Composite cable

The composite cable's crosslinked polyolefin sheath and resin-coated conductors improve terminal processability and low-temperature bending resistance, addressing the challenges of sheath removal and durability in composite cables.

JP2024138584APending Publication Date: 2024-10-09FURUKAWA ELECTRIC CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023049135
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

The sheath of composite cables is difficult to remove and lacks adequate bending resistance at low temperatures, compromising terminal processability and durability.

Method used

A composite cable design using a sheath made of crosslinked polyolefin material with a tensile modulus of 30 MPa or more at 23°C and 1000 MPa or less at -40°C, combined with conductors coated in resin layers, enhances flexibility and resistance to bending and heat.

Benefits of technology

The composite cable achieves excellent terminal processability, low-temperature bending resistance, and heat resistance, ensuring durability in harsh environments with frequent vibrations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138584000001_ABST
    Figure 2024138584000001_ABST
Patent Text Reader

Abstract

To provide a composite cable which is excellent in terminal workability, and bending resistance at low temperature.SOLUTION: A composite cable 1 has a plurality of electric wires 2 and 3 having resin layers 22 and 32 on the outer peripheries of conductors 21 and 31, and a sheath 4 coating the outer surfaces of the plurality of electric wires 2 and 3, where a crosslinked polyolefin material having tensile elastic modulus at 23°C of 30 MPa or more and tensile elastic modulus at -40°C of 1,000 MPa or less is used in the sheath 4. Terminal workability, low temperature bendability resistance, and heat resistance can be improved by setting of the tensile elastic modulus at each of the above temperatures.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite cable. [Background technology]

[0002] In recent years, composite cables consisting of multiple cables bundled together with a sheath have come to be used in machines and devices. For example, in a vehicle, in order to operate an anti-lock brake system (hereinafter referred to as ABS), an ABS cable (signal line) is used to transmit a signal from an ABS sensor disposed near the wheels to an ABS control device. Furthermore, with the widespread use of electric parking brakes (hereinafter referred to as EPBs), EPB cables (power lines) are being used to supply power from an EPB control device to an actuator of the EPB.

[0003] In the case of cables whose connection destinations are close to each other, such as the ABS cable and the EPB cable, a composite cable has been suitably used (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5541331 Summary of the Invention [Problem to be solved by the invention]

[0005] The sheath of the above composite cable cannot be easily removed by simply making a cut near the outer periphery, and terminal processability (sheath strippability) for removing the sheath is required. Furthermore, depending on the usage environment, the composite cable may be required to have bending resistance at low temperatures. The terminal workability of a composite cable can be improved by increasing the elastic modulus of the sheath material. However, setting the elastic modulus of the sheath material too high can cause a problem of reduced bending resistance at low temperatures.

[0006] The present invention has been made in consideration of the above problems, and has an object to provide a composite cable which is excellent in terminal workability and bending resistance at low temperatures. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention comprises: A plurality of electric wires each having a resin layer on the outer periphery of a conductor; A composite cable having a sheath covering the outer surfaces of the multiple electric wires, The sheath is characterized by using a crosslinked polyolefin material having a tensile modulus of elasticity of 30 MPa or more at 23°C and 1000 MPa or less at -40°C. Effect of the Invention

[0008] According to the present invention, a composite cable excellent in terminal processability, low-temperature bending resistance, and heat resistance can be provided. [Brief description of the drawings]

[0009] [Figure 1] This is a diagram showing a state in which the signal line of the composite cable is connected to the ABS sensor and the ABS control device, and the power line is connected to the EPB control device and the actuator. [Diagram 2] 1 is a cross-sectional view showing an example of the configuration of a composite cable according to an embodiment of the present invention, showing a four-core configuration. [Diagram 3] 1 is a cross-sectional view showing an example of the configuration of a composite cable according to an embodiment of the present invention, showing a six-core cable. [Figure 4] 1 is a diagram showing that a conductor of a power line or a signal line is formed by twisting together a plurality of wires. [Diagram 5]FIG. 5(a) shows a state in which four signal wires and power wires are twisted together within a composite cable, and FIG. 5(b) shows a state in which six signal wires and power wires are twisted together within a composite cable. [Figure 6] 1 is a table showing the composition of sheath materials in Examples and Comparative Examples and a series of various evaluations. [Figure 7] FIG. 7(a) is a plan view of a sample used to measure the tensile elastic modulus, and FIG. 7(b) is a cross-sectional view of a portion where elongation occurs due to tension. [Figure 8] FIG. 2 is a schematic view showing a test device for a low-temperature bending resistance test as viewed from the axial direction of a mandrel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [Outline of composite cable] Hereinafter, a composite cable according to the present invention will be described with reference to the drawings. However, the embodiments described below are subject to various limitations that are technically preferable for implementing the present invention, but the scope of the present invention is not limited to the following embodiments or illustrated examples. In the following description, "numeric value A to numerical value B" refers to a range of "numerical value A or more and numerical value B or less."

[0011] The composite cable 1 includes a signal wire 2 and a power wire 3 as a plurality of electric wires each having a resin layer 22, 32 around the outer periphery of a conductor 21, 31, and a sheath 4 that collectively covers the outer surfaces of the plurality of signal wires 2 and power wires 3. A plurality of signal lines 2 and a plurality of power lines 3 form a conductor core.

[0012] The composite cable 1 can be used as a cable for electronic control of various machines or devices, such as industrial machines, industrial robots, vehicles, and the like. In this embodiment, a composite cable 1 including electric wires for brake control of a vehicle that is assumed to be used in an environment close to the outside temperature where vibration occurs frequently will be described as an example.

