used in a variety of applications in the optical and electronic fields due to their excellent transparency, liquid repellency, durability, electrical properties, etc. In the optical field, amorphous fluoropolymers are used as optical components such as optical waveguides and pellicles, which are dust-proof films for semiconductor photomasks.

[0003] Among them, fluororesins containing oxolane rings have a bulky ring structure, making them amorphous and highly transparent and heat resistant. In addition, because they are composed only of carbon, fluorine, and oxygen, they have excellent electrical properties, chemical resistance, waterproofness, and liquid and oil repellency. Furthermore, because they are amorphous, they can be melt-molded.

[0004] Non-Patent Document 1 describes the synthesis and properties of a polymer (polyPFMMD) of perfluoro-2-methylene-4-methyl-1,3-dioxolane (PFMMD), which is a type of fluororesin containing an oxolane ring. PolyPFMMD has excellent heat resistance. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Macromolecules 2005,38,4237-4245 Summary of the Invention [Problem to be solved by the invention]

[0006] According to the investigations of the present inventors, the resin produced by the method of Non-Patent Document 1 has a problem in that the haze value of the melt-molded product is high.

[0007] The present invention has an object to solve the above-mentioned problems associated with fluororesins containing oxolane rings, and specifically, an object of the present invention to provide a fluororesin containing oxolane rings which produces a melt-molded product with a small haze value, and a method for producing the same. [Means for solving the problem]

[0008] The present invention is as follows. [1] A fluororesin containing a residue unit represented by the following general formula (1), and having a haze value of 2% or less when molded by hot press (thickness 1 mm). [ka] (In formula (1), Rf1, Rf2, Rf3 and Rf4 each independently represent one of the group consisting of a fluorine atom, a linear perfluoroalkyl group having 1 to 7 carbon atoms, a branched perfluoroalkyl group having 3 to 7 carbon atoms, or a cyclic perfluoroalkyl group having 3 to 7 carbon atoms, and the perfluoroalkyl group may have an etheric oxygen atom, and Rf1, Rf2, Rf3 and Rf4 may be bonded to each other to form a ring having 4 to 8 carbon atoms, and the ring may contain an etheric oxygen atom.) [2] The fluororesin according to [1], wherein the amount of insoluble matter when the fluororesin is dissolved in 1,1,1,2,3,4,4,5,5,5-decafluoro-3-methoxy-2-(trifluoromethyl)pentane is 0.2% by weight or less based on the fluororesin. [3] The bulk density of the fluororesin is 0.1 to 1.5 g / cm 3 The fluororesin according to [1] or [2], [4] The bulk density of the fluororesin is 0.12 to 0.25 g / cm 3 The fluororesin according to [1] or [2], [5] The fluororesin according to any one of [1] to [4], wherein a melt-molded product (thickness: 3 mm) of the fluororesin after heating at 280° C. for 24 hours has a yellowness index of 4 or less. [6] The weight average molecular weight of the fluororesin is 5×10 4 ~3×10 5 The fluororesin according to any one of [1] to [5], [7] A polymerization step (1) of polymerizing a monomer represented by the following general formula (4) in the presence of a radical polymerization initiator to obtain a fluororesin A containing a residue unit represented by general formula (5): an insoluble matter removal step (2) of removing insoluble matter from a mixture containing the fluororesin A containing a residue unit represented by general formula (5) obtained in the polymerization step and the solvent S2 to obtain a fluororesin A solution; The method includes a precipitation step (3) of precipitating fluororesin A from the fluororesin A solution obtained in the insoluble matter removal step, A manufacturing method for fluororesin in which the haze value of a hot press molded product (thickness 1 mm) is 2% or less. [ka] (In the formulas (4) and (5), Rf5, Rf6, Rf7, and Rf8 each independently represent one of the group consisting of a fluorine atom, a linear perfluoroalkyl group having 1 to 7 carbon atoms, a branched perfluoroalkyl group having 3 to 7 carbon atoms, or a cyclic perfluoroalkyl group having 3 to 7 carbon atoms, and the perfluoroalkyl group may have an etheric oxygen atom, and Rf5, Rf6, Rf7, and Rf8 may be bonded to each other to form a ring having 4 to 8 carbon atoms, and the ring may contain an etheric oxygen atom.) [8] The method according to [7], wherein the polymerization step (1) is any one of the following steps (1a), (1b) or (1c): (1a) a step of polymerizing a monomer represented by general formula (4) in the presence of a radical polymerization initiator and a good solvent b1 for the fluororesin A to obtain a mixture containing the fluororesin A and the good solvent b1; (1b) a step of polymerizing a monomer represented by general formula (4) in the presence of a radical polymerization initiator and a poor solvent c1 for fluororesin A to precipitate fluororesin A, recovering the precipitated fluororesin A, and mixing the recovered fluororesin A with a good solvent b1 for fluororesin A to obtain a mixture containing fluororesin A and the good solvent b1. (1c) A process of polymerizing a monomer represented by general formula (4) in the presence of a radical polymerization initiator and a poor solvent c1 for the fluororesin A, precipitating the fluororesin A, and mixing with a good solvent b1 for the fluororesin A to obtain a mixture containing the fluororesin A, the good solvent b1, and the poor solvent c1. [9] The production method according to [8], wherein the step (1a) is carried out in the presence of a radical polymerization initiator, a good solvent b1 for the fluororesin A, and a poor solvent c1 for the fluororesin A.

[10] The method according to any one of [7] to [9], wherein the insoluble matter removing step (2) is either the following step (2a) or (2b): (2a) a step of filtering a mixture containing fluororesin A and solvent S2 through a filter to remove insoluble matter; (2b) A step of subjecting the mixture containing fluororesin A and solvent S2 to centrifugation to remove insoluble matter.

[11] The method according to

[10] , wherein the solvent S2 is a good solvent b2 for the fluororesin A or a mixed solvent of the good solvent b2 and a poor solvent c2 for the fluororesin A.

[12] The method according to

[10] or

[11] , wherein the insoluble matter removal step (2) is (2a).

[13] The method according to any one of

[10] to

[12] , wherein the filter is a filter having a 99% capture particle size of 10 μm or less or a screen filter having a pore size of 10 μm or less.

[14] The method according to any one of [7] to

[13] , wherein the precipitation step (3) is any one of the following steps (3a), (3b), (3c) or (3d): (3a) a step of lowering the temperature of the fluororesin A solution to precipitate the fluororesin A; (3b) adding the fluororesin A solution to a poor solvent c3 for the fluororesin A to precipitate the fluororesin A; (3c) A step of precipitating fluororesin A by adding a poor solvent c3 for the fluororesin A solution to the fluororesin A solution (3d) A step of precipitating fluororesin A by volatilizing the solvent from the fluororesin A solution.

[15] The method according to

[14] , wherein the solvent for the fluororesin A solution in the precipitation step (3a) is a mixed solvent of a good solvent b3 for the fluororesin A and a poor solvent c3 for the fluororesin A.

[16] The method according to

[14] or

[15] , wherein in the precipitation step (3a), when the solution temperature T1 before the temperature is reduced is 30°C or higher and the solution temperature after the temperature is reduced is T2, T1-T2 is 5°C or higher.

[17] The production method according to any one of [7] to

[16] , further comprising a separation step (5) of separating the fluororesin A from the solution in which the fluororesin A has been precipitated obtained in the precipitation step (3) or from the solution to which the poor solvent c4 has been added in the poor solvent adding step (4), and a washing step (6) of washing the separated fluororesin A with the poor solvent c5.

[18] The polymerization step (1) is step (1b), and The method according to any one of

[14] to

[17] , wherein the precipitation step (3) is step (3a), (3b), (3c) or (3d).

[19] The method according to any one of

[14] to

[18] , wherein the precipitation step (3) is step (3a) or (3c).

[20] 18. The method according to claim 14, wherein the precipitating step (3) is any one of steps (3a), (3b) and (3c), and the solvent S2 is an aliphatic fluorine-containing solvent. [twenty one] 21. The method according to claim 7, wherein the insoluble matter removed in the insoluble matter removal step (2) comprises at least a fluororesin containing a residue unit represented by general formula (1). Effect of the Invention

[0009] According to the present invention, it is possible to provide a fluororesin which contains a residue unit represented by general formula (1) and has a haze value of 2% or less when molded by hot press (thickness 1 mm). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] <Fluororesin> The present invention relates to a fluororesin which contains a residue unit represented by the following general formula (1) and has a haze value of 2% or less when molded by hot press (thickness 1 mm). [ka] (In formula (1), Rf1, Rf2, Rf3 and Rf4 each independently represent one of the group consisting of a fluorine atom, a linear perfluoroalkyl group having 1 to 7 carbon atoms, a branched perfluoroalkyl group having 3 to 7 carbon atoms, or a cyclic perfluoroalkyl group having 3 to 7 carbon atoms, and the perfluoroalkyl group may have an etheric oxygen atom, and Rf1, Rf2, Rf3 and Rf4 may be bonded to each other to form a ring having 4 to 8 carbon atoms, and the ring may contain an etheric oxygen atom.) The invention will be described in detail below.

[0011] The present invention is a fluororesin containing a residue unit represented by a specific general formula (1). The fluororesin of the present invention is amorphous and has high transparency and high heat resistance because it has a bulky ring structure contained in the specific general formula (1). In addition, since it is composed only of carbon, fluorine, and oxygen, it has high electrical properties, chemical resistance, waterproofness, and liquid and oil repellency.

[0012] In the present invention, Rf1, Rf2, Rf3, and Rf4 in the residue unit represented by the general formula (1) each independently represent one of the group consisting of a fluorine atom, a linear perfluoroalkyl group having 1 to 7 carbon atoms, a branched perfluoroalkyl group having 3 to 7 carbon atoms, or a cyclic perfluoroalkyl group having 3 to 7 carbon atoms. The perfluoroalkyl group may have an etheric oxygen atom. Rf1, Rf2, Rf3, and Rf4 may be linked together to form a ring having 4 to 8 carbon atoms, and the ring may contain an etheric oxygen atom. Rf1, Rf2, Rf3, and Rf4 in the general formula (1) are respectively synonymous with Rf5, Rf6, Rf7, and Rf8 in the general formulas (4) and (5) described below, and specific examples of Rf1, Rf2, Rf3, and Rf4 described below are also specific examples of Rf5, Rf6, Rf7, and Rf8.

[0013] Examples of the linear perfluoroalkyl group having 1 to 7 carbon atoms include a trifluoromethyl group, a pentafluoroethyl group, a heptafluoropropyl group, a nonafluorobutyl group, an undecafluoropentyl group, a tridecafluorohexyl group, and a pentadecafluoroheptyl group. Examples of the branched perfluoroalkyl group having 3 to 7 carbon atoms include a heptafluoroisopropyl group, a nonafluoroisobutyl group, a nonafluorosec-butyl group, and a nonafluorotert-butyl group. Examples of the cyclic perfluoroalkyl group having 3 to 7 carbon atoms include a heptafluorocyclopropyl group, a nonafluorocyclobutyl group, and a tridecafluorocyclohexyl group. Examples of the linear perfluoroalkyl group having 1 to 7 carbon atoms, which may have an etheric oxygen atom, include a -CF2OCF3 group, a -(CF2)2OCF3 group, and a -(CF2)2OCF2CF3 group. Examples of cyclic perfluoroalkyl groups having 3 to 7 carbon atoms which may have an etheric oxygen atom include a 2-(2,3,3,4,4,5,5,6,6-decafluoro)-pyrinyl group, a 4-(2,3,3,4,4,5,5,6,6-decafluoro)-pyrinyl group, and a 2-(2,3,3,4,4,5,5-heptafluoro)-furanyl group.

