Gas barrier laminate and packaging bag
The gas barrier laminate with a paper base, resin layers, and vapor deposition layer addresses crack-induced deterioration, ensuring long-term water vapor barrier performance and reduced plastic use.
Patent Information
- Application Number
- JP2023049308
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional gas barrier laminates using paper base materials suffer from cracks in the gas barrier layer over time, leading to deterioration of water vapor barrier properties.
A gas barrier laminate comprising a paper base material, a first resin layer, and a vapor deposition layer, with specific dimensional change rates and layer configurations to suppress crack formation, including a second resin layer for improved adhesion and flexibility.
The laminate effectively maintains water vapor barrier properties over time, reducing plastic usage and contributing to environmental sustainability.
Smart Images

Figure 2024138698000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a gas barrier laminate and a packaging bag. [Background technology]
[0002] In many fields, such as food, beverages, pharmaceuticals, and chemicals, packaging materials are used according to the contents. Packaging materials are required to have gas barrier properties that prevent the permeation of water vapor, which can cause deterioration of the contents.
[0003] In recent years, the momentum for eliminating plastic has been growing due to growing environmental awareness triggered by the problem of marine plastic waste. From the viewpoint of reducing the amount of plastic materials used, the use of paper instead of plastic materials has been considered in various fields. For example, the following Patent Document 1 shows that the impact resistance and processability of heat seal paper can be improved by using a paper base material having specific parameters. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2021-188241 A Summary of the Invention [Problem to be solved by the invention]
[0005] In order to realize high gas barrier properties in paper packaging materials, it is conceivable to use a gas barrier laminate in which a vapor deposition layer is provided as a gas barrier layer on a paper substrate. However, it has been found that in the case of gas barrier laminates using conventional paper substrates, cracks may occur in the gas barrier layer over time, and the gas barrier properties, particularly the water vapor barrier properties, may deteriorate.
[0006] The present invention has been made in consideration of the above circumstances, and has an object to provide a gas barrier laminate using paper, in which deterioration of water vapor barrier properties over time is suppressed, and a packaging bag including the same. [Means for solving the problem]
[0007] The present invention relates to, for example, the following [1] to [7]. [1] A gas barrier laminate comprising a paper substrate, a first resin layer, and a deposition layer in this order, A gas barrier laminate, in which the rate of change in dimensions of the paper base material in a CD direction in a 40°C, 90% RH environment relative to the dimensions in a 40°C, 20% RH environment is 1% or less. [2] The gas barrier laminate according to [1], wherein the dimensional change rate is 0.7% or less. [3] The gas barrier laminate according to [1] or [2], wherein the first resin layer contains a polyurethane-based resin. [4] The gas barrier laminate according to any one of [1] to [3], wherein the first resin layer has a thickness of 0.3 to 10 μm. [5] The gas barrier laminate according to any one of [1] to [4], further comprising a second resin layer on the vapor deposition layer. [6] The gas barrier laminate according to [5], wherein the second resin layer contains a polyolefin resin. [7] A packaging bag comprising the gas barrier laminate according to any one of [1] to [6]. Effect of the Invention
[0008] According to the present invention, it is possible to provide a gas barrier laminate using paper, in which deterioration of water vapor barrier properties over time is suppressed, and a packaging bag including the gas barrier laminate. Since the gas barrier laminate uses paper, it can also contribute to reducing the amount of plastic materials used. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic cross-sectional view showing a gas barrier laminate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings as needed. However, the present invention is not limited to the following embodiments.
[0011] <Gas barrier laminate> Fig. 1 is a schematic cross-sectional view showing a gas barrier laminate according to one embodiment. The gas barrier laminate 10 according to one embodiment comprises, in this order, a paper substrate 1, a first resin layer 2, and a vapor deposition layer 3. As shown in the figure, the gas barrier laminate 10 may further comprise a second resin layer 4 on the vapor deposition layer 3.
[0012] The thickness of the gas barrier laminate 10 may be 20 μm or more, 30 μm or more, or 40 μm or more, and may be 150 μm or less, 100 μm or less, or 70 μm or less. When the thickness of the gas barrier laminate 10 is within the above range, the gas barrier laminate 10 can have better water vapor barrier properties.