[0013] Specifically, as shown in FIG. 1, the multiple signal lines 2 of the composite cable 1 include a signal line for transmitting a signal from a sensor 11 of an anti-lock braking system to a control device 12, and the multiple power supply lines 3 include a power supply line for supplying power from a control device 13 of an electric parking brake to an actuator 14, but this is not limited to this example.

[0014] 2 and 3 are cross-sectional views showing examples of the configuration of the composite cable 1 according to this embodiment. Fig. 2 shows a four-core cable having two signal lines 2 and two power lines 3. Fig. 3 shows a six-core cable having four signal lines 2 and two power lines 3. In this embodiment, the composite cable 1 includes a plurality of signal lines 2 and a plurality of power lines 3, and each of the signal lines 2 and the power lines 3 has an insulating resin layer 22, 32 on the outer periphery of a conductor 21, 31. The signal lines 2 and the power lines 3 are collectively covered with a sheath 4.

[0015] The outer diameter of the signal line 2 is not particularly limited, but from the standpoint of strength and flexibility, it is, for example, 0.5 to 2.5 mm, and more preferably 1.0 to 2.0 mm. The outer diameter of the power line 3 is not particularly limited, but from the standpoint of strength and flexibility, it is, for example, 1.0 to 5.0 mm, and more preferably 2.0 to 4.0 mm.

[0016] 4, the conductors 21, 31 of the signal line 2 and the power line 3 are conductors formed by twisting together a plurality of strands 21a, 31a. The strands 21a, 31a are made of copper, a copper alloy, aluminum, or an aluminum alloy. The cross-sectional shape of each of the wires 21a, 31a of the conductors 21, 31 may be circular (round wire) or rectangular (rectangular wire). The diameter of the wire is, for example, 0.05 to 0.2 mm. The number of wires may be more than one. The tensile strength of the wire is preferably 350 to 900 MPa. The tensile strength of the wire can be measured in accordance with JISC 3002.

[0017] In consideration of strength and flexibility, the outer diameter of the conductor 21 is, for example, 0.3 to 2.0 mm, more preferably 0.3 to 1.5 mm, and the outer diameter of the conductor 31 is, for example, 0.5 to 4.0 mm, more preferably 1.0 to 3.5 mm. The cross-sectional area of ​​conductor 21 is, for example, 0.05 to 2.0 SQ, and more preferably 0.05 to 1.25 SQ, and the cross-sectional area of ​​conductor 31 is, for example, 0.3 to 8.0 SQ, and more preferably 0.5 to 3.0 SQ. It is assumed that a larger current will flow through conductor 31 of power line 3 than through conductor 21 of signal line 2.

[0018] The resin layers 22, 32 of the signal line 2 and the power line 3 cover the conductors 21, 31. The resin layers 22, 32 are preferably made of a heat-resistant resin. There are no particular limitations on the heat-resistant resin as long as it has insulating properties and heat resistance, and examples of the heat-resistant resin include thermoplastic resin and thermosetting resin. Specific examples include (crosslinked) polyethylene, polyamide, polyamideimide (PAI), polyimide (PI), polyurethane, chloroprene rubber, and rubber made of ethylene-vinyl acetate copolymer (EVA rubber). The resin layer may contain various commonly used additives.

[0019] The (total) thickness of the resin layers 22, 32 is not particularly limited and can be appropriately determined depending on the application, etc. For example, in terms of heat resistance, flexibility, and abrasion resistance, the thickness is preferably 0.2 to 1.5 mm, and more preferably 0.2 to 1.0 mm. In the present invention, when the conductor 21, 31 is a twisted wire, the thickness of the resin layer 22, 32 indicates the shortest distance between the imaginary circumscribing circle of all the wires 21a, 31a constituting the conductor 21, 31 and the outer contour of the resin layer 22, 32 in a cross section perpendicular to the axis of the signal line 2 or power line 3.

[0020] The dashed circles including pairs of signal wires 2 in FIG. 2 and FIG. 3 indicate that the signal wires 2 are twisted together at predetermined intervals. In this manner, by configuring two or more of the multiple signal lines 2 to be twisted together, the twisted signal lines 2 become more flexible than when the signal lines 2 are not twisted together.

[0021] At the same time, when the composite cable 1 is pulled in the longitudinal direction, the twisted signal wires 2 can stretch in that direction. Therefore, when the composite cable 1 is subjected to repeated bending forces, the twisted signal wires 2 stretch, making it less likely to break.

[0022] Also, cross-linked polyethylene electric wires may be used for the signal line 2 and the power line 3. Examples of such electric wires include electric wires whose base resin is cross-linked polyethylene with a heat resistance temperature equivalent to 120°C, which corresponds to cross-linked polyethylene insulated heat-resistant low-voltage wire for automobiles (AEX) and ultra-thin cross-linked polyethylene insulated heat-resistant low-voltage wire for automobiles (AESSX), as specified in the Japan Automotive Engineering Society (JASO) D 611. The cross-linked polyethylene electric wire may be manufactured as appropriate, or a commercially available one may be used. Furthermore, the conductor core may have an insulated wire in addition to the signal wire 2 and the power wire 3. The insulated wire has the same configuration as the signal wire 2 and the power wire 3, except that the outer diameter of the insulated wire is larger than that of the signal wire 2 and smaller than that of the power wire 3.