[0014] A fluororesin in which at least one of Rf1, Rf2, Rf3, and Rf4 is a member of the group consisting of a linear perfluoroalkyl group having 1 to 7 carbon atoms, a branched perfluoroalkyl group having 3 to 7 carbon atoms, or a cyclic perfluoroalkyl group having 3 to 7 carbon atoms is preferred from the viewpoint of exhibiting excellent heat resistance.

[0015] Specific examples of the residue unit represented by general formula (1) include various residue units represented by the following formula (2).

[0016] [ka]

[0017] Among these, fluororesin containing a residue unit represented by the following general formula (3) is preferred because of its excellent heat resistance and moldability, and fluororesin containing a perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue unit is more preferred.

[0018] [ka]

[0019] The fluororesin of the present invention has a haze value of 2% or less in a melt molded product (thickness 1 mm). When the hot press molded product (thickness 1 mm) has a haze value of 2% or less, it has the advantage that when used as an optical component, an optical component with excellent transparency and performance can be obtained. The method for producing the fluororesin of the present invention having a haze value of 2% or less in a hot press molded product (thickness 1 mm) will be described later. The haze value is measured by the following method. A mold with a 1 mm thick plate with the center hollowed out is placed on a smooth metal plate with a polyimide film placed on it, and the fluororesin is placed on the hollowed out area, and then a polyimide film and a metal plate are placed on top of it, sandwiched, placed on a press, heated at 280 ° C for 10 minutes without pressure, then heat-pressed at 10 MPa and 280 ° C for 10 minutes in a press, and then depressurized and heat-pressed with a pressure of 10 MPa for 5 minutes, and then heat-pressed at 280 ° C and 10 MPa in a press, and then depressurized, and the molded product sandwiched between the metal plates is further sandwiched between metal plates for cooling and cooled to obtain a heat-press molded product (thickness 1 mm). The obtained heat-press molded product (thickness 1 mm) is measured according to JIS K7136 using a haze meter NDH5000 (light source: white LED) manufactured by Nippon Denshoku Kogyo Co., Ltd. to obtain a haze (%).

[0020] The fluororesin of the present invention has a haze value of 2% or less, preferably 1% or less, more preferably 0.8% or less, and more preferably 0.5% or less, when molded by hot press (thickness: 1 mm). There is no lower limit for the haze value, and the lower the better, but an example of the haze value is 0.01% or more.

[0021] The fluororesin of the present invention preferably has a yellowness index (hereinafter also referred to as "YI") of 6 or less for a melt-molded product (thickness 3 mm) that is heated at 280°C for 24 hours. When the melt-molded product (thickness 3 mm) has a yellowness index of 6 or less, an optical member having excellent transparency and excellent performance can be obtained when used as an optical member. YI is preferably 4 or less, more preferably 3 or less, more preferably 2 or less, and more preferably 1 or less. There is no lower limit for YI, and the lower the better, but for example, 0.01 or more can be mentioned. YI is measured by the following method. First, the transmittance of a fluororesin melt-molded product having a thickness of 3 mm is measured at a wavelength of 200 nm to 1500 nm using a spectrophotometer. Data at wavelengths of 380 nm to 780 nm is extracted from the measured transmittance data. From the transmittance data, the tristimulus values ​​X, Y, and Z of the XYZ color system are calculated in accordance with JIS Z8701, and YI under C light source is calculated in accordance with JIS K7373.

[0022] In consideration of, for example, handleability and moldability, the fluororesin of the present invention preferably has a bulk density of 0.1 to 1.5 g / cm. 3 The bulk density is 0.25 to 1.5 g / cm 3 More preferably, the density is 0.25 to 1.0 g / cm 3 It is more preferable that the bulk density is within a specific range. Furthermore, the inventors have found that the YI of the fluororesin of the present invention falls within a good range (see Examples 2, and 4 to 6). From this viewpoint, the bulk density is preferably 0.12 to 0.25 g / cm. 3 and preferably 0.14 to 0.22 g / cm 3 It is even more preferable that the bulk density is measured as follows. Fluororesin A is weighed out and placed in a 13.5 mL glass sample tube (the liquid level is 2.8 cm when 10 mL of water is placed in it) whose height per unit volume has been measured in advance, without applying vibration, and the bulk density can be calculated from the powder height and weight at that time according to the following formula. The bulk density at this time is called loose bulk density. Bulk density = (weight of powder (g)) / ((height of powder (cm) / 0.28 (cm / mL))

[0023] The weight average molecular weight Mw is not limited, but may be, for example, 1×10 3 ~5×10 7 The heat-press molded product has an excellent haze value, so the weight-average molecular weight Mw is 5×10 4 ~5×10 5 Furthermore, since the haze value of the hot press molded product is excellent, the weight average molecular weight Mw is preferably in the range of 5×10 4 ~3×10 5 When the weight average molecular weight Mw is in this range, the haze value of the hot press molded product is excellent, and the shear rate is preferably in the range of 10 -2 s, melt viscosity at 250℃ is 1×10 2 ~3×10 5 Pa·s, resulting in excellent melt molding processability. Furthermore, the defoaming property when melted is also excellent. Furthermore, by having the weight average molecular weight Mw in this range, the occurrence of cracks during heating and cooling is reduced. From the viewpoints of excellent haze value, excellent melt molding processability, and excellent defoaming property when melted, the fluororesin of the present invention preferably has a weight average molecular weight Mw of 5×10 4 ~2×10 5 By the weight average molecular weight Mw being in this range, the shear rate is 10 -2 s, melt viscosity at 250℃ is 1×10 2 ~2×10 4 From the viewpoints of excellent haze value, excellent melt molding processability, and excellent defoaming property when melted, it is more preferable that the weight average molecular weight Mw is 5×10 4 ~1.5×10 5 From the viewpoint of reducing the occurrence of cracks during heating and cooling, it is more preferably in the range of 6×10 4 ~1.5×10 5 The range is.

[0024] The weight average molecular weight Mw of the fluororesin of the present invention can be calculated from the elution times of the sample and the standard sample and the molecular weight of the standard sample by using gel permeation chromatography (GPC), for example, a standard polymethylmethacrylate with a known molecular weight as the standard sample and a solvent capable of dissolving both the standard sample and the fluororesin as the eluent. An example of the solution is Asahiklin AK-225 (manufactured by Asahi Glass Co., Ltd.) to which 10 wt % of 1,1,1,3,3,3-hexafluoro-2-propanol (manufactured by Wako Pure Chemical Industries, Ltd.) has been added relative to AK-225.

[0025] The molecular weight distribution Mw / Mn, which is the ratio of the weight average molecular weight Mw to the number average molecular weight Mn of the fluororesin of the present invention, is not particularly limited, but from the viewpoints of excellent haze value, suppressed yellowing after heating and melting, excellent melt molding processability, excellent defoaming property during melting, and less cracking during heating and cooling, the molecular weight distribution Mw / Mn is preferably 1.2 to 8, more preferably 1.2 to 5, even more preferably 1.5 to 3, and even more preferably 2.0 to 3. The number average molecular weight Mn can be measured by the same method as the above-mentioned method for measuring the weight average molecular weight Mw, and the molecular weight distribution Mw / Mn can be calculated by dividing the weight average molecular weight Mw by the number average molecular weight Mn.

[0026] The particle size of the fluororesin of the present invention is not particularly limited, but in order to provide excellent handleability during molding, the volume average particle size is preferably 1 to 10,000 μm, more preferably 1 to 2,000 μm, more preferably 1 to 1,000 μm, and even more preferably 10 to 1,000 μm. The volume average particle size of the fluororesin of the present invention can be evaluated by particle size distribution measurement (volume distribution) by laser diffraction scattering method. The particle size distribution by laser diffraction scattering method can be measured by dispersing the resin particles in water or an organic solvent such as methanol and measuring it. As an example of a laser scattering meter, Microtrack manufactured by Microtrack Bell Co., Ltd. can be mentioned. Volume average particle size, also known as Mean Volume Diameter, is the average particle size expressed on a volume basis. When the particle size distribution is divided into each particle size channel, the representative particle size value of each particle size channel is d, and the volume-based percentage of each particle size channel is v, it is expressed as Σ(vd) / Σ(v).

[0027] Since the fluororesin of the present invention has a small haze value, the amount of insoluble matter when dissolved in 1,1,1,2,3,4,4,5,5,5-decafluoro-3-methoxy-2-(trifluoromethyl)pentane (C2F5CF(OCH3)C3F7, manufactured by 3M Japan, Novec7300) is preferably 0.2% by weight or less, more preferably 0.1% by weight or less, even more preferably 0.05% by weight or less, and even more preferably 0.01% by weight or less relative to the fluororesin. The method for measuring the amount of insoluble matter is as follows. 1,1,1,2,3,4,4,5,5,5-decafluoro-3-methoxy-2-(trifluoromethyl)pentane (C2F5CF(OCH3)C3F7, manufactured by 3M Japan, Novec7300) is added to the fluororesin to prepare a solids concentration of 10% by weight. Dissolve at 50°C for 5 hours, and shake and stir to prepare a fluororesin solution. The solution was pressure-filtered using a pressure filter equipped with a PTFE membrane filter with a pore size of 0.1 μm, the weight of which had been recorded in advance, and then pressure-filtered using Novec 7300 from which foreign matter had been removed using a pore size of 0.1 μm. The Novec 7300 from which foreign matter had been removed was placed in the pressure filter and pressure-filtered repeatedly to wash away the remaining fluororesin. The filter was then removed and vacuum-dried, and the weight of the resulting filter was subtracted by the weight of the filter before filtration to determine the amount of matter remaining on the filter. The amount of matter remaining on the filter was then divided by the weight of the resin used to determine the percentage, thereby determining the amount of insoluble matter (wt %).

[0028] <Fluororesin manufacturing method> The method for producing a fluororesin of the present invention is a method for producing a fluororesin having a haze value of 10% or less in a melt-molded product (thickness: 1 mm), A polymerization step (1) of polymerizing a monomer represented by the following general formula (4) in the presence of a radical polymerization initiator to obtain a fluororesin A containing a residue unit represented by general formula (5): an insoluble matter removal step (2) of removing insoluble matter from a mixture of the fluororesin A containing the residue unit represented by general formula (5) obtained in the polymerization step and the solvent S2 to obtain a fluororesin A solution; and The method includes a precipitation step (3) of precipitating fluororesin A from the fluororesin A solution obtained in the insoluble matter removal step. [ka] [ka]

[0029] In formulas (4) and (5), Rf5, Rf6, Rf7, and Rf8 each independently represent one of the group consisting of a fluorine atom, a linear perfluoroalkyl group having 1 to 7 carbon atoms, a branched perfluoroalkyl group having 3 to 7 carbon atoms, or a cyclic perfluoroalkyl group having 3 to 7 carbon atoms, the perfluoroalkyl group may have an etheric oxygen atom, and Rf5, Rf6, Rf7, and Rf8 may be linked together to form a ring having 4 to 8 carbon atoms, and the ring may contain an etheric oxygen atom. Rf5, Rf6, Rf7, and Rf8 in formulas (4) and (5) are respectively synonymous with Rf1, Rf2, Rf3, and Rf4 in formula (1).