[0013] [Paper base material] The dimensional change rate in the cross direction, where the dimensional change is large, is important from the viewpoint of suppressing the deterioration of the water vapor barrier property over time. That is, the dimensional change rate in the cross direction of the dimensions of the paper base material 1 in a 40°C, 90% RH environment relative to the dimensions in a 40°C, 20% RH environment is 1% or less, but may be 0.9% or less, 0.7% or less, or 0.6% or less. The lower limit of the dimensional change rate is not particularly limited, but may be 0% or more, or 0.1% or more. By using such a paper base material 1, deterioration of the water vapor barrier properties of the gas barrier laminate over time is suppressed.
[0014] The present inventors speculate as follows about the reason why the above-mentioned effects are achieved. It is believed that the vapor deposition layer 3 has not only minute defects that may occur during the formation of the vapor deposition layer 3, but also a considerable number of minute cracks or defects due to scratches during transportation or scratches due to transfer-through when wound into a roll. If the dimensional change rate of the paper base material 1 exceeds 1%, large cracks caused by these minute cracks or defects (for example, cracks with a short side in the CD direction and a long side in the MD direction, an aspect ratio (MD / CD) of 10 or more, and a long side length of 3 μm or more) are likely to occur. This leads to a decrease in water vapor barrier properties. In contrast, by keeping the dimensional change rate at 1% or less, it is possible to prevent the minute cracks or defects in the vapor deposition layer 3 from becoming larger, and good water vapor barrier properties can be obtained.
[0015] On the other hand, since the dimensional change in the MD (Machine Direction) is extremely small compared to the CD, the dimensional change rate in the MD does not need to be specified in particular from the viewpoint of suppressing deterioration of the water vapor barrier property over time. However, the dimensional change rate in the MD of the paper base material 1 in a 40°C, 90% RH environment relative to the dimensions in a 40°C, 20% RH environment may be, for example, 0.15% or less.
[0016] The dimensional change rates in the MD and CD of the paper base material 1 in a 40° C., 90% RH environment relative to the dimensions in a 40° C., 20% RH environment were measured by the following method. (Dimensional change rate measurement method) The paper substrate is cut to a predetermined size (for example, 150 mm length in the MD or CD direction of the paper substrate × 20 mm width) to prepare a sample for measurement. This sample is left in a thermostatic chamber at 40°C and 20% RH for 24 hours, and then the length of the sample is measured in the thermostatic chamber. The sample is left in a thermo-hygrostat chamber at 40° C. and 90% RH for 24 hours, and then the length of the sample is measured in the thermo-hygrostat chamber. The dimensional change rate (%) of the sample in a 40° C., 90% RH environment relative to the size in a 40° C., 20% RH environment is calculated according to the following formula. {(Length at 40℃ 90% RH - Length at 40℃ 20% RH) / Length at 40℃ 20% RH} x 100
[0017] The dimensional change rate of the paper base material 1 can be adjusted, for example, by changing the fiber length of the fibers that make up the paper base material, the density of the paper base material, the filler content in the coating layer, the basis weight of the paper base material, the degree of chemical modification of the paper base material (for example, the degree of treatment with sulfuric acid solution in parchment paper), etc.
[0018] The MD and CD directions of the paper substrate can be determined, for example, as follows. When the paper substrate is a roll paper, the long conveying direction is the MD direction, and the direction perpendicular to the MD direction is the CD direction. In the paper substrate, the pulp fibers tend to be oriented in the MD direction, so the dimensional change of the paper substrate tends to be greater in the CD direction than in the MD direction, as described above. In addition, the MD direction and CD direction of the gas barrier laminate are the same as the MD direction and CD direction of the paper substrate, respectively, and the dimensional change of the gas barrier laminate also tends to be greater in the CD direction than in the MD direction. Therefore, the MD direction and CD direction of the paper substrate and the gas barrier laminate can be distinguished by the orientation direction of the fibers in the paper substrate and the difference in the dimensional change rate depending on the direction of the paper substrate or the gas barrier laminate. As an example of a method of distinction, the paper substrate or the gas barrier laminate cut into a circle with a diameter of about 5 cm is floated in water for about 2 minutes, and the axial direction of the curl when it curls can be judged as the MD direction.