[0023] As shown in FIGS. 5(a) and 5(b), in the composite cable 1, the twisted signal wires 2 and the power wires 3 are further twisted together inside the sheath 4 as a whole. This allows the composite cable 1 to stretch overall, improving overall flexibility and repeated bending resistance. FIG. 5(a) shows a case where the composite cable 1 has four cores (see FIG. 2), and FIG. 5(b) shows a case where the composite cable 1 has six cores (see FIG. 3). It should be noted that the present invention is not limited to the above example, and the signal lines 2 may be arranged in parallel without being twisted together, and the signal line 2 and the power line 3 may also be arranged in parallel without being twisted together.

[0024] [sheath] The sheath 4 may be a single layer or multiple layers, and the thickness of the sheath 4 can be appropriately determined depending on the application. The thickness of the sheath 4 is, for example, 0.5 to 3.0 mm, more preferably 0.8 to 2.0 mm, in terms of flexibility, bending resistance, and abrasion resistance. The thickness of the sheath 4 means the shortest distance between the circumscribing circle for the entirety of the multiple signal wires 2 and the multiple power wires 3 and the outer contour line of the sheath 4 in a cross section perpendicular to the axis of the composite cable 1. The cross-sectional shape of the composite cable 1 is circular, but may be other shapes. The outer diameter of the sheath 4 is equal to the outer diameter of the composite cable 1, and the size is, for example, 5.0 to 30.0 mm, more preferably 5.0 to 15.0 mm, in terms of flexibility, bending resistance, and abrasion resistance.

[0025] A cross-linked polyolefin material is used for the sheath 4. The cross-linked polyolefin material of the sheath 4 has a tensile modulus of elasticity of 30 MPa or more at 23°C and 1000 MPa or less at -40°C. That is, the sheath 4 maintains a relatively high tensile modulus of elasticity for a cross-linked polyolefin material at 23°C, while maintaining a relatively low tensile modulus of elasticity for a cross-linked polyolefin material at a low temperature of -40°C.

[0026] [Resin composition for forming sheath] The resin composition for forming the sheath is a polyolefin resin, which is crosslinked by electron beam crosslinking through irradiation with an electron beam, silane crosslinking through a silane crosslinking method, or other crosslinking methods when the sheath is formed.

[0027] [Base resin] The base resin is preferably a polyolefin resin, since it can be crosslinked by electron beam or can undergo a grafting reaction with a silane coupling agent, which will be described later. The polyolefin resin is not particularly limited as long as it is a resin made of a homopolymer or copolymer of a compound having an ethylenically unsaturated bond, and those used in ordinary electric wires or cables can be used. For example, polyethylene, polypropylene, ethylene-α-olefin copolymer, polyolefin copolymer having an acid copolymer component or an acid ester copolymer component, and rubber or elastomer of these polymers can be mentioned. Examples of rubber or elastomer include ethylene rubber, styrene elastomer, copolymer rubber of alkyl acrylate and ethylene (ethylene acrylic rubber), and the like. Among them, polyethylene, polypropylene, ethylene-α-olefin copolymer, polyolefin copolymer having an acid copolymer component, and the like are preferable. Polyethylene resin is more preferable because it has a large effect of improving abrasion resistance when used in combination with ethylene rubber or styrene elastomer. The polyolefin resin may be used alone or in combination of two or more kinds. In the present invention, the polyolefin resin or resin component may each be used alone or in combination of two or more kinds. The polyolefin resin may also contain an organic mineral oil, which will be described later.

[0028] The ethylene rubber is not particularly limited as long as it is a rubber (including elastomer) made of a copolymer obtained by copolymerizing a compound having an ethylenically unsaturated bond, and known rubbers can be used.Preferably, the ethylene rubber includes a binary copolymer rubber of ethylene and an α-olefin, a ternary copolymer rubber of ethylene, an α-olefin, and a diene, and the like.The diene component of the ternary copolymer may be a conjugated diene component or a non-conjugated diene component, but a non-conjugated diene component is preferred. As the α-olefin component, each α-olefin component having 3 to 12 carbon atoms is preferable. As the conjugated diene component, for example, each component such as butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, etc. are mentioned, and butadiene component, etc. are preferable. As a specific example of the non-conjugated diene component, for example, each component such as dicyclopentadiene (DCPD), ethylidenenorbornene (ENB), 1,4-hexadiene, etc. are mentioned. As the binary copolymer rubber, ethylene-propylene rubber (EPM) is preferred, and as the ternary copolymer rubber, ethylene-propylene-diene rubber (EPDM) is preferred. The ethylene rubber may be used alone or in combination of two or more kinds.

[0029] The styrene elastomer refers to a polymer having an aromatic vinyl compound as a constituent component in the molecule. Examples of such styrene elastomers include block copolymers and random copolymers of conjugated diene compounds and aromatic vinyl compounds, or hydrogenated products thereof. Examples of such styrene elastomers include styrene-ethylene-butylene-styrene block copolymers (SEBS), styrene-isoprene-styrene block copolymers (SIS), hydrogenated SIS, styrene-butadiene-styrene block copolymers (SBS), hydrogenated SBS, styrene-ethylene-ethylene-propylene-styrene block copolymers (SEEPS), styrene-ethylene-propylene-styrene block copolymers (SEPS), styrene-butadiene rubber (SBR), hydrogenated styrene-butadiene rubber (HSBR), etc. The styrene-based elastomers may be used alone or in combination of two or more.