[0030] Polymerization process (1) The polymerization step (1) is a step of polymerizing a monomer represented by general formula (4) in the presence of a radical polymerization initiator to obtain a fluororesin A containing a residue unit represented by general formula (5). There are no limitations on the polymerization method in the polymerization step (1), and examples of the polymerization method include solution polymerization, precipitation polymerization, bulk polymerization, emulsion polymerization, and suspension polymerization.

[0031] In the production method of the present invention, it is particularly preferred that the monomer represented by general formula (4) is perfluoro(4-methyl-2-methylene-1,3-dioxolane) represented by general formula (8) and the residue unit represented by general formula (5) is a perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue unit represented by general formula (9).

[0032] [ka]

[0033] [ka]

[0034] Examples of radical polymerization initiators for radical polymerization include bis(perfluorobenzoyl)peroxide (PFBPO), (CF3COO)2, (CF3CF2COO)2, (C3F7COO)2, (C4F9COO)2, (C5F 11 COO)2, (C6F 13 COO)2, (C7F 15 COO)2, (C8F 17 perfluoroorganic peroxides such as benzoyl peroxide, lauryl peroxide, octanoyl peroxide, acetyl peroxide, di-tert-butyl peroxide, tert-butylcumyl peroxide, dicumyl peroxide, tert-butyl peroxyacetate, perfluoro(di-trt-butyl peroxide), bis(2,3,4,5,6-pentafluorobenzoyl) peroxide, tert-butyl peroxybenzoate, tert-butyl perpivalate, and other organic peroxides; and azo initiators such as 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-butyronitrile), 2,2'-azobisisobutyronitrile, dimethyl-2,2'-azobisisobutyrate, and 1,1'-azobis(cyclohexane-1-carbonitrile).

[0035] The radical polymerization initiator is preferably a perfluoro organic peroxide, more preferably bis(perfluorobenzoyl)peroxide (PFBPO), from the viewpoints of small haze value, suppression of yellowing after heating and melting, excellent melt molding processability, excellent defoaming property during melting, and little cracking during heating and cooling. Here, the perfluoro organic peroxide refers to a compound having a structure in which the hydrogen atom of an organic peroxide is replaced by a fluorine atom.

[0036] The polymerization step (1) is suitably carried out in the presence of a solvent, and depending on the type of solvent, it can be, for example, either the following step (1a) or (1b). (1a) a step of polymerizing a monomer represented by general formula (4) in the presence of a radical polymerization initiator and a good solvent b1 for the fluororesin A to obtain a mixture containing the fluororesin A and the solvent b1; (1b) a step of polymerizing a monomer represented by general formula (4) in the presence of a radical polymerization initiator and a poor solvent c1 for fluororesin A to precipitate fluororesin A, recovering the precipitated fluororesin A, and mixing the recovered fluororesin A with a good solvent b1 to obtain a mixture containing fluororesin A and the good solvent b1. (1c) A process of polymerizing a monomer represented by general formula (4) in the presence of a radical polymerization initiator and a poor solvent c1 for the fluororesin A, precipitating the fluororesin A, and mixing with a good solvent b1 for the fluororesin A to obtain a mixture containing the fluororesin A, the good solvent b1, and the poor solvent c1.

[0037] In this specification, a good solvent for fluororesin A means an organic solvent capable of dissolving fluororesin A at 50° C. The term "dissolvable" refers to an organic solvent having a weight average molecular weight Mw of 5 to 15×10 4 This means that at least a part of the fluororesin A dissolves in the organic solvent, and for example, when a sample of the fluororesin A is immersed in a 20-fold amount (w / w) of an organic solvent at 50° C. for 5 hours or more, if 80% by weight or more of the sample of the fluororesin A dissolves in the solvent, the solvent can be considered as a good solvent. Here, the fluororesin A can be a fluororesin containing a residue unit represented by the general formula (3) above.

[0038] A poor solvent for fluororesin A means a solvent that does not easily dissolve fluororesin A, for example, a solvent having a weight average molecular weight Mw of 5 to 15 × 10 4 A poor solvent can be a solvent in which the amount of fluororesin A dissolved in the solvent is less than 20% by weight, preferably less than 10% by weight, when the fluororesin A sample is immersed in 20 times (w / w) the amount of solvent at 50°C for 5 hours or more and cooled to 25°C. Furthermore, in the present invention, a poor solvent for fluororesin A is also a solvent that can precipitate fluororesin A from a fluororesin A solution obtained by dissolving a fluororesin in a good solvent. The poor solvent is preferably a solvent that precipitates fluororesin A when a solution obtained by dissolving fluororesin A in a certain good solvent is dropped into a solvent in an amount 10 times the amount of the good solvent at 25°C. Here, fluororesin A can be a fluororesin containing a residue unit represented by the general formula (3) above.

[0039] In this specification, solvents are designated with the symbol S, and the solvent used in step (1) is designated with S1, the solvent used in step (2) with S2, the solvent used in step (3) with S3, the solvent used in step (4) with S4, and the solvent used in step (n) with Sn (n is an integer). Good solvents are designated with the symbol b, and the good solvent used in step (1) is designated with b1, the good solvent used in step (2) with b2, the good solvent used in step (3) with b3, the good solvent used in step (4) with b4, and the good solvent used in step (n) with bn (n is an integer). Poor solvents are designated with the symbol c, and the poor solvent used in step (1) is designated with c1, the poor solvent used in step (2) with c2, the poor solvent used in step (3) with c3, the poor solvent used in step (4) with c4, and the poor solvent used in step (n) with cn (n is an integer).

[0040] The solvent that can be a good solvent is preferably at least one selected from the group consisting of aliphatic fluorine-containing solvents such as perfluorocarbons, hydrochlorofluorocarbons, hydrofluorocarbons, hydrofluoroethers, and hydrofluoroolefins, or aromatic fluorine compounds. An aliphatic fluorine-containing solvent is more preferable because a fluororesin that exhibits good coloring when heated can be obtained. Further, at least one selected from the group consisting of perfluorohexane, perfluoro-N-methylmorpholine, perfluoro-N-propylmorpholine, perfluorotriethylamine, perfluoromethyldibutylamine, perfluorotributylamine, CF3CF2CHCl2, CF3CHFCHFCF2CF3, CF3CF2CF2CF2CF2CF2H, CF3(CF2)5CH2CH3, C4F9OCH3, C4F9OC2H5, 1,1,1,2,3,4,4,5,5,5-decafluoro-3-methoxy-2-(trifluoromethyl)pentane (C2F5CF(OCH3)C3F7), and hexafluorobenzene is more preferable.

[0041] Examples of such perfluorocarbons include Fluorinert FC-5052, FC-72, FC-770, FC-3283, FC-40, and FC-43 (all manufactured by 3M Japan Co., Ltd.); hydrochlorofluorocarbons such as Asahiklin AK-225 (manufactured by Asahi Glass Co., Ltd.); hydrofluorocarbons such as Vertrel XF (manufactured by Mitsui-Chemours Co., Ltd.), Asahiklin AC-2000, and AC-6000 (all manufactured by Asahi Glass Co., Ltd.); hydrofluoroethers such as Novec 7100, Novec 7200, and Novec 7300 (manufactured by 3M Japan Co., Ltd.); hydrofluoroolefins such as Opteon SF10 (manufactured by Mitsui-Chemours Co., Ltd.); and aromatic fluorine-containing solvents such as hexafluorobenzene. A specific example of a preferable good solvent is 1,1,1,2,3,4,4,5,5,5-decafluoro-3-methoxy-2-(trifluoromethyl)pentane (C2F5CF(OCH3)C3F7, manufactured by 3M Japan, Novec7300).

[0042] Since particles having a large bulk density and excellent powder handling properties can be obtained, the good solvent is preferably a fluorine-containing solvent, more preferably an aliphatic fluorine-containing solvent having a hydrogen atom in the molecule such as hydrofluorocarbon, hydrofluoroether, hydrochlorofluorocarbon, or hydrofluoroolefin; or an aromatic fluorine-containing solvent, even more preferably an aliphatic fluorine-containing solvent having a hydrogen atom in the molecule such as hydrofluorocarbon, hydrofluoroether, hydrochlorofluorocarbon, or hydrofluoroolefin, even more preferably a hydrofluorocarbon or hydrofluoroether, and particularly preferably a hydrofluoroether. Here, the aliphatic fluorine-containing solvent having a hydrogen atom may be saturated or unsaturated, and may be linear or cyclic.

[0043] Examples of solvents that can be poor solvents include 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 2,2,2-trifluoroethanol, 1,1,1,3,3,3-hexafluoroisopropanol, 1,2,2,3,3,4,4-heptafluorocyclopentane, 1H,1H-pentafluoropropanol, 1H,1H-heptafluorobutanol, 2-perfluorobutylethanol, 4, 4,4-trifluorobutanol, 1H,1H,3H-tetrafluoropropanol, 1H,1H,5H-octafluoropropanol, 1H,1H,7H-dodecafluoroheptanol, 1H,1H,3H-hexafluorobutanol, 2,2,3,3,3-pentafluoropropyl difluoromethyl ether, 2,2,3,3,3-pentafluoropropyl-1,1,2,2-tetrafluoroethyl ether, 1,1,2, Examples of the solvent include at least one selected from the group consisting of fluorine-containing solvents having a hydrogen atom in the molecule, such as 2-tetrafluoroethyl ethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, hexafluoroisopropyl methyl ether, 1,1,3,3,3-pentafluoro-2-trifluoromethylpropyl methyl ether, 1,1,2,3,3,3-hexafluoropropyl methyl ether, 1,1,2,3,3,3-hexafluoropropyl ethyl ether, and 2,2,3,4,4,4-hexafluorobutyl difluoromethyl ether; and fluorine-free organic solvents, such as hexane, heptane, toluene, acetone, methanol, ethanol, isopropanol, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, tetrahydrofuran, chloroform, dichloromethane, dichloroethane, and trichloroethane.

[0044] The poor solvent is preferably a fluorine-containing solvent, more preferably a fluorine-containing solvent having a hydrogen atom in the molecule, and more preferably at least one of the group consisting of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 2,2,2-trifluoroethanol, 1,1,1,3,3,3-hexafluoroisopropanol, and 1,2,2,3,3,4,4-heptafluorocyclopentane. From the viewpoint of economy, the poor solvent is preferably a fluorine-free organic solvent such as hexane, heptane, toluene, acetone, methanol, ethanol, isopropanol, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, tetrahydrofuran, chloroform, dichloromethane, dichloroethane, or trichloroethane. Further, non-chlorine-based solvents are more preferable because they have excellent yellowness, and examples of such solvents include hexane, heptane, toluene, acetone, methanol, ethanol, isopropanol, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, and tetrahydrofuran.

[0045] The polymerization step (1a) is a step in which polymerization is carried out in the presence of a good solvent b1 for the fluororesin A, and is preferably a step of solution polymerization in which the fluororesin A is dissolved in a solvent containing the good solvent b1.