[0019] The paper base material 1 is not particularly limited, but a paper base material that can keep the dimensional change rate to 1% or less can be selected and used. The paper base material 1 may be paper whose main component is plant-derived pulp. Specific examples of the paper base material 1 include fine paper, special fine paper, coated paper, art paper, cast-coated paper, imitation paper, craft paper, parchment paper, and glassine paper. The basis weight of the paper base material 1 is 20 g / m 2 or more, and 2 or more, and 2 or less, and2 It may be the following:
[0020] The paper base material 1 may have a coating layer at least on the side of the paper base material 1 that contacts the first resin layer 2. When the paper base material 1 has a coating layer, the paper base material 1 may have at least a paper layer and a coating layer. The coating layer may be provided on both surfaces of the paper base material 1. By providing a coating layer, it is possible to prevent the first resin layer 2 from penetrating into the paper, and it is also possible to play a role of filling in unevenness in the paper, making it easier to form the first resin layer 2 uniformly without defects. It also makes it easier to suppress dimensional changes in the paper base material 1. The coating layer may contain, for example, as a binder resin, various copolymers such as styrene-butadiene, styrene-acrylic, and ethylene-vinyl acetate copolymers, polyvinyl alcohol resin, cellulose resin, paraffin (wax), etc., and as a filler, clay, kaolin, calcium carbonate, talc, mica, etc. The coating layer may be a clay coating layer that contains at least clay as a filler.
[0021] When the paper base material 1 has a coating layer, the thickness of the coating layer may be 1.5 μm or more and 15 μm or less. The thickness of the coating layer may be 1.8 μm or more, 3 μm or more, 5 μm or more, or 6 μm or more. The thickness of the coating layer may be 12 μm or less, or 10 μm or less. If the thickness of the coating layer is within the above range, dimensional changes of the paper base material 1 are easily suppressed.
[0022] The thickness of the paper substrate 1 may be 20 μm or more, 30 μm or more, 40 μm or more, 100 μm or less, 80 μm, or 60 μm. When the thickness of the paper substrate 1 is within the above range, the gas barrier laminate 10 can have better water vapor barrier properties.
[0023] The ratio of the thickness of the coating layer to the thickness of the paper base 1 may be 3 to 25%, or 5 to 20%. If this ratio is within the above range, dimensional changes in the paper base 1 are easily suppressed.
[0024] The average fiber length of the fibers in the paper base 1 may be 100 μm or more and 2000 μm or less. The average fiber length of the fibers in the paper base 1 may be 200 μm or more, 400 μm or more, or 500 μm or more. The average fiber length of the fibers in the paper base 1 may be 1500 μm or less, 1300 μm or less, 1100 μm or less, or 1000 μm or less.
[0025] By setting the average fiber length of the fibers of the paper base material 1 to be equal to or greater than the lower limit, the fibers are easily entangled with each other, and dimensional changes caused when the paper base material swells are easily suppressed. In addition, the paper base material is easily able to maintain a strength suitable for use as a packaging material. By setting the average fiber length of the fibers in the paper base 1 to the above upper limit or less, the absolute value of the change in fiber length when the paper base swells tends to be small, making it easier to suppress dimensional changes in the paper base.
[0026] The average fiber diameter of the fibers in the paper base 1 is not particularly limited, but may be from 1 μm to 200 μm, from 5 μm to 150 μm, or from 5 μm to 100 μm.
[0027] The average fiber length and average fiber diameter of the fibers in the paper base material 1 are the average values of the fiber lengths and fiber diameters of 30 arbitrarily selected fibers, and are measured by the following method. (Method of measuring average fiber length and average fiber diameter) Paper (paper base material) cut to a specified size is immersed in 200 ml of 0.6% sodium hydroxide aqueous solution and stirred with a stirrer in a 50°C environment for 24 hours to disintegrate the fibers. The solution containing the disaggregated fibers is dropped onto a slide glass with a dropper and allowed to dry naturally. The fiber lengths and diameters of 30 fibers on the slide glass are measured using a microscope, and the average fiber length and average fiber diameter are calculated from the average values.