[0030] The polyethylene resin may be any polymer resin containing an ethylene component, such as high density polyethylene (HDPE), low density polyethylene (LDPE), ultra-high molecular weight polyethylene (UHMW-PE), linear low density polyethylene (LLDPE), and very low density polyethylene (VLDPE). Of these, linear low density polyethylene and low density polyethylene are preferred.

[0031] Examples of polyolefin copolymer resins having an acid copolymer component or an acid ester copolymer component include resins made of ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-alkyl(meth)acrylate copolymer (preferably having 1 to 12 carbon atoms), and the like.

[0032] The polypropylene resin may be any polymer containing a propylene component as the main component, and resins such as a propylene homopolymer (homopolypropylene resin), an ethylene-propylene random copolymer, or an ethylene-propylene block copolymer can be used. The ethylene-propylene random copolymer refers to a copolymer containing about 1 to 10 parts by mass of ethylene components, and the ethylene components are randomly incorporated into the propylene chain. The ethylene-propylene block copolymer refers to a copolymer containing about 5 to 20 parts by mass of ethylene or ethylene-propylene rubber (EPM) components, and has an island structure in which the ethylene or EPM components are present independently in the propylene component. In terms of appearance, the polypropylene resin is particularly preferably an ethylene-propylene random copolymer resin. The ethylene content is a value measured in accordance with the method described in ASTM D3900. The polypropylene resin is preferably contained in an amount of 5 to 30 parts by mass relative to 100 parts by mass of the base resin.

[0033] The organic mineral oil may be any oil that is commonly used in resin compositions, and may be used without any particular limitation, including paraffinic oil and naphthenic oil, with paraffinic oil being preferred. The organic mineral oil may be used alone or in combination of two or more kinds.

[0034] [Inorganic filler] The resin composition preferably contains the inorganic filler described below in addition to the above-mentioned base resin, and may contain various additives such as an antioxidant. The inorganic filler is not particularly limited, and examples thereof include metal hydrates such as compounds having hydroxyl groups or crystal water, such as aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whisker, hydrated aluminum silicate, hydrated magnesium silicate, basic magnesium carbonate, hydrotalcite, and talc. Other examples include boron nitride, silica (crystalline silica, amorphous silica, etc.), carbon black, clay, zinc oxide, tin oxide, titanium oxide, molybdenum oxide, antimony trioxide, silicone compounds, quartz, zinc borate, white carbon, zinc borate, zinc hydroxystannate, zinc stannate, etc. The inorganic filler may be used alone or in combination of two or more kinds. The inorganic filler is preferably contained in an amount of 10 parts by mass or more and 150 parts by mass or less per 100 parts by mass of the base resin.

[0035] [Sheath formation: when electron beam crosslinking is performed on the resin composition] The formation of the sheath 4 by the electron beam crosslinking method is carried out in the following procedure. First, each component is mixed to prepare a resin composition. The mixing method is not particularly limited as long as it is a method usually used for preparing a composition, and various mixing devices can be used. The mixing conditions are also not particularly limited and are set appropriately, but usually, the components are mixed while the base resin is melted. The resin composition thus obtained is then placed (molded) on the outer surface of the conductor core. The method of placement is not particularly limited, and examples thereof include extrusion molding, injection molding, and molding methods using other molding machines. A method of extrusion molding simultaneously with the conductor core is preferred. The molding temperature is set to a temperature at which the base resin melts depending on the various conditions such as the type of base resin and the extrusion speed (take-off speed), and can be set to, for example, 80 to 250°C. The preparation of the resin composition and the molding can be carried out simultaneously or successively.

[0036] In this manner, the layer of the resin composition disposed on the outer surface of the conductor core is crosslinked by irradiating it with electron beams. In the electron beam crosslinking resin composition, the degree of crosslinking can be improved by appropriately adding a methacrylate-based crosslinking assistant as a crosslinking assistant. As the crosslinking aid, a polyfunctional compound that is usually used for crosslinking of resins can be used, and examples thereof include polyfunctional vinyl compounds such as divinylbenzene and triallyl cyanurate, and polyfunctional (meth)acrylate compounds such as ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, and allyl methacrylate. The content of the crosslinking agent is preferably 1 to 5 parts by mass with respect to 100 parts by mass of the base resin. The conditions for irradiation with the electron beam are appropriately set depending on the type of base resin, the degree of crosslinking, and the like. In this manner, the composite cable 1 of the present invention having the sheath 4 made of the electron beam cross-linked resin composition can be produced.

[0037] [Sheath formation: when silane crosslinking is performed on the resin composition] The formation of the sheath 4 by the silane crosslinking method is carried out in the following procedure. First, prepare a silane crosslinkable resin composition. The silane crosslinkable resin composition may be prepared using a commercially available silane graft resin. The silane crosslinkable resin composition may also be prepared by melt mixing a base resin, a silane coupling agent, a silanol condensation catalyst, and preferably an inorganic filler in the presence of an organic peroxide at a temperature equal to or higher than the decomposition temperature of the organic peroxide.

[0038] The silane-crosslinkable resin composition thus prepared is placed on the outer peripheral surface of a conductive core. The silane crosslinkable resin composition may be disposed by any method that can cover the conductor core with the silane crosslinkable resin composition, and an appropriate molding method is applied. For example, the silane crosslinkable resin composition may be disposed by extrusion molding using an extruder, injection molding using an injection molding machine, or molding using other molding machines. Extrusion molding in which the conductive core and the silane crosslinkable resin composition are co-extruded is preferred. The extrusion molding can be carried out using a general-purpose extruder.