[0046] In the polymerization step (1a), the polymerization can be carried out in the presence of a poor solvent c1 for the fluororesin A in addition to the radical polymerization initiator and the good solvent b1 for the fluororesin A. The poor solvent c1 will be described later. By carrying out the polymerization in the presence of the poor solvent c1, there is an advantage that the amount of the poor solvent used in the precipitation step described later can be reduced. The content of the poor solvent c1 is preferably set to an extent that the fluororesin produced by polymerization in the polymerization step is not precipitated, and the ratio of the good solvent b1 to the poor solvent c1 can be, for example, in the range of 1 to 50% by weight of the poor solvent c1 relative to the total of the good solvent b1 and the poor solvent c1.

[0047] The polymerization step (1b) is a step of carrying out polymerization in the presence of a poor solvent c1 for the fluororesin A to precipitate the fluororesin A. The poor solvent c1 in the polymerization step (1b) can be water. When the poor solvent c1 is water, it is generally called suspension polymerization when no emulsifier is present, and is called emulsion polymerization when an emulsifier is present. Among them, it is preferable that the poor solvent c1 dissolves the monomer represented by the general formula (4), and it is more preferable that it is precipitation polymerization, since the haze of the hot press molded product is reduced. Here, precipitation polymerization means polymerization carried out in a solvent that dissolves the monomer and precipitates the polymer.

[0048] The poor solvent c1 is preferably a solvent that precipitates the fluororesin A dissolved in the good solvent b1 at the polymerization temperature (e.g., 30 to 70° C.). The poor solvent c1 preferably has a solubility of the fluororesin A in a 20-fold amount of the solvent of less than 20% by weight, more preferably less than 10% by weight.

[0049] The conditions in the polymerization step (1), such as the polymerization temperature, polymerization time, concentration of the radical polymerization initiator, concentration of the monomer, the ratio of the initiator to the monomer, and the amount of the solvent, can be appropriately determined in consideration of the types of the monomer, radical polymerization initiator, solvent, etc. to be used. Examples are as follows. The polymerization temperature is, for example, in the range of 30 to 70° C., and the polymerization time is, for example, in the range of 5 to 96 hours. The concentration of the radical polymerization initiator is, for example, in the range of 0.1 to 5 mol% relative to the monomer. The monomer concentration may be, for example, in the range of 5 to 40% by weight based on the total weight of the monomer and the solvent. However, these numerical ranges are merely examples and are not intended to be limiting. In particular, the monomer concentration is appropriately determined depending on the type of monomer and the type of solvent, and taking into consideration the solubility of the resulting polymer in the solvent.

[0050] In the polymerization, it is preferable to use a chain transfer agent in addition to the monomer and the radical polymerization initiator in order to reduce the haze value of the hot press molded product. There is no particular limitation on the chain transfer agent, but for example, an organic compound having 1 to 20 carbon atoms and containing at least one atom selected from the group consisting of hydrogen atoms and chlorine atoms can be used. Here, the chain transfer agent refers to a substance that has the effect of lowering the molecular weight by being present in the system during the radical polymerization of the fluororesin. Specific examples of the chain transfer agent include organic compounds having 1 to 20 carbon atoms and containing hydrogen atoms, such as toluene, acetone, ethyl acetate, tetrahydrofuran, methyl ethyl ketone, methanol, ethanol, and isopropanol; organic compounds having 1 to 20 carbon atoms and containing chlorine atoms, such as chloroform, dichloromethane, tetrachloromethane, chloromethane, dichloroethane, trichloroethane, tetrachloroethane, pentachloroethane, hexachloroethane, benzyl chloride, pentafluorobenzyl chloride, and pentafluorobenzoyl chloride. Among these, from the viewpoints of suppressing the haze value of a hot press molded product, suppressing yellowing after heating and melting, controlling the molecular weight of the fluororesin, providing excellent melt molding processability, excellent defoaming properties when melted, minimizing the occurrence of cracks during heating and cooling, and providing an excellent yield, it is preferable that the compound be an organic compound having 1 to 20 carbon atoms containing a chlorine atom, and more preferably be represented by general formula (A).

[0051] [ka]

[0052] (In formula (A), m is an integer of 0 to 3, n is an integer of 1 to 3, p is an integer of 0 to 1, q is an integer of 0 to 1, and m+n+p+q is 4. R 1 and R 2 R are each independently a hydrocarbon group having 1 to 19 carbon atoms or an oxygen atom, and the oxygen atom may form a double bond with the adjacent carbon atom. 1 and R 2The total number of carbon atoms in R is 1 to 19, and the hydrocarbon group may have one or more atoms selected from oxygen atoms, fluorine atoms, and chlorine atoms, and may not have a hydrogen atom. The hydrocarbon group may be linear, branched, alicyclic, or aromatic. 1 and R 2 may be linked to each other to form a ring having 3 to 19 carbon atoms.)

[0053] Among them, from the viewpoints of suppressing the haze value of a hot press molded product, suppressing yellowing after heat melting, controlling the molecular weight of the fluororesin, providing excellent melt moldability, excellent defoaming properties when melted, causing less cracking when heated and cooled, and providing an excellent yield, organic compounds having 1 to 20 carbon atoms and containing hydrogen atoms and chlorine atoms are more preferred. Examples of organic compounds having 1 to 20 carbon atoms and containing hydrogen atoms and chlorine atoms include chloroform, dichloromethane, chloromethane, dichloroethane, trichloroethane, tetrachloroethane, pentachloroethane, benzyl chloride, and pentafluorobenzyl chloride. In addition, in the organic compound having 1 to 20 carbon atoms containing hydrogen atoms and chlorine atoms, from the viewpoints of suppressing the haze value of the hot press molded product, suppressing yellowing after heating and melting, controlling the molecular weight of the fluororesin, excellent melt molding processability, excellent defoaming properties when melted, little cracking during heating and cooling, and excellent yield, the number ratio of hydrogen atoms to chlorine atoms is preferably in the range of hydrogen atoms:chlorine atoms = 1:9 to 9:1, and more preferably in the range of 1:9 to 5:5. In addition, from the viewpoints of suppressing the haze value of the hot press molded product, suppressing yellowing after heating and melting, controlling the molecular weight of the fluororesin, excellent melt molding processability, excellent defoaming properties when melted, little cracking during heating and cooling, and excellent yield, the organic compound having 1 to 20 carbon atoms containing hydrogen atoms and chlorine atoms is preferably represented by the following general formula (B) or (C), and more preferably represented by general formula (B).

[0054] [ka] (In formula (B), m and n each independently represent an integer of 1 to 3, p represents an integer of 0 to 1, q represents an integer of 0 to 1, and m+n+p+q represents 4. 1 and R 2 are each independently a hydrocarbon group having 1 to 19 carbon atoms, R 1 p and R 2 q The total number of carbon atoms in R is 0 to 19, and the hydrocarbon group may have one or more atoms selected from oxygen atoms, fluorine atoms, and chlorine atoms, and may not have a hydrogen atom. The hydrocarbon group may be linear, branched, alicyclic, or aromatic. 1 and R 2 may be linked to each other to form a ring having 3 to 19 carbon atoms.)

[0055] [ka]

[0056] (In formula (C), m, n, u, and v each independently represent an integer of 0 to 3, m+u represents an integer of 1 to 5, n+v represents an integer of 1 to 5, p, q, r, s, and t each independently represent an integer of 0 to 1, m+n+p+q represents 3, r+s+u+v represents 3, and R 1 , R 2 , R 3 , R 4 , R 5 are each independently a hydrocarbon group having 1 to 18 carbon atoms, R 1 , R 2 , R 3 , R 4 , R 5 The total number of carbon atoms in R is 0 to 18, and the hydrocarbon group may have one or more atoms selected from oxygen atoms, fluorine atoms, and chlorine atoms, and may not have a hydrogen atom. The hydrocarbon group may be linear, branched, alicyclic, or aromatic. 1 , R 2 , R 3 , R 4 , R 5Two or more groups selected from may be linked together to form a ring having 3 to 19 carbon atoms, and there may be a plurality of such rings.)

[0057] Examples of organic compounds having 1 to 20 carbon atoms and containing chlorine atoms represented by general formula (A) include chloroform, dichloromethane, tetrachloromethane, chloromethane, dichloroethane, trichloroethane, tetrachloroethane, pentachloroethane, hexachloroethane, benzyl chloride, pentafluorobenzyl chloride, and pentafluorobenzoyl chloride. Examples of organic compounds having 1 to 20 carbon atoms and containing hydrogen atoms and chlorine atoms represented by general formula (B) include chloroform, dichloromethane, chloromethane, dichloroethane, trichloroethane, tetrachloroethane, pentachloroethane, benzyl chloride, and pentafluorobenzyl chloride. Examples of organic compounds having 1 to 20 carbon atoms and containing hydrogen atoms and chlorine atoms represented by general formula (C) include 1,1,1-trichloroethane.

[0058] Furthermore, since a fluororesin that suppresses the haze value of a hot press molded product, suppresses yellowing after heat melting, balances defoaming properties and crack generation during melting, and has excellent defoaming properties and heat resistance during melting, low melt viscosity, and less crack generation, and further has an excellent yield, the amount of the chain transfer agent is preferably 0.01 to 95% by weight, more preferably 1 to 50% by weight, and even more preferably 3 to 50% by weight, based on the total amount of the monomer and the chain transfer agent.

[0059] Insoluble matter removal process (2) The insoluble matter removing step (2) is a step of removing insoluble matter from a mixture containing fluororesin A containing a residue unit represented by general formula (5) obtained in the polymerization step (1) and solvent S2 to obtain a fluororesin A solution. By providing the insoluble matter removing step, the haze of the obtained fluororesin hot melt molded product (1 mm thick) can be reduced to 2% or less. The insoluble matter contained in the mixture containing fluororesin A and solvent S2 or the fluororesin A solution can be determined by, for example, visually observing the mixture or the solution, or by filtering the mixture or the solution under pressure using a PTFE membrane filter having a pore size of 0.1 μm whose weight has been recorded in advance, and then repeatedly filtering the mixture or the solution under pressure using a good solvent such as Novec 7300 from which foreign matter has been removed using a filter having a pore size of 0.1 μm to wash the remaining resin, removing the filter, vacuum drying, subtracting the weight of the filter from the weight of the filter before filtration to calculate the amount of residue on the filter, or by observing the residue on the filter. The removal of at least a portion of the insoluble matter can be evaluated, for example, by visually observing the mixture or solution, or by a method in which fluororesin solution A is pressure-filtered through a PTFE membrane filter having a pore size of 0.1 μm and the weight of which has been recorded in advance, and then pressure-filtered using a good solvent such as Novec 7300 from which foreign matter has been removed using a pore size of 0.1 μm, and the process is repeated to wash the remaining resin, after which the filter is removed and vacuum-dried, and the weight of the filter is subtracted by the weight of the filter before filtration to calculate the amount of matter remaining on the filter, or by observing the matter remaining on the filter.