[0028] The density of the paper base material 1 is 0.9 g / cm 3 More than 1.5g / cm 3 The density of the paper substrate 1 may be 0.95 g / cm3 or more, 1.0 g / cm 3 or more, 1.1 g / cm 3 The density of the paper base material 1 may be 1.4 g / cm or more. 3 It may be less than 1.3 g / cm 3 It may be less than 1.2 g / cm 3 It may be the following. The density of paper base 1 is 0.9 g / cm 3 By setting the density of the paper substrate 1 to the above value, it is easy to suppress dimensional changes in the paper substrate 1, and the surface becomes smooth, so that the smoothness of the first resin layer 2 and the deposition layer 3 can be improved. As a result, the gas barrier laminate 10 can obtain better water vapor barrier properties. In addition, when the density of the paper substrate 1 is set to 1.5 g / cm 3 By setting it as follows, it is possible to form appropriate gaps between the fibers of the paper base material 1 and to alleviate the stress applied to the paper base material 1. As a result, it is possible to prevent cracks or defects in the vapor deposition layer 3 from becoming large, and the gas barrier laminate 10 can obtain better water vapor barrier properties. The density of the paper base material 1 is a value measured in accordance with JIS P8118.
[0029] The weight of the paper is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, based on the weight of the entire gas barrier laminate. If the weight of the paper is 50% by mass or more based on the weight of the entire gas barrier laminate, the amount of plastic material used can be sufficiently reduced, the gas barrier laminate as a whole can be said to be made of paper, and recyclability is excellent.
[0030] [First resin layer] The first resin layer 2 is provided on the surface of the paper base material 1 to improve adhesion between the paper base material 1 and a deposition layer 3 described below, and to improve the gas barrier properties of the gas barrier laminate. The first resin layer is also called an anchor coat layer. The first resin layer 2 may contain a polyurethane resin. The polyurethane resin has good wettability, and therefore has excellent coating stability, resulting in good adhesion between the paper substrate 1 and the deposition layer 3. Furthermore, the first resin layer 2 has good surface smoothness, which makes it easier to form a dense deposition layer 3, resulting in better water vapor barrier properties. Furthermore, a layer containing a polyurethane resin has higher rigidity than, for example, a layer containing a polyolefin resin, and therefore is less likely to follow dimensional changes in the paper substrate 1. Therefore, it is easier to prevent cracks or defects in the deposition layer 3 from becoming larger, and good water vapor barrier properties can be obtained. By using a polyurethane resin having water vapor barrier properties, further improvement in gas barrier properties can be expected.
[0031] From the viewpoint of water vapor barrier property, the polyurethane resin preferably contains at least one of a meta-xylylene diisocyanate-derived structural unit and a hydrogenated meta-xylylene diisocyanate-derived structural unit. When the polyurethane resin contains such a structural unit, it exhibits high cohesive strength due to hydrogen bonds and a stacking effect between xylylene groups, and therefore tends to have even better water vapor barrier property. From the viewpoint of coatability, the coating liquid used in forming the first resin layer 2 containing a polyurethane resin is preferably a coating liquid in which the polyurethane resin is dispersed in water, such as a dispersion or emulsion. An example of such a coating liquid is Takelac WPB manufactured by Mitsui Chemicals, Inc.
[0032] The first resin layer 2 may contain components other than the polyurethane resin, such as polyolefin, silane coupling agent, organic titanate, polyacrylic acid, polyester, polycarbonate, polyurea, polyamide, polyimide, melamine, and phenol.
[0033] The content of the polyurethane resin in the first resin layer 2 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass. If the content of the polyurethane resin is 50% by mass or more, it is easy to enjoy the above-mentioned effects and advantages of using the polyurethane resin.
[0034] The rigidity of the polyurethane resin can be evaluated by measuring the hardness of a layer containing the polyurethane resin by a nanoindentation method. The hardness of the layer containing a polyurethane resin measured by a nanoindentation method may be 0.2 GPa or more, and may be 0.3 GPa or more. The upper limit of the hardness is not particularly limited, but may be 1.0 GPa or less.