[0039] The silane crosslinkable resin composition is then contacted with moisture to cause crosslinking. This hydrolyzable silyl group of the silane coupling agent is hydrolyzed to a silanol (OH group bonded to a silicon atom), and the hydroxyl groups of the silanol are condensed with each other by the silanol condensation catalyst present in the silane crosslinkable resin composition. The above condensation reaction proceeds at room temperature in the presence of a silanol condensation catalyst, so there is no need to actively contact the silane crosslinkable resin composition arranged on the outer peripheral surface of the conductor core with water. However, in order to promote the crosslinking reaction, the silane crosslinkable resin composition may be brought into contact with moisture. For example, a method of actively contacting the composition with water, such as immersion in warm water, immersion in a moist heat bath, or exposure to high-temperature steam, can be adopted. When the silane crosslinkable resin composition comes into contact with moisture, the silane coupling agent that is strongly bonded to the inorganic filler is less likely to undergo a silanol condensation reaction, and maintains its bond with the inorganic filler, enabling strong adhesion (high affinity) between the base resin and the inorganic filler. On the other hand, the silane coupling agent that is weakly bonded to the inorganic filler undergoes a silanol condensation reaction, and crosslinks the base resins together via silanol bonds (siloxane bonds).

[0040] By the above procedure, a sheath 4 made of a silane crosslinked product of the silane crosslinkable resin composition is formed on the outer peripheral surface of the conductor core.

[0041] [Example] The present invention will be described in detail below based on examples, but the present invention is not limited thereto. Fig. 6 is a table showing the components of the material of the sheath 4 and the results of evaluation of the specific test for Examples 1 to 11 and Comparative Examples 1 to 5. 6, the numerical values ​​relating to the blending amounts in each example are in parts by mass unless otherwise specified. Furthermore, in each component column, a blank space means that the blending amount of the corresponding component is 0 parts by mass.

[0042] Details of the sheath material including each component (compound) shown in FIG. 6 are given below. [Base resin] Evolue SP0540 (product name), LLDPE (linear low-density polyethylene), manufactured by Prime Polymer Co., Ltd. Evaflex EV360 (product name), EVA (ethylene-vinyl acetate copolymer resin), manufactured by Mitsui DuPont Polychemicals Hi-Zex 5305E (product name), HDPE (high density polyethylene), manufactured by Prime Polymer SunAllomer PB222A (product name), PP (polypropylene), manufactured by SunAllomer Co., Ltd. Mitsui 3092M (product name), ethylene-propylene-diene rubber, manufactured by Mitsui Chemicals, Inc. Tuftec (registered trademark) N504 (product name), SEBS (styrene-based elastomer), manufactured by Asahi Kasei Corporation Diana Process Oil PW-90 (product name), organic mineral oil (paraffin-based oil), manufactured by Idemitsu Kosan Co., Ltd. [Inorganic filler] Magnesium hydroxide, manufactured by Konoshima Chemical Co., Ltd. [Silane coupling agent] KBM-1003 (product name), vinyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd. [Organic peroxide] Perhexa 25B (trade name), 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, manufactured by NOF Corporation [Silanol Condensation Catalyst] Adeka STAB OT-1 (product name), dioctyltin dilaurate, manufactured by ADEKA Corporation

[0043] [Making the conductor core] First, two pairs of signal wires made of cross-linked polyethylene electric wires with a conductor cross-sectional area of ​​0.25SQ, a conductor outer diameter of 1.4 [mm], and a resin layer thickness of 0.3 [mm] were twisted together to obtain a twisted wire (twisting rate 1%). The obtained twisted signal wire 2 was twisted together with two power wires made of cross-linked polyethylene electric wires with a conductor cross-sectional area of ​​1.8SQ, a conductor outer diameter of 2.6 [mm], and a resin layer thickness of 0.3 [mm] to produce the conductor core shown in Figure 2 (twisting rate 1.5%, the total twisting rate of each thin electric wire is about 2.5%).

[0044] [Examples 2, 4, and 7] A sheath was formed by electron beam crosslinking as described below to produce a four-core composite cable as shown in FIG. The components of the base resin section and the inorganic filler section of Examples 2, 4, and 7 in FIG. 6 were charged into a Banbury mixer and melt-mixed at 120 to 200°C for 10 minutes. The components were then discharged at a material discharge temperature of 200°C and passed through a feeder rudder to obtain pellets of the resin composition. A sheath was formed using the prepared conductor core and the obtained pellets as follows. That is, the obtained pellets were introduced into an extruder equipped with a screw with a diameter of 90 [mm] (ratio of effective screw length L to diameter D: L / D=24, compression section screw temperature 190 [°C], head temperature 200 [°C]). While melting the pellets in this extruder, they were directly extruded (placed) on the outer peripheral surface of the conductor core with a thickness of 1 [mm] to obtain a cable with an outer diameter of 8 [mm]. Next, the resin composition placed on the outer peripheral surface of the conductive core was irradiated with an electron beam at an accelerating voltage of 500 kV. In this manner, the composite cables (outer diameter 8 mm) of Examples 2, 4, and 7 each having a sheath with a layer thickness of 1 mm formed from an electron beam cross-linked product were manufactured.

[0045] [Examples 1, 3, 5, 6, 8 to 11, Comparative Examples 1, 2, 5] A sheath was formed by the silane crosslinking method as described below to produce the four-core composite cable shown in FIG. When the sheath was formed by the silane crosslinking method, 95 parts by mass of the total 100 parts by mass shown in each Example column in Figure 6 was used as the base resin to prepare the silane master batch, and the remaining 5 parts by mass was used to prepare the catalyst master batch.