[0060] The above fluororesin A solution is obtained by removing at least a part of the insoluble matter in the insoluble matter removal step (2), and it is preferable that at least a part of the removed insoluble matter is a fluororesin containing a residue unit represented by general formula (1), from the viewpoint that the finally obtained fluororesin A of the present invention has a reduced haze value. In this case, the structure of the insoluble matter, i.e., the inclusion of the residue unit represented by general formula (1), can be confirmed by microscopic FT-IR or the like, and can be evaluated, for example, by the following method. After the operation of passing 50 g of Novec 7300 through a 0.1 μm PTFE filter used for filtering the diluted resin solution and washing it is repeated five times, and after drying, the foreign matter on the filter is picked up, and the microscopic IR is measured and compared with the IR chart of the fluororesin containing the residue unit represented by general formula (1) to make a judgment. As shown in the examples, it was confirmed that the insoluble matter removed in the insoluble matter removal step (2) is a resin containing a residue unit represented by general formula (1), and the fluororesin A of the present invention from which at least a part of the insoluble matter has been removed has a reduced haze value.

[0061] The fluororesin A containing the residue unit represented by the general formula (5) obtained in the polymerization step (1) is obtained as a mixture with different solvents depending on the type of polymerization step. In the case of the polymerization step (1a), the fluororesin A is, for example, a mixture with a good solvent b1 or a mixed solvent of a good solvent b1 and a poor solvent c1. In this case, in the insoluble matter removal step (2), these solvents can be used as they are as the solvent S2. The mixture of the good solvent b1 or the mixed solvent of the good solvent b1 and the poor solvent c1 can be used as it is as the good solvent b2 or the mixed solvent of the good solvent b2 and the poor solvent c2. Alternatively, the solvent S2 can be obtained by further mixing with another solvent.

[0062] In the case of the polymerization step (1b), the fluororesin A is obtained as a precipitate. The solvent S2 can be obtained by recovering the precipitate of the fluororesin A obtained in the polymerization step (1b) by solid-liquid separation or the like, and, after washing and / or drying as necessary, forming a mixture containing the good solvent b2 or a mixed solvent of the good solvent b2 and the poor solvent c2.

[0063] When the solvent S2 is a mixed solvent, the content of the poor solvent c2 is preferably set in consideration of the concentration of the fluororesin A so that insoluble matter coexists but the fluororesin does not precipitate, and the ratio of the good solvent b2 to the poor solvent c2 can be, for example, in the range of 1 to 50% by weight of the poor solvent c2 relative to the total of the good solvent b2 and the poor solvent c2.

[0064] In either case, the concentration of fluororesin A in the mixture of fluororesin A and solvent S2 subjected to the insoluble matter removal step is preferably 1 to 40% by weight, and more preferably 5 to 30% by weight, from the viewpoint of effectively reducing haze in a heat-melt molded product of the fluororesin.

[0065] The insoluble matter removal step (2) can be, for example, either the following step (2a) or (2b). (2a) a step of filtering a mixture containing fluororesin A and solvent S2 through a filter to remove insoluble matter; (2b) A step of subjecting the mixture containing fluororesin A and solvent S2 to centrifugation to remove insoluble matter.

[0066] In the insoluble matter removal step (2a), the mixture containing the fluororesin A and the solvent S2 is filtered through a filter to remove the insoluble matter. The filtration method is not particularly limited, but examples include pressure filtration, reduced pressure filtration, and centrifugal filtration. The particulate matter removal performance of the filter used is not limited, but since the haze in the heat-melt molded product of the fluororesin A is effectively reduced, the 99% capture particle size of the filter is preferably 10 μm or less, more preferably 5 μm or less, more preferably 1 μm or less, more preferably 0.5 μm or less, even more preferably 0.2 μm or less, and even more preferably 0.1 μm or less. Here, the 99% capture particle size represents the particle size of particles that the filter can capture 99% or more, and is described in the catalog or technical documents of the filter, and can also be known by investigating the capture rate of standard particles with known particle sizes.

[0067] Examples of the material for the filter to be used include resins such as polypropylene, polyethylene, polyethylene terephthalate, nylon, PTFE (polytetrafluoroethylene), PES (polyethersulfone), cellulose mixed ester, cellulose acetate, polycarbonate, cellulose, nylon, polyamide, etc.; ceramics such as silica fiber and glass fiber; metals such as stainless steel and Hastelloy, etc., and among these, PTFE is preferred because it can effectively reduce haze in a heat-melt molded product of the fluororesin A. The filter may be either hydrophobic or hydrophilic.

[0068] Examples of the type of filter used include a depth filter and a screen filter. Examples of the screen filter include a mesh filter and a membrane filter. Among them, it is preferable to use a screen filter because it can effectively reduce haze in a heat-melt molded product of the fluororesin A, and it is more preferable to use a membrane filter, and it is more preferable to use a membrane filter made of PTFE. A depth filter is a filter that captures particles inside the filter, and a screen filter is a filter that captures particles on the surface of the filter. A membrane filter is a type of screen filter. In addition, since excellent filtering properties are obtained, multiple types of filters may be used in combination, for example, a combination of a depth filter and a screen filter, and a combination of screen filters with different captured particle sizes can be used. When a screen filter is combined with another filter such as a depth filter or a screen filter with a different captured particle size, it is preferable that the 99% captured particle size of the filter combined with the screen filter is 1 to 10 μm because excellent filtering properties are obtained.

[0069] Since haze in a heat-melt molded product of fluororesin A can be effectively reduced, it is preferable to use a screen filter with a pore size of 10 μm or less, more preferably to use a screen filter with a pore size of 5 μm or less, more preferably to use a screen filter with a pore size of 1 μm or less, even more preferably to use a screen filter with a pore size of 0.5 μm or less, and even more preferably to use a screen filter with a pore size of 0.2 μm or less. Generally, when the pore size of a membrane filter is C μm, the 99% captured particle size is below C μm, and depending on the product, 99.99% or more of particles of C μm are captured.

[0070] In the insoluble matter removal step (2b), the mixture containing the fluororesin A and the solvent S2 is centrifuged to remove the insoluble matter. There are no particular limitations on the method of centrifugation, but examples include a method in which the mixture containing the fluororesin A and the solvent S2 is placed in a container, and centrifugal force is applied to the container to cause the insoluble matter to settle and separate the solution, thereby removing the insoluble matter. The centrifugation method may be a batch type, a continuous type, or an intermediate type between the batch type and the continuous type.

[0071] Precipitation process (3) In the precipitation step (3), fluororesin A is precipitated from the fluororesin A solution obtained in the insoluble matter removal step. As the solvent S3 for the fluororesin A solution, the solvent S2 used for removing the insoluble matter in the insoluble matter removal step (2) may be used as is, or a solvent of a different type or composition may be used depending on the method.

[0072] The method for precipitating the polymer from the fluororesin A solution is not particularly limited, and the precipitation step (3) can be, for example, any one of the following steps (3a), (3b), (3c) or (3d). (3a) a step of lowering the temperature of the fluororesin A solution to precipitate the fluororesin A; (3b) adding the fluororesin A solution to a poor solvent c3 for the fluororesin A to precipitate the fluororesin A; (3c) A step of precipitating fluororesin A by adding a poor solvent c3 for the fluororesin A solution to the fluororesin A solution (3d) A step of precipitating fluororesin A by volatilizing the solvent from the fluororesin A solution.

[0073] The precipitation step (3a) is a step of lowering the temperature of the fluororesin A solution to precipitate the fluororesin A. As the solvent S3 of the fluororesin A solution, the solvent S2 used for removing the insoluble matter in the insoluble matter removal step (2) may be used as it is, or a solvent of a different type or composition may be used depending on the method. The good solvent b2 or a mixed solvent of the good solvent b2 and the poor solvent c2 used for removing the insoluble matter in the insoluble matter removal step (2) may be used as it is as the solvent in the precipitation step (3a). That is, the good solvent b2 or the mixed solvent of the good solvent b2 and the poor solvent c2 can be the good solvent b3 for the fluororesin A or the mixed solvent of the good solvent b3 for the fluororesin A and the poor solvent c3 for the fluororesin A, respectively. The concentration of the fluororesin A in the fluororesin A solution is preferably 1 to 40% by weight, more preferably 1 to 30% by weight, and even more preferably 2 to 20% by weight, from the viewpoint of obtaining particles having excellent productivity and excellent handling properties as a powder. From the viewpoint of obtaining particles having excellent productivity and excellent powder handling properties, the solvent S3 to be subjected to the precipitation step is preferably a mixed solvent of the good solvent b3 and the poor solvent c3. When the solvent S3 to be subjected to the precipitation step is a mixed solvent of the good solvent b3 and the poor solvent c3, the ratio of the good solvent b3 to the poor solvent c3 is preferably 10:90 to 99:1 by weight, more preferably 20:80 to 95:5, even more preferably 30:70 to 95:5, even more preferably 30:70 to 90:10, and even more preferably 30:70 to 80:20, since the productivity is excellent, particles having excellent powder handling properties are obtained, and coloring of the heat-melted product is reduced.

[0074] In the precipitation step (3a), the solution temperature T1 before the temperature is lowered is, for example, preferably 30° C. or higher, more preferably 40° C. or higher, and even more preferably 50° C. or higher, and when the solution temperature after the temperature is lowered is T2, T1-T2 is preferably 5° C. or higher, more preferably 10° C. or higher, more preferably 15° C. or higher, and even more preferably 20° C. or higher. This allows the precipitation of the fluororesin A to be carried out sufficiently.

[0075] In the precipitation step (3a), the temperature is preferably lowered over a period of 1 to 600 minutes, and more preferably over a period of 5 to 300 minutes, because this provides excellent productivity, excellent powder handling, and reduces coloring of the heat-melted product.

[0076] In the precipitation step (3a), the temperature is preferably decreased at a rate of 0.05 to 20°C per minute, and particularly preferably at a rate of 0.1 to 5°C per minute, since this provides excellent productivity and particles that are easy to handle as a powder.

[0077] The precipitation step (3b) is a step of precipitating fluororesin A by adding a poor solvent c3 for fluororesin A to the fluororesin A solution, and the precipitation step (3c) is a step of precipitating fluororesin A by adding a poor solvent c3 for the fluororesin A solution to the fluororesin A solution. The solvent S3 of the fluororesin A solution in the precipitation steps (3b) and (3c) may be the solvent S2 used for removing insoluble matter in the insoluble matter removal step (2). However, from the viewpoint that the precipitation of fluororesin A is easy by mixing with the poor solvent c3, it is preferable that the solvent s2 used for removing insoluble matter in the insoluble matter removal step (2) is a mixed solvent of the good solvent b2 and the poor solvent c2. From the viewpoint that the precipitation of fluororesin A is easy and the coloring of the heat-melted product is small, the precipitation step (3b) in which the fluororesin A is precipitated by adding the fluororesin A solution to the poor solvent c3 for fluororesin A is preferable. On the other hand, from the viewpoint of excellent handleability as a powder, the precipitating step (3c) of precipitating fluororesin A by adding a poor solvent c3 for the fluororesin A solution to the fluororesin A solution is preferred.

[0078] In any of the steps, since the productivity is excellent, particles are prevented from sticking to each other, and particles having excellent handleability as a powder are obtained, the weight ratio of the good solvent:poor solvent after mixing with the poor solvent c3 is preferably in the range of 10:90 to 90:10, more preferably 20:80 to 80:20, even more preferably 30:70 to 70:30, and even more preferably 30:70 to 60:40.