[0035] (Measurement method) The nanoindentation method is a measurement method in which a quasi-static indentation test is performed on a target object to obtain the mechanical properties of the sample. As a measurement device, a Hysitron TI-Premier (product name) manufactured by Bruker Japan Co., Ltd. can be used. As an indenter, a Berkovich type diamond indenter manufactured by Bruker Japan Co., Ltd. can be used.
[0036] The sample for measurement is not particularly limited as long as it can be appropriately measured (measured on a cross section) by the nanoindentation method, and for example, a laminate having a layer containing a polyurethane resin can be used. Examples of such a laminate include a paper base material and a first resin layer (a layer containing a polyurethane resin), or a paper base material, a first resin layer, and a second resin layer.
[0037] In nanoindentation measurements, a diamond indenter is first scanned across the cross section of the sample to obtain a topographical image of the sample, and the measurement position of the desired layer is specified. Then, in a displacement control mode at room temperature (25°C), the indenter is indented to a depth of 80 nm at a indentation speed of 80 nm / s, and the maximum depth is held for 1 second, after which the indenter is unloaded at a speed of 80 nm / s. To calculate the hardness, the relationship between the contact depth and the contact projection area between the indenter and the sample is calibrated in advance using fused quartz as a standard sample.Then, the unloading curve in the 60-95% range of the maximum load at the time of unloading is analyzed using the Oliver-Pharr method to calculate the hardness. The sample is cut into strips or wedges with a razor and embedded in resin. Toa Gosei's D-800 photocurable resin is used as the embedding resin, which is hardened by exposure to light after embedding. The hardened sample embedding resin is fixed in an insert for an AFM sample holder, and the sample is trimmed and cross-sectioned with a glass knife at room temperature (25°C), and then cross-sectioned with a diamond knife until it becomes mirror-like (cutting speed 1.0 mm / s, cut film thickness 200 nm). The cross-sectioned sample is fixed in an insert for an AFM sample holder and used for measurement by the nanoindentation method. A Leica ultramicrotome EM UC7 can be used as the cross-section cutting device. The cutting direction is parallel to the layer interface of the sample.
[0038] The thickness of the first resin layer 2 may be, for example, 0.3 μm or more, 0.5 μm or more, 1 μm or more, 2 μm or more, 10 μm or less, or 5 μm or less. If the thickness of the first resin layer 2 is 0.5 μm or more, the unevenness of the paper base material 1 described above can be efficiently filled, and the deposition layer 3 described later can be laminated uniformly. In addition, it can be a layer that is difficult to follow the dimensional change of the paper base material 1. If the thickness of the first resin layer 2 is 20 μm or less, the deposition layer 3 can be laminated uniformly while suppressing costs.
[0039] Examples of the solvent contained in the coating liquid for the first resin layer 2 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Furthermore, from the viewpoint of the environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.
[0040] The first resin layer 2 can be provided by applying a coating liquid containing the above-mentioned polyurethane resin and a solvent onto the paper substrate 1 and drying it. The average particle size of the polyurethane resin in the coating liquid is preferably large in order to reduce the contact area and suppress blocking. Although not particularly limited, the average particle size of the polyurethane resin may be 1 nm or more, 0.1 μm or more, 1 μm or less, 0.7 μm or less, or 0.5 μm or less.
[0041] [Vapour-deposited layer] Examples of the vapor-deposited layer 3 include a metal vapor-deposited layer and an inorganic oxide vapor-deposited layer. The vapor-deposited layer 3 may contain aluminum, and may be aluminum oxide (AlO x ), silicon oxide (SiO x ) etc.
[0042] The thickness of the deposition layer 3 may be appropriately set depending on the application, and may be 10 nm or more, 30 nm or more, 300 nm or less, or 100 nm or less. By setting the thickness of the deposition layer 3 to 10 nm or more, it is easy to ensure sufficient continuity of the deposition layer 3, and by setting the thickness to 300 nm or less, it is easy to sufficiently suppress the occurrence of curling and cracking, and it is easy to achieve sufficient gas barrier performance and flexibility. Furthermore, by setting the thickness of the deposition layer 3 to 30 nm or more and 100 nm or less, the deposition layer 3 becomes less likely to crack, and water vapor barrier property is more easily obtained.