[0046] To prepare the silane master batch, first, the silane coupling agent and organic peroxide described above were mixed (dry blended) at 25°C, and then the inorganic filler was added and mixed (dry blended) at 30°C. Next, the obtained mixture and the base resin in the amount shown in the base resin column of Figure 6 (excluding the catalyst master batch) were charged into a Banbury mixer and melt-mixed at 120 to 200 [°C] for 10 minutes, and then discharged at a material discharge temperature of 200 [°C] and passed through a feeder rudder to obtain pellets of the silane master batch. The silane-grafted resin was synthesized by inducing a silane-grafting reaction through melt mixing in the Banbury mixer.

[0047] To prepare the catalyst master batch, the base resin in the amount (for the catalyst master batch) shown in the base resin column in Figure 6 and the above-mentioned silanol condensation catalyst were charged into a Banbury mixer and melt-mixed at 170°C. The mixture was then discharged at a material discharge temperature of 180°C and passed through a feeder rudder to obtain pellets of the catalyst master batch.

[0048] Next, the prepared pellets of the silane master batch and the pellets of the catalyst master batch were dry blended. The obtained dry blend was introduced into an extruder equipped with a screw having a diameter of 90 [mm] (ratio of effective screw length L to diameter D: L / D=24, compression section screw temperature 190 [℃], head temperature 200 [℃]). While melt-mixing the dry blend (preparing a silane crosslinkable resin composition) in this extruder, it was directly extruded (placed) with a thickness of 1 [mm] onto the outer peripheral surface of the twisted conductor core to obtain a coated conductor with an outer diameter of 8 [mm]. Furthermore, the obtained coated conductor was left in an atmosphere of a temperature of 60°C and a relative humidity of 95% for 24 hours to come into contact with water. In this manner, composite cables (outer diameter 8 [mm]) of Examples 1, 3, 5, 6, 8 to 11 and Comparative Examples 1, 2, and 5 each having a sheath with a layer thickness of 1 [mm] formed of a silane crosslinked product were manufactured.

[0049] [Comparative Examples 3 and 4] Composite cables (outer diameter 8 mm) of Comparative Examples 3 and 4 having a sheath with a layer thickness of 1 mm formed from a non-crosslinked resin composition were manufactured in the same manner as in Examples 2 and 4, except that the resin composition placed on the outer surface of the conductor core was not irradiated with an electron beam.

[0050] [Evaluation test] The composite cables of Examples 1 to 11 and Comparative Examples 1 to 5 were subjected to the following various evaluations, and the results are shown in FIG.

[0051] [23℃ tensile modulus] For the sheaths of the composite cables of Examples 1 to 11 and Comparative Examples 1 to 5, the tensile modulus was measured according to the definition of JIS K 7161-1 (ISO 527-1). According to the above standard, the tensile modulus is defined as the slope of the stress / strain curve corresponding to the two points of 0.05% and 0.25% strain. Em = Δσ / Δε Em: Tensile modulus [MPa] Δσ: Stress difference between two points of 0.05% and 0.25% of the original average cross-sectional area Δε: Difference in strain between two points, 0.05% and 0.25%

[0052] For the above measurements, the sheath of each composite cable was punched out to prepare a Type 2 test specimen as defined in JIS K 7113 (see Figs. 7(a) and 7(b)). The testing machine used was one that conformed to JIS B 7721 and ISO 9513. A tensile load was applied to both ends of the test piece at a speed of 0.25 mm / min for one minute in an environment of 23° C., and the tensile load and the amount of deformation due to elongation were measured during that time. The tensile stress was calculated by dividing the tensile load by the cross-sectional area D×I of the portion indicated by the length G of the test piece. The strain was determined by dividing the amount of elongation at a portion of the test piece indicated by length G by the original length G. The tensile modulus was calculated from the tensile stress when a strain of 0.05% occurred and the tensile stress when a strain of 0.25% occurred in the above measurement.

[0053] From the obtained tensile modulus of elasticity, the tensile modulus at 23° C. was evaluated as good or bad. "A" below is good (passed), and "B" is bad (failed). A: When the tensile modulus at 23°C is 30 MPa or more B: When the tensile modulus at 23°C is less than 30 [MPa]

[0054] [-40℃ tensile modulus] For the sheaths of the composite cables of Examples 1 to 11 and Comparative Examples 1 to 5, the same measurements as for the tensile modulus at 23° C. were performed in an environment of −40° C., and the tensile modulus was calculated. From the tensile modulus thus obtained, the -40°C tensile modulus was evaluated as good or bad. "A" below indicates good (passed), and "B" indicates bad (failed). A: -40℃ tensile modulus is 1000[MPa] or less, judging it as "good". B: -40℃ tensile modulus exceeds 1000 [MPa], judged as "no".