[0079] In the precipitation step (3d), the solvent S3 is evaporated from the fluororesin A solution to precipitate the fluororesin A. From the viewpoint of removing the solvent S3 by evaporation, the solvent S3 can be a solvent with a relatively low boiling point. The volatilization operation of the solvent S3 can be carried out by a known method, and examples of the method include a method of volatilizing the solvent using a thin-film evaporator such as Exeva, a method of passing the solvent through a heated flash tank to volatilize the solvent, a method of heating the solution in an extruder using a volatilization extrusion device to volatilize the solvent, a method of dispersing the fluororesin A solution in a solvent that is not miscible with the fluororesin A solution such as water, and volatilizing the solvent by heating or introducing steam (when steam is introduced, this is generally called steam stripping), and a method of precipitating the fluororesin A by heating a fluororesin A solution containing a low-boiling good solvent and a high-boiling poor solvent and volatilizing the low-boiling good solvent, and the like. A combination of multiple methods may be used. In addition, after removing the solvent by these methods, the fluororesin A may be processed into pellets using a pelletizer or the like.

[0080] The precipitation steps (3a) to (3d) can also be used in appropriate combination. For example, the fluororesin A solution obtained in the insoluble matter removal step can be subjected to the precipitation step (3b) or (3c), and the remaining fluororesin A solution can be further subjected to the precipitation step (3a) or (3d) to further recover the remaining fluororesin A.

[0081] In the precipitation step, it is preferable to stir the fluororesin A solution, since this provides particles with excellent productivity and excellent powder handling properties, and examples of such methods include stirring with a stirring blade, stirring by vibration, etc. In any of the precipitation steps (3a) to (3d), it is preferable to stir the solution when precipitating the resin.

[0082] In the precipitation process, the particles obtained are highly productive and easy to handle as powder. The Pv value, which is the power of the agitator motor per unit agitation capacity, is 0.05 to 50 kW / m 3 It is preferable to precipitate a particulate solid by lowering the temperature while stirring so that the Pv value is 0.2 to 50 kW / m 3 More preferably, 0.5 to 30 kW / m 3 is even more preferable, and 0.5 to 10 kW / m 3 is particularly preferable. Here, the Pv value (kW / m 3 ) can be calculated using the following formula (10).

[0083]

number

[0084] In formula (10), Np is a dimensionless number called the power number, which varies depending on the shape of the impeller. This Np can be obtained from known literature, such as "Chemical Equipment, August 1995, pp. 71-79" and "Kobe Steel Pfaudler Technical Report, vol. 28, No. 8 (October 1984), pp. 13-16." In this case, if the ratio b / d of the blade width b to the impeller diameter d is different from that of the impeller described in the literature, it can be calculated using the following formula (11).

[0085] Actual Np = Np reported in the literature × (actual b / d) / (b / d reported in the literature) (11) (Here, Np: power number, b: impeller width (mm), d: impeller diameter (mm).)

[0086] In the present invention, the combination of the polymerization step (1), the insoluble matter removing step (2), and the precipitation step (3) is not particularly limited. However, from the viewpoint that the inclusion of a step of precipitating the fluororesin as particles results in a fluororesin with fewer impurities and reduces coloration of the heat-melted product, it is preferable that the polymerization step (1) is step (1a) or (1c) and the precipitation step (3) is step (3a), (3b), or (3c), for example, or that the polymerization step (1) is step (1b) and the precipitation step (3) is step (3a), (3b), (3c), or (3d). More preferably, the polymerization step (1) is step (1a), the insoluble matter removal step (2) is step (2a), and the precipitation step (3) is step (3a), (3b), or (3c). Also, it is preferable that the polymerization step (1) is step (1b), the insoluble matter removal step (2) is step (2a), and the precipitation step (3) is step (3a), (3b), (3c), or (3d). When the polymerization step (1) and the precipitation step (3) are combined in the above-mentioned combination, a particulate fluororesin A is obtained in either step, and further, a step such as washing the particulate fluororesin A can be performed, so that a fluororesin with little coloring in the heat-melted product is easily obtained, which is preferable. In addition, the precipitation step is preferably step (3a) or (3c) because particles with high bulk density and excellent handling properties as powder are obtained. Moreover, from the viewpoint of preventing an increase in torque in the particle precipitation step and achieving excellent productivity, the precipitation step is preferably the step (3a).

[0087] In the fluororesin A solution from which the resin is precipitated obtained in the precipitation step (3), it is preferable to carry out a poor solvent addition step (4) in which a poor solvent c4 is added, since this prevents the resulting resin from adhering to itself and gives a resin that is excellent in handleability as a powder. The amount of poor solvent c4 added in the poor solvent addition step (4) is preferably 0.1 times or more, and more preferably 0.5 times or more and 1 times or more, based on the weight of the fluororesin A-containing solution obtained in the precipitation step, since this provides excellent productivity, prevents particles from adhering to each other, and gives a resin that is excellent in handleability as a powder.

[0088] In the present invention, any other steps may be added, and a separation step (5) of extracting a solid by solid-liquid separation may be included after the precipitation step (3) or the poor solvent addition step (4). The solid-liquid separation method is not particularly limited, and examples thereof include pressure filtration, reduced pressure filtration, centrifugation, and centrifugal filtration. The size of the filter used is not limited, and examples thereof include filters with a capture particle size of 30 μm or less. The material of the filter used is not limited, and examples thereof include polypropylene, polyethylene, polyethylene terephthalate, nylon, PTFE, PES, and the like.

[0089] In the present invention, any other steps may be added, and may include a washing step for washing particles of fluororesin A and / or a drying step for drying the particles. In the washing step (6), it is preferable to use a poor solvent c6, which is an organic solvent that precipitates fluororesin A, preferably at 25° C. The drying method is not particularly limited, and examples thereof include vacuum drying, reduced pressure drying, normal pressure drying, air drying, shaking drying, hot air drying, and heat drying.

[0090] In the present invention, it is preferable to further include a separation step (5) of separating the fluororesin A from the solution in which the fluororesin A has been precipitated obtained in the precipitation step (3) or the solution to which the poor solvent c4 has been added in the poor solvent adding step (4), and a washing step (6) of washing the separated fluororesin A with the poor solvent c6. This allows the production of particles with a more excellent yellowness.

[0091] In addition, it is preferable to use a solvent filtered through a filter having a 99% capture particle size of 5 μm or less or a screen filter with a pore size of 5 μm or less as the poor solvent c6, because this can effectively reduce haze in the hot melt molded product. EXAMPLES

[0092] The present invention will be described in more detail below with reference to examples. However, the examples are merely illustrative of the present invention and are not intended to limit the present invention.

[0093] <Physical property measurement method> (1) Weight average molecular weight Mw Measurements were performed using gel permeation chromatography equipped with a column TSKgel SuperHZM-M manufactured by Tosoh Corporation and an RI detector. The eluent used was Asahiklin AK-225 (manufactured by Asahi Glass Co., Ltd.) to which 10 wt% of 1,1,1,3,3,3-hexafluoro-2-propanol (manufactured by Wako Pure Chemical Industries, Ltd.) was added. Standard polymethylmethacrylate manufactured by Agilent was used as the standard sample, and the weight average molecular weight Mw calculated in terms of polymethylmethacrylate was calculated from the elution times of the sample and the standard sample.

[0094] (2) Measurement of volume average particle size The volume average particle size (unit: μm) was measured using a Microtrac MT3000 manufactured by Microtrac Bell and methanol as the dispersion medium.

[0095] (3) Calculation of Pv value The Pv value, which is the power of the agitator motor per unit agitation volume, was calculated using the following formula. When using four diagonal paddle impellers (blade diameter 50 mm, angled at 45°), Np was set to 4.2.

number

[0096] (4) Haze measurement A mold with a 1 mm thick plate with the center hollowed out was placed on a smooth metal plate with a polyimide film placed on it, and the fluororesin was placed on the hollowed out area, and then a polyimide film and a metal plate were placed on top of it, sandwiched, placed on a press, heated at 280 ° C for 10 minutes without applying pressure, then heat-pressed at 10 MPa and 280 ° C for 10 minutes in a press, and then depressurized and heat-pressed with a pressure of 10 MPa for 5 minutes, and then heat-pressed at 280 ° C and 10 MPa in a press, and then depressurized, and the molded product sandwiched between the metal plates was further sandwiched between metal plates for cooling and cooled to obtain a heat-press molded product (thickness 1 mm). The obtained heat-press molded product (thickness 1 mm) was measured according to JIS K7136 using a haze meter NDH5000 (light source: white LED) manufactured by Nippon Denshoku Kogyo Co., Ltd. to obtain the haze (%).

[0097] (5) Measurement of insoluble matter 1,1,1,2,3,4,4,5,5,5-Decafluoro-3-methoxy-2-(trifluoromethyl)pentane (C2F5CF(OCH3)C3F7, manufactured by 3M Japan, Novec7300) is added to the fluororesin to prepare a solid concentration of 10% by weight. The solution is dissolved at 50°C for 5 hours and shaken to prepare a fluororesin solution. The solution is pressure-filtered using a pressure filter equipped with a PTFE membrane filter with a pore size of 0.1 μm whose weight has been recorded in advance, and Novec7300 from which foreign matter has been removed using a filter with a pore size of 0.1 μm is placed in the pressure filter and pressure-filtered repeatedly to wash the remaining fluororesin, and then the filter is removed and vacuum-dried. The weight of the obtained filter is subtracted by the weight of the filter before filtration to obtain the amount of residue on the filter, and the amount of residue on the filter is divided by the weight of the resin used to obtain the ratio to obtain the amount of insoluble matter (wt%).

[0098] (6) Measurement of bulk density Fluororesin A is weighed out and placed into a 13.5 mL glass sample tube (the liquid level when 10 mL of water is poured in is 2.8 cm) whose height per unit volume has been measured in advance, without applying any vibration, and the bulk density can be calculated from the powder height and weight at that time according to the following formula. The bulk density at this time is called the loose bulk density. Bulk density = (weight of powder (g)) / ((height of powder (cm) / 0.28 (cm / mL))

[0099] (7) Yellowness Index (YI) Measurement 2.0 g of fluororesin was weighed into a petri dish with an inner diameter of 26.4 mm (a flat petri dish with a lid and a receiver made by Flat Co., Ltd., only the receiver, the glass thickness at the bottom of the receiver was 1 mm), and the petri dish was placed in an inert oven (DN411I made by Yamato Scientific Co., Ltd.), and left to stand at room temperature for 30 minutes under an air flow (20 L / min), after which the temperature was raised to 280 ° C over 30 minutes, and then heated at 280 ° C for 24 hours. Thereafter, while maintaining the air flow (20 L / min), the oven door was kept closed, the inert oven was turned off, and the sample was left to cool for 12 hours, and then the sample was taken out to obtain a fluororesin heat-melted molded product with a thickness of 3 mm and a diameter of 26.4 mm on the petri dish. At this time, air compressed by a compressor and passed through a dehumidifier (dew point temperature -20 ° C or less) was used as the air. The obtained fluororesin heat melt molded product was measured for transmittance at each wavelength at 1 nm intervals from 200 nm to 1500 nm using a spectrophotometer (U-4100 manufactured by Hitachi High-Tech Science Corporation). Data at 5 nm intervals from wavelengths of 380 nm to 780 nm were extracted from the measured transmittance data, and the tristimulus values ​​X, Y, and Z of the XYZ color system were calculated according to the method of JIS Z8701. YI was calculated for the C light source (auxiliary illuminant C) according to the method of JIS K7373, and the YI of the fluororesin heat melt molded product including the petri dish was obtained. The YI of the petri dish alone (receiver only) was measured, and the YI of the fluororesin heat melt molded product with a thickness of 3 mm was obtained by subtracting the YI of the petri dish alone (receiver only) from the YI of the fluororesin molded product including the petri dish. The YI of the petri dish alone (receiver only) was 0.21.