[0043] The deposition layer 3 is preferably formed by a vacuum deposition method from the viewpoint of water vapor and oxygen gas barrier performance and film uniformity. There are known deposition methods such as vacuum deposition, sputtering, and chemical vapor deposition (CVD), but vacuum deposition is preferred because of its high deposition rate and high productivity. Among the vacuum deposition methods, deposition by electron beam heating is particularly preferred because the deposition rate is easily controlled by the irradiation area and electron beam current, and the deposition material can be heated and cooled in a short time.
[0044] [Second resin layer] The second resin layer 4 is provided on the surface of the vapor-deposited layer 3 so as to be in contact with the vapor-deposited layer 3. The second resin layer is also called an overcoat layer. The second resin layer may contain a polyolefin-based resin, and may contain a polyolefin-based resin having a polar group.
[0045] The polyolefin resin having a polar group may have at least one selected from a carboxy group, a salt of a carboxy group, a carboxylic anhydride group, and a carboxylic ester.
[0046] Examples of the polyolefin resin include ethylene and propylene. Examples of the polyolefin resin having a polar group include ethylene or propylene copolymerized with an unsaturated carboxylic acid (an unsaturated compound having a carboxy group such as acrylic acid or methacrylic acid, or a salt obtained by neutralizing the compound with a basic compound) or an unsaturated carboxylic acid ester, and other resins may also be used. In addition, ethylene or propylene copolymerized with vinyl acetate, an epoxy compound, a chlorine compound, a urethane compound, a polyamide compound, and other resins may also be used.
[0047] Specific examples of polyolefin resins having a polar group include copolymers of acrylic acid ester and maleic anhydride, ethylene-vinyl acetate copolymers, and ethylene-glycidyl methacrylate copolymers. From the viewpoint of coatability, the coating liquid used in forming the second resin layer 4 containing the polyolefin resin having a polar group is preferably a coating liquid in which the polyolefin resin having a polar group is dispersed in water, such as a dispersion or emulsion. An example of such a coating liquid is Chemipearl S500 manufactured by Mitsui Chemicals.
[0048] By including a polyolefin resin having a polar group, the flexibility of the second resin layer 4 is improved, and cracking of the deposition layer 3 after bending (folding) can be suppressed, and the polar group of the polyolefin resin improves the adhesion between the second resin layer 4 and the deposition layer 3. Furthermore, by including a polyolefin resin having a polar group, the second resin layer 4 becomes a dense layer due to the crystallinity of the polyolefin resin, and water vapor barrier properties are expressed. Furthermore, since the second resin layer 4 includes the polyolefin resin having the polar group, it can also function as a heat seal layer, so there is no need to provide a separate heat seal layer.
[0049] The second resin layer 4 may contain other components in addition to the polyolefin resin having a polar group, such as a silane coupling agent, an organic titanate, polyacrylic acid, polyester, polyurethane, polycarbonate, polyurea, polyamide, polyolefin having no polar group, polyimide, melamine, phenol, etc.
[0050] The content of the polyolefin resin having a polar group in the second resin layer 4 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass. If the content of the polyolefin resin having a polar group is 50% by mass or more, it is easy to enjoy the above-mentioned effects and advantages of using the polyolefin resin having a polar group.
[0051] The thickness of the second resin layer 4 may be, for example, 0.05 μm or more, 0.5 μm or more, 1 μm or more, 2 μm or more, 20 μm or less, 10 μm or less, or 5 μm or less. If the thickness of the second resin layer 4 is 0.05 μm or more, the layer can fully fulfill the role of the heat seal layer described above. If the thickness of the second resin layer 4 is 20 μm or less, the layer can fully exert adhesion to the deposition layer 3 and water vapor barrier properties while suppressing costs. If the thickness of the second resin layer 4 is 2 μm or more and 10 μm or less, the deposition layer 3 is less likely to crack, and water vapor barrier properties are more easily obtained.
[0052] Examples of the solvent contained in the coating liquid for the second resin layer 4 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Furthermore, from the viewpoint of the environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.