[0055] [Terminal workability test] The end portion of each of the composite cables of Examples 1 to 11 and Comparative Examples 1 to 5 was 100 mm long, and the peelability when stripping the sheath was evaluated. Specifically, a slit was made in the circumferential direction perpendicular to the axial direction of the composite cable, to a depth of 90% of the thickness of the covering of the composite cable. Next, in an environment of 23°C and relative humidity of 50%, the sheath of one composite cable was grasped at the slit, and the other composite cable was pulled out. The composite cables thus drawn were subjected to a terminal processability test for the sheath and evaluated according to the following criteria: "A" is excellent (pass), "B" is good (pass), and "C" is poor (fail). A: When there is no remaining sheath to be pulled from the pulled cable, and the elongation of the sheath end of the pulled cable is 0.6 mm or less. B: When there is no remaining sheath in the pulled cable and the elongation of the sheath end of the pulled cable is more than 0.6 mm but not more than 0.8 mm C: When the sheath that should have been pulled out remains in the pulled cable or when the extension of the sheath end of the pulled cable exceeds 0.8 mm

[0056] [Low temperature bending resistance test] The composite cables of Examples 1 to 11 and Comparative Examples 1 to 5 were subjected to a low-temperature bending resistance test. FIG. 8 is a schematic diagram of the test device used in this test, viewed from the axial direction of the mandrel. As shown in FIG. 8, the testing apparatus has two mandrels 51, 52 arranged horizontally and parallel to each other with a predetermined distance between them, and anti-swaying pressure plates 61, 62 arranged vertically below the mandrels 51, 52 with a predetermined distance between them. The composite cable 1 of Examples 1 to 11 or Comparative Examples 1 to 5 was arranged in a vertical direction between the mandrels 51 and 52 and between the pressers 61 and 62, and a weight W was attached to the lower end of the composite cable 1. In this state, the upper end of the composite cable 1 was repeatedly bent left and right so as to alternately contact the upper outer circumference of the left and right mandrels 51 or 52. The number of bending times was counted as one bending time when the composite cable 1 was bent so as to contact the outer circumference of either the left or right mandrel 51 or 52. The test conditions were a mandrel diameter of 20 [mm], a left and right bending angle of 90 [°], and a speed of 60 [bending / min], a weight of 2 [kg], a clearance between the cable and the mandrel of 1 [mm], and a length of bending was adjusted so that the upper side of the composite cable 1 contacted the upper outer circumference of each mandrel 51, 52, and the test was performed in an atmosphere of -40 [℃]. The composite cables 1 were connected in series in a loop shape and electricity was applied. That is, the multiple signal lines 2 and the multiple power lines 3 are connected to each other as a single electric wire by connecting the ends of the conductors 21 of the signal lines 2 of the composite cable 1, the ends of the conductors 31 of the power lines 3, or the ends of the conductors 21 of the signal lines 2 and the ends of the conductors 31 of the power lines 3. Then, the single electric wire was repeatedly bent while passing electricity through both ends of the wire. The number of times the wire was bent until breakage occurred was measured. The composite cable 1 was evaluated for pass / fail based on the number of times it could be bent until breakage occurred. "A" below indicates good (passed) and "B" indicates bad (failed). A: More than 50,000 times B: Less than 50,000 times

[0057] [Heat resistance test] The composite cables of Examples 1 to 11 or Comparative Examples 1 to 5 were wound around a mandrel having the same outer diameter as the composite cable, and placed in a thermostatic chamber at 250°C for 30 minutes, and evaluated for quality based on the presence or absence of cracks in the sheath. "A" below is good (passed), and "B" is bad (failed). A: If no cracks occurred (or were not confirmed) in the sheath B: If a crack occurs in the sheath

[0058] [Wear resistance test] The abrasion resistance test is a reference evaluation test that is required for composite cables depending on their applications. Using an abrasion tester and abrasion tape specified in JASO D 625-2, the sheath of the composite cable of Examples 1 to 11 or Comparative Examples 1 to 5 was completely worn away, and the abrasion tape length until the abrasion tape contacted the conductor core was measured. An alumina abrasive (grain size P180) was used for the abrasion tape, the feed rate was 1500±75 [mm / min], and the pressing load was 0.45 [kgf] (4.4 [N]). The quality was evaluated based on whether the length of the wear tape that was fed until it contacted the conductor core fell within the following criteria. "A" below is good (passed) and "B" is bad (failed). A:20[m] or more B: Less than 20m

[0059] [Low temperature limit test] The low temperature limit test is a reference evaluation test required for composite cables depending on their applications. The low temperature limit test was carried out in accordance with JIS C 3005 (ISO 527-1). The composite cables (outer diameter 8 mm) of Examples 1 to 11 or Comparative Examples 1 to 4 were cooled in a low-temperature bath at -60°C for 1 hour, then removed and immediately wrapped around a sample cylinder with an outer diameter of 40 mm three times at a uniform speed without any gaps, and the surface of the sheath was observed. The quality was evaluated based on whether cracks had occurred on the surface of the sheath. "A" below is good (passed) and "B" is bad (failed). A: No cracks on the sheath surface B: Cracks on the sheath surface

[0060] [Test Results] The evaluation results of the above tests for Examples 1 to 11 and Comparative Examples 1 to 5 are shown in the table of FIG. In Examples 1 to 11, a sheath was formed by crosslinking a base resin containing the polyolefin shown in Figure 6, and as a result, the tensile modulus at 23°C was able to be 30 [MPa] or more and the tensile modulus at -40°C was able to be 1000 [MPa] or less. Furthermore, it was shown that all of Examples 1 to 11, which satisfy the appropriate numerical range conditions for the 23°C tensile modulus and the -40°C tensile modulus, have good terminal processability, low-temperature bending resistance, and heat resistance as shown in the terminal processability test, low-temperature bending resistance test, and heat resistance test. Furthermore, in the case of a non-crosslinked sheath, even if the base resin contains polyolefin, as shown in Comparative Examples 3 and 4, it was shown that the heat resistance indicated by the heat resistance test was reduced.