[0100] Example 1 In a 75mL glass ampoule, 0.173g (0.000410 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide was added as an initiator, 20.0g (0.0820 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane) was added as a monomer, 80.00g of Novec7300 (3M Japan, C2F5CF(OCH3)C3F7) was added as a polymerization solvent, and 2.22g (0.0186 mol) of chloroform (Wako Pure Chemical Industries) was added as a chain transfer agent. The mixture was repeatedly subjected to nitrogen replacement and depressurization by freeze degassing, and then sealed under reduced pressure (monomer / solvent=20 / 80 (wt / wt)). The ampoule was placed in a thermostatic bath at 55°C and held for 24 hours to carry out radical solution polymerization, resulting in a viscous liquid in which the resin had dissolved. After cooling to room temperature, the ampoule was opened, and the resin solution was diluted with 100 g of Novec 7300 to adjust the viscosity, to prepare a diluted resin solution (solid content concentration 10% by weight). The diluted resin solution was placed in a pressure filtration device (manufactured by ADVANTEC) equipped with a PTFE membrane filter (manufactured by ADVANTEC T010A) with a pore size of 0.1 μm, and components insoluble in the solvent were removed by pressure filtration.

[0101] This solution was transferred to a 1000 mL separable flask equipped with a four-blade diagonal paddle stirring blade (blade diameter 50 mm, blade width 12 mm, diagonal 45°) heated to 50°C, a three-one motor, and a water bath, and heated to 50°C while stirring at 200 rpm and held for 5 minutes. Then, 270 g of Zeorora H (manufactured by Zeon Corporation, 1,2,2,3,3,4,4-heptafluorocyclopentane) was added, and the mixture was stirred at 200 rpm and held at 50°C for 5 minutes (Zeorolla H / Novec7300=60 / 40 (wt / wt)). While stirring at 600 rpm (Pv value: 8.1 kW / m 3), the water bath was removed, and the mixture was allowed to cool in the air until it reached 30°C in about 30 minutes, yielding a particulate solid. Then, while stirring at 600 rpm, 150 g of Zeorora H was added (Zeorolla H / Novec7300=70 / 30 (wt / wt)). The mixture was filtered by suction, washed twice with acetone, and vacuum dried under heating to obtain particles of fluororesin A. The resin obtained had a weight-average molecular weight of 7.2×10 4 The volume average particle size was 88 μm, and the particles were fine particles, with almost no coarse particles. At this time, the acetone used was previously filtered through a 0.1 μm PTFE filter. The evaluation results of the fluororesin are shown in Table 1. Meanwhile, the PTFE filter used for filtering the diluted resin solution was washed by passing 50 g of Novec7300 through it five times, and then dried. When the insoluble matter on the obtained filter was confirmed by micro-IR, it was confirmed that it contained a fluororesin component containing a perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue unit. By removing this resin component (unnecessary matter), the haze of the fluororesin was clearly reduced compared to Comparative Example 1.

[0102] Example 2 A solution of 0.0865 g (0.000205 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide as an initiator dissolved in 0.260 g of hexafluorobenzene was placed in a 30 mm diameter glass ampoule equipped with a magnetic stirrer, 10.0 g (0.0205 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane) as a monomer, 39.74 g of Zeorola-H (manufactured by Nippon Zeon, 1,2,2,3,3,4,4-heptafluorocyclopentane) as a polymerization solvent, and 1.111 g (0.00931 mol) of chloroform (manufactured by Wako Pure Chemical Industries, Ltd.) as a chain transfer agent were placed in the ampoule, which was equipped with a magnetic stirrer. The ampoule was then repeatedly subjected to nitrogen replacement by freeze degassing and depressurization, and then sealed under reduced pressure (amount of chain transfer agent: 10% by weight based on the total weight of the monomer and chain transfer agent). The ampoule was held upright and stirred with a magnetic stirrer at 55°C for 24 hours to carry out precipitation polymerization. The solution became cloudy and the resin precipitated in the polymerization solvent. After cooling to room temperature, the ampoule was opened, and the liquid containing the generated resin particles was filtered, washed with acetone, and vacuum dried to obtain a particulate perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin with a volume average particle size of 95 μm. 90 g of Novec7300 (manufactured by 3M Japan, C2F5CF(OCH3)C3F7) was added to 10.0 g of the obtained fluororesin, and the resin was dissolved by heating at 50°C for 4 hours to prepare a diluted resin solution (solid concentration 10% by weight). The diluted resin solution was placed in a pressure filtration device (manufactured by ADVANTEC) equipped with a PTFE membrane filter (manufactured by ADVANTEC T010A) with a pore size of 0.1 μm, and components insoluble in the solvent were removed by pressure filtration. 2 L of acetone was placed in a plastic cup equipped with an anchor blade, and the pressure-filtered diluted resin solution was added to a beaker while stirring to precipitate the resin. The precipitated resin was recovered by filtration, washed once with acetone, and vacuum-dried to obtain a powdered perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin. The weight-average molecular weight of the resulting fluororesin was 9.7×10 4The evaluation results of the fluororesin are shown in Table 1. At this time, the acetone used was previously filtered through a 0.1 μm PTFE filter. Meanwhile, the PTFE filter used for filtering the diluted resin solution was washed with 50 g of Novec7300, which was repeated five times, and then dried. When the insoluble matter on the obtained filter was confirmed by micro-IR, it was confirmed that it contained a fluororesin component containing a perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue unit. By removing this resin component (unnecessary matter), the haze of the fluororesin was clearly reduced compared to Comparative Example 1.

[0103] Example 3 In a 75mL glass ampoule, 0.173g (0.000410 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide was added as an initiator, 20.0g (0.0820 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane) was added as a monomer, 80.00g of Novec7300 (3M Japan, C2F5CF(OCH3)C3F7) was added as a polymerization solvent, and 2.22g (0.0186 mol) of chloroform (Wako Pure Chemical Industries) was added as a chain transfer agent. The mixture was repeatedly subjected to nitrogen replacement and depressurization by freeze degassing, and then sealed under reduced pressure (monomer / solvent=20 / 80 (wt / wt)). The ampoule was placed in a thermostatic bath at 55°C and held for 24 hours to carry out radical solution polymerization, resulting in a viscous liquid in which the resin had dissolved. After cooling to room temperature, the ampoule was opened, and the resin solution was diluted with 100 g of Novec 7300 to adjust the viscosity, to prepare a diluted resin solution (solid content concentration 10% by weight). The diluted resin solution was placed in a pressure filtration device (manufactured by ADVANTEC) equipped with a PTFE membrane filter (manufactured by ADVANTEC T010A) with a pore size of 0.1 μm, and components insoluble in the solvent were removed by pressure filtration.

[0104] This solution was transferred to a 1000 mL separable flask equipped with a four-blade diagonal paddle stirring impeller (blade diameter 50 mm, blade width 12 mm, angled at 45°), a three-one motor, and a water bath, which had been heated to 50°C, and stirred at 600 rpm (Pv value: 20.6 kW / m 3), and 420 g of Zeorora H (manufactured by Nippon Zeon, 1,2,2,3,3,4,4-heptafluorocyclopentane) was slowly added to obtain a particulate solid (Zeorolla H / Novec7300=70 / 30 (wt / wt), Pv value after addition: 6.1 kW / m 3 The mixture was filtered by suction, washed twice with acetone, and dried under vacuum under heating to obtain particles of fluororesin A. The resulting resin had a weight-average molecular weight of 7.9×10 4 The volume average particle size was 87 μm, and the particles were almost free of coarse particles. In this case, Zeorora H, Novec7300, and acetone used in the precipitation process and thereafter were filtered through a 0.1 μm PTFE filter in advance. The evaluation results of the fluororesin are shown in Table 1. On the other hand, the PTFE filter used for filtering the diluted resin solution was washed by passing 50 g of Novec7300 through it five times, and then dried. When the insoluble matter on the obtained filter was confirmed by micro-IR, it was confirmed that it contained a fluororesin component containing a perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue unit. By removing this resin component (unnecessary matter), the haze of the fluororesin was clearly reduced compared to Comparative Example 1.

[0105] Example 4 In a 75mL glass ampoule, 0.173g (0.000410 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide was added as an initiator, 20.0g (0.0820 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane) was added as a monomer, 80.00g of Novec7300 (3M Japan, C2F5CF(OCH3)C3F7) was added as a polymerization solvent, and 2.22g (0.0186 mol) of chloroform (Wako Pure Chemical Industries) was added as a chain transfer agent. The mixture was repeatedly subjected to nitrogen replacement and depressurization by freeze degassing, and then sealed under reduced pressure (monomer / solvent=20 / 80 (wt / wt)). The ampoule was placed in a thermostatic bath at 55°C and held for 24 hours to carry out radical solution polymerization, resulting in a viscous liquid in which the resin had dissolved. After cooling to room temperature, the ampoule was opened, and the resin solution was diluted with 100 g of Novec 7300 to adjust the viscosity, to prepare a resin dilution solution (solid concentration 10 wt%). The resin dilution solution was placed in a pressure filtration device (manufactured by ADVANTEC) equipped with a PTFE membrane filter (manufactured by ADVANTEC T010A) with a pore size of 0.1 μm, and components insoluble in the solvent were removed by pressure filtration. 2 L of acetone was placed in a plastic cup equipped with an anchor blade, and the resin dilution solution filtered under pressure was added to a beaker under stirring to precipitate the resin. The precipitated resin was recovered by filtration, washed twice with acetone, and vacuum dried to obtain a powdered perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin. The weight average molecular weight of the obtained fluororesin was 5.7 × 10 4 The acetone used was filtered through a 0.1 μm PTFE filter in advance. The evaluation results of the fluororesin are shown in Table 1. Meanwhile, the PTFE filter used to filter the diluted resin solution was washed five times with 50 g of Novec7300, and then dried. When the insoluble matter on the obtained filter was confirmed by micro-IR, it was confirmed that it contained a fluororesin component containing a perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue unit. By removing this resin component (unnecessary matter), the haze of the fluororesin was clearly reduced compared to Comparative Example 1.