[0053] The second resin layer 4 can be provided by applying a coating liquid containing the above-mentioned polyolefin resin having a polar group and a solvent on the deposition layer 3 and drying it. The melting point of the polyolefin resin having a polar group is preferably 70°C or more or 80°C or more, and more preferably 160°C or less or 120°C or less. If the melting point of the polyolefin resin having a polar group is low, there is an advantage that the start-up temperature during heat sealing can be lowered. If the melting point of the polyolefin resin having a polar group is high, there is a risk of blocking in a high-temperature environment. The average particle size of the polyolefin having a polar group is preferably large from the viewpoint of reducing the contact area and suppressing blocking. Although not particularly limited, the average particle size of the polyolefin resin having a polar group may be 1 nm or more, 0.1 μm or more, 1 μm or less, 0.7 μm or less, or 0.5 μm or less.
[0054] <Packaging bag> The packaging bag includes the gas barrier laminate. The packaging bag is produced by making the gas barrier laminate. Examples of the packaging bag include a gusset bag, a pillow bag, a three-side sealed bag, a standing pouch, and the like.
[0055] The packaging bag can contain food, medicine, and the like. It is particularly suitable for containing food, such as confectionery. Since the packaging bag according to the present embodiment includes the gas barrier laminate, it can be said that the water vapor barrier property of the packaging bag is unlikely to deteriorate over time. EXAMPLES
[0056] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0057] <Preparation of paper substrate> Manufactured by Fuji Kako Co., Ltd., Product name: Tokukomo S, thickness 47μm, basis weight 52.3g / m 2 , average fiber length 885.8 μm, with clay coat layer. Manufactured by Daio Paper Co., Ltd., product name: Ryuo Coat, thickness 50μm, basis weight 55g / m 2 , average fiber length 824.1 μm, with clay coat layer. Xianhe Co., Ltd. coated packaging paper, thickness 55μm, basis weight 60g / m 2 , average fiber length 877.6 μm, with clay coat layer. -Manufactured by UPM, product name: Asend, thickness 60μm, basis weight 65g / m 2 , average fiber length 1040.2 μm, with clay coat layer. Manufactured by UPM, product name: Brilliant Duo, thickness 55μm, basis weight 60g / m 2 , average fiber length 1471.8 μm, with clay coat layer.
[0058] <Preparation of gas barrier laminate> (Examples 1 to 4) A water dispersion containing a polyurethane resin (Takelac XWPB-LJ4 manufactured by Mitsui Chemicals) was applied onto the surface of the paper substrate shown in Table 1 using a bar coater (wet application amount 15 g / m 2 The mixture was cooled to a solid content of 20 mass %, and then dried in an oven to form a first resin layer (thickness: 3 μm, hardness measured by nanoindentation method: 0.36 GPa). On the formed first resin layer, Al was deposited by vacuum deposition to form an Al deposited layer (thickness: 50 nm), thereby obtaining a gas barrier laminate.
[0059] Example 5 A gas barrier laminate was obtained in the same manner as in Example 1, except that the vapor deposition layer was changed to an alumina vapor deposition layer (thickness: 30 nm) formed by vacuum vapor deposition.
[0060] Example 6 A gas barrier laminate was obtained in the same manner as in Example 1, except that the vapor deposition layer was replaced with a silica vapor deposition layer (thickness: 30 nm) formed by vacuum vapor deposition.
[0061] (Examples 7 to 10) A water dispersion containing a polyurethane resin (Takelac XWPB-LJ4 manufactured by Mitsui Chemicals) was applied onto the surface of the paper substrate shown in Table 1 using a bar coater (wet application amount 15 g / m 2 The mixture was cooled to a solid content of 20 mass %, and then dried in an oven to form a first resin layer (thickness: 3 μm, hardness measured by nanoindentation method: 0.36 GPa). On the formed first resin layer, Al was deposited by vacuum deposition to form an Al deposited layer (thickness: 50 nm). A water dispersion of polyolefin containing a salt of a carboxyl group (Chemipearl S500 manufactured by Mitsui Chemicals, Inc.) was applied onto the Al vapor deposition layer using a bar coater and dried in an oven to form a second resin layer (thickness 3 μm). This resulted in a gas barrier laminate.