[0061] Furthermore, among Examples 1 to 11, Examples 1 to 5, 8, and 9 which satisfy the two requirements of (1) the cross-linked polyolefin material of the sheath contains 5 to 30 parts by mass of polypropylene per 100 parts by mass of base resin, and (2) the cross-linked polyolefin material of the sheath contains 10 to 150 parts by mass of inorganic filler per 100 parts by mass of base resin, were shown to have good abrasion resistance as shown in the abrasion resistance test, which is a reference evaluation, and good low temperature limit property, which indicates the crack suppression effect at -60°C in the low temperature limit test.

[0062] [Technical Effects of the Invention Embodiments] The sheath 4 of the composite cable 1 uses a cross-linked polyolefin material with a tensile modulus of elasticity of 30 MPa or more at 23°C and 1000 MPa or less at -40°C. As a result, for a resin material at room temperature, it maintains a relatively high tensile modulus of elasticity, and for example, when connecting the composite cable 1, it is easy to process the terminals, improving workability, and the high workability makes it possible to perform good connections. On the other hand, as a resin material at low temperatures, it is possible to maintain a relatively low tensile modulus of elasticity and suppress the occurrence of cracks, fissures, etc. when bent. Therefore, once connected, the composite cable 1 can exhibit high durability, coupled with a good connection state, even in harsh environments where it is exposed to the outside air and vibration. Furthermore, since the sheath 4 of the composite cable 1 has the above-mentioned characteristics, it is possible to improve the terminal processability, low-temperature bending resistance, and heat resistance.

[0063] Furthermore, in the composite cable 1, the cross-linked polyolefin material of the sheath 4 contains 5 parts by mass or more and 30 parts by mass or less of polypropylene per 100 parts by mass of the base resin, and therefore it is possible to improve the abrasion resistance.

[0064] In addition, since the cross-linked polyolefin material of the sheath 4 of the composite cable 1 contains 10 parts by mass or more and 150 parts by mass or less of inorganic filler per 100 parts by mass of the base resin, it is possible to improve the abrasion resistance or the low temperature limit.

[0065] Furthermore, since composite cable 1 includes electric wires having conductors with different outer diameters, it becomes possible to wire electric wires with different transmission currents depending on the application or the like in a single unit.

[0066] The composite cable 1 also includes, as an electric wire, a signal line 2 for controlling the brakes of the vehicle. The composite cable 1 including the signal line 2 for brake control is wired from the main frame of the vehicle body to the vicinity of the wheels. In that case, it may be exposed to a harsh environment where the temperature is low due to the influence of the outside air and where relative vibration between the main frame and the wheels occurs frequently. Even in such a case, the signal line 2 can be effectively protected by the low-temperature bending resistance of the sheath 4 of the composite cable 1.

[0067] The composite cable 1 also includes, as multiple electric wires, a signal wire 2 for transmitting a signal from a sensor of the antilock braking system to a control device, and a power supply wire 3 for supplying power from the control device of the electric parking brake to an actuator. A composite cable 1 including a signal line 2 for brake control and a power line 3 for supplying power to the actuator is wired from the main frame of the vehicle to the vicinity of the wheels. In this case, the cable may be exposed to a harsh environment where the temperature is low due to the influence of the outside air and where relative vibration between the main frame and the wheels occurs frequently. Even in such a case, the signal line 2 and the power line 3 can be effectively protected by the low-temperature bending resistance of the sheath 4 of the composite cable 1.

[0068] [others] It goes without saying that the present invention is not limited to the above-described embodiment, and can be modified as appropriate without departing from the spirit of the present invention. For example, although the sheath 4 is formed in only one layer in FIGS. 2 and 3, it is also possible to form the sheath 4 in a plurality of layers.

[0069] In addition, since the part inside the vehicle in which the composite cable 1 is arranged may become relatively hot, it is also possible to configure the resin layers 22, 32, etc. of the signal line 2 and the power line 3 to be made of a heat-resistant resin, etc. [Explanation of symbols]

[0070] 1 Composite Cable 2 Signal Line 21 Conductor 21a Bare wire 22 Resin layer 3 Power line 31 Conductor 31a Bare wire 32 Resin layer 11 Sensors 12 Control Devices 13 Control Devices 14 Actuator

Claims

1. A plurality of electric wires each having a resin layer on the outer periphery of a conductor; A composite cable including a sheath covering an outer surface of the plurality of electric wires, A composite cable characterized in that the sheath is made of a cross-linked polyolefin material having a tensile modulus of elasticity of 30 MPa or more at 23°C and a tensile modulus of elasticity of 1000 MPa or less at -40°C.

2. 2. The composite cable according to claim 1, wherein the cross-linked polyolefin material contains 5 parts by mass or more and 30 parts by mass or less of polypropylene per 100 parts by mass of a base resin.

3. 2. The composite cable according to claim 1, wherein the cross-linked polyolefin material contains 10 parts by mass or more and 150 parts by mass or less of an inorganic filler per 100 parts by mass of a base resin.

4. 2. The composite cable according to claim 1, wherein the plurality of electric wires include electric wires having conductors with different outer diameters.

5. 5. The composite cable according to claim 4, wherein the plurality of electric wires includes electric wires for controlling a brake of a vehicle.

6. 5. The composite cable according to claim 4, wherein the plurality of electric wires include a signal wire for transmitting a signal from a sensor of an antilock braking system to a control device, and a power supply wire for supplying power from a control device of an electric parking brake to an actuator.

Citation Information

Patent Citations

  • Optical fiber with cured polymer coating

    JP2006502425A

  • Composite cable

    JP2020161397A

  • Polymer Composition for Cable Jackets

    JP2022520037A

  • Roaster

    JP1980041331A