[0106] Example 5 In a 75mL glass ampoule, 0.173g (0.000410 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide was added as an initiator, 20.0g (0.0820 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane) was added as a monomer, 80.00g of Novec7300 (3M Japan, C2F5CF(OCH3)C3F7) was added as a polymerization solvent, and 2.22g (0.0186 mol) of chloroform (Wako Pure Chemical Industries) was added as a chain transfer agent. The mixture was repeatedly subjected to nitrogen replacement and depressurization by freeze degassing, and then sealed under reduced pressure (monomer / solvent=20 / 80 (wt / wt)). The ampoule was placed in a thermostatic bath at 55°C and held for 24 hours to carry out radical solution polymerization, resulting in a viscous liquid in which the resin had dissolved. After cooling to room temperature, the ampoule was opened (solid content concentration 20% by weight). The resin solution was placed in a pressure filtration device (manufactured by ADVANTEC) equipped with a 5 μm pore size PTFE membrane filter (manufactured by ADVANTEC T500A), and components insoluble in the solvent were removed by pressure filtration. To adjust the viscosity, the resin solution was diluted with 100 g of Novec 7300 that had been previously filtered through a 0.1 μm PTFE filter to prepare a diluted resin solution (solid content concentration 10% by weight). 2 L of acetone was placed in a plastic cup equipped with an anchor blade, and the diluted resin solution filtered under pressure was added to a beaker under stirring to precipitate the resin. The precipitated resin was recovered by filtration, washed twice with acetone, and dried in vacuum to obtain a powdered perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin. The weight average molecular weight of the obtained fluororesin was 5.5 × 10 4 The acetone used was filtered through a 0.1 μm PTFE filter in advance. The evaluation results of the fluororesin are shown in Table 1. Meanwhile, the PTFE filter used to filter the diluted resin solution was washed five times with 50 g of Novec7300, and then dried. When the insoluble matter on the obtained filter was confirmed by micro-IR, it was confirmed that it contained a fluororesin component containing a perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue unit. By removing this resin component (unnecessary matter), the haze of the fluororesin was clearly reduced compared to Comparative Example 1.

[0107] Example 6 In a 75mL glass ampoule, 0.173g (0.000410 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide as an initiator, 20.0g (0.0820 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane), 80.00g of FC-72 (3M Japan, perfluorohexane) as a polymerization solvent, and 2.22g (0.0186 mol) of chloroform (Wako Pure Chemical Industries, Ltd.) as a chain transfer agent were placed, and the mixture was repeatedly subjected to nitrogen replacement and depressurization by freeze degassing, and then sealed under reduced pressure (monomer / solvent=20 / 80 (wt / wt)). The ampoule was placed in a thermostatic bath at 55°C and held for 24 hours to carry out radical solution polymerization, resulting in a viscous liquid in which the resin had dissolved. After cooling to room temperature, the ampoule was opened (solid concentration 20% by weight). After cooling to room temperature, the ampoule was opened, and the resin solution was diluted with 100 g of FC-72 to adjust the viscosity, to prepare a resin dilution solution (solid concentration 10 wt%). The resin dilution solution was placed in a pressure filtration device (manufactured by ADVANTEC) equipped with a 0.1 μm pore size PTFE membrane filter (manufactured by ADVANTEC T010A), and components insoluble in the solvent were removed by pressure filtration. 2 L of hexane was placed in a plastic cup equipped with an anchor blade, and the resin dilution solution filtered under pressure was added to a beaker under stirring to precipitate the resin. The precipitated resin was recovered by filtration, washed twice with acetone, and dried in vacuum to obtain a powdered perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin. The weight average molecular weight of the obtained fluororesin was 7.2 × 10 4The results were as follows. At this time, the hexane and acetone used were previously filtered through a 0.1 μm PTFE filter. The evaluation results of the fluororesin are shown in Table 1. Meanwhile, the PTFE filter used to filter the diluted resin solution was washed by passing 50 g of Novec7300 through it five times, and then dried. When the insoluble matter on the obtained filter was confirmed by micro-IR, it was confirmed that it contained a fluororesin component containing a perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue unit. By removing this resin component (unnecessary matter), the haze of the fluororesin was clearly reduced compared to Comparative Example 1.

[0108] Example 7 In a 75mL glass ampoule, 0.173g (0.000410 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide was added as an initiator, 20.0g (0.0820 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane) was added as a monomer, 80.00g of hexafluorobenzene (Tokyo Chemical Industry Co., Ltd.) was added as a polymerization solvent, and 2.22g (0.0186 mol) of chloroform (Wako Pure Chemical Industries, Ltd.) was added as a chain transfer agent. The mixture was repeatedly subjected to nitrogen replacement and depressurization by freeze degassing, and then sealed under reduced pressure (monomer / solvent=20 / 80 (wt / wt)). The ampoule was placed in a thermostatic bath at 55°C and held for 24 hours to carry out radical solution polymerization, resulting in a viscous liquid in which the resin had dissolved. The ampoule was opened after cooling to room temperature (solid concentration 20% by weight). After cooling to room temperature, the ampoule was opened, and the resin solution was diluted with 100 g of hexafluorobenzene to adjust the viscosity, to prepare a diluted resin solution (solid content concentration 10 wt%). The diluted resin solution was placed in a pressure filtration device (manufactured by ADVANTEC) equipped with a PTFE membrane filter (manufactured by ADVANTEC T010A) with a pore size of 0.1 μm, and components insoluble in the solvent were removed by pressure filtration. 2 L of chloroform was placed in a plastic cup equipped with an anchor blade, and the diluted resin solution filtered under pressure was added to a beaker under stirring to precipitate the resin. The precipitated resin was recovered by filtration and then vacuum dried to obtain a powdered perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin. The weight average molecular weight of the obtained fluororesin was 6.5 × 104 The evaluation results of the fluororesin are shown in Table 1. Meanwhile, the PTFE filter used for filtering the diluted resin solution was washed by passing 50 g of Novec7300 through it five times, and then dried. When the insoluble matter on the obtained filter was confirmed by IR microscopy, it was confirmed that it contained a fluororesin component containing a perfluoro(4-methyl-2-methylene-1,3-dioxolane) residue unit. By removing this resin component (unnecessary matter), the haze of the fluororesin was clearly reduced compared to Comparative Example 1.

[0109] Comparative Example 1 The procedure was carried out according to the description of Sample 93 in Table 2 of Non-Patent Document 1. However, since there was no description of the polymer concentration during reprecipitation purification, the polymer was diluted to 10 wt%. A 75 mL glass ampoule was charged with 0.0880 g (0.000209 mol) of bis(2,3,4,5,6-pentafluorobenzoyl) peroxide as an initiator, 20.0 g (0.0820 mol) of perfluoro(4-methyl-2-methylene-1,3-dioxolane) as a monomer, and 32.63 g of hexafluorobenzene as a polymerization solvent, and the mixture was repeatedly subjected to nitrogen replacement and depressurization by freeze degassing, and then sealed under reduced pressure (monomer / solvent=38 / 62 (wt / wt)). The ampoule was placed in a thermostatic bath at 60° C. and held for 24 hours to carry out radical solution polymerization, resulting in a viscous liquid in which the resin had dissolved. After cooling to room temperature, the ampoule was opened, and the resin solution was diluted with 147 g of hexafluorobenzene to adjust the viscosity, to prepare a diluted resin solution. 1 L of chloroform was placed in a beaker equipped with an anchor blade, and the diluted resin solution was added to the beaker under stirring to precipitate the resin. The precipitated resin was recovered by filtration and then vacuum dried to obtain an amorphous perfluoro(4-methyl-2-methylene-1,3-dioxolane) resin. The molded product of the obtained fluororesin after heating at 280°C for 24 hours had many bubbles, but the coloring was more intense than in Example 1 when observed visually, and was equal to or slightly more intense than Example 7. Furthermore, the size of the obtained fluororesin was measured with a ruler to find that the average size was about 10 mm. The weight-average molecular weight of the obtained fluororesin was 3.7 x 10 5The evaluation results of the fluororesin are shown in Table 1.

[0110] [Table 1]

[0111] Reference example 1 Fluororesin A prepared in Example 1 (weight average molecular weight Mw = 7.2 × 10 4 ) was immersed in various organic solvents in an amount 20 times (w / w) the amount of fluororesin A at 50°C for more than 5 hours, and the dissolution was confirmed visually, with the following results. Soluble: FC-72, FC-770, Novec7200, Novec7300, hexafluorobenzene. When the solutions dissolved in these solvents were cooled to 25°C, all of them maintained their dissolved state. There was almost no residue left in all of them, and the solubility was 90wt% or more. Insoluble: Zeorora H, AE-3000, trifluoroethanol, ethyl acetate, chloroform, acetone, hexane. In all cases, after cooling to 25°C, filtration, and drying, the recovery rate of fluororesin A exceeded 80%, and the solubility was less than 20 wt%.

[0112] Reference example 2 Fluorine resin A (weight average molecular weight Mw = 7.2 × 10 4 When a solution of fluororesin A prepared by dissolving fluororesin A in Novec 7300 at a solid content concentration of 10% by weight was added dropwise to the following organic solvent in an amount 10 times the amount of the fluororesin A solution at 25°C, the precipitation of a solid was visually confirmed, and the results are as follows. No solid precipitated: FC-72, FC-770, Novec 7200, Novec 7300, hexafluorobenzene. In all cases, no precipitate formed and the solubility was 90 wt% or more. Solids precipitated: Zeorora H, AE-3000, trifluoroethanol, ethyl acetate, chloroform, acetone, and hexane. In all cases, the recovery rate of fluororesin A after filtration and drying exceeded 80%, and the solubility was less than 20 wt%. [Industrial Applicability]

[0113] The present invention is useful in fields related to fluororesins.

Claims

1. A fluororesin containing a residue unit represented by the following general formula (1), which has a haze value of 2% or less when formed by hot press molding (thickness 1 mm) and a yellowness index of 2 or less when formed by melt molding at 280° C. for 24 hours (thickness 3 mm): The fluororesin has an amount of insoluble matter of 0.2% by weight or less when the fluororesin is dissolved in 1,1,1,2,3,4,4,5,5,5-decafluoro-3-methoxy-2-(trifluoromethyl)pentane. [Case 1] (In formula (1), Rf 1 , Rf 2 , Rf 3 and Rf 4 each independently represents one of the group consisting of a fluorine atom, a linear perfluoroalkyl group having 1 to 7 carbon atoms, a branched perfluoroalkyl group having 3 to 7 carbon atoms, or a cyclic perfluoroalkyl group having 3 to 7 carbon atoms, the perfluoroalkyl group may have an ether oxygen atom, and Rf 1 , Rf 2 , Rf 3 and Rf 4 may be linked together to form a ring having 4 to 8 carbon atoms, and the ring may contain an ether oxygen atom.

2. The bulk density of the fluororesin is 0.1 to 1.5 g / cm 3 The fluororesin according to claim 1,

3. The bulk density of the fluororesin is 0.12 to 0.25 g / cm 3 The fluororesin according to claim 1,

4. The weight average molecular weight of the fluororesin is 5×10 4 ~3×10 5 The fluororesin according to any one of claims 1 to 3, wherein

Citation Information

Patent Citations

  • JP1968029154B1

  • Production of the polymer ring and perfluorocyclobutane ring comprising a perfluorocyclobutane

    JP1992500388A

  • Method for producing fluororesin organosol, fluororesin organosol, and coating composition

    JP2013234209A

  • Production method of fluororesin particles containing fluorine-containing aliphatic ring structure

    JP2020059784A

  • Production method for fluorine-containing copolymer composition, coating composition, molded article and article having coating film

    WO2011129407A1