[0062] (Comparative Examples 1 to 4) Except for changing the paper base material as shown in Table 2, gas barrier laminates were obtained in the same manner as in Examples 1 and 5 to 7, respectively.
[0063] <Measurement of dimensional change rate> Each paper substrate was cut into a size of 150 mm length in the CD direction × 20 mm width to prepare a measurement sample. The sample was left in a thermo-hygrostat at 40°C and 20% RH for 24 hours, and then the length of the sample in the CD direction was measured using a glass scale in the thermo-hygrostat. The sample was left in a thermo-hygrostat at 40° C. and 90% RH for 24 hours, and then the length of the sample in the CD direction was measured using a glass scale in the thermo-hygrostat. The dimensional change rate (%) in the CD direction of the sample in a 40° C., 90% RH environment relative to the dimension in a 40° C., 20% RH environment was calculated using the following formula. {(Length at 40℃ 90% RH - Length at 40℃ 20% RH) / Length at 40℃ 20% RH} x 100 The same procedure was carried out on a sample cut to a size of 150 mm in length and 20 mm in width in the MD direction. The results are shown in Tables 1 and 2.
[0064] <Measurement of water vapor permeability> In order to observe the change in water vapor permeability over time, the water vapor permeability (g / m2) of the gas barrier laminate was measured under the following two conditions. 2 The results are shown in Tables 1 and 2. Condition 1: The gas barrier laminate obtained in each example was left in a thermo-hygrostat at 23° C. and 50% RH for 24 hours, and then the water vapor permeability of the gas barrier laminate was measured by the MOCON method. Condition 2: The gas barrier laminate obtained in each example was left in a thermo-hygrostat at 40° C. and 90% RH for 24 hours, and then the water vapor permeability of the gas barrier laminate was measured by the MOCON method. (MOCON method measurement conditions) Measurement equipment: MOCON, PERMATRAN3 / 34G Temperature and humidity: 40℃ 60% RH Conditioning: 60 minutes Measurement time: 30 minutes Number of measurements: 5 (data after 5 measurements used)
[0065] <Crack Observation> In the above "Water vapor permeability measurement", the water vapor measurement area of the sample where the water vapor permeability was measured under condition 2 was observed using an optical microscope (K.S. Olympus BX51 (magnification 5x)) with the maximum amount of transmitted light. Then, the presence or absence of cracks was judged according to the following criteria at 10 randomly observed points, and the number of points where cracks were observed was recorded. The results are shown in Tables 1 and 2. Criteria: When three or more pieces of transmitted light leakage were observed with the short side in the CD direction and the long side in the MD direction, the aspect ratio (MD / CD) being 10 or more, and the long side length being 3 μm or more, the observed location was determined to have a crack.
[0066] [Table 1]
[0067] [Table 2]
[0068] As shown in Tables 1 and 2, the gas barrier laminates of the Examples corresponding to the present invention significantly suppressed the deterioration of the water vapor barrier property over time (accelerated test) compared to the gas barrier laminates of the Comparative Examples. It can be said that the gas barrier laminate of the present invention can suppress the deterioration of the contents for a long period of time. [Explanation of symbols]
[0069] Reference Signs List 1: paper base material, 2: first resin layer, 3: vapor deposition layer, 4: second resin layer, 10: gas barrier laminate.
Claims
1. A gas barrier laminate comprising a paper substrate, a first resin layer, and a deposition layer in this order, A gas barrier laminate, in which the rate of change in dimensions of the paper base material in a CD direction in a 40°C, 90% RH environment relative to the dimensions in a 40°C, 20% RH environment is 1% or less.
2. The gas barrier laminate according to claim 1 , wherein the dimensional change rate is 0.7% or less.
3. The gas barrier laminate according to claim 1 , wherein the first resin layer comprises a polyurethane resin.
4. 3. The gas barrier laminate according to claim 1, wherein the first resin layer has a thickness of 0.3 to 10 μm.
5. The gas barrier laminate according to claim 1 or 2, further comprising a second resin layer on the vapor deposition layer.
6. The gas barrier laminate according to claim 5 , wherein the second resin layer contains a polyolefin resin.
7. A packaging bag comprising the gas barrier laminate according to claim 1 or 2.